Unidirectional material, fiber resin composite, and vibration-damping molded body
The use of high-fineness liquid crystal polyester fibers in a unidirectional fiber aggregate with a controlled thickness variation and high coverage rate within a hard matrix resin composite addresses the limitations of existing fiber-reinforced composites, enhancing vibration damping and handleability while ensuring structural integrity.
Patent Information
- Application Number
- PCT/JP2024/019714
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-05-29
- Publication Date
- 2024-12-05
AI Technical Summary
Existing fiber-reinforced composite materials with unidirectional fiber aggregates, particularly those using wholly aromatic polyester fibers, face limitations in vibration damping performance and handleability due to insufficient fineness and orientation variability, leading to poor vibration damping and ease of breakage.
A fiber resin composite and unidirectional material utilizing a unidirectional fiber aggregate of liquid crystal polyester fibers with a specific fineness of 2.5 dtex or more, high coverage rate, and controlled coefficient of variation in thickness, integrated with a hard matrix resin, to enhance vibration damping and handling properties.
The solution significantly improves vibration damping performance and handleability of the unidirectional material, reducing anisotropy and preventing cracks, while maintaining high toughness and uniform fiber distribution.
Smart Images

Figure JP2024019714_05122024_PF_FP_ABST
Abstract
Description
Unidirectional materials, fiber-resin composites and vibration-damping molded articles Related Applications
[0001] This application claims priority from Japanese Patent Application No. 2023-089882, filed on May 31, 2023, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a fiber-resin composite and molded article having excellent vibration damping properties, and a unidirectional material that can be contained therein.
[0003] It has been known that fiber-reinforced composite materials consisting of inorganic fibers and matrix resins can improve the mechanical strength inherent to the matrix resin by adding inorganic fibers. Meanwhile, technologies have been proposed to provide composite materials with vibration damping properties in addition to improving strength.
[0004] For example, Patent Document 1 (Japanese Patent No. 6499029) discloses a sheet-like material for producing vibration-damping members, which is a sheet-like material having a layer containing wholly aromatic polyester fibers and a matrix resin arranged on at least one outermost surface.
[0005] Furthermore, Patent Document 2 (WO 2015 / 151919) discloses a fiber-reinforced composite material formed by laminating a fiber structure (1) made only of inorganic fibers and a fiber structure (2) containing wholly aromatic polyester fibers, and impregnating these with a resin, characterized in that the outermost layer of the fiber-reinforced composite material is the fiber structure (1) made only of inorganic fibers, and at least one layer of the fiber structure (2) containing wholly aromatic polyester fibers is present in a layer other than the central layer.
[0006] Patent No. 6499029 International Publication No. 2015 / 151919
[0007] The sheet material for manufacturing vibration-damping members in Patent Document 1 is specifically directed to a plain weave fabric of wholly aromatic polyester fibers, and therefore does not describe at all how to improve handleability, which is a problem specific to unidirectional fiber assemblies.
[0008] Furthermore, although the fiber-reinforced composite material of Patent Document 2 specifically considers a unidirectional fiber assembly of wholly aromatic polyester fibers, the unidirectional fiber assembly uses wholly aromatic polyester fibers with a fineness of 2.3 dtex or less, which is insufficient in terms of utilizing the vibration damping performance provided by the wholly aromatic polyester fibers.
[0009] Therefore, an object of the present invention is to provide a unidirectional material that can improve vibration damping performance and handling properties by using a unidirectional fiber aggregate of liquid crystal polyester fibers, and a fiber resin composite and molded article containing the same.
[0010] The inventors of the present invention have found that it is preferable to use a unidirectional fiber assembly having a certain monofilament fineness or more in order to utilize the vibration damping performance provided by liquid crystal polyester fibers. However, they have also found that as the monofilament fineness increases, the vibration damping performance of the unidirectional fiber assembly varies due to the fiber orientation of the unidirectional fiber assembly, and that when used as a sheet-like material, the unidirectional fiber assembly is more likely to crack depending on the monofilament fineness. To overcome these drawbacks, the inventors have found that the above-mentioned drawbacks can be overcome by providing a unidirectional fiber assembly with a specific cover ratio and controlling the coefficient of variation of the thickness caused by the unidirectional fiber assembly, thereby completing the present invention.
[0011] That is, the present invention can be configured in the following aspects. [Aspect 1] A fiber resin composite comprising: a liquid crystal polyester fiber-containing layer containing a unidirectional fiber aggregate of liquid crystal polyester fibers and a matrix resin; and a reinforcing fiber-containing layer containing reinforcing fibers and a matrix resin, wherein the matrix resin of the liquid crystal polyester fiber-containing layer is a hard resin, the single fiber fineness of the liquid crystal polyester fiber in the liquid crystal polyester fiber-containing layer is 2.5 dtex or more (preferably 3.5 dtex or more, more preferably 5.0 dtex or more), the cover rate of the liquid crystal polyester fiber in the liquid crystal polyester fiber-containing layer is 91% or more (preferably 96% or more, more preferably 98% or more, even more preferably 99% or more), and the coefficient of variation of the cover thickness of the liquid crystal polyester fiber in the liquid crystal polyester fiber-containing layer is 0.33 or less (preferably 0.28 or less, more preferably 0.25 or less). [Aspect 2] A fiber resin composite according to Aspect 1, wherein the basis weight of the single layer of the liquid crystal polyester fiber-containing layer is 800 g / m 2 or less (preferably 15 to 800 g / m 2 , more preferably 30 to 400 g / m 2 , more preferably 50 to 300 g / m 2 , and even more preferably 50 to 270 g / m 2 , particularly preferably 50 to 200 g / m 2 , particularly preferably 50 to 150 g / m 2 [Aspect 3] The fiber-resin composite according to Aspect 1 or 2, wherein the liquid crystal polyester fiber has a single filament fineness of 5.0 dtex or more. [Aspect 4] The fiber-resin composite according to any one of Aspects 1 to 3, wherein the matrix resin of the reinforcing fiber-containing layer is a hard resin. [Aspect 5] The fiber-resin composite according to any one of Aspects 1 to 4, wherein the basis weight of the unidirectional fiber aggregate in the single layer containing the liquid crystal polyester fiber is 700 g / m 2 or less (preferably 10 g / m 2 700g / m or more 2 or less, more preferably 20 g / m 2 More than 300g / m 2More preferably 40 g / m or less 2 180g / m or more 2 A fiber-resin composite according to any one of Aspects 1 to 5, wherein the liquid crystal polyester fiber is a multifilament, and the twist number thereof is 100 T / m or less (preferably 10 T / m or less, more preferably 8 T / m or less). A fiber-resin composite according to any one of Aspects 1 to 6, wherein the fiber-resin composite is in the form of a tape. [Aspect 8] A unidirectional material comprising a unidirectional fiber aggregate of liquid crystal polyester fibers and a matrix resin, wherein the matrix resin is a hard resin, the liquid crystal polyester fiber has a single filament fineness of 2.5 dtex or more (preferably 3.5 dtex or more, more preferably 5.0 dtex or more), the cover rate of the liquid crystal polyester fiber in the unidirectional material is 91% or more (preferably 96% or more, more preferably 98% or more, even more preferably 99% or more), and the coefficient of variation of the cover thickness of the liquid crystal polyester fiber in the unidirectional material is 0.33 or less (preferably 0.28 or less, more preferably 0.25 or less). [Aspect 9] The unidirectional material according to Aspect 8, wherein the liquid crystal polyester fiber has a single filament fineness of 5.0 dtex or more. [Aspect 10] The unidirectional material according to Aspect 8 or 9, wherein the basis weight of the unidirectional fiber aggregate in the unidirectional material is 300 g / m 2 or less (preferably 10 g / m 2 More than 300g / m 2 or less, more preferably 25 g / m 2 More than 250g / m 2 More preferably 50 g / m or less 2 180g / m or more 2 less than, even more preferably 50 g / m 2 130g / m or more 2 less than 50 g / m 2 More than 100g / m 2A unidirectional material having a total fineness of 1000 dtex or more. [Aspect 11] The unidirectional material according to any one of Aspects 8 to 10, wherein the total fineness of the liquid crystal polyester fibers is 1000 dtex or more, and the relationship between the total fineness A (dtex), the end count B (lines / inch), and the twist count C (T / m) of the liquid crystal polyester fibers constituting the unidirectional fiber assembly, as expressed by A × B ÷ C, is 10,000 or more (preferably 12,000 or more). [Aspect 12] The unidirectional material according to any one of Aspects 8 to 10, wherein the total fineness of the liquid crystal polyester fibers is less than 1000 dtex, and the relationship between the total fineness A (dtex), the end count B (lines / inch), and the twist count C (T / m) of the liquid crystal polyester fibers constituting the unidirectional fiber assembly, as expressed by A × B ÷ C, is 2,000 or more (preferably 3,000 or more). [Aspect 13] The unidirectional material according to any one of aspects 8 to 12, wherein the basis weight is 350 g / m 2 or less (preferably 20 to 350 g / m 2 , more preferably 50 to 300 g / m 2 , more preferably 100 to 250 g / m 2 , and even more preferably 100 to 200 g / m 2 , particularly preferably 100 to 150 g / m 2 A unidirectional material according to any one of Aspects 8 to 13, wherein the liquid crystal polyester fiber is a multifilament and the twist number thereof is 100 T / m or less (preferably 10 T / m or less, more preferably 8 T / m or less). Aspect 15: A vibration-damping molded article comprising the fiber resin composite according to any one of Aspects 1 to 7 or the unidirectional material according to any one of Aspects 8 to 14. Aspect 16: A method for producing a fiber resin composite, comprising overlaying the unidirectional material according to Aspects 8 to 14 and a reinforcing fiber sheet containing reinforcing fibers and a matrix resin to form an integral mold.
