Polyol composition for producing rigid polyurethane foam
The polyol composition combining isophthalic acid-based polyester polyol, lignin, and phosphorus-based flame retardants addresses the semi-incombustibility and insulation challenges of rigid polyurethane foams, achieving improved fire safety and thermal performance.
Patent Information
- Application Number
- PCT/KR2024/004687
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-30
- Filing Date
- 2024-04-09
- Publication Date
- 2024-12-05
AI Technical Summary
Existing rigid polyurethane foams fail to meet enhanced semi-incombustibility evaluation standards for insulation materials, lacking sufficient flame retardancy and heat release reduction, which are critical for preventing fire spread in buildings.
A polyol composition comprising isophthalic acid-based polyester polyol, lignin, and phosphorus-based flame retardants, which improves dispersion stability, semi-incombustibility, and thermal insulation properties when combined with diphenylmethane diisocyanate, achieving specific particle size, polyisocyanurate, and residual diphenylmethane diisocyanate ratios.
The composition produces rigid polyurethane foam with excellent semi-incombustibility, reduced heat release rates, and enhanced thermal insulation, meeting stringent fire safety standards while maintaining dispersion stability and insulation efficiency.
Smart Images

Figure PCTKR2024004687-APPB-IMG-000001 
Figure PCTKR2024004687-APPB-IMG-000002 
Figure PCTKR2024004687-APPB-IMG-000003
Abstract
Description
Polyol composition for manufacturing rigid polyurethane foam
[0001] The present invention relates to a polyol composition for producing rigid polyurethane foam. More specifically, the present invention relates to a polyol composition for producing rigid polyurethane foam capable of producing rigid polyurethane foam having excellent dispersion stability, semi-non-flammability, and excellent insulation properties.
[0002]
[0003] Rigid polyurethane foam is one of the most sought-after insulation materials for industrial and thermal reasons. However, insulation is the most vulnerable to fire and heat among construction materials. Therefore, there are growing calls for strengthening standards for semi-combustibility (flame retardancy and reduction of hazardous gases) of insulation to prevent the spread of fire in the event of a fire.
[0004] In order to meet the strengthened quasi-combustibility evaluation standards for insulation materials, the heat release of the core material itself, excluding the face material (such as Al-GF film) surrounding the core material (such as rigid polyurethane foam), must meet the quasi-combustibility evaluation standards. However, existing rigid urethane foams cannot achieve the heat release rates that meet the quasi-combustibility evaluation standards.
[0005] Therefore, there is a need to develop a polyol composition for manufacturing rigid polyurethane foam with excellent flame retardancy (flame retardancy and reduction of harmful gases) and insulation properties.
[0006] The background technology of the present invention is disclosed in Korean Patent Publication No. 10-2009-0095889, etc.
[0007]
[0008] The purpose of the present invention is to provide a polyol composition for producing rigid polyurethane foam, which can produce rigid polyurethane foam having excellent dispersion stability, semi-non-combustibility, and excellent insulation properties.
[0009] The above and other objects of the present invention can all be achieved by the present invention described below.
[0010]
[0011] 1. One aspect of the present invention relates to a polyol composition for producing rigid polyurethane foam. The polyol composition for producing rigid polyurethane foam comprises an isophthalic acid-based polyester polyol; lignin; and a phosphorus-based flame retardant; and is characterized in that, after 7 days from production, the particle size of the dispersed phase measured with an optical microscope is about 30 ㎛ or less.
[0012] 2. In the above 1 specific example, the isophthalic acid-based polyester polyol can be represented by the following chemical formula 1:
[0013] [Chemical Formula 1]
[0014]
[0015] In the above chemical formula 1, L1 is a hydroxy group and A straight or branched chain alkylene group having 1 to 6 carbon atoms, which is substituted or unsubstituted with at least one of; or a hydroxy group and A straight or branched chain ether group having 2 to 6 carbon atoms, which is unsubstituted or substituted with at least one of; and L2 is a straight or branched chain alkylene group having 1 to 5 carbon atoms, which is unsubstituted or substituted with a hydroxy group; or a straight or branched chain ether group having 1 to 5 carbon atoms, which is unsubstituted or substituted with a hydroxy group; and m is an integer from 1 to 50 and n is an integer from 1 to 21.
[0016] 3. In the above 1 or 2 specific examples, the isophthalic acid-based polyester polyol may have a hydroxyl value (OH value) of about 10 to about 500 mgKOH / g.
[0017] 4. In the above 1 to 3 specific examples, the isophthalic acid-based polyester polyol may have a weight average molecular weight of about 200 to about 10,000 g / mol.
[0018] 5. In the above 1 to 4 specific examples, the phosphorus flame retardant may include at least one of a liquid phosphorus flame retardant including at least one of triethyl phosphate, diethylethylphosphonate, dimethylmethylphosphonate, dimethylpropylphosphonate, diphenylcresyl phosphate, and tricresyl phosphate; and a halogenated phosphorus flame retardant including at least one of tris(1-chloro-2-propyl)phosphate, tris(2-chloroethyl)phosphate, tris(1,3-dichloropropyl)phosphate, tris(2,3-dibromopropyl)phosphate, and tetrakis(2-chloroethyl)ethylenediphosphate.
