By using a lithium supplement agent with the chemical formula Li5a+2bFeaMbO4a+2b, combined with reducing metals and Li5FeO4 and Li2MO2 materials, the coating layer and metal elements doped, the irreversible capacity loss of lithium-ion secondary batteries and the performance of existing lithium supplement materials is solved. The problem of insufficient results enables higher battery capacity and safety performance.
Patent Information
- Application Number
- PCT/CN2024/094691
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-05
- Filing Date
- 2024-05-22
- Publication Date
- 2024-12-12
AI Technical Summary
During the first charging and discharging process of existing lithium-ion secondary batteries, solid electrolyte interface masks are generated on the negative electrode surface of the battery, resulting in irreversible capacity loss of lithium ions, reducing the efficiency and cycle life of Coulomb. In addition, the existing lithium supplementary materials have low capacity and residual alkali value. High and high gas production limit the improvement of battery performance.
Using lithium supplement agent with the chemical formula Li5a+2bFeaMbO4a+2b, the Fe content is controlled by adding reducing metal elements such as nickel, manganese, and iron, and combining with Li5FeO4 and Li2MO2 materials, the cladding layer and metal elements are doped. Improve the capacity, stability and safety performance of lithium supplements.
It improves the capacity, stability and safety performance of lithium supplements, reduces gas production and residual alkali value, enhances electrochemical performance, and extends the cycle life and energy density of the battery.
Smart Images

Figure CN2024094691_12122024_PF_FP_ABST
Abstract
Description
Lithium supplement and preparation method thereof, positive electrode sheet and secondary battery
[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on June 5, 2023, with application number 202310659133.9, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The present application relates to the field of energy technology, and in particular to a lithium supplement and a preparation method thereof, a positive electrode sheet and a secondary battery. Background Art
[0003] During the first charge and discharge process of a battery, such as a lithium-ion secondary battery, a large amount of solid electrolyte interface film (SEI film) will be generated on the surface of the battery's negative electrode, consuming the limited lithium ions and electrolyte in the battery, resulting in irreversible capacity loss, leading to a decrease in the coulombic efficiency of the lithium-ion secondary battery, and directly affecting the cycle life and energy density of the lithium-ion secondary battery. Currently, this part of the irreversible capacity loss can be eliminated by replenishing lithium at the positive electrode, thereby improving the battery's energy density and other electrical properties. However, existing lithium replenishment materials have the problems of low capacity or high residual alkalinity and high gas production, which is not conducive to the promotion and application of lithium replenishment materials and limits the improvement of lithium-ion secondary battery performance.
[0004] Summary of the Invention
[0005] The present application provides a lithium supplement agent and a preparation method thereof, a positive electrode plate and a secondary battery.
[0006] In a first aspect, the present application provides a lithium supplement agent, the lithium supplement agent comprising a core, the core comprising a first material phase, the first material phase being Li 5a+2b Fe a M b O 4a+2b , wherein 0.5≤a<1, 0<b≤0.5, and a+b=1, and M is a reducing metal element.
[0007] In this application, the core of the lithium supplement comprises a chemical formula of Li 5a+2b Fe a M b O 4a+2b The first material phase, due to the addition of reducing metals, the content of O is low, Li 5a+2b Fe a M b O 4a+2b The residual alkalinity value is low, and the gas production during charging is small, which improves the processing performance, safety performance and electrochemical performance of the lithium supplement. In this application, controlling the Fe content to be greater than or equal to the M content can enable the lithium supplement to maintain a high capacity level, ensuring the lithium supplement effect while improving the stability of the lithium supplement.
[0008] In one embodiment, the reducing metal element includes at least one metal element selected from divalent nickel, divalent manganese, divalent iron, and divalent cobalt. Divalent nickel, divalent manganese, divalent iron, and divalent cobalt can reduce Li 5a+2b Fe a M b O 4a+2b The oxygen content makes the lithium supplement agent produce less gas during the charging process, thereby improving the safety and electrochemical performance of the lithium supplement agent.
[0009] In one embodiment, the core further includes a second material phase, and the second material phase is Li 5 FeO 4 . The second material phase can increase the capacity of the lithium supplement agent and achieve a better lithium supplement effect.
[0010] In one embodiment, the second material phase is doped with the first material phase. The second material phase and the first material phase are mixed to facilitate the preparation of the lithium supplement.
[0011] In one embodiment, the second material phase is filled in the gaps between the first material phases, thereby increasing the compaction density of the lithium supplement agent, thereby increasing the capacity of the lithium supplement agent and achieving a better lithium supplement effect.
[0012] In one embodiment, the first material is bonded to the outer surface of the second material phase. 5a+2b Fe a M b O 4a+2b The residual alkali value of the lithium supplement is lower than that of Li5FeO4. The first material phase is coated on the outer surface of the second material phase to reduce the overall residual alkali value of the lithium supplement, thereby improving the processing performance and safety performance of the lithium supplement.
[0013] In one embodiment, the core further includes a third material phase, which is Li2MO2 and is bonded to the outer surface of the first material phase. The third material phase can reduce gas production in the lithium supplement, thereby improving the safety and electrochemical performance of the lithium supplement.
[0014] In one embodiment, the lithium supplement is further doped with a metal element, wherein the metal element includes at least one of aluminum, titanium, zirconium, vanadium, manganese, and cerium. Doping the lithium supplement with metal elements such as aluminum, titanium, zirconium, vanadium, manganese, and cerium can improve the structural stability of the lithium supplement or enhance the conductivity of the material.
[0015] In one embodiment, the surface residual alkali value of the lithium supplement agent is 0%-1.5%.
[0016] In one embodiment, the particle size D50 of the lithium supplement agent is 0.5 μm-38 μm.
[0017] In one embodiment, the specific surface area of the lithium supplement is 0.1 m 2 / g-20m 2 / g.
[0018] In one embodiment, the lithium supplement further includes a coating layer, which is located on the outer surface of the core and includes at least one of an isolation coating layer, an ion conductor coating layer, an electronic conductor coating layer, a single atomic deposition layer, and an oxide nanofilm layer.
[0019] In one embodiment, the isolation coating layer includes at least one of a ceramic substance, a high molecular polymer, and a carbon material.
[0020] In one embodiment, the electronic conductor coating layer comprises at least one of a carbon material, a conductive polymer, or a conductive oxide.
[0021] In one embodiment, the material of the ion conductor coating layer includes at least one of a perovskite-type, a NASICON-type, a garnet-type, or a polymer-type solid electrolyte.
[0022] In one embodiment, the mass ratio of the core to the coating layer is 100:(0.01-15).
[0023] In one embodiment, the coating layer has a thickness of 1 nm to 400 nm.
[0024] In one embodiment, the water absorption rate of the lithium supplement agent is less than 20 ppm / s at 25° C. and 30%-35% relative humidity in air.
[0025] In one embodiment, the water absorption rate of the lithium supplement agent is less than 10 ppm / s at 25° C. and 30%-35% relative humidity in air.
[0026] In one embodiment, the lithium supplement agent has a water absorption rate of less than 10 ppm / s at 25° C. and 20%-25% relative humidity in air.
[0027] In one embodiment, the water absorption rate of the lithium supplement agent is less than 5 ppm / s at 25° C. and 20%-25% relative humidity in air.
[0028] In a second aspect, the present application provides a method for preparing a lithium supplement, the method comprising:
[0029] Adding lithium source, iron source and M source into the complexing agent solution and stirring to obtain gel;
[0030] The gel is sintered in a protective atmosphere to obtain the core of the lithium supplement agent.
[0031] Wherein, the preparation method of the lithium supplement is used to prepare the lithium supplement as described above.
