Electrolyte solution for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery containing same
The use of specific bicyclic sulfate ester or phosphate ester compounds in non-aqueous electrolytes for batteries with Si or silicon oxide electrodes addresses capacity retention and gas suppression issues, enhancing the performance and stability of non-aqueous electrolyte secondary batteries.
Patent Information
- Application Number
- PCT/JP2024/020724
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-08
- Filing Date
- 2024-06-06
- Publication Date
- 2024-12-12
AI Technical Summary
Non-aqueous electrolyte secondary batteries, particularly those using Si or silicon oxide as negative electrode active materials, face challenges in maintaining capacity retention and suppressing gas generation during high-temperature storage, with existing additives like silane compounds and phosphate esters showing limited effectiveness.
Incorporating specific bicyclic sulfate ester compounds or phosphate ester compounds with unsaturated bonds into the non-aqueous electrolyte, combined with an ionic salt and organic solvents, to enhance the electrolyte's performance by forming a protective film on the electrode surfaces.
The proposed electrolyte solution significantly improves capacity retention after cycling and reduces gas generation during high-temperature storage, offering better durability and stability for non-aqueous electrolyte secondary batteries.
Smart Images

Figure JP2024020724_12122024_PF_FP_ABST
Abstract
Description
Electrolyte for non-aqueous electrolyte secondary battery and non-aqueous electrolyte secondary battery using the same
[0001] The present disclosure relates to an electrolyte solution for a nonaqueous electrolyte secondary battery, which contains a sulfate ester compound having a specific bicyclic structure (or spiro structure) or a phosphate ester having a specific unsaturated bond, and a nonaqueous electrolyte secondary battery using the same.
[0002] In recent years, energy storage systems for applications requiring high energy density in information-related devices or communication devices, i.e., small devices such as personal computers, video cameras, digital still cameras, and mobile phones, as well as large devices requiring high power, such as electric vehicles, hybrid vehicles, auxiliary power sources for fuel cell vehicles, and power storage devices, have attracted attention. Non-aqueous electrolyte secondary batteries, such as lithium-ion batteries, lithium batteries, lithium-ion capacitors, and sodium-ion batteries, have been actively developed as candidates. Non-aqueous electrolyte secondary batteries are required to achieve high levels of battery characteristics, such as cycle characteristics, input / output characteristics, storage characteristics, continuous charging characteristics, and safety. Furthermore, in recent years, there has been an increasing demand for higher capacity automotive batteries to extend driving range.
[0003] Although many of these nonaqueous electrolyte secondary batteries have already been put to practical use, further improvements in terms of increasing capacity are desired. In particular, when alloy-based active materials, particularly active materials containing Si atoms, are used as negative electrode active materials, high battery capacity is expected, but it is known that battery performance deteriorates significantly with long-term use. Therefore, efforts have been made to increase capacity and improve durability, for example, to extend the driving range of automobiles. To date, optimization of various battery components, including the active materials of the positive and negative electrodes, has been investigated as a means of improving the high-temperature characteristics and battery characteristics (cycling characteristics) of nonaqueous electrolyte secondary batteries. Nonaqueous electrolyte-related technologies are no exception, and various additives have been proposed to suppress deterioration due to electrolyte decomposition on the surfaces of active positive and negative electrodes.
[0004] Patent Documents 1 and 2 propose a method of suppressing deterioration of cycle characteristics and storage characteristics and suppressing gas generation by adding a silane compound having an unsaturated bond or a cyclic sulfur compound such as ethylene sulfate to a non-aqueous electrolyte. Patent Documents 3 to 7 propose a method of suppressing cycle characteristics and an increase in internal resistance by adding a silane compound having an unsaturated bond to a non-aqueous electrolyte, thereby improving high-temperature storage characteristics and low-temperature characteristics. Patent Document 8 proposes a method of suppressing deterioration of cycle characteristics and increasing initial capacity by adding a phosphorus compound having an unsaturated bond to a non-aqueous electrolyte. Patent Document 9 also proposes a method of improving cycle characteristics and the effect of suppressing resistance increase by adding a phosphate ester or sulfonate ester having an unsaturated bond to a non-aqueous electrolyte. Patent Documents 10 and 11 report a method of improving high-temperature stability, low-temperature characteristics, and cycle characteristics by adding a spiro structure or a dimerized sulfate ester compound to a non-aqueous electrolyte.
[0005] International Publication No. 2016 / 133169 Pamphlet International Publication No. 2017 / 138452 Pamphlet JP 2016-027028 A JP 2016-035820 A JP 2019-102459 A JP 2020-087690 A JP 2019-106362 A US-A1-2003 / 0113635 International Publication No. 2012 / 120597 Pamphlet US-A1-2016 / 0359196 EP-A1-003205655
[0006] However, it has been found that, for example, in a non-aqueous electrolyte solution containing a silane compound having an unsaturated bond as described in Patent Documents 1 to 7, a phosphate ester having an unsaturated bond as described in Patent Document 8, or a phosphate ester or sulfonate ester having an unsaturated bond as described in Patent Document 9, when Si or silicon oxide (for example, with a content of 0.1 to 50% by mass) is used as the negative electrode active material, the cycle characteristics of the non-aqueous electrolyte secondary battery are likely to deteriorate due to repeated charge and discharge, and there is room for further improvement.
[0007] Furthermore, it has been found that nonaqueous electrolyte solutions containing the spiro structure or dimerized sulfate ester compounds described in Patent Documents 10 and 11 tend to increase the amount of gas generated during high-temperature storage in nonaqueous electrolyte secondary batteries that use Si, particularly silicon oxide (for example, with a content of 0.1 to 50% by mass), as the negative electrode active material, and that there is room for further improvement. Therefore, the present disclosure relates to providing an electrolyte solution for nonaqueous electrolyte secondary batteries that can achieve at least one of improved capacity retention after cycling and reduced gas generation during high-temperature storage in nonaqueous electrolyte secondary batteries that contain Si and / or silicon oxide as the negative electrode, and a nonaqueous electrolyte secondary battery using the same.
[0008] As a result of intensive research into achieving the above object, the present inventors have found that the above object can be achieved by incorporating (III) a specific bicyclic sulfate ester compound or (IV) a specific phosphate ester compound in a nonaqueous electrolyte solution used in a nonaqueous electrolyte secondary battery containing Si and / or silicon oxide as a negative electrode active material, together with (I) a nonaqueous organic solvent and (II) a solute that is an ionic salt, and have completed the present invention.
[0009] That is, the present disclosure relates to a nonaqueous electrolyte for a nonaqueous electrolyte secondary battery including a negative electrode containing Si and / or silicon oxide as a negative electrode active material, the nonaqueous electrolyte comprising: (I) a nonaqueous organic solvent; (II) a solute that is an ionic salt; and (III) the following compounds: (1) a bicyclic sulfate ester compound represented by the following general formula (1) (hereinafter also simply referred to as "the compound represented by formula (1)"), (2) a phosphate ester represented by the following general formula (3) (hereinafter also simply referred to as "the compound represented by formula (3)"), or (3) a combination of a bicyclic sulfate ester compound represented by the following general formula (1) and a silane compound having an unsaturated bond represented by the following general formula (2) (hereinafter also simply referred to as "the compound represented by formula (2)") and / or a phosphate ester represented by the following general formula (3).
[0010] [In general formula (1), R 1each independently represents a hydrogen atom, a halogen atom, a linear alkyl group having 1 to 12 carbon atoms, or a branched alkyl group having 3 to 12 carbon atoms, and the alkyl group may contain an oxygen atom between a carbon atom-carbon atom bond, and any hydrogen atom in the alkyl group may be substituted with a fluorine atom.]
[0011] Si(R 2 ) x (R 3 ) 4-x (2) [In general formula (2), R 2 each independently represents an alkenyl group or an alkynyl group, R 3 each independently represents a group selected from the group consisting of a fluorine atom, an alkyl group, an alkoxy group, an aryl group, and an aryloxy group, a hydrogen atom of which may be substituted with a fluorine atom, and x is an integer of 2 to 4.
[0012] PO (OR 4 ) y (OR 5 ) 3-y (3) [In general formula (3), R 4 each independently represents an alkenyl group or an alkynyl group, R 5 represents an alkyl group or an aryl group, and a hydrogen atom in these groups may be substituted with a fluorine atom, and y is an integer of 2 to 3.] Furthermore, if necessary, graphite may be used in combination with Si and / or silicon oxide as the negative electrode active material.
[0013] Preferred aspects of the present disclosure are, for example, as follows: 1. A nonaqueous electrolyte solution for a nonaqueous electrolyte secondary battery containing a negative electrode containing Si and / or silicon oxide as a negative electrode active material, the nonaqueous electrolyte solution comprising the following components: (I) a nonaqueous organic solvent, (II) a solute which is an ionic salt, and (III) a compound represented by formula (1). 2. A nonaqueous electrolyte solution for a nonaqueous electrolyte secondary battery containing a negative electrode containing Si and / or silicon oxide as a negative electrode active material, the nonaqueous electrolyte solution comprising the following components: (I) a nonaqueous organic solvent, (II) a solute which is an ionic salt, and (IV) a compound represented by formula (3). 3. 3. A non-aqueous electrolyte for a non-aqueous electrolyte secondary battery containing a negative electrode containing Si and / or silicon oxide as a negative electrode active material, the non-aqueous electrolyte comprising the following components: (I) a non-aqueous organic solvent, (II) a solute which is an ionic salt, (III) a compound represented by formula (1), and (V) a compound represented by formula (2) and / or a compound represented by formula (3). 1 4. The non-aqueous electrolyte solution according to 1 or 3 above, wherein at least one of the groups is a hydrogen atom.
