High-density compression-molded bonded samarium-iron-nitrogen magnet having extremely low void volume fraction, and preparation method therefor
By employing vacuum overflow molding and rapid high-pressure molding technology, the void problem in samarium iron nitrogen magnets has been solved, improving magnet density and magnetic properties, achieving efficient utilization of rare earth resources, and making it suitable for high-performance miniaturized electrical appliances and motors.
Patent Information
- Application Number
- PCT/CN2025/108051
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-07
- Filing Date
- 2025-07-11
- Publication Date
- 2026-11-12
AI Technical Summary
In the existing molding and bonding process of samarium iron nitride magnets, the bridging effect between samarium iron nitride magnetic powder particles results in a large number of tiny voids in the magnet, leading to low density and limiting the improvement of its magnetic properties.
By employing vacuum resin compression molding technology and rapid high-pressure compression molding technology, high-temperature liquefied resin is used to fill the voids with a binder that has good fluidity under vacuum, and combined with rapid high-pressure compression molding, the void ratio of the magnet is significantly reduced and the density is improved.
It significantly improves the density and magnetic properties of samarium iron nitrogen magnets, increases rare earth utilization efficiency, avoids material decomposition at high temperatures, and enhances the weather resistance and economic value of the product.
Smart Images

Figure PCTCN2025108051-APPB-I100001 
Figure PCTCN2025108051-APPB-I100002 
Figure PCTCN2025108051-APPB-I100003
Abstract
Description
A high-density molded bonded samarium iron nitrogen magnet with extremely low void volume ratio and its preparation method Technical Field
[0001] This invention belongs to the field of magnet technology, specifically relating to a high-density molded bonded samarium iron nitride magnet with an extremely low void volume ratio and its preparation method. Background Technology
[0002] The field of magnetic materials includes two categories: sintered magnets and bonded magnets. With the continuous development of consumer electronics, especially the trend of miniaturization, lightweighting, and high performance in electrical appliances and motors, the market demand for bonded magnets is increasing. Technical issues
[0003] Samarium iron nitride (SMR) magnets possess high magnetocrystalline anisotropy and Curie temperature, and relatively low rare-earth content, making them a promising new type of rare-earth permanent magnet material. However, SMR is prone to decomposition at high temperatures, preventing its fabrication using traditional high-temperature sintering processes. Low-temperature molding processes are typically employed. These processes generally involve compression molding, injection molding, and calendering. Existing compression-bonded SMR magnet fabrication methods often utilize conventional pressure molding, which, due to powder friction loss, struggles to achieve high-density magnets. Furthermore, the inability to sinter later leads to bridging effects between magnetic powder particles, resulting in numerous micro-voids within the magnet, forming magnetoresistance regions and limiting further improvement in magnetic properties. As shown in Table 1, taking a common compression-molded SMR magnet with 2.4% resin by mass as an example, based on volume density calculations, under conventional fabrication conditions, the volume percentage of voids in the compression-molded SMR magnet is as high as 8% or more; its isotropic sample column has a measured density of 5.96 g / cm³. 3 Under certain conditions, its maximum magnetic energy product BHmax is only about 7.0, which greatly restricts the performance of molded bonded samarium iron nitrogen magnets, preventing them from achieving large-scale market application to this day.
[0004] Table 1. Volume calculation of each component after pressing 100 grams of clinker with a resin content of 2.4% into magnets.
[0005]
[0006] Therefore, how to solve the bridging effect between samarium iron nitride magnetic powder particles in the preparation of molded bonded samarium iron nitride magnets, which leads to a large number of tiny voids between particles in the magnet and thus results in low density of the molded bonded samarium iron nitride magnets, has become the main problem-solving direction of this invention. Technical solutions
[0007] To address the problems existing in the background technology, this invention provides a high-density molded bonded samarium iron nitride magnet with an extremely low void volume ratio and its preparation method. Through vacuum overflow molding, the excellent fluidity of the high-temperature liquefied resin, exhibited by a lower boiling point under vacuum, is utilized to effectively fill the voids within the magnet and allow excess resin to overflow from the contact points between magnetic powder particles. Combined with rapid high-pressure molding technology, the void ratio of the magnet is significantly reduced, thereby significantly improving the density of the samarium iron nitride magnet and ultimately achieving a significant improvement in the magnetic properties of the magnet. This invention, employing a molding method, greatly improves the rare earth utilization efficiency in the preparation process of samarium iron nitride magnets, achieving extremely high economic and social value.