[0012] As used herein, the singular forms "a," "an," and "the" are intended to include the plural forms, including "at least one," unless the content clearly dictates otherwise. As used herein, the terms "and / or," "at least one," and "one or more" include any and all combinations of the associated listed items.
[0013] It should be noted that any combination of at least two elements disclosed in the claims and / or the specification is included in the present invention, and in particular any combination of two or more of the claims described in the claims is included in the present invention.
[0014] According to the present invention, it is possible to improve the handling properties of a unidirectional material containing liquid crystal polyester fibers, while improving the vibration damping performance of a fiber resin composite.
[0015] The present invention will be more clearly understood from the following description of preferred embodiments with reference to the accompanying drawings. However, the examples and drawings are merely for illustration and explanation purposes and should not be used to define the scope of the present invention. The scope of the present invention is defined by the appended claims.
[0023] Fig. 1 is an exploded schematic cross-sectional view illustrating a method of stacking when producing a fiber-resin composite according to one embodiment of the present invention.
[0024] Fig. 2 is a schematic perspective view showing a flat fiber-resin composite according to one embodiment of the present invention.
[0025] Fig. 3 is an enlarged cross-sectional photograph of a selected measurement point in the fiber-resin composite obtained in Example 1.
[0026] Fig. 4 is a schematic cross-sectional view illustrating a fiber-resin composite according to one embodiment of the present invention.
[0027] Fig. 5 is a schematic cross-sectional view illustrating a fiber-resin composite according to another embodiment of the present invention.
[0016] A fiber resin composite according to one embodiment of the present invention includes a liquid crystal polyester fiber-containing layer containing a unidirectional fiber aggregate of liquid crystal polyester fibers and a matrix resin, and a reinforcing fiber-containing layer containing reinforcing fibers and a matrix resin.
[0017] (Liquid Crystal Polyester Fiber) The liquid crystal polyester fiber contained in the liquid crystal polyester fiber-containing layer can be produced, for example, by melt-spinning a liquid crystal polyester and, if necessary, solid-phase polymerizing the spun raw yarn. Liquid crystal polyester is a polyester that exhibits optical anisotropy (liquid crystallinity) in the molten phase. This can be confirmed, for example, by placing a sample on a hot stage, heating it under a nitrogen atmosphere, and observing the transmitted light through the sample with a polarizing microscope. Furthermore, the liquid crystal polyester is composed of structural units derived from, for example, aromatic diols, aromatic dicarboxylic acids, aromatic hydroxycarboxylic acids, etc., and the chemical structure of these structural units is not particularly limited as long as it does not impair the effects of the present invention. Furthermore, the liquid crystal polyester may also contain structural units derived from aromatic diamines, aromatic hydroxyamines, or aromatic aminocarboxylic acids, as long as it does not impair the effects of the present invention.
[0018] For example, preferred structural units include those shown in Table 1. Here, Y's may be present in a number ranging from 1 to the maximum number that can be substituted on the aromatic ring, and are each independently selected from the group consisting of a hydrogen atom, a halogen atom (e.g., a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, etc.), an alkyl group (e.g., an alkyl group having 1 to 4 carbon atoms such as a methyl group, an ethyl group, an isopropyl group, a t-butyl group, etc.), an alkoxy group (e.g., a methoxy group, an ethoxy group, an isopropoxy group, an n-butoxy group, etc.), an aryl group (e.g., a phenyl group, a naphthyl group, etc.), an aralkyl group [e.g., a benzyl group (phenylmethyl group), a phenethyl group (phenylethyl group), etc.], an aryloxy group (e.g., a phenoxy group), an aralkyloxy group (e.g., a benzyloxy group, etc.), and the like.
[0019] More preferred structural units include the structural units described in Examples (1) to (18) shown in the following Tables 2, 3, and 4. When the structural unit in the formula is a structural unit that can exhibit multiple structures, two or more of such structural units may be combined and used as structural units that constitute the polymer.
[0020]
[0021]
[0022]
[0023] In the structural units of Tables 2, 3, and 4, n is an integer of 1 or 2, and each of the structural units n=1 and n=2 may exist alone or in combination; Y1 and Y2 each independently represent a hydrogen atom, a halogen atom (e.g., a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, etc.), an alkyl group (e.g., an alkyl group having 1 to 4 carbon atoms such as a methyl group, an ethyl group, an isopropyl group, a t-butyl group, etc.), an alkoxy group (e.g., a methoxy group, an ethoxy group, an isopropoxy group, an n-butoxy group, etc.), an aryl group (e.g., a phenyl group, a naphthyl group, etc.), an aralkyl group [benzyl group (phenylmethyl group), phenethyl group (phenylethyl group), etc.], an aryloxy group (e.g., a phenoxy group), an aralkyloxy group (e.g., a benzyloxy group, etc.), etc. Among these, preferred Y1 and Y2 include a hydrogen atom, a chlorine atom, a bromine atom, or a methyl group.
[0024] Examples of Z include substituents represented by the following formulas.
[0025] The liquid crystal polyester may preferably be a combination having two or more types of naphthalene skeletons as constituent units.
[0026] The liquid crystal polyester may preferably contain both a structural unit (A) derived from hydroxybenzoic acid and a structural unit (B) derived from hydroxynaphthoic acid. For example, the structural unit (A) may be represented by the following formula (A), and the structural unit (B) may be represented by the following formula (B). From the viewpoint of improving melt moldability, the ratio of the structural unit (A) to the structural unit (B) may preferably be in the range of 9 / 1 to 1 / 1, more preferably 7 / 1 to 1 / 1, and even more preferably 5 / 1 to 1 / 1.
[0027]
[0028] The total of the structural units (A) and the structural units (B) may be, for example, 65 mol % or more, more preferably 70 mol % or more, and even more preferably 80 mol % or more, based on the total structural units. Liquid crystal polyesters in which the structural units (B) account for 4 to 45 mol % of the polymer are particularly preferred.
[0029] The melting point of the liquid crystal polyester preferably used in the present invention is preferably 250 to 360°C, more preferably 260 to 320°C. Here, the melting point is the main absorption peak temperature observed when measured using a differential scanning calorimeter (DSC; Mettler "TA3000") in accordance with JIS K7121:2012. Specifically, 10 to 20 mg of a sample is placed in an aluminum pan in the DSC apparatus, and nitrogen is passed through as a carrier gas at 100 cc / min, and the endothermic peak is measured when the temperature is increased from room temperature (e.g., 25°C) at a rate of 20°C / min. If a clear peak does not appear in the first run of DSC measurement due to the type of polymer, the polymer may be heated at a heating rate of 50°C / min to a temperature 50°C higher than the expected flow temperature, held at that temperature for 3 minutes until completely melted, cooled to 50°C at a heating rate of -80°C / min, and then measured for an endothermic peak at a heating rate of 20°C / min.
[0030] The liquid crystal polyester may contain thermoplastic polymers such as polyethylene terephthalate, modified polyethylene terephthalate, polyolefin, polycarbonate, polyamide, polyphenylene sulfide, polyether ether ketone, and fluororesin, as long as the effects of the present invention are not impaired. Furthermore, various additives may be added, such as inorganic substances such as titanium oxide, kaolin, silica, and barium oxide, colorants such as carbon black, dyes, and pigments, antioxidants, ultraviolet absorbers, and light stabilizers.
[0031] The liquid crystal polyester fiber may be a non-conjugated fiber or a conjugated fiber. The cross-sectional shape of the liquid crystal polyester fiber is not particularly limited, and may be a normal fiber having a round cross section (including a cocoon shape), or a fiber having a modified cross section other than a round cross section. In the case of a modified cross section fiber, the cross-sectional shape may be, for example, any of a square, polygonal, triangular, hollow, flat, multi-lobed, cross, dogbone, T-shaped, V-shaped, etc. Modified cross section fibers are often non-conjugated fibers.
[0032] Examples of the composite fiber include a core-sheath type composite fiber in which the core component is a liquid crystal polyester and the sheath component is a flexible thermoplastic resin; and a hybrid composite fiber in which the core component is a liquid crystal polyester and the sheath component has a sea-island structure in which the sea component is a flexible thermoplastic resin and the island component is a liquid crystal polyester.
[0033] Examples of flexible thermoplastic resins include resins that do not have aromatic rings on the main chain, and resins that have aromatic rings on the main chain and have four or more atoms on the main chain between the aromatic rings.Specific examples of such resins include polyolefins; polyamides; polycarbonates; polyphenylene sulfide (abbreviated as PPS); polyesters such as polyethylene terephthalate, modified polyethylene terephthalate, amorphous polyarylate, and polyethylene naphthalate (abbreviated as PEN); polyether ether ketones; and fluororesins.
[0034] The liquid crystal polyester fiber may contain 50% by weight or more of liquid crystal polyester, preferably 80% by weight or more, more preferably 90% by weight or more, even more preferably 95% by weight or more, and still more preferably 99.9% by weight or more.
[0035] The liquid crystal polyester fiber may be a monofilament or a multifilament, as long as the effects of the present invention can be achieved. From the viewpoint of vibration damping performance, the liquid crystal polyester fiber may have a single yarn fineness of 2.5 dtex or more, preferably 3.5 dtex or more, and more preferably 5.0 dtex or more, in both the monofilament and the multifilament. When the single yarn fineness is within the above range, the vibration damping performance provided by the liquid crystal polyester fiber can be effectively utilized.
[0036] In the case of monofilaments, the single yarn fineness may be, for example, 2.5 to 100 dtex, preferably 5 to 80 dtex, and more preferably 8 to 60 dtex, whereas in the case of multifilaments, the single yarn fineness may be, for example, 2.5 to 20 dtex, preferably 3.5 to 15 dtex, more preferably 5.0 to 10 dtex, and even more preferably 5.0 to 7.0 dtex.