[0014] 5. The above R 2 are each independently a group selected from the group consisting of a vinyl group, a 2-propenyl group, a 1-propenyl group, an ethynyl group, and a 2-propynyl group, and 3 are each independently a group selected from the group consisting of a fluorine atom, a methyl group, an ethyl group, a propyl group, a 2,2,2-trifluoroethyl group, a 2,2,3,3-tetrafluoropropyl group, a 1,1,1-trifluoroisopropyl group, a 1,1,1,3,3,3-hexafluoroisopropyl group, a 2,2,2-trifluoroethoxy group, a 2,2,3,3-tetrafluoropropoxy group, a 2,2,3,3,3-pentafluoropropoxy group, a 1,1,1-trifluoroisopropoxy group, and a 1,1,1,3,3,3-hexafluoroisopropoxy group. 2 At least one of the (4-x) R 37. The nonaqueous electrolyte solution according to the above 3 or 5, wherein at least one of R is a methyl group or a fluorine atom. 8. The nonaqueous electrolyte solution according to the above 3, wherein R is 3 or 4. 4 are each independently a group selected from the group consisting of a 1-propenyl group, a 2-propenyl group, an ethynyl group, a 2-propynyl group, and a 2-butynyl group, and 5 9. The nonaqueous electrolyte solution according to the above 2 or 3, wherein R is an alkyl group. 4 are each independently a group selected from the group consisting of a 2-propenyl group, a 2-propynyl group, and a 2-butynyl group, and 5 is a methyl group or an ethyl group. 10. The nonaqueous electrolyte according to the above 2 or 3, wherein y is 3. 11. The nonaqueous electrolyte according to the above 1 or 3, wherein the concentration of the compound represented by formula (1) is 0.1 to 5 mass % relative to the total amount of the nonaqueous electrolyte. 12. The nonaqueous electrolyte according to the above 2 or 3, wherein the concentration of the compound represented by formula (3) is 0.01 to 5 mass % relative to the total amount of the nonaqueous electrolyte. 13. The nonaqueous electrolyte according to the above 3, wherein the concentration of the compound represented by formula (2) is 0.01 to 5 mass % relative to the total amount of the nonaqueous electrolyte. 14. The nonaqueous electrolyte according to any one of the above 1 to 13, wherein the negative electrode active material further contains graphite. 15. 15. The nonaqueous electrolyte solution according to item 14, wherein the content of the Si and / or silicon oxide is 0.1 to 50 mass% with respect to the total amount of the Si and / or silicon oxide and graphite contained in the negative electrode active material.
[0015] 16. The non-aqueous electrolyte solution according to any one of items 1 to 15 above, wherein the non-aqueous organic solvent is at least one selected from the group consisting of cyclic esters, chain esters, cyclic ethers, chain ethers, sulfone compounds, and sulfoxide compounds. 17. The non-aqueous electrolyte solution according to item 16 above, wherein the cyclic ester is a cyclic carbonate. 18. The non-aqueous electrolyte solution according to item 16 above, wherein the chain ester is a chain carbonate. 19. The non-aqueous electrolyte solution according to any one of items 1 to 15 above, wherein the non-aqueous organic solvent is at least one selected from the group consisting of propylene carbonate, ethylene carbonate, butylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, γ-butyrolactone, γ-valerolactone, methyl acetate, methyl propionate, ethyl propionate, tetrahydrofuran, 2-methyltetrahydrofuran, dioxane, dimethoxyethane, diethyl ether, dimethyl sulfoxide, and sulfolane. 20. The non-aqueous electrolyte according to any one of items 1 to 19, wherein the solute, which is an ionic salt, is composed of a cation and an anion, the cation being selected from the group consisting of alkali metal ions, alkaline earth metal ions, and quaternary ammonium ions, and the anion being selected from the group consisting of hexafluorophosphate, tetrafluoroborate, perchlorate, hexafluoroarsenate, hexafluoroantimonate, and bis(fluorosulfonyl)imide. 21. The non-aqueous electrolyte according to item 20, wherein the alkali metal ion is a lithium ion or a sodium ion.
[0016] 22. Further, lithium difluorophosphate, sodium difluorophosphate, lithium fluorosulfate, sodium fluorosulfate, lithium trifluoromethanesulfonate, sodium trifluoromethanesulfonate, lithium difluorobis(oxalato)phosphate, sodium difluorobis(oxalato)phosphate, lithium difluorooxalatoborate, sodium difluorooxalatoborate, lithium bis(oxalato)borate, sodium bis(oxalato)borate, lithium tetrafluorooxalatophosphate, sodium tetrafluorooxalatophosphate, lithium tris(oxalato)phosphate, sodium tris(oxalato)phosphate, lithium difluoro(malonato)borate, sodium difluoro(malonato)borate, lithium tetrafluoro(malonato)phosphate, sodium tetrafluoro(malonato)phosphate, lithium monofluorophosphate, sodium monofluorophosphate, lithium bis(difluorophosphoryl)imide, sodium bis(difluorophosphoryl)imide, lithium (difluorophosphoryl)(fluorosulfonyl)imide, (difluorophosphoryl)(fluoro sulfonyl)imide sodium, bis(trifluoromethanesulfonyl)imide lithium, bis(trifluoromethanesulfonyl)imide sodium, bis(pentafluoroethanesulfonyl)imide lithium, bis(pentafluoroethanesulfonyl)imide sodium, (trifluoromethanesulfonyl)(pentafluoroethanesulfonyl)imide lithium, (trifluoromethanesulfonyl)(pentafluoroethanesulfonyl)imide sodium, (trifluoromethanesulfonyl)(fluorosulfonyl)imide lithium, (trifluoromethanesulfonyl)(fluorosulfonyl)imide sodium, (pentafluoroethanesulfonyl)(fluorosulfonyl)imide lithium, (pentafluoroethanesulfonyl)(fluorosulfonyl)imide sodium, tris(trifluoromethanesulfonyl)methide lithium, tris(trifluoromethanesulfonyl)methide sodium, lithium acrylate, sodium acrylate, lithium methacrylate, sodium methacrylate, lithium methyl sulfate, sodium methyl sulfate, lithium ethyl sulfate,22. The non-aqueous electrolyte solution according to any one of items 1 to 21 above, further comprising at least one selected from the group consisting of cyclohexylbenzene, cyclohexylfluorobenzene, biphenyl, 2-fluorobiphenyl, t-butylbenzene, t-amylbenzene, 2-fluorotoluene, fluorobenzene, vinylene carbonate, a vinylene carbonate oligomer (having a number average molecular weight of 170 to 5000 in terms of polystyrene), vinylethylene carbonate, difluoroanisole, fluoroethylene carbonate, 1,6-diisocyanatohexane, ethynylethylene carbonate, trans-difluoroethylene carbonate, methyl propargyl carbonate, ethyl propargyl carbonate, dipropargyl carbonate, maleic anhydride, succinic anhydride, 1,3-propane sultone, 1,3-propene sultone, 1,4-butane sultone, dimethylvinylene carbonate, 1,3,2-dioxa 23. The non-aqueous electrolyte solution according to any one of items 1 to 22 above, containing at least one selected from the group consisting of thiolane-2,2-dioxide, 4-propyl-1,3,2-dioxathiolane-2,2-dioxide, methylenemethane disulfonate, dimethylenemethane disulfonate, trimethylenemethane disulfonate, methyl methanesulfonate, methanesulfonyl fluoride, ethenesulfonyl fluoride, phenyl difluorophosphate, 1,2-ethanedisulfonic anhydride, tris(trimethylsilyl)borate, succinonitrile, (ethoxy)pentafluorocyclotriphosphazene, tetrafluoro(picolinato)phosphate, difluoro(picolinato)borate, and 1,3-dimethyl-1,3-divinyl-1,3-di(1,1,1,3,3,3-hexafluoroisopropyl)disiloxane. 24. A non-aqueous electrolyte secondary battery comprising: a negative electrode containing Si and / or silicon oxide as a negative electrode active material; a positive electrode; and the non-aqueous electrolyte solution according to any one of items 1 to 23 above. 25. The non-aqueous electrolyte secondary battery according to item 24 above, wherein the negative electrode active material further contains graphite.
[0017] When used in a nonaqueous electrolyte secondary battery containing Si and / or silicon oxide as the negative electrode active material, the nonaqueous electrolyte solution of the present disclosure can exhibit at least one of an improvement in the capacity retention rate after cycling of the nonaqueous electrolyte secondary battery and a reduction in the amount of gas generated during high-temperature storage.
[0018] The composition of the electrolyte solution for a nonaqueous electrolyte secondary battery according to the present disclosure will be described in detail below. Regarding Component (I) (Nonaqueous Organic Solvent): The nonaqueous organic solvent used in the electrolyte solution for a nonaqueous electrolyte secondary battery according to the present disclosure is not particularly limited as long as it can dissolve component (II), the compound represented by formula (1), the compound represented by formula (2), and the compound represented by formula (3), which will be described in detail below, and any nonaqueous organic solvent can be used. Specific examples of such non-aqueous organic solvents include cyclic carbonates that are also cyclic esters, such as propylene carbonate (hereinafter sometimes referred to as "PC"), ethylene carbonate (hereinafter sometimes referred to as "EC"), and butylene carbonate; chain carbonates that are also chain esters, such as diethyl carbonate (hereinafter sometimes referred to as "DEC"), dimethyl carbonate (hereinafter sometimes referred to as "DMC"), and ethyl methyl carbonate (hereinafter sometimes referred to as "EMC"); cyclic esters such as γ-butyrolactone and γ-valerolactone; chain esters such as methyl acetate, methyl propionate, and ethyl propionate (hereinafter sometimes referred to as "EP"); cyclic ethers such as tetrahydrofuran, 2-methyltetrahydrofuran, and dioxane; chain ethers such as dimethoxyethane and diethyl ether; sulfone compounds such as dimethyl sulfoxide and sulfolane; and sulfoxide compounds. The nonaqueous organic solvents of the present disclosure may be used singly or in any combination and ratio of two or more depending on the application. Among these, propylene carbonate, ethylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, methyl propionate, and ethyl propionate are particularly preferred from the viewpoints of electrochemical stability against oxidation-reduction and chemical stability related to heat and reactions with the solute.
[0019] Furthermore, it is preferable that the nonaqueous organic solvent contains, for example, one or more cyclic carbonates having a high dielectric constant and one or more chain carbonates or chain esters having a low liquid viscosity, since this increases the ionic conductivity of the electrolyte solution. Specifically, it is more preferable to use a nonaqueous organic solvent containing the following combinations: (1) Combination of EC and EMC, (2) Combination of EC and DEC, (3) Combination of EC, DMC and EMC, (4) Combination of EC, DEC and EMC, (5) Combination of EC, EMC and EP, (6) Combination of PC and DEC, (7) Combination of PC and EMC, (8) Combination of PC and EP, (9) Combination of PC, DMC and EMC, (10) Combination of PC, DEC and EMC, (11) Combination of PC, DEC and EP, (12) Combination of PC, EC and EMC, (13) Combination of PC, EC, DMC and EMC, (14) Combination of PC, EC, DEC and EMC, (15) Combination of PC, EC, EMC and EP
[0020] Regarding Component (II) (Solute as an Ionic Salt): The solute used in the electrolyte for a nonaqueous electrolyte secondary battery of the present disclosure is an ionic salt consisting of a pair of any cation and anion. As long as it exists in an ionic state as a cation and an anion in a nonaqueous organic solvent, various ionic salt solutes can be used without particular limitation. Specific examples of such ionic salt solutes include alkali metal ions such as lithium ion and sodium ion, alkaline earth metal ions, and quaternary ammonium ions as cations, and anions such as hexafluorophosphate, tetrafluoroborate, perchlorate, hexafluoroarsenate, hexafluoroantimonate, and bis(fluorosulfonyl)imide as anions. The ionic salt solutes of the present disclosure may be used singly or in any combination and ratio depending on the application. Among these, in consideration of the energy density, output characteristics, lifespan, etc. of the battery, lithium, sodium, magnesium, quaternary ammonium, etc. are preferably used as the cation, and hexafluorophosphate, tetrafluoroborate, bis(fluorosulfonyl)imide, etc. are preferably used as the anion.