[0008] To achieve the above objectives, the present invention provides a method for preparing a high-density molded bonded samarium iron nitrogen magnet with an extremely low void volume ratio.
[0009] This invention is achieved through the following technical solution:
[0010] In the first aspect, the raw materials of the samarium iron nitride magnet, by mass percentage, include: 0.5%-20% wt% binder, 0.05%-2% wt% lubricant, and the balance being one or more of samarium iron nitride magnetic powder, samarium iron nitride mixed magnetic powder, or samarium iron nitride surface modified magnetic powder.
[0011] The preparation method includes the following steps:
[0012] S1. Dissolve the binder with an organic solvent to obtain an organic binder solution; S2. Mix samarium iron nitride magnetic powder or a mixture of samarium iron nitride magnetic powder and the organic binder solution evenly to form a mixture. After the solvent evaporates and the mixture dries, crush it to 40-300 mesh to obtain a mixture; S3. Add a lubricant to the mixture and mix evenly to obtain clinker suitable for pressing; S4. Preheat the pressing mold, and at the same time preheat the clinker to 20-120℃ to fully soften the clinker. Fill the clinker into the preheated pressing mold cavity; S5. Close the mold and press under pressure, with a pressing force of 6-50 T / cm. 2 The pressing and holding time is 0.3 seconds to 150 seconds. At the same time, the mold cavity is evacuated to remove the air between the powder particles. As the air between the particles is extracted, the liquefied binder in the preheated clinker fills the original air gaps under pressure to form a dense structure. After the holding pressure is completed, the vacuum state of the mold cavity is ended and the mold is demolded to obtain the magnet blank. After the magnet blank is cured in a stepped manner, it is machined, coated and magnetized to obtain a high-density molded bonded samarium iron nitride magnet with an extremely low void volume ratio.
[0013] Furthermore, to modify properties such as temperature resistance and coercivity, the samarium iron nitrogen magnetic powder is samarium iron nitrogen magnetic powder and its modified magnetic powder containing one or more of the elements cobalt, praseodymium, neodymium, dysprosium, terbium, lanthanum, cerium, and zirconium, or samarium iron nitrogen magnetic powder and its mixed magnetic powder containing one or more of the elements neodymium iron boron powder, ferrite powder, samarium cobalt powder, iron triboron powder, and aluminum nickel cobalt powder.
[0014] Furthermore, the samarium iron nitrogen (SFI) surface-modified magnetic powder is prepared by surface modification treatment of SFI magnetic powder or a mixture of SFI magnetic powder and SFI magnetic powder: Step 1, dissolving a titanate or silane coupling agent in anhydrous ethanol or acetone to form a treatment solution; Step 2, mixing the treatment solution and magnetic powder at a mass ratio of 0.1-10:100 and stirring at 40-60℃ for 5-60 minutes; Step 3, vacuum drying to remove the solvent, forming a dense coupling agent coating layer, thus obtaining the SFI surface-modified magnetic powder.
[0015] Furthermore, the binder is one or more thermoplastic resins selected from polyamide, polyether, polyolefin, polyester, and polyaldehyde, or one or more thermosetting resins selected from phenolic resin and epoxy resin, used to bond and mold magnetic powder to form a magnet with a certain mechanical strength.
[0016] Furthermore, the lubricant is one or more of calcium stearate, zinc stearate, graphite, and molybdenum disulfide, used in the pressing process of magnetic powder clinker to reduce the friction between magnetic powder particles and between magnetic powder particles and the mold.
[0017] Furthermore, in step S1, the organic solvent is one or more of acetone, ethyl acetate, and anhydrous ethanol.
[0018] Furthermore, in step S4, due to the effect of preheating, the clinker agglomerates cannot be filled into the mold cavity of the pressing mold by ordinary powder filling method. Therefore, it is necessary to inject the clinker into the mold cavity of the pressing mold by pressure injection.
[0019] Furthermore, in step S5, if the adhesive is a thermosetting resin, the preheating temperature of the preheating mold is 120-200℃; or if the adhesive is a thermoplastic resin, the preheating temperature of the preheating mold is 120-300℃.
[0020] Furthermore, in step S5, when the adhesive is a thermosetting resin as the main adhesive type, and when a void ratio of less than 0.1% is required, a vacuum pressing holding time of 20-240 minutes can be selected.