[0019] 6. In the above 1 to 5 specific examples, the phosphorus flame retardant may include a liquid phosphorus flame retardant.
[0020] 7. In the above 1 to 6 specific examples, the phosphorus flame retardant may include a liquid phosphorus flame retardant and a halogenated phosphorus flame retardant.
[0021] 8. In the above 1 to 6 specific examples, the polyol composition for producing the rigid polyurethane foam may include about 100 parts by weight of the isophthalic acid-based polyester polyol; about 0.5 to about 7 parts by weight of the lignin; and about 15 to about 40 parts by weight of the phosphorus-based flame retardant.
[0022] 9. In the above 1 to 8 specific examples, the polyol composition for producing the rigid polyurethane foam may further include about 5 to about 40 parts by weight of a blowing agent with respect to about 100 parts by weight of the isophthalic acid-based polyester polyol.
[0023] 10. In the above 1 to 9 specific examples, the rigid polyurethane foam manufactured by mixing and reacting the polyol composition for manufacturing the rigid polyurethane foam and diphenylmethane diisocyanate may have a particle size of the dispersed phase of about 30 ㎛ or less in a 10 cm × 10 cm × 1 cm sized specimen measured with an optical microscope.
[0024] 11. In the above 1 to 10 specific examples, the weight ratio of the isophthalic acid-based polyester polyol and the diphenylmethane diisocyanate may be about 1:1.5 to about 1:3.
[0025] 12. In the above 1 to 11 specific examples, the rigid polyurethane foam may have a polyisocyanurate ratio (PIR ratio) of about 4.5 to about 7 according to the following formula 1, and a residual diphenylmethane diisocyanate ratio (MDI ratio) of about 0.1 to about 0.5 according to the following formula 2:
[0026] [Formula 1]
[0027] Polyisocyanurate ratio (PIR ratio) = PIR / (PUR + Urea + PIR + MDI)
[0028] [Formula 2]
[0029] Residual diphenylmethane diisocyanate ratio (MDI ratio) = MDI / (PUR + Urea + PIR + MDI)
[0030] In the above formulas 1 and 2, PUR + Urea + PIR + MDI is a phenyl group (1,565 to 1,625 cm) commonly included in polyurethane, urea, polyisocyanurate and diphenylmethane diisocyanate. -1 FT-IR absorbance value of the range), and PIR is the polyisocyanurate structure containing isocyanurate group (1,340 to 1,465 cm -1 FT-IR absorbance values of the range) and MDI is the isocyanate group (2,200 to 2,317 cm -1 FT-IR absorbance values of the range).
[0031] 13. In the above 1 to 12 specific examples, the rigid polyurethane foam has a heat release rate of about 3 to about 8 MJ / m measured using a cone calorimeter according to KS F ISO 5660-1. 2 It could be.
[0032] 14. In the above specific examples 1 to 13, the rigid polyurethane foam may have an average behavioral cessation time of about 9 minutes to about 12 minutes in a closed space in which combustion gas of the rigid polyurethane foam specimen is injected, as measured according to KS F 2271.
[0033] 15. In the above specific examples 1 to 14, the rigid polyurethane foam may have a thermal conductivity of about 0.017 to about 0.024 W / m·K as measured according to KS M 3809.
[0034]
[0035] The present invention has the effect of providing a polyol composition for manufacturing rigid polyurethane foam having excellent semi-non-combustibility, insulation properties, etc.
[0036]
[0037] Hereinafter, the present invention will be described in detail as follows.
[0038] A polyol composition for producing a rigid polyurethane foam according to the present invention comprises (A) an isophthalic acid-based polyester polyol; (B) lignin; and (C) a phosphorus-based flame retardant.
[0039] In this specification, “a to b” indicating a numerical range is defined as “≥a and ≤b”.
[0040]
[0041] (A) Isophthalic acid polyester polyol
[0042] According to one specific example of the present invention, an isophthalic acid-based polyester polyol has excellent reactivity with diphenylmethane isocyanate and can improve the semi-non-flammability, insulation, compressive strength, etc. of rigid polyurethane foam. An isophthalic acid-based polyester polyol represented by the following chemical formula 1 can be used.
[0043] [Chemical Formula 1]
[0044]
[0045] In the above chemical formula 1, L1 is a hydroxy group and A straight or branched chain alkylene group having 1 to 6 carbon atoms, which is substituted or unsubstituted with at least one of; or a hydroxy group and A straight or branched chain ether group having 2 to 6 carbon atoms, which is unsubstituted or substituted with at least one of; and L2 is a straight or branched chain alkylene group having 1 to 5 carbon atoms, which is unsubstituted or substituted with a hydroxy group; or a straight or branched chain ether group having 1 to 5 carbon atoms, which is unsubstituted or substituted with a hydroxy group; and m is an integer from 1 to 50 and n is an integer from 1 to 21.