[0021] The concentration of the ionic salt solute in the electrolyte solution for a nonaqueous electrolyte secondary battery according to the present disclosure (hereinafter referred to as the "solute concentration") is not particularly limited as long as it is a concentration that can fully exhibit the function of the ionic salt solute. For example, the lower limit may be 0.5 mol / L or more, preferably 0.7 mol / L or more, more preferably 0.9 mol / L or more, and the upper limit may be 5 mol / L or less, preferably 4 mol / L or less, more preferably 2 mol / L or less. A concentration of 0.5 mol / L or more is preferable because the ionic conductivity is less likely to decrease, and the cycle characteristics and output characteristics of the nonaqueous electrolyte battery are less likely to decrease. On the other hand, a concentration of 5 mol / L or less is preferable because the viscosity of the electrolyte solution for a nonaqueous electrolyte battery is less likely to increase, and the ionic conductivity is less likely to decrease. When two or more types of ionic salt solutes are used, the total concentration of the solutes is preferably within the above-mentioned range.
[0022] The liquid temperature when dissolving the ionic salt solute in the nonaqueous organic solvent is not particularly limited, but is preferably -20 to 80°C, more preferably 0 to 60°C, for example.
[0023] Description of Component (III), Component (IV), and Component (V) Compound represented by formula (1) (also simply referred to as "compound (1)") Compound (1) used in the electrolyte solution for a nonaqueous electrolyte secondary battery of the present disclosure is a bicyclic sulfate ester compound represented by the following formula (1): In the formula, R 1 are each independently a hydrogen atom, a halogen atom, a linear alkyl group having 1 to 12 carbon atoms, or a branched alkyl group having 3 to 12 carbon atoms, and the alkyl group may contain an oxygen atom between a carbon atom-carbon atom bond. Any hydrogen atom in the alkyl group may be substituted with a fluorine atom.
[0024] Examples of halogen atoms include fluorine atoms, chlorine atoms, and bromine atoms, with fluorine atoms being particularly preferred as halogen atoms. Suitable examples of linear alkyl groups having 1 to 12 carbon atoms include alkyl groups having 1 to 6 carbon atoms, such as methyl, ethyl, n-propyl, n-butyl, and n-pentyl. Suitable examples of branched alkyl groups having 3 to 12 carbon atoms include isopropyl, isobutyl, sec-butyl, tert-butyl, neopentyl, isopentyl, sec-pentyl, 3-pentyl, and tert-pentyl. The alkyl groups may contain an oxygen atom between carbon-carbon bonds, and any hydrogen atoms in the alkyl groups may be substituted with a fluorine atom. Examples of groups containing an oxygen atom between a carbon atom-carbon atom bond in an alkyl group include alkoxyalkyl groups, specific examples of which include a methoxymethyl group, an ethoxymethyl group, a propoxymethyl group, a methoxyethyl group, an ethoxyethyl group, and a 1-methylethoxymethyl group. Furthermore, examples of alkyl groups in which any hydrogen atom in the alkyl group has been substituted with a fluorine atom include a trifluoromethyl group, a 2,2-difluoroethyl group, a 2,2,2-trifluoroethyl group, a 2,2,3,3-tetrafluoropropyl group, a 1,1,1,3,3,3-hexafluoroisopropyl group, a 1-trifluoromethylethyl group, and a 1,2-difluoropropyl group. 1 It is preferred that at least one of R is a hydrogen atom, and particularly preferred that all R 1 is preferably a hydrogen atom.
[0025] As specific examples of Compound (1) used in the electrolyte for a nonaqueous electrolyte secondary battery according to the present disclosure, the following compounds can be suitably cited as representative bicyclic sulfate compounds. These compounds are referred to in the present disclosure as Compound 1-1 and Compound 1-2, respectively, by their compound numbers, as follows. These compounds are known compounds, and their production methods are disclosed, for example, in Can. J. Chem., 79, 1040-1048 (2001), etc. The compound (1) is generally blended in an amount of 0.1 to 5 mass %, preferably 0.1 to 4 mass %, based on 100 mass % of the total amount of the non-aqueous electrolyte.
[0026] Regarding the compound represented by formula (2) (also simply referred to as "compound (2)"), the compound (2) used in the electrolyte solution for the nonaqueous electrolyte secondary battery of the present disclosure is a silane compound represented by the following general formula (2): Si(R 2 ) x (R 3 ) 4-x (2) In the general formula (2), x is an integer of 2 to 4. 2 are each independently an alkenyl group or an alkynyl group, each of which preferably has 2 to 5 carbon atoms, more preferably 2 or 3. 3 each independently represents a group selected from the group consisting of a fluorine atom, an alkyl group, an alkoxy group, an aryl group, and an aryloxy group, and a hydrogen atom of these groups may be substituted with a fluorine atom.
[0027] R 2 Specific examples of the R groups are, independently, vinyl, 2-propenyl, 1-propenyl, ethynyl, 2-propynyl, etc. 2 It is important that the compound has two or more alkenyl or alkynyl groups represented by the formula (2). That is, in general formula (2), x is 2 or more. Furthermore, it is preferable that the x is 3 or 4 from the viewpoint of cycle characteristics and / or gas suppression effects, and it is particularly preferable that the x is 4.
[0028] R 3 The alkyl group as the alkyl group is preferably an alkyl group having 1 to 5, preferably 1 to 3, carbon atoms, and may be a straight-chain alkyl group or a branched alkyl group. Suitable examples of the straight-chain alkyl group include a methyl group, an ethyl group, and a propyl group. Suitable examples of the branched alkyl group include an isopropyl group and an isobutyl group. Suitable examples of the alkoxy group include an alkoxy group corresponding to the above straight-chain or branched alkyl group, and specific examples thereof include a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, and the like. The hydrogen atoms of these alkyl groups or alkoxy groups may be substituted with fluorine atoms, and suitable examples of such fluorinated alkyl groups or alkoxy groups include a 2,2,2-trifluoroethyl group, a 2,2,3,3-tetrafluoropropyl group, a 1,1,1-trifluoroisopropyl group, a 1,1,1,3,3,3-hexafluoroisopropyl group, a 2,2,2-trifluoroethoxy group, a 2,2,3,3-tetrafluoropropoxy group, a 2,2,3,3,3-pentafluoropropoxy group, a 1,1,1-trifluoroisopropoxy group, and a 1,1,1,3,3,3-hexafluoroisopropoxy group. R 3 At least one of the x R's may be, in particular, a methyl group or a fluorine atom. 2 At least one of the R 3 At least one of these is preferably a methyl group or a fluorine atom.
[0029] Suitable examples of the aryl group include a phenyl group. The aryl group may have a hydrogen atom substituted with a fluorine atom. Suitable examples of such fluorine-substituted aryl groups include a pentafluorophenyl group. An aryloxy group is an oxy group corresponding to an aryl group, and similarly suitable examples include aryloxy groups having a fluorine atom. Specific examples of Compound (2) include the following compounds, which are representative examples of silane compounds (2). These compounds are referred to in this disclosure by the two series numbers listed below as compound numbers below the chemical formula. All of these compounds are known compounds, and their production methods are disclosed in, for example, JP 2000-143677 A, JP 2004-256494 A, and JP 05-104541 A.
[0030]
[0031]
[0032] The compound (2) is generally used in an amount of 0.01 to 5 mass %, preferably 0.1 to 2.5 mass %, based on 100 mass % of the total amount of the non-aqueous electrolyte.
[0033] Regarding the compound represented by formula (3) (also simply referred to as "compound (3)"), the compound (3) used in the electrolyte solution for a nonaqueous electrolyte secondary battery of the present disclosure is a compound represented by the following general formula (3): PO(OR 4 ) y (OR 5 ) 3-y (3) In the general formula (3), y is 2 or 3. 4 R each independently represents an alkenyl group or an alkynyl group. Each of these groups preferably has 2 to 5 carbon atoms, more preferably 2 to 3. In particular, a phosphate ester containing multiple alkynyl groups is preferred. 4Specifically, each independently is preferably a vinyl group, a 2-propenyl group, a 1-propenyl group, an ethynyl group, a 2-propynyl group, a 1-propynyl group, a 2-butynyl group, etc., and among these, a 2-propenyl group, a 2-propynyl group, a 2-butynyl group, etc. are preferred. 4 In other words, y in the formula is 2 or more. When y is 3, it is particularly preferable from the viewpoint of improving cycle characteristics and / or gas suppression.
[0034] R when y is 2 5 represents an alkyl group or an aryl group, and the hydrogen atoms of these groups may be substituted with fluorine atoms. 5 The alkyl group as the alkyl group is preferably an alkyl group having 1 to 5 carbon atoms, preferably 1 to 3 carbon atoms, and may be a linear or branched alkyl group. Suitable linear alkyl groups include, for example, a methyl group, an ethyl group, and a propyl group. Suitable branched alkyl groups include, for example, an isopropyl group and an isobutyl group. Furthermore, a hydrogen atom of the alkyl group may be substituted with a fluorine atom. Suitable examples of such fluorine-substituted alkyl groups include, for example, a 2,2,2-trifluoroethyl group, a 2,2,3,3-tetrafluoropropyl group, a 1,1,1-trifluoroisopropyl group, and a 1,1,1,3,3,3-hexafluoroisopropyl group. Suitable examples of aryl groups include a phenyl group. An aryl group in which a hydrogen atom is substituted with a fluorine atom may also be used. Suitable examples of such fluorine-substituted aryl groups include a pentafluorophenyl group.
[0035] As specific examples of compound (3), the following compounds can be preferably mentioned as representative compounds. In the present disclosure, these compounds are referred to by the three series of numbers written below the chemical formula as compound numbers, as follows. All of these compounds are known compounds.