[0021] Furthermore, the pressing mold includes a mold temperature control system and a mold cavity vacuum control system.
[0022] Furthermore, when the binder in step S7 is a thermosetting resin, the step-by-step curing treatment method for the magnet green blank is as follows: first, heat to 60-80℃ and hold for 5-120 minutes to eliminate most of the pressing stress while the product temperature deformation is small; then heat to 120-200℃ and hold for 5-240 minutes until cured.
[0023] Furthermore, the magnet green blank undergoes a continuous, stepped curing process.
[0024] Furthermore, in step S7, after the product is demolded, the processing method can be selected from one or more of the following: machining, electrical discharge machining, chemical processing, and laser processing to improve the dimensional accuracy of the product, including but not limited to turning, grinding, wire cutting, electrical discharge machining, chemical etching, and laser processing.
[0025] Furthermore, step S7, the coating treatment, involves adding a protective coating using one or more methods such as electrophoretic epoxy, sprayed epoxy, zinc plating, nickel plating, chromium plating, Pyrene coating, and Dacromet coating.
[0026] Secondly, the present invention provides a high-density molded bonded samarium iron nitride magnet with extremely low void volume ratio prepared by the above preparation method, wherein the samarium iron nitride magnet has a density of 6.0-7.2 g / cm³ and the void volume ratio of the magnet is less than 3%. Beneficial effects
[0027] This application has the following beneficial effects:
[0028] 1. Vacuum overflow molding utilizes the excellent fluidity of the liquefied adhesive resin under vacuum conditions, which exhibits a lower boiling point, to effectively fill the voids within the magnet. Excess resin overflows from the contact points between magnetic powder particles, significantly reducing the void ratio of the magnet. This, in turn, significantly increases the density of the samarium iron nitride magnet under the same pressure conditions and reduces the degree of magnetic powder particle breakage, ultimately resulting in a significant improvement in the magnetic properties of the magnet.
[0029] 2. When the binder content in the raw materials of samarium iron nitride magnets is less than 1 wt% by mass, the powder bridging effect becomes more pronounced. To overcome this bridging effect, this technical solution employs ultra-high pressure rapid prototyping technology combined with vacuum overflow molding technology. This effectively overcomes the powder bridging effect under these conditions, significantly shortens the distance between microparticles in the bonded magnet, effectively increases the magnetization effect of the microparticles and the interaction force after magnetization, and significantly improves the density of the magnet to 7.2 g / cm³. 3 This achieves the goal of significantly improving the magnetic properties of the magnet.
[0030] 3. The preparation method of the present invention is simple and efficient, and can achieve magnet forming at a lower temperature, avoiding the decomposition of samarium iron nitrogen material at high temperature.
[0031] 4. Surface treatment of samarium iron nitrogen magnetic powder yields secondary modified magnetic powder and a dense coupling agent coating layer, which improves the oxidation resistance of the samarium iron nitrogen magnetic powder and reduces magnetic property loss.
[0032] 5. Using samarium iron nitrogen magnetic powder as the magnetic phase, the product's weather resistance is significantly stronger than that of molded bonded neodymium iron boron products with equivalent performance.
[0033] 6. Compared with other injection molding and calendering methods, the use of compression molding greatly improves the rare earth utilization efficiency in the preparation process of samarium iron nitride magnets, achieving extremely high economic and social value. Embodiments of the present invention
[0034] The embodiments of the present invention will be described in detail below with reference to the examples. However, those skilled in the art will understand that the following examples are only for illustrating the present invention and should not be regarded as limiting the scope of the present invention. Specific conditions not specified in the examples shall be carried out according to conventional conditions or conditions recommended by the manufacturer. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially. Example 1:
[0035] This embodiment provides a method for preparing a high-density molded bonded samarium iron nitride magnet with extremely low void volume ratio obtained by the above preparation method, including the following steps:
[0036] The raw materials, by mass percentage, for a method of preparing a high-density molded bonded samarium iron nitride magnet with extremely low void volume ratio include: 2.4% wt% epoxy thermosetting resin as binder and 0.25% lubricant. wt%, the balance being one or more of samarium iron nitrogen magnetic powder or samarium iron nitrogen surface-modified magnetic powder; it should be noted that if the magnet product is used in a heavily corrosion-resistant environment, the samarium iron nitrogen magnetic powder used to modify the temperature resistance, corrosion resistance, coercivity, etc. can be samarium iron nitrogen magnetic powder and its modified magnetic powder containing one or more of cobalt, praseodymium, neodymium, dysprosium, terbium, lanthanum, cerium, zirconium, or a mixed magnetic powder containing one or more of neodymium iron boron powder, ferrite powder, samarium cobalt powder, iron triboron powder, and aluminum nickel cobalt powder. Otherwise, samarium iron nitrogen magnetic powder is used. However, for better explanation of the technical characteristics of this technical solution, we choose commercially available samarium iron nitrogen magnetic powder here.
