Rubber composition

A rubber composition with a high content of aliphatic diol and dicarboxylic acid in a polycondensate polyester network addresses the challenge of achieving wear resistance and storage modulus in tire applications, enhancing stability and fuel efficiency by reducing heat generation.

WO2024247492A1PCT designated stage expired Publication Date: 2024-12-05KAO CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014204
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-30
Filing Date
2024-04-08
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing rubber compositions for tires fail to achieve both high wear resistance and storage modulus, particularly when using natural rubber, and often result in increased heat generation and loss tangent, which affects fuel efficiency.

Method used

A rubber composition containing natural rubber and a polycondensate polyester with a high content of aliphatic diol and dicarboxylic acid, where the aliphatic diol is 85% by mass and the dicarboxylic acid is 50% by mass or more, forming a polyester network that enhances elongation crystallization and storage modulus, while reducing heat generation.

Benefits of technology

The rubber composition achieves excellent wear resistance and high storage modulus, reducing heat generation and loss tangent, thereby improving fuel efficiency and stability in tire applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

Provided is a rubber composition that contains a rubber component and a polyester. The rubber component includes natural rubber. The polyester is a condensation polymer of an alcohol component and a carboxylic acid component. The content of aliphatic diols having 2-16 carbon atoms in the alcohol component is 85 mass% or more. The content of aliphatic dicarboxylic acid compounds having 2-16 carbon atoms in the carboxylic acid component is 50 mass% or more. Also provided are: a molded rubber body obtained by vulcanizing the rubber composition; a tire member that includes the molded rubber body; use of the rubber composition as an abrasion resistance improver; and a method for improving abrasion resistance of a molded rubber body containing a rubber component and a polyester.
Need to check novelty before this filing date? Find Prior Art

Description

rubber composition

[0001] The present invention relates to a rubber composition, a rubber molded article, a tire component, a method for producing a rubber composition, a method for producing a rubber molded article, and a method for improving the abrasion resistance of a rubber molded article.

[0002] Rubber is an amorphous and soft polymeric substance, primarily composed of organic polymers such as natural rubber and synthetic rubber, and is a material (elastic rubber) with a high elastic limit and a low elastic modulus. Taking advantage of these properties of rubber, rubber compositions containing rubber are used in a variety of fields, including tires, seals, and vibration-isolating and vibration-damping materials. Rubber compositions for tire applications, etc., are blended with inorganic fillers to improve the elastic modulus. Furthermore, a technique for blending polyesters has been proposed to utilize the properties of rubber and satisfy various required physical properties.

[0003] For example, Japanese Patent Laid-Open No. 2020-94113 (Patent Document 1) discloses a rubber composition that exhibits a high degree of SNOW performance, WET performance, low rolling resistance, and steering stability. The rubber composition contains a rubber component, a filler, and at least one thermoplastic resin (C) selected from the group consisting of a styrene-alkylene block copolymer and a polyester polyol resin having an aromatic ring, and a polymer material (D) that does not have a diene skeleton in the molecular skeleton. A rubber composition containing these components is disclosed. Japanese Patent Laid-Open No. 2012-136586 (Patent Document 2) discloses a rubber composition containing a specific low-polarity diene rubber, a specific thermoplastic polyester resin, and a specific high-polarity diene rubber in specific proportions as a rubber composition that can achieve high elasticity while suppressing a significant decrease in tensile elongation and ensuring processability. International Publication No. 2021 / 193795 (Patent Document 3) discloses a rubber additive and a rubber composition that are made of a polyester, which is a polycondensate of a specific alcohol component and a specific carboxylic acid component, and that contain the rubber additive, which are rubber additives and rubber compositions that can produce rubber molded articles that are resistant to deformation and have low heat buildup even when deformed.

[0004] The present invention relates to a rubber composition comprising a rubber component and a polyester, wherein the rubber component comprises natural rubber, the polyester is a polycondensate of an alcohol component and a carboxylic acid component, the alcohol component contains an aliphatic diol having from 2 to 16 carbon atoms in an amount of 85% by mass or more, and the carboxylic acid component contains an aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms in an amount of 50% by mass or more.

[0005] In the rubber compositions of Patent Documents 1 and 2, the blending of aromatic polyesters was mainly investigated, but the abrasion resistance of tire molded articles containing natural rubber using aliphatic polyesters was not investigated, and both abrasion resistance and storage modulus were insufficient. Furthermore, as described in Patent Document 3, the present inventors have discovered rubber molded articles that are resistant to deformation and generate little heat even when deformed by using aliphatic polyesters as rubber additives, but the abrasion resistance of tire molded articles containing natural rubber has not been sufficiently investigated. The present invention relates to a rubber composition that can give a rubber molded article that has excellent abrasion resistance and a high storage modulus, a rubber molded article using the same, a tire component, a method for producing a rubber composition, a method for producing a rubber molded article, and a method for improving the abrasion resistance of a rubber molded article.

[0006] The present invention relates to the following [1] to [6]. [1] A rubber composition containing a rubber component and a polyester, wherein the rubber component contains natural rubber, the polyester is a polycondensate of an alcohol component and a carboxylic acid component, the alcohol component contains an aliphatic diol having from 2 to 16 carbon atoms in a content of 85% by mass or more, and the carboxylic acid component contains an aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms in a content of 50% by mass or more. [2] A rubber molded article obtained by vulcanizing the rubber composition described in [1] above. [3] A tire component including the rubber molded article described in [2] above. [4] A method for producing the rubber composition described in [1] above, comprising the following steps (1) and (2): [5] A method for producing a rubber molded article, comprising a step of vulcanizing the rubber composition described in [1] above. [6] A method for improving the wear resistance of a rubber molded article comprising a rubber component and a polyester, wherein the rubber component contains natural rubber, the polyester is a polycondensate of an alcohol component and a carboxylic acid component, the alcohol component contains an aliphatic diol having from 2 to 16 carbon atoms in an amount of 85% by mass or more, and the carboxylic acid component contains an aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms in an amount of 50% by mass or more. [7] A method for improving the wear resistance of a rubber molded article, comprising a step of vulcanizing the rubber composition described in [1] above. [8] A method for improving the wear resistance of a rubber molded article, wherein the rubber component contains natural rubber, the polyester is a polycondensate of an alcohol component and a carboxylic acid component, the alcohol component contains an aliphatic diol having from 2 to 16 carbon atoms in an amount of 85% by mass or more, and the carboxylic acid component contains an aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms in an amount of 50% by mass or more.

[0007] According to the present invention, it is possible to provide a rubber composition that can give a rubber molded article having excellent abrasion resistance and a high storage modulus, a rubber molded article using the same, a tire component, a method for manufacturing a rubber composition, a method for manufacturing a rubber molded article, and a method for improving the abrasion resistance of a rubber molded article. Furthermore, according to the present invention, it is possible to reduce the loss tangent of the rubber molded article and reduce the heat buildup of the rubber molded article.

[0008] [Rubber Composition] The rubber composition of the present invention is a rubber composition containing a rubber component and a polyester, wherein the rubber component contains natural rubber, the polyester is a polycondensate of an alcohol component and a carboxylic acid component, the alcohol component contains an aliphatic diol having from 2 to 16 carbon atoms in a content of 85% by mass or more, and the carboxylic acid component contains an aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms in a content of 50% by mass or more.

[0009] The rubber composition of the present invention can produce rubber molded articles that have excellent abrasion resistance and a high storage modulus. The reason for this is not entirely clear, but it is believed to be as follows: The natural rubber contained as the rubber component of the present invention exhibits so-called strain-induced crystallization, in which molecules are oriented and crystallized by stretching. Natural rubber tends to exhibit significant stress relaxation due to this strain-induced crystallization. On the other hand, the polyester of the present invention is obtained by polycondensation of an alcohol component containing an aliphatic diol having 2 to 16 carbon atoms and a carboxylic acid component containing an aliphatic dicarboxylic acid compound having 2 to 16 carbon atoms. Since both the alcohol component and the carboxylic acid component of the polyester are aliphatic compounds having 2 to 16 carbon atoms, the polyester is incompatible with the rubber component containing natural rubber in the rubber composition and rubber molded article, forming fine crystals and forming a polyester network within the rubber component. Therefore, the polyester is believed to serve as a nucleus for strain-induced crystallization of the natural rubber contained in the rubber component. Thus, since the rubber composition of the present invention contains natural rubber and the polyester, the resulting rubber molded article is believed to exhibit excellent abrasion resistance due to the accelerated strain-induced crystallization. Furthermore, since the rubber molded article of the present invention has the polyester network as described above, the obtained rubber molded article can exhibit a high storage modulus, and is expected to have excellent handling stability when used in tire components, etc. Furthermore, since the rubber composition of the present invention has the polyester network as described above, the obtained rubber molded article is unlikely to have a large loss tangent (tan δ) even during deformation, and heat buildup can be reduced, and is expected to have excellent fuel economy when used in tire components, etc.

