TPU with cyclic additives
The composition of thermoplastic polyurethane with specific molecular weight and functional groups addresses the issue of blooming and mechanical properties, achieving reduced blooming and retained flexibility and strength.
Patent Information
- Application Number
- PCT/EP2024/065086
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-01
- Filing Date
- 2024-05-31
- Publication Date
- 2024-12-05
AI Technical Summary
Existing thermoplastic polyurethanes have a reduced tendency to blooming but lack sufficient mechanical properties.
A composition comprising a thermoplastic polyurethane reaction product of diisocyanate, polyol, and chain extender, with an additional component having a molecular weight of 50 to 500 g/mol, featuring ether and ester functional groups, which reduces blooming while maintaining good mechanical properties.
The composition exhibits a significantly reduced tendency to blooming with retained cold flexibility and mechanical properties, making it suitable for various applications.
Smart Images

Figure IMGF000031_0001 
Figure IMGF000031_0002 
Figure IMGF000032_0001
Abstract
Description
[0001] TPU with cyclic additives
[0002] The present invention relates to a composition comprising at least a thermoplastic polyurethane being the reaction product of at least one diisocyanate (11), at least one polyol (P1), and at least one chain extender (C1), and at least one component (CA1) with a molecular weight Mn in the range of from 50 to 500 g / mol, determined by GPC according to DIN 55672-1 (2016-03-01), using DMF as the flow agent and PM MA as the standard for the detection of oligomers < 500 g / mol, using a UV detector at a wavelength of 254 nm for differentiation from additives and detection of the oligomers by using a refractive index (Rl) detector, wherein the polyol (P1) comprises functional groups (F1) selected from ether groups and ester groups in the polymer backbone and the component (CA1 ) comprises functional groups (F2) selected from ether groups and ester groups. Furthermore, the present invention is directed to a Process for preparing a composition comprising a thermoplastic polyurethane and at least one component (CA1) according to the present invention and the use of a composition according to the present invention for the production of shaped bodies, coatings, hoses, films, nonwoven articles or fibers, foamed parts, particle foams, added manufacturing filaments, 3D printing, injection molding parts for the use in industrial applications, consumer goods including sports, automotive, agriculture, construction applications.
[0003] Processes for producing polyurethanes are already known from the prior art. A common occurrence in the case of polyurethanes based on polyester polyols having high molecular weights is blooming, which leads to unwanted material properties including the optic appearance of the material. This effect can be controlled only with difficulty. The prior art discloses various strategies for reducing blooming effects. There are many descriptions of the use of chain termination reagents or the use of particular polyester polyols based on propylene glycols for reduction of the blooming effects.
[0004] For instance, WO15 / 000722 A1 discloses polyurethanes based on at least one polyisocyanate and at least one polyester polyol, where the polyester polyol is based on at least one polyhydric alcohol and a mixture of at least two dicarboxylic acids, where at least one of the at least two dicarboxylic acids has been obtained at least partly from renewable raw materials, and to processes for producing such polyurethanes and shaped bodies comprising such polyurethanes. WO 2019 / 002263 discloses thermoplastic polyurethanes obtainable or obtained by reacting at least a polyisocyanate composition comprising at least one polyisocyanate, at least one chain extender, and at least one polyol composition, wherein the polyol composition comprises at least one polyester polyol (P1 ) which is obtainable by reacting an aliphatic dicarboxylic acid having 2 to 12 carbon atoms and a mixture (M 1) comprising propane-1 ,3-diol and a further diol (D1 ) having 2 to 12 carbon atoms, preferably butane-1 ,4-diol. The polyurethanes disclosed show a low tendency to blooming.
[0005] EP 0687695 A1 relates to the controlled reduction of the blooming effect by addition of a monofunctional alcohol for thermoplastic polyurethanes based on polyester polyols. US8790763 discloses the reduction of blooming by the use of a polyester polyol with 1 ,3- propylene glycol as repeat unit.
[0006] WO 2012 / 173911 A1 describes the production of thermoplastic polyurethanes having reduced blooming by the use of polyester polyols with biobased glycols.
[0007] US 2003 / 0036621 relates to the reduction of blooming in the case of thermoplastic polyurethanes by chain termination additions such as monofunctional alcohols (with chain length > C14, monoisocyanates or monoamines).
[0008] WO 2009 / 103767 A1 discloses the production of thermoplastic polyurethanes having reduced deposit formation by the use of various mixtures of alkanediols as chain extender.
[0009] However, the processes known from the prior art frequently lead to polyurethanes that do have a reduced tendency to blooming but do not have sufficiently good mechanical properties.
[0010] It was therefore an object of the present invention to provide thermoplastic polyurethanes having a reduced tendency to blooming with good mechanical properties.
[0011] This object is achieved in accordance with the invention by a composition comprising at least the components (i) and (ii):
[0012] (i) a thermoplastic polyurethane being the reaction product of at least one diisocyanate (11 ), at least one polyol (P1 ), and at least one chain extender (C1 ), and
[0013] (ii) at least one component (CA1 ) with a molecular weight Mn in the range of from 50 to 500 g / mol, determined by GPC according to DIN 55672-1 (2016-03-01 ), using DMF as the flow agent and PM MA as the standard for the detection of oligomers < 500 g / mol, using a UV detector at a wavelength of 254 nm for differentiation from additives and detection of the oligomers by using a refractive index (Rl) detector, wherein the polyol (P1 ) comprises functional groups (F1) selected from ether groups and ester groups in the polymer backbone and the component (CA1) comprises functional groups (F2) selected from ether groups and ester groups.
[0014] It has been found that, surprisingly, the composition according to the invention have a significantly reduced tendency to blooming with retention of good cold flexibility and mechanical properties.
[0015] The composition according to the present invention comprises at least the components (i) and (ii) and may comprise further components. The thermoplastic polyurethane present as component (i) is the reaction product of at least one diisocyanate (11 ), at least one polyol (P1), and at least one chain extender (C1). The polyol (P1 ) used in the preparation comprises functional groups (F1) selected from ether groups and ester groups in the polymer backbone according to the present invention. According to the present invention, functional groups in the polymer backbone may also be the functional groups connecting the monomer units. Preferably, at least a part of the functional groups (F1) are functional groups connecting the monomer units of polyol (P1). In the context of the present invention, polyol (P1) preferably is a polyetherpolyol or a polyesterpolyol. The component (CA1) has a molecular weight Mn in the range of from 50 to 500 g / mol, determined-by GPC according to DIN 55672-1 (2016-03-01), using DMF as the flow agent and PM MA as the standard and comprises functional groups (F2) selected from ether groups and ester groups. Preferably, component (CA1) is an oligomer and the functional groups (F2) connect the monomer units. More preferable, component (CA1) a oligomer without reactive functional groups, in particular a cyclic oligomer. The polyol (P1) and the component (CA1) may also comprise further functional groups. Preferably, polyol (P1) and the component (CA1) comprise only functional groups selected from ether groups and ester groups.
[0016] In the context of the present invention, functional groups (F1) and (F2) may be the same or different. According to the present invention, it is thus possible that the thermoplastic polyurethane is based on a polyesterpolyol and component (CA1) comprises ester groups or that the thermoplastic polyurethane is based on a polyesterpolyol and component (CA1) comprises ether groups or that the thermoplastic polyurethane is based on a polyetherpolyol and component (CA1) comprises ester groups or that hat the thermoplastic polyurethane is based on a polyetherpolyol and component (CA1) comprises ether groups.
[0017] According to a further embodiment, the present invention is also directed to the composition as disclosed above, wherein the functional groups (F1) and (F2) are the same, for example, (F1) and (F2) are ether groups or (F1) and (F2) are ester groups.
[0018] According to a further embodiment, the present invention is also directed to the composition as disclosed above, wherein the component (CA1) is a polyester, preferably a cyclic polyester.
[0019] Suitable polyesters as component (CA1) are for example the reaction products of a dicar- boyxylic acid (a1) and a diol (d1). Suitable dicarboxylic acids and diols are in principle known and may for example be selected from the dicarboxylic acids and diols disclosed above. Preferably, the dicarboxylic acid (a1) is selected from the group consisting of adipic acid, succinic acid, or a mixture thereof. Suitable diols (d1) may for example be ethanediol, propanediol, butanediol, pentanediol, and hexanediol or a mixture thereof.
[0020] According to a further embodiment, the present invention is also directed to the composition as disclosed above, wherein the component (CA1) is a polyester being the reaction product of a dicarboxylic acid (a1) and a diol (d1), the dicarboxylic acid (a1) being selected from the group consisting of adipic acid, succinic acid, or a mixture thereof, and the diol (d1) is selected from the group consisting of ethanediol, propanediol, butanediol, pentanediol, and hexanediol or a mixture thereof. It has been found that also mixtures of diols may be used. According to a further embodiment, the present invention therefore is also directed to the composition as disclosed above, wherein a mixture of two diols selected from the group consisting of ethanediol, propanediol, butanediol, pentanediol, and hexanediol is used as diol (d1 ).
[0021] According to the present invention, polyol (P1) is used for the preparation of the thermoplastic polyurethane. It is also possible to use mixtures of two or more polyols. Suitable polyols are in principle known to the person skilled in the art.
[0022] Preferably, the polyol (P1 ) is a polyesterpolyol. Suitable polyesterpolyols are in principle known to the person skilled in the art.
[0023] Preferably in accordance with the invention, the polyol (P1) is selected from the group consisting of polyester polyols and more preferably from linear polyester polyols.
[0024] According to a further embodiment, the present invention is also directed to the composition as disclosed above, wherein the polyol (P1) is a polyesterpolyol.
[0025] Suitable polyester polyols, especially polyester diols, may be prepared, for example, from dicarboxylic acids having 2 to 12 carbon atoms, preferably 4 to 10 carbon atoms, and polyhydric alcohols. Examples of useful dicarboxylic acids include: aliphatic dicarboxylic acids, such as succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid and sebacic acid, or aromatic dicarboxylic acids, such as phthalic acid, isophthalic acid and terephthalic acid. The dicarboxylic acids may be used individually or in the form of mixtures, for example in the form of a mixture of succinic acid, sebacic acid and adipic acid. For preparation of the polyester diols, it may possibly be advantageous to use, rather than the dicarboxylic acids, the corresponding dicarboxylic acid derivatives such as carboxylic diesters having 1 to 4 carbon atoms in the alcohol radical, for example dimethyl terephthalate or dimethyl adipate, carboxylic anhydrides, for example succinic anhydride, glutaric anhydride or phthalic anhydride, or carbonyl chlorides. Examples of polyhydric alcohols are glycols having 2 to 10, preferably 2 to 6, carbon atoms, for example ethylene glycol, diethylene glycol, butane-1 ,4-diol, pentane-1 ,5-diol, hexane-1 ,6-diol, decane-1 , 10- diol, 2,2-dimethylpropane-1 ,3-diol, propane-1 ,3-diol, 2-methylpropane-1 ,3-diol, 3-methylpen- tane-1 ,5-diol or dipropylene glycol. The polyhydric alcohols may be used individually or as mixtures, for example in the form of a butane-1 ,4-diol and / or propane-1 ,3-diol mixture. In addition, it is also possible to include small amounts of up to 3% by weight of the total reaction mixture of higher-functionality polyols of low molecular weight, for example 1 ,1 ,1 -trimethylolpropane or pentaerythritol. Preference is given in accordance with the invention to the use of exclusively bifunctional starting compounds.
