Release film for molding ceramic green sheet

The release film with a polyester base and an antistatic layer addresses antistatic and transportability issues in ceramic green sheet molding, enhancing the quality and reducing defects in multilayer ceramic capacitors by using a release film with a specific antistatic layer configuration.

WO2024247759A1PCT designated stage expired Publication Date: 2024-12-05TOYOBO CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018264
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-30
Filing Date
2024-05-17
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional release films for molding ceramic green sheets face issues with antistatic performance, film transportability, and surface smoothness, leading to defects like pinholes, short circuits, and misalignment in multilayer ceramic capacitors, especially with the miniaturization and increased capacity of these components.

Method used

A release film with a polyester base material, a release layer, and an antistatic layer containing an antistatic resin and wax, where the two surfaces of the base material have different roughness, and the antistatic layer has a specific wax content and thickness, ensuring excellent antistatic properties and smoothness.

Benefits of technology

The solution effectively suppresses electrification during transportation and peeling, improves film transportability, and prevents pinhole formation and misalignment, ensuring high-quality ceramic green sheet molding with reduced defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The purpose of the present invention is to provide a release film for molding a ceramic green sheet, wherein the release film achieves both antistatic performance and film transportability, suppresses falling of an antistatic agent, and has smoothness. This release film for molding a ceramic green sheet has a release layer, a polyester film serving as a substrate, and an antistatic layer in this order. The roughnesses of two surfaces of the substrate are different, the antistatic layer contains an antistatic resin and wax, the region surface average roughness (Sa1) of the release layer is less than 10 nm, and the region surface average roughness (Sa1) of the release layer and the region surface average roughness (Sa2) of the antistatic layer satisfy 0.02<Sa1 / Sa2<0.5.
Need to check novelty before this filing date? Find Prior Art

Description

Release film for ceramic green sheet molding

[0001] The present invention relates to a release film for molding ceramic green sheets, and more particularly to a release film used when molding ultra-thin ceramic green sheets.

[0002] Conventionally, release films, which have a polyester film as a base material and a release layer laminated thereon, have been used as process films for molding ceramic green sheets such as adhesive sheets, cover films, polymer films, and optical lenses.

[0003] The release film is also used as a process film for molding ceramic green sheets, which require high smoothness for multilayer ceramic capacitors, ceramic substrates, etc. Ceramic green sheets are molded by coating a release film with a slurry containing ceramic components such as barium titanate and a binder resin and drying it. Electrodes are printed on the molded ceramic green sheets, which are then peeled off from the release film. The resulting ceramic green sheets are then laminated, pressed, fired, and coated with external electrodes to produce multilayer ceramic capacitors.

[0004] In recent years, as multilayer ceramic capacitors have become smaller and larger in capacity, the thickness of ceramic green sheets has also tended to decrease. In the manufacturing process of thinner ceramic green sheets, slight protrusions on the release film can cause defects such as pinholes during the coating and drying process of the ceramic green sheets, resulting in short circuits in multilayer ceramic capacitors using the ceramic green sheets. Therefore, there is a demand for release films with a smooth release surface on which the ceramic green sheets are coated.

[0005] However, as the release film becomes smoother, the amount of static electricity increases when the film roll is unwound and wound up, which poses an operational problem.

[0006] To address the above-mentioned problems, various efforts have been made to impart antistatic properties to release films for producing ceramic green sheets. Patent Document 1 discloses mixing an antistatic component into the release layer itself, while Patent Document 2 discloses providing an antistatic layer as an undercoat layer before providing the release layer.

[0007] On the other hand, a technique has been proposed in which an antistatic layer is provided on the surface opposite to the processing surface on which the ceramic green sheet is provided, as in Patent Document 3. Also, Patent Document 4 has proposed an antistatic layer formed on the side opposite to the release layer of a release film, which contains a cationic polymer compound and a slippage improver.

[0008] JP 2011-206996 A JP 2010-155459 A JP 2006-130724 A JP 10-315373 A

[0009] In the process of printing electrodes on molded ceramic green sheets, an electrode paste is screen-printed on the ceramic green sheet surface of a roll of release film with the ceramic green sheet, and then the sheet is continuously placed in a dryer to dry and then wound up into a roll. During this process, the surface opposite the electrode-printed surface, i.e., the surface of the release film opposite the processing surface where the ceramic green sheet is to be placed, comes into contact with a support in the dryer, resulting in friction during transport. This can lead to various problems, such as the introduction of foreign matter due to charging caused by friction and misalignment of the printing process due to friction-related film transport problems.

[0010] Furthermore, although the techniques described in Patent Documents 1 and 2 are effective in suppressing the generation of charge upon peeling when the ceramic green sheet is peeled from the release film, they do not take into consideration the generation of charge during transportation.

[0011] The techniques of Patent Documents 3 and 4 are effective in terms of antistatic properties, but do not take into consideration the transportability of the release film, and are unable to solve problems such as deviations in the printing process due to problems with film transport caused by friction.Furthermore, no consideration is given to the peeling off of the antistatic layer due to friction between the antistatic layer and the support in the dryer, which has led to new problems due to the peeling off of the antistatic substance, etc.

[0012] The present invention has been made in view of the problems of the prior art, and aims to provide a release film for molding ceramic green sheets that satisfies both antistatic properties and film transportability, suppresses the detachment of the antistatic layer, and has smoothness.

[0013] As a result of extensive research to solve the above problems, the present inventors have found that the above object can be achieved by a release film having the following configuration, and have completed the present invention.

[0014] That is, the present invention has the following configurations. [1] A release film for molding ceramic green sheets, comprising a release layer, a polyester film as a substrate, and an antistatic layer, in this order, wherein the substrate has two surfaces with different roughnesses, the antistatic layer contains an antistatic resin and a wax, the area surface average roughness (Sa1) of the release layer is less than 10 nm, and the area surface average roughness (Sa1) of the release layer and the area surface average roughness (Sa2) of the antistatic layer satisfy the following formula: 0.02<Sa1 / Sa2<0.5. [2] The release film for molding ceramic green sheets according to [1] above, wherein the content of the wax is 1% by mass or more and 60% by mass or less, relative to 100% by mass of the total solids content in the antistatic layer. [3] The release film for molding ceramic green sheets according to [1] above or [2] above, wherein the wax includes a polyolefin wax. [4] The release film for molding a ceramic green sheet according to any one of [1] to [3] above, wherein the antistatic layer has a thickness of 0.005 to 0.1 μm. [5] The release film for molding a ceramic green sheet according to any one of [1] to [4] above, wherein the antistatic resin is an acrylic resin having a cationic functional group.

[0015] The release film for molding ceramic green sheets of the present invention not only has excellent antistatic properties but also has excellent flatness of the release layer, so it can be suitably used for molding ceramic green sheets in the thin layer region.

[0016] For example, in the process of printing electrodes on a molded ceramic green sheet, the present invention can suppress charging due to friction when the surface of the release film opposite the processing surface where the ceramic green sheet is placed comes into contact with a support in a dryer and the sheet is transported while experiencing friction.

[0017] The present invention can suppress charging during transport, thereby preventing the inclusion of foreign matter due to charging caused by friction. Furthermore, the transportability is good, and poor film winding and wrinkles that may occur during film transport can be suppressed.

[0018] Furthermore, the present invention provides a good balance between good antistatic properties and windability, which can prevent breakage of the green sheet when molding the thin layer region of the ceramic green sheet, and can also prevent misalignment of the printed electrodes.

[0019] Additionally, the present invention not only suppresses the generation of charge when the ceramic green sheet is peeled off from the release film, but also suppresses the generation of charge during transportation.

[0020] The present invention also provides excellent adhesion between the substrate and the antistatic layer, preventing the antistatic layer from falling off due to friction between the antistatic layer and the support in the dryer. Furthermore, it can suppress process contamination and pinhole formation in the green sheet caused by the antistatic resin falling off the antistatic layer, thereby solving new problems caused by the falling antistatic resin.

[0021] The present invention will now be described in more detail.

[0022] [Polyester Film] The polyester constituting the polyester film used as the substrate in the release film of the present invention is not particularly limited, and a film molded version of a polyester commonly used as a release film substrate can be used. However, a crystalline linear saturated polyester composed of an aromatic dibasic acid component and a diol component is preferred. For example, polyethylene terephthalate, polyethylene-2,6-naphthalate, polybutylene terephthalate, polytrimethylene terephthalate, or a copolymer primarily composed of these resin components is more preferred, with a polyester film formed from polyethylene terephthalate being particularly preferred. The polyethylene terephthalate preferably contains 90 mol% or more, more preferably 95 mol% or more, of ethylene terephthalate repeating units. While small amounts of other dicarboxylic acid components and diol components may be copolymerized, from a cost perspective, polyethylene terephthalate produced solely from terephthalic acid and ethylene glycol is preferred. Furthermore, known additives, such as antioxidants, light stabilizers, UV absorbers, and crystallization agents, may be added within limits that do not impair the effects of the film of the present invention. The polyester film is preferably a polyethylene terephthalate film due to its high bidirectional elastic modulus.

[0023] The intrinsic viscosity of the polyethylene terephthalate film is preferably 0.50 to 0.70 dl / g, more preferably 0.52 to 0.62 dl / g. When the intrinsic viscosity is 0.50 dl / g or more, breakage is less likely to occur during the stretching process, which is preferable. Conversely, when the intrinsic viscosity is 0.70 dl / g or less, cuttability is good when cutting to a predetermined product width, and dimensional defects do not occur, which is preferable. In addition, it is preferable to thoroughly vacuum dry the raw material.

[0024] The method for producing the polyester film of the present invention is not particularly limited, and any conventionally used method can be used. For example, the polyester can be melted in an extruder, extruded into a film, and cooled on a rotating cooling drum to obtain an unstretched film, which can then be uniaxially or biaxially stretched. A biaxially stretched film can be obtained by sequentially biaxially stretching a uniaxially stretched film in the longitudinal or transverse direction, or by simultaneously biaxially stretching an unstretched film in the longitudinal and transverse directions.

[0025] In the present invention, the stretching temperature during stretching of the polyester film is preferably equal to or higher than the second-order transition temperature (Tg) of the polyester, and the stretching is preferably 1 to 8 times, particularly 2 to 6 times, in both the longitudinal and transverse directions.

[0026] The polyester film preferably has a thickness of 12 to 50 μm, more preferably 12 to 38 μm, and even more preferably 15 to 31 μm. A film thickness of 12 μm or more is preferred because there is no risk of deformation due to heat during film production, the release layer processing step, or the molding of the ceramic green sheet. On the other hand, a film thickness of 50 μm or less is preferred in terms of reducing the environmental load because the amount of film discarded after use is not excessively large, and further preferred from an economical standpoint because less material is used per area of ​​the release film.