[0010] <Rubber Component> The rubber composition of the present invention contains natural rubber. When the rubber component contains natural rubber, strain-induced crystallization is promoted using the polyester described below as a nucleus, and the resulting rubber molded article is therefore excellent in abrasion resistance and can exhibit a high storage modulus. Examples of natural rubber include SMR, SIR, STR, and RSS. Preferably, one or more selected from SMR20, STR20, RSS#3, and RSS#4 are used. More preferably, one or more selected from RSS#3 and RSS#4 are used. RSS#3 is more preferred. Furthermore, the natural rubber can be modified before use. Examples of modified natural rubber include epoxidized natural rubber and hydrogenated natural rubber.

[0011] In the rubber composition of the present invention, the rubber component preferably further contains a synthetic rubber. By including a synthetic rubber in the rubber component, the abrasion resistance and storage modulus of the resulting rubber molded article can be improved. As the synthetic rubber, a diene-based synthetic rubber is preferred. As the diene-based synthetic rubber, one or more selected from polyisoprene rubber (IR), polybutadiene rubber (BR), styrene-butadiene copolymer rubber (SBR), acrylonitrile-butadiene copolymer rubber (NBR), chloroprene rubber (CR), butyl rubber (IIR), and polyisobutylene are preferred, as they improve the abrasion resistance and storage modulus of the resulting rubber molded article, with styrene-butadiene copolymer rubber (SBR) being more preferred. Among the above diene-based synthetic rubbers, the copolymer rubber may be either a block copolymer or a random copolymer, but a random copolymer is preferred from the viewpoint of improving the abrasion resistance and storage modulus of the resulting rubber molded article. The rubber component may be used alone or in combination of two or more types. Styrene-butadiene copolymer rubber (SBR) is a rubber that does not exhibit strain-induced crystallization. However, in the present invention, even if the rubber component contains styrene-butadiene copolymer rubber (SBR), the abrasion resistance and storage modulus of the resulting rubber molded article can be improved.

[0012] In the present invention, when the rubber component further contains a synthetic rubber, the mass ratio of the content of the natural rubber to the synthetic rubber (natural rubber / synthetic rubber) is preferably 50 / 50 or more, more preferably 60 / 40 or more, even more preferably 80 / 20 or more, and still more preferably 90 / 10 or more, from the viewpoint of improving the abrasion resistance and storage modulus of the obtained rubber molded article and from the viewpoint of reducing the loss tangent of the obtained rubber molded article. Furthermore, from the viewpoint of improving the abrasion resistance and storage modulus of the obtained rubber molded article and from the viewpoint of reducing the loss tangent of the obtained rubber molded article, it is preferable that the content of the natural rubber in the rubber component is 100% by mass.

[0013] <Polyester> In the present invention, the polyester is a polycondensate of an alcohol component and a carboxylic acid component, in which the content of an aliphatic diol having from 2 to 16 carbon atoms in the alcohol component is 85% by mass or more, and the content of an aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms in the carboxylic acid component is 50% by mass or more.

[0014] (Alcohol Component) In the present invention, the alcohol component of the polyester contains 85% by mass or more of an aliphatic diol having 2 to 16 carbon atoms in the alcohol component, from the viewpoint of improving the abrasion resistance and storage modulus of the resulting rubber molded article. If the content of the aliphatic diol having 2 to 16 carbon atoms in the alcohol component is less than 85% by mass, the abrasion resistance cannot be improved and the storage modulus cannot be sufficiently increased, which is undesirable. Furthermore, a content of the aliphatic diol having 2 to 16 carbon atoms in the alcohol component of 85% by mass or more is also preferable because it can reduce the loss tangent of the resulting rubber molded article. The content of the aliphatic diol having 2 to 16 carbon atoms in the alcohol component is preferably 90% by mass or more, more preferably 92% by mass or more, even more preferably 95% by mass or more, and even more preferably substantially 100% by mass.

[0015] The chain hydrocarbon group in the aliphatic diol may be linear or branched, but is preferably a linear hydrocarbon group from the viewpoint of improving the abrasion resistance and storage modulus of the resulting rubber molded article and from the viewpoint of reducing the loss tangent of the resulting rubber molded article, and the hydroxy group is preferably located at the end of the hydrocarbon chain. That is, the aliphatic diol is more preferably an α,ω-linear alkanediol having from 2 to 16 carbon atoms. From the same viewpoints as above, the number of carbon atoms in the aliphatic diol is 2 or more, preferably 4 or more, more preferably 6 or more, and even more preferably 8 or more, and from the viewpoint of improving the crystallinity of the polyester in the rubber composition and the rubber molded article, it is preferably 14 or less, more preferably 12 or less.

[0016] Examples of aliphatic diols having from 2 to 16 carbon atoms, particularly α,ω-linear alkanediols having from 2 to 16 carbon atoms, include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, and 1,14-tetradecanediol. Among these, one or more selected from ethylene glycol, 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, and 1,12-dodecanediol are preferred, and one or more selected from ethylene glycol, 1,4-butanediol, 1,10-decanediol, and 1,12-dodecanediol are more preferred.

[0017] The alcohol component may contain an alcohol other than an aliphatic diol having from 2 to 16 carbon atoms, provided that the object of the present invention is not impaired. Examples of alcohol components other than an aliphatic diol having from 2 to 16 carbon atoms include aromatic diols such as alkylene oxide adducts of bisphenol A, trihydric or higher polyhydric alcohols such as glycerin, pentaerythritol, and trimethylolpropane, and monohydric alcohols. The above alcohol components may be used alone or in combination of two or more.

[0018] (Carboxylic Acid Component) In the present invention, the carboxylic acid component of the polyester contains 50% by mass or more of an aliphatic dicarboxylic acid compound having 2 to 16 carbon atoms in the carboxylic acid component, from the viewpoint of improving the abrasion resistance and storage modulus of the resulting rubber molded article. If the content of the aliphatic dicarboxylic acid compound having 2 to 16 carbon atoms in the carboxylic acid component is less than 50% by mass, the abrasion resistance of the resulting rubber molded article cannot be improved, and the storage modulus cannot be sufficiently increased, making it impossible to improve the storage modulus, which is undesirable. Furthermore, a content of the aliphatic dicarboxylic acid compound having 2 to 16 carbon atoms in the alcohol component of 50% by mass or more is also preferable from the viewpoint of reducing the loss tangent of the resulting rubber molded article. The content of the aliphatic dicarboxylic acid compound having 2 to 16 carbon atoms in the carboxylic acid component is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, still more preferably 90% by mass or more, and even more preferably substantially 100% by mass.

[0019] The chain hydrocarbon group in the aliphatic dicarboxylic acid compound may be linear or branched, but from the viewpoint of improving the abrasion resistance and storage modulus of the resulting rubber molded article and from the viewpoint of reducing the loss tangent of the resulting rubber molded article, it is preferably a linear hydrocarbon group, and the carboxy group is preferably located at the end of the hydrocarbon chain. That is, the aliphatic dicarboxylic acid compound is more preferably an α,ω-linear aliphatic dicarboxylic acid having from 2 to 16 carbon atoms. From the same viewpoint as above, the number of carbon atoms in the aliphatic dicarboxylic acid compound is preferably 4 or more and preferably 14 or less.

[0020] Examples of aliphatic dicarboxylic acid compounds having from 2 to 16 carbon atoms, particularly α,ω-linear aliphatic dicarboxylic acids having from 2 to 16 carbon atoms, include succinic acid (carbon number: 4), fumaric acid (carbon number: 4), sebacic acid (carbon number: 10), dodecanedioic acid (carbon number: 12), tetradecanedioic acid (carbon number: 14), hexadecanedioic acid (carbon number: 16), and succinic acids having an alkyl group or alkenyl group on the side chain. Aliphatic dicarboxylic acid compounds also include their acid anhydrides and their alkyl esters having from 1 to 3 carbon atoms. Of these, one or more selected from succinic acid, sebacic acid, dodecanedioic acid, tetradecanedioic acid, and hexadecanedioic acid are preferred, one or more selected from succinic acid, sebacic acid, dodecanedioic acid, and tetradecanedioic acid are more preferred, and one or more selected from succinic acid, sebacic acid, and dodecanedioic acid are even more preferred. In the present invention, the carboxylic acid component includes not only free acid but also anhydrides that decompose to generate an acid during the reaction, and alkyl esters having from 1 to 3 carbon atoms. However, the number of carbon atoms in the alkyl ester moiety is not included in the number of carbon atoms in the aliphatic dicarboxylic acid compound.

[0021] The carboxylic acid component may contain other carboxylic acid compounds other than aliphatic dicarboxylic acid compounds having from 2 to 16 carbon atoms, as long as the object of the present invention is not impaired. Examples of other carboxylic acid compounds include aromatic dicarboxylic acid compounds such as terephthalic acid and isophthalic acid, trivalent or higher polyvalent carboxylic acid compounds such as trimellitic acid and pyromellitic acid, and monovalent carboxylic acid compounds.