[0037] The preparation method includes the following steps:
[0038] S1. Magnetic powder modification: Samarium iron nitrogen magnetic powder is surface treated to obtain surface-modified Samarium iron nitrogen magnetic powder;
[0039] The surface treatment method is as follows: Step 1: Dissolve the titanate coupling agent in anhydrous ethanol to form a treatment solution; Step 2: Mix the treatment solution with magnetic powder at a mass ratio of 5:100 and stir, then treat at 40℃ for 5 minutes; Step 3: Vacuum dry to remove the solvent, forming a dense coupling agent coating layer.
[0040] S2. Preparation of Clinker: Step 1: Dissolve the binder epoxy thermosetting resin in the organic solvent acetone to obtain an organic solution of the binder epoxy thermosetting resin; Step 2: Mix the samarium iron nitrogen surface-modified magnetic powder with the binder epoxy thermosetting resin organic solution to form a mixture. After the solvent evaporates and the mixture is dried, crush it to 250 mesh to obtain a mixture; Step 3: Add the mixture to the lubricant calcium stearate and mix evenly to obtain clinker suitable for pressing;
[0041] S3. Clinker Vacuum Overflow Molding: Precisely operated with the cooperation of a mold temperature control system and a mold cavity vacuum control system. The mold is preheated to 120°C, and the clinker is simultaneously preheated to 120°C to fully soften it. The clinker is then injected into the preheated mold cavity using pressure injection. The mold is then closed, pressed, and held under pressure at a pressure of 17T / cm. 2 The pressing and holding time is 10 seconds. At the same time, the mold cavity is evacuated to remove the air between the powder particles. As the air between the particles is extracted, the liquefied binder in the preheated clinker fills the original air gaps under pressure to form a dense structure. After the pressing is completed, the vacuum state of the mold cavity is ended and the mold is demolded to obtain the magnet blank.
[0042] S4. Curing treatment of thermosetting adhesive magnet blanks: First, heat to 60℃ and hold for 30 minutes. Under the condition that the product temperature deformation is small, most of the pressing stress is eliminated. Then, heat to 160℃ and hold for 100 minutes until fully cured to form a magnet blank. If the magnet product has a complex shape or large size and has high product precision requirements, the magnet blank can be cured in stages multiple times to reduce the deformation caused by later thermal stress from affecting dimensional accuracy.
[0043] S5. Blank processing and corrosion protection: The magnet blank is machined to improve the dimensional accuracy of the product, then electrophoretic epoxy is used for corrosion protection, and finally magnetized and packaged to obtain a high-density molded bonded samarium iron nitrogen magnet. Example 2:
[0044] The difference between this embodiment and Embodiment 1 lies in reducing the surface modification steps of the samarium iron nitride magnetic powder: This embodiment provides a method for preparing a high-density molded bonded samarium iron nitride magnet with an extremely low void volume ratio, comprising the following steps:
[0045] The raw materials for a method of preparing a high-density molded bonded samarium iron nitride magnet with extremely low void volume ratio include, by mass percentage: 2.4% wt% binder of thermosetting epoxy resin, 0.25% wt% lubricant, and the balance being samarium iron nitride magnetic powder or samarium iron nitride mixed modified magnetic powder; it should be noted that if the magnet product is used in a heavily corrosion-resistant environment, samarium iron nitride mixed modified magnetic powder can be used, otherwise samarium iron nitride magnetic powder is used.
