Resin composition
The resin composition, featuring a block copolymer and cyclic ester compound, addresses the limitations of polylactic acid by enhancing crystallinity and heat resistance while maintaining transparency, offering a balanced performance in biodegradability and mechanical properties.
Patent Information
- Application Number
- PCT/JP2024/019967
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-02
- Filing Date
- 2024-05-31
- Publication Date
- 2024-12-05
AI Technical Summary
Polylactic acid, a bioplastic, exhibits limitations such as brittleness, inferior viscosity, flexibility, impact resistance, and heat resistance, making it less suitable for various applications, and existing techniques to improve these drawbacks do not fully satisfy the need for a material with excellent biodegradability, heat resistance, and transparency.
A resin composition comprising a block copolymer with polylactic acid units and a cyclic ester compound, where the block copolymer is derived from aliphatic diol and dicarboxylic acid, and the cyclic ester compound is used in specific concentrations to enhance crystallinity, tensile properties, and heat resistance while maintaining transparency.
The resin composition achieves an excellent balance of biodegradability, crystallinity, tensile properties, and heat resistance, providing a material suitable for a wide range of applications with improved performance over traditional polylactic acid.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
resin composition
[0001] The present invention relates to a resin composition that suppresses deterioration in tensile properties and transparency, improves crystallinity and melting point, and has excellent heat resistance. The present invention also relates to a resin composition that has an excellent balance of biodegradability, heat resistance, and transparency.
[0002] From the perspective of environmental protection, bioplastics are being actively developed. Polylactic acid, a bioplastic, is made from renewable plant-derived resources such as corn, produced by photosynthesis, and is expected to be used in a wide range of fields. However, polylactic acid is known to be brittle compared to petroleum-based plastics, inferior in viscosity, flexibility, impact resistance, and heat resistance, and is also prone to hydrolysis. This limits its use as a resin material. Attempts to overcome the drawbacks of polylactic acid have been investigated, for example, by using specific plasticizers or nucleating agents (see, for example, Patent Document 1). Another technique involves copolymerizing polylactic acid with polyesters using monomers with specific carbon numbers (see, for example, Patent Document 2). Another technique involves using specific plasticizers or nucleating agents (see, for example, Patent Document 3). Another technique involves using a composition of polylactic acid and a block copolymer obtained by copolymerizing a specific polyester with polylactic acid (see, for example, Patent Document 4).
[0003] JP 2015-044984 A JP 8-157577 A JP 2018-62573 A JP 2001-335623 A
[0004] Although the techniques described in Patent Documents 1 to 4 have improved the drawbacks of polylactic acid to some extent, they have not been fully satisfactory. In particular, from the viewpoint of versatility, final products made from bioplastic materials are desired to have excellent heat resistance while maintaining biodegradability under a wide range of conditions, or to have excellent impact resistance, heat resistance, and transparency while maintaining biodegradability. However, when the crystallinity of polylactic acid is increased in order to improve heat resistance, the tensile properties and transparency tend to decrease.
[0005] Therefore, an object of the present invention is to provide a resin composition that has biodegradability over a wide range of conditions and an excellent balance of crystallinity, tensile properties, transparency, and heat resistance. Another object of the present invention is to provide a resin composition that has an excellent balance of biodegradability, heat resistance, and transparency.
[0006] As a result of intensive research to solve the above problems, the present inventors have conceived the following invention and found that the above problems can be solved.
[0007] [1] A resin composition containing a block copolymer (I) and a cyclic ester compound (II), wherein the block copolymer (I) comprises block structural units (A) mainly composed of polylactic acid units (a) and block structural units (B) mainly composed of polyester units (b) containing units derived from an aliphatic diol (b1) and an aliphatic dicarboxylic acid (b2), and the content of the cyclic ester compound (II) is 0.01 to 15 mass% relative to 100 mass% of the total of the block copolymer (I) and the cyclic ester compound (II). [2] The resin composition according to [1] above, wherein the cyclic ester compound (II) comprises a structure derived from an aliphatic diol (c1) and an aliphatic dicarboxylic acid (c2). [3] The resin composition according to [2] above, wherein the aliphatic diol (c1) and the aliphatic diol (b1) are the same, and the aliphatic dicarboxylic acid (c2) and the aliphatic dicarboxylic acid (b2) are the same. [4] The resin composition according to any one of [1] to [3] above, wherein the aliphatic diol (b1) is an aliphatic diol having 4 or more carbon atoms and an alkyl group as a branched chain. [5] The resin composition according to any one of [1] to [4] above, wherein the block copolymer (I) has a number average molecular weight of 2,000 to 200,000. [6] The resin composition according to any one of [1] to [5] above, wherein the block structural unit (B) has a number average molecular weight of less than 80,000. [7] The resin composition according to any one of [1] to [6] above, wherein the aliphatic dicarboxylic acid (b2) has 4 or more and 12 or less carbon atoms. [8] The resin composition according to any one of [1] to [7] above, wherein the aliphatic diol (b1) has 9 or less carbon atoms. [9] The resin composition according to any one of [1] to [8] above, wherein the branched chain in the aliphatic diol (b1) is a methyl group.
[10] The resin composition according to any one of [1] to [9] above, having a melting point of 110° C. or higher and lower than 180° C.
[11] The resin composition according to any one of [1] to
[10] above, further comprising an aliphatic polyester-based resin (III), wherein the content of the cyclic ester compound (II) is 0.005 to 10 mass% relative to 100 mass% in total of the block copolymer (I), the cyclic ester compound (II), and the aliphatic polyester-based resin (III).
[12] The resin composition according to
[11] above, wherein the aliphatic polyester resin (III) is at least one selected from the group consisting of biomass resins and biodegradable resins.
[13] The resin composition according to
[11] or
[12] above, wherein the aliphatic polyester resin (III) is a polylactic acid resin.
[14] The resin composition according to any one of [1] to [4] and [6] to
[13] above, wherein the block copolymer (I) has a number-average molecular weight of 5,000 to 400,000.
[15] The resin composition according to any one of [1] to [5] and [7] to
[14] above, wherein the block structural unit (B) has a number-average molecular weight of 1,000 or more but less than 300,000.
[16] The resin composition according to any one of [1] to
[15] above, wherein the block copolymer (I) has a glass transition temperature of -80°C or more and 15°C or less.
[17] The resin composition according to any one of [1] to
[16] above, wherein the glass transition temperature of the block copolymer (I) is -80°C or higher and -45°C or lower.
[18] The resin composition according to any one of [1] to
[17] above, wherein the melting point of the block copolymer (I) is 110°C or higher and lower than 180°C.
[19] The resin composition according to any one of [1] to
[18] above, wherein the block structural unit (A) contains a structural unit derived from poly-L-lactic acid or a structural unit derived from poly-D-lactic acid.
[20] The resin composition according to any one of [1] to
[19] above, wherein the block structural unit (A) accounts for 5% by mass or higher and 95% by mass or lower, relative to 100% by mass of the total of the block structural units (A) and the block structural units (B).
[0008] According to the present invention, it is possible to provide a resin composition that has biodegradability over a wide range of conditions and an excellent balance of crystallinity, tensile properties, transparency, and heat resistance. Also, according to the present invention, it is possible to provide a resin composition that has an excellent balance of biodegradability, heat resistance, and transparency.
[0009] The following describes an embodiment of the present invention. However, the embodiment described below is merely an example for embodying the technical concept of the present invention, and the present invention is not limited to the following description. Furthermore, although preferred embodiments are shown in this specification, a combination of two or more of the individual preferred embodiments is also a preferred embodiment. For matters indicated as numerical ranges, when there are several numerical ranges, the lower and upper limits can be selectively combined to form a preferred embodiment. Note that, in this specification, a numerical range such as "XX to YY" means "XX or more and YY or less." In this specification, the term "~ unit" (where "~" indicates a polymer) means "a structural unit derived from ~." For example, "polylactic acid unit" means "a structural unit derived from polylactic acid," and "polyester unit" means "a structural unit derived from polyester." In this specification, "main chain" refers to the longest molecular chain in a molecule. Furthermore, "branched chain" refers to a molecular chain other than the main chain in a molecule. In this specification, "L-lactic acid unit" refers to a structural unit derived from L-lactic acid in the block structural unit (A). In addition, when the block structural unit (A) contains a structural unit derived from lactide and the structural unit derived from lactide contains a structural unit derived from L-lactic acid, the portion corresponding to the L-lactic acid is also included in the L-lactic acid unit. In this specification, "D-lactic acid unit" means a structural unit derived from D-lactic acid in the block structural unit (A). In addition, when the block structural unit (A) contains a structural unit derived from lactide and the structural unit derived from lactide contains a structural unit derived from D-lactic acid, the portion corresponding to the D-lactic acid is also included in the D-lactic acid unit. In this specification, "poly DL-lactic acid" means polylactic acid containing L-lactic acid units and D-lactic acid units. Examples of poly DL-lactic acid include block copolymers containing poly L-lactic acid blocks and poly D-lactic acid blocks, and random copolymers containing L-lactic acid units and D-lactic acid units randomly. In this specification, "DL-lactic acid" means a mixture of D-lactic acid and L-lactic acid. As used herein, "DL-lactide" refers to a mixture of D-lactide and L-lactide.As used herein, "meso-lactide" refers to lactide formed from one unit each of D-lactic acid and L-lactic acid. As used herein, "melting point" refers to the melting peak temperature, and when there are multiple melting peaks, refers to the melting peak temperature of the melting peak that is highest in the melting point range. The melting point can be determined using a differential scanning calorimeter, and specifically, can be measured by the method described in the Examples.
[0010] [Resin Composition] A resin composition according to a first embodiment of the present invention contains a block copolymer (I) and a cyclic ester compound (II). The block copolymer (I) contains block structural units (A) primarily composed of polylactic acid units (a) and block structural units (B) primarily composed of polyester units (b) derived from an aliphatic diol (b1) and an aliphatic dicarboxylic acid (b2). The resin composition contains 0.01 to 15% by mass of the cyclic ester compound (II) relative to 100% by mass of the total of the block copolymer (I) and the cyclic ester compound (II). The present inventors conducted extensive research into resin compositions that exhibit biodegradability over a wide range of conditions and an excellent balance of crystallinity, tensile properties, transparency, and heat resistance. As a result, the present inventors discovered that a resin composition containing a specific block copolymer (I) containing block structural units (A) and block structural units (B) and a specific amount of the cyclic ester compound (II) can satisfy the aforementioned characteristics.
[0011] The reason why the resin composition according to the first embodiment of the present invention has an excellent balance of crystallinity, tensile properties, transparency, and heat resistance is unclear and may be due to a combination of various factors, but is presumed to be as follows. Because the cyclic ester compound (II) contains an ester structure, it is highly compatible with the block copolymer (I) which also contains an ester structure. As a result, even when the crystallinity of the resin composition is improved, the deterioration of tensile properties and transparency is suppressed. Furthermore, because the cyclic ester compound (II) is cyclic, it has a low degree of molecular freedom and contributes to the effect of a crystal nucleating agent, i.e., to improving the crystallinity and melting point (improving heat resistance). For the above reasons, it is presumed that the resin composition according to the first embodiment has an excellent balance of crystallinity, tensile properties, transparency, and heat resistance.
[0012] A resin composition according to a second embodiment of the present invention is the resin composition according to the first embodiment, further comprising an aliphatic polyester resin (III), wherein the content of the cyclic ester compound (II) is 0.005 to 10 mass% relative to 100 mass% of the total of the block copolymer (I), the cyclic ester compound (II), and the aliphatic polyester resin (III). As a result of various studies, the present inventors have found that the resin composition according to the second embodiment, which contains a specific block copolymer (I), a specific amount of the cyclic ester compound (II), and the aliphatic polyester resin (III), has an excellent balance of biodegradability, heat resistance, and transparency.
[0013] The reason why the resin composition according to the second embodiment of the present invention has an excellent balance of biodegradability, heat resistance, and transparency is unclear and may be due to a combination of various factors, but is presumed to be as follows. Because the cyclic ester compound (II) contains an ester structure, it is highly compatible with the block copolymer (I) and aliphatic polyester resin (III) that also contain an ester structure. This prevents a decrease in transparency even when the crystallinity of the resin composition is improved. Furthermore, because the cyclic ester compound (II) is cyclic, it has a low degree of molecular freedom and thus contributes to the effect of a crystal nucleating agent, i.e., to improving the crystallinity and the glass transition temperature (improving heat resistance). For the above reasons, it is presumed that the resin composition according to the second embodiment has an excellent balance of biodegradability, heat resistance, and transparency.
[0014] <Block Copolymer (I)> The block copolymer (I) contains block structural units (A) mainly composed of polylactic acid units (a) and block structural units (B) mainly composed of polyester units (b) containing units derived from an aliphatic diol (b1) and an aliphatic dicarboxylic acid (b2).
[0015] <Block structural unit (A)> <Polylactic acid unit (a)> The block structural unit (A) is mainly composed of polylactic acid unit (a). The "main component" refers to the unit that is contained in the block structural unit (A) at the highest content ratio. The content ratio of polylactic acid unit (a) in the block structural unit (A) is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 85% by mass or more, and even more preferably 90% by mass or more, and may be 100% by mass. There is no upper limit to the amount of polylactic acid unit (a) contained in the block structural unit (A), and it may be, for example, 100% by mass or less.