[0022] The total content of the aliphatic diol having from 2 to 16 carbon atoms and the aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms is preferably 85% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and still more preferably substantially 100% by mass, based on the raw material monomers for the polyester.

[0023] The content of the aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms relative to 100 parts by mole of the aliphatic diol having from 2 to 16 carbon atoms is preferably 75 parts by mole or more, more preferably 85 parts by mole or more, and is preferably 115 parts by mole or less, more preferably 110 parts by mole or less, and even more preferably 105 parts by mole or less.

[0024] (Production of Polyester) In the present invention, the polyester can be produced by a known method. For example, the polycondensation reaction of the alcohol component and the carboxylic acid component can be carried out in an inert gas atmosphere, in the presence of an esterification catalyst, an esterification promoter, a polymerization inhibitor, and the like, as necessary, at a temperature of preferably 160°C to 240°C, more preferably 190°C to 230°C. Examples of the esterification catalyst include tin catalysts, titanium catalysts, and metal compounds such as antimony trioxide, zinc acetate, and germanium dioxide. From the viewpoint of esterification reaction efficiency, tin compounds such as dibutyltin oxide and tin(II) 2-ethylhexanoate, and titanium compounds such as titanium diisopropylate bis(triethanolaminate) are preferred. The amount of the esterification catalyst used is preferably 0.01 to 1.5 parts by mass, more preferably 0.1 to 1.0 part by mass, per 100 parts by mass of the total amount of the alcohol component and the carboxylic acid component.

[0025] The esterification promoter is preferably a pyrogallol compound, and specific examples include pyrogallol, gallic acid, gallic acid esters, benzophenone derivatives, and catechin derivatives. From the viewpoint of reactivity, gallic acid is preferred. The amount of the esterification promoter used is preferably 0.001 to 0.5 parts by mass, more preferably 0.01 to 0.1 parts by mass, per 100 parts by mass of the total amount of the alcohol component and the carboxylic acid component. Examples of the polymerization inhibitor include tert-butylcatechol. The amount of the polymerization inhibitor used is preferably 0.001 to 0.5 parts by mass, more preferably 0.01 to 0.1 parts by mass, per 100 parts by mass of the total amount of the alcohol component and the carboxylic acid component.

[0026] In the present invention, from the viewpoint of improving the abrasion resistance and storage modulus of the resulting rubber molded article and from the viewpoint of reducing the loss tangent of the resulting rubber molded article, the weight average molecular weight of the polyester is preferably 3,000 or more, more preferably 5,000 or more, even more preferably 6,000 or more, still more preferably 7,000 or more, still more preferably 10,000 or more, and is preferably 100,000 or less, more preferably 50,000 or less, still more preferably 40,000 or less, and still more preferably 35,000 or less. The weight average molecular weight of the polyester can be measured by the method described in the examples.

[0027] The polyester of the present invention is preferably a crystalline polyester from the viewpoint of improving the abrasion resistance of the resulting rubber molded article. When a solid polyester is heated, the resin state of a crystalline polyester changes rapidly from a solid state to a molten state at the melting point. On the other hand, the resin state of an amorphous polyester changes gradually from a solid state to a molten state at the glass transition temperature. In the present invention, a polyester having a recognized melting point is defined as a crystalline polyester. In the present invention, the melting point of the polyester is preferably 60°C or higher, more preferably 70°C or higher, even more preferably 75°C or higher, from the viewpoint of improving the abrasion resistance and storage modulus of the resulting rubber molded article and reducing the loss tangent of the resulting rubber molded article, and is preferably 150°C or lower, more preferably 130°C or lower, even more preferably 120°C or lower. The melting point of the polyester can be measured by the method described in the examples.

[0028] In the present invention, the larger the endothermic value ΔH of the melting endothermic peak of the polyester measured by DSC, the higher the crystalline nature of the polyester tends to be. Therefore, the larger the endothermic value ΔH of the melting endothermic peak of the polyester measured by DSC, the more likely it is to serve as a nucleus for elongation-induced crystallization of natural rubber, and the more likely it is to promote elongation-induced crystallization of the resulting rubber molded article, thereby making it easier to improve the abrasion resistance in particular. In the present invention, the endothermic value ΔH of the melting endothermic peak of the polyester measured by DSC, from the viewpoint of improving the abrasion resistance and storage modulus of the resulting rubber molded article and reducing the loss tangent of the resulting rubber molded article, is preferably 50 J / g or more, more preferably 70 J / g or more, even more preferably 80 J / g or more, still more preferably 90 J / g or more, and is preferably 180 J / g or less, more preferably 170 J / g or less, even more preferably 160 J / g or less, and still more preferably 150 J / g or less. The endothermic value ΔH of the polyester can be adjusted to the above range by adjusting the monomer composition, the molecular weight of the polyester, etc. The endothermic heat ΔH of the polyester can be measured by the method described in the examples.

[0029] The Hansen solubility parameter (SP value) of the polyester in the present invention is preferably 16 (MPa) 1 / 2 More preferably, 17.0 (MPa) 1 / 2 More preferably, 17.5 (MPa) 1 / 2 More preferably, 18.0 (MPa) 1 / 2 More preferably, 18.5 (MPa) 1 / 2 and preferably 24.0 (MPa) 1 / 2 More preferably, 23.5 (MPa) or less 1 / 2 More preferably, 23.0 (MPa) or less 1 / 2 By setting the SP value of the polyester within the above range, it becomes easier to form fine crystals without being miscible with the rubber component in the rubber composition and the rubber molded article, which can easily serve as nuclei for elongated crystals, improving abrasion resistance. It also becomes easier to form a polyester network in the rubber component, improving the storage modulus.

[0030] The SP value can be calculated using solubility parameter calculation software (Hansen Solubility Parameters in Practice 4th Edition 4.1.03). In this specification, the SP value used is the Hansen solubility parameter. The Hansen solubility parameter is calculated based on the chemical structure by dividing the types of interaction energy acting between the molecules of a substance into three. Specifically, the SP value δ is calculated using the following formula, which divides the Hildebrand solubility parameter into three components: δ = (δ d 2 +δ p 2 +δ h 2 ) 1 / 2 where δ d is the London dispersion force term, δ p is the molecular polarization term, δ h is the hydrogen bond term. Each δ d , δ p , δ h These are described in detail in "HANSEN SOLBILITY PARAMETERS" A User's Handbook Second Edition. If the SP value cannot be determined by the above method, the values ​​described in "Solubility Parameter Values" VII, pp. 675-714 of Polymer Handbook Fourth Edition (published by Wiley, 1999) may be used.

[0031] The polyester in the present invention may be a modified polyester that has been modified to such an extent that its properties are not substantially impaired. Examples of modified polyesters include urethane-modified polyesters in which polyesters are modified with urethane bonds, epoxy-modified polyesters in which polyesters are modified with epoxy bonds, and composite resins having two or more resin components including a polyester component and an addition polymerization resin component. The polyester according to the present invention preferably contains 98% by mass or more of polyester moieties, more preferably consists essentially of polyester moieties, and even more preferably consists essentially of polyester moieties.

[0032] <Inorganic Filler> The rubber composition of the present invention preferably further contains an inorganic filler. By containing an inorganic filler, the abrasion resistance and storage modulus of the resulting rubber molded article can be improved. The inorganic filler is not particularly limited, and examples thereof include silica and carbon black. Furthermore, alumina, calcium carbonate, clay, talc, zeolite, diatomaceous earth, etc. can be used as needed. Among these, the inorganic filler is preferably one or more selected from silica and carbon black. The inorganic filler can be used alone or in combination of two or more.

[0033] (Silica) There is no particular limitation on the silica used, and examples thereof include wet silica, dry silica, and colloidal silica. Among these, wet silica, which is mainly composed of hydrous silica, is preferred. Wet silica includes precipitated silica, gel silica, and sol-gel silica, with precipitated silica being more preferred. The BET specific surface area of ​​the silica (measured in accordance with ISO 5794 / 1) is preferably 50 m from the viewpoint of dispersibility of silica in the rubber composition and rubber molded article and rubber reinforcement. 2 / g or more, more preferably 100m 2 / g or more, more preferably 150m 2 / g or more, and preferably 350m 2 / g or less, more preferably 300m 2 / g or less, more preferably 250m 2From the viewpoints of dispersibility of silica in the rubber composition and the rubber molded article and rubber reinforcement properties, the average secondary particle size of silica is preferably 10 μm or more, more preferably 15 μm or more, and even more preferably 18 μm or more, and is preferably 100 μm or less, more preferably 80 μm or less, and even more preferably 50 μm or less.

[0034] An example of a commercially available silica product is Nipsil AQ (BET specific surface area: 205 m) manufactured by Tosoh Silica Corporation. 2 / g), Nipsil KQ (BET specific surface area: 240 m 2 / g), Ultrasil VN3 (BET specific surface area: 175 m), manufactured by Evonik 2 / g) and the like.

