Perovskite solar cell and preparation method therefor, and photovoltaic module

By incorporating a composite protective layer of boron nitride and graphene into perovskite solar cells, the stability problem of perovskite solar cells has been solved, enabling efficient and low-cost production and improving cell performance and lifespan.

WO2024244083A1PCT designated stage expired Publication Date: 2024-12-05SHENZHEN HANKE NEW MATERIAL TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/103101
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-30
Filing Date
2023-06-28
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The poor long-term stability of perovskite solar cells limits their further development and the fabrication methods of other functional layers.

Method used

A composite protective layer, including a boron nitride layer and a graphene material layer, is set on the perovskite layer. Each functional layer is prepared by sputtering to improve stability and production efficiency.

Benefits of technology

This improved the long-term stability of perovskite solar cells, reduced production costs and energy consumption, enhanced carrier conductivity, and broadened the fabrication process of functional layers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023103101_05122024_PF_FP_ABST
    Figure CN2023103101_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure provides a perovskite solar cell and a preparation method therefor, and a photovoltaic module. The perovskite solar cell comprises a substrate, a first charge extraction layer (120), a perovskite layer (130), a composite protective layer (140), and a second charge extraction layer (150), wherein the composite protective layer (140) comprises a boron nitride layer (141) and a graphene material layer (142) which are sequentially stacked on the perovskite layer (130).
Need to check novelty before this filing date? Find Prior Art

Description

Perovskite solar cell and preparation method thereof, photovoltaic module

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on May 30, 2023, with application number 202310621856X and invention name “Perovskite solar cells and their preparation methods, photovoltaic modules”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present disclosure relates to the technical field of solar cells, and in particular to a perovskite solar cell and a preparation method thereof, and a photovoltaic module. Background Art

[0003] Perovskite solar cells are solar cells that use a compound with a perovskite structure as a light-absorbing layer. Compared to the currently commonly used crystalline silicon solar cells, perovskite solar cells have advantages such as a wider absorption range and a higher absorption coefficient. In the laboratory, the efficiency of perovskite solar cells has gradually increased from the initial 3.8% to more than 25.7% today. In addition, perovskite solar cells can also be combined with crystalline silicon solar cells to form a stacked structure to broaden the overall absorption spectrum range of the solar cell. Although perovskite solar cells have the above advantages, the long-term stability of perovskite solar cells is still a major problem hindering their further development. In addition, the poor stability of perovskite materials also limits the preparation methods of other functional layers of solar cells.

[0004] Summary of the Invention

[0005] According to some embodiments of the present disclosure, a perovskite solar cell is provided, which includes: a substrate, a first charge extraction layer, a perovskite layer, a composite protective layer, and a second charge extraction layer; the first charge extraction layer, the perovskite layer, the composite protective layer, and the second charge extraction layer are sequentially stacked on the substrate, and the composite protective layer includes a boron nitride layer and a graphene material layer sequentially stacked on the perovskite layer.

[0006] In some embodiments of the present disclosure, the thickness of the boron nitride layer is ≤10 nm.

[0007] In some embodiments of the present disclosure, the thickness of the graphene material layer is ≤10 nm.

[0008] In some embodiments of the present disclosure, the boron nitride layer is in direct contact with the perovskite layer, and the graphene material layer is in direct contact with the boron nitride layer.

[0009] In some embodiments of the present disclosure, the first charge extraction layer is an electron transport layer, and a material of the first charge extraction layer is selected from one or more of fullerene, tin oxide, tungsten sulfide, zinc oxide, titanium oxide, tungsten oxide, and indium gallium zinc oxide.

[0010] In some embodiments of the present disclosure, the second charge extraction layer is a hole transport layer, and a material of the second charge extraction layer is selected from one or more of nickel oxide, copper oxide, copper sulfide, molybdenum sulfide, vanadium oxide, tungsten oxide and copper thiocyanate.

[0011] Furthermore, the present disclosure also provides a method for preparing a perovskite solar cell, which comprises the following steps:

[0012] providing a substrate;

[0013] preparing a first charge extraction layer on the substrate;

[0014] forming a perovskite layer on the first charge extraction layer;

[0015] sequentially preparing a boron nitride layer and a graphene material layer on the perovskite layer to form a composite protective layer;

[0016] A second charge extraction layer is prepared on the graphene material layer.

[0017] In some embodiments of the present disclosure, the thickness of the boron nitride layer is ≤10 nm.

[0018] In some embodiments of the present disclosure, the thickness of the graphene material layer is ≤10 nm.

[0019] In some embodiments of the present disclosure, the boron nitride layer is in direct contact with the perovskite layer, and the graphene material layer is in direct contact with the boron nitride layer.

[0020] In some embodiments of the present disclosure, the first charge extraction layer is an electron transport layer, and a material of the first charge extraction layer is selected from one or more of fullerene, tin oxide, tungsten sulfide, zinc oxide, titanium oxide, tungsten oxide, and indium gallium zinc oxide.

[0021] In some embodiments of the present disclosure, the second charge extraction layer is a hole transport layer, and a material of the second charge extraction layer is selected from one or more of nickel oxide, copper oxide, copper sulfide, molybdenum sulfide, vanadium oxide, tungsten oxide and copper thiocyanate.

[0022] In some embodiments of the present disclosure, the boron nitride layer is prepared by sputtering, and the graphene material layer is prepared by sputtering.

[0023] In some embodiments of the present disclosure, in the step of preparing the boron nitride layer, hexagonal boron nitride is used as a sputtering target, the sputtering power is controlled to be 200W to 350W, and the sputtering time is controlled to be 1min to 10min.

[0024] In some embodiments of the present disclosure, in the step of preparing the graphene material layer, graphite is used as a sputtering target, the sputtering power is controlled to be 300W to 400W, and the sputtering time is controlled to be 1 min to 10 min.

[0025] In some embodiments of the present disclosure, the first charge extraction layer, the perovskite layer, the boron nitride layer, the graphene material layer and the second charge extraction layer are sequentially prepared in a sputtering chamber by sputtering.

[0026] In some embodiments of the present disclosure, the substrate includes a base material and a first electrode disposed on the base material. Before preparing the first charge extraction layer, the step of plasma cleaning the base material is further included.

