Biodegradable resin composition, molded body, and multilayer body
The biodegradable resin composition with specific aliphatic-aromatic polyester and filler properties addresses the issue of pigment-induced coloration and oxidation in packaging materials, ensuring effective color resistance and sustainability for food and drink packaging applications.
Patent Information
- Application Number
- PCT/JP2024/019503
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-29
- Filing Date
- 2024-05-28
- Publication Date
- 2024-12-05
AI Technical Summary
Aliphatic-aromatic polyesters used in food and drink packaging materials tend to be colored by pigments, leading to unsightly discoloration and potential oxidation issues, which affects their performance and environmental impact.
A biodegradable resin composition comprising an aliphatic-aromatic polyester with a specific ester group content, polybutylene succinate terephthalate, and a filler, which minimizes pigment penetration and oxidation, ensuring excellent color resistance and mouth-opening properties.
The composition effectively prevents coloration from food and drink pigments, maintains excellent opening properties, and enhances environmental sustainability by being biodegradable, making it suitable for food and drink packaging.
Smart Images

Figure JP2024019503_05122024_PF_FP_ABST
Abstract
Description
Biodegradable resin composition, molded article, and laminate
[0001] The present invention relates to a biodegradable resin composition, a molded article, and a laminate.
[0002] Paper cups have traditionally been widely used as disposable beverage packaging. The surface of the paper used in paper cups is generally laminated with a non-biodegradable resin such as polyethylene to prevent beverage penetration and leakage. Therefore, paper cups are typically incinerated after use, and if they leak into the environment, the resin layer remains there semi-permanently. In addition to paper cups, various other disposable plastic food and beverage packaging materials are also used, which poses problems from the perspectives of environmental pollution and resource conservation. If biodegradable resins were used for these packaging materials, they could be composted together with food and beverage residues without separation, and would be biodegradable even if they were to leak into the environment, thereby contributing to environmental protection.
[0003] Aliphatic-aromatic polyesters such as polybutylene adipate terephthalate (PBAT) are widely used as biodegradable polyester resins that combine similar flexibility, breaking strength, and good moldability to polyethylene. The development of technologies related to aliphatic-aromatic polyesters, as well as technologies for coating paper with coating agents containing aliphatic-aromatic polyesters, has been extensively pursued. For example, Patent Document 1 discloses a technology for obtaining an aliphatic-aromatic polyester resin whose main structural units are aliphatic dicarboxylic acid units, aromatic dicarboxylic acid units, and aliphatic diol units and / or alicyclic diol units, in which the ratio (molar ratio) of the aliphatic dicarboxylic acid units to the aromatic dicarboxylic acid units is set within a specific range, the resin has a specific glass transition temperature, and further, a specific branched structure is incorporated, thereby achieving excellent thermal stability, molding stability, and mechanical properties. Patent Document 2 also discloses a technology for obtaining a coating agent that has excellent fluidity and adhesion and can be suitably applied to paper by incorporating an aliphatic-aromatic polyester with a specific melt volume flow rate (MVR) and specific other components.
[0004] International Publication No. 2022 / 014434 Special Publication No. 2012-504195
[0005] As described above, it is known that aliphatic-aromatic polyesters are used in food and beverage packaging materials. However, when aliphatic-aromatic polyesters are used in food and beverage packaging materials, there is a problem that discoloration by pigments contained in the food and beverage is likely to occur, leaving room for improvement. Therefore, the present invention aims to solve the above problem, and one aspect of the present invention aims to provide a biodegradable resin composition using an aliphatic-aromatic polyester that can be used to produce a molded article that is resistant to discoloration by pigments contained in food and beverages, as well as molded articles and laminates (hereinafter sometimes referred to as "molded articles, etc.") that are resistant to discoloration by pigments contained in food and beverages. Another aspect of the present invention aims to provide a biodegradable resin composition that can produce a molded article that is resistant to discoloration by pigments contained in food and beverages and has excellent opening properties, as well as molded articles, etc., and laminates that are resistant to discoloration by pigments contained in food and beverages and have excellent opening properties.
[0006] As a result of investigations into the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by using an aliphatic-aromatic polyester having an ester group content within a specific range, and have thus completed the present invention.
[0007] That is, the gist of the present invention resides in the following items. [1] A biodegradable resin composition containing an aliphatic-aromatic polyester and a filler, wherein the content of the aliphatic-aromatic polyester relative to the biodegradable resin composition is 20% by mass or more and 99% by mass or less, the content of the filler relative to the biodegradable resin composition is 0.3% by mass or more and 50.0% by mass or less, and the content of ester groups contained in the aliphatic-aromatic polyester is 9.6 mol / kg or more. [2] The biodegradable resin composition according to [1], wherein the aliphatic-aromatic polyester has a glass transition temperature in the range of -27 to 0°C. [3] The biodegradable resin composition according to [1] or [2], wherein the aliphatic-aromatic polyester contains at least polybutylene succinate terephthalate. [4] The biodegradable resin composition according to [3], wherein the polybutylene succinate terephthalate has a biobased carbon content of 50% or more as measured according to ISO 16620-2. [5] The biodegradable resin composition according to [3], wherein the proportion of structural units derived from terephthalic acid among all structural units derived from dicarboxylic acids contained in the aliphatic-aromatic polyester is 15 to 70 mol %. [6] The biodegradable resin composition according to any one of [1] to [5], further comprising an aliphatic polyester. [7] The biodegradable resin composition according to any one of [1] to [6], wherein the biobased carbon content measured according to ISO 16620-2 is 20% or more. [8] A molded article made from the biodegradable resin composition according to any one of [1] to [7]. [9] The molded article according to [8], which is a food and beverage packaging material.
[10] The molded article according to [9], wherein the food and beverage packaging material is a food and beverage container.
[11] A laminate having a substrate and a layer made from the biodegradable resin composition according to any one of [1] to [7].
[12] The laminate according to
[11] , which is a food and beverage packaging material.
[13] The laminate according to
[12] , wherein the food and beverage packaging material is a food and beverage container.
[14] Polybutylene succinate terephthalate having an ester group content of 9.6 mol / kg or more and a bio-based carbon content of 20% or more as measured by ISO 16620-2.
[15] The polybutylene succinate terephthalate according to
[14] , which has a biobased carbon content of 50% or more as measured according to ISO 16620-2.
[16] A molded article comprising the polybutylene succinate terephthalate according to
[14] or
[15] .
[17] The molded article according to
[16] , which is a food and beverage packaging material.
[18] The molded article according to
[17] , wherein the food and beverage packaging material is a food and beverage container.
[19] A laminate having a substrate and a layer comprising the polybutylene succinate terephthalate according to
[14] or
[15] .
[20] The laminate according to
[19] , which is a food and beverage packaging material.
[21] The laminate according to
[20] , wherein the food and beverage packaging material is a food and beverage container.
[0008] According to one aspect of the present invention, it is possible to obtain a biodegradable resin composition using an aliphatic-aromatic polyester that can be used to produce a molded article that is resistant to discoloration by pigments contained in food and beverages, as well as a molded article that is resistant to discoloration by pigments contained in food and beverages. Also, according to another aspect of the present invention, it is possible to obtain a biodegradable resin composition that can give a molded article that is resistant to discoloration by pigments contained in food and beverages and has excellent opening properties, as well as a molded article and laminate that are resistant to discoloration by pigments contained in food and beverages and has excellent opening properties.
[0009] 1 is a graph showing the shape of the crystallization peak in temperature-drop measurement using a differential scanning calorimeter in Examples 4 to 6.
[0010] The present invention is not limited to the following description and can be modified as desired without departing from the spirit and scope of the present invention. In this specification, when a numerical value or physical property value is enclosed before and after the prefix "to", the lower and upper limits are included as endpoints. Furthermore, when a numerical range is described in stages, any combination of the upper and lower limits of each numerical range is also disclosed. In this specification, "mass %," "mass ppm," and "parts by mass" are synonymous with "weight %," "weight ppm," and "parts by weight." Furthermore, in this specification, the expression "A or B" can be interpreted as "at least one selected from the group consisting of A and B." Although multiple embodiments are described in this specification, various conditions in each embodiment can be applied to each other to the extent applicable. Furthermore, in this specification, a structural unit derived from A is also referred to as an "A unit."
[0011] <Biodegradable Resin Composition> A biodegradable resin composition according to one embodiment of the present invention (hereinafter sometimes simply referred to as "composition") comprises an aliphatic-aromatic polyester and a filler, the aliphatic-aromatic polyester being contained in a proportion of 20% by mass or more and 99% by mass or less relative to the composition, and the filler being contained in a proportion of 0.3% by mass or more and 50.0% by mass or less relative to the composition. The aliphatic-aromatic polyester has an ester group content of 9.6 mol / kg or more.