[0037] When the liquid crystal polyester fiber is a multifilament, the total fineness can be appropriately set depending on the single yarn fineness and twist number of the liquid crystal polyester fiber, and may be, for example, 100 dtex or more, preferably 300 dtex or more, and more preferably 500 dtex or more. The upper limit is not particularly limited, and may be, for example, 5000 dtex or less, and preferably 3000 dtex or less. When the liquid crystal polyester fiber is a multifilament, the total fineness may be, for example, 100 to 5000 dtex, preferably 300 to 5000 dtex, and more preferably 500 to 3000 dtex.
[0038] The number of filaments constituting the multifilament may be, for example, 3 or more, preferably 5 or more, more preferably 15 or more, and even more preferably 25 or more. The number of filaments can be appropriately set depending on the single yarn fineness, but may be 500 or less, or from the viewpoint of thinning, preferably 300 or less, and more preferably 200 or less. The number of filaments constituting the multifilament may be, for example, 3 to 500, preferably 5 to 500, more preferably 15 to 300, and even more preferably 25 to 200.
[0039] The multifilament may be loosely twisted (e.g., 100 T / m or less), but is preferably substantially untwisted (e.g., 10 T / m or less, preferably 8 T / m or less). By having the twist number within the above range, it is possible to increase the cover rate and reduce the coefficient of variation of the cover thickness. Furthermore, if necessary, the multifilament may be subjected to an opening treatment and / or a smoothing treatment. The twist number is a value measured by the method described in the Examples below. In the following, a multifilament with a twist number exceeding 0 T / m (e.g., 0.1 T / m or more) may be referred to as a yarn.
[0040] (Unidirectional fiber assembly) The unidirectional fiber assembly is a fiber assembly in which the above-mentioned liquid crystal polyester fibers are arranged in one direction, and threads perpendicular to the one direction may be stitched as necessary. The proportion of liquid crystal polyester fibers in the unidirectional fiber assembly may be, for example, 90% by mass or more, preferably 95% by mass or more, and more preferably 99% by mass or more. The end count of the liquid crystal polyester fibers in the unidirectional fiber assembly can be appropriately set depending on the total fineness and twist number of the liquid crystal polyester fibers, and may be, for example, 5 fibers / inch or more, preferably 7 fibers / inch or more, and more preferably 10 fibers / inch or more. The upper limit of the end count is not particularly limited, but may be 100 fibers / inch or less, preferably 50 fibers / inch or less, more preferably 40 fibers / inch or less, and even more preferably 20 fibers / inch or less. The end count of the liquid crystal polyester fibers in the unidirectional fiber assembly may be, for example, 5 to 100 fibers / inch, preferably 7 to 50 fibers / inch, more preferably 10 to 40 fibers / inch, and even more preferably 10 to 20 fibers / inch. The end count is a value measured by the method described in the Examples below.
[0041] The basis weight of the unidirectional fiber aggregate is, for example, 10 g / m 2 or more, preferably 25 g / m 2 More preferably, 50 g / m 2 Although the upper limit is not particularly limited, from the viewpoint of thinning, it may be, for example, 300 g / m 2 or less, preferably 250 g / m 2 or less, more preferably 180 g / m 2 less than 130 g / m 2 less than, and even more preferably less than 100 g / m 2 The basis weight of the unidirectional fiber aggregate may be, for example, 10 g / m 2 More than 300g / m 2 or less, preferably 25 g / m 2 More than 250g / m 2 or less, more preferably 50 g / m 2180g / m or more 2 less than 50 g / m 2 130g / m or more 2 less than, even more preferably 50 g / m 2 More than 100g / m 2 The basis weight can be calculated by arranging the fibers in a 50 cm width while maintaining the pick count per width used in the unidirectional material, sampling a 2 m length, and measuring the bone dry mass after 4 hours at 105°C, as long as the unidirectional fiber aggregate is not yet integrated with the matrix resin. After integration with the matrix resin, the bone dry mass can be calculated by obtaining a cut piece of a predetermined area from the unidirectional material, removing the matrix resin from the cut piece by dissolving it in a solvent, or the like, and then dividing the bone dry mass of the resulting unidirectional fiber aggregate by the area of the cut piece.
[0042] For example, in a unidirectional fiber assembly, the twist number and the pick number may be determined depending on the total fineness of the liquid crystal polyester fiber (yarn). When the total fineness of the liquid crystal polyester fiber constituting the unidirectional fiber assembly is 1000 dtex or more, the relationship between the total fineness A (dtex), the pick number B (lines / inch), and the twist number C (T / m) of the liquid crystal polyester fiber constituting the unidirectional fiber assembly, as a value of A × B ÷ C, may be, for example, 10,000 or more, preferably 12,000 or more. The upper limit is not particularly limited, but may be about 30,000. In general, the larger the total fineness and the pick number, the more uniform the distribution of the liquid crystal polyester fiber in the unidirectional material. Furthermore, the smaller the twist number, the greater the spread of the liquid crystal polyester fiber per yarn in the unidirectional material.
[0043] On the other hand, when the total fineness of the liquid crystal polyester fibers constituting the unidirectional fiber assembly is less than 1000 dtex, the value of A×B÷C described above may be 2000 or more, preferably 3000 or more. The upper limit is not particularly limited, but may be about 5000. That is, when the total fineness of the liquid crystal polyester fibers is small, the number of twists of the yarn can be intentionally increased to increase the fiber pick count, and as a result, the distribution of the liquid crystal polyester fibers in the unidirectional material can be made uniform.
[0044] (Hard Resin) The matrix resin of the liquid crystal polyester fiber-containing layer is a hard resin. The hard resin is not particularly limited as long as it has a durometer hardness of 90 or more, and may be a thermoplastic resin or a thermosetting resin. These resins may be used alone or in combination. Here, the durometer hardness refers to the value measured according to JIS K 6253-3:2012 (Type A, for general rubber, spring load value 550-8050 mN, needle shape: tip diameter 0.79 mm, 35° truncated cone, indenter height: 2.50 mm). By using a hard resin as the matrix resin of the liquid crystal polyester fiber-containing layer, the fiber-resin composite can exhibit vibration damping properties while providing rigidity. The content of the hard resin in the matrix resin of the liquid crystal polyester fiber-containing layer may be 50% by mass or more, preferably 70% by mass or more, more preferably 90% by mass or more, and particularly preferably 100% by mass, i.e., the entire matrix resin in the liquid crystal polyester fiber-containing layer is a hard resin. As the preferred hard resin, the resins exemplified below are used.
[0045] Examples of the thermoplastic resin include polyester-based resins (e.g., polyethylene terephthalate, modified polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, etc.), polyolefin-based resins (e.g., polypropylene, modified polypropylene, polyethylene, etc.), polyamide-based resins (e.g., aliphatic polyamides such as polyamide 6, polyamide 66, polyamide 12, and polyamide 6-12, semi-aromatic polyamides such as polyamide 9T and polyamide 66IT, and alicyclic polyamides), styrene-based resins (e.g., polystyrene, etc.), polycarbonate-based resins, (meth)acrylic resins, polyether-based resins, ionomer resins (e.g., olefin-based ionomers, fluorine-based ionomers, etc.), polyetherimide-based resins, polyphenylene sulfide-based resins, and polyether ketone-based resins (e.g., PEEK, PEK, etc.).
[0046] Examples of thermosetting resins include phenolic resins (novolac-type phenolic resins, resol-type phenolic resins), epoxy-type resins, vinyl ester-type resins, unsaturated polyester-type resins, cyanate-type resins, crosslinked methacrylic resins, melamine-type resins, diallyl phthalate-type resins, silicone-type resins, maleimide-type resins, polyimide-type resins, etc. The matrix resin of the liquid crystal polyester fiber-containing layer can be appropriately set depending on the type of matrix resin of the reinforcing fiber-containing layer, but from the viewpoint of vibration damping performance, for example, thermosetting resins are preferred, and among them, epoxy-type resins, polyimide-type resins, unsaturated polyester-type resins, cyanate-type resins, etc. are preferred.
[0047] The proportion of the liquid crystal polyester fiber contained in the liquid crystal polyester fiber-containing layer may be, for example, 10% by weight or more per layer, preferably 13% by weight or more, and more preferably 15% by weight or more. It may also be 80% by weight or less, preferably 70% by weight or less. The proportion of the liquid crystal polyester fiber contained in the liquid crystal polyester fiber-containing layer may be, for example, 10 to 80% by weight per layer, preferably 13 to 80% by weight, and more preferably 15 to 70% by weight.
[0048] (Unidirectional Material) The unidirectional material contains the unidirectional fiber aggregate of the liquid crystal polyester fiber described above and a hard resin as a matrix resin. Therefore, the unidirectional material has the characteristics such as the fiber placement count and basis weight described in the section on the unidirectional fiber aggregate described above. The method of integrating the unidirectional fiber aggregate with the unidirectional fiber aggregate can be selected depending on the type of matrix resin. For example, when the matrix resin is a thermosetting resin, the unidirectional fiber aggregate may be impregnated with or coated with a thermosetting resin dissolved in a solvent to form a unidirectional material preformed into a sheet. Alternatively, the unidirectional fiber aggregate may be overlaid with a semi-cured sheet of thermosetting resin to form a unidirectional material preformed into a sheet.
[0049] When the matrix resin is a thermoplastic resin, the unidirectional fiber assembly may be impregnated with or coated with a pre-molten thermoplastic resin to form a sheet-like unidirectional material, or a sheet-like thermoplastic resin may be superimposed on the unidirectional fiber assembly and heated and compressed to form an integrated unidirectional material.