[0016] The polylactic acid constituting the polylactic acid unit (a) may be prepared by direct condensation of lactic acid or by ring-opening polymerization of lactide. The lactic acid may be, for example, at least one selected from the group consisting of L-lactic acid, D-lactic acid, and DL-lactic acid. The lactide may be, for example, at least one selected from the group consisting of L-lactide, D-lactide, DL-lactide, and meso-lactide. Furthermore, the polylactic acid may be poly-L-lactic acid, poly-D-lactic acid, poly-DL-lactic acid, or an intramolecular stereocomplex or intermolecular stereocomplex polylactic acid obtained by mixing poly-L-lactic acid and poly-D-lactic acid. From the viewpoints of cost, availability of raw materials, and ease of handling of the block copolymer (I), poly-L-lactic acid, poly-D-lactic acid, and poly-DL-lactic acid are preferred, with poly-L-lactic acid and poly-D-lactic acid being more preferred. On the other hand, from the viewpoints of synthesis cost, complexity, and processability of the block copolymer (I), it is preferable that the polylactic acid is not an intramolecular stereocomplex polylactic acid or an intermolecular stereocomplex polylactic acid. From the viewpoint of even better biodegradability and hydrolysis resistance, it is preferable that the block structural units (A) contain structural units derived from poly-L-lactic acid or structural units derived from poly-D-lactic acid. Furthermore, from the viewpoint of even better biodegradability and hydrolysis resistance, the block structural units (A) preferably contain structural units derived from poly-L-lactic acid or structural units derived from poly-D-lactic acid in an amount of preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more. For example, in one preferred embodiment, the block structural units (A) are composed of structural units derived from poly-L-lactic acid or structural units derived from poly-D-lactic acid, i.e., the structural units derived from poly-L-lactic acid or structural units derived from poly-D-lactic acid account for 100% by mass.
[0017] <Units (a') Other than Polylactic Acid Units (a)> The block structural unit (A) may or may not contain units (a') other than the polylactic acid unit (a). The monomer constituting the unit (a') is not particularly limited as long as the effects of the present invention are not impaired, and examples thereof include an intermolecular cyclic ester and a lactone. Examples of α-hydroxycarboxylic acids that form intermolecular cyclic esters include glycolic acid, α-hydroxybutyric acid, α-hydroxyisobutyric acid, α-hydroxyvaleric acid, α-hydroxycaproic acid, α-hydroxyisocaproic acid, α-hydroxyheptanoic acid, α-hydroxyoctanoic acid, α-hydroxydecanoic acid, α-hydroxymyristic acid, α-hydroxystearic acid, and alkyl-substituted derivatives thereof. Examples of lactones include β-propiolactone, β-butyrolactone, pivalolactone, γ-butyrolactone, δ-valerolactone, β-methyl-δ-valerolactone, ε-caprolactone, etc. The content of units (a′) in the block structural units (A) is preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 15% by mass or less, and still more preferably 10% by mass or less.
[0018] <Number-Average Molecular Weight of Block Structural Unit (A)> The number-average molecular weight of the block structural unit (A) is not limited as long as the effects of the present invention are not impaired. On the other hand, from the viewpoints of productivity, biodegradability, mechanical properties, glass transition temperature, crystalline melting enthalpy, etc., the number-average molecular weight of the block structural unit (A) is preferably 500 or more, more preferably 1,000 or more, even more preferably 1,500 or more, still more preferably 3,000 or more, still more preferably 5,000 or more, still more preferably 10,000 or more, and preferably 200,000 or less, more preferably 150,000 or less, still more preferably 100,000 or less, still more preferably 50,000 or less, still more preferably 30,000 or less, still more preferably 20,000 or less. That is, the number average molecular weight of the block structural unit (A) is preferably 500 to 200,000, more preferably 1,000 to 150,000, even more preferably 1,500 to 100,000, even more preferably 3,000 to 50,000, even more preferably 5,000 to 30,000, even more preferably 5,000 to 20,000, and even more preferably 10,000 to 20,000. Within the above numerical range, productivity in synthesizing the block copolymer (I) is good. When the block copolymer (I) has multiple block structural units (A), the number average molecular weight of the block structural unit (A) refers to the sum of all blocks. The number average molecular weight of the block structural unit (A) can be determined from the number average molecular weight of the block copolymer (I) described below and the mass content of the block structural unit (A).
[0019] <Block Structural Unit (B)> The block structural unit (B) is mainly composed of polyester units (b). The term "main component" refers to the unit with the highest content among the units constituting the block structural unit (B). The content of polyester units (b) in the block structural unit (B) is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 85% by mass or more, and particularly preferably 90% by mass or more. It may even contain 100% by mass. There is no upper limit to the amount of polyester units (b) contained in the block structural unit (B), and it may be, for example, 100% by mass or less. The polyester units (b) contain units derived from an aliphatic diol (b1) and an aliphatic dicarboxylic acid (b2). Specifically, the polyester units (b) contain units derived from a polyester obtained by reacting an aliphatic diol (b1) with an aliphatic dicarboxylic acid (b2). The polyester unit (b) may or may not contain units derived from monomers other than the aliphatic diol (b1) and the aliphatic dicarboxylic acid (b2). The monomers other than the aliphatic diol (b1) and the aliphatic dicarboxylic acid (b2) are not particularly limited as long as they do not impair the effects of the present invention. The total amount of the aliphatic diol (b1) and the aliphatic dicarboxylic acid (b2) in the polyester unit (b) is preferably 90 mol% or more, more preferably 95 mol% or more, even more preferably 99 mol% or more, and may be 100 mol%.
[0020] <Aliphatic Diol (b1)> The number of carbon atoms in the aliphatic diol acid (b1) is not limited as long as the effects of the present invention are not impaired. The "number of carbon atoms" refers to the total number of carbon atoms in the aliphatic diol (b1), including the carbon atoms constituting the alkyl group. In the first embodiment of the present invention, from the viewpoints of monomer availability, hydrolysis resistance, biodegradability, and the like, the number of carbon atoms in the aliphatic diol (b1) is preferably 4 to 12, more preferably 5 to 10, even more preferably 6 to 9, and even more preferably 6. In the second embodiment of the present invention, from the viewpoint of exhibiting excellent impact resistance (particularly impact resistance at low temperatures), the number of carbon atoms is preferably 4 or more, more preferably 5 or more, and even more preferably 6 or more. In terms of exhibiting even better biodegradability, the number of carbon atoms is preferably 30 or less, more preferably 18 or less, and even more preferably 9 or less. That is, in the second embodiment of the present invention, the number of carbon atoms in the aliphatic diol (b1) is preferably 4 to 30, more preferably 5 to 18, and even more preferably 6 to 9.
[0021] When the aliphatic diol (b1) has an alkyl group as a branched chain, the block structural unit (B) becomes flexible, and the block copolymer (I) exhibits excellent tensile properties, biodegradability, and impact resistance, and has improved hydrolysis resistance. Therefore, the aliphatic diol (b1) preferably has an alkyl group as a branched chain, and more preferably is an aliphatic diol having 4 or more carbon atoms and an alkyl group as a branched chain. Here, the "branched chain" in the aliphatic diol (b1) refers to a partial structure branched from the "main chain" of the aliphatic diol (b1), and no hydroxyl group is bonded to its terminal.
[0022] Furthermore, when the aliphatic diol (b1) has an alkyl group as a branched chain, the block structural unit (B) is more likely to become an amorphous polymer. Therefore, when the block structural unit (B) biodegrades, microorganisms are more likely to penetrate into the polymer structure, which is thought to make it more biodegradable under a wide range of conditions. On the other hand, when the block structural unit (B) is not an amorphous polymer, it is thought that microorganisms are less likely to penetrate into the polymer structure during biodegradation. However, being an amorphous polymer is only one factor that affects biodegradability. This is because biodegradation and hydrolysis are thought to be caused by a combination of various factors, such as whether microorganisms recognize the amorphous structure as food, whether enzymes and microorganisms are easily accessible, steric hindrance of the main chain, melting point, and crystallinity. Therefore, a resin composition containing a block copolymer (I) containing an amorphous polymer does not necessarily have good biodegradability.
[0023] In the aliphatic diol (b1), the number of branched chains is preferably 1 or 2, more preferably 1. The branched chains are preferably methyl groups, ethyl groups, and propyl groups, more preferably methyl groups and ethyl groups, and even more preferably methyl groups. When the aliphatic diol (b1) has multiple branched chains, the respective branched chains may be the same or different. From the viewpoints of easy reaction with dicarboxylic acids, easy production of a triblock copolymer, and even more excellent biodegradability and hydrolysis resistance, the aliphatic diol (b1) preferably has hydroxyl groups at both ends of the main chain.
[0024] Examples of the aliphatic diol (b1) include 2-methyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 2-ethyl-1,3-propanediol, 2-ethyl-2-methyl-1,3-propanediol, 2-methyl-1,4-butanediol, 1,2-pentanediol, 1,3-pentanediol, 2,3-pentanediol, 2,4-pentanediol, 2-methyl-2,4-pentanediol, 1,4-pentanediol, and 2-methyl- Examples of the aliphatic diol (b1) include 1,5-pentanediol, 3-methyl-1,5-pentanediol, 2-methyl-2,4-pentanediol, 2-ethyl-1,5-pentanediol, 2,4-dimethyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 1,2-hexanediol, 1,3-hexanediol, 1,4-hexanediol, 1,5-hexanediol, 2-ethyl-1,6-hexanediol, and 2-methyl-1,8-octanediol. The aliphatic diol (b1) is preferably 2-methyl-1,3-propanediol, 3-methyl-1,5-pentanediol, or 2,4-diethyl-1,5-pentanediol, more preferably 3-methyl-1,5-pentanediol. One type of aliphatic diol (b1) may be used alone, or two or more types may be used in combination.
[0025] <Aliphatic Dicarboxylic Acid (b2)> The number of carbon atoms in the aliphatic dicarboxylic acid (b2) is not limited as long as the effects of the present invention are not impaired. Meanwhile, in the first embodiment of the present invention, from the viewpoints of productivity, hydrolysis resistance, biodegradability, and the like, the number of carbon atoms in the aliphatic dicarboxylic acid (b2) is preferably 4 to 12, more preferably 5 to 10, and even more preferably 6 to 8. Furthermore, in the second embodiment of the present invention, from the viewpoints of exhibiting excellent impact resistance (particularly impact resistance at low temperatures), the number of carbon atoms in the aliphatic dicarboxylic acid (b2) is preferably 4 or more, more preferably 5 or more, and even more preferably 6 or more. From the viewpoint of exhibiting even more excellent biodegradability, the number of carbon atoms is preferably 12 or less, more preferably 10 or less, and even more preferably 8 or less. That is, in the second embodiment of the present invention, the number of carbon atoms in the aliphatic dicarboxylic acid (b2) is preferably 4 to 12, more preferably 5 to 10, and even more preferably 6 to 8.
[0026] Examples of the aliphatic dicarboxylic acid (b2) include succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, and decanedicarboxylic acid. Succinic acid, adipic acid, and sebacic acid are preferred, and adipic acid is more preferred. The aliphatic dicarboxylic acid (b2) may be used alone or in combination of two or more.
[0027] <Content of aromatic carboxylic acid units in polyester units (b)> The content of aromatic carboxylic acid units in polyester units (b) is preferably 20% by mass or less. When the content is 20% by mass or less, biodegradability is improved. Here, the aromatic carboxylic acid units also include heteroaromatic carboxylic acid units containing heteroatoms. The aromatic carboxylic acid units may contain one or both of heteroaromatic carboxylic acid units containing heteroatoms and heteroaromatic carboxylic acid units not containing heteroatoms, or may contain only heteroaromatic carboxylic acid units not containing heteroatoms. From this viewpoint, the content of aromatic carboxylic acid units in polyester units (b) is more preferably 15% by mass or less, even more preferably 10% by mass or less, even more preferably 5% by mass or less, and even more preferably 1% by mass or less, and polyester units (b) may not contain aromatic carboxylic acid units.
[0028] <Preferred Combinations of Aliphatic Diol (b1) and Aliphatic Dicarboxylic Acid (b2)> From the viewpoint of exhibiting even more excellent biodegradability, hydrolysis resistance, tensile properties, impact resistance, heat resistance, and the like, preferred combinations of 2-methyl-1,3-propanediol and succinic acid, 3-methyl-1,5-pentanediol and succinic acid, 2,4-diethyl-1,5-pentanediol and succinic acid, 2-methyl-1,3-propanediol and adipic acid, 3-methyl-1,5-pentanediol and adipic acid, and 2,4-diethyl-1,5-pentanediol and succinic acid are preferred. A combination of 3-methyl-1,5-pentanediol and succinic acid, a combination of 2,4-diethyl-1,5-pentanediol and succinic acid, a combination of 3-methyl-1,5-pentanediol and adipic acid, and a combination of 2,4-diethyl-1,5-pentanediol and adipic acid are examples of more preferred embodiments, and a combination of 3-methyl-1,5-pentanediol and adipic acid is an example of a further preferred embodiment.
[0029] <Ratio of Aliphatic Diol (b1) and Aliphatic Dicarboxylic Acid (b2)> The molar ratio of the aliphatic diol (b1) and the aliphatic dicarboxylic acid (b2) charged when reacting them [aliphatic diol (b1) / aliphatic dicarboxylic acid (b2)] is preferably 1.4 / 1 to 1 / 1.4, more preferably 1.2 / 1 to 1 / 1.2.
[0030] <Units (b') Other Than Polyester Units (b)> The block structural unit (B) may or may not contain units (b') other than the polyester units (b). The monomer constituting the units (b') is not particularly limited as long as the effects of the present invention are not impaired, and examples thereof include polyamide and polyurethane. The content of the units (b') in the block structural unit (B) is preferably 50% by mass or less, more preferably 30% by mass or less, even more preferably 20% by mass or less, still more preferably 15% by mass or less, and particularly preferably 10% by mass or less.