[0012] Conventionally, when aliphatic-aromatic polyesters are used as packaging materials for food and beverages, they have a problem of being prone to discoloration due to the pigments contained in the food and beverages. Aliphatic-aromatic polyesters are typically semi-crystalline resins, having both crystalline and amorphous portions. The inventors speculated that these amorphous portions have a large free volume between polymer chains, and that the pigments contained in the food and beverages penetrate into this free volume, resulting in discoloration. The inventors then hypothesized that the penetration of pigment molecules could be suppressed if the ester groups contained in the aliphatic-aromatic polyester form hydrogen bonds with adjacent polymer chains. As a result of extensive research, they discovered that the above-mentioned discoloration problem could be suppressed by using the above-mentioned composition, in which the content of ester groups contained in the aliphatic-aromatic polyester is increased above a desired value. The composition according to this embodiment will be described in detail below.
[0013] [Configuration of Aliphatic-Aromatic Polyester] Aliphatic-aromatic polyester (hereinafter sometimes simply referred to as "polyester") is a polyester containing, as main structural units, an aliphatic dicarboxylic acid unit, an aromatic dicarboxylic acid unit, and an aliphatic diol unit. The aliphatic-aromatic polyester may contain structural units other than the above-mentioned diol unit and dicarboxylic acid unit. The aromatic compound unit may contain an aromatic dicarboxylic acid unit, but may also contain an aromatic diol unit. One type of aliphatic-aromatic polyester may be used alone, or two or more types may be used in combination. In this specification, the "main structural unit" in an aliphatic-aromatic polyester usually refers to a structural unit that is contained in a total of 80 mol% or more of the total 100 mol% of all structural units constituting the aliphatic-aromatic polyester, and there are cases where no structural units other than the main structural unit are contained. The configuration of the aliphatic-aromatic polyester is as follows: 1 It can be identified by H-NMR, pyrolysis gas chromatography, etc.
[0014] (Diol) Specific types of diols that provide diol units are listed below, and at least one type of aliphatic-aromatic polyester may contain constituent units derived from the listed diols.
[0015] As the diol that provides the diol unit, any diol that is usually used as a raw material for polyester can be used without any particular limitation. As the diol, at least an aliphatic diol is used, and an aromatic diol may also be used. The structure of the diol may be a linear structure, a branched chain structure, or a cyclic structure.
[0016] The number of carbon atoms in the aliphatic diol is not particularly limited, but is usually 2 to 20. From the viewpoints of moldability, mechanical strength, and controlling the content of ester groups within a desired range, the number of carbon atoms is preferably 2 to 12, more preferably 2 to 6, and particularly preferably 2 to 4.
[0017] Examples of aliphatic diols include alkylene diols such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, and neopentyl glycol; oxyalkylene diols such as diethylene glycol, polyethylene glycol, polypropylene glycol, or polytetramethylene ether glycol; or cycloalkylene diols such as 1,2-cyclohexanediol, 1,4-cyclohexanediol, 1,2-cyclohexanedimethanol, or 1,4-cyclohexanedimethanol. From the viewpoint of biodegradability, among these, ethylene glycol, 1,3-propanediol, and 1,4-butanediol are preferred, ethylene glycol or 1,4-butanediol are more preferred, and 1,4-butanediol is particularly preferred. These aliphatic diols may or may not be derivatives thereof.
[0018] Specific examples of aromatic diols include xylylene glycol, 4,4'-dihydroxybiphenyl, 2,2-bis(4'-hydroxyphenyl)propane, 2,2-bis(4'-β-hydroxyethoxyphenyl)propane, bis(4-hydroxyphenyl)sulfone, bis(4-β-hydroxyethoxyphenyl)sulfonic acid, etc. These aromatic diols may or may not be derivatives thereof.
[0019] The above aliphatic diol compounds and / or aromatic diol compounds may be compounds having a structure in which one or more kinds of compounds are mutually dehydrated and condensed.
[0020] The diol may be used alone or in combination of two or more kinds.
[0021] Furthermore, ethylene glycol, 1,3-propanediol, 1,4-butanediol, and the like derived from plant materials can be used.
[0022] Total Content of Diol Units in Aliphatic-Aromatic Polyester The total content of diol units in an aliphatic-aromatic polyester is not particularly limited, but from the viewpoint of flowability and melt tension, it is usually 10 mol% or more, preferably 30 mol% or more, more preferably 40 mol% or more, and even more preferably 45 mol% or more, relative to 100 mol% of all constituent units constituting the aliphatic-aromatic polyester. Furthermore, the total content of diol units in an aliphatic-aromatic polyester is calculated based on the smallest ester unit of the aliphatic-aromatic polyester. Therefore, the total content of diol units is the ratio of the number of moles of the smallest diol units to the total number of moles when the smallest ester unit of the aliphatic-aromatic polyester is counted as 1 mole. Furthermore, the "total content" refers to the ratio of the number of moles of one type of diol unit to the number of moles of all ester units when the aliphatic-aromatic polyester contains one type of diol unit, and refers to the ratio of the total number of moles of the two or more types of diol units to the number of moles of all ester units when the aliphatic-aromatic polyester contains two or more types of diol units.
[0023] (Dicarboxylic acid) As the dicarboxylic acid that gives the dicarboxylic acid unit, at least an aliphatic dicarboxylic acid and an aromatic dicarboxylic acid are used, and as these aliphatic dicarboxylic acids and aromatic dicarboxylic acids and any other dicarboxylic acids, those that are usually used as raw materials for polyesters can be used without any particular limitation. The structure of the dicarboxylic acid may be a linear structure, a branched chain structure, or may have a ring structure.
[0024] Specific types of dicarboxylic acids that provide dicarboxylic acid units are listed below, and at least one type of polyester may contain structural units derived from the listed dicarboxylic acids.
[0025] The number of carbon atoms in the aliphatic dicarboxylic acid is not particularly limited, but is usually 2 to 36, preferably 3 to 12, more preferably 3 to 10, even more preferably 3 to 6, and particularly preferably 4. When the number of carbon atoms in the aliphatic dicarboxylic acid is equal to or greater than the lower limit of the above range, good moldability can be obtained. On the other hand, when the number of carbon atoms in the aliphatic dicarboxylic acid is equal to or less than the upper limit of the above range, mechanical properties can be further improved.
[0026] Specific examples of aliphatic dicarboxylic acids include aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, succinic anhydride, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, brassylic acid, maleic acid, fumaric acid, and dimer acid. Among these, saturated aliphatic dicarboxylic acids such as succinic acid, succinic anhydride, adipic acid, and sebacic acid are preferred from the viewpoints of thermal stability and crystallinity. Succinic acid is particularly preferred. Succinic acid (carbon number 4) has a lower carbon number than other dicarboxylic acids such as adipic acid (carbon number 6) and sebacic acid (carbon number 10), allowing for a higher ester group content and making it easier to adjust to the range described herein. As the aliphatic dicarboxylic acid unit, a succinic acid unit may be used alone or in combination of two or more types, but it is most preferred to use a succinic acid unit alone. These aliphatic diols may or may not be derivatives thereof.
[0027] The number of carbon atoms in the aromatic dicarboxylic acid is not particularly limited, but is usually 6 to 30, preferably 6 to 25, more preferably 6 to 15, and even more preferably 6 to 8. When the number of carbon atoms in the aromatic dicarboxylic acid is equal to or greater than the lower limit of the above range, thermal stability can be further improved. On the other hand, when the number of carbon atoms in the aromatic dicarboxylic acid is equal to or less than the upper limit of the above range, moldability can be further improved.
[0028] Specific examples of aromatic dicarboxylic acids include terephthalic acid, 2,5-furandicarboxylic acid, phthalic acid, isophthalic acid, dibromoisophthalic acid, sulfoisophthalic acid, 1,4-phenylenedioxydicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 4,4'-diphenylketonedicarboxylic acid, 4,4'-diphenoxyethanedicarboxylic acid, 4,4'-diphenylsulfonedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, hexahydrophthalic acid, hexahydroisophthalic acid, and hexahydroterephthalic acid. Among these, from the viewpoint of obtaining appropriate flexibility and crystallinity, terephthalic acid, 2,5-furandicarboxylic acid, and isophthalic acid are preferred, and terephthalic acid is particularly preferred. These aromatic dicarboxylic acids may or may not be derivatives of these. For example, derivatives of the aromatic dicarboxylic acids exemplified above are preferred, and among them, lower alkyl esters having 1 to 4 carbon atoms, acid anhydrides, and the like are mentioned. Specific examples of derivatives of aromatic dicarboxylic acid compounds include lower alkyl esters such as methyl esters, ethyl esters, propyl esters, and butyl esters of the above-listed aromatic dicarboxylic acids; and cyclic acid anhydrides of the above-listed aromatic dicarboxylic acids such as succinic anhydride.