[0050] In the unidirectional material, the unidirectional fiber aggregate is distributed with a coverage of 91% or more, preferably 96% or more, more preferably 98% or more, and even more preferably 99% or more. The upper limit of the coverage is preferably 100%. Here, the coverage refers to the proportion of liquid crystal polyester fibers present among measurement points set every 100 μm in a 2 mm width of the unidirectional fiber aggregate of liquid crystal polyester fibers in the unidirectional material. In the unidirectional material, the coverage exhibited by the unidirectional fiber aggregate may be simply referred to as the coverage of the unidirectional material hereinafter. In addition, the thickness of the liquid crystal polyester fiber (cover thickness) can be measured at the measurement point used to measure the coverage. The coverage and cover thickness are values measured by the methods described in the examples below.
[0051] By controlling the cover ratio of the unidirectional material, for example, when the matrix resin is a thermosetting resin, prepreg cracking can be prevented, improving the handleability of the unidirectional material. Furthermore, when the matrix resin is a thermoplastic resin, fiber disorder in the unidirectional fiber aggregate can be prevented, improving the handleability of the unidirectional material. The cover ratio of the unidirectional material can be measured in accordance with the method used for measuring fiber-resin composites, which will be described later. The cover ratio can be adjusted to a desired range by appropriately adjusting not only the basis weight of the unidirectional fiber aggregate, but also the number of twists of the liquid crystal polyester fiber, and the relationship between the total fineness, the number of ends, and the number of twists of the liquid crystal polyester fiber.
[0052] In measuring the cover ratio of a unidirectional material, the unidirectional material may be measured as is as long as the state of the unidirectional fiber aggregate in the unidirectional material can be maintained, but from the viewpoint of fixing the aligned state of the unidirectional fiber aggregate, the unidirectional material may be entirely embedded in a resin or the like and once fixed, and then the measurement may be performed using the unidirectional material. In addition, when the liquid crystal polyester fiber-containing layer in the fiber resin composite is formed of a single layer of unidirectional material, the cover ratio obtained by the liquid crystal polyester fiber-containing layer present in the fiber resin composite may be used as is.
[0053] The coefficient of variation of the cover thickness due to the unidirectional fiber aggregate in the unidirectional material is 0.33 or less. The coefficient of variation of the cover thickness may be preferably 0.28 or less, more preferably 0.25 or less, and by adjusting it to a smaller value, toughness can be improved. The coefficient of variation can be calculated by dividing the variation (standard deviation) of the cover thickness by the cover thickness (average value). The coefficient of variation of the cover thickness within the above range can be achieved by appropriately adjusting the number of twists of the liquid crystal polyester fiber as well as the relationship between the total fineness, end count, and twist number of the liquid crystal polyester fiber.
[0054] The cover thickness (average value) of the unidirectional fiber aggregate in the unidirectional material is preferably thin, and may be, for example, 300 μm or less, preferably 250 μm or less, and more preferably 200 μm or less. There is no particular lower limit, but it may be 5 μm or more, 15 μm or more, or 100 μm or more. The cover thickness may be, for example, 5 to 300 μm, preferably 15 to 250 μm, and more preferably 100 to 200 μm. Having a cover thickness within the above range allows for greater freedom in the number and direction of layers of the unidirectional material and in the design.
[0055] The unidirectional material may be used in the form of a sheet or a tape. When the unidirectional material is used in the form of a tape, the width can be appropriately set depending on the application, but may be, for example, 0.5 to 20 mm, preferably 0.8 to 10 mm, and more preferably 1 to 6 mm.
[0056] The thickness of the unidirectional material can be appropriately selected depending on the thickness of other components, but from the viewpoint of thinning, it may be, for example, 0.01 to 0.4 mm, preferably 0.03 to 0.3 mm, and more preferably 0.05 to 0.2 mm. The thickness of the unidirectional material is a value measured by the method described in the examples below.
[0057] The weight of the unidirectional material is, for example, 350 g / m from the viewpoint of thinning. 2 or less, preferably 300 g / m 2 or less, more preferably 250 g / m 2 Below, 200g / m 2 Below, 150g / m 2 or less, for example, 20 g / m 2 or more, preferably 50 g / m 2 More preferably, 100 g / m 2 The weight per unit area of the unidirectional material may be, for example, 20 to 350 g / m 2 and preferably 50 to 300 g / m 2 , more preferably 100 to 250 g / m 2, more preferably 100 to 200 g / m 2 , and even more preferably 100 to 150 g / m 2 may be.
[0058] (Liquid Crystal Polyester Fiber-Containing Layer) The liquid crystal polyester fiber-containing layer may be a single layer or multiple layers in the fiber-resin composite. Furthermore, each liquid crystal polyester fiber-containing layer may be formed from one unidirectional material or multiple unidirectional materials. For example, the number of unidirectional materials per single liquid crystal polyester fiber-containing layer can be appropriately selected from 1 to 6.
[0059] The total basis weight of the liquid crystal polyester fiber-containing layer in the fiber resin composite is not particularly limited, but for example, in a composite having a thickness of 1.5 mm or more, it is 30 g / m 2 or more, preferably 60 g / m 2 More preferably, 100 g / m 2 For example, it may be 1000 g / m or more. 2 or less, preferably 800 g / m 2 or less, more preferably 700 g / m 2 For example, it may be 30 to 1000 g / m 2 and preferably 60 to 800 g / m 2 , more preferably 100 to 700 g / m 2 For example, in a fiber resin composite having a thickness of less than 1.5 mm, the total basis weight of the liquid crystal polyester fiber-containing layer in the fiber resin composite may be, for example, 15 g / m 2 or more, preferably 30 g / m 2 More preferably, 50 g / m 2 For example, it may be 700 g / m or more. 2 or less, preferably 600 g / m 2 or less, more preferably 550 g / m 2 For example, it may be 15 to 700 g / m 2 and preferably 30 to 600 g / m 2, more preferably 50 to 550 g / m 2 Here, the total basis weight of the liquid crystal polyester fiber-containing layer is a value of the total amount when a fiber resin composite has a plurality of liquid crystal polyester fiber-containing layers. When obtaining the basis weight of the liquid crystal polyester fiber-containing layer from the fiber resin composite, the liquid crystal polyester fiber-containing layer can be cut out from the fiber resin composite for each layer, and the basis weight can be calculated as the sum of the basis weights of the liquid crystal polyester fiber-containing layers cut out.
[0060] The basis weight of the liquid crystal polyester fiber-containing layer in a single layer is not particularly limited, but is preferably 15 g / m 2 or more, preferably 30 g / m 2 More preferably, 50 g / m 2 For example, it may be 800 g / m or more. 2 or less, preferably 400 g / m 2 or less, more preferably 300 g / m 2 More preferably 270 g / m or less 2 or less, and even more preferably 200 g / m 2 Particularly preferably 150 g / m 2 The basis weight of the single layer containing the liquid crystal polyester fiber may be, for example, 15 to 800 g / m 2 and preferably 30 to 400 g / m 2 , more preferably 50 to 300 g / m 2 , more preferably 50 to 270 g / m 2 , and even more preferably 50 to 200 g / m 2 , particularly preferably 50 to 150 g / m 2 By adjusting the basis weight of the single layer containing the liquid crystal polyester fiber, it is possible to efficiently control the vibration damping occurring in the composite.
[0061] Furthermore, the basis weight of the unidirectional fiber aggregate in the single layer containing the liquid crystal polyester fiber is, for example, 10 g / m 2 or more, preferably 20 g / m 2 More preferably, 40 g / m 2It may be 700 g / m or more. 2 or less, preferably 300 g / m 2 or less, more preferably 180 g / m 2 The basis weight of the unidirectional fiber aggregate in the single layer of the liquid crystal polyester fiber-containing layer may be, for example, 10 g / m 2 700g / m or more 2 or less, preferably 20 g / m 2 More than 300g / m 2 or less, more preferably 40 g / m 2 180g / m or more 2 It may be less than.
[0062] (Reinforcing fiber-containing layer) The reinforcing fibers contained in the reinforcing fiber-containing layer are not particularly limited as long as they can reinforce the matrix resin. They may be organic fibers or inorganic fibers, and may be used alone or in combination of two or more. Examples of inorganic fibers include glass fibers, carbon fibers, various ceramic fibers (e.g., silicon carbide fibers, silicon nitride fibers, silica fibers, alumina fibers, zirconia fibers, boron fibers, basalt fibers, etc.), various metal fibers (e.g., gold, silver, copper, iron, nickel, titanium, potassium titanate, stainless steel, etc.). Examples of organic fibers include polyparaphenylene benzobisoxazole fibers (PBO fibers), polyphenylene sulfide fibers, aramid fibers (para-aramid fibers, meta-aramid fibers), liquid crystal polyester fibers (excluding unidirectional fiber aggregates of liquid crystal polyester fibers), polysulfonamide fibers, phenolic resin fibers, polyimide fibers, and fluorine fibers. Of these, it is preferable to use carbon fiber, glass fiber, alumina fiber, boron fiber, silicon carbide fiber, potassium titanate fiber, stainless steel fiber, PBO fiber, aramid fiber, etc.
[0063] The reinforcing fibers may be monofilaments or multifilaments. They may be used as short fibers or long fibers. In the case of short fibers, they may be chopped strands. Alternatively, they may be reinforcing fiber assemblies such as woven fabrics (plain weave fabrics, etc.), knitted fabrics, nonwoven fabrics, non-crimped fabrics, and unidirectional fiber assemblies (excluding unidirectional fiber assemblies of liquid crystal polyester fibers).
[0064] The single yarn fineness of the reinforcing fibers can be appropriately selected depending on the shape of the filament, and may be, for example, 0.1 to 600 dtex, preferably 0.5 to 500 dtex, and more preferably 1 to 300 dtex. The total fineness of the reinforcing fibers may be, for example, 100 dtex or more, preferably 300 dtex or more, and more preferably 500 dtex or more. There is no particular upper limit, but it may be, for example, 5000 dtex or less, preferably 3000 dtex or less.