[0032] In one embodiment, the method for preparing the lithium supplement further comprises: mixing the core and the coating material, and sintering them under a protective atmosphere to obtain the lithium supplement.
[0033] In a third aspect, the present application provides a method for preparing a lithium supplement, the method comprising:
[0034] The solutions of the iron source and the M source are mixed with a precipitant solution to precipitate and obtain a precursor;
[0035] After the lithium source and the precursor are mixed, sintering is performed under a protective atmosphere to obtain the core of the lithium supplement agent;
[0036] Wherein, the preparation method of the lithium supplement is used to prepare the lithium supplement as described above.
[0037] In one embodiment, the preparation method of the lithium supplement further comprises: mixing the core and the coating material, and sintering under a protective atmosphere to obtain the lithium supplement.
[0038] In a fourth aspect, the present application provides a positive electrode plate, which includes the lithium supplement agent as described above, or includes the lithium supplement agent prepared by the preparation method of the lithium supplement agent as described above.
[0039] In a fifth aspect, the present application provides a secondary battery, which includes a negative electrode plate, a separator, and the positive electrode plate as described above.
[0040] In one embodiment, the secondary battery is a lithium-ion battery, and in the lithium-ion battery, the first delithiation capacity of the lithium supplement agent is greater than or equal to 550 mAh / g.
[0041] In one embodiment, the ratio of the first-cycle gas production of the lithium supplement agent to the first-cycle gas production of the corresponding Li5FeO4 is less than or equal to 50%. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments of the present application will be described below.
[0043] FIG1 is a schematic structural diagram of a lithium supplement provided by one embodiment of the present application;
[0044] FIG2 is an X-ray diffraction (XRD) diagram of a lithium supplement agent provided in one embodiment of the present application. DETAILED DESCRIPTION
[0045] The technical solutions in the embodiments of the present application will be described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments.
[0046] As used herein, the terms "first," "second," and the like are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of the technical features being referred to. Thus, a feature specified as "first" or "second" may explicitly or implicitly include one or more of the features. Throughout the description of this application, unless otherwise specified, "plurality" means two or more.
[0047] In addition, in this article, directional terms such as "upper" and "lower" are defined relative to the orientation of the structure schematically placed in the accompanying drawings. It should be understood that these directional terms are relative concepts. They are used for relative description and clarification, and they can change accordingly according to changes in the orientation of the structure.
[0048] For ease of understanding, the English abbreviations and related technical terms involved in the embodiments of this application are explained and described below.
[0049] Relative humidity: refers to the percentage of water vapor pressure in the air to the saturated water vapor pressure at the same temperature.
[0050] ppm: parts per million, which means one part per million. For gases, ppm refers to the mole fraction or volume fraction; for solutions, ppm refers to the mass concentration.
[0051] During the first charge and discharge process of a battery, such as a lithium-ion secondary battery, a large amount of solid electrolyte interface film (SEI film) will be produced on the surface of the negative electrode of the battery, which consumes the limited lithium ions and electrolyte in the battery, greatly reducing the capacity of lithium ions and causing irreversible capacity loss. During the first discharge, the lithium ions deintercalated from the negative electrode are much smaller than the lithium ions deintercalated from the positive electrode during charging, resulting in a decrease in the coulombic efficiency of the lithium-ion secondary battery, which directly affects the cycle life and energy density of the lithium-ion secondary battery. To address this problem, the loss of this part of the irreversible capacity can usually be eliminated by replenishing lithium at the positive electrode, thereby improving the battery energy density and other electrical properties. However, existing lithium replenishment materials have the problems of low capacity, high residual alkalinity value and high gas production, which are not conducive to the promotion and application of lithium replenishment materials and limit the improvement of the performance of lithium-ion secondary batteries.
[0052] Please refer to FIG1 . The present application provides a lithium supplement agent 1 . The lithium supplement agent 1 includes a core 10 . The core 10 includes a first material phase. The first material phase is Li 5a+2b Fe a M b O 4a+2b, wherein 0.5≤a<1, 0<b≤0.5, and a+b=1, and M is a reducing metal element.
[0053] Here, Li represents lithium, Fe represents iron, and O represents oxygen. The reducing metal is a metal with reducing properties that easily combines with oxygen and can inhibit the generation of oxygen by the lithium supplement material.
[0054] Lithium replenisher 1 is applied to the battery's positive electrode to pre-lithiate the positive electrode, adding lithium to the battery's interior to replenish lithium ions before operation. In one embodiment, lithium replenisher 1 can be applied by coating the outer surface of the battery's positive electrode tab or by embedding the lithium replenisher 1 into the outer surface of the battery's positive electrode tab. In other embodiments, lithium replenisher 1 can be added during the preparation of the battery's positive electrode tab, dispersing the lithium replenisher 1 onto the outer surface and interior of the tab.
[0055] The lithium supplement 1 includes a core 10, which has a high lithium content. During the first charge process, the lithium (Li) in the core 10 can be released and migrated to the negative electrode of the battery, offsetting the irreversible lithium loss caused by the formation of the SEI film, thereby improving the total capacity and energy density of the battery.
[0056] The lithium supplement agent 1 provided in the present application has a high lithium supplement capacity, produces little gas during charging, and has high safety performance.
[0057] In the prior art, lithium ferrite, lithium nickelate, or lithium manganate is typically used as the lithium replenisher 1. When lithium ferrite (Li5FeO4) is used as the lithium replenisher 1, the capacity of lithium ferrite is high, but lithium ferrite produces a large amount of gas during charging, which increases battery impedance and reduces battery safety and electrochemical performance. In addition, lithium ferrite has a high residual alkalinity value, which easily causes gelation of the slurry during the slurry mixing process, resulting in poor slurry fluidity, which seriously affects the processing performance of the lithium replenisher 1. When lithium nickelate (such as Li2NiO2) or lithium manganate (such as Li2MnO2) is used as the lithium replenisher 1, although the gas production of lithium nickelate / lithium manganate during charging is small and the residual alkalinity value is low, the capacity of lithium nickelate / lithium manganate is low, and the lithium replenishment effect is poor, which limits the improvement of battery performance.
[0058] In this application, the chemical formula of the first material phase in the lithium supplement 1 is Li 5a+2b Fe a M b O 4a+2b , Li 5a+2b Fe a M b O 4a+2b It can maintain a high capacity level, and due to the addition of reducing metal elements, the activity of combining with water is reduced, Li 5a+2b Fe a M b O4a+2b The residual alkalinity value is low, and the gas generation during charging is small, which improves the processing performance, safety performance and electrochemical performance of the lithium supplement agent 1. In this application, controlling the Fe content to be greater than or equal to the M content can ensure the lithium supplement effect of the lithium supplement agent 1 while improving the stability of the lithium supplement agent 1.
[0059] In one embodiment, the value range of a is 0.5≤a≤0.8. Within this range, the lithium supplement agent 1 has a lower residual alkalinity value and less gas production, and has better processing performance, safety performance, and electrochemical performance. The lithium supplement agent 1 not only has a good lithium supplement effect, but also has good stability.
[0060] In one embodiment, the reducing metal element includes at least one metal element selected from divalent nickel, divalent manganese, divalent iron, and divalent cobalt. For example, when M is selected from Ni, the chemical formula of the core 10 is Li 5a+2b Fe a Ni b O 4a+2b When M is selected from Mn, the chemical formula of the core 10 is Li 5a+2b Fe a Mn b O 4a+2b When M is selected from Ni and Mn, the chemical formula of the core 10 is Li 5a+2b Fe a Ni b1 Mn b2 O 4a+2b , where b1+b2=b.