[0029] The above aliphatic dicarboxylic acids and aromatic dicarboxylic acids may each be used alone or in combination of two or more kinds.
[0030] Furthermore, succinic acid, sebacic acid, etc., derived from plant materials can be used.
[0031] Total content of dicarboxylic acid units in aliphatic-aromatic polyesters The total content of dicarboxylic acid units in aliphatic-aromatic polyesters is not particularly limited, but from the viewpoint of flowability and melt tension, it is usually 10 mol% or more, preferably 30 mol% or more, more preferably 40 mol% or more, and even more preferably 45 mol% or more, relative to 100 mol% of all structural units constituting the polyester. It is also usually 90 mol% or less, preferably 70 mol% or less, more preferably 60 mol% or less, and even more preferably 55 mol% or less. That is, the content of dicarboxylic acid units in the polyester is preferably 10 mol% or more and 90 mol% or less, particularly preferably 30 mol% or more and 70 mol% or less, particularly preferably 40 mol% or more and 60 mol% or less, and especially preferably 45 mol% or more and 55 mol% or less, relative to 100 mol% of all structural units constituting the polyester.
[0032] In addition, the total content of aromatic dicarboxylic acid units in the polyester is not particularly limited, but the total proportion of aromatic dicarboxylic acid units in the constituent units (100 mol%) derived from all dicarboxylic acids contained in the polyester is, from the viewpoint of biodegradability and moldability, usually 10 mol% or more, preferably 15 mol% or more, more preferably 20 mol% or more, and even more preferably 35 mol% or more, and is usually 90 mol% or less, preferably 70 mol% or less, more preferably 60 mol% or less, and even more preferably 55 mol% or less. That is, the proportion of aromatic dicarboxylic acid units in the constituent units (100 mol%) derived from all dicarboxylic acids contained in the polyester is preferably 10 mol% or more and 90 mol% or less, particularly preferably 15 mol% or more and 70 mol% or less, more preferably 20 mol% or more and 60 mol% or less, and particularly preferably 35 mol% or more and 55 mol% or less. This range is particularly preferred as the proportion of terephthalic acid units in the constituent units (100 mol%) derived from all dicarboxylic acids contained in the polyester. When the ratio is equal to or greater than the lower limit of the above range, the glass transition temperature of the polyester can be more reliably prevented from becoming too low, and a sufficient coloration suppression effect can be achieved. Furthermore, when the ratio is equal to or less than the upper limit of the above range, the biodegradation rate of the polyester can be more reliably prevented from becoming too slow. The calculation of the total content of dicarboxylic acid units and the total content of aromatic dicarboxylic acid units in the aliphatic-aromatic polyester is based on the smallest ester unit in the aliphatic-aromatic polyester, as with the total content of diol units in the aliphatic-aromatic polyester. Furthermore, the "total content of carboxylic acid units" refers to the ratio of the moles of one dicarboxylic acid unit to the moles of all ester units when the aliphatic-aromatic polyester contains one type of dicarboxylic acid unit; when the aliphatic-aromatic polyester contains two or more types of dicarboxylic acid units, it refers to the ratio of the total moles of the two or more dicarboxylic acid units to the moles of all ester units. The same applies to the total content of aromatic dicarboxylic acid units.
[0033] The total content of aliphatic-aromatic polyesters in the composition is 20% by mass or more, preferably 24% by mass or more, more preferably 30% by mass or more, and even more preferably 50% by mass or more. Furthermore, this total content is 99% by mass or less, and may be 97% by mass or less, 95% by mass or less, or even 90% by mass or less. That is, the content is 20% by mass or more and 99% by mass or less, preferably 24% by mass or more and 97% by mass or less, more preferably 30% by mass or more and 95% by mass or less, and particularly preferably 50% by mass or more and 90% by mass or less. Note that, when the composition contains one type of aliphatic-aromatic polyester, the "total content of aliphatic-aromatic polyesters" refers to the ratio (mass ratio) of that one type of aliphatic-aromatic polyester to the composition. When the composition contains two or more types of aliphatic-aromatic polyesters, the "total content of aliphatic-aromatic polyesters" refers to the ratio (mass ratio) of the total amount of those two or more aliphatic-aromatic polyesters to the composition. When the content is equal to or greater than the lower limit of the above range, a composition having excellent flexibility, good moldability, and excellent discoloration resistance can be obtained.
[0034] The content of ester groups contained in the aliphatic-aromatic polyester is 9.6 mol / kg or more, preferably 9.7 mol / kg or more, particularly preferably 9.8 mol / kg or more, and more preferably 9.9 mol / kg or more, from the viewpoint of forming hydrogen bonds between adjacent polymer chains and thereby suppressing penetration of dye molecules. There is no particular upper limit to the content, but from the viewpoint of further improving the moldability of the biodegradable resin composition according to this embodiment containing the aliphatic-aromatic polyester and more reliably preventing thermal degradation during molding, the content is preferably 13.6 mol / kg or less, more preferably 12.6 mol / kg or less, and even more preferably 11.6 mol / kg or less. That is, the content of ester groups contained in the aliphatic-aromatic polyester is preferably 9.6 mol / kg or more and 13.6 mol / kg or less, particularly preferably 9.7 mol / kg or more and 12.6 mol / kg or less, further preferably 9.8 mol / kg or more and 11.6 mol / kg or less, and particularly preferably 9.9 mol / kg or more and 11.6 mol / kg or less. Furthermore, the content can be adjusted by the type and polymerization ratio of diol and dicarboxylic acid, which are the constituent units of the aliphatic-aromatic polyester. The content of the ester groups can be adjusted by dissolving the polyester in deuterated chloroform and then 1 Measurement is carried out using H-NMR (for example, NMR "AVANCE 400" manufactured by Bruker), and the polymerization ratio of each constituent unit, such as the smallest dicarboxylic acid unit and the smallest diol unit, constituting the aliphatic-aromatic polyester can be evaluated from the chemical shift and integral ratio.
[0035] (Other Copolymerization Components) In the production of the aliphatic-aromatic polyester, constituent components (other copolymerization components) other than the above diols and dicarboxylic acids may be copolymerized. Examples of copolymerization components that can be used in this case include hydroxycarboxylic acids such as lactic acid, glycolic acid, hydroxybutyric acid, hydroxycaproic acid, 2-hydroxy-3,3-dimethylbutyric acid, 2-hydroxy-3-methylbutyric acid, 2-hydroxyisocaproic acid, malic acid, and citric acid; esters, lactones, and hydroxycarboxylic acid polymers of these hydroxycarboxylic acids; trifunctional or higher polyhydric alcohols such as glycerin, trimethylolpropane, and pentaerythritol; and trifunctional or higher polycarboxylic acids such as propanetricarboxylic acid, pyromellitic acid, and trimellitic acid benzophenonetetracarboxylic acid, or anhydrides of the trifunctional or higher polycarboxylic acids.
[0036] Furthermore, adding a small amount of a trifunctional or higher functional hydroxycarboxylic acid, a trifunctional or higher functional alcohol, or a trifunctional or higher functional carboxylic acid makes it easier to obtain a polyester with high viscosity. Specifically, as the trifunctional or higher functional hydroxycarboxylic acid, malic acid or citric acid is preferred, with malic acid being particularly preferred. As a component constituting the trifunctional or higher functional polyhydric alcohol unit, glycerin, trimethylolpropane, pentaerythritol, or the like is preferred. These may be used alone or in combination of two or more.
[0037] The content of the tri- or higher functional compound is preferably 0.001 to 5 mol %, and more preferably 0.05 to 0.5 mol %, relative to 100 mol % of all dicarboxylic acid components in the polyester raw material. Below the upper limit of this range, the formation of gel (unmelted material) in the resulting polyester can be more reliably prevented, while above the lower limit, the advantage of using the multifunctional compound (usually, the viscosity of the resulting polyester can be increased) can be more reliably obtained.
[0038] The aliphatic-aromatic polyester may contain each of the above structural units, and specific examples include polybutylene succinate terephthalate (PBST), polybutylene adipate terephthalate (PBAT), polyethylene succinate terephthalate (PEST), polybutylene sebacate terephthalate (PBSeT), etc. Among these, from the viewpoint of obtaining a resin composition with excellent discoloration resistance, polybutylene succinate terephthalate or polyethylene succinate terephthalate is preferred, and polybutylene succinate terephthalate composed of units of 1,4-butanediol, succinic acid, and terephthalic acid is particularly preferred.