[0036] The amount of compound (3) used in the electrolyte solution for nonaqueous electrolyte secondary batteries of the present disclosure is generally 0.01 to 5 mass%, preferably 0.1 to 2.5 mass%, based on the total amount of the nonaqueous electrolyte solution being 100 mass%. Compound (2) and / or compound (3) may be used in combination with compound (1). In this case, the total concentration of compound (1), compound (2), and / or compound (3) is preferably, for example, 0.1 to 5 mass%, preferably 0.5 to 4 mass%, based on the total amount of the nonaqueous electrolyte solution. The electrolyte solution for nonaqueous electrolyte secondary batteries of the present disclosure, when used in a nonaqueous electrolyte secondary battery containing a negative electrode having Si and / or silicon oxide as the negative electrode active material, exhibits a good balance of both excellent cycle characteristics and excellent gas suppression characteristics by using compound (1) in combination with compound (2) and / or compound (3).
[0037] Regarding additives, the electrolyte solution for a non-aqueous electrolyte battery of the present disclosure may contain additives commonly used in this technical field in any proportion, as long as the gist of the present disclosure is not impaired. When the non-aqueous electrolyte solution of the present disclosure contains the additives, the content of the additives may be 0.01% by mass or more and 10% by mass or less, based on the total amount of the non-aqueous electrolyte solution. Examples of such additives include cyclohexylbenzene, cyclohexylfluorobenzene, biphenyl, 2-fluorobiphenyl, t-butylbenzene, t-amylbenzene, 2-fluorotoluene, fluorobenzene, vinylene carbonate (hereinafter sometimes referred to as "VC"), vinylene carbonate oligomer (having a number average molecular weight of 170 to 5000 in terms of polystyrene), vinylethylene carbonate, difluoroanisole, fluoroethylene carbonate (hereinafter sometimes referred to as "FEC"), 1,6-diisocyanatohexane, ethynylethylene carbonate, trans-difluoroethylene carbonate, methylpropargyl carbonate, ethylpropargyl carbonate, dipropargyl carbonate, maleic anhydride, succinic anhydride, 1,3-propane sultone, 1,3- Examples of suitable amines include propene sultone, 1,4-butane sultone, dimethylvinylene carbonate, 1,3,2-dioxathiolane-2,2-dioxide, 4-propyl-1,3,2-dioxathiolane-2,2-dioxide, methylenemethane disulfonate, dimethylenemethane disulfonate, trimethylenemethane disulfonate, methyl methanesulfonate, methanesulfonyl fluoride, ethenesulfonyl fluoride, phenyl difluorophosphate, 1,2-ethanedisulfonic anhydride, tris(trimethylsilyl)borate, succinonitrile, (ethoxy)pentafluorocyclotriphosphazene, tetrafluoro(picolinato)phosphate, difluoro(picolinato)borate, and 1,3-dimethyl-1,3-divinyl-1,3-di(1,1,1,3,3,3-hexafluoroisopropyl)disiloxane.
[0038] Further, examples of the additives include lithium difluorophosphate, sodium difluorophosphate, lithium fluorosulfate, sodium fluorosulfate, lithium trifluoromethanesulfonate, sodium trifluoromethanesulfonate, lithium difluorobis(oxalato)phosphate, sodium difluorobis(oxalato)phosphate, lithium difluorooxalatoborate, sodium difluorooxalatoborate, lithium bis(oxalato)borate, sodium bis(oxalato)borate, lithium tetrafluorooxalatophosphate, sodium tetrafluorooxalatophosphate, lithium tris(oxalato)phosphate, sodium tris(oxalato)phosphate, lithium difluoro(malonato)borate, sodium difluoro(malonato)borate, lithium tetrafluoro(malonato)phosphate, sodium tetrafluoro(malonato)phosphate, lithium monofluorophosphate, sodium monofluorophosphate, lithium bis(difluorophosphoryl)imide, sodium bis(difluorophosphoryl)imide, lithium (difluorophosphoryl)(fluorosulfonyl)imide, (difluorophosphoryl)(fluorosulfonyl)imide, tris(trifluoromethanesulfonyl)methide sodium, bis(trifluoromethanesulfonyl)imide lithium, bis(trifluoromethanesulfonyl)imide sodium, bis(pentafluoroethanesulfonyl)imide lithium, bis(pentafluoroethanesulfonyl)imide sodium, (trifluoromethanesulfonyl)(pentafluoroethanesulfonyl)imide lithium, (trifluoromethanesulfonyl)(pentafluoroethanesulfonyl)imide sodium, (trifluoromethanesulfonyl)(fluorosulfonyl)imide lithium, (trifluoromethanesulfonyl)(fluorosulfonyl)imide sodium, (pentafluoroethanesulfonyl)(fluorosulfonyl)imide lithium, (pentafluoroethanesulfonyl)(fluorosulfonyl)imide sodium, tris(trifluoromethanesulfonyl)methide lithium, tris(trifluoromethanesulfonyl)methide sodium, carboxylic acid salts such as lithium acrylate, sodium acrylate, lithium methacrylate, and sodium methacrylate, lithium methyl sulfate, sodium methyl sulfate,Examples of suitable electrolytes include sulfate esters such as lithium ethyl sulfate and sodium ethyl sulfate. Furthermore, as in the case of non-aqueous electrolyte batteries known as lithium polymer batteries, the electrolyte for non-aqueous electrolyte batteries can be quasi-solidified with a gelling agent or cross-linked polymer.
[0039] Regarding nonaqueous electrolyte secondary batteries, the configuration of a nonaqueous electrolyte secondary battery using the electrolyte solution for nonaqueous electrolyte secondary batteries of the present disclosure will be described. The nonaqueous electrolyte secondary battery of the present disclosure basically employs the configuration used in general nonaqueous electrolyte secondary batteries. That is, it comprises a positive electrode and a negative electrode capable of absorbing and releasing lithium, a current collector, a separator, a container, and the like. In particular, even when applied to nonaqueous electrolyte secondary batteries employing a negative electrode using a specific negative electrode active material, which is desired from the viewpoint of high capacity, the electrolyte solution for nonaqueous electrolyte secondary batteries of the present disclosure can exhibit at least one of improved capacity retention after cycling and reduced gas generation during high-temperature storage, which have not been achieved until now. That is, when used in nonaqueous electrolyte secondary batteries containing Si and / or silicon oxide as the negative electrode active material, the electrolyte solution for nonaqueous electrolyte secondary batteries of the present disclosure provides an electrolyte for nonaqueous electrolyte secondary batteries that can exhibit at least one of improved capacity retention after cycling and reduced gas generation during high-temperature storage.
[0040] [Positive Electrode] The positive electrode may contain, as a positive electrode active material, at least one selected from the group consisting of an oxide containing at least nickel and a phosphate containing nickel.
[0041] [Positive Electrode Active Material] In the case of a lithium ion secondary battery in which the cations in the non-aqueous electrolyte are mainly lithium, the positive electrode active material constituting the positive electrode is not particularly limited as long as it contains at least one selected from the group consisting of nickel-containing oxides and nickel-containing phosphates and is a variety of chargeable and dischargeable materials. Examples of the positive electrode active material include (A) a lithium transition metal composite oxide containing nickel or, in addition to nickel, one or more metals selected from the group consisting of manganese, cobalt, and aluminum, and having a layered structure; (B) a lithium manganese composite oxide having a spinel structure and containing nickel; (C) a lithium-containing olivine-type phosphate containing nickel; and (D) a lithium-excess layered transition metal oxide having a layered rock salt structure and containing nickel.
[0042] (A) Lithium Transition Metal Composite Oxide) Positive Electrode Active Material (A) Examples of lithium transition metal composite oxides containing nickel or nickel plus one or more metals selected from the group consisting of manganese, cobalt, and aluminum and having a layered structure include lithium-nickel composite oxide, lithium-nickel-cobalt composite oxide, lithium-nickel-cobalt-aluminum composite oxide, lithium-nickel-manganese composite oxide, and lithium-nickel-manganese-cobalt composite oxide. These lithium transition metal composite oxides may also be used in which some of the transition metal atoms constituting the main component are replaced with other elements such as Al, Ti, V, Cr, Fe, Cu, Zn, Mg, Ga, Zr, Si, B, Ba, Y, and Sn. Specific examples of lithium-nickel composite oxides include LiNiO and lithium nickel oxide (LiNiO) particles doped with different elements such as Mg, Zr, Al, and Ti, with aluminum oxide coating on the particle surface.
[0043] The lithium-nickel-cobalt composite oxide and the lithium-nickel-cobalt-aluminum composite oxide are represented by the following general formula [1-1]: Li a Ni 1-b-c Co b M 1 cO2 [1-1] In formula [1-1], M 1 is at least one element selected from the group consisting of Al, Fe, Mg, Zr, Ti, and B, and a satisfies the conditions of 0.9≦a≦1.2, and b and c satisfy the conditions of 0.1≦b≦0.3 and 0≦c≦0.1. These can be prepared, for example, in accordance with the manufacturing method described in JP-A-2009-137834. Specifically, LiNi 0.8 Co 0.2 O2 and LiNi 0.85 Co 0.10 Al 0.05 O2, LiNi 0.87 Co 0.10 Al 0.03 O2, LiNi 0.6 Co 0.3 Al 0.1 O2 and the like are preferred.
[0044] Specific examples of lithium-nickel-manganese composite oxides include LiNi 0.5 Mn 0.5 O2, LiCo 0.5 Mn 0.5 O2, etc.
[0045] Examples of the lithium-nickel-manganese-cobalt composite oxide include lithium-containing composite oxides represented by the following general formula [1-2]: Li d Ni e Mn f Co g M 2 h O2 [1-2] In formula [1-2], M 2 is at least one element selected from the group consisting of Al, Fe, Mg, Zr, Ti, B, and Sn, d is 0.9≦d≦1.2, and e, f, g, and h satisfy the conditions of e+f+g+h=1, 0≦e≦0.9, 0≦f≦0.5, 0≦g≦0.5, and h≧0.
[0046] The lithium-nickel-manganese-cobalt composite oxide preferably contains manganese in the range shown in the general formula [1-2] in order to enhance the structural stability and improve the safety of the lithium secondary battery at high temperatures, and more preferably further contains cobalt in the range shown in the general formula [1-2] in order to enhance the high-rate characteristics of the lithium ion secondary battery. Specifically, for example, a lithium-nickel-manganese-cobalt composite oxide having a charge / discharge range of 4.3 V or more, such as Li[Ni 1 / 3 Mn 1 / 3 Co 1 / 3 ]O2 (hereinafter, sometimes referred to as "NCM111"), Li[Ni 0.45 Mn 0.35 Co 0.2 ]O2, Li[Ni 0.5 Mn 0.3 Co 0.2 ]O2, Li[Ni 0.6 Mn 0.2 Co 0.2 ]O2 (hereinafter, sometimes referred to as "NCM622"), Li[Ni 0.8 Mn 0.1 Co 0.1 ]O2 (hereinafter, sometimes referred to as "NCM811"), Li[Ni 0.49 Mn 0.3 Co 0.2 Zr 0.01 ]O2, Li[Ni 0.49 Mn 0.3 Co 0.2 Mg 0.01 ]O2 and the like are preferred.
