Pellets and method for producing same

The use of pellets with a fibrous filler dispersed in liquid crystal polyester addresses gas generation issues in high-temperature environments by allowing gas volatilization during molding, improving the quality of molded products by minimizing gas formation.

WO2024247702A1PCT designated stage expired Publication Date: 2024-12-05SUMITOMO CHEM CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017701
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-05-13
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional liquid crystal polyester compositions experience gas generation, particularly high boiling point components, in high-temperature environments, which affects the quality of molded products.

Method used

The development of pellets containing liquid crystal polyester and a fibrous filler, where the fibrous filler is sufficiently dispersed and exposed, reducing gas generation by allowing volatilization of gas components during molding, and the use of a specific content ratio and distribution of fibrous filler to minimize gas formation.

Benefits of technology

The approach effectively suppresses gas generation in high-temperature environments, enhancing the quality of molded articles by ensuring that gas components are removed during the molding process, thereby reducing the amount of gas produced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The present invention provides pellets which each contain a liquid crystal polyester and a fibrous filler (A). The ratio (N1 / C1) of the number N1 ( / mm2) of spots per unit area, the spots being derived from the fibrous filler (A), observed in a cross-section of each pellet, the cross-section being perpendicular to the extrusion direction, to the content ratio C1 of the fibrous filler (A) is 3,500 to 20,000 inclusive.
Need to check novelty before this filing date? Find Prior Art

Description

Pellets and their manufacturing method

[0001] The present disclosure relates to pellets and methods for making same.

[0002] Liquid crystal polyesters are used in a variety of applications due to their high fluidity, heat resistance and dimensional accuracy.

[0003] Liquid crystal polyesters are usually used as liquid crystal polyester compositions containing fillers and the like to satisfy required properties depending on the application. For example, Patent Document 1 describes a liquid crystal polyester composition containing glass fibers having a non-circular cross-sectional shape.

[0004] Japanese Patent Application Laid-Open No. 2008-013703

[0005] However, conventional liquid crystal polyester compositions have a problem in that a small amount of gas is generated from the surface of the molded article in a high temperature environment.

[0006] An object of the present disclosure is to provide pellets containing a liquid crystalline polyester that can be used to form a molded article in which gas generation (particularly high-boiling point components) is suppressed under high-temperature conditions. Another object of the present disclosure is to provide a method for producing the pellets.

[0007] The present disclosure provides, for example, the following: [1] A pellet containing a liquid crystal polyester and a fibrous filler (A), wherein the content ratio C of the fibrous filler (A) is 1 The number N of spots per unit area derived from the fibrous filler (A) observed in a cross section perpendicular to the extrusion direction of the pellet 1 ( / mm 2 ) ratio (N 1 / C 1 [2] The content ratio C of the fibrous filler (A) is 3,500 or more and 20,000 or less. 1The pellet according to [1], wherein the average circle-equivalent diameter of the spots is 0.05 or more and 0.40 or less. [3] The pellet according to [1] or [2], wherein the average circle-equivalent diameter of the spots is 9 μm or more and 13 μm or less. [4] The pellet according to any one of [1] to [3], wherein the fibrous filler (A) contains glass fiber. [5] The pellet according to any one of [1] to [4], wherein the liquid crystal polyester contains a monomer unit derived from an aromatic hydroxycarboxylic acid. [6] The pellet according to [5], wherein the content of the monomer unit is 50 mol % or more with respect to the total of all monomer units constituting the liquid crystal polyester. [7] The method includes a step of melt-kneading and molding a liquid crystal polyester and a fibrous filler to obtain pellets, wherein the step is carried out by melt-kneading and molding a liquid crystal polyester and a fibrous filler to obtain pellets, and the content ratio C of the fibrous filler (A) in the pellets is 0.05 or more and 0.40 or less. 1 The number N of spots per unit area derived from the fibrous filler (A) observed in a cross section perpendicular to the extrusion direction of the pellet 1 ( / mm 2 ) ratio (N 1 / C 1 The method for producing pellets is a step of performing the melt-kneading and the molding so that the molecular weight distribution of the polymer is 3,500 or more and 20,000 or less.

[0008] According to the present disclosure, it is possible to provide pellets containing a liquid crystalline polyester capable of forming a molded article in which generation of gas (particularly high-boiling point components) in a high-temperature environment is suppressed. Furthermore, according to the present disclosure, it is possible to provide a method for producing the pellets.

[0009] Preferred embodiments of the present disclosure will be described in detail below.

[0010] The pellets of this embodiment (hereinafter also simply referred to as "pellets") contain a liquid crystal polyester and a fibrous filler (A). In this embodiment, the content ratio C of the fibrous filler (A) 1 The number N of spots per unit area derived from the fibrous filler (A) observed in a cross section perpendicular to the extrusion direction of the pellet 1 ( / mm 2 ) ratio (N 1 / C 1) is 3,500 or more and 20,000 or less. In this specification, the content ratio C 1 can be said to be the ratio of the total mass of the fibrous filler (A) to the total mass of the pellets.

[0011] The pellets of this embodiment can form a molded article in which generation of gas (particularly high boiling point components) in a high temperature environment is suppressed.

