Magnesium oxide-based composite and method for preparing same

The magnesium oxide-based composite with ytterbium enhances hygroscopic resistance and stability by incorporating ytterbium into the magnesium oxide crystal structure, addressing the limitations of existing magnesium oxide fillers in semiconductor encapsulation and improving heat dissipation in electronic devices.

WO2024248318A1PCT designated stage expired Publication Date: 2024-12-05SOULMATERIAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/004980
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-02
Filing Date
2024-04-12
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Magnesium oxide-based fillers for semiconductor encapsulation suffer from low hygroscopic resistance, leading to moisture absorption and degradation of physical properties, which affects heat dissipation and stability in high-power electronic devices.

Method used

A magnesium oxide-based composite incorporating ytterbium (Yb) element and magnesium oxide crystal grains, with ytterbium oxide added as a precursor, is synthesized through a process involving sintering and dispersion in a polymer matrix to enhance hygroscopic resistance and reduce manufacturing costs.

Benefits of technology

The composite exhibits improved moisture absorption resistance, maintaining physical property stability and reducing weight increase rates during testing, while allowing for lower sintering temperatures and broader application in electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024004980_05122024_PF_FP_ABST
    Figure KR2024004980_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a magnesium oxide-based composite comprising an ytterbium (Yb) element and magnesium oxide (MgO) crystal grains, and a method for preparing same.
Need to check novelty before this filing date? Find Prior Art

Description

Magnesium oxide-based composite and method for producing the same

[0001] The present invention relates to a magnesium oxide-based composite and a method for producing the same.

[0002] Electronic devices are composed of electronic components such as laminates, printed wiring boards, and multilayer wiring boards. Recent electronic devices are equipped with large-capacity power elements and manufactured with high-density internal structures, requiring higher levels of heat dissipation and moisture resistance than before. Silica and alumina have been primarily used as fillers in existing semiconductor encapsulation resin compositions. However, silica's low thermal conductivity makes it insufficient for the increased heat generation resulting from increased integration, power, and speed, posing a problem for the stable operation of semiconductors. Meanwhile, alumina, which has a higher thermal conductivity than silica, improves heat dissipation, but its excessively high hardness leads to increased wear on kneaders, molding machines, and molds.

[0003] Accordingly, magnesium oxide, which has higher thermal conductivity than silica and alumina, is being considered as a material for resin fillers for semiconductor encapsulation. However, magnesium oxide powder has a problem in that it has a higher hygroscopicity than silica powder, making it difficult to maintain stable physical properties. Specifically, when magnesium oxide powder is used as a resin filler for semiconductor encapsulation, the magnesium oxide reacts with moisture in the air to form magnesium hydroxide on the surface of the magnesium oxide, which causes the volume of the filler to expand, resulting in problems such as cracking and reduced thermal conductivity. Therefore, research is needed to improve the hygroscopicity of magnesium oxide to ensure long-term physical property stability.

[0004] [Prior Art Literature]

[0005] Republic of Korea Patent Publication No. 10-1878963

[0006] The present invention aims to provide a magnesium oxide-based composite and a method for manufacturing the same, which can improve the low moisture absorption resistance of existing magnesium oxide and secure long-term physical property stability.

[0007] However, the technical problems to be solved by the present invention are not limited to the problems mentioned above, and other problems not mentioned can be clearly understood by those skilled in the art from the description below.

[0008] One embodiment of the present invention provides a magnesium oxide-based composite comprising ytterbium (Yb) element and magnesium oxide (MgO) crystal grains.

[0009] Another embodiment of the present invention provides a method for producing the magnesium oxide-based composite. Specifically, the method comprises the steps of: (A) producing a sintering mixture comprising magnesium oxide or a magnesium oxide precursor and ytterbium oxide; (B) pretreating the sintering mixture, including at least one of coating, granulating, press molding, and injection molding; and (C) sintering the sintering mixture to crystallize it.

[0010] Another embodiment of the present invention provides an organic-inorganic composite in which particles composed of the magnesium oxide-based composite are dispersed within a polymer matrix.

[0011] A magnesium oxide-based composite according to one embodiment of the present invention has excellent moisture absorption resistance, and can solve problems such as deterioration of physical properties due to low moisture absorption resistance of existing magnesium oxide.

[0012] The effects of the present invention are not limited to the effects mentioned above, and other effects not mentioned will be clearly understood by those skilled in the art from the description below.

[0013] Figure 1 shows an example of evaluation criteria according to sintering temperature according to examples and comparative examples.

[0014] Figure 2 shows the weight increase rate after the moisture absorption test according to the content of Yb2O3 and the sintering temperature in Examples 1 to 11.

[0015] Figure 3 shows SEM images of composites according to Examples 6 to 11 at a sintering temperature of 1,550°C.

[0016] Figure 4 shows the results of surface EDS analysis at the crystal grain position of a composite manufactured according to an example.