[0031] <Number-Average Molecular Weight of Block Structural Unit (B)> The number-average molecular weight of the block structural unit (B) is not limited as long as the effects of the present invention are not impaired. In the first embodiment of the present invention, the number-average molecular weight of the block structural unit (B) is preferably less than 200,000, more preferably less than 100,000, even more preferably less than 80,000, and still more preferably less than 50,000 from the viewpoint of productivity, and is preferably 1,000 or more, more preferably 4,000 or more, even more preferably 8,000 or more, and still more preferably 10,000 or more from the viewpoint of melting point and tensile properties. That is, in the first embodiment of the present invention, the number-average molecular weight of the block structural unit (B) is preferably 1,000 or more and less than 200,000, more preferably 4,000 or more and less than 100,000, even more preferably 8,000 or more and less than 80,000, and still more preferably 10,000 or more and less than 50,000. In a second embodiment of the present invention, from the viewpoint of productivity, the number average molecular weight of the block structural unit (B) is preferably less than 300,000, more preferably less than 100,000, even more preferably less than 80,000, and still more preferably less than 50,000, and from the viewpoints of the glass transition temperature, crystalline melting enthalpy, etc., the number average molecular weight of the block structural unit (B) is preferably 1,000 or more, more preferably 4,000 or more, even more preferably 8,000 or more, still more preferably 10,000 or more, and still more preferably 20,000 or more. That is, in the second embodiment of the present invention, the number average molecular weight of the block structural unit (B) is preferably 1,000 or more and less than 300,000, more preferably 4,000 or more and less than 100,000, even more preferably 8,000 or more and less than 80,000, still more preferably 10,000 or more and less than 50,000, and still more preferably 20,000 or more and less than 50,000. The number average molecular weight of the block structural unit (B) can be determined by gel permeation chromatography (GPC) from the number average molecular weight of the block copolymer (I) described below and the mass content of the block structural unit (B), and specifically, can be measured by the method described in the Examples.
[0032] <Structural Unit Proportion in Block Copolymer (I)> The proportion of the block structural unit (A) is preferably 5% by mass or more and 95% by mass or less, relative to 100% by mass of the total of the block structural unit (A) and the block structural unit (B). When the proportion of the block structural unit (A) is 5% by mass or more, the heat resistance of the resin composition tends to be even more excellent. Furthermore, when the proportion of the block structural unit (A) is 95% by mass or less, the tensile properties and biodegradability of the resin composition tend to be even more excellent, and the tensile properties are even more excellent. From the viewpoint of heat resistance, the proportion of the block structural unit (A) is more preferably 10% by mass or more, and even more preferably 15% by mass or more. Furthermore, from the viewpoint of biodegradability and tensile properties, the proportion of the block structural unit (A) is more preferably 80% by mass or less, even more preferably 75% by mass or less, even more preferably 70% by mass or less, and even more preferably 60% by mass or less. The proportion of the block structural unit (A) is 1 It can be determined by H-NMR, specifically by the method described in the Examples.
[0033] The total content of the block structural unit (A) and the block structural unit (B) in the block copolymer (I) is preferably 90% by mass or more, more preferably 95% by mass or more, and may be 100% by mass. There is no upper limit to the total content of the block structural unit (A) and the block structural unit (B) in the block copolymer (I), and it may be, for example, 100% by mass or less.
[0034] The block copolymer (I) may or may not contain units other than the block structural unit (A) and the block structural unit (B). The units other than the block structural unit (A) and the block structural unit (B) are not particularly limited as long as the effects of the present invention are not impaired. The content of units other than the block structural unit (A) and the block structural unit (B) in the block copolymer (I) is preferably 10% by mass or less, more preferably 5% by mass or less.
[0035] <Number Average Molecular Weight of Block Copolymer (I)> In the first embodiment of the present invention, from the viewpoints of heat resistance and tensile properties, the number average molecular weight of the block copolymer (I) is preferably 2,000 or more, more preferably 5,000 or more, even more preferably 10,000 or more, and still more preferably 20,000 or more. Furthermore, in the first embodiment of the present invention, from the viewpoints of processability of the resin composition and productivity of the block copolymer (I), the number average molecular weight of the block copolymer (I) is preferably 450,000 or less, more preferably 350,000 or less, even more preferably 250,000 or less, still more preferably 200,000 or less, still more preferably 150,000 or less, and may be 100,000 or less. That is, in the first embodiment of the present invention, the number average molecular weight of the block copolymer (I) is preferably 2,000 to 450,000, more preferably 2,000 to 400,000, even more preferably 2,000 to 350,000, still more preferably 2,000 to 250,000, still more preferably 2,000 to 200,000, still more preferably 5,000 to 150,000, still more preferably 10,000 to 100,000, and still more preferably 20,000 to 100,000.
[0036] In a second embodiment of the present invention, from the viewpoint of heat resistance, the number average molecular weight of the block copolymer (I) is preferably 5,000 or more, more preferably 10,000 or more, even more preferably 15,000 or more, and even more preferably 20,000 or more. From the viewpoint of ease of production and processability, the number average molecular weight of the block copolymer (I) is preferably 400,000 or less, more preferably 200,000 or less, and even more preferably 100,000 or less. That is, in the second embodiment of the present invention, the number average molecular weight of the block copolymer (I) is preferably 5,000 to 400,000, more preferably 10,000 to 200,000, and even more preferably 15,000 to 100,000. The number average molecular weight of the block copolymer (I) can be determined by gel permeation chromatography (GPC), specifically, by the method described in the Examples.
[0037] <<Bonding Form of Block Copolymer (I)>> The bonding form of the block copolymer (I) is preferably a triblock type or a diblock type, and more preferably a triblock type. The block copolymer (I) may be a mixture of a triblock type and a diblock type. Specifically, the bonding form is preferably [block structural unit (A)]-[block structural unit (B)]-[block structural unit (A)].
[0038] <<Melting Point of Block Copolymer (I)>> The melting point of the block copolymer (I) is preferably 110°C or higher and lower than 180°C. When the melting point of the block copolymer (I) is 110°C or higher, the block copolymer (I) is less likely to soften even at temperatures equal to or higher than the glass transition temperature thereof, resulting in excellent heat resistance. Furthermore, when the melting point of the block copolymer (I) is lower than 180°C, the melting point is not too high, resulting in excellent processability, for example, ease of melt processing. Therefore, the melting point of the block copolymer (I) is preferably 115°C or higher, more preferably 120°C or higher, even more preferably 125°C or higher, and preferably 175°C or lower, more preferably 170°C or lower, even more preferably 160°C or lower, and even more preferably 155°C or lower. That is, the melting point of the block copolymer (I) is preferably 115°C or higher and 175°C or lower, more preferably 115°C or higher and 170°C or lower, even more preferably 120°C or higher and 160°C or lower, and even more preferably 125°C or higher and 155°C or lower. The melting point of the block copolymer (I) can be determined by a differential scanning calorimeter, specifically by the method described in the examples.
[0039] <Glass Transition Temperature of Block Copolymer (I)> In one embodiment of the present invention, the glass transition temperature of the block copolymer (I) is preferably −80° C. or higher and 15° C. or lower, more preferably −80° C. or higher and −10° C. or lower, and even more preferably −80° C. or higher and −15° C. or lower. Within the above numerical range, the resin composition tends to have excellent flexibility and impact resistance. From the viewpoint of impact resistance at low temperatures, the glass transition temperature of the block copolymer (I) is preferably −20° C. or lower, more preferably −25° C. or lower, even more preferably −30° C. or lower, and may be −35° C. or lower, or may be −45° C. or lower. The glass transition temperature of the block copolymer (I) is preferably −80° C. or higher, and the lower limit is preferably lower; however, it may be, for example, −70° C. or higher, −60° C. or higher, or −50° C. or higher. In another embodiment of the present invention, the glass transition temperature of the block copolymer (I) is preferably −80° C. or higher to −20° C. or lower, more preferably −80° C. or higher to −25° C. or lower, even more preferably −80° C. or higher to −30° C. or lower, still more preferably −80° C. or higher to −35° C. or lower, and still more preferably −80° C. or higher to −45° C. In yet another embodiment of the present invention, the glass transition temperature of the block copolymer (I) is preferably −70° C. or higher to −20° C. or lower, more preferably −70° C. or higher to −30° C. or lower.
[0040] In another embodiment of the present invention, the glass transition temperature may be −60° C. or higher and −10° C. or lower, −60° C. or higher and −20° C. or lower, −60° C. or higher and −30° C. or lower, −50° C. or higher and −30° C. or lower, −50° C. or higher and −35° C. or lower, or −50° C. or higher and −45° C. The glass transition temperature of the block copolymer (I) can be determined by differential scanning calorimetry.
[0041] <Method for Producing Block Copolymer (I)> Known production methods can be used to produce the block copolymer (I). (1) A known method for producing the block copolymer (I) may be, for example, a method of synthesizing a polyester constituting the polyester unit (b) and polymerizing the polyester with lactide. The polyester can be synthesized by a known method. For example, a polyester can be synthesized by reacting an aliphatic diol (b1) with an aliphatic dicarboxylic acid (b2) using an esterification catalyst (e.g., tin octoate, tin chloride, tin oxide). When polymerizing a polyester with lactide, it is preferable to use a ring-opening polymerization catalyst (e.g., tin octoate, tin chloride, tin oxide). The polymerization reaction can be performed using solution polymerization, melt polymerization, interfacial polycondensation, etc., and known polymerization reaction conditions can be set for each.
[0042] (2) Furthermore, a known method for producing the block copolymer (I) may be, for example, a method in which polylactic acid constituting the polylactic acid unit (a) and a polyester constituting the polyester unit (b) are separately synthesized and then the polylactic acid and the polyester are reacted. Polylactic acid can be synthesized by a known method. For example, polylactic acid may be synthesized by reacting lactic acid by a direct condensation method, or polylactic acid may be synthesized by reacting lactide by a ring-opening polymerization method. When polymerizing polylactic acid and polyester, it is preferable to use an esterification catalyst (e.g., tin octoate, tin chloride, tin oxide). Examples of the polymerization reaction include solution polymerization, melt polymerization, and interfacial polycondensation, and known polymerization reaction conditions can be set for each.
[0043] <Cyclic Ester Compound (II)> The cyclic ester compound (II) is not particularly limited, and may be a cyclized product of a hydroxycarboxylic acid such as an intermolecular cyclic ester of an α-hydroxycarboxylic acid, a γ-hydroxycarboxylic acid, or a 3-hydroxycarboxylic acid, a condensed cyclized product of an alcohol such as a lactone with a carboxylic acid, or a cyclic compound having another ester structure. Examples of α-hydroxycarboxylic acids that form intermolecular cyclic esters include glycolic acid, L- and / or D-lactic acid, α-hydroxybutyric acid, α-hydroxyisobutyric acid, α-hydroxyvaleric acid, α-hydroxycaproic acid, α-hydroxyisocaproic acid, α-hydroxyheptanoic acid, α-hydroxyoctanoic acid, α-hydroxydecanoic acid, α-hydroxymyristic acid, α-hydroxystearic acid, and alkyl-substituted derivatives thereof. Examples of lactones include β-propiolactone, β-butyrolactone, pivalolactone, γ-butyrolactone, δ-valerolactone, β-methyl-δ-valerolactone, and ε-caprolactone. Other examples of cyclic compounds having an ester structure include dioxanones such as trimethylene carbonate. When the cyclic ester has an asymmetric carbon, it may be in the D-form, L-form, or racemic form. These cyclic esters can be used alone or in combination of two or more.
[0044] From the viewpoint of obtaining a resin composition having an excellent balance of crystallinity, tensile properties, transparency, and heat resistance, and from the viewpoint of obtaining a resin composition having an excellent balance of biodegradability, heat resistance, and transparency, the cyclic ester compound (II) preferably contains a structure derived from an aliphatic diol (c1) and an aliphatic dicarboxylic acid (c2), that is, is preferably a cyclic ester compound obtained by reacting an aliphatic diol (c1) with an aliphatic dicarboxylic acid (c2).
[0045] The aliphatic diol (c1) is not particularly limited, and examples thereof include the same as the aliphatic diol (b1) described above. The aliphatic dicarboxylic acid (c2) is not particularly limited, and examples thereof include the same as the aliphatic dicarboxylic acid (b2) described above. Specific examples of the cyclic ester compound (II) containing a structure derived from the aliphatic diol (c1) and the aliphatic dicarboxylic acid (c2) include, for example, the cyclic ester compound obtained by reacting the aliphatic diol (b1) with the aliphatic dicarboxylic acid (b2) described above. Preferred combinations of the aliphatic diol (c1) and the aliphatic dicarboxylic acid (c2) are the same as the preferred combinations of the aliphatic diol (b1) and the aliphatic dicarboxylic acid (b2) described above. From the viewpoint of obtaining a resin composition having an excellent balance of crystallinity, tensile properties, transparency, and heat resistance, the cyclic ester compound (II) containing a structure derived from an aliphatic diol (c1) and an aliphatic dicarboxylic acid (c2) is preferably a cyclic ester compound obtained by reacting 3-methyl-1,5-pentanediol and adipic acid. Also, from the viewpoint of obtaining a resin composition having an excellent balance of crystallinity, tensile properties, transparency, and heat resistance, it is preferable that the aliphatic diol (c1) and the aliphatic diol (b1) are the same, and the aliphatic dicarboxylic acid (c2) and the aliphatic dicarboxylic acid (b2) are the same.