[0027] In some embodiments of the present disclosure, after preparing the second charge extraction layer, the method further includes preparing a second electrode on the second charge extraction layer, and the second electrode is prepared by sputtering.

[0028] According to some embodiments of the present disclosure, a photovoltaic component is also provided, which includes a packaging structure and a perovskite solar cell encapsulated by the packaging structure, wherein the perovskite solar cell includes: a substrate, a first charge extraction layer, a perovskite layer, a composite protective layer and a second charge extraction layer; the first charge extraction layer, the perovskite layer, the composite protective layer and the second charge extraction layer are sequentially stacked on the substrate, and the composite protective layer includes a boron nitride layer and a graphene material layer sequentially stacked on the perovskite layer.

[0029] In some embodiments of the present disclosure, the thickness of the boron nitride layer is ≤10 nm.

[0030] In some embodiments of the present disclosure, the thickness of the graphene material layer is ≤10 nm.

[0031] In some embodiments of the present disclosure, the boron nitride layer is in direct contact with the perovskite layer, and the graphene material layer is in direct contact with the boron nitride layer.

[0032] In some embodiments of the present disclosure, the first charge extraction layer is an electron transport layer, and a material of the first charge extraction layer is selected from one or more of fullerene, tin oxide, tungsten sulfide, zinc oxide, titanium oxide, tungsten oxide, and indium gallium zinc oxide.

[0033] In some embodiments of the present disclosure, the second charge extraction layer is a hole transport layer, and a material of the second charge extraction layer is selected from one or more of nickel oxide, copper oxide, copper sulfide, molybdenum sulfide, vanadium oxide, tungsten oxide and copper thiocyanate.

[0034] The details of one or more embodiments of the present disclosure are set forth in the accompanying drawings and the description below. Other features, objects, and advantages of the present disclosure will become apparent from the description, drawings, and claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, without paying any creative work, they can also obtain drawings of other embodiments based on these drawings.

[0036] FIG1 is a schematic diagram of a perovskite solar cell;

[0037] FIG2 is a schematic diagram of the steps of the method for preparing the perovskite solar cell in FIG1 ;

[0038] FIG3 is a schematic structural diagram of a substrate;

[0039] FIG4 is a schematic diagram showing the structure of preparing a first charge extraction layer based on the structure shown in FIG3 ;

[0040] FIG5 is a schematic diagram of the structure of preparing a perovskite layer based on the structure shown in FIG4 ;

[0041] FIG6 is a schematic diagram of the structure of preparing a boron nitride layer and a graphene material layer based on the structure shown in FIG5 ;

[0042] FIG7 is a schematic diagram showing the structure of a second charge extraction layer prepared on the basis of the structure shown in FIG6 ;

[0043] Among them, the various figure numbers and their meanings are as follows: 100, substrate; 110, first electrode; 120, first charge extraction layer; 130, perovskite layer; 140, composite protective layer; 141, boron nitride layer; 142, graphene material layer; 150, second charge extraction layer; 160, second electrode. DETAILED DESCRIPTION

[0044] To facilitate understanding of the present disclosure, a more comprehensive description of the present disclosure will be provided below with reference to the accompanying drawings. The drawings illustrate preferred embodiments of the present disclosure. However, the present disclosure can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a more thorough and comprehensive understanding of the present disclosure.

[0045] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this disclosure pertains. The terms used herein in the specification of this disclosure are for the purpose of describing specific embodiments only and are not intended to limit this disclosure. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0046] It should be understood that when an element or layer is referred to as being "on," "adjacent to," "connected to," or "coupled to" another element or layer, it can be directly on, adjacent to, connected to, or coupled to the other element or layer, or there can be intervening elements or layers. The manner of electrical connection is used to indicate that current can be conducted between multiple electrically connected elements, and the specific manner can be that one element directly contacts another element, or that one element is connected to another element through other conductive elements. In contrast, when an element is referred to as being "directly on," "directly adjacent to," "directly connected to," or "directly coupled to" another element or layer, there are no intervening elements or layers. It should be understood that although the terms first, second, third, etc. may be used to describe various elements, components, regions, layers, and / or parts, these elements, components, regions, layers, and / or parts should not be limited by these terms. These terms are merely used to distinguish one element, component, region, layer, or part from another element, component, region, layer, or part. Thus, a first element, component, region, layer or section discussed below could be termed a second element, component, region, layer or section without departing from the teachings of the present disclosure.

[0047] Spatially relative terms such as "under," "beneath," "below," "under," "above," "above," etc., may be used herein for convenience of description to describe the relationship of one element or feature shown in the figures to other elements or features. It should be understood that the spatially relative terms are intended to include different orientations of the device in use and operation in addition to the orientations shown in the figures. For example, if the device in the drawings is flipped, then the elements or features described as "under" or "beneath" or "beneath" the other elements will be oriented as "over" the other elements or features. Thus, the exemplary terms "under" and "under" may include both the upper and lower orientations. The device may be oriented otherwise (rotated 90 degrees or in other orientations) and the spatial descriptors used herein are interpreted accordingly.

[0048] The purpose of the terms used herein is only to describe specific embodiments and is not intended to limit the present disclosure. When used herein, the singular forms "a", "an", and "the" are intended to include the plural forms, unless the context clearly indicates otherwise. It should also be understood that the terms "comprising" and / or "comprising", when used in this specification, determine the presence of the features, integers, steps, operations, elements and / or parts, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, parts and / or groups. When used herein, the term "and / or" includes any and all combinations of the relevant listed items.

[0049] The present disclosure provides a perovskite solar cell, which includes: a substrate, a first charge extraction layer, a perovskite layer, a composite protective layer and a second charge extraction layer; the first charge extraction layer, the perovskite layer, the composite protective layer and the second charge extraction layer are sequentially stacked on the substrate, and the composite protective layer includes a boron nitride layer and a graphene material layer sequentially stacked on the perovskite layer.

[0050] The boron nitride layer may include hexagonal boron nitride, and the graphene material layer may include graphene. The lattice structures of hexagonal boron nitride and graphene are similar, both being hexagonal planar structures. Therefore, graphene and hexagonal boron nitride have good lattice matching. Graphene and hexagonal boron nitride can exhibit strong permeation barriers even with a very small number of layers, thus effectively inhibiting contact between the perovskite material and other external materials.