[0012] The reason why such an effect is exhibited is considered as follows: The fibrous filler aggregated in the pellet is observed as a single spot on the cross section of the pellet. 1 / C 1 A larger ratio (N) means that the fibrous filler is more open and dispersed in the pellet. 1 / C 1 A smaller ratio (N) means that the fibrous filler is more aggregated in the pellet. 1 / C 1 ) is sufficiently large, and it can be said that the fibrous filler is sufficiently spread in the pellets. In the pellets of this embodiment, the fibrous filler is sufficiently spread, so that the ends of the fibrous filler are easily exposed to the surface of the molded article. With the ends of the fibrous filler exposed, gas components (especially high-boiling-point components) inside the molded article are easily volatilized by heating during molding and discharged to the outside of the molded article. In other words, it is thought that the molded article formed from the pellets of this embodiment has components that cause gas generation removed in advance by heating during molding, and therefore generates less gas in a high-temperature environment. Furthermore, it can be said that the pellets of this embodiment are such that the sizing agent contained in the fiber bundles of the fibrous filler is sufficiently thermally decomposed during pellet production, so that the fibers are loosened and well dispersed in the resin. Therefore, in the pellets of this embodiment, gas generation from the remaining sizing agent is suppressed.

[0013] Each component contained in the pellets will be described in detail below.

[0014] (1) Liquid Crystalline Polyester The liquid crystal polyester may be any polyester that exhibits liquid crystallinity in a molten state. The pellets may contain only one type of liquid crystal polyester, or two or more types.

[0015] The flow initiation temperature of the liquid crystal polyester may be 250° C. or higher, or 270° C. or higher. The flow initiation temperature of the liquid crystal polyester may be 400° C. or lower, 360° C. or lower, or 340° C. or lower. That is, the flow initiation temperature of the liquid crystal polyester may be, for example, 250° C. or higher and 400° C. or lower, 250° C. or higher and 360° C. or lower, 250° C. or higher and 340° C. or lower, 270° C. or higher and 400° C. or lower, 270° C. or higher and 360° C. or lower, or 270° C. or higher and 340° C. or lower.

[0016] In this specification, the flow initiation temperature of the liquid crystal polyester is measured using a flow tester, and the liquid crystal polyester is subjected to a pressure of 9.8 MPa (100 kg / cm 2 The liquid crystalline polyester is melted while being heated at a rate of 4°C / min under a load of 1000 kJ / min, and the molten liquid crystalline polyester is extruded from a nozzle having an inner diameter of 1 mm and a length of 10 mm, and the temperature is the temperature at which the viscosity of the extruded liquid crystalline polyester is 4800 Pa·s (48,000 poise).

[0017] The liquid crystal polyester has constituent units (also referred to as monomer units) derived from raw material monomers. The liquid crystal polyester may have a main monomer unit (for example, 90 mol% or more, 95 mol% or more, or 99 mol% or more of the monomer units relative to the total of all monomer units, preferably all monomer units) derived from an aromatic compound. A liquid crystal polyester in which all monomer units are derived from an aromatic compound is also referred to as a wholly aromatic liquid crystal polyester.

[0018] Typical examples of liquid crystal polyesters include polymers having monomer units derived from aromatic hydroxycarboxylic acids (preferably polymers having two or more types of monomer units derived from aromatic hydroxycarboxylic acids), polymers having monomer units derived from aromatic dicarboxylic acids and monomer units derived from aromatic diols, and polymers having monomer units derived from aromatic hydroxycarboxylic acids, monomer units derived from aromatic dicarboxylic acids and monomer units derived from aromatic diols.

[0019] Examples of the monomer unit derived from an aromatic hydroxycarboxylic acid include a monomer unit represented by the following formula (I): Examples of the monomer unit derived from an aromatic dicarboxylic acid include a monomer unit represented by the following formula (II): Examples of the monomer unit derived from an aromatic diol include a monomer unit represented by the following formula (III) (wherein X and Y are oxygen atoms):

[0020] In this specification, "derived" means that in the monomer units of the liquid crystal polyester formed by polymerization of the raw material monomers, the chemical structure of the functional group that contributes to polymerization of the raw material monomers has changed, but other structural changes have not occurred. Here, "derived" is a concept that also includes cases where the monomer unit is derived from a polymerizable derivative of the raw material monomer (for example, a compound obtained by converting the functional group that contributes to polymerization of the raw material monomers into another polymerizable group).

[0021] The liquid crystal polyester may have a monomer unit represented by the following formula (I) (hereinafter also referred to as "monomer unit (I)"). In this specification, CO in the formula represents a carbonyl group. 1 -CO- (I) [wherein, Ar 1 represents a phenylene group, a naphthylene group, or a biphenylylene group. 1 Some or all of the hydrogen atoms in the group represented by the formula (I) may be substituted with a halogen atom, an alkyl group, or an aryl group.

[0022] The liquid crystal polyester may further have a monomer unit represented by the following formula (II) (hereinafter also referred to as "monomer unit (II)") and / or a monomer unit represented by the following formula (III) (hereinafter also referred to as "monomer unit (III)"). 2 -CO- (II) -X-Ar 3 -Y- (III) [wherein, Ar 2 and Ar 3 each independently represents a phenylene group, a naphthylene group, a biphenylylene group, or a group represented by the following formula (IV): X and Y each independently represent an oxygen atom or an imino group (—NH—). 2 Some or all of the hydrogen atoms of the group represented by Ar may be substituted with a halogen atom, an alkyl group or an aryl group. 3 Some or all of the hydrogen atoms of the group represented by the formula (I) may be substituted with a halogen atom, an alkyl group or an aryl group. 4 -Z-Ar 5 - (IV) [wherein, Ar 4 and Ar 5 each independently represents a phenylene group or a naphthylene group, and Z represents an oxygen atom, a sulfur atom, a carbonyl group, a sulfonyl group, or an alkanediyl group.

[0023] Ar 1 , Ar 2 or Ar 3 Examples of halogen atoms that can substitute for hydrogen atoms in include fluorine, chlorine, bromine and iodine atoms.