[0026] The molecular weight of the polyol (P1 ) used may vary within wide ranges. Suitable examples include polyols that have an average molecular weight in the range from 500 to 3500 g / mol, further preferably in the range from 800 to 3000 g / mol. The molecular weight of the polyesterpolyol used may also vary within wide ranges. Suitable examples include polyesterpolyols that have an average molecular weight in the range from 2000 to 3500 g / mol, further preferably in the range from 2500 to 3200 g / mol.
[0027] Typically, the polyesterpolyol (P1 ) used is the reaction product of a dicarboxylic acid (a2) and a diol (d2). In case mixtures of dicarboxylic acids are used, the ratio typically is in the range of from 9:1 to 1 :9, preferably in the range of from 8:2 to 2:8.
[0028] Preferably, the dicarboxylic acid (a2) being selected from the group consisting of adipic acid, succinic acid, or a mixture thereof. Preferably, the diol (d2) is selected from the group consisting of ethanediol, propanediol, butanediol, pentanediol, and hexanediol or a mixture thereof.
[0029] According to a further embodiment, the present invention is also directed to the composition as disclosed above, wherein the polyol is a polyesterpolyol being the reaction product of a dicarboxylic acid (a2) and a diol (d2), the dicarboxylic acid (a2) being selected from the group consisting of adipic acid, succinic acid, or a mixture thereof, and the diol (d2) is selected from the group consisting of ethanediol, propanediol, butanediol, pentanediol, and hexanediol or a mixture thereof.
[0030] In the context of the present invention, it is particularly preferable that diol (d1) and diol (d2) are the same. Also the dicarboxylic acid (a1) and dicarboxylic acid (a2) may be the same in the context of the present invention.
[0031] According to the invention, polyol (P1) may also be a polyetherpolyol, for example a polyetherpolyol such as polytetramethylene ether glycol, polyethylene glycol, or polypropylene glycol.
[0032] According to a further embodiment, the present invention is also directed to the composition as disclosed above, wherein the polyol (P1) is a polyetherpolyol. According to a further embodiment, the present invention is also directed to the composition as disclosed above, wherein the polyol is a polyetherpolyol selected from the group consisting of polyethtyleneglycol, polypropyleneglycol, polytrimethyleneglycol and polytetramethyleneglycol.
[0033] The molecular weight of the polyetherpolyol used may also vary within wide ranges. Suitable examples include polyetherpolyols that have an average molecular weight in the range from 600 to 3000 g / mol, preferably in the range from 800 to 2000 g / mol. , further preferably in the range from 1000 to 1800 g / mol.
[0034] In case the polyol (P1) is a polyetherpolyol, component (CA1) may also be a polyester or a polyether. Preferably, in case polyol (P1 ) is a polyetherpolyol, component (CA1) preferably also comprises ether groups. Component (CA1) may for example be a cyclic polyether, such as for example a crown ether. Suitable components are in principle known to the person skilled in the art and may for example be oligomers of ethylene oxide, 1 ,2-propylene oxide, 1 ,3-propylene oxide, or 1 ,4-butylene oxide.
[0035] According to a further embodiment, the present invention is also directed to the composition as disclosed above, wherein the component (CA1) is a polyether, preferably a cyclic polyether.
[0036] According to a further embodiment, the present invention is also directed to the composition as disclosed above, wherein the component (CA1) is a cyclic oligomer of ethylene oxide, 2-propyl- ene oxide, 1 ,3-propylene oxide, or 1 ,4-butylene oxide.
[0037] According to the present invention, it is also possible to use mixtures of two or more polyols for the preparation of the thermoplastic polyurethane. The polyols used or the polyol composition preferably have an average functionality in the range from 1.7 and 2.3, preferably in the range from 1.9 and 2.1 , especially 2.
[0038] Suitable polyols are described, for example, in "Kunststoffhandbuch [Plastics Handbook], volume 7, Polyurethane [Polyurethanes]”, Carl Hanser Verlag, 3rd edition 1993, chapter 3.1.
[0039] According to the invention, the polyol composition may also comprise a solvent. Suitable solvents are known per se to those skilled in the art.
[0040] According to the invention, a chain extender (C1) is used for the preparation of the thermoplastic polyurethane. Suitable chain extenders are known per se to those skilled in the art.
[0041] Chain extenders used are compounds having at least two groups reactive toward isocyanates. Groups reactive toward isocyanates may especially be NH, OH or else SH groups. Suitable examples are diamines or else diols or water. Preference is given to using at least one chain extender selected from the group consisting of compounds having at least two isocyanatereactive groups having a molecular weight of < 500 g / mol.
[0042] In a further embodiment, the present invention therefore also relates to a process for producing a polyurethane as described above, wherein the chain extender (C1) is selected from the group consisting of diols, diamines and / or water.
[0043] Chain extenders used may, for example, be commonly known aliphatic, araliphatic, aromatic and / or cycloaliphatic compounds having a molecular weight of 50 to 499 g / mol, preferably bifunctional compounds, for example alkanediols having 2 to 10 carbon atoms in the alkylene radical, for example diols selected from the group consisting of C2 to C6 diols, preferably butane-1 ,4-diol, hexane-1 ,6-diol and / or di-, tri-, tetra-, penta-, hexa-, hepta-, octa-, nona- and / or decaalkylene glycols having 3 to 8 carbon atoms, preferably unbranched alkanediols, especially propane-1 ,3-diol, butane-1 ,4-diol and hexane-1 ,6-diol. It is further preferably possible here to use aliphatic, araliphatic, aromatic and / or cycloaliphatic diols having a molecular weight of 50 g / mol to 220 g / mol. Preference is given to alkanediols having 2 to 12 carbon atoms in the alkylene radical, especially di-, tri-, tetra-, penta-, hexa-, hepta-, octa-, nona- and / or decaalkylene glycols. For the present invention, particular preference is given to ethanediol, propanediol, butanediol, pentanediol, hexanediol, or mixtures thereof.
[0044] It is also possible in accordance with the invention to use mixtures of two or more chain extenders.
[0045] Within the context of the present invention the employed amount of the chain extender and the polyol composition may be varied within broad ranges. For example, in the context of the present invention, the chain extender (C1) may be used in an amount in the range from 1 :40 to 10:1 , based on the polyol (P1) used.
[0046] According to a further embodiment, the present invention is also directed to the composition as disclosed above, wherein the chain extender (C1) is selected from the group consisting of ethanediol, propanediol, butanediol, pentanediol, hexanediol, or mixtures thereof.
[0047] According to the invention, a diisocyanate (11) is used for the preparation of the thermoplastic polyurethane. Preferred diisocyanates within the context of the present invention are aliphatic or aromatic diisocyanates, especially aromatic diisocyanates.
[0048] In addition, in the context of the present invention, prereacted products may be used as isocyanate components, in which a polyol is reacted with an isocyanate in a preceding reaction step. The products obtained have essentially isocyanate end groups and may be used in accordance with the invention.
[0049] Aliphatic diisocyanates used are customary aliphatic and / or cycloaliphatic diisocyanates, for example tri-, tetra-, penta-, hexa-, hepta- and / or octamethylene diisocyanate, 2- methylpentamethylene 1 ,5-diisocyanate, 2-ethyltetramethylene 1 ,4-diisocyanate, hexamethylene 1 ,6-diisocyanate (HDI), pentamethylene 1 ,5-diisocyanate, butylene 1 ,4- diisocyanate, trimethylhexamethylene 1 ,6-diisocyanate, 1 ,3-Bis(isocyanatemethyl) cyclohexan (H6XDI), 1 -isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane (isophorone diisocyanate, IPDI), 1 ,4- and / or 1 ,3-bis(isocyanatomethyl)cyclohexane (HXDI), cyclohexane 1 ,4- diisocyanate, 1 -methylcyclohexane 2,4- and / or 2, 6-diisocyanate, methylene dicyclohexyl 4,4'-, 2,4'- and / or 2, 2'-diisocyanate (H12MDI).
[0050] Preferred aliphatic polyisocyanates are hexamethylene 1 ,6-diisocyanate (HDI), pentamethylene 1 ,5-diisocyanate, 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane and methylene dicyclohexyl 4,4'-, 2,4'- and / or 2, 2'-diisocyanate (H12MDI). Suitable aromatic diisocyanates are especially naphthylene 1 ,5-diisocyanate (NDI), tolylene 2,4- and / or 2,6-diisocyanate (TDI), diphenylmethane 2,2'-, 2,4'- and / or 4, 4'-diisocyanate (MDI), 3,3’- dimethyl-4,4’-diisocyanatodiphenyl (TODI), xylylene diisocyanates (XDI), p-phenylene diisocyanate (PDI), diphenylethane 4,4’-diisocyanate (EDI), diphenylmethane diisocyanate, 3,3’- dimethyldiphenyl diisocyanate, diphenylethane 1 ,2-diisocyanate and / or phenylene diisocyanate.
[0051] It is also possible in the context of the present invention to use higher-functionality isocyanates, by way of example triisocyanates, for example triphenylmethane 4,4’,4”-triisocyanate, and also the cyanurates of the aforementioned diisocyanates, and the oligomers obtainable by partial reaction of diisocyanates with water, for example the biurets of the aforementioned diisocyanates, and additionally oligomers obtainable by controlled reaction of semiblocked diisocyanates with polyols having an average of more than two and preferably three or more hydroxyl groups.
[0052] For example, the polyisocyanate (11 ) may be selected from the group consisting of diphenylmethane 2,2‘-, 2,4'- and 4, 4'-di isocyanate (MDI), tolylene 2,4- and 2,6-diisocyanate (TDI), hexamethylene diisocyanate (HDI), 1 -isocyanato-4-[(4- isocyanatocyclohexyl)methyl]cyclohexane (H12MDI) or naphthalene 1 ,5-diisocyanate (NDI).
