New polyester material for a high-performance polymer applications
A polyester material with a specific composition and processing method addresses the limitations of existing polymers by enhancing thermal stability and mechanical properties, offering a sustainable and cost-effective solution for photovoltaic applications with improved light transmission and durability.
Patent Information
- Application Number
- PCT/IB2024/055212
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-01
- Filing Date
- 2024-05-29
- Publication Date
- 2024-12-05
AI Technical Summary
Current high-performance polymers for photovoltaic applications, such as EVA and PET, lack optimal optical, mechanical, and electrical properties while being durable, flexible, and resistant to environmental factors, and are not environmentally sustainable or cost-effective.
A polyester material comprising terephthalic acid residues, 60-70 mole % of a first diol residue, 10-30 mole % of a second diol residue, and 10-30 mole % of a third diol residue, with specific processing steps, which enhances thermal stability, mechanical properties, and light transmission, surpassing the limitations of existing materials.
The new polyester material exhibits improved thermal stability, mechanical properties, and reduced optical property loss over time, making it suitable for high-performance photovoltaic applications while being environmentally sustainable and cost-effective.
Smart Images

Figure IB2024055212_05122024_PF_FP_ABST
Abstract
Description
[0001] NEW POLYESTER MATERIAL FOR A HIGH- PERFORMANCE POLYMER APPLICATIONS
[0002] FIELD OF THE INVENTION
[0003] The invention relates a new polyester material for a high-performance polymer to ensure the best properties in terms of light transmission, mechanical and hydrolysis resistance, suitable for photovoltaic application, and methods of preparation thereof.
[0004] BACKGROUND OF THE INVENTION
[0005] The development of photovoltaic technology has led to a significant increase in the demand for high-performance materials suitable for the production of photovoltaic modules. These modules consist of a solar cell, an encapsulation layer, a front sheet and a back sheet that protects the cell from external factors such as UV radiation, humidity, and temperature fluctuations.
[0006] A common material used for this application is glass and more recently plastic material such as PET, but it has different limitations in terms of durability, stability, and resistance to environmental stress.
[0007] To overcome these limitations, researchers have investigated various approaches to modify PET, such as blending it with other polymers or adding functional groups to its molecular structure. However, these modifications typically result in reduced mechanical properties or increased production costs.
[0008] Thus, there is a need for a high-performance polymer suitable for photovoltaic applications that can overcome the limitations of currently available materials, such as EVA and PET, while also being environmentally sustainable and cost-effective. The technical problem of the current prior art is the lack of a polymer formulation that can provide optimal optical, mechanical, and electrical properties while also being durable, flexible, and resistant to environmental factors.
[0009] SUMMARY OF THE INVENTION
[0010] The present invention relates to a new polyester material for a high-performance polymer to ensure the best properties in terms of light transmission, mechanical and hydrolysis resistance, suitable for photovoltaic application.
[0011] The Authors of the present invention defined certain parameters (KPI) required to consider a polyester material as suitable as high-performance polymer, represented in the table below:
[0012] Table 1. Target KPIs
[0013] The Authors of the invention have surprisingly found that a polyester material comprising a dicarboxylic acid component, in particular terephtalic acid residues, and a glycol component comprising 60 to 70 mole % of a first diol residue, 10 to 30 mole % of a second diol residue, and 10 to 30 mole % of a third diol residue, meets all the target KPIs as shown in the table below:
[0014] Table 2. Preferred embodiment of the polymer of the invention meets target KPIs Furthermore, the polyester material of the invention surprisingly shows improved properties with respect to a reference polymer, hereinafter called the benchmark polymer, as shown in the table below: Table 3.
[0015]
[0016] Table 3 - Comparison between the benchmark polymer and the polymer of the invention
[0017] Regarding the thermos-mechanical properties, it is particularly interesting to make a comparison between the benchmark and the polyester of the invention. At temperature lower than 100°C the polyester of the invention shows a higher modulus compared to the benchmark polymer and a lower loss of modulus at 90°C, this means that the polymer of the invention is also able to maintain the mechanical properties with the increase in temperature.
[0018] Hence, in addition to meeting all the project’s KPIs, the polyester of the invention has the following advantages:
[0019] • High thermal properties and thermal stability up to 90°C
[0020] • High optical properties with an excellent light transmission
[0021] • Very reduced loss in optical properties over time.
[0022] Objects of the present invention are:
[0023] - a polyester material comprising: a) a dicarboxylic acid component comprising terephthalic acid residues, and b) a glycol component comprising 60 to 70 mole % of a first diol residue, 10 to 30 mole % of a second diol residue, and 10 to 30 mole % of a third diol residue; wherein the total mole in % of the dicarboxylic acid is 100% mole and the total mole in % of the glycol compenets is 100%;
[0024] - an article of manufacturing comprising or consisting of the polyester according to any one of the embodiments herein disclosed;
[0025] - a photovoltaic module comprising a solar cell element encapsulated by an encapsulant and disposed between a front sheet and a backsheet, characterized in that the front sheet and / or the backsheet comprises a support comprising or consisting of the polyester material according to any one of the embodiments herein disclosed;
[0026] - a method for the preparation of a polyester comprising the following steps: i) providing an admixture of a) a dicarboxylic acid component, and b) a glycol component comprising 60 to 70 mole % of a first diol, 10 to 30 mole % of a second diol, and 10 to 30 mole % of a third diol, wherein the total mole in % of the dicarboxylic acid is 100% mole and the total mole in % of the glycol compenets is 100%; ii) heating the admixture of step i) at a temperature from 175 to 200°C, for 1 ,5h in the presence of nitrogen flux; iii) heating the admixture of step ii) at a temperature from 200 to 240°C, for 1 ,0h with nitrogen flux; iv) heating the admixture of step iii) at a temperature from 255 to 280°C, for 0,5h with nitrogen flux; v) heating the admixture of step iv) at a temperature from 255 to 280°C, for 0,5h with gradual reduction of pressure; vi) heating the admixture of step v) at a temperature from 255 to 280°C for at maximum 3, Oh with full vacuum; vii) application of nitrogen flux and reaction stop.