[0039] [Characteristics of Aliphatic-Aromatic Polyesters] (Bio-Based Carbon Content) The bio-based carbon content of the aliphatic-aromatic polyester measured according to ISO 16620-2 is not particularly limited. However, from the viewpoint of suppressing carbon dioxide emissions and obtaining even better discoloration resistance, it is preferably 20% or more, more preferably 35% or more, and even more preferably 50% or more. Furthermore, there is no particular need to set an upper limit, and it may be 100%, 80% or less, 70% or less, or 60% or less. That is, the bio-based carbon content is preferably 20% or more and 100% or less, particularly preferably 35% or more and 80% or less, more preferably 50% or more and 70% or less, and particularly preferably 50% or more and 60% or less. Increasing the bio-based carbon content reduces fossil fuel consumption and carbon dioxide emissions, which is beneficial from the perspective of protecting the global environment. In addition, even better discoloration resistance can be obtained. While the mechanism behind this is not fully understood, it is presumed that the increased crystallization rate during molding results in the formation of numerous fine crystals, thereby further inhibiting the penetration of the dye. In the composition according to this embodiment, the bio-based carbon content of the aliphatic-aromatic polyester having an ester group content of 9.6 mol / kg or more, preferably 9.7 mol / kg or more, may satisfy the above range, but it is preferable that the components contained in the composition as a whole satisfy the above range of bio-based carbon content. The bio-based carbon content of the composition will be described later. The bio-based carbon content can be controlled by adjusting the ratio of monomer units produced from plant-derived raw materials to all structural units constituting one or more polyesters. The bio-based carbon content may be satisfied by one polyester contained in the composition, or by the entire one or more polyesters, and is preferably satisfied by at least one polyester. The bio-based carbon content is calculated in accordance with ISO 16620-2 based on the ratio of carbon-14 ( 14C). It can also be determined by calculation from the bio-based carbon content and polymerization ratio of each of the raw materials, the aliphatic diol component, the aliphatic dicarboxylic acid component, and the aromatic dicarboxylic acid component. In this specification, the "biodegradable resin (polyester)" does not necessarily mean that the entirety of one type of resin (polyester) is biodegradable; only a portion of one type of resin (polyester) is biodegradable, and it is preferable that the bio-based content satisfies the above-mentioned range, for example.
[0040] (Melting point, glass transition temperature) The melting point (Tm) of the aliphatic-aromatic polyester is not particularly limited, but is usually 50 ° C or higher, preferably 70 ° C or higher, more preferably 80 ° C or higher, and even more preferably 85 ° C or higher. Also, it is usually 200 ° C or lower, preferably 180 ° C or lower, more preferably 170 ° C or lower, and even more preferably 160 ° C or lower. That is, the melting point (Tm) is preferably 50 ° C or higher and 200 ° C or lower, particularly preferably 70 ° C or higher and 180 ° C or lower, more preferably 80 ° C or higher and 170 ° C or lower, and particularly preferably 85 ° C or higher and 160 ° C or lower. If the melting point is higher than the lower limit of the range, it will be better in terms of heat resistance. Furthermore, if the melting point is lower than the upper limit of the range, it will be easier to mold. The glass transition temperature (Tg) of the aliphatic-aromatic polyester is not particularly limited, but is preferably −27°C or higher, more preferably −25°C or higher, even more preferably −22°C or higher, and preferably 0°C or lower, more preferably −5°C or lower, and even more preferably −10°C or lower. That is, the glass transition temperature (Tg) is preferably −27°C or higher and 0°C or lower, particularly preferably −25°C or higher and −5°C or lower, and even more preferably −22°C or higher and −10°C or lower. When the glass transition temperature is above the lower limit of the above range, the free volume of the amorphous portion at the actual use temperature does not become too large, so the coloration suppression effect of the ester group can be more reliably obtained. Furthermore, when the glass transition temperature is below the upper limit of the above range, the resin becomes flexible and tenacious, so problems such as cracking, peeling from the substrate, and deterioration in texture can be more reliably prevented. The melting point and glass transition temperature can be measured using a differential scanning calorimeter. Specifically, about 5 mg of a sample is precisely weighed, heated and melted under a nitrogen gas flow at a flow rate of 40 mL / min, cooled to −50° C. or below, and then heated at a rate of 10° C. / min, during which the glass transition temperature and melting point can be measured. The above melting point and glass transition temperature may be satisfied by one type of polyester, or by all of one or more types of polyesters, and it is preferable that at least one type of polyester satisfies these requirements.
[0041] [Method for producing polyester] The method for producing polyester is not particularly limited, and known methods such as the method disclosed in Patent Document 1 can be used. The method for producing polyester will be described below, but it is merely an example, and the method for producing polyester is not limited to this embodiment. The polycondensation reaction in this case can be performed under appropriate conditions that have been conventionally used, and is not particularly limited. Usually, a method is used in which the degree of polymerization is further increased by carrying out a pressure reduction operation after the esterification and / or transesterification reaction has progressed.
[0042] In the production of an aliphatic-aromatic polyester resin, the amounts of the diol component, the dicarboxylic acid component, and any other copolymerization components used are determined so that the aliphatic-aromatic polyester resin produced has a desired composition. Usually, the diol component and the dicarboxylic acid component are reacted in substantially equimolar amounts, but the diol component is usually used in an excess of 1 to 20 mol % over the dicarboxylic acid component because it is distilled off during the esterification or transesterification reaction.
[0043] The reaction temperature is not particularly limited as long as it is a temperature at which the esterification reaction can be carried out, but is preferably 200° C. or higher, and more preferably 210° C. or higher, in terms of being able to increase the reaction rate, and is preferably 270° C. or lower, more preferably 260° C. or lower, and particularly preferably 250° C. or lower, in order to prevent discoloration of the polyester. That is, the reaction temperature is preferably 200° C. or higher and 270° C. or lower, particularly preferably 210° C. or higher and 260° C. or lower, and even more preferably 210° C. or higher and 250° C. or lower.
[0044] The reaction time is not particularly limited, but is preferably 1 hour or more, and is preferably 10 hours or less, and more preferably 4 hours or less. That is, the reaction time is preferably 1 hour or more and 10 hours or less, and particularly preferably 1 hour or more and 4 hours or less.
[0045] The reaction vessel is then evacuated to increase the degree of polymerization.
[0046] The reaction pressure is not particularly limited, but is usually 0.01 kPa or more, preferably 0.03 kPa or more, and usually 1.4 kPa or less, preferably 0.4 kPa or less. That is, the reaction pressure is preferably 0.01 kPa or more and 1.4 kPa or less, and particularly preferably 0.03 kPa or more and 0.4 kPa or less. When the pressure during the polycondensation reaction is within the above range, for example, it is possible to prevent a decrease in molecular weight and coloration of the polyester due to thermal decomposition that accompanies a long polycondensation time, and it is possible to more easily produce a polyester that exhibits sufficient properties for practical use.
[0047] The reaction temperature is not particularly limited, but is usually 215°C or higher, preferably 220°C or higher, and usually 270°C or lower, preferably 260°C or lower. That is, the reaction temperature is preferably 215°C or higher and 270°C or lower, and particularly preferably 220°C or higher and 260°C or lower. When the reaction temperature is above the lower limit of the above range, the polycondensation reaction rate is increased, preventing the long time required for the production of a polyester with a high polymerization degree and eliminating the need for a high-power stirrer, which is economically advantageous. On the other hand, when the reaction temperature is below the upper limit of the above range, thermal decomposition of the polyester resin during production is unlikely to occur, and a polyester with a high polymerization degree can be more easily produced.
[0048] The reaction time is not particularly limited, but is usually 1 hour or more and usually 15 hours or less, preferably 10 hours or less, and more preferably 8 hours or less. That is, the reaction time is preferably 1 hour or more and 15 hours or less, particularly preferably 1 hour or more and 10 hours or less, and even more preferably 1 hour or more and 8 hours or less. A reaction time of 1 hour or more allows for sufficient reaction, making it easier to obtain a polyester with a high degree of polymerization, and also improving the mechanical properties of the molded article. On the other hand, a reaction time of 15 hours or less can more reliably prevent a decrease in molecular weight due to thermal decomposition of the polyester-based resin, thereby improving the mechanical properties of the molded article. Furthermore, an increase in the amount of carboxyl group terminals due to thermal decomposition, which adversely affects the durability of the polyester-based resin, can be more reliably prevented.
[0049] By controlling the temperature, time and reaction pressure of the polycondensation reaction within the above ranges, a polyester resin having a desired intrinsic viscosity can be obtained.