[0065] (Matrix Resin) The reinforcing fiber-containing layer may contain either a hard resin or a soft resin as the matrix resin. Examples of hard resins include the hard resins exemplified in the liquid crystal polyester fiber-containing layer. Examples of soft resins include various thermoplastic elastomer resins, such as polyolefin elastomer resins, ethylene-vinyl ester copolymers, polyvinyl chloride elastomer resins, polyurethane elastomer resins, polystyrene elastomer resins, polyester elastomer resins, polyacrylic elastomer resins, polyamide elastomer resins, polydiene elastomer resins, chlorinated polyethylene elastomer resins, and fluororesin elastomer resins.
[0066] The reinforcing fiber-containing layer can be formed by a known method depending on the shape of the reinforcing fibers and the type of matrix resin. For example, when the reinforcing fibers are short fibers, the short fibers may be mixed with the matrix resin. For example, when the matrix resin is a thermosetting resin, a reinforcing fiber sheet material may be formed by impregnating or applying a thermosetting resin dissolved in a solvent to a reinforcing fiber aggregate. Alternatively, a semi-cured sheet of thermosetting resin may be superimposed on the reinforcing fiber aggregate to form a reinforcing fiber sheet material temporarily formed into a sheet.
[0067] When the matrix resin is a thermoplastic resin, a reinforcing fiber sheet material may be formed by impregnating or applying a pre-molten thermoplastic resin to a reinforcing fiber assembly, or a sheet-like material of a thermoplastic resin may be superimposed on the reinforcing fiber assembly and integrated by heating and compressing to form a reinforcing fiber sheet material.
[0068] (Fiber Resin Composite) The fiber resin composite includes a liquid crystal polyester fiber-containing layer containing a unidirectional fiber aggregate of liquid crystal polyester fibers and a matrix resin, and a reinforcing fiber-containing layer containing reinforcing fibers and a matrix resin, wherein the matrix resin of the liquid crystal polyester fiber-containing layer is a hard resin, the single fiber fineness of the liquid crystal polyester fiber in the liquid crystal polyester fiber-containing layer is 2.5 dtex or more, the coverage of the liquid crystal polyester fiber in the liquid crystal polyester fiber-containing layer is 91% or more, and the variation coefficient of the cover thickness of the liquid crystal polyester fiber in the liquid crystal polyester fiber-containing layer is 0.33 or less.
[0069] The fiber resin composite can be produced by stacking one or more of the unidirectional material and one or more of the reinforcing fiber sheets, and joining and integrating them by a known molding method (e.g., hot molding) depending on the type of matrix resin and the desired shape.
[0070] 1 is an exploded schematic cross-sectional view illustrating a method for laminating components when fabricating a fiber-resin composite according to one embodiment of the present invention. The fiber-resin composite 10 includes a reinforcing fiber-containing layer 11 containing reinforcing fibers and a matrix resin, and liquid crystal polyester fiber-containing layers 121 and 122 disposed above and below the reinforcing fiber-containing layer, respectively.
[0071] Here, the liquid crystal polyester fiber-containing layer 121 is formed by stacking and integrating two unidirectional materials 121a and 121b, and the liquid crystal polyester fiber-containing layer 122 is formed by stacking two unidirectional materials 122a and 122b. When a liquid crystal polyester fiber-containing layer is formed by stacking and integrating a plurality of unidirectional materials, the liquid crystal polyester fiber-containing layer is considered to be a single layer. Each of these unidirectional materials contains a unidirectional fiber aggregate 200 of liquid crystal polyester fibers.
[0072] The reinforcing fiber-containing layer 11 is formed by stacking and integrating four reinforcing fiber sheets 11a, 11b, 11c, and 11d. Each of these reinforcing fiber sheets contains a reinforcing fiber aggregate 300.
[0073] When forming a fiber resin composite, the liquid crystal polyester fibers contained in adjacent unidirectional materials may be integrated together, for example, the unidirectional fiber aggregates 200 of liquid crystal polyester fibers contained in the unidirectional materials 121a and 121b may be integrated together in the liquid crystal polyester fiber-containing layer 121.
[0074] In Fig. 1, the unidirectional fiber aggregates 200 and the reinforcing fiber aggregates 300 are depicted as protruding from the matrix resin, but the unidirectional fiber aggregates and the reinforcing fiber aggregates do not necessarily have to protrude from the matrix resin. Furthermore, although the matrix resin and the unidirectional fiber aggregates are clearly distinguished in the drawing, in a composite, for example, adjacent unidirectional materials may be integrated, and the unidirectional fiber aggregates present in each unidirectional material may be perceived as integrated. For example, in a liquid crystal polyester fiber-containing layer 121 formed by integrating unidirectional materials 121a and 121b, the unidirectional fiber aggregates 200 are often integrated to the extent that they are indistinguishable from each other in appearance.
[0075] When the unidirectional material and the reinforcing fiber sheet are laminated together, if the material has fibers aligned in one direction, the fibers of the materials may be arranged so that the longitudinal directions of the fibers cross each other.
[0076] The heating temperature when molding a fiber resin composite, for example, by heat molding, can be set appropriately depending on, for example, the type of matrix resin. In the case of a thermosetting resin, it is preferable to mold it using a known technique at a temperature equal to or higher than the heat curing temperature to completely cure it. When heating, the heating temperature may be set in multiple stages to reach the heat curing temperature, as necessary. The heat curing temperature can be set appropriately depending on the type of resin. In the case of a thermoplastic resin, it is preferable to mold it using a known technique at a temperature equal to or higher than the melting point or heat distortion temperature of the resin to integrate it. When heating, the heating temperature may be set in multiple stages, but is preferably set in a single stage. The heating temperature may preferably be equal to or lower than (melting point + 50)°C or equal to or lower than (heat distortion temperature + 50)°C.
[0077] Furthermore, when compression molding, the pressure can be set appropriately depending on the type of matrix resin, but in the case of a thermosetting resin, it is preferable to compression mold it in a semi-cured state to completely cure it. For example, when using a vacuum press molding machine, the pressure may be in the range of 0.3 to 6.0 MPa, preferably 0.5 to 5.0 MPa, and more preferably 0.8 to 4.0 MPa. The pressure may be changed in multiple stages. In the case of a thermoplastic resin, integration may also be performed using a similar pressure. The pressure may be changed in multiple stages, but it is preferable to change it in one stage.
[0078] The ratio (weight ratio) of the unidirectional material to the reinforcing fiber sheet used in the fiber-resin composite may be, for example, 2 / 5 to 1 / 40 (unidirectional material / reinforcing fiber sheet), preferably 1 / 4 to 1 / 30, and more preferably 1 / 5 to 1 / 20.
[0079] The arrangement of the unidirectional material and the reinforcing fiber sheet, and the arrangement of the liquid crystal polyester fiber-containing layer and the reinforcing fiber-containing layer are not particularly limited, but from the viewpoint of making it easier to exhibit vibration damping performance, it is preferable that at least one liquid crystal polyester fiber-containing layer is located on the outside in the fiber-resin composite.
[0080] In the fiber-resin composite, the unidirectional fiber aggregate is distributed in the liquid crystal polyester fiber-containing layer at a coverage of 91% or more, preferably 96% or more, more preferably 98% or more, and even more preferably 99% or more. The upper limit of the coverage is preferably 100%. The coverage is the same as that in the unidirectional material described above.
[0081] The method for determining the cover ratio will be outlined with reference to Figures 2 and 3. Figure 2 is a schematic perspective view showing a flat fiber-resin composite according to one embodiment of the present invention. The fiber-resin composite 10 is composed of a liquid crystal polyester fiber-containing layer containing a unidirectional fiber aggregate of liquid crystal polyester fibers and a matrix resin, and a reinforcing fiber-containing layer containing reinforcing fibers and a matrix resin. In Figure 2, the longitudinal direction of the fibers of the unidirectional fiber aggregate in the fiber-resin composite 10 is indicated by a double-headed arrow.
[0082] In determining the coverage of the liquid crystal polyester fiber in the liquid crystal polyester fiber-containing layer in the fiber resin composite, slice images in the width direction (cross-sectional images perpendicular to the longitudinal direction L) are taken at five arbitrarily selected locations, as shown by dotted lines, from one end to the other in the longitudinal direction L of the fibers of the unidirectional fiber aggregate, using X-ray CT to capture cross-sectional photographs so as to include a 2 mm-wide liquid crystal polyester fiber-containing layer. In the cross-sectional photographs taken with X-ray CT, the boundaries of each layer (for example, the boundaries between the liquid crystal polyester fiber-containing layer and the reinforcing fiber-containing layer) can be visually identified.
[0083] For reference, FIG. 3 shows an enlarged cross-sectional photograph of a selected measurement point in the fiber-resin composite obtained in Example 1. In the photograph in FIG. 3 , two liquid crystal polyester fiber-containing layers are disposed above and below the reinforcing fiber-containing layer 11 in the thickness direction T of the fiber-resin composite 10, as an upper layer 121 and a lower layer 122. First, for each liquid crystal polyester fiber-containing layer 121, 122, the liquid crystal polyester fiber-containing layer is divided into 20 equal parts every 100 μm in the width direction W from one end to the other end of an arbitrarily selected 2 mm width. Next, 21 lines are drawn in the thickness direction of the liquid crystal polyester fiber-containing layer at 21 points, including both ends. However, for either end, the end most suitable for measurement is used, and the thickness of the liquid crystal polyester fiber-containing layer is actually measured at 20 points.
[0084] When the total number of data points at all measurement points is N, the coverage ratio is calculated by the following formula, where n is the total number of data points at which the liquid crystal polyester fiber is not present among the measurement points: Coverage ratio (%) = [(N-n) / N] x 100
[0085] Furthermore, the average and standard deviation of the thickness at each measurement point are determined to be the thickness of the liquid crystalline polyester fiber in the liquid crystalline polyester fiber-containing layer (cover thickness) and the cover thickness variation. More specifically, the cover thickness and the cover thickness variation are values measured by the method described in the Examples below.
