Heterojunction cell and manufacturing method therefor

By introducing a protective layer to cover the electroplated electrodes in a heterojunction cell, the efficiency loss caused by wet chemical treatment is solved, the conversion efficiency of the cell is improved and the metallization cost is reduced, and higher optical utilization and cell performance are achieved.

WO2026232700A1PCT designated stage Publication Date: 2026-11-12TRINA SOLAR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/109144
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2025-07-17
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

The efficiency loss caused by wet chemical treatment during the metallization process of existing heterojunction solar cells affects the conversion efficiency and performance of the cells.

Method used

The design employs a protective layer covering the electroplated electrode. By placing a protective layer between the transparent conductive layer and the doped layer, wet corrosion is avoided. This is combined with the electroplating process to form the electrode, reducing the number of wet processing steps.

Benefits of technology

It improves battery conversion efficiency, reduces metallization costs, minimizes optical utilization loss, and enhances overall battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2025109144_12112026_PF_FP_ABST
    Figure CN2025109144_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to a heterojunction cell and a manufacturing method therefor, and a photovoltaic module. The heterojunction cell comprises: a substrate; a first intrinsic silicon layer and a first doped layer sequentially stacked on a first surface of the substrate; a first transparent conductive layer and a protective layer stacked on the side of the first doped layer facing away from the substrate, wherein the first transparent conductive layer covers a portion of the first surface, and the protective layer completely covers the first surface; and a first electroplated electrode located on the side of the protective layer facing away from the substrate, and electrically connected to the first transparent conductive layer, wherein the first surface comprises an isolation region not covered by the first transparent conductive layer; and a partial structure of the protective layer is stacked on the portion of the first doped layer corresponding to the isolation region.
Need to check novelty before this filing date? Find Prior Art

Description

Heterojunction solar cells and their fabrication methods

[0001] Related applications

[0002] This application claims priority to Chinese patent application filed on May 9, 2025, with application number 202510596712.2, entitled "Heterojunction Cell and Method of Fabrication Thereof, Photovoltaic Module", the entire contents of which are incorporated herein by reference. Technical Field

[0003] This application relates to the field of solar cell technology, and in particular to a heterojunction solar cell and its fabrication method. Background Technology

[0004] In recent years, with the rapid development of the photovoltaic industry, both domestic and international markets have placed increasingly higher demands on the conversion efficiency and performance of solar cells and photovoltaic modules. This has driven industry manufacturers to actively research new cell and module structures and related processes. Heterojunction (HJT) cells have advantages such as low light decay and low temperature coefficient, and can reduce energy consumption while minimizing thermal damage to the silicon substrate, making them an important direction for the future development of high-efficiency cells. In heterojunction cells of related technologies, in order to reduce metallization costs, reduce metal grid line width, improve optical utilization, and improve cell efficiency, electroplating is usually used to form electrodes. Specifically, after the TCO thin film is prepared, a seed layer is first prepared, and then a patterned mask layer electrode pattern is formed through a photolithography process. The photolithography process includes processes such as film application, exposure, and development. Then, the electrodes are prepared by electroplating. After electroplating, the mask layer and seed layer need to be etched away by wet etching. However, heterojunction cells using electroplated electrodes suffer from efficiency loss due to the need for various wet chemical treatments. Summary of the Invention

[0005] This application provides a heterojunction solar cell, including:

[0006] Substrate;

[0007] A first intrinsic silicon layer and a first doped layer are sequentially stacked on the first surface of the substrate;

[0008] A first transparent conductive layer and a protective layer are stacked on the side of the first doped layer away from the substrate. The first transparent conductive layer covers a portion of the first surface, and the protective layer completely covers the first surface.

[0009] The first electroplating electrode is located on the side of the protective layer away from the substrate and is electrically connected to the first transparent conductive layer.

[0010] The first surface includes an isolation region not covered by the first transparent conductive layer; a portion of the protective layer is stacked on the corresponding isolation region of the first doped layer.

[0011] In some embodiments, the protective layer further covers at least a portion of the side surface of the substrate, the side surface of the substrate being adjacent to the first surface.

[0012] In some embodiments, the outer contour edge of the protective layer coincides with the edge of the first surface.

[0013] In some embodiments, a first transparent conductive layer is disposed on the surface of the first doped layer away from the substrate;

[0014] The protective layer is located on the side of the first transparent conductive layer that is away from the substrate;

[0015] The first electroplating electrode is disposed on the protective layer and is electrically connected to the first transparent conductive layer through the protective layer.

[0016] In some embodiments, the outer contour edge of the protective layer coincides with the edge of the first surface;

[0017] A portion of the protective layer is stacked on the surface of the first transparent conductive layer away from the substrate, and another portion of the protective layer is stacked on the surface of the portion of the first doped layer corresponding to the isolation region.

[0018] In some embodiments, the protective layer further covers at least a portion of the side surface of the substrate, wherein the side surface of the substrate is adjacent to the first surface.

[0019] In some embodiments, the heterojunction solar cell further includes a second intrinsic silicon layer, a second doped layer and a second transparent conductive layer sequentially stacked on a second surface of the substrate, wherein the doping type of the second doped layer is opposite to that of the first doped layer, and the second surface is disposed opposite to the first surface.

[0020] The second transparent conductive layer covers at least a portion of the second surface and the side surface of the substrate, and on the side surface of the substrate, a portion of the structure of the protective layer is stacked onto the side of the second transparent conductive layer opposite to the substrate.

[0021] In some embodiments, the protective layer includes a transparent conductive oxide layer, which includes at least one of ITO, IMO, AZO, SCOT, and SnOx.

[0022] In some embodiments, the thickness of the protective layer is 5-15 nm.

[0023] In some embodiments, a protective layer is disposed on the surface of the first doped layer away from the substrate; a first transparent conductive layer is located on the side of the protective layer away from the substrate.

[0024] The first electroplating electrode is disposed on the first transparent conductive layer.

[0025] In some embodiments, the outer contour edge of the protective layer coincides with the edge of the first surface.

[0026] In some embodiments, the protective layer further covers at least a portion of the side surface of the substrate, wherein the side surface of the substrate is adjacent to the first surface.

[0027] In some embodiments, the heterojunction solar cell further includes a second intrinsic silicon layer, a second doped layer and a second transparent conductive layer sequentially stacked on a second surface of the substrate, wherein the doping type of the second doped layer is opposite to that of the first doped layer, and the second surface is disposed opposite to the first surface.

[0028] The second doped layer covers at least a portion of the second surface and side surface, the first doped layer covers at least a portion of the first surface and side surface, and on the side surface of the substrate, a portion of the structure of the first doped layer is stacked onto the side of the second doped layer opposite to the substrate.

[0029] On the side of the substrate, a protective layer is at least partially stacked on the surface of the first doped layer away from the substrate;

[0030] The second transparent conductive layer covers at least a portion of the second surface and the side surface of the substrate, and on the side surface of the substrate, a portion of the structure of the second transparent conductive layer is stacked onto the side of the protective layer opposite to the substrate.

[0031] In some embodiments, on the side of the substrate, the outer contour edge of the protective layer coincides with the outer contour edge of the first doped layer.

[0032] In some embodiments, the first doped layer includes an oxygen-free microcrystalline host layer, and the protective layer includes an oxygen-doped amorphous silicon layer.

[0033] In some embodiments, the first doped layer further includes an oxygen-containing microcrystalline sublayer, which is stacked between the first intrinsic silicon layer and the oxygen-free microcrystalline host layer.

[0034] In some embodiments, the thickness of the protective layer is no greater than 3 nm.

[0035] In some embodiments, a portion of the protective layer covering one side has a structure stacked onto the first doped layer and another portion of the structure stacked onto the second doped layer.

[0036] In some embodiments, the heterojunction solar cell further includes a second intrinsic silicon layer, a second doped layer and a second transparent conductive layer sequentially stacked on a second surface of the substrate, wherein the doping type of the second doped layer is opposite to that of the first doped layer, and the second surface is disposed opposite to the first surface.

[0037] The second transparent conductive layer covers at least a portion of the second surface and the side surface of the substrate, wherein a portion of the structure of the protective layer is stacked onto the side of the second transparent conductive layer opposite to the substrate.

[0038] In some embodiments, the protective layer comprises a transition metal oxide, and the conductivity type of the protective layer is the same as that of the first doped layer; or

[0039] The protective layer includes a dielectric passivation layer, such as a tunneling layer; or

[0040] The protective layer includes a transparent conductive oxide layer.

[0041] In some embodiments, when the protective layer comprises a transition metal oxide, the thickness of the protective layer is 5-30 nm.

[0042] In some embodiments, when the protective layer includes a dielectric passivation layer, the thickness of the protective layer is 0.5-3 nm.

[0043] In some embodiments, when the protective layer comprises a transparent conductive oxide layer, the thickness of the protective layer is 5-15 nm.

[0044] In some embodiments, the substrate further includes a second surface disposed opposite to the first surface, and a side surface adjacent to the first surface and the second surface;

[0045] The heterojunction cell also includes a second electroplated electrode, and a second intrinsic silicon layer, a second doped layer and a second transparent conductive layer sequentially stacked on the second surface. The doping type of the second doped layer is opposite to that of the first doped layer. The second electroplated electrode is electrically connected to the second transparent conductive layer.

[0046] In some embodiments, the heterojunction cell further includes a first metal seed layer and / or a second metal seed layer, wherein the first metal seed layer is stacked on the surface of the first electroplated electrode facing the substrate, and the second metal seed layer is stacked on the surface of the second electroplated electrode facing the substrate.

[0047] In some embodiments, the heterojunction cell further includes an electrode protective layer, wherein the electrode protective layer located on one side of the first surface is stacked on the surface of the first electroplated electrode opposite to the substrate, and / or the electrode protective layer located on one side of the second surface is stacked on the surface of the second electroplated electrode opposite to the substrate.

[0048] In some embodiments, the first intrinsic silicon layer covers at least a portion of the first surface and side surface;

[0049] The second intrinsic silicon layer covers at least a portion of the second surface and side surface, and on the side surface of the substrate, a portion of the structure of the second intrinsic silicon layer is stacked onto the side of the first intrinsic silicon layer opposite to the substrate.

[0050] The second doped layer covers at least a portion of the second surface and side surface, and on the side surface of the substrate, a portion of the structure of the second doped layer is stacked onto the side of the first intrinsic silicon layer opposite to the substrate.

[0051] The first doped layer covers at least a portion of the first surface and side surface, and on the side surface of the substrate, a portion of the structure of the first doped layer is stacked onto the side of the second doped layer opposite to the substrate.

[0052] In some embodiments, portions of the outer contour edge of the first transparent conductive layer are spaced from the edge of the first surface to define an annular isolation region on the first surface.

[0053] This application also provides a heterojunction solar cell, including:

[0054] Substrate;

[0055] A first intrinsic silicon layer and a first doped layer are sequentially stacked on the first surface of the substrate;

[0056] A first transparent conductive layer and a protective layer are stacked on the side of the first doped layer facing away from the substrate. The first transparent conductive layer covers a portion of the first surface, and the protective layer completely covers the first surface.

[0057] The first electrode is located on the side of the protective layer away from the substrate and is electrically connected to the first transparent conductive layer.

[0058] The first surface includes an isolation region not covered by the first transparent conductive layer; a portion of the protective layer is stacked on the corresponding isolation region of the first doped layer.