[0027] The polyester film substrate may be a single layer or a multilayer of two or more layers, but is preferably a laminated polyester film having a flat layer A substantially free of inorganic particles on at least one side. In the case of a laminated polyester film having a multilayer structure of two or more layers, it is preferable to have a lubrication layer that can contain particles on the side opposite the layer that is substantially free of inorganic particles. The layer structure may be a layer structure such as release layer / flat layer / lubrication layer / antistatic layer, or release layer / flat layer / core layer / lubrication layer / antistatic layer, where the layer on the side to which the release layer is applied is the flat layer A, the layer on the opposite side is the lubrication layer, and the other core layer is the core layer. Of course, the core layer C may be a multilayer structure. In the polyester film substrate of the present invention, the flat layer A that forms the surface to which the release layer is applied preferably does not substantially contain inorganic particles. In this case, the area surface average roughness (Sa) of the flat layer A is preferably 10 nm or less. When Sa is 10 nm or less, the thickness of the release layer is 2.0 μm or less, and even thinner, even if it is 0.5 μm or less, pinholes and the like are less likely to occur during molding of the laminated ultrathin ceramic green sheet, which is preferable. The smaller the regional average surface roughness (Sa) of the flat layer A, the more preferable it is, but it may be 0.1 nm or more. However, when an anchor coat layer or the like described below is provided on the flat layer A, it is preferable that the coat layer does not substantially contain inorganic particles, and it is preferable that the regional average surface roughness (Sa) after lamination of the coat layer is within the above range.

[0028] In order to make the present invention easier to understand, the area surface average roughness of the release layer surface on the substrate is sometimes referred to as (Sa1), but unless otherwise specified, the area surface average roughness (Sa1) means the area surface average roughness of the release layer.

[0029] In the present invention, "substantially free of inorganic particles" is defined as a content of inorganic elements quantified by fluorescent X-ray analysis of 50 ppm or less, preferably 10 ppm or less, and most preferably below the detection limit. This is because even if inorganic particles are not actively added to the film, contaminants derived from foreign matter or dirt adhering to the raw material resin or the production line or equipment in the film manufacturing process may peel off and be mixed into the film.

[0030] When the polyester film substrate in the present invention is a laminated film, the lubrication layer forming the surface opposite to the flat layer A on which the release layer is applied preferably contains particles, particularly silica particles and / or calcium carbonate particles, from the viewpoints of the film's lubricity and ease of air escape. The particle content is preferably 5,000 to 15,000 ppm in total in the lubrication layer. In this case, the area surface average roughness (Sa) of the lubrication layer is preferably in the range of 1 to 40 nm, more preferably in the range of 5 to 35 nm.

[0031] The present invention has an antistatic layer on the side of the polyester film opposite to the side on which the release layer is provided. Here, when the polyester film has a lubrication layer, the antistatic layer is disposed on the lubrication layer. By having the average surface roughness (Sa) of the film region constituting the lubrication layer within the above range, it is possible to prevent the average roughness (Ra2) of the antistatic layer from becoming excessive.

[0032] To facilitate understanding of the present invention, the area surface average roughness of the surface of the substrate facing the antistatic layer is sometimes referred to as (Sa2), but unless otherwise specified, the area surface average roughness (Sa2) means the area surface average roughness of the antistatic layer.

[0033] By setting the area surface average roughness (Sa) of the film of the easy-slip layer within the above range and further including an antistatic resin and a wax in the antistatic layer, the area surface average roughness (Ra2) of the antistatic layer can exhibit the relationship expressed as 0.02<Sa1 / Sa2<0.5.

[0034] Although not intended to be limited to any particular theory, the synergistic effect of the antistatic resin and wax of the present invention prevents the surface shape of the polyester film from being directly transferred to the antistatic layer, and leads to the regional average surface roughness (Sa2) of the antistatic layer.

[0035] Therefore, (Sa1 / Sa2) falls within a predetermined range, and the present invention can, for example, provide a good balance of good antistatic properties and winding properties, suppress damage to the green sheet when molding the ceramic green sheet in the thin layer region, and further suppress misalignment of the printed electrodes.

[0036] When the total amount of silica particles and / or calcium carbonate particles in the lubricating layer is 5000 ppm or more and Sa is 1 nm or more, air can be uniformly released when the film is wound into a roll, and the film has a good wound appearance and good flatness, making it suitable for producing an ultrathin ceramic green sheet. Also, when the total amount of silica particles and / or calcium carbonate particles is 15000 ppm or less and Sa is 40 nm or less, the lubricant is less likely to aggregate and large protrusions are not formed, so that defects such as pinholes do not occur in the ceramic green sheet even when the ultrathin ceramic green sheet is wound after molding, which is preferable.

[0037] As the particles contained in the lubrication layer, silica particles and / or calcium carbonate particles are more preferably used from the viewpoints of transparency and cost. In addition to silica and / or calcium carbonate, inert inorganic particles and / or heat-resistant organic particles can also be used, and other usable inorganic particles include alumina-silica composite oxide particles and hydroxyapatite particles. Heat-resistant organic particles include cross-linked polyacrylic particles, cross-linked polystyrene particles, and benzoguanamine particles. When silica particles are used, porous colloidal silica is preferred, and when calcium carbonate particles are used, light calcium carbonate that has been surface-treated with a polyacrylic acid-based polymer compound is preferred from the viewpoint of preventing the lubricant from falling off.

[0038] The average particle diameter of the particles added to the lubrication layer is preferably 0.1 μm or more and 2.0 μm or less, and particularly preferably 0.5 μm or more and 1.0 μm or less. An average particle diameter of 0.1 μm or more is preferable because the release film has good slip properties. Furthermore, an average particle diameter of 2.0 μm or less is preferable because there is no risk of pinholes being generated on the surface of the release layer due to coarse particles. The average particle diameter of the particles can be measured by observing the particles on the cross section of the processed film using a scanning electron microscope, observing 100 particles, and calculating the average particle diameter. The shape of the particles is not particularly limited as long as it satisfies the objectives of the present invention, and spherical particles and irregular, non-spherical particles can be used. The particle diameter of irregular particles can be calculated as the equivalent circle diameter. The equivalent circle diameter is calculated by dividing the area of ​​the observed particles by pi (π), calculating the square root, and then multiplying it by two.

[0039] The lubrication layer may contain two or more types of particles made of different materials, or may contain particles of the same type but with different average particle sizes.

[0040] When the lubrication layer does not contain particles, it is also preferable to provide the lubrication layer with a coating layer containing particles. The means for providing this coating layer is not particularly limited, but it is preferable to provide it by the so-called in-line coating method in which the coating is applied during the film formation of the polyester film. Furthermore, when a coating layer that provides lubrication is provided on the surface of the polyester film on the side on which the release layer is not laminated, the polyester film does not need to have a flat layer and a lubrication layer, and may be made of a single-layer polyester film that does not substantially contain inorganic particles.

[0041] As will be described later, an antistatic layer may be provided simultaneously with the lubricious coating layer by in-line coating.

[0042] The area surface average roughness (Sa) of the lubrication layer is preferably 40 nm or less, more preferably 35 nm or less, and even more preferably 30 nm or less.On the other hand, the area surface average roughness of the lubrication layer needs to be larger than the area surface average roughness of the flat layer, so it is preferably 10 nm or more.In addition, even when the surface of the lubrication layer or the monolayer polyester film on the side on which the release layer is not laminated is made slippery by a coating layer, the Sa of the surface is measured by the surface on which the coating layer is laminated, and it is preferably in the same range as the area surface average roughness (Sa) of the lubrication layer B.For example, the area surface average roughness (Sa) of the film of the coating layer (slippery layer) may be 10 nm or more and 40 nm or less, or 10 nm or more and 35 nm or less.

[0043] (Coat Layer (Slippery Layer)) The coat layer on the surface of the polyester film on which the release layer is not laminated preferably contains at least a binder resin and particles.

[0044] (Binder Resin of Slippery Layer) The binder resin constituting the coating layer (slippery layer) is not particularly limited, and specific examples of polymers include polyester resin, acrylic resin, urethane resin, polyvinyl resin (such as polyvinyl alcohol), polyalkylene glycol, polyalkyleneimine, methyl cellulose, hydroxycellulose, starch, etc. Among these, polyester resin, acrylic resin, and urethane resin are preferably used from the viewpoint of particle retention and adhesion. Furthermore, considering compatibility with polyester film, polyester resin is particularly preferred. In order to achieve solubility and dispersibility in solvents and further adhesion to the base film and other layers, the binder polyester is preferably a copolymer polyester. The polyester resin may be polyurethane-modified. Furthermore, another preferred binder resin constituting the coating layer (sometimes referred to as a slippery layer or a slippery coating layer) on a polyester base film is urethane resin. Examples of urethane resins include polycarbonate polyurethane resin. Furthermore, polyester resins and polyurethane resins may be used in combination, and the other binder resins described above may be used in combination.

[0045] (Crosslinking agent for coating layer) In the present invention, the coating layer may be formed containing a crosslinking agent in order to form a crosslinked structure in the coating layer. By including a crosslinking agent, it becomes possible to further improve adhesion under high temperature and high humidity conditions. Specific examples of crosslinking agents include urea-based, epoxy-based, melamine-based, isocyanate-based, oxazoline-based, carbodiimide-based, and aziridine-based crosslinkers. Furthermore, in order to promote the crosslinking reaction, a catalyst or the like can be used as needed.

[0046] (Particles in Coating Layer) The easy-to-slip coating layer preferably contains lubricant particles to impart slipperiness to the surface. The particles may be inorganic particles or organic particles, and are not particularly limited. Examples of suitable inorganic particles include: (1) inorganic particles such as silica, kaolinite, talc, light calcium carbonate, heavy calcium carbonate, zeolite, alumina, barium sulfate, carbon black, zinc oxide, zinc sulfate, zinc carbonate, zirconium oxide, titanium dioxide, satin white, aluminum silicate, diatomaceous earth, calcium silicate, aluminum hydroxide, hydrated halloysite, calcium carbonate, magnesium carbonate, calcium phosphate, magnesium hydroxide, and barium sulfate; and (2) organic particles such as acrylic or methacrylic, vinyl chloride, vinyl acetate, nylon, styrene / acrylic, styrene / butadiene, polystyrene / acrylic, polystyrene / isoprene, polystyrene / isoprene, methyl methacrylate / butyl methacrylate, melamine, polycarbonate, urea, epoxy, urethane, phenol, diallyl phthalate, and polyester. Silica is particularly preferred for providing the coating layer with adequate slip properties.

[0047] The average particle size of the particles is preferably 10 nm or more, more preferably 20 nm or more, and even more preferably 30 nm or more. When the average particle size of the particles is 10 nm or more, the particles are less likely to aggregate and lubricity can be ensured, which is preferable.

[0048] The average particle size of the particles is preferably 1000 nm or less, more preferably 800 nm or less, and even more preferably 600 nm or less. When the average particle size of the particles is 1000 nm or less, transparency is maintained and the particles do not fall off, which is preferable.

[0049] Furthermore, for example, it is also preferable to mix small particles having an average particle size of about 10 to 270 nm with large particles having an average particle size of about 300 to 1000 nm, in order to achieve both slipperiness and smoothness by reducing the average length of the roughness curve element (RSm) while maintaining small the regional surface average roughness (Sa) and maximum protrusion height (RP) described below, and it is particularly preferable to combine small particles having an average particle size of 30 nm to 250 nm with large particles having an average particle size of 350 to 600 nm. When small particles and large particles are mixed, it is preferable to make the mass content of the small particles larger than the mass content of the large particles relative to the total solid content of the coating layer.