[0053] In a further embodiment, the present invention therefore also relates to a process for producing a polyurethane as described above, wherein the polyisocyanate (11) is selected from the group consisting of diphenylmethane 2,2‘-, 2,4'- and 4,4'-diisocyanate (MDI), tolylene 2,4- and 2,6- diisocyanate (TDI), hexamethylene diisocyanate (HDI), 1 -isocyanato-4-[(4- isocyanatocyclohexyl)methyl]cyclohexane (H12MDI) or naphthalene 1 ,5-diisocyanate (NDI).
[0054] The polyisocyanate (I2) is preferably selected from the group consisting of diphenylmethane 2,2 ‘-, 2,4'- and 4, 4'-di isocyanate (MDI), tolylene 2,4- and 2,6-diisocyanate (TDI), hexamethylene diisocyanate (HDI), 1-isocyanato-4-[(4-isocyanatocyclohexyl)methyl]cyclohexane (H12MDI) and naphthalene 1 ,5-diisocyanate (NDI).
[0055] According to a further embodiment, the present invention is also directed to the composition as disclosed above, wherein isocyanate is selected from the group consisting of diphenylmethane 2,2‘-, 2,4'- and 4,4'-diisocyanate (MDI), hexamethylene diisocyanate (HDI), p-phenylene diisocyanate (PDI), 1-isocyanato-4-[(4-isocyanatocyclohexyl)methyl]cyclohexane (H12MDI), naphthalene 1 ,5-diisocyanate (NDI), 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane (isophorone diisocyanate, I PDI) and mixtures thereof.
[0056] In case mixtures of two isocyantes are used, the isocyanates are typically used in a ratio of 1 :20 to 1 :3.
[0057] It has been found that the presence of component (CA1 ) in admixture with the thermoplastic polyurethane according to the present invention results in improved properties of the composition. The amount of the component (CA1) in the composition may vary depending on the thermoplastic polyurethane and the component (CA1) used. Typically the amount of migrateable parts is in the composition is in the range of from 70 to 300 ppm, in particular in the range of from 50 to 500 ppm by weight based on the total composition.
[0058] The amount of migratable parts is determined by GPC according to DIN 55672-1 (2016-03-01), using DMF as the flow agent and PM MA as the standard for the detection of oligomers < 500 g / mol. The differentiation from additives is achieved by using a UV detector at a wavelength of 254 nm and detection of the oligomers by using a refractive index (Rl) detector.
[0059] According to a further embodiment, the present invention is also directed to the composition as disclosed above, wherein the proportion of the component (CA1) in the composition based on the migrateable parts is in the range from 50 to 500 ppm by weight based on the total composition.
[0060] The amount of components (CA1) which is determined using GPC might be higher, for example up to 4% based on the total composition.
[0061] The proportion of the thermoplastic polyurethane in the composition may also vary and typically is in the range from 75% to 99.9% by weight based on the total composition, preferably in the range from 80% to 99.9% by weight based on the total composition.
[0062] According to a further embodiment, the present invention is also directed to the composition as disclosed above, wherein the proportion of the thermoplastic polyurethane in the composition is in the range from 75% to 99.9% by weight based on the total composition.
[0063] The molecular weight of the thermoplastic polyurethane may vary within wide ranges. It is particularly advantageous for the thermoplastic polyurethane to have a molecular weight in the range from 20 000 to 500 000 g / mol, determined by means of GPC, more preferably in the range from 50 000 to 300 000 g / mol. , in particular in the range of from 80 000 to 250 000 g / mol, preferably in the range of from 90 000 to 200 000 g / mol.
[0064] According to the invention, further additives may be added to the composition. Additives and auxiliaries are known per se to those skilled in the art. It is also possible in accordance with the invention to use combinations of two or more additives.
[0065] In the context of the present invention the term “additive” is more particularly understood to mean catalysts, auxiliaries and additives, especially stabilizers, nucleating agents, release agents, demolding aids, fillers, flame retardants or crosslinkers.
[0066] Suitable additives are for example stabilizers, nucleating agents, fillers, for example silicates.
[0067] Examples of auxiliaries and additives include surface-active substances, flame retardants, nucleating agents, oxidation stabilizers, antioxidants, lubricants and demolding aids, dyes and pigments, stabilizers, for example against hydrolysis, light, heat or discoloration, inorganic and / or organic fillers, reinforcers and plasticizers. Suitable auxiliaries and additives can be found, for example, in Kunststoffhandbuch, volume VII, edited by Vieweg and Hochtlen, Carl Hanser Verlag, Munich 1966 (p. 103-113).
[0068] According to a further aspect, the present invention is also directed to a process for preparing a composition comprising a thermoplastic polyurethane and at least one component (CA1) with a molecular weight Mn in the range of from 50 to 500 g / mol, determined according to.... In the context of the present invention, it is for example possible to mix the component (CA1) and the thermoplastic polyurethane in a suitable device. It is also possible to add component (CA1) to one or more of the components used for the preparation of the thermoplastic polyurethane. It is for example possible to add component (CA1) in a suitable amount to the polyol (P1) or to the chain extender used.
[0069] In case component (CA1 ) is added to the polyol or the chain extender, the amount of component (CA1) is adjusted to obtain a suitable amount of component (CA1) in the resulting thermoplastic polyurethane. Suitable amounts may for example be in the range of from 10 to 2000 ppm based on the weight of the polyol component.
[0070] According to the present invention it is also possible to use suitable polyols which may comprise component (CA1) due to their preparation process. In case the polyol comprises component (CA1) due to its preparation process, the amount of component (CA1) may be adjusted, for example by using suitable purification steps. According to the present invention, it is also possible to adjust the amount of component (CA1 ) in the polyol by adjusting the conditions of the preparation process of the polyol, for example the temperature, pressure or the catalyst and the reaction time used, to obtain a polyol containing a suitable amount of component (CA1). The polyol may comprise further components with a molecular weight of less than 500 g / mol, for example reactive oligomers which can react with isocyanate groups. Preferably, the amount of components with a molecular weight of less than 500 g / mol with no functional groups which can react with the isocyanate groups is adjusted in the range of from 30 to 2000 ppm based on the weight of the polyol component or 50 to 1000 ppm. The amount may also be adjusted depending on the polyol and isocyanate used.
[0071] The determination of the amount of low molecular weight by-products in the polyol preferably is carried out by GPC according to DIN 55672-1 (2016-03-01), however, with THF as flow agent and PEG as standard for the detection of oligomers < 500 g / mol. Differentiation from additives typically is made by UV detector at a wavelength of 254 nm and detection of the oligomers typically is made by refractive index (Rl) detector. In addition, the proportion of oligomers < 500 g / mol can be determined by thermal desorption GC-MS according to VDA 278 (FOG run only). For determining the amount of migrateable parts, the proportion of oligomers < 500 g / mol was determined by thermal desorption GC-MS according to VDA 278 (FOG run only) by weighing 2- 4 mg at 120 °C for 10 minutes. The evaluation was carried out using the total ion chromatogram (TIC). The values given are calculated as hexadecane equivalents (ppmHdE). For the determination of the low molecular weight fraction in the thermoplastic polyurethane typically GPC is used. According to the present invention, the proportion of low molecular weight compounds can be quantitatively analyzed by GPC using dimethylformamide (DMF) as the eluent at a flow rate of 1 .50 mL / min. A PSS SDV linear XL 5 pm column is used and the solution is calibrated against the homologues of polymethyl methacrylate with toluene as the standard. The content determined according to this method (total low molecular weight content) is typically up to 3.5% based on the total composition.
[0072] Additionally, the content of migrateable parts can be determined. For determining the content of migrateable parts, the injection molded plates typically are first stored at 100 °C for 20 h and then the oligomer content with a molecular weight 500 g / mol is determined via thermal desorption GC-MS analogous to VDA 278 (FOG run only) with a desorption time of 60 minutes. Evaluation was carried out using the total ion chromatogram (TIC). The values given are calculated as hexadecane equivalents (ppmHdE) (method 2). The respective content is given as the total content of migrateable parts in the context of the present invention. The proportion of the mono cycle (for example consisting of ADS and 1 ,4-butanediol) or, in the case of the ether, the crown ether, in particular the crown ether consisting of three THF molecules was determined by the peak size (method 3). The respective content is given in the context of the present invention as the content of cyclic migrateable parts.
[0073] Preferably, the total content of migrateable parts of compounds with a molecular weight Mn in the range of from 50 to 500 g / mol in the thermoplastic polyurethane is greater than 130 ppmHde, in particular in the range of from 130 to 400 ppmHde. The content of cyclic migrateable parts typically is in the range of from 55 to 280 ppmHde, in particular in the range of from 60 to 270 ppmHdE based on the total composition.
[0074] Thus, according to a further embodiment, the present invention is also directed to a composition as disclosed above, wherein the proportion of component (CA1) given as the content of cyclic migrateable parts in the composition is in the range from 55 to 280 ppmHde by weight based on the total composition.
[0075] According to a further aspect, the present invention is also directed to a process for preparing a composition comprising a thermoplastic polyurethane and at least one component (CA1) with a molecular weight Mn in the range of from 50 to 500 g / mol, determined by GPC according to DIN 55672-1 (2016-03-01), using DMF as the flow agent and PM MA as the standard for the detection of oligomers < 500 g / mol, using a UV detector at a wavelength of 254 nm for differentiation from additives and detection of the oligomers by using a refractive index (Rl) detector wherein the thermoplastic polyurethane is prepared by reacting at least components (a), (b) and (c):
[0076] (a) at least one diisocyanate (11)
[0077] (b) at least one polyol composition (PC1 ) and
[0078] (c) at least one chain extender (C1 ), wherein the polyol composition comprises at least one polyol (P1) and at least one component (CA1 ), and wherein the polyol (P1) comprises functional groups (F1 ) selected from ether groups and ester groups in the polymer backbone and the component (CA1) comprises functional groups (F2) selected from ether groups and ester groups.
[0079] Further additives any auxiliaries or catalysts may be used as component (d) for the preparation of the thermoplastic polyurethane.
[0080] According to the invention, the polyol composition (PC1 ) comprising a polyol (P1) is reacted with the diisocyanate (11). The polyol composition (PC1 ) comprises at least one polyol (P1 ) and may comprise further polyols or further components, for example solvents. According to the invention, the diisocyanate (11 ) may comprise further components, for example solvents.
[0081] The reaction can be conducted in apparatuses that are known per se to the person skilled in the art, for example heatable / coolable stirred tanks or reaction extruders. The reaction typically is conducted at temperatures known per se to the person skilled in the art, for example at a temperature in the range from 20 to 250°C, preferably in the range from 40 to 130°C, further preferably at a temperature in the range from 70 to 90°C.