[0046] The method for producing the cyclic ester compound (II) is not particularly limited, but it can be produced by a known condensation reaction using a hydroxycarboxylic acid or an alcohol and a carboxylic acid as raw materials.
[0047] <Aliphatic Polyester Resin (III)> In the present embodiment, the aliphatic polyester resin (III) is preferably at least one selected from the group consisting of biomass resins and biodegradable resins from the viewpoint of environmental protection. Examples of the aliphatic polyester resin (III) include polylactic acid (PLA), polycaprolactone (PCL), poly(caprolactone / butylene succinate) (PCLBS), polybutylene succinate (PBS), poly(butylene succinate / adipate) (PBSA), poly(butylene succinate / carbonate) (PEC), poly(ethylene terephthalate / succinate) (PETS), poly(butylene adipate / terephthalate) (PBAT), poly(tetramethylene adipate / terephthalate) (PTMT), polyethylene succinate (PES), polyglycolic acid (PGA), polyethylene furanoate (PEF), polyhydroxyalkanoate (PHA) [e.g., polyhydroxybutyrate (PHB), polyhydroxybutyrate valerate (PHBV), etc.], and copolymers containing these. The aliphatic polyester resin (III) may be used alone or in combination of two or more.
[0048] The aliphatic polyester resin (III) is preferably PLA, PBS, PBSA, or PBAT, from the viewpoint of exhibiting even better heat resistance, tensile properties, and biodegradability, and more preferably PLA or its copolymer, i.e., polylactic acid resin.
[0049] From the viewpoint of exhibiting even better heat resistance, the melting point of the aliphatic polyester resin (III) is preferably 100° C. or higher, more preferably 110° C. or higher, even more preferably 130° C. or higher, still more preferably 140° C. or higher, still more preferably 155° C. or higher, and still more preferably 170° C. or higher. From the viewpoint of moldability, the melting point of the aliphatic polyester resin (III) is preferably 300° C. or lower, more preferably 270° C. or lower, still more preferably 240° C. or lower, still more preferably 220° C. or lower, and still more preferably 200° C. or lower.
[0050] When a polylactic acid resin is used as the aliphatic polyester resin (III), examples of the polylactic acid resin include at least one selected from the group consisting of a homopolymer of L-lactic acid, a homopolymer of D-lactic acid, a copolymer of L-lactic acid and D-lactic acid, a homopolymer of DL-lactic acid, a copolymer of DL-lactic acid and L-lactic acid, a copolymer of DL-lactic acid and D-lactic acid, and a polymer of lactide, which is a cyclic dimer of lactic acid. The polylactic acid resin may also be a copolymer of lactic acid with an aliphatic hydroxycarboxylic acid other than lactic acid, an aliphatic dicarboxylic acid, an aliphatic diol, an aromatic dicarboxylic acid, or the like. The copolymer preferably contains 70 mol% or more, more preferably 80 mol% or more, and even more preferably 90 mol% or more, of structural units derived from lactic acid. Among these, the polylactic acid resin is preferably a homopolymer of L-lactic acid, a homopolymer of D-lactic acid, or a copolymer of L-lactic acid and D-lactic acid, with a homopolymer of L-lactic acid being more preferred. The polylactic acid resin may be used alone or in combination of two or more kinds.
[0051] Commercially available polylactic acid resins may be used, such as the "INGEO series" manufactured by NatureWorks, Inc., the "Luminy series" manufactured by Total Corbion, the "Revode" series manufactured by Zhejiang Hisun Biomaterials Co., Ltd., and the "SUPLA" series manufactured by SUPLA Material Technology Co., Ltd.
[0052] The weight-average molecular weight of the polylactic acid resin is preferably 50,000 or more, more preferably 100,000 or more, and even more preferably 150,000 or more, from the viewpoint of heat resistance. From the viewpoint of moldability and compatibility with the block copolymer (I), it is preferably 600,000 or less, more preferably 550,000 or less, and even more preferably 500,000 or less. That is, the weight-average molecular weight of the polylactic acid resin is preferably 50,000 to 600,000, more preferably 100,000 to 550,000, and even more preferably 150,000 to 500,000. The weight-average molecular weight of the polylactic acid resin can be determined in terms of standard polystyrene by gel permeation chromatography (GPC). When using a commercially available product, the catalog value may be used.
[0053] <Content Ratio> <First Embodiment> A resin composition according to a first embodiment of the present invention contains, relative to 100% by mass of the total of the block copolymer (I) and the cyclic ester compound (II), preferably 85% by mass or more and less than 100% by mass, more preferably 90% by mass or more and less than 100% by mass, even more preferably 92% by mass or more and less than 100% by mass, still more preferably 96% by mass or more and less than 100% by mass, still more preferably 98% by mass or more and less than 100% by mass, and still more preferably 98% by mass or more and less than 100% by mass. With this content ratio, a resin composition with even more excellent heat resistance, tensile properties, and transparency can be obtained.
[0054] The resin composition according to the first embodiment of the present invention contains 0.01 to 15% by mass of the cyclic ester compound (II) relative to 100% by mass of the block copolymer (I) and the cyclic ester compound (II). From the viewpoint of obtaining a resin composition having an excellent balance of crystallinity, tensile properties, transparency, and heat resistance, the content of the cyclic ester compound (II) relative to 100% by mass of the block copolymer (I) and the cyclic ester compound (II) in the resin composition according to the first embodiment is preferably 0.02% by mass or more, more preferably 0.04% by mass or more, even more preferably 0.1% by mass or more, even more preferably 0.2% by mass or more, even more preferably 0.3% by mass or more, and is preferably 12% by mass or less, more preferably 8% by mass or less, even more preferably 4% by mass or less, even more preferably 3% by mass or less, and even more preferably 1% by mass or less. The content of the cyclic ester compound (II) can be determined by gas chromatography, specifically, by the method described in the Examples. That is, the content of the cyclic ester compound (II) relative to 100% by mass of the total of the block copolymer (I) and the cyclic ester compound (II) in the resin composition according to the first embodiment is preferably 0.02% by mass or more and 12% by mass or less, more preferably 0.04% by mass or more and 8% by mass or less, even more preferably 0.1% by mass or more and 4% by mass or less, still more preferably 0.2% by mass or more and 3% by mass or less, and still more preferably 0.3% by mass or more and 1% by mass or less.
[0055] The resin composition according to the first embodiment of the present invention preferably contains 4 to 95 mass %, more preferably 8 to 80 mass %, even more preferably 12 to 70 mass %, and still more preferably 17 to 60 mass % of the block structural unit (A) relative to 100 mass % of the total of the block copolymer (I) and the cyclic ester compound (II). The above content ratios allow for a resin composition with even better heat resistance and tensile properties.
[0056] The resin composition according to the first embodiment of the present invention preferably contains 4 to 95 mass %, more preferably 8 to 80 mass %, even more preferably 12 to 70 mass %, and still more preferably 17 to 60 mass % of the block structural unit (B) relative to 100 mass % of the total of the block copolymer (I) and the cyclic ester compound (II). The above content ratios allow for a resin composition with even better heat resistance and tensile properties.
[0057] In the resin composition according to the first embodiment of the present invention, the total content of the block copolymer (I) and the cyclic ester compound (II) is preferably 85% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, still more preferably 98% by mass or more, and even more preferably 99% by mass or more. In the resin composition according to the first embodiment, the total content of the block copolymer (I) and the cyclic ester compound (II) may be 100% by mass or less. With this content, the effects of the present invention are more significantly exhibited.
[0058] Second Embodiment A resin composition according to a second embodiment of the present invention contains the block copolymer (I) in an amount of preferably 0.5 to 50% by mass, more preferably 1 to 40% by mass, even more preferably 1.5 to 30% by mass, and still more preferably 2 to 20% by mass, relative to 100% by mass of the total of the block copolymer (I), the cyclic ester compound (II), and the aliphatic polyester resin (III). This content ratio allows for a resin composition with even better biodegradability, heat resistance, and transparency.
[0059] The resin composition according to the second embodiment of the present invention preferably contains 0.5 to 50 mass %, more preferably 1 to 40 mass %, even more preferably 1.5 to 30 mass %, and still more preferably 2 to 20 mass % of the block copolymer (I) relative to 100 mass % of the total of the block copolymer (I) and the aliphatic polyester resin (III). The above content ratios allow for a resin composition with even better biodegradability, heat resistance, and transparency.
[0060] From the viewpoint of obtaining a resin composition having an excellent balance of biodegradability, heat resistance, and transparency, the resin composition according to the second embodiment of the present invention preferably contains 0.005 to 10 mass%, more preferably 0.01 to 10 mass%, even more preferably 0.015 to 5 mass%, still more preferably 0.025 to 3 mass%, and even more preferably 0.03 to 2 mass% of the cyclic ester compound (II) relative to 100 mass% of the total of the block copolymer (I), the cyclic ester compound (II), and the aliphatic polyester resin (III). The content of the cyclic ester compound (II) can be determined by gas chromatography, and specifically, can be measured by the method described in the Examples.
[0061] The resin composition according to the second embodiment of the present invention preferably contains 50 to 99.5% by mass, more preferably 60 to 99% by mass, even more preferably 70 to 98.5% by mass, and still more preferably 80 to 98% by mass of the aliphatic polyester resin (III) relative to 100% by mass of the total of the block copolymer (I), the cyclic ester compound (II), and the aliphatic polyester resin (III). The above content ratios allow for a resin composition with even better biodegradability, heat resistance, and transparency.
[0062] The resin composition according to the second embodiment of the present invention preferably contains 50 to 99.5% by mass, more preferably 60 to 99% by mass, even more preferably 70 to 98.5% by mass, and still more preferably 80 to 98% by mass of the aliphatic polyester resin (III) relative to 100% by mass of the total of the block copolymer (I) and the aliphatic polyester resin (III). The above content ratios allow for a resin composition with even better biodegradability, heat resistance, and transparency.
[0063] The resin composition according to the second embodiment of the present invention preferably contains 0.1 to 40% by mass, more preferably 0.3 to 30% by mass, even more preferably 0.5 to 25% by mass, and still more preferably 1 to 15% by mass of the block structural unit (A) relative to 100% by mass of the total of the block copolymer (I), the cyclic ester compound (II), and the aliphatic polyester resin (III). The above content ratios allow for a resin composition with even better heat resistance and transparency.
[0064] The resin composition according to the second embodiment of the present invention preferably contains 0.2 to 40% by mass, more preferably 0.5 to 30% by mass, even more preferably 1 to 20% by mass, and still more preferably 1.5 to 15% by mass of the block structural unit (B) relative to 100% by mass of the total of the block copolymer (I), the cyclic ester compound (II), and the aliphatic polyester resin (III). The above content ratios allow for a resin composition with even better biodegradability and heat resistance.
[0065] In the resin composition according to the second embodiment of the present invention, the total content of the block copolymer (I), the cyclic ester compound (II), and the aliphatic polyester resin (III) is preferably 80% by mass or more, more preferably 85% by mass or more, even more preferably 90% by mass or more, still more preferably 95% by mass or more, and even more preferably 98% by mass or more. In the resin composition according to the second embodiment of the present invention, the total content of the block copolymer (I), the cyclic ester compound (II), and the aliphatic polyester resin (III) may be 100% by mass or less. With the above content ratio, the effects of the present invention are more significantly exhibited.
[0066] <Other Components> The resin composition according to the first embodiment of the present invention may contain, in addition to the block copolymer (I) and the cyclic ester compound (II), a plasticizer, a resin other than the block copolymer (I) and the aliphatic polyester-based resin (III), an additive, etc. Furthermore, the resin composition according to the second embodiment of the present invention may contain, in addition to the block copolymer (I), the cyclic ester compound (II), and the aliphatic polyester-based resin (III), a plasticizer, a resin other than the block copolymer (I) and the aliphatic polyester-based resin (III), an additive, etc.
[0067] <Plasticizer> A plasticizer may be added to the resin composition for the purpose of adjusting the viscosity to a level suitable for molding or for the purpose of obtaining a molded product with the desired hardness. There are no particular limitations on the plasticizer, but plasticizers that are biodegradable in any of industrial compost, household compost, soil, and marine environments are preferred. Suitable examples include plant esters such as rapeseed oil and castor oil, synthetic esters such as triacetin, diethyl phthalate, and triethyl citrate, polyols and derivatives thereof such as ethylene glycol and trimethylolpropane, and sugars such as sorbitol. These may be used alone or in combination of two or more. When using the above-mentioned plasticizer, the content of the plasticizer in the resin composition may be appropriately determined depending on the desired physical properties of the resin composition.
[0068] <<Resins Other than Block Copolymer (I) and Aliphatic Polyester Resin (III)>> The resins other than the block copolymer (I) and the aliphatic polyester resin (III) are not particularly limited, but are preferably resins that are biodegradable in any of industrial compost, household compost, soil, and marine environments. Suitable examples include polyvinyl alcohol, cellulose resins such as cellulose acetate, starch and its esters, and 4-nylon. These may be used alone or in combination of two or more. When a resin other than the block copolymer (I) and the aliphatic polyester resin (III) is used, the content of the resin in the resin composition may be determined appropriately depending on the desired physical properties of the resin composition.
[0069] <<Additives>> Examples of additives include inorganic fillers, softeners, heat aging inhibitors, antioxidants, hydrolysis inhibitors, light stabilizers, antistatic agents, release agents, flame retardants, foaming agents, pigments, dyes, brighteners, ultraviolet absorbers, and lubricants. These may be used alone or in combination of two or more. When using the above additives, the content of the additives in the resin composition may be appropriately determined depending on the desired physical properties of the resin composition.