[0061] Divalent nickel, divalent manganese, divalent iron and divalent cobalt can reduce the 5a+2b Fe a M b O 4a+2b The amount of gas produced during the charging process improves the safety and electrochemical performance of the lithium supplement 1.
[0062] In one embodiment, the core 10 further includes a second material phase, which is Li 5 FeO 4 . The second material phase can increase the capacity of the lithium supplement agent 1 and achieve a better lithium supplement effect.
[0063] In one embodiment, the second material phase is doped with the first material phase. The second material phase and the first material phase are mixed to facilitate the preparation of the lithium supplement agent 1.
[0064] In one embodiment, the second material phase is filled in the gaps between the first material phases, thereby increasing the compaction density of the lithium supplement agent 1 , thereby increasing the capacity of the lithium supplement agent 1 and achieving a better lithium supplement effect.
[0065] In one embodiment, the first material is bonded to the outer surface of the second material phase. 5a+2b Fe a M b O 4a+2b The residual alkali value of the lithium supplement 1 is lower than that of Li5FeO4. The first material phase is coated on the outer surface of the second material phase to reduce the overall residual alkali value of the lithium supplement 1, thereby improving the processing performance and safety performance of the lithium supplement 1.
[0066] In one embodiment, the core 10 further includes a third material phase, which is Li2MO2, bonded to the outer surface of the first material phase. The third material phase can reduce gas production in the lithium supplement 1 and improve its safety and electrochemical performance.
[0067] In one embodiment, the lithium supplement agent 1 is further doped with a metal element, wherein the metal element includes at least one of aluminum, titanium, zirconium, vanadium, manganese, and cerium. Doping the lithium supplement agent 1 with a metal element such as aluminum, titanium, zirconium, vanadium, manganese, and cerium can improve the structural stability of the lithium supplement agent 1.
[0068] In one embodiment, the surface residual alkali value of the lithium supplement 1 is 0%-1.5%. The surface residual alkali value of the lithium supplement 1 affects its processing performance and stability. It is understood that the higher the surface residual alkali value of the lithium supplement 1, the stronger the alkalinity of the lithium supplement 1, the poorer the stability of the lithium supplement 1, and the lithium supplement 1 is more likely to react with air and electrolyte, directly affecting the electrochemical performance of the lithium supplement 1 and reducing battery safety. In addition, a high surface residual alkali value of the lithium supplement 1 can easily cause gelation of the lithium supplement 1 during slurry preparation, resulting in poor slurry fluidity, which seriously affects the processing performance of the lithium supplement 1.
[0069] The surface residual alkali value of the lithium supplement agent 1 provided in the present application is within the range of 0%-1.5%. The surface residual alkali value of the lithium supplement agent 1 is low, which improves the stability and processing performance of the lithium supplement agent 1, so that the lithium supplement agent 1 can achieve the function of efficient lithium supplementation.
[0070] In one embodiment, the surface residual alkali value of the lithium supplement agent 1 is 0%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4% or 1.5%.
[0071] In one embodiment, the residual alkali value on the surface of the lithium supplement agent 1 is 0%-1%. Within this range, the performance of the lithium supplement agent 1 is more excellent. More preferably, the residual alkali value on the surface of the lithium supplement agent 1 is 0%-0.5%.
[0072] In one embodiment, the particle size D50 of the lithium supplement 1 is 0.5 μm-38 μm. The particle size D50 refers to the particle size corresponding to when the cumulative particle size distribution percentage of the lithium supplement 1 reaches 50%.
[0073] It is understandable that if the particle size of the lithium supplement agent 1 is too small, the lithium supplement agent 1 is likely to agglomerate, making it difficult for the lithium inside the lithium supplement agent 1 to escape when replenishing active lithium to the negative electrode, thereby reducing the lithium replenishment effect of the lithium supplement agent 1; and if the particle size of the lithium supplement agent 1 is too large, it is not conducive to the electronic and ionic conduction of the lithium supplement agent 1, and is not conducive to the preparation of the slurry of the lithium supplement agent 1. When the lithium supplement agent 1 is coated on the positive electrode of the battery, the large particle size easily scratches the aluminum foil, which is not conducive to the preparation of the positive electrode sheet with the lithium supplement agent 1.
[0074] In this embodiment, the particle size D50 of the lithium supplement 1 is controlled between 0.5 μm and 38 μm, which ensures the rapid release of lithium ions while improving the dispersibility of the lithium supplement 1, facilitating the use of the lithium supplement 1 and protecting the electrode.
[0075] In one embodiment, the particle size D50 of the lithium supplement agent 1 can be 0.5 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm, 21 μm, 22 μm, 23 μm, 24 μm, 25 μm, 26 μm, 27 μm, 28 μm, 29 μm, 30 μm, 31 μm, 32 μm, 33 μm, 34 μm, 35 μm, 36 μm, 37 μm or 38 μm.
[0076] In one embodiment, the particle size D50 of the lithium supplement agent 1 is 3 μm-15 μm. Within this range, the performance of the lithium supplement agent 1 is even better.
[0077] In one embodiment, the specific surface area of the lithium supplement 1 is 0.1 m 2 / g-20m 2 / g. In one embodiment, the specific surface area is measured using the BET (Brunauer-Emmett-Teller) specific surface area method, and the specific surface area is the BET specific surface area. It is understood that if the specific surface area of the lithium supplement agent 1 is too small, it will not be conducive to improving the conductivity and lithium ion extraction and insertion capacity of the lithium supplement agent 1. If the specific surface area of the lithium supplement agent 1 is too large, the density of the lithium supplement agent 1 is generally low, and the volumetric energy density is low.
[0078] In this embodiment, the specific surface area of the lithium supplement agent 1 is controlled to be 0.1 m 2 / g-20m 2 / g, not only can the conductivity and lithium ion extraction and insertion capabilities of the lithium supplement agent 1 be improved, but also the volume energy density of the lithium supplement agent 1 can be improved.
[0079] In one embodiment, the specific surface area of the lithium supplement agent 1 can be 0.1 m 2 / g, 0.5m 2 / g、1m 2 / g, 2m 2 / g、3m 2 / g、4m 2 / g、5m 2 / g、6m 2 / g、7m 2 / g、8m 2 / g、9m 2 / g、10m 2 / g、11m 2 / g、12m 2 / g、13m 2 / g、14m 2 / g、15m 2 / g、16m 2 / g、17m 2 / g、18m 2 / g、19m 2 / g or 20m 2 / g.
[0080] In one embodiment, the lithium supplement 1 further includes a coating layer 20, which is located on the outer surface of the core 10. The coating layer 20 may fully or partially cover the outer surface of the core 10. The coating layer 20 can protect the core 10. It is understood that if the coating layer 20 is not applied and only the core 10 is used as the lithium supplement 1, on the one hand, the outer surface of the core 10 has residual alkali, which reduces the stability of the lithium supplement 1. Moreover, when the lithium supplement 1 is applied to the positive electrode of the battery, the lithium supplement 1 is more likely to cause gelation of the slurry during the slurry mixing process, resulting in poor slurry fluidity, affecting the processing performance of the lithium supplement 1. On the other hand, the surface of the lithium supplement 1 usually contains a large amount of free lithium. A high free lithium content will deteriorate the high-temperature storage performance of the battery, leading to problems such as flatulence and performance degradation during battery storage.
[0081] In this application, on the one hand, the chemical formula of the core 10 is configured as Li 5a+2b Fe a M b O 4a+2bWhile reducing the residual alkalinity value on the outer surface of the core 10, the coating layer 20 is provided on the outer surface of the core 10 to further reduce the residual alkalinity value of the lithium supplement 1, thereby improving the stability and processing performance of the lithium supplement 1. Furthermore, the coating layer 20 reduces the free lithium content on the outer surface of the lithium supplement 1, facilitating storage of the lithium supplement 1.
