Prepreg and molded article

The prepreg composition using urethane (meth)acrylate, ethylenically unsaturated monomers, and halogen-free phosphorus-based flame retardants addresses environmental concerns and achieves excellent flame retardancy in fiber-reinforced resin composites, ensuring rapid curing and compliance with UL standards.

WO2024247743A1PCT designated stage expired Publication Date: 2024-12-05DIC CORP

Patent Information

Application Number
PCT/JP2024/018119
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-30
Filing Date
2024-05-16
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional prepregs containing halogen-containing compounds for flame retardancy pose environmental concerns, and there is a need for a halogen-free solution that achieves excellent flame retardancy in fiber-reinforced resin composite materials, particularly for applications like lithium-ion battery casings.

Method used

A prepreg composition comprising urethane (meth)acrylate, an ethylenically unsaturated monomer, a polymerization initiator, reinforcing fibers, and a halogen-free phosphorus-based flame retardant, which includes specific polyisocyanates and polyols, ensures excellent flame retardancy without using halogen-containing compounds.

Benefits of technology

The prepreg composition achieves rapid curing and excellent flame retardancy in molded articles, meeting UL standards, while preventing environmental impact from halogen release, with the halogen-free phosphorus compounds ensuring effective flame retardancy and improved heat resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The present invention addresses the problem of providing: a prepreg capable of achieving excellent flame retardancy even without containing a halogen-containing compound; and a molded article thereof. A prepreg according to the present invention contains a urethane (meth)acrylate (A), an ethylenically unsaturated monomer (B) other than the urethane (meth)acrylate (A), a polymerization initiator (C), a reinforcing fiber (D), and a flame retardant (E). The urethane (meth)acrylate (A) is a reaction product of a polyisocyanate (a1) and a polyol (a2) having an ethylenically unsaturated group and an aromatic skeleton, and / or a reaction product of a polyisocyanate (a1), a polyol (a3) having an aromatic skeleton without having an ethylenically unsaturated group, and a hydroxyalkyl (meth)acrylate (a4), and the flame retardant (E) contains at least one halogen-free phosphorus compound.
Need to check novelty before this filing date? Find Prior Art

Description

Prepregs and molded products

[0001] The present invention relates to a prepreg and a molded article thereof.

[0002] Fiber-reinforced resin composite materials reinforced with reinforcing fibers such as carbon fiber and glass fiber have attracted attention for their lightweight yet excellent heat resistance and mechanical strength, and are increasingly being used in a variety of structural applications, including automobile and aircraft housings and various components. For example, a method for molding such fiber-reinforced resin composite materials involves using an intermediate material called a prepreg, in which reinforcing fibers are impregnated with a thermosetting resin, and then curing and molding the prepreg by autoclave molding or press molding.

[0003] Prepregs are required to be flame retardant depending on the application, such as in construction or automobile battery cases. In particular, lithium-ion secondary batteries, which are often used as batteries for electric vehicles, contain organic solvents and are therefore liable to ignite. To ensure safety during use, prepregs used to mold battery cases for housing such lithium-ion secondary batteries are required to meet the flame retardancy standards set by UL (Underwriters Laboratories, Inc.).

[0004] Conventionally, as a flame-retardant prepreg, a prepreg containing a halogen-containing compound such as brominated phenol as a flame retardant has been known (see, for example, Patent Document 1). However, the halogen-containing compound has the disadvantage of being an environmental concern.

[0005] Special Publication No. 2009-521666

[0006] The problem to be solved by the present invention is to provide a prepreg and a molded article thereof that can achieve excellent flame retardancy without containing a halogen-containing compound.

[0007] The present inventors have found that a prepreg containing a specific urethane (meth)acrylate, a specific ethylenically unsaturated monomer, a polymerization initiator, reinforcing fibers, and a specific flame retardant can solve the above-mentioned problems, and have completed the present invention.

[0008] That is, the present invention relates to a prepreg comprising a urethane (meth)acrylate (A), an ethylenically unsaturated monomer (B) other than the urethane (meth)acrylate (A), a polymerization initiator (C), reinforcing fibers (D), and a flame retardant (E), wherein the urethane (meth)acrylate (A) is a reaction product of a polyisocyanate (a1) and a polyol (a2) having an ethylenically unsaturated group and an aromatic skeleton, and / or a reaction product of the polyisocyanate (a1), a polyol (a3) ​​having no ethylenically unsaturated group but an aromatic skeleton, and a hydroxyalkyl (meth)acrylate (a4), and the flame retardant (E) comprises one or more halogen-free phosphorus compounds.

[0009] The prepreg of the present invention can achieve excellent flame retardancy in molded articles obtained from the prepreg, even without containing a halogen-containing compound.