[0059] In some embodiments, the substrate further includes a second surface disposed opposite to the first surface, and a side surface adjacent to the first surface and the second surface;

[0060] The heterojunction solar cell further includes a second electrode, and a second intrinsic silicon layer, a second doped layer and a second transparent conductive layer sequentially stacked on the second surface. The doping type of the second doped layer is opposite to that of the first doped layer, and the second electrode is electrically connected to the second transparent conductive layer.

[0061] This application also provides a heterojunction solar cell, including:

[0062] Substrate;

[0063] A first intrinsic silicon layer and a first doped layer are sequentially stacked on the first surface of the substrate;

[0064] A first transparent conductive layer and a protective layer are stacked on the side of the first doped layer opposite to the substrate, the first transparent conductive layer covering a portion of the first surface; and

[0065] The first electrode is located on the side of the protective layer opposite to the substrate and is electrically connected to the first transparent conductive layer.

[0066] Wherein, the first surface includes an isolation area not covered by the first transparent conductive layer; the protective layer partially or completely covers the isolation area.

[0067] This application also provides a heterojunction solar cell, including:

[0068] Substrate;

[0069] A first intrinsic silicon layer and a first doped layer are sequentially stacked on the first surface of the substrate;

[0070] A first transparent conductive layer and a protective layer are stacked on the side of the first doped layer opposite to the substrate. The first transparent conductive layer covers a portion of the first surface, and the protective layer completely covers the first surface.

[0071] The first electrode is located on the side of the protective layer opposite to the substrate and is electrically connected to the first transparent conductive layer.

[0072] The first surface includes an isolation region not covered by the first transparent conductive layer; on the first surface, the protective layer is disposed only between the first electrode and the first transparent conductive layer, or only between the first transparent conductive layer and the first doped layer.

[0073] This application also provides a heterojunction solar cell, including:

[0074] Substrate;

[0075] A first intrinsic silicon layer and a first doped layer are sequentially stacked on the first surface of the substrate;

[0076] A first transparent conductive layer and a protective layer are stacked on the side of the first doped layer opposite to the substrate. The first transparent conductive layer covers a portion of the first surface, and the protective layer completely covers the first surface.

[0077] The first electrode is located on the side of the protective layer opposite to the substrate and is electrically connected to the first transparent conductive layer.

[0078] The first surface includes an isolation area not covered by the first transparent conductive layer; on the first surface, the protective layer only covers the isolation area.

[0079] This application also provides a method for fabricating a heterojunction solar cell, including:

[0080] A substrate is provided, the substrate including a substrate, and a first intrinsic silicon layer and a first doped layer sequentially stacked on a first surface of the substrate;

[0081] A first transparent conductive layer and a protective material layer are formed on the side of the first doped layer away from the substrate. The first transparent conductive layer covers a portion of the first surface, and the first surface includes an isolation region not covered by the first transparent conductive layer. The protective material layer completely covers the first surface, and a portion of the structure of the protective material layer is stacked on the corresponding isolation region of the first doped layer.

[0082] A first electroplating electrode is formed by electroplating on the side of the protective material layer away from the substrate, and the first electroplating electrode is electrically connected to the first transparent conductive layer.

[0083] In some embodiments, the step of forming a protective material layer includes:

[0084] The second surface of the substrate is oriented towards the support frame of the carrier plate;

[0085] A protective material layer is formed on the side of the first doped layer away from the substrate;

[0086] The protective material layer completely covers the first surface and at least a portion of the side surface of the substrate; or, the protective material layer completely covers the first surface, and the outer contour edge of the protective material layer coincides with the edge of the first surface.

[0087] In some embodiments, the step of forming the first transparent conductive layer includes:

[0088] The first surface of the substrate is oriented towards the support frame of the carrier plate;

[0089] A first transparent conductive layer is formed on the side of the first doped layer away from the substrate, and the location of the formation of the first transparent conductive layer corresponds to the hollow portion of the bearing frame.

[0090] In some embodiments, the step of forming a first transparent conductive layer and a protective material layer stacked on each other on the side of the first doped layer away from the substrate specifically includes:

[0091] A first transparent conductive layer is formed on the surface of the first doped layer that is away from the substrate.

[0092] A protective material layer is formed on the surface of the first transparent conductive layer away from the substrate.

[0093] In some embodiments, the step of forming a first transparent conductive layer on the surface of the first doped layer away from the substrate specifically includes:

[0094] The first surface of the substrate is oriented toward the support frame of the carrier plate, and the portion of the first doped layer located on the first surface is supported by the support frame.

[0095] In the portion of the first doped layer covering one side of the first surface, the area not obscured by the bearing frame forms a first transparent conductive layer.

[0096] In some embodiments, the step of forming a protective material layer on the surface of the first transparent conductive layer away from the substrate specifically includes:

[0097] The second surface of the substrate is supported on one side of the support frame of the carrier plate;

[0098] A protective material layer is formed on the surface of the first transparent conductive layer away from the substrate; the protective material layer is partially stacked on the surface of the first transparent conductive layer away from the substrate, and partially stacked on the surface of the portion of the isolation region corresponding to the first doped layer.

[0099] In some embodiments, the substrate further includes a second intrinsic silicon layer and a second doped layer sequentially stacked on a second surface of the substrate, the second surface being disposed opposite to the first surface; the step of forming the first transparent conductive layer and the step of forming the protective material layer further includes:

[0100] A second transparent conductive layer is formed on the side of the second doped layer away from the substrate.

[0101] In some embodiments, the substrate further includes a side surface adjacent to the first surface and the second surface;

[0102] The second transparent conductive layer covers at least a portion of the side surface of the second surface and the substrate;

[0103] The protective material layer also covers at least a portion of the side surface, and a portion of the protective material layer is stacked onto the side of the second transparent conductive layer opposite to the substrate; or

[0104] The outer contour edge of the protective material layer coincides with the edge of the first surface.

[0105] In some embodiments, the step of forming a first transparent conductive layer and a protective material layer stacked on each other on the side of the first doped layer away from the substrate specifically includes:

[0106] A protective material layer is formed on the surface of the first doped layer away from the substrate.

[0107] A first transparent conductive layer is formed on the surface of the protective material layer away from the substrate.

[0108] In some embodiments, the substrate further includes a second intrinsic silicon layer and a second doped layer sequentially stacked on a second surface of the substrate, the second surface being disposed opposite to the first surface; the substrate also includes a side surface adjacent to the first surface and the second surface;

[0109] The step of forming a protective material layer on the substrate-away surface of the first doped layer includes:

[0110] A second transparent conductive layer is formed on the surface of the second doped layer away from the substrate, the second transparent conductive layer covering at least a portion of the second surface and side surfaces.

[0111] In some embodiments, the step of forming a protective material layer on the substrate-away surface of the first doped layer specifically includes:

[0112] A protective material layer is formed on the side of the first doped layer away from the substrate. The protective material layer completely covers the first surface and at least a portion of the side surface, and the protective material layer is stacked onto the second transparent conductive layer.

[0113] In some embodiments, the step of forming a first transparent conductive layer on the surface of the protective material layer away from the substrate specifically includes:

[0114] The first surface of the substrate is oriented toward the support frame of the carrier plate, and the portion of the protective material layer located on the first surface is supported by the support frame.

[0115] In the portion of the protective material layer covering one side of the first surface, the area not obscured by the bearing frame forms a first transparent conductive layer.

[0116] In some embodiments, the substrate further includes a second surface disposed opposite to the first surface, and a side surface adjacent to the first surface and the second surface;

[0117] The step of forming a protective material layer on the substrate-away surface of the first doped layer includes:

[0118] A protective material layer is formed on the side of the first doped layer away from the substrate, the protective material layer covering at least a portion of the first surface and side surface.

[0119] In some embodiments, the step of forming a first transparent conductive layer on the surface of the protective material layer away from the substrate specifically includes:

[0120] The first surface of the substrate is oriented toward the support frame of the carrier plate, and the portion of the protective material layer located on the first surface is supported by the support frame.

[0121] In the portion of the protective material layer covering one side of the first surface, the area not obscured by the bearing frame forms a first transparent conductive layer.

[0122] In some embodiments, the substrate further includes a second intrinsic silicon layer and a second doped layer sequentially stacked on the second surface;

[0123] Following the step of forming the first transparent conductive layer on the substrate-facing surface of the protective material layer, the following steps are also included:

[0124] A second transparent conductive layer is formed on the surface of the second doped layer away from the substrate. The second transparent conductive layer covers a portion of the second surface and side surfaces, and is stacked onto the protective material layer.

[0125] In some embodiments, the substrate further includes a second intrinsic silicon layer and a second doped layer sequentially stacked on a second surface of the substrate, the second surface being disposed opposite to the first surface;

[0126] In the step of forming a protective material layer on the surface of the first doped layer away from the substrate:

[0127] A protective material layer covers at least a portion of the first surface and side surface, on which the protective material layer is stacked onto the side of the second doped layer opposite to the substrate.

[0128] In some embodiments, in the step of forming a protective material layer on the surface of the first doped layer away from the substrate:

[0129] A protective material layer covers at least a portion of the first surface and side surface; on the side surface, the outer contour edge of the protective material layer coincides with the outer contour edge of the first doped layer.

[0130] In some embodiments, the first doped layer includes an oxygen-free microcrystalline host layer;

[0131] The steps for forming the protective material layer include:

[0132] An oxygen-containing amorphous silicon layer is formed on the surface of the first doped layer away from the substrate as a protective material layer. The oxygen-containing amorphous silicon layer has the same doping type as the first doped layer.

[0133] In some embodiments, the first doped layer further includes an oxygen-containing microcrystalline sublayer, which is stacked between the first intrinsic silicon layer and the oxygen-free microcrystalline host layer.

[0134] In some embodiments, the oxygen-containing microcrystalline sublayer and the oxygen-free microcrystalline host layer are formed by the following steps:

[0135] Hydrogen, silane, diborane, and carbon dioxide gases are introduced into the reaction chamber, wherein the molar volume ratio of hydrogen, silane, diborane, and carbon dioxide gases is 300:1:0.005:0.2 to 600:1:0.01:0.5, and the reaction pressure in the reaction chamber is 4-6 mbar, so as to form an oxygen-containing microcrystalline film layer on the substrate-away surface of the first intrinsic silicon layer.

[0136] Hydrogen, silane, and diborane gases are introduced into the reaction chamber, wherein the molar volume ratio of hydrogen, silane, and diborane gases is 300:1:0.01 to 500:1:0.04, and the reaction pressure in the reaction chamber is 2-3 mbar, so as to form an oxygen-free microcrystalline host layer on the surface of the oxygen-containing microcrystalline film layer away from the substrate.

[0137] In some embodiments, the step of forming an oxygen-doped amorphous silicon layer as a protective material layer includes:

[0138] Hydrogen, silane, diborane, and carbon dioxide gases are introduced into the reaction chamber, wherein the molar volume ratio of hydrogen, silane, diborane, and carbon dioxide gases is 8:1:3:1 to 12:1:5:1.5; the reaction pressure in the reaction chamber is about 2-3 mbar, so as to form an oxygen-doped amorphous silicon layer on the surface of the oxygen-free microcrystalline host layer.

[0139] In some embodiments, the protective material layer comprises a transition metal oxide, and the conductivity type of the protective material layer is the same as that of the first doped layer; or

[0140] The protective material layer includes a dielectric passivation layer, such as a tunneling layer; or

[0141] The protective material layer includes a transparent conductive oxide layer.

[0142] In some embodiments, the substrate further includes a second intrinsic silicon layer and a second doped layer sequentially stacked on a second surface of the substrate, the second surface being disposed opposite to the first surface;

[0143] Other methods for fabricating heterojunction solar cells include:

[0144] A second transparent conductive layer is formed on the surface of the second doped layer that is away from the substrate.