[0082] According to the invention, it is also possible for the process to comprise further steps, for example a pretreatment of the components or an aftertreatment of the thermoplastic polyurethane obtained, for example a heat treatment. Accordingly, in a further embodiment, the present invention also relates to a process for producing a thermoplastic polyurethane as described above, wherein the thermoplastic polyurethane obtained is heat-treated after the reaction.
[0083] The present invention therefore also relates to a polyurethane obtainable or obtained by the process of the invention.
[0084] With regard to the preferred embodiments, reference is made to the above statements relating to the process of the invention. In a further embodiment, the present invention therefore also relates to a polyurethane as described above, wherein the polyurethane is thermoplastic.
[0085] The polyurethane of the invention and the polyurethane obtained or obtainable by a process of the invention can be processed further by processes known to the person skilled in the art to give the desired films, moldings, rolls, fibers, automobile trim, hoses, cable connectors, bellows, trailing cables, cable sheaths, gaskets, belts or damping elements, for example injection molding, calendering or extrusion. The polyurethane produced in accordance with the invention may advantageously be used especially in all applications specific to thermoplastic polyurethanes. The present invention therefore also relates to the use of a thermoplastic polyurethane obtainable or obtained by a process as described above or of a polyurethane as described above for production of shaped bodies, adhesives, coatings, hoses, films, nonwoven articles or fibers.
[0086] According to a further aspect, the present invention is also directed to the use of a composition as disclosed above or a composition prepared according to the process as disclosed above for the production of shaped bodies, coatings, tubes, rolls, belts, damping elements, cable sheaths, hoses, films, nonwoven articles or fibers, foamed parts, particle foams, added manufacturing filaments, 3D printing, extrusion parts, injection molding parts, agriculture, construction applications.
[0087] Expanded thermoplastic polyurethane beads according to the present invention belong to the group of particle foams, which are also referred to as foamed pellets (or bead foams, particle foam, expanded thermoplastic elastomer particles or expanded thermoplastic polyurethane beads). Particle foams and moldings (also referred to as molded article) made therefrom, based on thermoplastic polyurethanes or other thermoplastic elastomers, are in principle known (for example WO 94 / 20568A1 , WO 2007 / 082838 A1 , WO2017 / 030835 A1 , WO 2013 / 153190 A1 , WO 2010 / 010010 A1 ) and can be used in many ways.
[0088] A foamed pellet or also a particle foam or bead foam in the sense of the present invention refers to a foam in the form of a particle, the average length of the particles preferably being in the range of 1 to 10 mm. In the case of non-spherical, e.g., oval particles average length means the longest dimension by length, (determined by 3D evaluation of the granules, for example by means of dynamic image analysis with an optical measuring device named “PartAn 3D”, Microtrac).
[0089] The single foam granules according to the present invention preferably have an average mass in the range of 0.1 to 50 mg, preferable in the range between 0.5 and 45 mg. The average mass means in this context the arithmetic mean based on a sample size of 10 different particles wherein each particle is weighted three times.
[0090] The foamed pellets according to the invention usually have a bulk density of 30 g / l to 250 g / l, preferably 50 g / l to 200 g / l, more preferably 70 g / l to 180 g / l. The bulk density is measured analogously to DIN ISO 60:1999, wherein the determination of the above values in contrast to the standard, a vessel with 10 I volume is used instead of a vessel with 0.1 I volume, since especially for the foam particles with low density and large mass a measurement with only 0.1 I volume is too inaccurate.
[0091] Processes for producing foamed pellets and molded bodies comprising the foamed pellets are in principle known to the person skilled in the art and are for example disclosed in WO 2013 / 153190 A1. The shape of the pellets used according to the present invention may vary. It is possible to use rounded, non-spherical, e.g. elongated or cylindrical particles as well as pellets with e.g. flatted surface spots.
[0092] The shape and dimensions of the foamed pellets in the molded body may differ from the shape and dimensions of the foamed pellets used in the process due to the process conditions. It is for example possible that rounded foamed pellets are used in the process and the foamed pellets in the molded body have a rounded, non-spherical shape, e.g. elongated or cylindrical pellets as well as pellets with e.g. flatted surface spots. The average length of the foamed pellets in the molded body may for example be in the range of from 1 to 15 mm, preferably 1 to 8 mm. In the case of non-spherical, e.g. elongated or cylindrical particles mean the longest dimension by length.
[0093] Fusing the foamed pellets is preferably carried out in a mold to shape the molded body obtained. In principle, all suitable methods for fusing foamed pellets can be used according to the present invention, for example fusing at elevated temperatures, such as for example steam chest molding, molding at high frequencies, for example using electromagnetic radiation, processes using a double belt press, or variotherm processes.
[0094] Further embodiments of the present invention are apparent from the claims and the examples. It will be appreciated that the features of the object / processes / uses according to the invention that are mentioned above and elucidated below are usable not only in the combination specified in each case but also in other combinations without departing from the scope of the invention. Thus, for example, the combination of a preferred feature with a particularly preferred feature or of a feature not characterized further with a particularly preferred feature etc. is also encompassed implicitly even if this combination is not mentioned explicitly.
[0095] The present invention is illustrated in more detail by the following embodiments and combinations of embodiments which are apparent from the corresponding dependency references and other references. In particular, it should be noted that in every case where a range of embodiments is mentioned, for example in the context of an expression such as “the process according to any of embodiments 1 to 4”, each embodiment in this range is deemed to be explicitly disclosed to those skilled in the art, i.e. the wording of this expression is to be understood by those skilled in the art as synonymous with “the process according to any of embodiments 1 , 2, 3 and 4”.
[0096] 1 . A composition comprising at least the components (i) and (ii):
[0097] (i) a thermoplastic polyurethane being the reaction product of at least one diisocyanate (11), at least one polyol (P1), and at least one chain extender (C1), and
[0098] (ii) at least one component (CA1) with a molecular weight Mn in the range of from 50 to 500 g / mol, determined by GPC according to DIN 55672-1 (2016-03-01), using DMF as the flow agent and PM MA as the standard, wherein the polyol (P1) comprises functional groups (F1) selected from ether groups and ester groups in the polymer backbone and the component (CA1) comprises functional groups (F2) selected from ether groups and ester groups.
[0099] 2. The composition according to embodiment 1 , wherein the functional groups (F1) and (F2) are the same.
[0100] 3. The composition according to embodiment 1 or 2, wherein the polyol (P1) is a polyesterpolyol.
[0101] 4. The composition according to any of embodiments 1 to 3, wherein the component (CA1 ) is a polyester, preferably a cyclic polyester.
[0102] 5. The composition according to any of embodiments 1 to 4, wherein the component (CA1) is a polyester being the reaction product of a dicarboxylic acid (a1) and a diol (d1), the dicarboxylic acid (a1) being selected from the group consisting of adipic acid, succinic acid, or a mixture thereof, and the diol (d1) is selected from the group consisting of ethanediol, propanediol, butanediol, pentanediol, and hexanediol or a mixture thereof.
[0103] 6. The composition according to embodiment 5, wherein a mixture of two diols selected from the group consisting of ethanediol, propanediol, butanediol, pentanediol, and hexanediol is used as diol (d1).
[0104] 7. The composition according to any of embodiments 1 to 6, wherein the polyol is a polyesterpolyol being the reaction product of a dicarboxylic acid (a2) and a diol (d2), the dicarboxylic acid (a2) being selected from the group consisting of adipic acid, succinic acid, or a mixture thereof, and the diol (d2) is selected from the group consisting of ethanediol, propanediol, butanediol, pentanediol, and hexanediol or a mixture thereof.
[0105] 8. The composition according to embodiment 1 or 2, wherein the polyol (P1) is a polyeth- erpolyol.
[0106] 9. The composition according to any of embodiments 1 to 8, wherein the component (CA1 ) is a polyether, preferably a cyclic polyether.
[0107] 10. The composition according to any of embodiments 1 to 9, wherein the component (CA1 ) is a cyclic oligomer of ethylene oxide, 1 ,2-propylene oxide, 1 ,3-propylene oxide, 1 ,4-butyl- ene oxide
[0108] 11 . The composition according to any of embodiments 1 to 10, wherein the polyol (P1 ) is a polyetherpolyol selected from the group consisting of polyethtyleneglycol, polypropyleneglycol, polytrimethyleneglycol and polytetramethyleneglycol. 12. The composition according to any of embodiments 1 to 11 , wherein the chain extender (C1 ) is selected from the group consisting of ethanediol, propanediol, butanediol, pentanediol, hexanediol, or mixtures thereof.
[0109] 13. The composition according to any one of embodiments 1 to 12, wherein isocyanate is selected from the group consisting of methylenediphenyl diisocyanate (MDI), hexamethylene 1 ,6-diisocyanate (HDI), p-phenylene diisocyanate (PDI), 2,2'-diisocyanate (H12MDI), naphthylene 1 ,5-diisocyanate (NDI), isophorone diisocyanate (IPDI) and mixtures thereof.
[0110] 14. The composition according to any of embodiments 1 to 13, wherein the proportion of component (CA1 ) given as the content of cyclic migrateable parts in the composition is in the range from 55 to 280 ppmHde by weight based on the total composition .
[0111] 15. The composition according to any of embodiments 1 to 13, wherein the proportion of component (CA1 ) given as the content of cyclic migrateable parts in the composition is in the range from 55 to 280 ppmHde by weight based on the total composition, wherein the content of migrateable parts is determined using the injection molded plates which are first stored at 100 °C for 20 h and then the oligomer content with a molecular weight 500 g / mol is determined via thermal desorption GC-MS analogous to VDA 278 (FOG run only) with a desorption time of 60 minutes, the evaluation is carried out using the total ion chromatogram (TIC) and the content is calculated as hexadecane equivalents (ppmHdE) and the proportion of the oligomers is determined by the peak size.
[0112] 16. The composition according to any of embodiments 1 to 15, wherein the proportion of the thermoplastic polyurethane in the composition is in the range from 75% to 99.9% by weight based on the total composition.
[0113] 17. Process for preparing a composition comprising a thermoplastic polyurethane and at least one component (CA1) with a molecular weight Mn in the range of from 50 to 500 g / mol, determined by GPC according to DIN 55672-1 (2016-03-01), using DMF as the flow agent and PM MA as the standard, wherein the thermoplastic polyurethane is prepared by reacting at least components (a), (b) and (c):
[0114] (a) at least one diisocyanate (11 )
[0115] (b) at least one polyol composition (PC1 ) and
[0116] (c) at least one chain extender (C1 ), wherein the polyol composition comprises at least one polyol (P1) and at least one component (CA1), and wherein the polyol (P1) comprises functional groups (F1) selected from ether groups and ester groups in the polymer backbone and the component (CA1) comprises functional groups (F2) selected from ether groups and ester groups.