[0086] In the fiber-resin composite, the liquid crystalline polyester fiber-containing layer may have a cover thickness coefficient of variation of 0.33 or less, preferably 0.28 or less, and more preferably 0.25 or less. The coefficient of variation can be calculated by dividing the cover thickness variation by the cover thickness.
[0087] The fiber resin composite has a basis weight of, for example, 200 g / m 2 or more, preferably 500 g / m 2 More preferably, 700 g / m 2 For example, it may be 20,000 g / m or more. 2 or less, preferably 18000 g / m 2 or less, more preferably 15000 g / m 2 The fiber-resin composite may have a basis weight of, for example, 200 to 20,000 g / m 2 and preferably 500 to 18,000 g / m 2 , more preferably 700 to 15,000 g / m 2 may be.
[0088] The total basis weight of the unidirectional fiber aggregate of the liquid crystal polyester fiber in the fiber resin composite is, for example, 60 g / m from the viewpoint of vibration damping performance. 2 or more, preferably 80 g / m 2 More preferably, 100 g / m 2 For example, it may be 1000 g / m or more. 2 or less, preferably 800 g / m 2 or less, more preferably 500 g / m 2 The total basis weight of the unidirectional fiber aggregate in the fiber-resin composite may be, for example, 60 to 1000 g / m 2 and preferably 80 to 800 g / m 2 , more preferably 100 to 500 g / m 2 may be.
[0089] When a fiber resin composite has multiple liquid crystal polyester fiber-containing layers, for example, when a reinforcing fiber-containing layer is sandwiched between liquid crystal polyester fiber-containing layers, such as liquid crystal polyester fiber-containing layers 121 and 122, the interlayer distance between these liquid crystal polyester fiber-containing layers may be, for example, less than 50 μm, preferably less than 25 μm, and more preferably less than 10 μm, from the viewpoints of vibration damping performance and thinning.
[0090] The fiber-resin composite of the present invention has excellent vibration damping performance because it includes a liquid crystal polyester fiber-containing layer with a high coverage. The content (wt%) of the liquid crystal polyester fiber-containing layer in the fiber-resin composite is preferably 5 wt% or more, more preferably 10 wt% or more, and even more preferably 15 wt% or more. The upper limit is not particularly limited, but may be 90 wt% or less, 80 wt% or less, 70 wt% or less, 60 wt% or less, or 50 wt% or less.
[0091] The fiber resin composite can reduce the anisotropy of vibration damping performance. For example, when a vibration damping performance test is performed on a fiber resin composite, using a 15 mm wide × 200 mm long test piece (0 degrees) whose length direction is the parallel alignment direction of the liquid crystal polyester fibers in the fiber resin composite, and a 15 mm wide × 200 mm long test piece (90 degrees) whose length direction is perpendicular to the parallel alignment direction of the liquid crystal polyester fibers in the fiber resin composite, the anisotropy, expressed as the value obtained by dividing the vibration damping ratio of the test piece (0 degrees) by the vibration damping ratio of the test piece (90 degrees), may be, for example, 0.5 or more, preferably 0.6 or more, and may be, for example, 1.5 or less, preferably 1.3 or less, more preferably 1.1 or less, or may be 0.8 or less. The anisotropy, expressed by the value obtained by dividing the vibration damping ratio (0 degrees) of the test specimen by the vibration damping ratio (90 degrees) of the test specimen, may be, for example, 0.5 to 1.5, preferably 0.6 to 1.3, more preferably 0.6 to 1.1, and even more preferably 0.6 to 0.8. Furthermore, the vibration damping ratio (0 degrees) may be, for example, 0.5 or more, preferably 0.6 or more, and may be, for example, 1.5 or less, preferably 1.2 or less. The vibration damping ratio (0 degrees) may be, for example, 0.5 to 1.5, preferably 0.6 to 1.2. The vibration damping performance test is performed by the method described in the Examples below.
[0092] The fiber-resin composite may be used as a sheet or a tape. When the fiber-resin composite is used as a tape, the width of the fiber-resin composite may be, for example, 0.5 to 20 mm, preferably 0.8 to 10 mm, and more preferably 1 to 6 mm.
[0093] The thickness of the fiber resin composite can be appropriately selected depending on the application, but from the viewpoint of thinning, it may be, for example, 40 to 3500 μm, and preferably 50 to 3000 μm.
[0094] The total weight of the reinforcing fibers in the fiber resin composite is, for example, 500 g / m 2 or more, preferably 600 g / m 2More preferably, 700 g / m 2 More preferably, 800 g / m 2 For example, it may be 15,000 g / m or more. 2 or less, preferably 13,000 g / m 2 or less, more preferably 10,000 g / m 2 More preferably, 3000 g / m or less 2 The total weight of the reinforcing fibers in the fiber-resin composite may be, for example, 500 to 15,000 g / m 2 and preferably 600 to 13,000 g / m 2 , more preferably 700 to 10,000 g / m 2 , more preferably 800 to 3000 g / m 2 may be.
[0095] The total basis weight of the reinforcing fiber-containing layer in the fiber resin composite is, for example, 500 g / m 2 or more, preferably 800 g / m 2 More preferably, 1000 g / m 2 For example, it may be 15,000 g / m or more. 2 or less, preferably 13,000 g / m 2 or less, more preferably 10,000 g / m 2 More preferably, 4000 g / m or less 2 The total weight of the reinforcing fibers in the fiber-resin composite may be, for example, 500 to 15,000 g / m 2 and preferably 800 to 13,000 g / m 2 , more preferably 1000 to 10000 g / m 2 , more preferably 1000 to 4000 g / m 2 Here, the total basis weight of the reinforcing fiber-containing layer is the value of the total amount when a plurality of reinforcing fiber-containing layers are present in the fiber-resin composite. When obtaining the basis weight of the reinforcing fiber-containing layer from the fiber-resin composite, the reinforcing fiber-containing layer can be cut out for each layer from the fiber-resin composite and calculated as the sum of the basis weights of the cut-out reinforcing fiber-containing layers.
[0096] The toughness of the fiber-resin composite may be, for example, 4.5 or more, preferably 5.0 or more, and more preferably 5.1 or more. The upper limit is not particularly limited, but may be, for example, 8.0 or less. The toughness of the fiber-resin composite is a value measured by the method described in the examples below.
[0097] The shape of the fiber-resin composite may be a planar shape (plate-like) or a three-dimensional shape. The three-dimensional shape is not particularly limited, and may be, for example, a cylindrical shape, a columnar shape, or a curved shape. The fiber-resin composite may also have a functional layer on at least one outermost surface. The functional layer is a layer formed for the purpose of improving design, UV protection, etc., and examples thereof include a coating layer and an ultraviolet protection layer. These coating layers and ultraviolet protection layers can be made of known materials.
[0098] For example, Fig. 4 is a schematic cross-sectional view illustrating a rod-shaped fiber resin composite according to one embodiment of the present invention. The rod-shaped fiber resin composite 20 has one liquid crystal polyester fiber-containing layer 221 arranged around the circumference and a reinforcing fiber-containing layer 22 arranged inside the liquid crystal polyester fiber-containing layer 221. In Fig. 4, the portion 212 is hollow. As shown in Fig. 4, a preferred embodiment has at least one liquid crystal polyester fiber-containing layer located outside the reinforcing fiber-containing layer. Another preferred embodiment has a liquid crystal polyester fiber-containing layer as the outermost layer.
[0099] 5 is a schematic cross-sectional view illustrating a plate-shaped fiber resin composite according to another embodiment. The plate-shaped fiber resin composite 30 includes a liquid crystal polyester fiber-containing layer 311 disposed as one outermost layer, a liquid crystal polyester fiber-containing layer 313 disposed as the other outermost layer, and a reinforcing fiber-containing layer 312 sandwiched between the two liquid crystal polyester fiber-containing layers 311 and 313. As shown in FIG. 5 , a preferred embodiment has at least one liquid crystal polyester fiber-containing layer located outside the reinforcing fiber-containing layer. Another preferred embodiment has a plate-shaped structure in which at least one outermost layer is a liquid crystal polyester fiber-containing layer, and both outermost layers may be liquid crystal polyester-containing layers.
[0100] (Vibration-damping molded article) The vibration-damping molded article may be a molded article formed solely from a fiber-resin composite, or may be a molded article composed of a fiber-resin composite and other components. It may also be a molded article formed solely from a unidirectional material, or may be a molded article formed from a unidirectional material and other components. In either case, the vibration-damping molded article has vibration-damping properties derived from the fiber-resin composite. Here, vibration-damping properties mean a reduction in the amplitude of vibration.
[0101] The molded article may be produced by bonding the fiber-resin composite and other components with a bonding material such as an adhesive, or by integrating the uncured fiber-resin composite and other components by heat treatment and / or pressure bonding, to produce a molded article composed of the fiber-resin composite and other components.
[0102] Other materials used in the vibration-damping molded article can be appropriately selected depending on the application, and examples include materials formed from various plastics, metals, wood, rubber (natural rubber, silicone rubber, etc.), leather, artificial leather, fabrics (woven or knitted fabrics, nonwoven fabrics), paper, etc. These may be used alone or in combination of two or more.
[0103] Examples of vibration-damping molded articles include bicycle frame shapes (e.g., cylindrical shapes), interior panels for vehicles such as automobiles, trains, and airplanes, housings for household electrical appliances such as hair dryers, refrigerators, and microwave ovens, and long objects such as golf clubs and fishing rods.