[0050] (Reaction Catalyst) The aliphatic-aromatic polyester resin is usually produced in the presence of a catalyst. The catalyst can be arbitrarily selected from catalysts that can be used in the production of known polyester resins, as long as it does not significantly impair the effects of the present invention.
[0051] The catalyst generally used is a compound containing at least one metal element selected from Groups 1 to 14 of the periodic table. To reduce the polyester terminal concentration, which affects the thermal stability of the polyester, a metal element selected from Groups 3 to 6 of the periodic table that exhibits Lewis acidity is more preferred. Specific examples of the metal element include scandium, titanium, zirconium, vanadium, molybdenum, and tungsten. Titanium and zirconium are particularly preferred due to their availability, and titanium is even more preferred due to its reaction activity.
[0052] In the present embodiment, as the catalyst, a compound containing an organic group, such as a carboxylate, an alkoxy salt, an organic sulfonate, or a β-diketonate salt, containing the above-mentioned metal element; or an inorganic compound, such as an oxide or halide of the above-mentioned metal element, or a mixture thereof, is preferably used.
[0053] In this embodiment, the catalyst is preferably a liquid during polymerization or a compound that dissolves in the ester oligomer or polyester, because the polymerization rate increases when the catalyst is in a molten or dissolved state during polymerization. Furthermore, while polycondensation is preferably performed without a solvent, a small amount of solvent may be used separately to dissolve the catalyst. Examples of solvents for dissolving the catalyst include alcohols such as methanol, ethanol, isopropanol, or butanol; the aforementioned diols such as ethylene glycol, butanediol, or pentanediol; ethers such as diethyl ether or tetrahydrofuran; nitriles such as acetonitrile; hydrocarbon compounds such as heptane or toluene; water; or mixtures thereof. To dissolve the catalyst, the catalyst can be diluted with a diol such as 1,4-butanediol or ethylene glycol. In this case, the diol can also function as a raw material for the polyester.
[0054] The titanium compound is preferably a tetraalkyl titanate or a hydrolyzate thereof, and specific examples thereof include tetra-n-propyl titanate, tetraisopropyl titanate, tetra-n-butyl titanate, tetra-t-butyl titanate, tetraphenyl titanate, tetracyclohexyl titanate, tetrabenzyl titanate, mixed titanates thereof, and hydrolyzates thereof.
[0055] Furthermore, as the titanium compound, a liquid obtained by mixing an alcohol, a Group 2 metal compound in the long periodic table (Nomenclature of Inorganic Chemistry IUPAC Recommendations 2005) (hereinafter, sometimes referred to as a Group 2 metal compound in the long periodic table), a phosphate ester compound, or a titanium compound may also be used.
[0056] The amount of catalyst added is not particularly limited, but the lower limit of the amount of metal relative to the polyester produced is usually 0.1 mass ppm or more, preferably 0.5 mass ppm or more, more preferably 1 mass ppm or more, and the upper limit is usually 3000 mass ppm or less, preferably 1000 mass ppm or less, more preferably 250 mass ppm or less, and particularly preferably 130 mass ppm or less. That is, the catalyst addition amount is preferably 0.1 mass ppm or more and 3000 mass ppm or less, particularly preferably 0.5 mass ppm or more and 1000 mass ppm or less, more preferably 1 mass ppm or more and 250 mass ppm or less, more preferably 1 mass ppm or more and 130 mass ppm or less. This range is particularly preferably applicable when a metal compound is used as a polycondensation catalyst. Using an amount of catalyst below the upper limit of the above range is not only economically advantageous, but also more reliably prevents a decrease in the thermal stability and hydrolysis resistance of the polyester due to an increase in the number of carboxyl group terminals and the residual catalyst concentration. Furthermore, by ensuring that the polymerization activity is at least as high as the lower limit of the above range, thermal decomposition during polyester production due to reduced polymerization activity can be more reliably prevented, and polyesters exhibiting practically useful physical properties can be more easily obtained.
[0057] [Other Components] The composition may contain components other than the polyesters described above, such as polyesters other than the aliphatic-aromatic polyesters described above, resins other than polyesters, carbodiimide compounds, isocyanate compounds, fillers, or plasticizers. In particular, when a resin other than polyester is contained, it is preferable to use a biodegradable resin as the resin. For example, polycaprolactone, polyamide, polyvinyl alcohol, cellulose ester, or the like, or fine powders of animal or plant substances such as starch, cellulose, paper, wood flour, chitin / chitosan, coconut shell powder, or walnut shell powder, or mixtures thereof may be blended. Furthermore, in order to adjust the physical properties and processability of the molded article, additives such as heat stabilizers, plasticizers, lubricants, antiblocking agents, nucleating agents, inorganic fillers, colorants, pigments, UV absorbers, or light stabilizers, modifiers, crosslinking agents, or the like may be added.
[0058] <Nucleating Agent> Examples of the nucleating agent that can be used include silicate compounds such as talc, mica, clay, and zeolite; metal salts of phenylphosphonate such as zinc phenylphosphonate, calcium phenylphosphonate, and magnesium phenylphosphonate; metal soaps, which are salts of fatty acids such as lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, oleic acid, and erucic acid with metal ions such as zinc, calcium, magnesium, and aluminum; fatty acid amides such as stearamide, 12-hydroxystearamide, erucamide, and ethylenebisstearamide; cellulose powder; and polyethylene wax. Among these, talc or polyethylene wax is preferred from the viewpoints of moldability improvement effect and cost, and talc is most preferred from the viewpoint of minimal adverse effects when released into the environment. From the viewpoints of transparency and smoothness, the particle size of the talc is preferably 2.50 μm or less in median diameter, more preferably 1.50 μm or less, even more preferably 1.00 μm or less, and most preferably 0.7 μm or less. On the other hand, from the viewpoint of preventing dust scattering and adhesion to equipment and facilitating production, the median diameter is preferably 0.05 μm or more, more preferably 0.10 μm or more, even more preferably 0.2 μm or more, and most preferably 0.3 μm or more. That is, the median particle diameter of talc is preferably 0.05 μm or more and 2.50 μm or less, particularly preferably 0.10 μm or more and 1.50 μm or less, more preferably 0.20 μm or more and 1.00 μm or less, and particularly preferably 0.30 μm or more and 0.70 μm or less. The nucleating agent may be added during the esterification reaction or at any stage after the esterification reaction. Addition during the esterification reaction is more preferred because it facilitates pelletization after the reaction is completed. When talc is added as a nucleating agent during the esterification reaction, the amount added is preferably 0.001 part by mass or more, more preferably 0.01 part by mass or more, even more preferably 0.05 part by mass or more, and most preferably 0.15 part by mass or more, relative to 100 parts by mass of the resulting aliphatic-aromatic polyester resin, and is preferably 0.5 part by mass or less, more preferably 0.4 part by mass or less, even more preferably 0.3 part by mass or less, and most preferably 0.25 part by mass or less.That is, when talc is added as a nucleating agent during the esterification reaction, the amount added is preferably 0.001 to 0.5 parts by mass, more preferably 0.01 to 0.4 parts by mass, even more preferably 0.05 to 0.3 parts by mass, and most preferably 0.15 to 0.25 parts by mass, relative to 100 parts by mass of the resulting aliphatic-aromatic polyester resin. By adding an amount within the above range, a more sufficient moldability improvement effect can be obtained, the transparency and smoothness of the molded article are less likely to be impaired, and a decrease in reaction rate and an increase in loss due to an increase in the viscosity of the composition can be more reliably prevented.
[0059] The composition may further contain a polyester other than the aliphatic-aromatic polyester from the viewpoint of obtaining appropriate hardness and opening properties during molding. The polyester other than the aliphatic-aromatic polyester preferably contains an aliphatic polyester from the viewpoint of obtaining good biodegradability. In this specification, the aliphatic polyester is not an aliphatic-aromatic polyester, but a polyester containing aliphatic diol and aliphatic dicarboxylic acid units as main structural units, or a polyester containing aliphatic oxycarboxylic acid units as main structural units.
[0060] Examples of aliphatic polyesters include polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), polybutylene succinate sebacate (PBSSe), polycaprolactone (PCL), poly(3-hydroxybutyrate) (PHB), poly(3-hydroxybutyrate / 3-hydroxyvalerate) (PHBV), poly(3-hydroxybutyrate / 3-hydroxyhexanoate) (PHBH), and polylactic acid (PLA). From the viewpoints of heat resistance, moldability, biodegradability, and the like, polybutylene succinate, polybutylene succinate adipate, polybutylene succinate sebacate, poly(3-hydroxybutyrate / 3-hydroxyhexanoate), and polylactic acid are preferred, and polybutylene succinate or polybutylene succinate sebacate is particularly preferred.
