Biodegradable aliphatic polyester composition, and preparation method therefor and use thereof

By optimizing the composition and reaction conditions of the aliphatic polyester composition, the problems of high migration amount and low heat sealing strength of biodegradable aliphatic polyester materials in the prior art are solved, and foods with high heat sealing strength and low migration amount are achieved Contact performance meets the needs of packaging materials.

WO2024244326A1PCT designated stage expired Publication Date: 2024-12-05KINGFA SCI & TECH CO LTD +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/133425
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2023-11-22
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The existing biodegradable aliphatic polyester materials have high migration volume and low heat seal strength, making it difficult to meet food contact performance and packaging needs.

Method used

By optimizing the composition of the aliphatic polyester composition, regulating the content and proportion of cyclic esterides, combining crosslinking agents and chain growth agents, specific esterification and polycondensation reaction conditions are adopted to reduce the precipitation of cyclic esterides and increase heat seal strength and control the full migration amount in food contact performance.

Benefits of technology

It significantly reduces the precipitation of cyclic esterides, improves the heat sealing strength of the film material, meets the standards of food contact performance, and ensures the biodegradability and high heat sealing performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023133425_05122024_PF_FP_ABST
    Figure CN2023133425_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of degradable materials, and provides a biodegradable aliphatic polyester composition, and a preparation method therefor and the use thereof. The biodegradable aliphatic polyester composition of the present invention comprises a biodegradable aliphatic polyester and a cyclic esterified substance. The biodegradable aliphatic polyester comprises: a component A, i.e. a dicarboxylic acid compound; and a component B, i.e. 1,4-butanediol, which having at least the equimolar amount of the component A. The cyclic esterified substance comprises compounds as shown in formula (I) and formula (II). The content of the cyclic esterified substance is 0.6-1.1 wt.% on the basis of the total weight of the biodegradable aliphatic polyester composition, and the mass ratio of the compounds as shown in formula (I) to formula (II) is 2-6 : 1. By controlling polymeric monomers of the biodegradable aliphatic polyester composition and rationally regulating and controlling the proportion of the compounds as shown in formula (I) and formula (II), the present invention greatly reduces the precipitation of the cyclic ester and effectively improves the heat-sealing strength.
Need to check novelty before this filing date? Find Prior Art

Description

A biodegradable aliphatic polyester composition and its preparation method and application Technical Field

[0001] The present invention relates to the technical field of degradable materials, in particular to a biodegradable aliphatic polyester composition and a preparation method and application thereof. Background Art

[0002] Polybutylene succinate-adipate (PBSA) is produced through esterification and polycondensation of three monomers: succinic acid, adipic acid, and 1,4-butanediol. The molar ratio of succinic acid to adipic acid in its molecular structure significantly affects its product performance. When the succinic acid content is high, the product performance tends to be more similar to polybutylene succinate (PBS), with a higher melting point, crystallinity, and heat resistance, but it struggles to meet home composting requirements. When the adipic acid content is high, the product performance tends to be more similar to polybutylene adipate (PBA), which, while having excellent home composting properties, has a low melting point and poor heat resistance, making it difficult to meet practical requirements. Commercially available PBSA products generally adopt a molecular structure design approach based on the needs of the end application, taking into account various performance aspects.

[0003] PBSA has excellent processing properties and can be processed using common molding equipment through methods such as extrusion, injection molding, blow molding, spinning, blister molding, lamination, and foaming. The product has a wide range of applications, including packaging, such as plastic wrap and courier bags; daily necessities, such as disposable tableware; and agricultural applications, such as biodegradable mulch films. For packaging and daily necessities, food contact performance is particularly critical because the materials they use come into direct contact with the human body.

[0004] EU Food Contact Regulation EU 10-2011 requires that the total migration amount of food contact materials during food contact testing be less than or equal to 10 mg / dm 2 During the synthesis of biodegradable polyesters, monomeric diacids and diols readily undergo esterification, forming small-molecule compounds such as cyclic esters or polyester oligomers. These cyclic esters or polyester oligomers are prone to migration and precipitation during use. Furthermore, factors such as monomer residues, transfer of impurities within the monomers, and polyester degradation can further affect the food contact performance of polyester materials.

[0005] Furthermore, when using aliphatic polyester as the base resin for biodegradable courier bags, manufacturers typically produce the packaging film for courier bags first, accumulating a sufficient amount of film before centralizing printing and bag production. Film that has been stored for a period of time can easily weaken during the heat-sealing process, leading to quality issues such as "bursting" of the courier bags.

[0006] Japanese Patent JP2002003606 discloses a method for cleaning aliphatic polyesters using one or more solvents selected from aliphatic ketones, cyclic aliphatic ethers, and aliphatic monoesters to reduce the oligomer content in the aliphatic polyester resin. This method is complex, and the organic solvents used remain in the resin, making them difficult to remove. Furthermore, the organic solvents used can affect the food contact performance of the material.

[0007] Therefore, it is necessary to develop a biodegradable aliphatic polyester material with small migration of cyclic esters and high heat sealing strength.

[0008] Summary of the Invention

[0009] The purpose of the present invention is to overcome the defects of high migration and low heat-sealing strength of biodegradable aliphatic polyesters in the prior art and to provide a biodegradable aliphatic polyester composition with low overall migration and high heat-sealing strength.

[0010] Another object of the present invention is to provide a method for preparing the biodegradable aliphatic polyester composition.

[0011] Another object of the present invention is to provide applications of the biodegradable aliphatic polyester composition.

[0012] To achieve the above object, the present invention adopts the following technical solutions:

[0013] A biodegradable aliphatic polyester composition comprising:

[0014] Component i), a biodegradable aliphatic polyester, wherein the biodegradable aliphatic polyester comprises:

[0015] Component A, the dicarboxylic acid compound, based on the total molar amount of component A, comprises:

[0016] a1, 68-82 mol% of succinic acid,

[0017] a2, 18 to 32 mol% of adipic acid;

[0018] Component B, 1,4-butanediol in an amount at least equimolar to that of component A;

[0019] Component ii), a cyclic ester represented by formula (I) and formula (II),

[0020] Wherein n and m in formula (I) and formula (II) are positive integers ranging from 1 to 8;

[0021] Based on the total weight of the biodegradable aliphatic polyester composition, the content of the cyclic ester is 0.6-1.1 wt.%, and the mass ratio η of the compounds represented by formula (I) to formula (II) is 2-6:1.

[0022] In the biodegradable aliphatic polyester composition of the present invention, the content of cyclic esters can be measured by the following method:

[0023] Weigh 25 g of a biodegradable aliphatic polyester composition and add it to a Soxhlet extractor. Extraction is performed using ethanol as the solvent. The temperature of the condensed water is controlled to ensure that the temperature of the ethanol solution in the Soxhlet extractor is 45-55°C. After continuous extraction for 48 hours, the extract is dried. 50 ml of ethanol is added to the dried residue, stirred, and then filtered. The filter cake is washed with ethanol until no 1,4-butanediol is present in the washing liquid (gas chromatography is used to determine whether 1,4-butanediol is present in the washing liquid). The filter cake is dried to a constant weight. The mass of the resulting filter cake is the weight of the cyclic ester in the 25 g biodegradable aliphatic polyester composition.