[0047] ((B) Lithium manganese composite oxide having a spinel structure) Positive electrode active material (B) Examples of lithium manganese composite oxides having a spinel structure include spinel-type lithium manganese composite oxides represented by the general formula [1-3]: Li j (Mn 2-k M 3 k )O4 [1-3] In formula [1-3], M 3contains Ni and may contain at least one metal element selected from the group consisting of Co, Fe, Mg, Cr, Cu, Al, and Ti. j is 1.05≦j≦1.15, and k is 0<k≦0.20. Specifically, for example, LiMn 1.9 Ni 0.1 O4, LiMn 1.5 Ni 0.5 O4, etc.
[0048] ((C) Lithium-containing olivine-type phosphate) Positive electrode active material (C) Examples of the lithium-containing olivine-type phosphate include those represented by the following general formula [1-4]: LiFe 1-n M 4 n PO4 [1-4] In formula [1-4], M 4 contains Ni and may also contain at least one selected from Co, Mn, Cu, Zn, Nb, Mg, Al, Ti, W, Zr, and Cd, where n is 0<n≦1. Specifically, LiNiPO4 and the like are suitable examples.
[0049] ((D) Lithium-Rich Layered Transition Metal Oxide) Positive Electrode Active Material (D) Examples of lithium-rich layered transition metal oxides having a layered rock salt structure include those represented by the following general formula [1-5]: xLiM 5 O2・(1-x)Li2M 6 O3 [1-5] In formula [1-5], x is a number satisfying 0<x<1, and M 5 has an average oxidation number of 3 + At least one metal element is selected from the group consisting of: M 6 has an average oxidation number of 4 + In formula [1-5], M is at least one metal element. 5 is preferably one metal element selected from trivalent Mn, Ni, Co, Fe, V, and Cr, but may be divalent and tetravalent metals in equal amounts to make the average oxidation number trivalent.
[0050] In addition, in the formula [1-5], M 6 is preferably one or more metal elements selected from Mn, Zr and Ti. 5and M 6 Nickel is always included in either of the following. 0.5 Mn 0.5 O2] 0.5[Li2MnO3] and 0.5[LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2]・0.5[Li2MnO3], 0.5[LiNi 0.375 Co 0.25 Mn 0.375 O2]・0.5[Li2MnO3], 0.5[LiNi 0.375 Co 0.125 Fe 0.125 Mn 0.375 O2]・0.5[Li2MnO3], 0.45[LiNi 0.375 Co 0.25 Mn 0.375 Suitable examples of the positive electrode active material (D) represented by the general formula [1-5] include 0.10[LiTiO] and 0.45[LiMnO]. The positive electrode active material (D) represented by the general formula [1-5] is known to exhibit high capacity upon high-voltage charging of 4.4 V (based on Li) or higher (see, for example, U.S. Patent No. 7,135,252). These positive electrode active materials can be prepared according to the manufacturing methods described in, for example, JP 2008-270201 A, WO 2013 / 118661 A, and JP 2013-030284 A.
[0051] The positive electrode active material may contain at least one selected from the above (A) to (D) as a main component, but other components that may be contained include, for example, transition element chalcogenides such as FeS, TiS, TiO, VO, MoO, and MoS, conductive polymers such as polyacetylene, polyparaphenylene, polyaniline, and polypyrrole, activated carbon, radical-generating polymers, and carbon materials.
[0052] [Positive Electrode Current Collector] The positive electrode has a positive electrode current collector. As the positive electrode current collector, for example, aluminum, stainless steel, nickel, titanium, or an alloy thereof can be used.
[0053] [Positive Electrode Active Material Layer] The positive electrode comprises, for example, a positive electrode active material layer formed on at least one surface of a positive electrode current collector. The positive electrode active material layer is composed of, for example, the above-described positive electrode active material, a binder, and, if necessary, a conductive agent. Examples of binders include polytetrafluoroethylene, polyvinylidene fluoride, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, styrene butadiene rubber (SBR), carboxymethyl cellulose, methyl cellulose, cellulose acetate phthalate, hydroxypropyl methyl cellulose, and polyvinyl alcohol. Examples of conductive agents that can be used include carbon materials such as acetylene black, ketjen black, furnace black, carbon fiber, graphite (granular graphite or flake graphite), and fluorinated graphite. For the positive electrode, it is preferable to use acetylene black or ketjen black, which have low crystallinity.
[0054] [Negative Electrode] As described above, Si and / or silicon oxide (hereinafter, sometimes referred to as "SiOx") is used as the negative electrode active material. Graphite may also be used in combination, if necessary. Specifically, the negative electrode active material in the present disclosure contains Si and / or silicon oxide. Silicon oxide is a compound represented by SiOx, where x has a value of 0.5 to 1.5. The negative electrode active material may be silicon metal or silicon oxide (SiOx). When graphite is included as the negative electrode active material, the content of Si and / or silicon oxide contained in the negative electrode active material is generally 0.1 to 50% by mass, preferably 0.1 to 30% by mass, where the total amount of the Si and / or silicon oxide and graphite contained in the negative electrode active material is 100% by mass.
[0055] The graphite used can be various types of artificial graphite or natural graphite. Because graphite undergoes very little change in its crystalline structure during lithium absorption and desorption, it can achieve high energy density and excellent cycle characteristics. The shape of the graphite can be fibrous, spherical, granular, or flaky. Amorphous carbon or graphite coated with amorphous carbon is more preferred because it reduces the reactivity between the material surface and the electrolyte. In the case of a lithium-ion secondary battery in which the cations in the nonaqueous electrolyte are mainly lithium, the graphite can be doped and dedoped with lithium ions. Examples of such graphite include graphite with a d value of the lattice plane (002 plane) of 0.340 nm or less in X-ray diffraction and graphite with a d value of the lattice plane (002 plane) of more than 0.340 nm in X-ray diffraction. These negative electrode active materials can be used alone or in combination of two or more.
[0056] [Negative Electrode Current Collector] The negative electrode has a negative electrode current collector. As the negative electrode current collector, for example, copper, stainless steel, nickel, titanium, or an alloy thereof can be used.
[0057] [Negative Electrode Active Material Layer] (c) The negative electrode has, for example, a negative electrode active material layer formed on at least one surface of a negative electrode current collector. The negative electrode active material layer is composed of, for example, the above-mentioned negative electrode active material, a binder, and, if necessary, a conductive agent. Examples of the binder include polytetrafluoroethylene, polyvinylidene fluoride, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, styrene butadiene rubber (SBR), carboxymethyl cellulose, methyl cellulose, cellulose acetate phthalate, hydroxypropyl methyl cellulose, and polyvinyl alcohol. Examples of the conductive agent that can be used include carbon materials such as acetylene black, ketjen black, furnace black, and carbon fiber.
[0058] [Method for producing electrodes (positive and negative electrodes)] The electrodes can be obtained, for example, by dispersing and kneading the active material, binder, and optionally conductive agent in predetermined amounts in a solvent such as N-methyl-2-pyrrolidone (NMP) or water, applying the resulting paste to a current collector, and drying to form an active material layer. The resulting electrode is preferably compressed by a method such as a roll press to adjust it to an electrode with an appropriate density.
[0059] [Separator] The nonaqueous electrolyte battery of the present disclosure may include a separator. Examples of separators used to prevent contact between the positive electrode and the negative electrode include nonwoven fabrics or porous sheets made of polyolefins such as polypropylene and polyethylene, cellulose, paper, or glass fiber. These films are preferably microporous so that the electrolyte can penetrate and ions can easily pass through. Examples of polyolefin separators include microporous polymer films such as porous polyolefin films, which electrically insulate the positive electrode and negative electrode and are permeable to lithium ions. Specific examples of porous polyolefin films include porous polyethylene films alone, or multilayer films formed by stacking porous polyethylene films and porous polypropylene films. Other examples include composite films of porous polyethylene and polypropylene films. The nonaqueous electrolyte of the present disclosure is impregnated and retained in the separator. There are no particular limitations on the impregnation method, and any known method may be used. Specifically, the electrolyte can be finally injected into a battery equipped with a positive electrode, a separator, and a negative electrode to impregnate the battery.
[0060] [Exterior Body] When constructing a nonaqueous electrolyte secondary battery containing the electrolyte solution for nonaqueous electrolyte secondary batteries of the present disclosure, suitable exterior bodies for the electrolyte solution for nonaqueous electrolyte secondary batteries include, for example, coin-shaped, cylindrical, or rectangular metal cans, as well as laminate exterior bodies. Suitable metal can materials include, for example, nickel-plated steel sheets, stainless steel sheets, nickel-plated stainless steel sheets, aluminum or its alloys, nickel, and titanium. Suitable laminate exterior bodies include, for example, aluminum laminate films, SUS laminate films, and laminate films of silica-coated polypropylene, polyethylene, etc.
[0061] The configuration of the nonaqueous electrolyte secondary battery according to this embodiment is not particularly limited, but may be, for example, a configuration in which an electrode element in which a positive electrode and a negative electrode are arranged opposite each other, and a nonaqueous electrolyte are enclosed in an exterior body. The shape of the nonaqueous electrolyte secondary battery is not particularly limited, but an electrochemical device in the shape of a coin, cylinder, square, aluminum laminate sheet, or the like is assembled from the above-mentioned components.
[0062] A nonaqueous electrolyte secondary battery containing the electrolyte solution for nonaqueous electrolyte secondary batteries of the present disclosure can be produced, for example, by impregnating a separator with the electrolyte solution for nonaqueous electrolyte secondary batteries, and assembling the separator between a positive electrode having at least one selected from the group consisting of nickel-containing oxides and phosphates as a positive electrode active material, and a negative electrode containing Si and / or silicon oxide (SiOx) as a negative electrode active material.
[0063] Hereinafter, the present disclosure will be described in more detail with reference to Examples, Comparative Examples, and Reference Examples, but the scope of the present disclosure is not limited by these Examples, Comparative Examples, and Reference Examples. In the following description, the specific comparative compounds used in the Comparative Examples are the following compounds. These compounds are referred to by the numbers written below their chemical formulas.