[0010] The prepreg of the present invention contains a urethane (meth)acrylate (A), an ethylenically unsaturated monomer (B) other than the urethane (meth)acrylate (A), a polymerization initiator (C), reinforcing fibers (D), and a flame retardant (E), wherein the urethane (meth)acrylate (A) is a reaction product of a polyisocyanate (a1) and a polyol (a2) having an ethylenically unsaturated group and an aromatic skeleton, and / or a reaction product of the polyisocyanate (a1), a polyol (a3) ​​having no ethylenically unsaturated group but an aromatic skeleton, and a hydroxyalkyl (meth)acrylate (a4), and the flame retardant (E) contains one or more halogen-free phosphorus compounds.

[0011] The polyisocyanate (a1) preferably contains a polyisocyanate having a cyclic skeleton, since this further improves the heat resistance of the molded article. These polyisocyanates (a1) can be used alone or in combination of two or more.

[0012] Examples of the polyisocyanate (a1) include 2,4'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, carbodiimide-modified products of 4,4'-diphenylmethane diisocyanate, polymethylene polyphenyl polyisocyanate, nurate-modified products, biuret-modified products, urethane imine-modified products of diphenylmethane diisocyanate, polyol-modified products modified with polyols having a number average molecular weight of 1,000 or less such as diethylene glycol and dipropylene glycol, tolylene diisocyanate (TDI), tolidine diisocyanate, Examples of suitable polyisocyanates include aromatic polyisocyanates such as isocyanate, xylylene diisocyanate, 1,5-naphthalene diisocyanate, and tetramethylxylene diisocyanate; alicyclic polyisocyanates such as isophorone diisocyanate (IPDI), hydrogenated diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, and norbornene diisocyanate; and aliphatic polyisocyanates such as hexamethylene diisocyanate, nurate-modified hexamethylene diisocyanate, biuret-modified hexamethylene diisocyanate, and adducts thereof, and dimer acid diisocyanate. Among these, 2,4'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, carbodiimide-modified 4,4'-diphenylmethane diisocyanate, and polymethylene polyphenyl polyisocyanate are preferred because they further improve the heat resistance of molded articles. These polyisocyanates (a1) can be used alone or in combination of two or more kinds.

[0013] The polyol (a2) has an ethylenically unsaturated group and an aromatic skeleton. Multifunctional epoxy (meth)acrylates are preferred because they provide improved heat resistance. Examples include reaction products of bisphenol-type epoxy resins such as bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, bisphenol fluorene-type epoxy resins, and biscresol fluorene-type epoxy resins, as well as novolac-type epoxy resins such as phenol novolac-type epoxy resins and cresol novolac-type epoxy resins, with (meth)acrylic acid. Preferably, they are obtained by reacting an epoxy resin having an epoxy equivalent weight in the range of 180 to 500 with (meth)acrylic acid. The number of functional groups is preferably 1.5 to 3.0 in terms of the balance between heat resistance and strength properties.

[0014] The polyol (a3) ​​has no ethylenically unsaturated groups and an aromatic skeleton. Examples include alkylene oxide adducts of bisphenol compounds such as alkylene oxide adducts of bisphenol A, alkylene oxide adducts of bisphenol S, and alkylene oxide adducts of bisphenol F; alkylene oxide adducts of dihydroxybenzene compounds such as 1,3-bis(2-hydroxyethoxy)benzene and 1,4-bis(2-hydroxyethoxy)benzene; alkylene oxide adducts of biphenol compounds such as 2'-[(1,1'-biphenyl-4,4'-diyl)bisoxy]bisethanol; alkylene oxide adducts of dihydroxynaphthalene compounds, and 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene. Among these, alkylene oxide adducts of bisphenol compounds are preferred from the viewpoint of a balance of compatibility, heat resistance, water resistance, and strength properties. More preferred are ethylene oxide adducts of bisphenol compounds, with an average number of moles added of 2 to 10 moles.

[0015] Examples of the hydroxyalkyl (meth)acrylate (a4) include 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxy-n-butyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxy-n-butyl (meth)acrylate, and 3-hydroxy-n-butyl (meth)acrylate. Among these, 2-hydroxyethyl (meth)acrylate is preferred from the viewpoint of the balance of strength properties. These hydroxyalkyl (meth)acrylates (a4) can be used alone or in combination of two or more.

[0016] If necessary, polyols other than the polyols (a2) to (a4) can be used in combination as raw materials for the urethane (meth)acrylate (A). Examples of other polyols that can be used include polyester polyols, acrylic polyols, polyether polyols, polycarbonate polyols, and polyalkylene polyols.

[0017] The molar ratio (a3 / a4) of the polyol (a3) ​​to the hydroxyalkyl (meth)acrylate (a4) is preferably 60 / 40 to 20 / 80, more preferably 50 / 50 to 30 / 70, since this further improves heat resistance and curability.