[0046] The preparation method includes the following steps:
[0047] S1. Preparation of Clinker: Step 1: Dissolve the thermoplastic binder resin in the organic solvent acetone to obtain an organic solution of the thermoplastic binder resin; Step 2: Mix the samarium iron nitrogen magnetic powder with the organic solution of the thermosetting binder resin evenly to form a mixture. After the solvent evaporates and the mixture is dried, crush it to 250 mesh to obtain a mixture; Step 3: Add the mixture to the lubricant calcium stearate and mix evenly to obtain a clinker suitable for pressing;
[0048] S2. Clinker Vacuum Overflow Molding: Precisely operated with the cooperation of a mold temperature control system and a mold cavity vacuum control system, the pressing mold is preheated to 120℃, and the clinker is simultaneously preheated to 120℃ to fully soften it. The clinker is then injected into the preheated pressing mold cavity using pressure injection. The mold is then closed, pressed, and held under pressure at a pressure of 17T / cm. 2 The pressing and holding time is 10 seconds. At the same time, the mold cavity is evacuated to remove the air between the powder particles. As the air between the particles is extracted, the liquefied binder in the preheated clinker fills the original air gaps under pressure to form a dense structure. After the pressing is completed, the vacuum state of the mold cavity is ended and the demolding process is carried out to obtain the magnet blank.
[0049] S3. Curing treatment of magnet blanks: First, heat to 60℃ and hold for 30 minutes. Under the condition that the product temperature deformation is small, most of the pressing stress is eliminated. Then heat to 160℃ and hold for 100 minutes until cured to form a magnet blank. If the magnet product has a complex shape or large size and has high product precision requirements, the magnet blank can be cured in stages multiple times to reduce the deformation caused by thermal stress in the later stage and affect the dimensional accuracy.
[0050] S4. Blank processing and corrosion protection: The magnet blank is machined to improve the dimensional accuracy of the product, then electrophoretic epoxy is used for corrosion protection, and finally magnetized and packaged to obtain a high-density molded bonded samarium iron nitrogen magnet.
[0051] Comparative Example 1:
[0052] The difference between this comparative example and Example 1 lies in reducing the vacuum grease-filling molding and preheating steps of the clinker and mold in the vacuum grease-filling molding process: a method for preparing a high-density molded bonded samarium iron nitrogen magnet with an extremely low void volume ratio is provided, comprising the following steps:
[0053] The raw materials for a method of preparing a high-density molded bonded samarium iron nitride magnet with extremely low void volume ratio include, by mass percentage: 2.4% wt% binder of thermosetting epoxy resin, 0.25% wt% lubricant, and the balance being samarium iron nitride magnetic powder or samarium iron nitride mixed modified magnetic powder; it should be noted that if the magnet product is used in a heavily corrosion-resistant environment, samarium iron nitride mixed modified magnetic powder can be used, otherwise samarium iron nitride magnetic powder is used.
[0054] The preparation method includes the following steps:
[0055] S1. Magnetic powder modification: Samarium iron nitrogen magnetic powder is surface treated to obtain surface-modified Samarium iron nitrogen magnetic powder;
[0056] The surface treatment method is as follows: Step 1: Dissolve the titanate coupling agent in anhydrous ethanol to form a treatment solution; Step 2: Mix the treatment solution with magnetic powder at a mass ratio of 5:100 and stir, then treat at 40℃ for 5 minutes; Step 3: Vacuum dry to remove the solvent, forming a dense coupling agent coating layer.
[0057] S2. Preparation of Clinker: Step 1: Dissolve the thermosetting resin of the binder in the organic solvent acetone to obtain an organic solution of thermoplastic resin of the binder; Step 2: Mix the surface-treated samarium iron nitrogen surface-modified magnetic powder with the organic solution of thermoplastic resin of the binder to form a mixture. After the solvent evaporates and the mixture is dried, crush it to 250 mesh to obtain a mixture; Step 3: Add the mixture to the lubricant calcium stearate and mix evenly to obtain a clinker suitable for pressing;
[0058] S3. Clinker Molding: The clinker is loaded into the mold cavity of the pressing die; the die is closed, pressed, and held under pressure at a pressure of 17T / cm. 2 The pressing and holding time is 10 seconds, and then the demolding process is carried out to obtain the magnet blank;
[0059] S4. Curing treatment of magnet blanks: First, heat to 60℃ and hold for 30 minutes. Under the condition that the product temperature deformation is small, most of the pressing stress is eliminated. Then, heat to 120℃ and hold for 100 minutes until cured to form a magnet blank. If the magnet product has a complex shape or large size and has high product precision requirements, the magnet blank can be cured in stages multiple times to reduce the deformation caused by thermal stress in the later stage and affect the dimensional accuracy.