[0035] (Carbon Black) There are no particular limitations on the carbon black used, and examples thereof include high-, medium-, or low-structure carbon blacks of grades such as SAF, ISAF, IISAF, N339, HAF, FEF, GPF, and SRF, as well as carbon and silica dual-phase fillers in which silica is supported on the surface of carbon black. Among these, SAF, ISAF, IISAF, N339, HAF, and FEF grade carbon blacks are preferred. The DBP absorption of the carbon black (measured in accordance with ASTM D2414-65T) is preferably 70 cm 3 / 100g or more, more preferably 80cm 3 / 100g or more, more preferably 90cm 3 / 100g or more. 2 AS, measured in accordance with JIS K 6217-2:2017) is preferably 50 m 2 / g or more, more preferably 60m 2 / g or more, more preferably 70m 2 / g or more.

[0036] (Sulfur) The rubber composition of the present invention preferably contains sulfur as a vulcanizing agent, since it is vulcanized to form a rubber molded article. Examples of sulfur include powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, highly dispersible sulfur, and soluble sulfur, which are commonly used in the rubber industry. The sulfur may be used alone or in combination of two or more kinds.

[0037] <Other Components> In addition to the above-described components, the rubber composition of the present invention may contain, if desired, various additives commonly used in the rubber industry, such as a silane coupling agent, an antioxidant, a scorch inhibitor, a softener, stearic acid, process oil, zinc oxide, and a vulcanization accelerator, within a range that does not impair the object of the present invention.

[0038] (Process Oil) The process oil preferably has a pour point of 40° C. or lower. From the viewpoint of improving the processability of the rubber composition, the process oil is preferably one or more selected from aromatic process oil, naphthenic process oil, and paraffinic process oil, and more preferably naphthenic process oil.

[0039] <Content of Each Component in Rubber Composition> In the rubber composition of the present invention, the content of the polyester is preferably 1.0 part by mass or more, more preferably 1.2 parts by mass or more, and even more preferably 1.4 parts by mass or more, per 100 parts by mass of the rubber component, from the viewpoint of improving the abrasion resistance and storage modulus of the obtained rubber molded article and from the viewpoint of reducing the loss tangent of the obtained rubber molded article; and from the viewpoint of maintaining the physical properties of the rubber component, the content of the polyester is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, even more preferably 20 parts by mass or less, still more preferably 15 parts by mass or less, and still more preferably 12 parts by mass or less.

[0040] In addition, in the rubber composition of the present invention, the mass ratio of the polyester content to the natural rubber content ([polyester content] / [natural rubber content]) is preferably 0.01 or more, more preferably 0.02 or more, from the viewpoint of improving the abrasion resistance and storage modulus of the resulting rubber molded article, and is preferably 0.20 or less, more preferably 0.10 or less, and even more preferably 0.05 or less, from the viewpoint of reducing the loss tangent of the resulting rubber molded article.

[0041] From the viewpoint of maintaining the physical properties of the rubber component, the content of the rubber component in the rubber composition is preferably 30% by mass or more, more preferably 35% by mass or more, even more preferably 40% by mass or more, still more preferably 45% by mass or more, and is preferably 80% by mass or less, more preferably 75% by mass or less, even more preferably 70% by mass or less, still more preferably 65% ​​by mass or less.

[0042] The content of the inorganic filler is preferably 30 parts by mass or more, more preferably 35 parts by mass or more, even more preferably 40 parts by mass or more, and still more preferably 45 parts by mass or more, per 100 parts by mass of the rubber component, from the viewpoint of improving the abrasion resistance and storage modulus of the obtained rubber molded body, and is preferably 200 parts by mass or less, more preferably 180 parts by mass or less, even more preferably 150 parts by mass or less, still more preferably 100 parts by mass or less, and still more preferably 80 parts by mass or less, from the viewpoint of reducing the heat buildup of the rubber molded body.

[0043] From the viewpoint of sufficiently vulcanizing the unvulcanized rubber composition, the sulfur content is preferably 0.3 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 0.8 parts by mass or more, and is preferably 3 parts by mass or less, more preferably 2.5 parts by mass or less, even more preferably 2 parts by mass or less, per 100 parts by mass of the uncrosslinked rubber component.

[0044] When the rubber composition of the present invention further contains a process oil, from the viewpoint of improving the processability of the rubber composition, the amount of the process oil per 100 parts by mass of the rubber component is preferably 4 parts by mass or more and 16 parts by mass or less, more preferably 6 parts by mass or more and 14 parts by mass or less, and even more preferably 8 parts by mass or more and 12 parts by mass or less.

[0045] <Production of Rubber Composition> The method for producing a rubber composition of the present invention includes the following steps (1) and (2): step (1): kneading a composition comprising a rubber component and a polyester, wherein the rubber component comprises natural rubber, the polyester is a polycondensate of an alcohol component and a carboxylic acid component, the alcohol component contains an aliphatic diol having from 2 to 16 carbon atoms in an amount of 85% by mass or more, and the carboxylic acid component contains an aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms in an amount of 50% by mass or more; and step (2): further adding and mixing sulfur.

[0046] More specifically, in step (1), a rubber mixture is preferably obtained by kneading a rubber component, a polyester, and, if necessary, an inorganic filler, a silane coupling agent, an antioxidant, a scorch inhibitor, a softener, stearic acid, a process oil, etc., using a kneader. Examples of kneaders include a Banbury mixer, a roll, and an intensive mixer. The kneading temperature is preferably 140°C or higher, more preferably 143°C or higher, and even more preferably 145°C or higher, from the viewpoints of improving the dispersibility of the polyester in the rubber composition and improving the abrasion resistance and storage modulus of the resulting rubber molded product, and is preferably 165°C or lower, more preferably 160°C or lower, and even more preferably 155°C or lower.

[0047] Step (2) is a step of further adding and mixing sulfur after step (1). More specifically, in step (2), sulfur, and, if necessary, zinc oxide and a vulcanization accelerator (sulfenamide-based, guanidine-based, etc.) are preferably added and mixed. The mixing temperature in step (2) is preferably less than 140°C, more preferably 130°C or less, even more preferably 125°C or less, and still more preferably 120°C or less, from the viewpoint of preventing the vulcanization reaction from occurring.

[0048] [Rubber Molded Article] The rubber molded article of the present invention is obtained by vulcanizing the above-described rubber composition of the present invention, i.e., the unvulcanized rubber composition. The unvulcanized rubber composition can be molded by a known method and heated or heated and pressurized at preferably 140°C or higher, more preferably 145°C or higher, and preferably 200°C or lower, more preferably 180°C or lower, to form a vulcanized rubber molded article. The contents and preferred ranges of the rubber component, polyester, inorganic filler, and other additives in the rubber molded article of the present invention are the same as those for the rubber composition. Since the rubber molded article of the present invention is obtained by vulcanizing the above-described rubber composition of the present invention, it has excellent abrasion resistance and storage modulus, and can therefore be suitably used as rubber molded articles for tires, tire inner liners, treads, tread bases, carcasses, sidewalls, bead portions, and other tire components, as well as various rubber belts, various seals, vibration-isolating and vibration-damping materials, shoe soles, and other such tire components.

[0049] <Method for manufacturing rubber molded article> The method for manufacturing a rubber molded article of the present invention includes a step of vulcanizing the rubber composition of the present invention described above. Specifically, the step of vulcanizing the rubber composition is a step of molding and processing the rubber composition of the present invention described above into a desired shape, and heating or heating and pressurizing the molded article at 140°C or higher, more preferably 145°C or higher, and preferably 200°C or lower, more preferably 180°C or lower, to obtain a rubber molded article. The contents of the rubber component, polyester, and additives such as inorganic filler in the obtained rubber molded article, and their preferred ranges, are the same as those for the rubber composition.

[0050] [Tire Component] The tire component of the present invention includes the rubber molded article of the present invention described above. Since the tire component of the present invention includes the rubber molded article of the present invention described above, it is excellent in abrasion resistance and storage modulus. Examples of the tire component of the present invention include an inner liner, tread, tread base, carcass, sidewall, bead portion, etc. of a tire.

[0051] [Method for Improving Abrasion Resistance] The method for improving the abrasion resistance of a rubber molded article of the present invention is a method for improving the abrasion resistance of a rubber molded article containing a rubber component and a polyester, wherein the rubber component contains natural rubber, the polyester is a polycondensate of an alcohol component and a carboxylic acid component, the alcohol component contains an aliphatic diol having from 2 to 16 carbon atoms in an amount of 85% by mass or more, and the carboxylic acid component contains an aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms in an amount of 50% by mass or more. In the method for improving abrasion resistance of the present invention, the rubber molded article contains natural rubber as the rubber component and also contains the polyester, which is thought to promote strain-induced crystallization of the rubber molded article, thereby improving the abrasion resistance of the rubber molded article. In the method for improving the abrasion resistance of a rubber molded article of the present invention, the contents and preferred ranges of the rubber component, polyester, inorganic filler, sulfur, and other additives in the rubber molded article are the same as those for the rubber composition.