[0051] In the perovskite solar cell of at least one embodiment of the present disclosure, a first charge extraction layer, a perovskite layer, a composite protective layer and a second charge extraction layer are stacked in sequence. The composite protective layer includes a boron nitride layer and a graphene material layer stacked in sequence. The boron nitride layer has a high lattice matching degree with the graphene material layer and can be used as a preparation substrate for the graphene material layer. Therefore, the composite protective layer can be stably arranged on the perovskite layer. Furthermore, the composite protective layer can have high mechanical strength and chemical stability while maintaining light transmittance. On the one hand, it prevents external impurities from affecting the perovskite layer and improves the long-term stability of the perovskite solar cell. On the other hand, it can also protect the perovskite layer when preparing the second charge extraction layer and other functional layers located above the perovskite layer, which can broaden the actual preparation process of the second charge extraction layer and other functional layers, so that the second charge extraction layer and other functional layers can be prepared with a simpler process.

[0052] To facilitate understanding of the specific structure of the perovskite solar cell provided by the present disclosure, FIG1 is a schematic diagram of a perovskite solar cell.

[0053] 1 , a perovskite solar cell includes a substrate, a first charge extraction layer 120, a perovskite layer 130, a composite protective layer 140, and a second charge extraction layer 150; the first charge extraction layer 120, the perovskite layer 130, the composite protective layer 140, and the second charge extraction layer 150 are sequentially stacked on the substrate, and the composite protective layer 140 includes a boron nitride layer 141 and a graphene material layer 142 sequentially stacked on the perovskite layer 130.

[0054] Furthermore, in some examples of this embodiment, the substrate of the perovskite solar cell includes a base material 100 and a first electrode 110 , and the perovskite solar cell further includes a second electrode 160 .

[0055] The substrate 100 is used to support each functional layer. In some examples of this embodiment, the substrate 100 can be a transparent material. For example, the substrate 100 can be selected from glass or a transparent polymer material. The transparent polymer material can be polyethylene terephthalate (PET) or polyimide (PI). In this embodiment, the substrate 100 is polyethylene terephthalate.

[0056] In some examples of this embodiment, the material of the first electrode 110 may include a transparent conductive metal oxide. For example, the transparent conductive oxide may be selected from one or more of indium tin oxide, indium gallium zinc oxide, aluminum zinc oxide, and fluorine-doped tin oxide. In this embodiment, the transparent conductive oxide may be indium tin oxide.

[0057] In some examples of this embodiment, the first charge extraction layer 120 may be an electron transport layer. Furthermore, the material of the first charge extraction layer 120 may be selected from one or more of fullerene, tin oxide, tungsten sulfide, zinc oxide, titanium oxide, tungsten oxide, and indium gallium zinc oxide. The electron transport layer is used to conduct carriers generated by the perovskite layer 130 to the external electrode, thereby forming a usable current.

[0058] In some examples of this embodiment, the thickness of the first charge extraction layer 120 may be 10 nm to 100 nm. Further, the thickness of the first charge extraction layer 120 may be 10 nm, 20 nm, 30 nm, 50 nm, 80 nm, or 100 nm, or the thickness of the first charge extraction layer 120 may also be within a range between the above thicknesses.

[0059] The perovskite layer 130 is used to absorb light and generate photogenerated carriers. The perovskite layer 130 refers to a semiconductor material having a perovskite lattice structure. In some examples of this embodiment, the material of the perovskite layer 130 may include a compound of the general formula ABX3, where A may be selected from one or more of cesium ions, formamidinium ions (FA), and methylamine ions (MA), B may be selected from lead ions, and X may be selected from halide ions. In this embodiment, the material of the perovskite layer 130 may be iodine lead methylamine (MAPbI3).

[0060] In some examples of this embodiment, the thickness of the perovskite layer 130 may be 100 nm to 1000 nm. Further, the thickness of the perovskite layer 130 may be 100 nm, 200 nm, 300 nm, 500 nm, 800 nm, or 1000 nm, or the thickness of the perovskite layer 130 may also be within the range between the above thicknesses.

[0061] In some examples of this embodiment, the boron nitride layer 141 is in direct contact with the perovskite layer 130. Furthermore, the boron nitride layer 141 covers a surface of the perovskite layer 130 away from the first charge extraction layer 120. The boron nitride layer 141 may include hexagonal boron nitride, which has a layered structure.

[0062] In some examples of this embodiment, the thickness of the boron nitride layer 141 is ≤10 nm. For example, the thickness of the boron nitride layer 141 can be 1 nm to 10 nm. Furthermore, the thickness of the boron nitride layer 141 can be 1 nm, 2 nm, 3 nm, 5 nm, 8 nm, or 10 nm, or the thickness of the boron nitride layer 141 can be within a range between the aforementioned thicknesses. By setting the thickness of the boron nitride layer 141 to be relatively thin, carriers are facilitated to tunnel through the boron nitride layer 141, thereby minimizing carrier loss.

[0063] In some examples of this embodiment, the graphene material layer 142 is in direct contact with the boron nitride layer 141 . Furthermore, the graphene material layer 142 covers a surface of the boron nitride layer 141 that is away from the perovskite layer 130 .

[0064] In some examples of this embodiment, the thickness of the graphene material layer 142 is ≤ 10 nm. For example, the thickness of the graphene material layer 142 may be 1 nm to 10 nm. Furthermore, the thickness of the graphene material layer 142 may be 1 nm, 2 nm, 3 nm, 5 nm, 8 nm, or 10 nm, or the thickness of the graphene material layer 142 may be within a range between the aforementioned thicknesses.

[0065] By using a stacked boron nitride layer 141 and a graphene material layer 142 as the composite protective layer 140, with the boron nitride layer 141 directly disposed on the surface of the perovskite layer 130, it can passivate the perovskite layer 130. Furthermore, the lattice of the boron nitride layer 141 is closely matched to that of graphene. Using it as a substrate for the graphene material layer 142 ensures that the composite protective layer 140 is relatively stable and does not fall off. This composite protective layer 140 effectively protects the perovskite layer 130, ensuring the long-term stability of the perovskite layer 130 without substantially affecting carrier conductivity.