[0117] 18. The process according to embodiment 17, wherein the functional groups (F1) and (F2) are the same.
[0118] 19. The process according to embodiment 17 or 18, wherein the polyol (P1) is a polyesterpolyol.
[0119] 20. The process according to any of embodiments 17 to 19, wherein the component (CA1 ) is a polyester, preferably a cyclic polyester.
[0120] 21 . The process according to any of embodiments 17 to 20, wherein the component (CA1 ) is a polyester being the reaction product of a dicarboxylic acid (a1) and a diol (d1), the dicarboxylic acid (a1) being selected from the group consisting of adipic acid, succinic acid, or a mixture thereof, and the diol (d1) is selected from the group consisting of ethanediol, propanediol, butanediol, pentanediol, and hexanediol or a mixture thereof.
[0121] 22. The process according to embodiment 21 , wherein a mixture of two diols selected from the group consisting of ethanediol, propanediol, butanediol, pentanediol, and hexanediol is used as diol (d1).
[0122] 23. The process according to any of embodiments 17 to 22, wherein the polyol is a polyesterpolyol being the reaction product of a dicarboxylic acid (a2) and a diol (d2), the dicarboxylic acid (a2) being selected from the group consisting of adipic acid, succinic acid, or a mixture thereof, and the diol (d2) is selected from the group consisting of ethanediol, propanediol, butanediol, pentanediol, and hexanediol or a mixture thereof.
[0123] 24. The process according to embodiment 17 or 18, wherein the polyol (P1) is a polyetherpolyol .
[0124] 25. The process according to any of embodiments 17 to 24, wherein the component (CA1 ) is a polyether, preferably a cyclic polyether.
[0125] 26. The process according to any of embodiments 17 to 25, wherein the component (CA1 ) is a cyclic oligomer of ethylene oxide, 1 ,2-propylene oxide, 1 ,3-propylene oxide, 1 ,4-butyl- ene oxide
[0126] 27. The process according to any of embodiments 17 to 26, wherein the polyol (P1 ) is a polyetherpolyol selected from the group consisting of polyethtyleneglycol, polypropyleneglycol, polytrimethyleneglycol and polytetramethyleneglycol. 28. The process according to any of embodiments 17 to 27, wherein the chain extender (C1 ) is selected from the group consisting of ethanediol, propanediol, butanediol, pentanediol, hexanediol, or mixtures thereof.
[0127] 29. The process according to any one of embodiments 17 to 28, wherein isocyanate is selected from the group consisting of methylenediphenyl diisocyanate (MDI), hexamethylene 1 ,6-diisocyanate (HDI), p-phenylene diisocyanate (PDI), 2,2'-diisocyanate (H12MDI), naphthylene 1 ,5-diisocyanate (N DI), isophorone diisocyanate (I PDI) and mixtures thereof.
[0128] 30. The process according to any of embodiments 17 to 29, wherein the proportion of component (CA1 ) given as the content of cyclic migrateable parts in the composition is in the range from 55 to 280 ppmHde by weight based on the total composition .
[0129] 31 . The process according to any of embodiments 17 to 29, wherein the proportion of component (CA1 ) given as the content of cyclic migrateable parts in the composition is in the range from 55 to 280 ppmHde by weight based on the total composition, wherein the content of migrateable parts is determined using the injection molded plates which are first stored at 100 °C for 20 h and then the oligomer content with a molecular weight 500 g / mol is determined via thermal desorption GC-MS analogous to VDA 278 (FOG run only) with a desorption time of 60 minutes, the evaluation is carried out using the total ion chromatogram (TIC) and the content is calculated as hexadecane equivalents (ppmHdE) and the proportion of the oligomers is determined by the peak size.
[0130] 32. The process according to any of embodiments 17 to 31 , wherein the proportion of the thermoplastic polyurethane in the composition is in the range from 75% to 99.9% by weight based on the total composition.
[0131] 33. The use of a composition according to any of embodiments 1 to 16 or a composition prepared according to the process according to any of embodiments 17 to 32 for the production of shaped bodies, coatings, tubes, rolls, belts, damping elements, cable sheaths, hoses, films, nonwoven articles or fibers, foamed parts, particle foams, added manufacturing filaments, 3D printing, extrusion parts, injection molding parts for the use in industrial applications, consumer goods including sports, automotive, agriculture, construction applications.
[0132] 34. A composition comprising at least the components (i) and (ii):
[0133] (i) a thermoplastic polyurethane being the reaction product of at least one diisocyanate (11), at least one polyol (P1 ), and at least one chain extender (C1), and
[0134] (ii) at least one component (CA1) with a molecular weight Mn in the range of from 50 to 500 g / mol, determined by GPC according to DIN 55672-1 (2016-03-01 ), using DMF as the flow agent and PM MA as the standard, wherein the polyol (P1 ) comprises functional groups (F1 ) selected from ether groups and ester groups in the polymer backbone and the component (CA1) comprises functional groups (F2) selected from ether groups and ester groups, wherein the polyol (P1 ) is a polyesterpolyol and the component (CA1) is a polyester, preferably a cyclic polyester. The composition according to embodiment 34, wherein the functional groups (F1) and (F2) are the same. The composition according to any of embodiments 34 or 35, wherein the component (CA1 ) is a polyester being the reaction product of a dicarboxylic acid (a1 ) and a diol (d1), the dicarboxylic acid (a1 ) being selected from the group consisting of adipic acid, succinic acid, or a mixture thereof, and the diol (d1 ) is selected from the group consisting of ethanediol, propanediol, butanediol, pentanediol, and hexanediol or a mixture thereof. The composition according to embodiment 36, wherein a mixture of two diols selected from the group consisting of ethanediol, propanediol, butanediol, pentanediol, and hexanediol is used as diol (d1 ). The composition according to any of embodiments 34 to 37, wherein the polyol is a polyesterpolyol being the reaction product of a dicarboxylic acid (a2) and a diol (d2), the dicarboxylic acid (a2) being selected from the group consisting of adipic acid, succinic acid, or a mixture thereof, and the diol (d2) is selected from the group consisting of ethanediol, propanediol, butanediol, pentanediol, and hexanediol or a mixture thereof. The composition according to any of embodiments 34 to 38, wherein the chain extender (C1 ) is selected from the group consisting of ethanediol, propanediol, butanediol, pentanediol, hexanediol, or mixtures thereof. The composition according to any one of embodiments 34 to 39, wherein isocyanate is selected from the group consisting of methylenediphenyl diisocyanate (MDI), hexamethylene 1 ,6-diisocyanate (H DI), p-phenylene diisocyanate (PDI), 2,2'-diisocyanate (H12MDI), naphthylene 1 ,5-diisocyanate (NDI), isophorone diisocyanate (I PDI) and mixtures thereof. The composition according to any of embodiments 34 to 40, wherein the proportion of component (CA1 ) given as the content of cyclic migrateable parts in the composition is in the range from 55 to 280 ppmHde by weight based on the total composition . The composition according to any of embodiments 34 to 40, wherein the proportion of component (CA1) given as the content of cyclic migrateable parts in the composition is in the range from 55 to 280 ppmHde by weight based on the total composition, wherein the content of migrateable parts is determined using the injection molded plates which are first stored at 100 °C for 20 h and then the oligomer content with a molecular weight 500 g / mol is determined via thermal desorption GC-MS analogous to VDA 278 (FOG run only) with a desorption time of 60 minutes, the evaluation is carried out using the total ion chromatogram (TIC) and the content is calculated as hexadecane equivalents (ppmHdE) and the proportion of the oligomers is determined by the peak size. The composition according to any of embodiments 34 to 42, wherein the proportion of the thermoplastic polyurethane in the composition is in the range from 75% to 99.9% by weight based on the total composition. Process for preparing a composition comprising a thermoplastic polyurethane and at least one component (CA1) with a molecular weight Mn in the range of from 50 to 500 g / mol, determined by GPC according to DIN 55672-1 (2016-03-01), using DMF as the flow agent and PM MA as the standard, wherein the thermoplastic polyurethane is prepared by reacting at least components (a), (b) and (c):
[0135] (a) at least one diisocyanate (11 )
[0136] (b) at least one polyol composition (PC1 ) and
[0137] (c) at least one chain extender (C1 ), wherein the polyol composition comprises at least one polyol (P1 ) and at least one component (CA1), and wherein the polyol (P1 ) comprises functional groups (F1) selected from ether groups and ester groups in the polymer backbone and the component (CA1) comprises functional groups (F2) selected from ether groups and ester groups, wherein the polyol (P1 ) is a polyesterpolyol and the component (CA1) is a polyester, preferably a cyclic polyester. The use of a composition according to any of embodiments 34 to 43 or a composition prepared according to the process according to embodiment 44 for the production of shaped bodies, coatings, tubes, rolls, belts, damping elements, cable sheaths, hoses, films, nonwoven articles or fibers, foamed parts, particle foams, added manufacturing filaments, 3D printing, extrusion parts, injection molding parts for the use in industrial applications, consumer goods including sports, automotive, agriculture, construction applications. A composition comprising at least the components (i) and (ii):
[0138] (i) a thermoplastic polyurethane being the reaction product of at least one diisocyanate (11), at least one polyol (P1 ), and at least one chain extender (C1), and (ii) at least one component (CA1 ) with a molecular weight Mn in the range of from 50 to 500 g / mol, determined by GPC according to DIN 55672-1 (2016-03-01 ), using DMF as the flow agent and PM MA as the standard, wherein the polyol (P1 ) comprises functional groups (F1) selected from ether groups and ester groups in the polymer backbone and the component (CA1) comprises functional groups (F2) selected from ether groups and ester groups. wherein the polyol (P1 ) is a polyetherpolyol and the component (CA1 ) is a polyether, preferably a cyclic polyether.
[0139] 47. The composition according to embodiment 46, wherein the functional groups (F 1 ) and (F2) are the same.
[0140] 48. The composition according to any of embodiments 46 to 47, wherein the component (CA1 ) is a cyclic oligomer of ethylene oxide, 1 ,2-propylene oxide, 1 ,3-propylene oxide, 1 ,4-butylene oxide
[0141] 49. The composition according to any of embodiments 46 to 48, wherein the polyol (P1 ) is a polyetherpolyol selected from the group consisting of polyethtyleneglycol, polypropyleneglycol, polytrimethyleneglycol and polytetramethyleneglycol.
[0142] 50. The composition according to any of embodiments 46 to 49, wherein the chain extender (C1 ) is selected from the group consisting of ethanediol, propanediol, butanediol, pentanediol, hexanediol, or mixtures thereof.
