Solid polymer electrolyte composition containing cyclic siloxane-based compound, and solid polymer electrolyte and secondary battery comprising same

A composition of cyclic siloxane and polyalkylene oxide-based compounds in a solid polymer electrolyte addresses the limitations of existing electrolytes by enhancing ionic conductivity and mechanical strength, enabling efficient roll-to-roll production and improved battery performance.

WO2024248395A1PCT designated stage expired Publication Date: 2024-12-05KOREA RES INST OF CHEM TECH +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/006948
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-01
Filing Date
2024-05-23
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Current lithium secondary batteries face safety issues due to flammable liquid electrolytes, and solid polymer electrolytes, such as oxide-based and sulfide-based ones, have limitations in mechanical strength, stability, and interfacial resistance, while polymer-based electrolytes require high viscosity for roll-to-roll production, which complicates their commercialization.

Method used

A composition for a solid polymer electrolyte containing a cyclic siloxane-based compound as a plasticizer, combined with a polyalkylene oxide-based compound, a crosslinking agent, and a lithium salt, with a viscosity of 100 to 150 cP, enabling in-situ crosslinking polymerization and roll-to-roll production, improving ionic conductivity and mechanical strength.

Benefits of technology

The solution provides a solid polymer electrolyte with enhanced ionic conductivity, stabilization of the lithium metal anode, and improved charge/discharge cycle characteristics, facilitating the commercialization of lithium secondary batteries with improved safety and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024006948_05122024_PF_FP_ABST
    Figure KR2024006948_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a solid polymer electrolyte composition containing a cyclic siloxane-based compound, and a solid polymer electrolyte and a secondary battery comprising the same. Provided are: a solid polymer electrolyte precursor which is obtained by mixing a cyclic siloxane-based compound and a polyalkyleneoxide-based compound and adjusting the viscosity thereof, thereby improving impregnation properties and battery characteristics of a solid polymer electrolyte, and which is suitable for in-situ crosslinking polymerization; and the solid polymer electrolyte, which can be applied to a roll-to-roll production process.
Need to check novelty before this filing date? Find Prior Art

Description

Composition for solid polymer electrolyte containing a cyclic siloxane compound, and solid polymer electrolyte and secondary battery containing the same

[0001] The present invention relates to a composition for a solid polymer electrolyte containing a cyclic siloxane compound, and a solid polymer electrolyte and a secondary battery comprising the same.

[0002] The need for lithium secondary batteries has increased recently due to the widespread adoption of small electronic devices like smartphones and tablet PCs, as well as the growing demand for environmentally friendly electric vehicles that can address air pollution. Lithium secondary batteries are electrochemical devices that convert electrical energy into chemical energy for storage and then convert it back into electricity when needed. They are comprised of four core components: a cathode, anode, a separator, and an electrolyte.

[0003] Current commercial liquid electrolyte lithium secondary batteries continue to face safety concerns, such as volume expansion, explosion, and ignition. To minimize these issues, it is essential to commercialize solid electrolytes that do not pose a risk of leakage, replacing highly flammable liquid electrolytes with flammable and explosive liquid electrolytes. Solid electrolytes currently under development can be categorized into oxide, sulfide, and polymer electrolytes. While oxide solid electrolytes offer excellent stability in air and can be used in high-voltage ranges, their poor mechanical properties make them prone to breakage and their high interfacial resistance between the electrode and electrolyte hinder their commercialization. Sulfide solid electrolytes, however, boast high ionic conductivity and good interfacial resistance between the electrode and electrolyte, but they are vulnerable to moisture and air and have poor chemical and electrochemical stability when in contact with electrode active materials and other materials.

[0004] Meanwhile, polymer-based solid electrolytes have superior chemical and thermal stability compared to liquid electrolytes, and unlike oxide-based and sulfide-based solid electrolytes, they can be manufactured using the in situ crosslinking polymerization method, allowing for rapid and realistic commercialization by utilizing the roll-to-roll process used in the production of existing liquid electrolyte batteries. By applying a liquid polymer electrolyte precursor to the liquid electrolyte injection system currently being mass-produced, and simply adding a thermal crosslinking polymerization process, stable solid electrolyte batteries can be mass-produced on a large scale.

[0005] Cyclic siloxane plasticizers, which are one of the solid polymer electrolytes, exhibit excellent thermal and electrochemical stability and high mechanical strength, but their high viscosity results in poor battery characteristics and impregnation properties, making them difficult to apply to roll-to-roll production processes that require impregnation of the support in a short period of time.

[0006] The purpose of the present invention is to provide a solid polymer electrolyte containing a cyclic siloxane compound having low viscosity and excellent impregnation properties, and a composition for a solid polymer electrolyte used to produce the same.

[0007] Another object of the present invention is to provide a solid polymer electrolyte composition having a viscosity suitable for in situ crosslinking polymerization.

[0008] Another object of the present invention is to provide a solid polymer electrolyte for a secondary battery that can be used in a roll-to-roll production process and a composition for a solid polymer electrolyte used to manufacture the same.

[0009] Another object of the present invention is to provide a solid polymer electrolyte for a secondary battery having improved cycle characteristics, etc. in a secondary battery involving metal deposition, and a composition for a solid polymer electrolyte used to manufacture the same.

[0010] The problems to be solved by the present invention are not limited to the problem(s) mentioned above, and other problems not mentioned will be clearly understood by those skilled in the art from the description below.