[0082] In one embodiment, the coating layer 20 includes at least one of an isolation coating layer 21 , an ion conductor coating layer 22 , an electronic conductor coating layer 23 , a single-atom deposition layer, and an oxide nanofilm layer.
[0083] In one embodiment, the coating 20 is an isolation coating 21. The isolation coating 21 can isolate the core 10 from moisture and carbon dioxide. The isolation coating 21 can protect the core 10 and improve its stability, thereby ensuring the lithium replenishment function of the core 10. It also ensures the stability and uniformity of the lithium replenishment agent 1 in the electrode active slurry and active layer, as well as good processing performance. The isolation coating 21 can be located on a portion of the outer surface of the core 10 or can cover the entire outer surface of the core 10, and this is not limited in this application.
[0084] In one embodiment, the isolation coating layer 21 comprises at least one of a ceramic, a polymer, and a carbon material. The ceramic comprises at least one of alumina, silica, boehmite, silicon nitride, silicon carbide, and boron nitride. The polymer comprises one or more of polyvinylidene fluoride, sodium alginate, sodium carboxymethyl cellulose, polyacrylic acid, polyacrylic acid salt, polyacrylonitrile, polyamide, polyimide, polyvinyl pyrrolidone, polyethylene oxide (PEO), polypyrrole (PPy), polytetrafluoroethylene (PTFE), and polyurethane (PU). The carbon material comprises at least one of graphene, carbon nanotubes, carbon nanospheres, carbon nanofibers, graphite, and carbon black.
[0085] In one embodiment, the coating 20 is an ion conductor coating 22. The ion conductor coating 22 enhances the ionic conductivity of the lithium supplement 1. The ion conductor coating 22 facilitates the outward transport of lithium ions from the lithium supplement 1; it also assists in enhancing ion transport within the electrode. The ion conductor coating 22 can have a dense or loose structure and can fully or partially coat the outer surface of the core 10.
[0086] In one embodiment, the material of the ion conductor coating layer 22 includes at least one of a perovskite type, a NASICON type, a garnet type or a polymer type solid electrolyte. 3x La 2 / 3-x TiO3(LLTO), specifically Li 0.5 La 0.5TiO3、Li 0.33 La 0.57 TiO3、Li 0.29 La 0.57 TiO3、Li 0.33 Ba 0.25 La 0.39 TiO3、(Li 0.33 La 0.56 ) 1.005 Ti 0.99 Al 0.01 O3、Li 0.5 La 0.5 Ti 0.95 Zr 0.05 At least one of O3, etc. NASICON type such as but not limited to Li 1.4 Al 0.4 Ti 1.6 (PO4)3(LATP). Garnet type includes Li7La3Zr2O 12 (LLZO), Li 6.4 La3Zr 1.4 Ta 0.6 O 12 , Li 6.5 La3Zr 1.5 Ta 0.5 O 12 At least one of the polymer solid electrolytes includes at least one of PEO / PPO / PVDF etc. which dissolves lithium salt.
[0087] In one embodiment, the coating 20 is an electronic conductor coating 23. The electronic conductor coating 23 can enhance the electronic conductivity of the lithium supplement 1. The electronic conductor coating 23 helps reduce the internal impedance of the electrode and also serves as a conductive agent within the electrode. The electronic conductor coating 23 can have a dense or loose structure and can fully or partially coat the outer surface of the core 10.
[0088] In one embodiment, the electronic conductor coating layer 23 comprises at least one of a carbon material, a conductive polymer, or a conductive oxide. The carbon material includes at least one of graphene, carbon nanotubes, carbon nanospheres, carbon nanofibers, graphite, and carbon black. The conductive polymer may be, but is not limited to, the conductive polymer contained in the isolation coating layer 21. The conductive oxide includes at least one of In2O3, ZnO, and SnO2.
[0089] In one embodiment, the coating layer 20 is a deposition layer, and the deposition layer includes a single atomic deposition layer and / or an oxide nanofilm layer obtained by atomic layer deposition technology. Specifically, the deposition layer can be a single atomic deposition layer obtained by atomic layer deposition technology, and the level can be a single atomic layer or nanolayer composed of atoms or molecules. Optionally, when the deposition layer is a single atomic deposition layer, different atomic deposition agents can be selected according to the different materials thereof, including but not limited to one or more of trimethylaluminum, triethylaluminum, triisobutylaluminum, tetrakis(diethylamino)titanium, triethylsilane, tetraethylsilane, and tetrakis(ethylmethylamino)zirconium.
[0090] Alternatively, the deposited layer may be an oxide nanofilm. For example, the oxide nanofilm may be formed by reacting the aforementioned monoatomic deposition layer with oxygen, and may be made of aluminum oxide, titanium dioxide, silicon dioxide, zirconium dioxide, or the like. Alternatively, a nanoscale oxide layer may be formed directly on the outer layer of the core 10 using vapor deposition technology. Of course, the oxide nanofilm may also be formed using other techniques.
[0091] In one embodiment, the coating layer 20 includes at least two of an isolation coating layer 21, an ion conductor coating layer 22, and an electron conductor coating layer 23. For example, in one embodiment, the coating layer 20 includes the isolation coating layer 21 and the ion conductor coating layer 22, and the ion conductor coating layer 22 is coated on the outer surface of the core 10, and the isolation coating layer 21 is coated on the outer surface of the ion conductor coating layer 22.
[0092] In one embodiment, the coating layer 20 includes an isolation coating layer 21 and an electronic conductor coating layer 23 , wherein the isolation coating layer 21 coats the outer surface of the core 10 , and the electronic conductor coating layer 23 coats the outer surface of the isolation coating layer 21 .
[0093] In one embodiment, the coating layer 20 includes an isolation coating layer 21, an ion conductor coating layer 22, and an electronic conductor coating layer 23 (as shown in Figure 1), and the ion conductor coating layer 22 is coated on the outer surface of the core 10, the isolation coating layer 21 is coated on the outer surface of the ion conductor coating layer 22, and the electronic conductor coating layer 23 is coated on the outer surface of the isolation coating layer 21.
[0094] In one embodiment, when the coating layer 20 includes two or more coating layers 20 , the coating order between the coating layers 20 can be set as needed and is not limited to the types listed above.
[0095] In one embodiment, the mass ratio of the core 10 to the coating 20 is 100:(0.01-15). The mass ratio of the core 10 to the coating 20 affects the performance of the lithium supplement 1. If the coating 20 content is too low, the coating 20 will have a weak effect, making it difficult for the coating 20 to isolate the core 10 from the external environment, and thus failing to effectively protect the core 10 and improve the electronic or ionic conductivity of the lithium supplement 1. If the coating 20 content is too high, the proportion of the lithium supplement 1 in the positive electrode material will be reduced, thereby reducing the amount of lithium supplemented. In addition, it will increase the processing difficulty of the lithium supplement 1.
[0096] In this embodiment, the mass ratio of the core 10 to the coating layer 20 is controlled within the range of 100:(0.01-15). This optimal coating layer 20 mass ratio not only improves the processing properties of the lithium supplement 1 and enhances the bonding strength between the coating layer 20 and the core 10, but also prevents the coating layer 20 from excessively increasing the mass of the lithium supplement 1, thereby preventing the coating layer 20 from excessively increasing the mass of the lithium supplement 1 and affecting the energy density and capacity of the lithium supplement 1. Furthermore, the coating layer 20 can better isolate the core 10 from the external environment, thereby protecting the core 10 and improving the electronic or ionic conductivity of the lithium supplement 1.