[0050] From the viewpoint of reducing pinholes, it is preferable that recycled materials are not used for the flat layer, which is the layer on which the release layer is provided, in order to prevent the inclusion of particles such as lubricants.

[0051] The thickness ratio of the flat layer, which is the layer on which the release layer is provided, is preferably 20% to 50% of the total thickness of the base film. If it is 20% or more, the film is less likely to be affected from the inside by particles contained in the lubrication layer B, etc., and the area surface average roughness Sa can easily satisfy the above range, which is preferable. If it is 50% or less of the total thickness of the base film, the proportion of recycled raw materials used in the lubrication layer can be increased, which is preferable because it reduces the environmental impact.

[0052] From an economical standpoint, layers other than the flat layer (the lubrication layer or the aforementioned core layer) may be made from 50 to 90% by mass of recycled raw materials such as film scraps or PET bottles. Even in this case, it is preferable that the type and amount of lubricant contained in the lubrication layer B, its particle size, and the area surface average roughness (Sa) satisfy the above-mentioned ranges.

[0053] In addition, in order to improve the adhesion of a release layer or the like to be applied later, a coating layer may be provided on the surface of the flat layer before stretching or after uniaxial stretching in the film-forming process, and corona treatment or the like may also be performed. When a coating layer is also provided, the Sa of each layer is substituted with the measured value of the coating layer surface. Furthermore, when these coating layers are provided on the surface of the flat layer A, it is preferable that they do not contain particles.

[0054] (Antistatic Layer) In the present invention, an antistatic layer is provided on the side of the polyester film opposite to the side having the release layer, and the antistatic layer contains an antistatic resin and wax.

[0055] Furthermore, the average roughness (Sa1) of the release layer described below is less than 10 nm, and the average roughness (Ra1) of the release layer and the average roughness (Ra2) of the antistatic layer satisfy the following formula: 0.02<Sa1 / Sa2<0.5. The antistatic layer contains an antistatic resin and a wax, and (Ra1 / Ra2) satisfies the specified condition. Therefore, in the present invention, for example, in the process of printing electrodes on a molded ceramic green sheet, when the surface of the release film opposite the processing surface where the ceramic green sheet is to be provided is in contact with a support in a dryer and the sheet is transported while experiencing friction, it is possible to suppress charging due to friction.

[0056] The present invention can suppress charging during transport, thereby preventing the inclusion of foreign matter due to charging caused by friction. Furthermore, the transportability is good, and poor film winding and wrinkles that may occur during film transport can be suppressed.

[0057] Furthermore, the present invention provides a good balance between good antistatic properties and windability, which can prevent breakage of the green sheet when molding the thin layer region of the ceramic green sheet, and can also prevent misalignment of the printed electrodes.

[0058] Additionally, the present invention not only suppresses the generation of charge when the ceramic green sheet is peeled off from the release film, but also suppresses the generation of charge during transportation.

[0059] The present invention also provides excellent adhesion between the substrate and the antistatic layer, preventing the antistatic layer from falling off due to friction between the antistatic layer and the support in the dryer. Furthermore, it can suppress process contamination and pinhole formation in the green sheet caused by the antistatic resin falling off the antistatic layer, thereby solving new problems caused by the falling off of the antistatic resin.

[0060] The antistatic resin constituting the antistatic layer in the release film of the present invention includes a resin having a chargeable or hydrophilic functional group. As the antistatic resin, a vinyl resin having a chargeable or hydrophilic functional group is preferred.

[0061] For example, the antistatic resin may be a polymer type of known antistatic agent, such as an anionic antistatic agent such as an alkyl sulfate type or an alkyl phosphate type, a cationic antistatic agent such as a quaternary ammonium salt type, a quaternary ammonium resin type or an imidazoline type, a nonionic antistatic agent such as a sorbitan type or an ether type, or a polymeric conductive agent such as a composite of poly(3,4-ethylenedioxythiophene) and polystyrene sulfonic acid. Resins having cationic functional groups are preferred as the antistatic resin, and acrylic resins having cationic functional groups are particularly preferred.

[0062] By using the organic antistatic agent as described above, even if conductive organic matter falls off or gets mixed into the ceramic green sheets, it disappears during the firing process of the multilayer ceramic capacitor, making it possible to prevent problems caused by residual conductive material.

[0063] Preferably, the antistatic resin is a cationic antistatic agent. For example, by including a cationic antistatic agent and a wax that is solid under environmental conditions at 25°C, the antistatic layer can achieve a surface resistivity value and a surface resistivity value after abrasion within a predetermined range, thereby suppressing charging due to friction. Furthermore, since charging during transport can be suppressed, the inclusion of foreign matter due to charging due to friction can be suppressed. Furthermore, transportability is also good, and poor film winding and wrinkles that may occur during film transport can be suppressed.

[0064] Furthermore, the present invention provides a good balance between good antistatic properties and windability, which can prevent breakage of the green sheet when molding the thin layer region of the ceramic green sheet, and can also prevent misalignment of the printed electrodes.

[0065] Additionally, the present invention not only suppresses the generation of charge when the ceramic green sheet is peeled off from the release film, but also suppresses the generation of charge during transportation.

[0066] Furthermore, the antistatic layer contains a cationic antistatic agent and a wax that is solid at 25°C, which provides excellent adhesion between the substrate and the antistatic layer, preventing the antistatic layer from falling off due to friction between the antistatic layer and the support in the dryer. Furthermore, process contamination caused by the antistatic resin falling off from the antistatic layer and the generation of pinholes in the green sheet can be suppressed, thereby solving new problems caused by the falling off of the antistatic resin.

[0067] Furthermore, it is essential to add wax to the antistatic layer in the release film of the present invention as a component that imparts easy slippage. Furthermore, in the present invention, by including a wax component in the antistatic layer, it is possible to bring the surface resistivity after abrasion into the range described in this specification.

[0068] This is presumably because the interaction between the antistatic resin contained in the antistatic layer and the wax improves the abrasion resistance of the antistatic layer, thereby preventing a sudden increase in the surface resistivity after the abrasion test.

[0069] As the wax, known waxes such as polyester wax and polyolefin wax can be used, and for example, polyolefin wax is preferred.

[0070] It is presumed that the inclusion of a polyolefin wax in the antistatic layer improves the abrasion resistance of the antistatic layer due to the interaction between the antistatic resin and the wax, thereby preventing a sudden increase in the surface resistivity after the abrasion test. The polyolefin wax may contain one or more polyethylene-based waxes and polypropylene-based waxes.

[0071] Preferably, the wax, particularly the polyolefin wax, is solid under the environmental condition of 25° C. This is because if the wax exists as a liquid at room temperature, there is a possibility that the wax will be significantly transferred to the release layer when the release film is wound into a roll.

[0072] Furthermore, since the wax is solid under an environmental condition of 25° C., it is possible to prevent the surface shape of the polyester film from being directly transferred to the antistatic layer. Without being limited to a specific theory, it is presumed that, since the wax is solid under an environmental condition of 25° C., the surface shape of the polyester film, such as surface roughness and surface height, is alleviated in the antistatic layer, thereby leading to the surface shape of the antistatic layer.

[0073] The melting point or softening point of the wax, particularly the polyolefin wax, is not particularly limited, but is preferably 170° C. or lower, and more preferably, for example, 150° C. or lower, or 120° C. or lower. When the melting point or softening point of the wax is 170° C. or lower, the wax becomes more easily deformed upon friction, and the slipperiness can be promoted.

[0074] In one embodiment, the polyolefin wax has a melting or softening point of 170°C or less, and may be 150°C or less, for example, a melting or softening point of 120°C or less, and is solid at an ambient condition of 25°C.

[0075] The form of the wax is not particularly limited, but is preferably an aqueous dispersion of wax in which the wax is dispersed in an aqueous medium, or an aqueous solution of wax in which the wax is dissolved in an aqueous medium.

[0076] This is because the wax is dispersed or dissolved in an aqueous medium to easily mix with the electrostatic composition that constitutes the antistatic layer. The number average particle size of the wax particles in the aqueous dispersion of wax is not particularly limited, but is 5 μm or less, for example, 0.1 μm or more, from the viewpoints of storage stability and mixing stability.

[0077] In the present invention, the ratio of the mass of the compound having an Si atom to the mass of the wax contained in the antistatic layer is preferably 1 / 50 or less, more preferably 1 / 100 or less. In particular, in the present invention, it is desirable that the antistatic layer contains wax as a lubricant and that the antistatic layer does not substantially contain a compound having an Si atom, particularly a compound having a siloxane bond. This is to prevent the compound having a siloxane bond from being significantly transferred to the release layer when the release film is wound into a roll.

[0078] In the present invention, the phrase "substantially free of compounds having Si atoms" can be defined by the surface Si atomic ratio of the antistatic layer. Specifically, the Si atomic ratio (at %) contained in the antistatic layer is less than 1.0 (at %), preferably 0.5 (at %), or may be less than 0.1 (at %), and most preferably a content below the detection limit.

[0079] This is because even if compounds having Si atoms, particularly compounds having siloxane bonds, are not actively added to the film, contaminants derived from foreign substances and dirt adhering to the raw material resin or the lines and equipment used in the film manufacturing process may peel off and become mixed into the film.

[0080] The Si element ratio can be measured, for example, by ESCA. An example of the device used is a K-Alpha+ (manufactured by Thermo Fisher Scientific). Detailed measurement conditions are as follows: For example, a narrow scan is performed on the five elements C, O, N, S, and Si on the surface of the antistatic layer using a measurement device, and the Si element ratio (at %) can be calculated from the results using the following formula: (In the present invention, the Si element ratio is defined as the proportion (at %) of Si among the five elements C, O, N, S, and Si.) Si element ratio (at %) = {Si / (C + O + N + S + Si)} × 100 ... Formula. During analysis, background removal was performed using the Shirley method. The surface Si element ratio was calculated as the average value of measurement results from three or more locations.

[0081] Measurement conditions: Excitation X-ray: Monochromatized AlKa ray, X-ray output: 12 kV, 6 mA, Photoelectron escape angle: 90°, Spot size: 400 mmf (approximately), Pass energy: 50 eV, Step: 0.1 eV. The wax content in 100% by mass of the total solid content of the antistatic layer is 1% by mass or more and 65% by mass or less. The wax mixing ratio is, for example, 10% by mass or more and 60% by mass or less, or 14% by mass or more and 56% by mass or less.

[0082] By setting the wax ratio to 1% by mass or more, sufficient lubricity can be ensured between the release layer and the antistatic layer, or between the antistatic layer and various metal materials or rubber materials, such as transport rolls during the green sheet molding process or supports in a dryer, etc. Furthermore, deterioration of the antistatic ability due to peeling of the antistatic layer can be suppressed.

[0083] On the other hand, if the wax ratio is 65% by mass or less, excess wax can be prevented from contaminating the release layer or the transport process during the green sheet molding process, and the film can be prevented from meandering during transport or from causing poor winding when wound up due to excessive slippage.