[0011] According to one aspect of the present invention, the present invention provides a composition for a solid polymer electrolyte, comprising: a cyclic siloxane-based compound as a first plasticizer; a polyalkylene oxide-based compound as a second plasticizer; a crosslinking agent; a lithium salt; and a curing initiator.

[0012] The viscosity of the above composition may be 100 to 150 cP.

[0013] The viscosity of the above composition may be controlled according to the mixing weight ratio of the first plasticizer and the second plasticizer.

[0014] The weight ratio of the first plasticizer and the second plasticizer may be 7:3 to 1:9.

[0015] The composition may include 40 to 80 wt% of a first plasticizer and a second plasticizer, 10 to 50 wt% of a crosslinking agent, 5 to 40 wt% of a lithium salt, and 0.1 to 5 wt% of a curing initiator.

[0016] The above cyclic siloxane compound can be represented by chemical formula 1.

[0017] [Chemical Formula 1]

[0018]

[0019] In the above chemical formula 1, R1 and R2 are each hydrogen or a methyl group, and m and n are each integers from 0 to 20.

[0020] The above polyalkylene oxide compound can be represented by the following chemical formula 2 or chemical formula 3.

[0021] [Chemical Formula 2]

[0022]

[0023] [Chemical Formula 3]

[0024]

[0025] In the above chemical formulas 2 and 3, R3, R4, R5, R3', R4', and R5' is hydrogen or methyl group, and R6, R7, R6', and R7' is a chain or branched alkyl group having 1 to 10 carbon atoms, and o, p, q, x, y, and z are each integers from 0 to 20.

[0026] The above crosslinking agent can be represented by the following chemical formula 4 or chemical formula 5.

[0027] [Chemical Formula 4]

[0028]

[0029] [Chemical Formula 5]

[0030]

[0031] In the above chemical formulas 4 and 5, R 1, R 2, and R3 are each hydrogen or a methyl group, and m, n and t are each integers from 0 to 20.

[0032] According to another aspect of the present invention, the present invention provides a solid polymer electrolyte manufactured by including the solid polymer electrolyte composition described above.

[0033] The above solid polymer electrolyte may be manufactured by an in situ crosslinking polymerization method.

[0034] According to another aspect of the present invention, the present invention provides a lithium secondary battery manufactured including the above-described solid polymer electrolyte.

[0035] The above solid polymer electrolyte may be coated using a roll-to-roll process.

[0036] According to the present invention, a solid polymer electrolyte composition containing a cyclic siloxane compound having low viscosity and excellent impregnation properties is provided, and further, a solid polymer electrolyte manufactured from the composition can provide an excellent separator function.

[0037] According to the present invention, by mixing a polyalkylene oxide compound with a cyclic siloxane compound, a composition for a solid polymer electrolyte having a viscosity that can be used in an in situ crosslinking polymerization method is provided, and there is an effect of providing a solid polymer electrolyte that can be used in a roll-to-roll production process.

[0038] According to the present invention, by using a solid polymer electrolyte in which a cyclic siloxane compound and a polyalkylene oxide compound are mixed as plasticizers, there is an effect of providing a lithium secondary battery having improved ionic conductivity, stabilization of a lithium metal negative electrode, rate characteristics, and charge / discharge cycle characteristics.

[0039] The effects of the present invention are not limited to the effects described above, and should be understood to include all effects that can be inferred from the detailed description of the present invention or the composition of the invention described in the claims.

[0040] Figure 1 shows the contact angle and viscosity measurement results for a support and electrode of a solid polymer electrolyte precursor according to one embodiment of the present invention (Comparative Example 1, Example 2, Comparative Example 2).

[0041] FIG. 2a is a graph showing the results of thermogravimetric analysis of a cyclic siloxane polymer and a linear polyalkylene oxide polymer according to one embodiment of the present invention, and FIG. 2b is a graph showing the results of thermogravimetric analysis of a film manufactured with a solid polymer electrolyte according to one embodiment of the present invention (Comparative Example 1, Example 2, Comparative Example 2).

[0042] FIG. 3a is a graph showing the results of a cyclic voltammetry measurement of a solid polymer electrolyte according to one embodiment of the present invention (Comparative Example 1, Comparative Example 2), and FIG. 3b is a graph showing the results of a linear voltammetry measurement of a solid polymer electrolyte according to one embodiment of the present invention (Comparative Example 1, Comparative Example 2).

[0043] Figure 4 is a graph showing the results of measuring the tensile strength of a solid polymer electrolyte according to one embodiment of the present invention (Comparative Example 1, Comparative Example 2).

[0044] Figure 5 is a graph showing the results of measuring the ionic conductivity of a solid polymer electrolyte according to one embodiment of the present invention (Comparative Example 1, Example 2-5, Comparative Example 2).

[0045] FIG. 6 is a graph showing the results of a lithium electrodeposition / stripping experiment in a lithium symmetric cell manufactured with a solid polymer electrolyte according to one embodiment of the present invention (Comparative Example 1, Example 2).

[0046] FIGS. 7A to 7E are graphs showing charge and discharge rate characteristics of lithium secondary batteries according to one embodiment of the present invention (FIG. 7A: Comparative Example 1, FIG. 7B: Example 1, FIG. 7C: Example 2, FIG. 7D: Example 3, FIG. 7E: Example 5), and FIG. 7F is a graph comparing discharge capacities according to cycles of lithium secondary batteries according to each of the above embodiments.