[0145] A second electroplated electrode is formed on one side of the second surface of the substrate by electroplating.

[0146] In some embodiments, the protective material layer completely covers the first surface and covers at least a portion of the side surface of the substrate;

[0147] The steps of forming the first electroplating electrode and forming the second electroplating electrode further include removing at least a portion of the protective material layer to form a protective layer.

[0148] In some embodiments, the portion of the protective material layer that is removed includes the portion of the protective material layer located on one side; or

[0149] The removed portions of the protective material layer include the portions covering one side and the portion covering the isolation area; or

[0150] The portion of the protective material layer that is removed includes the portion of the protective material layer covering one side of the side and the portion of the protective material layer corresponding to the non-metallic contact area of ​​the first surface.

[0151] In some embodiments, the steps of forming the first electroplating electrode and forming the second electroplating electrode specifically include:

[0152] A first metal seed material layer is formed on one side of the first surface of the substrate, and a second metal seed material layer is formed on the surface of the second transparent conductive layer opposite to the substrate, wherein the first metal seed material layer is located on the one of the first transparent conductive layer and the protective material layer that is farther away from the substrate;

[0153] A first electroplating electrode is formed by electroplating a patterned mask layer on the surface of a first metal seed material layer, and a second electroplating electrode is formed by electroplating a second metal seed material layer.

[0154] Remove the mask layer;

[0155] The portion of the first metal seed material layer not covered by the first electroplating electrode is removed to form the first metal seed layer, and the portion of the second metal seed material layer not covered by the second electroplating electrode is removed to form the second metal seed layer.

[0156] In some embodiments, the patterned mask layer is formed by the following steps:

[0157] A patterned first mask material layer is formed on the side of the first metal seed material layer and the second metal seed material layer away from the substrate. The first mask material layer is hollowed out at the position of the metal contact area of ​​the first surface and at the position of the metal contact area of ​​the second surface.

[0158] An insulating adhesive is applied to one side of the substrate.

[0159] In some embodiments, after removing the portion of the first metal seed material layer not covered by the first electroplating electrode and removing the portion of the second metal seed material layer not covered by the second electroplating electrode, the method further includes forming an electrode protective layer on the surfaces of the first and second electroplating electrodes.

[0160] In some embodiments, the steps of removing the portion of the first metal seed material layer not covered by the first electroplating electrode, removing the portion of the second metal seed material layer not covered by the second electroplating electrode, and / or forming the electrode protective layer further include removing at least a portion of the protective material layer to form a protective material layer.

[0161] In some embodiments, the substrate further includes a second intrinsic silicon layer and a second doped layer sequentially stacked on a second surface of the substrate, the second surface being disposed opposite to the first surface;

[0162] The specific steps for providing a substrate include:

[0163] A first intrinsic silicon layer is formed on a first surface of the substrate, and a second intrinsic silicon layer is formed on a second surface of the substrate;

[0164] A second doped layer is formed on the surface of the second intrinsic silicon layer away from the substrate, and a first doped layer is formed on the surface of the first intrinsic silicon layer away from the substrate.

[0165] In some embodiments, the substrate further includes a side surface adjacent to the first surface and the second surface;

[0166] The first intrinsic silicon layer covers at least a portion of the first surface and side surface;

[0167] The second intrinsic silicon layer covers at least a portion of the second surface and side surface, and a portion of the structure of the second intrinsic silicon layer is stacked onto the side of the first intrinsic silicon layer away from the substrate.

[0168] The second doped layer covers at least a portion of the second surface and side surface, and a portion of the structure of the second doped layer is stacked onto the side of the first intrinsic silicon layer away from the substrate.

[0169] The first doped layer covers at least a portion of the first surface and side surface, and a portion of the structure of the first doped layer is stacked onto the side of the second doped layer opposite to the substrate.

[0170] This application also provides a heterojunction battery, which is manufactured using the above-described heterojunction battery manufacturing method.

[0171] This application also provides a photovoltaic module, including at least one cell string, the cell string including at least two heterojunction cells as described above. Attached Figure Description

[0172] Figure 1 is a schematic diagram of the structure of a heterojunction battery provided in an embodiment of this application.

[0173] Figure 2 is a schematic diagram of the structure of a heterojunction battery provided in another embodiment of this application.

[0174] Figure 3 is a schematic diagram of the structure of a heterojunction battery provided in another embodiment of this application.

[0175] Figure 4A is a schematic diagram of the structure of a heterojunction battery provided in another embodiment of this application.

[0176] Figure 4B is a schematic diagram of the structure of a heterojunction battery provided in another embodiment of this application.

[0177] Figure 5 is a schematic diagram of the structure of a heterojunction battery provided in another embodiment of this application.

[0178] Figure 6 is a structural schematic diagram of a heterojunction battery provided in another embodiment of this application.

[0179] Figure 7 is a schematic diagram of the structure of a heterojunction battery provided in another embodiment of this application.

[0180] Figure 8 is a flowchart illustrating the fabrication method of a heterojunction solar cell provided in an embodiment of this application.

[0181] Figures 9A-13 are schematic diagrams of the various stages of a heterojunction solar cell fabrication method according to an embodiment of this application, wherein:

[0182] Figure 9A is a schematic diagram of the substrate.

[0183] Figure 9B is a schematic diagram of the substrate being supported by the support frame.

[0184] Figure 10 is a schematic diagram of forming a first transparent conductive layer and a second transparent conductive layer on a substrate.

[0185] Figure 11 is a schematic diagram of the formation of the protective material layer.

[0186] Figure 12 is a schematic diagram of the formation of the first metal seed layer and the second metal seed layer.

[0187] Figure 13 is a schematic diagram of the formation of the patterned first mask material layer and insulating adhesive.

[0188] Figures 14A-17 are schematic diagrams of the various stages of a heterojunction solar cell fabrication method according to another embodiment of this application, wherein:

[0189] Figure 14A is a schematic diagram of the formation of the protective material layer.

[0190] Figure 14B is a schematic diagram of a substrate forming a protective material layer supported by a support frame.

[0191] Figure 15 is a schematic diagram of the formation of the first transparent conductive layer and the second transparent conductive layer.

[0192] Figure 16 is a schematic diagram of the formation of the first metal seed layer and the second metal seed layer.

[0193] Figure 17 is a schematic diagram of the formation of the patterned first mask material layer and insulating adhesive.

[0194] Figures 18-21 are schematic diagrams of the various stages of a heterojunction solar cell fabrication method according to another embodiment of this application, wherein:

[0195] Figure 18 is a schematic diagram of the formation of the second transparent conductive layer.

[0196] Figure 19 is a schematic diagram of the formation of the protective material layer and the first transparent conductive layer.

[0197] Figure 20 is a schematic diagram of the formation of the first metal seed layer and the second metal seed layer.

[0198] Figure 21 is a schematic diagram of the formation of the patterned first mask material layer and insulating adhesive.

[0199] Figure 22 is a schematic diagram of the structure of a heterojunction battery provided in an embodiment of this application.

[0200] Figures 23-26 are schematic diagrams of the various stages of the fabrication method of a heterojunction solar cell provided in another embodiment of this application, wherein:

[0201] Figure 23 is a schematic diagram of forming a protective material layer on a substrate.

[0202] Figure 24 is a schematic diagram of the formation of the first transparent conductive layer and the second transparent conductive layer.

[0203] Figure 25 is a schematic diagram of the formation of the first metal seed layer and the second metal seed layer.

[0204] Figure 26 is a schematic diagram of the formation of the patterned first mask material layer and insulating adhesive.

[0205] Figure 27 is a schematic diagram of the structure of a heterojunction battery provided in another embodiment of this application.

[0206] Figure 28 is a top view of the first transparent conductive layer on the first surface of the substrate according to an embodiment of this application.

[0207] Explanation of reference numerals: 100, Heterojunction solar cell; 101, Substrate; 10, Substrate; 21, First intrinsic silicon layer; 22, Second intrinsic silicon layer; 31, First doped layer; 32, Second doped layer; 41, First transparent conductive layer; 42, Second transparent conductive layer; 50, Protective layer; 500, Protective material layer; 61, First metal seed layer; 610, First metal seed material layer; 62, Second metal seed layer; 620, Second metal seed material layer; 71, First mask material layer; 72, Insulating adhesive; 73, Electrode protective layer; 81, First electroplated electrode; 82, Second electroplated electrode; F, First surface; S, Second surface; C, Side surface; W, Isolation region; Z, Metal contact region. Detailed Implementation

[0208] To make the above-mentioned objectives, features, and advantages of this application more apparent and understandable, the specific embodiments of this application are described in detail below with reference to the accompanying drawings. Many specific details are set forth in the following description to provide a thorough understanding of this application. However, this application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of this application. Therefore, this application is not limited to the specific embodiments disclosed below.

[0209] It should be understood that the terms “comprising,” “including,” “having,” “containing,” and any derivative thereof used in this application shall be regarded as non-exclusively including the features referred to by the term and do not imply the exclusion of the existence of any additional features unless otherwise stated or implied.

[0210] In some cases, for the sake of brevity and / or to aid in understanding the scope of this disclosure, a single embodiment may combine multiple features. It should be understood that in such cases, these multiple features may be provided individually (e.g., in different embodiments) or in any other suitable combination. Conversely, when different features are described in different embodiments, these different features may be combined to form a single embodiment unless otherwise stated or implied. This principle also applies to the claims, whose claims may be rearranged in any combination, i.e., any claim may be modified to include any feature defined in the other claims.

[0211] In this application, unless otherwise stated or implied, the phrase “at least one” followed by a list of items refers to any combination of the listed items, including individual members. Whether the expression is “at least one of a, b, or c” or “at least one of a, b, and c”, it is intended to cover: a, b, c, combinations of a and b, combinations of a and c, combinations of b and c, and combinations of a, b, and c.

[0212] In the description of this application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc., indicating the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this application.

[0213] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of this application, "multiple" means at least two, such as two, three, etc., unless otherwise explicitly specified.

[0214] In this application, unless otherwise expressly specified and limited, the terms "installation," "connection," "joining," and "fixing," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication of two components or the interaction between two components, unless otherwise expressly limited. Those skilled in the art can understand the specific meaning of the above terms in this application according to the specific circumstances.

[0215] In this application, unless otherwise expressly specified and limited, "above" or "below" the second feature can mean that the first feature is in direct contact with the second feature, or that the first feature is in indirect contact with the second feature through an intermediate medium. Furthermore, "above," "on top of," and "over" the second feature can mean that the first feature is directly above or diagonally above the second feature, or simply that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature can mean that the first feature is directly below or diagonally below the second feature, or simply that the first feature is at a lower horizontal level than the second feature.

[0216] It should be noted that when an element is referred to as being "fixed to" or "set on" another element, it can be directly on the other element or there may be an intervening element. When an element is considered to be "connected to" another element, it can be directly connected to the other element or there may be an intervening element. The terms "vertical," "horizontal," "upper," "lower," "left," "right," and similar expressions used herein are for illustrative purposes only and do not represent the only possible implementation.

[0217] The following description, in conjunction with the accompanying drawings, illustrates the heterojunction solar cell, its fabrication method, and photovoltaic module according to embodiments of this application.

[0218] It should be noted that the accompanying drawings of this application only illustrate the structure of one corner of the heterojunction solar cell 100 in a longitudinal sectional view along the thickness direction. The same applies to other parts of the heterojunction solar cell 100 not shown in the sectional view, and will not be described further here. Furthermore, since only one corner is shown in these drawings, only a schematic diagram of the film structure on one side of the heterojunction solar cell 100 is displayed. The film structure covering at least some of the other sides of the heterojunction solar cell 100 is the same, and will not be described further here.