[0084] In addition to the wax for the conductive organic substance, the antistatic layer may contain a binder, a crosslinking agent, a curing catalyst, etc., to the extent that the antistatic property and the lubricity are not impaired. Furthermore, when the antistatic layer and the lubricity layer are simultaneously formed by the in-line coating method as described above, particles may be added as a lubricity component.

[0085] The thickness of the antistatic layer is preferably 0.005 to 0.1 μm, and particularly preferably 0.01 to 0.05 μm. If the thickness of the antistatic layer is 0.005 μm or less, it will not function as an antistatic layer. On the other hand, if the thickness of the antistatic layer is 0.1 μm or more, peeling of the coating film from the antistatic layer will occur, which is undesirable.

[0086] The area surface average roughness (Sa2) of the antistatic layer is 10 nm or more and 40 nm or less, and may be 10 nm or more and 35 nm or less.

[0087] The average roughness (Sa1) of the release layer and the average roughness (Sa2) of the antistatic layer satisfy the following formula: 0.02<Sa1 / Sa2<0.5. Preferably, 0.03<Sa1 / Sa2<0.35, and may be 0.03<Sa1 / Sa2<0.25, for example, 0.035<Sa1 / Sa2<0.25, and may be 0.035<Sa1 / Sa2<0.150.

[0088] By satisfying these conditions, the release surface maintains its smoothness, and the surface opposite the release surface has a suitable surface roughness, making it possible to ensure easy slippage of the entire film.

[0089] On the other hand, if Sa1 / Sa2 is 0.02 or less, the opposite side (antistatic layer) may be too rough compared to the smoothness of the release surface of the film, which may cause the particles that make up the smooth surface to easily fall off, or the roughness of the opposite side may be transferred to the release surface, resulting in the risk of pinholes occurring during the production of ceramic green sheets.

[0090] If Sa1 / Sa2 is 0.5 or more, the film may have insufficient slipperiness.

[0091] The surface resistivity [Rs value] of the antistatic layer is 1.0×10 6 ~1.0 x 10 12 (Ω / □), preferably 1.5×10 9 ~1.0 x 10 11 (Ω / □).

[0092] By having the surface resistivity within the above range, when the release film is used for processing, it is possible to achieve the effect of suppressing charging when the film is wound into a roll and unwound, and frictional charging when the film comes into contact with the processing machine base.

[0093] In the present invention, with regard to the relationship between the surface resistivity, the measurement method of which is described in the Examples, and the surface resistivity after abrasion, the antistatic layer having the configuration of the present invention can reduce fluctuations in the surface resistivity even after abrasion. That is, the present invention can prevent the antistatic layer from peeling off from the polyester substrate and from being partially scraped off, even after the antistatic layer is abraded.

[0094] The above relationship between the surface resistivity of the antistatic layer and the surface resistivity after abrasion can prevent the antistatic layer from falling off due to friction between the antistatic layer and the support in the dryer. Furthermore, process contamination caused by the antistatic resin falling off the antistatic layer and the generation of pinholes in the green sheet can be suppressed, and new problems caused by the falling off of the antistatic resin can also be solved.

[0095] In the antistatic layer of the present invention, the dynamic friction coefficient (μd) is, for example, more than 0.10 μd and not more than 0.45 μd, or may be more than 0.12 μd and not more than 0.40 μd, or may be more than 0.12 μd and not more than 0.35 μd, for example, 0.13 μd or more and not more than 0.26 μd.

[0096] In the present invention, by ensuring that the dynamic friction coefficient is within the above range and that Sa1 / Sa2 satisfies a predetermined relationship, it is possible to achieve a good balance between suppressing particle shedding and suppressing unwinding electrification.

[0097] (Release Layer) The material constituting the release layer of the release film for molding ceramic green sheets according to this embodiment is not particularly limited as long as it satisfies the flatness required for the release layer. For example, known materials such as silicone compounds, fluorine compounds, alkyd compounds, melamine compounds, and epoxy compounds can be used.

[0098] In one embodiment, the release layer includes polydimethylsiloxane. It may also include at least two types of polydimethylsiloxane. For example, the release layer may include a vinyl-modified silicone resin having at least one vinyl group in the polydimethylsiloxane structure as the first polydimethylsiloxane, and a polymethylhydrogensiloxane having at least one hydrosilyl group in the polydimethylsiloxane structure as the second polydimethylsiloxane.

[0099] By including polydimethylsiloxane in the release layer and the antistatic layer of the present invention, the difference in surface free energy between the release layer and the antistatic layer is reduced, which prevents the wax in the antistatic layer from migrating to the release layer and allows the antistatic layer to maintain its abrasion resistance even after long-term storage.

[0100] The film thickness of the release layer in the present invention is preferably 0.001 to 0.2 μm, more preferably 0.005 to 0.1 μm, as the thickness after drying. A thickness of 0.001 μm or more is preferred because a release layer with excellent releasability can be obtained. A thickness of 0.2 μm or less is preferred because it is not necessary to increase the solid content concentration of the release layer components or the coating amount, and excellent coatability can be obtained when applying the release layer to a substrate film.

[0101] In the present invention, the method for forming the release layer is not particularly limited, and a method is used in which a coating liquid in which a release compound is dissolved or dispersed is spread by coating or the like on one side of the polyester film substrate, the solvent is removed by drying, and then the resulting layer is cured. Alternatively, the release layer may be provided simultaneously with the formation of the polyester film by an in-line coating method.

[0102] The area surface average roughness (Sa1) of the release layer is 0.1 nm or more and 10 nm or less, for example, 0.3 nm or more and 8 nm or less. For example, the area surface average roughness (Sa1) of the release layer is within the range of the surface average roughness (Sa1) of the surface of the substrate facing the release layer ±2 nm, and may be in the range of ±1.5 nm or ±1.2 nm. By including the first and second polydimethylsiloxanes according to the present invention, the release layer exhibits high smoothness and excellent ceramic peeling force, and further, the difference in surface free energy between the release layer and the antistatic layer can be reduced.

[0103] (Release Film for Molding Ceramic Green Sheet) The release film for molding ceramic green sheet of the present invention has a release layer on one side of a polyester film and an antistatic layer on the side opposite to the side having the release layer on one side of the polyester film.

[0104] In the present invention, the release layer and the antistatic layer are provided separately on both sides of the polyester film, and the average roughness (Sa1) of the release layer is small and the average roughness (Sa2) of the antistatic layer is larger than that, preferably satisfying the relationship 0.02<Sa1 / Sa2<0.5, so that the antistatic layer does not inhibit the releasability or flatness of the release layer, and the exposed antistatic layer can prevent unwinding charging during film transport.

[0105] Furthermore, with the above structure, it is possible to prevent the generation of charge when the ceramic green sheet is peeled off. Although the mechanism behind this is unclear, it is thought that the charge generated during peeling is quickly transferred to the antistatic layer on the back side.

[0106] On the other hand, by adding a wax component to the antistatic layer, it is possible to overcome problems such as a release layer with a large average roughness damaging the release layer, or the convex parts of the antistatic layer being scraped off and falling off during film transport.

[0107] The order in which the release layer and the antistatic layer are provided on the film is not particularly limited. The antistatic layer may be provided after the release layer is provided, or the release layer may be provided after the antistatic layer is provided together with the lubricating coating layer by in-line coating. Furthermore, the release layer and the antistatic layer may be provided simultaneously, regardless of whether in-line coating or off-line coating is used.

[0108] (Second embodiment) In another embodiment, the present invention provides the following release film for molding a ceramic green sheet.

[0109] A release film for molding ceramic green sheets, comprising: a polyester film as a substrate; a release layer on one side of the polyester film; and an antistatic layer on the side of the polyester film opposite to the side with the release layer, wherein the substrate has two sides with different roughnesses; the polyester film contains particles on the release layer side and the antistatic layer side; the antistatic layer contains an antistatic resin and a wax; the release layer has a regional surface average roughness (Sa1) of 3 nm or more and less than 10 nm; and the regional surface average roughness (Sa1) of the release layer and the regional surface average roughness (Sa2) of the antistatic layer satisfy the following formula: 0.02<Sa1 / Sa2<0.5.

[0110] In this embodiment, the polyester film as the substrate contains particles at least on the release layer side and the antistatic layer side, and preferably the average surface roughness of the area on the release layer side is smaller than the average surface roughness of the area on the antistatic layer side.

[0111] The area on the mold layer side has an average surface roughness of 3 nm to 10 nm, for example, 3 nm to 8 nm, while the area on the antistatic layer side has an average surface roughness of 5 nm to 25 nm, for example, 5 nm to 20 nm.

[0112] Furthermore, the average surface roughness (Sa1) of the release layer and the average surface roughness (Sa2) of the antistatic layer satisfy the following formula: 0.02<Sa1 / Sa2<0.5.

[0113] For example, in the process of printing electrodes on a molded ceramic green sheet, such a release film can suppress charging due to friction when the surface of the release film opposite the processing surface where the ceramic green sheet is to be placed comes into contact with a support in a dryer and the sheet is transported while experiencing friction.

[0114] The present invention can suppress charging during transport, thereby preventing the inclusion of foreign matter due to charging caused by friction. Furthermore, the transportability is good, and poor film winding and wrinkles that may occur during film transport can be suppressed.

[0115] Furthermore, the present invention provides a good balance between good antistatic properties and windability, which can prevent breakage of the green sheet when molding the thin layer region of the ceramic green sheet, and can also prevent misalignment of the printed electrodes.

[0116] Additionally, the present invention not only suppresses the generation of charge when the ceramic green sheet is peeled off from the release film, but also suppresses the generation of charge during transportation.

[0117] The present invention also provides excellent adhesion between the substrate and the antistatic layer, preventing the antistatic layer from falling off due to friction between the antistatic layer and the support in the dryer. Furthermore, it can suppress process contamination and pinhole formation in the green sheet caused by the antistatic resin falling off the antistatic layer, thereby solving new problems caused by the falling off of the antistatic resin.

[0118] Conditions other than the average surface roughness of the substrate, such as the composition of the substrate, the release layer, the antistatic layer, and other various conditions constituting the present invention, can be the same as those described in this specification.

[0119] In this embodiment, the relationship may be 0.1<Sa1 / Sa2<0.5, or 0.2<Sa1 / Sa2<0.5.

[0120] In another aspect, the present invention provides a method for producing a release film for molding a ceramic green sheet.

[0121] In one embodiment, the method of the present invention includes applying a release layer-forming coating liquid to a polyester film as a substrate. In this step, the release layer-forming coating liquid is applied to the surface of the polyester film having the release layer, and the surface is substantially free of particles.

[0122] Preferably, the substrate coated with the release layer-forming coating liquid is loaded into the first drying oven within a time period of 0.1 to 10 seconds after the application of the coating liquid. This is particularly preferably 0.1 to 5 seconds. The drying temperature in the first drying oven may be 70°C to 110°C, or 80°C to 100°C. Furthermore, following the first drying oven, the resulting laminated film may be loaded into a second drying oven. The drying temperature in the second drying oven may be 80°C to 130°C. Preferably, the drying temperature in the first drying oven is set lower than the drying temperature in the second drying oven. In addition to the first and second drying ovens, an additional drying oven may be provided.