[0060] S5. Blank processing and corrosion protection: The magnet blank is machined to improve the dimensional accuracy of the product, then electrophoretic epoxy is used for corrosion protection, and finally magnetized and packaged to obtain a high-density molded bonded samarium iron nitrogen magnet.
[0061] Comparative Example 2:
[0062] The difference between this comparative example and Example 1 lies in reducing the vacuum pressing and preheating of the clinker under vacuum conditions in the vacuum grease filling process of clinker vacuum grease filling molding: a method for preparing a high-density molded bonded samarium iron nitrogen magnet with an extremely low void volume ratio is provided, comprising the following steps:
[0063] The raw materials for a method of preparing a high-density molded bonded samarium iron nitride magnet with extremely low void volume ratio include, by mass percentage: 2.4% wt% binder of thermoplastic polyamide resin, 0.25% wt% lubricant, and the balance being samarium iron nitride magnetic powder or samarium iron nitride mixed modified magnetic powder; it should be noted that if the magnet product is used in a heavily corrosion-resistant environment, samarium iron nitride mixed modified magnetic powder can be used, otherwise samarium iron nitride magnetic powder is used.
[0064] The preparation method includes the following steps:
[0065] S1. Magnetic powder modification: Samarium iron nitrogen magnetic powder is surface treated to obtain surface-modified Samarium iron nitrogen magnetic powder;
[0066] The surface treatment method is as follows: Step 1, dissolve the titanate coupling agent in anhydrous ethanol to form a treatment solution; Step 2, mix the treatment solution with magnetic powder at a mass ratio of 5:100 and stir, then treat at 40℃ for 5 minutes; Step 3, vacuum dry to remove the solvent, forming a dense coupling agent coating layer.
[0067] S2. Preparation of Clinker: Step 1: Dissolve the thermoplastic binder resin in the organic solvent acetone to obtain an organic solution of the thermoplastic binder resin; Step 2: Mix the surface-treated samarium iron nitrogen surface-modified magnetic powder with the organic solution of the thermoplastic binder resin to form a mixture. After the solvent evaporates and the mixture is dried, crush it to 250 mesh to obtain a mixture; Step 3: Add the mixture to the lubricant calcium stearate and mix evenly to obtain a clinker suitable for pressing;
[0068] S3. Clinker Molding: Preheat the pressing mold to 120℃, then fill the mold cavity with clinker; close the mold and press and hold the pressure, with a pressing force of 17T / cm. 2 The pressing and holding time is 10 seconds; after the pressing is completed, the magnet blank is demolded to obtain the magnet blank.
[0069] S4. Curing treatment of magnet blanks: First, heat to 60℃ and hold for 30 minutes. Under the condition that the product temperature deformation is small, most of the pressing stress is eliminated. Then, heat to 120℃ and hold for 100 minutes until cured to form a magnet blank. If the magnet product has a complex shape or large size and has high product precision requirements, the magnet blank can be cured in stages multiple times to reduce the deformation caused by thermal stress in the later stage and affect the dimensional accuracy.
[0070] S5. Blank processing and corrosion protection: The magnet blank is machined to improve the dimensional accuracy of the product, then electrophoretic epoxy is used for corrosion protection, and finally magnetized and packaged to obtain a high-density molded bonded samarium iron nitrogen magnet.
[0071] Proof of effectiveness:
[0072] For Examples 1-2 and Comparative Examples 1-2, 100 grams of clinker were selected and pressed into magnets. The volumes of each component were calculated, and the performance of the magnets was tested. Results: See Table 2.
[0073] Table 2. Calculation of the volume and performance of each component of the magnets prepared in Examples 1-2 and Comparative Examples 1-2 of the present invention.
[0074]
[0075] To demonstrate that the high-density, high-density molded bonded samarium iron nitride magnet preparation method with extremely low void volume ratio provided in this application possesses both high density and magnetic properties, the following experiments were conducted.
[0076] Experimental Example 1
[0077] The effect of preheating temperature on the properties of samarium iron nitrogen magnets in vacuum grease molding:
[0078] Following the temperature changes for clinker preheating and mold preheating as recorded in Table 3, samarium iron nitride magnets were prepared using the preparation method of Example 1. The volume of each component of the prepared magnets and their performance were measured and calculated. The results are shown in Table 3.
[0079] Table 3. Effects of clinker preheating and mold preheating temperatures on the volume and properties of each component in a 100g magnet.