[0024] Ar 1 , Ar 2 or Ar 3 The alkyl group that can substitute for a hydrogen atom in may be linear, branched, or cyclic. The alkyl group may be, for example, an alkyl group having 1 to 10 carbon atoms. Examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, an s-butyl group, a t-butyl group, an n-hexyl group, a 2-ethylhexyl group, an n-octyl group, and an n-decyl group.

[0025] Ar1 , Ar 2 or Ar 3 The aryl group capable of substituting a hydrogen atom in may be a single ring or a condensed ring. The aryl group may be, for example, an aryl group having 6 to 20 carbon atoms. Examples of the aryl group include a phenyl group, an o-tolyl group, an m-tolyl group, a p-tolyl group, a 1-naphthyl group, and a 2-naphthyl group. The aryl group may be a group in which a hydrogen atom in an aromatic ring is substituted with an alkyl group, such as a tolyl group.

[0026] Ar 1 , Ar 2 or Ar 3 When a hydrogen atom of is substituted with the above-mentioned group, the number of substitutions may be one or two, or may be one.

[0027] The alkanediyl group in Z may be linear or branched. The alkanediyl group may be an alkanediyl group having 1 to 10 carbon atoms. Examples of the alkanediyl group include a methylene group, an ethanediyl group, a propanediyl group (e.g., a propane-2,2-diyl group), a butanediyl group, and an octanediyl group (e.g., an octane-3,3-diyl group).

[0028] The monomer unit (I) can be, for example, Ar 1 is a phenylene group, 1 is a naphthylene group or a monomer unit Ar 1 may be a monomer unit in which Ar is a biphenylylene group; 1 is a phenylene group or a monomer unit Ar 1 may be a monomer unit in which Ar is a naphthylene group, 1 is a 1,4-phenylene group or a monomer unit Ar 1 The liquid crystal polyester may have one or more kinds of monomer units (I).

[0029] The monomer unit (II) is, for example, Ar 2 is a phenylene group, 2 is a naphthylene group, 2is a biphenylylene group, or Ar 2 is a diphenylether-diyl group, and Ar 2 is a phenylene group, 2 is a naphthylene group, or Ar 2 may be a monomer unit in which Ar is a biphenylylene group, 2 is a phenylene group, or Ar 2 may be a monomer unit in which the monomer unit (II) is a naphthylene group. The phenylene group may be a 1,4-phenylene group or a 1,3-phenylene group. The naphthylene group may be a 2,6-naphthylene group or a 2,7-naphthylene group. The biphenylylene group may be a 4,4'-biphenylylene group. The diphenylether-diyl group may be a diphenylether-4,4'-diyl group. The liquid crystal polyester may have one or more types of monomer units (II).

[0030] The monomer unit (II) is, for example, Ar 2 is a 1,4-phenylene group, 2 is a 1,3-phenylene group, 2 is a 2,6-naphthylene group, 2 is a 2,7-naphthylene group, 2 is a 4,4'-biphenylylene group, or Ar 2 is a diphenylether-4,4'-diyl group, and Ar 2 is a 1,4-phenylene group, 2 is a 1,3-phenylene group, or Ar 2 may be a monomer unit in which the aryl group is a 2,6-naphthylene group.

[0031] The monomer unit (III) is, for example, Ar 3 is a phenylene group, 3 is a naphthylene group, or Ar 3 may be a monomer unit in which Ar is a biphenylylene group; 3 is a phenylene group, or Ar3 may be a monomer unit in which Ar is a biphenylylene group, 3 is a 1,4-phenylene group, or Ar 3 The liquid crystal polyester may have one or more kinds of monomer units (III).

[0032] The monomer unit (III) may be a monomer unit (III) in which X and Y are each an oxygen atom.

[0033] The monomer unit (I) may be a monomer unit represented by the following formula (Ia) (hereinafter also referred to as "monomer unit (Ia)"), the monomer unit (II) may be a monomer unit represented by the following formula (IIa) (hereinafter also referred to as "monomer unit (IIa)"), and the monomer unit (III) may be a monomer unit represented by the following formula (IIIa) (hereinafter also referred to as "monomer unit (IIIa)"): 11 -CO- (Ia) -CO-Ar 12 -CO- (IIa) -O-Ar 13 -O- (IIIa) [wherein, Ar 11 represents a 1,4-phenylene group or a 2,6-naphthylene group. 12 represents a 1,4-phenylene group, a 1,3-phenylene group, a 2,6-naphthylene group, a 2,7-naphthylene group, a 4,4'-biphenylylene group, or a diphenylether-4,4'-diyl group. 13 represents a 1,4-phenylene group or a 4,4'-biphenylylene group. 11 , Ar 12 or Ar 13 Some or all of the hydrogen atoms in the group represented by the formula (I) may be independently substituted with a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an aryl group having 6 to 20 carbon atoms.]

[0034] The liquid crystal polyester may be, for example, a polymer having the monomer unit (Ia), a polymer having the monomer unit (Ia) and the monomer unit (IIa), or a polymer having the monomer unit (Ia), the monomer unit (IIa), and the monomer unit (IIIa).

[0035] The liquid crystal polyester preferably has a monomer unit derived from an aromatic hydroxycarboxylic acid (hereinafter also referred to as "monomer unit A"). The majority of the monomer units (e.g., 50 mol % or more) may be monomer unit A, or all of the monomer units may be monomer unit A.

[0036] The liquid crystal polyester may have, as the monomer unit A, at least one monomer unit selected from the group consisting of a monomer unit derived from p-hydroxybenzoic acid and a monomer unit derived from 2-hydroxy-6-naphthoic acid.