[0018] The molar ratio (NCO / OH) of the isocyanate group (NCO) of the isocyanate compound to the hydroxyl group (OH) of the compound having a hydroxyl group, which are raw materials for the urethane (meth)acrylate (A), is preferably 0.7 to 1.3, more preferably 0.8 to 1.1, and even more preferably 0.8 to 1.0, in view of the balance between heat resistance and strength properties.

[0019] Examples of the ethylenically unsaturated monomer (B) include dimethacrylate of an ethylene oxide adduct of bisphenol A, tricyclodecane dimethanol dimethacrylate, 1,12-dodecanediol dimethacrylate, hydrogenated bisphenol A dimethacrylate, polytetramethylene glycol dimethacrylate, 9,9-bis[4-(2-methacryloyloxyethoxy)phenyl]fluorene, dimethacrylate of an ethylene oxide adduct of isosorbide, dimethacrylate of an ethylene oxide adduct of hydrogenated bisphenol A, trimethacrylate of an ethylene oxide adduct of trimethylolpropane, tetramethacrylate of an ethylene oxide adduct of pentaerythritol, and hexamethacrylate of an ethylene oxide adduct of dipentaerythritol. In view of the balance of curability, heat resistance, and strength properties, the molecular weight is preferably 320 to 2,000, and the (meth)acrylic group equivalent is preferably 150 to 1,000, and more preferably 150 to 500. Similarly, in view of the balance between curability, heat resistance, and strength properties, the number of functional groups is preferably 2 to 4, and more preferably 2.

[0020] The content of the ethylenically unsaturated monomer (B) in the total of the urethane (meth)acrylate (A) and the ethylenically unsaturated monomer (B) (hereinafter abbreviated as "content (B)") is preferably 5 to 50 mass%, and more preferably 10 to 40 mass%, because this further improves the balance between prevention of contamination of the working environment, prepreg handleability, and molded product quality and productivity.

[0021] The polymerization initiator (C) is not particularly limited, but is preferably an organic peroxide, such as a diacyl peroxide compound, a peroxyester compound, a hydroperoxide compound, a ketone peroxide compound, an alkyl perester compound, a percarbonate compound, a peroxyketal, etc., which can be appropriately selected depending on the molding conditions. These polymerization initiators (C) can be used alone or in combination of two or more.

[0022] Among these, it is preferable to use a polymerization initiator having a temperature of 60° C. or higher and 110° C. or lower to obtain a 10-hour half-life for the purpose of shortening the molding time. A polymerization initiator having a temperature of 70° C. or higher and 105° C. or lower is preferable because the prepreg has a long life at room temperature and can be cured in a short time (within 5 minutes) by heating, and by using it in the prepreg of the present invention, the curability and moldability are superior. Examples of such polymerization initiators include 1,6-bis(t-butylperoxycarbonyloxy)hexane, 1,1-bis(t-butylperoxy)cyclohexane, 1,1-bis(t-amylperoxy)cyclohexane, 1,1-bis(t-hexylperoxy)cyclohexane, t-butylperoxydiethyl acetate, t-butylperoxyisopropyl carbonate, t-butylperoxy 2-ethylhexyl carbonate, t-amylperoxyisopropyl carbonate, t-amylperoxy 2-ethylhexyl carbonate, t-hexylperoxyisopropyl carbonate, di-tert-butylperoxyhexahydroterephthalate, t-amylperoxytrimethylhexanoate, t-amylperoxyisononatoate, t-hexylperoxy-2-ethylhexanoate, and n-butyl 4,4-di(t-butylperoxy)valerate. The most suitable organic peroxide is selected and used depending on the molding conditions.

[0023] The amount of the polymerization initiator (C) added is preferably in the range of 0.5 to 3 parts by mass per 100 parts by mass of the total of the urethane (meth)acrylate (A) and the ethylenically unsaturated monomer (B), because this provides excellent curing characteristics and storage stability.

[0024] Examples of the reinforcing fiber (D) include carbon fiber, glass fiber, silicon carbide fiber, alumina fiber, boron fiber, metal fiber, and organic fibers such as aramid fiber, vinylon fiber, and Tetron fiber. Carbon fiber or glass fiber is preferred, and carbon fiber is more preferred, because it allows the production of molded products with higher strength and elasticity. These reinforcing fibers (D) can be used alone or in combination of two or more.

[0025] As the carbon fiber, various types such as polyacrylonitrile, pitch, and rayon can be used, but among these, polyacrylonitrile is preferred because high strength carbon fibers can be easily obtained.

[0026] The shape of the reinforcing fiber (D) is not particularly limited, and examples thereof include reinforcing fiber tows in which reinforcing fiber filaments are bundled, unidirectional materials in which reinforcing fiber tows are aligned in one direction, woven fabrics or short-cut reinforcing fibers, and nonwoven fabrics or papers made of short-cut reinforcing fibers. However, it is preferable to use unidirectional materials as reinforcing fibers and laminate and mold them, as this can provide high mechanical properties.