[0052] The present invention further includes the following aspects: <1> A rubber composition comprising a rubber component and a polyester, wherein the rubber component comprises natural rubber, the polyester is a polycondensate of an alcohol component and a carboxylic acid component, the alcohol component contains an aliphatic diol having from 2 to 16 carbon atoms in a content of 85% by mass or more, and the carboxylic acid component contains an aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms in a content of 50% by mass or more. <2> The rubber composition according to <1>, wherein the mass ratio of the polyester content to the natural rubber content ([polyester content] / [natural rubber content]) is 0.01 or more and 0.20 or less. <3> A rubber composition comprising a rubber component and a polyester, wherein the rubber component comprises natural rubber, the polyester is a polycondensate of an alcohol component and a carboxylic acid component, the alcohol component contains an aliphatic diol having from 2 to 16 carbon atoms in an amount of 85% by mass or more, the carboxylic acid component contains an aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms in an amount of 50% by mass or more, and the mass ratio of the polyester content to the natural rubber content ([polyester content] / [natural rubber content]) is 0.01 or more and 0.20 or less. <4> The rubber composition according to any one of <1> to <3>, wherein the rubber component further contains a synthetic rubber. <5> The rubber composition according to <4>, wherein the mass ratio of the natural rubber content to the synthetic rubber content (natural rubber / synthetic rubber) is 50 / 50 or more. <6> A rubber composition comprising a rubber component and a polyester, wherein the rubber component comprises natural rubber and synthetic rubber, the polyester is a polycondensate of an alcohol component and a carboxylic acid component, the alcohol component contains an aliphatic diol having from 2 to 16 carbon atoms in an amount of 85% by mass or more, the carboxylic acid component contains an aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms in an amount of 50% by mass or more, the mass ratio of the natural rubber to the synthetic rubber (natural rubber / synthetic rubber) is 50 / 50 or more, and the mass ratio of the polyester to the natural rubber ([polyester content] / [natural rubber content]) is 0.01 or more and 0.20 or less. <7> The rubber composition according to any one of <1> to <6>, wherein the aliphatic diol is an α,ω-linear alkanediol having from 2 to 16 carbon atoms.<8> The rubber composition according to any one of <1> to <7>, wherein the aliphatic dicarboxylic acid compound is an α,ω-linear aliphatic dicarboxylic acid having from 2 to 16 carbon atoms, preferably an α,ω-linear aliphatic dicarboxylic acid having from 4 to 14 carbon atoms, more preferably an α,ω-linear aliphatic dicarboxylic acid having from 6 to 14 carbon atoms, and even more preferably an α,ω-linear aliphatic dicarboxylic acid having from 6 to 14 carbon atoms. <9> The rubber composition according to any one of <1> to <8>, wherein the content of the aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms in the carboxylic acid component is 60% by mass or more, preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and still more preferably substantially 100% by mass. <10> The rubber composition according to any one of <1> to <9>, wherein the carbon number of the aliphatic dicarboxylic acid compound is 4 to 14. <11> The rubber composition according to any one of <1> to <10>, wherein the total content of the aliphatic diol having from 2 to 16 carbon atoms and the aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms is 85% by mass or more, preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably substantially 100% by mass, in the raw material monomers for the polyester. <12> The rubber composition according to any one of <1> to <11>, wherein the content of the aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms per 100 mole parts of the aliphatic diol having from 2 to 16 carbon atoms is 75 to 115 mole parts, preferably 85 to 110 mole parts, more preferably 85 to 115 mole parts, even more preferably 85 to 110 mole parts, and still more preferably 85 to 105 mole parts. <13> The rubber composition according to any one of <1> to <12>, wherein the weight average molecular weight of the polyester is 3,000 or more and 100,000 or less, preferably 5,000 or more and 50,000 or less, more preferably 6,000 or more and 40,000 or less, even more preferably 7,000 or more and 35,000 or less, and still more preferably 10,000 or more and 35,000 or less. <14> The rubber composition according to any one of <1> to <13>, wherein the melting point of the polyester is 60°C or more and 150°C or less, preferably 70°C or more and 130°C or less, and more preferably 75°C or more and 120°C or less.<15> The rubber composition according to any one of <4> to <14>, wherein the synthetic rubber is a diene-based synthetic rubber.<16> The rubber composition according to any one of <4> to <15>, wherein the synthetic rubber comprises a diene-based synthetic rubber, preferably one or more selected from polyisoprene rubber (IR), polybutadiene rubber (BR), styrene-butadiene copolymer rubber (SBR), acrylonitrile-butadiene copolymer rubber (NBR), chloroprene rubber (CR), butyl rubber (IIR), and polyisobutylene, and more preferably styrene-butadiene copolymer rubber (SBR).<17> The rubber composition according to any one of <4> to <16>, wherein the mass ratio of the content of the natural rubber to the synthetic rubber (natural rubber / synthetic rubber) is 60 / 40 or more, preferably 80 / 20 or more, and more preferably 90 / 10 or more. <18> The rubber composition according to any one of <1> to <17>, wherein the mass ratio of the polyester content to the natural rubber content ([polyester content] / [natural rubber content]) is 0.02 or more and 0.10 or less, preferably 0.02 or more and 0.05 or less. <19> The rubber composition according to any one of <1> to <18>, further containing an inorganic filler. <20> The rubber composition according to any one of <1> to <19>, further containing process oil, wherein the content of the process oil is 4 parts by mass or more and 16 parts by mass or less per 100 parts by mass of the rubber component. <21> The rubber composition according to any one of <1> to <20>, wherein the content of the polyester is 1.0 part by mass or more and 30 parts by mass or less, preferably 1.2 parts by mass or more and 25 parts by mass or less, more preferably 1.4 parts by mass or more and 20 parts by mass or less, even more preferably 1.4 parts by mass or more and 15 parts by mass or less, and still more preferably 1.4 parts by mass or more and 12 parts by mass or less per 100 parts by mass of the rubber component. <22> The rubber composition according to any one of <1> to <21>, wherein the content of the rubber component in the rubber composition is 30% by mass or more and 80% by mass or less, preferably 35% by mass or more and 75% by mass or less, more preferably 40% by mass or more and 70% by mass or less, and even more preferably 45% by mass or more and 65% by mass or less. <23> A rubber molded article obtained by vulcanizing the rubber composition according to any one of <1> to <22>. <24> A tire component comprising the rubber molded article according to <23>.<25> A method for producing the rubber composition according to any one of <1> to <22>, comprising the following steps (1) and (2): step (1): kneading a composition comprising a rubber component and a polyester, wherein the rubber component comprises natural rubber, the polyester is a polycondensate of an alcohol component and a carboxylic acid component, the alcohol component having an aliphatic diol content of 2 to 16 carbon atoms of 85% by mass or more, and the carboxylic acid component having an aliphatic dicarboxylic acid compound content of 2 to 16 carbon atoms of 50% by mass or more; and step (2): further adding and mixing sulfur. <26> A method for producing a rubber molded product, comprising the step of vulcanizing the rubber composition according to any one of <1> to <22>.