[0219] The following description uses electroplated electrodes as an example, but those skilled in the art will understand that the electrodes in the heterojunction cell 100 of this application are not limited to being formed by electroplating. For example, the first electrode and / or the second electrode can be formed by depositing a metal layer and patterning, or by screen printing, etc.

[0220] Referring to Figures 1, 2, 4A, and 5-7, some embodiments of the heterojunction solar cell 100 provided in this application include: a substrate 10, a first intrinsic silicon layer 21, a first doped layer 31, a first transparent conductive layer 41, a protective layer 50, and a first electroplated electrode 81.

[0221] A first intrinsic silicon layer 21 and a first doped layer 31 are sequentially stacked on the first surface F of the substrate 10. A first transparent conductive layer 41 and a protective layer 50 are stacked on the side of the first doped layer 31 facing away from the substrate 10. The first transparent conductive layer 41 covers a portion of the first surface F, and the protective layer 50 completely covers the first surface F. A first electroplating electrode 81 is located on the side of the protective layer 50 facing away from the substrate 10 and is electrically connected to the first transparent conductive layer 41. The first surface F includes an isolation region W not covered by the first transparent conductive layer 41, and a portion of the structure of the protective layer 50 is stacked on the corresponding isolation region W of the first doped layer 31, completely covering the isolation region W. In some embodiments, the protective layer 50 is in contact with a portion of the corresponding isolation region W of the first doped layer 31. By providing the protective layer 50, with a portion of its structure stacked on the corresponding isolation region W of the first doped layer 31, and the first electroplating electrode 81 located on the side of the protective layer 50 facing away from the substrate 10, the formation step of the protective layer 50 precedes the first electroplating electrode 81. During the electroplating process to form the first electroplated electrode 81, the portion of the isolation region W corresponding to the first doped layer 31 is protected by the protective layer 50 and is therefore not corroded by the plating solution. No defects are generated in the surface structure of the portion of the isolation region W corresponding to the first doped layer 31. Compared to related technologies where the first doped layer is partially etched away, resulting in insufficient lateral conductivity and poor carrier collection ability, the lateral conductivity and carrier collection ability of the first doped layer 31 in this embodiment are not affected, effectively avoiding the decrease in battery efficiency caused by corrosion and damage to the first doped layer 31. Furthermore, since the protective layer 50 is stacked on the portion of the isolation region W corresponding to the first doped layer 31, the passivation ability of the first doped layer 31 is also improved, thus improving the efficiency of the heterojunction battery 100. Furthermore, the fact that the protective layer 50 completely covers the first surface F further enhances the back reflection effect on the first surface F side.

[0222] Additionally, it should be noted that the term "coverage" in the embodiments of this application refers to the size relationship of the set area. For example, one structure covers another structure. "Covering" a certain part or area refers to the overlapping part or area generated when one structure is projected onto the other structure along the stacking direction of the two structures. It does not limit whether the two structures are in direct contact. For example, if the first transparent conductive layer 41 covers a part of the first surface F, it means that the orthographic projection of the first transparent conductive layer 41 on the first surface F is only located in a local area of ​​the first surface F. In fact, the first transparent conductive layer 41 and the first surface F are separated by at least the first intrinsic silicon layer 21 and the first doped layer 31, and the first transparent conductive layer 41 and the first surface F will not be in direct contact. If the protective layer 50 completely covers the first surface F, it means that the orthographic projection of the protective layer 50 on the first surface F coincides with the first surface F. In fact, the protective layer 50 and the first surface F are separated by at least the first intrinsic silicon layer 21 and the first doped layer 31, and the protective layer 50 and the first surface F will not be in direct contact.

[0223] In some implementations, the protective layer 50 is conductive, for example, it may be a transparent conductive oxide layer. In some embodiments, the sheet resistance of the protective layer 50 is greater than the sheet resistance of the first transparent conductive layer 41.

[0224] In other embodiments, the protective layer 50 is a P-type or N-type semiconductor layer, and its conductivity type (i.e., P-type or N-type) is the same as that of the first doped layer 31, and it can be part of a heterojunction structure. For example, the protective layer 50 can be a doped silicon layer or a transition metal oxide layer.

[0225] In some other embodiments, the protective layer 50 is a dielectric passivation layer, such as a tunneling layer, which allows charge carriers to tunnel through.

[0226] In some embodiments, the substrate 10 further includes a second surface S disposed opposite to the first surface F, and a side surface C adjacent to the first surface F and the second surface S. The first intrinsic silicon layer 21 and the first doped layer 31 are sequentially stacked on the first surface F of the substrate 10, meaning that the first intrinsic silicon layer 21 is stacked on the first surface F, and the first doped layer 31 is stacked on the surface of the first intrinsic silicon layer 21 that is away from the substrate 10.

[0227] The first transparent conductive layer 41 and the protective layer 50 are stacked on the side of the first doped layer 31 facing away from the substrate 10. This means that the first transparent conductive layer 41 and the protective layer 50 are stacked on top of each other. For example, as shown in Figures 1, 2, and 3, the first transparent conductive layer 41 is stacked on the surface of the first doped layer 31 facing away from the substrate 10, and the protective layer 50 is stacked on the surface of the first transparent conductive layer 41 facing away from the substrate 10. In some other embodiments, as shown in Figures 4A, 4B, 5, 6, and 7, the protective layer 50 is stacked on the surface of the first doped layer 31 facing away from the substrate 10, and the first transparent conductive layer 41 is stacked on the surface of the protective layer 50 facing away from the substrate 10.

[0228] The first electroplated electrode 81 is located on the side of the protective layer 50 facing away from the substrate 10 and is electrically connected to the first transparent conductive layer 41. The first electroplated electrode 81 can be an electrode formed by an electroplating process.

[0229] As previously described, the first transparent conductive layer 41 covers a portion of the first surface F, which includes an isolation region W not covered by the first transparent conductive layer 41. This means that when viewed from the first surface F side of the heterojunction cell 100, a portion of the first surface F is not obscured by the first transparent conductive layer 41 and is exposed from it. In other words, when the first transparent conductive layer 41 is projected orthogonally onto the first surface F, the isolation region W is the portion of the first surface F that does not overlap with the projection of the first doped layer 31. In some embodiments, a portion of the structure of the protective layer 50 is stacked on the corresponding isolation region W of the first doped layer 31, and combined with the fact that the protective layer 50 completely covers the first surface F, the protective layer 50 can completely cover the corresponding isolation region W of the first doped layer 31.

[0230] Referring to FIG28, in some embodiments, each portion on the outer contour edge of the first transparent conductive layer 41 is spaced from the edge of the first surface F to define an annular isolation region W on the first surface F.

[0231] The isolation region W is the area on the first surface F of the heterojunction battery 100. The uncoated area formed by the first transparent conductive layer 41 during the coating process due to the shielding of the carrier plate is directly opposite the isolation region W, and its width is generally between 0.2 mm and 1 mm. In some embodiments, the protective layer 50 covers the portion of the first doped layer 31 corresponding to the isolation region W. On the one hand, this prevents the sputtered material during the formation of the first metal seed layer 61 (described later) from directly depositing onto the surface of the first doped layer 31, affecting the battery performance and reliability. On the other hand, it can effectively protect the exposed surface of the first doped layer 31 from damage caused by the wet chemical solution during the post-electroplating process.

[0232] In some embodiments, referring to Figures 1-7, the heterojunction solar cell 100 further includes a second intrinsic silicon layer 22, a second doped layer 32, and a second transparent conductive layer 42 sequentially stacked on the second surface S of the substrate 10. The doping type of the second doped layer 32 is opposite to that of the first doped layer 31. Additionally, the heterojunction solar cell 100 includes a second electroplating electrode 82, which is disposed on one side of the second surface S of the substrate 10 and is electrically connected to the second transparent conductive layer 42.

[0233] In this embodiment, the second intrinsic silicon layer 22, the second doped layer 32, and the second transparent conductive layer 42 are all configured to cover at least a portion of the second surface S and the side surface C of the substrate 10. Alternatively, in some other embodiments, at least one of the second intrinsic silicon layer 22, the second doped layer 32, and the second transparent conductive layer 42 may only cover the second surface S. Similarly, the first intrinsic silicon layer 21 and the first doped layer 31 are both configured to cover at least a portion of the first surface F and the side surface C of the substrate 10. Alternatively, in some other embodiments, at least one of the first intrinsic silicon layer 21 and the first doped layer 31 may only cover the first surface F.

[0234] For example, as shown in Figures 1-7, in one possible implementation, a first intrinsic silicon layer 21 covers at least a portion of the first surface F and the side surface C. A second intrinsic silicon layer 22 covers at least a portion of the second surface S and the side surface C, and on the side surface C of the substrate 10, a portion of the structure of the second intrinsic silicon layer 22 is stacked onto the side of the first intrinsic silicon layer 21 facing away from the substrate 10. A second doped layer 32 covers at least a portion of the second surface S and the side surface C, and on the side surface C of the substrate 10, a portion of the structure of the second doped layer 32 is stacked onto the side of the first intrinsic silicon layer 21 facing away from the substrate 10. A first doped layer 31 covers at least a portion of the first surface F and the side surface C, and on the side surface C of the substrate 10, a portion of the structure of the first doped layer 31 is stacked onto the side of the second doped layer 32 facing away from the substrate 10. It is understood that the stacking relationship between the various film layers is not limited to this and can be configured according to actual needs.

[0235] It is understandable that when referring to a layer covering a surface, such as "covering the first surface F" or "covering the second surface S", it can mean that the layer completely covers the surface or only covers part of the surface.

[0236] In some embodiments, referring again to Figures 1-7, the heterojunction solar cell 100 further includes a first metal seed layer 61 and / or a second metal seed layer 62. The first metal seed layer 61 is stacked on the surface of the first electroplating electrode 81 facing the substrate 10, and the second metal seed layer 62 is stacked on the surface of the second electroplating electrode 82 facing the substrate 10. This arrangement facilitates the formation of the first electroplating electrode 81 and the second electroplating electrode 82 during the electroplating process. The coverage area of ​​the first metal seed layer 61 and the first electroplating electrode 81 on it on the first surface F can substantially completely overlap. The coverage area of ​​the second metal seed layer 62 and the second electroplating electrode 82 on it on the second surface S can substantially completely overlap.

[0237] In some embodiments, the heterojunction solar cell 100 further includes an electrode protective layer 73. The electrode protective layer 73, located on one side of the first surface F, is stacked on the surface of the first electroplated electrode 81 facing away from the substrate 10, and its coverage area can substantially completely overlap with the coverage area of ​​the first electroplated electrode 81 on the first surface F. The electrode protective layer 73, located on one side of the second surface S, is stacked on the surface of the second electroplated electrode 82 facing away from the substrate 10. The electrode protective layer 73 can be, for example, a chemical plating protective layer, and its coverage area can substantially completely overlap with the coverage area of ​​the second electroplated electrode 82 on the second surface S.

[0238] In some embodiments, the substrate 10 may be a crystalline silicon wafer, N-type or P-type doped. The first surface F may be a backlight surface with a textured structure, or the first surface F may be a polished structure. The second surface S may be a light-receiving surface with a textured structure.