[0047] FIGS. 8A-8C are graphs showing charge / discharge cycle characteristics of a lithium secondary battery according to one embodiment of the present invention (FIG. 8A: Example 2, FIG. 8B: Example 3, FIG. 8C: Example 5), and FIG. 8D is a graph comparing discharge capacities according to cycles of lithium secondary batteries according to each of the above embodiments.

[0048] FIGS. 9A-9C are graphs showing charge / discharge rate characteristics of a lithium secondary battery according to one embodiment of the present invention (FIG. 9A: Example 1A, FIG. 9B: Example 2A, FIG. 9C: Example 3A), and FIG. 9D is a graph comparing discharge capacities according to cycles of lithium secondary batteries according to each of the above embodiments.

[0049] FIGS. 10A to 10D are graphs showing charge and discharge cycle characteristics of a lithium secondary battery according to one embodiment of the present invention (FIG. 10A: Example 1A, FIG. 10B: Example 2A, FIG. 10C: Example 3A, FIG. 10D: Example 5A), and FIG. 10E is a graph comparing discharge capacities according to cycles of lithium secondary batteries according to each of the above embodiments.

[0050] Before describing the present invention in detail, it should be understood that the terms or words used in this specification should not be interpreted as being unconditionally limited to their usual or dictionary meanings, and that the inventor of the present invention may appropriately define and use the concepts of various terms in order to explain his or her invention in the best possible manner, and further, that these terms or words should be interpreted as meanings and concepts that are consistent with the technical idea of ​​the present invention.

[0051] That is, it should be noted that the terms used in this specification are only used to describe preferred embodiments of the present invention, and are not intended to specifically limit the contents of the present invention, and that these terms are defined in consideration of various possibilities of the present invention.

[0052] Additionally, in this specification, it should be noted that singular expressions may include plural expressions unless the context clearly indicates a different meaning, and similarly, even if expressed in plural, may include a singular meaning.

[0053] Throughout this specification, whenever a component is described as "including" another component, it may mean that the component may further include any other component, rather than excluding any other component, unless specifically stated otherwise.

[0054] In addition, in the following description of the present invention, a detailed description of a configuration that is judged to unnecessarily obscure the gist of the present invention, for example, a known technology including a prior art, may be omitted.

[0055] Hereinafter, the present invention will be described in more detail.

[0056] The present invention provides a composition for a solid polymer electrolyte, comprising a cyclic siloxane-based compound as a first plasticizer; a polyalkylene oxide-based compound as a second plasticizer; a crosslinking agent; a lithium salt; and a curing initiator.

[0057] The plasticizer of the present invention is intended to improve ion conductivity by improving lithium salt dissociation and lithium ion conductivity, and may be included in an amount of 40 to 80 wt% with respect to the entire composition.

[0058] The above plasticizer includes a cyclic siloxane compound (first plasticizer) and a polyalkylene oxide compound (second plasticizer), and the cyclic siloxane compound and the polyalkylene oxide compound may be polymers.

[0059] As the first plasticizer, the cyclic siloxane compound can be represented by chemical formula 1.

[0060] [Chemical Formula 1]

[0061]

[0062] In the above chemical formula 1, R1 and R2 are each hydrogen or a methyl group, and m and n are each integers from 0 to 20.

[0063] As the second plasticizer, the polyalkylene oxide compound may be a linear polyalkylene oxide represented by the following chemical formula 2 or a branched polyalkylene oxide represented by the following chemical formula 3.

[0064] As the linear alkylene oxide, polyalkylene glycol dialkyl ether can be used, and as the branched polyalkylene oxide, ethylene oxide-propylene oxide or trivalent polyalkylene oxide can be used.

[0065] [Chemical Formula 2]

[0066]

[0067] [Chemical Formula 3]

[0068]

[0069] In the above chemical formulas 2 and 3, R3, R4, R5, R3', R4', and R5' is hydrogen or methyl group, and R6, R7, R6', and R7' is a chain or branched alkyl group having 1 to 10 carbon atoms, and o, p, q, x, y, and z are each integers from 0 to 20.

[0070] The crosslinking agent of the present invention can crosslink a polymer electrolyte by forming a three-dimensional network structure by including an acrylic group in its molecular structure, and can also control the physical properties of the electrolyte by controlling the chain length of the polyalkylene oxide included in the molecular structure, and can be included in an amount of 10 to 50 wt% with respect to the entire composition.

[0071] The above crosslinking agent can be represented by the following chemical formula 4 or chemical formula 5.

[0072] [Chemical Formula 4]

[0073]

[0074] [Chemical Formula 5]

[0075]

[0076] In the above chemical formulas 4 and 5, R1, R2, and R3 are each hydrogen or a methyl group, and m, n, and t are each integers from 0 to 20.

[0077] The lithium salt of the present invention may be one used for manufacturing a polymer electrolyte in the present technical field, and examples thereof include LiTFSI, LiClO4, LiCF3SO3, LiBF4, LiPF6, LiAsF6, Li(CF3SO2)2N, etc. The lithium salt may be included in an amount of 5 to 40 wt% based on the total composition.