[0061] The content of polyesters other than aliphatic-aromatic polyesters in the composition is not particularly limited, but is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, and preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less. That is, the content is preferably 5% by mass or more and 80% by mass or less, particularly preferably 10% by mass or more and 70% by mass or less, and more preferably 15% by mass or more and 60% by mass or less. When the content is equal to or greater than the lower limit of the above range, it is possible to more easily adjust the hardness and surface slipperiness of molded articles, etc. Furthermore, when the content is equal to or less than the upper limit of the above range, it is possible to more easily obtain a composition having excellent flexibility, breaking strength, and moldability.
[0062] The biodegradable resin composition according to one embodiment of the present invention further contains a filler from the viewpoints of mold releasability, opening property, shortening of molding time, etc., particularly from the viewpoint of obtaining a molded product with good opening property. Examples of fillers include talc, clay, mica, calcium carbonate, barium sulfate, titanium oxide, basic magnesium sulfate, zeolite, aluminosilicate, etc., and from the viewpoint of obtaining the effect of shortening molding time with a small amount, talc, calcium carbonate, or aluminosilicate is preferred, with talc being particularly preferred.
[0063] The content of the filler in the composition is preferably 0.3% by mass or more, more preferably 1.0% by mass or more, and also 50.0% by mass or less, more preferably 30.0% by mass or less, and more preferably 15.0% by mass or less. That is, the content is 0.3% by mass or more and 50.0% by mass or less, preferably 1.0% by mass or more and 30.0% by mass or less, and more preferably 1.0% by mass or more and 15.0% by mass or less. If the content is above the lower limit of the above range, effects such as excellent opening properties of molded products, good demoldability, and shortened molding time can be more easily obtained. Furthermore, if the content is below the upper limit of the above range, excellent breaking strength and excellent moldability can be more easily obtained.
[0064] <Characteristics of Biodegradable Resin Composition> (Bio-based Carbon Content) The total bio-based carbon content of the biodegradable resin composition as measured according to ISO 16620-2 is not particularly limited, but is preferably 20% or more, more preferably 35% or more, and even more preferably 50% or more. Furthermore, there is no particular upper limit, and it may be 100%, 90% or less, 80% or less, or 70% or less. That is, the bio-based carbon content is preferably 20% or more and 100% or less, particularly preferably 35% or more and 90% or less, more preferably 50% or more and 80% or less, and particularly preferably 50% or more and 70% or less. Increasing the bio-based carbon content reduces fossil fuel consumption and carbon dioxide emissions, which is beneficial from the perspective of protecting the global environment. Note that the bio-based carbon content does not have to be satisfied by the aliphatic-aromatic polyester described above; it is sufficient that it is satisfied by the entire composition. For example, the composition may contain an aliphatic-aromatic polyester with a bio-based carbon content of 0% and an aliphatic polyester with a bio-based carbon content of 49%, and the content of each component may be appropriately adjusted to fall within the above range. The bio-based carbon content can be controlled by adjusting the proportion of monomer units produced from plant-derived raw materials relative to the total structural units constituting one or more polyesters contained in the composition. The bio-based carbon content is calculated in accordance with ISO 16620-2 as the ratio of carbon-14 ( 14 C). Furthermore, for example, when determining the biobased carbon content of a polyester contained in a composition, it can also be determined by calculation from the biobased carbon contents and polymerization ratios of the aliphatic diol component, the aliphatic dicarboxylic acid component, and the aromatic dicarboxylic acid component, which are raw materials. In this specification, a "biodegradable resin composition" typically refers to a resin composition having the above-mentioned biobased carbon content of at least 20%.
[0065] <Method for producing biodegradable resin composition> The method for producing the biodegradable resin composition is not particularly limited, and known methods can be applied. For example, a production method having a mixing step of mixing the above-mentioned polyester with other optional components can be adopted. However, this production method may have steps other than the mixing step. Furthermore, the production of the biodegradable resin composition is not limited to this method.
[0066] In the mixing step, the method for mixing the polyester and other optional components is not particularly limited, and known methods can be employed. Furthermore, optional components can be mixed together as needed. Examples include a method in which the polyester and other optional components are melt-mixed all at once in an extruder, or a method in which they are each fed into a kneader from separate feeders and melt-mixed. It is also possible to adjust the concentration of each component by first preparing a masterbatch containing the polyester and other optional components, then diluting it with the polyester and kneading it again. Single-screw or twin-screw extruders can be used as extruders. The resin kneaded in the twin-screw extruder can be pelletized using a pelletizer or underwater cutter. If a molded product is subsequently produced, the pellets can be used in various subsequent molding processes. Alternatively, the polyester, other optional components, and other raw material pellets can be directly fed into a molding machine to prepare the composition and simultaneously produce a molded product such as a film.
[0067] <Polybutylene succinate terephthalate (PBST)> Another embodiment of the present invention relates to polybutylene succinate terephthalate (hereinafter also referred to simply as "polybutylene succinate terephthalate"), which has an ester group content of 9.6 mol / kg or more, preferably 9.7 mol / kg or more, and a bio-based carbon content of 20% or more as measured in accordance with ISO 16620-2. Because the polybutylene succinate terephthalate has an ester group content above a specific range, it can achieve the effect of being less susceptible to discoloration by pigments contained in food and beverages, similar to the above-described composition.
[0068] Polybutylene succinate terephthalate is a polyester having 1,4-butanediol as a diol unit, succinic acid as an aliphatic dicarboxylic acid unit, and terephthalic acid as an aromatic dicarboxylic acid unit, although these diols and dicarboxylic acids may or may not be derivatives thereof.
[0069] The content of 1,4-butanediol in polybutylene succinate terephthalate is not particularly limited, and the total content of diol units in the aliphatic-aromatic polyester described in the above section on composition can be similarly applied. The content of terephthalic acid units in polybutylene succinate terephthalate is not particularly limited, and the proportion of aromatic dicarboxylic acid units in the dicarboxylic acid units described in the above section on composition can be similarly applied.
[0070] The content of ester groups contained in polybutylene succinate terephthalate is not particularly limited as long as it is 9.6 mol / kg or more, and as a preferred condition, the content of ester groups contained in the aliphatic-aromatic polyester described in the section on the composition above can be similarly applied.
[0071] The bio-based carbon content of polybutylene succinate terephthalate measured according to ISO 16620-2 is not particularly limited as long as it is 20% or more, and as a preferred condition, the bio-based carbon content of the aliphatic-aromatic polyester described in the section on the composition above can be similarly applied.
[0072] <Molded Article> A molded article according to another embodiment of the present invention is a molded article made from the biodegradable resin composition described above, or a molded article made from the polybutylene succinate terephthalate described above. Hereinafter, these molded articles will be collectively referred to as "molded article." The method for producing the molded article is not particularly limited, and the molded article can be obtained by molding using a known polyester molding method. The molding method is not particularly limited, and known methods such as compression molding, laminate molding, injection molding, extrusion molding, vacuum molding, pressure molding, blow molding, inflation molding, or stretch molding can be used. More specifically, for example, a method in which a film-like material, sheet-like material, or cylindrical material extruded to a predetermined thickness from a T-die, I-die, or round die is cooled and solidified using a cooling roll, water, compressed air, or the like can be mentioned.
[0073] <Laminate> A laminate according to another embodiment of the present invention is a laminate having a layer made of the biodegradable resin composition described above, or a laminate having a layer made of the polybutylene succinate terephthalate described above. Hereinafter, these laminates will be collectively referred to as "laminates." The method for producing the laminate is not particularly limited, and the laminate can be molded into a molded product using a known laminate molding method. The molding method is not particularly limited, and examples that can be used include a method in which the biodegradable resin composition described above and other materials are simultaneously laminated by multilayer extrusion molding such as multilayer T-die molding, multilayer blow molding, multilayer inflation molding, or multilayer pipe molding; a method in which the biodegradable resin composition described above is heated and melted onto another substrate (paper, sheet, film, etc.) and extruded or injection molded; a method in which the biodegradable resin composition described above, which has been molded into a film or sheet, is bonded to another substrate; a method in which another material is vapor-deposited or coated onto the biodegradable resin composition described above, which has been molded into a film or sheet; and a method in which the biodegradable resin composition described above is dissolved in a solvent and coated onto another substrate. Two or more of these methods may be combined, for example, a method of adhering another substrate to a sheet-like laminate obtained by multilayer extrusion molding can be used. Furthermore, the sheet-like laminate can be molded into a desired shape by secondary processing such as vacuum forming, pressure forming, press forming, punching, crimping, or fusion bonding.