[0123] The resulting laminated film is then irradiated with ultraviolet light on a cooling roll to form a release layer. The release layer obtained through such a process can satisfy the various physical properties and effects described in this specification.

[0124] Although not limited to any particular theory, it is believed that in the manufacturing method of the present invention, by controlling the transport time to the first drying oven, the drying temperature in the first drying oven, and the drying temperature in the second drying oven to the above conditions, the first polydimethylsiloxane and the second polydimethylsiloxane contained in the release layer can be kept well dispersed. As a result, the difference in surface free energy between the release layer and the antistatic layer can be reduced, the wax in the antistatic layer can be prevented from migrating to the release layer, and the abrasion resistance of the antistatic layer can be maintained even after long-term storage.

[0125] The production method of the present invention further includes a step of forming an antistatic layer on the surface of the obtained release-coated film opposite to the release layer, for example, by providing a lubrication layer on a polyester film as a substrate and applying an antistatic layer-forming coating liquid to the lubrication layer.

[0126] Preferably, the laminate film coated with the antistatic layer-forming coating liquid is loaded into the first drying oven within a time period of 0.1 to 10 seconds after the application of the coating liquid. This time period is particularly preferably 0.1 to 5 seconds. The drying temperature in the first drying oven may be 70°C to 110°C, or 80°C to 100°C. Furthermore, the resulting laminate film may be loaded into a second drying oven following the first drying oven. The drying temperature in the second drying oven may be 80°C to 130°C. Preferably, the drying temperature in the first drying oven is set lower than the drying temperature in the second drying oven. In addition to the first and second drying ovens, an additional drying oven may be provided.

[0127] In this specification, the first drying oven and the second drying oven may be the same oven, or a first drying oven and a second drying oven may be provided separately for the step of forming the release layer and the step of forming the antistatic layer, respectively. In either step, it is sufficient that the above-mentioned drying conditions are applicable.

[0128] The antistatic layer obtained through such a process can satisfy the various physical properties and effects described in this specification, and further, a release film for molding a ceramic green sheet can be obtained that satisfies the various physical properties and effects described in this specification.

[0129] Although not intended to be limited to any particular theory, in the production method of the present invention, by controlling the transport time to the first drying oven, the drying temperature in the first drying oven, and the drying temperature in the second drying oven to the above-mentioned conditions, the synergistic effect of the antistatic resin and wax contained in the antistatic layer is achieved, and the surface shape of the polyester film is not directly transferred to the antistatic layer, resulting in the regional average surface roughness (Sa2) of the antistatic layer.

[0130] Therefore, the (Sa1 / Sa2) ratio according to the present invention falls within a predetermined range, and the release film obtained by the manufacturing method of the present invention can have, for example, a good balance of good antistatic properties and winding properties, can suppress damage to the green sheet when molding the ceramic green sheet in the thin layer region, and can also suppress misalignment of the printed electrodes.

[0131] In addition, the difference in surface free energy between the release layer and the antistatic layer can be reduced, the wax in the antistatic layer can be prevented from migrating to the release layer, and the abrasion resistance of the antistatic layer can be maintained even after long-term storage.

[0132] The release film of the present invention is produced, for example, through the above steps.

[0133] (Ceramic Green Sheet) The ceramic green sheet of the present invention is not particularly limited as long as it contains a resin. In one embodiment, the release film of the present invention is a release film for molding a ceramic green sheet containing an inorganic compound. Examples of inorganic compounds include metal particles, metal oxides, and minerals, such as calcium carbonate, silica particles, aluminum particles, and barium titanate particles. Because the present invention has a highly smooth release layer, even in an embodiment in which the ceramic green sheet contains such an inorganic compound, defects that can be attributed to inorganic compounds, such as breakage of the ceramic green sheet and difficulty in peeling the ceramic green sheet from the release layer, can be suppressed.

[0134] The resin component forming the ceramic green sheet can be appropriately selected depending on the application. In one embodiment, the ceramic green sheet containing an inorganic compound is a ceramic green sheet. For example, the ceramic green sheet can contain barium titanate as the inorganic compound. Furthermore, the resin component can contain, for example, a polyvinyl butyral resin.

[0135] In one embodiment, the ceramic green sheet has a thickness of 0.2 μm or more and 1.0 μm or less. For example, the present invention can provide a method for producing a release film for producing a ceramic green sheet containing such an inorganic compound. Furthermore, the method for producing a release film for molding a ceramic green sheet according to the present invention may include a step of molding a ceramic green sheet having a thickness of 0.2 μm or more and 1.0 μm or less.

[0136] Furthermore, the laminated polyester film constituting the release film of the present invention has a planar layer substantially free of inorganic particles on the release layer side and a lubrication layer that can contain particles on the antistatic layer side. In the present invention, the antistatic layer contains wax, which makes it possible to prevent particles from falling off the lubrication layer. Furthermore, particle falling off can be prevented more effectively than in conventional release films.

[0137] This is because the presence of wax can suppress the force acting on the particles when the conveying roll and the lubricious layer rub against each other strongly during the production of a multilayer ceramic capacitor.

[0138] Furthermore, the release film of the present invention can significantly suppress charging when the film is unwound. By significantly suppressing charging when the film is unwound, it is possible to suppress process defects such as adhesion of foreign matter caused by charging of the film during the ceramic green sheet production process and generation of sparks, and as a result, it is possible to produce multilayer ceramic capacitors of higher quality.

[0139] (Ceramic green sheet and multilayer ceramic capacitor) Generally, a multilayer ceramic capacitor has a rectangular parallelepiped ceramic body. First internal electrodes and second internal electrodes are alternately provided inside the ceramic body along the thickness direction. The first internal electrodes are exposed at a first end face of the ceramic body. A first external electrode is provided on the first end face. The first internal electrode is electrically connected to the first external electrode at the first end face. The second internal electrode is exposed at a second end face of the ceramic body. A second external electrode is provided on the second end face. The second internal electrode is electrically connected to the second external electrode at the second end face.

[0140] In one aspect, the release film of the present invention is a release film for producing ceramic green sheets and is used to produce such multilayer ceramic capacitors. For example, a method for producing a ceramic green sheet in which the release film for producing a ceramic green sheet of the present invention is used to form a ceramic green sheet can form a ceramic green sheet having a thickness of 0.2 μm or more and 1.0 μm or less. More specifically, the ceramic green sheet is produced, for example, as follows. First, using the release film of the present invention as a carrier film, a ceramic slurry for forming a ceramic element is applied and dried. Ultrathin ceramic green sheets with a thickness of 0.2 to 1.0 μm are in demand. A conductive layer for forming a first or second internal electrode is printed on the applied and dried ceramic green sheet. A ceramic green sheet, a ceramic green sheet printed with a conductive layer for forming a first internal electrode, and a ceramic green sheet printed with a conductive layer for forming a second internal electrode are appropriately laminated and pressed to obtain a mother laminate. The mother laminate is then divided into multiple pieces to produce a green ceramic element. The green ceramic element is then fired to obtain a ceramic element. Thereafter, first and second external electrodes are formed to complete the multilayer ceramic capacitor.

[0141] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples. The property values ​​used in the present invention were evaluated using the following methods.

[0142] (Area surface roughness Sa) Measurement was performed using a non-contact surface shape measurement system (VertScan R550H-M100) under the following conditions: The area surface average roughness (Sa) was calculated by averaging five measurements.

[0143] (Measurement conditions) Measurement mode: WAVE mode Objective lens: 50x 0.5x Tube lens Measurement area: 187 μm x 139 μm (Analysis conditions) Surface correction: 4th order correction Interpolation processing: Full interpolation

[0144] (Peel strength of ceramic green sheet) Slurry composition I consisting of the materials listed below was stirred and mixed for 10 minutes, and then dispersed for 10 minutes using a bead mill with zirconia beads having a diameter of 0.5 mm to obtain a primary dispersion. Slurry composition II consisting of the materials listed below was then added to the primary dispersion so that the ratio of (slurry composition I):(slurry composition II) was 3.4:1.0, and secondary dispersion was performed for 10 minutes using a bead mill with zirconia beads having a diameter of 0.5 mm to obtain a ceramic slurry.

[0145] (Slurry composition I) Toluene 22.3 parts by mass Ethanol 18.3 parts by mass Barium titanate (average particle size 100 nm) 57.5 parts by mass Homogenol L-18 (Kao Corporation) 1.9 parts by mass (Slurry composition II) Toluene 39.6 parts by mass Ethanol 39.6 parts by mass Dioctyl phthalate 3.3 parts by mass Polyvinyl butyral (S-LEC BM-S, manufactured by Sekisui Chemical Co., Ltd.) 16.3 parts by mass 1-ethyl-3-methylimidazolium ethyl sulfate 0.5 parts by mass Next, the release surface of the obtained release film sample was coated using an applicator so that the slurry after drying would be 1.0 μm, and the coating was dried at 60 ° C. for 1 minute, thereby obtaining a release film with a ceramic green sheet. The resulting release film with the ceramic green sheet was neutralized using a static eliminator (Keyence Corporation, SJ-F020), and then peeled using a peel tester (Kyowa Interface Science Co., Ltd., VPA-3, load cell load 0.1 N) at a peel angle of 90°, a peel temperature of 25°C, and a peel speed of 10 m / min. The peeling direction was such that double-sided adhesive tape (Nitto Denko Corporation, No. 535A) was attached to a SUS plate attached to the peel tester, and the release film was fixed on top of it by adhering the ceramic green sheet side to the double-sided tape, and the release film side was pulled to peel it off.

[0146] (Evaluation of pinholes in ceramic green sheets) A ceramic green sheet having a thickness of 1 μm was molded on the release surface of a release film in the same manner as in the evaluation of the releasability of the ceramic slurry. The release film was then peeled off from the molded ceramic green sheet-attached release film to obtain a ceramic green sheet. Light was applied to an area of ​​25 cm2 in the central region in the film width direction of the obtained ceramic green sheet from the side opposite to the side on which the ceramic slurry was applied, and the occurrence of pinholes through which light was visible was observed and visually evaluated according to the following criteria: ○: No pinholes occurred ×: One or more pinholes occurred

[0147] (Slipperiness of Antistatic Layer) Using a Tensilon universal testing machine (RTG-1210, manufactured by A&D Co., Ltd.), the surface of the antistatic layer of the film was placed in contact with a SUS plate, and the static friction coefficient (μs) and dynamic friction coefficient (μd) of the contact surface were measured in accordance with JIS K-7125 under the following conditions: Test piece: width 50 mm x length 60 mm Load: 4.4 kg Test speed: 200 mm / min Friction material: SUS plate

[0148] (Surface Resistivity of Antistatic Layer) After leaving the film in an atmosphere of 23°C and 65% RH for 24 hours, the surface resistivity (Ω / □) of the film surface, i.e., the surface resistivity of the antistatic layer, was measured in that atmosphere using a surface resistance measuring device (Hirestar-IP, manufactured by Mitsubishi Petrochemical Co., Ltd.) at an applied voltage of 500 V.