[0046] In specific examples, L1 is -CH2-CH2-; -CH2-C(CH3)2-CH2-; -CH2-C(CH2CH3)(CH2OH)-CH2-; -CH2-CH(CH3)-CH2-; -CH2-CH2-O-CH2-CH2-; -CH2-CH2-O-CH2-CH2-O-CH2-CH2-; ; ; ; ; ; or , and n is an integer from 3 to 21.
[0047] In specific examples, L2 is -CH2-; -C(CH3)2-CH2-; -C(CH2CH3)(CH2OH)-CH2-; -CH(CH3)-CH2-; -CH2-OCH2-CH2-; or -CH2-O-CH2-CH2-O-CH2-CH2-.
[0048] In a specific example, L1 may be -CH2-CH2- and L2 may be -CH2-.
[0049] In a specific example, the isophthalic acid-based polyester polyol can be produced by reacting isophthalic acid and an alcohol represented by the following chemical formula 2 to produce a polyol represented by the following chemical formula 3, and by reacting the polyol represented by the following chemical formula 3 with a compound represented by the following chemical formula 4.
[0050] [Chemical Formula 2]
[0051]
[0052] [Chemical Formula 3]
[0053]
[0054] [Chemical Formula 4]
[0055]
[0056] In the above chemical formulas 2 to 4, L3 is a straight or branched chain alkylene group having 2 to 6 carbon atoms, substituted or unsubstituted with a hydroxy group; or a straight or branched chain ether group having 2 to 6 carbon atoms, substituted or unsubstituted with a hydroxy group, m is an integer from 1 to 50, and n is an integer from 3 to 21.
[0057] In a specific example, the compound represented by the above chemical formula 2 may be added in a ratio of about 1.1 mol to about 2.5 mol per 1 mol of the above isophthalic acid, and the reaction of the isophthalic acid and the alcohol represented by the above chemical formula 2 may be performed under atmospheric pressure and about 140 to about 240°C.
[0058] In a specific example, the compound represented by the above chemical formula 4 may be added in a ratio of about 0.01 mol to about 0.1 mol with respect to 1 mol of the polyol represented by the above chemical formula 3, and the reaction of the compound represented by the above chemical formula 4 and the polyol represented by the above chemical formula 3 may be performed in the presence of an acid-base catalyst under conditions of atmospheric pressure and about 100 to about 220°C.
[0059] In a specific example, the isophthalic acid-based polyester polyol may have a hydroxyl value (OH value) of about 10 to about 500 mgKOH / g as measured according to JIS K1557-1:2007. Within this range, a required rigid polyurethane foam can be formed.
[0060] In a specific example, the isophthalic acid-based polyester polyol may have a weight average molecular weight of about 200 to about 10,000 g / mol as measured by gel permeation chromatography (GPC).
[0061]
[0062] (B) Lignin
[0063] According to one specific example of the present invention, lignin can be applied as a polyol composition with isophthalic acid-based polyester polyol, phosphorus-based flame retardant, etc., to improve the semi-non-combustibility, insulation, etc. of rigid urethane foam, and can be applied in a solution state together with the phosphorus-based flame retardant.
[0064] In a specific example, the lignin may be in the form of granules, powder, etc. When the lignin is in the form of granules, the particle size may be about 3 mm or less, and when the lignin is in the form of powder, the particle size may be about 200 μm or less. When the lignin is completely dissolved in a solution with triethyl phosphate, the particle size in the solution may be less than about 1 μm. Within the above range, the rigid polyurethane foam may have excellent semi-combustibility, rigidity, etc.
[0065] In a specific example, the presence or absence of lignin in the rigid polyurethane foam can be confirmed through Pyrolyzer-Gas chromatography / Mass spectrometry (Py-GC / MS) analysis. In the chemical analysis results, the presence or absence of peaks of methoxy phenol, methoxy cresol, and methoxy vinylphenol, which are some of the lignin-containing substances, can be confirmed, thereby confirming whether lignin is applied to the rigid polyurethane foam.
[0066] In a specific example, the lignin may be included in an amount of about 0.5 to about 7 parts by weight, for example, about 1 to about 3 parts by weight, based on about 100 parts by weight of the isophthalic acid-based polyester polyol. Within this range, the rigid urethane foam may have excellent semi-combustibility, rigidity, etc.
[0067]
[0068] (C) Inherited flame retardant
[0069] According to one specific example of the present invention, a phosphorus-based flame retardant is applied as a polyol composition with isophthalic acid-based polyester polyol and lignin, etc., and can improve the semi-non-combustibility, insulation, etc. of rigid urethane foam. A conventional phosphorus-based flame retardant applied to urethane foam, etc. can be used, and can be applied in a solution state together with the lignin.
