Method for manufacturing contact lens using raw material in which MPC is dispersed
The method of dispersing MPC in contact lens raw materials and using radiation-induced crosslinking addresses the challenges of material loss and uneven polymerization in conventional processes, improving the mechanical and moisture retention properties of contact lenses.
Patent Information
- Application Number
- PCT/KR2024/007306
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-05-28
- Filing Date
- 2024-05-29
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional contact lens manufacturing processes face challenges with the use of 2-methacryloyloxyethylphosphorylcholine (MPC) due to its ultrafine powder state, leading to material loss and uneven polymerization, resulting in residual unreacted monomers and the need for additional processing steps to remove cross-linking agents and initiators, which affects the safety and durability of the lenses.
A method involving the dispersion of MPC in a raw material mixture with hydrophilic monomers and additives, followed by radiation-induced crosslinking, which allows for controlled polymerization and eliminates the need for thermal cross-linking agents and initiators, thereby improving the mechanical properties and reducing material loss.
This method enhances the mechanical properties and durability of contact lenses by ensuring uniform crosslinking, reducing unreacted monomers, and preventing economic losses associated with MPC loss, while maintaining the moisture and protein inhibition properties of MPC.
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
Method for manufacturing contact lenses using MPC-dispersed raw materials
[0001] The present invention relates to a method for manufacturing a contact lens using a raw material in which MPC is dispersed, and more specifically, to a method for manufacturing a contact lens comprising a first step of manufacturing a raw material in which 2-methacryloyl oxyethyl phosphorylcholine is dispersed, a second step of mixing a hydrophilic monomer and an additive with the raw material, and a third step of injecting the mixture of the second step into a mold for manufacturing a contact lens and polymerizing the mixture to obtain a contact lens.
[0002] The demand for contact lenses is increasing day by day as they have various functions such as vision correction, treatment, and beauty. These contact lenses can be divided into hard contact lenses and soft contact lenses depending on the material. Hard contact lenses are made of hard materials that do not absorb moisture, such as glass or acrylic resin, and soft contact lenses are made of soft materials with high moisture content, such as hydrogel (hydrophilic polymer) and silicone hydrogel. Contact lenses, which first appeared in the 1880s, were made of glass, but since then, materials that are more comfortable to wear and provide better oxygen supply to the eyes have been developed. Currently, most contact lenses are made of oxygen-permeable materials (hard contact lenses) and lenses made of hydrogel or silicone hydrogel materials (soft contact lenses).
[0003] Typically, soft contact lenses are manufactured using polymers produced by polymerizing raw materials. This polymer production process utilizes a chemical method that adds cross-linkers and initiators that form free radicals, and then polymerizes at a certain temperature for a certain period of time. This polymerization method, which necessarily requires cross-linkers and initiators, not only necessitates a post-polymerization process to remove the added substances, but also causes problems such as reduced lens functionality if any residue remains. Furthermore, although this polymerization process converts monomers into hydrogel polymers, the polymerization reaction does not occur uniformly across all monomers, resulting in unreacted monomers remaining, which can compromise the safety and durability of the contact lens. Therefore, the development of new methods to resolve the problems that arise during the polymerization of contact lens raw materials is necessary.
[0004] Meanwhile, 2-methacryloyloxyethyl phosphorylcholine (MPC) is a material used to coat artificial organs that replace human organs. It can be used in the human body without rejection, so it is used as a medical material for implants, artificial hearts, artificial joints, and hemodialysis filters. It also has a bacterial deposition inhibitory function, so it is used as a surface coating agent for dental resins. In addition to these functions, MPC has functions such as protein adsorption inhibition and moisture retention. It improves the comfort of contact lenses by inhibiting the adsorption of proteins present in tears to contact lenses, and increases moisture content to moisturize, thereby preventing dry eyes caused by wearing contact lenses. Therefore, it is used as a raw material for contact lenses. While there are various advantages to using MPC as a raw material for contact lenses, there is a problem that it is difficult to use MPC in large quantities due to difficulties in the manufacturing process. For example, when using a large amount of MPC, which is generally stored frozen, moisture condenses due to the condensation point of the MPC, which deteriorates its physical properties. In addition, since expensive MPC is in an ultrafine powder state, it is inevitable that losses will occur during the process of measuring a large amount of MPC. This loss of MPC inevitably leads to economic losses. Therefore, it is necessary to develop a technology to apply MPC stably and efficiently while using a large amount of MPC as a raw material for contact lenses.