[0037] The number of monomer units A in the liquid crystal polyester having monomer units A may be 20 mol% or more, 30 mol% or more, 40 mol% or more, 50 mol% or more, 55 mol% or more, or 60 mol% or more, relative to the total of all monomer units of the liquid crystal polyester. Furthermore, the number of monomer units A in the liquid crystal polyester having monomer units A may be 100 mol% or less, 95 mol% or less, 90 mol% or less, 85 mol% or less, or 80 mol% or less, relative to the total of all monomer units of the liquid crystal polyester. That is, the number of the monomer units A in the liquid crystal polyester having the monomer units A is, for example, 20 mol% or more and 100 mol% or less, 20 mol% or more and 95 mol% or less, 20 mol% or more and 90 mol% or less, 20 mol% or more and 85 mol% or less, 20 mol% or more and 80 mol% or less, 30 mol% or more and 100 mol% or less, 30 mol% or more and 95 mol% or less, 30 mol% or more and 90 mol% or less, 30 mol% or more and 85 mol% or less, 30 mol% or more and 80 mol% or less, 40 mol% or more and 100 mol% or less, 40 mol% or more and 95 mol% or less, 40 mol% or more and 90 mol% or less, 40 mol% or more and 90 mol% or less, 40 mol% or more and 85 mol% or less, 40 mol% or more and 80 mol% or less, 50 mol% or more and 100 mol% or less, 50 mol% or more and 95 mol% or less, 50 mol% or more and 90 mol% or less, 50 mol% or more and 85 mol% or less, 50 mol% or more and 80 mol% or less, 55 mol% or more and 100 mol% or less, 55 mol% or more and 95 mol% or less, 55 mol% or more and 90 mol% or less, 55 mol% or more and 85 mol% or less, 55 mol% or more and 80 mol% or less, 60 mol% or more and 100 mol% or less, 60 mol% or more and 95 mol% or less, 60 mol% or more and 90 mol% or less, 60 mol% or more and 85 mol% or less, or 60 mol% or more and 80 mol% or less.

[0038] When the liquid crystal polyester is a polymer having two or more kinds of monomer units (I), at least one Ar of the monomer units (I) 1 When the liquid crystal polyester is a polymer having the monomer unit (I) and the monomer unit (II), Ar of the monomer unit (I) may be a naphthylene group. 1 and Ar of the monomer unit (II)2 When the liquid crystal polyester is a polymer having the monomer unit (I), the monomer unit (II), and the monomer unit (III), at least one of Ar of the monomer unit (I) may be a naphthylene group. 1 , Ar of the monomer unit (II) 2 and Ar of the monomer unit (III) 3 At least one of the groups may be a naphthylene group.

[0039] When the liquid crystal polyester has the monomer unit (I), the monomer unit (II) and the monomer unit (III), the number of the monomer unit (I) may be, for example, 30 mol% or more, 40 mol% or more, 45 mol% or more, 50 mol% or more, or 55 mol% or more, based on the total of all the monomer units of the liquid crystal polyester. Also, when the liquid crystal polyester has the monomer unit (I), the monomer unit (II) and the monomer unit (III), the number of the monomer unit (I) may be, for example, 80% or less, or 70% or less, based on the total of all the monomer units of the liquid crystal polyester. That is, when the liquid crystal polyester has the monomer unit (I), the monomer unit (II), and the monomer unit (III), the number of the monomer unit (I) may be, for example, 30 mol% or more and 80 mol% or less, 30 mol% or more and 70 mol% or less, 40 mol% or more and 80 mol% or less, 40 mol% or more and 70 mol% or less, 45 mol% or more and 80 mol% or less, 45 mol% or more and 70 mol% or less, 50 mol% or more and 80 mol% or less, 50 mol% or more and 70 mol% or less, 55 mol% or more and 80 mol% or less, or 55 mol% or more and 70 mol% or less, based on the total of all the monomer units of the liquid crystal polyester.

[0040] When the liquid crystal polyester has the monomer unit (I), the monomer unit (II) and the monomer unit (III), the number of the monomer unit (II) may be, for example, 35 mol% or less, or 30 mol% or less, based on the total of all the monomer units of the liquid crystal polyester. Also, when the liquid crystal polyester has the monomer unit (I), the monomer unit (II) and the monomer unit (III), the number of the monomer unit (II) may be, for example, 5 mol% or more, 10 mol% or more, or 15 mol% or more, based on the total of all the monomer units of the liquid crystal polyester. That is, when the liquid crystal polyester has the monomer unit (I), the monomer unit (II), and the monomer unit (III), the number of the monomer unit (II) may be, for example, 5 mol% or more and 35 mol% or less, 5 mol% or more and 30 mol% or less, 10 mol% or more and 35 mol% or less, 10 mol% or more and 30 mol% or less, 15 mol% or more and 35 mol% or less, or 15 mol% or more and 30 mol% or less, relative to the total of all the monomer units of the liquid crystal polyester.

[0041] When the liquid crystal polyester has the monomer unit (I), the monomer unit (II) and the monomer unit (III), the number of the monomer unit (III) may be, for example, 35 mol% or less, or 30 mol% or less, based on the total of all the monomer units of the liquid crystal polyester. Also, when the liquid crystal polyester has the monomer unit (I), the monomer unit (II) and the monomer unit (III), the number of the monomer unit (III) may be, for example, 5 mol% or more, 10 mol% or more, or 15 mol% or more, based on the total of all the monomer units of the liquid crystal polyester. That is, when the liquid crystal polyester has the monomer unit (I), the monomer unit (II), and the monomer unit (III), the number of the monomer unit (III) may be, for example, 5 mol% or more and 35 mol% or less, 5 mol% or more and 30 mol% or less, 10 mol% or more and 35 mol% or less, 10 mol% or more and 30 mol% or less, 15 mol% or more and 35 mol% or less, or 15 mol% or more and 30 mol% or less, relative to the total of all the monomer units of the liquid crystal polyester.