[0097] In one embodiment, the mass ratio of the core 10 to the coating layer 20 is 100:0.01, 100:0.05, 100:0.1, 100:0.5, 100:1, 100:2, 100:3, 100:4, 100:5, 100:6, 100:7, 100:8, 100:9, 100:10, 100:11, 100:12, 100:13, 100:14 or 100:15.
[0098] In one embodiment, the mass ratio of the core 10 to the coating layer 20 is 100:(0.01-10). Within this range, the performance of the lithium supplement 1 is more excellent. More preferably, the mass ratio of the core 10 to the coating layer 20 is 100:(0.01-5).
[0099] In one embodiment, the coating layer 20 has a thickness of 1 nm to 400 nm. The thickness of the coating layer 20 affects the performance of the lithium supplement 1. If the coating layer 20 is too thin, it is difficult for the coating layer 20 to isolate the core 10 from the external environment, and it cannot effectively protect the core 10 and improve the electronic conductivity or ionic conductivity of the lithium supplement 1. If the coating layer 20 is too thick, it will reduce the proportion of the lithium supplement 1 in the positive electrode material, thereby reducing the amount of lithium supplementation. In addition, it will increase the interfacial resistance of the core 10 and increase the processing difficulty of the lithium supplement 1.
[0100] In this embodiment, the thickness of the coating layer 20 is controlled within the range of 1 nm to 400 nm. A suitable coating layer 20 thickness, on the one hand, improves the processing properties of the lithium supplement 1 and enhances the bonding strength between the coating layer 20 and the core 10. On the other hand, the coating layer 20 does not excessively increase the mass of the lithium supplement 1, thus preventing excessive mass of the coating layer 20 from affecting the energy density and capacity of the lithium supplement 1. Furthermore, the coating layer 20 can better isolate the core 10 from the external environment, thereby protecting the core 10 and improving the electronic or ionic conductivity of the lithium supplement 1.
[0101] In one embodiment, the coating layer 20 has a thickness of 1 nm, 5 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, or 400 nm.
[0102] In one embodiment, the water absorption rate of the lithium supplement 1 is less than 20 ppm / s in air at 25°C and 30%-35% relative humidity. The water absorption rate of the lithium supplement 1 affects the processing performance and stability of the lithium supplement 1. Generally, the greater the water absorption rate of the lithium supplement 1, the faster the lithium supplement 1 absorbs water vapor in the air. The lithium supplement 1 easily reacts with ambient moisture and forms a large amount of residual alkali on the surface, making the lithium supplement 1 alkaline. When the residual alkali content is too high, the stability of the lithium supplement 1 is poor and it is easy to react with air and electrolyte, directly affecting the electrochemical performance of the lithium supplement 1 and reducing battery safety. During the slurry mixing process, the slurry is easily gelled, and the slurry has poor fluidity, which seriously affects the processing performance of the lithium supplement 1.
[0103] In this embodiment, the water absorption rate of the lithium supplement agent 1 is less than 20 ppm / s in air at 25°C and 30%-35% relative humidity. The water absorption rate of the lithium supplement agent 1 is controlled to be low, ensuring that the lithium supplement agent 1 does not quickly absorb moisture in the air. This is beneficial to ensure that the lithium supplement agent 1 is effectively isolated from water vapor, protect the stability of the core 10, and ensure that the gram capacity of the lithium supplement agent 1 is fully utilized, thereby achieving efficient lithium supplementation.
[0104] In one embodiment, the water absorption rate of the lithium supplement agent 1 in air at 25° C. and 30%-35% relative humidity is 20 ppm / s, 19 ppm / s, 18 ppm / s, 17 ppm / s, 16 ppm / s, 15 ppm / s, 14 ppm / s, 13 ppm / s, 12 ppm / s, 11 ppm / s, 10 ppm / s, 9 ppm / s, 8 ppm / s, 7 ppm / s, 6 ppm / s, 5 ppm / s, 4 ppm / s, 3 ppm / s, 2 ppm / s, or 1 ppm / s.
[0105] In one embodiment, the water absorption rate of the lithium supplement agent 1 is less than 10 ppm / s in air at 25° C. and 30%-35% relative humidity. Under this condition, the performance of the lithium supplement agent 1 is even better.
[0106] In one embodiment, the lithium supplement agent has a water absorption rate of less than 10 ppm / s at 25°C and 20%-25% relative humidity. The water absorption rate of the lithium supplement agent 1 affects the processing performance and stability of the lithium supplement agent 1. In this embodiment, controlling the water absorption rate of the lithium supplement agent 1 to a low level ensures that the lithium supplement agent 1 does not rapidly absorb moisture from the air. This effectively isolates the lithium supplement agent 1 from water vapor, protects the stability of the core 10, and ensures the full gram capacity of the lithium supplement agent 1, thereby achieving efficient lithium supplementation.
[0107] In one embodiment, the water absorption rate of the lithium supplement agent 1 in air at 25° C. and 20%-25% relative humidity is 10 ppm / s, 9 ppm / s, 8 ppm / s, 7 ppm / s, 6 ppm / s, 5 ppm / s, 4 ppm / s, 3 ppm / s, 2 ppm / s or 1 ppm / s.
[0108] In one embodiment, the water absorption rate of the lithium supplement agent is less than 5 ppm / s at 25° C. and 20%-25% relative humidity. Under this condition, the performance of the lithium supplement agent 1 is even better.
[0109] In one embodiment, the water absorption test method is as follows:
[0110] First, control the room humidity at 25°C, 20-25% or 30-35% relative humidity.
[0111] Second, take out 0.3-0.5g of sample from the glove box, one sample at a time, and take out another sample from the glove box after the test.
[0112] Third, place the weighing bottle in an analytical balance with a precision of 1 / 100,000, close the hatch, and reset to zero.
[0113] Fourth, weigh 0.17-0.19 g of the sample to be tested into the container. Use a spoon to spread the material. Close the hatch. After stabilizing for 3-5 seconds, start the timer and record the mass on the analytical balance as the value at 0 min. Next, record the values at 5 min, 10 min, 15 min, and 20 min, and calculate the average absorption data for 10-20 minutes.
[0114] Calculation formula:
[0115] Unit: ppm / s. Where t1 and t2 represent time, w0 represents initial mass, w t1 represents the mass at t1, w t2 represents the mass at t2.
[0116] The present application provides a method for preparing a lithium supplement 1. The method for preparing the lithium supplement 1 is used to prepare the lithium supplement 1 described above. The method for preparing the lithium supplement 1 includes steps S1-1 and S2-1. The specific steps are as follows:
[0117] Step S1-1, adding a lithium source, an iron source, and a M source to a complexing agent solution, and stirring to obtain a gel;
[0118] Step S2-1: sintering the gel in a protective atmosphere to obtain the core 10 of the lithium supplement 1.
[0119] In one embodiment, the preparation method of the lithium supplement agent 1 further includes step S3 - 1 : mixing the core 10 and the coating material, and sintering them under a protective atmosphere to obtain the lithium supplement agent 1 .
[0120] Wherein, the M source is a nickel source and / or a manganese source. In step S1-1, a lithium source, an iron source and an M source are added to a complexing agent solution to prepare a gel. The lithium source, the iron source and the M source in the gel are evenly mixed and well dispersed, which facilitates the formation of an ordered structure during subsequent sintering. In one embodiment, in step S1-1, the mixed solution of the lithium source, the iron source, the M source and the complexing agent can be stirred under low-temperature heating conditions to facilitate the dissolution of the lithium source, the iron source and the M source, and at least a portion of the solution is evaporated to facilitate the formation of a gel. Exemplarily, the heating temperature can be 60°C-90°C.