[0070] In a specific example, the phosphorus flame retardant may be a liquid phosphorus flame retardant such as triethyl phosphate, diethyl ethyl phosphonate, dimethyl methyl phosphonate, dimethyl propyl phosphonate, diphenyl cresyl phosphate, tricresyl phosphate, or a combination thereof; and a halogenated phosphorus flame retardant such as tris(1-chloro-2-propyl) phosphate, tris(2-chloroethyl) phosphate, tris(1,3-dichloropropyl) phosphate, tris(2,3-dibromopropyl) phosphate, tetrakis(2-chloroethyl) ethylene diphosphate, or a combination thereof; used alone or in combination of two or more thereof. For example, a liquid phosphorus flame retardant alone or a combination of a liquid phosphorus flame retardant and a halogenated phosphorus flame retardant may be used. Specifically, triethyl phosphate (TEP) alone or a combination of triethyl phosphate (TEP) and tris(1-chloro-2-propyl)phosphate (TCPP) may be used, but is not limited thereto.
[0071] In a specific example, the lignin and the liquid phosphorus-based flame retardant may have a weight ratio of about 1:2.5 to about 1:15. Within this range, the lignin and the liquid phosphorus-based flame retardant may be applied to the polyol composition in a solution state.
[0072] In a specific example, when the weight ratio of the lignin and the liquid phosphorus flame retardant is about 1:7, the combined amount of the lignin and the triethyl phosphate may be about 20 to about 25 parts by weight with respect to about 100 parts by weight of polyol. Within this range, the formability and semi-flammability of the rigid urethane foam may be excellent.
[0073] In a specific example, the phosphorus flame retardant may be included in an amount of about 15 to about 40 parts by weight, for example, about 17 to about 35 parts by weight, based on about 100 parts by weight of the isophthalic acid-based polyester polyol. Within this range, the formability and semi-flammability of the rigid urethane foam may be excellent.
[0074] In a specific example, when the phosphorus-based flame retardant is a combination (mixture) of a liquid phosphorus-based flame retardant and a halogenated phosphorus-based flame retardant, the liquid phosphorus-based flame retardant may be included in an amount of about 15 to about 30 parts by weight, for example, about 15 to about 25 parts by weight, based on about 100 parts by weight of the isophthalic acid-based polyester polyol, and the halogenated phosphorus-based flame retardant may be included in an amount of about 2 to about 8 parts by weight, for example, about 4 to about 6 parts by weight, based on about 100 parts by weight of the isophthalic acid-based polyester polyol. In the above range, the semi-non-combustibility, processability, etc. of the rigid polyurethane foam may be excellent.
[0075]
[0076] (D) Foaming agent
[0077] A polyol composition for producing a rigid polyurethane foam according to one specific embodiment of the present invention may further include a blowing agent. The blowing agent may be applied to the polyol composition together with an isophthalic acid-based polyester polyol, lignin, a phosphorus-based flame retardant, etc., so as to function as a blowing agent without hindering the insulation properties of the rigid polyurethane foam or causing problems with moldability, processability, etc., and a conventional blowing agent used in rigid polyurethane foam may be used.
[0078] In specific examples, the blowing agent may be 1-chloro-3,3,3-trifluoropropene (LBA), cyclopentane (CP), HFC series blowing agents (HFC-141b (1,1-dichloro-1-fluoroethane), HFC-245fa (1,1,1,3,3-pentafluoropropane), HFC-365mfc (1,1,1,3,3-pentafluorobutane), etc.), combinations thereof, etc.
[0079] In a specific example, the blowing agent may be 1-chloro-3,3,3-trifluoropropene (LBA) alone, or a mixture of 1-chloro-3,3,3-trifluoropropene (LBA) and cyclopentane (CP). The mixing ratio of 1-chloro-3,3,3-trifluoropropene (LBA) and cyclopentane (CP) may be from about 3:1 to about 10:1, but is not limited thereto.
[0080] In a specific example, the content of the foaming agent may be about 5 to about 40 parts by weight, for example, about 10 to about 35 parts by weight, based on about 100 parts by weight of the isophthalic acid-based polyester polyol. The amount (content) of the foaming agent may be varied to control the free foaming density of the rigid polyurethane foam, and within the above range, the insulation properties and foaming efficiency may be excellent.
[0081]
[0082] A polyol composition according to one embodiment of the present invention may further include additives used in conventional polyol compositions, as long as they do not impair the purpose and effects of the present invention. Examples of the additives include, but are not limited to, a foam stabilizer, a surface-active substance, a foam stabilizer, a cell regulator, a filler, a dye, a pigment, and combinations thereof. When the additives are used, the content thereof may be about 0.001 to about 40 parts by weight, for example, about 0.05 to about 25 parts by weight, based on about 100 parts by weight of the isophthalic acid-based polyester polyol.
[0083]
[0084] A polyol composition according to one specific example of the present invention may include a continuous phase (components excluding lignin) and a dispersed phase (lignin), and the particle size of the dispersed phase measured with an optical microscope after 7 days from the preparation of the polyol composition is about 30 ㎛ or less (the dispersed phase may appear non-existent). If the particle size is outside the above range, the dispersion stability of the polyol composition may be reduced, and there is a concern that the semi-non-combustibility (flame retardancy and reduction of harmful gases), insulation properties, etc. of the rigid polyurethane foam prepared therefrom may be reduced.