[0042] When the liquid crystal polyester has the monomer unit (I), the monomer unit (II), and the monomer unit (III), the ratio of the number of the monomer units (II) to the number of the monomer units (III) ([number of the monomer units (II)] / [number of the monomer units (III)]) may be 0.9 / 1 to 1 / 0.9, 0.95 / 1 to 1 / 0.95, or 0.98 / 1 to 1 / 0.98.

[0043] The liquid crystal polyester may have monomer units other than the monomer unit (I), the monomer unit (II) and the monomer unit (III), but the number of such monomer units is preferably 10% or less, more preferably 5% or less, even more preferably 2% or less, still more preferably 1% or less, and particularly preferably 0%, based on the total number of all monomer units of the liquid crystal polyester.

[0044] In this specification, the number of each monomer unit contained in the liquid crystal polyester is determined by the analytical method described in JP 2000-19168 A. Specifically, the liquid crystal polyester is depolymerized by reacting it with a lower alcohol in a supercritical state, and the depolymerization product (monomers that derive each monomer unit) is quantified by liquid chromatography, whereby the number of each monomer unit relative to the total monomer units can be calculated.

[0045] The liquid crystal polyester can be produced by polymerizing raw material monomers corresponding to the monomer units that constitute the polyester, for example, according to the method described in Japanese Patent No. 6439027.

[0046] The content of the liquid crystal polyester may be, for example, 60% by mass or more, 70% by mass or more, or 80% by mass or more, based on the total amount of the pellets. The content of the liquid crystal polyester may be, for example, 95% by mass or less, 90% by mass or less, or 88% by mass or less, based on the total amount of the pellets. That is, the content of the liquid crystal polyester may be, for example, 60% by mass or more to 95% by mass or less, 60% by mass or more to 90% by mass or less, 60% by mass or more to 88% by mass or less, 70% by mass or more to 95% by mass or less, 70% by mass or more to 90% by mass or less, 70% by mass or more to 88% by mass or less, 80% by mass or more to 95% by mass or less, 80% by mass or more to 90% by mass or less, or 80% by mass or more to 88% by mass or less, based on the total amount of the pellets.

[0047] (2) Fibrous Filler The pellets contain a fibrous filler (A).

[0048] Examples of the fibrous filler (A) include glass fibers. The proportion of glass fibers in the fibrous filler (A) may be, for example, 90% by mass or more, 95% by mass or more, 99% by mass or more, or 100% by mass.

[0049] The proportion of fibrous filler (A-1) having a fiber length of 50 μm or less in the fibrous filler (A) is 0.5% by mass or less, and may be 0.3% by mass or less, 0.1% by mass or less, or 0.05% by mass or less. If the amount of fibrous filler (A-1) having a fiber length of 50 μm or less is small, fibrous filler (A') having a fiber length of more than 50 μm is likely to be exposed on the surface of the molded article. When the fibrous filler (A') is exposed to the surface, gas components (especially high-boiling point components) inside the molded article are likely to volatilize due to heating during molding and be discharged outside the molded article. Therefore, when the amount of fibrous filler (A-1) having a fiber length of 50 μm or less is within the above range, the amount of gas generated in a high-temperature environment is more significantly suppressed.

[0050] The proportion of the fibrous filler (A-1) having a fiber length of 50 μm or less in the fibrous filler (A) may be 0% by mass. Alternatively, the fibrous filler (A) may contain a small amount of the fibrous filler (A-1) having a fiber length of 50 μm or less, and in this case, the proportion of the fibrous filler (A-1) may be, for example, 0.001% by mass or more, 0.005% by mass or more, or 0.01% by mass or more.

[0051] The number average fiber length of the fibrous filler (A) may be, for example, 50 μm or more, 100 μm or more, or 200 μm or more, which tends to increase the mechanical strength of the molded article.

[0052] The number average fiber length of the fibrous filler (A) may be, for example, 1500 μm or less, 1000 μm or less, or 500 μm or more, which tends to further improve the detail filling ability in the molded article.

[0053] The fiber length distribution of the fibrous filler (A) (proportion of fibrous filler (A-1), proportion of fibrous filler (A-2), number average fiber length) is measured by the following method. <Measurement of fiber length distribution> 4 g of pellets are heated at 600°C for 4 hours to obtain ash. The obtained ash is dispersed in ethylene glycol to prepare a preparation, which is observed under an optical microscope at a magnification of 500. Of the fibers that fall within the field of view (fibers with both ends within the field of view), the fiber lengths of fibers that are equal to or longer than the fiber diameter are measured. The fiber lengths of 500 or more fibers are measured to determine the fiber length distribution.

[0054] The fiber diameter (single fiber diameter) of the fibrous filler (A) may be, for example, 5 μm or more, 6 μm or more, or 9 μm or more. The fiber diameter (single fiber diameter) of the fibrous filler (A) may be, for example, 17 μm or less, 15 μm or less, or 12 μm or less. That is, the fiber diameter (single fiber diameter) of the fibrous filler (A) may be, for example, 5 μm or more and 17 μm or less, 5 μm or more and 15 μm or less, 5 μm or more and 12 μm or less, 6 μm or more and 17 μm or less, 6 μm or more and 15 μm or less, 6 μm or more and 12 μm or less, 9 μm or more and 17 μm or less, 9 μm or more and 15 μm or less, or 9 μm or more and 12 μm or less.

