Compound, starting material for thin film formation, thin film, and method for producing thin film
The use of a compound with a specific structure as a raw material for forming thin films addresses the challenge of achieving high-quality molybdenum or tungsten thin films with low residual carbon, resulting in films with enhanced thermal stability and productivity for diverse applications.
Patent Information
- Application Number
- PCT/JP2024/018446
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-02
- Filing Date
- 2024-05-20
- Publication Date
- 2024-12-05
AI Technical Summary
Existing methods for producing thin films containing molybdenum or tungsten atoms face challenges in achieving high-quality films with low residual carbon content.
A compound with a specific structure, represented by general formulas (1), (2), and (3), is used as a raw material for forming thin films, which allows for the production of high-quality molybdenum-containing or tungsten-containing thin films with low residual carbon through chemical vapor deposition or atomic layer deposition methods.
The compound enables the formation of thin films with low residual carbon content, high thermal stability, and high productivity, suitable for various applications including electronic devices and semiconductor devices.
Smart Images

Figure JP2024018446_05122024_PF_FP_ABST
Abstract
Description
Compound, raw material for forming thin film, thin film, and method for manufacturing thin film
[0001] The present invention relates to a compound having a specific structure, a thin film-forming material, a thin film produced using the thin film-forming material, and a method for producing a thin film.
[0002] It is known that thin films containing molybdenum atoms or tungsten atoms can be used in electronic devices, semiconductor devices, liquid crystal components, coating materials, heat-resistant materials, alloys, aircraft components, and the like.
[0003] Examples of methods for producing the above-mentioned thin films include sputtering, ion plating, MOD methods such as coating pyrolysis and sol-gel methods, and chemical vapor deposition. However, chemical vapor deposition (hereinafter sometimes simply referred to as CVD) methods including atomic layer deposition (hereinafter sometimes simply referred to as ALD) methods are the most suitable production processes because they have many advantages such as excellent composition controllability and step coverage, suitability for mass production, and the ability to achieve hybrid integration.
[0004] Many different raw materials have been reported as elemental molybdenum or tungsten sources for use in chemical vapor deposition. For example, Patent Document 1 discloses molybdenum-oxo-tetra(alkoxide) and tungsten-oxo-tetra(alkoxide), and Patent Documents 2 and 3 disclose bis(alkylimido)-bis(alkylamido)molybdenum. Furthermore, Patent Document 4 discloses tungsten chloride, and Patent Document 5 discloses a tungsten diazabutadiene compound.
[0005] JP-T-2017-532385 A JP-T-2016-516892 A JP-A-2018-150627 JP-A-2015-221940 JP-T-2014-534952 A
[0006] However, when a thin film is produced using the compounds described in Patent Documents 1 to 5, there is a problem in that it is difficult to obtain a high-quality thin film containing molybdenum atoms or tungsten atoms with little residual carbon.
[0007] Therefore, an object of the present invention is to provide a thin film-forming material capable of producing a high-quality thin film containing molybdenum atoms or tungsten atoms with little residual carbon (hereinafter, sometimes referred to as a "molybdenum-containing thin film or a tungsten-containing thin film"), and a method for producing a thin film using the same.
[0008] As a result of extensive research, the present inventors have found that the above-mentioned problems can be solved by using a compound having a specific structure, and have thus completed the present invention.
[0009] That is, the present invention is a compound represented by the following general formula (1).
[0010]
[0011] (In the formula, R 1 and R 2 each independently represents an alkyl group having 1 to 5 carbon atoms; A 1 represents an alkanediyl group having 1 to 8 carbon atoms, L 1 represents a group represented by the following general formula (L-1) or (L-2), M 1 represents a molybdenum atom or a tungsten atom; α, β, and γ represent integers of 1 or more, and the sum of 2α, β, and γ is 6.
[0012]
[0013] (In the formula, R 11 ~R 13 each independently represents an alkyl group having 1 to 5 carbon atoms, and * represents a bond.
[0014] Another embodiment of the present invention is a thin film-forming material containing the above compound.
[0015] Yet another embodiment of the present invention is a thin film produced using the above-mentioned thin film-forming material.
[0016] Yet another embodiment of the present invention is a method for producing a thin film, which comprises forming a thin film containing molybdenum atoms or tungsten atoms on the surface of a substrate using the above-mentioned thin film-forming material.
[0017] The compound represented by the following general formula (2) can be obtained by the same procedure as in the general formula (1) above, except that L1 is the same as the compound represented by (L-1).
[0018]
[0019] (In the formula, R 1 , R 2 , R 11 and R 12 each independently represents an alkyl group having 1 to 5 carbon atoms; A 1 represents an alkanediyl group having 1 to 8 carbon atoms, M 1 represents a molybdenum atom or a tungsten atom; α, β, and γ represent integers of 1 or more, and the sum of 2α, β, and γ is 6.
[0020] The compound represented by the following general formula (3) can be obtained by the same procedure as in the general formula (1) above, except that L 1 is the same as the compound represented by (L-2).
[0021]
[0022] (In the formula, R 1 , R 2 and R 13 each independently represents an alkyl group having 1 to 5 carbon atoms; A 1 represents an alkanediyl group having 1 to 8 carbon atoms, M 1 represents a molybdenum atom or a tungsten atom; α, β, and γ represent integers of 1 or more, and the sum of 2α, β, and γ is 6.
[0023] The compound of the present invention can provide a thin film-forming material that can produce a high-quality molybdenum-containing thin film or tungsten-containing thin film with little residual carbon, and a method for producing a thin film using the same.
[0024] Fig. 1 is a schematic diagram showing an example of an ALD apparatus used in a thin film manufacturing method according to one embodiment of the present invention. Fig. 2 is a schematic diagram showing another example of an ALD apparatus used in a thin film manufacturing method according to one embodiment of the present invention. Fig. 3 is a schematic diagram showing another example of an ALD apparatus used in a thin film manufacturing method according to one embodiment of the present invention. Fig. 4 is a schematic diagram showing another example of an ALD apparatus used in a thin film manufacturing method according to one embodiment of the present invention.
[0025] A. Compound The compound of the present invention is a compound represented by the following general formula (1):
[0026]
[0027] In general formula (1), R 1 and R 2 each independently represents an alkyl group having 1 to 5 carbon atoms; A 1 represents an alkanediyl group having 1 to 8 carbon atoms, L 1 represents a group represented by the following general formula (L-1) or (L-2), M 1 represents a molybdenum atom or a tungsten atom, α, β, and γ represent integers of 1 or more, and the sum of 2α, β, and γ is 6.
[0028]
[0029] In general formulas (L-1) and (L-2), R 11 ~R 13 each independently represents an alkyl group having 1 to 5 carbon atoms, and * represents a bond.
[0030] R 1 , R 2 , R 11 , R 12 and R 13 Examples of the alkyl group having 1 to 5 carbon atoms represented by the formula (I) include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, an isopentyl group, and a neopentyl group.
[0031] R 1 As R, an alkyl group having 3 to 5 carbon atoms is preferred, an alkyl group having 3 to 4 carbon atoms is more preferred, an isopropyl group or a tert-butyl group is even more preferred, and a tert-butyl group is most preferred, because it facilitates the efficient production of a high-quality molybdenum-containing thin film or a tungsten-containing thin film having a low melting point, a high vapor pressure, high thermal stability, and little residual carbon. 2As the alkyl group, an alkyl group having 1 to 3 carbon atoms is preferred, a methyl group or an ethyl group is more preferred, and a methyl group is most preferred, because it facilitates the efficient production of a high-quality molybdenum-containing thin film or a tungsten-containing thin film having a low melting point, a high vapor pressure, and high thermal stability, and which has little residual carbon.