[0024] The mass ratio of the compounds represented by formula (I) and formula (II) in the cyclic ester can be measured by the following method:

[0025] 20 mg of the dried filter cake was dissolved in deuterated chloroform and then measured at room temperature using a Bruker AV 500 NMR spectrometer. 1 H-NMR, calibrated with the chloroform solvent peak at around 7.26 ppm.

[0026] According to the literature, in the compound represented by formula (I), the chemical shift of the four hydrogen atoms of the two CH2 units of succinic acid adjacent to the carbonyl group appears at around 2.63 ppm; in the compound represented by formula (II), the chemical shift of the four hydrogen atoms of the two CH2 units of adipic acid adjacent to the carbonyl group appears at around 2.33 ppm; thus, in the biodegradable aliphatic polyester mixture, the molar ratio of the repeating units of the compound represented by formula (I) and the compound represented by formula (II) can be determined by the integrated area of ​​the two peaks at 2.63 ppm and 2.33 ppm (I SA and I AA )express:

[0027] Relative to the total molar amount of the repeating units of the compounds represented by formula (I) and formula (II),

[0028] The molar content of the repeating unit of the compound represented by formula (I) is m I =I SA / (I SA +I AA )×100%,

[0029] The molar content of the repeating unit of the compound represented by formula (II) is m II =I AA / (I SA +I AA )×100%.

[0030] In the biodegradable aliphatic polyester mixture, the mass ratio η of the compounds represented by formula (I) and formula (II) can be calculated by combining the molar mass of the repeating units of the compounds represented by formula (I) and formula (II), and the specific calculation method is as follows: η=(m I ×172.2) / (m II ×200.2)×100%.

[0031] Wherein, the molar mass of the repeating unit of the compound represented by formula (I) is 172.2 g / mol,

[0032] The molar mass of the repeating unit of the compound represented by formula (II) is 200.2 g / mol.

[0033] The pH value of succinic acid is about 2.7, and the pH value of adipic acid is between 4.4 and 5.4. For esterification reactions, under the same reaction conditions, the lower the pH value of the system, the more favorable it is for the esterification reaction to occur. Therefore, when synthesizing PBSA, succinic acid is more likely to undergo esterification than adipic acid, and correspondingly, it is also easier to form the cyclic ester represented by formula (I). In terms of molecular structure, when the number of repeating units is the same, the molecular weight of the cyclic ester represented by formula (I) is smaller than that of the cyclic ester represented by formula (II), and it is easier to migrate and precipitate. In terms of product properties, the cyclic ester represented by formula (I) is an oily substance, while the cyclic ester represented by formula (II) is a crystal. The precipitation of the oily substance on the surface of the film is more likely to cause the heat-sealing adhesive properties of the film to fail.

[0034] The present invention greatly reduces the precipitation of cyclic esters by regulating the mass ratio of the compounds represented by formula (I) and formula (II), and effectively solves the problem of low heat-sealing strength of the film material after storage.

[0035] Preferably, the component A, based on the total molar amount of component A, comprises:

[0036] a1, 72-78 mol% of succinic acid,

[0037] a2, 22 to 28 mol% of adipic acid.

[0038] Preferably, the mass ratio of the compounds represented by formula (I) to formula (II) is 3.2-4.8:1.

[0039] Preferably, the biodegradable aliphatic polyester composition may further include a crosslinking agent having at least three functional groups. The weight content of the crosslinking agent having at least three functional groups is 0-3 wt.%, preferably 0.01-2 wt.%, more preferably 0.05-1 wt.%, and particularly preferably 0.3-0.4 wt.%, based on the total weight of the biodegradable aliphatic polyester composition.

[0040] The cross-linking agent having at least three functional groups is particularly preferably a compound having 3 to 6 hydroxyl groups. Optionally, the cross-linking agent is at least one of tartaric acid, citric acid, malic acid, trimethylolpropane, trimethylolethane, pentaerythritol, polyether triol, glycerol, trimellitic acid, trimellitic acid, trimellitic anhydride, pyromellitic acid, and pyromellitic dianhydride. Polyols such as trimethylolpropane, pentaerythritol, and glycerol are preferred, with glycerol being particularly preferred.

[0041] Preferably, the biodegradable aliphatic polyester composition may further include a chain extender (component C).

[0042] Preferably, the chain extender comprises one or more of the following components:

[0043] c1, isocyanate,

[0044] c2, peroxide,

[0045] c3, epoxide,

[0046] c4, oxazoline, oxazine, caprolactam and / or carbodiimide.

[0047] Preferably, the biodegradable aliphatic polyester composition has a total migration amount less than or equal to 10 mg / dm according to EU 10-2011 standard and OM6 test conditions with 10% ethanol as the simulated liquid. 2 , preferably less than or equal to 7 mg / dm 2 .

[0048] The present invention also protects a method for preparing the above-mentioned biodegradable aliphatic polyester composition, comprising the following steps:

[0049] S1-i. Component a1 is mixed with a portion of component B, an alkaline compound is added to adjust the pH of the system to 3.2 to 5.8, and a catalyst is added or not added to obtain a slurry A. The slurry A is subjected to an esterification or transesterification reaction until the viscosity of the esterified product is 5 to 15 ml / g as measured according to DIN 53728-3-1985, thereby obtaining a first esterified product.

[0050] S1-ii. Component a2 is mixed with the remaining component B, a basic compound is added to adjust the pH of the system to 5.2 to 5.8, and a catalyst is added or not added to obtain a slurry B. The slurry B is subjected to an esterification or transesterification reaction until the viscosity of the esterified product is 7 to 16 ml / g as measured according to DIN 53728-3-1985, to obtain a second esterified product.

[0051] S2. The first esterification product and the second esterification product obtained in steps S1-i and S1-ii are mixed to obtain a mixture of esterification products, and the mixture is pre-polycondensed until the viscosity of the prepolymer is 24 to 55 ml / g as measured according to DIN 53728-3-1985;

[0052] S3. Polycondensing the prepolymer obtained in step S2 until the viscosity of the polycondensation product thereof measured according to DIN 53728-3-1985 is 143 to 226 ml / g, namely the biodegradable aliphatic polyester composition.

[0053] Step S1-i and step S1-ii can be performed simultaneously or interchangeably, and there is no specific order of precedence.

[0054] Preferably, in step S1-i, the ratio of component a1 to component B in slurry A is: 1.0 molar equivalent of component a1: 1.0 to 1.8 molar equivalents, preferably 1.05 to 1.60 molar equivalents, particularly preferably 1.15 to 1.50 molar equivalents of component B.

[0055] Preferably, in step S1-ii, the ratio of component a2 to component B in slurry B is: 1.0 molar equivalent of component a2: 1.1 to 2.2 molar equivalents, preferably 1.2 to 1.8 molar equivalents, particularly preferably 1.3 to 1.6 molar equivalents of component B.

[0056] Preferably, in step S1, 0 to 3 wt.%, preferably 0.01 to 2 wt.%, more preferably 0.05 to 1 wt.%, and particularly preferably 0.3 to 0.4 wt.% of a cross-linking agent having at least three functional groups, based on the total weight of the biodegradable aliphatic polyester composition, may also be included.

[0057] Preferably, in step S1, all or part of the catalyst is metered in. The catalysts used typically include zinc, aluminum, and, in particular, titanium compounds. Another advantage of titanium catalysts such as tetrabutyl titanate or tetraisopropyl titanate over the tin, antimony, cobalt, and lead compounds commonly used in the literature is that residual amounts of the catalyst remaining in the product or downstream products are less toxic. This is particularly important in biodegradable polyesters, as these enter the environment directly, for example, in the form of compost bags or mulch films. The catalyst is preferably a titanium catalyst.