[0078] Examples of the photocurable initiator of the present invention include ethylbenzoin ether, isopropylbenzoin ether, α-methylbenzoin ethyl ether, benzoin phenyl ether, α-acyl oxime ester, α,α-diethoxy acetophenone, 1,1-dichloroacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one [Darocur 1173 from Ciba Geigy], 1-hydroxycyclohexyl phenyl ketone [Irgacure 184 from Ciba Geigy], Darocur 1116, Irgacure 907, etc., and anthraquinone, 2-ethyl anthraquinone, 2-chloro anthraquinone, thioxanthone, isopropyl thioxanthone, Examples of the curing initiator include chlorothioxanthone, benzophenone, p-chlorobenzophenone, benzyl benzoate, benzoyl benzoate, and Michler's ketone. Examples of the thermosetting initiator include azoisobutyronitrile and peroxide. The curing initiator may be included in an amount of 0.1 to 5 wt% based on the total composition.

[0079] The viscosity of the composition is preferably 100 to 150 cP, more preferably 100 to 140 cP. If the viscosity of the composition is less than the above range, lithium dendrites are formed due to the low mechanical strength of the polymer electrolyte after crosslinking polymerization, and a short circuit problem occurs. If the viscosity exceeds the above range, there are problems such as low impregnation properties, deterioration of rate characteristics and cycle stability, and in particular, as the loading value of the electrode increases, there is a problem that the battery characteristics deteriorate even more.

[0080] In addition, the viscosity of the solid polymer electrolyte composition of the present invention can be controlled according to the mixing weight ratio of the cyclic siloxane compound (first plasticizer) and the polyalkylene oxide compound (second plasticizer).

[0081] The mixing weight ratio of the above cyclic siloxane compound (first plasticizer) and the polyalkylene oxide compound (second plasticizer) may be 3:7 to 1:9, or 3:7, 4:6, 5:5, 6:4, 7:3, 8:2, 9:1, and more preferably 5:5 to 1:9 or 5:5, 6:4, 7:3, 8:2, 9:1.

[0082] According to an embodiment of the present invention, the viscosity can be controlled by mixing a cyclic siloxane-based compound (first plasticizer) and a polyalkylene oxide-based compound (second plasticizer) in the above weight ratio. When the mixed plasticizer with controlled viscosity is applied to a solid polymer electrolyte and a lithium secondary battery, the battery performance such as ionic conductivity, stabilization of the lithium metal negative electrode, rate characteristics, and charge / discharge cycle characteristics is improved. In addition, when the mixed plasticizer with controlled viscosity is used, there is an effect that in situ crosslinking polymerization and roll-to-roll processes can be applied.

[0083] The present invention provides a solid polymer electrolyte manufactured by including the solid polymer electrolyte composition described above.

[0084] The above solid polymer electrolyte may be manufactured by in situ crosslinking polymerization of the above-described solid electrolyte composition.

[0085] The present invention provides a lithium secondary battery manufactured including the above-described solid polymer electrolyte.

[0086] The above lithium secondary battery may be one in which the above-described solid polymer electrolyte is coated using a roll-to-roll process.

[0087] Example

[0088] Hereinafter, the present invention will be described in detail with examples to specifically illustrate it. However, the examples according to the present invention may be modified in various ways, and the scope of the present invention should not be construed as being limited to the examples described below. These examples are provided to more fully explain the present invention to those of average skill in the art.

[0089] <Materials>

[0090] 1. Cyclotetrasiloxane polymer: Cyclotetrasiloxane-polyethylene glycol (CTS-PEG), number average molecular weight 1,057

[0091]

[0092] 2. Polyalkylene oxide polymer:

[0093] ㉮ Polyethylene glycol dimethyl ether (PEGDME), number average molecular weight 464, as a linear polyalkylene oxide polymer,

[0094] ㉯ Poly(ethylene glycol)dimethyl ether (PEGDME), a low molecular weight linear polyalkylene oxide polymer, number average molecular weight 250

[0095]

[0096] ㉰ Trimethylolpropane ethyl ether (TMPEE), a trivalent polyalkylene oxide polymer, number average molecular weight 572

[0097]

[0098] ㉱ Ethylene oxide-propylene oxide plasticizer [EO-PO copolymer, number average molecular weight 572]

[0099]

[0100] 3. Crosslinking agent:

[0101] ㉮ Bisphenol A ethoxylate diacrylate [Ethoxylated(4) bisphenol A diacrylate (Bis A), number average molecular weight 688)

[0102]

[0103] Cyclotetrasiloxane-acrylate [Cyclotetrasiloxane-acrylate, average molecular weight 1,217]

[0104]

[0105] 4. Lithium salt: Lithium bis((trifluoromethyl)sulfonyl)amide [Lithium bis((trifluoromethyl)sulfonyl)amide, LiTFSI]

[0106] 5. Curing initiator: tert-Butyl peroxypivalate (t-BPP)

[0107] <Comparative Examples and Examples>

[0108] The polymer electrolyte precursors of the comparative examples and examples were prepared by mixing the components listed in Table 1.

[0109]

[0110] (The content unit of each component in Table 1 is g, and cyclic siloxane: polyalkylene oxide is the weight ratio)

[0111] <Experimental Example 1: Contact Angle and Viscosity Measurement>

[0112] The polymer electrolyte precursors manufactured in Comparative Examples 1 and 2 and Example 2 were dropped onto the electrode active material coated on a polyvinylidene fluoride-polyacrylonitrile membrane (PVDF-PAN) as a support and an aluminum foil current collector, and the contact angle and viscosity characteristics were measured, and the results are shown in Fig. 1.