[0027] In each part of the present description, the term “comprising” can be replaced by the term “consisting of’.
[0028] Further advantages and / or embodiments of the present invention will be evident from the following detailed description.
[0029] DETAILED DESCRIPTION OF THE FIGURES
[0030] Fig. 1. DSC graph of the benchmark polymer
[0031] Fig. 2. Graph of the mechanical properties of the benchmark polymer
[0032] Fig. 3. Graph of flexural properties of the benchmark polymer
[0033] Fig. 4. Graph of the thermomechanical properties of the benchmark polymer
[0034] Fig. 5. DSC graph of the preferred embodiment of the polymer of the invention Fig. 6. Graph of the mechanical properties of the preferred embodiment of the polymer of the invention
[0035] Fig. 7. DMA of the preferred embodiment of the polymer of the invention
[0036] Fig. 8. Optical transmittance of the preferred embodiment of the polymer of the invention Fig. 9. Comparison of the thermos-mechanical properties of the benchmark and of the preferred embodiment of the polymer of the invention
[0037] GLOSSARY
[0038] As used herein, the term "polyester material" includes copolyesters and is understood to mean a synthetic polymer prepared by the reaction of one or more difunctional and / or multifunctional carboxylic acids with one or more difunctional hydroxyl compounds and / or multifunctional hydroxyl compounds.
[0039] As used herein, the term “polymer of the invention” corresponds to the “polyester material”. Typically, the difunctional carboxylic acid can be a dicarboxylic acid and the difunctional hydroxyl compound can be a dihydric alcohol such as, for example, glycols and diols. The term "glycol" as used in this application includes, but is not limited to, diols, glycols, and / or multifunctional hydroxyl compounds, for example, branching agents. Alternatively, the difunctional carboxylic acid may be a hydroxy carboxylic acid such as, for example, p- hydroxybenzoic acid, and the difunctional hydroxyl compound may be an aromatic nucleus bearing 2 hydroxyl substituents such as, for example, hydroquinone.
[0040] The term "residue", as used herein, means any organic structure incorporated into a polymer through a polycondensation and / or an esterification reaction from the corresponding monomer.
[0041] As used herein, therefore, the term dicarboxylic acid is intended to include dicarboxylic acids and any derivative of a dicarboxylic acid, including its associated acid halides, esters, halfesters, salts, half-salts, anhydrides, mixed anhydrides, or mixtures thereof, useful in a reaction process with a diol to make polyester.
[0042] Furthermore, as used in this application, the term "diacid" includes multifunctional acids, for example, branching agents.
[0043] As used herein, the term "terephthalic acid" is intended to include terephthalic acid itself and residues thereof as well as any derivative of terephthalic acid, including its associated acid halides, esters, half-esters, salts, half-salts, anhydrides, mixed anhydrides, or mixtures thereof or residues thereof useful in a reaction process with a diol to make polyester.
[0044] As used herein, the measurement unit “mole %” referred to the diols or diol residues of the glycol component represents the mole % of said diols or diol residues with respect to the total glycol component.
[0045] In the present invention, the complex viscosity can be determined using a rotational rheometer. The tests were performed in Frequency Sweep mode with the following instrumental parameters:
[0046] • Measurement module: Plate / Plate - Diameter: 25mm • Temperature: 280°C
[0047] • Oscillation amplitude: 5%
[0048] • Frequency range: 100Hz - 0,1 Hz.
[0049] In the present invention, the glass transition temperature (Tg) can be determined using a DSC3 instrument by Mettler Toledo at a scan rate of 10°C / min.
[0050] In the present invention, the elastic modulus, the tensile strength, the elongation at maximum load and the elongation at break are measured by a electronic dynamometer Zwich Roell, according to the test method reported in the ISO 527.
[0051] In thre present invention, the storage modulus can be determined using a DMA (Dynamic Mechanic Analyzer) TA model Q800.
[0052] ASTM D 5418 Dual Cantilever - operative parameters:
[0053] Starting temperature: 30°C
[0054] Final temperature: 200°C
[0055] Temperature rate: 3 C7min
[0056] Frequence: 1 Hz
[0057] Amplitude: 10 microns.
[0058] In the present invention, the absorbance or transmittance can be determined using a UV / Vis spectrometer with a cell made of Quartz SUPRASIL®, 10mm optical path, wherein the polymer is dissolved in a 50 / 50 - Chloroform / Hexafluoroisopropanol (0,05 mg / ml) and then analysed, or according to ASTM D1003-13.
[0059] DETAILED DESCRIPTION OF THE INVENTION
[0060] The present invention relates to a polyester material comprising: a) a dicarboxylic acid component comprising terephthalic acid residues, and b) a glycol component comprising 60 to 70 mole % of a first diol residue, 10 to 30 mole % of a second diol residue, and 10 to 30 mole % of a third diol residue, wherein the total mole in % of the dicarboxylic acid is 100% mole and the total mole in % of the glycol compenets is 100%.
[0061] In an embodiment, said terephtalic acid residues are at least 70% of the dicarboxylic acid component, preferably at least 90% of the dicarboxylic acid component, still more preferably at least 99% of the dicarboxylic acid component, even more preferably 100% of the dicarboxylic acid component.
[0062] In an embodiment, said first, second and third diol residue are selected from a list comprising, Ethylene glycole, 1 ,4-cyclohexanedimethanol, Isosorbide, Neopentyl glycol, Bisphenol-S, 2,2,4,4-Tetramethyl-1 ,3cyclobutanediol or 1 ,4-Benzenedimethanol residues. In a preferred embodiment, said first diol residue is 1 ,4-cyclohexanedimethanol.