[0058] Preferably, the addition amount of the titanium catalyst is 40-180 ppm (calculated as Ti element content) based on the total weight of the biodegradable aliphatic polyester composition.

[0059] Preferably, during step S1-i, preparing the first esterified product, the esterification or transesterification reaction temperature is 150-210°C, preferably 150-200°C, and the pressure is 0.7-1.1 bar, preferably 0.85-1.0 bar. Step S1 can be carried out in a mixing apparatus, with a typical reaction time of 3-5 hours, to produce an esterified product having a viscosity of 5-15 ml / g as measured according to DIN 53728-3-1985.

[0060] Preferably, during step S1-ii, preparing the second esterified product, the esterification or transesterification reaction temperature is 185-225°C, preferably 190-215°C, and the pressure is 0.8-1.1 bar, preferably 0.9-1.0 bar. Step S1 can be carried out in a mixing apparatus, with a typical reaction time of 2-4 hours, to produce an esterified product having a viscosity of 7-16 ml / g as measured according to DIN 53728-3-1985.

[0061] Excess diol components are generally removed by distillation and returned to the circuit, for example after purification by distillation.

[0062] In step S1, by adding an alkaline compound and adjusting the pH of the system, the succinic acid and adipic acid can be partially alkalized, effectively reducing the esterification reaction rate of succinic acid, adipic acid, and 1,4-butanediol, thereby effectively reducing the content of the cyclic esters represented by formula (I) and formula (II). In step S1-i, the pH of the system is preferably adjusted to 4.2 to 5.4.

[0063] Preferably, the alkaline compound is a carbonate and / or a hydroxide.

[0064] Optionally, the carbonate is at least one of sodium carbonate, sodium bicarbonate, potassium carbonate, and potassium bicarbonate. Preferably, the carbonate is sodium carbonate.

[0065] Optionally, the hydroxide is sodium hydroxide and / or potassium hydroxide. Preferably, the hydroxide is sodium hydroxide.

[0066] Preferably, in step S2, the mixture of esterified products and the remaining catalyst are added to a reactor suitable for a pre-condensation reaction to carry out a pre-condensation reaction; the reaction temperature is 225-260°C, preferably 235-248°C; the pressure is 0.2-0.7 bar, preferably 0.32-0.55 bar; and the reaction time is 75-180 minutes, thereby producing a prepolymer having a viscosity of 24-55 ml / g as measured according to DIN 53728-3-1985. In a preferred embodiment, the intrinsic viscosity of the prepolymer is controlled to be 32-46 ml / g.

[0067] Preferably, in step S3, a catalyst deactivator is mixed with the prepolymer, if appropriate. Suitable deactivators are, in particular, phosphorus compounds: either organic phosphites such as phosphorous acid, or phosphoric acid. It should be noted that if a highly active titanium catalyst is used, a deactivator can be added. The amount of deactivator added can be 0.001 to 0.1 wt.%, preferably 0.01 to 0.05 wt.%, based on the amount of polymer after step S3. The Ti / P ratio (mol / mol) is preferably set at 1.1 to 1.5:1, particularly preferably 1.1 to 1.3:1.

[0068] If appropriate, a color stabilizer for the condensation process is mixed with the prepolymer in step S3. Suitable color stabilizers are, in particular, phosphorus compounds, such as phosphoric acid, phosphorous acid, triphenyl phosphite, triphenyl phosphate, sodium hypophosphite, and sodium phosphite. These phosphorus compounds can also be used in the form of mixtures. The use of color stabilizers generally results in a reduced condensation rate. Triphenyl phosphate is a particularly suitable color stabilizer because it has no adverse effect on the condensation rate.

[0069] The color stabilizer may be added in an amount of 0.001 to 1.5 wt.%, preferably 0.01 to 1.0 wt.%, based on the total weight of the biodegradable aliphatic polyester composition. The Ti / P ratio (mol / mol) is preferably set to 1.0:0.3 to 1.0, particularly preferably 1.0:0.5 to 1.0.

[0070] In step S3, if appropriate, an activator for the condensation process is mixed with the prepolymer. Suitable activators are, in particular, phosphorus compounds. For example, disodium hydrogen phosphate, calcium hypophosphite, calcium phosphite, calcium phosphate, sodium hypophosphite, sodium phosphite, triphenyl phosphite, triphenyl phosphate, trimethyl phosphate, triethyl phosphate, tripropyl phosphate, and tributyl phosphate. These phosphorus compounds can also be used in the form of mixtures. Particularly suitable activators are disodium hydrogen phosphate and sodium phosphite.

[0071] Based on the total weight of the biodegradable aliphatic polyester composition, the activator may be added in an amount of 0.001 to 1.5 wt.%, preferably 0.01 to 1.0 wt.%. The Ti / P ratio (mol / mol) is preferably set to 1.0 to 1.5:1, particularly preferably 1.1 to 1.3:1.

[0072] The combination of color stabilizers and activators is of particular concern, an example being triphenyl phosphate / disodium hydrogen phosphate.

[0073] The polycondensation process described in step S3 takes place in a finisher. Reactors such as rotating disk reactors or cage reactors have proven particularly suitable finishers. The reaction temperature is typically set at 235-260°C, preferably 240-255°C, and the pressure is typically set at 0.2-5 mbar, preferably 0.5-3 mbar. Typical reaction times are 45-110 minutes, preferably 60-90 minutes, producing a polycondensation product having a viscosity of 143-226 ml / g, as measured according to DIN 53728-3-1985.

[0074] If necessary, step S4, chain extension reaction, can also be carried out. The polycondensation product described in step S3 is added together with the chain extender (component C) to an extruder, or to a continuous kneader (List reactor), or to a static mixer. The static mixer can use SMR, SMX or SMXL components, or a combination thereof. Examples of List reactors are: single-shaft DISCOTHERM B or double-shaft CRP or ORP reactors. Available extruders are single-screw extruders or twin-screw extruders. The preferred chain extension reaction of the present invention is carried out in an extruder, and after chain extension, the viscosity number of the chain extension product finally obtained is 167 to 242 ml / g measured according to DIN 53728-3-1985.

[0075] Preferably, the chain extender (component C) comprises one or more of the following components:

[0076] c1, isocyanate,

[0077] c2, peroxide,

[0078] c3, epoxide,

[0079] c4, oxazoline, oxazine, caprolactam and / or carbodiimide.

[0080] The isocyanate described in the present invention can use aromatic diisocyanates or aliphatic diisocyanates. For example, the aromatic diisocyanate can be toluene 2,4-diisocyanate, toluene 2,6-diisocyanate, diphenylmethane 2,2'-diisocyanate, diphenylmethane 2,4'-diisocyanate, diphenylmethane 4,4'-diisocyanate, naphthalene 1,5-diisocyanate or xylene diisocyanate.

[0081] Among them, diphenylmethane 2,2'-diisocyanate, 2,4'-diisocyanate, or 4,4'-diisocyanate is particularly preferably used.

[0082] Isocyanates that can also be used include tris(4-isocyanato-phenyl)methane having three rings. Such polynuclear aromatic diisocyanates can be formed, for example, during the production of diisocyanates having one or two rings.