[0066] In conventional technology, the perovskite layer 130 is typically in direct contact with the charge extraction layer to ensure high carrier transfer efficiency between the perovskite layer 130 and the charge extraction layer. In the perovskite solar cell provided herein, a composite protective layer 140 is further provided between the perovskite layer 130 and the second charge extraction layer 150. This composite protective layer 140 ensures the long-term stability of the perovskite layer 130 without substantially affecting carrier conductivity. Furthermore, this composite protective layer 140 has a strong barrier capability against high-speed particles generated during the subsequent sputtering process, enabling the second charge extraction layer 150 to be prepared by sputtering.

[0067] In some examples of this embodiment, the second charge extraction layer 150 may be a hole transport layer. Furthermore, the material of the second charge extraction layer 150 may be selected from one or more of nickel oxide, copper oxide, copper sulfide, molybdenum sulfide, vanadium oxide, tungsten oxide, and copper thiocyanate. The hole transport layer is used to conduct holes generated by the perovskite layer 130 to the external electrode, thereby generating a usable current.

[0068] In some examples of this embodiment, the thickness of the second charge extraction layer 150 may be 10 nm to 100 nm. Further, the thickness of the second charge extraction layer 150 may be 10 nm, 20 nm, 30 nm, 50 nm, 80 nm, or 100 nm, or the thickness of the second charge extraction layer 150 may also be within a range between the above thicknesses.

[0069] In some examples of this embodiment, the material of the second electrode 160 may be a metal material. For example, the material of the second electrode 160 may be selected from one or more of copper, silver, aluminum, gold, and molybdenum.

[0070] In some examples of this embodiment, the thickness of the second electrode 160 may be 50 nm to 500 nm. Further, the thickness of the second electrode 160 may be 50 nm, 100 nm, 200 nm, 300 nm, 400 nm, or 500 nm, or the thickness of the second electrode 160 may be within a range between the above thicknesses.

[0071] It is understood that in the perovskite solar cell of this embodiment, the layers stacked sequentially on the substrate can be prepared sequentially according to their stacking order. In this embodiment, the hole transport layer is disposed above the perovskite layer 130. However, in other embodiments, the hole transport layer can also be disposed below the perovskite layer 130 and the electron transport layer can be disposed above the perovskite layer 130. This also falls within the scope of the perovskite solar cell provided by the present disclosure.

[0072] Figure 2 is a schematic diagram of the steps of the method for preparing the perovskite solar cell in Figure 1. Referring to Figure 2, the method for preparing the perovskite solar cell includes steps S1 to S5.

[0073] Step S1, providing a substrate.

[0074] FIG3 is a schematic structural diagram of a substrate.

[0075] In some examples of this embodiment, as shown in FIG. 3 , in some examples of this embodiment, the substrate includes a base material 100 and a first electrode 110 disposed on the base material 100 .

[0076] In some examples of this embodiment, the step of providing a substrate includes: providing a base material 100 , and preparing a first electrode 110 on the base material 100 .

[0077] In this embodiment, the substrate 100 can be selected from glass or transparent polymer materials. In this embodiment, the substrate 100 is polyethylene terephthalate.

[0078] In some examples of this embodiment, the length of the substrate 100 can range from 1 m to 10,000 m. It is understood that for a longer substrate 100, the substrate 100 can be gradually moved to gradually form the various material layers located on the surface of the substrate 100. This is a continuous production method that can effectively improve the production efficiency of the perovskite solar cell.

[0079] In some examples of this embodiment, the material of the first electrode 110 may include a transparent conductive metal oxide. In this embodiment, the transparent conductive oxide may be indium tin oxide.

[0080] In some examples of this embodiment, the step of forming the first electrode 110 on the substrate 100 may include placing the substrate 100 in a magnetron sputtering chamber, performing a plasma cleaning process on the substrate 100, and then sputtering and depositing a material for the first electrode 110 on the surface of the substrate 100. During the plasma cleaning process, a protective gas is used. For example, a mixture of argon and nitrogen may be used to perform the plasma cleaning process on the substrate 100.

[0081] In some examples of this embodiment, after the first electrode 110 is sputter-deposited on the surface of the substrate 100, a first laser scribing process may be performed on the first electrode 110 to form a patterned first electrode 110. The purpose of forming the patterned first electrode 110 is to ultimately prepare a plurality of perovskite solar cells.

[0082] Step S2: preparing a first charge extraction layer 120 on the substrate.

[0083] FIG4 is a schematic structural diagram of preparing the first charge extraction layer 120 based on the structure shown in FIG3 .

[0084] In some examples of this embodiment, the first charge extraction layer 120 may be an electron transport layer. Furthermore, the material of the first charge extraction layer 120 may be selected from one or more of fullerene, tin oxide, tungsten sulfide, zinc oxide, titanium oxide, tungsten oxide, and indium gallium zinc oxide. In this embodiment, the material of the first charge extraction layer 120 is tin oxide.

[0085] In some examples of this embodiment, the first charge extraction layer 120 may be prepared by sputtering. For example, tin oxide may be used as a target material to prepare the first charge extraction layer 120 on the first electrode 110. Furthermore, the first charge extraction layer 120 may be prepared by magnetron sputtering.

[0086] In some examples of this embodiment, the thickness of the first charge extraction layer 120 may be controlled to be 10 nm to 100 nm.

[0087] Among them, magnetron sputtering is a large-scale and large-scale preparation method with the advantages of simple process and high preparation efficiency. To further improve efficiency, the sputtering chamber for preparing the first charge extraction layer 120 can be the same as the sputtering chamber for preparing the first electrode 110, or the sputtering chamber for preparing the first charge extraction layer 120 can be connected to the sputtering chamber for preparing the first electrode 110. It can be understood that when the sputtering chambers are the same, it is only necessary to simultaneously set multiple sputtering targets in the sputtering chamber to prepare the first charge extraction layer 120 and the first electrode 110 respectively.

[0088] Step S3 , forming a perovskite layer 130 on the first charge extraction layer 120 .

[0089] FIG5 is a schematic diagram showing a structure of preparing a perovskite layer 130 based on the structure shown in FIG4 .

[0090] In some examples of this embodiment, the material of the perovskite layer 130 may include a compound of the general formula ABX3, where A may be selected from one or more of cesium ions, formamidinium ions (FA), and methylamine ions (MA), B may be selected from lead ions, and X may be selected from halide ions. In this embodiment, the material of the perovskite layer 130 may be methylammonium iodide (MAPbI3).