[0085]
[0086] A polyol composition for producing a rigid polyurethane foam according to one specific example of the present invention can form a rigid polyurethane foam by reacting with diphenylmethane diisocyanate (MDI). As the diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate (P-MDI) or the like can be used.
[0087] In a specific example, the rigid polyurethane foam can be manufactured by mixing and reacting the polyol composition for manufacturing the rigid polyurethane foam and the diphenylmethane diisocyanate.
[0088] In a specific example, the weight ratio of the isophthalic acid-based polyester polyol and the diphenylmethane diisocyanate may be from about 1:1.5 to about 1:3, for example, from about 1:1.7 to about 1:2.3. Within the above range, a rigid polyurethane foam having the following polyisocyanurate ratio (PIR ratio) and residual diphenylmethane diisocyanate ratio (MDI ratio) can be formed, with reduced gas toxicity and excellent semi-non-flammability, insulation, rigidity, etc.
[0089] In a specific example, the reaction is carried out in the presence of a catalyst including an organometallic catalyst, at a temperature condition of about 30 to about 70° C., for example, about 40 to about 50° C., and at a pressure of about 0.8 to about 1.5 kgf / cm. 2 , for example, about 0.9 to about 1.2 kgf / cm 2 It can be performed under pressure conditions. In the above range, a rigid polyurethane foam having the polyisocyanurate ratio (PIR ratio) and the residual diphenylmethane diisocyanate ratio (MDI ratio) can be obtained, and the rigid polyurethane foam can have excellent semi-combustibility, insulation, rigidity, etc.
[0090] In specific examples, examples of the organometallic catalyst include potassium-2-ethylhexanoate, tin(II)2-ethylhexanoate, and combinations thereof. In addition, examples of catalysts that can be used together with the organometallic catalyst include amine catalysts such as pentamethyldiethylenetriamine (PMDETA) and N,N-dimethylcyclohexylamine (DMCHA).
[0091] In a specific example, the rigid polyurethane foam may include a continuous phase (components excluding lignin) and a dispersed phase (lignin), and the particle size of the dispersed phase in a 10 cm × 10 cm × 1 cm sample measured with an optical microscope is about 30 ㎛ or less (the dispersed phase may appear non-existent). If the above range is exceeded, there is a concern that the semi-non-combustibility (flame retardancy and reduction of harmful gases), insulation, etc. of the rigid polyurethane foam may be reduced.
[0092] In a specific example, the rigid urethane foam may include a polyurethane structure (urethane reaction), an isocyanurate structure (trimerization reaction), a urea structure (urea reaction), etc., by the reaction of the polyol composition for producing the rigid urethane foam and the diphenylmethane diisocyanate, and the polyisocyanurate ratio (PIR ratio) according to the following formula 1 may be about 4.5 to about 7, for example, about 4.8 to about 6.5, and the residual diphenylmethane diisocyanate ratio (MDI ratio) according to the following formula 2 may be about 0.1 to about 0.5, for example, about 0.1 to about 0.3.
[0093] [Formula 1]
[0094] Polyisocyanurate ratio (PIR ratio) = PIR / (PUR + Urea + PIR + MDI)
[0095] [Formula 2]
[0096] Residual diphenylmethane diisocyanate ratio (MDI ratio) = MDI / (PUR + Urea + PIR + MDI)
[0097] In the above formulas 1 and 2, PUR + Urea + PIR + MDI is a phenyl group (1,565 to 1,625 cm) commonly included in polyurethane, urea, polyisocyanurate and diphenylmethane diisocyanate. -1 FT-IR absorbance value of the range), and PIR is the polyisocyanurate structure containing isocyanurate group (1,340 to 1,465 cm-1 FT-IR absorbance values of the range) and MDI is the isocyanate group (2,200 to 2,317 cm -1 FT-IR absorbance values of the range).
[0098] Within the above polyisocyanurate ratio (PIR ratio) range, it can have excellent semi-non-combustibility (flame retardancy and reduction of harmful gases), insulation, and rigidity.
[0099] Within the above residual diphenylmethane diisocyanate ratio (MDI ratio) range, semi-non-combustibility (flame retardancy and reduction of harmful gases), insulation, rigidity, etc. can be excellent.
[0100] In a specific example, the rigid polyurethane foam has a density of about 30 to about 50 kg / m as measured according to JIS K7222. 3 , for example, about 35 to about 45 kg / m 3 It could be.
[0101] In a specific example, the rigid polyurethane foam has a heat release rate of about 3 to about 8 MJ / m measured using a cone calorimeter according to KS F ISO 5660-1. 2 , for example, about 4 to about 7 MJ / m 2 It could be.
[0102] In a specific example, the rigid polyurethane foam may have an average behavioral cessation time of about 9 minutes to about 12 minutes, for example, about 9 minutes 30 seconds to about 11 minutes, of experimental mice in a closed space injected with combustion gas of the rigid polyurethane foam specimen measured according to KS F 2271.