[0070] <Crystalline Melting Enthalpy of Resin Composition> From the viewpoint of heat resistance, the crystalline melting enthalpy of the resin composition according to the first embodiment of the present invention is preferably higher than the crystalline melting enthalpy of the block copolymer (I). The rate of increase ((ΔHm2 / ΔHm1) × 100-100(%)) of the crystalline melting enthalpy (ΔHm2) of the resin composition according to the first embodiment of the present invention relative to the crystalline melting enthalpy (ΔHm1) of the block copolymer (I) is preferably 0.5% or more, more preferably 1.0% or more, even more preferably 2.0% or more, still more preferably 5.0% or more, and even more preferably 10.0% or more. There is no particular upper limit to the rate of increase, and it may be 500% or less, 300% or less, 200% or less, 100% or less, 50% or less, or 20% or less.
[0071] From the viewpoint of heat resistance, the crystalline melting enthalpy of the resin composition according to the second embodiment of the present invention is preferably higher than the crystalline melting enthalpy of a mixture of block copolymer (I) and aliphatic polyester (III) (a mixture of block copolymer (I) and aliphatic polyester (III) in the same ratio as the block copolymer (I) and aliphatic polyester (III) contained in a comparative resin composition). The rate of increase ((ΔHm2 / ΔHm1) × 100-100(%)) of the crystalline melting enthalpy (ΔHm2) of the resin composition according to the second embodiment of the present invention relative to the crystalline melting enthalpy (ΔHm1) of the mixture is preferably 0.2% or more, more preferably 0.5% or more, even more preferably 1.0% or more, still more preferably 3.0% or more, and even more preferably 5.0% or more. There is no particular upper limit to the rate of increase, and it may be 300% or less, 200% or less, 100% or less, 50% or less, 20% or less, or 10% or less. The crystalline fusion enthalpy of the resin composition can be determined by a differential scanning calorimeter, and specifically, can be measured by the method described in the examples.
[0072] <Melting Point of Resin Composition> From the viewpoint of heat resistance, the melting point of the resin composition according to the first embodiment of the present invention is preferably higher than the melting point of the block copolymer (I) by 0.1°C or more, more preferably by 0.3°C or more, even more preferably by 0.5°C or more, still more preferably by 0.8°C or more, still more preferably by 1.0°C or more, still more preferably by 1.5°C or more, and still more preferably by 2.0°C or more. There is no particular upper limit for the difference between the melting point of the resin composition according to the first embodiment of the present invention and the melting point of the block copolymer (I), and the upper limit may be 70°C or less, 50°C or less, 30°C or less, 10°C or less, or 5°C or less. The melting point of the resin composition can be determined using a differential scanning calorimeter, and specifically, can be measured by the method described in the examples.
[0073] <Glass Transition Temperature of Resin Composition> When the aliphatic polyester resin (III) is a polylactic acid resin, the glass transition temperature of the resin composition according to the second embodiment of the present invention is preferably 50° C. or higher, more preferably 55° C. or higher, even more preferably 58° C. or higher, still more preferably 59° C. or higher, and even more preferably 60° C. or higher from the viewpoint of heat resistance, and is preferably 75° C. or lower, more preferably 70° C. or lower from the viewpoint of processability. Furthermore, from the viewpoint of heat resistance, the glass transition temperature is preferably 0.1° C. or higher, more preferably 0.3° C. or higher, even more preferably 0.5° C. or higher, and even more preferably 1.0° C. or higher than the glass transition temperature of a mixture of block copolymer (I) and aliphatic polyester (III) (a mixture of block copolymer (I) and aliphatic polyester (III) in the same ratio as the block copolymer (I) and aliphatic polyester (III) contained in a comparative resin composition). The upper limit of the difference between the glass transition temperature of the resin composition according to the second embodiment of the present invention and the glass transition temperature of the block copolymer (I) is not particularly limited, and may be 50° C. or less, 30° C. or less, 10° C. or less, 5° C. or less, or 3° C. or less. The glass transition temperature of the resin composition can be determined by a differential scanning calorimeter, and specifically, can be measured by the method described in the examples.
[0074] <Elongation at break of resin composition> The elongation at break retention rate of the resin composition according to the first embodiment of the present invention, which is calculated by the following formula (1), is, from the viewpoint of moldability, preferably 90% or more, more preferably 95% or more, even more preferably 97% or more, still more preferably 99% or more, and still more preferably 100% or more, and the upper limit is not particularly limited, and may be 3000% or less, 2000% or less, 1000% or less, 500% or less, 300% or less, 200% or less, 150% or less, or 120% or less. Breaking elongation (T2) of resin composition according to the first embodiment of the present invention / Breaking elongation (T1) of block copolymer (I) × 100 (%) (1) In this specification, the term "breaking elongation" refers to a value obtained by preparing a 100 μm thick press sheet using the resin composition or the block copolymer (I) at 140° C., 40 kN, and 1 min, annealing the press sheet at 110° C. for 3 hours, punching the sheet into a dumbbell-shaped No. 3 test piece, and then measuring the elongation at break at a tensile speed of 5 mm / min using the test piece in accordance with JIS K7161-1:2014, and can be measured by the method described in the examples.
[0075] <<Haze Change Rate of Resin Composition>> From the viewpoint of visibility, the rate of change (%) of the haze (absolute value) of the resin composition according to the first embodiment of the present invention relative to the haze (absolute value) of the block copolymer (I) is preferably 99% or less, more preferably 97% or less, even more preferably 95% or less, even more preferably 90% or less, and even more preferably 85% or less. There is no particular lower limit, and it may be 0.1% or more, more preferably 1% or more, even more preferably 10% or more, even more preferably 50% or more, and even more preferably 80% or more. Note that, in this specification, the rate of change (%) of the haze (absolute value) of the resin composition according to the first embodiment of the present invention relative to the haze (absolute value) of the block copolymer (I) is measured and calculated by the following methods (i) to (iii). (i) A press sheet having a thickness of 125 μm is prepared using the resin composition according to the first embodiment at 140° C., 40 kN, and 1 min to obtain a measurement sheet (s2). A measurement sheet (s1) is also obtained for the block copolymer (I) by the same method. (ii) The haze of the obtained measurement sheets (s1) and (s2) is measured in accordance with JIS K7136:2000 using a haze meter "HZ-1" (manufactured by Suga Test Instruments Co., Ltd.). (iii) Using the haze of the obtained measurement sheet (s1) (measurement sheet (S1)) and the haze of the measurement sheet (s2) (measurement sheet (S2)), the rate of change (%) of the haze (absolute value) of the resin composition according to the first embodiment of the present invention (measurement sheet (S2)) relative to the haze (absolute value) of the block copolymer (I) (measurement sheet (S1)) is calculated using the following formula (2):(Measurement sheet (S2) / Measurement sheet (S1)) × 100 (%) (2) The haze (absolute value) of the resin composition according to the second embodiment of the present invention relative to the haze (absolute value) of a mixture of block copolymer (I) and aliphatic polyester (III) (a mixture of block copolymer (I) and aliphatic polyester (III) in the same ratio as the block copolymer (I) and aliphatic polyester (III) contained in the resin composition according to the second embodiment of the present invention, which is a comparison object) is preferably 99% or less, more preferably 97% or less, even more preferably 95% or less, still more preferably 90% or less, and even more preferably 85% or less, from the viewpoint of visibility. The lower limit is not particularly limited, and may be 0.1% or more, 1% or more, 10% or more, 50% or more, or 80% or more. In this specification, the percentage change (%) in the haze (absolute value) of the resin composition according to the second embodiment of the present invention relative to the haze (absolute value) of the mixture of the block copolymer (I) and the aliphatic polyester (III) is measured and calculated by the following methods (iv) to (vi). (iv) The resin composition according to the second embodiment is subjected to a pressure reduction heat press ("IMC-183B" manufactured by Imoto Machinery Co., Ltd.) using an oil rotary pump to reduce the pressure to 0.1 MPaG, preheating at 200°C for 5 minutes, and pressing at 40 kN for 1 minute. Thereafter, the resin composition is pressed at 20 kgf / cm using a cooling press equipped with water flow cooling. 2The mixture is pressed at 100°C for 1 minute to produce a press plate with a thickness of 0.125 mm. A 50 x 50 mm square piece is cut out from the obtained press plate and crystallized in a 110°C thermostatic chamber for 3 hours to obtain a measurement sheet (s2'). A measurement sheet (s1') is also obtained by the same method for a mixture of block copolymer (I) and aliphatic polyester (III) (a mixture of block copolymer (I) and aliphatic polyester (III) in the same ratio as the block copolymer (I) and aliphatic polyester (III) contained in the resin composition according to the second embodiment of the present invention, which is used for comparison). (v) The haze of the obtained measurement sheets (s1') and (s2') is measured in accordance with JIS-K7136:2000 using a "Spectral Haze Meter SH7000" manufactured by Nippon Denshoku Industries Co., Ltd. (light source D65). (vi) Using the haze of the obtained measurement sheet (s1') (measurement sheet (S1')) and the haze of the measurement sheet (s2') (measurement sheet (S2')), the rate of change (%) of the haze (absolute value) of the resin composition according to the second embodiment of the present invention (measurement sheet (S2')) relative to the haze (absolute value) (measurement sheet (S1')) of a mixture of block copolymer (I) and aliphatic polyester (III) (a mixture of block copolymer (I) and aliphatic polyester (III) in the same ratio as the block copolymer (I) and aliphatic polyester (III) contained in the resin composition according to the second embodiment of the present invention, which is used for comparison) is calculated from the following formula (3): (measurement sheet (S2') / measurement sheet (S1')) × 100 (%) (3) Haze can be specifically measured by the method described in the examples.
[0076] [Method for Producing Resin Composition] The method for producing the resin composition according to the first embodiment of the present invention is not particularly limited, and it is sufficient to uniformly mix the block copolymer (I), the cyclic ester compound (II), and, if necessary, additives. Furthermore, the method for producing the resin composition according to the second embodiment of the present invention is not particularly limited, and it is sufficient to uniformly mix the block copolymer (I), the cyclic ester compound (II), the aliphatic polyester resin (III), and, if necessary, additives. In the first and second embodiments, the cyclic ester compound (II) may be synthesized simultaneously during the synthesis of the block copolymer (I) and mixed with the block copolymer (I). Examples of mixing methods include melt-kneading using a single-screw extruder, a multi-screw extruder, a Banbury mixer, a heated roll, a Brabender, various kneaders, etc., or melt-kneading methods in which each component is fed through a separate feed port. Alternatively, the components may be pre-blended before melt-kneading. Examples of pre-blending methods include using a mixer such as a Henschel mixer, a high-speed mixer, a V-blender, a ribbon blender, a tumbler blender, or a conical blender. The temperature during melt-kneading can be arbitrarily selected preferably within the range of 140 to 220° C., taking into consideration the melting points and decomposition temperatures of the block copolymer (I) and the cyclic ester compound (II).
[0077] The present invention will be specifically explained below with reference to examples and comparative examples, but the present invention is not limited to these.
[0078] The compounds used in the examples and comparative examples are as follows. 3-Methyl-1,5-pentanediol (manufactured by Kuraray Co., Ltd.) Adipic acid (manufactured by Tokyo Chemical Industry Co., Ltd.) Stannous octoate (manufactured by Tokyo Chemical Industry Co., Ltd.) Toluene (manufactured by Kishida Chemical Co., Ltd.) L-lactide (manufactured by Tokyo Chemical Industry Co., Ltd.) Methanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 2,4-Diethyl-1,5-pentanediol (manufactured by Tokyo Chemical Industry Co., Ltd.) 2-Methyl-1,3-propanediol (manufactured by Tokyo Chemical Industry Co., Ltd.) Succinic acid (manufactured by Tokyo Chemical Industry Co., Ltd.) 1,4-Butanediol (manufactured by Tokyo Chemical Industry Co., Ltd.) Propylene glycol (manufactured by Tokyo Chemical Industry Co., Ltd.) Di-n-alkyl Adipate [Plasticizer] (manufactured by Tokyo Chemical Industry Co., Ltd.) N,N'-Ethylenebisoctadecanoic acid [mixture of fatty acids] [consists of C 14 , C 16 and C 18 ] (Tokyo Chemical Industry Co., Ltd.)