[0143] 51 . The composition according to any one of embodiments 46 to 50, wherein isocyanate is selected from the group consisting of methylenediphenyl diisocyanate (MDI), hexamethylene 1 ,6-diisocyanate (HDI), p-phenylene diisocyanate (PDI), 2,2'-diisocyanate (H12MDI), naphthylene 1 ,5-diisocyanate (NDI), isophorone diisocyanate (IPDI) and mixtures thereof.
[0144] 52. The composition according to any of embodiments 46 to 51 , wherein the proportion of component (CA1 ) given as the content of cyclic migrateable parts in the composition is in the range from 55 to 280 ppmHde by weight based on the total composition .
[0145] 53. The composition according to any of embodiments 46 to 51 , wherein the proportion of component (CA1 ) given as the content of cyclic migrateable parts in the composition is in the range from 55 to 280 ppmHde by weight based on the total composition, wherein the content of migrateable parts is determined using the injection molded plates which are first stored at 100 °C for 20 h and then the oligomer content with a molecular weight 500 g / mol is determined via thermal desorption GC-MS analogous to VDA 278 (FOG run only) with a desorption time of 60 minutes, the evaluation is carried out using the total ion chromatogram (TIC) and the content is calculated as hexadecane equivalents (ppmHdE) and the proportion of the oligomers is determined by the peak size.
[0146] 54. The composition according to any of embodiments 46 to 53, wherein the proportion of the thermoplastic polyurethane in the composition is in the range from 75% to 99.9% by weight based on the total composition.
[0147] 55. Process for preparing a composition comprising a thermoplastic polyurethane and at least one component (CA1) with a molecular weight Mn in the range of from 50 to 500 g / mol, determined by GPC according to DIN 55672-1 (2016-03-01 ), using DMF as the flow agent and PM MA as the standard, wherein the thermoplastic polyurethane is prepared by reacting at least components (a), (b) and (c):
[0148] (a) at least one diisocyanate (11 )
[0149] (b) at least one polyol composition (PC1 ) and
[0150] (c) at least one chain extender (C1 ), wherein the polyol composition comprises at least one polyol (P1) and at least one component (CA1), and wherein the polyol (P1 ) comprises functional groups (F1) selected from ether groups and ester groups in the polymer backbone and the component (CA1) comprises functional groups (F2) selected from ether groups and ester groups, wherein the polyol (P1 ) is a polyetherpolyol and the component (CA1 ) is a polyether, preferably a cyclic polyether.
[0151] 56. The use of a composition according to any of embodiments 46 to 54 or a composition prepared according to the process according to embodiment 55 for the production of shaped bodies, coatings, tubes, rolls, belts, damping elements, cable sheaths, hoses, films, nonwoven articles or fibers, foamed parts, particle foams, added manufacturing filaments, 3D printing, extrusion parts, injection molding parts for the use in industrial applications, consumer goods including sports, automotive, agriculture, construction applications.
[0152] 57. A composition comprising at least the components (i) and (ii):
[0153] (i) a thermoplastic polyurethane being the reaction product of at least one diisocyanate (11), at least one polyol (P1 ), and at least one chain extender (C1), and
[0154] (ii) at least one component (CA1) with a molecular weight Mn in the range of from 50 to 500 g / mol, determined by GPC according to DIN 55672-1 (2016-03-01 ), using DMF as the flow agent and PM MA as the standard, wherein the polyol (P1) comprises functional groups (F1) selected from ether groups and ester groups in the polymer backbone and the component (CA1) comprises functional groups (F2) selected from ether groups and ester groups, wherein the proportion of component (CA1) given as the content of cyclic migrateable parts in the composition is in the range from 55 to 280 ppmHde by weight based on the total composition.
[0155] 58. A composition comprising at least the components (i) and (ii):
[0156] (i) a thermoplastic polyurethane being the reaction product of at least one diisocyanate (11), at least one polyol (P1), and at least one chain extender (C1), and
[0157] (ii) at least one component (CA1 ) with a molecular weight Mn in the range of from 50 to 500 g / mol, determined by GPC according to DIN 55672-1 (2016-03-01), using DMF as the flow agent and PM MA as the standard, wherein the polyol (P1) comprises functional groups (F1) selected from ether groups and ester groups in the polymer backbone and the component (CA1) comprises functional groups (F2) selected from ether groups and ester groups, wherein the proportion of component (CA1) given as the content of cyclic migrateable parts in the composition is in the range from 55 to 280 ppmHde by weight based on the total composition, and wherein the content of migrateable parts is determined using the injection molded plates which are first stored at 100 °C for 20 h and then the oligomer content with a molecular weight 500 g / mol is determined via thermal desorption GC-MS analogous to VDA 278 (FOG run only) with a desorption time of 60 minutes, the evaluation is carried out using the total ion chromatogram (TIC) and the content is calculated as hexadecane equivalents (ppmHdE) and the proportion of the oligomers is determined by the peak size.
[0158] 59. The composition according to embodiment 57 or 58, wherein the functional groups (F1) and (F2) are the same.
[0159] 60. The composition according to any of embodiments 57 to 59, wherein the polyol (P1 ) is a polyesterpolyol.
[0160] 61 . The composition according to any of embodiments 57 to 60, wherein the component (CA1) is a polyester, preferably a cyclic polyester.
[0161] 62. The composition according to any of embodiments 57 to 61 , wherein the component (CA1) is a polyester being the reaction product of a dicarboxylic acid (a1) and a diol (d1), the dicarboxylic acid (a1) being selected from the group consisting of adipic acid, succinic acid, or a mixture thereof, and the diol (d1) is selected from the group consisting of ethanediol, propanediol, butanediol, pentanediol, and hexanediol or a mixture thereof. 63. The composition according to embodiment 62, wherein a mixture of two diols selected from the group consisting of ethanediol, propanediol, butanediol, pentanediol, and hexanediol is used as diol (d1 ).
[0162] 64. The composition according to any of embodiments 57 to 63, wherein the polyol is a polyesterpolyol being the reaction product of a dicarboxylic acid (a2) and a diol (d2), the dicarboxylic acid (a2) being selected from the group consisting of adipic acid, succinic acid, or a mixture thereof, and the diol (d2) is selected from the group consisting of ethanediol, propanediol, butanediol, pentanediol, and hexanediol or a mixture thereof.
[0163] 65. The composition according to any of embodiments 57 to 59, wherein the polyol (P1 ) is a polyetherpolyol.
[0164] 66. The composition according to any of embodiments 57 to 65, wherein the component (CA1 ) is a polyether, preferably a cyclic polyether.
[0165] 67. The composition according to any of embodiments 57 to 66, wherein the component (CA1 ) is a cyclic oligomer of ethylene oxide, 1 ,2-propylene oxide, 1 ,3-propylene oxide, 1 ,4-butylene oxide
[0166] 68. The composition according to any of embodiments 57 to 67, wherein the polyol (P1 ) is a polyetherpolyol selected from the group consisting of polyethtyleneglycol, polypropyleneglycol, polytrimethyleneglycol and polytetramethyleneglycol.
[0167] 69. The composition according to any of embodiments 57 to 68, wherein the chain extender (C1 ) is selected from the group consisting of ethanediol, propanediol, butanediol, pentanediol, hexanediol, or mixtures thereof.
[0168] 70. The composition according to any one of embodiments 57 to 69, wherein isocyanate is selected from the group consisting of methylenediphenyl diisocyanate (MDI), hexamethylene 1 ,6-diisocyanate (HDI), p-phenylene diisocyanate (PDI), 2,2'-diisocyanate (H12MDI), naphthylene 1 ,5-diisocyanate (NDI), isophorone diisocyanate (I PDI) and mixtures thereof.
[0169] 71 . The composition according to any of embodiments 57 to 70, wherein the proportion of component (CA1 ) given as the content of cyclic migrateable parts in the composition is in the range from 55 to 280 ppmHde by weight based on the total composition .
[0170] 72. The composition according to any of embodiments 57 to 71 , wherein the proportion of the thermoplastic polyurethane in the composition is in the range from 75% to 99.9% by weight based on the total composition. 73. Process for preparing a composition comprising a thermoplastic polyurethane and at least one component (CA1) with a molecular weight Mn in the range of from 50 to 500 g / mol, determined by GPC according to DIN 55672-1 (2016-03-01), using DMF as the flow agent and PM MA as the standard, wherein the thermoplastic polyurethane is prepared by reacting at least components (a), (b) and (c):
[0171] (a) at least one diisocyanate (11)
[0172] (b) at least one polyol composition (PC1) and
[0173] (c) at least one chain extender (C1 ), wherein the polyol composition comprises at least one polyol (P1) and at least one component (CA1), and wherein the polyol (P1) comprises functional groups (F1) selected from ether groups and ester groups in the polymer backbone and the component (CA1) comprises functional groups (F2) selected from ether groups and ester groups, wherein the proportion of component (CA1) given as the content of cyclic migrateable parts in the composition is in the range from 55 to 280 ppmHde by weight based on the total composition.
[0174] 74. The use of a composition according to any of embodiments 57 to 72 or a composition prepared according to the process according to embodiment 73 for the production of shaped bodies, coatings, tubes, rolls, belts, damping elements, cable sheaths, hoses, films, nonwoven articles or fibers, foamed parts, particle foams, added manufacturing filaments, 3D printing, extrusion parts, injection molding parts for the use in industrial applications, consumer goods including sports, automotive, agriculture, construction applications.
[0175] Examples
[0176] 1. Materials
[0177] The following materials were used:
[0178] Polyol A: Polyesterpolyol with an OH number of 35.9 and only primary OH- groups
[0179] (based on 1 ,2-ethanediol and 1 ,4-butanediol (ratio 1 :1) and adipic acid, functionality: 2), which was purified in a separate step
[0180] Polyol B: Polyesterpolyol with an OH number of 35.9 and only primary OH- groups
[0181] (based on 1 ,2-ethanediol and 1 ,4-butanediol (ratio 1 :1) and adipic acid, functionality: 2) Polyol C: Polyesterpolyol with an OH number of 56.1 and only primary OH- groups
[0182] (based on 1 ,2-ethanediol and 1 ,4-butanediol (ratio 1 :1 ) and adipic acid, functionality: 2), which was purified in a separate step
[0183] Polyol D: Polyesterpolyol with an OH number of 56.1 and only primary OH- groups
[0184] (based on 1 ,2-ethanediol and 1 ,4-butanediol (ratio 1 :1 ) and adipic acid, functionality: 2)
[0185] Polyol E: Polyesterpolyol with an OH number of 36.5 and and only primary OH- groups (based on 1 ,6-hexanediol and 1 ,4-butanediol (ratio 1 :1 ) and adipic acid, functionality: 2)
[0186] Polyol F: Polyetherpolyol with an OH number of 56.0 and only primary OH- groups
[0187] (based on tetramethyleneoxid, functionality: 2)
[0188] Polyol G: Polyetherpolyol with an OH number of 112.0 and only primary OH-groups
[0189] (based on tetramethyleneoxid, functionality: 2)
[0190] Diisocyanate 1 : aromatic isocyanat (4,4‘-Methylendiphenyldiisocyanat)
[0191] KV 1 : 1 ,4-butanediol stabilizer 1 : polymeric carbodiimid catalyst: Titanium(IV) butoxid (TTB), CAS: 5593-70-4 tin(ll) 2-ethylhexanoate (SDO), CAS: 301-10-0 Preparation of ester polyols Polyol A
[0192] 611.97 kg of adipic acid, 138.24 kg of monoethylene glycol, 200.71 kg of 1 ,4-butanediol and 1 ppm of TTB are placed in a 1000 liter stainless steel reactor equipped with oil heating, temperature control, nitrogen inlet, distillation column and stirrer. The reactor is preheated to approx. 80°C and the raw materials are dosed while the stirrer is running. The target temperature is set to 240°C. As the reaction progresses, water is released, which is removed via the column. After reaching 80% of the calculated nominal amount of distillate, 5 ppm SDO are added and the pressure is reduced to 60 mbar within an hour. The water of reaction formed is distilled off continuously until an acid number (AN) of less than 0.6 mgKOH / g is reached.