[0103] In a specific example, the rigid polyurethane foam may have a thermal conductivity of about 0.017 to about 0.024 W / m·K, for example, about 0.018 to about 0.023 W / m·K, as measured according to KS M 3809.
[0104]
[0105] Hereinafter, the present invention will be described in more detail through examples; however, these examples are for the purpose of explanation only and should not be construed as limiting the present invention.
[0106]
[0107] Example
[0108] Below, the specifications of each component used in the examples and comparative examples are as follows.
[0109] (A) Isophthalic acid polyester polyol
[0110] Isophthalic acid polyester polyol (Manufacturer: Lotte Chemical, Product name: FIP-2210) was used.
[0111] (B) Lignin
[0112] Lignin (Manufacturer: Stora Enso, Product Name: Lineo) was used.
[0113] (C) Inherited flame retardant
[0114] (C1) Triethyl phosphate (Manufacturer: Kempia, Product name: Triethyl phosphate) was used.
[0115] (C2) Tris(1-chloro-2-propyl)phosphate (Manufacturer: Nanochem, Product name: 1-chloro-2-propanol phosphate) was used.
[0116] (D) Foaming agent
[0117] (D1) 1-Chloro-3,3,3-trifluoropropene (Manufacturer: Honeywell, Product name: Solstice LBA) was used.
[0118] (D2) Cyclopentane (CP, manufacturer: Yeocheon NCC, product name: cyclo-pentane) was used.
[0119] (E) Diphenylmethane diisocyanate
[0120] (E1) 4,4'-diphenylmethane diisocyanate (P-MDI, manufacturer: BASF, product name: LUPRANATE M50) was used.
[0121] (E2) 4,4'-diphenylmethane diisocyanate (P-MDI, manufacturer: BASF, product name: LUPRANATE M20S) was used.
[0122]
[0123] Examples 1 to 3 and Comparative Example 1
[0124] Lignin (B) and phosphorus-based flame retardant (C) were added in a solution state to polyester polyol (A) and blowing agent (D) in the amounts as described in Table 1 below, and mixed to prepare a polyol composition for manufacturing rigid polyurethane foam, and then, in the presence of a catalyst including potassium 2-ethylhexanoate, at a temperature condition of about 50°C and a pressure of about 1.0 kgf / cm 2 Under pressure conditions, diphenylmethane diisocyanate (E) was mixed into the polyol composition for producing rigid polyurethane foam and reacted (freely foamed) to produce rigid polyurethane foam. The physical properties of the produced rigid polyurethane foam were evaluated using the following method, and the results are shown in Table 1 below.
[0125]
[0126] Comparative Example 2
[0127] A polyol composition for manufacturing rigid polyurethane foam was manufactured by simply mixing polyester polyol (A), lignin (B), phosphorus flame retardant (C), and blowing agent (D) in the contents as described in Table 1 below, and then, in the presence of a catalyst including potassium 2-ethylhexanoate, at a temperature condition of about 50°C and a pressure of about 1.0 kgf / cm 2 Under pressure conditions, diphenylmethane diisocyanate (E) was mixed into the polyol composition for producing rigid polyurethane foam, and the mixture was reacted (freely foamed) to produce rigid polyurethane foam. The physical properties of the produced rigid polyurethane foam were evaluated using the following method, and the results are shown in Table 1 below.
[0128]
[0129] Method of measuring physical properties
[0130] (1) Dispersed phase particle size of polyol composition (unit: ㎛): After preparing the polyol compositions of the examples and comparative examples, they were sealed and left for 7 days, and then one drop of each polyol composition was dropped on a slide glass, and a transparent cover glass measuring 2.5 cm × 2.5 cm was covered thereon, and the dispersed phase particle size was measured using an optical microscope (magnification: 10 to 20 times).
[0131] (2) Dispersed phase particle size of rigid polyurethane foam (unit: ㎛): The dispersed phase particle size was measured in a 10 cm × 10 cm × 1 cm sized specimen using an optical microscope (magnification: 10 to 20 times).
[0132] (3) Polyisocyanurate ratio (PIR ratio) and residual diphenylmethane diisocyanate ratio (MDI ratio): The polyisocyanurate ratio and residual diphenylmethane diisocyanate ratio of the rigid polyurethane foam were calculated according to the following equations 1 and 2.
[0133] [Formula 1]
[0134] Polyisocyanurate ratio (PIR ratio) = PIR / (PUR + Urea + PIR + MDI)
[0135] [Formula 2]
[0136] Residual diphenylmethane diisocyanate ratio (MDI ratio) = MDI / (PUR + Urea + PIR + MDI)
[0137] In the above formulas 1 and 2, PUR + Urea + PIR + MDI is a phenyl group (1,565 to 1,625 cm) commonly included in polyurethane, urea, polyisocyanurate and diphenylmethane diisocyanate. -1FT-IR absorbance value of the range), and PIR is the polyisocyanurate structure containing isocyanurate group (1,340 to 1,465 cm -1 FT-IR absorbance values of the range) and MDI is the isocyanate group (2,200 to 2,317 cm -1 FT-IR absorbance values of the range).