[0053] <27> A method for producing a rubber composition, comprising the following steps (1) and (2): step (1): kneading a composition comprising a rubber component and a polyester, wherein the rubber component contains natural rubber, the polyester is a polycondensate of an alcohol component and a carboxylic acid component, the alcohol component having an aliphatic diol content of 2 to 16 carbon atoms of 85% by mass or more, and the carboxylic acid component having an aliphatic dicarboxylic acid compound content of 2 to 16 carbon atoms of 50% by mass or more; and step (2): further adding and mixing sulfur. <28> A method for producing a rubber composition according to <27>, wherein the mass ratio of the polyester content to the natural rubber content in the composition in step (1) ([polyester content] / [natural rubber content]) is 0.01 or more and 0.20 or less. <29> A method for producing a rubber composition, comprising the following steps (1) and (2): Step (1): kneading a composition comprising a rubber component and a polyester, wherein the rubber component comprises natural rubber, the polyester is a polycondensate of an alcohol component and a carboxylic acid component, the alcohol component having an aliphatic diol with from 2 to 16 carbon atoms in a content of 85% by mass or more, the carboxylic acid component having an aliphatic dicarboxylic acid compound with from 2 to 16 carbon atoms in a content of 50% by mass or more, and the mass ratio of the polyester content to the natural rubber content ([polyester content] / [natural rubber content]) is 0.01 or more and 0.20 or less. Step (2): further adding and mixing sulfur. <30> A method for producing a rubber composition according to any one of <27> to <29>, wherein the rubber component further comprises a synthetic rubber. <31> A method for producing a rubber composition according to <30>, wherein the mass ratio of the natural rubber content to the synthetic rubber content (natural rubber / synthetic rubber) in the composition of step (1) is 50 / 50 or more. <32> A method for producing a rubber composition, comprising the following steps (1) and (2):Step (1): A step of kneading a composition that includes a rubber component and a polyester, wherein the rubber component includes natural rubber, the polyester is a polycondensate of an alcohol component and a carboxylic acid component, the alcohol component contains an aliphatic diol having from 2 to 16 carbon atoms in an amount of 85% by mass or more, the carboxylic acid component contains an aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms in an amount of 50% by mass or more, the mass ratio of the contents of the natural rubber and the synthetic rubber (natural rubber / synthetic rubber) is 50 / 50 or more, and the mass ratio of the content of the polyester to the content of the natural rubber ([content of polyester] / [content of natural rubber]) is 0.01 or more and 0.20 or less. Step (2): A step of further adding and mixing sulfur. <33> A method for producing a rubber composition according to any one of <27> to <32>, wherein the aliphatic diol is an α,ω-linear alkanediol having from 2 to 16 carbon atoms. <34> The method for producing a rubber composition according to any one of <27> to <33>, wherein the aliphatic dicarboxylic acid compound is an α,ω-linear aliphatic dicarboxylic acid having from 2 to 16 carbon atoms, preferably an α,ω-linear aliphatic dicarboxylic acid having from 4 to 14 carbon atoms, more preferably an α,ω-linear aliphatic dicarboxylic acid having from 6 to 14 carbon atoms, and even more preferably an α,ω-linear aliphatic dicarboxylic acid having from 6 to 14 carbon atoms. <35> The method for producing a rubber composition according to any one of <27> to <34>, wherein the content of the aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms in the composition in step (1) is 60% by mass or more, preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and still more preferably substantially 100% by mass, of the carboxylic acid component. <36> The method for producing a rubber composition according to any one of <27> to <35>, wherein the number of carbon atoms in the aliphatic dicarboxylic acid compound is 4 to 14. <37> The method for producing a rubber composition according to any one of <27> to <36>, wherein the total content of the aliphatic diol having from 2 to 16 carbon atoms and the aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms in the composition in step (1) is 85% by mass or more, preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably substantially 100% by mass, based on the raw material monomers for the polyester.<38> The method for producing a rubber composition according to any one of <27> to <37>, wherein the content of the aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms per 100 mole parts of the aliphatic diol having from 2 to 16 carbon atoms in the composition of step (1) is from 75 to 115 mole parts, preferably from 85 to 110 mole parts, more preferably from 85 to 115 mole parts, even more preferably from 85 to 110 mole parts, and still more preferably from 85 to 105 mole parts. <39> The method for producing a rubber composition according to any one of <27> to <38>, wherein the weight average molecular weight of the polyester is from 3,000 to 100,000, preferably from 5,000 to 50,000, more preferably from 6,000 to 40,000, even more preferably from 7,000 to 35,000, and still more preferably from 10,000 to 35,000. <40> A method for producing a rubber composition according to any one of <27> to <39>, wherein the polyester has a melting point of 60°C or higher and 150°C or lower, preferably 70°C or higher and 130°C or lower, and more preferably 75°C or higher and 120°C or lower. <41> A method for producing a rubber composition according to any one of <30> to <40>, wherein the synthetic rubber is a diene-based synthetic rubber. <42> A method for producing a rubber composition according to any one of <30> to <41>, wherein the synthetic rubber comprises a diene-based synthetic rubber, preferably one or more selected from polyisoprene rubber (IR), polybutadiene rubber (BR), styrene-butadiene copolymer rubber (SBR), acrylonitrile-butadiene copolymer rubber (NBR), chloroprene rubber (CR), butyl rubber (IIR), and polyisobutylene, and more preferably styrene-butadiene copolymer rubber (SBR). <43> The method for producing a rubber composition according to any one of <30> to <42>, wherein the mass ratio of the content of the natural rubber to the content of the synthetic rubber in the composition in step (1) (natural rubber / synthetic rubber) is 60 / 40 or more, preferably 80 / 20 or more, and more preferably 90 / 10 or more. <44> The method for producing a rubber composition according to any one of <27> to <43>, wherein the mass ratio of the content of the polyester to the content of the natural rubber in the composition in step (1) ([polyester content] / [natural rubber content]) is 0.02 or more and 0.10 or less, preferably 0.02 or more and 0.05 or less.<45> The method for producing a rubber composition according to any one of <27> to <44>, wherein the composition in step (1) further contains an inorganic filler. <46> The method for producing a rubber composition according to any one of <27> to <45>, wherein the composition in step (1) further contains a process oil, and the content of the process oil is 4 parts by mass or more and 16 parts by mass or less per 100 parts by mass of the rubber component. <47> The method for producing a rubber composition according to any one of <27> to <46>, wherein the content of the polyester in the composition in step (1) is 1.0 part by mass or more and 30 parts by mass or less, preferably 1.2 parts by mass or more and 25 parts by mass or less, more preferably 1.4 parts by mass or more and 20 parts by mass or less, even more preferably 1.4 parts by mass or more and 15 parts by mass or less, and still more preferably 1.4 parts by mass or more and 12 parts by mass or less per 100 parts by mass of the rubber component. <48> The method for producing a rubber composition according to any one of <27> to <47>, wherein the content of the rubber component in the composition of step (1) is 30% by mass or more and 80% by mass or less, preferably 35% by mass or more and 75% by mass or less, more preferably 40% by mass or more and 70% by mass or less, and even more preferably 45% by mass or more and 65% by mass or less. <49> Use of the rubber composition according to any one of <1> to <22> for improving abrasion resistance.