[0064] Comparative Example Compound
[0065] [Preparation of Nonaqueous Electrolytes in Examples and Comparative Examples] <Comparative Example 1-1> (Preparation of LiPF Solution) In a glove box with a dew point of −60° C. or less, EC, EMC, and DEC were mixed in a volume ratio of EC:EMC:DEC = 3:5:2. Thereafter, while maintaining the internal temperature at 40° C. or less, LiPF in an amount to give a concentration of 0.9 mol / L relative to the total amount of nonaqueous electrolyte, and FEC in an amount to give a concentration of 10.0 mass% relative to the total amount of nonaqueous electrolyte were added, and the mixture was stirred for 1 hour to dissolve, thereby preparing a comparative nonaqueous electrolyte 1-1.
[0066] <Example 1-1> (Preparation of non-aqueous electrolyte 1-1) In a glove box with a dew point of -60 ° C. or less, EC, EMC, and DEC were mixed in a volume ratio of EC: EMC: DEC = 3: 5: 2. Then, while maintaining the internal temperature at 40 ° C. or less, a concentration of 0.9 mol / L of LiPF 6 was obtained with respect to the total amount of non-aqueous electrolyte, a concentration of 10.0 mass% of FEC with respect to the total amount of non-aqueous electrolyte, a concentration of 0.5 mass% of compound (1) (1-1), and a concentration of 0.5 mass% of compound (2) (2-3) were added, and the non-aqueous electrolyte 1-1 of Example 1-1 was prepared by adding the compound (2-3), and stirring for 1 hour to dissolve.
[0067] Examples 1-2 to 1-12 (Preparation of Non-Aqueous Electrolyte Solutions 1-2 to 1-12) Non-aqueous electrolyte solutions 1-2 to 1-12 of the examples were prepared in the same manner as in the preparation of non-aqueous electrolyte solution 1-1 of the example, except that the types and contents of compound (1), compound (2), and the comparative compound were changed as shown in Table 1.
[0068] Examples 2-1 to 2-20 and Comparative Example 2-1 (Preparation of Non-aqueous Electrolytes 2-1 to 2-20, and Comparative Non-aqueous Electrolyte 2-1) Non-aqueous electrolytes 2-1 to 2-20 of the Examples and comparative non-aqueous electrolyte 2-1 were prepared in the same manner as in the preparation of non-aqueous electrolyte 1-1 of the Examples, except that the types and contents of compound (1), compound (3), and the comparative compound were changed as shown in Table 2.
[0069] <Comparative Example 3-1> (Preparation of LiPF Solution) In a glove box with a dew point of −60° C. or less, EC, EMC, and DEC were mixed in a volume ratio of EC:EMC:DEC = 3:5:2. Thereafter, while maintaining the internal temperature at 40° C. or less, LiPF in an amount to give a concentration of 0.9 mol / L relative to the total amount of nonaqueous electrolyte, FEC in an amount to give a concentration of 5.0 mass% relative to the total amount of nonaqueous electrolyte, and VC in an amount to give a concentration of 1.0 mass% were added, and the mixture was stirred for 1 hour to dissolve, thereby preparing a comparative nonaqueous electrolyte solution 3-1.
[0070] <Example 3-1> (Preparation of non-aqueous electrolyte 3-1) In a glove box with a dew point of -60 ° C. or less, EC, EMC, and DEC were mixed in a volume ratio of EC: EMC: DEC = 3: 5: 2. Then, while maintaining the internal temperature at 40 ° C. or less, the total amount of non-aqueous electrolyte was adjusted to a concentration of 0.9 mol / L, and the total amount of non-aqueous electrolyte was adjusted to a concentration of 5.0 mass% of FEC, and the amount of VC was adjusted to a concentration of 1.0 mass%, and the amount of compound (1) corresponding to the compound (1-1), and the amount of compound (2) corresponding to the compound (2-3), and as other additives, the amount of lithium difluorophosphate was added to a concentration of 1.0 mass%, and the mixture was stirred for 1 hour to dissolve. Thus, the non-aqueous electrolyte 3-1 of the example was prepared.
[0071] Examples 3-2 to 3-6 (Preparation of Non-Aqueous Electrolytes 3-2 to 3-6) Non-aqueous electrolytes 3-2 to 3-6 of the examples were obtained in the same manner as in the preparation of non-aqueous electrolyte 3-1 of the examples, except that the type and content of compound (1), compound (2), compound (3), or other additives and solutes were changed as shown in Table 3 below. For reference, Table 3 also lists Examples 1-3V, 1-5V, and 1-6V, which used non-aqueous electrolytes 1-3V, 1-5V, and 1-6V prepared using the "other additives and solutes" shown in Table 3 for non-aqueous electrolytes 1-3, 1-5, and 1-6 of the non-aqueous electrolytes of Example 1 series. Furthermore, for reference, Table 3 also lists Examples 2-3V, 2-5V, and 2-7V, which are nonaqueous electrolyte solutions 2-3V, 2-5V, and 2-7V prepared using the "other additives / solutes" shown in Table 3 instead of "other additives" for nonaqueous electrolyte solutions 2-3, 2-5, and 2-7 of the nonaqueous electrolyte solutions of Example 2 series.
[0072] Reference Example 4-1 and Comparative Example 4-1 (Preparation of Comparative Non-Aqueous Electrolyte 4-1) In a glove box with a dew point of −60° C. or less, EC, EMC, and DEC were mixed in a volume ratio of EC:EMC:DEC = 3:5:2. Thereafter, while maintaining the internal temperature at 40° C. or less, LiPF in an amount so that the concentration was 0.9 mol / L relative to the total amount of non-aqueous electrolyte, and FEC in an amount so that the concentration was 10.0 mass% relative to the total amount of non-aqueous electrolyte were added, and the mixture was stirred for 1 hour to dissolve, thereby preparing a comparative non-aqueous electrolyte 4-1.
[0073] <Example 4-1> (Preparation of non-aqueous electrolyte 4-1) In a glove box with a dew point of -60 ° C. or less, EC, EMC, and DEC were mixed in a volume ratio of EC: EMC: DEC = 3: 5: 2. Then, while maintaining the internal temperature at 40 ° C. or less, a concentration of 0.9 mol / L of LiPF 6 was obtained with respect to the total amount of non-aqueous electrolyte, a concentration of 10.0 mass% of FEC with respect to the total amount of non-aqueous electrolyte, a concentration of 0.5 mass% of compound (1) (1-1), and a concentration of 0.5 mass% of compound (2) (2-12) were added, and the non-aqueous electrolyte 4-1 of the example was prepared by stirring and dissolving for 1 hour.
[0074] Examples 4-2 to 4-3, Reference Examples 4-2 to 4-3, and Examples 4-2V to 4-3V (Preparation of Non-Aqueous Electrolytes 4-2 to 4-3, and Non-Aqueous Electrolytes 4-2V to 4-3V) Non-aqueous electrolytes 4-2 to 4-3, and non-aqueous electrolytes 4-2V to 4-3V were prepared in the same manner as in the preparation of non-aqueous electrolyte 4-1 of the Examples, except that the type and content of compound (1), compound (2), and / or compound (3) were changed as shown in Table 4.
[0075] Reference Example 4-4 and Example 4-4V (Preparation of Non-Aqueous Electrolyte 4-4V) In a glove box with a dew point of −60° C. or less, EC, EMC, and DEC were mixed in a volume ratio of EC:EMC:DEC = 3:5:2. Thereafter, while maintaining the internal temperature at 40° C. or less, LiPF 6 was added in an amount to give a concentration of 0.9 mol / L relative to the total amount of non-aqueous electrolyte, FEC in an amount to give a concentration of 10.0 mass% relative to the total amount of non-aqueous electrolyte, and VC in an amount to give a concentration of 0.5 mass%. The mixture was stirred for 1 hour to dissolve, thereby preparing non-aqueous electrolyte 4-4V. In Table 4 below, the Reference Example is shown as being used in a non-aqueous electrolyte secondary battery containing a negative electrode that uses only graphite as the negative electrode active material.
[0076] <Example 4-4> (Preparation of non-aqueous electrolyte 4-4) In a glove box with a dew point of -60 ° C. or less, EC, EMC, and DEC were mixed in a volume ratio of EC: EMC: DEC = 3: 5: 2. Then, while maintaining the internal temperature at 40 ° C. or less, a concentration of 0.9 mol / L of LiPF6 was added to the total amount of non-aqueous electrolyte, a concentration of 10.0 mass% of FEC was added to the total amount of non-aqueous electrolyte, a concentration of 1.0 mass% of the compound (1) corresponding to the compound (1-1), a concentration of 0.5 mass% of the compound (2) corresponding to the compound (2-3), and other additives were added to the amount of VC to a concentration of 0.5 mass%, and the non-aqueous electrolyte 4-4 was prepared by stirring and dissolving for 1 hour.
[0077] Examples 4-5 to 4-7 Preparation of Non-Aqueous Electrolytes 4-5 to 4-7 Non-aqueous electrolytes 4-5 to 4-7 were prepared in the same manner as in the preparation of non-aqueous electrolyte 4-4, except that the type of compound (2) or compound (3) was changed as shown in Table 4.
[0078] [Preparation of non-aqueous electrolyte battery] (Preparation of NCM811 positive electrode) LiNi 0.8 Co 0.1 Mn 0.1 A positive electrode composite paste was prepared by mixing 92.0% by mass of O2 powder with 3.5% by mass of polyvinylidene fluoride (PVDF) as a binder and 4.5% by mass of acetylene black as a conductive material, and then adding N-methyl-2-pyrrolidone. This paste was applied to both sides of aluminum foil (A1085), dried, pressed, and then punched out to a 4 cm x 5 cm piece to obtain a test NCM811 positive electrode.
[0079] (Preparation of NCM622 positive electrode) LiNi 0.6 Co 0.2 Mn 0.2 A positive electrode composite paste was prepared by mixing 90.0% by mass of O powder with 5.0% by mass of PVDF as a binder and 5.0% by mass of acetylene black as a conductive material, and then adding N-methyl-2-pyrrolidone. This paste was applied to both sides of aluminum foil (A1085), dried, pressed, and then punched out to a 4 cm x 5 cm piece to obtain a test NCM622 positive electrode.
[0080] (Preparation of NCM111 positive electrode) Li[Ni 1 / 3 Mn 1 / 3 Co 1 / 3 A positive electrode composite paste was prepared by mixing 90.0% by mass of ]O powder with 5.0% by mass of PVDF as a binder and 5.0% by mass of acetylene black as a conductive material, and then adding N-methyl-2-pyrrolidone. This paste was applied to both sides of aluminum foil (A1085), dried, pressed, and then punched out to a 4 cm x 5 cm piece to obtain a test NCM111 positive electrode.