[0138] Here, FT-IR measurements were taken using the ATR mode of the iS50 model IR measuring instrument, a Thermo Scientific product, and were performed at 8 cm -1 At a resolution of 400 to 4,000 cm -1 The section was measured at room temperature. Specifically, the cross-section of the polyurethane foam specimen was brought into contact with the diamond cell of the ATR, and the screw at the top was turned so that the cross-section was in close contact with the measuring device, and then the measurement was performed. After the FT-IR measurement, the spectrum was measured using OMNIC Spectra software, and the absorbance peak value (FT-IR absorbance value) in the specified wavelength range was measured.
[0139] (4) Heat release rate (unit: MJ / m) 2 ): According to KS F ISO 5660-1, the heat release rate of rigid polyurethane foam specimens was measured using a cone calorimeter (manufacturer: FESTEC, device name: Cone Calorimeter).
[0140] (5) Gas toxicity assessment: According to KS F 2271, the average behavioral cessation time of laboratory mice was measured in a closed space injected with combustion gas from a rigid polyurethane foam specimen.
[0141] (6) Thermal conductivity (unit: W / m·K): The thermal conductivity of rigid polyurethane foam specimens was measured according to KS M 3809.
[0142]
[0143] Comparative Example 12312 (A) (parts by weight) 100 100 100 100 100 (B) (parts by weight) 1.5 1.5 1.5 - 1.5 (C1) (parts by weight) 20 20 20 20 20 (C2) (parts by weight) 5.5 5.5 5.5 5.5 5.5 5.5 (D1) (parts by weight) 3 1 1 8.5 3 1 3 1 3 1 (D2) (parts by weight) - 8.5 --- (E1) (parts by weight) 18 2 1 8 2 - 18 2 1 8 2 (E2) (parts by weight) -- 18 2 -- Dispersed phase particle size of polyol composition (㎛) ≤ 30 ≤ 30 ≤ 30 ≤ 30 ≥ 600 Dispersed phase particle size of rigid polyurethane foam (㎛) ≤ 30 ≤ 30 ≤ 30 ≤ 30 ≥ 600 PIR ratio5.75.85.65.45.8MDI ratio0.20.20.20.20.2Heat release rate (MJ / m 2 )5.57.05.85.86.0 Gas toxicity assessment10 minutes 3 seconds9 minutes 40 seconds9 minutes 30 seconds7 minutes 30 seconds7 minutes 45 seconds Thermal conductivity (W / m K)0.0180.0210.0180.0190.019
[0144]
[0145] From the above results, it can be seen that the polyol composition for manufacturing rigid polyurethane foam of the present invention has excellent dispersion stability (particle size of the dispersed phase) even after 7 days from manufacturing, and the rigid urethane foam manufactured therefrom has excellent semi-non-combustibility (reduced heat release rate, reduced gas toxicity), insulation (thermal conductivity), etc.
[0146] On the other hand, in the case of Comparative Example 1 where lignin was not applied, it can be seen that the semi-non-combustibility (gas toxicity) etc. is reduced, and in the case of Comparative Example 2 where lignin and phosphorus flame retardant were not applied in a solution state, it can be seen that the dispersion stability of the polyol composition for manufacturing rigid polyurethane foam is reduced, and it can be seen that the particle size of the dispersed phase including lignin exceeds the upper limit of the present invention, and the semi-non-combustibility (gas toxicity) etc. is reduced.
[0147]
[0148] The present invention has been described above, focusing on specific embodiments. Those skilled in the art will appreciate that the present invention can be implemented in modified forms without departing from its essential characteristics. Therefore, the disclosed embodiments should be considered illustrative rather than limiting. The scope of the present invention is set forth in the claims, not the foregoing description, and all differences within the scope equivalent thereto should be construed as being encompassed by the present invention.
Claims
1. Isophthalic acid polyester polyol; lignin; and Including flame retardants; A polyol composition for manufacturing a rigid polyurethane foam, characterized in that the particle size of the dispersed phase measured with an optical microscope is about 30 ㎛ or less after 7 days from manufacturing.
2. In the first paragraph, the isophthalic acid-based polyester polyol is a polyol composition for producing a rigid polyurethane foam, characterized in that it is represented by the following chemical formula 1: [Chemical Formula 1] In the above chemical formula 1, L1 is a hydroxy group and A straight or branched chain alkylene group having 1 to 6 carbon atoms, which is substituted or unsubstituted with at least one of; or a hydroxy group and A straight or branched chain ether group having 2 to 6 carbon atoms, which is unsubstituted or substituted with at least one of; and L2 is a straight or branched chain alkylene group having 1 to 5 carbon atoms, which is unsubstituted or substituted with a hydroxy group; or a straight or branched chain ether group having 1 to 5 carbon atoms, which is unsubstituted or substituted with a hydroxy group; and m is an integer from 1 to 50 and n is an integer from 1 to 21.
3. A polyol composition for producing rigid polyurethane foam, characterized in that the isophthalic acid-based polyester polyol in claim 1 or 2 has a hydroxyl value (OH value) of about 10 to about 500 mgKOH / g.