[0054] <50> A method for improving the abrasion resistance of a rubber molded article containing a rubber component and a polyester, wherein the rubber component contains natural rubber, the polyester is a polycondensate of an alcohol component and a carboxylic acid component, the alcohol component contains an aliphatic diol having from 2 to 16 carbon atoms in a content of 85% by mass or more, and the carboxylic acid component contains an aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms in a content of 50% by mass or more. <51> The method for improving the abrasion resistance of a rubber molded article according to <50>, wherein the mass ratio of the polyester content to the natural rubber content in the rubber molded article ([polyester content] / [natural rubber content]) is 0.01 or more and 0.20 or less. <52> A method for improving the abrasion resistance of a rubber molded article containing a rubber component and a polyester, wherein the rubber component contains natural rubber, the polyester is a polycondensate of an alcohol component and a carboxylic acid component, the alcohol component contains an aliphatic diol having from 2 to 16 carbon atoms in a content of 85% by mass or more, the carboxylic acid component contains an aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms in a content of 50% by mass or more, and the mass ratio of the polyester content to the natural rubber content ([polyester content] / [natural rubber content]) is 0.01 or more and 0.20 or less. <53> The method for improving the abrasion resistance of a rubber molded article according to any one of <50> to <52>, wherein the rubber component further contains a synthetic rubber. <54> The method for improving the abrasion resistance of a rubber molded article according to <53>, wherein the mass ratio of the natural rubber content to the synthetic rubber content (natural rubber / synthetic rubber) in the rubber molded article is 50 / 50 or more.<55> A method for improving the abrasion resistance of a rubber molded article containing a rubber component and a polyester, wherein the rubber component contains natural rubber, the polyester is a polycondensate of an alcohol component and a carboxylic acid component, the alcohol component contains an aliphatic diol having from 2 to 16 carbon atoms in an amount of 85% by mass or more, the carboxylic acid component contains an aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms in an amount of 50% by mass or more, the mass ratio of the natural rubber to the synthetic rubber (natural rubber / synthetic rubber) is 50 / 50 or more, and the mass ratio of the polyester to the natural rubber ([polyester content] / [natural rubber content]) is 0.01 or more and 0.20 or less. <56> The method for improving the abrasion resistance of a rubber molded article according to any one of <50> to <55>, wherein the aliphatic diol is an α,ω-linear alkanediol having from 2 to 16 carbon atoms. <57> The method for improving the abrasion resistance of a rubber molded article according to any one of <50> to <56>, wherein the aliphatic dicarboxylic acid compound is an α,ω-linear aliphatic dicarboxylic acid having from 2 to 16 carbon atoms, preferably an α,ω-linear aliphatic dicarboxylic acid having from 4 to 14 carbon atoms, more preferably an α,ω-linear aliphatic dicarboxylic acid having from 6 to 14 carbon atoms, and even more preferably an α,ω-linear aliphatic dicarboxylic acid having from 6 to 14 carbon atoms. <58> The method for improving the abrasion resistance of a rubber molded article according to any one of <50> to <57>, wherein the content of the aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms in the rubber molded article is 60% by mass or more, preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and still more preferably substantially 100% by mass, of the carboxylic acid component. <59> The method for improving the abrasion resistance of a rubber molded article according to any one of <50> to <58>, wherein the number of carbon atoms in the aliphatic dicarboxylic acid compound is 4 to 14. <60> The method for improving the abrasion resistance of a rubber molded body according to any one of <50> to <59>, wherein the total content of the aliphatic diol having from 2 to 16 carbon atoms and the aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms in the rubber molded body is 85% by mass or more, preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably substantially 100% by mass, based on the raw material monomers for the polyester.<61> The method for improving the abrasion resistance of a rubber molded article according to any one of <50> to <60>, wherein the content of the aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms per 100 mole parts of the aliphatic diol having from 2 to 16 carbon atoms in the rubber molded article is from 75 to 115 mole parts, preferably from 85 to 110 mole parts, more preferably from 85 to 115 mole parts, even more preferably from 85 to 110 mole parts, and still more preferably from 85 to 105 mole parts. <62> The method for improving the abrasion resistance of a rubber molded article according to any one of <50> to <61>, wherein the weight-average molecular weight of the polyester is from 3,000 to 100,000, preferably from 5,000 to 50,000, more preferably from 6,000 to 40,000, even more preferably from 7,000 to 35,000, and still more preferably from 10,000 to 35,000. <63> The method for improving the abrasion resistance of a rubber molded article according to any one of <50> to <62>, wherein the melting point of the polyester is 60°C or higher and 150°C or lower, preferably 70°C or higher and 130°C or lower, and more preferably 75°C or higher and 120°C or lower. <64> The method for improving the abrasion resistance of a rubber molded article according to any one of <53> to <63>, wherein the synthetic rubber is a diene-based synthetic rubber. <65> The method for improving the abrasion resistance of a rubber molded article according to any one of <53> to <64>, wherein the synthetic rubber comprises a diene-based synthetic rubber, preferably one or more selected from polyisoprene rubber (IR), polybutadiene rubber (BR), styrene-butadiene copolymer rubber (SBR), acrylonitrile-butadiene copolymer rubber (NBR), chloroprene rubber (CR), butyl rubber (IIR), and polyisobutylene, and more preferably styrene-butadiene copolymer rubber (SBR). <66> The method for improving the abrasion resistance of a rubber molded body according to any one of <53> to <65>, wherein the mass ratio of the natural rubber to the synthetic rubber (natural rubber / synthetic rubber) in the rubber molded body is 60 / 40 or more, preferably 80 / 20 or more, and more preferably 90 / 10 or more.<67> The method for improving the abrasion resistance of a rubber molded body according to any one of <50> to <66>, wherein the mass ratio of the polyester content to the natural rubber content in the composition in step (1) ([polyester content] / [natural rubber content]) is 0.02 or more and 0.10 or less, preferably 0.02 or more and 0.05 or less. <68> The method for improving the abrasion resistance of a rubber molded body according to any one of <50> to <67>, wherein the rubber molded body further contains an inorganic filler. <69> The method for improving the abrasion resistance of a rubber molded body according to any one of <50> to <68>, wherein the rubber molded body further contains process oil, and the content of the process oil per 100 parts by mass of the rubber component is 4 parts by mass or more and 16 parts by mass or less. <70> The method for improving the abrasion resistance of a rubber molded body according to any one of <50> to <69>, wherein the content of the polyester in the rubber molded body is 1.0 part by mass or more and 30 parts by mass or less, preferably 1.2 parts by mass or more and 25 parts by mass or less, more preferably 1.4 parts by mass or more and 20 parts by mass or less, even more preferably 1.4 parts by mass or more and 15 parts by mass or less, and still more preferably 1.4 parts by mass or more and 12 parts by mass or less, per 100 parts by mass of the rubber component. <71> The method for improving the abrasion resistance of a rubber molded body according to any one of <50> to <70>, wherein the content of the rubber component in the rubber molded body is 30% by mass or more and 80% by mass or less, preferably 35% by mass or more and 75% by mass or less, more preferably 40% by mass or more and 70% by mass or less, and even more preferably 45% by mass or more and 65% by mass or less.

[0055] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. Each property value was measured and evaluated by the following methods.

[0056] <Measurement of Melting Point of Polyester and Endothermic Amount ΔH of Melting Endothermic Peak by Differential Scanning Calorimetry (DSC)> 0.02 g of a freeze-dried polyester powder sample was weighed into an aluminum pan, and using a differential scanning calorimeter (manufactured by TA Instruments, product name: Q-100), the sample was cooled from room temperature (20°C) to 0°C at a temperature decrease rate of 10°C / min, allowed to stand for 1 minute, and then heated to 180°C at a temperature increase rate of 10°C / min, while measuring the melting point. The temperature of the highest endothermic peak observed was taken as the melting point of the polyester. The endothermic amount ΔH (J / g) per 1 g of polyester was calculated from the area of ​​the melting endothermic peak.

[0057] <Measurement of SP value of polyester> Calculation was performed based on the Hansen solubility parameter using solubility parameter calculation software (Hansen Solubility Parameters in Practice 4th Edition 4.1.03). In calculating the SP value, the specific gravity of the polyester was set to 1.0.

[0058] <Measurement of Weight-Average Molecular Weight of Polyester> The molecular weight distribution was measured by the following gel permeation chromatography (GPC) method, and the weight-average molecular weight (Mw) of the polyester was determined. (1) The polymer was dissolved in chloroform so that the concentration of the sample solution prepared was 0.5 g / 100 mL. Next, this solution was filtered using a fluororesin filter (manufactured by Sumitomo Electric Industries, Ltd., product name: FP-200) with a pore size of 2 μm to remove insoluble components, and a sample solution was obtained. (2) Using a molecular weight measuring device (manufactured by Tosoh Corporation, product name: CO-8010, analytical column: GMHXL+G3000HXL), chloroform was passed as the eluent at a flow rate of 1 ml per minute, and the column was stabilized in a thermostatic bath at 40°C. 100 μL of the sample solution was injected therein and measurement was performed. The molecular weight of the sample was calculated based on a calibration curve prepared in advance. The calibration curve used here was a mixture of several types of monodisperse polystyrene (monodisperse polystyrene manufactured by Tosoh Corporation; 2.63 × 10 3 , 2.06 × 10 4 , 1.02 × 10 5, monodisperse polystyrene manufactured by GL Sciences Inc.; 2.10 × 10 3 , 7.00 x 10 3 , 5.04 × 10 4 (number average molecular weight)) was prepared and used as a standard sample.

[0059] Production Examples 1 to 5 (Production of Polyesters A to D and M) The raw material monomers shown in Table 1 and 20 g of tin(II) 2-ethylhexanoate were placed in a 10 L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple, and the mixture was maintained at 140°C for 6 hours, then heated to 200°C over 6 hours, reacted at 200°C for 1 hour, and then reacted at 8.3 kPa for 1 hour to obtain polyesters A to D and M. The results are shown in Table 1.

[0060] Details of each component shown in Table 1 are as follows: [Alcohol components] EG: Ethylene glycol 1,2-PD: 1,2-propanediol 1,4-BD: 1,4-butanediol 1,10-DD: 1,10-decanediol 1,12-DD: 1,12-dodecanediol [Carboxylic acid components] Succinic acid Sebacic acid DDA: Dodecanedioic acid TPA: Terephthalic acid TMA: Trimellitic acid

[0061]

[0062] Examples 1 to 9, Comparative Examples 1 to 6, and Reference Examples 1 to 4 The raw material components shown in Tables 2 to 5 were prepared, and the components excluding zinc oxide, sulfur, and vulcanization accelerators 1 and 2 were kneaded in accordance with the formulations shown in Tables 2 to 5 using a Banbury mixer at a maximum temperature of 150°C for 4 minutes. Next, zinc oxide, sulfur, and vulcanization accelerator 1 or 2 were added, and the mixture was kneaded at a maximum temperature of 110°C for 2 minutes to obtain an unvulcanized rubber composition. The obtained unvulcanized rubber composition was heated at 160°C for 30 minutes to obtain a sheet-shaped vulcanized rubber molding. The thickness of the sheet-shaped vulcanized rubber molding was 2 mm.