[0121] In step S2-1, the gel is sintered under a protective atmosphere to prevent the M source from being oxidized. In one embodiment, a protective gas is introduced in step S2-1 to control the oxygen content to be below 50 ppm. The lithium source, the iron source, and the M source react at high temperature to generate a chemical formula of Li 5a+2b Fe a M b O 4a+2b of kernel 10.
[0122] In step S3-1, the coating material is a material capable of forming an isolation coating layer 21, an ion conductor coating layer 22, and an electronic conductor coating layer 23. Sintering the core 10 and the coating material under a protective atmosphere prevents oxidation of the M element. In one embodiment, a protective gas is introduced in step S3-1 to control the oxygen content to below 50 ppm.
[0123] In one embodiment, when the coating material is carbon, a carbon layer is formed on the outer surface of the core 10. The method of forming the carbon layer includes the following steps: dispersing the core 10 in a carbon source, and forming a carbon layer on the surface of the core 10 after carbonization.
[0124] It is worth noting that when the lithium supplement 1 does not require the coating layer 20 , step S3 - 1 can be omitted.
[0125] In one embodiment, after obtaining the gel in step S1-1, the gel is dried. During the drying process, the iron compound precipitates first, forming seed crystals that grow into the core 10. After drying to a certain degree, the iron and M compounds precipitate together to form a coating layer. After drying, the precursor is calcined at 300-700°C to obtain a precursor, in which the first material in the precursor is bonded to the outer surface of the second material phase. In one embodiment, the preparation method of the lithium supplement 1 also includes the step of doping with a metal element, as follows: the obtained precursor is crushed and placed in anhydrous ethanol. The surface doping element compound is added while stirring, and the precursor is dried while stirring. After drying, the precursor is calcined at 800°C to obtain the core 10 coated with the doping element.
[0126] The lithium supplement agent 1 prepared in this application contains multiple heterogeneous elements, is high in purity, has a low surface residual alkalinity value, and has a high lithium supplement capacity. Furthermore, the lithium supplement agent 1 has a more stable structure, effectively reducing the release of oxygen species and thus reducing gas generation. Furthermore, the coating layer on the surface of the lithium supplement agent 1 effectively isolates moisture, oxygen, and other substances from contact with the core 10, improving the structural stability of the lithium supplement agent 1 and achieving a stable lithium supplement effect. It also improves the electronic and ionic conductivity of the lithium supplement agent 1, increasing the rate of lithium ion release during charging. The lithium supplement agent 1 provided in this application has even superior performance.
[0127] In one embodiment, the sintering temperature of the gel is 400° C.-1000° C., and the sintering time is 3 h-20 h.
[0128] In one embodiment, the core 10 and the coating material are sintered at a temperature of 500° C. to 800° C. for a time of 1 hour to 10 hours.
[0129] In one embodiment, the lithium source is one or more of lithium oxide, lithium hydroxide, lithium acetate, lithium carbonate, lithium fluoride, and lithium chloride.
[0130] In one embodiment, the iron source is one or more of ferric acetate, ferric nitrate, ferric sulfate, ferric hydroxide, ferric chloride, and ferric oxide.
[0131] In one embodiment, the manganese source is one or more of manganese acetate, manganese nitrate, manganese monoxide, manganese sulfate, manganese hydroxide, and manganese dichloride.
[0132] In one embodiment, the nickel source is one or more of nickel acetate, nickel nitrate, nickel oxide, nickel sulfate, nickel hydroxide, and nickel chloride.
[0133] In one embodiment, the complexing agent is at least one of citric acid, ammonium citrate, maleic acid, oxalic acid, ammonium oxalate, ascorbic acid, polyethylene glycol, polyvinyl pyrrolidone, glycerol, isopropanolamine, hydrogen peroxide, and the like.
[0134] In one embodiment, the complexing agent solution is a solution formed by dissolving the complexing agent in a solvent, wherein the solvent is one or more of methanol, glycerol, ethanol and water.
[0135] In one embodiment, the protective atmosphere is one or more of nitrogen, helium, argon, and neon.
[0136] The present application provides a method for preparing a lithium supplement 1. The method for preparing the lithium supplement 1 is used to prepare the lithium supplement 1 described above. The method for preparing the lithium supplement 1 includes steps S1-2 and S2-2. The specific steps are as follows:
[0137] Step S1-2, mixing the solution of the iron source and the M source with a precipitant solution, and precipitating to obtain a precursor;
[0138] Step S2-2, after the lithium source and the precursor are mixed, sintering is performed under a protective atmosphere to obtain the core 10 of the lithium supplement agent 1;
[0139] In one embodiment, the preparation method of the lithium supplement agent 1 further includes step S3-2: mixing the core 10 and the coating material, and sintering them under a protective atmosphere to obtain the lithium supplement agent 1.
[0140] Wherein, M source is nickel source and / or manganese source. The solution of iron source and M source refers to the solution containing iron source and M source simultaneously. In step S1-2, the solution of iron source and M source is mixed with precipitant solution, refers to that the solution of iron source and M source is added to precipitant solution to carry out precipitation reaction, or the precipitant solution is added to the solution of iron source and M source to carry out precipitation reaction. After the precipitation reaction, filtering obtains a solid precursor in which the iron source and M source are uniformly mixed. At this time, the precursor is an iron-based lithium supplement material precursor containing M.
[0141] In step S2-2, the lithium source and the precursor are mixed and sintered, and the lithium source reacts with iron and M to generate a chemical formula of Li 5a+2b Fe a M b O 4a+2b The core 10 is sintered under a protective atmosphere to prevent oxidation of the M source. In one embodiment, a protective gas is introduced in step S2-2 to control the oxygen content to below 50 ppm.
[0142] In step S3-2, the coating material is a material capable of forming an isolation coating layer 21, an ion conductor coating layer 22, and an electronic conductor coating layer 23. Sintering the core 10 and the coating material under a protective atmosphere prevents oxidation of the M element. In one embodiment, a protective gas is introduced in step S3-2 to control the oxygen content to below 50 ppm.
[0143] The lithium supplement agent 1 prepared in this application contains multiple heterogeneous elements, is high in purity, has a low surface residual alkalinity value, and has a high lithium supplement capacity. Furthermore, the lithium supplement agent 1 has a more stable structure, effectively reducing the release of oxygen species and thus reducing gas generation. Furthermore, the coating layer on the surface of the lithium supplement agent 1 effectively isolates moisture, oxygen, and other substances from contact with the core 10, improving the structural stability of the lithium supplement agent 1 and achieving a stable lithium supplement effect. It also improves the electronic and ionic conductivity of the lithium supplement agent 1, increasing the rate of lithium ion release during charging. The lithium supplement agent 1 provided in this application has even superior performance.
[0144] In one embodiment, the sintering temperature of the lithium source and the precursor is 600° C.-1000° C., and the sintering time is 1 hour-24 hours.
[0145] In one embodiment, the core 10 and the coating material are sintered at a temperature of 500° C. to 800° C. for a time of 1 hour to 10 hours.
[0146] In one embodiment, the lithium source is one or more of lithium oxide, lithium hydroxide, lithium acetate, lithium carbonate, lithium fluoride, and lithium chloride. The iron source is one or more of ferric acetate, ferric nitrate, ferric sulfate, ferric hydroxide, ferric chloride, and ferric oxide. The manganese source is one or more of manganese acetate, manganese nitrate, manganese monoxide, manganese sulfate, manganese hydroxide, and manganese dichloride. The nickel source is one or more of nickel acetate, nickel nitrate, nickel oxide, nickel sulfate, nickel hydroxide, and nickel chloride.