[0005] Accordingly, the inventors of the present invention have made extensive research efforts to overcome the problems of the above-mentioned conventional technologies, and as a result, when manufacturing a contact lens through a first step of manufacturing a raw material in which 2-methacryloyl oxyethyl phosphorylcholine is dispersed, a second step of mixing a hydrophilic monomer and an additive with the raw material, and a third step of injecting the mixture of the second step into a mold for manufacturing a contact lens and polymerizing it, the step of manufacturing a raw material in which 2-methacryloyl oxyethyl phosphorylcholine is dispersed allows a large amount of a raw material, such as 2-methacryloyl oxyethyl phosphorylcholine (MPC), which is difficult to control in quantity, to be included, thereby improving the functional properties of the contact lens. In addition, when a raw material in which 2-methacryloyl oxyethyl phosphorylcholine is dispersed is used as a raw material for contact lenses, crosslinking control is possible during polymerization of the entire raw material for contact lenses, thereby suppressing unreacted monomers from remaining in the polymer, thereby improving the mechanical properties of the contact lens. In addition to improving the physical properties, it was confirmed that problems arising from the use of crosslinking agents and initiators could be resolved by reacting the polymerization reaction of raw materials through irradiation, and this led to the completion of the present invention.
[0006] Accordingly, the main purpose of the present invention is to provide a method for manufacturing a contact lens using a crosslinked polymer that can improve the functionality and mechanical properties of the contact lens.
[0007] According to one aspect of the present invention, the present invention provides a method for manufacturing a contact lens, comprising a first step of manufacturing a raw material in which 2-methacryloyl oxyethyl phosphorylcholine (MPC) is dispersed, a second step of mixing a hydrophilic monomer and an additive with the raw material, and a third step of injecting the mixture of the second step into a mold for manufacturing a contact lens and then polymerizing the mixture to obtain a contact lens.
[0008] In the past, in the manufacturing process of contact lenses, raw materials such as 2-methacryloyloxyethyl phosphorylcholine (MPC), which is used in the manufacturing of soft contact lenses, were in an ultrafine powder state, so there were problems in that expensive raw materials were lost during the process of measuring them, and in the process of polymerizing the entire raw material, the polymerization reaction was not uniform, so unreacted monomers remained, and an additional process for removing crosslinking agents, initiators, etc. included in the polymerization process had to be performed. Therefore, the inventors of the present invention confirmed that the above problems can be solved when some raw materials, including MPC, are dispersed by radiation to first manufacture a crosslinked raw material and then the crosslinked raw material is used as a raw material for manufacturing contact lenses, and thus the present invention was completed.
[0009] In the method for manufacturing a contact lens of the present invention, the raw material in which the MPC is dispersed may be one manufactured by mixing MPC and a silicone monomer or hydrophilic monomer used in manufacturing a soft contact lens and irradiating the mixed mixture, but is preferably one in which 2-methacryloyloxyethylphosphorylcholine (MPC) is dispersed in at least one of hydroxyethyl methacrylate (HEMA) and propenoic acid-2-methyl-2-hydroxy-3-[3-[1,3,3,3-tetramethyl-1-[(trimethylsilyl)oxy]-1-disiloxanyl]propoxy]propyl ester (SiGMA), and specifically, it is manufactured by mixing HEMA or SiGMA into MPC as a raw material, or mixing MPC, HEMA, and SiGMA, and then dispersing and crosslinking them through irradiation. The silicone monomer or hydrophilic monomer can be freely selected and combined depending on the type of contact lens to be manufactured.