[0193] A polyester polyol with a hydroxyl number of 38 mgKOH / g, an acid number of 0.5 mgKOH / g and a viscosity of 1550 mPas at 75° C is obtained.
[0194] The polyol A was then purified using a thin-film evaporator (DSV). For this purpose, the polyol was heated to 120°C and metered into the DSV using a gear pump. The DSV was tempered to 240°C and at a speed of 400 rpm. At the same time, a vacuum of <5 mbar was applied. The dosing speed is approx. 1 kg / h.
[0195] 2.2 Polyol B
[0196] 611.97 kg of adipic acid, 138.24 kg of monoethylene glycol, 200.71 kg of 1 ,4-butanediol and 1 ppm of TTB are placed in a 1000 liter stainless steel reactor equipped with oil heating, temperature control, nitrogen inlet, distillation column and stirrer. The reactor is preheated to approx. 80°C and the raw materials are dosed while the stirrer is running. The target temperature is set to 240°C. As the reaction progresses, water is released, which is removed via the column. After reaching 80% of the calculated nominal amount of distillate, 5 ppm SDO are added and the pressure is reduced to 60 mbar within an hour. The water of reaction formed is distilled off continuously until an AN of less than 0.6 mgKOH / g is reached.
[0197] A polyester polyol with a hydroxyl number of 38 mgKOH / g, an acid number of 0.5 mgKOH / g and a viscosity of 1550 mPas at 75° C is obtained
[0198] 2.3 Polyol C
[0199] 1656.75 g of adipic acid, 756.08 g of 1 ,4-butanediol and 495.75 g of 1 ,6-hexanediol are placed in a 4 liter round-bottom flask equipped with a thermometer, nitrogen inlet, heating mantle, distillation column, condenser and stirrer and heated to 120° C heated. After the adipic acid and the 1 ,6-hexanediol have melted completely, the stirrer is switched on at a speed of 200 rpm and the temperature is set to 180. degree. After 180° C has been reached and the water of reaction which has already formed has been distilled off, the temperature is set to 240° C. and further water of reaction is distilled off. After 90% of the calculated water of condensation has been separated off and the temperature has reached 240° C, 10 ppm SDO are metered in and the pressure in the apparatus is reduced to 60 mbar. The water of condensation formed is distilled off continuously until an acid number of less than 0.6 mg KOH / g is reached. A polyol with a hydroxyl number of 56 mgKOH / g and an acid number of 0.6 mgKOH / g is obtained.
[0200] The polyol was then purified using a thin film evaporator (DSV). For this purpose, the polyol was heated to 120° C and metered into the DSV using a gear pump. The DSV was heated to 240° C and at a speed of 400 rpm. At the same time, a vacuum of <5 mbar was applied. The dosing speed is approx. 1 kg / h. The polyol C with a hydroxyl number of 51 mgKOH / g and an acid number of 0.6 mgKOH / g was obtained.
[0201] 2.4 Polyol D
[0202] 1656.75 g of adipic acid, 756.08 g of 1 ,4-butanediol and 495.75 g of 1 ,6-hexanediol are placed in a 4 liter round-bottom flask equipped with a thermometer, nitrogen inlet, heating mantle, distillation column, condenser and stirrer and heated to 120° C heated. After the adipic acid and the 1 ,6-hexanediol have melted completely, the stirrer is switched on at a speed of 200 rpm and the temperature is set to 180. degree. After 180° C has been reached and the water of reaction which has already formed has been distilled off, the temperature is set to 240° C and further water of reaction is distilled off. After 90% of the calculated water of condensation has been separated off and the temperature has reached 240° C, 10 ppm SDO are metered in and the pressure in the apparatus is reduced to 60 mbar. The water of condensation formed is distilled off continuously until an acid number of less than 0.6 mg KOH / g is reached. A polyol D with a hydroxyl number of 56 mgKOH / g and an acid number of 0.6 mgKOH / g is obtained. Polyol E
[0203] 1656.75 g of adipic acid, 558.6 g of 1 ,4-butanediol and 558.6 g of 1 ,6-2-methylpropane- 1 ,3-diol are placed in a 4 liter round-bottomed flask equipped with a thermometer, nitrogen inlet, heating mantle, distillation column, condenser and stirrer and heated to 120 °C. After the adipic acid has completely melted, the stirrer is switched on at a speed of 200 rpm and the temperature is set to 180°C. After 180° C has been reached and the water of reaction which has already formed has been distilled off, the temperature is set to 240° C and further water of reaction is distilled off. After 90% of the calculated water of condensation has been separated off and the temperature has reached 240° C, 10 ppm SDO are metered in and the pressure in the apparatus is reduced to 60 mbar. The water of condensation formed is distilled off continuously until an acid number of less than 0.6 mg KOH / g is reached. A polyol E with a hydroxyl number of 37.4 mgKOH / g and an acid number of 0.6 mgKOH / g is obtained. Polyol F
[0204] PolyTHF is produced by polymerizing THF in the presence of acetic anhydride (ESA). To this end, THF and ESA are continuously fed through the polymerization reactors in a specified ratio of 0.03-0.04. In the reactor, at temperatures of around 40 °C, polyTHF diacetate forms as a precursor to polyTHF over a fixed bed catalyst consisting of activated alumina. After the unreacted THF has been separated off, the crude polyTHF diacetate is converted to polyTH F by transesterification with an excess of methanol by catalysis by sodium methoxide at temperatures of around 70-80° C (at about 100 mbar overpressure). This also produces methyl acetate (methyl ethyl acetate), which is removed from the transesterification equilibrium by distillation. After reaching equilibrium, the transesterification mass is sent to neutralization with an acidic ion exchanger. In the further processing, excess methanol is removed by evaporation. Low-molecular fractions (polyTHF oligomers) are evaporated from the polyTHF to adjust the average molar mass or molecular weight distribution. Polyol G PolyTHF is produced by polymerizing THF in the presence of acetic anhydride (ESA). To this end, THF and ESA are continuously fed through the polymerization reactors in a specified ratio of 0.03-0.04. In the reactor, at temperatures of around 40 °C, polyTHF diacetate forms as a precursor to polyTHF over a fixed bed catalyst consisting of activated alumina. After the unreacted THF has been separated off, the crude polyTHF diacetate is converted to polyTHF by transesterification with an excess of methanol by catalysis by sodium methoxide at temperatures of around 70-80° C (at about 100 mbar overpressure). This also produces methyl acetate (methyl ethyl acetate), which is removed from the transesterification equilibrium by distillation. After reaching equilibrium, the transesterification mass is sent to neutralization with an acidic ion exchanger. In the further processing, excess methanol is removed by evaporation. Low-molecular fractions (polyTHF oligomers) are evaporated from the polyTHF to adjust the average molar mass or molecular weight distribution. Methods: Viscosity
[0205] Unless otherwise stated, the viscosity of the polyols was determined at 25 °C in accordance with DIN EN ISO 3219 (1994) using a Rheotec RC 20 rotational viscometer using the CC 25 DIN spindle (spindle diameter: 12.5 mm; measuring cylinder inner diameter: 13.56 mm) at a shear rate of 50 1 / s. OH number
[0206] The hydroxyl number was determined using the acetic anhydride method DIN 53240 (1971-12) and is given in mg KOH / g. Acid number
[0207] The acid number was determined in accordance with DIN EN 1241 (1998-05) and is given in mg KOH / g. Determination of low molecular weight by-products in the polyol
[0208] The determination of the amount of low molecular weight by-products in the polyol was carried out by GPC according to DIN 55672-1 (2016-03-01 ), however, with THF as flow agent and PEG as standard for the detection of oligomers < 500 g / mol. Differentiation from additives was made by UV detector at a wavelength of 254 nm and detection of the oligomers was made by refractive index (Rl) detector. In addition, the proportion of oligomers < 500 g / mol was determined by thermal desorption GC-MS according to VDA 278 (FOG run only) by weighing 2-4 mg at 120 °C for 10 minutes. The evaluation was carried out using the total ion chromatogram (TIC). The values given are calculated as hexadecane equivalents (ppmHdE). The fraction of mono cycle (ADS glycol) was determined by the peak size. In the case of ether polyol, calibration was carried out against n=4 crown ethers based on THF.
[0209] Table 1 : amount of components with Mn < 500 g / mol-in the polyols TPU Synthesis:
[0210] A thermoplastic polyurethane (TPU) was synthesized from diisocyanate, chain extender (KV), stabilizer and polyol according to the recipes in Table 2 in a reaction vessel with stirring. The starting temperature was 80 °C. After a reaction temperature of 110° C had been reached, the solution was poured onto a heating plate heated to 125° C and the TPU plate obtained was granulated after tempering (15 h, 80° C).
[0211] The hard segment content (HSC) is defined by the following formula having the following definitions:
[0212] MKVX: molar mass of the chain extender x in g / mol ITIKVX: mass of the chain extender x in g
[0213] M|SO: molar mass of the employed isocyanate in g / mol mges: total mass of all starting materials in g x: number of chain extenders. Table 2: Composition of the TPUs
[0214] 5
[0215] 5. Properties of the TPUs
[0216] The blooming behavior was analyzed on untempered 2 mm thick injection molded sheets using an alternating climate test and storage under standard climate. For the alternating climate test, the specimens were stored for 2 weeks, alternating between 12 hours at -18 °C and at room temperature (25 °C). The results are summarized in Table 3.