[0104] In the vibration-damping molded article, the liquid crystal polyester fiber-containing layer can damp vibration. The liquid crystal polyester fiber-containing layer can be appropriately disposed depending on the source of vibration. For example, in the case of a long object, when one end serves as the vibration source, the liquid crystal polyester fiber-containing layer may be disposed at a predetermined distance from the vibration source in the longitudinal direction (for example, 0 to 100 cm, preferably 30 to 100 cm, more preferably 50 to 100 cm).
[0105] Furthermore, for example, when the vibration source is external, the vibration received through the air may be used as the vibration source, and the liquid crystal polyester fiber-containing layer may be arranged within a predetermined distance (for example, 5 mm or less, preferably 1 mm or less, more preferably 0.5 mm or less) from the outermost layer. The vibration-damping molded article may also have a functional layer on the outermost surface. The functional layer is a layer formed for the purpose of improving design and UV protection, and examples thereof include a coating layer and an UV protection layer. These coating layers and UV protection layers can be made of known materials.
[0106] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0107] [Example 1] (Production of unidirectional material) Liquid crystal polyester fiber (LCP fiber) Vectran HT1670 dtex (single yarn fineness 5.6 dtex) manufactured by Kuraray Co., Ltd. was twisted and oiled, and yarns with a twist of 1.16 T / m were aligned in one direction to a pick count of 12.2 threads / inch to form a unidirectional fiber assembly. Next, a mixture of epoxy resin and curing agent was applied to release paper using a coater to obtain a resin sheet. The obtained resin sheet was placed on and bonded to a unidirectional fiber assembly of liquid crystal polyester fiber to produce a semi-cured unidirectional material. The basis weight of the liquid crystal polyester fiber (unidirectional fiber assembly) in this unidirectional material was 80 g / m. 2 It was.
[0108] (Production of Composite) Two pieces of 200 mm x 200 mm were cut out from this unidirectional material and laminated onto a commercially available reinforcing fiber sheet (carbon fiber prepreg "Pyrofil" manufactured by Mitsubishi Chemical Corporation, product name: TR350C075S (unidirectional prepreg), single fiber fineness 0.7 dtex, reinforcing fiber basis weight 75 g / m 2Thirteen sheets of the liquid crystal polyester fiber (polymer: acrylic resin, matrix resin: high-toughness epoxy) were stacked with the fiber longitudinal direction aligned, and two of the cut-out pieces were sandwiched with the fiber longitudinal direction aligned, forming a sandwich. This stack was sandwiched between a pair of release sheets and pressed in a vacuum press molding machine at a temperature of 130°C and a pressure of 2 MPa for 1 hour to cure the thermosetting resin and produce a fiber-resin composite. The basis weight of the liquid crystal polyester fiber in the composite was 160 g / m 2 It was.
[0109] [Example 2] A composite was produced and evaluated in the same manner as in Example 1, except that the number of unidirectional materials was changed to four, the number of reinforcing fiber sheets was changed to 11, and the composite was produced by sandwiching the 11 stacked reinforcing fiber sheets between two unidirectional materials.
[0110] [Example 3] A composite was produced and evaluated in the same manner as in Example 1, except that Vectran HT560 dtex (single yarn fineness 5.6 dtex) manufactured by Kuraray Co., Ltd. was used as the liquid crystal polyester fiber, twisted, and oiled, and then arranged so that yarns with a twist number of 5.32 T / m were arranged at 36.6 strands per inch, and then bonded to an epoxy resin sheet to produce a unidirectional material.
[0111] Example 4 A composite can also be produced in the same manner as in Example 1 using a unidirectional material prepared by twisting Vectran HT560 dtex (single yarn fineness 5.6 dtex) manufactured by Kuraray Co., Ltd. as a liquid crystal polyester fiber, applying an oil, arranging yarns with a twist number of 5.32 T / m at 36.6 strands per inch, and applying polycarbonate resin to the material to form a sheet.
[0112] [Comparative Example 1] A composite was produced and evaluated in the same manner as in Example 1, except that Vectran HT1670 dtex (single yarn fineness: 5.6 dtex) manufactured by Kuraray Co., Ltd. was used as the liquid crystal polyester fiber, which was twisted and coated with an oil, and a unidirectional material was produced using a yarn with a twist number of 3.68 T / m.
[0113] [Comparative Example 2] A composite was produced and evaluated in the same manner as in Example 1, except that Vectran HT1670 dtex (single filament fineness: 5.6 dtex) manufactured by Kuraray Co., Ltd. was used as the liquid crystal polyester fiber, which was twisted, oiled, and arranged so that the number of threads per inch was 6.4, and then laminated with an epoxy resin sheet to produce a unidirectional material.
[0114] [Comparative Example 3] A composite was produced and evaluated in the same manner as in Example 3, except that Vectran HT560 dtex (single filament fineness 5.6 dtex) manufactured by Kuraray Co., Ltd. was used as the liquid crystal polyester fiber, which was twisted, oiled, and arranged so that the number of threads per inch was 12.2, and then laminated with an epoxy resin sheet to produce a unidirectional material.
[0115] Comparative Example 4 A composite was produced and evaluated in the same manner as in Example 1, except that instead of the liquid crystal polyester fiber, Kevlar (registered trademark) 1670 dtex (single yarn fineness 1.7 dtex) manufactured by DuPont-Toray Co., Ltd. was used as an aramid fiber, which was twisted and oiled to produce a unidirectional material using a yarn with a twist number of 0.84 T / m.
[0116] Various physical properties of the obtained fiber resin composites are shown in Table 5. In the above examples and comparative examples, various physical properties were measured by the following methods.
[0117] [Fineness (dtex)] The yarn fineness was measured based on JIS L 1013:2021. The single yarn fineness was calculated by dividing the yarn fineness by the number of filaments constituting the yarn. The yarn fineness (total fineness) may be measured by disassembling the fiber aggregate constituting the fiber-resin composite and obtaining the yarns constituting the fiber aggregate.
[0118] [Number of twists (T / m)] Using a three-core twist detector ST0125 manufactured by Matsui Seiki Seisakusho, the number of twists of 50 cm of fiber was measured 10 times under a load of 0.03 g / dtex, and the average value was converted to the number of twists per meter to calculate the twist.
[0119] [Weight (g / m) of fiber (fiber aggregate) in unidirectional material 2) ] Maintaining the pick count per width used for unidirectional materials, the vibration-damping fibers were aligned in a 50 cm width, and a 2 m length was sampled. The bone-dry mass after 105°C x 4 hours was measured and calculated. Note that liquid crystal polyester fiber (LCP fiber) was used as the vibration-damping fiber in Examples 1 to 3 and Comparative Examples 1 to 3, and aramid fiber was used in Comparative Example 4. The same applies to the following descriptions.
[0120] [Unidirectional material, reinforced fiber sheet basis weight (g / m 2 For the unidirectional material and the reinforcing fiber sheet, two 25 cm x 25 cm test pieces were taken, and the bone dry masses were measured after 4 hours at 105°C, and the mass was calculated from the average of the two pieces.
[0121] [Thickness of Reinforced Fiber Sheet] The thickness of the reinforcing fiber sheet constituting the fiber resin composite was measured using a thickness measuring device according to JIS L 1096:2010 Method A.
[0122] [Total basis weight of vibration-damping fiber-containing layer, reinforcing fiber-containing layer, basis weight of fiber-resin composite (g / m 2 ) was calculated by multiplying the basis weight of the unidirectional material or reinforcing fiber sheet by the number of layers. The basis weight of the fiber-resin composite was calculated as the sum of the total basis weight of the vibration-damping fiber-containing layer and the total basis weight of the reinforcing fiber-containing layer.
[0123] [Content (wt %) of vibration-damping fiber-containing layer in fiber-resin composite] Calculated by the formula (total basis weight of vibration-damping fiber-containing layer) / (basis weight of fiber-resin composite).
[0124] [Cross-section imaging conditions] The coverage rate and cover thickness of the vibration-damping fiber were determined by analysis using images captured using the following device and imaging conditions using a fiber-resin composite. Device: Carl Zeiss X-ray CT "Xradia 520 Versa." The sample was directly fixed to a jig and imaged using the X-ray CT. The imaging direction was a slice image output in the width direction perpendicular to the fiber alignment direction of the unidirectional material. The imaging conditions were a radiation source intensity of 80 kV, output of 7 W, and pixel size of 3.0 μm, and 3,201 images were captured. For the following image analysis, five images were arbitrarily selected from the images obtained (images including a 2 mm-wide vibration-damping fiber-containing layer) and image analysis was performed.
[0125] [Cover Thickness (mm), Coverage (%)] Five randomly selected photographs were each divided into 20 equal parts, from one end to the other of a 2 mm width, and one of the 21 measurement points, including both ends, was excluded. The thickness of the liquid crystal polyester fiber (cover thickness) was measured at each of the 20 measurement points. Regarding the exclusion of the end, any end that was difficult to measure due to a lack of field of view or the like was preferentially excluded. If neither end was eligible for exclusion, one of the ends was selected. In the Examples and Comparative Examples, since there were two vibration-damping fiber-containing layers (two rows), the presence or absence of liquid crystal polyester fiber was visually confirmed and the thickness was measured at a total of 40 points in each layer (row) in five photographs. The percentage of the total number n of data points where liquid crystal polyester fiber was not present out of a total of 200 points was used as the coverage, and was calculated using the following formula: [Coverage (%)] = ([200 - n] / 200) x 100
[0126] [Average Cover Thickness and Coefficient of Variation] The average and standard deviation of the cover thickness measured at a total of 200 points by the above method were determined, and the coefficient of variation was calculated by dividing the standard deviation by the average.
[0127] [Thickness of Composite] The thickness of the composite was measured with a micrometer in accordance with JIS K 7074: 1988. The average value of measurements at five points was taken as the thickness of the composite.