[0083] For the purposes of the present invention, the aliphatic diisocyanate may be any linear or branched alkylene diisocyanate or cycloalkylene diisocyanate containing 2 to 20 carbon atoms, preferably 3 to 12 carbon atoms, such as hexamethylene diisocyanate, pentamethylene diisocyanate, isophorone diisocyanate, and methylene di(4-isocyanatocyclohexane) diisocyanate. Hexamethylene diisocyanate is particularly preferred.

[0084] The amount of isocyanate used, based on the total weight of the biodegradable aliphatic polyester composition, can be 0.05 to 2% by weight, particularly preferably 0.1 to 1.5% by weight.

[0085] The peroxide of the present invention can be one or more of the following compounds:

[0086] Benzoyl peroxide, 1,1-di(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-di(tert-butylperoxy)methylcyclododecane, n-butyl 4,4-di(butylperoxy)valerate, dicumyl peroxide, tert-butyl peroxybenzoate, dibutyl peroxide, α,α-di(tert-butylperoxy)diisopropylbenzene, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)hex-3-yne, and tert-butylcumene peroxide.

[0087] The amount of peroxide used may be 0.05 to 2 wt %, particularly preferably 0.2 to 1 wt %, based on the total weight of the biodegradable aliphatic polyester composition.

[0088] The epoxide of the present invention may be one or more of: diglycidyl ether, hexamethylene diglycidyl ether, sorbitol diglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, diglycerol polyglycidyl ether, glycerol polyglycidyl ether, trimethylolpropane polyglycidyl ether, resorcinol diglycidyl ether, neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, dipropylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether and polybutylene glycol diglycidyl ether, or a copolymer containing epoxy groups based on styrene, acrylate and / or methacrylate.

[0089] The amount of epoxide used may be 0.05 to 2 wt%, preferably 0.2 to 1 wt%, based on the total weight of the biodegradable aliphatic polyester composition.

[0090] The dioxazoline of the present invention may preferably be 2,2′-di(2-oxazoline), di(2-oxazolinyl)methane, 1,2-di(2-oxazolinyl)ethane, 1,3-di(2-oxazolinyl)propane or 1,4-di(2-oxazolinyl)butane, in particular 1,4-di(2-oxazolinyl)benzene, 1,2-di(2-oxazolinyl)benzene or 1,3-di(2-oxazolinyl)benzene.

[0091] The dioxazine is preferably 2,2′-di(2-dioxazine), di(2-dioxazinyl)methane, 1,2-di(2-dioxazinyl)ethane, 1,3-di(2-dioxazinyl)propane or 1,4-di(2-dioxazinyl)butane, in particular 1,4-di(2-dioxazinyl)benzene, 1,2-di(2-dioxazinyl)benzene or 1,3-di(2-dioxazinyl)benzene.

[0092] The carbodiimide may be: N,N′-di-2,6-diisopropylphenylcarbodiimide, N,N′-di-o-tolylcarbodiimide, N,N′-diphenylcarbodiimide, N,N′-dioctyldecylcarbodiimide, N,N′-di-2,6-dimethylphenylcarbodiimide, N-tolyl-N′-cyclohexylcarbodiimide, N,N′-di-2,6-di-tert-butylphenylcarbodiimide, N,N′-di-2,4,6-triisobutylphenylcarbodiimide, diisopropylcarbodiimide, dimethylcarbodiimide, diisobutylcarbodiimide, dioctylcarbodiimide, tert-butylisopropylcarbodiimide, di-β-naphthylcarbodiimide and di-tert-butylcarbodiimide.

[0093] The amount of oxazoline, oxazine, caprolactam and / or carbodiimide used, based on the total weight of the biodegradable aliphatic polyester composition, can be 0.05 to 2 weight %, preferably 0.2 to 1 weight %.

[0094] The chain extension reaction is carried out at a reaction temperature of 170 to 240°C, preferably 180 to 220°C, under superatmospheric or atmospheric pressure, depending on the system used. A residence time of 2 to 15 minutes, preferably 4 to 10 minutes, is used.

[0095] The present invention also protects the use of the biodegradable aliphatic polyester composition in preparing fresh-keeping film.

[0096] The present invention also protects a biodegradable mixture comprising the following components in percentage by weight:

[0097] i) 5 to 95 wt.% of the biodegradable aliphatic polyester composition, based on the total weight of components i) and ii),

[0098] ii) 5 to 95 wt.% of at least one or more components selected from aliphatic-aromatic copolyesters, aliphatic polyesters, starch, cellulose, polyhydroxyalkanoate, polyglycolic acid and polylactic acid, based on the total weight of components i) and ii),

[0099] iii) 0 to 35 wt.% of talc, based on the total weight of components i) to iv),

[0100] iv) 0 to 20 wt.% of calcium carbonate, based on the total weight of components i) to iv).

[0101] The present invention also protects the use of the biodegradable mixture in preparing heat-sealing films.

[0102] Specifically, the heat-sealing film may be a courier bag.

[0103] The express bag made of the biodegradable polyester mixture described in the present invention has a heat sealing strength greater than or equal to 10N / 15mm after being stored for 10 days at 25±5°C and 50%±10% humidity according to the QB / T2358-1998 standard, effectively solving the problem of poor heat sealing strength and easy "bursting" of the film material after storage.

[0104] The biodegradable aliphatic polyester composition and biodegradable mixture mentioned in the present invention are biodegradable.

[0105] For the purposes of the present invention, a substance or a mixture of substances is characterized as "biodegradable" if it shows a percentage degree of biodegradation as defined in DIN EN 13432 of at least 90%.

[0106] According to DIN EN 13432, during the composting process, CO2-free air is introduced into mature compost and the compost is subjected to a specific temperature profile. Biodegradability is defined as the percentage of biodegradation expressed as the ratio of the net amount of CO2 released by the sample (after subtracting the amount of CO2 released by the compost without the sample) to the maximum amount of CO2 that the sample could release (calculated from the carbon content of the sample). After only a few days of composting, biodegradable polyesters and biodegradable polyester blends often show visible signs of degradation, such as fungal growth, cracking, and perforation.

[0107] Other methods for determining biodegradability are described, for example, in ASTM D5338 and ASTM D6400.

[0108] Compared with the prior art, the present invention has the following beneficial effects:

[0109] The present invention develops a biodegradable aliphatic polyester composition. By optimizing the composition of the biodegradable aliphatic polyester composition and rationally regulating the total amount and ratio of cyclic esters represented by formula (I) and formula (II) in the biodegradable aliphatic polyester composition, the heat sealing strength of the film material is effectively improved while the total migration amount of the film material is reduced. DETAILED DESCRIPTION

[0110] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below with reference to specific embodiments, but the embodiments do not limit the present invention in any form.

[0111] The raw materials in the examples and comparative examples can all be obtained commercially;

[0112] The method for evaluating the overall migration of the biodegradable aliphatic polyester composition of the present invention is as follows:

[0113] The method for evaluating the overall migration of the biodegradable aliphatic polyester composition refers to the EU food contact standard EU 10-2011. According to the OM6 test conditions, 10% ethanol is selected as a simulant, and the biodegradable aliphatic polyester composition is made into a sample with a thickness of 50±5μm. The overall migration test is carried out. 10% ethanol is selected as a simulant for food contact testing to obtain the overall migration of the biodegradable aliphatic polyester composition. Each sample is tested in parallel with two samples, and the average value is taken.