[0032] A 1 Examples of the alkanediyl group having 1 to 8 carbon atoms represented by the formula (I) include a methylene group, an ethylene group, a propane-1,3-diyl group, a propane-1,2-diyl group, a butylene group, a butane-1,3-diyl group, a butane-2,3-diyl group, a butane-1,2-diyl group, a pentane-1,5-diyl group, a pentane-1,3-diyl group, a pentane-1,4-diyl group, a pentane-2,3-diyl group, a hexane-1,6-diyl group, a hexane-1,2-diyl group, a hexane-1,3-diyl group, a hexane-1,4-diyl group, a hexane-2,5-diyl group, a hexane-2,4-diyl group, a hexane-3,4-diyl group, a heptylene group, an octylene group, an ethane-1,1-diyl group, and a propane-2,2-diyl group.
[0033] A 1 As the alkanediyl group, an alkanediyl group having 1 to 6 carbon atoms is preferred, an alkanediyl group having 2 to 5 carbon atoms is more preferred, an alkanediyl group having 2 to 4 carbon atoms is even more preferred, an alkanediyl group having 3 carbon atoms is still more preferred, and a propane-1,2-diyl group is most preferred, because these groups facilitate the efficient production of high-quality molybdenum-containing or tungsten-containing thin films having a low compound melting point, a high vapor pressure, high thermal stability, and little residual carbon.
[0034] Regarding α, β, and γ, α is preferably 1, β is preferably 1 to 2, and more preferably 1, and γ is preferably 2 to 3, and more preferably 3, because these compounds facilitate the efficient production of high-quality molybdenum-containing thin films or tungsten-containing thin films having a low melting point, a high vapor pressure, high thermal stability, and little residual carbon.
[0035] L 1As L, a group represented by general formula (L-1) is preferred because it is easy to produce a high-quality molybdenum-containing thin film or tungsten-containing thin film with a low melting point, high vapor pressure, high thermal stability, and little residual carbon with good productivity. 1 is a group represented by general formula (L-1), R 11 and R 12 As the L, an alkyl group having 1 to 3 carbon atoms is preferred, a methyl group or an ethyl group is more preferred, and a methyl group is most preferred, because it allows the compound to have a low melting point, a high vapor pressure, high thermal stability, and to easily produce a high-quality molybdenum-containing thin film or a tungsten-containing thin film with little residual carbon with good productivity. 1 is a group represented by general formula (L-2), R 13 As the alkyl group, an alkyl group having 1 to 3 carbon atoms is preferred, a methyl group or an ethyl group is more preferred, and a methyl group is most preferred, because it facilitates the efficient production of a high-quality molybdenum-containing thin film or a tungsten-containing thin film having a low melting point, a high vapor pressure, and high thermal stability, and which has little residual carbon.
[0036] Preferred specific examples of the compound represented by general formula (1) used in the thin-film-forming material of the present invention include the following compounds No. 1 to No. 144, but the present invention is not limited to these compounds. In the following chemical formulas, "Me" represents a methyl group, "Et" represents an ethyl group, "iPr" represents an isopropyl group, and "tBu" represents a tert-butyl group.
[0037]
[0038]
[0039]
[0040]
[0041]
[0042]
[0043]
[0044]
[0045] The compound of the present invention is not particularly limited by its production method, and can be produced by applying a well-known synthesis method. For example, the compound represented by general formula (1) can be obtained by mixing imino-amino-molybdenum or imino-amino-tungsten having a corresponding structure with an alcohol having a corresponding structure in the presence or absence of a solvent, stirring and reacting the mixture, then mixing an aminoalcohol having a corresponding structure with the mixture, stirring and reacting the mixture, removing the solvent, and distilling the mixture.
[0046] B. Thin-Film-Forming Raw Material The thin-film-forming raw material of the present invention contains a compound represented by the general formula (1) above. The thin-film-forming raw material of the present invention may contain a compound represented by the general formula (1) as a precursor of a thin film, and its composition varies depending on the type of thin film desired. For example, when producing a thin film containing only molybdenum or tungsten atoms as the metal, the thin-film-forming raw material does not contain metal compounds and metalloid compounds other than molybdenum or tungsten. On the other hand, when producing a thin film containing molybdenum or tungsten atoms and a metal and / or metalloid other than molybdenum or tungsten atoms, the thin-film-forming raw material may contain, in addition to the compound represented by the general formula (1), a compound containing the desired metal and / or a compound containing a metalloid (hereinafter sometimes referred to as "other precursors").
[0047] B1. Other Precursors In the case of a multi-component ALD method using a plurality of precursors, other precursors that can be used together with the compound represented by general formula (1) are not particularly limited, and well-known general precursors used as raw materials for forming thin films in the ALD method can be used.
[0048] Examples of the other precursor include compounds of silicon or a metal with one or more compounds selected from the group consisting of compounds used as organic ligands, such as alcohol compounds, glycol compounds, β-diketone compounds, cyclopentadiene compounds, and organic amine compounds. Examples of the metal species of the precursor include lithium, sodium, potassium, magnesium, calcium, strontium, barium, titanium, zirconium, hafnium, vanadium, niobium, tantalum, chromium, molybdenum, tungsten, manganese, iron, osmium, ruthenium, cobalt, rhodium, iridium, nickel, palladium, platinum, copper, silver, gold, zinc, aluminum, gallium, indium, germanium, lead, antimony, bismuth, radium, scandium, yttrium, lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and lutetium.
[0049] Examples of alcohol compounds that can be used as organic ligands for the other precursors include alkyl alcohols such as methanol, ethanol, propanol, isopropyl alcohol, butanol, sec-butyl alcohol, isobutyl alcohol, tert-butyl alcohol, pentyl alcohol, isopentyl alcohol, and tert-pentyl alcohol; 2-methoxyethanol, 2-ethoxyethanol, 2-butoxyethanol, 2-(2-methoxyethoxy)ethanol, 2-methoxy-1-methylethanol, 2-methoxy-1,1-dimethylethanol, 2-ethoxy-1,1-dimethylethanol, and 2-isopropoxy-1,1-dimethylethanol. ether alcohols such as 2-butoxy-1,1-dimethylethanol, 2-(2-methoxyethoxy)-1,1-dimethylethanol, 2-propoxy-1,1-diethylethanol, 2-sec-butoxy-1,1-diethylethanol, and 3-methoxy-1,1-dimethylpropanol; and dialkylamino alcohols such as dimethylaminoethanol, ethylmethylaminoethanol, diethylaminoethanol, dimethylamino-2-pentanol, ethylmethylamino-2-pentanol, dimethylamino-2-methyl-2-pentanol, ethylmethylamino-2-methyl-2-pentanol, and diethylamino-2-methyl-2-pentanol.
[0050] Examples of glycol compounds used as organic ligands for the other precursors include 1,2-ethanediol, 1,2-propanediol, 1,3-propanediol, 2,4-hexanediol, 2,2-dimethyl-1,3-propanediol, 2,2-diethyl-1,3-propanediol, 1,3-butanediol, 2,4-butanediol, 2,2-diethyl-1,3-butanediol, 2-ethyl-2-butyl-1,3-propanediol, 2,4-pentanediol, 2-methyl-1,3-propanediol, 2-methyl-2,4-pentanediol, 2,4-hexanediol, and 2,4-dimethyl-2,4-pentanediol.