[0113] To measure the contact angle, the polymer electrolyte precursor was dropped onto the support and electrode, respectively, and then digitally photographed. The right and left angles were calculated and the average value was used to indicate the contact angle. In addition, the viscosity was measured using a rotational viscometer to numerically confirm the viscosity difference confirmed through the contact angle. The polymer electrolyte precursors manufactured in Comparative Examples 1 and 2 and Example 2 were prepared into compositions in 10 mL units, and the viscosity was measured and indicated below the contact angle.

[0114] The contact angle measurement test conditions were a 22-gauge needle and a temperature of 25°C. Contact angles were measured digitally using software Generated by Surfaceware 7. Furthermore, contact angle measurements were performed three times for each sample, and the average angle value was taken.

[0115] The viscosity measurement test conditions were compared through the average value after measuring three times using a rotational viscometer with an SC4-31(31) spindle and a rotational speed of 250 rpm.

[0116] Referring to Fig. 1, the cyclic siloxane polymer electrolyte precursor of Comparative Example 1 showed a contact angle of about 40° with the support, indicating low impregnation due to high viscosity, and a high viscosity of 165.7 cP. On the other hand, the polyalkylene oxide polymer electrolyte precursor of Comparative Example 2 showed a low contact angle of about 20° due to low viscosity, and a low viscosity of 110.5 cP. The polymer electrolyte precursor in which the cyclic siloxane polymer and the polyalkylene oxide polymer are mixed in a weight ratio of 1:1 shows a contact angle with respect to the support similar to that of the low-viscosity polyalkylene oxide polymer electrolyte precursor. The contact angle with respect to the electrode also showed a value of 23° with respect to the cyclic siloxane polymer electrolyte precursor of Comparative Example 1, indicating relatively low impregnation, whereas after mixing it with the polyalkylene oxide polymer electrolyte precursor in a weight ratio of 1:1 to lower the viscosity, it showed high impregnation. As a result of viscosity measurement, the viscosity was 138.1 cP, which was lower than that of the cyclic siloxane polymer electrolyte precursor of Comparative Example 1.

[0117] The viscosity of the polymer electrolyte precursor (plasticizer + crosslinker + lithium salt) according to an embodiment of the present invention was measured and shown in Table 2.

[0118]

[0119] <Experimental Example 2: Thermal Stability Measurement>

[0120] To evaluate the thermal stability of the polymer electrolytes according to Comparative Examples 1 and 2 and Example 2, they were analyzed using a thermogravimetric analyzer (TGA).

[0121] The results of thermogravimetric analysis for the polymer electrolyte precursors of Comparative Examples 1 and 2 are shown in Fig. 2a. During thermogravimetric analysis, the weight loss of the sample was measured in real time while the temperature was increased from room temperature to 800°C at a rate of 10°C per minute in a nitrogen reflux atmosphere of 50 ml per minute.

[0122] Referring to Fig. 2a, the cyclic siloxane polymer (CTS-PEG) of Comparative Example 1 experienced a rapid weight loss after 320°C, whereas the linear polyalkylene oxide polymer (PEGDME) of Comparative Example 2 experienced a rapid weight loss around 160°C. These TGA analysis results indicate that the cyclic siloxane polymer is a polymer with high thermal stability up to about 200°C. Meanwhile, it can be seen that the cyclic siloxane polymer retains about 5% of its thermal weight above 400°C after thermal decomposition. These results demonstrate that the cyclic siloxane polymer, CTS-PEG, contains a silica inorganic substance with high thermal stability.

[0123] The polymer electrolyte precursor compositions manufactured in Comparative Examples 1 and 2 and Example 2 were coated on a substrate and cured by heating (90°C, 30 minutes) to manufacture a polymer solid electrolyte in the form of a film (thickness 300 μm). The results of thermogravimetric analysis for each of these are shown in Fig. 2b.

[0124] Referring to Fig. 2b, the polymer electrolyte according to Comparative Example 2 exhibited a decomposition temperature of 210°C, while the polymer electrolyte according to Comparative Example 1 exhibited a decomposition temperature of 350°C, indicating that the cyclic siloxane polymer exhibited high thermal properties even within the polymer electrolyte. The polymer electrolyte according to Example 2 (cyclic siloxane: polyalkylene oxide = 1:1 weight ratio mixed) exhibited a rapid weight loss after 270°C. These TGA analysis results indicate that the polymer electrolyte manufactured with the cyclic siloxane polymer has high thermal stability up to about 140°C, and can exhibit relatively high thermal stability even within a polymer electrolyte in which the cyclic siloxane polymer and the linear polyalkylene oxide polymer are mixed.

[0125] <Experimental Example 3: Electrochemical Stability Evaluation>

[0126] To compare the electrochemical stability of the polymer electrolytes according to Comparative Examples 1 and 2, measurements were made using cyclic voltammetry and linear voltammetry.

[0127] Coin cells were manufactured by placing a film impregnated with a polymer electrolyte on a support on a lithium metal anode, and then cured by applying heat (90°C for 30 minutes), and the change in current versus voltage was evaluated. Cyclic voltammetry and linear voltammetry were performed at a scan rate of 1.0 mV s. -1 The test was conducted under conditions of 25 ℃, and the results are shown in Fig. 3a and Fig. 3b, respectively.