[0091] In some examples of this embodiment, the perovskite layer 130 may be prepared by sputtering. For example, the perovskite layer 130 is prepared by magnetron sputtering.

[0092] When the perovskite layer 130 is prepared by sputtering, a perovskite material can be used as a target material. For example, iodine lead methylamine can be used as the perovskite target material. It is understood that iodine lead methylamine is easily deteriorated in air. Therefore, the perovskite target material can be placed directly in the sputtering chamber after preparation to ensure its quality.

[0093] In some examples of this embodiment, the thickness of the perovskite layer 130 may be controlled to be 100 nm to 1000 nm.

[0094] To further improve efficiency, the sputtering chamber for preparing the perovskite layer 130 can be the same as the sputtering chamber for preparing the first charge extraction layer 120 , or the sputtering chamber for preparing the perovskite layer 130 can be connected to the sputtering chamber for preparing the first charge extraction layer 120 .

[0095] Step S4 , sequentially preparing a boron nitride layer 141 and a graphene material layer 142 on the perovskite layer 130 .

[0096] FIG6 is a schematic structural diagram of preparing a boron nitride layer 141 and a graphene material layer 142 based on the structure shown in FIG5 .

[0097] 6 , the boron nitride layer 141 and the graphene material layer 142 constitute a composite protective layer 140 disposed on the perovskite layer 130 .

[0098] In some examples of this embodiment, the boron nitride layer 141 is in contact with the perovskite layer 130 , and the graphene material layer 142 is in contact with the boron nitride layer 141 .

[0099] In some examples of this embodiment, the boron nitride layer 141 is prepared by magnetron sputtering, and the graphene material layer 142 is prepared by magnetron sputtering.

[0100] In some examples of this embodiment, in the step of preparing the boron nitride layer 141 , hexagonal boron nitride is used as a sputtering target.

[0101] In some examples of this embodiment, during the step of preparing the boron nitride layer 141, the power of the magnetron sputtering can be controlled to be 200W to 350W. A lower sputtering power can be used when preparing the boron nitride layer 141, which can minimize damage to the perovskite layer 130 during the preparation of the boron nitride layer 141. In this case, the boron nitride layer 141 is primarily used as a growth substrate for the subsequently prepared graphene material layer 142, and allows the graphene material layer 142 to be stably bonded to the perovskite layer 130, thereby providing better barrier properties.

[0102] In some examples of this embodiment, the sputtering time can be controlled to be 1 to 10 minutes during the step of preparing the boron nitride layer 141. By controlling the sputtering time, the thickness of the boron nitride layer 141 can be controlled, thereby minimizing the impact of the introduction of the boron nitride layer 141 on carrier conduction.

[0103] In some examples of this embodiment, in the step of preparing the graphene material layer 142 , graphite may be used as a sputtering target.

[0104] In some examples of this embodiment, in the step of preparing the graphene material layer 142, the power of the magnetron sputtering can be controlled to be 300W to 400W. For example, the sputtering power can be controlled to be 300W, 320W, 350W, 380W, or 400W, or the sputtering power can be controlled to be in a range between any two of the above powers. Among them, the boron nitride layer 141 can serve as a growth substrate for the graphene material layer 142. Since hexagonal boron nitride has a lattice similar to that of graphene, during the magnetron sputtering process, the graphite target can spontaneously form a graphene material layer 142 on the hexagonal boron nitride. In addition, the pre-prepared boron nitride layer 141 can also block particles during the sputtering process. This can reduce the impact of the sputtering process on the perovskite layer 130 while forming a denser graphene material layer 142.

[0105] In some examples of this embodiment, during the step of preparing the graphene material layer 142, the sputtering time is controlled to be 1 to 10 minutes. By controlling the sputtering time, the thickness of the graphene material layer 142 can be controlled, thereby minimizing the impact of the introduction of the graphene material layer 142 on carrier conduction.

[0106] In some examples of this embodiment, the sputtering chamber for preparing the boron nitride layer 141 and the graphene material layer 142 can be the same as the sputtering chamber for preparing the perovskite layer 130, or the sputtering chamber for preparing the boron nitride layer 141 and the graphene material layer 142 can be connected to the sputtering chamber for preparing the perovskite layer 130, which can improve the preparation efficiency of the boron nitride layer 141 and the graphene material layer 142.

[0107] Step S5 , forming a second charge extraction layer 150 on the graphene material layer 142 .

[0108] FIG. 7 is a schematic structural diagram of a second charge extraction layer 150 prepared based on the structure shown in FIG. 6 .

[0109] 7 , the second charge extraction layer 150 is disposed on the graphene material layer 142 .

[0110] In some examples of this embodiment, the second charge extraction layer 150 may be a hole transport layer. Further, the material of the second charge extraction layer 150 may be selected from nickel oxide (NiO x ), copper oxide (CuO x ), copper sulfide, molybdenum sulfide, vanadium oxide (VO x ), one or more of tungsten oxide and copper thiocyanate. Wherein, an inorganic material is used as the hole transport layer, and the hole transport layer can also be prepared by sputtering.

[0111] In some examples of this embodiment, the second charge extraction layer 150 may be prepared by sputtering. For example, nickel oxide may be used as a target material to prepare the second charge extraction layer 150 on the graphene material layer 142. Furthermore, the second charge extraction layer 150 may be prepared by magnetron sputtering.

[0112] Conventional technologies typically use organic materials as hole transport layers and employ coating methods rather than sputtering. Although sputtering offers higher production efficiency, the high-energy particles generated during the sputtering process directly bombard the pre-prepared perovskite layer 130, significantly damaging the surface of the perovskite layer 130 and leading to a significant decrease in the performance of the perovskite solar cell.

[0113] In this embodiment, since the graphene material layer 142 is prepared in advance, during the process of forming the second charge extraction layer 150 by sputtering, the graphene material layer 142 blocks the bombardment of the material of the second charge extraction layer 150. This can reduce or avoid damage to the perovskite layer 130 while achieving the second charge extraction layer 150 by sputtering.

[0114] In some examples of this embodiment, the thickness of the second charge extraction layer 150 may be 10 nm to 100 nm.