[0055] Content C of fibrous filler (A) 1 may be, for example, 0.05 or more, 0.1 or more, or 0.12 or more, based on the total amount of the pellets. 1 may be, for example, 0.4 or less, 0.35 or less, 0.3 or less, or 0.2 or less, based on the total amount of the pellets. 1 may be, for example, 0.05 or more and 0.4 or less, 0.1 or more and 0.35 or less, 0.1 or more and 0.3 or less, 0.1 or more and 0.2 or less, 0.12 or more and 0.3 or less, 0.12 or more and 0.3 or less, or 0.12 or more and 0.2 or less, based on the total amount of pellets.

[0056] Content C of fibrous filler (A) 1 is measured by the following method. 1 Measurement of ash content> 4 g of pellets are heated at 600°C for 4 hours to obtain ash content. From the obtained ash content, ash corresponding to the fibrous filler (A) is selected as necessary, and the mass of the ash corresponding to the fibrous filler (A) is measured. The content of the fibrous filler (A) is determined from this mass and the mass of the pellets used for incineration. Note that if the blending amount of the fibrous filler (A) in the pellets is known in advance, the content of the fibrous filler (A) may be determined from this blending amount.

[0057] The glass fibers used to prepare pellets usually contain a binder, and the amount of binder can be estimated by measuring the ignition loss of the glass fibers. The ignition loss of the glass fibers can be measured in accordance with JIS R3420. The ignition loss of the glass fibers (i.e., the amount of binder) may be 0.2% or more, 0.25% or more, or 0.3% or more, or 1%, 0.8% or less, or 0.5% or less, based on the total amount of glass fibers.

[0058] The pellets may contain one or more resins other than the liquid crystal polyester, such as polyolefins, cyclic polyolefins, polyvinyl chloride, polysulfones, (meth)acrylic resins, polyphenylene ether resins, polyacetal resins, polyamide resins, imide resins, polystyrene resins, cellulose resins, polyether ether ketone resins, fluororesins, polycarbonate resins, and thermosetting resins.

[0059] The pellets may contain one or more additives other than the fibrous filler, such as a filler, a colorant, a dispersant, a plasticizer, an antioxidant, a curing agent, a flame retardant, a heat stabilizer, an ultraviolet absorber, an antistatic agent, a surfactant, a lubricant, and a mold release agent.

[0060] In the pellet of this embodiment, the content ratio C of the fibrous filler (A) 1 The number N of spots per unit area derived from the fibrous filler (A) observed in a cross section perpendicular to the extrusion direction of the pellet 1 ( / mm 2 ) ratio (N 1 / C 1 ) is 3500 or more, and may be, for example, 4000 or more, 4200 or more, or 4500 or more. This makes the above-mentioned effect more pronounced. 1 / C 1 ) is 20,000 or less, and may be, for example, 18,000 or less or 15,000 or less, or 10,000 or less, 8,000 or less, or 6,000 or less. In this case, it can be said that breakage of the fibrous filler (A) is further suppressed, and thermal damage to the resin during melt-kneading tends to be further reduced, and the amount of gas generated tends to be further reduced. That is, the above ratio (N 1 / C 1) is, for example, 3500 or more and 20,000 or less, 3500 or more and 18,000 or less, 3500 or more and 15,000 or less, 3500 or more and 10,000 or less, 3500 or more and 8,000 or less, 3500 or more and 6,000 or less, 4,000 or more and 20,000 or less, 4,000 or more and 18,000 or less, 4,000 or more and 15,000 or less, 4,000 or more and 10,000 or less, 4,000 or more and 8,000 or less, 4,000 or more and 6,000 or less, 4 It may be 200 or more and 20,000 or less, 4,200 or more and 18,000 or less, 4,200 or more and 15,000 or less, 4,200 or more and 10,000 or less, 4,200 or more and 8,000 or less, 4,200 or more and 6,000 or less, 4,500 or more and 20,000 or less, 4,500 or more and 18,000 or less, or 4,500 or more and 15,000 or less, 4,500 or more and 10,000 or less, 4,500 or more and 8,000 or less, or 4,500 or more and 6,000 or less.

[0061] The above number N 1 is measured by the following method: 1 Measurement of X-ray CT image of a cross section of the pellet perpendicular to the extrusion direction during melt-kneading is obtained under the following conditions. The image of any cross section is binarized under the following image analysis conditions, and the number of spots corresponding to the fibrous filler (A) in the cross section is measured. The extrusion direction during melt-kneading can be determined by visually observing the appearance of the pellet. - X-ray CT image capturing conditions Apparatus: Nano3DX (manufactured by Rigaku Corporation) Imaging mode: Continuous Scan Lens: 2160 Radiation source: Mo Binning: 1 Exposure time: 7 s Number of images captured: 1000 XD distance: 5 mm - Image analysis Software used: Luzex AP (manufactured by Nireco Corporation) Binarization method: Binarized in automatic mode according to the manual of the attached software.

[0062] The average circle-equivalent diameter of the spots and the circle-equivalent diameter of the cross section of the pellet are also calculated from the image.

[0063] The size of the pellets in this embodiment is not particularly limited. The length of the pellets in the extrusion direction may be, for example, 2.0 mm or more, 2.2 mm or more, or 2.5 mm or more. The length of the pellets in the extrusion direction may be, for example, 8.0 mm or less, 6.0 mm or less, or 4.0 mm or less.

[0064] The equivalent circle diameter of the cross section perpendicular to the extrusion direction of the pellets may be, for example, 2 mm or more, 2.2 mm or more, or 2.5 mm or more, and the equivalent circle diameter of the cross section perpendicular to the extrusion direction of the pellets may be, for example, 8 mm or less, 6 mm or less, or 4 mm or less.