[0147] In one embodiment, the precipitant is at least one of aqueous ammonia, sodium hydroxide, potassium hydroxide, magnesium hydroxide, lithium hydroxide, and calcium hydroxide.
[0148] The present application provides a positive electrode plate, which includes the lithium supplement agent 1 as described above, or includes the lithium supplement agent 1 prepared by the preparation method of the lithium supplement agent 1 as described above.
[0149] The present application provides a secondary battery, which includes a negative electrode plate, a separator, and the positive electrode plate as described above.
[0150] In one embodiment, the secondary battery is a lithium-ion battery, and the initial lithium decomposition capacity of the lithium supplement agent 1 is greater than or equal to 550 mAh / g. The initial lithium decomposition capacity of the lithium supplement agent 1 is high, which can achieve a good lithium supplement effect.
[0151] In one embodiment, the ratio of the first-cycle gas production to the corresponding Li5FeO4 is less than or equal to 50%. Compared with Li5FeO4, the first-cycle gas production of the lithium supplement 1 provided in this application is lower, thereby improving battery safety and electrochemical performance.
[0152] In order to illustrate the beneficial effects of the method of the present application, the present application also provides the following examples and comparative examples:
[0153] Example 1
[0154] Example 1 provides a lithium supplement agent, including a core and a coating layer, wherein the chemical formula of the core is Li 3.5 Fe 0.5 Ni 0.5 O3, the coating layer is carbon material, and the mass ratio of the core to the coating layer is 100:5.
[0155] The preparation method of the lithium supplement in Example 1 comprises the following steps:
[0156] Step 1: dissolving a citric acid complexing agent in an ethanol aqueous solution, and then dissolving lithium hydroxide: ferric acetate: nickel acetate in a molar ratio of 7:1:1, and stirring the solution at 60-90° C. until a dry gel is formed.
[0157] Step 2: sinter the dry gel prepared in step 1 at 750° C. under a protective atmosphere with the oxygen content controlled below 50 ppm for 3-20 hours to prepare a core.
[0158] Step 3: Evenly mix the core prepared in step 2 with a carbon source, and sinter at 300° C. under a protective atmosphere to obtain a lithium supplement material.
[0159] Example 2
[0160] Example 2 provides a lithium supplement agent, which is different from the structure of Example 1 in that the chemical formula of the core of the lithium supplement agent in Example 2 is Li 3.8 Fe 0.6 Mn 0.4 O 3.2 .
[0161] Example 3
[0162] Example 3 provides a lithium supplement agent, which is different from the structure of Example 1 in that the chemical formula of the core of the lithium supplement agent in Example 3 is Li 4.4 Fe 0.8 Ni 0.2 O 3.6 .
[0163] Example 4
[0164] Example 4 provides a lithium supplement agent, which is different from the structure of Example 1 in that the core of the lithium supplement agent in Example 4 contains Li 3.5 Fe 0.5 Ni 0.5 O3 phase and Li5FeO4 phase.
[0165] Example 5
[0166] Example 5 provides a lithium supplement agent, which is different from the structure of Example 1 in that the core of the lithium supplement agent in Example 5 contains Li 4.4 Fe 0.8 Ni 0.2 O 3.6 phase and Li2NiO2 phase.
[0167] Example 6
[0168] Example 6 provides a lithium supplement agent, which is different from the structure of Example 1 in that the core of the lithium supplement agent in Example 6 contains Li 4.4 Fe 0.8 Ni 0.2 O 3.6 phase and Li2MnO4 phase.
[0169] Example 7
[0170] Example 7 provides a lithium supplement. The structure of the lithium supplement is different from that of Example 1 in that, in Example 7, the mass ratio of the core to the coating layer is 100:15.
[0171] Example 8
[0172] Example 8 provides a lithium supplement agent. The structure of the lithium supplement agent is different from that of Example 1 in that the lithium supplement agent is doped with the metal element cerium. In Example 8, the core is prepared by a coprecipitation method. The preparation method of the lithium supplement agent in Example 8 includes the following steps:
[0173] Step 1: dripping ammonia water into a solution of ferric acetate, nickel acetate and cerium acetate, heat-treating the mixed solution and performing a precipitation reaction to generate an iron-based lithium-supplementing material precursor containing Ni.
[0174] Step 2: Mix lithium hydroxide and the iron-based lithium-supplementing material precursor containing M in step 1 in a molar ratio, sinter them at 600-1000° C. for 1-24 hours under a protective atmosphere, and then cool them naturally to obtain a core.
[0175] Step 3: Mix the core and the carbon source, and sinter at 500-800° C. for 1-10 hours under a protective atmosphere to obtain a lithium supplement containing a coating layer structure.
[0176] Comparative Example 1
[0177] Comparative Example 1 provides a lithium supplement agent, which differs from the structure of Example 1 in that, in Comparative Example 1, the core of the lithium supplement agent contains only the lithium-rich compound Li5FeO4.
[0178] Comparative Example 2
[0179] Comparative Example 2 provides a lithium supplement agent, which is different from the structure of Example 1 in that the core of the lithium supplement agent in Comparative Example 2 contains only the lithium-rich compound Li2.6 Fe 0.2 Ni 0.8 O 2.4 .
[0180] Comparative Example 3
[0181] Comparative Example 3 provides a lithium supplement agent, which differs from the structure of Example 1 in that, in Comparative Example 3, the core of the lithium supplement agent contains only the lithium-rich compound Li2NiO2.
[0182] Comparative Example 4
[0183] No lithium supplement is added to the subsequent positive electrode sheets.
[0184] The lithium supplement provided in the above examples and comparative examples were assembled into positive electrode sheets and lithium-ion batteries according to the following methods:
[0185] Positive electrode sheet: A lithium supplement and lithium iron manganese phosphate were mixed in a mass ratio of 2:98 to obtain a mixture. The mixture was mixed with polyvinylidene fluoride and SP-Li in a mass ratio of 95:3:2 and ball-milled to obtain a positive electrode slurry. The positive electrode slurry was coated on the surface of aluminum foil, roll-pressed, and vacuum-dried at 110°C overnight to obtain a positive electrode sheet.
[0186] Negative electrode: graphite negative electrode;
[0187] Electrolyte: Ethylene carbonate and ethyl methyl carbonate were mixed in a volume ratio of 3:7, and LiPF6 was added to form an electrolyte. The concentration of LiPF6 was 1 mol / L.
[0188] Diaphragm: Polypropylene microporous separator;
[0189] Lithium-ion battery assembly: preparation into battery soft pack.
[0190] Related performance tests
[0191] 1. Related tests of lithium supplements
[0192] The core materials of the lithium supplement agent in Examples 1 to 8 were subjected to X-ray diffraction (XRD) analysis, wherein the XRD pattern in Example 1 is shown in FIG2 . As can be seen in FIG2 , the core materials of the lithium supplement agent contain characteristic diffraction peaks of lithium ferrite Li5FeO4 and lithium nickelate Li2NiO2, and the diffraction peaks of Li5FeO4 and Li2NiO2 are relatively strong and have comparable intensities, indicating that the core materials of the lithium supplement agent contain lithium-rich compounds Li 3.5 Fe 0.5 Ni 0.5 O3.
[0193] The XRD patterns of the other embodiments also have corresponding characteristic diffraction peaks.
[0194] The electrochemical performance of each lithium-ion battery assembled in the above lithium-ion battery embodiment was tested as shown in Table 1, and the test conditions were as follows:
[0195] Constant current and constant voltage charging, the first cycle charge and discharge voltage is 2.0-4.3V, the current is 0.1C, and the cut-off current is 0.01C.