[0017] Figure 5 shows the results of surface EDS analysis of a region provided at a grain boundary as a separate phase in a composite manufactured according to an example.

[0018] Figure 6 shows the EDS mapping results of the region provided at the grain boundary as a separate phase of Figure 5.

[0019] Figure 7 shows the XRD analysis results before and after the hygroscopicity test of the composite according to Example 3 at a sintering temperature of 1,550°C.

[0020] Figure 8 shows the XRD analysis results before and after the hygroscopicity test of the composite according to Example 6 at a sintering temperature of 1,550°C.

[0021] Figure 9 shows SEM images of the surface of the composite of Example 6 according to the sintering temperature.

[0022] Hereinafter, the present invention will be described in detail.

[0023] The present invention can have various modifications and various embodiments, and specific embodiments are illustrated in the drawings and described in detail in the detailed description.

[0024] However, this is not intended to limit the present invention to specific embodiments, and should be understood to encompass all modifications, equivalents, and alternatives falling within the spirit and technical scope of the present invention. In describing the present invention, detailed descriptions of related known technologies will be omitted if they are deemed to obscure the gist of the present invention.

[0025] The terminology used in this specification is for the purpose of describing specific embodiments only and is not intended to limit the present invention. Singular expressions include plural expressions unless the context clearly dictates otherwise.

[0026] In this specification, when a part is said to "include" a certain component, this does not mean that it excludes other components, but rather that it may include other components, unless specifically stated otherwise.

[0027] In this specification, when it is said that a member is located "on" another member, this includes not only cases where the member is in contact with the other member, but also cases where another member exists between the two members.

[0028] In this specification, ytterbium oxide includes ytterbium(II) oxide (YbO) and ytterbium(III) oxide (Yb2O3), and may specifically be ytterbium(III) oxide.

[0029] Hereinafter, the present invention will be described in detail.

[0030] One embodiment of the present invention provides a magnesium oxide-based composite comprising ytterbium (Yb) element and magnesium oxide (MgO) crystal grains.

[0031] The magnesium oxide-based composite according to the present invention is characterized by including ytterbium (Yb) element in a magnesium oxide-based base material. The magnesium oxide-based composite according to the present invention can significantly reduce or prevent the formation of magnesium hydroxide formed on the surface of magnesium oxide due to absorption of moisture in the air due to the presence of the ytterbium (Yb) element. Through this, the magnesium oxide-based composite according to the present invention has the advantage of overcoming the limited use due to the low hygroscopicity of conventional magnesium oxide. In addition, the magnesium oxide-based composite according to the present invention can also have the advantage of lowering the sintering temperature during manufacturing, thereby lowering the manufacturing cost, due to the presence of the ytterbium (Yb) element.

[0032] The magnesium oxide-based composite according to the present invention may be a sintered body using magnesium oxide containing ytterbium (Yb) as a base material, and may be a ceramic using magnesium oxide as a base material. In addition, the magnesium oxide-based composite according to the present invention may be a solid solution containing ytterbium (Yb) element within a magnesium oxide crystal structure. Furthermore, the magnesium oxide-based composite according to the present invention may be a solid solution containing ytterbium (Yb) element and other metal elements within a magnesium oxide crystal structure.

[0033] According to one embodiment of the present invention, the ytterbium (Yb) element may be provided by substituting for the magnesium (Mg) element position of the magnesium oxide (MgO) crystal. More specifically, the ytterbium (Yb) element may be provided as a substitute for the Mg element position of the unit cell of the magnesium oxide crystal grain. 2+ At least part of Yb 2+ or Yb 3+ It may be equipped with a replacement.

[0034] In addition, according to one embodiment of the present invention, the ytterbium (Yb) element may be included in the form of ytterbium oxide on the interface and / or surface of the magnesium oxide (MgO) crystal. Specifically, the ytterbium oxide may exist as another phase at the magnesium oxide grain boundary. In this case, the ytterbium oxide may exist irregularly on the surface of the magnesium oxide-based composite.

[0035] According to one embodiment of the present invention, the ytterbium (Yb) element may be provided as a substitute for the magnesium (Mg) element position of the magnesium oxide (MgO) crystal, and may also be included in the form of ytterbium oxide on the surface of the magnesium oxide (MgO) crystal.