[0149] (Surface Resistivity of Antistatic Layer After Abrasion Test) The film was rubbed with the load head of a Gakushin-type friction tester (manufactured by Yamaguchi Scientific Industry Co., Ltd.) using pearl paper (Toyobo Ester Film P4255-35, manufactured by Toyobo Co., Ltd.) with gauze (Hakujuji Gauze, manufactured by Hakujuji Co., Ltd.) at the contact point between the load head and the film, with the load of the head being 200 gf / 25 mm2 (5 mm × 5 mm) [0.0785 MPa], and the antistatic layer of the film was rubbed back and forth 10 times. After leaving the film to stand for 24 hours in an atmosphere of 23°C and 65% RH, the surface resistivity (Ω / □) of the rubbed area of ​​the film surface, i.e., the antistatic layer, was measured using a surface resistance measurement device (Hiresta-IP, manufactured by Mitsubishi Petrochemical Co., Ltd.) at an applied voltage of 500 V.

[0150] (Particle shedding) A film (3 cm (film width direction) x 20 cm (film length direction)) was attached to a rub fastness tester (RT-200, manufactured by Daiei Scientific Instruments Co., Ltd.) with the antistatic layer facing up, and aluminum foil (thickness 80 μm, arithmetic average surface roughness 0.03 μm) was used at the contact point between the load head (2 cm x 2 cm, 200 g) and the sample film, and the film was reciprocated 10 times over a distance of 10 cm at a speed of 2 seconds per reciprocation. The obtained film was placed on a black mount, and it was visually confirmed whether powder had fallen off. ○: No powder shedding was observed on the black mount. △: Slight powder shedding was observed overall on the black mount. ×: Powder shedding was observed overall on the black mount.

[0151] (Charge upon unwinding of release film roll) The release film for producing green sheets obtained in each example and each comparative example was wound up into a roll having a width of 400 mm and a length of 5000 m to obtain a release film roll. This release film roll was stored for 30 days in an environment of 40°C and humidity of 50% or less, and then the amount of charge when rewinding at 100 m / min was measured using "KSD-0103" manufactured by Kasuga Electric Co., Ltd. The amount of charge was measured at a point 100 mm immediately after unwinding, and every 500 m of the unwinding length, and the average value was calculated. ○: Less than ±5 kV △: ±5 kV or more, less than 10 kV ×: ±10 kV or more

[0152] (Preparation of polyethylene terephthalate pellets (PET(I))) A continuous esterification reactor consisting of a three-stage complete mixing vessel equipped with a stirrer, a partial condenser, a raw material inlet, and a product outlet was used. TPA (terephthalic acid) was supplied at 2 ton / h, EG (ethylene glycol) was supplied at 2 moles per mole of TPA, and antimony trioxide was supplied in an amount such that the Sb atom concentration in the produced PET was 160 ppm. The resulting slurry was continuously supplied to a first esterification reactor of the esterification reactor and reacted at normal pressure for an average residence time of 4 hours at 255°C. Next, the reaction product in the first esterification reactor was continuously removed from the system and fed to a second esterification reactor, and EG distilled off from the first esterification reactor was fed into the second esterification reactor in an amount of 8 mass% based on the produced PET. Further, an EG solution containing magnesium acetate tetrahydrate in an amount such that the Mg atoms would be 65 ppm based on the produced PET, and an EG solution containing TMPA (trimethyl phosphate) in an amount such that the P atoms would be 40 ppm based on the produced PET were added, and the reaction was carried out at atmospheric pressure for an average residence time of 1 hour at 260°C. Next, the reaction product in the second esterification reactor was continuously removed from the system and fed to a third esterification reactor, and the reaction product was dispersed at 39 MPa (400 kg / cm) using a high-pressure disperser (manufactured by Nippon Seiki Co., Ltd.). 2 0.2% by mass of porous colloidal silica having an average particle size of 0.9 μm, which had been subjected to dispersion treatment at a pressure of 1000 kJ / cm² and an average number of treatments of 5, and 0.4% by mass of synthetic calcium carbonate having an average particle size of 0.6 μm and having an ammonium salt of polyacrylic acid attached thereto at 1% by mass per calcium carbonate, were added as 10% EG slurry, and the reaction was carried out at atmospheric pressure for an average residence time of 0.5 hours at 260°C. The esterification reaction product produced in the third esterification reactor was continuously fed to a three-stage continuous polycondensation reactor for polycondensation, filtered through a filter made of sintered stainless steel fibers with a 95% cut diameter of 20 μm, then ultrafiltered, extruded into water, cooled, and cut into chips to obtain PET chips with an intrinsic viscosity of 0.60 dl / g (hereinafter abbreviated as PET(I)). The lubricant content in the PET chips was 0.6% by mass.

[0153] (Preparation of polyethylene terephthalate pellets (PET(II))) Meanwhile, in the production of the above-mentioned PET(I) chips, PET chips with an intrinsic viscosity of 0.62 dl / g containing no particles such as calcium carbonate or silica were obtained (hereinafter abbreviated as PET(II)).

[0154] (Production of Laminated Film F1) After drying, these PET chips were melted at 285 ° C. and melted at 290 ° C. in separate melt extruders. The mixture was filtered through two stages: a filter made of sintered stainless steel fibers with a 95% cut diameter of 15 μm, and a filter made of sintered stainless steel particles with a 95% cut diameter of 15 μm. The resulting mixture was merged in a feed block, and PET (I) was laminated as the lubricious layer (non-release surface layer) and PET (II) as the flat layer (release surface layer). The resulting mixture was extruded (cast) into a sheet at a speed of 45 m / min, electrostatically bonded to a casting drum at 30 ° C., and cooled to obtain an unstretched polyethylene terephthalate sheet with an intrinsic viscosity of 0.59 dl / g. The layer ratio was adjusted to PET (I) / (II) = 60% by mass / 40% by mass based on the output of each extruder. The unstretched sheet was then heated with an infrared heater and stretched 3.5 times in the machine direction at a roll temperature of 80°C using the speed difference between the rolls. It was then introduced into a tenter and stretched 4.2 times in the transverse direction at 140°C. It was then heat-treated at 210°C in a heat-setting zone. It was then relaxed 2.3% in the transverse direction at 170°C to obtain a biaxially stretched polyethylene terephthalate film F1 with a thickness of 31 μm. The planar layer A of the resulting film F1 had an Sa of 1 nm, and the lubricity layer B had an Sa of 28 nm.

[0155] (Production of Laminated Film F2) Laminated film F2 was prepared in the same manner as laminated film F1, using PET (II) on both the flat layer and the lubricious layer. The laminate was extruded (cast) into a sheet at a speed of 45 m / min, electrostatically bonded to a casting drum at 30°C using an electrostatic bonding method, and cooled to obtain an unstretched polyethylene terephthalate sheet with an intrinsic viscosity of 0.59 dl / g. This unstretched PET sheet was heated to 100°C using a group of heated rolls and an infrared heater, and then stretched 3.5 times in the longitudinal direction using a group of rolls with different peripheral speeds to obtain a uniaxially stretched PET film. Next, the following lubricious coating solution was applied to one side of the PET film using a bar coater and then dried at 80°C for 15 seconds. The coating thickness was adjusted to 0.1 μm after final stretching and drying. The film was then stretched 4.0 times in the width direction at 150°C in a tenter, and while the length of the film in the width direction was fixed, it was heated at 230°C for 0.5 seconds and further subjected to a 3% width direction relaxation treatment at 230°C for 10 seconds to obtain an inline coated polyester film F2 having a thickness of 31 µm. The flat layer A of the obtained film F2 had an Sa of 1 nm, and the lubricity layer B had an Sa of 6 nm.

[0156] (Slip-resistant coating liquid) Water 45.82 parts by mass Isopropyl alcohol 35.00 parts by mass Acrylic polyol resin 10.36 parts by mass (NeoCryl A-614 manufactured by DSM Coating Resins, Tg 74°C, acid value 55%, solid content 32% by mass) Oxazoline-based crosslinking agent D-1 5.68 parts by mass (solid content 25% by mass) Acrylic particle water dispersion 2.37 parts by mass (Nippon Shokubai, product name MX200W, average particle size 350 nm, solid content 10% by mass) Acrylic particle water dispersion 0.47 parts by mass (Nippon Shokubai, product name MX300W, average particle size 450 nm, solid content 10% by mass) Surfactant H-1 (fluorine-based, solid content 10% by mass) 0.30 parts by mass

[0157] (Production of Laminated Film F3) A 25 μm thick E5101 (Toyobo Ester (registered trademark) film, manufactured by Toyobo Co., Ltd.) was used as the laminated film F3. The laminated film F3 was configured so that particles were contained in the flat layer and the lubricious layer. The Sa of the flat layer A of the laminated film F3 was 12 nm, and the Sa of the lubricious layer B was 12 nm.

[0158] (Production of Laminated Film F4) A 38 μm thick A4000 (Toyobo Ester (registered trademark) film, manufactured by Toyobo Co., Ltd.) was used as the laminated film F4. A4000 does not contain particles. The flat layer A of the laminated film F4 had an Sa of 2 nm, and the lubricity layer B had an Sa of 2 nm.

[0159] (Production of Laminated Film F5) A 31 μm thick X3 (Toyobo Ester (registered trademark) film, manufactured by Toyobo Co., Ltd.) was used as the laminated film F5. The laminated film F5 contained particles in the flat layer and the lubricious layer. The Sa of the flat layer A of the laminated film F5 was 6 nm, and the Sa of the lubricious layer B was 15 nm.

[0160] (Production of Laminated Film F6) Laminated film F6 was a 38 μm thick A4000 (Toyobo Ester (registered trademark) film, manufactured by Toyobo Co., Ltd.) film with one side subjected to sand matting. The side of the film subjected to sand matting was the smooth surface, and the opposite side was the flat layer. The flat layer A of laminated film F6 had an Sa of 3 nm, and the smooth layer B had an Sa of 200 nm.

[0161] (Example 1) A release layer forming material R1 was prepared by adjusting the ratio of vinyl groups to hydrosilyl groups to 2.0, using a vinyl-modified silicone resin (weight average molecular weight: 466,000) having at least one vinyl group in the polydimethylsiloxane structure as the first polydimethylsiloxane and a polymethylhydrogensiloxane having at least one hydrosilyl group in the polydimethylsiloxane structure as the second polydimethylsiloxane, and the ratio of vinyl groups to hydrosilyl groups to 2.0. The following release layer forming coating liquid M1 containing the release layer forming material R1 was then prepared.