[0051] Examples of the β-diketone compound used as the organic ligand for the other precursors include acetylacetone, hexane-2,4-dione, 5-methylhexane-2,4-dione, heptane-2,4-dione, 2-methylheptane-3,5-dione, 5-methylheptane-2,4-dione, 6-methylheptane-2,4-dione, 2,2-dimethylheptane-3,5-dione, 2,6-dimethylheptane-3,5-dione, 2,2,6-trimethylheptane-3,5-dione, 2,2,6,6-tetramethylheptane-3,5-dione, octane-2,4-dione, 2,2,6-trimethyloctane-3,5-dione, 2,6-dimethyloctane-3,5-dione, 2,9-dimethylnonane-4,6-dione, 2-methyl- Examples of suitable fluorine-substituted alkyl β-diketones include 6-ethyldecane-3,5-dione and 2,2-dimethyl-6-ethyldecane-3,5-dione; 1,1,1-trifluoropentane-2,4-dione, 1,1,1-trifluoro-5,5-dimethylhexane-2,4-dione, 1,1,1,5,5,5-hexafluoropentane-2,4-dione and 1,3-diperfluorohexylpropane-1,3-dione; and ether-substituted β-diketones include 1,1,5,5-tetramethyl-1-methoxyhexane-2,4-dione, 2,2,6,6-tetramethyl-1-methoxyheptane-3,5-dione and 2,2,6,6-tetramethyl-1-(2-methoxyethoxy)heptane-3,5-dione.
[0052] Examples of the cyclopentadiene compound used as the organic ligand of the other precursors include cyclopentadiene, methylcyclopentadiene, ethylcyclopentadiene, propylcyclopentadiene, isopropylcyclopentadiene, butylcyclopentadiene, sec-butylcyclopentadiene, isobutylcyclopentadiene, tert-butylcyclopentadiene, dimethylcyclopentadiene, tetramethylcyclopentadiene, and pentamethylcyclopentadiene.
[0053] Examples of the organic amine compound used as the organic ligand of the other precursor include methylamine, ethylamine, propylamine, isopropylamine, butylamine, sec-butylamine, tert-butylamine, isobutylamine, dimethylamine, diethylamine, dipropylamine, diisopropylamine, ethylmethylamine, propylmethylamine, and isopropylmethylamine.
[0054] The other precursors mentioned above are known in the art, and their production methods are also known. For example, when an alcohol compound is used as the organic ligand, the precursor can be produced by reacting the inorganic salt of the metal or a hydrate thereof described above with an alkali metal alkoxide of the alcohol compound. Examples of the inorganic salt of the metal or a hydrate thereof include metal halides and nitrates. Examples of the alkali metal alkoxide include sodium alkoxide, lithium alkoxide, and potassium alkoxide.
[0055] In the multi-component ALD method as described above, there are a method in which each component of the thin film-forming raw material is vaporized and supplied independently (hereinafter, sometimes referred to as a "single source method"), and a method in which a mixed raw material in which multi-component raw materials are mixed in advance to a desired composition is vaporized and supplied (hereinafter, sometimes referred to as a "cocktail source method"). In the single source method, the other precursor is preferably a compound whose thermal decomposition and / or oxidative decomposition behavior is similar to that of the compound represented by general formula (1). In the cocktail source method, the other precursor is preferably a compound whose thermal decomposition and / or oxidative decomposition behavior is similar to that of the compound represented by general formula (1) and which does not undergo deterioration due to chemical reactions or the like when mixed.
[0056] When other precursors are contained, it is preferable to determine the content thereof according to the composition of the desired film. For example, if the composition of the desired film is Ti, 0.5 W 0.5When the thin-film-forming raw material of the present invention is used as the precursor containing tungsten atoms and a precursor containing one titanium atom in the molecule is used as the precursor containing titanium atoms, it is preferable to mix 1 mol of the precursor containing titanium atoms with 1 mol of the thin-film-forming raw material of the present invention. However, from the viewpoint of easily and productively producing a high-quality molybdenum-containing thin film or tungsten-containing thin film having a low melting point, high vapor pressure, high thermal stability, and little residual carbon, the content of the other precursor is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, even more preferably 10 parts by mass or less, particularly still more preferably 5 parts by mass or less, and most preferably 0 part by mass, i.e., no other precursor is included, relative to 100 parts by mass of the thin-film-forming raw material.
[0057] B2. Organic Solvent In the case of a cocktail source method in a multi-component ALD method, a mixture of the compound represented by general formula (1) and other precursors, or a mixed solution obtained by dissolving such a mixture in an organic solvent, can be used as a thin film-forming raw material.
[0058] The organic solvent is not particularly limited, and any well-known organic solvent can be used. Examples of the organic solvent include acetates such as ethyl acetate, butyl acetate, and methoxyethyl acetate; ethers such as tetrahydrofuran, tetrahydropyran, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, dibutyl ether, and dioxane; ketones such as methyl butyl ketone, methyl isobutyl ketone, ethyl butyl ketone, dipropyl ketone, diisobutyl ketone, methyl amyl ketone, cyclohexanone, and methylcyclohexanone; hydrocarbons such as hexane, cyclohexane, methylcyclohexane, dimethylcyclohexane, ethylcyclohexane, heptane, octane, toluene, and xylene; hydrocarbons having a cyano group such as 1-cyanopropane, 1-cyanonobutane, 1-cyanohexane, cyanocyclohexane, cyanobenzene, 1,3-dicyanopropane, 1,4-dicyanobutane, 1,6-dicyanohexane, 1,4-dicyanocyclohexane, and 1,4-dicyanobenzene; pyridine, lutidine, and the like. These organic solvents may be used alone or in combination of two or more depending on the solubility of the solute, the relationship between the temperature used and the boiling point, the flash point, and the like.
[0059] When the thin film-forming raw material of the present invention is a mixed liquid containing the organic solvent, from the viewpoint of facilitating the formation of a high-quality molybdenum-containing thin film or tungsten-containing thin film with little residual carbon, the total amount of precursors in the thin film-forming raw material is preferably adjusted to 0.01 mol / L to 2.0 mol / L, and more preferably adjusted to 0.05 mol / L to 1.0 mol / L.
[0060] Here, the total amount of precursors refers to the amount of the compound represented by general formula (1) when the thin film-forming raw material does not contain any precursors other than the compound represented by general formula (1). When the thin film-forming raw material contains other precursors in addition to the compound represented by general formula (1), the total amount refers to the total amount of the compound represented by general formula (1) and the other precursors.
[0061] B3. Nucleophilic Reagent The thin-film-forming material of the present invention may contain a nucleophilic reagent, if necessary, to improve the stability of the compound represented by general formula (1) and other precursors. Examples of the nucleophilic reagent include ethylene glycol ethers such as glyme, diglyme, triglyme, and tetraglyme; crown ethers such as 18-crown-6, dicyclohexyl-18-crown-6, 24-crown-8, dicyclohexyl-24-crown-8, and dibenzo-24-crown-8; ethylenediamine, N,N'-tetramethylethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, 1,1,4,7,7-pentamethyldiethylenetriamine, and 1,1,4,7,10,10-hexamethyltriethylenetetramine; Examples of suitable nucleophilic reagents include polyamines such as triethoxytriethyleneamine, cyclic polyamines such as cyclam and cyclen, heterocyclic compounds such as pyridine, pyrrolidine, piperidine, morpholine, N-methylpyrrolidine, N-methylpiperidine, N-methylmorpholine, tetrahydrofuran, tetrahydropyran, 1,4-dioxane, oxazole, thiazole, and oxathiolane, β-ketoesters such as methyl acetoacetate, ethyl acetoacetate, and 2-methoxyethyl acetoacetate, and β-diketones such as acetylacetone, 2,4-hexanedione, 2,4-heptanedione, 3,5-heptanedione, and dipivaloylmethane. From the viewpoint of ease of adjusting stability, the amount of these nucleophilic reagents used is preferably in the range of 0.1 mol to 10 mol, and more preferably in the range of 1 mol to 4 mol, per mol of the total amount of precursor.