[0074] The substrate is not particularly limited as long as it can be used as a food and beverage packaging material, and examples thereof include paper, a resin sheet, a sheet made of an inorganic material, cloth, a nonwoven fabric, wood, etc. Among these, in terms of biodegradability, paper, a biodegradable resin sheet, a biodegradable nonwoven fabric, a biodegradable cloth such as cotton, silk, or rayon, wood, etc. are particularly preferred.
[0075] The number of layers constituting the laminate is not particularly limited as long as it is two or more layers and at least one of the layers is a layer made of the biodegradable resin composition described above, and can be appropriately designed depending on the application, and specifically, it may be two or more layers, three or more layers, four or more layers, or ten or fewer layers, five or fewer layers, three or fewer layers, or two layers. That is, the number of layers in the laminate is preferably two to ten layers, particularly preferably two to seven layers, even more preferably two to five layers, and even more preferably two to three layers.
[0076] <Uses> The uses of the molded article, laminate, and polybutylene succinate terephthalate made from the biodegradable resin composition described above are not limited, but are preferably food and beverage packaging materials from the viewpoint of being less susceptible to discoloration by pigments contained in food and beverages. Specific food and beverage packaging materials include food and beverage containers, food and beverage wrap, food and beverage shrink film, bags, wrapping paper, etc., with food and beverage containers being preferred. Specific embodiments of the food and beverage containers are not particularly limited, and examples include cups (particularly paper cups), beverage packs, plates, trays, etc.
[0077] Specific embodiments of the present invention will be described in more detail below using examples, but the present invention is not limited to the following examples as long as the gist of the invention is not exceeded. Note that the values of various production conditions and evaluation results in the following examples represent preferred upper or lower limit values in the embodiments of the present invention, and preferred ranges may be defined by a combination of the above-mentioned upper or lower limit values and the values in the following examples or values between the examples.
[0078] <Analysis, Measurement, and Evaluation Methods> The analysis methods, measurement methods of various physical properties, and evaluation methods in the present examples are as follows.
[0079] [Content of ester groups and proportion of terephthalic acid units in polyester] After dissolving the polyester in deuterated chloroform, the polyester was analyzed using a Bruker NMR "AVANCE 400". 1 H-NMR was measured, and the polymerization ratio of each structural unit, such as dicarboxylic acid units and diol units, constituting the polyester was evaluated from the chemical shift and integral ratio. From this evaluation, the content of ester groups and the ratio of structural units derived from terephthalic acid to all dicarboxylic acid units were determined.
[0080] [Glass Transition Temperature and Melting Point of Polyester] The glass transition temperature (Tg) of the polyester was measured using a differential scanning calorimeter (manufactured by Seiko Corporation, product name: DSC220). Specifically, about 5 mg of a sample was taken, heated and melted in a nitrogen gas flow at a flow rate of 40 mL / min, cooled at a rate of 10°C / min, and then the glass transition temperature and melting point were measured while the temperature was increased at a rate of 10°C / min.
[0081] [Crystallization Peak Temperature and Half Width of Polyester] In measuring the glass transition temperature and melting point, the DSC curve obtained by measuring while cooling at a rate of 10°C / min after heating and melting was plotted with temperature on the horizontal axis and heat flux heat generation on the vertical axis as positive. When the line connecting the start and end points of the exothermic peak was subtracted from the curve as the baseline, the temperature at which the exothermic heat generation was maximum was determined as the crystallization peak temperature. The full width at half maximum of the exothermic peak, i.e., the temperature difference between the two points where the height from the baseline is half of the maximum value, was determined as the half width of the crystallization peak. The smaller the half width of the crystallization peak, the faster the crystallization rate.
[0082] [Bio-based carbon content] The bio-based carbon content of each polyester resin was evaluated in accordance with ISO 16620-2. Specifically, the composition was burned, carbon dioxide was collected, and the carbon atoms in the composition were recovered as graphite by reducing it with hydrogen and a catalyst. Next, the carbon isotope ratio was measured using an accelerator mass spectrometer. Carbon isotope ratios are present in the atmosphere at a certain rate. 14Because carbon is present in biomass (bio-based carbon), the same proportion of carbon is present in biomass. 14 C is included. 14 Since C decreases with a half-life of 5730 years, carbon derived from fossil resources 14 Therefore, the standard amount of carbon in the modern atmosphere is 14 C ratio in the sample 14 The bio-based carbon content was determined by calculating the proportion of C.
[0083] [Staining Resistance] (1) Preparation of Beverage Standard Solution (Coffee) Nestle Japan Co., Ltd.'s "Regular Soluble Coffee Nescafé Gold Blend (Stick Black)" was dissolved in hot water at a specified concentration (2 g of coffee per 140 g of hot water), and the resulting solution was cooled overnight in a 4°C refrigerator. (Black Tea) 160 mL of hot water was added to a Unilever Japan Co., Ltd. "Lipton Yellow Label" tea bag and extracted for 2 minutes. The tea bag was removed and the resulting solution was cooled overnight in a 4°C refrigerator. (2) Immersion Test A rectangular test piece approximately 30 mm wide and 60 mm long was prepared from a molded resin composition. The test piece was suspended so that its lower half was immersed in the beverage standard solution and allowed to stand in a 4°C refrigerator for a predetermined period of time. The test piece was then removed, washed with tap water, wiped dry, and air-dried. (3) Color Difference Measurement The color of the test piece was measured by the transmission method using a "ZE7700" colorimeter manufactured by Nippon Denshoku Industries Co., Ltd. The color difference between the part immersed in the beverage standard solution and the part not immersed was measured as ΔE according to JIS Z8781-4. * ab (CIELAB 1976 L * a * b * The smaller this value, the smaller the degree of coloration and the better the color resistance.
[0084] [Biodegradability] The film-like test specimens were cut into rectangles measuring 50 mm x 30 mm and buried in a 1:1 mass ratio mixture of horticultural soil ("Cultivation soil for flowers and vegetables" manufactured by Iris Ohyama Co., Ltd.) and compost (inoculant source for biodegradation tests, manufactured by Yawata Bussan Co., Ltd.) with a moisture content of 20% RH contained in a sealed plastic container, and the container was then closed and placed in a thermostatic chamber at 40° C. Each test specimen was periodically removed and observed, and it was confirmed that all of the test specimens had disappeared 31 weeks after the start of the test.
[0085] [Opening Property] The opening property (ease of unfolding a folded and tightly adhered cylindrical film into its original cylindrical shape) of a resin composition film molded using an inflation molding machine was evaluated on a 5-point scale according to the following criteria. A higher score indicates easier processing into films, bags, etc. 5 points: Can be easily unfolded into a cylindrical shape with fingers with almost no resistance. 4 points: There was some resistance when peeling the adhered film, but it could be unfolded without any problems with fingers alone. 3 points: It was difficult to peel with fingers alone, but it could be opened using adhesive tape. 2 points: It was possible to peel using adhesive tape, but the resistance was so great that stretching and tearing occurred, making it impossible to obtain a good film. 1 point: The adhered film could not be peeled even with adhesive tape. The method using adhesive tape here refers to a method in which weak adhesive tape is applied to both sides of a folded film and attached with one end open, and then the two adhesive tapes are peeled apart from the open side to peel off the adhered film together with the adhesive tape.
[0086] <Materials> [Resin] (Aliphatic-aromatic polyester) (A1) Polybutylene succinate terephthalate (PBST) synthesized in Production Example 1 described later (bio-based carbon content: 22%, ester group content: 10.3 mol / kg)
[0087] (A2) Polybutylene succinate terephthalate (PBST) synthesized by Production Example 2 described later (bio-based carbon content: 63%, ester group content: 10.2 mol / kg)
[0088] (A3) Polybutylene adipate terephthalate (PBAT): "Ecoflex C1200" manufactured by BASF (bio-based carbon content: 0%, ester group content: 9.5 mol / kg)
[0089] (A4) Polybutylene succinate terephthalate (PBST) synthesized by Production Example 3 described later (bio-based carbon content: 20%, ester group content: 10.2 mol / kg)
[0090] (A5) Polybutylene succinate terephthalate (PBST) synthesized in Production Example 4 described later (bio-based carbon content: 18%, ester group content: 10.1 mol / kg)
[0091] (A6) Polybutylene succinate terephthalate (PBST) synthesized in Production Example 5 described later (bio-based carbon content: 15%, ester group content: 10.0 mol / kg)
[0092] (Aliphatic Polyester) (B1) Polybutylene succinate (PBS): "BioPBS FZ91PB" manufactured by PTT MCC Biochem (bio-based carbon content: 49%, ester group content: 11.6 mol / kg)
[0093] [Additives] (Inorganic filler) Talc: "Microace K-1" manufactured by Nippon Talc Co., Ltd. (This talc does not contain carbon atoms and therefore does not affect the evaluation of the bio-based carbon content of the resin composition.)