[0162] (Release layer forming coating liquid M1) Methyl ethyl ketone 64.3 parts by weight Toluene 34.0 parts by weight Release layer forming material R1 1.5 parts by weight Adhesion imparting agent 0.1 parts by weight (Dow Toray Industries, Inc. SD7200 (reaction product of vinyltriacetoxysilane and glycidoxypropyltrimethoxysilane, solids concentration 90% by weight)) Catalyst 0.1 parts by weight (Dow Toray Industries, Inc. SRX212 (platinum complex of 1,1,3,3-tetramethyl-1,3-divinyldisiloxane, solids concentration 5% by weight)) Onto the planar layer A of the laminated film F1, the release layer forming coating liquid M1 having the following composition was applied using reverse gravure so that the coating amount after drying would be 20 nm. Thereafter, the processing speed was adjusted so that the film entered the first drying oven 0.5 seconds later, and the film was continuously heated and dried at a first drying oven temperature of 90 ° C. and a second drying oven temperature of 120 ° C. After the drying process, the film was irradiated on a cooling roll using an ultraviolet irradiator (Heraeus, H bulb) with an integrated light dose of 100 mJ / cm 2 The release layer was cured by irradiating it with ultraviolet light.

[0163] On the obtained release coated film's lubrication layer B, antistatic layer-forming coating solution R1 having the following composition was applied using reverse gravure so that the coating thickness after drying would be 15 nm. Thereafter, the processing speed was adjusted so that the film entered the first drying oven 0.5 seconds later, and the film was continuously heated and dried at a first drying oven temperature of 90°C and a second drying oven temperature of 120°C to obtain a release film for molding ceramic green sheets.

[0164] (Antistatic layer forming coating liquid R1) Water 34.6 parts by mass Methanol 64.4 parts by mass Cationic antistatic agent (Elecond PQ-10, solid content concentration 50% by mass, manufactured by Soken Chemical & Engineering Co., Ltd.) 0.4 parts by mass Polyethylene wax (Hitec E68A, solid content concentration 20% by mass, manufactured by Toho Chemical Industry Co., Ltd.) 0.6 parts by mass The softening point of the polyethylene wax used in the examples was 110° C. Furthermore, the above-mentioned various physical properties of the obtained release film were evaluated, and as a result, good results were obtained as shown in Table 2A.

[0165] Example 2 A release layer-forming coating solution M1 having the following composition was applied onto the planar layer A of the laminated film F2 using reverse gravure so that the coating thickness after drying would be 20 nm. The processing speed was then adjusted so that the film entered the first drying oven 0.5 seconds later, and the film was continuously heated and dried at a first drying oven temperature of 90°C and a second drying oven temperature of 120°C. After the drying process, the film was irradiated on a cooling roll with an ultraviolet irradiator (Heraeus, H bulb) at an integrated light dose of 100 mJ / cm. 2 The release layer was cured by irradiating it with ultraviolet light.

[0166] A release film for molding ceramic green sheets was obtained in the same manner as in Example 1, except that antistatic layer-forming coating solution R1 was applied onto the lubrication layer B of the obtained release coated film using reverse gravure so that the coating thickness after drying would be 15 nm. As a result of evaluating the various physical properties of the obtained release film, good results were obtained as shown in Table 2A.

[0167] (Example 3) A release film for molding ceramic green sheets was obtained in the same manner as in Example 1, except that the antistatic layer-forming coating solution R2 having the following composition was applied onto the lubrication layer of the release coated film using reverse gravure so that the coating amount after drying would be 15 nm.

[0168] (Antistatic layer forming coating liquid R2) Water 34.8 parts by mass Methanol 64.4 parts by mass Cationic antistatic agent (Elecond PQ-10 manufactured by Soken Chemical & Engineering Co., Ltd.) 0.5 parts by mass Polyethylene wax (Hitec E68A manufactured by Toho Chemical Industry Co., Ltd.) 0.3 parts by mass Furthermore, the above-mentioned various physical properties of the obtained release film were evaluated, and good results were obtained as shown in Table 2A.

[0169] (Example 4) A release film for molding ceramic green sheets was obtained in the same manner as in Example 1, except that the antistatic layer-forming coating solution R3 having the following composition was applied onto the lubrication layer of the release coated film using reverse gravure so that the coating thickness after drying would be 15 nm.

[0170] (Antistatic layer forming coating liquid R3) Water 34.4 parts by mass Methanol 64.4 parts by mass Cationic antistatic agent (Elecond PQ-10 manufactured by Soken Chemical & Engineering Co., Ltd.) 0.3 parts by mass Polyethylene wax (Hitec E68A manufactured by Toho Chemical Industry Co., Ltd.) 0.9 parts by mass Furthermore, the above-mentioned various physical properties of the obtained release film were evaluated, and good results were obtained as shown in Table 2A.

[0171] (Example 5) A release film for molding ceramic green sheets was obtained in the same manner as in Example 1, except that the antistatic layer-forming coating solution R4 having the following composition was applied onto the lubrication layer of the release coated film using reverse gravure so that the coating thickness after drying would be 15 nm.

[0172] (Antistatic layer forming coating liquid R4) Water 35.1 parts by mass Methanol 64.4 parts by mass Cationic antistatic agent (Elecond PQ-10 manufactured by Soken Chemical & Engineering Co., Ltd.) 0.2 parts by mass Polyethylene wax (Hitec E68A manufactured by Toho Chemical Industry Co., Ltd.) 0.3 parts by mass Furthermore, the above-mentioned various physical properties of the obtained release film were evaluated, and good results were obtained as shown in Table 2A.

[0173] (Example 6) A release film for molding ceramic green sheets was obtained in the same manner as in Example 1, except that the antistatic layer-forming coating solution R5 having the following composition was applied onto the lubrication layer of the release coated film using reverse gravure so that the coating thickness after drying would be 23 nm.

[0174] (Antistatic layer forming coating liquid R5) Water 34.1 parts by mass Methanol 64.4 parts by mass Cationic antistatic agent (Elecond PQ-10 manufactured by Soken Chemical & Engineering Co., Ltd.) 0.6 parts by mass Polyethylene wax (Hitec E68A manufactured by Toho Chemical Industry Co., Ltd.) 0.9 parts by mass Furthermore, the above-mentioned various physical properties of the obtained release film were evaluated, and good results were obtained as shown in Table 2A.

[0175] (Example 7) A release film for molding ceramic green sheets was obtained in the same manner as in Example 1, except that the antistatic layer-forming coating solution R6 having the following composition was applied onto the lubrication layer of the release coated film using reverse gravure so that the coating thickness after drying would be 15 nm.

[0176] (Antistatic layer forming coating liquid R6) Water 35.1 parts by mass Methanol 64.4 parts by mass Cationic antistatic agent (Elecond PQ-10 manufactured by Soken Chemical & Engineering Co., Ltd.) 0.4 parts by mass Polyethylene wax (Hitec E68A manufactured by Toho Chemical Industry Co., Ltd.) 0.1 parts by mass Furthermore, as a result of evaluating the various physical properties of the obtained release film as described above, a film with sufficient slipperiness was obtained, as shown in Table 2A.

[0177] (Example 8) A release film for molding ceramic green sheets was obtained in the same manner as in Example 1, except that the antistatic layer-forming coating solution R7 having the following composition was applied onto the lubrication layer of the release coated film using reverse gravure so that the coating thickness after drying would be 15 nm.

[0178] (Antistatic layer forming coating liquid R7) Water 34.1 parts by mass Methanol 64.4 parts by mass Cationic antistatic agent (Elecond PQ-10 manufactured by Soken Chemical & Engineering Co., Ltd.) 0.3 parts by mass Polyethylene wax (Hitec E68A manufactured by Toho Chemical Industry Co., Ltd.) 1.2 parts by mass Furthermore, as a result of evaluating the various physical properties of the obtained release film as described above, a film with slightly higher slipperiness was obtained, as shown in Table 2A.

[0179] (Example 9) A release film for molding ceramic green sheets was obtained in the same manner as in Example 1, except that the antistatic layer-forming coating solution R8 having the following composition was applied onto the lubrication layer of the release coated film using reverse gravure so that the coating thickness after drying would be 15 nm.

[0180] (Antistatic layer forming coating solution R8) Water 34.8 parts by mass Methanol 64.4 parts by mass Cationic antistatic agent (Elecond PQ-10 manufactured by Soken Chemical & Engineering Co., Ltd.) 0.4 parts by mass Polyethylene wax (AQUACER 531 manufactured by BYK-Chemie Co., Ltd.) 0.4 parts by mass The softening point of the polyethylene wax used in the examples was 130° C. Furthermore, the above-mentioned various physical properties of the obtained release film were evaluated, and as a result, a film with sufficient particle shedding properties was obtained, as shown in Table 2A.

[0181] (Example 10) A release film for molding ceramic green sheets was obtained in the same manner as in Example 1, except that the antistatic layer-forming coating solution R9 having the following composition was applied onto the lubrication layer of the release coated film using reverse gravure so that the coating thickness after drying would be 15 nm.

[0182] (Antistatic layer forming coating solution R9) Water 34.8 parts by mass Methanol 64.4 parts by mass Cationic antistatic agent (Elecond PQ-10 manufactured by Soken Chemical & Engineering Co., Ltd.) 0.4 parts by mass Polypropylene wax (AQUACER 593 manufactured by BYK-Chemie Co., Ltd.) 0.4 parts by mass The softening point of the polyethylene wax used in the examples was 160° C. Furthermore, the above-mentioned various physical properties of the obtained release film were evaluated, and as a result, a film with sufficient particle shedding properties was obtained, as shown in Table 2A.

[0183] (Production Example 11) A release layer-forming coating solution M1 having the following composition was applied to one side of a laminated film F5 using reverse gravure so that the coating thickness after drying would be 20 nm. The processing speed was then adjusted so that the film entered the first drying oven 0.5 seconds later, and the film was continuously heated and dried at a first drying oven temperature of 90°C and a second drying oven temperature of 120°C. After the drying process, the film was irradiated on a cooling roll with an ultraviolet irradiator (Heraeus, H bulb) at an integrated light dose of 100 mJ / cm. 2 The release layer was cured by irradiating it with ultraviolet light.

[0184] A release film for molding ceramic green sheets was obtained in the same manner as in Example 1, except that the antistatic layer-forming coating solution R1 was applied to the other surface of the obtained release coated film using reverse gravure so that the coating thickness after drying would be 15 nm. Furthermore, the above-mentioned various physical properties of the obtained release film were evaluated, and as a result, good results were obtained, as shown in Table 2A.

[0185] (Example 12) A release film for molding ceramic green sheets was obtained in the same manner as in Example 1, except that the antistatic layer-forming coating solution R13 having the following composition was applied onto the lubrication layer of the release coated film using reverse gravure so that the coating amount after drying would be 15 nm.

[0186] (Antistatic layer forming coating solution R13) Water 33.3 parts by mass Methanol 64.4 parts by mass Anionic antistatic resin (EL Polymer WS-52R manufactured by Shin-Nakamura Chemical Co., Ltd.) 2 parts by mass Polyethylene wax (Hitec E68A manufactured by Toho Chemical Industry Co., Ltd.) 0.3 parts by mass Fluorine-based surfactant (Megafac F-444 manufactured by DIC Corporation) 0.03 parts by mass Furthermore, as a result of evaluating the various physical properties of the obtained release film as described above, the surface resistance value was found to be slightly high, as shown in Table 2A.

[0187] (Example 13) A release film for molding ceramic green sheets was obtained in the same manner as in Example 1, except that the antistatic layer-forming coating solution R14 having the following composition was applied onto the lubrication layer of the release coated film using reverse gravure so that the coating thickness after drying would be 15 nm.