[0036] According to one embodiment of the present invention, the content of the ytterbium (Yb) element may be 0.02 at.% or more and 6 at.% or less with respect to the magnesium (Mg) element (with respect to 100 at.% of the Mg element). Specifically, the content of the ytterbium (Yb) element may be 0.02 at.% or more and 5 at.% or less, 0.02 at.% or more and 4 at.% or less, 0.02 at.% or more and 3 at.% or less, 0.02 at.% or more and 2 at.% or less, 0.04 at.% or more and 2 at.% or less, 0.04 at.% or more and 0.4 at.% or less, 0.1 at.% or more and 2 at.% or less, 0.09 at.% or more and 0.5 at.% or less, or 0.1 at.% or more and 0.4 at.% or less with respect to the magnesium (Mg) element. When the content of the ytterbium (Yb) element is within the above range, the moisture absorption resistance of the magnesium oxide-based composite can be significantly improved, and further, the sintering temperature during manufacturing can be lowered. In addition, when the content of the ytterbium (Yb) element is less than the above range, the effect of improving the moisture absorption resistance of the magnesium oxide-based composite may not be sufficient, and when the content of the ytterbium (Yb) element exceeds the above range, the growth of magnesium oxide crystal grains may be hindered due to the ytterbium (Yb) element or ytterbium oxide.

[0037] The content of the above ytterbium (Yb) element can be measured by a method known in the art, for example, by EDS, WDS, EPMA, XRF, or Rietveld refinement of neutron and X-ray diffraction, and can also be measured by ICP analysis.

[0038] According to one embodiment of the present invention, the magnesium oxide-based composite may further include at least one additional metal element selected from the group consisting of Ti, Nb, Zr, Ga, Mn, B, Fe, Sn, Si, V, Ta, Sb, Y, Eu, Er and Al.

[0039] The above additional metal element may be derived from at least one additional additive selected from the group consisting of oxides, hydroxides or carbonates comprising at least one selected from the group consisting of Ti, Nb, Zr, Ga, Mn, B, Fe, Sn, Si, V, Ta, Sb, Y, Eu, Er and Al.

[0040] Specifically, the additional metal element may be provided as a substitute for the magnesium (Mg) element position of the magnesium oxide (MgO) crystal, such as the aforementioned ytterbium (Yb) element, and / or may be provided on the surface of the magnesium oxide (MgO) crystal in the form of an additional oxide or compound (for example, at least one of an oxide of the additional metal; an oxide of ytterbium (Yb) and the additional metal; an oxide of magnesium and the additional metal; an oxide of magnesium, ytterbium (Yb) and the additional metal; and a reaction oxide (compound) thereof). The additional metal element may be applied to the magnesium oxide-based composite together with the ytterbium (Yb) element to improve moisture absorption resistance and / or to lower the sintering temperature, thereby bringing about the effect of reducing the manufacturing cost.

[0041] According to one embodiment of the present invention, the content of the additional metal element may be 0.02 at.% or more and 5 at.% or less with respect to the magnesium (Mg) element. Specifically, the content of the additional metal element may be 0.02 at.% or more and 5 at.% or less, 0.02 at.% or more and 4 at.% or less, 0.02 at.% or more and 3 at.% or less, 0.02 at.% or more and 2 at.% or less, 0.02 at.% or more and 1 at.% or less, 0.05 at.% or more and 5 at.% or less, 0.05 at.% or more and 4 at.% or less, 0.05 at.% or more and 3 at.% or less, 0.05 at.% or more and 2 at.% or less, 0.05 at.% or more and 1 at.% or less, 0.05 at.% or more and 0.5 at.% or less, or 0.1 at.% or more and 0.5 at.% or less, with respect to the magnesium (Mg) element.

[0042] According to one embodiment of the present invention, when the magnesium oxide-based composite further includes the additional metal element, the content of the ytterbium (Yb) element may be 0.02 at.% or more and 1 at.% or less, 0.02 at.% or more and 0.5 at.% or less, 0.02 at.% or more and 0.25 at.% or less, 0.02 at.% or more and 0.15 at.% or less, or 0.02 at.% or more and 0.1 at.% or less with respect to the magnesium (Mg) element. When the additional metal element is further included in the magnesium oxide-based composite, the content of the ytterbium (Yb) element may be less compared to when the ytterbium (Yb) element is applied alone. When the magnesium oxide-based composite further includes the additional metal element, and the content range of the ytterbium (Yb) element is within the above range, the growth of magnesium oxide crystal grains of the magnesium oxide-based composite is not hindered or the growth of magnesium oxide crystal grains is promoted, and moisture absorption resistance can be greatly improved.

[0043] According to one embodiment of the present invention, the magnesium oxide-based composite may have a weight increase rate of less than 1% after a moisture absorption test for 72 hours under an atmosphere of 85°C and 85%RH. Specifically, the magnesium oxide-based composite may have a weight increase rate of less than 0.7%, or less than 0.5%, after a moisture absorption test for 72 hours under an atmosphere of 85°C and 85%RH. The weight increase rate of the conventional magnesium oxide in the moisture absorption test was generally more than 10%, and even when the sintering temperature was increased, the weight increase rate showed a result exceeding 1%. In contrast, the magnesium oxide-based composite according to the present invention shows a greatly improved moisture absorption resistance result compared to the conventional magnesium oxide.

[0044] According to one embodiment of the present invention, the content of the magnesium oxide crystal grains may be at least 90 wt% with respect to the entire composite. Specifically, the content of the magnesium oxide crystal grains may be at least 92 wt% or 95 wt% with respect to the entire composite.