[0027] When short cut reinforcing fibers are used, it is preferable to use carbon fibers cut to 2.5 to 50 mm, as this will improve the flowability in the mold during molding and the appearance of the molded product.

[0028] In the case of woven fabrics, examples include plain weave, twill weave, satin weave, and non-crimped fabrics, such as sheets in which fiber bundles are aligned in one direction or sheets in which sheets are layered at different angles and stitched to prevent unraveling.

[0029] Weight of reinforced fiber (fiber 1m 2 The weight per unit area is not particularly limited, but is preferably 10 g / m 2 ~650g / m 2 The basis weight is preferably 10 g / m 2 When the weight is 650 g / m or more, the unevenness of the fiber width is small and the mechanical properties are good, which is preferable. 2 If the weight is less than 500g / m, the resin impregnation is good, which is preferable. 2 More preferably, 50 to 300 g / m 2 is particularly preferred.

[0030] The content of the reinforcing fiber (D) in the prepreg of the present invention is preferably in the range of 20 to 85 mass %, more preferably in the range of 40 to 80 mass %, since the mechanical strength of the obtained molded article is further improved.

[0031] The flame retardant (E) contains one or more halogen-free phosphorus compounds. A halogen-free phosphorus compound is a compound containing phosphorus but not halogen. By including the flame retardant (E), the prepreg of the present invention can obtain excellent flame retardancy in molded articles obtained from the prepreg. Furthermore, since the flame retardant (E) is halogen-free (halogen-free), the environmental impact of halogen release during the manufacturing process of the prepreg or molded article can be prevented. However, if a compound that does not contain halogen or phosphorus is used as the flame retardant, the molded article cannot obtain excellent flame retardancy.

[0032] Examples of the halogen-free phosphorus compound include red phosphorus, phosphonate esters, ammonium polyphosphate salts, phosphate esters, aromatic phosphate esters, aromatic condensed phosphate esters, phosphazenes, etc. Commercially available products include Novaexcel 140, Nonnene 73, FCP-770, DAIGUARD-880, TPP, TCP, CDP, PX-110, CR-733S, CR-741, PX-200, DAIGUARD-580, DAIGUARD-850, Lavitol FP-110, and Lavitol FP-100.

[0033] When the prepreg is heated, radicals generated by decomposition of the polymerization initiator (C) are added to the ethylenically unsaturated monomer (B), causing the polymerization reaction to proceed. The heat of polymerization generated during the polymerization reaction shortens the time it takes for the prepreg to reach the desired peak temperature during heating, allowing the prepreg to achieve rapid curing. However, in the case of halogen-free phosphorus compounds containing active hydrogen, the active hydrogen deactivates the radicals, hindering the progress of the polymerization reaction. As a result, the time it takes for the prepreg to reach the desired peak temperature during heating is delayed, or the peak temperature may not be reached at all. Therefore, it is preferable to use a halogen-free phosphorus compound that does not contain active hydrogen.

[0034] On the other hand, even if a halogen-free phosphorus compound containing active hydrogen is a salt compound, the salt has low solubility in the resin component of the prepreg, making it difficult for the active hydrogen to deactivate the radicals, thereby suppressing the active hydrogen from interfering with the progress of the polymerization reaction. As a result, it is possible to prevent the prepreg from experiencing a delay in reaching the desired peak temperature during heating or from failing to reach the peak temperature, thereby achieving rapid curing of the prepreg. In other words, it is preferable to use a salt compound as the halogen-free phosphorus compound. The salt compound may or may not contain active hydrogen. Furthermore, in consideration of flame retardancy, availability, price, etc., ammonium phosphate salt is more preferable as the halogen-free salt compound.

[0035] That is, the halogen-free phosphorus compound is preferably a phosphorus compound not containing active hydrogen or an ammonium phosphate. The ammonium phosphate may contain active hydrogen or may not contain active hydrogen. However, in this specification, the active hydrogen-free phosphorus compound does not include an active hydrogen-free ammonium phosphate.

[0036] Examples of the phosphorus compound not containing active hydrogen include ammonium polyphosphate, phosphoric acid, phosphate salts, polyphosphoric acid, polyphosphate salts, etc. Commercially available products include FCP-770, FCP-790, phosphoric acid, sodium phosphate, polyphosphoric acid, sodium polyphosphate, etc.

[0037] Commercially available products of the ammonium phosphate include FCP-770 and FCP-790.