[0094] (Lubricant) Erucamide: "Diamid L-200" manufactured by Mitsubishi Chemical Corporation (bio-based carbon content: 0%)
[0095] <Production of Polyester> [Production Example 1] A reaction vessel equipped with a stirrer, a nitrogen inlet, a heater, a thermometer, and a pressure reduction port was charged with raw materials: 110 parts by mass of succinic acid (biomass-derived), 127 parts by mass of terephthalic acid (petroleum-derived), 168 parts by mass of 1,4-butanediol (petroleum-derived), and 0.46 parts by mass of trimethylolpropane. The molar ratio of succinic acid to terephthalic acid was 55:45, the molar ratio of 1,4-butanediol to the total molar amount of succinic acid and terephthalic acid was 1.1, and the amount of trimethylolpropane was 0.10 mol% relative to the total structural units of the polymer to be produced. While stirring the contents of the vessel, nitrogen gas was introduced into the vessel, and the system was substituted by vacuum to create a nitrogen atmosphere. Next, the temperature in the system was raised to 185°C while stirring, and the reaction was carried out at this temperature for 45 minutes to 1 hour. Next, the temperature was raised to 220°C over 1 hour and 30 minutes. Thereafter, the temperature was raised to 230°C over 1 hour, and at the same time, the pressure was reduced to 0.07 kPa or less over 1 hour and 30 minutes. Polymerization was continued while maintaining the heated and reduced pressure state, and polymerization was terminated when a predetermined viscosity was reached, yielding an aliphatic-aromatic polyester (A1).
[0096] [Production Example 2] An aliphatic-aromatic polyester (A2) was obtained in the same manner as in Production Example 1, except that the petroleum-derived 1,4-butanediol was changed to biomass-derived 1,4-butanediol.
[0097] [Production Example 3] An aliphatic-aromatic polyester (A4) was obtained in the same manner as in Production Example 1, except that the amount of succinic acid (biomass-derived) was changed to 100 parts by mass and the amount of terephthalic acid (petroleum-derived) was changed to 140 parts by mass. The molar ratio of succinic acid to terephthalic acid was 50:50.
[0098] [Production Example 4] An aliphatic-aromatic polyester (A5) was obtained in the same manner as in Production Example 1, except that the amounts of succinic acid (biomass-derived) and terephthalic acid (petroleum-derived) were changed to 90 parts by mass and 155 parts by mass, respectively, and the molar ratio of succinic acid to terephthalic acid was 45:55.
[0099] [Production Example 5] An aliphatic-aromatic polyester (A6) was obtained in the same manner as in Production Example 1, except that the amounts of succinic acid (biomass-derived) and terephthalic acid (petroleum-derived) were changed to 80 parts by mass and 169 parts by mass, respectively, and the molar ratio of succinic acid to terephthalic acid was 40:60.
[0100] <Production of Compositions> [Examples 1 to 3, Comparative Examples 1 to 4] Resins and additives were mixed in the proportions shown in Table 1, and the mixture was melt-kneaded and pelletized in a twin-screw extruder with a screw diameter of 30 mm at a set temperature of 150°C to obtain compositions. The bio-based carbon content of each composition was calculated from the bio-based carbon content and blending ratio of the raw materials, and is shown in Table 1. Specifically, for example, in Example 2, the carbon content of (A1) was 61%, the bio-based carbon content was 22%, the carbon content of (B1) was 56%, the bio-based carbon content was 49%, the carbon content of the lubricant was 78%, and the bio-based carbon content was 0%, so the bio-based carbon content of the total carbon contained in the composition can be calculated as follows: (75 x 0.61 x 0.22 + 25 x 0.56 x 0.49 + 0.12 x 0.78 x 0) / (75 x 0.61 + 25 x 0.56 + 0.12 x 0.78) = 0.28, or 28%. The pelletized composition was fed to a single-screw extruder with a screw diameter of 40 mm and an inflation molding machine equipped with an annular die with a diameter of 60 mm and a lip gap of 1.6 mm, and molded at a set temperature of 160°C and a blow ratio of 3.0 to obtain a film with a thickness of 30 μm. The resulting film was subjected to a color resistance test after immersion for 7 hours. The results are shown in Table 1.
[0101] [Examples 4 to 8, Comparative Example 5] Aliphatic-aromatic polyester resins (A1) to (A3) were molded into sheets having a thickness of 120 μm using a press molding machine set at 180°C. These films were subjected to a discoloration resistance test with an immersion time of 2 hours, and the results are shown in Table 2. Table 2 also lists the ester group content of each resin, the proportion of structural units derived from terephthalic acid among all structural units derived from dicarboxylic acids, the glass transition temperature, and the bio-based carbon content of each composition. For Examples 4 to 6, the crystallization peak temperature and half-width were analyzed, and the results are shown in Table 2. The DSC curves for these resins are shown in Figure 1.
[0102]
[0103]
[0104] Tables 1 and 2 show that aliphatic-aromatic polyesters having an ester group content of 9.6 mol / kg or more and resin compositions containing 20% by mass or more of such aliphatic-aromatic polyesters have excellent resistance to discoloration caused by food and beverages, and are therefore suitable for use in food and beverage packaging, particularly food and beverage containers. Example 1 and Comparative Example 4 show that excellent opening properties can be achieved by including a filler in the resin composition. Examples 1 to 3 show that even better opening properties can be achieved by including an aliphatic polyester in the resin composition. Furthermore, Table 2 and Examples 4 to 6 in FIG. 1 show that aliphatic-aromatic polyesters with a high biobased carbon content tend to have a smaller half-width of the crystallization peak, a faster crystallization rate, and even better discoloration resistance.
Claims
1. A biodegradable resin composition comprising an aliphatic-aromatic polyester and a filler, wherein the content of the aliphatic-aromatic polyester in the biodegradable resin composition is 20% by mass or more and 99% by mass or less, the content of the filler in the biodegradable resin composition is 0.3% by mass or more and 50.0% by mass or less, and the content of ester groups contained in the aliphatic-aromatic polyester is 9.6 mol / kg or more.
2. The biodegradable resin composition according to claim 1, wherein the glass transition temperature of the aliphatic-aromatic polyester is within the range of -27 to 0°C.
3. The biodegradable resin composition according to claim 1 or 2, wherein the aliphatic-aromatic polyester contains at least polybutylene succinate terephthalate.
4. The biodegradable resin composition according to claim 3, wherein the polybutylene succinate terephthalate has a bio-based carbon content of 50% or more as measured according to ISO 16620-2.
5. The biodegradable resin composition according to claim 3, wherein the proportion of structural units derived from terephthalic acid among all structural units derived from dicarboxylic acids contained in the aliphatic-aromatic polyester is 15 to 70 mol %.
6. The biodegradable resin composition according to claim 1 or 2, further comprising an aliphatic polyester.
7. The biodegradable resin composition according to claim 1 or 2, which has a bio-based carbon content of 20% or more as measured according to ISO 16620-2.
8. A molded article made of the biodegradable resin composition according to claim 1 or 2.
9. The molded article according to claim 8, which is a packaging material for food and drink.
10. The molded article according to claim 9, wherein the food and beverage packaging material is a food and beverage container.
11. A laminate having a substrate and a layer made of the biodegradable resin composition according to claim 1 or 2.
12. The laminate according to claim 11, which is a food and drink packaging material.
13. The laminate according to claim 12, wherein the food or beverage packaging material is a food or beverage container.
14. Polybutylene succinate terephthalate having an ester group content of 9.6 mol / kg or more and a bio-based carbon content of 20% or more as measured by ISO 16620-2.
15. The polybutylene succinate terephthalate according to claim 14, having a bio-based carbon content of 50% or more as measured by ISO 16620-2.
16. A molded article comprising the polybutylene succinate terephthalate according to claim 14 or 15.
17. The molded article according to claim 16, which is a packaging material for food and drink.
18. The molded article according to claim 17, wherein the food and beverage packaging material is a food and beverage container.
19. A laminate comprising a substrate and a layer made of the polybutylene succinate terephthalate according to claim 14 or 15.
20. The laminate of claim 19 which is a food and drink packaging material.
21. The laminate of claim 20, wherein the food or beverage packaging material is a food or beverage container.
Citation Information
Patent Citations
How to coat paper
JP2012504195A
Method of producing plant-derived polyester and polyester obtained by the method
JP2011122144A
Polyester resin composition, film obtained by molding resin composition and bag obtained by molding film
JP2014156539A
Polyester resin composition and film obtained by molding the polyester resin composition
JP2014156540A
Aliphatic-aromatic polyester resin and molded item thereof
WO2022014434A1