[0114] The evaluation method of the heat seal strength of the express packaging film in the present invention is as follows:

[0115] The heat sealing strength of the film was tested with reference to QB / T2358-1998 standard, with a film thickness of 25±2μm and a film width of 15mm.

[0116] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in this technical field.

[0117] Example 1

[0118] Example 1 provides a biodegradable aliphatic polyester composition, the preparation method of which is as follows:

[0119] S1-i. 195 kg of succinic acid, 210 kg of 1,4-butanediol, and 1.2 kg of glycerol were mixed, a 1,4-butanediol solution containing sodium hydroxide was added, and the pH of the system was adjusted to 5.4 to obtain slurry A. The slurry A was transferred to a stirred reactor, and the reaction mixture was esterified at a temperature of 150 ° C and a pressure of 1.0 bar for 3 hours. The viscosity of the obtained first ester was 5 ml / g;

[0120] S1-ii. Physically mix 68 kg of adipic acid, 65 kg of 1,4-butanediol, and 0.21 kg of tetrabutyl titanate. Add a 1,4-butanediol solution containing sodium hydroxide and adjust the pH of the mixture to 5.6 to obtain slurry B. Transfer slurry B to a stirred reactor. Esterify the reaction mixture at 215°C and 0.9 bar for 4 hours. The resulting second ester has a viscosity of 16 ml / g.

[0121] S2. The first esterification product and the second esterification product obtained in steps S1-i and S1-ii were mixed, and the mixture was transferred to a stirred vertical reactor. 0.16 kg of tetrabutyl titanate was added, and the reaction mixture was pre-polycondensed at 248° C. and a pressure of 0.32 bar in the reactor for 120 minutes. The viscosity of the resulting prepolymer was 46 ml / g.

[0122] S3. The prepolymer obtained in step S2 was transferred to a horizontal reactor with stirring and polycondensed at 245°C and a pressure of 1.3 mbar for 90 minutes. The viscosity of the resulting biodegradable aliphatic polyester composition was 188 ml / g.

[0123] The total content and mass ratio η of the compounds represented by formula (I) and formula (II) in the biodegradable aliphatic polyester composition are shown in Table 1.

[0124] Example 2

[0125] Example 2 provides a biodegradable aliphatic polyester composition, the preparation method of which is as follows:

[0126] S1-i. 195 kg of succinic acid, 215 kg of 1,4-butanediol, and 1.5 kg of glycerol were mixed, a 1,4-butanediol solution containing sodium carbonate was added, and the pH of the system was adjusted to 4.2 to obtain slurry A. The slurry A was transferred to a stirred reactor, and the reaction mixture was esterified at a temperature of 210 ° C and a pressure of 0.70 bar for 3 hours. The viscosity of the obtained first ester was 15 ml / g;

[0127] S1-ii. 94 kg of adipic acid, 93 kg of 1,4-butanediol, and 0.23 kg of tetrabutyl titanate were physically mixed, and a 1,4-butanediol solution containing sodium carbonate was added. The pH of the mixture was adjusted to 5.5 to obtain slurry B. Slurry B was transferred to a stirred reactor. The reaction mixture was esterified at 225°C and 0.8 bar for 3 hours. The resulting second ester had a viscosity of 14 ml / g.

[0128] S2. The first esterification product and the second esterification product obtained in steps S1-i and S1-ii were mixed, and the mixture was transferred to a stirred vertical reactor. 0.19 kg of tetrabutyl titanate was added, and the reaction mixture was pre-polycondensed at 250° C. and a pressure of 0.25 bar in the reactor for 180 minutes. The viscosity of the resulting prepolymer was 55 ml / g.

[0129] S3. The prepolymer obtained in step S2 was transferred to a horizontal reactor with stirring and polycondensed at 240°C and a pressure of 2.0 mbar for 100 minutes. The viscosity of the resulting biodegradable aliphatic polyester composition was 187 ml / g.

[0130] The total content and mass ratio η of the compounds represented by formula (I) and formula (II) in the biodegradable aliphatic polyester composition are shown in Table 1.

[0131] Example 3

[0132] Example 3 provides a biodegradable aliphatic polyester composition, the preparation method of which is as follows:

[0133] S1-i. 195 kg of succinic acid, 215 kg of 1,4-butanediol, and 1.3 kg of glycerol were mixed, a 1,4-butanediol solution containing sodium hydroxide was added, and the pH of the system was adjusted to 5.8 to obtain slurry A. The slurry A was transferred to a stirred reactor, and the reaction mixture was esterified at a temperature of 180 ° C and a pressure of 1.0 bar for 3 hours. The viscosity of the obtained first ester was 13 ml / g;

[0134] S1-ii. 76 kg of adipic acid, 70 kg of 1,4-butanediol and 0.24 kg of tetrabutyl titanate were physically mixed, a 1,4-butanediol solution containing sodium hydroxide was added, and the pH value of the system was adjusted to 5.8 to obtain slurry B. The slurry B was transferred to a stirred reactor, and the reaction mixture was esterified at a temperature of 190 ° C and a pressure of 1.0 bar for 3 hours to obtain a second esterified product with a viscosity of 7 ml / g;

[0135] S2. The first esterification product and the second esterification product obtained in steps S1-i and S1-ii were mixed, and the mixture was transferred to a stirred vertical reactor. 0.16 kg of tetrabutyl titanate was added, and the reaction mixture was pre-polycondensed at 245° C. and a pressure of 0.30 bar in the reactor for 140 minutes. The viscosity of the resulting prepolymer was 34 ml / g.

[0136] S3. The prepolymer obtained in step S2 was transferred to a horizontal reactor with stirring and subjected to polycondensation at 244°C and a pressure of 1.4 mbar for 90 minutes. The viscosity of the resulting biodegradable aliphatic polyester composition was 173 ml / g.

[0137] The total content and mass ratio η of the compounds represented by formula (I) and formula (II) in the biodegradable aliphatic polyester composition are shown in Table 1.

[0138] Example 4

[0139] Example 4 provides a biodegradable aliphatic polyester composition, which is prepared as follows:

[0140] S1-i. 195 kg of succinic acid, 210 kg of 1,4-butanediol, and 1.3 kg of glycerol were mixed, a 1,4-butanediol solution containing sodium hydroxide was added, and the pH of the system was adjusted to 4.6 to obtain slurry A. The slurry A was transferred to a stirred reactor, and the reaction mixture was esterified at a temperature of 170 ° C and a pressure of 0.85 bar for 3 hours. The viscosity of the obtained first ester was 10 ml / g;

[0141] S1-ii. 53 kg of adipic acid, 52 kg of 1,4-butanediol, and 0.22 kg of tetrabutyl titanate were physically mixed, and a 1,4-butanediol solution containing sodium hydroxide was added. The pH of the mixture was adjusted to 5.4 to obtain slurry B. Slurry B was transferred to a stirred reactor. The reaction mixture was esterified at 200°C and 1.0 bar for 4 hours. The resulting second ester had a viscosity of 12 ml / g.

[0142] S2. The first esterification product and the second esterification product obtained in steps S1-i and S1-ii were mixed, and the mixture was transferred to a stirred vertical reactor. 0.15 kg of tetrabutyl titanate was added, and the reaction mixture was pre-polycondensed at 242° C. and a pressure of 0.28 bar in the reactor for 135 minutes. The viscosity of the resulting prepolymer was 35 ml / g.