[0063] In another embodiment, said second diol residue is 2,2,4,4-tetramethyl-1 ,3- cyclobutanediol residue.
[0064] In an embodiment, said third diol residue is 1 ,4-benzenedimethanol residue.
[0065] In a preferred embodiment, said first diol residue is 1 ,4-cyclohexanedimethanol, said second diol residue is 2,2,4,4-tetramethyl-1 ,3-cyclobutanediol residue and said third diol residue is 1 ,4-benzenedimethanol residue.
[0066] In a more preferred embodiment, said polyester material comprises: a) a dicarboxylic acid component comprising at least 99% of terephtalic acid residues, and b) a glycol component comprising 60 to 70 mole % of 1 ,4-cyclohexanedimethanol residues, 10 to 30 mole % of 2,2,4, 4-tetramethyl-1 ,3-cyclobutanediol residues and 10 to 30 mole % of 1 ,4-benzenedimethanol residues, wherein the total mole in % of the dicarboxylic acid is 100% mole and the total mole in % of the glycol compenets is 100%. In a preferred embodiment, said 2,2,4,4-tetramethyl-1 ,3-cyclobutanediol residues are present in a concentration from 15 to 25 mole %, preferably from 17 to 20 mole%, more preferably 18,5 mole %.
[0067] The Authors of the present invention have also found that the compounds 2, 2,4,4- tetramethyl-1 ,3-cyclobutanediol and 1 ,4-benzenedimethanol show a synergistic effect in improving different properties of the polyester of the present invention. In an embodiment, said polyester material further comprises an additive. Preferably, said additive is a thermal stabilizer, an UV blocking additive, a light stabilizer, a polymeric chain extender, fiberglass, fireproof agent, branching agents. In an embodiment, said thermal stabilizer comprises at least one phosphorus compound comprising esters or salts of any one of the following: phosphoric acid, phosphorous acid, phosphonic acid, phosphinic acid, phosphonous acid, alkyl phosphate esters, aryl phosphate esters, (trimethyl phosphate, triphenyl phosphate, tributiyl phosphate, etc.), phenylphosphonic acid, phenylphosphinic acid. said UV blocking additive is selected from at least one of benzotriazoles, hydroxyphenyl benzotriazoles, benzophenones, hydroxyphenyl triazines, cyanoacrylates and organic nickel compounds; said light stabilizer are hindered amine light stabilizers (HALS); said polymeric chain extender include, but are not limited to, multifunctional (including, but not limited to, bifunctional) isocyanates, multifunctional epoxides, including for example, epoxylated novolacs, and phenoxy resins. In certain embodiments, chain extenders may be added at the end of the polymerization process or after the polymerization process. If added after the polymerization process, chain extenders can be incorporated by compounding or by addition during conversion processes such as injection molding or extrusion. The amount of chain extender used can vary depending on the specific monomer composition used and the physical properties desired but is generally about 0.1 percent by weight to about 10 percent by weight, preferably about 0.1 to about 5 percent by weight based on the total weight of the polyester.
[0068] The catalyst may be based on any conventional catalyst, such as alkali metal compounds, alkaline earth metal compounds, zinc compounds, lead compounds, manganese compounds, cobalt compounds, aluminium compounds, antimony compounds, titanium compounds, tin compounds, germanium compounds, or phosphorus compounds. Non-limiting examples of catalyst suitable for the present invention are Sb20s, Ti(OBu)4, GeC>2, Dibutyl-Tin(IV)-Oxide, or mixtures thereof. In a further embodiment, said polyester comprises from 40 to 60% w / w of said dycarboxilic acid residue; and from 30 to 40% w / w of said first diol residue; and from 5 to 15% w / w of said second diol residue; and from 5 to 15% w / w of said third diol residue.
[0069] In a preferred embodiment, said polyester comprises from 40 to 60% w / w of terephtalic acid residues; and from 30 to 40% w / w of 1 ,4-cyclohexanedimethanol residues; and from 5 to 15% w / w of 2,2,4, 4- tetramethyl- 1 ,3-cyclobutanediol residues; and from 5 to 15% w / w of 1 ,4-benzenedimethanol residues.
[0070] In an embodiment, said dicarboxylic acid component and / or said first diol residue and / or said second diol residue and / or said third diol residue is obtained from a recycling process.
[0071] In an embodiment, said polyester has a Tgfrom about 100 to about 120°C measured by DSC (differential scanning calorimetry) at a scan rate of 10°C / min, and / or a loss of storage modulus at 90°C measured according to ASTM D 5418 of less than 5%.
[0072] In an embodiment, the polydispersity index (Mw / Mn) of the polyester is from 2.5 to 5.
[0073] In another embodiment, the ratio between the cis isomers and the trans isomers of 2,2,4,4-tetramethyl-1 ,3-cyclobutanediol is from 30:70 to 50:50, preferably 45:55.
[0074] A further object of the present invention is an article of manufacturing comprising or consisting of the polyester material according to any one of the embodiments herein disclosed. In an embodiment, said article of manufacturing is in the form of a backsheet and / or a front sheet for a photovoltaic module, a fiber, a film, a molded article, a container, a sheet or an injection molded article.
[0075] In another aspect, the present invention relates to a photovoltaic module comprising a solar cell element encapsulated by an encapsulant and disposed between a front sheet and a backsheet, characterized in that the backsheet and / or the front sheet comprises a support comprising or consisting of the polyester material according to any one of the embodiments herein disclosed.
[0076] A further object of the present invention is a method for the preparation of a polyester material comprising the following steps: i) providing an admixture of a) a dicarboxylic acid component, and b) a glycol component comprising 60 to 70 mole % of a first diol, 10 to 30 mole % of a second diol, and 10 to 30 mole % of a third diol, wherein the total mole in % of the dicarboxylic acid is 100% mole and the total mole in % of the glycol compenets is 100%; ii) heating the admixture of step i) at a temperature from 175 to 200°C, for 1 ,5h in the presence of nitrogen flux; iii) heating the admixture of step ii) at a temperature from 200 to 240°C, for 1 ,0h with nitrogen flux; iv) heating the admixture of step iii) at a temperature from 255 to 280°C, for 0,5h with nitrogen flux; v) heating the admixture of step iv) at a temperature from 255 to 280°C, for 0,5h with gradual reduction of pressure; vi) heating the admixture of step v) at a temperature from 255 to 280°C for at maximum 3, Oh with full vacuum; vii) application of nitrogen flux and reaction stop.