[0045] According to one embodiment of the present invention, the magnesium oxide-based composite may be a particle of any one shape of an amorphous shape, a sphere, an ellipse, a donut shape, and a plate shape, or a structure of a predetermined shape. In addition, the magnesium oxide-based composite may be in a powder form, a film form, or a predetermined bulk form. In addition, the magnesium oxide-based composite may be in the form of a fine particle of any one shape of an amorphous shape, a sphere, an ellipse, a donut shape, and a plate shape, or a granular powder form. When the magnesium oxide-based composite according to the present invention is in a powder form, it may have a particle size of 1 μm to 200 μm, or 2 μm to 150 μm. The particle size may refer to an average particle size of the powder.

[0046] The structure of the above predetermined shape may be a structure formed by a mold for implementing the predetermined shape.

[0047] Another embodiment of the present invention provides a method for producing a composite based on magnesium oxide as described above.

[0048] Specifically, another embodiment of the present invention provides a method for producing a magnesium oxide-based composite, comprising the steps of: (A) preparing a sintering mixture comprising magnesium oxide or a magnesium oxide precursor and ytterbium oxide; (B) pretreating the sintering mixture, including at least one of coating, granulating, press molding, and injection molding; and (C) sintering the sintering mixture to crystallize it.

[0049] According to one embodiment of the present invention, the magnesium oxide precursor may include at least one of magnesium hydroxide powder, magnesium hydrogen carbonate powder, magnesium carbonate powder, and magnesia (MgO) powder.

[0050] According to one embodiment of the present invention, the step of (A1) dispersing the sintering mixture in a solvent may be further included. Specifically, the magnesium oxide precursor, ytterbium oxide, and optionally, an additional additive to be described later may be added to the solvent to disperse and dissolve them. For example, when the magnesium oxide precursor is magnesium hydroxide powder, magnesium bicarbonate powder, and / or magnesium carbonate powder, the solvent may be water (distilled water). In another example, when the magnesium oxide precursor is magnesia (MgO) powder, an organic solvent may be used to prevent reaction with water. Examples of the organic solvent that may be used include anhydrous alcohols such as ethanol, methanol, and propanol, but the present invention is not limited thereto, and any organic solvent that does not affect the purpose and effect of the present invention may be used without limitation.

[0051] According to one embodiment of the present invention, the sintering mixture may further include a binder and / or a dispersant. The binder and / or dispersant may be further included in the solvent and dispersed and dissolved therein.

[0052] According to one embodiment of the present invention, the binder may be an organic binder, and when an organic binder is used, it is suitable because it is combusted through sintering and does not remain in the final magnesium oxide-based composite. The organic binder may be used without limitation as one used in the present technical field, and may include at least one selected from the group consisting of a cellulose binder, polyvinyl alcohol, polyvinylpyrrolidone, polyethylene glycol, a gel binder, and starch.

[0053] According to one embodiment of the present invention, the dispersant can be added to uniformly disperse the components introduced into the solvent, and any one used in the present technical field can be used without limitation, and for example, polycarboxylate ammonium salt and alkylol ammonium salt can be applied.

[0054] According to one embodiment of the present invention, step (A1) can uniformly mix the components within the solvent using a physical mixing method such as a ball mill. When a ball mill is used in step (A1), not only is the individual components within the solvent homogeneously mixed, but it also has the advantage of controlling the powder dispersed within the solvent to a more uniform size.

[0055] According to one embodiment of the present invention, the coating in step (B) may be applied when the final magnesium oxide-based composite needs to be provided on the surface of a specific electronic component or manufactured in a plate shape. In addition, the granulation in step (B) may be applied when the final magnesium oxide-based composite needs to be manufactured into spherical particles. In addition, the press molding in step (B) may be a method of molding by placing the sintering mixture in a predetermined mold and then applying a predetermined pressure, and various methods generally used in the art may be applied. Furthermore, the injection molding in step (B) may include any one of a slip casting method in which the sintering mixture is slurried and injected into a mold, an injection molding method in which the slurry of the sintering mixture is slurried and injected into an extruder, and a cast molding method in which the sintering mixture is poured into a mold and molded.

[0056] According to one embodiment of the present invention, step (B) may be to granulate the sintering mixture and then mold it into a predetermined shape. Specifically, step (B) may be to granulate the sintering mixture and then press mold it or injection mold it. Through this, the particle size of the sintering mixture before sintering can be controlled, and further, a sintered body can be manufactured in a desired shape.

[0057] According to one embodiment of the present invention, the granulation may be performed by granulating the sintering mixture using a spray drying method. When the spray drying method is used, more homogeneous granules with controlled particle size can be formed, thereby providing the advantage of producing a magnesium oxide-based composite of spherical fine particles in a simple manner.