[0239] In some embodiments, the first intrinsic silicon layer 21, in addition to silicon, further comprises at least one of elements such as oxygen, carbon, and nitrogen, which can be doped into the silicon layer as dopants. The first intrinsic silicon layer 21 can be amorphous or microcrystalline, predominantly amorphous. The first intrinsic silicon layer 21 can completely cover the first surface F and the side surface C, and can partially extend to the second surface S. Alternatively, the first intrinsic silicon layer 21 can only cover the first surface F and the side surface C.

[0240] The host material of the first doped layer 31 can be silicon, and can be N-type or P-type doped. In some embodiments, the first doped layer 31 further contains at least one of oxygen, carbon, nitrogen, etc., which can be doped into the host material as dopants. The first doped layer 31 can be amorphous or microcrystalline, predominantly microcrystalline. The first doped layer 31 can completely cover the first surface F and the side surface C, and can partially extend to the second surface S. Alternatively, the first doped layer 31 can only cover the first surface F and the side surface C.

[0241] The first transparent conductive layer 41 may include a composite film structure formed by stacking one or more different transparent conductive films. The transparent conductive film layer may be, for example, at least one of indium tin oxide (ITO) film, indium molybdenum oxide (IMO) film, aluminum-doped zinc oxide (AZO) film, SCOT film, and tin oxide (SnOx) film.

[0242] The material of the first metal seed layer 61 may include metals or metal alloys such as copper, aluminum, nickel, and titanium. The thickness of the first metal seed layer 61 may be 10-200 nm.

[0243] The material of the first electroplating electrode 81 may include low-cost metals such as copper or nickel-copper alloys. The thickness of the first electroplating electrode 81 may be 5-20 μm.

[0244] In some embodiments, the second intrinsic silicon layer 22, in addition to silicon, further comprises at least one of elements such as oxygen, carbon, and nitrogen, which can be doped into the silicon layer as dopants. The second intrinsic silicon layer 22 can be amorphous or microcrystalline, predominantly amorphous. The second intrinsic silicon layer 22 can completely cover the second surface S and the side surface C, and can partially extend into the first surface F. Alternatively, the second intrinsic silicon layer 22 can only cover the second surface S and the side surface C.

[0245] The host material of the second doped layer 32 can be silicon, and it can be N-type or P-type doped. The doping type of the second doped layer 32 is opposite to that of the first doped layer 31. In some embodiments, the second doped layer 32 further contains at least one of oxygen, carbon, nitrogen, etc., which can be doped into the host material as dopants. The second doped layer 32 can be amorphous or microcrystalline, predominantly microcrystalline. The second doped layer 32 can completely cover the second surface S and the side surface C, and can partially extend the structure to the first surface F. Alternatively, the second doped layer 32 can only cover the second surface S and the side surface C. Alternatively, the second doped layer 32 can only cover the second surface S.

[0246] The second transparent conductive layer 42 may include a composite film structure formed by stacking one or more different transparent conductive films. The transparent conductive film layer may be, for example, at least one of ITO film, IMO film, AZO film, SCOT film, and SnOx film.

[0247] The material of the second electroplating electrode 82 may include low-cost metals such as copper or nickel-copper alloys. The thickness of the first electroplating electrode 81 may be 5-20 μm.

[0248] The material of the second metal seed layer 62 may include metals or metal alloys such as copper, aluminum, nickel, and titanium. The thickness of the second metal seed layer 62 may be 10-200 nm.

[0249] The material of the electrode protective layer 73 may include at least one of nickel, tin, silver, etc.

[0250] In this embodiment, the protective layer 50 can, for example, be configured as shown in Figures 2, 4A, 5, and 7, completely covering the first surface F and at least a portion of the side surface C of the substrate 10. Alternatively, in other embodiments, as shown in Figures 1 and 6, the protective layer 50 can completely cover the first surface F, with the outer contour edge of the protective layer 50 coinciding with the edge of the first surface F. That is, the protective layer 50 is entirely located on one side of the first surface F and does not extend to the side surface C.

[0251] In this embodiment of the application, as described above, the first transparent conductive layer 41 and the protective layer 50 are stacked on the side of the first doped layer 31 away from the substrate 10, and their stacking order can be interchanged.

[0252] Referring to Figures 1, 2, and 3, in some embodiments, a first transparent conductive layer 41 is disposed on the surface of the first doped layer 31 facing away from the substrate 10. A protective layer 50 is located on the side of the first transparent conductive layer 41 facing away from the substrate 10. A first electroplating electrode 81 is disposed on the protective layer 50 and electrically connected to the first transparent conductive layer 41 through the protective layer 50. In this configuration, the first transparent conductive layer 41 is first formed on the first doped layer 31, and then the protective layer 50 is deposited and formed on the first transparent conductive layer 41.

[0253] Further, referring to Figure 1, the protective layer 50 completely covers the first surface F, and the outer contour edge of the protective layer 50 coincides with the edge of the first surface F. At this time, a portion of the protective layer 50 is stacked on the surface of the first transparent conductive layer 41 facing away from the substrate 10, and another portion of the protective layer 50 is stacked on the surface of the first doped layer 31 corresponding to the isolation region W. This arrangement of the protective layer 50 completely covers and protects the exposed surface of the first doped layer 31, and avoids it being positioned on the side C, which is beneficial for improving battery efficiency.

[0254] Referring to Figure 2, in other embodiments, the protective layer 50 may completely cover the first surface F and at least a portion of the side surface C of the substrate 10. The coverage area of ​​the protective layer 50 on the side surface C can be set according to actual needs; for example, it may completely cover the side surface C or only cover the portion of the side surface C adjacent to the first surface F.

[0255] The second transparent conductive layer 42 may cover at least a portion of the second surface S and the side surface C of the substrate 10. In some embodiments, on the side surface C of the substrate 10, a portion of the protective layer 50 is stacked onto the side of the second transparent conductive layer 42 facing away from the substrate 10. The coverage area of ​​the second transparent conductive layer 42 on the side surface C can be set according to actual needs; for example, it may cover the portion of the side surface C adjacent to the second surface S, or it may completely cover the side surface C.

[0256] In some embodiments, the protective layer 50 may cover part but not all of the first surface F. For example, referring to FIG3, the outer contour edge of the protective layer 50 may coincide with the edge of the first electroplated electrode 81. Thus, the protective layer 50 is actually stacked between the first transparent conductive layer 41 and the first electroplated electrode 81. In the case where the heterojunction cell 100 also includes a first metal seed layer 61, the protective layer 50 is stacked between the first metal seed layer 61 and the first transparent conductive layer 41. In some embodiments, after the first electroplated electrode 81 is formed, the protective layer 50 in other areas can be removed using the first electroplated electrode 81 as a mask to obtain the heterojunction cell 100 of FIG3. It is understood that in the final structure of the heterojunction cell 100, the protective layer 50 is not necessarily to be removed; removing the protective layer 50 in other areas is an optional step.

[0257] In some embodiments, such as the examples in Figures 1, 2, and 3, the protective layer 50 is sandwiched between the first transparent conductive layer 41 and the first electroplated electrode 81. To prevent the protective layer 50 from affecting the carrier collection efficiency, the protective layer 50 can be made of a conductive material. In some embodiments, the protective layer 50 includes a transparent conductive oxide layer, which includes at least one of an ITO film, an IMO film, an AZO film, a SCOT film, and a SnOx film. Further, the thickness of the protective layer 50 is 5-15 nm. In some embodiments, the material of the protective layer 50 may include SnOx. Because the SnOx-containing film layer has better chemical resistance and lower conductivity relative to the first transparent conductive layer 41, it can effectively serve as a protective layer while also preventing short circuits that may occur when the protective layer 50 is in contact with both the first transparent conductive layer 41 and the second transparent conductive layer 42.

[0258] Furthermore, the protective layer 50 is a single-layer structure or a composite layer structure consisting of multiple layers of sub-films made of different materials. The single-layer structure may include one of ITO film, IMO film, AZO film, SCOT film, and SnOx film. The film materials of each sub-film layer in the composite layer structure may be different, and the sub-film layers may be one of ITO film, IMO film, AZO film, SCOT film, and SnOx film.

[0259] It is understood that the material of the protective layer 50 is not limited to the embodiment in which the protective layer 50 is sandwiched between the first transparent conductive layer 41 and the first electroplated electrode 81, but can also be used in the embodiment in which the protective layer 50 is sandwiched between the first doped layer 31 and the first transparent conductive layer 41.

[0260] Referring to Figures 4A, 4B, 5, 6, and 7, in some embodiments, the protective layer 50 is disposed on the surface of the first doped layer 31 facing away from the substrate 10. A first transparent conductive layer 41 is located on the side of the protective layer 50 facing away from the substrate 10. In this case, the first electroplating electrode 81 is disposed on the first transparent conductive layer 41.

[0261] In some embodiments, referring to FIG6, the protective layer 50 completely covers the first surface F, and the outer contour edge of the protective layer 50 coincides with the edge of the first surface F. Thus, the protective layer 50 is only disposed on one side of the first surface F and not on the side surface C. The protective layer 50 can be insulated from the second transparent conductive layer 42 extending to the side surface C, which can further improve the battery efficiency of the heterojunction cell 100. It is understood that even if the protective layer 50 extends to the side surface C and simultaneously contacts the first transparent conductive layer 41 and the second transparent conductive layer 42, the resulting efficiency loss will be far less than the efficiency gain brought to the heterojunction cell 100 by the presence of the protective layer 50. In some embodiments, the protective layer 50 can be made of a material with high sheet resistance, which can effectively avoid this efficiency loss. That is, the sheet resistance of the protective layer 50 can be greater than the sheet resistance of the second transparent conductive layer 42.

[0262] In other embodiments, referring to Figures 4A, 5, and 7, the protective layer 50 completely covers the first surface F and covers at least a portion of the side surface C of the substrate 10.

[0263] Referring to Figures 4A and 7, in some embodiments, the second doped layer 32 covers at least a portion of the second surface S and the side surface C, the first doped layer 31 covers at least a portion of the first surface F and the side surface C, and on the side surface C of the substrate 10, a portion of the structure of the first doped layer 31 is stacked onto the side of the second doped layer 32 opposite to the substrate 10.

[0264] On the side surface C of the substrate 10, a protective layer 50 is at least partially stacked on the surface of the first doped layer 31 facing away from the substrate 10. A second transparent conductive layer 42 covers at least a portion of the second surface S and the side surface C of the substrate 10. On the side surface C of the substrate 10, a portion of the structure of the second transparent conductive layer 42 is stacked onto the side of the protective layer 50 facing away from the substrate 10. That is, on the side surface C, a portion of the structure of the second transparent conductive layer 42 is stacked on the second doped layer 32, and a portion is stacked on the protective layer 50. The portion of the second transparent conductive layer 42 on the side surface C may completely cover the side surface C, or may only cover the portion of the side surface C adjacent to the second surface S.

[0265] In some embodiments, referring to FIG4A, in the portion of the protective layer 50 covering side C, a portion of the structure is stacked to the first doped layer 31, and another portion of the structure is stacked to the second doped layer 32. That is, the protective layer 50 extends to the second doped layer 32.

[0266] In other embodiments, referring to FIG7, the outer contour edge of the protective layer 50 coincides with the outer contour edge of the first doped layer 31. That is, the area of ​​the protective layer 50 coincides with the area of ​​the first doped layer 31. In this case, the first doped layer 31 may include an oxygen-free microcrystalline host layer, and the protective layer 50 may be an oxygen-doped amorphous silicon layer. This gives the protective layer 50 better corrosion resistance. In this case, the thickness of the protective layer 50 is no greater than 3 nm. In the example of FIG7, the protective layer 50 can be formed after the formation of the first doped layer 31, so as to be stacked on the surface of the first doped layer 31.