[0128] Referring to the results of the cyclic oscillation injection method measurement in Fig. 3a, the cyclic siloxane polymer electrolyte (CTS-PEG SPE) hardly generated peaks for the reduction reaction in the negative voltage scanning direction and the oxidation reaction in the positive voltage scanning direction. On the other hand, the alkylene oxide polymer electrolyte (PEGDME SPE) generated peaks for the reduction and oxidation reactions at ±0.01 mA cm -2 Since it appears relatively large, it was confirmed that it has lower electrochemical stability compared to cyclic siloxane polymer electrolyte.

[0129] Referring to the linear voltage measurement results of Fig. 3b, it can be confirmed that the cyclic siloxane polymer electrolyte (CTS-PEG SPE) has much higher electrochemical stability than the alkylene oxide polymer electrolyte (PEGDME SPE).

[0130] <Experimental Example 4: Mechanical Strength Evaluation>

[0131] In order to evaluate the mechanical properties of the polymer electrolyte films according to Comparative Examples 1 and 2, a tensile strength test was conducted, and the resulting strain-stress graph is shown in Fig. 4.

[0132] For the tensile strength test, the support was cut into 1 cm × 7 cm pieces, impregnated with the polymer electrolytes of Comparative Examples 1 and 2, and then cured by applying heat (90°C, 30 min) to prepare a specimen. Measurements were performed using a Lloyd-TA1 Texture Analyzer, and the tensile test conditions were a speed of 20.0 mm / min and a temperature of 25°C. Ten tensile tests were performed on each sample, and the average property value was taken, from which the tensile strength value of the polymer electrolyte was calculated.

[0133] Referring to Figure 4, the cyclic siloxane polymer electrolyte (CTS-PEG SPE) exhibited a tensile strength of 15.27 MPa, and the alkylene oxide polymer electrolyte (PEGDME SPE) exhibited a tensile strength of 6.83 MPa. It can be clearly seen that when the cyclic siloxane polymer was applied, the mechanical strength increased by more than two times due to the inclusion of silica inorganic matter.

[0134] <Experimental Example 5: Evaluation of Ionic Conductivity Characteristics>

[0135] The ionic conductivity of the polymer electrolyte according to Comparative Examples 1 and 2 and Example 2-5 was measured, and the results are shown in Fig. 5 and Table 3.

[0136] For the ionic conductivity evaluation test, coin cells with a SUS / solid polymer electrolyte / SUS structure were manufactured, and the coin cells were connected in a temperature-controllable oven, and the AC impedance was measured at each temperature range using an impedance meter (Zennium XC). The temperatures at which the ionic conductivity was measured were 25 ℃, 45 ℃, and 60 ℃, respectively.

[0137] Referring to the ionic conductivity evaluation results in Fig. 5 and Table 3, the solid polymer electrolyte (CTS-PEG) according to Comparative Example 1 has a conductivity of 5.63×10 at 25°C. -5 S cm -1 Although it exhibits low ionic conductivity, the solid polymer electrolyte (PEGDME) according to comparative example 2 has a conductivity of 1.42×10-4 S cm -1 The ionic conductivity was clearly increased, and the lower the viscosity, the higher the ionic conductivity tended to be. In particular, in the solid polymer electrolyte according to Example 2 [mixed solid polymer to which 8 wt.% of high-viscosity cyclic siloxane polymer and 72 wt.% of low-viscosity linear polyalkylene oxide polymer were applied], the ionic conductivity was 1.01×10 at 60°C. -3 S cm -1 It shows high ionic conductivity, and it can be confirmed that there is an effect of improving ionic conductivity by controlling viscosity through a mixed polymer electrolyte.

[0138]

[0139] <Experimental Example 6: Evaluation of Reaction Stability with Lithium Metal>

[0140] In order to evaluate the reaction stability of the solid polymer electrolyte with lithium metal, a lithium plating / stripping test was performed in a lithium symmetric cell with the solid polymer electrolyte interposed between two lithium electrodes, and the results are shown in Fig. 6.

[0141] The lithium plating / stripping test was performed at 45°C, sequentially performing 10 cycles of 36,000-second electrodeposition and 36,000-second stripping at 0.1 mA per lithium area, 10 cycles of 18,000-second electrodeposition and 18,000-second stripping at 0.2 mA, 10 cycles of 7,200-second electrodeposition and 7,200-second stripping at 0.5 mA, and 10 cycles of 3,600-second electrodeposition and 3,600-second stripping at 1.0 mA.

[0142] Referring to Figure 6, when evaluating the voltage change in an environment where the deposition and stripping of repeated Li ions are increased, no significant difference was observed when the deposition and stripping were performed at low rates, but at 1.0 mA / cm 2When electrodepositing and stripping at a high speed, it was confirmed that the polymer electrolyte in which the cyclic siloxane and linear polyalkylene oxide of Example 2 were mixed in a 1:1 ratio had a lower overvoltage than the cyclic siloxane polymer electrolyte of Comparative Example 1. The polymer electrolyte of Comparative Example 1 showed an overvoltage of ±0.25 V, whereas the polymer electrolyte in which the polyalkylene oxide and cyclic siloxane of Example 2 were mixed in a 1:1 ratio showed an overvoltage of ±0.15 V, confirming its high stability. Through this, it was confirmed that when the polymer electrolyte with controlled viscosity was applied, it greatly contributed to stabilizing the lithium metal negative electrode in an environment in which charging and discharging were performed at a high speed.