[0062] B4. Impurities It is desirable that the thin-film-forming raw material of the present invention contain as little impurity metal elements, impurity halogens such as impurity chlorine, and impurity organic components as possible other than the components constituting the thin-film. The impurity metal element content is preferably 100 ppb or less per element, more preferably 10 ppb or less, and the total content is preferably 1 ppm or less, more preferably 100 ppb or less. In particular, when used as a gate insulating film, gate film, barrier layer, or wiring layer of an LSI, it is necessary to reduce the content of alkali metal elements and alkaline earth metal elements, which affect the electrical properties of the resulting thin film. The impurity halogen content is preferably 100 ppm or less, more preferably 10 ppm or less, and even more preferably 1 ppm or less. The total content of impurity organic components is preferably 500 ppm or less, more preferably 50 ppm or less, and even more preferably 10 ppm or less. Furthermore, since moisture can cause particle generation in the thin film-forming raw materials and during thin film formation, it is advisable to remove as much moisture as possible from the precursor, organic solvent, and nucleophilic reagent before use in order to reduce the moisture content of each. The moisture content of each of the precursor, organic solvent, and nucleophilic reagent is preferably 10 ppm or less, more preferably 1 ppm or less. By keeping the impurity metal element content, impurity halogen content, impurity organic content, and moisture content below the above-mentioned values, the thin film-forming raw material of the present invention can easily form a high-quality molybdenum-containing thin film or tungsten-containing thin film with little residual carbon.
[0063] In order to reduce or prevent particle contamination of the thin film to be formed, it is preferable that the thin film-forming raw material of the present invention contains as few particles as possible. Specifically, from the viewpoint of facilitating the production of a uniform molybdenum-containing thin film or tungsten-containing thin film, the number of particles larger than 0.3 μm per mL of the thin film-forming raw material is preferably 100 or less, and the number of particles larger than 0.2 μm per mL of the thin film-forming raw material is preferably 100 or less, in particle measurement in the liquid phase using a light-scattering liquid-borne particle detector.
[0064] C. Thin Film Manufacturing Method Next, the thin film manufacturing method of the present invention will be described. The thin film manufacturing method of the present invention uses the above-mentioned thin film-forming raw material to form a molybdenum-containing thin film or a tungsten-containing thin film on the surface of a substrate. In the present invention, from the viewpoint of facilitating the formation of a high-quality molybdenum-containing thin film or a tungsten-containing thin film with little residual carbon, a method of manufacturing a thin film by a CVD method or an ALD method is preferred. In particular, a method of manufacturing a thin film by an ALD method is preferred because it has many advantages, such as excellent composition controllability and step coverage, suitability for mass production, and the ability to be hybrid-integrated.
[0065] A method for producing a molybdenum-containing thin film or a tungsten-containing thin film by a CVD method includes introducing a source gas obtained by vaporizing the thin film-forming source into a film-forming chamber in which a substrate is placed, and heating and / or converting the compound represented by general formula (1) in the source gas into plasma to decompose the compound or react the compound with a reactive gas to form a molybdenum-containing thin film or a tungsten-containing thin film on the surface of the substrate. A method for producing a molybdenum-containing thin film or a tungsten-containing thin film by an ALD method includes the steps of: introducing a source gas obtained by vaporizing the thin film-forming source into a film-forming chamber and depositing the compound represented by general formula (1) in the source gas on the surface of the substrate to form a precursor thin film; and introducing a reactive gas into the film-forming chamber and reacting the precursor thin film with the reactive gas to form a thin film containing molybdenum atoms or tungsten atoms.
[0066] Hereinafter, each step of the thin film manufacturing method will be described using the ALD method as an example. The thin film forming raw materials used in the thin film manufacturing method of the present invention are the same as those explained in the above section [Thin film forming raw materials], so explanations will be omitted. There are no particular restrictions on the method of transporting and supplying raw materials, manufacturing conditions, manufacturing equipment, etc., and well-known general conditions and methods can be used.
[0067] A well-known ALD apparatus can be used as an apparatus for producing a thin film using the thin film-forming raw material of the present invention. Specific examples of the apparatus include an apparatus capable of supplying a precursor by bubbling, as shown in FIGS. 1 and 3, and an apparatus having a vaporization chamber 102, as shown in FIGS. 2 and 4. Another example is an apparatus capable of performing plasma treatment on a reactive gas 202, as shown in FIGS. 3 and 4. It should be noted that the apparatus is not limited to a single-wafer apparatus equipped with a film-forming chamber 100 as shown in FIGS. 1 to 4, but an apparatus capable of simultaneously processing multiple wafers using a batch furnace can also be used. These apparatuses can also be used as CVD apparatuses.
[0068] C1. Precursor thin film formation step In the precursor thin film formation step, a source gas obtained by vaporizing a thin film-forming source material M is introduced into the film formation chamber 100, and the compound represented by the general formula (1) above is deposited on the surface of the substrate S to form a precursor thin film.
[0069] (1) Introduction of Raw Material Gas Methods for introducing the raw material gas obtained by vaporizing the thin film forming raw material M into the film forming chamber 100 in which the substrate S is placed include a gas transport method, a liquid transport method, a single source method, a cocktail source method, etc.
[0070] 1 and 3, an example of the gas transport method is a method in which thin film forming raw material M is heated and / or vaporized by a heater 103 or the like in a raw material container 101 in which the thin film forming raw material M is stored to form a raw material gas, and the raw material gas is introduced into a film formation chamber 100 in which a substrate S is placed, together with a carrier gas 201 such as argon, nitrogen, or helium, as necessary. An example of the liquid transport method is a method in which thin film forming raw material M is transported in a liquid or solution state to a vaporization chamber 102, and the thin film forming raw material M is heated and / or vaporized in the vaporization chamber 102 to form a raw material gas, and the raw material gas is introduced into the film formation chamber 100 together with the carrier gas 201, as necessary, as shown in FIGS. 2 and 4. The flow rate of each gas is adjusted by a mass flow controller (MFC) 104.
[0071] The single-source method is a method for transporting and supplying a thin-film-forming raw material M containing multiple precursor components, and examples thereof include a method in which each precursor is independently vaporized and supplied. The cocktail-source method is, for example, a method in which a mixed raw material in which multiple precursor components are mixed in advance to a desired composition is vaporized and supplied. The thin-film-forming raw material M containing multiple precursor components may contain the above-mentioned nucleophilic reagent, etc.
[0072] The step of vaporizing the thin film forming raw material M of the present invention to form a raw material gas may be carried out in the raw material container 101 or in the vaporization chamber 102, as described above. In either case, from the viewpoint of facilitating the formation of a high-quality thin film, it is preferable to vaporize the thin film forming raw material M at a temperature of 0°C to 200°C. Furthermore, when the thin film forming raw material is vaporized in the raw material container 101 or the vaporization chamber 102 to form a raw material gas, the pressure inside the raw material container 101 and the pressure inside the vaporization chamber 102 are preferably within the range of 1 Pa to 10,000 Pa, from the viewpoint of achieving good vaporization of the thin film forming raw material M.