[0081] (Silicon-containing graphite anode used in the experiments in Tables 1, 2 and 4 (in the table, "graphite + SiO x ") Preparation of artificial graphite powder 72.0 mass % SiO xA negative electrode composite paste was prepared by mixing 20.0% by mass of (x=1), 3.0% by mass of conductive material (HS-100), 2.0% by mass of carbon nanofiber (VGCF), 2.0% by mass of styrene butadiene rubber, and 1.0% by mass of sodium carboxymethyl cellulose with water. This paste was applied to one side of copper foil, dried, pressed, and then punched out to a 4 cm x 5 cm piece to obtain a silicon-containing graphite negative electrode for testing.
[0082] (Silicon-containing graphite negative electrode used in the experiment related to Table 3 (in the table, "graphite + SiO x ") Preparation of artificial graphite powder 82.0 mass % SiO x A negative electrode composite paste was prepared by mixing 10.0% by mass of (x=1), 3.0% by mass of conductive material (HS-100), 2.0% by mass of carbon nanofiber (VGCF), 2.0% by mass of styrene butadiene rubber, and 1.0% by mass of sodium carboxymethyl cellulose with water. This paste was applied to one side of copper foil, dried, pressed, and then punched out to a 4 cm x 5 cm piece to obtain a silicon-containing graphite negative electrode for testing.
[0083] (Preparation of Graphite Negative Electrode (referred to as "Graphite" in the Tables)) 98.0% by mass of artificial graphite powder was mixed with 1.0% by mass of styrene-butadiene rubber, 1.0% by mass of carboxymethyl cellulose, and water to prepare a negative electrode composite paste. This paste was applied to one side of copper foil, dried and pressed, and then punched out to a 4 cm x 5 cm piece to obtain a test graphite negative electrode.
[0084] (Preparation of Nonaqueous Electrolyte Batteries) In an argon atmosphere with a dew point of −50° C. or less, terminals were welded to the above-described NCM811 positive electrode, NCM622 positive electrode, or NCM111 positive electrode. Then, two polyethylene separators (5 cm × 6 cm) were sandwiched between them. The outer surface of the separator was then sandwiched between two silicon-containing graphite negative electrodes or two graphite negative electrodes with pre-welded terminals, with the negative electrode active material facing the positive electrode active material. The resultant battery was then placed in an aluminum-laminated bag with an opening on one side. After vacuum-injecting the nonaqueous electrolyte, the opening was heat-sealed to prepare aluminum-laminated nonaqueous electrolyte batteries of the Examples and Comparative Examples. The nonaqueous electrolytes used were those listed in Tables 1 to 4. Using the cells prepared in the above manner, the cycle characteristics and the amount of gas generated during high-temperature storage were evaluated as described below.
[0085] [Evaluation of Nonaqueous Electrolyte Battery] <Cycle Characteristics Test> A charge / discharge test was carried out at an ambient temperature of 25° C. to evaluate the cycle characteristics. As an initial conditioning, charging was performed up to 4.2 V and discharging was performed up to 2.5 V at a current density of 1.9 mA / cm. 2 This constitutes one cycle, and a total of three charge / discharge cycles were performed to stabilize the battery. The discharge capacity measured in the fourth cycle was taken as the initial charge / discharge capacity. The battery was then charged to 4.2 V and discharged to 2.5 V at a current density of 1.9 mA / cm. 2 The charge / discharge cycle was repeated about 500 times, and the deterioration of the cell was evaluated based on the discharge capacity retention rate after 500 cycles. The discharge capacity retention rate after 500 cycles was calculated using the following formula.
[0086] (Discharge capacity retention rate after 500 cycles) Discharge capacity retention rate (%) = (Discharge capacity after 500 cycles) × 100 / (Initial charge / discharge capacity) The values of the discharge capacity retention rate after 500 cycles for all Examples listed in Table 1 are relative values when the discharge capacity retention rate after 500 cycles for Comparative Example 1-1 is set to 100. The values of the discharge capacity retention rate after 500 cycles for all Examples listed in Table 2 are relative values when the discharge capacity retention rate after 500 cycles for Comparative Example 2-1 is set to 100. The values of the discharge capacity retention rate after 500 cycles for all Examples listed in Table 3 are relative values when the discharge capacity retention rate after 500 cycles for Comparative Example 3-1 is set to 100. The values of the discharge capacity retention rate after 500 cycles for all Examples listed in Table 4 are relative values when the discharge capacity retention rate after 500 cycles for Comparative Example 4-1 is set to 100. The discharge capacity retention rate after 500 cycles shown in all the reference examples in Table 4 is a relative value when the discharge capacity retention rate after 500 cycles of Reference Example 4-1 is set to 100.
[0087] <Gas generation amount during high temperature storage (80°C)> At an ambient temperature of 25°C, the gas generation amount was measured using a constant current / constant voltage method up to a maximum charging voltage of 4.2 V, with a current density of 0.38 mA / cm 2 After charging at 100°C, the battery was stored at an ambient temperature of 80°C for 10 days. The volume of the battery was measured before and after storage, and the difference was taken as the amount of gas generated. The numerical values of the amount of gas generated for all Examples listed in Table 1 are relative values when the amount of gas generated in Comparative Example 1-1 is set to 100. The numerical values of the amount of gas generated for all Examples listed in Table 2 are relative values when the amount of gas generated in Comparative Example 2-1 is set to 100. The numerical values of the amount of gas generated for all Examples listed in Table 3 are relative values when the amount of gas generated in Comparative Example 3-1 is set to 100. The numerical values of the amount of gas generated for all Examples listed in Table 4 are relative values when the amount of gas generated in Comparative Example 4-1 is set to 100. The numerical values of the amount of gas generated for all Reference Examples listed in Table 4 are relative values when the amount of gas generated in Reference Example 4-1 is set to 100.
[0088] According to the results shown in Table 1 below, when compound (1) and compound (2) are used in combination (Examples 1-1 to 1-8), it has been confirmed that in nonaqueous electrolyte secondary batteries containing Si and / or silicon oxide (SiOx) as the negative electrode active material, the post-cycling capacity retention rate can be improved and the amount of gas generated during high-temperature storage can be suppressed. In particular, it can be seen that even when compound (1) is used alone (Examples 1-9 and 1-10), at least the post-cycling capacity retention rate can be improved. Furthermore, the same results were obtained when compound (1) was used in combination with a comparative compound different from compound (2) (Examples 1-11 and 1-12). Although the detailed mechanism is unknown, it is presumed that this is due to the decomposition of sulfate ester compound (1) having a bicyclic structure during charge and discharge, resulting in the formation of a high-quality coating on the negative electrode surface.
[0089] In the present disclosure, graphite is not necessarily required as the negative electrode active material. For example, a "negative electrode containing Si as a negative electrode active material" formed using Si powder, as described in paragraph 0094 of JP 2022-191483 A, may be applied to the present disclosure.
[0090]
[0091] According to the results shown in Table 2 below, when compound (1) and compound (3) are used in combination (Examples 2-1 to 2-8), it has been confirmed that the post-cycle capacity retention rate can be improved and the amount of gas generation during high-temperature storage can be suppressed in nonaqueous electrolyte secondary batteries containing a negative electrode containing Si and / or silicon oxide (SiOx) as the negative electrode active material. It is also understood that at least the post-cycle capacity retention rate can be improved when compound (1) is used alone (Examples 2-9 and 2-10) or when a comparative compound different from compound (1) is used in combination with compound (3) (Examples 2-19 and 2-20). Furthermore, it is also understood that at least the suppression of gas generation during high-temperature storage can be improved when compound (3) is used alone (Examples 2-11 to 2-14). This situation was similar when compound (3) was used in combination with a sulfate ester compound having a structure different from that of compound (1) (i.e., not having a spiro structure) (Examples 2-15 to 2-18). Therefore, it is clear that compound (3) alone can exhibit at least one of the effects of improving the capacity retention rate after cycling and suppressing the amount of gas generated during high-temperature storage.
[0092]
[0093] According to the results shown in Table 3 below, by using compound (1), compound (2), and / or compound (3), and further using lithium difluorophosphate, lithium difluorobis(oxalato)phosphate, or lithium bis(difluorophosphoryl)imide as other additives or additional solutes in combination, it was confirmed that the capacity retention rate after cycling was further improved compared to Examples not containing such additives. Also, by using compound (1), compound (2), and / or compound (3), and further using lithium fluorosulfate, lithium (difluorophosphoryl)(fluorosulfonyl)imide, or lithium bis(fluorosulfonyl)imide as other additives or additional solutes in combination, it was confirmed that the amount of gas generated during high-temperature storage was further reduced compared to Examples not containing such additives.
[0094]
[0095] Furthermore, from the results shown in Table 4 below, it was confirmed that when nonaqueous electrolytes 4-2V to 4-4V containing compound (1) alone were used in nonaqueous electrolyte secondary batteries using graphite as the negative electrode active material, they exhibited an effect of improving the post-cycling capacity retention rate and an effect of suppressing the amount of gas generation during high-temperature storage, as in Reference Examples 4-2 to 4-4. However, it is understood that even when used in nonaqueous electrolyte secondary batteries using Si and / or silicon oxide (SiOx) and graphite as the negative electrode active material, at least the post-cycling capacity retention rate can be improved. Furthermore, it was confirmed that when compound (1) was used in combination with compound (2) and / or compound (3), the post-cycling capacity retention rate was improved and the amount of gas generation during high-temperature storage could be suppressed. That is, when compound (1) was used in combination with compound (2) and / or compound (3), it was confirmed that when Si and / or silicon oxide was contained as the negative electrode active material, both the effect of improving the post-cycling capacity retention rate and the effect of suppressing the amount of gas generation during high-temperature storage could be improved. Although the detailed mechanism is unclear, it is speculated that when the negative electrode active material contains Si and / or silicon oxide, compound (1) having a spiro structure and compound (2) or compound (3) having a plurality of groups having unsaturated bonds co-decompose during charging and discharging, thereby forming a high-quality coating on the surface of the negative electrode.
[0096]
Claims
1. A nonaqueous electrolyte for a nonaqueous electrolyte secondary battery containing a negative electrode containing Si and / or silicon oxide as a negative electrode active material, the nonaqueous electrolyte comprising the following components: (I) a nonaqueous organic solvent; (II) a solute which is an ionic salt; and (III) a compound represented by the following formula (1): [In general formula (1), R 1 each independently represents a hydrogen atom, a halogen atom, or a linear alkyl group having 1 to 12 carbon atoms or a branched alkyl group having 3 to 12 carbon atoms, and an oxygen atom may be contained between a carbon atom-carbon atom bond in the alkyl group, and any hydrogen atom in the alkyl group may be substituted with a fluorine atom.