[0115] In some examples of this embodiment, the sputtering chamber for preparing the second charge extraction layer 150 can be the same as the sputtering chamber for preparing the graphene material layer 142, or the sputtering chamber for preparing the second charge extraction layer 150 can be connected to the sputtering chamber for preparing the graphene material layer 142, which can improve the preparation efficiency of the second charge extraction layer 150.

[0116] In some examples of this embodiment, after forming the second charge extraction layer 150, a second laser scribing process may be performed on the second charge extraction layer 150, the perovskite layer 130, and the first charge extraction layer 120. It is understood that the position of the second laser scribing process may be slightly offset from the position of the first laser scribing process to facilitate series connection of the multiple perovskite solar cells ultimately prepared.

[0117] In some examples of this embodiment, after preparing the second charge extraction layer 150 , a step of preparing the second electrode 160 may be further included.

[0118] In some examples of this embodiment, the material of the second electrode 160 may be a metal material. For example, the material of the second electrode 160 may be selected from one or more of copper, silver, aluminum, gold, and molybdenum.

[0119] In some examples of this embodiment, the thickness of the second electrode 160 may be 50 nm to 500 nm.

[0120] When sputtering a metal target, a relatively high sputtering power is usually required, which may also affect the perovskite layer 130. Therefore, conventional techniques generally use evaporation to prepare electrodes instead of sputtering.

[0121] In some examples of this embodiment, the second electrode 160 may also be prepared by sputtering, such as magnetron sputtering. It will be appreciated that in this preparation method, the graphene material layer 142 is pre-prepared. By preparing a relatively dense, planar graphene material layer 142, the energy of the metal particles during the sputtering process can be reduced, thereby reducing or avoiding damage to the perovskite layer 130.

[0122] In some examples of this embodiment, the sputtering chamber for preparing the second electrode 160 can be the same as the sputtering chamber for preparing the second charge extraction layer 150, or the sputtering chamber for preparing the second electrode 160 can be connected to the sputtering chamber for preparing the second charge extraction layer 150, which can improve the preparation efficiency of the second electrode 160.

[0123] It can be understood that in this embodiment, the first charge extraction layer 120, the perovskite layer 130, the boron nitride layer 141, the graphene material layer 142 and the second charge extraction layer 150 are sequentially prepared in a magnetron sputtering chamber by magnetron sputtering. Therefore, most of the film layers in the perovskite solar cell disclosed in the present invention can be prepared by a continuous sputtering method. Sputtering is a low-cost, large-area preparation method, and the preparation of each layer by a continuous sputtering method can further improve the production efficiency of the perovskite solar cell. In addition, the boron nitride layer 141 and the graphene material layer 142 prepared by the sputtering method can reduce the negative impact of the sputtering method on the efficiency of the perovskite solar cell while improving its production efficiency.

[0124] It can be understood that the perovskite solar cell shown in FIG1 can be prepared through the preparation method of steps S1 to S5.

[0125] It is understood that in the preparation method of the perovskite solar cell of this embodiment, the electron transport layer is prepared first, and then the hole transport layer is prepared on the perovskite layer. However, in other embodiments, the hole transport layer can be prepared first, and then the electron transport layer is prepared on the perovskite layer. This also falls within the scope of the perovskite solar cell provided by the present disclosure.

[0126] In addition, conventional techniques typically employ coating to prepare the perovskite layer and charge extraction layer, and evaporation to prepare the electrode. These preparation methods require the use of multiple solvents and require additional drying, annealing, and transport operations, resulting in significantly higher manufacturing costs, higher energy consumption, and significantly longer production times. For example, the preparation method of the above-described embodiment employs sputtering to sequentially prepare the perovskite layer, composite protective layer, second charge extraction layer, and second electrode. These methods can be sequentially prepared on a single sputtering production line without the need for drying or annealing, offering the advantages of lower cost, lower energy consumption, and faster production times, making it an ideal method for producing solar cells.

[0127] Furthermore, the present disclosure provides a photovoltaic module comprising an encapsulation structure and a perovskite solar cell encapsulated by the encapsulation structure. The perovskite solar cell is the perovskite solar cell provided in the above embodiment, or a perovskite solar cell prepared by the method for preparing a perovskite solar cell provided in the above embodiment.

[0128] To facilitate understanding of the embodiments and advantages of the perovskite solar cell and its preparation method disclosed herein, the present disclosure also provides the following examples and comparative examples.

[0129] Example 1

[0130] An ethylene terephthalate film was provided as a substrate, the substrate was placed in a magnetron sputtering chamber, argon and nitrogen were introduced, and the substrate was plasma cleaned for 30 minutes;

[0131] sputtering indium tin oxide on the surface of the substrate as a first electrode;

[0132] Sputtering tin oxide (SnO2) with a thickness of 20 nm on the first electrode as an electron transport layer;

[0133] A 300 nm thick layer of iodine lead methylamine was sputtered on the electron transport layer as a perovskite layer;

[0134] Boron nitride was used as the target material, the sputtering power was controlled to 250W, the sputtering time was 3 minutes, and a hexagonal boron nitride layer with a thickness of 2 nm was sputtered on the perovskite layer as a boron nitride layer;

[0135] Graphite was used as a target material, the sputtering power was controlled to be 350 W, the sputtering time was 5 min, and graphene with a thickness of 5 nm was sputtered on the boron nitride layer as a graphene material layer;

[0136] Molybdenum disulfide (MoS2) with a thickness of 20 nm was sputter-deposited on the graphene material layer as a hole transport layer;

[0137] Silver with a thickness of 200 nm was sputter-deposited on the hole transport layer as a second electrode.