[0077] In an embodiment of the method of the present invention, said dicarboxylic acid component is Dimethyl terephthalate (DMT), or terepthalic acid.
[0078] In an embodiment of the method of the present invention, the glycol component is in excess with respect to the dicarboxylic acid component.
[0079] In particular, nitrogen flux means that the reaction is carried out in a nitrogen atmosphere; gradual reduction of pressure means that the pressure is lowered in about 30 minutes from atmospheric pressure to 0,3 mmHg; reaction stop means that after returning the system to nitrogen flow, the heating is stopped, the system cooled down to room temperature and subsequently the polymer is recovered.
[0080] In an embodiment, said temperature of step ii) is preferably from 180 to 195°C, and most preferably 190°C. In an embodiment, said temperature of step iii) is preferably 220°C.
[0081] In an embodiment, said temperature of step iv) is preferably 265°C.
[0082] In an embodiment, said temperature of step v) is preferably 265°C.
[0083] In an embodiment, said temperature of step vi) is preferably 265°C.
[0084] In a preferred embodiment, said heating steps ii)-vi) are carried out in the presence of a catalyst system, wherein said catalyst system may be based on any conventional catalyst, such as alkali metal compounds, alkaline earth metal compounds, zinc compounds, lead compounds, manganese compounds, cobalt compounds, aluminium compounds, antimony compounds, titanium compounds, tin compounds, germanium compounds, or phosphorus compounds. Non-limiting examples of catalyst suitable for the present invention are Sb20s, Ti(OBu)4, GeC>2, Dibutyl-Tin(IV)-Oxide, or mixtures thereof.
[0085] Catalyst amounts can range from 10 ppm to 20,000 ppm or 10 to 10,000 ppm, or 10 to 5000 ppm or 10 to 1000 ppm or 10 to 500 ppm, or 10 to 300 ppm or 10 to 250 based on the catalyst metal and based on the weight of the polymer resulting from the polymerization. The process can be carried out in either a batch or continuous process.
[0086] In an embodiment, said first, second and third diol are selected from a list comprising, ethylene Glycole, 1 ,4-cyclohexanedimethanol, Isosorbide, Neopentyl glycol, Bisphenol- S bis(2hydroxyethyl)ether, 2,2,4,4-Tetramethyl-1 ,3cyclobutanediol or 1 ,4- Benzenedimethanol residues.
[0087] In a preferred embodiment, said first diol is 1,4-cyclohexanedimethanol.
[0088] In another embodiment, said second diol residue is 2,2,4,4-tetramethyl-1 ,3- cyclobutanediol.
[0089] In an embodiment, said third diol residue is 1 ,4-benzenedimethanol.
[0090] In a preferred embodiment, said first diol residue is 1 ,4-cyclohexanedimethanol, said second diol residue is 2,2,4,4-tetramethyl-1 ,3-cyclobutanediol residue and said third diol residue is 1 ,4-benzenedimethanol residue.
[0091] In an embodiment, a branching agent is further admixed in step i).
[0092] In a more preferred embodiment, said admixture of step i) of the method comprises: a) a dicarboxylic acid component comprising at least 99% of DMT, and b) a glycol component comprising 60 to 70 mole % of 1 ,4-cyclohexanedimethanol, 10 to 30 mole % of 2,2,4,4-tetramethyl-1 ,3-cyclobutanediol and 10 to 30 mole % of 1 ,4- benzenedimethanol.
[0093] Hence, in an embodiment, the method of the present invention comprises the following steps: i) providing an admixture of a) a dicarboxylic acid component comprising DMT, and b) a glycol component comprising 60 to 70 mole % of 1 ,4-cyclohexanedimethanol, 10 to 30 mole % of 2,2,4,4-tetramethyl-1 ,3-cyclobutanediol, and 10 to 30 mole % of 1 ,4- benzenedimethanol, wherein the total mole in % of the dicarboxylic acid is 100% mole and the total mole in % of the glycol compenets is 100% ii) heating the admixture of step i) at a temperature from 175 to 200°C, for 1 ,5h in the presence of nitrogen flux; iii) heating the admixture of step ii) at a temperature from 200 to 240°C, for 1 ,0h with nitrogen flux; iv) heating the admixture of step iii) at a temperature from 255 to 280°C, for 0,5h with nitrogen flux; v) heating the admixture of step iv) at a temperature from 255 to 280°C, for 0,5h with gradual reduction of pressure; vi) heating the admixture of step v) at a temperature from 255 to 280°C for at maximum 3, Oh with full vacuum; vii) application of nitrogen flux and reaction stop;
[0094] In a further embodiment, said dicarboxylic acid component and / or said first diol and / or said second diol and / or said third diol is obtained from a recycling process.
[0095] Further object of the present invention is a polyester material obtainable by the method according to any one of the embodiments herein disclosed.
[0096] EXAMPLES
[0097] 1. The “benchmark” polymer
[0098] After scouting and testing a large number of commercial polyesters from different chemical families on the market, the Authors found out that the best solution that meets most of the KPIs .(hereinafter will be called benchmark polymer). Other solutions such as PEN blends and modified PETG for high temperature have been discarded for their inability to pass the dump heat test (i.e. one of the I EC requirements for PV applications). All polymers belonging to the polyester family are composed by an acid part and a glycol part: the standard PET is composed of Terephthalic acid for 100% (mol / acid mol) of the acid component and Ethylene glycol for 100% (mol / glycol mol) for the glycol component. The chemical nature and the relative quantity of the building block monomers of the benchmark polymer was obtained by nuclear magnetic resonance.