[0143] Experimental Example 7: Rate Test

[0144] A lithium secondary battery was manufactured using a polymer electrolyte manufactured using the linear polyalkylene oxide polymer, a negative electrode of lithium metal, and a positive electrode having a positive electrode active material of LFP (LiFePO4), and a charge / discharge rate test was performed, and the results are shown in FIGS. 7a to 7f.

[0145] The charge / discharge rate test (C-rate) was conducted with the upper charge voltage limit set at 4.0 V and the lower discharge voltage limit set at 2.5 V during the charge / discharge cycle. The test temperature was 60°C, and the charge / discharge cycle was repeated 5 times for each rate.

[0146] Figure 7a is a discharge curve according to the rate of the polymer electrolyte (CTS-PEG) of Comparative Example 1, according to which, at low rates of 0.1 C and 0.2 C, each of 150 mAh g -1 Wow 130 mAh g -1Although the capacity was expressed at high rates of 0.5 C and 1.0 C, the capacity expression was almost nonexistent. Through this, it can be observed that the battery characteristics were low due to the problems of impregnation and ion transfer when high-viscosity CTS-PEG was applied. In addition, referring to Figures 7b to 7e, as the weight ratio of low-viscosity linear polyalkylene oxide increased, the capacity at high rates of 0.5 C and 1.0 C increased. Based on the first cycle of 1.0 C, when only high-viscosity cyclic siloxane polymer was applied, the capacity expression was 6 mAh g -1 The capacity was shown as 81 mAh g, but as the viscosity was lowered, -1 , 106 mAh g -1 , 118 mAh g -1 , 151 mAh g -1 It can be confirmed that the increased capacity is effective in improving battery characteristics. Referring to the discharge capacity comparison graph according to cycle in Fig. 7f, the effect of improving rate characteristics through viscosity control described above can be compared at a glance.

[0147] <Experimental Example 8: Charge / Discharge Cycle Test>

[0148] In order to confirm the capacity change rate results for 100 cycles of the lithium secondary battery manufactured in Experimental Example 7, the charge / discharge cycle characteristics were measured.

[0149] During the charge / discharge cycle, the upper limit voltage for charging was 4.0 V, the lower limit voltage for discharging was 2.5 V, the test temperature was 60 ℃, and the charge / discharge was repeated 100 times under the conditions of 0.3 C CC for charging and 0.5 C CC for discharging. The results of the 0.3 C / 0.5 C charge / discharge curve graphs for every 10 cycles are shown in Fig. 8.

[0150] Figures 8a to 8c illustrate capacity retention change curves after 100 cycles compared to the initial capacity. The lithium secondary battery in which the high-viscosity cyclic siloxane polymer and the low-viscosity linear polyalkylene oxide polymer of Figure 8a were mixed in the same ratio showed a capacity decrease from the initial cycle, and the capacity retention rate was only 69% after 100 cycles. On the other hand, the lithium secondary battery in which the high-viscosity cyclic siloxane polymer and the low-viscosity linear polyalkylene oxide polymer of Figure 8b were mixed in a 3:7 ratio showed a gradual capacity decrease until the 70th cycle, but a rapid decrease in discharge capacity thereafter, and showed a capacity retention rate of 68% after 100 cycles. The lithium secondary battery in which the high-viscosity cyclic siloxane polymer and the low-viscosity linear polyalkylene oxide polymer are mixed in a ratio of 1:9 in Fig. 8c exhibited a capacity retention rate of 99% after 100 cycles, demonstrating significantly higher performance with almost no capacity decrease. The cycle life test confirmed that adjusting the viscosity of the mixed polymer electrolyte was effective in improving the cycle life in an actual battery environment. In addition, the effect of improving cycle characteristics through the viscosity adjustment can be compared at a glance through the discharge capacity comparison graph according to the cycle in Fig. 8d.

[0151] <Experimental Example 9: Rate Test (Trivalent Polyalkylene Oxide Polymer)>

[0152] In order to confirm whether the same behavior is observed when a trivalent polyalkylene oxide polymer is mixed with a high-viscosity cyclic siloxane polymer in addition to a linear polyalkylene oxide polymer, polymer electrolyte precursors of Examples 1A, 2A, and 3A using a trivalent polyalkylene oxide polymer instead of a linear polyalkylene oxide polymer were prepared, and lithium secondary batteries were prepared in the same manner as in Experimental Example 7, followed by rate tests. The rate test results for the lithium secondary batteries according to Examples 1A, 2A, and 3A are shown in FIGS. 9A to 9D.

[0153] The charge / discharge rate test (C-rate) was conducted at a test temperature of 45°C with an upper charge limit voltage of 4.0 V and a lower discharge limit voltage of 2.5 V during the charge / discharge cycle, and 5 cycles of charge / discharge were repeated for each rate.

[0154] Referring to FIGS. 9a to 9c, similarly to the case of the mixed polymer electrolyte using the linear polyalkylene oxide polymer of Experimental Example 7, in the case of the high viscosity of FIG. 9a, the capacity development at high rates of 0.5 C and 1.0 C is not good, whereas in FIGS. 9b and 9c, where the ratio of the low viscosity trivalent polyalkylene oxide polymer is increased, the capacity development at high rates is good, proving that it is possible to improve battery characteristics through viscosity control.