[0058] According to one embodiment of the present invention, the ytterbium oxide can serve as a precursor of the ytterbium (Yb) element in the above-described magnesium oxide-based composite. According to one embodiment of the present invention, the ytterbium oxide can be included in an amount of 0.01 mol% or more and 3 mol% or less with respect to 1 mol of magnesium oxide in the final magnesium oxide-based composite. Specifically, the ytterbium oxide may be present in an amount of 0.01 mol% to 2.5 mol%, 0.01 mol% to 2 mol%, 0.01 mol% to 1.5 mol%, 0.01 mol% to 1 mol%, 0.02 mol% to 1 mol%, 0.02 mol% to 0.2 mol%, 0.05 mol% to 1 mol%, 0.045 mol% to 0.25 mol%, or 0.05 mol% to 0.2 mol%, based on 1 mol of magnesium oxide of the final magnesium oxide-based composite. When the content of the ytterbium oxide is controlled as described above, it may be controlled in the same manner as the content of the ytterbium (Yb) element in the magnesium oxide-based composite as described above.

[0059] According to one embodiment of the present invention, the sintering mixture may further include at least one additional additive selected from the group consisting of oxides, hydroxides or carbonates including at least one selected from the group consisting of Ti, Nb, Zr, Ga, Mn, B, Fe, Sn, Si, V, Ta, Sb, Y, Eu, Er and Al. Specifically, the additional additive is TiO2, Ti(OH)4, Ti(CO3) 2, Nb2O5, ZrO2, Zr(OH)4, Zr(CO3) 2, Ga2O3, B2O3, Fe2O3, SnO2, MnO2, Mn2O3, SiO2, V2O5, V2O3, VO2, VO, V(OH)5, V2(CO3) 5,At least one selected from the group consisting of Ta2O5, Sb2O5, Y2O3, Eu2O3, Al2O3, Al(OH)3 and Al2(CO3)3 may be present. The additional additive may be a precursor of an additional metal element in the aforementioned magnesium oxide-based composite.

[0060] According to one embodiment of the present invention, the additional additive may be included in an amount of 0.01 mol% or more and 1 mol% or less with respect to 1 mol of magnesium oxide of the final magnesium oxide-based composite. Specifically, the additional additive may be included in an amount of 0.02 mol% or more and 1 mol% or less, 0.02 mol% or more and 0.5 mol% or less, 0.02 mol% or more and 0.25 mol% or less, 0.02 mol% or more and 0.15 mol% or less, or 0.02 mol% or more and 0.1 mol% or less with respect to 1 mol of magnesium oxide of the final magnesium oxide-based composite. When the amount of the additional additive is adjusted as described above, it may be adjusted in the same manner as the amount of the additional metal element in the magnesium oxide-based composite as described above.

[0061] According to one embodiment of the present invention, the total content of the ytterbium oxide and the additional additive may be included in an amount of 0.01 mol% or more and 10 mol% or less with respect to 1 mol of magnesium oxide of the final magnesium oxide-based composite. Specifically, when the additional additive is further included, the total content of the ytterbium oxide and the additional additive may be 0.01 mol% or more and 5 mol% or less, 0.01 mol% or more and 3 mol% or less, 0.01 mol% or more and 2 mol% or less, 0.02 mol% or more and 1 mol% or less, or 0.1 mol% or more and 0.5 mol% or less with respect to 1 mol of magnesium oxide of the final magnesium oxide-based composite.

[0062] The reason why the content of the above ytterbium oxide or the above additional additive is based on the magnesium oxide of the final magnesium oxide-based composite is that when the magnesium oxide precursor is a magnesium salt such as magnesium hydroxide powder, magnesium bicarbonate powder, or magnesium carbonate powder, it is converted into a magnesium oxide phase through sintering treatment, and therefore the content of the above ytterbium oxide can be controlled regardless of the type of the magnesium oxide precursor.

[0063] According to one embodiment of the present invention, the sintering temperature in step (C) may be 1,000°C to 1,800°C. Specifically, the sintering temperature may be controlled depending on the content of the ytterbium oxide. The sintering temperature may be 1,250°C to 1,800°C, 1,350°C to 1,800°C, 1,400°C to 1,800°C, 1,400°C to 1,700°C, 1,400°C to 1,600°C, 1,500°C to 1,700°C, or 1,500°C to 1,600°C, depending on the content of the ytterbium oxide. In addition, in the case where the additional additive is applied together with the ytterbium oxide in step (C), sintering may be possible at a low sintering temperature, such as 1000°C to 1,500°C, 1,200°C to 1,600°C, or 1,250°C to 1,450°C, depending on the increase in diffusion.

[0064] Another embodiment of the present invention provides an organic-inorganic composite in which particles composed of the magnesium oxide-based composite are dispersed within a polymer matrix.