[0267] In some embodiments, referring to FIG4B, the protective layer 50 may cover part but not all of the first surface F, and the area of ​​the protective layer 50 on one side of the first surface F is the same as the area of ​​the first transparent conductive layer 41. The protective layer 50 may further cover at least a portion of the side surface C of the substrate 10. In some embodiments, after forming the first transparent conductive layer 41 and the second transparent conductive layer 42, the protective layer 50 in other areas can be removed using the first transparent conductive layer 41 and the second transparent conductive layer 42 as a mask to obtain the heterojunction cell 100 of FIG4B. That is, compared with FIG4A, it is obtained by removing the portion of the protective layer 50 located on the isolation region W. It can be understood that in the final structure of the heterojunction cell 100, the protective layer 50 is not necessarily to be removed, and the removal of the protective layer 50 in other areas is an optional step.

[0268] In some embodiments, the first doped layer 31 may further include an oxygen-containing microcrystalline sublayer, which is stacked between the first intrinsic silicon layer 21 and the oxygen-free microcrystalline host layer. In this way, during the formation of the first doped layer 31, the oxygen-containing microcrystalline sublayer can serve as an incubation layer, and the oxygen-free microcrystalline host layer is deposited on the oxygen-containing microcrystalline sublayer, which is beneficial for crystallization.

[0269] Referring to FIG5, in some embodiments, the second transparent conductive layer 42 covers at least a portion of the second surface S and the side surface C of the substrate 10. On the side surface C of the substrate 10, a portion of the structure of the protective layer 50 is stacked onto the side of the second transparent conductive layer 42 facing away from the substrate 10. That is, on the side surface C, the second transparent conductive layer 42 is inside the heterojunction cell 100, and the protective layer 50 is on the outside.

[0270] In some embodiments, particularly those of FIG4A, FIG5, and FIG6, the protective layer 50 comprises a transition metal oxide, and the conductivity type of the protective layer 50 is the same as that of the first doped layer 31.

[0271] In other embodiments, the protective layer 50 includes a dielectric passivation layer.

[0272] In other embodiments, the protective layer 50 includes a transparent conductive oxide layer.

[0273] In embodiments where the protective layer 50 comprises a transition metal oxide, the transition metal oxide can be an undoped carrier transport layer. When the first doped layer 31 is p-type doped, the conductivity type of the transition metal oxide is also p-type, and the protective layer 50 can include at least one of MO3, V2O5, CrO3, NiO, Cu2O, CoO, and ReO3. When the first doped layer 31 is n-type doped, the conductivity type of the transition metal oxide is also n-type, and the protective layer 50 can include at least one of TiO2, ZnO, Ta2O5, Nb2O5, CdO, MgO, BaO, SnO2, LiF, TiN, and TaN. When the protective layer 50 comprises a transition metal oxide, the thickness of the protective layer 50 can be 5-30 nm. It is understood that while the protective layer 50 protects the corresponding isolation region W of the first doped layer 31, it can also provide field passivation because its conductivity type is the same as that of the first doped layer 31.

[0274] In embodiments where the protective layer 50 includes a dielectric passivation layer, the material of the dielectric passivation layer can be SiOx, AlOx, etc., and the thickness of the protective layer 50 can be 0.5-3 nm. In this case, the protective layer 50 can effectively passivate the surface of the first doped layer 31 while protecting the corresponding isolation region W portion of the first doped layer 31. Due to the relatively thin thickness, carriers can effectively tunnel through.

[0275] In an example where the protective layer 50 includes a transparent conductive oxide layer, the transparent conductive oxide layer may include, for example, SnOx, ITO, IMO, SCOT, AZO, etc. In this case, the thickness of the protective layer 50 can be 5-15 nm. Exemplarily, the material of the protective layer 50 can be selected to better match the work function of the first doped layer 31. Alternatively, the work function can be adjusted through the deposition process. For example, if the first doped layer 31 is p-type doped, a TCO material with a high work function can be selected as the protective layer 50, or the work function of the protective layer 50 can be increased by adjusting the oxygen content during the TCO material deposition process, etc., so that it has a smaller contact resistance with the p-type first doped layer 31.

[0276] In some embodiments, referring to FIG27, the protective layer 50 may cover only a portion of the corresponding isolation region W of the first doped layer 31 on the first surface F side. For example, the portion of the protective layer 50 on the first surface F may completely overlap with the isolation region W. The protective layer 50 may further cover the side surface C. The structure and material of each film layer, such as the first intrinsic silicon layer 21, the first doped layer 31, the first transparent conductive layer 41, the second intrinsic silicon layer 22, the second doped layer 32, and the second transparent conductive layer 42, are the same as described above and have been discussed in detail previously, so they will not be repeated here.

[0277] In this embodiment, the protective layer 50 may include materials such as thermosetting / thermoplastic resins, UV-curable resins, and nanomaterials. For example, a coating of silicone resin, epoxy resin, or nano-silica may be used, and it can be applied by spraying, spin coating, or other methods to cover the corresponding isolation region W of the first doped layer 31 and the side surface C, forming a protective layer. This protective layer 50 can have good chemical resistance and a certain back reflection effect, which can improve the current of the heterojunction cell.

[0278] The following describes a method for manufacturing a heterojunction solar cell 100 provided in the embodiments of this application. It can be understood that the heterojunction solar cell 100 of the above embodiments can be manufactured by, but is not limited to, the following methods.

[0279] For the specific embodiments shown in the accompanying drawings, heterojunction cells fabricated using the methods described in Figures 9A-13 can be referred to Figures 1, 2, and 3. Heterojunction cells fabricated using the methods described in Figures 14A-17 can be referred to Figure 4A. Heterojunction cells fabricated using the methods described in Figures 18-21 can be referred to Figures 5, 6, and 22. Heterojunction cells fabricated using the methods described in Figures 23-26 can be referred to Figure 7.

[0280] Referring to Figures 8, 9A-26, this application provides a method for fabricating a heterojunction solar cell, the method comprising:

[0281] S10. A substrate 101 is provided, the substrate 101 including a substrate 10, and a first intrinsic silicon layer 21 and a first doped layer 31 sequentially stacked on the first surface F of the substrate 10.

[0282] S20. A first transparent conductive layer 41 and a protective material layer 500 are formed on the side of the first doped layer 31 away from the substrate 10. The first transparent conductive layer 41 covers a portion of the first surface F, and the first surface F includes an isolation region W not covered by the first transparent conductive layer 41. The protective material layer 500 completely covers the first surface F, and a portion of the structure of the protective material layer 500 is stacked on the corresponding isolation region W of the first doped layer 31.

[0283] S30. A first electroplating electrode 81 is formed on the side of the protective material layer 500 away from the substrate 10 by electroplating. The first electroplating electrode 81 is electrically connected to the first transparent conductive layer 41.

[0284] By forming a protective material layer 500, a portion of the protective material layer 500 is stacked on the corresponding isolation region W of the first doped layer 31. A first electroplating electrode 81 is formed on the side of the protective material layer 500 facing away from the substrate 10 through electroplating. During the electroplating process of the first electroplating electrode 81, the portion of the corresponding isolation region W of the first doped layer 31 is protected by the protective material layer 500 and therefore will not be eroded by the plating solution. The surface structure of the portion of the corresponding isolation region W of the first doped layer 31 will not have defects. Compared to related technologies where the first doped layer is partially etched away, resulting in insufficient lateral conductivity and poor carrier collection ability, the lateral conductivity and carrier collection ability of the first doped layer 31 are not affected, thus effectively avoiding the decrease in battery efficiency caused by corrosion and damage to the first doped layer 31. Furthermore, since the protective material layer 500 is stacked on the portion of the first doped layer 31 corresponding to the isolation region W, the passivation ability of the first doped layer 31 is also improved, thereby improving the efficiency of the heterojunction battery 100. Furthermore, the protective material layer 500 completely covers the first surface F, which can further enhance the anti-reflection effect on one side of the first surface F.

[0285] In some embodiments, in step S20, the step of forming the protective material layer 500:

[0286] Referring to Figures 11, 14A, 19, and 23, the second surface S side of the substrate 101 is oriented toward the bearing frame of the carrier plate, and a protective material layer 500 is formed on the side of the first doped layer 31 facing away from the substrate 10.

[0287] The protective material layer 500 completely covers the first surface F and at least a portion of the side surface C of the substrate 10. Alternatively, the protective material layer 500 completely covers the first surface F, and the outer contour edge of the protective material layer 500 coincides with the edge of the first surface F.

[0288] This configuration ensures that the protective material layer 500 can fully cover the first surface F without leaving any uncovered areas, particularly covering the surface of the corresponding isolation region W of the first doped layer 31. During this process, the protective material layer 500 also forms on the side surface C.

[0289] In some embodiments, in step S20, the step of forming the first transparent conductive layer 41:

[0290] Referring to Figures 9B, 10, 14B, 15, 19, and 24, the first surface F of the substrate 101 faces the supporting frame 1 of the carrier plate. A first transparent conductive layer 41 is formed on the side of the first doped layer 31 facing away from the substrate 10, and the formation position of the first transparent conductive layer 41 corresponds to the hollow portion of the supporting frame 1. At this time, the isolation region W on the first surface F is also the part of the area facing the supporting frame 1 of the carrier plate. Corresponding to the shape of the supporting frame 1, the isolation region W can be square when viewed from the first surface F.

[0291] In some embodiments, such as for the heterojunction battery 100 with the structure shown in Figures 1-3, a first transparent conductive layer 41 may be formed first, followed by a protective material layer 500.

[0292] During fabrication, referring to Figures 10 and 11, step S20, which involves forming a first transparent conductive layer 41 and a protective material layer 500 stacked on the surface of the first doped layer 31 facing away from the substrate 10, may specifically include:

[0293] A first transparent conductive layer 41 is formed on the surface of the first doped layer 31 away from the substrate 10.

[0294] A protective material layer 500 is formed on the surface of the first transparent conductive layer 41 that is away from the substrate 10.

[0295] Specifically, in some embodiments, referring to Figures 9A, 9B, and 10, the step of forming a first transparent conductive layer 41 on the surface of the first doped layer 31 facing away from the substrate 10 specifically includes:

[0296] The first surface F side of the substrate 101 is oriented toward the support frame 1 of the carrier plate, and the portion of the first doped layer 31 located on the first surface F side is supported on the support frame 1.

[0297] In the portion of the first doped layer 31 covering one side of the first surface F, the area not obscured by the bearing frame 1 forms a first transparent conductive layer 41.

[0298] Further, referring to FIG11, the step of forming a protective material layer 500 on the surface of the first transparent conductive layer 41 facing away from the substrate 10 specifically includes:

[0299] The second surface S side of the substrate 101 is supported by the support frame of the carrier plate.

[0300] A protective material layer 500 is formed on the surface of the first transparent conductive layer 41 facing away from the substrate 10. The protective material layer 500 is partially stacked on the surface of the first transparent conductive layer 41 facing away from the substrate 10, and partially stacked on the surface of the portion of the first doped layer 31 corresponding to the isolation region W. This arrangement facilitates the protective material layer 500 completely covering one side of the first surface F. In some embodiments, the protective material layer 500 may also cover the entire side surface C.

[0301] In some embodiments, referring to Figures 9A, 10, and 11, the substrate 101 further includes a second intrinsic silicon layer 22 and a second doped layer 32 sequentially stacked on the second surface S of the substrate 10, with the second surface S disposed opposite to the first surface F. The process includes, after the step of forming the first transparent conductive layer 41 and before the step of forming the protective material layer 500, the following steps are also included:

[0302] A second transparent conductive layer 42 is formed on the side of the second doped layer 32 facing away from the substrate 10.