[0073] Examples of materials for the substrate S placed in the film formation chamber 100 include silicon; ceramics such as silicon nitride, titanium nitride, tantalum nitride, titanium oxide, molybdenum oxide, zirconium oxide, hafnium oxide, and lanthanum oxide; glass; and metals such as metallic cobalt and metallic molybdenum. The substrate S may have a plate-like, spherical, fibrous, or flake-like shape. The surface of the substrate S may be flat or may have a three-dimensional structure such as a trench structure.
[0074] (2) Formation of Precursor Thin Film The precursor thin film can be formed by depositing (adsorbing) a compound represented by general formula (1) in a source gas introduced into a film formation chamber 100 containing a substrate S on the surface of the substrate S. At this time, the substrate S may be heated, or the interior of the film formation chamber 100 may be heated. The conditions for forming the precursor thin film are not particularly limited, and for example, the reaction temperature (the temperature of the substrate when the compound is deposited on the surface of the substrate), the reaction pressure (the pressure inside the film formation chamber when the compound is deposited on the surface of the substrate), the deposition rate, etc. can be appropriately determined depending on the type of thin film-forming raw material M. From the viewpoint of facilitating the formation of a uniform precursor thin film, the reaction temperature is preferably in the range of 0°C to 500°C, more preferably in the range of 100°C to 400°C, and particularly preferably in the range of 200°C to 300°C.
[0075] The reaction pressure when forming the precursor thin film is preferably 1 to 10,000 Pa, more preferably 10 to 1,000 Pa.
[0076] C2. Thin Film Formation Step In the thin film formation step, a reactive gas 202 is introduced into the film formation chamber 100, and the precursor thin film is reacted with the reactive gas 202 to form a molybdenum-containing thin film or a tungsten-containing thin film.
[0077] Examples of the reactive gas 202 include oxidizing gases such as oxygen, ozone, nitrogen dioxide, nitric oxide, water vapor, hydrogen peroxide, formic acid, acetic acid, and acetic anhydride; reducing gases such as hydrogen; organic amine compounds such as monoalkylamines, dialkylamines, trialkylamines, and alkylenediamines; and nitriding gases such as hydrazine and ammonia. These reactive gases 202 may be used alone or in combination of two or more. Among these reactive gases 202, a reactive gas 202 containing at least one selected from the group consisting of hydrogen, ammonia, oxygen, ozone, and water vapor is preferred, as it facilitates the formation of high-quality molybdenum-containing or tungsten-containing thin films with minimal residual carbon. Because the compound represented by general formula (1) has the property of reacting favorably with an oxidizing gas, it is more preferred to use an oxidizing gas such as ozone as the reactive gas 202.
[0078] The heating temperature within the film formation chamber 100 or the substrate S in the thin film formation process may be in the range of room temperature to 500°C. From the viewpoint of facilitating the formation of a high-quality molybdenum-containing thin film or tungsten-containing thin film, the heating temperature is preferably in the range of 100°C to 400°C, and more preferably in the range of 200°C to 300°C. Furthermore, the pressure within the film formation chamber 100 in the thin film formation process is preferably 1 to 10,000 Pa, and more preferably 10 to 1,000 Pa. In the thin film formation process, a voltage may be applied to the reactive gas 202 to generate plasma using an RF matching system 106 connected to a radio frequency (RF) power source 105 installed in the film formation chamber 100. In this case, since excessive power can cause significant damage to the substrate S, a power of 10 W to 1,500 W is preferred, and a power of 50 W to 600 W is more preferred.
[0079] C3. Other Steps The method for producing a thin film of the present invention may include other steps such as an evacuation step, an annealing step, and a reflow step.
[0080] (1) Exhaust Step The thin film manufacturing method of the present invention preferably further includes an exhaust step of exhausting (203) source gases, unreacted reactive gases, and by-product gases from the film formation chamber 100 after the formation of the precursor thin film in the precursor thin film formation step or after the formation of the molybdenum-containing thin film or tungsten-containing thin film in the thin film formation step. Ideally, the undeposited source gases, reactive gases, and by-product gases are completely exhausted from the film formation chamber 100, but complete exhaust is not always necessary. Examples of exhaust methods include a method of purging the film formation chamber 100 with an inert gas (purge gas 204) such as helium, nitrogen, or argon, a method of exhausting (203) the system by reducing the pressure while controlling the degree of pressure reduction using a vacuum pump 107 and an automatic pressure controller 108, and a combination of these methods. When reducing the pressure inside the system, the degree of reduction in pressure is preferably within the range of 0.01 Pa to 300 Pa, and more preferably within the range of 0.01 Pa to 100 Pa from the viewpoint of facilitating the exhaust of the raw material gas, unreacted reactive gas, and by-product gas.
[0081] (2) Annealing and Reflow Processes The thin film manufacturing method of the present invention may further include an annealing process after thin film formation in order to improve the electrical properties of the molybdenum-containing thin film or tungsten-containing thin film. In the annealing process, annealing treatment may be performed in an inert atmosphere, an oxidizing atmosphere, or a reducing atmosphere, and a reflow process may be provided if step filling is required. From the viewpoint of facilitating the production of high-quality molybdenum-containing thin films or tungsten-containing thin films with little residual carbon, the temperature in the annealing process is preferably within the range of 250°C to 500°C.
[0082] C4. Film Formation Cycle The thin film manufacturing method of the present invention may be a method in which the thin film formation step is performed only once, or a method in which the thin film formation step is performed two or more times, but a method in which the thin film formation step is performed two or more times is preferred. In the present invention, a precursor thin film formation step, an evacuation step, a thin film formation step, and an evacuation step are performed in sequence to form a molybdenum-containing thin film or a tungsten-containing thin film through a series of operations, which constitutes one cycle. This cycle may be repeated multiple times until a molybdenum-containing thin film or a tungsten-containing thin film of the required thickness is obtained, thereby forming a molybdenum-containing thin film or a tungsten-containing thin film having a desired thickness. The film thickness of the formed molybdenum-containing thin film or tungsten-containing thin film can be controlled by the number of cycles. The deposition rate of the molybdenum-containing thin film or the tungsten-containing thin film obtained per cycle is preferably within the range of 0.001 nm / min to 100 nm / min, more preferably within the range of 0.005 nm / min to 50 nm / min, from the viewpoint of facilitating the production of a uniform molybdenum-containing thin film or a tungsten-containing thin film.
[0083] C5. Thin Film Manufacturing Method Other Than the ALD Method In the present embodiment, a method for manufacturing a molybdenum-containing thin film or a tungsten-containing thin film by the ALD method has been described, but the method for manufacturing a thin film of the present disclosure is not limited to the above, and may be, for example, a method for forming a molybdenum-containing thin film or a tungsten-containing thin film by a CVD method, in which a compound represented by general formula (1) in a source gas obtained by vaporizing a thin film-forming raw material M is heated and / or plasmatized (hereinafter, "heating and / or plasmatization" may be referred to as heating or the like) to decompose the compound or to react the compound with a reactive gas 202, thereby forming a molybdenum-containing thin film or a tungsten-containing thin film.
[0084] As shown in FIGS. 1 to 4 , the thin film formation process is performed in a film formation chamber 100 in which a substrate S is placed. In the thin film formation process, compounds in a source gas introduced into the film formation chamber 100 are decomposed by heating or the like, and a layer of metallic molybdenum or molybdenum-containing, or a layer of metallic tungsten or tungsten-containing, is deposited on the surface of the substrate S, thereby forming a molybdenum-containing thin film or a tungsten-containing thin film. Note that FIGS. 1 to 4 show an example in which compounds in a source gas introduced into the film formation chamber 100 are heated in the presence of a reactive gas 202. In this example, a molybdenum-containing thin film or a tungsten-containing thin film is formed by reaction of the compounds with the reactive gas 202. In this case, not only the compounds but also the reactive gas 202 are heated and / or converted into plasma.