4. A polyol composition for producing rigid polyurethane foam, characterized in that the isophthalic acid-based polyester polyol according to any one of claims 1 to 3 has a weight average molecular weight of about 200 to about 10,000 g / mol.
5. A polyol composition for producing a rigid polyurethane foam, characterized in that the phosphorus-based flame retardant according to any one of claims 1 to 4, comprises at least one of a liquid phosphorus-based flame retardant comprising at least one of triethyl phosphate, diethylethylphosphonate, dimethylmethylphosphonate, dimethylpropylphosphonate, diphenylcresyl phosphate, and tricresyl phosphate; and a halogenated phosphorus-based flame retardant comprising at least one of tris(1-chloro-2-propyl)phosphate, tris(2-chloroethyl)phosphate, tris(1,3-dichloropropyl)phosphate, tris(2,3-dibromopropyl)phosphate, and tetrakis(2-chloroethyl)ethylenediphosphate.
6. A polyol composition for producing rigid polyurethane foam, characterized in that the phosphorus-based flame retardant according to any one of claims 1 to 5 comprises a liquid phosphorus-based flame retardant.
7. A polyol composition for producing rigid polyurethane foam, characterized in that the phosphorus flame retardant according to any one of claims 1 to 6 comprises a liquid phosphorus flame retardant and a halogenated phosphorus flame retardant.
8. A polyol composition for producing a rigid polyurethane foam, characterized in that the polyol composition for producing a rigid polyurethane foam according to any one of claims 1 to 7, comprises about 100 parts by weight of the isophthalic acid-based polyester polyol; about 0.5 to about 7 parts by weight of the lignin; and about 15 to about 40 parts by weight of the phosphorus-based flame retardant.
9. A polyol composition for producing a rigid polyurethane foam, characterized in that the polyol composition for producing a rigid polyurethane foam according to any one of claims 1 to 8 further comprises about 5 to about 40 parts by weight of a blowing agent relative to about 100 parts by weight of the isophthalic acid-based polyester polyol.
10. In the 9th paragraph, the polyol composition for producing rigid polyurethane foam and the rigid polyurethane foam produced by mixing and reacting diphenylmethane diisocyanate are characterized in that the particle size of the dispersed phase in a 10 cm × 10 cm × 1 cm sized specimen measured with an optical microscope is about 30 ㎛ or less.
11. A polyol composition for producing rigid polyurethane foam, characterized in that the weight ratio of the isophthalic acid-based polyester polyol and the diphenylmethane diisocyanate in the 10th paragraph is about 1:1.5 to about 1:
3.
12. A polyol composition for producing a rigid polyurethane foam according to claim 10 or 11, characterized in that the polyol composition for producing a rigid polyurethane foam has a polyisocyanurate ratio (PIR ratio) of about 4.5 to about 7 according to the following formula 1, and a residual diphenylmethane diisocyanate ratio (MDI ratio) of about 0.1 to about 0.5 according to the following formula 2: [Formula 1] Polyisocyanurate ratio (PIR ratio) = PIR / (PUR + Urea + PIR + MDI) [Formula 2] Residual diphenylmethane diisocyanate ratio (MDI ratio) = MDI / (PUR + Urea + PIR + MDI) In the above formulas 1 and 2, PUR + Urea + PIR + MDI is a phenyl group (1,565 to 1,625 cm) commonly included in polyurethane, urea, polyisocyanurate and diphenylmethane diisocyanate. -1 FT-IR absorbance value of the range), and PIR is the polyisocyanurate structure containing isocyanurate group (1,340 to 1,465 cm -1 FT-IR absorbance values of the range) and MDI is the isocyanate group (2,200 to 2,317 cm -1 FT-IR absorbance values of the range).
13. In any one of the 10th to 12th clauses, the rigid polyurethane foam has a heat release rate of about 3 to about 8 MJ / m measured by a cone calorimeter according to KS F ISO 5660-1. 2 A polyol composition for producing rigid polyurethane foam, characterized by:
14. A polyol composition for manufacturing a rigid polyurethane foam, characterized in that the rigid polyurethane foam according to any one of claims 10 to 13 has an average behavioral cessation time of about 9 to about 12 minutes in a closed space in which combustion gas of a rigid polyurethane foam specimen is injected, as measured according to KS F 2271.
15. A polyol composition for producing a rigid polyurethane foam, characterized in that the rigid polyurethane foam has a thermal conductivity of about 0.017 to about 0.024 W / m·K as measured according to KS M 3809, in any one of the claims 10 to 14.
Citation Information
Patent Citations
Incombustible, heat-insulating foamed polyurethane building material
JP2006326943A
A composition in the form of a dispersion comprising a lignin, a method for the manufacturing thereof and use thereof
KR1020150017359A
Rigid polyurethane foam and preparation method thereof
KR1020160062559A
Bio-polyol composition and bio-polyurethane foam material
US20150183948A1
Rigid polyurethane foam and manufacturing method therefor
WO2023277362A1