[0099] Acid component:
[0100] • Terephthalic acid -^100,0% (mol / acid mol)
[0101] It is used for the production of all polyesters with aliphatic or aromatic diols as the comonomer(s). Glycol components:
[0102] • 1 ,4-Cyclohexanedimethanol — > 65,0% (mol / glycol mol)
[0103] • 2,2,4,4-Tetramethyl-1 ,3-cyclobutanediol — > 35,0% (mol / glycol mol)
[0104] The characteristics and properties of the benchmark polymer are listed and described in the following sections:
[0105] • Density
[0106] • Viscosity
[0107] • Thermal properties
[0108] • Mechanical properties
[0109] • Thermo-mechanical properties
[0110] • Optical properties
[0111] 1.1 Density
[0112] TEST: The density of the benchmark polymer has been determined using the test method described in ISO 1183 part 1.
[0113] INSTRUMENT: Precision balance by Mettler Toledo with density kit
[0114] RESULTS: The result is around 1.2 g / cc, which is inferior to the density of semicrystalline polyesters on the market, which means a lighter PV module.
[0115] The density is lower because the polymer is completely amorphous, without crystal formation. The randomic distribution of the polymer macro-molecules occupy more space than the crystalline, or “packed”, distribution of the same macro-molecules.
[0116] 1.2 Viscosity
[0117] TEST: The benchmark polymer was also analysed by rotational rheometer in order to evaluate the complex viscosity (I q*l), which is derived from oscillatory frequency sweep measurements plotted against the angular frequency (co).
[0118] INSTUMENT: Rotational rheometer
[0119] RESULTS: The complex viscosities of the benchmark polymer measured at 0, 1 Hz, 1 ,08 Hz e 100 Hz:
[0120] Table 4. Viscosity of the benchmark polymer 1.3 Thermal properties
[0121] TEST: In order to determine the thermal characteristic of the benchmark polymer, a DSC (Differential scanning calorimetry) analysis has been carried out. DSC is a thermal analysis apparatus measuring how physical properties of a sample change, along with temperature against time. In other words, the device is a thermal analysis instrument that determines the temperature and heat flow associated with material transitions as a function of time and temperature.
[0122] INSTRUMENT: DSC3 by Mettler Toledo
[0123] RESULTS: For our purposes, the most important parameter is the Tg (glass transition temperature), that represents the transition from a hard and relatively "glassy" state into a viscous or rubbery state and it’s an important parameter because it represents a dramatic change in the mechanical properties.
[0124] The graph of Tg is reported in Fig. 1 , and their values in the Table 3 below.
[0125] The glass transition temperature, as suggested by the name, is a transition and not a sudden change, so it’s common to report the value at the beginning of the transition, called “T onset”, and the value at the middle of the transition, called “T midpoint”.
[0126] Table 5 - Glass transition temperature of benchmark polymer
[0127] For the purposes of the invention, the most significant value is the Tg at the onset value, which as shown by the graph this polymer is around 118°C, so it means that the benchmark polymer maintains most of its properties until it reaches this temperature.
[0128] 1.4 Tensile test;
[0129] INSTRUMENT: Electronic dynamometer Zwick Roell
[0130] RESULTS: The collected results are below reported and in Fig. 2:
[0131] Table 6 - Mechanical properties of the benchmark polymer
[0132] 1.5 Bending test TEST: As the solar panel is subject to its own weight and deformation could occur, the flexural properties have also been tested according to the test method reported in the ISO 178 for the determination of the flexural properties of rigid and semi-rigid plastics: 8 samples 10.11 mm long and 4.01mm thick are tested, as per above mentioned norm. The test allows to evaluate the following parameters: • FLEXURAL STRESS: also known as bending strength, it is defined as the maximum stress in a material just before it yields in a bending test.
[0133] • FLEXURAL STRAIN: It is the nominal fractional change in the length of an element of the outer surface of the test specimen at midspan, where the maximum strain occurs INSTRUMENT: Electronic dynamometer INSTRON model 5500R RESULTS: The collected results are belove reported and in Fig. 3:
[0134] Table 7 - Flexural properties of the benchmark polymer
[0135] The values obtained are in line with the values expected and are suitable for solar panel application.
[0136] 1.6 Thermo-mechanical properties
[0137] TEST: In order to evaluate how the mechanical properties, change with temperature a DMA (Dynamic Mechanical Analysis) analysis has been carried out.
[0138] It is most useful for studying the viscoelastic behaviour of polymers: a sinusoidal stress is applied and the strain in the material is measured, allowing one to determine the complex modulus. This approach can be used to locate the glass transition temperature of the material, as well as to identify transitions corresponding to other molecular motions. The most important value for this specific application is the Storage Modulus, which is the measure of the elastic response of a material, it is also called the inphase component.
[0139] INSTRUMENT: DMA Dynamic Mechanic Analyzer TA model Q800
[0140] RESULTS: The collected results are reported in Fig. 4
[0141] At 50°C the storage modulus is around 1170 MPa and at 90°C is 1023 MPa, so there’s a loss of about 12.5%, which is in line with the KPIs.
[0142] While the Softening Point (Loss Modulus Maximum) is 117.41 °C. It can be observed that the softening point is very close the value of the Tg, this is because they basically represent the same thing, that is the temperature where maximum loss of the mechanical properties occurs.
[0143] 1.7 Optical properties
[0144] TEST: In order to determine the light transmission of this polymer we run a test according to ASTM D1003-13- Standard Test Method for Haze and Luminous Transmittance of Transparent Plastics.
[0145] The test allows to evaluate the following parameters: • TOTAL LUMINOUS TRANSMITTANCE: It is a measure of the amount of light that passes through a transparent material
[0146] • DIFFUSE LUMINOUS TRANSMITTANCE: It is the fraction of diffusely transmitted visible light, basically it is the component scattered in all directions.