[0079] The physical properties of the polymers and resin compositions in the examples and comparative examples were measured or evaluated by the following methods. (1) Number-average molecular weight (Mn) The number-average molecular weight (Mn) of the polymer was determined by gel permeation chromatography (GPC) in terms of standard polystyrene. The Mn of the block structural unit (B) was determined from the Mn of the block copolymer (I) and the mass content of the block structural unit (B). <GPC measurement conditions> Apparatus: GPC apparatus "HLC-8220" manufactured by Tosoh Corporation Separation column: "TSKgel SuperMultiporeHZ-M (column diameter = 4.6 mm, column length = 15 cm)" manufactured by Tosoh Corporation (two columns connected in series) Eluent: tetrahydrofuran (THF) Eluent flow rate: 0.35 mL / min Column temperature: 40°C Detection method: refractive index (RI) Injection volume: 10 μL Concentration: 1 mg / 1 mL (block copolymer or polymer / THF)
[0080] (2) Hard Ratio (% by Mass) (% by Mass of Block Structure Unit (A) Mainly Containing Polylactic Acid Unit (a)) 1 The hard ratio of the block polymer was calculated by H-NMR. The molar ratio of the block structural unit (A) to the block structural unit (B) was calculated from the area ratio of the signal at around 5.2 ppm derived from the polylactic acid unit in the obtained spectrum to the signal at around 0.9 ppm derived from the structural unit (B) mainly composed of polyester unit (b). The molar ratio was multiplied by the molecular weight of the block structural unit to obtain a mass ratio, and the mass ratio of (A) when adjusted so that the sum of the mass ratios became 100 was taken as the hard ratio. 1 H-NMR measurement conditions> Apparatus: Nuclear magnetic resonance apparatus "JNM-ECX400" manufactured by JEOL Ltd. Solvent: deuterated chloroform Measurement temperature: 50°C Number of accumulations: 1024 Measurement conditions: Temperature rise rate 10°C / min
[0081] (3) Biodegradability (Compost) Biodegradability in compost was measured in accordance with ISO 14855-2:2018. In Examples 1 to 10 and Comparative Examples 1 to 10, if the decomposition rate after 15 days was 20% by mass or more, it was evaluated as A; if it was 10% by mass or more but less than 20% by mass, it was evaluated as B; and if it was 5% by mass or more but less than 10% by mass, it was evaluated as C. In Examples 11 to 24 and Comparative Examples 11 to 15, if the decomposition rate after 15 days was 10% by mass or more, it was evaluated as A; and if it was less than 10% by mass, it was evaluated as B.
[0082] (4) Biodegradability (activated sludge) Biodegradability in activated sludge was measured in accordance with ISO 14851: 2019. If the decomposition rate after 90 days was 5% by mass or more, it was evaluated as A, and if it was less than 5% by mass, it was evaluated as B.
[0083] (5) Breaking Elongation Using the resin compositions obtained in the Examples and Comparative Examples, a 100 μm thick press sheet was prepared at 140°C, 40 kN, and 1 min. The press sheet was annealed at 110°C for 3 hours and then punched into a dumbbell-shaped No. 3 test piece. Using the test piece, measurements were carried out at a tensile speed of 5 mm / min in accordance with JIS K7161-1:2014. Similarly, test pieces were prepared for the block copolymers (I) and polymers obtained in the Examples and Comparative Examples, and measurements were carried out in the same manner. For Examples 1 to 12 and Comparative Examples 6 and 7, the breaking elongation retention rate was calculated from the following formula (I-i): Breaking elongation of resin composition (T2) / Breaking elongation of block copolymer alone contained in resin composition (T1)×100(%) (I-i)
[0084] (6) Glass transition temperature (°C), melting point (°C), and crystalline melting enthalpy (J / g) The glass transition temperature, melting point, and crystalline melting enthalpy of a block copolymer, a polymer, a resin composition, and a mixture A of a block copolymer and an aliphatic polyester (a mixture of a block copolymer and an aliphatic polyester in the same ratio as the block copolymer and the aliphatic polyester contained in the resin composition to be compared) were measured using a differential scanning calorimeter in accordance with JIS K7121:2012. Specifically, the glass transition temperature, melting point, and crystalline melting enthalpy were measured using a differential scanning calorimeter in accordance with JIS K7121:2012 under the following measurement conditions: nd The glass transition temperature (°C), melting point (°C) and crystalline melting enthalpy (J / g) were measured in this specification. In this specification, the midpoint glass transition temperature in JIS K7121:2012 is defined as the glass transition temperature, and nd The heat of fusion in the melting curve during the run is defined as the crystalline melting enthalpy. <Measurement conditions for glass transition temperature (°C), melting point (°C), and crystalline melting enthalpy (J / g)> Apparatus: Mettler Toledo differential scanning calorimeter "DSC822" A measurement sample (block copolymer, polymer, or resin composition) at 25°C was heated to 200°C at a temperature increase rate of 10°C / min (1 stAfter holding the sample at 200°C for 5 minutes, it was cooled from 200°C at a rate of 10°C / min to 75°C and held at 75°C for 30 minutes (crystallization). It was then cooled from 75°C at a rate of 10°C / min to -50°C, then cooled from -50°C at a rate of 5°C / min to -75°C, and held at -75°C for 5 minutes. It was then heated from -75°C at a rate of 10°C / min to 250°C (2 nd run). Furthermore, for Examples 1 to 24 and Comparative Examples 6, 7, 13, and 14, the rate of increase ((ΔHm2 / ΔHm1) × 100-100(%)) of the crystalline melting enthalpy (ΔHm2) of the resin composition relative to the crystalline melting enthalpy (ΔHm1) of the block copolymer contained in the resin composition was calculated. Furthermore, for Examples 13 to 24 and Comparative Examples 13 and 14, the increase in the glass transition temperature (Tg2) of the resin composition relative to the glass transition temperature (Tg1) of mixture A (Tg2-Tg1 (°C)) was calculated.
[0085] (8) Haze In Examples 1 to 12 and Comparative Examples 1 to 10, the haze was measured by the following methods (i) to (iii), and the rate of change in haze was calculated. (i) Using the obtained resin composition, a 125 μm thick press sheet was prepared at 140°C, 40 kN, and 1 min to obtain a measurement sheet (s2). Similarly, a measurement sheet (s1) was obtained for the block copolymer (I) using the same method. (ii) The haze of the obtained measurement sheets (s1) and (s2) was measured in accordance with JIS K7136:2000 using a haze meter "HZ-1" (manufactured by Suga Test Instruments Co., Ltd.). (iii) Using the haze of the obtained measurement sheet (s1) (measurement sheet (S1)) and the haze of the measurement sheet (s2) (measurement sheet (S2)), the rate of change (%) of the haze (absolute value) of the resin composition according to the first embodiment of the present invention (measurement sheet (S2)) relative to the haze (absolute value) of the block copolymer (I) (measurement sheet (S1)) was calculated from the following formula (2): (measurement sheet (S2) / measurement sheet (S1)) x 100 (%) (2) In Examples 13 to 24 and Comparative Examples 11 to 15, the haze was measured by the following methods (iv) to (vi), and the rate of change of the haze was calculated. (iv) The obtained resin composition was subjected to a reduced pressure heat press ("IMC-183B" manufactured by Imoto Machinery Co., Ltd.) using an oil rotary pump to reduce the pressure to 0.1 MPaG, preheated at 200°C for 5 minutes, and then pressed at 40 kN for 1 minute. Thereafter, the pressure was increased to 20 kgf / cm using a cooling press equipped with water flow cooling. 2The mixture was pressed at 100°C for 1 minute to produce a press plate with a thickness of 0.125 mm. A 50 x 50 mm square piece was cut out from the obtained press plate and crystallized in a 110°C thermostatic bath for 3 hours to obtain a measurement sheet (s2'). Furthermore, a measurement sheet (s1') was obtained by the same method for a mixture A of a block copolymer and an aliphatic polyester (a mixture of a block copolymer and an aliphatic polyester in the same ratio as the block copolymer and aliphatic polyester contained in the resin composition for comparison). (v) The haze of the obtained measurement sheets (s1') and (s2') was measured in accordance with JIS-K7136:2000 using a "Spectral Haze Meter SH7000" manufactured by Nippon Denshoku Industries Co., Ltd. (light source D65). (vi) Using the haze of the obtained measurement sheet (s1') (measurement sheet (S1')) and the haze of the measurement sheet (s2') (measurement sheet (S2')), the rate of change (%) of the haze (absolute value) of the resin composition according to the second embodiment of the present invention (measurement sheet (S2')) relative to the haze (absolute value) of the mixture A (measurement sheet (S1')) was calculated from the following formula (3): (measurement sheet (S2') / measurement sheet (S1')) x 100 (%) (3)
[0086] (9) Gas Chromatography Gas chromatography measurements were performed under the following measurement conditions using the resin compositions obtained in the examples and comparative examples. The area percentage (GC%) of the cyclic ester compound was determined by gas chromatography analysis, and then the content of the cyclic ester compound in the resin composition was calculated by the absolute calibration curve method. <Gas Chromatography Measurement Conditions> Apparatus: "GC-2014" manufactured by Shimadzu Corporation Column: "DB-1" manufactured by Agilent Technologies Inc. (inner diameter 0.25 mm, length 30.0 m, film thickness 1.00 μm) Carrier gas: Helium (120.0 kPaG) was passed through at a flow rate of 1.36 mL / min. Detector: FID Analysis conditions: Injection temperature: 200°C, Detection temperature: 250°C Heating conditions: 50 to 110°C: 10°C / min, 110 to 180°C: 40°C / min, 180 to 280°C: 10°C / min
[0087] Example 1 A flask equipped with a vacuum pump and an apparatus for distilling off the generated liquid and collecting the distillate was charged with 3-methyl-1,5-pentanediol and adipic acid in a molar ratio of 3-methyl-1,5-pentanediol / adipic acid = 1.1 / 1. Tin octoate was then added in an amount of 0.1% by mass relative to the total amount of 3-methyl-1,5-pentanediol and adipic acid. The mixture was heated at 160°C under normal pressure in a nitrogen atmosphere for 3 hours, and then heated at 220°C for 3 hours to distill off water, thereby carrying out a reaction. The distillate was stored separately. The pressure was then reduced to 2,000 Pa and the reaction was continued for 3 hours. The pressure was then reduced to 80 Pa and the reaction was continued while appropriately monitoring the reaction until the number average molecular weight reached 9,500, thereby synthesizing a polymer composed of structural units (B') primarily composed of polyester units. After the reaction was completed, the pressure was returned to normal and the temperature was cooled to 80°C. Toluene was then added to dilute the solution to a solids content of 40% by mass, and the toluene solution was then added to methanol in an amount twice the total volume of the solution. The supernatant was discarded, and the same amount of methanol as the amount of toluene solution added was added again for washing. The supernatant was discarded, and the recovered insoluble matter was dried at 40°C using a vacuum dryer to remove organic volatiles, thereby obtaining a polymer composed of structural units (B') primarily composed of polyester units (b). Toluene was added again to the purified polymer composed of structural units (B') to dilute the toluene solution of the polymer composed of structural units (B') to a solids content of 33% by mass. The temperature was then raised to 140°C, whereby 10% by mass of the toluene added was distilled off to dehydrate the system. Thereafter, the toluene solution of the polymer comprising the structural unit (B') was cooled to 80°C, and the polymer comprising the structural unit (B') and L-lactide were added so that the ratio of the polymer comprising the structural unit (B') / L-lactide was 50 / 50. The amount of toluene distilled off as described above was further added, and the solids content of the toluene solution of the polymer comprising the structural unit (B') and L-lactide was adjusted to 50 mass%.Thereafter, when the temperature of the solution was raised to 100°C, tin octylate was added in an amount of 0.1% by mass relative to the polymer consisting of structural units (B'), and the reaction was carried out for 4 hours to synthesize a block copolymer (I) consisting of block structural units (A) mainly composed of polylactic acid units (a) and block structural units (B) mainly composed of polyester units (b), thereby obtaining a toluene solution of the block copolymer (I). This solution was further diluted with toluene to a solid content of 40% by mass, and the toluene solution with a solid content of 40% by mass was then added to methanol in an amount twice the total volume of the solution to precipitate a solid. The supernatant methanol was discarded, and an equal amount of methanol to the amount of the toluene solution added was added again for washing. The methanol was discarded, and the recovered solid was dried in a vacuum dryer at 40°C to remove organic volatiles, thereby obtaining a block copolymer (I-1) consisting of block structural units (A) mainly composed of polylactic acid units (a) and block structural units (B) mainly composed of polyester units (b). The number average molecular weight (Mn) of the resulting block copolymer (I) was 19,000.
[0088] In addition, the distillate obtained during synthesis of the polymer comprising the structural unit (B'), toluene, and water were charged into a separatory funnel in a mass ratio of distillate / toluene / water = 1 / 10 / 10, and 4-methyl-1,7-dioxacyclotridecane-8,13-dione contained in the distillate was extracted into toluene. The toluene layer was added to an eggplant flask, and the toluene was evaporated by air drying overnight at 20°C. After that, the mixture was dried in a vacuum dryer at 20°C at 100 Pa for 1 hour to obtain crystals of 4-methyl-1,7-dioxacyclotridecane-8,13-dione, which is the cyclic ester compound (II).
[0089] 19 parts by mass of the obtained block copolymer (I) was dissolved in 80 parts by mass of toluene to prepare a polymer solution. A cyclic ester compound (II) (4-methyl-1,7-dioxacyclotridecane-8,13-dione) composed of 3-methyl-1,5-pentanediol and adipic acid was added to the polymer solution in an amount of 0.03 parts by mass per 100 parts by mass of the total of the block copolymer (I) and the cyclic ester compound (II). A mixed solution was obtained. The mixed solution was air-dried overnight at 25°C and then dried for 3 hours in a vacuum dryer set at 40°C to obtain a resin composition containing the cyclic ester compound (II). The obtained resin composition was subjected to the above-described measurements and evaluations. The results are shown in Table 1.
[0090] Examples 2 to 5 Resin compositions containing block copolymers (I) composed of block structural units (A) mainly composed of polylactic acid units (a) and block structural units (B) mainly composed of polyester units (b), and cyclic ester compounds (II) were obtained in the same manner as in Example 1, except that the amount of cyclic ester compound (II) (4-methyl-1,7-dioxacyclotridecane-8,13-dione) composed of 3-methyl-1,5-pentanediol and adipic acid was changed to the amount shown in Table 1. The obtained resin compositions were subjected to the above-described measurements and evaluations. The results are shown in Table 1.