[0010] In addition, the radiation can be irradiated at 1 to 100 kGy by selecting one of gamma rays, electron rays, ion beams, and x-rays, and it is preferable to irradiate electron rays at 1 to 50 kGy. In this case, if the polymerization reaction is carried out using radiation rather than a thermal polymerization reaction using a crosslinking agent, initiator, etc., not only does it not require a process for removing the crosslinking agent and initiator, but also there is no problem caused by the crosslinking agent and initiator remaining in the polymer.
[0011] In the method for manufacturing a contact lens of the present invention, when the raw material in which the MPC is dispersed is a combination of 2-methacryloyloxyethylphosphorylcholine (MPC) and hydroxyethyl methacrylate (HEMA), the MPC may be comprised in an amount of 5 to 15 wt% and the HEMA may be comprised in an amount of 5 to 20 wt%. In addition, when the raw material in which the MPC is dispersed is a combination of 2-methacryloyloxyethylphosphorylcholine (MPC) and propenoic acid-2-methyl-2-hydroxy-3-[3-[1,3,3,3-tetramethyl-1-[(trimethylsilyl)oxy]-1-disiloxanyl]propoxy]propyl ester (SiGMA), the MPC may be comprised in an amount of 1 to 10 wt% and the SiGMA may be comprised in an amount of 0.1 to 20 wt%. Here, it is preferable that the sum of the two raw materials, i.e., MPC and HEMA, or MPC and SiGMA, does not exceed 25 wt%, more preferably 20 wt%, based on the total weight of the contact lens raw material. In this way, the content of MPC included in the maximum 25 wt% based on the total weight of the contact lens raw material is measured to be less than the amount of MPC compared to the case where all contact lens manufacturing raw materials are conventionally manufactured by simple mixing and polymerization, so that measurement control is easy, and thus the loss of expensive MPC is small, thereby preventing economic loss. In addition, when the MPC raw material dispersed and cross-linked according to the present invention is used as a contact lens raw material, since it already contains cross-linked MPC, there is no need to additionally cross-link MPC, so that MPC loss due to unnecessary MPC measurement can be prevented, thereby preventing economic loss, and in addition, unreacted monomers can be suppressed from remaining in the polymer, thereby preventing the problem of deterioration in the stability and durability of the contact lens.
[0012] In the method for manufacturing a contact lens of the present invention, when the crosslinking polymerization raw material is a combination of 2-methacryloyloxyethylphosphorylcholine (MPC), hydroxyethyl methacrylate (HEMA), and propenoic acid-2-methyl-2-hydroxy-3-[3-[1,3,3,3-tetramethyl-1-[(trimethylsilyl)oxy]-1-disiloxanyl]propoxy]propyl ester (SiGMA), it may be composed of 0.1 to 2.5 wt% of MPC, 2 to 10 wt% of HEMA, and 12.5 to 22.5 wt% of SiGMA, and it is preferable that the sum of the three raw materials does not exceed 30 wt%, preferably 25 wt%, based on the total weight of the contact lens raw material.
[0013] In the method for manufacturing a contact lens of the present invention, the hydrophilic monomer may be any hydrophilic monomer conventionally used in contact lenses, but is preferably at least one selected from the group consisting of 2-hydroxyethyl methacrylate (2-HEMA), N,N-dimethylacrylamide (DMA), N-vinyl pyrrolidone (NVP), N-vinyl-N-methyl acrylamide, ethylene glycol dimethacrylate (EGDMA), methyl methacrylate (MMA), azobis isobutyronitrile (AIBN), and polyethylene glycol monomethacrylate.