[0147] • HAZE: It is measured as the percentage of incident light scattered by more than 2.5° through the plastic specimen. Basically, it is used to describe the “cloudiness” or “milkiness” of a sample. Mathematically it the ratio between diffuse luminous transmittance and total luminous transmittance.
[0148] INSTRUMENT: spectrophotometer Hunterlab - model ColorQUEST - CIELab - D65 - 10°:
[0149] Table 8 - Optical transmittance of the benchmark polymer
[0150] The light transmittance of the benchmark polymer is approximately 90% at a thickness of 2 mm, which is in agreement with the KPI.
[0151] 1.9 Conclusion
[0152] A summarization of the most significant parameters is below reported:
[0153]
[0154] Table 9 - Summary of the properties of the benchmark polymer
[0155] The benchmark polymer covers most of the technical KPIs. Although the benchmark polymer is a high performing polymer which meets the technical KPIs, unfortunately it doesn’t meet the one of the most important target, that is the price target since the benchmark polymer is a specialty and a niche product for a purchase of industrial application, since it contains a specialty monomer.
[0156] Additionally, the benchamark polymer is produced using virgin ingredients derived from petrol cracking, while one of the aim of the invention is to deliver PV modules that are mostly, if not completely, recycled and recyclable.
[0157] 2. The preferred embodiment of the polymer of the invention
[0158] Starting from the raw materials the development of a new polymer, by means of small- scale polymerizations (which consist of the production of approximately 50-100g per bulk polycondensation reaction) was conducted.
[0159] Indicatively, bulk polycondensation reactions were carried out with the aim of obtaining copolymers which, in addition to the properties sought allowed their use in the sector of interest, and that can also be chemically depolymerized with relatively simple processes (e.g. hydrolysis) in order to be able to recover most of the starting monomers with a view to circular economy starting from an adequate eco-design of the material, even before the finished product.
[0160] In total, more than 60 syntheses have been conducted in order to test these different monomers and to find the best combination of properties. The polymers synthesized on a laboratory scale have been characterized mainly to evaluate their physical properties, especially with particular attention to the possible formation of crystalline phases that could create problems in terms of transparency. 2.1 Synthesis activities
[0161] In order to synthetize and find the polymer that meets all the KPIs, many monomers have been considered: based on the properties and industrial availability the following ones have been selected:
[0162] Branching:
[0163] Table 10. Monomers considered and researched
[0164] The synthesis activities can be categorized in three distinct blocks, which will be separately explained below.
[0165] • BLOCK 1 : Polyesters based on DMN (Dimethyl 2,6 Naphthalenedicarboxylate)
[0166] • BLOCK 2: Polyesters based on BPS (Bisphenol-S bis(2-hydroxyethyl)ether) BLOCK 3: Polyesters based on CBDO (2,2,4,4-Tetramethyl-1 ,3-cyclobutanediol)
[0167] Polymeric syntheses can be performed using different catalytic systems and different polymerization procedures; during the project development we used and tested different catalytic system and polymerization procedures.
[0168] Catalytic system MIX-1 - ppm on total initial charge:
[0169] • 500ppm as Sb of Sb20s based catalyst (added at the beginning)
[0170] • 200ppm as Ti of Ti(OBu)4 based catalyst (added at the beginning)
[0171] • 100ppm as P of polyphosphoric acid (added before vacuum steps)
[0172] Catalytic system MIX-2 - ppm on total initial charge:
[0173] • 250ppm as Ge of GeC>2 based catalyst (added at the beginning)
[0174] • 25ppm as Ti of Ti(OBu)4 based catalyst (added at the beginning)
[0175] • 100ppm as P of polyphosphoric acid (added before vacuum steps)
[0176] Catalytic system MIX-3 - ppm on total initial charge:
[0177] • 100ppm as Ti of Ti(OBu)4 based catalyst (added at the beginning)
[0178] • 100ppm as P of Tris(nonylphenyl) phosphite (TNPP) (added at the beginning)
[0179] Catalytic system MIX-4 - ppm on total initial charge:
[0180] • 200ppm as Sn based catalyst Dibutyl-Tin(IV)-Oxide (added at the beginning)
[0181] Polymerization procedure PRO-2:
[0182] 1 ,5h @190°C with Nitrogen flux
[0183] 1 ,0h @220°C with Nitrogen flux
[0184] 0,5h @265°C with Nitrogen flux
[0185] 0,5h @265°C with gradual reduction of pressure (vacuum application)
[0186] Max 3, Oh @265°C with full vacuum
[0187] Application of Nitrogen flux and reaction stop
[0188] BLOCK 1 : We started the activity with polymers based on DMN (Dimethyl 2,6 naphthalenedicarboxylate) because it’s very well known that this monomer boots the Tg of polymer and it’s commercially available in a relatively high amount. We tested different percentage of this monomer with DMT and ISOS to study its behaviour and properties: a detailed table showing the synthesis performed is shown below.
[0189] Table 11 - First block of synthesis activity
[0190] We encountered some problems with the resulted polyesters, because even though they have a high Tg up to 100°C, we realized that DMN and ISOS gave to the polymer some hydrolytic instability, among other smaller issues like loss in light transmittance due the nature of DMN (which is responsible for some light absorption in the late UV spectrum). Furthermore, in order to have an important boost in Tg high amounts of DMN and unfortunately this monomer is commercially available only at a high price.
[0191] BLOCK 2: Due to the potential to give to the polymer a boost in Tg, whilst it has a low industrial cost: we also explored the possibility to use a derivate of bisphenol-S: the BPS (bisphenol-S bis(2-hydroxyethyl)) ether.
[0192] In the following table are reported the detailed synthesis that we performed:
[0193] Table 12- Second block of synthesis activity
[0194] During the testing of the samples produced with BPS it became evident very soon that this monomer gives to the polymer am intrinsic lower hydrolytic stability compared to CBDO.