[0138] Example 2

[0139] An ethylene terephthalate film was provided as a substrate, the substrate was placed in a magnetron sputtering chamber, argon and nitrogen were introduced, and the substrate was plasma cleaned for 30 minutes;

[0140] sputtering indium tin oxide on the surface of the substrate as a first electrode;

[0141] Sputtering tin oxide (SnO2) with a thickness of 20 nm on the first electrode as an electron transport layer;

[0142] A 300 nm thick layer of iodine lead methylamine was sputtered on the electron transport layer as a perovskite layer;

[0143] Boron nitride was used as the target material, the sputtering power was controlled to 250W, the sputtering time was 3 minutes, and a 5 nm thick hexagonal boron nitride layer was sputtered on the perovskite layer as a boron nitride layer;

[0144] Graphite was used as a target material, the sputtering power was controlled to be 350 W, the sputtering time was 5 min, and graphene with a thickness of 8 nm was sputtered on the boron nitride layer to serve as a graphene material layer;

[0145] Molybdenum disulfide (MoS2) with a thickness of 20 nm was sputter-deposited on the graphene material layer as a hole transport layer;

[0146] Silver with a thickness of 200 nm was sputter-deposited on the hole transport layer as a second electrode.

[0147] Comparative Example 1

[0148] An ethylene terephthalate film was provided as a substrate, the substrate was placed in a magnetron sputtering chamber, argon and nitrogen were introduced, and the substrate was plasma cleaned for 30 minutes;

[0149] sputtering indium tin oxide on the surface of the substrate as a first electrode;

[0150] Sputtering tin oxide (SnO2) with a thickness of 20 nm on the first electrode as an electron transport layer;

[0151] A 300 nm thick layer of iodine lead methylamine was sputtered on the electron transport layer as a perovskite layer;

[0152] Molybdenum disulfide (MoS2) was sputter-deposited on the perovskite layer with a thickness of 20 nm as a hole transport layer;

[0153] Silver with a thickness of 200 nm was sputter-deposited on the hole transport layer as a second electrode.

[0154] Comparative Example 2

[0155] An ethylene terephthalate film was provided as a substrate, the substrate was placed in a magnetron sputtering chamber, argon and nitrogen were introduced, and the substrate was plasma cleaned for 30 minutes;

[0156] sputtering indium tin oxide on the surface of the substrate as a first electrode;

[0157] Sputtering tin oxide (SnO2) with a thickness of 20 nm on the first electrode as an electron transport layer;

[0158] A 300 nm thick layer of iodine lead methylamine was sputtered on the electron transport layer as a perovskite layer;

[0159] Graphite was used as a target material, the sputtering power was controlled to be 350 W, the sputtering time was 5 min, and graphene with a thickness of 5 nm was sputtered on the perovskite layer as a graphene material layer;

[0160] Molybdenum disulfide (MoS2) with a thickness of 20 nm was sputter-deposited on the graphene material layer as a hole transport layer;

[0161] Silver with a thickness of 200 nm was sputter-deposited on the hole transport layer as a second electrode.

[0162] Comparative Example 3

[0163] An ethylene terephthalate film was provided as a substrate, the substrate was placed in a magnetron sputtering chamber, argon and nitrogen were introduced, and the substrate was plasma cleaned for 30 minutes;

[0164] sputtering indium tin oxide on the surface of the substrate as a first electrode;

[0165] Sputtering tin oxide (SnO2) with a thickness of 20 nm on the first electrode as an electron transport layer;

[0166] A 300 nm thick layer of iodine lead methylamine was sputtered on the electron transport layer as a perovskite layer;

[0167] Boron nitride was used as the target material, the sputtering power was controlled to 250W, the sputtering time was 3 minutes, and a hexagonal boron nitride layer with a thickness of 2 nm was sputtered on the perovskite layer as a boron nitride layer;

[0168] Molybdenum disulfide (MoS2) with a thickness of 20 nm was sputter-deposited on the boron nitride layer as a hole transport layer;

[0169] Silver with a thickness of 200 nm was sputter-deposited on the hole transport layer as a second electrode.

[0170] Experiment: The initial conversion efficiency of the perovskite cells of the above-mentioned embodiments and comparative examples was tested, as well as the working time when the conversion efficiency of the perovskite cells of the above-mentioned embodiments and comparative examples dropped to 90% of the initial conversion efficiency, which was recorded as T90 life. The results can be seen in Table 1.

[0171] Table 1

[0172] As shown in Table 1, the initial conversion efficiency of the solar cells prepared in Example 1 and Example 2 can reach more than 14%, and their T90 life can reach more than 1500h. This result is similar to the conversion efficiency obtained when the hole transport layer is prepared by coating and the second electrode is prepared by evaporation in the traditional technology. This shows that the overall composite protective layer formed by first preparing the boron nitride layer and then preparing the graphene material layer can play a good protective role on the perovskite layer without basically damaging the perovskite layer, thereby enabling the perovskite solar cell to maintain a good initial conversion efficiency.

[0173] In contrast, in Comparative Example 1, no boron nitride layer and graphene material layer were prepared, and its initial conversion efficiency was only 7.45%, and its T90 lifespan was significantly lower. This was mainly because during the sputtering process of preparing the hole transport layer and the second electrode, high-energy particles caused significant damage to the perovskite layer. In Comparative Example 2, only a graphene material layer was prepared, and its initial conversion efficiency was lower than that of Comparative Example 1. This was mainly because the sputtering of the graphene material layer significantly damaged the perovskite layer. However, it had a slightly higher T90 lifespan, which was mainly due to the blocking effect of the graphene material layer. In Comparative Example 3, only a boron nitride layer was prepared, and its initial conversion efficiency was similar to that of Comparative Example 1, and its T90 lifespan was basically the same as that of Comparative Example 1, indicating that the boron nitride layer alone was unable to block the damage caused to the perovskite layer by high-energy particles generated during the subsequent sputtering process.

[0174] As in the preparation method of Example 1 and Example 2, a sputtering method is used to sequentially prepare a perovskite layer, a composite protective layer, a second charge extraction layer, and a second electrode. These can be sequentially prepared on a sputtering production line without the need for drying or annealing treatment. This method has the advantages of low cost, low energy consumption, and fast production time, and is an ideal method for producing solar cells.

[0175] Please note that the above embodiments are for illustrative purposes only and are not intended to limit the present disclosure.

[0176] It should be understood that, unless otherwise expressly stated herein, there is no strict order restriction for the execution of the steps of , and these steps may be executed in other orders. Moreover, at least a portion of the steps of may include multiple sub-steps or multiple stages, and these sub-steps or stages are not necessarily executed at the same time, but may be executed at different times. The execution order of these sub-steps or stages is not necessarily sequential, but may be executed in rotation or alternation with other steps or at least a portion of the sub-steps or stages of other steps.

[0177] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.