[0038] Components other than those described above may also be used as components of the prepreg of the present invention, and may contain, for example, a thermosetting resin, a thermoplastic resin, a polymerization inhibitor, a curing accelerator, a filler, a low-shrinkage agent, a release agent, a thickener, a viscosity reducer, a pigment, an antioxidant, a plasticizer, an antibacterial agent, an ultraviolet stabilizer, a reinforcing material, a photocuring agent, etc.

[0039] Examples of the thermosetting resin include vinyl ester resin, unsaturated polyester resin, phenol resin, melamine resin, furan resin, bismaleimide resin, etc. These thermosetting resins can be used alone or in combination of two or more.

[0040] Examples of the thermoplastic resin include polyamide resin, polyethylene terephthalate resin, polybutylene terephthalate resin, polycarbonate resin, polyurethane resin, polypropylene resin, polyethylene resin, polystyrene resin, acrylic resin, polybutadiene resin, polyisoprene resin, and resins modified by copolymerization or the like. Among these, polyamide resin and polyurethane resin are preferred because of their high brittleness-improving effect. These thermoplastic resins can be used alone or in combination of two or more. Thermoplastic resins can be added in particulate form or melted and mixed. When particulate thermoplastic resins are used, the particle size is preferably 30 μm or less, more preferably 5 to 20 μm, from the viewpoint of dispersibility in fibers.

[0041] Examples of the polymerization inhibitor include hydroquinone, trimethylhydroquinone, p-t-butylcatechol, t-butylhydroquinone, toluhydroquinone, p-benzoquinone, naphthoquinone, hydroquinone monomethyl ether, phenothiazine, copper naphthenate, copper chloride, etc. These polymerization inhibitors can be used alone or in combination of two or more.

[0042] Examples of the curing accelerator include metal soaps such as cobalt naphthenate, cobalt octenate, vanadyl octenate, copper naphthenate, and barium naphthenate, and metal chelate compounds such as vanadyl acetylacetate, cobalt acetylacetate, and iron acetylacetonate. Examples of amines include N,N-dimethylamino-p-benzaldehyde, N,N-dimethylaniline, N,N-diethylaniline, N,N-dimethyl-p-toluidine, N-ethyl-m-toluidine, triethanolamine, m-toluidine, diethylenetriamine, pyridine, phenylmorpholine, piperidine, and diethanolaniline. These curing accelerators can be used alone or in combination of two or more.

[0043] The fillers include inorganic compounds and organic compounds, and can be used to adjust the physical properties of the molded product, such as strength, elastic modulus, impact strength, and fatigue durability.

[0044] Examples of the inorganic compound include calcium carbonate, magnesium carbonate, barium sulfate, mica, talc, kaolin, clay, celite, asbestos, barite, baryta, silica, silica sand, dolomite limestone, gypsum, aluminum fine powder, hollow balloons, alumina, glass powder, aluminum hydroxide, kansuiite, zirconium oxide, antimony trioxide, titanium oxide, molybdenum dioxide, and iron powder.

[0045] Examples of the organic compounds include powders of natural polysaccharides such as cellulose and chitin, and synthetic resin powders. Examples of synthetic resin powders include organic powders composed of hard resins, soft rubbers, elastomers, or polymers (copolymers), and particles having a multilayer structure such as a core-shell type. Specific examples include acrylic particles, polyamide particles, particles composed of butadiene rubber and / or acrylic rubber, urethane rubber, silicone rubber, polyimide resin powder, fluororesin powder, and phenolic resin powder. These fillers can be used alone or in combination of two or more.

[0046] Examples of the release agent include zinc stearate, calcium stearate, paraffin wax, polyethylene wax, carnauba wax, etc. Preferred examples include paraffin wax, polyethylene wax, carnauba wax, etc. These release agents can be used alone or in combination of two or more.

[0047] Examples of the thickener include metal oxides and hydroxides such as magnesium oxide, magnesium hydroxide, calcium oxide, and calcium hydroxide, and acrylic resin-based fine particles, and can be selected appropriately depending on the handleability of the prepreg of the present invention. These thickeners can be used alone or in combination of two or more.

[0048] The prepreg of the present invention can be obtained by the following steps: Step 1: impregnating the reinforcing fibers (D) with a resin solution prepared by mixing the polyisocyanate (a1), the polyol (a2), and / or (a3), the hydroxyalkyl (meth)acrylate (a4), the ethylenically unsaturated monomer (B), the polymerization initiator (C), and the flame retardant (E) using a known mixer such as a planetary mixer or a kneader; sandwiching the resulting mixture between release PET films from above; and rolling the resulting mixture with a rolling mill to obtain a sheet; and Step 2: allowing the resulting mixture to stand at room temperature to 50°C to react the isocyanate groups of the polyisocyanate (a1) with the hydroxyl groups of the polyol (a2), and / or (a3) ​​and (a4). In step 1, a resin solution in which the polyisocyanate (a1), the polyol (a2), and / or (a3) ​​and (a4) have been partially reacted in advance can also be used, as long as the impregnation ability into the fiber is not impaired.