[0014] In the method for manufacturing a contact lens of the present invention, the contact lens is composed of 1 to 25 wt% of a raw material in which 2-methacryloyloxyethylphosphorylcholine (MCP) is dispersed, 65 to 95 wt% of a hydrophilic monomer, and 3 to 15 wt% of an additive, wherein the additive may include at least one selected from the group consisting of an initiator, a crosslinking agent, a wettability enhancing agent, an excipient, a stabilizer, a buffer, a solvent, a viscosity controlling agent, and a pH controlling agent. In this case, when a raw material in which MPC is dispersed is used as a contact lens polymer composition, it is possible to control crosslinking to occur uniformly throughout the entire polymerization process of the raw material, thereby suppressing unreacted monomers that have not been polymerized from remaining in the polymer, thereby improving the mechanical properties, chemical properties, tensile strength, and processability of the contact lens, and reducing the defect rate.
[0015] In the method for manufacturing a contact lens of the present invention, the polymerization in the third step is crosslinking through thermal curing, and specifically, an infrared (IR) lamp is irradiated on a mold into which a mixture is injected for 10 to 60 minutes at 100 to 150°C, which enables uniform transfer of heat to the mold, thereby minimizing the occurrence of defects and thus improving the completeness of the product.
[0016] A contact lens can be manufactured by including a process for sterilizing a polymer for contact lenses manufactured through the above method.
[0017] The manufacturing process of a contact lens according to the present invention will be described in more detail.
[0018] First, a contact lens polymerization solution containing a crosslinking polymerization raw material, a hydrophilic monomer, and an additive is injected into an upper and lower mold.
[0019] Next, the liquid for manufacturing contact lenses is filled. At this time, conventionally, the liquid for manufacturing lenses was filled into a silicone tube to carry out the above step, but in this case, there was a problem that the liquid discharge shape and amount were not consistent. In order to solve the above problem, the present invention uses a quantitative discharge dispenser and a specially processed needle to enable a quantitative supply of the liquid, and improves the quality of the lens by improving the edge and thickness defects of the lens by smoothly supplying it to the center.
[0020] After assembling the upper and lower molds into which the above liquid has been injected, curing polymerization is performed to obtain a contact lens. At this time, the conventional curing process was performed using a dry oven method that dries with hot air at 110℃ to 130℃. However, since the lens mold is hemispherical, a temperature difference between the edge and the lowest part of the mold is inevitable, making it difficult to supply heat evenly, resulting in frequent occurrence of defects such as improper curing (polymerization) or wrinkles. In order to solve the above problems, in the present invention, the curing process is performed at 100℃ to 150℃ for 10 to 60 minutes using an infrared (IR) lamp, which enables even heat transfer to the mold, thereby minimizing the occurrence of defects and improving the completeness of the product. After the above curing (polymerization) process is completed, the contact lens is separated from the mold.
[0021] As described above, the method for manufacturing a contact lens of the present invention can include a large amount of a raw material, such as 2-methacryloyloxyethylphosphorylcholine (MPC), which is difficult to control in quantity, through a step of manufacturing a raw material in which 2-methacryloyloxyethylphosphorylcholine is dispersed and cross-linked, thereby improving the functional properties of the contact lens. In addition, when a primarily cross-linked raw material is used as a raw material for a contact lens, cross-linking control is possible during polymerization of the entire raw material for the contact lens, thereby suppressing unreacted monomers from remaining in the polymer, thereby improving the mechanical properties of the contact lens and resolving the problem of deterioration in safety and durability of the contact lens. In addition, by irradiating the polymerization reaction of the raw material with radiation or infrared rays, the problem caused by the use of a cross-linking agent and an initiator can be resolved.
[0022] Hereinafter, the present invention will be described in more detail through examples. These examples are intended merely to illustrate the present invention, and therefore, the scope of the present invention is not to be construed as being limited by these examples.
[0023] Examples 1 to 8: Manufacturing of contact lenses
[0024] Contact lenses were manufactured through the following three steps.