[0085] In this case, the heating temperature in the film formation chamber 100 or the substrate S and the conditions for generating plasma are the same as those in the thin film formation process in the ALD method.
[0086] Furthermore, the compound represented by the general formula (1) of the present invention can also be used as a raw material for forming a thin film by a MOD method such as a sputtering method, an ion plating method, a coating pyrolysis method, or a sol-gel method, in addition to the above-mentioned ALD method and CVD method.
[0087] D. Thin Films Produced Using Thin-Film-Forming Raw Materials Thin films produced using the thin-film-forming raw material M of the present invention include thin films of metallic molybdenum, molybdenum oxide, molybdenum nitride, metallic tungsten, tungsten oxide, and tungsten nitride. The above-described thin-film production method can efficiently produce thin films of molybdenum oxide and tungsten oxide. The thin films of the present invention can be produced as desired by appropriately selecting other precursors, reactive gases, and production conditions in the above-described thin-film production method. Because the thin films of the present invention have excellent electrical and optical properties, they can be widely used in the production of, for example, electrode materials for memory devices such as DRAM devices, wiring materials used in semiconductor devices such as logic devices, insulating materials, diamagnetic films used in the recording layers of hard disks, and catalyst materials for polymer electrolyte fuel cells. Furthermore, the carbon content in the thin film is preferably 1 atm% or less, more preferably 0.5 atm% or less, and even more preferably 0.1 atm% or less.
[0088] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0089] Example 1: Preparation of Compound No. 10 A 300 mL four-neck flask was charged with 15.0 g (0.046 mol) of bis(t-butylimino)bis(dimethylamino)molybdenum and 112 ml of tetrahydrofuran, and the mixture was stirred for 30 minutes under ice cooling. 4.4 g (0.276 mol) of methanol was added dropwise under ice cooling, and the mixture was stirred for 30 minutes. Next, 6.15 g (0.069 mol) of 2-(dimethylamino)ethanol was added dropwise under ice cooling, and the mixture was then returned to room temperature and stirred for 16 hours. The solvent was then removed, and the residue was distilled at a bath temperature of 128°C, a pressure of 52 Pa, and an overhead temperature of 104°C to obtain Compound No. 10 as a transparent orange liquid. The yield was 11.4 g, a 71% yield.
[0090] (Analytical value) (1) 1H-NMR (heavy benzene) 1.30ppm (9H, singlet), 2.31-2.34ppm (2H, triplet), 2.39ppm (6H, singlet) , 4.28-4.31ppm (2H, triplet), 4.49ppm (6H, singlet), 4.58ppm (3H, singlet) (2) Elemental analysis (metal analysis: ICP-AES) Mo content: 28.0 mass% (theoretical value 27.6 mass%)
[0091] Example 2: Preparation of Compound No. 11 A 100 mL three-neck flask was charged with 1.80 g (0.0055 mol) of bis(t-butylimino)bis(dimethylamino)molybdenum and 14 ml of tetrahydrofuran, and the mixture was stirred for 30 minutes under ice cooling. 0.53 g (0.0165 mol) of methanol was added dropwise under ice cooling, and the mixture was stirred for 30 minutes. Next, 0.50 g (0.0055 mol) of 1-(dimethylamino)-2-propanol was added dropwise under ice cooling, and the mixture was then returned to room temperature and stirred for 16 hours. The solvent was then removed, and the residue was distilled at a bath temperature of 100°C and a pressure of 26 Pa to obtain Compound No. 11 as a transparent orange liquid. The yield was 1.22 g, a 61% yield.
[0092] (Analytical values) (1) 1H-NMR (heavy benzene) 1.15-1.17ppm (3H, double), 1.30ppm (9H, singlet), 1.89-1.92ppm (1H, double doublet), 2.36ppm (3H, singlet), 2.45-2.50ppm (4H, multilet), 4.40-4.47ppm (1H , multilet), 4.48ppm (3H, singlet), 4.52ppm (3H, singlet), 4.59ppm (3H, singlet) (2) Elemental analysis (metal analysis: ICP-AES) Mo content: 27.0 mass% (theoretical value 26.5 mass%)
[0093] Example 3: Preparation of Compound No. 12 A 100 mL three-neck flask was charged with 1.83 g (0.0053 mol) of bis(t-butylimino)bis(dimethylamino)molybdenum and 13 ml of tetrahydrofuran, and the mixture was stirred for 30 minutes under ice cooling. 0.51 g (0.0159 mol) of methanol was added dropwise under ice cooling, and the mixture was stirred for 30 minutes. Next, 0.63 g (0.0053 mol) of 1-(dimethylamino)-2-methyl-2-propanol was added dropwise under ice cooling, and the mixture was then returned to room temperature and stirred for 16 hours. The solvent was then removed, and the residue was distilled at a bath temperature of 108°C and a pressure of 62 Pa to obtain Compound No. 12 as a transparent orange liquid. The yield was 0.90 g, a 45% yield.
[0094] (Analytical value) (1) 1H-NMR (heavy benzene) 1.30ppm (9H, singlet), 1.31ppm (6H, singlet), 2.43ppm (2H, singlet) , 2.49ppm (6H, singlet), 4.55ppm (6H, singlet), 4.58ppm (3H, singlet) (2) Elemental analysis (metal analysis: ICP-AES) Mo content: 25.8% by mass (theoretical value 25.5% by mass)
[0095] Example 4: Preparation of Compound No. 82 A 300 mL three-neck flask was charged with 28.5 g (0.069 mol) of bis(t-butylimino)bis(dimethylamino)tungsten and 189 ml of tetrahydrofuran, and the mixture was stirred for 1 hour under ice cooling. 6.15 g (0.069 mol) of 2-(dimethylamino)ethanol was added dropwise under ice cooling, and the mixture was stirred for 2 hours. Next, 8.8 g (0.276 mol) of methanol was added dropwise under ice cooling, and the mixture was allowed to warm to room temperature and stirred for 18 hours. The solvent was then removed, and the residue was distilled at a bath temperature of 109°C, a pressure of 16 Pa, and an overhead temperature of 81°C to obtain Compound No. 82 as a pale yellow, transparent liquid. The yield was 25.5 g, or 85%.
[0096] (Analytical value) (1) 1H-NMR (heavy benzene) 1.34ppm (9H, singlet), 2.26-2.29ppm (2H, triplet), 2.35ppm (6H, singlet) , 4.39-4.41ppm (2H, triplet), 4.59ppm (6H, singlet), 4.64ppm (3H, singlet) (2) Elemental analysis (metal analysis: ICP-AES) W content: 41.6% by mass (theoretical value 42.1% by mass)
[0097] Example 5: Preparation of Compound No. 83 A 100 mL three-neck flask was charged with 1.84 g (4.44 mmol) of bis(t-butylimino)bis(dimethylamino)tungsten and 10 mL of tetrahydrofuran, and the mixture was stirred. 0.46 g (4.44 mmol) of 1-dimethylamino-2-propanol was added dropwise to the mixture under ice cooling, and the mixture was stirred for 1 hour. Next, 0.57 g (17.7 mmol) of methanol was added dropwise under ice cooling, and the mixture was allowed to warm to room temperature and stirred for 18 hours. The solvent was then removed, and the residue was distilled at a bath temperature of 100°C and a pressure of 50 Pa to obtain Compound No. 83 as a pale yellow, transparent liquid. The yield was 1.28 g, a 64% yield.