[0065] According to one embodiment of the present invention, the polymer matrix may be formed of at least one resin selected from the group consisting of a silicone resin, a urethane resin, an epoxy resin, and a thermoplastic resin. The silicone resin, urethane resin, epoxy resin, and thermoplastic resin may be materials for forming a matrix commonly used in the art. For example, the thermoplastic resin may include a polyolefin resin and a polyester resin. In addition, the thermoplastic resin may include at least one of general-purpose plastics such as PE, PP, PMMA, PS, and ABS; engineering plastics such as PBT, PC, PPO, POM, and nylon; super engineering plastics such as PPS, PI, PTFE, and PEEK; and eco-friendly plastics such as PBAT and PLA.

[0066] According to one embodiment of the present invention, the magnesium oxide-based composite can be used for at least one of a heat transfer material, a heat dissipation material, a wear-resistant material, an insulating material, a flame retardant material, and a reinforcing material. Specifically, since the magnesium oxide-based composite has excellent thermal conductivity and moisture absorption resistance, it can be applied to a heat dissipation layer, a heat dissipation filler, etc. in a semiconductor device, but is not limited thereto, and can be applied to the application of existing alumina and / or silica, and more broadly, it can be applied without limitation to a heat transfer material, a wear-resistant material, an insulating material, a flame retardant material, and a reinforcing material on a polymer resin.

[0067] Hereinafter, the present invention will be described in detail using examples. However, the examples according to the present invention may be modified in various ways, and the scope of the present invention is not limited to the examples described below. The examples in this specification are provided to more fully explain the present invention to those of ordinary skill in the art.

[0068] [Examples 1 to 13]

[0069] A mixture was prepared by adding Mg(OH)2 powder as a magnesium precursor, Yb2O3 powder, PVA (Polyvinyl alcohol) as a binder, and Polycarboxylate Ammonium salt as a dispersant to distilled water and stirring to disperse and dissolve them. At this time, the content of Yb2O3 powder was adjusted as shown in Table 1 below. Then, the prepared mixture was further mixed and ground through a ball mill using ZrO2 beads to prepare a slurry having a solid content of 20 vol.%. Then, it was granulated using a spray drying method under the conditions of 230°C and an atomizer rotation speed of 10,000 rpm. Then, the granulated particles were sintered at a temperature as shown in Table 1 below to prepare a magnesium oxide-based composite. Furthermore, the weight increase rate after the manufactured composite was subjected to a moisture absorption test for 72 hours under an atmosphere of 85°C and 85%RH is shown in Table 2 below. In addition, Table 2 below shows the content (at.%) of the Yb element and additional metal elements relative to the Mg element of the manufactured composite.

[0070] [Examples 14 and 15]

[0071] A mixture was prepared by adding MgO powder as a magnesium precursor, Yb2O3 powder, PVB (Polyvinyl butyral) as a binder, and Alkylolammonium salt as a dispersant to ethyl alcohol and stirring to disperse and dissolve them. At this time, the content of Yb2O3 powder was adjusted as shown in Table 1 below. Then, the prepared mixture was further mixed and ground through a ball mill using ZrO2 beads to prepare a slurry having a solid content of 20 vol.%. Then, it was granulated using a spray drying method under the conditions of 90 ℃ and an atomizer rotation speed of 8,000 rpm. Then, the granulated particles were sintered at the temperature shown in Table 1 below to prepare a magnesium oxide-based composite. Furthermore, the weight increase rate after a moisture absorption resistance test for the prepared composite under an atmosphere of 85 ℃ and 85% RH for 72 hours is shown in Table 2 below. Additionally, Table 2 below shows the content (at.%) of Yb element relative to Mg element of the manufactured composite.

[0072] [Comparative Example 1]

[0073] A magnesium oxide sintered body was manufactured in the same manner as in Example 1, except that Yb2O3 powder was not applied. Furthermore, the weight increase rate of the manufactured sintered body after a hygroscopicity test for 72 hours under an atmosphere of 85°C and 85% RH is shown in Table 2 below.

[0074] [Comparative Example 2]

[0075] A magnesium oxide sintered body was manufactured in the same manner as in Example 14, except that Yb2O3 powder was not applied. Furthermore, the weight increase rate of the manufactured sintered body after a hygroscopicity test for 72 hours under an atmosphere of 85°C and 85% RH is shown in Table 2 below.

[0076] [Comparative Example 3]

[0077] A magnesium oxide-based composite was manufactured in the same manner as in Example 1, except that instead of Yb2O3 powder, TiO2 and Nb2O5 were added in the amounts shown in Table 1 below. Furthermore, the weight increase rate of the manufactured composite after a hygroscopicity test for 72 hours under an atmosphere of 85°C and 85%RH is shown in Table 2 below. In addition, Table 2 below shows the content (at.%) of metal elements with respect to the Mg element of the manufactured composite.