[0025] (Step 1) Preparation of cross-linked raw materials
[0026] A cross-linked raw material is manufactured by mixing MPC, 2-HEMA, and SiGMA, or MPC, 2-HEMA, and SiGMA in the amounts described in Table 1 below, and then irradiating the mixture.
[0027] Example (weight%) Ingredients 123456782-HEMA15.8815.881510--73MPC9.129.1254.1170.52SiGMA----0.5191520
[0028] (Step 2) Preparation of a mixture containing a cross-linked raw material A mixture is prepared by mixing a hydrophilic monomer and an additive with the raw material prepared in Step 1 in the amounts described in Table 2 and stirring at 300 to 500 rpm.
[0029] Ingredient Example (weight%) 123456781 Raw material of step 25252014.11.52522.525 Hydrophilic monomer (2-HEMA) 66.266.264.479.993697370 Additive Initiator 1.51.51.51.51.51.51.51.51.5 Crosslinking agent 5.55.55.53.53.53.52.53.0 Other 1.81.88.6-0.50.50.50.5
[0030] (Step 3) Contact lens manufacturing The mixture manufactured in Step 2 is injected into a mold for manufacturing contact lenses and polymerized through heat curing to obtain a contact lens.
[0031] Comparative Examples 1 to 7: Manufacturing of Contact Lenses
[0032] After weighing and mixing each component listed in Table 3 below, the mixture is stirred at 300 to 500 rpm until all the components are dissolved, and the stirred mixture is injected into a mold for manufacturing contact lenses and polymerized through heat curing to obtain a contact lens.
[0033] Comparative Example (Wt%) Ingredients 12345672-HEMA 82.0879.489.993698073SiGMA---0.5191520MPC9.1254.1170.52Additive Initiator 1.51.51.51.511.51.5Crosslinking Agent 5.55.53.53.53.52.53.0Others 1.88.6-0.50.50.50.5
[0034] Comparative Example 8: Manufacturing of Contact Lenses The manufacturing method was the same as in Examples 1 to 8, but a small amount of MPC was used to manufacture contact lenses. The specific manufacturing method is as follows.
[0035] (Step 1) Preparation of cross-linked raw materials
[0036] MPC and 2-HEMA are mixed in the amounts described in Table 4 below and then irradiated to produce raw materials for MPC and 2-HEMA.
[0037] Ingredient comparison example 8 (weight%) 2-HEMA17.00MPC0.8
[0038] (Step 2) Preparation of a mixture containing a cross-linked raw material A hydrophilic monomer and an additive are mixed with the raw material prepared in Step 1 in the amounts described in Table 5, and the mixture is prepared by stirring at 300 to 500 rpm.
[0039] Example 8 of comparative ingredients (weight%) Step 1 raw material 17.8 hydrophilic monomer (2-HEMA) 77.7 additive initiator 1 crosslinking agent 3 other 0.5
[0040] (Step 3) Contact lens manufacturing The mixture manufactured in Step 2 is injected into a mold for manufacturing contact lenses and polymerized through heat curing to obtain a contact lens.
[0041] Experimental Example 1: Evaluation of the physical properties of contact lenses
[0042] The tensile strength and water contact angle of the contact lenses of Examples 1 to 8 and the contact lenses of Comparative Examples 1 to 7 were evaluated, and the results are shown in Tables 6 and 7 below.
[0043] To determine tensile strength, the sample is first removed from its container and placed in a cleaning cube. The sample is equilibrated in a standard saline solution (PBS) at (20±0.5)°C for at least 30 minutes. Next, the sample is mounted on a measuring jig for a compression and tensile testing device (CUTM-10, CAS). The testing device is operated to apply tensile force to the sample at a specified tensile rate until the sample is destroyed. Once the sample is destroyed, the maximum output force is measured to derive the results. The appropriate tensile strength range for contact lenses is 1.0 to 2.0 (N f / ㎠). If the tensile strength is lower than the appropriate range, the lens may tear easily during the production process or may not maintain its shape, which may lead to manufacturing defects. Furthermore, even after the product is manufactured, the lens may tear easily when handled by the consumer. Conversely, if the tensile strength exceeds the above range, the comfort of the wearer may deteriorate.