[0303] In this embodiment, the second transparent conductive layer 42 covers at least a portion of the second surface S and the side surface C of the substrate 10. In some embodiments, referring to FIG11, the protective material layer 500 may also cover at least a portion of the side surface C, and a portion of the structure of the protective material layer 500 may be stacked on the side of the second transparent conductive layer 42 facing away from the substrate 10. Alternatively, in other embodiments, the outer contour edge of the protective material layer 500 may coincide with the edge of the first surface F. The coincidence of the outer contour edge of the protective material layer 500 with the edge of the first surface F means that the entire protective material layer 500 is located on one side of the first surface F.

[0304] In other embodiments, such as for the heterojunction cell 100 with the structure shown in Figures 4A-7, a protective material layer 500 may be formed first, followed by the formation of a first transparent conductive layer 41.

[0305] During fabrication, refer to Figures 14A, 14B, 15, 19, 23, and 24. Step S20, which involves forming a first transparent conductive layer 41 and a protective material layer 500 stacked on the surface of the first doped layer 31 facing away from the substrate 10, may specifically include:

[0306] A protective material layer 500 is formed on the surface of the first doped layer 31 away from the substrate 10.

[0307] A first transparent conductive layer 41 is formed on the surface of the protective material layer 500 away from the substrate 10.

[0308] Specifically, in some embodiments, referring to Figures 4A and 14A-17, Figure 7 and 23-26, the step of forming a protective material layer 500 on the surface of the first doped layer 31 facing away from the substrate 10 includes:

[0309] A protective material layer 500 is formed on the side of the first doped layer 31 facing away from the substrate 10. The protective material layer 500 covers at least a portion of the first surface F and the side surface C. The protective material layer 500 may cover the entire side surface C or cover the area of ​​the side surface C adjacent to the first surface F.

[0310] It is understandable that in this step, the protective material layer 500 can be formed with one side of the second surface S of the substrate 101 supported by the support frame of the carrier plate. This facilitates the formation of a protective material layer 500 that covers the entire surface of the first surface F.

[0311] Further, referring to Figures 14B, 15, and 24, the step of forming a first transparent conductive layer 41 on the surface of the protective material layer 500 facing away from the substrate 10 specifically includes:

[0312] The first surface F side of the substrate 101 is oriented toward the bearing frame 1 of the carrier plate, and the portion of the protective material layer 500 located on the first surface F side is supported by the bearing frame 1.

[0313] In the portion of the protective material layer 500 covering one side of the first surface F, a first transparent conductive layer 41 is formed in the area not obscured by the bearing frame 1.

[0314] In some embodiments, the substrate 101 further includes a second intrinsic silicon layer 22 and a second doped layer 32 sequentially stacked on the second surface S. Continuing to refer to Figures 15 and 24, after the step of forming the first transparent conductive layer 41 on the surface of the protective material layer 500 facing away from the substrate 10, the method further includes:

[0315] A second transparent conductive layer 42 is formed on the surface of the second doped layer 32 facing away from the substrate 10. The second transparent conductive layer 42 covers at least a portion of the second surface S and the side surface C, and the second transparent conductive layer 42 is stacked onto the protective material layer 500. The second transparent conductive layer 42 may cover the entire side surface C, or the second transparent conductive layer 42 may only cover the area of ​​the side surface C adjacent to the second surface S.

[0316] In some embodiments, referring to Figures 4A and 11, in the step of forming a protective material layer 500 on the surface of the first doped layer 31 facing away from the substrate 10:

[0317] The protective material layer 500 covers at least a portion of the first surface F and the side surface C. On the side surface C, the protective material layer 500 is stacked onto the side of the second doped layer 32 opposite to the substrate 10.

[0318] In other embodiments, referring to Figures 7 and 23, in the step of forming a protective material layer 500 on the surface of the first doped layer 31 facing away from the substrate 10:

[0319] The protective material layer 500 covers at least a portion of the first surface F and the side surface C. On the side surface C, the outer contour edge of the protective material layer 500 coincides with the outer contour edge of the first doped layer 31. That is, the protective material layer 500 and the first doped layer 31 have the same film layer coverage.

[0320] Referring again to Figures 7 and 23, the first doped layer 31 may include an oxygen-free microcrystalline host layer.

[0321] The steps for forming the protective material layer 500 include:

[0322] An oxygen-doped amorphous silicon layer is formed on the surface of the first doped layer 31 away from the substrate 10 as a protective material layer 500. The oxygen-doped amorphous silicon layer has the same doping type as the first doped layer 31. Since the oxygen-doped amorphous silicon layer has better resistance to chemical corrosion, it provides better protection for the first doped layer 31.

[0323] In some embodiments, the first doped layer 31 further includes an oxygen-containing microcrystalline film layer, which is stacked between the first intrinsic silicon layer 21 and the oxygen-free microcrystalline host layer.

[0324] Furthermore, the oxygen-containing microcrystalline sublayer and the oxygen-free microcrystalline host layer included in the first doped layer 31 can be formed by the following steps:

[0325] Hydrogen, silane, diborane, and carbon dioxide gases are introduced into the reaction chamber. The molar volume ratio of hydrogen, silane, diborane, and carbon dioxide gases can be from 300:1:0.005:0.2 to 600:1:0.01:0.5. The reaction pressure in the reaction chamber can be 4-6 mbar, so as to form an oxygen-containing microcrystalline film layer on the surface of the first intrinsic silicon layer 21 away from the substrate 10.

[0326] Hydrogen, silane, and diborane gases are introduced into the reaction chamber. The molar volume ratio of hydrogen, silane, and diborane gases can be from 300:1:0.01 to 500:1:0.04. The reaction pressure in the reaction chamber can be 2-3 mbar, so as to form an oxygen-free microcrystalline host layer on the surface of the oxygen-containing microcrystalline film layer away from the substrate 10.

[0327] Furthermore, the step of forming an oxygen-doped amorphous silicon layer as a protective material layer 500 may include:

[0328] Hydrogen, silane, diborane, and carbon dioxide gases are introduced into the reaction chamber, wherein the molar volume ratio of hydrogen, silane, diborane, and carbon dioxide gases can be from 8:1:3:1 to 12:1:5:1.5. The reaction pressure inside the reaction chamber can be approximately 2-3 mbar to form an oxygen-doped amorphous silicon layer on the surface of the oxygen-free microcrystalline substrate.

[0329] In some embodiments, such as the heterojunction cell 100 illustrated in Figures 5, 6, and 22, in conjunction with Figures 18-22, the step of forming a protective material layer 500 on the surface of the first doped layer 31 facing away from the substrate 10 further includes:

[0330] A second transparent conductive layer 42 is formed on the surface of the second doped layer 32 facing away from the substrate 10. The second transparent conductive layer 42 covers at least a portion of the second surface S and the side surface C. The second transparent conductive layer 42 may cover the entire side surface C, or it may only cover the area of ​​the side surface C adjacent to the second surface S.

[0331] In some embodiments, referring to FIG19, the step of forming a protective material layer 500 on the surface of the first doped layer 31 facing away from the substrate 10 specifically includes:

[0332] A protective material layer 500 is formed on the side of the first doped layer 31 away from the substrate 10. The protective material layer 500 completely covers the first surface F and covers at least a portion of the side surface C. The protective material layer 500 is stacked onto the second transparent conductive layer 42.

[0333] In some embodiments, before forming the protective material layer 500, the second surface S side of the substrate 101 can be oriented towards the support frame of the carrier plate, and the second transparent conductive layer 42 can be supported on the support frame. In this way, the formed protective material layer 500 can cover the entire first surface F.

[0334] In some embodiments, the step of forming a first transparent conductive layer 41 on the surface of the protective material layer 500 facing away from the substrate 10 specifically includes:

[0335] The first surface F side of the substrate 101 is oriented toward the bearing frame of the carrier plate, and the portion of the protective material layer 500 located on the first surface F side is supported by the bearing frame.

[0336] In the portion of the protective material layer 500 covering one side of the first surface F, a first transparent conductive layer 41 is formed in the area not obscured by the bearing frame.

[0337] In some embodiments, such as for the heterojunction solar cell 100 illustrated in FIG4A, FIG5, FIG6, and FIG22, the protective material layer 500 may include a transition metal oxide, and the conductivity type of the protective material layer 500 is the same as that of the first doped layer 31. Alternatively, the protective material layer 500 may include a dielectric passivation layer. Or, the protective material layer 500 may include a transparent conductive oxide layer.

[0338] In embodiments where the protective material layer 500 includes a transition metal oxide, the transition metal oxide can be an undoped carrier transport layer. When the first doped layer 31 is p-type doped, the conductivity type of the transition metal oxide is also p-type. The protective material layer 500 can include, for example, at least one of MO3, V2O5, CrO3, NiO, Cu2O, CoO, and ReO3. When the first doped layer 31 is n-type doped, the conductivity type of the transition metal oxide is also n-type. The protective material layer 500 can include, for example, at least one of TiO2, ZnO, Ta2O5, Nb2O5, CdO, MgO, BaO, SnO2, LiF, TiN, and TaN. When the protective material layer 500 includes a transition metal oxide, the thickness of the protective material layer 500 can be 5-30 nm. It is understood that while the protective material layer 500 protects the corresponding isolation region W of the first doped layer 31, it can also provide field passivation because its conductivity type is the same as that of the first doped layer 31.

[0339] In embodiments where the protective material layer 500 includes a dielectric passivation layer, the dielectric passivation layer can be made of materials such as SiOx or AlOx, and the thickness of the protective material layer 500 can be 0.5-3 nm. In this case, the protective material layer 500 can effectively passivate the surface of the first doped layer 31 while also protecting the corresponding isolation region W portion of the first doped layer 31. Due to its relatively thin thickness, it allows for effective carrier tunneling.

[0340] In an example where the protective material layer 500 includes a transparent conductive oxide layer, the transparent conductive oxide layer may include, for example, SnOx, ITO, IMO, SCOT, AZO, etc. In this case, the thickness of the protective material layer 500 can be 5-15 nm. Exemplarily, the material of the protective material layer 500 can be selected to better match the work function of the first doped layer 31. Alternatively, the work function can be adjusted through the deposition process. For example, if the first doped layer 31 is p-type doped, a TCO material with a high work function is selected as the protective material layer 500, or the work function of the protective material layer 500 can be increased by adjusting the oxygen content during the TCO material deposition process, etc., so that it has a smaller contact resistance with the p-type first doped layer 31.

[0341] In some embodiments, the method for fabricating a heterojunction solar cell further includes:

[0342] A second electroplating electrode 82 is formed on one side of the second surface S of the substrate 10 by electroplating.

[0343] In the embodiments described above, the protective material layer 500 completely covers the first surface F and at least a portion of the side surface C of the substrate 10. Alternatively, the protective material layer 500 only completely covers the first surface F and is not formed on other surfaces.

[0344] In some embodiments, during the steps of forming the first electroplated electrode 81 and the second electroplated electrode 82, at least a portion of the protective material layer 500 is also removed to form the protective layer 50. For example, the heterojunction cell 100 shown in FIG1, 3, 6, 22, 27.