[0091] Example 6 A resin composition containing a block copolymer (I) composed of block structural units (A) mainly composed of polylactic acid units (a) and block structural units (B) mainly composed of polyester units (b) and a cyclic ester compound (II) was obtained in the same manner as in Example 5, except that a polymer composed of structural units (B') having a number average molecular weight of 23,800 was synthesized and used. The obtained resin composition was subjected to the above-described measurements and evaluations. The results are shown in Table 1.
[0092] Example 7 A resin composition containing a block copolymer (I) consisting of block structural units (A) mainly composed of polylactic acid units (a) and block structural units (B) mainly composed of polyester units (b) and a cyclic ester compound (II) was obtained in the same manner as in Example 5, except that a cyclic ester compound (II) (3-methyl-1,5-dioxacycloundecane-6,11-dione) was used. The obtained resin composition was subjected to the above-described measurements and evaluations. The results are shown in Table 2.
[0093] Example 8 A resin composition containing a block copolymer (I) composed of a block structural unit (A) mainly composed of a polylactic acid unit (a) and a block structural unit (B) mainly composed of a polyester unit (b) and a cyclic ester compound (II) was obtained in the same manner as in Example 3, except that 2-methyl-1,3-propanediol was used instead of 3-methyl-1,5-pentanediol to synthesize a polymer composed of the structural unit (B') shown in Table 2 and that a cyclic ester compound (II) (3-methyl-1,5-dioxacycloundecane-6,11-dione) was used. The obtained resin composition was subjected to the above-described measurements and evaluations. The results are shown in Table 2.
[0094] Example 9 A resin composition containing a block copolymer (I) composed of a block structural unit (A) mainly composed of a polylactic acid unit (a) and a block structural unit (B) mainly composed of a polyester unit (b) and a cyclic ester compound (II) was obtained in the same manner as in Example 5, except that 2-methyl-1,3-propanediol was used instead of 3-methyl-1,5-pentanediol, the reaction time was adjusted to synthesize a polymer composed of the structural unit (B') shown in Table 2, and a cyclic ester compound (II) (3-methyl-1,5-dioxacycloundecane-6,11-dione) was used. The obtained resin composition was subjected to the above-described measurements and evaluations. The results are shown in Table 2.
[0095] Example 10 A resin composition containing a block copolymer (I) composed of block structural units (A) mainly composed of polylactic acid units (a) and block structural units (B) mainly composed of polyester units (b) and a cyclic ester compound (II) was obtained in the same manner as in Example 5, except that 2,4-diethyl-1,5-pentanediol was used instead of 3-methyl-1,5-pentanediol and the reaction time was adjusted to synthesize a polymer composed of structural units (B') shown in Table 2. The obtained resin composition was subjected to the above-described measurements and evaluations. The results are shown in Table 2.
[0096] Example 11 A resin composition containing a block copolymer (I) composed of a block structural unit (A) mainly composed of a polylactic acid unit (a) and a block structural unit (B) mainly composed of a polyester unit (b) and a cyclic ester compound (II) was obtained in the same manner as in Example 3, except that succinic acid was used instead of adipic acid and the reaction time was adjusted to synthesize a polymer composed of the structural unit (B') shown in Table 2. The obtained resin composition was subjected to the above-described measurements and evaluations. The results are shown in Table 2.
[0097] Example 12 A resin composition containing a block copolymer (I) composed of a block structural unit (A) mainly composed of a polylactic acid unit (a) and a block structural unit (B) mainly composed of a polyester unit (b) and a cyclic ester compound (II) was obtained in the same manner as in Example 5, except that succinic acid was used instead of adipic acid and the reaction time was adjusted to synthesize a polymer composed of the structural unit (B') shown in Table 2. The obtained resin composition was subjected to the above-described measurements and evaluations. The results are shown in Table 2.
[0098] Comparative Example 1 A resin composition was obtained in the same manner as in Example 1, except that the cyclic ester compound (II) composed of 3-methyl-1,5-pentanediol and adipic acid was not used. The obtained resin composition was subjected to the above-described measurements and evaluations. The results are shown in Table 3. The obtained resin composition had a lower melting point than the resin compositions obtained in the examples. This is thought to be because the resin composition did not contain the cyclic ester compound (II).
[0099] Comparative Example 2 A resin composition was obtained in the same manner as in Example 7, except that the cyclic ester compound (II) composed of 3-methyl-1,5-pentanediol and adipic acid was not used. The obtained resin composition was subjected to the above-described measurements and evaluations. The results are shown in Table 3. The obtained resin composition had a lower degree of crystallinity than the resin compositions obtained in the examples. This is thought to be because the resin composition did not contain the cyclic ester compound (II).
[0100] Comparative Example 3 A resin composition was obtained in the same manner as in Example 8, except that the cyclic ester compound (II) composed of 3-methyl-1,5-pentanediol and adipic acid was not used. The obtained resin composition was subjected to the above-described measurements and evaluations. The results are shown in Table 3. The obtained resin composition had a higher haze value and a lower melting point value compared to the resin compositions obtained in the examples. This is thought to be because the resin composition did not contain the cyclic ester compound (II).
[0101] Comparative Example 4 A resin composition was obtained in the same manner as in Example 10, except that the cyclic ester compound (II) composed of 2,4-diethyl-1,5-pentanediol and adipic acid was not used. The obtained resin composition was subjected to the above-described measurements and evaluations. The results are shown in Table 3. The obtained resin composition had a higher haze value and a lower melting point value compared to the resin compositions obtained in the examples. This is thought to be because the resin composition did not contain the cyclic ester compound (II).
[0102] Comparative Example 5 A resin composition was obtained in the same manner as in Example 11, except that the cyclic ester compound (II) composed of 3-methyl-1,5-pentanediol and succinic acid was not used. The obtained resin composition was subjected to the above-described measurements and evaluations. The results are shown in Table 3. The obtained resin composition had a higher haze value and a lower melting point value compared to the resin compositions obtained in the examples. This is thought to be because the resin composition did not contain the cyclic ester compound (II).
[0103] Comparative Example 6 A resin composition containing a block copolymer consisting of block structural units (A) mainly composed of polylactic acid units (a) and block structural units (B) mainly composed of polyester units (b) and a di-n-alkyl adipate was obtained in the same manner as in Example 1, except that a di-n-alkyl adipate (plasticizer), an ester compound without a cyclic structure, was used instead of the cyclic ester compound (II) in an amount of 5 parts by mass per 100 parts by mass of the total of the block copolymer (I) and the di-n-alkyl adipate. The obtained resin composition was subjected to the above-described measurements and evaluations. The results are shown in Table 4. The obtained resin composition had a lower elongation at break than the resin compositions obtained in the Examples. This is thought to be because the ester compound without a cyclic structure has a high degree of molecular freedom, making the resin composition too flexible.
[0104] Comparative Example 7 A resin composition containing a block copolymer consisting of block structural units (A) mainly composed of polylactic acid units (a) and block structural units (B) mainly composed of polyester units (b) and a nucleating agent was obtained in the same manner as in Example 1, except that the nucleating agent N,N'-Ethylenebisoctadecanamide was used in place of the cyclic ester compound (II) in an amount of 5 parts by mass per 100 parts by mass of the block copolymer (I) and the nucleating agent combined. The obtained resin composition was subjected to the above-described measurements and evaluations. The results are shown in Table 4. The obtained resin composition had a lower elongation at break and a higher haze than the resin compositions obtained in the examples. This is thought to be due to poor compatibility between the nucleating agent and the block copolymer.
[0105] Comparative Example 8 A resin composition was obtained in the same manner as in Example 1, except that the cyclic ester compound (II) composed of 3-methyl-1,5-pentanediol and adipic acid was not used. The obtained resin composition was subjected to the above-described measurements and evaluations. The results are shown in Table 4. The obtained resin composition had a higher haze value and a lower melting point value compared to the resin compositions obtained in the examples. This is thought to be because the resin composition did not contain the cyclic ester compound (II).
[0106] Comparative Example 9 A resin composition containing a polymer consisting of structural units (B') mainly composed of polyester units (b) and a cyclic ester compound (II) was obtained in the same manner as in Example 1, except that a polymer consisting of structural units (B') mainly composed of polyester units (b) was used instead of the block copolymer (I), and 5.0 parts by mass of a cyclic ester compound (II) (4-methyl-1,7-dioxacyclotridecane-8,13-dione) composed of 3-methyl-1,5-pentanediol and adipic acid was used per 100 parts by mass of the total of the polymer consisting of structural units (B') mainly composed of polyester units (b) and the cyclic ester compound (II). The obtained resin composition was subjected to the above-described measurements and evaluations. The results are shown in Table 4. Because the polymer consisting of structural units (B') mainly composed of polyester units (b) was a liquid resin, it was not possible to measure the crystallinity, melting point, elongation at break, and haze of the obtained resin composition. This is believed to be because the block copolymer (I) contained in the resin composition does not contain the block structural unit (A).
[0107] Comparative Example 10: 0.1% by mass of tin octoate was added to L-lactide at 200°C, and the reaction was continued until the number average molecular weight reached 19,000, yielding polylactic acid (a polymer composed of structural units (A) primarily composed of polylactic acid units (a)). A resin composition containing polylactic acid and cyclic ester compound (II) was obtained in the same manner as in Example 1, except that the resulting polylactic acid was used instead of block copolymer (I), and 5.0 parts by mass of cyclic ester compound (II) (4-methyl-1,7-dioxacyclotridecane-8,13-dione) composed of 3-methyl-1,5-pentanediol and adipic acid was used per 100 parts by mass of the total of polylactic acid and cyclic ester compound (II). The resulting resin composition was subjected to the above-described measurements and evaluations. The results are shown in Table 4. The resulting resin composition had poor biodegradability, low elongation at break, and high haze, which is believed to be due to the absence of the block copolymer (I) containing the structural unit (B') mainly composed of the flexible polyester unit (b).
[0108]
[0109]
[0110]
[0111]
[0112] The abbreviations in Tables 1 to 4 represent the following compounds: PLLA: poly-L-lactic acid MPD: 3-methyl-1,5-pentanediol MPDiol: 2-methyl-1,3-propanediol DEPD: 2,4-diethyl-1,5-pentanediol AA: adipic acid SA: succinic acid
[0113] As shown in Examples 1 to 12, a resin composition according to a first embodiment of the present invention, which contains a block copolymer (I) including block structural units (A) mainly composed of specific polylactic acid units (a) and block structural units (B) mainly composed of polyester units (b), and a cyclic ester compound (II), has biodegradable properties over a wide range of conditions and an excellent balance of crystallinity, tensile properties, transparency, and heat resistance. Therefore, the resin composition according to the first embodiment of the present invention is extremely useful industrially.
[0114] Example 13 A flask equipped with a vacuum pump and an apparatus capable of distilling off the liquid generated was charged with 3-methyl-1,5-pentanediol and adipic acid in a molar ratio of 3-methyl-1,5-pentanediol / adipic acid = 1.1 / 1, and tin octoate was added in an amount of 0.1% by mass relative to the total amount of 3-methyl-1,5-pentanediol and adipic acid. The mixture was heated at 160°C under a nitrogen atmosphere and normal pressure for 3 hours, and then heated at 220°C for 3 hours to carry out a reaction while distilling off water. The pressure was then reduced to 2,000 Pa and the reaction was continued for 3 hours. The pressure was then reduced to 80 Pa and the reaction was continued while appropriately checking until the number average molecular weight reached 9,500, thereby synthesizing a polymer composed of structural units (B') mainly composed of polyester units. The distillate, toluene, and water were charged into a separatory funnel in a mass ratio of distillate / toluene / water = 1 / 10 / 10, and 4-methyl-1,7-dioxacyclotridecane-8,13-dione contained in the distillate was extracted into toluene. The toluene layer was added to a recovery flask and air-dried overnight at 20 ° C. to volatilize the toluene, and then dried in a vacuum dryer at 20 ° C. and 100 Pa for 1 hour to obtain crystals of 4-methyl-1,7-dioxacyclotridecane-8,13-dione, which is the cyclic ester compound (II). After the reaction was completed, the pressure was returned to normal and the temperature was cooled to 80 ° C., and the solution was diluted with toluene to a solids content of 40% by mass, and then the toluene solution was added to methanol in an amount twice the total volume of the solution. The supernatant was discarded, and methanol in an amount equal to the amount of the toluene solution added was added again for washing. The supernatant was discarded, and the recovered insoluble matter was dried at 40°C using a vacuum dryer to remove organic volatiles, yielding a polymer composed of structural units (B') primarily composed of polyester units (b). Toluene was added again to the purified polymer composed of structural units (B') to dilute the toluene solution of the polymer composed of structural units (B') to a solids content of 33% by mass, and the temperature was then raised to 140°C to distill off 10% by mass of the toluene added, thereby dehydrating the system.Thereafter, the toluene solution of the polymer comprising the structural unit (B') was cooled to 80°C, and the polymer comprising the structural unit (B') and L-lactide were added so that the polymer comprising the structural unit (B') / L-lactide ratio was 50 / 50. The amount of toluene distilled off as described above was then added, and the solids content of the toluene solution of the polymer comprising the structural unit (B') and L-lactide was adjusted to 50% by mass. Then, when the temperature of the solution was raised to 100°C, tin octoate was added in an amount of 0.1% by mass relative to the polymer comprising the structural unit (B'), and the mixture was allowed to react for 4 hours to synthesize a block copolymer (I-1) comprising a block structural unit (A) mainly composed of polylactic acid units (a) and a block structural unit (B) mainly composed of polyester units (b), thereby obtaining a toluene solution of the block copolymer (I-1). This solution was further diluted with toluene to a solids content of 40% by mass, and the toluene solution with a solids content of 40% by mass described above was then added to methanol in an amount twice the total volume of the solution to precipitate a solid. The supernatant methanol was discarded, and methanol in the same amount as the toluene solution added was added again for washing. The methanol was discarded, and the recovered solid was dried in a vacuum dryer at 40°C to remove organic volatiles, yielding a block copolymer (I-1) consisting of block structural units (A) mainly composed of polylactic acid units (a) and block structural units (B) mainly composed of polyester units (b). The obtained block copolymer was subjected to the above-mentioned measurements and evaluations. The results are shown in Table 5. The resulting block copolymer (I-1), 4-methyl-1,7-dioxacyclotridecane-8,13-dione as the cyclic ester compound (II), and the polylactic acid polymer "INGEO 2500HP" (manufactured by NatureWorks Co., Ltd.) as the aliphatic polyester resin (III) were added to a kneader Labo Plastomill (manufactured by Toyo Seiki Seisaku-sho, Ltd., product name "3S150", roller mixer model "R60") in the mass ratios shown in Table 5, and melt-kneaded for 5 minutes at a cylinder temperature of 210 ° C. and a screw rotation speed of 50 rpm to obtain a resin composition. The resulting resin composition was subjected to the above-mentioned measurements and evaluations. The results are shown in Table 5.