[0178] The technical features of the above embodiments can be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

Claims

1. A perovskite solar cell, comprising: A substrate, a first charge extraction layer, a perovskite layer, a composite protective layer, and a second charge extraction layer; The first charge extraction layer, the perovskite layer, the composite protective layer and the second charge extraction layer are sequentially stacked on the substrate, and the composite protective layer includes a boron nitride layer and a graphene material layer sequentially stacked on the perovskite layer. 2 . The perovskite solar cell according to claim 1 , wherein the thickness of the boron nitride layer is ≤10 nm.

3. The perovskite solar cell according to any one of claims 1 to 2, wherein the thickness of the graphene material layer is ≤10 nm. 4 . The perovskite solar cell according to claim 1 , wherein the boron nitride layer is in direct contact with the perovskite layer, and the graphene material layer is in direct contact with the boron nitride layer.

5. The perovskite solar cell according to any one of claims 1 to 4, wherein the first charge extraction layer is an electron transport layer, and a material of the first charge extraction layer is selected from one or more of fullerene, tin oxide, tungsten sulfide, zinc oxide, titanium oxide, tungsten oxide and indium gallium zinc oxide.

6. According to the perovskite solar cell according to any one of claims 1 to 5, the second charge extraction layer is a hole transport layer, and the material of the second charge extraction layer is selected from one or more of nickel oxide, copper oxide, copper sulfide, molybdenum sulfide, vanadium oxide, tungsten oxide and copper thiocyanate.

7. A method for preparing a perovskite solar cell, comprising the following steps: providing a substrate; preparing a first charge extraction layer on the substrate; preparing a perovskite layer on the first charge extraction layer; sequentially preparing a boron nitride layer and a graphene material layer on the perovskite layer to form a composite protective layer; A second charge extraction layer is prepared on the graphene material layer.

8. The method for preparing a perovskite solar cell according to claim 7, wherein the thickness of the boron nitride layer is ≤10 nm. 9 . The method for preparing a perovskite solar cell according to claim 7 , wherein the thickness of the graphene material layer is ≤10 nm. 10 . The method for preparing a perovskite solar cell according to claim 7 , wherein the boron nitride layer is in direct contact with the perovskite layer, and the graphene material layer is in direct contact with the boron nitride layer.

11. The method for preparing a perovskite solar cell according to any one of claims 7 to 10, wherein the first charge extraction layer is an electron transport layer, and a material of the first charge extraction layer is selected from one or more of fullerene, tin oxide, tungsten sulfide, zinc oxide, titanium oxide, tungsten oxide and indium gallium zinc oxide.

12. According to the method for preparing a perovskite solar cell according to any one of claims 7 to 11, the second charge extraction layer is a hole transport layer, and the material of the second charge extraction layer is selected from one or more of nickel oxide, copper oxide, copper sulfide, molybdenum sulfide, vanadium oxide, tungsten oxide and copper thiocyanate.

13. The method for preparing a perovskite solar cell according to any one of claims 7 to 12, wherein the boron nitride layer is prepared by sputtering, and the graphene material layer is prepared by sputtering.

14. The method for preparing a perovskite solar cell according to any one of claims 7 to 13, wherein in the step of preparing the boron nitride layer, hexagonal boron nitride is used as a sputtering target, the sputtering power is controlled to be 200 W to 350 W, and the sputtering time is controlled to be 1 min to 10 min.

15. The method for preparing a perovskite solar cell according to any one of claims 7 to 14, wherein in the step of preparing the graphene material layer, graphite is used as a sputtering target, the sputtering power is controlled to be 300W to 400W, and the sputtering time is controlled to be 1 min to 10 min.

16. According to the method for preparing a perovskite solar cell according to any one of claims 7 to 15, the first charge extraction layer, the perovskite layer, the boron nitride layer, the graphene material layer and the second charge extraction layer are prepared in sequence in a sputtering chamber by sputtering.

17. The method for preparing a perovskite solar cell according to any one of claims 7 to 16, wherein the substrate comprises a base material and a first electrode disposed on the base material, and before preparing the first charge extraction layer, further comprises a step of plasma cleaning the base material.

18. The method for preparing a perovskite solar cell according to any one of claims 7 to 17, further comprising the step of preparing a second electrode on the second charge extraction layer after preparing the second charge extraction layer, wherein the second electrode is prepared by sputtering.

19. A photovoltaic module, comprising a packaging structure and a perovskite solar cell packaged by the packaging structure, wherein the perovskite solar cell comprises: A substrate, a first charge extraction layer, a perovskite layer, a composite protective layer, and a second charge extraction layer; The first charge extraction layer, the perovskite layer, the composite protective layer and the second charge extraction layer are sequentially stacked on the substrate, and the composite protective layer includes a boron nitride layer and a graphene material layer sequentially stacked on the perovskite layer. 20 . The photovoltaic module according to claim 19 , wherein the thickness of the boron nitride layer is ≤10 nm.

21. The photovoltaic module according to any one of claims 19 to 20, wherein the thickness of the graphene material layer is ≤10 nm. 22 . The photovoltaic module according to claim 19 , wherein the boron nitride layer is in direct contact with the perovskite layer, and the graphene material layer is in direct contact with the boron nitride layer.

23. The photovoltaic module according to any one of claims 19 to 22, wherein the first charge extraction layer is an electron transport layer, and a material of the first charge extraction layer is selected from one or more of fullerene, tin oxide, tungsten sulfide, zinc oxide, titanium oxide, tungsten oxide and indium gallium zinc oxide.

24. The photovoltaic module according to any one of claims 19 to 23, wherein the second charge extraction layer is a hole transport layer, and a material of the second charge extraction layer is selected from one or more of nickel oxide, copper oxide, copper sulfide, molybdenum sulfide, vanadium oxide, tungsten oxide and copper thiocyanate.

Citation Information

Patent Citations

  • Perovskite solar cells and their fabrication methods, photovoltaic modules

    CN116347908B

  • Perovskite battery having graphene barrier layer and preparation method

    CN106449985A

  • Quantum dot light-emitting diode and preparation method thereof

    CN113036043A

  • Method for improving stability of perovskite solar cell device

    CN115666191A

  • Perovskite solar cell, preparation method thereof and photovoltaic module

    CN116347908A