[0155] <Experimental Example 10: Charge-Discharge Cycle Test (Trivalent Polyalkylene Oxide Polymer)>

[0156] In order to confirm the results of capacity change rate over 100 cycles when the viscosity was adjusted using a trivalent polyalkylene oxide polymer as a low-viscosity polymer, as in Experimental Example 9, a charge / discharge cycle test was performed on lithium secondary batteries according to Examples 1A, 2A, 3A, and 5A.

[0157] During the charge / discharge cycle, the upper limit voltage for charging was 4.0 V, the lower limit voltage for discharging was 2.5 V, the test temperature was 45°C, and the charge / discharge was repeated 100 times under the conditions of 0.3 C CC for charging and 0.3 C CC for discharging. The results of the 0.3 C / 0.3 C charge / discharge curve graphs for every 10 cycles are shown in Figures 10a to 10e.

[0158] Referring to FIGS. 10a to 10e, as confirmed through the above-described Example 8 and FIG. 8, it can be confirmed that the cycle life of the battery is improved by lowering the viscosity to a level of 100 to 140 cP through mixing with a low-viscosity polymer.

[0159] So far, specific examples of a solid polymer electrolyte composition containing a cyclic siloxane compound according to one embodiment of the present invention, and a solid polymer electrolyte and a secondary battery including the same have been described, but it is obvious that various modifications are possible within the scope of the present invention.

[0160] Therefore, the scope of the present invention should not be limited to the described embodiments, but should be defined not only by the claims described below but also by equivalents of the claims.

[0161] That is, it should be understood that the above-described embodiments are exemplary in all respects and not restrictive, and the scope of the present invention is indicated by the claims to be described later rather than the detailed description, and all changes or modified forms derived from the meaning and scope of the claims and their equivalent concepts should be interpreted as being included in the scope of the present invention.

[0162] The present invention provides a solid polymer electrolyte composition containing a cyclic siloxane compound having low viscosity and excellent impregnation properties, including a mixture of a cyclic siloxane compound and a polyalkylene oxide compound as a plasticizer, and a solid polymer electrolyte and a secondary battery including the same.

Claims

1. Cyclic siloxane compound as a first plasticizer; Polyalkylene oxide compound as a second plasticizer; crosslinking agent; lithium salt; and Containing a curing initiator, Composition for solid polymer electrolyte.

2. In paragraph 1, Characterized in that the viscosity of the above composition is 100 to 150 cP, Composition for solid polymer electrolyte.

3. In paragraph 1, The viscosity of the above composition is Characterized in that it is controlled according to the mixing weight ratio of the first plasticizer and the second plasticizer. Composition for solid polymer electrolyte.

4. In paragraph 1, The weight ratio of the first plasticizer and the second plasticizer is characterized by a ratio of 7:3 to 1:9, Composition for solid polymer electrolyte.

5. In paragraph 1, The composition is characterized in that it contains 40 to 80 wt% of a first plasticizer and a second plasticizer, 10 to 50 wt% of a crosslinking agent, 5 to 40 wt% of a lithium salt, and 0.1 to 5 wt% of a curing initiator. Composition for solid polymer electrolyte.

6. In paragraph 1, The above cyclic siloxane compound is represented by chemical formula 1, Composition for solid polymer electrolyte. [Chemical Formula 1] In the above chemical formula 1, R1 and R2 are each hydrogen or methyl group, m and n are integers from 0 to 20, respectively.

7. In paragraph 1, The above polyalkylene oxide compound is Represented by the following chemical formula 2 or chemical formula 3, Composition for solid polymer electrolyte. [Chemical Formula 2] [Chemical Formula 3] In the above chemical formulas 2 and 3, R3, R4, R5, R3', R4', and R5' is each hydrogen or methyl group, R6, R7, R6', and R7' is a chain or branched alkyl group having 1 to 10 carbon atoms, o, p, q, x, y, and z are each integers from 0 to 20.

8. In paragraph 1, The above crosslinking agent is represented by the following chemical formula 4 or chemical formula 5: Composition for solid polymer electrolyte. [Chemical Formula 4] [Chemical Formula 5] In the above chemical formulas 4 and 5, R 1, R 2, and R3 are each hydrogen or methyl group, m, n, and t are integers from 0 to 20, respectively.

9. A solid polymer electrolyte manufactured by including the solid polymer electrolyte composition of paragraph 1.

10. In paragraph 9, Characterized in that it is manufactured by an in situ crosslinking polymerization method, Solid polymer electrolyte.

11. A lithium secondary battery manufactured including the solid polymer electrolyte of Article 9.

12. In paragraph 11, Characterized in that the above solid polymer electrolyte is coated by a roll-to-roll process, Lithium secondary battery.

Citation Information

Patent Citations

  • Composition for lithium ion conductive electrolyte and production method for lithium ion conductive electrolyte

    JP2006185831A

  • Polymer solid electrolyte, lithium ion secondary battery, and method of manufacturing lithium ion secondary battery

    JP2023050364A

  • Cyclic siloxane-based compounds and solid polymerelectrolyte composite containing the same

    KR1020060102414A

  • Apparatus for producing lithium polymer battery using continuous roll-to-roll system by direct solution casting technology and method for producing lithium polymer battery using the sam ...

    KR1020130071333A

  • Multifunctional machined distribution wire supporting mechanism for electric pole installation

    KR102583139B1