[0115] Examples 14 to 17 Resin compositions were obtained by melt-kneading in the same manner as in Example 13, except that the mass ratio of 4-methyl-1,7-dioxacyclotridecane-8,13-dione, which is the cyclic ester compound (II), was changed to the amount shown in Table 5. The obtained resin compositions were subjected to the above-described measurements and evaluations. The results are shown in Table 5.
[0116] Example 18 Block copolymer (I-2) was obtained in the same manner as in Example 10, except that the number average molecular weight was adjusted by adjusting the reaction time during synthesis of the polymer consisting of structural unit (B') having polyester unit (b) as the main unit, the mass ratio of L-lactide used was changed, and the dilution concentration during synthesis was appropriately changed to a concentration that was easy to handle. The obtained block copolymer (I-2), 4-methyl-1,7-dioxacyclotridecane-8,13-dione as the cyclic ester compound (II), and the polylactic acid polymer "INGEO 2500HP" as the aliphatic polyester resin (III) were melt-kneaded in the same manner as in Example 13 to obtain a resin composition in the mass ratio shown in Table 5. The obtained resin composition was subjected to the above-mentioned measurements and evaluations. The results are shown in Table 5.
[0117] Example 19 A resin composition was obtained by melt-kneading in the same manner as in Example 18, except that 3-methyl-1,5-dioxacycloundecane-6,11-dione, a condensed cyclization product of 2-methyl-1,3-propanediol and adipic acid, was used instead of 4-methyl-1,7-dioxacyclotridecane-8,13-dione as the cyclic ester compound (II). The obtained resin composition was subjected to the above-described measurements and evaluations. The results are shown in Table 6.
[0118] Example 20 Block copolymer (I-3) was obtained in the same manner as in Example 15, except that 2-methyl-1,3-propanediol was used instead of 3-methyl-1,5-pentanediol, the number average molecular weight was adjusted by adjusting the reaction time during synthesis of the polymer composed of structural unit (B') having polyester units as the main unit, and the dilution concentration during synthesis was appropriately changed to a concentration that was easy to handle. The obtained block copolymer (I-3), 4-methyl-1,7-dioxacyclotridecane-8,13-dione as the cyclic ester compound (II), and the polylactic acid polymer "INGEO 2500HP" as the aliphatic polyester resin (III) were melt-kneaded in the same manner as in Example 18 to obtain a resin composition in the mass ratio shown in Table 1. The obtained resin composition was subjected to the above-mentioned measurements and evaluations. The results are shown in Table 6.
[0119] Example 21 A resin composition was obtained by melt-kneading the block copolymer (I-3) obtained in Example 20, 3-methyl-1,5-dioxacycloundecane-6,11-dione as the cyclic ester compound (II), and the polylactic acid polymer "INGEO 2500HP" as the aliphatic polyester resin (III) in the mass ratios shown in Table 5 in the same manner as in Example 20. The obtained resin composition was subjected to the above-described measurements and evaluations. The results are shown in Table 6.
[0120] Example 22 Block copolymer (I-4) was obtained in the same manner as in Example 18, except that 2,4-diethyl-1,5-pentanediol was used instead of 3-methyl-1,5-pentanediol, the number average molecular weight was adjusted by adjusting the reaction time during synthesis of the polymer composed of structural unit (B') having polyester units as the main unit, and the dilution concentration during synthesis was appropriately changed to a concentration that was easy to handle. The obtained block copolymer (I-4), 2,6-diethyl-1,7-dioxacyclotridecane-8,13-dione (a condensed cyclization product of 2,4-diethyl-1,5-pentanediol and adipic acid) as the cyclic ester compound (II), and the polylactic acid polymer "INGEO 2500HP" as the aliphatic polyester resin (III) were melt-kneaded in the same manner as in Example 18 to obtain a resin composition in the mass ratio shown in Table 6. The obtained resin composition was subjected to the above-mentioned measurements and evaluations. The results are shown in Table 6.
[0121] Example 23 Block copolymer (I-5) was obtained in the same manner as in Example 18, except that propylene glycol was used instead of 3-methyl-1,5-pentanediol, succinic acid was used instead of adipic acid, the number average molecular weight was adjusted by adjusting the reaction time during synthesis of the polymer consisting of structural unit (B') having polyester units as the main unit, and the dilution concentration during synthesis was appropriately changed to a concentration that was easy to handle. The obtained block copolymer (I-5), 2-methyl-1,4-dioxacycyclooctane-5,8-dione (a condensed cyclized product of propylene glycol and succinic acid) as the cyclic ester compound (II), and the polylactic acid polymer "INGEO 2500HP" as the aliphatic polyester resin (III) were melt-kneaded in the same manner as in Example 18 to obtain a resin composition in the mass ratio shown in Table 6. The obtained resin composition was subjected to the above-described measurements and evaluations. The results are shown in Table 6.
[0122] Example 24 Block copolymer (I-6) was obtained in the same manner as in Example 18, except that 1,4-butanediol was used instead of 3-methyl-1,5-pentanediol, succinic acid was used instead of adipic acid, the number average molecular weight was adjusted by adjusting the reaction time during synthesis of the polymer composed of structural unit (B') having polyester units as the main unit, and the dilution concentration during synthesis was appropriately changed to a concentration that was easy to handle. The obtained block copolymer (I-6), 1,6-dioxacyclodecane-7,10-dione (a condensed cyclized product of 1,4-butanediol and succinic acid) as the cyclic ester compound (II), and the polylactic acid polymer "INGEO 2500HP" as the aliphatic polyester resin (III) were melt-kneaded in the same manner as in Example 15 to obtain a resin composition in the mass ratio shown in Table 6. The obtained resin composition was subjected to the above-described measurements and evaluations. The results are shown in Table 6.
[0123] [Comparative Example 11] A resin composition was obtained by melt-kneading in the same manner as in Example 13, except that the cyclic ester compound (II) was not used. The obtained resin composition was subjected to the above-mentioned measurements and evaluations. The results are shown in Table 7.
[0124] [Comparative Example 12] A resin composition was obtained by melt-kneading in the same manner as in Example 18, except that the cyclic ester compound (II) was not used. The obtained resin composition was subjected to the above-mentioned measurements and evaluations. The results are shown in Table 7.
[0125] [Comparative Example 13] A resin composition was obtained by melt-kneading in the same manner as in Example 13, except that Di-n-alkyl Adipate (Plasticizer), an ester compound without a cyclic structure, was used instead of the cyclic ester compound (II). The obtained resin composition was subjected to the above-described measurements and evaluations. The results are shown in Table 7.
[0126] Comparative Example 14 A resin composition was obtained by melt-kneading in the same manner as in Example 13, except that N,N'-Ethylenebisoctadecanamide, a nucleating agent, was used instead of the cyclic ester compound (II). The obtained resin composition was subjected to the above-described measurements and evaluations. The results are shown in Table 7.
[0127] Comparative Example 15 A resin composition was obtained by melt-kneading in the same manner as in Example 13, except that the mass ratio of 4-methyl-1,7-dioxacyclotridecane-8,13-dione, which is the cyclic ester compound (II), was changed to the amount shown in Table 7. The obtained resin composition was subjected to the above-described measurements and evaluations. The results are shown in Table 7.
[0128]
[0129]
[0130]
[0131] The abbreviations in Tables 5 to 7 represent the following compounds: PLLA: Poly-L-lactic acid MPD: 3-methyl-1,5-pentanediol DEPD: 2,4-diethyl-1,5-pentanediol MPDiol: 2-methyl-1,3-propanediol 1,4-BD: 1,4-butanediol PG: Propylene glycol AA: Adipic acid SA: Succinic acid
[0132] As shown in Examples 13 to 24, the resin composition according to the second embodiment of the present invention, which contains a block copolymer (I) having a specific structure, an aliphatic polyester resin (III), and a cyclic ester compound (II), was confirmed to have an excellent balance of biodegradability, heat resistance, and transparency. On the other hand, the resin compositions obtained in Comparative Examples 11 and 12 were inferior in heat resistance because they did not contain the cyclic ester compound (II). The resin composition obtained in Comparative Example 13 was inferior in heat resistance because it contained an ester compound without a cyclic structure instead of the cyclic ester compound (II). The resin composition obtained in Comparative Example 14 was inferior in transparency because it contained a crystal nucleating agent instead of the cyclic ester compound (II). The resin composition obtained in Comparative Example 15 had a very low glass transition temperature and poor transparency due to the high content of the cyclic ester compound (II).
[0133] As shown in the results of Examples 13 to 24, the resin composition according to the second embodiment of the present invention has an excellent balance of biodegradability, heat resistance, and transparency. Therefore, the resin composition according to the second embodiment of the present invention is highly industrially useful.
Claims
1. A resin composition containing a block copolymer (I) and a cyclic ester compound (II), wherein the block copolymer (I) contains a block structural unit (A) mainly composed of a polylactic acid unit (a) and a block structural unit (B) mainly composed of a polyester unit (b) containing a unit derived from an aliphatic diol (b1) and an aliphatic dicarboxylic acid (b2), and the content of the cyclic ester compound (II) is 0.01 to 15 mass% relative to 100 mass% in total of the block copolymer (I) and the cyclic ester compound (II).
2. The resin composition according to claim 1, wherein the cyclic ester compound (II) contains a structure derived from an aliphatic diol (c1) and an aliphatic dicarboxylic acid (c2).
3. The resin composition according to claim 2, wherein the aliphatic diol (c1) and the aliphatic diol (b1) are the same, and the aliphatic dicarboxylic acid (c2) and the aliphatic dicarboxylic acid (b2) are the same.
4. The resin composition according to claim 1, wherein the aliphatic diol (b1) is an aliphatic diol having 4 or more carbon atoms and an alkyl group as a branched chain.
5. The resin composition according to claim 1, wherein the block copolymer (I) has a number average molecular weight of 2,000 to 200,000.
6. The resin composition according to claim 1, wherein the block structural unit (B) has a number average molecular weight of less than 80,000.
7. The resin composition according to claim 1, wherein the aliphatic dicarboxylic acid (b2) has 4 or more and 12 or less carbon atoms.
8. The resin composition according to claim 4, wherein the aliphatic diol (b1) has 9 or less carbon atoms.
9. The resin composition according to claim 4, wherein the branched chain in the aliphatic diol (b1) is a methyl group.
10. The resin composition according to claim 1, having a melting point of 110°C or higher and lower than 180°C.
11. The resin composition according to claim 1, further comprising an aliphatic polyester resin (III), the content of the cyclic ester compound (II) being 0.005 to 10 mass% relative to 100 mass% in total of the block copolymer (I), the cyclic ester compound (II), and the aliphatic polyester resin (III).
12. The resin composition according to claim 11, wherein the aliphatic polyester resin (III) is at least one selected from the group consisting of biomass resins and biodegradable resins.
13. The resin composition according to claim 11 or 12, wherein the aliphatic polyester resin (III) is a polylactic acid resin.
14. The resin composition according to claim 11, wherein the block copolymer (I) has a number average molecular weight of 5,000 to 400,000.
15. The resin composition according to claim 1 or 11, wherein the number average molecular weight of the block structural unit (B) is 1,000 or more and less than 300,000.
16. The resin composition according to claim 1 or 11, wherein the glass transition temperature of the block copolymer (I) is -80°C or higher and 15°C or lower.
17. The resin composition according to claim 1 or 11, wherein the glass transition temperature of the block copolymer (I) is -80°C or higher and -45°C or lower.
18. The resin composition according to claim 1 or 11, wherein the melting point of the block copolymer (I) is 110°C or higher and lower than 180°C.
19. The resin composition according to claim 1 or 11, wherein the block structural unit (A) contains a structural unit derived from poly-L-lactic acid or a structural unit derived from poly-D-lactic acid.
20. A resin composition according to claim 1 or 11, wherein the block structural unit (A) is 5% by mass or more and 95% by mass or less relative to 100% by mass of the total of the block structural unit (A) and the block structural unit (B).
Citation Information
Patent Citations
Production of transparent lactic acid copolyester, and packaging material
JP1996157577A
Impact resistance-imparting agent and polyester composition containing it
JP2001335623A
Polylactic acid resin composition
JP2015044984A
Polylactic acid resin composition
JP2018062573A
Production of lactic acid copolyester and packaging material
JP1995173266A
Cited By
Nonwoven fabric and method for producing same
WO2026048821A1