[0080]
[0081] Experimental Example 2
[0082] The effect of unit pressing force on the performance of samarium iron nitride magnets in vacuum grease fitting molding:
[0083] According to the changes in unit pressing force of clinker recorded in Table 4, the preparation method of Example 1 was adopted. Due to the grease overflow phenomenon that occurred under high pressure due to the 2.4% mass percentage of binder content, in order to further understand the changes in magnet performance under effective binder composition, the binder content was further reduced to 1.0% mass percentage in this experiment. This is because the lower the binder content, the more obvious the powder bridging effect, and the more severe the voids in the magnet caused by the bridging effect. Then, samarium iron nitride magnets were prepared by increasing the unit pressing force and combining vacuum grease overflow molding. The volume of each component of the prepared magnet and the performance calculation were measured. The results are shown in Table 4.
[0084] Table 4. Effect of unit pressing force on the volume and properties of each component of the magnet
[0085]
[0086] Experimental Example 3
[0087] The effect of unit pressing and holding time on the performance of samarium iron nitrogen magnets during vacuum grease injection molding:
[0088] Following the changes in unit pressing force of clinker as recorded in Table 5, samarium iron nitride magnets were prepared using the preparation method of Example 1. The volume of each component of the prepared magnets and the performance calculations were performed. The results are shown in Table 5.
[0089] Table 5. Effects of holding time on the volume and properties of various components of the magnet
[0090]
[0091] Results Analysis
[0092] Analysis of Examples 1-2 and Comparative Examples 1-2, and conclusions in Table 2, show that the samarium iron nitride magnet material prepared by the high-density molded bonded samarium iron nitride magnet with extremely low void volume ratio provided by the present invention, under conventional pressure molding conditions, utilizes vacuum overflow molding technology. This technology leverages the excellent fluidity of the high-temperature liquefied binder resin, which exhibits a lower boiling point under vacuum, to effectively fill voids within the magnet. Excess resin overflows from the contact points between magnetic powder particles, significantly reducing the magnet void ratio to below 3%. This significantly improves the density of the samarium iron nitride magnet under the same pressure conditions, ultimately achieving a significant improvement in the magnet's magnetic properties.
[0093] Table 3 further clarifies that by controlling and changing the temperature of the preheating pressing mold and the preheated clinker, the vacuum overflow molding technology can effectively fill the voids in the magnet by liquefying the adhesive resin at high temperature, thus solving the problem of the magnet void ratio.
[0094] As shown in Table 4, when the binder content in the raw materials of the samarium iron nitride magnet is less than 1 wt%, the powder bridging effect is more pronounced. To overcome this bridging effect, the solution employs ultra-high pressure rapid prototyping technology combined with the vacuum overflow molding technology in Example 1. This effectively overcomes the powder bridging effect under these conditions, significantly shortens the distance between microparticles in the bonded magnet, effectively increases the magnetization effect of the microparticles and the interaction force after magnetization, and significantly improves the density of the magnet to 7.0 g / cm³. 3, The magnet coercivity can reach 12.653 KOe. If the proportion of adhesive is further reduced to 0.5-0.8 wt% and the unit compressive force is increased to 50 T / cm, the coercivity can be further improved. 2 The density of the magnet can reach 7.2 g / cm³. 3 The magnet coercivity can reach 13.529 KOe.
[0095] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not describe the various possible combinations separately.
[0096] Furthermore, various different embodiments of the present invention can be combined in any way, as long as they do not violate the spirit of the present invention, they should also be regarded as the content disclosed by the present invention.