[0078] Sintering temperature (℃) of granules containing magnesium oxide precursor additive (mol% of MgO 1 mol of the final composite) Yb2O3TiO2Y2O3Nb2O51,4501,5501,650Example 1 Mg(OH) 20.01---X△○Example 2 Mg(OH) 20.02---X△○Example 3 Mg(OH) 20.03---X△○Example 4 Mg(OH) 20.04---X△○Example 5 Mg(OH) 20.08---X○○Example 6 Mg(OH) 20.12---X○○Example 7 Mg(OH) 20.16---X○○Example 8 Mg(OH) 20.20---△ ○○Example 9Mg(OH)20.30---△△○Example 10Mg(OH)20.50---△△○Example 11Mg(OH)21.0---△△○Example 12Mg(OH)20.040.2--○○○Example 13Mg(OH)20.04-0.07-X○○Example 14MgO0.02---X△○Example 15MgO0.04---X△○Comparative Example 1Mg(OH)2----XX△Comparative Example 2MgO----XXXComparative Example 3Mg(OH)2-0.2-0.06○--

[0079] The content of additional metal elements (at.%) compared to Mg in the final composite of the magnesium oxide precursor was determined by sintering temperature (℃), and the weight increase rate of the granules after 72 h test at 85℃ and 85%RH (%) was determined by sintering temperature (℃). YbTiYNb1,450℃1,550℃1,650℃Example 1Mg(OH)20.020---14.314.970.46Example 2Mg(OH)20.040---13.624.230.40Example 3Mg(OH)20.060---11.643.280.36Example 4Mg(OH)20.080- --13.051.550.33Example 5Mg(OH)20.160---12.680.990.22Example 6Mg(OH)20.240---11.000.470.07Example 7Mg(OH)20.320---7.570.170.08Example 8Mg(OH)20.400---3.890.220.06Example 9Mg (OH)20.600---4.501.180.04Example 10Mg(OH)21.000---4.501.020.17Example 11Mg(OH)22.000---4.711.040.25Example 12Mg(OH)20.0800.20--0.0280.030.00Example 13Mg(OH)20.080-0.1 40-5.610.410.25Example 14MgO0.040---6.833.870.43Example 15MgO0.080---5.1901.610.40Comparative Example 1Mg(OH)2----31.4514.491.35Comparative Example 2MgO----23.00--Comparative Example 3Mg(OH)2-0.20-0.1200.50--

[0080] In the above Table 1, the evaluation of the degree of crystallinity according to the sintering temperature of the granules was performed based on the following criteria.

[0081] - ××: A state in which no sintering has occurred and no crystal grains have been formed.

[0082] - ×: A state in which sintering is minimal and grain growth is very low, resulting in very poor density.

[0083] - △: A state in which sintering has been achieved to a certain extent and grain growth is low, and the density is normal or insufficient.

[0084] - ○: A state in which sintering has occurred and grain growth is sufficiently high, resulting in high density.

[0085]

[0086] Figure 1 shows an example of evaluation criteria according to sintering temperature according to examples and comparative examples.

[0087] Figure 2 shows the weight increase rate after the moisture absorption resistance test according to the content of Yb2O3 and the sintering temperature in Examples 1 to 11. Referring to Figure 2, the higher the sintering temperature, the more the moisture absorption resistance tends to increase, and when the content of Yb2O3 is about 0.5 mol% with respect to MgO, the moisture absorption resistance appears to converge.

[0088] Fig. 3 shows SEM images of the composites according to Examples 6 to 11 at a sintering temperature of 1,550°C. Referring to Fig. 3, it can be confirmed that ytterbium oxide exists as a separate phase on the surface of the manufactured composites. Specifically, it can be confirmed that as the content of Yb2O3 increases, the amount of ytterbium oxide as a separate phase on the surface of the manufactured composite tends to increase, and it was confirmed that the presence of an excessive amount of ytterbium oxide hinders the growth of crystal grains, thereby affecting the reduction of the density of the sintered body.

[0089] Figure 4 shows the results of surface EDS analysis at the crystal grain locations of a composite manufactured according to an embodiment. Referring to Figure 4, the crystal grains of the manufactured composite are presumed to be MgO crystal grains containing trace amounts of Yb element.

[0090] Fig. 5 shows the results of surface EDS analysis of a region provided at a grain boundary as a separate phase in a composite manufactured according to an embodiment. And, Fig. 6 shows the results of EDS mapping of a region provided at a grain boundary as a separate phase of Fig. 5. Referring to Figs. 5 and 6, the region formed as a separate phase is confirmed to be a mixture of ytterbium oxide and magnesium oxide, and is presumed to be a crystal grain of ytterbium oxide containing a trace amount of Mg element.

[0091] Figure 7 shows the XRD analysis results before and after the moisture absorption resistance test of the composite according to Example 3 at a sintering temperature of 1,550°C. Referring to Figure 7, it was confirmed that the composite according to Example 3 at a sintering temperature of 1,550°C, which showed a weight increase rate of 3.28% after the moisture absorption resistance test, had some magnesium hydroxide formed on the surface.