[0195] Also, the BPS showed some instability during the synthesis, which results in a yellowish polymer, so a lower light transmission. Even though we tried many different combinations of monomers and procedures, the result was always similar, which lead us to think that this is an intrinsic characteristic of the monomer.
[0196] More in details, at the end of the polymerization, the sample HPET-029 had yellowish colour due to the presence of the reagent BPS and melt viscosity was not good, too. H PET-030, synthesized with higher quantity of BPS, showed more problems than HPET- 029. In order to try to solve these problems, the reagent BPS was purified via recrystallization by methanol. The purified BPS was used to synthesize sample HPET- 031. Polymerization of the sample HPET-031 run better than HPET-030, but yellowish colour and a relatively low melt viscosity were observed. BLOCK 3: 2,2,4,4-Tetramethyl-1,3-cyclobutanediol (CBDO) gives the polymer a high boost in Tg and high hydrolytic stability.
[0197] 1 ,4-Benzenedimethanol (BDM), is quite rigid and it helps increasing the polymer glass transition temperature (Tg). In the following table are reported the detailed synthesis that we performed:
[0198] Table 13- Third block of synthesis activity
[0199] The polymers have been analysed using the same technique explained in the previous chapter: the analysis shown that that the most suitable polymer was H PET-057, having the following chemical composition:
[0200] Acid component:
[0201] • Terephthalic acid 100,0% (mol / acid mol)
[0202] Glycol components:
[0203] • 1 ,4-Cyclohexanedimethanol 65,0% (mol / glycol mol)
[0204] • 2,2,4,4-Tetramethyl-1,3-cyclobutanediol 18.5% (mol / glycol mol)
[0205] • 1 ,4-Benzenedimethanol 16.5% (mol / glycol mol)
[0206] H PET-057 has been found to be the most performing and suitable synthesis and is considered the preferred embodiment of the polymer of the invention, a detailed description of the properties can be found in the next sections, so to understand the reasons why we picked this specific polymer. 2.2 Characteristics and properties of the preferred embodiment of the polymer of the invention
[0207] 2.2.1 Viscosity
[0208] TEST: The preferred embodiment of the polymer of the invention was also analysed by rotational rheometer in order to evaluate the complex viscosity (lq*l), which is derived from oscillatory frequency sweep measurements plotted against the angular frequency (w).
[0209] INSTUMENT: Rotational rheometer
[0210] RESULTS: The complex viscosities of the preferred embodiment of the polymer of the invention measured at 0,1 Hz, 1,08 Hz e 100 Hz:
[0211] Table 14 - Viscosity of the preferred embodiment of the polymer of the invention
[0212] 2.2.2 Thermal properties
[0213] TEST: In order to determine the thermal characteristic of the newly synthesized polyester, a DSC (Differential scanning calorimetry) analysis has been carried out.
[0214] INSTRUMENT: DSC3 by Mettler Toledo
[0215] RESULTS: For our purposes, the most important parameter is the Tg (glass transition temperature), that represents the transition from a hard and relatively "glassy" state into a viscous or rubbery state and it’s an important parameter because it represents a dramatic change in the mechanical properties.
[0216] Table 15- Tg of the preferred embodiment of the polymer of the invention
[0217] As show in Fig. 5 the custom polyester has a Tg of around 109°C.
[0218] 2.2.3 Mechanical properties TEST: In order to evaluate the tensile properties of the polymer a test has been carried out according to the test method reported in the ISO 527 with 5 injection-molded specimens of type 1 BA.
[0219] INSTRUMENT: Electronic dynamometer Zwick Roell
[0220] RESULTS: The collected results are reported in Fig. 6 and in the table below
[0221] Table 16 - Mechanical properties of the preferred embodiment of the polymer of the invention
[0222] The results obtained are in line with the results obtained for the benchmark polymer.
[0223] 2.2.4 Thermo-mechanical properties
[0224] TEST: In order to evaluate how the mechanical properties, change with temperature a DMA (Dynamic mechanical analysis) analysis has been carried out.
[0225] It is most useful for studying the viscoelastic behaviour of polymers: a sinusoidal stress is applied and the strain in the material is measured, allowing one to determine the complex modulus. This approach can be used to locate the glass transition temperature of the material, as well as to identify transitions corresponding to other molecular motions.
[0226] The most important value for this specific application is the Storage Modulus, which is the measure of the elastic response of a material but not the same as Young’s modulus, it is also called the inphase component.
[0227] INSTRUMENT: DMA Dynamic Mechanic Analyzer TA model Q800
[0228] RESULTS: The collected results are reported in Fig. 7. At 50°C the storage modulus is around 1257 MPa and at 90°C is 1243 MPa, so there’s a loss of about 1.1 %, which is in line with the KPIs, while the Softening Point (Loss Modulus Maximum) is 104.29°C. It can be observed that the softening point is very close the value of the Tg, that is the temperature where maximum loss of the mechanical properties occurs.
[0229] 2.2.5 Optical properties
[0230] TEST: The custom polyester was analysed by UV / Vis spectroscopy in solution in order to evaluate the absorbance (or transmittance) of the polymeric raw materials, that are not affected by processing.
[0231] INSTRUMENT: UV / Vis Spectrometer with a cell made of Quartz SUPRASIL®, 10mm optical path.
[0232] RESULTS: Polymers was dissolved in a 50 / 50 - Chloroform / Hexafluoroisopropanol (0,05 mg / ml) and then analysed. UV / Vis spectra is reported in Fig. 8. As shown by the graph the transmittance is almost impeccable in the visible region (above 400 nm), there is a very small absorption in the late UV region / early visible region, due to the particular chemical structure of the monomer 1 ,4-Benzenedimethanol. 3. Comparison between the benchmark and preferred embodiment of the polymer of the inventions
[0233] In the following table a comparison is made between the most important properties of the benchmark polymer and the preferred embodiment of the polymer of the invention.