[0044] The water contact angle was measured by first removing the sample from the container and placing it in a cleaning cube in a standard saline solution (PBS) at (20±0.5)℃ and equilibrating it for at least 30 minutes. After the above pretreatment, remove any moisture from the surface of the sample and confirm that there are no cracks on the exterior of the sample. After the inspection, place the convex side of the sample facing upward on the stage and confirm that there is no empty space between the stage and the sample. Insert the stage into the fixed stage of a contact angle measuring device (Phoenix 10, SIO Co., Ltd.) and allow a certain amount of water droplets to form on the tip of the needle. Then, adjust the height of the stage to bring the sample into contact with the water droplets formed on the tip of the needle. At this time, the contact angle between the sample and the water droplets was measured using a titration method. The appropriate range of the water contact angle for contact lenses is 15 to 50˚. If the water contact angle falls outside the above range, long-term wearing comfort may be reduced.
[0045] Example Item (Unit) 12345678 Tensile strength (N f / ㎠) 1.521.761.181.641.361.321.351.36 Water contact angle (˚ ) 19.8718.2720.4525.6738.530.240.235.6
[0046] Comparative Example Item (Unit) 12345678 Tensile Strength (N f / ㎠) 1.360.71.041.010.880.860.900.68 Water Contact Angle (˚ ) 45.8102.4472.0362.259.261.365.368.45
[0047] As a result of confirming the tensile strength and water contact angle, which are the most important physical properties of the lens, it was confirmed that in the case of contact lenses manufactured using a mixture containing the crosslinking raw material in which MPC was first dispersed (Examples 1 to 8), the values of the tensile strength and water contact angle were within the appropriate range, whereas in the case of contact lenses manufactured using a simple mixture (Comparative Examples 1 to 7), the values of the tensile strength and water contact angle were outside the appropriate range. In addition, even when the crosslinking raw material in which MPC was first dispersed was prepared and the contact lenses manufactured using a mixture containing the same (Comparative Example 8), it was confirmed that the values of the tensile strength and water contact angle were outside the appropriate range even when the MPC content was low. Experimental Example 2: Confirmation of the oxygen permeability of contact lenses
[0048] The oxygen permeability of the contact lens of Example 1, which was shown to have the most appropriate properties as a contact lens through the above Experimental Example 1, was compared with the oxygen permeability of the contact lens of Comparative Example 1, which was manufactured using the same MPC content as Example 1 but a different manufacturing method, and the oxygen permeability of the contact lens of Comparative Example 8, which was manufactured using the same manufacturing method as Example 1 but a different MCP content, and the results are shown in Table 8 below.
[0049] Oxygen permeability is measured by first taking the sample out of the container, placing it in a cleaning cube, storing it in a standard saline solution (PBS) at (20±2)℃ for 24 hours, and then equilibrating it at (30±1.0)℃ for at least 2 hours. Then, before measuring the oxygen permeability of the sample, measure the thickness of the sample (thickness gauge, VL-50-B, Mitutoyo Corporation), and measure the thickness of at least four samples that are substantially different in thickness before proceeding with the test. For the test, fix the sample that has completed inspection so that it is in contact with the cathode of the sensor inside the polarography cell, and press the front of the sample firmly with a nylon mesh so that the sample is placed between the plyography cell and the nylon mesh. Then, the sensor system of the test device (oxygen permeability meter (201-T, Rehder Development Company)) measured the current value of the sample while maintaining the temperature at (30±0.5)℃, and the oxygen permeability value was derived using the thickness value measured before the test. The appropriate range of oxygen permeability of contact lenses is 18 to 25.