Claims
1. A method for preparing a high-density molded bonded samarium iron nitride magnet with extremely low void volume ratio, characterized in that, The raw materials of the samarium iron nitride magnet, by mass percentage, include: 0.5%-20% wt% binder, 0.05%-2% wt% lubricant, and the balance being one or more of samarium iron nitride magnetic powder, samarium iron nitride mixed magnetic powder, or samarium iron nitride surface modified magnetic powder; The preparation method includes the following steps: S1. Dissolve the binder with an organic solvent to obtain an organic binder solution; S2. Mix samarium iron nitride magnetic powder or a mixture of samarium iron nitride magnetic powder and the organic binder solution evenly to form a mixture. After the solvent evaporates and the mixture dries, crush it to 40-300 mesh to obtain a mixture; S3. Add a lubricant to the mixture and mix evenly to obtain clinker suitable for pressing; S4. Preheat the pressing mold, and at the same time preheat the clinker to 20-120℃ to fully soften the clinker. Fill the clinker into the preheated pressing mold cavity; S5. Close the mold and press under pressure, with a pressing force of 6-50 T / cm. 2 The pressing and holding time is 0.3 seconds to 150 seconds. At the same time, the mold cavity is evacuated to remove the air between the powder particles. As the air between the particles is extracted, the liquefied binder in the preheated clinker fills the original air gaps under pressure to form a dense structure. S6. After the holding pressure is completed, the vacuum state of the mold cavity is ended and the mold is demolded to obtain the magnet blank. S7. After the magnet blank is cured in a stepped manner, it is machined, coated and magnetized to obtain a high-density molded bonded samarium iron nitride magnet with an extremely low void volume ratio. The internal void volume of the magnet blank accounts for less than 3%.
2. The method for preparing a high-density molded bonded samarium iron nitride magnet with extremely low void volume ratio according to claim 1, characterized in that, The samarium iron nitrogen magnetic powder is samarium iron nitrogen magnetic powder and its modified magnetic powder containing one or more of the elements cobalt, praseodymium, neodymium, dysprosium, terbium, lanthanum, cerium, and zirconium, or samarium iron nitrogen magnetic powder and its mixed magnetic powder containing one or more of the elements neodymium iron boron powder, ferrite powder, samarium cobalt powder, iron triboron powder, and aluminum nickel cobalt powder.
3. The method for preparing a high-density molded bonded samarium iron nitride magnet with extremely low void volume ratio according to claim 1, characterized in that, The samarium iron nitrogen surface-modified magnetic powder is obtained by surface modification treatment of samarium iron nitrogen magnetic powder or samarium iron nitrogen mixed magnetic powder: Step 1, dissolve titanate or silane coupling agent in anhydrous ethanol or acetone to form a treatment solution; Step 2, mix the treatment solution and magnetic powder at a mass ratio of 0.1-10:100 and stir at 40-60℃ for 5-60 minutes; Step 3, vacuum dry to remove solvent, form a dense coupling agent coating layer, and obtain samarium iron nitrogen surface-modified magnetic powder.
4. The method for preparing a high-density molded bonded samarium iron nitride magnet with extremely low void volume ratio according to claim 1, characterized in that, The binder is one or more thermoplastic resins selected from polyamide, polyether, polyolefin, polyester, and polyaldehyde, or the binder is one or more thermosetting resins selected from phenolic resin and epoxy resin.
5. The method for preparing a high-density molded bonded samarium iron nitride magnet with extremely low void volume ratio according to claim 1, characterized in that, The lubricant is one or more of calcium stearate, zinc stearate, graphite, and molybdenum disulfide.
6. The method for preparing a high-density molded bonded samarium iron nitride magnet with extremely low void volume ratio according to claim 1, characterized in that, In step S1, the organic solvent is one or more of acetone, ethyl acetate, and anhydrous ethanol.
7. The method for preparing a high-density molded bonded samarium iron nitride magnet with extremely low void volume ratio according to claim 1 or 2, characterized in that, The preheating temperature of the preheating pressing mold in step S4 is 120-200℃ if the adhesive is a thermosetting resin or 120-300℃ if the adhesive is a thermoplastic resin.
8. The method for preparing a high-density molded bonded samarium iron nitride magnet with extremely low void volume ratio according to claim 1, characterized in that, The step-by-step curing method for the magnet green blank in step S7 is as follows: first, heat to 60-80℃ and hold for 5-120 minutes, then heat to 120-250℃ and hold for 5-240 minutes until cured.
9. The method for preparing a high-density molded bonded samarium iron nitride magnet with extremely low void volume ratio according to claim 1, characterized in that, The magnet green blank undergoes a repeated, stepped curing process.
10. A high-density molded bonded samarium iron nitride magnet with extremely low void volume ratio prepared by the preparation method according to any one of claims 1-10, characterized in that, The density of the samarium iron nitrogen magnet is 6.0-7.2 g / cm³. 3 The internal cavity volume of the samarium iron nitrogen magnet is less than 3%; The samarium iron nitrogen magnet also includes a surface protective coating, which can be one or more of the following: epoxy coating, sprayed epoxy coating, zinc plating, nickel plating, chromium plating, Pyrelin coating, and Dacromet coating.