[0092] Fig. 8 shows the XRD analysis results before and after a moisture absorption test of a composite according to Example 6 at a sintering temperature of 1,550°C. Referring to Fig. 8, it was confirmed that no magnesium hydroxide was detected on the surface of the composite according to Example 6 at a sintering temperature of 1,550°C, which showed a weight increase rate of 0.47% after the moisture absorption test.

[0093] Figure 9 shows SEM images of the surface of the composite of Example 6 according to the sintering temperature. Referring to Figure 9, it can be confirmed that the grain size tends to increase as the sintering temperature increases, and it can be confirmed that the growth of MgO grains is well achieved even at low temperatures below 1,700°C due to the addition of Yb2O3.

Claims

1. A magnesium oxide-based composite comprising ytterbium (Yb) element and magnesium oxide (MgO) crystal grains.

2. In claim 1, A magnesium oxide-based complex, wherein the above ytterbium (Yb) element is substituted for the magnesium (Mg) element position of the above magnesium oxide (MgO) crystal.

3. In claim 1, A magnesium oxide-based composite, wherein the above ytterbium (Yb) element is included in the form of ytterbium oxide on the surface of the magnesium oxide (MgO) crystal.

4. In claim 1, A magnesium oxide-based composite, wherein the content of the ytterbium (Yb) element is 0.02 at.% or more and 6 at.% or less with respect to the magnesium (Mg) element.

5. In claim 1, A magnesium oxide-based composite, wherein the magnesium oxide-based composite further comprises at least one additional metal element selected from the group consisting of Ti, Nb, Zr, Ga, Mn, B, Fe, Sn, Si, V, Ta, Sb, Y, Eu, Er and Al.

6. In claim 1, A magnesium oxide-based composite having a weight increase of less than 1% after a hygroscopicity test for 72 hours under an atmosphere of 85°C and 85%RH.

7. In claim 1, A magnesium oxide-based composite, wherein the content of the magnesium oxide crystal grains is at least 90 wt% with respect to the entire composite.

8. In claim 1, The above magnesium oxide-based composite is a magnesium oxide-based composite having a particle shape of any one of amorphous, spherical, oval, donut-shaped and plate-shaped or a structure of a predetermined shape. 9.(A) A step of preparing a sintering mixture comprising magnesium oxide or a magnesium oxide precursor and ytterbium oxide; (B) a step of pretreating the mixture for sintering, including at least one of coating, granulation, press molding, and injection molding; and (C) a step of crystallizing the sintering mixture by sintering; including; Method for producing a magnesium oxide-based composite.

10. In claim 9, A method for producing a magnesium oxide-based composite, wherein the above ytterbium oxide is included in an amount of 0.01 mol% or more and 3 mol% or less per 1 mol of magnesium oxide of the final magnesium oxide-based composite.

11. In claim 9, A method for producing a magnesium oxide-based composite, wherein the sintering temperature in step (C) is 1,000 ℃ to 1,800 ℃.

12. In claim 9, A method for producing a magnesium oxide-based composite, wherein the sintering mixture further comprises at least one additional additive selected from the group consisting of oxides, hydroxides or carbonates, including at least one selected from the group consisting of Ti, Nb, Zr, Ga, Mn, B, Fe, Sn, Si, V, Ta, Sb, Y, Eu, Er and Al.

13. In claim 12, A method for producing a magnesium oxide-based composite, wherein the above additional additive is included in a content of 0.01 mol% or more and 1 mol% or less with respect to 1 mol of magnesium oxide of the final magnesium oxide-based composite.

14. In claim 12, A method for producing a magnesium oxide-based composite, wherein the total content of the above ytterbium oxide and the above additional additive is included so as to be 0.01 mol% or more and 10 mol% or less with respect to 1 mol of magnesium oxide of the final magnesium oxide-based composite.

15. In claim 9, (A1) A method for producing a magnesium oxide-based composite, further comprising the step of dispersing the sintering mixture in a water-soluble solvent.

16. In claim 9, A method for producing a magnesium oxide-based composite, wherein the granulation is performed by granulating the sintering mixture using a spray drying method.

17. An organic-inorganic composite comprising particles composed of a magnesium oxide-based composite according to claim 1 dispersed within a polymer matrix.

18. In claim 17, An organic-inorganic composite, wherein the polymer matrix is ​​formed of at least one resin selected from the group consisting of a silicone resin, a urethane resin, an epoxy resin, and a thermoplastic resin.

Citation Information

Patent Citations

  • Mgo vapor-deposited material and its production

    JP2000290062A

  • High-density magnesium oxide-based sintered compact and its production, and member for plasma treatment apparatus

    JP2000313655A

  • Magnesium oxide vapor deposition material and method for producing the same

    JP2009298655A

  • Sintered magnesium oxide and method for producing the same

    JP2010143798A

  • MgO-based vapor deposition material and method for producing the same