[0050] Item Example 1 Comparative Example 1 Comparative Example 8 Oxygen Permeability 22.4 18.8 38.66
[0051] As a result, as can be confirmed in Table 7 above, even if the MPC content is the same as Example 1, if the crosslinking raw material in which MPC is dispersed is not used primarily (Comparative Example 1), or if the amount of MPC is small even if the crosslinking raw material in which MPC is dispersed primarily is used, it was confirmed that the oxygen permeability value was outside the appropriate range.
Claims
1. A first step for manufacturing a raw material in which 1.2-methacryloyl oxyethyl phosphorylcholine is dispersed; A second step of mixing hydrophilic monomers and additives into the above raw materials; and A method for manufacturing a contact lens, comprising a third step of injecting the mixture of the second step into a mold for manufacturing a contact lens and polymerizing it to obtain a contact lens.
2. In paragraph 1, A method for manufacturing a contact lens, characterized in that the raw material in the first step is hydroxyethyl methacrylate and propenoic acid-2-methyl-2-hydroxy-3-[3-[1,3,3,3-tetramethyl-1-[(trimethylsilyl)oxy]-1-disiloxanyl]propoxy]propyl ester, in which 2-methacryloyloxyethylphosphorylcholine is dispersed.
3. In paragraph 1, A method for manufacturing a contact lens, characterized in that the above raw material is dispersed and crosslinked by radiation irradiation.
4. In paragraph 1, A method for manufacturing a contact lens, characterized in that the raw material in the first step comprises 5 to 15 wt% of 2-methacryloyloxyethylphosphorylcholine and 5 to 20 wt% of hydroxyethyl methacrylate.
5. In paragraph 1, A method for manufacturing a contact lens, characterized in that the raw materials in the first step are composed of 1 to 10 wt% of 2-methacryloyloxyethylphosphorylcholine and 0.1 to 20 wt% of propenoic acid-2-methyl-2-hydroxy-3-[3-[1,3,3,3-tetramethyl-1-[(trimethylsilyl)oxy]-1-disiloxanyl]propoxy]propyl ester.
6. In paragraph 1, A method for manufacturing a contact lens, characterized in that the raw materials in the first step are composed of 0.1 to 2.5 wt% of 2-methacryloyloxyethylphosphorylcholine, 2 to 10 wt% of hydroxyethyl methacrylate, and 12.5 to 22.5 wt% of propenoic acid-2-methyl-2-hydroxy-3-[3-[1,3,3,3-tetramethyl-1-[(trimethylsilyl)oxy]-1-disiloxanyl]propoxy]propyl ester.
7. In paragraph 1, A method for manufacturing a contact lens, characterized in that the hydrophilic monomer is at least one selected from the group consisting of 2-hydroxyethyl methacrylate (2-HEMA), N,N-dimethylacrylamide (DMA), N-vinyl pyrrolidone (NVP), N-vinyl-N-methyl acrylamide, ethylene glycol dimethacrylate (EGDMA), methyl methacrylate (MMA), azobis isobutyronitrile (AIBN), and polyethylene glycol monomethacrylate.
8. In paragraph 1, A method for manufacturing a contact lens, characterized in that the contact lens comprises 1 to 25 wt% of a raw material in which 2-methacryloyl oxyethyl phosphorylcholine is dispersed, 65 to 95 wt% of a hydrophilic monomer, and 3 to 15 wt% of an additive.
9. In paragraph 1, A method for manufacturing a contact lens, characterized in that the polymerization in the third step is crosslinked through thermal curing.
Citation Information
Patent Citations
Monomer composition and contact lens
JP2007009060A
Pupil-only photochromic contact lenses displaying desirable optics and comfort
KR1020130054262A
Lens comprising low and high molecular weight polyamides
KR1020150030252A
Dental Treatment Solution
KR1020220106387A
Radiation polymerization method of biocompatible and hydrophilic silicone-containing monomer and hydrophilic monomer
KR102297515B1