[0063] Details of each component shown in Tables 2 to 5 are as follows. [Rubber components] NR: RSS#3 SBR1: Solution-polymerized SBR manufactured by JSR Corporation, trade name: HPR850, styrene content: 27.5 mass% SBR2: Emulsion-polymerized SBR manufactured by Nippon Zeon Co., Ltd., trade name: NIPOL1502, styrene content: 23.5 mass% [Polyesters] Polyesters A to D and M obtained in Production Examples 1 to 5 [Inorganic fillers] Silica: Product name: Nipsil AQ manufactured by Tosoh Silica Corporation, BET specific surface area: 205 m 2 / g Carbon black: Furnace black manufactured by Beilum Carbon Chemical Co., Ltd., trade name: N234, DBP absorption: 125 cm 3 / 100g, N 2 AS: 117m 2 / g [Other additives] Silane coupling agent: Evonik, trade name: Si75 Process oil: naphthenic process oil, Japan Sun Oil Co., Ltd., trade name: SUNTHENE 410 Stearic acid: Kao Corporation, trade name: Lunac S-70V Antiaging agent: N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, Ouchi Shinko Chemical Industry Co., Ltd., trade name: Nocrac 6C Zinc oxide: Fujifilm Wako Pure Chemical Industries, Ltd., reagent, zinc oxide (primary grade) Sulfur: Fujifilm Wako Pure Chemical Industries, Ltd., reagent, sulfur (powder, chemical grade) Vulcanization accelerator 1: sulfenamide-based vulcanization accelerator N-tert-butyl-2-benzothiazylsulfenamide (TBBS), Sanshin Chemical Industry Co., Ltd., "Suncerer NS" Vulcanization accelerator 2: sulfenamide vulcanization accelerator, N-cyclohexyl-2-benzothiazolylsulfenamide, manufactured by Ouchi Shinko Chemical Industry Co., Ltd., product name: Noccela CZ-G

[0064] <Evaluation of Abrasion Resistance> Test specimens with a 50 mm diameter, 10 mm thick hole the size of a dedicated mandrel were prepared from the obtained sheet-like vulcanized rubber molding. Using an FPS abrasion tester (AB-2012) manufactured by Ueshima Seisakusho, the FPS abrasion volume was measured under the following conditions: a METABRIT (grain size 240, abrasive grain A) manufactured by Noritake Coated Abrasives Co., Ltd. as the abrasion surface; a sample speed of 80 m / min; a load of 40 N; a talc feeder speed of 0.4 rpm; a set temperature of 35°C; and a slip ratio of 10%. The measurement results are shown in Tables 2 to 5. Table 2 shows the FPS abrasion volume of Reference Example 1; Table 3 shows the FPS abrasion volume of Reference Example 2; Table 4 shows the FPS abrasion volume of Reference Example 3; and Table 5 shows the FPS abrasion volume of Reference Example 4, all of which are relative values, with the FPS abrasion volume being set to 100. A smaller relative value of the FPS abrasion volume indicates a smaller abrasion volume and better abrasion resistance.

[0065] <Evaluation of Storage Modulus (G')> Using a viscoelasticity measuring device (ARES-G2, manufactured by TA Instruments), the storage modulus (G') of the obtained sheet-shaped vulcanized rubber moldings was measured under conditions of a temperature of 50°C, a dynamic strain of 5%, and a frequency of 10 Hz. The measurement results are shown in Tables 2 to 5. With regard to the measured storage moduli, Table 2 shows the storage modulus (G') of Reference Example 1, Table 3 shows the storage modulus (G') of Reference Example 2, Table 4 shows the storage modulus (G') of Reference Example 3, and Table 5 shows the storage modulus (G') of Reference Example 4, all relative values ​​being set to 100. A larger relative value of the storage modulus (G') indicates a larger storage modulus, which in turn indicates higher block rigidity when used in tires and the like, and superior vehicle handling stability when used in tire components.

[0066] <Evaluation of Loss Tangent (tan δ)> Using a viscoelasticity measuring device (ARES-G2, manufactured by TA Instruments), the loss tangent (tan δ) of the obtained sheet-shaped vulcanized rubber moldings was measured under conditions of a temperature of 50°C, a dynamic strain of 5%, and a frequency of 10 Hz. The measurement results are shown in Tables 2 to 5. With regard to the measured loss tangent (tan δ), Table 2 shows the loss tangent (tan δ) of Reference Example 1, Table 3 shows the loss tangent (tan δ) of Reference Example 2, Table 4 shows the loss tangent (tan δ) of Reference Example 3, and Table 5 shows the loss tangent (tan δ) of Reference Example 4, all of which are taken as 100. The smaller the relative value of the loss tangent (tan δ), the smaller the rolling resistance of the tire when used in a tire component, and the smaller the heat buildup and the more excellent the fuel economy.

[0067]

[0068]

[0069]

[0070]

[0071] Tables 2 to 5 confirm that the rubber molded articles obtained in Examples 1 to 9 of the present invention have superior abrasion resistance and a higher storage modulus than the rubber molded articles obtained in Comparative Examples 1 to 6. It can also be confirmed that the rubber molded articles obtained in Examples 1 to 5 have a reduced loss tangent compared to the rubber molded article obtained in Comparative Example 1. Furthermore, a comparison of Reference Example 1 with Comparative Examples 3 to 6 confirms that Comparative Examples 3 to 6, which contain polyester but no natural rubber, have lower abrasion resistance than Reference Example 1, which contains neither natural rubber nor polyester. This confirms that even when the rubber composition and rubber molded article contain polyester, those that do not contain natural rubber as a rubber component cannot improve abrasion resistance.

[0072] According to the present invention, it is possible to provide a rubber composition having excellent abrasion resistance and a high storage modulus, a rubber molded article using the same, a tire component, and a method for improving the abrasion resistance of a rubber composition. The obtained rubber molded article is particularly suitable for use in various tires for passenger cars, small and medium trucks, and large vehicles (large trucks, buses, construction vehicles, etc.), tire components such as tire treads, various rubber belts, various sealing materials, vibration-isolating and vibration-damping materials, shoe soles, etc.

Claims

1. A rubber composition comprising a rubber component and a polyester, wherein the rubber component comprises natural rubber, the polyester is a polycondensate of an alcohol component and a carboxylic acid component, the alcohol component contains an aliphatic diol having 2 to 16 carbon atoms in an amount of 85 mass% or more, and the carboxylic acid component contains an aliphatic dicarboxylic acid compound having 2 to 16 carbon atoms in an amount of 50 mass% or more.

2. The rubber composition according to claim 1, wherein the aliphatic diol is an α,ω-straight-chain alkanediol having from 2 to 16 carbon atoms.

3. The rubber composition according to claim 1 or 2, wherein the aliphatic dicarboxylic acid compound is an α,ω-straight-chain aliphatic dicarboxylic acid having from 2 to 16 carbon atoms.

4. The rubber composition according to any one of claims 1 to 3, wherein the weight average molecular weight of the polyester is 3,000 or more and 100,000 or less.

5. A rubber composition according to any one of claims 1 to 4, wherein the melting point of the polyester is 60°C or higher and 150°C or lower.

6. The rubber composition according to any one of claims 1 to 5, wherein the rubber component further contains a synthetic rubber.

7. The rubber composition according to claim 6, wherein the synthetic rubber is a diene-based synthetic rubber.

8. The rubber composition according to claim 6 or 7, wherein the mass ratio of the content of the natural rubber to the content of the synthetic rubber (natural rubber / synthetic rubber) is 50 / 50 or more.

9. The rubber composition according to any one of claims 1 to 8, further comprising an inorganic filler.

10. The rubber composition according to any one of claims 1 to 9, further comprising a process oil, the content of the process oil being 4 parts by mass or more and 16 parts by mass or less per 100 parts by mass of the rubber component.

11. The rubber composition according to any one of claims 1 to 10, wherein the content of the polyester is 1.0 part by mass or more and 30 parts by mass or less per 100 parts by mass of the rubber component.

12. A rubber composition according to any one of claims 1 to 11, wherein the mass ratio of the polyester content to the natural rubber content ([polyester content] / [natural rubber content]) is 0.01 or more and 0.20 or less.

13. A rubber molded article obtained by vulcanizing the rubber composition according to any one of claims 1 to 12.

14. A tire component comprising the rubber molding according to claim 13.

15. A method for producing a rubber composition according to any one of claims 1 to 12, comprising the following steps (1) and (2): step (1): kneading a composition comprising a rubber component and a polyester, wherein the rubber component comprises natural rubber, the polyester is a polycondensate of an alcohol component and a carboxylic acid component, the alcohol component contains an aliphatic diol having from 2 to 16 carbon atoms in an amount of 85 mass% or more, and the carboxylic acid component contains an aliphatic dicarboxylic acid compound having from 2 to 16 carbon atoms in an amount of 50 mass% or more; and step (2): further adding and mixing sulfur.

16. A method for producing a rubber molded article, comprising a step of vulcanizing the rubber composition according to any one of claims 1 to 12.

17. Use of the rubber composition according to any one of claims 1 to 12 as an abrasion resistance improver.

18. A method for improving the abrasion resistance of a rubber molded body containing a rubber component and a polyester, wherein the rubber component contains natural rubber, the polyester is a polycondensate of an alcohol component and a carboxylic acid component, the alcohol component contains an aliphatic diol having 2 to 16 carbon atoms inclusively being 85% by mass or more, and the carboxylic acid component contains an aliphatic dicarboxylic acid compound having 2 to 16 carbon atoms inclusively being 50% by mass or more.

Citation Information

Patent Citations

  • Rubber composition

    JP2012136586A

  • Rubber composition and tire

    JP2020094113A

  • Rubber composition and pneumatic tire using the same

    JP2007039585A

  • Additive for rubber

    WO2021193795A1