[0049] The thickness of the prepreg of the present invention is preferably 0.02 to 1.0 mm. A thickness of 0.02 mm or more is preferred because it is easy to handle for lamination, and a thickness of 1 mm or less is preferred because it allows for good resin impregnation. A thickness of 0.05 to 0.5 mm is even more preferred.

[0050] As a method for obtaining a molded article from the prepreg obtained above, for example, the release PET film is peeled from the prepreg, 8 to 30 prepregs are laminated, and the laminate is then placed in a mold preheated to 110°C to 160°C, the mold is clamped using a compression molding machine, the prepreg is shaped, and a molding pressure of 0.1 to 10 MPa is maintained to cure the prepreg, and the molded article is then removed to obtain the molded article.

[0051] Molded articles obtained from the prepreg of the present invention are excellent in bending strength, interlaminar shear strength, etc., and can therefore be suitably used for automobile components, railway vehicle components, aerospace aircraft components, ship components, housing equipment components, sports components, light vehicle components, construction and civil engineering components, housings for office automation equipment, etc.

[0052] The present invention will be described in more detail below with reference to specific examples.

[0053] (1) Preparation of Resin Composition for Prepreg A mixture of polymethylene polyphenyl polyisocyanate and diphenylmethane diisocyanate ("Millionate" manufactured by Tosoh Corporation) was used. 29.0 parts by mass of 4,4'-diphenylmethane diisocyanate (hereinafter abbreviated as "MDI"), 9.9 parts by mass of hydroxyethyl methacrylate (hereinafter abbreviated as "HEMA"), 6.3 parts by mass of Newpol BPE-20 (manufactured by Sanyo Chemical Industries, Ltd.: EO adduct of bisphenol A, hydroxyl group equivalent: 164 g / eq), 8.9 parts by mass of Newpol BPE-40 (manufactured by Sanyo Chemical Industries, Ltd.: EO adduct of bisphenol A, hydroxyl group equivalent: 204 g / eq), 0.7 parts by mass of PEG-300 (manufactured by Sanyo Chemical Industries, Ltd.: polyethylene glycol, hydroxyl group equivalent: 150 g / eq), 6.3 parts by mass of a thermoplastic resin described below, and MIRAMER as a polymerizable monomer. A prepreg resin composition (1) was obtained by mixing 12.0 parts by weight of M-245 (Bigen Specialty Chemical Co., Ltd.: bifunctional methacrylate monomer), 1.0 part by weight of a polymerization initiator (Kayaku Nouryon Co., Ltd.: "Trigonox 122-C80", an organic peroxide), and 30.0 parts by weight of Firecut P-770 (Suzuhiro Chemical Co., Ltd.: ammonium polyphosphate) as a halogen-free flame retardant. The ammonium polyphosphate contained in the halogen-free flame retardant is a halogen-free ammonium phosphate salt containing active hydrogen. The thermoplastic resin was synthesized by mixing 71 parts by weight of PTMG1000 (Mitsubishi Chemical Co., Ltd.: polytetramethylene ether glycol), 3 parts by weight of 1,4-butanediol (hereinafter abbreviated as "1,4-BG"), and 26 parts by weight of MDI, casting the mixture into a vat, and reacting it at 90°C for 24 hours. The weight average molecular weight of the resulting thermoplastic resin was 50,000.

[0054] (2) Preparation of Prepreg The obtained resin composition for prepreg was applied to one side of a release PET film, and then carbon fiber ("TRK979PQRW" manufactured by Mitsubishi Chemical Corporation) was impregnated therein by a hand lay-up method so that the carbon fiber volume content was 55%. The film was then covered with the same release PET film and aged at 45°C for 24 hours to prepare prepreg (1).

[0055] (3) Evaluation of Prepreg The obtained prepreg was cut and laminated to obtain test pieces A measuring 50 mm in length, 50 mm in width, and 2.2 mm in thickness. A rapid-cure evaluation test was performed on the obtained test pieces A. A thermocouple was sandwiched between two test pieces A and pressed with upper and lower hot plates (press pressure: 0.5 MPa). The temperatures of the upper and lower hot plates were 135°C when the polymerization initiator contained in the prepreg resin composition was Trigonox 122-C80, and 105°C when the polymerization initiator was Trigonox 421-70 (described below). The cure time (hereinafter abbreviated as "CT"), which is the time it took for the thermocouple temperature to reach the peak top temperature from 30°C, was measured. The temperature of the test environment was 23±3°C. <Evaluation> ◯: CT was within 60 seconds. ×: CT was longer than 60 seconds.