[0098] (Analytical value) (1) 1H-NMR (heavy benzene) 1.12ppm (3H, doublet), 1.34ppm (9H, singlet), 1.87-1.91ppm (1H, multiplet), 2.31ppm (3H, singlet), 2.39-2.47ppm ( 4H, multiplet), 4.42-4.47ppm (1H, multiplet), 4.58ppm (3H, singlet), 4.61ppm (3H, singlet), 4.65ppm (3H, singlet) (2) Elemental analysis (metal analysis: ICP-AES) W content: 40.6 mass% (theoretical value 40.8 mass%)
[0099] Example 6: Preparation of Compound No. 84 A 100 mL three-neck flask was charged with 1.78 g (4.31 mmol) of bis(t-butylimino)bis(dimethylamino)tungsten and 10 mL of tetrahydrofuran, and the mixture was stirred. 0.50 g (4.31 mmol) of 1-dimethylamino-2-methyl-2-propanol was added dropwise to the mixture under ice cooling, and the mixture was stirred for 1 hour. Next, 0.55 g (17.2 mmol) of methanol was added dropwise under ice cooling, and the mixture was then returned to room temperature and stirred for 18 hours. The solvent was then removed, and the residue was distilled at a bath temperature of 100°C and a pressure of 50 Pa to obtain Compound No. 84 as a pale yellow, transparent liquid. The yield was 0.95 g, a 48% yield.
[0100] (Analytical value) (1) 1H-NMR (heavy benzene) 1.27ppm (6H, singlet), 1.34ppm (9H, singlet), 2.39ppm (2H, singlet) , 2.46ppm (6H, singlet), 4.63ppm (6H, singlet), 4.65ppm (3H, singlet) (2) Elemental analysis (metal analysis: ICP-AES) W content: 39.2 mass% (theoretical value 39.6 mass%)
[0101] Example 7: Preparation of Compound No. 100 A 100 mL three-neck flask was charged with 1.73 g (4.18 mmol) of bis(t-butylimino)bis(dimethylamino)tungsten and 10 ml of tetrahydrofuran, and the mixture was stirred. 0.37 g (4.18 mmol) of 2-(dimethylamino)ethanol was added dropwise to the mixture under ice cooling, and the mixture was stirred for 1 hour. Next, 0.77 g (16.7 mmol) of ethanol was added dropwise under ice cooling, and the mixture was allowed to warm to room temperature and stirred for 18 hours. The solvent was then removed, and the residue was distilled at a bath temperature of 105°C and a pressure of 50 Pa to obtain Compound No. 100 as a pale yellow, transparent liquid. The yield was 1.13 g, a 57% yield.
[0102] (Analytical value) (1) 1H-NMR (heavy benzene) 1.32-1.37ppm (18H, multiplet), 2.34-2.37ppm (2H, multiplet), 2.43ppm (6 H, singlet), 4.42-4.45ppm (2H, multiplet), 4.70-4.80ppm (6H, multiplet) (2) Elemental analysis (metal analysis: ICP-AES) W content: 38.6% by mass (theoretical value 38.4% by mass)
[0103] [Evaluation Example] Evaluation of Compound Properties The compounds obtained in Examples 1 to 7 and the following Comparative Compounds 1 and 2 were evaluated as follows. Note that "Me" in the following Comparative Compound 1 represents a methyl group, and "sBu" represents a sec-butyl group. (1) Evaluation of State and Melting Point The state of the compound at normal pressure and 25°C was observed visually. For compounds that were solid at 25°C, the melting point was measured using a micro melting point measurement device. Compounds with low melting points have excellent transport properties and can be considered preferable as thin film-forming raw materials. The results are shown in Table 1. (2) Temperature (°C) at 50% mass loss in normal pressure TG-DTA Measurements were performed using a TG-DTA at 760 Torr, an Ar flow rate of 100 mL / min, a heating rate of 10°C / min, and a scanning temperature range of 30°C to 600°C. The temperature (°C) at which the weight of the test compound had decreased by 50% by mass was evaluated as the "temperature (°C) at 50% mass loss in normal pressure TG-DTA." The lower the temperature (°C) at which the test compound lost 50% by mass in the atmospheric pressure TG-DTA, the lower the temperature at which vapor was obtained. The results are shown in Table 1 below. (3) Temperature (°C) at which the test compound lost 50% by mass in the reduced pressure TG-DTA: Using a TG-DTA, measurements were performed at 10 Torr, an Ar flow rate of 50 mL / min, a heating rate of 10°C / min, and a scanning temperature range of 30°C to 600°C. The temperature (°C) at which the test compound lost 50% by mass was evaluated as the "temperature (°C) at which the test compound lost 50% by mass in the reduced pressure TG-DTA." The lower the temperature (°C) at which the test compound lost 50% by mass in the reduced pressure TG-DTA, the lower the temperature at which vapor was obtained. The results are shown in Table 1 below. (4) Thermal Stability Evaluation The thermal decomposition onset temperature was measured using a DSC measurement device. Materials with a high thermal decomposition onset temperature are less likely to undergo thermal decomposition and can be considered preferable as thin film-forming raw materials. The results are shown in Table 1.
[0104]
[0105]
[0106] As shown in Table 1 above, Comparative Compounds 1 and 2 both have melting points of about 60°C and are solid at 25°C, whereas the compounds obtained in Examples 1 to 7 are all liquid at 25°C, and therefore, it was found that they are compounds with particularly excellent transportability.
[0107] Furthermore, the temperature of Comparative Compound 1 at 50% mass loss by TG-DTA under atmospheric pressure could not be measured due to decomposition, whereas the temperatures of the compounds obtained in Examples 1 to 3 at 50% mass loss by TG-DTA under atmospheric pressure were all 215°C or lower, indicating that they were compounds with high vapor pressure. The temperatures of the compounds obtained in Examples 2 and 3 at 50% mass loss by TG-DTA under atmospheric pressure were all 205°C or lower, indicating that they were compounds with particularly high vapor pressure. While the temperature of Comparative Compound 2 at 50% mass reduction by atmospheric pressure TG-DTA was 242°C, the compounds obtained in Examples 4 to 7 all had temperatures of 200°C or lower at 50% mass reduction by atmospheric pressure TG-DTA, indicating that they are compounds with high vapor pressure. The compounds obtained in Examples 4 to 6 all had temperatures of 195°C or lower at 50% mass reduction by atmospheric pressure TG-DTA, indicating that they are compounds with even higher vapor pressure. The compounds obtained in Examples 5 and 6 all had temperatures of 190°C or lower at 50% mass reduction by atmospheric pressure TG-DTA, indicating that they are compounds with particularly high vapor pressure.
[0108] Furthermore, while the temperature of Comparative Compound 1 at 50% mass loss by reduced pressure TG-DTA was 135°C, the temperatures of all of the compounds obtained in Examples 1 to 3 at 50% mass loss by reduced pressure TG-DTA were 125°C or lower, indicating that they were compounds with high vapor pressure. The temperatures of all of the compounds obtained in Examples 2 and 3 at 50% mass loss by reduced pressure TG-DTA were 115°C or lower, indicating that they were compounds with particularly high vapor pressure. While the temperature of Comparative Compound 2 at 50% mass reduction by reduced pressure TG-DTA was 163°C, the temperatures of all of the compounds obtained in Examples 4 to 7 at 50% mass reduction by reduced pressure TG-DTA were 125°C or lower, indicating that they are compounds with high vapor pressure. The temperatures of all of the compounds obtained in Examples 4 to 6 at 50% mass reduction by reduced pressure TG-DTA were 115°C or lower, indicating that they are compounds with even higher vapor pressure. The temperatures of all of the compounds obtained in Examples 5 and 6 at 50% mass reduction by reduced pressure TG-DTA were 110°C or lower, indicating that they are compounds with particularly high vapor pressure.