2. A nonaqueous electrolyte for a nonaqueous electrolyte secondary battery containing a negative electrode containing Si and / or silicon oxide as a negative electrode active material, the nonaqueous electrolyte comprising the following components: (I) a nonaqueous organic solvent, (II) a solute which is an ionic salt, and (IV) a compound represented by the following formula (3): PO(OR 4 ) y (OR 5 ) 3-y (3) [In general formula (3), R 4 each independently represents an alkenyl group or an alkynyl group; R 5 represents an alkyl group or an aryl group, a hydrogen atom of which may be substituted with a fluorine atom, and y is an integer of 2 to 3.
3. A nonaqueous electrolyte for a nonaqueous electrolyte secondary battery containing a negative electrode containing Si and / or silicon oxide as a negative electrode active material, the nonaqueous electrolyte comprising the following components: (I) a nonaqueous organic solvent; (II) a solute which is an ionic salt; (III) a compound represented by the following formula (1); and (V) a compound represented by the following formula (2) and / or a compound represented by the following formula (3). [In general formula (1), R 1 each independently represents a hydrogen atom, a halogen atom, or a linear alkyl group having 1 to 12 carbon atoms or a branched alkyl group having 3 to 12 carbon atoms, and an oxygen atom may be contained between a carbon atom-carbon atom bond in the alkyl group, and any hydrogen atom in the alkyl group may be substituted with a fluorine atom. ] Si(R 2 ) x (R 3 ) 4-x (2) [In general formula (2), R 2 each independently represents an alkenyl group or an alkynyl group; R 3 each independently represents a group selected from the group consisting of a fluorine atom, an alkyl group, an alkoxy group, an aryl group, and an aryloxy group, a hydrogen atom of which may be substituted with a fluorine atom, and x is an integer of 2 to 4. 4 ) y (OR 5 ) 3-y (3) [In general formula (3), R 4 each independently represents an alkenyl group or an alkynyl group; R 5 represents an alkyl group or an aryl group, a hydrogen atom of which may be substituted with a fluorine atom, and y is an integer of 2 to 3.
4. The above eight R 1 The nonaqueous electrolyte according to claim 1 or 3, wherein at least one of the groups is a hydrogen atom.
5. The above R 2 are each independently selected from the group consisting of a vinyl group, a 2-propenyl group, a 1-propenyl group, an ethynyl group, and a 2-propynyl group, 3 are each independently selected from the group consisting of a fluorine atom, a methyl group, an ethyl group, a propyl group, a 2,2,2-trifluoroethyl group, a 2,2,3,3-tetrafluoropropyl group, a 1,1,1-trifluoroisopropyl group, a 1,1,1,3,3,3-hexafluoroisopropyl group, a 2,2,2-trifluoroethoxy group, a 2,2,3,3-tetrafluoropropoxy group, a 2,2,3,3,3-pentafluoropropoxy group, a 1,1,1-trifluoroisopropoxy group, and a 1,1,1,3,3,3-hexafluoroisopropoxy group.
6. The x R 2 At least one of the (4−x) R 3 6. The nonaqueous electrolyte according to claim 3, wherein at least one of the groups is a methyl group or a fluorine atom.
7. The nonaqueous electrolyte according to claim 3, wherein x is 3 or 4.
8. The above R 4 are each independently selected from the group consisting of 1-propenyl, 2-propenyl, ethynyl, 2-propynyl, and 2-butynyl groups, and R 5 The nonaqueous electrolyte according to claim 2 or 3, wherein is an alkyl group.
9. The above R 4 are each independently a group selected from the group consisting of a 2-propenyl group, a 2-propynyl group, and a 2-butynyl group, 5 The nonaqueous electrolyte according to claim 2, 3 or 8, wherein is a methyl group or an ethyl group.
10. The nonaqueous electrolyte according to claim 2 or 3, wherein y is 3.
11. The non-aqueous electrolyte according to claim 1 or 3, wherein the concentration of the compound represented by formula (1) is 0.1 to 5 mass % based on the total amount of the non-aqueous electrolyte.
12. The non-aqueous electrolyte according to claim 2 or 3, wherein the concentration of the compound represented by formula (3) is 0.01 to 5 mass % based on the total amount of the non-aqueous electrolyte.
13. The nonaqueous electrolyte according to claim 3, wherein the concentration of the compound represented by formula (2) is 0.01 to 5 mass % based on the total amount of the nonaqueous electrolyte.
14. The nonaqueous electrolyte according to any one of claims 1 to 13, wherein the negative electrode active material further contains graphite.
15. The nonaqueous electrolyte according to claim 14, wherein the content of the Si and / or silicon oxide is 0.1 to 50 mass % based on the total amount of the Si and / or silicon oxide and graphite contained in the negative electrode active material.
16. The nonaqueous electrolyte solution according to any one of claims 1 to 15, wherein the nonaqueous organic solvent is at least one selected from the group consisting of cyclic esters, chain esters, cyclic ethers, chain ethers, sulfone compounds, and sulfoxide compounds.
17. The nonaqueous electrolyte according to claim 16, wherein the cyclic ester is a cyclic carbonate.
18. The nonaqueous electrolyte according to claim 16, wherein the chain ester is a chain carbonate.
19. The nonaqueous electrolyte according to any one of claims 1 to 15, wherein the nonaqueous organic solvent is at least one selected from the group consisting of propylene carbonate, ethylene carbonate, butylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, γ-butyrolactone, γ-valerolactone, methyl acetate, methyl propionate, ethyl propionate, tetrahydrofuran, 2-methyltetrahydrofuran, dioxane, dimethoxyethane, diethyl ether, dimethyl sulfoxide, and sulfolane.
20. The nonaqueous electrolyte according to any one of claims 1 to 19, wherein the solute which is an ionic salt is composed of a cation and an anion, the cation being selected from the group consisting of an alkali metal ion, an alkaline earth metal ion, and a quaternary ammonium, and the anion being selected from the group consisting of hexafluorophosphate, tetrafluoroborate, perchlorate, hexafluoroarsenate, hexafluoroantimonic acid, and bis(fluorosulfonyl)imide.
21. The nonaqueous electrolyte according to claim 20, wherein the alkali metal ion is a lithium ion or a sodium ion.
22. Further, lithium difluorophosphate, sodium difluorophosphate, lithium fluorosulfate, sodium fluorosulfate, lithium trifluoromethanesulfonate, sodium trifluoromethanesulfonate, lithium difluorobis(oxalato)phosphate, sodium difluorobis(oxalato)phosphate, lithium difluorooxalatoborate, sodium difluorooxalatoborate, lithium bis(oxalato)borate, sodium bis(oxalato)borate, lithium tetrafluorooxalatophosphate, sodium tetrafluorooxalatophosphate, lithium tris(oxalato)phosphate, sodium tris(oxalato)phosphate, lithium difluoro(malonato)borate, sodium difluoro(malonato)borate, lithium tetrafluoro(malonato)phosphate, sodium tetrafluoro(malonato)phosphate, lithium monofluorophosphate, sodium monofluorophosphate, lithium bis(difluorophosphoryl)imide, sodium bis(difluorophosphoryl)imide, lithium (difluorophosphoryl)(fluorosulfonyl)imide, (difluorophosphoryl)(fluoro) sulfonyl)imide sodium, bis(trifluoromethanesulfonyl)imide lithium, bis(trifluoromethanesulfonyl)imide sodium, bis(pentafluoroethanesulfonyl)imide lithium, bis(pentafluoroethanesulfonyl)imide sodium, (trifluoromethanesulfonyl)(pentafluoroethanesulfonyl)imide lithium, (trifluoromethanesulfonyl)(pentafluoroethanesulfonyl)imide sodium, (trifluoromethanesulfonyl)(fluorosulfonyl)imide lithium, (trifluoromethanesulfonyl)(fluorosulfonyl)imide sodium, (pentafluoroethanesulfonyl)(fluorosulfonyl)imide lithium, (pentafluoroethanesulfonyl)(fluorosulfonyl)imide sodium, tris(trifluoromethanesulfonyl)methide lithium, tris(trifluoromethanesulfonyl)methide sodium, lithium acrylate, sodium acrylate, lithium methacrylate, sodium methacrylate, lithium methyl sulfate, sodium methyl sulfate, lithium ethyl sulfate,The non-aqueous electrolyte solution according to any one of claims 1 to 21, comprising at least one selected from the group consisting of sodium ethyl sulfate and sodium ethyl sulfate.
23. In addition, cyclohexylbenzene, cyclohexylfluorobenzene, biphenyl, 2-fluorobiphenyl, t-butylbenzene, t-amylbenzene, 2-fluorotoluene, fluorobenzene, vinylene carbonate, vinylene carbonate oligomers (number average molecular weight in terms of polystyrene: 170 to 5000), vinylethylene carbonate, difluoroanisole, fluoroethylene carbonate, 1,6-diisocyanatohexane, ethynylethylene carbonate, trans-difluoroethylene carbonate, methylpropargyl carbonate, ethylpropargyl carbonate, dipropargyl carbonate, maleic anhydride, succinic anhydride, 1,3-propane sultone, 1,3-propene sultone, 1,4-butane sultone, dimethylvinylene carbonate, 1,3,2-dioxathione, 1,3-propane ... Oran-2,2-dioxide, 4-propyl-1,3,2-dioxathiolane-2,2-dioxide, methylenemethane disulfonate, dimethylenemethane disulfonate, trimethylenemethane disulfonate, methyl methanesulfonate, methanesulfonyl fluoride, ethenesulfonyl fluoride, phenyl difluorophosphate, 1,2-ethanedisulfonic anhydride, tris(trimethylsilyl)borate, succinonitrile, (ethoxy)pentafluorocyclotriphosphazene, tetrafluoro(picolinato)phosphate, difluoro(picolinato)borate, and 1,3-dimethyl-1,3-divinyl-1,3-di(1,1,1,3,3,3-hexafluoroisopropyl)disiloxane. The nonaqueous electrolyte according to any one of claims 1 to 22, containing at least one selected from the group consisting of disiloxane.
24. A nonaqueous electrolyte secondary battery comprising: a negative electrode containing Si and / or silicon oxide as a negative electrode active material; a positive electrode; and the nonaqueous electrolyte according to any one of claims 1 to 23.
25. The nonaqueous electrolyte secondary battery according to claim 24, wherein the negative electrode active material further contains graphite.
Citation Information
Patent Citations
Organic electrolyte solution of 3,3,9,9-tetraoxide-2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane for use in a lithium battery
EP3205655A1
Method for vulcanizing green tire
JP1993104541A
Production of silicon compound
JP2000143677A
Method for producing vinylsilane
JP2004256494A
Positive electrode material for lithium ion battery
JP2008270201A
Cited By
Non-aqueous electrolyte and sodium ion battery containing same
CN120376752A