[0056] (4) Evaluation of Molded Articles The resulting prepregs were laminated to a total thickness of 2 mm. The resulting laminate was filled into the center of a flat plate mold coated with a mold release agent and compression-molded using a compression molding machine under conditions of 4 MPa pressure, an upper mold temperature of 140°C, a lower mold temperature of 135°C, and a molding time of 3 minutes. The resulting molded article, test piece B, was then cut into strips measuring 125 mm in length and 13 mm in width. A vertical combustion test was conducted in accordance with UL94V. The upper end of test piece B was attached vertically to a clamp, and cotton was placed 300 mm below test piece B. A blue flame (20 mm high) of methane gas was applied to the lower end of test piece B using a gas burner for 10 seconds to measure the combustion time. If combustion lasted less than 30 seconds, the flame was applied for an additional 10 seconds to measure the combustion time. The presence or absence of ignition of the cotton due to the dropping of the material and the presence or absence of combustion at the clamp attachment position were observed. These procedures were performed on five test pieces B. The criteria are shown in Table 1.

[0057]

[0058] In this example, a prepreg resin composition was prepared in the same manner as in Example 1, except that Lavitol FP-110 (manufactured by Mitsui Fine Chemicals, Inc.: phosphazene-based) was used as the halogen-free flame retardant instead of Firecut P-770. The phosphazene compound contained in the halogen-free flame retardant is a phosphorus compound that does not contain halogen and does not contain active hydrogen. Note that the phosphazene compound does not fall under the category of ammonium phosphate salt. Using the obtained prepreg resin composition, a prepreg was produced in the same manner as in Example 1. Test piece A was produced from the obtained prepreg and evaluated in the same manner as in Example 1. Furthermore, test piece B was produced as a molded article from the obtained prepreg and evaluated in the same manner as in Example 1.

[0059] In this example, a prepreg resin composition was prepared in the same manner as in Example 1, except that 20.0 parts by mass of CR-733S (aromatic condensed phosphate ester manufactured by Daihachi Chemical Industry Co., Ltd.) was used as the halogen-free flame retardant instead of 30.0 parts by mass of Firecut P-770. A prepreg was produced in the same manner as in Example 1 using the obtained prepreg resin composition. Test piece A was produced from the obtained prepreg in the same manner as in Example 1 and evaluated. Furthermore, test piece B was produced as a molded article from the obtained prepreg in the same manner as in Example 1 and evaluated.

[0060] In this example, a prepreg resin composition was prepared in the same manner as in Example 1, except that 2.0 parts by mass of "Trigonox 421-70" (organic peroxide) manufactured by Kayaku Nouryon Co., Ltd. was used as the polymerization initiator instead of 1.0 part by mass of Trigonox 122-C80. A prepreg was produced in the same manner as in Example 1 using the obtained prepreg resin composition. Test piece A was produced from the obtained prepreg and evaluated in the same manner as in Example 1. Furthermore, using the obtained prepreg, test piece B was produced as a molded body in the same manner as in Example 1 and evaluated, except that the molding conditions were changed to a pressure of 4 MPa, an upper mold temperature of 110°C, a lower mold temperature of 105°C, and a molding time of 8 minutes.

[0061] In this example, a prepreg resin composition was prepared in the same manner as in Example 1, except that 2.0 parts by mass of "Trigonox 421-70" (organic peroxide) manufactured by Kayaku Nouryon Co., Ltd. was used as the polymerization initiator instead of 1.0 part by mass of Trigonox 122-C80. A prepreg was produced in the same manner as in Example 1 using the obtained prepreg resin composition. Test piece A was produced from the obtained prepreg and evaluated in the same manner as in Example 1. Furthermore, using the obtained prepreg, test piece B was produced as a molded body in the same manner as in Example 1 and evaluated, except that the molding conditions were changed to a pressure of 4 MPa, an upper mold temperature of 110°C, a lower mold temperature of 105°C, and a molding time of 8 minutes.

[0062] In this example, a prepreg resin composition was prepared in the same manner as in Example 1, except that 2.0 parts by mass of "Trigonox 421-70" (organic peroxide) manufactured by Kayaku Nouryon Co., Ltd. was used as the polymerization initiator instead of 1.0 part by mass of Trigonox 122-C80, and 20.0 parts by mass of CR-733S (aromatic condensed phosphate ester manufactured by Daihachi Chemical Industry Co., Ltd.) was used as the halogen-free flame retardant instead of 30.0 parts by mass of Firecut P-770. Using the resulting prepreg resin composition, a prepreg was produced in the same manner as in Example 1. Test piece A was produced from the resulting prepreg in the same manner as in Example 1 and evaluated. Furthermore, using the resulting prepreg, test piece B was produced as a molded body in the same manner as in Example 1 and evaluated, except that the molding conditions were changed to a pressure of 4 MPa, an upper mold temperature of 110°C, a lower mold temperature of 105°C, and a molding time of 8 minutes.