[0065] The pellets of this embodiment may be produced, for example, by the following method.

[0066] (Method for Producing Pellets) The method for producing pellets of this embodiment may include a step of melt-kneading and molding a liquid crystal polyester and a fibrous filler (hereinafter also referred to as fibrous filler (a)) to obtain pellets.

[0067] In the above step, the content ratio C of the fibrous filler (A) in the pellets 1 The number N of spots per unit area derived from the fibrous filler (A) observed in a cross section perpendicular to the extrusion direction of the pellet 1 ( / mm 2 ) ratio (N 1 / C 1 The melt-kneading and molding are carried out so that the molecular weight (Mw) of the polymer is 3,500 or more and 20,000 or less.

[0068] The fibrous filler (a) may be, for example, a fiber bundle obtained by bundling fibrous fillers with a bundling agent.

[0069] As the above-mentioned process, for example, the method of adding fibrous filler (a) to the melt of liquid crystal polyester, kneading, and extrusion molding can be mentioned.In this method, for example, by lengthening the time from adding the fibrous filler (a) to the melt of liquid crystal polyester until kneading (for example, by lengthening the length from the inlet of the fibrous filler to the kneading disk part), and by lengthening the kneading time (for example, by lengthening the length of the kneading disk part), the bundling agent that binds the fibrous filler decomposes, the generated gas volatilizes, the fibrous filler is loosened in the melt, and the aggregates of the fibrous filler are unlikely to remain in the pellet.

[0070] When the liquid crystal polyester and the fibrous filler are kneaded, the fibrous filler blended in the liquid crystal polyester may break, forming a fibrous filler with a short fiber length. If the fibrous filler is crushed without breaking, a significantly short fibrous filler (A-1) is likely to be formed. Therefore, in the above process, by selecting a method that reduces crushing of the fibrous filler, pellets containing 0.5% by mass or less of the fibrous filler (A-1) are likely to be obtained. For example, by extending the time between adding the fibrous filler (a) to the melt of the liquid crystal polyester and kneading, crushing of the fibrous filler tends to be reduced. By extending the time between adding the fibrous filler (a) and kneading, the fibrous filler (a) is loosened in the melt, and the formation of the fibrous filler (A-1) due to crushing of aggregates of the fibrous filler (a) (e.g., fiber bundles bonded with a sizing agent) is suppressed.

[0071] The above process may be carried out, for example, using a twin-screw extruder.

[0072] The pellets of this embodiment can be suitably applied to parts for communication devices, electrical devices, electronic devices, medical devices, automobiles, home appliances, industrial machinery, daily necessities, etc. These parts can be produced by molding the pellets of this embodiment by, for example, injection molding, compression molding, extrusion molding, blow molding, etc.

[0073] Although one embodiment of the invention according to the present disclosure has been described above, the invention according to the present disclosure is not limited to the above embodiment.

[0074] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the examples, percentages and parts representing the content or amount used are by mass unless otherwise specified.

[0075] Example 1 (1) Production of Liquid Crystal Polyester A reactor equipped with a stirrer, torque meter, nitrogen gas inlet tube, thermometer, and reflux condenser was charged with 1118.8 g (8.10 mol) of p-hydroxybenzoic acid, 547.4 g (3.00 mol) of 2-hydroxy-6-naphthoic acid, 1235.3 g (12.1 mol) of acetic anhydride, and 0.17 g of 1-methylimidazole. After thoroughly purging the reactor with nitrogen gas, the temperature was raised to 140°C over 15 minutes under a nitrogen gas stream, and the temperature was maintained at 140°C and refluxed for 1 hour. Thereafter, the temperature was raised to 280°C over 3 hours and 40 minutes while distilling off the by-product acetic acid. The point at which an increase in torque was observed was considered the end of the reaction, and the contents were removed. The flow initiation temperature of the resulting solid content was 235°C. The obtained solid was cooled to room temperature and crushed in a coarse crusher. The mixture was heated from room temperature (25°C) to 235°C over 1 hour in a nitrogen atmosphere, then heated from 235°C to 240°C over 4 hours and 10 minutes, and held at 240°C for 5 hours to carry out solid-state polymerization. The obtained solid-state polymer was cooled to room temperature to obtain a powdered liquid crystal polyester (1). The flow initiation temperature of the obtained liquid crystal polyester (1) was 277°C.

[0076] (2) Production of Pellets Using a twin-screw extruder (Shibaura Machine, TEM48S), liquid crystal polyester (1) and glass fiber (Nippon Electric Glass, ECS03T-786H, loss on ignition: 0.35%) were kneaded to produce pellets containing liquid crystal polyester (1) and glass fiber. Specifically, liquid crystal polyester (1) was supplied through the main feed port of the twin-screw extruder, glass fiber was supplied through the side feed port, and kneading was carried out. The kneaded mixture was extruded from the nozzle of the extruder to obtain strands. The supply amount was 85 parts by mass of liquid crystal polyester (1) and 15 parts by mass of glass fiber. The strands were cooled by spraying water to solidify them, and then further cooled while blowing air to remove the water. The solidified strands were cut with a pelletizer to obtain pellets containing liquid crystal polyester (1) and glass fiber.

[0077] (Comparative Example 1) Pellets containing liquid crystal polyester (1) and glass fiber were obtained in the same manner as in Example 1, except that the position of the side feed port was moved downstream, the length from the side feed port to the kneading disc section was set to 0.9 times that of Example 1, and the length of the kneading disc section was set to 0.5 times that of Example 1.