[0234] Table 17 - Comparison between the benchmark polymer and the preferred embodiment of the polymer of the invention Regarding the thermo-mechanical properties, it is particularly interesting to make a comparison between the benchmark and the preferred embodiment of the polymer of the invention. In Fig. 9 is represented the comparison of the graph obtained with DMA analysis of the two polymers. As it is shown in Fig. 9, at temperature lower than 100°C the custom shows a higher modulus compared to the benchmark polymer and a lower loss of modulus at 90°C, this means that the preferred embodiment of the polymer of the invention is able to maintain the mechanical properties with the increase in temperature.
Claims
CLAIMS1. A polyester material comprising: a) a dicarboxylic acid component comprising terephthalic acid residues, and b) a glycol component comprising 60 to 70 mole % of a first diol residue, 10 to 30 mole % of a second diol residue, and 10 to 30 mole % of a third diol residue. wherein the total mole in % of the dicarboxylic acid is 100% mole and the total mole in % of the glycol compenets is 100%.
2. The polyester material according to claim 1 , wherein said first, second and third diol residue are selected from a list comprising, ethylene Glycole, 1 ,4- cyclohexanedimethanol, Isosorbide, Neopentyl glycol, Bisphenol-S bis(2hydroxyethyl)ether, 2,2,4,4-Tetramethyl-1 ,3cyclobutanediol or 1 ,4-Benzenedimethanol residues.
3. The polyester material according to any one of the preceding claims, wherein said first diol residue is 1 ,4-cyclohexanedimethanol, and / or said second diol residue is 2, 2,4,4- tetramethyl-1 ,3-cyclobutanediol residue, and / or said third diol residue is 1 ,4- benzenedimethanol residue, preferably wherein said dicarboxylic acid component and / or said first, second and / or third diol are obtained from a recycling process.
4. The polyester material according to any one of the preceding claims, wherein said 2,2,4,4-tetramethyl-1 ,3-cyclobutanediol residues are present in a concentration from 15 to 25 mole %, preferably from 17 to 20 mole%, more preferably 18,5 mole %.
5. The polyester material according to any one of the preceding claims, further comprising an additive, preferably wherein said additive is a thermal stabilizer, an UV blocking additive, a light stabilizer, a polymeric chain extender, fiberglass, fireproff agents, branching agents.
6. The polyester material according to any one of the preceding claims, wherein the polyester further comprises the residue of at least one catalyst comprising a transition metal or reaction products thereof.
7. The polyester material according to any one of the preceding claims, wherein said polyester has a Tgfrom about 100 to about 120°C measured by a DSC analysis at a scan rate of 10°C / min; and / or and / or a loss of storage modulus at 90°C measured according to ASTM D 5418 of less than 5%.
8. An article of manufacturing comprising or consisting of the polyester according to any one of claims from 1 to 6.
9. The article of manufacturing according to claim 8, in the form of a backsheet and / or a front sheet for a photovoltaic module, a fiber, a film, a molded article, a container, a sheet or an injection molded article.
10. A photovoltaic module comprising a solar cell element encapsulated by an encapsulant and disposed between a front sheet and a backsheet, characterized in that the backsheet and / or the front sheet comprises a support comprising or consisting of the polyester material according to any one of claims 1 to 9.
11. A method for the preparation of a polyester comprising the following steps: i) providing an admixture of a) a dicarboxylic acid component, and b) a glycol component comprising 60 to 70 mole % of a first diol, 10 to 30 mole % of a second diol, and 10 to 30 mole % of a third diol, wherein the total mole in % of the dicarboxylic acid is 100% mole and the total mole in % of the glycol compenets is 100%; ii) heating the admixture of step i) at a temperature from 175 to 200°C, for 1 ,5h in the presence of nitrogen flux; iii) heating the admixture of step ii) at a temperature from 200 to 240°C, for 1 ,0h with nitrogen flux; iv) heating the admixture of step iii) at a temperature from 255 to 280°C, for 0,5h with nitrogen flux; v) heating the admixture of step iv) at a temperature from 255 to 280°C, for 0,5h with gradual reduction of pressure; vi) heating the admixture of step v) at a temperature from 255 to 280°C for at maximum 3, Oh with full vacuum; vii) application of nitrogen flux and reaction stop.
12. The method according to claim 11 , wherein said dicarboxylic acid component is terephtalic acid or DMT.
13. The method according to any one of claims 11 or 12, wherein said heating steps ii)-vi) are carried out in the presence of a catalyst system, preferably based on alkali metal compounds, alkaline earth metal compounds, zinc compounds, lead compounds, manganese compounds, cobalt compounds, aluminium compounds, antimony compounds, titanium compounds, tin compounds, germanium compounds, or phosphorus compounds..
14. The method according to any one of claims 11 to 13, wherein said first, second and third diol are selected from a list comprising ethylene Glycole, 1 ,4- cyclohexanedimethanol, Isosorbide, Neopentyl glycol, Bisphenol-S bis(2hydroxyethyl)ether, 2,2,4,4-Tetramethyl-1 ,3cyclobutanediol or 1 ,4-Benzenedimethanol.
15. The method according to any one of claims 11 to 14, wherein said first diol is 1 ,4- cyclohexanedimethanol and / or said second diol is 2,2,4,4-tetramethyl-1 ,3- cyclobutanediol, and / or said third diol is 1 ,4-benzenedimethanol, preferably wherein said dicarboxylic acid component and / or said first, second and / or third diol are obtained from a recycling process.
Citation Information
Patent Citations
Compositions for metal packaging coatings
US20180223126A1
Tough shrinkable films
US20190211167A1
Crystallizable shrinkable films and thermoformable sheets made from resins blends
US20210395446A1
Polyester film and preparation method thereof
US20220119602A1
Catalyst systems for crystallizable reactor grade resins with recycled content
US20220372217A1