[0217] The blooming / migration properties are assessed using surface optics. The intensity of the white crystalline deposits was assessed visually. The blooming / migration properties of the obtained TPUs were classified as follows:
[0218] + = good (no visible deposits) o = medium (only punctiform / blotchy deposits)
[0219] - = poor (full-surface deposits)
[0220] - - = extremely poor (heavy full-surface deposits)
[0221] The processability in injection molding was examined with a DEMAG ergotech 200 / 500- 610 injection molding machine with a 0 40 mm three-zone screw. To do this, the TPU granules, which did not contain any other demolding aids such as wax or soap, were first dried at 90 °C for 3 hours. The processing temperatures of the various screw zones are between 190 °C and 230 °C. On the one hand, a cylinder (0 80 mm outside, 40 mm deep) with a wall thickness of 8 mm was produced in a jaw mold as an injection molding. An open hot runner nozzle is used to inject onto an 8-fold cold runner star sub-manifold. On the other hand, a disc (0 125 mm, 27 mm thick) was produced in a jaw mold as an additional injection molding. Gating was done via a central cold runner sprue. The demolding took place via a ring ejector, which stripped the sleeve from the core located in the cavity for demolding. A force sensor on the ejector system transmits the force required to strip off the case.
[0222] + = good (< 13000 N) bad (> 13000 N)
[0223] In addition, the production of expanded particle foam (eTPU) in the extrusion process (as for example disclosed in WO 2013 / 153190 A1) was examined and the blocking properties of the eTPU obtained in 200 L octabins were observed after a storage time of two months at room temperature.
[0224] + = good (eTPU foam beads were individual) o = medium (eTPU foam beads stuck together slightly, but could be separated again with a light touch)
[0225] - = bad (foam beads stuck together, so that when the octabin is tipped out, chunks of foam beads stuck together can also be seen were)
[0226] The low-temperature flexibility (cold-flex) was measured on test specimens tempered for 20 h / 100 °C using dynamic mechanical analysis (DMA) according to DIN EN ISO 6721- 1 :2011-08 with a heating rate of 2 K / min and a frequency of 1 Hz determined under torsion. Here, the maximum of the loss factor (tan 5) was evaluated with "+" equal to > -25°C and equal to < - 25°C.
[0227] The soft-phase crystallization was determined by differential scanning calorimetry (DSC) according to DIN EN ISO 11357-3:2013 with a heating rate of 20 °C / min of injection- molded plates that were tempered at 100 °C for 20 h became. Before the DSC measurements, the TPU was dried at 100° C for 10 minutes. In the case of the presence of an exothermic melting peak with a maximum < 40 °C in the first heating run, the samples were rated the absence of "+".
[0228] Table 3: properties of the TPUS. + = good, o = medium, - = bad, - - = very bad
[0229] The mechanical values of the thermoplastic polyurethanes obtained are listed in Table 4.
[0230] The mechanics were determined at room temperature using the following methods on 2 mm thick injection molded plates that had been tempered at 100 °C for 20 h.
[0231] Shore hardness DIN ISO 7619-1 :2012 determined after an indentation time of 3 s tensile strength DIN 53504:2017-03, S2 test specimen, speed 200 mm / min elongation at break DIN 53504:2017-03, S2 test specimen, speed 200 mm / min
[0232] Tabelle 4: Mechanical properties of the TPUs
[0233] 6. Determination of the low molecular weight fraction in the TPU
[0234] 5 The proportion of low molecular weight fraction was quantitatively analyzed by GPC using dimethylformamide (DMF) as the eluent at a flow rate of 1 .50 mL / min. A PSS SDV linear XL 5 pm column was used and the solution was calibrated against the homologues of polymethyl methacrylate with toluene as the standard.
[0235] 10 The injection molded plates were first stored at 100 °C for 20 h and then the oligomer content <500 g / mol was determined via thermal desorption GC-MS analogous to VDA 278 (FOG run only) with a desorption time of 60 minutes. Evaluation was carried out using the total ion chromatogram (TIC). The values given are calculated as hexadecane equivalents (ppmHdE). The proportion of the mono cycle (consisting of ADS and 1 ,4-butanediol) or, in
[0236] 15 the case of the ether, the crown ether consisting of three TH F molecules was determined by the peak size.
[0237] Table 5: Amount of components with Mn < 500 g / mol in den TPUs.
[0238] * TPU was stored 2 at room temperature prior to the measurement.
[0239] ** Polyol worked up via thin-film evaporator once, conditions for the purification step are described in section 2 with respect to the preparation of the polyols
[0240] *** Polyol worked up via thin-film evaporator twice, conditions for the purification step are described in section 2 with respect to the preparation of the polyols
[0241] Literature cited:
[0242] W0 15 / 000722 A1
[0243] WO 2019 / 002263
[0244] EP 0687695 A1
[0245] WO 2012 / 173911 A1
[0246] US 2003 / 0036621
[0247] WO 2009 / 103767 A1
[0248] WO 94 / 20568A1
[0249] WO 2007 / 082838 A1
[0250] WO2017 / 030835 A1
[0251] WO 2013 / 153190 A1
[0252] WO 2010 / 010010 A1
[0253] "Kunststoffhandbuch [Plastics Handbook], volume 7, Polyurethane [Polyurethanes]”, Carl
[0254] Hanser Verlag, 3rd edition 1993, chapter 3.1
[0255] Kunststoffhandbuch, volume VII, edited by Vieweg and Hochtlen, Carl Hanser Verlag, Munich 1966 (p. 103-113)
Claims
Claims1 . A composition comprising at least the components (i) and (ii):(i) a thermoplastic polyurethane being the reaction product of at least one diisocyanate (11), at least one polyol (P1), and at least one chain extender (C1), and(ii) at least one component (CA1 ) with a molecular weight Mn in the range of from 50 to 500 g / mol, determined by GPC according to DIN 55672-1 (2016-03-01), using DMF as the flow agent and PM MA as the standard, wherein the polyol (P1) comprises functional groups (F1) selected from ether groups and ester groups in the polymer backbone and the component (CA1) comprises functional groups (F2) selected from ether groups and ester groups, and wherein the functional groups (F1) and (F2) are the same.
2. The composition according to claim 1 , wherein (F1) and (F2) are ether groups or (F1) and (F2) are ester groups.
3. The composition according to claim 1 or 2, wherein the polyol (P1) is a polyesterpolyol.
4. The composition according to any of claims 1 to 3, wherein the component (CA1 ) is a polyester, preferably a cyclic polyester.
5. The composition according to any of claims 1 to 4, wherein the component (CA1 ) is a polyester being the reaction product of a dicarboxylic acid (a1) and a diol (d1), the dicarboxylic acid (a1) being selected from the group consisting of adipic acid, succinic acid, or a mixture thereof, and the diol (d1) is selected from the group consisting of ethanediol, propanediol, butanediol, pentanediol, and hexanediol or a mixture thereof.
6. The composition according to claim 5, wherein a mixture of two diols selected from the group consisting of ethanediol, propanediol, butanediol, pentanediol, and hexanediol is used as diol (d1).
7. The composition according to any of claims 1 to 6, wherein the polyol is a polyesterpolyol being the reaction product of a dicarboxylic acid (a2) and a diol (d2), the dicarboxylic acid (a2) being selected from the group consisting of adipic acid, succinic acid, or a mixture thereof, and the diol (d2) is selected from the group consisting of ethanediol, propanediol, butanediol, pentanediol, and hexanediol or a mixture thereof.
8. The composition according to claim 1 or 2, wherein the polyol (P1) is a polyetherpolyol.
9. The composition according to any of claims 1 to 8, wherein the component (CA1) is a polyether, preferably a cyclic polyether.
10. The composition according to any of claims 1 to 9, wherein the component (CA1) is a cyclic oligomer of ethylene oxide, 1 ,2-propylene oxide, 1 ,3-propylene oxide, 1 ,4-butylene oxide11 . The composition according to any of claims 1 to 10, wherein the polyol (P1) is a polyetherpolyol selected from the group consisting of polyethtyleneglycol, polypropyleneglycol, polytrimethyleneglycol and polytetramethyleneglycol.
12. The composition according to any of claims 1 to 11 , wherein the chain extender (C1 ) is selected from the group consisting of ethanediol, propanediol, butanediol, pentanediol, hexanediol, or mixtures thereof.
13. The composition according to any one of claims 1 to 12, wherein isocyanate is selected from the group consisting of methylenediphenyl diisocyanate (MDI), hexamethylene 1 ,6- diisocyanate (H DI), p-phenylene diisocyanate (PDI), 2,2'-diisocyanate (H12MDI), naphthylene 1 ,5-diisocyanate (N DI), isophorone diisocyanate (I PDI) and mixtures thereof.
14. The composition according to any of claims 1 to 13, wherein the proportion of component (CA1 ) given as the content of cyclic migrateable parts in the composition is in the range from 55 to 280 ppmHde by weight based on the total composition.
15. The composition according to any of claims 1 to 14, wherein the proportion of the thermoplastic polyurethane in the composition is in the range from 75% to 99.9% by weight based on the total composition.
16. Process for preparing a composition comprising a thermoplastic polyurethane and at least one component (CA1) with a molecular weight Mn in the range of from 50 to 500 g / mol, determined by GPC according to DIN 55672-1 (2016-03-01 ), using DMF as the flow agent and PM MA as the standard, wherein the thermoplastic polyurethane is prepared by reacting at least components (a), (b) and (c):(a) at least one diisocyanate (11 )(b) at least one polyol composition (PC1 ) and(c) at least one chain extender (C1 ), wherein the polyol composition comprises at least one polyol (P1) and at least one component (CA1), and wherein the polyol (P1 ) comprises functional groups (F1) selected from ether groups and ester groups in the polymer backbone and the component (CA1) comprises functional groups (F2) selected from ether groups and ester groups.
17. The use of a composition according to any of claims 1 to 15 or a composition prepared according to the process according to claim 16 for the production of shaped bodies, coatings, tubes, rolls, belts, damping elements, cable sheaths, hoses, films, nonwoven articles or fibers, foamed parts, particle foams, added manufacturing filaments, 3D printing, extrusion parts, injection molding parts for the use in industrial applications, consumer goods including sports, automotive, agriculture, construction applications.
Citation Information
Patent Citations
Bloom-free thermoplastic polyurethane compositions
EP0687695A1
Process for making bloom-free thermoplastic polyurethane compositions
US20030036621A1
Thermoplastic polyurethane with reduced tendency to bloom
US8790763B2
Thermoplastic polyurethane-based foamed materials
WO1994020568A1
Foams based on thermoplastic polyurethanes
WO2007082838A1
Cited By
Low-shrinkage and high-resilience supercritical polyurethane foaming bead and preparation method thereof
CN119306917A