[0143] S3. The prepolymer obtained in step S2 was transferred to a horizontal reactor with stirring and polycondensed at 245°C and a pressure of 1.5 mbar for 90 minutes. The viscosity of the resulting biodegradable aliphatic polyester composition was 175 ml / g.

[0144] The total content and mass ratio η of the compounds represented by formula (I) and formula (II) in the biodegradable aliphatic polyester composition are shown in Table 1.

[0145] Example 5

[0146] Example 5 provides a biodegradable aliphatic polyester composition, the preparation method of which is as follows:

[0147] S1-i. 195 kg of succinic acid, 215 kg of 1,4-butanediol, and 1.3 kg of glycerol were mixed, a 1,4-butanediol solution containing sodium hydroxide was added, and the pH of the system was adjusted to 3.2 to obtain slurry A. The slurry A was transferred to a stirred reactor, and the reaction mixture was esterified at a temperature of 190 ° C and a pressure of 0.7 bar for 3 hours. The viscosity of the obtained first ester was 9 ml / g;

[0148] S1-ii. Physically mix 76 kg of adipic acid, 70 kg of 1,4-butanediol, and 0.21 kg of tetrabutyl titanate. Add a 1,4-butanediol solution containing sodium hydroxide and adjust the pH of the mixture to 5.2 to obtain slurry B. Transfer slurry B to a stirred reactor. Esterify the reaction mixture at 195°C and 0.9 bar for 4 hours. The resulting second ester has a viscosity of 10 ml / g.

[0149] S2. The first esterification product and the second esterification product obtained in steps S1-i and S1-ii were mixed, and the mixture was transferred to a stirred vertical reactor. 0.13 kg of tetrabutyl titanate was added, and the reaction mixture was pre-polycondensed at 245° C. and a pressure of 0.35 bar in the reactor for 75 minutes. The viscosity of the resulting prepolymer was 24 ml / g.

[0150] S3. The prepolymer obtained in step S2 was transferred to a horizontal reactor with stirring and polycondensed at 248°C and a pressure of 1.2 mbar for 110 minutes. The viscosity of the resulting biodegradable aliphatic polyester composition was 169 ml / g.

[0151] The total content and mass ratio η of the compounds represented by formula (I) and formula (II) in the biodegradable aliphatic polyester composition are shown in Table 1.

[0152] Example 6

[0153] Example 6 provides a biodegradable aliphatic polyester composition, the preparation method of which is as follows:

[0154] S1-i. 195 kg of succinic acid, 215 kg of 1,4-butanediol, and 1.3 kg of glycerol were mixed, a 1,4-butanediol solution containing sodium hydroxide was added, and the pH of the system was adjusted to 4.5 to obtain slurry A. The slurry A was transferred to a stirred reactor, and the reaction mixture was esterified at a temperature of 200 ° C and a pressure of 0.8 bar for 4 hours. The viscosity of the obtained first ester was 11 ml / g;

[0155] S1-ii. 114 kg of adipic acid, 105 kg of 1,4-butanediol, and 0.28 kg of tetrabutyl titanate were physically mixed, and a 1,4-butanediol solution containing sodium hydroxide was added. The pH of the mixture was adjusted to 5.7 to obtain slurry B. Slurry B was transferred to a stirred reactor. The reaction mixture was esterified at 180°C and a pressure of 0.9 bar for 3 hours. The resulting second ester had a viscosity of 9 ml / g.

[0156] S2. The first esterification product and the second esterification product obtained in steps S1-i and S1-ii were mixed, and the mixture was transferred to a stirred vertical reactor. 0.17 kg of tetrabutyl titanate was added, and the reaction mixture was pre-polycondensed at 245° C. and a pressure of 0.55 bar in the reactor for 110 minutes. The viscosity of the resulting prepolymer was 29 ml / g.

[0157] S3. The prepolymer obtained in step S2 was transferred to a horizontal reactor with stirring and polycondensed at 245°C and a pressure of 1.8 mbar for 100 minutes. The viscosity of the resulting biodegradable aliphatic polyester composition was 162 ml / g.

[0158] The total content and mass ratio η of the compounds represented by formula (I) and formula (II) in the biodegradable aliphatic polyester composition are shown in Table 1.

[0159] Example 7

[0160] Example 7 provides a biodegradable aliphatic polyester composition, which is prepared as follows:

[0161] S1-i. 195 kg of succinic acid, 215 kg of 1,4-butanediol, and 1.3 kg of glycerol were mixed, a 1,4-butanediol solution containing sodium hydroxide was added, and the pH of the system was adjusted to 4.0 to obtain slurry A. The slurry A was transferred to a stirred reactor, and the reaction mixture was esterified at a temperature of 210 ° C and a pressure of 0.85 bar for 4 hours. The viscosity of the obtained first ester was 14 ml / g;

[0162] S1-ii. 114 kg of adipic acid, 105 kg of 1,4-butanediol, and 0.28 kg of tetrabutyl titanate were physically mixed, and a 1,4-butanediol solution containing sodium hydroxide was added. The pH of the mixture was adjusted to 5.5 to obtain slurry B. Slurry B was transferred to a stirred reactor. The reaction mixture was esterified at 190°C and 0.8 bar for 4 hours. The resulting second ester had a viscosity of 13 ml / g.

[0163] S2. The first esterification product and the second esterification product obtained in steps S1-i and S1-ii were mixed, and the mixture was transferred to a stirred vertical reactor. 0.19 kg of tetrabutyl titanate was added, and the reaction mixture was pre-polycondensed at 248° C. and a pressure of 0.40 bar in the reactor for 110 minutes. The viscosity of the resulting prepolymer was 35 ml / g.

[0164] S3. The prepolymer obtained in step S2 was transferred to a horizontal reactor with stirring and polycondensed at 245°C and a pressure of 1.8 mbar for 95 minutes. The viscosity of the resulting biodegradable aliphatic polyester composition was 176 ml / g.

[0165] The total content and mass ratio η of the compounds represented by formula (I) and formula (II) in the biodegradable aliphatic polyester composition are shown in Table 1.

[0166] Example 8

[0167] Example 8 provides a biodegradable aliphatic polyester composition, the preparation method of which is as follows:

[0168] S1-i. 195 kg of succinic acid, 215 kg of 1,4-butanediol, and 1.3 kg of glycerol were mixed, a 1,4-butanediol solution containing sodium hydroxide was added, and the pH of the system was adjusted to 5.7 to obtain slurry A. The slurry A was transferred to a stirred reactor, and the reaction mixture was esterified at a temperature of 160 ° C and a pressure of 1.0 bar for 5 hours. The viscosity of the obtained first ester was 8 ml / g;

[0169] S1-ii. 53 kg of adipic acid, 52 kg of 1,4-butanediol, and 0.26 kg of tetrabutyl titanate were physically mixed, and a 1,4-butanediol solution containing sodium hydroxide was added. The pH of the mixture was adjusted to 5.6 to obtain slurry B. Slurry B was transferred to a stirred reactor. The reaction mixture was esterified at 200°C and 0.9 bar for 4 hours. The resulting second ester had a viscosity of 10 ml / g.

[0170] S2. The first esterification product and the second esterification product obtained in steps S1-i and S1-ii were mixed, and the mixture was transferred to a stirred vertical reactor. 0.17 kg of tetrabutyl titanate was added, and the reaction mixture was pre-polycondensed at 246° C. and a pressure of 0.70 bar in the reactor for 100 minutes. The viscosity of the resulting prepolymer was 26 ml / g.