[0078] <Content ratio C of fibrous filler 1 Measurement of fibrous filler content C> 4 g of pellets were heated at 600°C for 4 hours to obtain ash. The mass of the obtained ash was measured, and the mass was calculated from the mass and the mass of the pellets used for incineration. 1 asked for.

[0079] <Number N 1Measurement of X-ray CT image of the cross section of the pellet perpendicular to the extrusion direction during melt-kneading was obtained under the following conditions. The image of any cross section was binarized under the following image analysis conditions, and the number of spots corresponding to the fibrous filler (A) in the cross section was measured. Furthermore, from the above image, the average circle-equivalent diameter of the spots and the circle-equivalent diameter of the cross section of the pellet were measured. - X-ray CT image capturing conditions Apparatus: Nano3DX (manufactured by Rigaku Corporation) Imaging mode: Continuous Scan Lens: 2160 Radiation source: Mo Binning: 1 Exposure time: 7 s Number of images captured: 1000 XD distance: 5 mm - Image analysis Software used: Luzex AP (manufactured by Nireco Corporation) Binarization method: Binarized in automatic mode according to the manual of the attached software.

[0080]

[0081] <Circle equivalent diameter of spot> Number N 1 The average circle-equivalent diameter of the spots was measured from the images obtained by the measurement. As a result, the average circle-equivalent diameter of the spots in Example 1 was 11.7 μm. On the other hand, the average circle-equivalent diameter of the spots in Comparative Example 1 was 20.9 μm, suggesting that the glass fibers in the pellets of Comparative Example 1 were not sufficiently opened.

[0082] <Measurement of Fiber Length Distribution of Glass Fiber> The fiber length distribution of the glass fiber was measured for the pellets obtained in Example 1 and Comparative Example 1 using the following method. 4 g of pellets were heated at 600°C for 4 hours to obtain ash. The obtained ash was dispersed in ethylene glycol to prepare a preparation, which was then observed under an optical microscope at a magnification of 500x. Of the fibers that fell within the field of view (fibers with both ends within the field of view), the fiber lengths of fibers having a length equal to or greater than the fiber diameter were measured. The fiber lengths of 500 or more fibers were measured to determine the fiber length distribution. From the obtained fiber length distribution, the proportion of fibrous filler (A-1) having a fiber length of 50 μm or less and the number average fiber length of the fibrous filler were determined. The results are shown in Table 2.

[0083]

[0084] <Evaluation of Amount of Gas Generated> The amount of gas generated for the pellets obtained in Example 1 and Comparative Example 1 was evaluated by the following method. A dumbbell test piece with a thickness of 0.8 mm was prepared by injection molding using the pellets. The parallel portion of this test piece was cut into a 5 mm square to obtain a measurement sample of 5 mm x 5 mm x 0.8 mm. 4 g of the measurement sample was sealed in a vial and sealed with a septum. The sample sealed in the vial was heated at 120°C for 20 hours, and then the amount of gas generated was measured under the following conditions using a headspace gas chromatograph (GC-2030AF, manufactured by Shimadzu Corporation). <Conditions> Column: Restek Rtx-1301 (inner diameter: 0.25 mm, length: 60 m, film thickness: 1.4 μm) Column temperature: held at 60°C for 5 minutes, heated to 220°C at 10°C / min, held at 220°C for 15 minutes Carrier gas: helium Split ratio: 10 Carrier gas flow rate: 10 mL / min Acetone, acetic acid, phenol, and acetic phenol were quantified using the calibration curve. For peaks derived from other components, components with retention times of 15.5 minutes or less were converted to acetone, and components with retention times greater than 15.5 minutes were converted to phenol. The measured amounts of low-boiling components with retention times of 15.5 minutes or less and high-boiling components with retention times greater than 15.5 minutes are shown in Table 3.

[0085]

[0086] As shown in Table 3, the pellets of Example 1 suppressed the generation of gas (particularly high boiling point components) in a high temperature environment compared to the pellets of Comparative Example 1.

Claims

1. A pellet containing a liquid crystal polyester and a fibrous filler (A), wherein the content ratio of the fibrous filler (A) is C 1 The number N of spots per unit area derived from the fibrous filler (A) observed in a cross section perpendicular to the extrusion direction of the pellet 1 ( / mm 2 ) ratio (N 1 / C 1 ) is 3,500 or more and 20,000 or less.

2. Content C of the fibrous filler (A) 1 The pellet according to claim 1, wherein the ratio is 0.05 or more and 0.4 or less.

3. The pellet according to claim 1, wherein the average equivalent circle diameter of the spots is 9 μm or more and 13 μm or less.

4. The pellet of claim 1, wherein said fibrous filler (A) comprises glass fibers.

5. The pellet according to claim 1, wherein the liquid crystal polyester contains monomer units derived from an aromatic hydroxycarboxylic acid.

6. The pellet according to claim 5, wherein the content of said monomer unit is 50 mol % or more based on the total of all monomer units constituting said liquid crystal polyester.

7. A process for obtaining pellets by melt-kneading and molding a liquid crystal polyester and a fibrous filler, wherein the process is carried out to obtain a pellet having a content C of the fibrous filler (A) in the pellets. 1 The number N of spots per unit area derived from the fibrous filler (A) observed in a cross section perpendicular to the extrusion direction of the pellet 1 ( / mm 2 ) ratio (N 1 / C 1 The method for producing pellets, comprising the step of performing the melt-kneading and the molding so that the molecular weight distribution of the polymer is 3,500 or more and 20,000 or less.

Citation Information

Patent Citations

  • Liquid crystal polyester resin pellet, method for manufacturing the same, and method for manufacturing molded article

    JP2021028373A

  • Injection molded article and method for manufacturing same

    WO2021029263A1