[0128] [Toughness of Composite] The toughness of the composite was calculated by measuring the maximum strength (GPa) and maximum strain (%) of a test piece having a length of 100 mm and a width of 15 mm, with the length direction being the parallel direction of the vibration-damping fibers, using a three-point bending jig at a support distance of 40 mm and a speed of 5 mm / min, in accordance with JIS K 7074:1988, and then calculating the product of these values.
[0129] [Vibration Damping Performance] The fiber-resin composites obtained in the Examples and Comparative Examples were cut with a common water jet cutter to obtain test pieces 15 mm wide x 200 mm long (0°) in the direction parallel to the paralleling direction of the vibration-damping fibers, and test pieces 15 mm wide x 200 mm long (90°) in the direction perpendicular to the paralleling direction. The tip of an edge knife was fixed to the center of the test piece in the longitudinal direction with instant adhesive, and the edge knife was fixed to the impedance head of a center-support standing wave excitation device.
[0130] The centrally supported standing wave excitation apparatus was placed in a thermostatic chamber (KATO, SP-43CI-A), and the vibration damping ratio was measured at 20°C. The centrally supported standing wave excitation apparatus consisted of the following equipment: Thermometer: ND500 (CHINO) FFT analyzer: CF-52202 (ONO SOKKI) Power amplifier: 371-A (EMIC) Exciter: 512-A (EMIC) Amplifier: 2692-OS2 (Bruel & Kjaer) Impedance head: 8001 (Bruel & Kjaer)
[0131] [Anisotropy] The vibration damping ratio of the test piece (0 degrees) divided by the vibration damping ratio of the test piece (90 degrees) was calculated and used as an index of the anisotropy of the vibration damping ratio. The closer the divided value is to 1, the smaller the anisotropy.
[0132] [Handling of Unidirectional Material] When the matrix resin is a thermosetting resin, the unidirectional material was temporarily stored in a freezer, then removed from the freezer and returned to room temperature, after which 200 mm x 200 mm cut-out pieces were obtained. Pieces that could be removed cleanly without cracking or other defects when peeled from the release paper were rated A, and pieces that were torn and difficult to stack were rated B. When the matrix resin is a thermoplastic resin, the unidirectional material was pre-molded into a sheet by impregnating or applying the matrix resin to a unidirectional fiber aggregate, and the presence or absence of fiber disorder in the unidirectional fiber aggregate was measured to evaluate the handleability of the unidirectional material.
[0133] The physical properties of the resulting fiber-resin composite are shown in Table 5.
[0134] As shown in Table 5, in all of Examples 1 to 3, the coverage of the liquid crystal polyester fiber (vibration-damping fiber) in the unidirectional material or liquid crystal polyester fiber-containing layer (vibration-damping fiber-containing layer) was high and the coefficient of variation of the cover thickness was small. Therefore, despite the high monofilament fineness of the liquid crystal polyester fiber, the unidirectional material or liquid crystal polyester fiber-containing layer covered with the liquid crystal polyester fiber at a uniform thickness not only achieved high vibration-damping performance of the fiber-resin composite, but also suppressed its anisotropy. Furthermore, the unidirectional material was easy to handle, and cracks were not generated due to gaps between the fibers of the unidirectional fiber aggregate. As a result, the generation of gaps between the fibers in the fiber-resin composite was suppressed. Furthermore, the toughness, which is related to bending properties, also showed a value of 5.0 or higher. Comparing Examples 1 and 3 with Comparative Example 1, Examples 1 and 3, which had a smaller coefficient of variation of the cover thickness, achieved improved toughness.
[0135] On the other hand, in Comparative Example 1, although the cover rate was high, the coefficient of variation of the cover thickness was high, so that when the unidirectional material was handled, cracks occurred due to gaps between the fibers of the unidirectional fiber aggregate, and as a result, it was not possible to prevent gaps from occurring between the fibers in the fiber-resin composite. Furthermore, in Comparative Examples 2 and 3, the cover rate was insufficient, and in Comparative Example 3, the coefficient of variation of the cover thickness was also high, so the vibration damping performance was poor in the 0-degree direction, resulting in anisotropy. Furthermore, when the unidirectional material was handled, cracks occurred due to gaps between the fibers of the unidirectional fiber aggregate, and as a result, it was not possible to prevent gaps from occurring between the fibers in the fiber-resin composite.
[0136] In Comparative Example 4, in which aramid fiber with a small single fiber fineness was used instead of the liquid crystal polyester fiber, the variation coefficient of the cover ratio and cover thickness was poor, but cracks did not occur in the unidirectional material, probably because of the small single fiber fineness. However, the vibration damping performance was poor in the 0-degree direction, resulting in anisotropy. In addition, all of the Comparative Examples had inferior toughness compared to the Examples, with values of less than 5.0.
[0137] The fiber-resin composite of the present invention can be suitably used in various applications requiring vibration damping performance, for example, as housings for transportation machinery such as automobiles, trains, ships, and aircraft; sporting goods such as bats, tennis rackets, badminton rackets, golf clubs, and fishing rods; audio equipment such as headphone stereos and music players; and household electrical appliances such as hair dryers, refrigerators, and microwave ovens.
[0138] As described above, the preferred embodiment of the present invention has been described, but various additions, modifications, or deletions can be made without departing from the spirit of the present invention, and such additions, modifications, or deletions are also included within the scope of the present invention.
[0139] DESCRIPTION OF SYMBOLS 10, 20, 30... Fiber resin composite 11, 22, 312... Reinforced fiber-containing layer 11a, 11b, 11c, 11d... Reinforced fiber sheet 121, 122, 221, 311, 313... Liquid crystal polyester fiber-containing layer 121a, 121b, 122a, 122b... Unidirectional material 200... Unidirectional fiber aggregate 300... Reinforced fiber aggregate L... Longitudinal direction W... Width direction T... Thickness direction
Claims
1. A fiber resin composite comprising: a liquid crystal polyester fiber-containing layer containing a unidirectional fiber aggregate of liquid crystal polyester fibers and a matrix resin; and a reinforcing fiber-containing layer containing reinforcing fibers and a matrix resin, wherein the matrix resin of the liquid crystal polyester fiber-containing layer is a hard resin, the single yarn fineness of the liquid crystal polyester fiber in the liquid crystal polyester fiber-containing layer is 2.5 dtex or more, the coverage rate of the liquid crystal polyester fiber in the liquid crystal polyester fiber-containing layer is 91% or more, and the variation coefficient of the cover thickness of the liquid crystal polyester fiber in the liquid crystal polyester fiber-containing layer is 0.33 or less.
2. The fiber resin composite according to claim 1, wherein the weight of the liquid crystal polyester fiber-containing layer per unit area is 800 g / m 2 The following is a fiber resin composite:
3. A fiber resin composite according to claim 1, wherein the liquid crystal polyester fiber has a single filament fineness of 5.0 dtex or more.
4. A fiber-resin composite according to claim 1, in which the matrix resin of the reinforcing fiber-containing layer is a hard resin.
5. The fiber resin composite according to claim 1, wherein the basis weight of the unidirectional fiber aggregate in a single layer containing liquid crystal polyester fiber is 700 g / m 2 The following is a fiber resin composite:
6. A fiber-resin composite according to claim 1, in which the twist number of the liquid crystal polyester fiber is 100 T / m or less.
7. A fiber-resin composite according to claim 1, which is in the form of a tape.
8. A unidirectional material comprising a unidirectional fiber aggregate of liquid crystal polyester fibers and a matrix resin, wherein the matrix resin is a hard resin, the single fiber fineness of the liquid crystal polyester fibers is 2.5 dtex or more, the coverage rate of the liquid crystal polyester fibers in the unidirectional material is 91% or more, and the coefficient of variation of the thickness of the liquid crystal polyester fibers in the unidirectional material is 0.33 or less.
9. The unidirectional material according to claim 8, wherein the liquid crystal polyester fiber has a single filament fineness of 5.0 dtex or more.
10. The unidirectional material according to claim 8, wherein the basis weight of the unidirectional fiber aggregate in the unidirectional material is 300 g / m 2 The following is a unidirectional material.
11. A unidirectional material as described in claim 8, wherein the total fineness of the liquid crystal polyester fibers is 1,000 dtex or more, and the relationship among the total fineness A (dtex), the number of fibers per inch (B), and the number of twists C (T / m) of the liquid crystal polyester fibers constituting the unidirectional fiber assembly is 10,000 or more as a value of A x B ÷ C.
12. A unidirectional material as described in claim 8, wherein the total fineness of the liquid crystal polyester fibers is less than 1000 dtex, and the relationship among the total fineness A (dtex), the number of fibers per inch (B) and the number of twists C (T / m) of the liquid crystal polyester fibers constituting the unidirectional fiber assembly is 2000 or more as the value of A×B÷C.
13. The unidirectional material according to claim 8, having a basis weight of 350 g / m 2 The following is a unidirectional material.
14. The unidirectional material according to claim 8, wherein the twist number of the liquid crystal polyester fiber is 100 T / m or less.
15. A vibration-damping molded article comprising the fiber-resin composite according to any one of claims 1 to 7 or the unidirectional material according to any one of claims 8 to 14.
16. A method for producing a fiber-resin composite, comprising overlapping and integrally molding the unidirectional material according to any one of claims 8 to 14 with a reinforcing fiber sheet containing reinforcing fibers and a matrix resin.
Citation Information
Patent Citations
Sheet material for manufacturing vibration damping member, vibration damping member using said sheet material, and manufacturing method thereof
JP6499029B2
Fiber-reinforced resin material and method for producing the same
JP2014083836A
Fiber-reinforced composite material
WO2015151919A1
Filamentary tape and composite material including said tape
WO2019156033A1
Conductive yarn and article having wiring line that is formed of conductive yarn
WO2021215190A1
Cited By
High-tensile-strength polyester base cloth and preparation method thereof
CN119932809A