[0109] Furthermore, while the thermal decomposition onset temperature of Comparative Compound 1 was 192°C, the compounds obtained in Examples 1 to 3 all had thermal decomposition onset temperatures of 215°C or higher, indicating that they were highly thermally stable compounds. The compounds obtained in Examples 1 and 2 all had thermal decomposition onset temperatures of 225°C or higher, indicating that they were particularly highly thermally stable compounds. While the thermal decomposition onset temperature of Comparative Compound 2 was 257°C, the compounds obtained in Examples 4 to 7 all had thermal decomposition onset temperatures of 265°C or higher, indicating that they were highly thermally stable compounds. The compounds obtained in Examples 4, 5, and 7 all had thermal decomposition onset temperatures of 275°C or higher, indicating that they were particularly highly thermally stable compounds.
[0110] <Production of Thin Films by ALD Method> Using the compounds of the present invention obtained in Examples 1 to 7 and Comparative Compounds 1 and 2 as chemical vapor deposition sources, molybdenum oxide thin films and tungsten oxide thin films were produced on silicon substrates S by ALD method under the following conditions using the apparatus shown in FIG. 1. The film thickness of the obtained thin films was measured by X-ray reflectivity method, the compounds of the thin films were confirmed by X-ray diffraction method, and the carbon content in the thin films was measured by X-ray photoelectron spectroscopy. The results are shown in Table 2.
[0111] Examples 8 to 14, Comparative Examples 1 and 2: Production of Molybdenum Oxide and Tungsten Oxide Thin Films by ALD (Conditions) Reaction temperature (temperature of substrate S): 250°C, reactive gas 202: ozone (Steps) A series of steps (1) to (4) below constitute one cycle, and were repeated 100 times. (1) The vapor of thin film-forming raw material M, vaporized under conditions of a heating temperature of 80°C for the source material container 101 and a pressure of 100 Pa inside the source material container 101, was introduced into the film-forming chamber 100 and deposited for 10 seconds at a system pressure of 100 Pa. (Precursor thin film forming step) (2) Unreacted raw material was removed by argon purging for 30 seconds. (Exhaust step) (3) Reactive gas 202 was introduced into the film-forming chamber 100 and reacted for 0.1 seconds at a system pressure of 100 Pa. (Thin film forming step) (4) Unreacted raw material was removed by argon purging for 120 seconds. (Exhaust step)
[0112]
[0113] The carbon content in the molybdenum oxide thin film obtained by the ALD method was 3 atm% in Comparative Example 1, while it was less than the detection limit of 0.1 atm% in Examples 8 to 10. The carbon content in the tungsten oxide thin film obtained by the ALD method was 4 atm% in Comparative Example 2, while it was less than the detection limit of 0.1 atm% in Examples 11 to 14. This demonstrates that high-quality molybdenum oxide or tungsten oxide thin films can be obtained by using the compound of the present invention. Furthermore, the film thickness of the obtained thin film was 4.3 nm in Comparative Example 1, while it was 5.8 nm or more in Examples 8 to 10, demonstrating that molybdenum oxide thin films could be obtained with high productivity by using the compound of the present invention. In particular, the film thickness of the obtained thin film was 6.2 nm in Example 9, demonstrating higher productivity in obtaining molybdenum oxide thin films. The film thickness of the obtained thin film was 4.4 nm in Comparative Example 2, while it was 5.4 nm or more in Examples 11 to 14, demonstrating that tungsten oxide thin films could be obtained with high productivity by using the compound of the present invention. In particular, in Examples 11 to 13, the thickness of the resulting thin film was 5.8 nm or more, and tungsten oxide thin films were obtained with higher productivity. In Example 12, the thickness of the resulting thin film was 6.3 nm, and tungsten oxide thin films were obtained with particularly high productivity.
[0114] As described above, the compounds of the present invention have low melting points, high vapor pressures, and high thermal stability. Furthermore, when used as thin film formation sources by the ALD method, high-quality thin films could be obtained with high productivity, demonstrating their superiority as thin film formation sources for chemical vapor deposition. Among these, Compounds Nos. 10-12 and 82-84 have low melting points, high vapor pressures, and high thermal stability. Furthermore, when used as thin film formation sources by the ALD method, thin films could be obtained with high productivity, demonstrating their superiority as thin film formation sources for chemical vapor deposition. In particular, Compounds Nos. 11 and 83 have low melting points, high vapor pressures, and high thermal stability. Furthermore, when used as thin film formation sources by the ALD method, thin films could be obtained with particularly high productivity, demonstrating their superiority as thin film formation sources for chemical vapor deposition.
[0115] REFERENCE SIGNS LIST 100 Film formation chamber 101 Source container 102 Vaporization chamber 103 Heater 104 Mass flow controller (MFC) 105 Radio frequency (RF) power supply 106 RF matching system 107 Vacuum pump 108 Automatic pressure controller 109 Cold trap 201 Carrier gas 202 Reactive gas 203 Exhaust 204 Purge gas M Thin film forming source material S Substrate
Claims
1. A compound represented by the following general formula (1): In the formula, R 1 and R 2 each independently represents an alkyl group having 1 to 5 carbon atoms; A 1 represents an alkanediyl group having 1 to 8 carbon atoms; L 1 represents a group represented by the following formula (L-1) or (L-2), M 1 represents a molybdenum atom or a tungsten atom; α, β, and γ represent integers of 1 or more, and the sum of 2α, β, and γ is 6. (In the formula, R 11 ~R 13 each independently represents an alkyl group having 1 to 5 carbon atoms, and * represents a bond.
2. The compound of claim 1, wherein α and β are 1 and γ is 3.
3. A thin film forming material containing the compound according to claim 1 or 2.
4. A thin film produced by using the thin film forming material according to claim 3.
5. A method for producing a thin film, comprising forming a thin film containing molybdenum atoms or tungsten atoms on the surface of a substrate using the thin film forming material according to claim 3.
6. A method for producing a thin film according to claim 5, comprising introducing a source gas obtained by vaporizing the thin film-forming source into a film-forming chamber in which a substrate is placed, and heating and / or plasmatizing the compound represented by general formula (1) in the source gas to decompose the compound or react the compound with a reactive gas to form a thin film containing molybdenum atoms or tungsten atoms on the surface of the substrate.
7. A method for producing a thin film according to claim 5, comprising the steps of: introducing a source gas obtained by vaporizing the thin film forming source into a film formation chamber, and depositing the compound represented by general formula (1) in the source gas on the surface of a substrate to form a precursor thin film; and introducing a reactive gas into the film formation chamber, and reacting the precursor thin film with the reactive gas to form a thin film containing molybdenum atoms or tungsten atoms.
Citation Information
Patent Citations
Group 6 Film-Forming Composition for Deposition of a Group 6 Transition Metal-Containing Film
JP2017525156A
Tungsten precursor and method of forming tungsten-containing layer using the same
JP2019004138A
Substantially carbon-free molybdenum- and tungsten-containing films in the manufacture of semiconductor devices
JP2022544674A
Tungsten compound, raw material for thin film formation and method for producing thin film
WO2019039103A1
Thin film-forming material, thin film manufacturing method, thin film, and molybdenum compound