[0171] S3. The prepolymer obtained in step S2 was transferred to a stirred horizontal reactor and subjected to polycondensation at 248°C and a pressure of 1.6 mbar for 90 minutes. The viscosity of the resulting biodegradable aliphatic polyester composition was 163 ml / g.

[0172] The total content and mass ratio η of the compounds represented by formula (I) and formula (II) in the biodegradable aliphatic polyester composition are shown in Table 1.

[0173] Example 9

[0174] Example 9 provides a biodegradable aliphatic polyester composition, the preparation method of which is as follows:

[0175] S1-i. 195 kg of succinic acid, 215 kg of 1,4-butanediol, and 1.5 kg of glycerol were mixed, a 1,4-butanediol solution containing sodium carbonate was added, and the pH of the system was adjusted to 4.2 to obtain slurry A. The slurry A was transferred to a stirred reactor, and the reaction mixture was esterified at a temperature of 210 ° C and a pressure of 0.7 bar for 3 hours. The viscosity of the obtained first ester was 15 ml / g;

[0176] S1-ii. Physically mix 94 kg of adipic acid, 93 kg of 1,4-butanediol, and 0.23 kg of tetrabutyl titanate. Add a 1,4-butanediol solution containing sodium carbonate and adjust the pH of the mixture to 5.4 to obtain slurry B. Transfer slurry B to a stirred reactor. Esterify the reaction mixture at 225°C and 0.8 bar for 3 hours. The resulting esterified product has a viscosity of 14 ml / g.

[0177] S2. The first esterification product and the second esterification product obtained in steps S1-i and S1-ii were mixed, and the mixture was transferred to a stirred vertical reactor. 0.10 kg of tetrabutyl titanate was added, and the reaction mixture was pre-polycondensed at 235° C. and a pressure of 0.60 bar in the reactor for 75 minutes. The viscosity of the resulting prepolymer was 25 ml / g.

[0178] S3. The prepolymer obtained in step S2 was transferred to a horizontal reactor with stirring and polycondensed at 242°C and a pressure of 2.2 mbar for 85 minutes. The viscosity of the final product was 143 ml / g.

[0179] S4. The final polymer product in step S3 was passed through a static mixer, 1.0 kg of hexamethylene diisocyanate was added, and the mixture was mixed and reacted at 210°C for 7 minutes to obtain a biodegradable aliphatic polyester composition having a viscosity of 190 ml / g.

[0180] The total content and mass ratio η of the compounds represented by formula (I) and formula (II) in the biodegradable aliphatic polyester composition are shown in Table 1.

[0181] Comparative Example 1

[0182] Comparative Example 1 provides a biodegradable aliphatic polyester composition, the preparation method of which is as follows:

[0183] S1-i. 195 kg of succinic acid, 210 kg of 1,4-butanediol, and 1.2 kg of glycerol were mixed to obtain slurry A. The slurry A was transferred to a stirred reactor, and the reaction mixture was esterified at a temperature of 190 ° C and a pressure of 1.1 bar for 3 hours. The viscosity of the first ester was 10 ml / g.

[0184] S1-ii. 53 kg of adipic acid, 52 kg of 1,4-butanediol, and 0.20 kg of tetrabutyl titanate were physically mixed to obtain slurry B. Slurry B was transferred to a stirred reactor. The reaction mixture was esterified at 210°C and 1.0 bar for 3 hours. The resulting second ester had a viscosity of 12 ml / g.

[0185] S2. The first esterification product and the second esterification product obtained in steps S1-i and S1-ii were mixed, and the mixture was transferred to a stirred vertical reactor. 0.14 kg of tetrabutyl titanate was added, and the reaction mixture was pre-polycondensed at 245° C. and a pressure of 0.28 bar in the reactor for 110 minutes. The viscosity of the resulting prepolymer was 41 ml / g.

[0186] S3. The prepolymer obtained in step S2 was transferred to a horizontal reactor with stirring and subjected to polycondensation at 248°C and a pressure of 1.5 mbar for 90 minutes. The viscosity of the resulting biodegradable aliphatic polyester composition was 186 ml / g.

[0187] The total content and mass ratio η of the compounds represented by formula (I) and formula (II) in the biodegradable aliphatic polyester composition are shown in Table 1.

[0188] Comparative Example 2

[0189] Comparative Example 2 provides a biodegradable aliphatic polyester composition, the preparation method of which is as follows:

[0190] S1-i. 195 kg of succinic acid, 225 kg of 1,4-butanediol, and 1.2 kg of glycerol were mixed, a 1,4-butanediol solution containing sodium hydroxide was added, and the pH of the system was adjusted to 4.4 to obtain slurry A. The slurry A was transferred to a stirred reactor, and the reaction mixture was esterified at a temperature of 200 ° C and a pressure of 0.8 bar for 6 hours. The viscosity of the obtained first ester was 17 ml / g;

[0191] S1-ii. 53 kg of adipic acid, 52 kg of 1,4-butanediol, and 0.24 kg of tetrabutyl titanate were physically mixed to obtain slurry B. Slurry B was transferred to a stirred reactor. The reaction mixture was esterified at 220°C and 0.70 bar for 5 hours. The resulting second ester had a viscosity of 19 ml / g.

[0192] S2. The first esterification product and the second esterification product obtained in steps S1-i and S1-ii were mixed, and the mixture was transferred to a stirred vertical reactor. 0.18 kg of tetrabutyl titanate was added, and the reaction mixture was pre-polycondensed at 245° C. and a pressure of 0.2 bar in the reactor for 150 minutes. The viscosity of the resulting prepolymer was 59 ml / g.

[0193] S3. The prepolymer obtained in step S2 was transferred to a stirred horizontal reactor and subjected to polycondensation at 243°C and a pressure of 2.0 mbar for 80 minutes. The viscosity of the resulting biodegradable aliphatic polyester was 192 ml / g.

[0194] The total content and mass ratio η of the compounds represented by formula (I) and formula (II) in the biodegradable aliphatic polyester composition are shown in Table 1.

[0195] Comparative Example 3

[0196] Comparative Example 3 provides a biodegradable aliphatic polyester composition, the preparation method of which is as follows:

[0197] S1-i. 195 kg of succinic acid, 225 kg of 1,4-butanediol and 1.2 kg of glycerol were mixed, a 1,4-butanediol solution containing sodium hydroxide was added, and the pH of the succinic acid was adjusted to 5.1 to obtain slurry A. The slurry A was transferred to a stirred reactor, and the reaction mixture was esterified at a temperature of 160 ° C and a pressure of 0.9 bar for 5 hours. The viscosity of the obtained first ester was 9 ml / g;

[0198] S1-ii. 33 kg of adipic acid, 28 kg of 1,4-butanediol, and 0.23 kg of tetrabutyl titanate were physically mixed to obtain slurry B. Slurry B was transferred to a stirred reactor. The reaction mixture was esterified at 205°C and 1.0 bar for 3 hours. The resulting second ester had a viscosity of 11 ml / g.

[0199] S2. The first esterification product and the second esterification product obtained in steps S1-i and S1-ii were mixed, and the mixture was transferred to a stirred vertical reactor. 0.13 kg of tetrabutyl titanate was added, and the reaction mixture was pre-polycondensed at 252° C. and a pressure of 0.50 bar in the reactor for 110 minutes. The viscosity of the resulting prepolymer was 28 ml / g.