[0063] Comparative Example 1 In this comparative example, a resin composition for prepreg was prepared in the same manner as in Example 1, except that no flame retardant was added. A prepreg was produced using the obtained resin composition for prepreg in the same manner as in Example 1. Test piece A was produced from the obtained prepreg in the same manner as in Example 1 and evaluated. Furthermore, test piece B was produced as a molded article from the obtained prepreg in the same manner as in Example 1 and evaluated.

[0064] Comparative Example 2 In this comparative example, a resin composition for prepreg was prepared in the same manner as in Example 1, except that 20.0 parts by mass of MC-6000 (melamine cyanurate-based, manufactured by Nissan Chemical Industries, Ltd.) was used as the halogen-free flame retardant instead of 30.0 parts by mass of Firecut P-770. The melamine cyanurate contained in the halogen-free flame retardant is a phosphorus-free compound. A prepreg was produced in the same manner as in Example 1 using the obtained resin composition for prepreg. Test piece A was produced from the obtained prepreg in the same manner as in Example 1 and evaluated. Furthermore, test piece B was produced as a molded article from the obtained prepreg in the same manner as in Example 1 and evaluated.

[0065] Comparative Example 3 In this comparative example, a prepreg resin composition was prepared in the same manner as in Example 1, except that 2.0 parts by mass of "Trigonox 421-70" (organic peroxide) manufactured by Kayaku Nouryon Co., Ltd. was used as the polymerization initiator instead of 1.0 part by mass of Trigonox 122-C80, and no flame retardant was added. Using the obtained prepreg resin composition, a prepreg was produced in the same manner as in Example 1. Test piece A was produced from the obtained prepreg and evaluated in the same manner as in Example 1. Furthermore, using the obtained prepreg, test piece B was produced as a molded body in the same manner as in Example 1 and evaluated, except that the molding conditions were changed to a pressure of 4 MPa, an upper mold temperature of 110°C, a lower mold temperature of 105°C, and a molding time of 8 minutes.

[0066] Tables 2 and 3 below show the formulations of the resin compositions for prepregs, the evaluation results of the prepregs, and the evaluation results of the molded articles.

[0067]

[0068]

[0069] The prepregs of Examples 1 to 6 contain a halogen-free phosphorus compound as a flame retardant. As shown in Tables 2 and 3, the molded articles produced from the prepregs of Examples 1 to 6 were all UL94 rated V-0 or V-1. This confirmed that the prepregs of Examples 1 to 6 can produce molded articles with excellent flame retardancy. Furthermore, the prepregs of Examples 1 to 6 all had a short time to reach the peak top temperature, confirming that they had excellent fast-curing properties.

[0070] On the other hand, the prepregs of Comparative Examples 1 and 3 did not contain any flame retardant. Furthermore, the prepreg of Comparative Example 2 contained a compound that did not contain either halogen or phosphorus as a flame retardant. As shown in Table 3, the molded articles produced from the prepregs of Comparative Examples 1 to 3 did not fall into any of the UL94 ratings of V-0 to V-2. This confirmed that the prepregs of Comparative Examples 1 to 3 could not produce molded articles with excellent flame retardancy. Furthermore, the prepreg of Comparative Example 2 took a long time to reach the peak top temperature, confirming poor fast-curing properties.

Claims

1. A prepreg comprising a urethane (meth)acrylate (A), an ethylenically unsaturated monomer (B) other than the urethane (meth)acrylate (A), a polymerization initiator (C), reinforcing fibers (D), and a flame retardant (E), wherein the urethane (meth)acrylate (A) is a reaction product of a polyisocyanate (a1) and a polyol (a2) having an ethylenically unsaturated group and an aromatic skeleton, and / or a reaction product of the polyisocyanate (a1), a polyol (a3) ​​having no ethylenically unsaturated group but an aromatic skeleton, and a hydroxyalkyl (meth)acrylate (a4), and the flame retardant (E) comprises one or more halogen-free phosphorus compounds.

2. The prepreg according to claim 1, wherein the halogen-free phosphorus compound is a phosphorus compound that does not contain active hydrogen.

3. The prepreg according to claim 1, wherein the halogen-free phosphorus compound is an ammonium phosphate salt.

4. A molded article which is a cured product of the prepreg according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Flame retardant comprising reactive group-containing cyclic phosphazene compound and method for producing the same

    JP2008088217A

  • Photosensitive composition, photosensitive film, photosensitive laminate, method for forming permanent pattern, and printed board

    JP2012073589A

  • Flame-retardant resin composition

    JP2012193300A

  • Prepreg and molded article

    WO2021131564A1

  • Resin composition, prepreg, resin-coated film, resin-coated metal foil, metal-clad laminate, and wiring board

    WO2022259851A1

Cited By

  • Prepreg and fiber-reinforced plastic

    WO2026126699A1