[0188] (Antistatic layer forming coating liquid R14) Water 34.6 parts by mass Methanol 64.4 parts by mass Cationic antistatic agent (Elecond PQ-10 manufactured by Soken Chemical & Engineering Co., Ltd., solid content concentration 50% by mass) 0.4 parts by mass Polyethylene wax (Hitec E68A manufactured by Toho Chemical Industry Co., Ltd., solid content concentration 20% by mass) 0.01 parts by mass The above-mentioned various physical properties of the obtained release film were evaluated, and as shown in Table 2A, a film with slightly higher slipperiness was obtained.

[0189] (Example 14) A release film for molding ceramic green sheets was obtained in the same manner as in Example 1, except that an antistatic layer-forming coating solution R15 having the following composition was applied onto the lubrication layer of the release coated film using reverse gravure so that the coating thickness after drying would be 15 nm.

[0190] (Antistatic layer forming coating liquid R15) Water 35.1 parts by mass Methanol 64.4 parts by mass Cationic antistatic agent (TIE-615A manufactured by Takemoto Oil & Fat Co., Ltd.) 0.2 parts by mass Polyethylene wax (Hitec E68A manufactured by Toho Chemical Industry Co., Ltd.) 0.3 parts by mass Furthermore, as a result of evaluating the above-mentioned various physical properties of the obtained release film, good results were obtained as shown in Table 2A.

[0191] Comparative Example 1 A release layer-forming coating solution M1 having the following composition was applied to one side of a laminated film F3 using reverse gravure so that the coating thickness after drying would be 20 nm. The processing speed was then adjusted so that the film entered the first drying oven 0.5 seconds later, and the film was continuously heated and dried at a first drying oven temperature of 90°C and a second drying oven temperature of 120°C. After the drying process, the film was irradiated on a cooling roll with an ultraviolet irradiator (Heraeus, H bulb) at an integrated light dose of 100 mJ / cm. 2 The release layer was cured by irradiating it with ultraviolet light.

[0192] A release film for molding ceramic green sheets was obtained in the same manner as in Example 1, except that antistatic layer-forming coating solution R1 was applied to the other surface of the obtained release coated film using reverse gravure so that the coating thickness after drying would be 15 nm. The above-mentioned various physical properties of the obtained release film were evaluated, and as a result, many pinholes were generated in the ceramic green sheet, as shown in Table 2B.

[0193] (Comparative Example 2) A release film for molding a ceramic green sheet was obtained in the same manner as in Example 1, except that an antistatic layer was not provided on the lubricity layer of the release coated film. The above-mentioned various physical properties of the obtained release film were evaluated, and as a result, as shown in Table 2B, the surface resistance value was poor, and therefore the unwinding charging was significantly poor.

[0194] Comparative Example 3 A release film for molding ceramic green sheets was obtained in the same manner as in Example 1, except that an antistatic layer-forming coating solution R10 having the following composition and containing no wax was applied onto the lubrication layer of the release coated film using reverse gravure so that the coating thickness after drying was 15 nm.

[0195] (Antistatic layer forming coating liquid R10) Water 35.2 parts by mass Methanol 64.4 parts by mass Cationic antistatic agent (Elecond PQ-10 manufactured by Soken Chemical & Engineering Co., Ltd.) 0.4 parts by mass Furthermore, as a result of evaluating the above-mentioned various physical properties of the obtained release film, a film was obtained which was significantly inferior in terms of lubricity, abrasion resistance and particle shedding property, as shown in Table 2B.

[0196] Comparative Example 4: A release layer-forming coating solution M1 having the following composition was applied to one side of a laminated film F4 using reverse gravure so that the coating thickness after drying would be 20 nm. The processing speed was then adjusted so that the film entered the first drying oven 0.5 seconds later, and the film was continuously heated and dried at a first drying oven temperature of 90°C and a second drying oven temperature of 120°C. After the drying process, the film was irradiated on a cooling roll with an ultraviolet irradiator (Heraeus, H bulb) at an integrated light dose of 100 mJ / cm. 2 The release layer was cured by irradiating it with ultraviolet light.

[0197] A release film for molding ceramic green sheets was obtained in the same manner as in Example 1, except that antistatic layer-forming coating solution R1 was applied to the other surface of the obtained release coated film using reverse gravure so that the coating thickness after drying would be 15 nm. The above-mentioned various physical properties of the obtained release film were evaluated, and as a result, a film with significantly poor lubricity was obtained, as shown in Table 2B.

[0198] Comparative Example 5: A release layer-forming coating solution M1 having the following composition was applied to one side of a laminated film F5 using reverse gravure so that the coating thickness after drying would be 20 nm. The processing speed was then adjusted so that the film entered the first drying oven 0.5 seconds later, and the film was continuously heated and dried at a first drying oven temperature of 90°C and a second drying oven temperature of 120°C. After the drying process, the film was irradiated on a cooling roll with an ultraviolet irradiator (Heraeus, H bulb) at an integrated light dose of 100 mJ / cm. 2The release layer was cured by irradiating it with ultraviolet light.

[0199] A release film for molding ceramic green sheets was obtained in the same manner as in Example 1, except that antistatic layer-forming coating solution R1 was applied to the other surface of the obtained release coated film using reverse gravure so that the coating thickness after drying would be 15 nm. The above-mentioned various physical properties of the obtained release film were evaluated, and as a result, as shown in Table 2B, many pinholes were generated during the coating of the ceramic slurry.

[0200] (Comparative Example 6) Except for not providing a release layer on the film planar layer, a release film for molding ceramic green sheets was obtained in the same manner as in Example 1. The above-mentioned various physical properties of the obtained release film were evaluated, and as a result, a film with significantly poor ceramic peeling force was obtained, as shown in Table 2B.

[0201] (Comparative Example 7) A release film for molding ceramic green sheets was obtained in the same manner as in Example 1, except that the antistatic layer-forming coating solution R11 having the following composition was applied onto the lubrication layer of the release coated film using reverse gravure so that the coating thickness after drying was 15 nm.

[0202] (Antistatic layer forming coating liquid R11) Water 34.6 parts by mass Methanol 64.4 parts by mass Cationic antistatic agent (Elecond PQ-10, manufactured by Soken Chemical & Engineering Co., Ltd.) 0.4 parts by mass Silicone grafted acrylic resin (Simac US-450, manufactured by Toagosei Co., Ltd.) 0.6 parts by mass As a result of evaluating the various physical properties of the obtained release film as described above, a film with poor particle shedding properties was obtained, as shown in Table 2B.

[0203] (Comparative Example 8) A release film for molding ceramic green sheets was obtained in the same manner as in Example 1, except that the antistatic layer-forming coating solution R12 having the following composition was applied onto the lubrication layer of the release coated film using reverse gravure so that the coating thickness after drying was 15 nm.

[0204] (Antistatic layer forming coating liquid R12) Water 34.6 parts by mass Methanol 64.4 parts by mass Cationic antistatic agent (Elecond PQ-10 manufactured by Soken Chemical & Engineering Co., Ltd.) 0.4 parts by mass Polyether modified polydimethylsiloxane (BYK-307 manufactured by BYK-Chemie Co., Ltd.) 0.6 parts by mass As a result of evaluating the above various physical properties of the obtained release film, a film with poor surface resistivity after abrasion was obtained, as shown in Table 2B.

[0205] The various components used, their physical properties, etc. are shown in Tables 1A, 1B, 2A, and 2B.

[0206]

[0207]

[0208]

[0209]

[0210] The invention of the examples satisfies the requirements of the present invention. As a result, for example, in the process of printing electrodes on a molded ceramic green sheet, when the surface of the release film opposite to the processing surface where the ceramic green sheet is provided comes into contact with a support in a dryer and the sheet is transported while experiencing friction, it is possible to suppress charging due to friction.

[0211] The present invention can suppress charging during transport, thereby preventing the inclusion of foreign matter due to charging caused by friction. Furthermore, the transportability is good, and poor film winding and wrinkles that may occur during film transport can be suppressed.

[0212] Furthermore, the present invention provides a good balance between good antistatic properties and windability, which can prevent breakage of the green sheet when molding the thin layer region of the ceramic green sheet, and can also prevent misalignment of the printed electrodes.

[0213] Additionally, the present invention not only suppresses the generation of charge when the ceramic green sheet is peeled off from the release film, but also suppresses the generation of charge during transportation.

[0214] The present invention also provides excellent adhesion between the substrate and the antistatic layer, preventing the antistatic layer from falling off due to friction between the antistatic layer and the support in the dryer. Furthermore, it can suppress process contamination caused by the antistatic resin falling off from the antistatic layer and pinhole formation in the green sheet, thereby solving new problems caused by the falling off of the antistatic resin. In particular, in the present invention, the inclusion of wax in the antistatic layer effectively suppresses particle shedding, and a film with excellent surface resistivity after abrasion was obtained.

[0215] On the other hand, in Comparative Example 1, the two surfaces of the polyester film substrate had similar roughness, resulting in pinholes in the ceramic green sheet. Comparative Example 2 did not have an antistatic layer, resulting in poor particle shedding and unwinding charging. Comparative Example 3 did not have wax, resulting in insufficient particle shedding.

[0216] In Comparative Example 4, the roughness of both sides of the polyester film substrate was similarly small, resulting in poor unwinding charging.In Comparative Example 5, the roughness of the AS side of the polyester film substrate was excessively large, resulting in the occurrence of numerous pinholes during ceramic slurry coating.

[0217] Comparative Example 6 did not have a release layer, and ceramic releasability was poor, making it impossible to adequately evaluate. Comparative Example 7 did not contain wax in the antistatic layer, resulting in a film with poor particle shedding properties. Comparative Example 8 did not contain wax in the antistatic layer, resulting in a film with poor surface resistivity after abrasion.

[0218] The release film of the present invention can particularly suppress the occurrence of defects when molding a ceramic green sheet.

Claims

1. A release film for molding ceramic green sheets, comprising, in this order, a release layer, a polyester film as a base material, and an antistatic layer, wherein the base material has two surfaces with different roughnesses, the antistatic layer contains an antistatic resin and a wax, the regional surface average roughness (Sa1) of the release layer is less than 10 nm, and the regional surface average roughness (Sa1) of the release layer and the regional surface average roughness (Sa2) of the antistatic layer satisfy the following formula: 0.02<Sa1 / Sa2<0.

5.

2. The release film for molding ceramic green sheets according to claim 1, wherein the content of said wax is 1% by mass or more and 60% by mass or less relative to 100% by mass of the total solid content in said antistatic layer.

3. The release film for molding ceramic green sheets according to claim 1, wherein the wax comprises a polyolefin wax.

4. The release film for molding ceramic green sheets according to claim 1, wherein the antistatic layer has a thickness of 0.005 to 0.1 μm.

5. The release film for molding ceramic green sheets according to claim 1, wherein the antistatic resin is an acrylic resin having a cationic functional group.

Citation Information

Patent Citations

  • Mold release film with ceramic sheet

    JP2002273715A

  • Release film roll for manufacturing thin ceramic sheet

    JP2003145685A

  • Mold release film roll

    JP2022128855A