[0200] S3. The prepolymer obtained in step S2 was transferred to a horizontal reactor with stirring and polycondensed at 251°C and a pressure of 1.3 mbar for 75 minutes. The viscosity of the resulting biodegradable aliphatic polyester composition was 163 ml / g.

[0201] The total content and mass ratio η of the compounds represented by formula (I) and formula (II) in the biodegradable aliphatic polyester composition are shown in Table 1.

[0202] The food contact performance of the biodegradable aliphatic polyester compositions prepared in the above examples and comparative examples was evaluated, and the total migration amount was tested. The results are shown in Table 1.

[0203] Table 1

[0204] According to the test results in Table 1, it can be seen that the biodegradable aliphatic polyester compositions prepared in various embodiments of the present invention were prepared into films with a thickness of 25±2 μm. The food contact test was conducted under OM6 conditions with 10% ethanol as the simulated liquid. The total migration amount of the samples was ≤10 mg / dm 2 .

[0205] In Comparative Examples 1 to 3, the weight ratio η of the compound represented by formula (I) to the compound represented by formula (II) in the biodegradable aliphatic polyester composition is greater than 6:1, and the total migration amount of the obtained biodegradable aliphatic polyester composition samples is also too large.

[0206] Application Examples

[0207] Application Examples 1 to 3 provide a biodegradable mixture, respectively. The component contents are shown in Table 2. The preparation methods are as follows:

[0208] According to Table 2, the components were mixed and added to a twin-screw extruder (L / D = 48; diameter 40 mm) for melt mixing and extrusion granulation. The extrusion temperature was 140-200 ° C, the screw speed was 300 rpm, and the vacuum was -0.50 to -0.65 kg / cm 2 , obtaining a biodegradable mixture.

[0209] Table 2 Component contents of application examples 1 to 3 (wt.%)

[0210] The biodegradable mixtures of Examples 1 to 3 were subjected to food contact tests and heat seal strength tests. The results are shown in Table 3.

[0211] Table 3

[0212] It can be seen that the biodegradable mixture prepared by using the biodegradable aliphatic polyester composition of the present application not only has an extremely low total migration amount, but also has high heat sealing strength and excellent heat sealing performance.

[0213] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the essence and scope of the technical solutions of the present invention.

Claims

1. A biodegradable aliphatic polyester composition, It is characterized in that include: Component i), a biodegradable aliphatic polyester, wherein the biodegradable aliphatic polyester comprises: Component A, a dicarboxylic acid compound, based on the total molar amount of component A, comprises: a1, 68-82 mol% succinic acid, a2, 18 to 32 mol% of adipic acid; Component B, 1,4-butanediol in an amount at least equimolar to that of component A; Component ii), a cyclic ester represented by formula (I) and formula (II), Wherein n and m in formula (I) and formula (II) are positive integers ranging from 1 to 8; Based on the total weight of the biodegradable aliphatic polyester composition, the content of the cyclic ester is 0.6-1.1 wt.%, and the mass ratio η of the compounds represented by formula (I) and formula (II) is 2-6:

1.

2. The biodegradable aliphatic polyester composition according to claim 1, It is characterized in that The component A, based on the total molar amount of the component A, comprises: a1, 72-78 mol% succinic acid, a2, 22 to 28 mol% of adipic acid.

3. The biodegradable aliphatic polyester composition according to claim 1, It is characterized in that At least one of the following (1) to (2): (1) The mass ratio of the compounds represented by formula (I) to formula (II) is (3.2-4.8):1; (2) The biodegradable aliphatic polyester composition is based on the EU 10-2011 standard, according to the OM6 test conditions, with 10% ethanol as the simulated liquid, and the total migration amount is less than or equal to 10 mg / dm 2 .

4. The biodegradable aliphatic polyester composition according to claim 1, It is characterized in that The biodegradable aliphatic polyester composition may further include component C, a chain extender: The chain extender includes one or more of the following components: c1, isocyanate, c2, peroxide, c3, epoxide, c4, oxazoline, oxazine, caprolactam and / or carbodiimide.

5. A method for preparing the biodegradable aliphatic polyester composition according to any one of claims 1 to 4, It is characterized in that The steps include: S1-i. Component a1 is mixed with a portion of component B, an alkaline compound is added to adjust the pH value of the system to 3.2 to 5.8, a catalyst is added or not added to obtain a slurry A, and the slurry A is subjected to an esterification or transesterification reaction until the viscosity of the esterified product is 5 to 15 ml / g as measured according to DIN 53728-3-1985, to obtain a first esterified product; S1-ii. Component a2 is mixed with the remaining component B, an alkaline compound is added to adjust the pH value of the system to 5.2 to 5.8, a catalyst is added or not added and the mixture is mixed to obtain a slurry B, and the slurry B is subjected to an esterification or transesterification reaction until the viscosity of the esterified product is 7 to 16 ml / g as measured according to DIN 53728-3-1985, to obtain a second esterified product; S2. The first esterification product and the second esterification product obtained in steps S1-i and S1-ii are mixed to obtain a mixture of esterification products, and the mixture is pre-polycondensed until the viscosity of the prepolymer is 24 to 55 ml / g as measured according to DIN 53728-3-1985; S3. polycondensing the prepolymer obtained in step S2 until the viscosity of the polycondensation product thereof measured according to DIN 53728-3-1985 is 143 to 226 ml / g, that is, the biodegradable aliphatic polyester composition.

6. The preparation method according to claim 5, It is characterized in that At least one of the following (1) to (2): (1) The alkaline compound is a carbonate and / or a hydroxide; (2) In step S2, the viscosity of the prepolymer product measured according to DIN 53728-3-1985 is 32 to 46 ml / g.

7. The preparation method according to claim 5, It is characterized in that The method further comprises step S4, mixing the polycondensation product of step S3 and a chain extender to carry out a chain extension reaction; the viscosity of the chain extension product obtained through the chain extension reaction is 167-242 ml / g as measured according to DIN 53728-3-1985.

8. Use of the biodegradable aliphatic polyester composition according to any one of claims 1 to 4 in cling film.

9. A biodegradable mixture, It is characterized in that The composition comprises the following weight percentages: i) based on the total weight of components i) and ii), 5 to 95 wt.% of the Biodegradable aliphatic polyester composition, ii) based on the total weight of components i) and ii), 5 to 95 wt.% of at least one or more components selected from aliphatic-aromatic copolyesters, aliphatic polyesters, starch, cellulose, polyhydroxyalkanoate, polyglycolic acid and polylactic acid, iii) 0 to 35 wt.% of talc, based on the total weight of components i) to iv), iv) 0 to 20 wt.% of calcium carbonate, based on the total weight of components i) to iv).

10. Use of the biodegradable mixture according to claim 9 in preparing a heat-sealing film.

Citation Information

Patent Citations

  • Biodegradable polyester composition

    CN105585827A

  • Polyester resin composition and method for producing same

    CN106103540A

  • Production method for poly(butylene succinate-co-butylene adipate) with low color value

    CN106867207A

  • Food-grade PBS biodegradable polyester synthesized based on acid removal and preparation method of food-grade PBS biodegradable polyester

    CN115197402A

  • Biodegradable aliphatic polyester as well as preparation method and application thereof

    CN115785413A