[0196] The relevant performance test results are shown in Table 1 below:
[0197] Table 1 Performance test results
[0198] It can be seen from Examples 1-8 and Comparative Example 1 that the addition of the lithium supplement can increase the initial charge capacity of the battery, which means that the lithium supplement provided in this application can improve battery performance.
[0199] It can be seen from Examples 1-3 and Comparative Examples 1-3 that the core includes the Li 5a+2b Fe a M b O 4a+2b , and meets 0.5≤a<1, 0<b≤0.5, and when a+b=1, the battery has a lower water absorption rate. And when the a value gradually increases, the battery's first charge gram capacity increases, the lithium replenishment gram capacity is greatly improved, the water absorption rate decreases, and the gas production only increases slightly. In addition, compared with Comparative Example 1, Examples 1-3 have lower gas production. Compared with Comparative Examples 2-3, Examples 1-3 have higher lithium replenishment gram capacity. In general, the Li 5a+2b Fe a M b O 4a+2b The core has better overall performance and a lower water absorption rate, which makes the battery have higher safety performance.
[0200] As can be seen from Examples 1 and 4, the addition of the Li₅FeO₄ phase to the lithium supplement core increases the battery's initial charge capacity, significantly improves the lithium supplement capacity, reduces the water absorption rate, and maintains minimal change in gas production. This indicates that the addition of the Li₅FeO₄ phase to the lithium supplement core improves battery performance, particularly by increasing the lithium supplement capacity and reducing the water absorption rate.
[0201] As can be seen from Examples 3, 5, and 6, adding a Li₂NiO₂ phase or a Li₂MnO₄ phase to the lithium supplement core significantly reduces battery gas production. The initial charge capacity and water absorption rate remain similar, but a certain amount of lithium supplement capacity is lost. Furthermore, the Li₂MnO₄ phase provides a lower water absorption rate and gas production. This indicates that adding a Li₂NiO₂ phase or a Li₂MnO₄ phase to the lithium supplement core is beneficial for reducing battery gas production.
[0202] As can be seen from Examples 1 and 7, increasing the coating thickness can reduce the battery's water absorption rate and gas production to a certain extent, but it also reduces the lithium replenishment capacity and initial charge capacity. This shows that by appropriately controlling the coating thickness, the water absorption rate and gas production can be reduced while maintaining high lithium replenishment capacity and initial charge capacity.
[0203] From Example 1 and Example 8, after doping the lithium supplement agent with cerium, although the water absorption rate, lithium supplement gram capacity and first charge gram capacity of the battery do not change much, the lithium supplement agent doped with cerium has a lower gas production.
[0204] The lithium supplement agent and its preparation method, positive electrode sheet and secondary battery provided in the embodiments of the present application are introduced in detail above. Specific examples are used herein to illustrate the principles and embodiments of the present application. The description of the above embodiments is only used to help understand the method and core idea of the present application. At the same time, for those skilled in the art, according to the ideas of the present application, there may be changes in the specific embodiments and application scope. In summary, the content of this specification should not be understood as limiting the present application.
Claims
1. A lithium supplement, characterized in that: The lithium supplement comprises a core, the core comprises a first material phase, and the first material phase is Li 5a+2b Fe a M b O 4a+2b , wherein 0.5≤a<1, 0<b≤0.5, and a+b=1, and M is a reducing metal element.
2. The lithium supplement according to claim 1, characterized in that: The reducing metal element includes at least one metal element selected from the group consisting of divalent nickel, divalent manganese, divalent iron, and divalent cobalt.
3. The lithium supplement according to claim 1, characterized in that: The inner core also includes a second material phase, which is Li5FeO4.
4. The lithium supplement according to claim 3, characterized in that: The second material phase is doped with the first material phase; or The second material phase fills the gaps between the first material phases; or The first material is bonded to an outer surface of the second material phase.
5. The lithium supplement according to claim 1, characterized in that: The inner core also includes a third material phase, and the third material phase is Li2MO2.
6. The lithium supplement according to claim 5, characterized in that: The third material is bonded to an outer surface of the first material phase.
7. The lithium supplement according to claim 1, characterized in that: The lithium supplement is further doped with metal elements, and the metal elements include at least one of aluminum, titanium, zirconium, vanadium, manganese, and cerium.
8. The lithium supplement according to claim 1, characterized in that: The lithium supplement further includes a coating layer, and the coating layer is located on the outer surface of the core.
9. The lithium supplement according to claim 8, characterized in that: The coating layer includes at least one of an isolation coating layer, an ion conductor coating layer, and an electronic conductor coating layer.
10. The lithium supplement according to claim 8, characterized in that: The coating layer includes a single atomic deposition layer and / or an oxide nanofilm layer.
11. The lithium supplement according to claim 8, characterized in that: The mass ratio of the core to the coating is 100:(0.01-15); and / or The coating layer has a thickness of 1 nm to 400 nm.
12. The lithium supplement according to claim 1, characterized in that: The particle size D50 of the lithium supplement agent 1 is 0.5 μm-38 μm; and / or The specific surface area of the lithium supplement is 0.1 m 2 / g-20m 2 / g.
13. The lithium supplement according to claim 8, characterized in that: The surface residual alkali value of the lithium supplement agent is 0%-1.5%; and / or The water absorption rate of the lithium supplement agent is less than 20 ppm / s in air at 25°C and 30%-35% relative humidity; and / or At 25° C. and 20%-25% relative humidity in air, the water absorption rate of the lithium supplement agent is less than 10 ppm / s.
14. A method for preparing a lithium supplement, characterized in that: The preparation method of the lithium supplement comprises: Adding lithium source, iron source and M source into the complexing agent solution and stirring to obtain a gel; The gel is sintered in a protective atmosphere to obtain the core of the lithium supplement agent.
15. A method for preparing a lithium supplement, characterized in that: The preparation method of the lithium supplement comprises: The solution of the iron source and the M source is mixed with the precipitant solution to precipitate and obtain a precursor; After the lithium source and the precursor are mixed evenly, sintering is performed under a protective atmosphere to obtain the core of the lithium supplement agent.
16. A positive electrode plate, characterized in that: The positive electrode plate includes the lithium supplement agent according to any one of claims 1 to 13, or includes the lithium supplement agent prepared by the preparation method of the lithium supplement agent according to any one of claims 14 to 15.
17. A secondary battery, characterized in that: The secondary battery comprises a negative electrode sheet, a separator and the positive electrode sheet as claimed in claim 16.
18. The secondary battery according to claim 17, wherein the secondary battery is a lithium-ion battery, wherein the lithium-supplementing gram capacity of the lithium-supplementing agent is greater than or equal to 550 mAh / g; and / or The ratio of the first-cycle gas production of the lithium supplement agent to the first-cycle gas production of the corresponding Li5FeO4 is less than or equal to 50%.
Citation Information
Patent Citations
Composite lithium supplement additive and preparation method and application thereof
CN113036106A
Lithium-rich iron-based composite material as well as preparation method and application thereof
CN115347187A
Lithium supplement material and preparation method and application thereof
CN115548479A
Lithium supplement agent and preparation method thereof, positive pole piece and secondary battery
CN116505103A
Lithium ion secondary battery
JP2007287446A
Cited By
Lithium ferrite lithium supplement agent prepared by step-by-step lithium adding method and preparation method of lithium ferrite lithium supplement agent
CN119349647A
Lithium iron phosphate positive electrode material and preparation method thereof
CN120072933A
Lithium-rich lithium supplement agent with high air stability and preparation method thereof
CN120221659A
Lithium supplement intermediate as well as preparation method and application thereof
CN120328625A
Lithium ion battery positive electrode lithium supplementing material, preparation method thereof, positive electrode material and lithium ion battery
CN120637461A