[0345] In embodiments where the protective material layer 500 is partially removed, as shown in Figures 1 and 6, the removed portion of the protective material layer 500 includes the portion of the protective material layer 500 located on side C. Alternatively, as shown in Figure 22, the removed portion of the protective material layer 500 includes the portions covering side C and the isolation area W. Alternatively, as shown in Figure 3, the removed portion of the protective material layer 500 includes the portion covering side C and the portion corresponding to the non-metallic contact area of ​​the first surface F, i.e., removing the protective material layer 500 from the area other than the first electroplating electrode 81.

[0346] In some other embodiments, the step of removing part of the protective material layer 500 described above may be omitted. In this case, the protective material layer 500 is directly used as the protective layer 50, resulting in, for example, the heterojunction cell 100 shown in FIG2, FIG4A, FIG5, and FIG7.

[0347] In some embodiments, referring to Figures 12 and 13, 16 and 17, 20 and 21, 25 and 26, the steps of forming the first electroplating electrode 81 and forming the second electroplating electrode 82 specifically include:

[0348] A first metal seed material layer 610 is formed on one side of the first surface F of the substrate 10, and a second metal seed material layer 620 is formed on the surface of the second transparent conductive layer 42 that is away from the substrate 10. The first metal seed material layer 610 is located on the one that is farther away from the substrate 10, the first transparent conductive layer 41 and the protective material layer 500.

[0349] A first electroplating electrode 81 is formed by electroplating a patterned mask layer on the surface of a first metal seed material layer 610, and a second electroplating electrode 82 is formed by electroplating a patterned mask layer on the surface of a second metal seed material layer 620.

[0350] Remove the mask layer; and

[0351] The portion of the first metal seed material layer 610 not covered by the first electroplating electrode 81 is removed to form the first metal seed layer 61, and the portion of the second metal seed material layer 620 not covered by the second electroplating electrode is removed to form the second metal seed layer 62.

[0352] In some embodiments, the patterned mask layer is formed by the following steps:

[0353] A patterned first mask material layer 71 is formed on the side of the first metal seed material layer 610 and the second metal seed material layer 620 facing away from the substrate 10. The first mask material layer 71 is cut out at the position corresponding to the metal contact area Z of the first surface F, and also cut out at the position corresponding to the metal contact area Z of the second surface S. Insulating adhesive 72 is coated on the side surface C of the substrate 10. In this way, all surfaces of the substrate 101 are covered, exposing only the positions where the first electroplating electrode 81 and the second electroplating electrode 82 will be formed.

[0354] In some embodiments, after removing the portion of the first metal seed material layer 610 not covered by the first electroplating electrode 81 and the portion of the second metal seed material layer 620 not covered by the second electroplating electrode, the method further includes forming an electrode protective layer 73 on the surfaces of the first electroplating electrode 81 and the second electroplating electrode 82. The electrode protective layer 73 may be, for example, a chemical plating protective layer.

[0355] In some embodiments, at least a portion of the protective material layer 500 is removed to form a protective layer 50 in the steps of removing the portion of the first metal seed material layer 610 not covered by the first electroplating electrode 81, removing the portion of the second metal seed material layer 620 not covered by the second electroplating electrode 82, and / or forming the electrode protective layer 73. Since the steps of removing the portion of the first metal seed material layer 610 not covered by the first electroplating electrode 81, removing the portion of the second metal seed material layer 620 not covered by the second electroplating electrode, and / or forming the electrode protective layer 73 are all acidic, if the material of the protective layer 50 is not acid-resistant, the exposed portion of the protective layer 50 may be at least partially removed in these two steps.

[0356] In some embodiments, referring to FIG6, step S10, the step of providing a substrate 101 specifically includes:

[0357] A first intrinsic silicon layer 21 is formed on the first surface F of the substrate 10, and a second intrinsic silicon layer 22 is formed on the second surface S of the substrate 10; and

[0358] A second doped layer 32 is formed on the surface of the second intrinsic silicon layer 22 away from the substrate 10, and a first doped layer 31 is formed on the surface of the first intrinsic silicon layer 21 away from the substrate 10.

[0359] In the above steps, the first intrinsic silicon layer 21 covers at least a portion of the first surface F and the side surface C. The second intrinsic silicon layer 22 covers at least a portion of the second surface S and the side surface C, and a portion of the structure of the second intrinsic silicon layer 22 is stacked onto the side of the first intrinsic silicon layer 21 facing away from the substrate 10. The second doped layer 32 covers at least a portion of the second surface S and the side surface C, and a portion of the structure of the second doped layer 32 is stacked onto the side of the first intrinsic silicon layer 21 facing away from the substrate 10. The first doped layer 31 covers at least a portion of the first surface F and the side surface C, and a portion of the structure of the first doped layer 31 is stacked onto the side of the second doped layer 32 facing away from the substrate 10.

[0360] The following examples illustrate the fabrication method of heterojunction solar cells according to embodiments of this application.

[0361] Example 1

[0362] The method for fabricating a heterojunction cell in this embodiment is used to form the heterojunction cell 100 illustrated in Figures 1, 2, and 3.

[0363] Methods for fabricating heterojunction solar cells include:

[0364] Step A: Prepare a silicon wafer as substrate 10, clean it, and texturize it. Texturing can be done on both sides, or texturing can be done on the second surface S of substrate 10 while polishing the first surface F of substrate 10. It is understood that, in this embodiment, the texturized structure of the first surface F and / or the second surface S is omitted for ease of observation.

[0365] Step B: Referring to Figure 9A, a first intrinsic silicon layer 21 is formed on the first surface F of the substrate 10, and a second intrinsic silicon layer 22 is formed on the second surface S of the substrate 10. The first intrinsic silicon layer 21 covers the first surface F and partially covers the side surface C. The second intrinsic silicon layer 22 covers the second surface S and partially covers the side surface C. A portion of the second intrinsic silicon layer 22 also covers the first intrinsic silicon layer 21. The first intrinsic silicon layer 21 and the second intrinsic silicon layer 22 are generally formed using a plate-type device, therefore it is a single-sided film deposition method.

[0366] Step C: Continuing with reference to FIG9A, a second doped layer 32 is formed on the surface of the second intrinsic silicon layer 22 facing away from the substrate 10, and a first doped layer 31 is formed on the surface of the first intrinsic silicon layer 21 facing away from the substrate 10, thus forming the substrate 101. A portion of the second doped layer 32 is located on one side of the second surface S, and a portion is located on the side surface C. The portion of the second doped layer 32 located on the side surface C covers the portion of the second intrinsic silicon layer 22 located on the side surface C, and also covers a portion of the first intrinsic silicon layer 21. A portion of the first doped layer 31 is located on one side of the first surface F, and a portion is located on the side surface C. The portion of the first doped layer 31 located on the side surface C covers the portion of the first intrinsic silicon layer 21 located on the side surface C, and also covers a portion of the second doped layer 32.

[0367] Step D: Referring to Figure 10, the substrate 10 with the first doped layer 31 formed is placed on a carrier plate (not shown). That is, with the first surface F of the substrate 10 facing the carrier plate, the side of the substrate 10 with the first doped layer 31 formed is placed on the support frame of the carrier plate. The portion of the edge of the first doped layer 31 corresponding to the isolation region W is blocked by the support frame of the carrier plate, and a local area inside the edge of the first doped layer 31 is exposed from the cutout area of ​​the support frame of the carrier plate. A first transparent conductive layer 41 is formed on the surface of the first doped layer 31 exposed from the support frame of the carrier plate. The first transparent conductive layer 41 is not formed on the portion of the first doped layer 31 that is blocked by the support frame of the carrier plate and corresponds to the isolation region W. Then, a second transparent conductive layer 42 is formed on the surface of the second doped layer 32 away from the substrate 10. Part of the structure of the second transparent conductive layer 42 is located on the side C. In the portion of the second transparent conductive layer 42 located on the side C, part of it can cover the second doped layer 32 and part of it can cover the first doped layer 31.

[0368] Step E: Referring to Figure 11, the structure formed in step D is flipped upside down so that the second surface S of the substrate 10 faces the carrier plate (the lower side in Figure 11). The side of the substrate 10 with the second doped layer 32 is supported on the carrier frame of the carrier plate. A protective material layer 500 is formed on the surface of the first transparent conductive layer 41 facing away from the substrate 10. The protective material layer 500 covers the entire first surface F and covers the corresponding isolation region W of the first doped layer 31. Part of the structure of the protective material layer 500 is also located on the side surface C. The portion of the protective material layer 500 covering the side surface C partially covers the portion of the first doped layer 31 located on the side surface and partially covers the portion of the second transparent conductive layer 42 located on the side surface.

[0369] Step F, Referring to Figure 12, a first metal seed material layer 610 is formed on the surface of the protective material layer 500 away from the substrate 10. The first metal seed material layer 610 is located on the first surface F and does not cover the isolation area W. A second metal seed material layer 620 is formed on the surface of the second transparent conductive layer 42 away from the substrate 10. Part of the structure of the second metal seed material layer 620 is located on one side of the second surface S, and part of the structure is located on the side C.

[0370] Step G, referring to Figure 13, print or spin-coat a front-side photoresist / photosensitive ink on one side of the first surface F and the second surface S of the structure formed in step F. After exposure and development, a patterned first mask material layer 71 is formed. The positions on the first mask material layer 71 corresponding to the metal contact areas Z of the first surface F and the second surface S are cut out. The remaining parts of the first surface F and the second surface S are covered by the first mask material layer 71, that is, the positions on the first metal seed material layer 610 and the second metal seed material layer 620 where the gate lines will be formed are exposed. And apply insulating adhesive 72 or other protective material to the side surface C of the structure formed in step F to edge the side surface C. Then, copper is electroplated to form a first electroplating electrode 81 on the first metal seed material layer 610 on the first surface F side of the substrate 10, and a second electroplating electrode 82 on the second metal seed layer 620 on the second surface S side of the substrate 10.

[0371] Then, a chemical solution, typically an alkaline solution, is used to clean and remove the first mask material layer 71 and the insulating adhesive 72. Since the corresponding isolation region W of the first doped layer 31 is covered by the protective material layer 500, the alkaline solution will not damage the first doped layer 31.

[0372] Step H, referring to Figures 13 and 2, uses a metal etching solution (e.g., H2SO4 + H2O2) to clean and remove the portion of the first metal seed material layer 610 not covered by the first electroplating electrode 81 to form the first metal seed layer 61. Similarly, it cleans and removes the portion of the second metal seed material layer 620 not covered by the second electroplating electrode 82 to form the second metal seed layer 62. Then, an electrode protective layer 73 (e.g., tin / silver) is formed on the side of the first and second electroplating electrodes 81 and 82 facing away from the substrate 10 by chemical plating or other methods, forming the heterojunction cell 100 as shown in Figure 2. The formation method of the electrode protective layer 73 is not limited to chemical plating; electroplating can also be used. It should be noted that in this step, the portion of the protective material layer 500 located on the side C or the first surface F may be partially removed to form the protective layer. In the example of Figure 2, part of the protective material layer 500 is located on one side of the first surface F, and part is located on the side C. That is, in the example of Figure 2, the protective material layer 500 is not removed. This heterojunction cell in Figure 2 is designated A1. In the example of Figure 1, after the protective material layer 500 is partially removed, the entire protective layer 50 formed is located on one side of the first surface F. This heterojunction cell in Figure 1 is designated A2. In the example of Figure 3, only the region of the protective material layer 500 corresponding to the metal contact area Z of the first surface F is retained to form the protective layer 50. That is, only the portion of the protective material layer 500 located under the first electroplating electrode 81 is retained, and the rest is removed. This heterojunction cell in Figure 3 is designated A3.

[0373] Example 2

[0374] The method for fabricating a heterojunction cell in this embodiment is used to form the heterojunction cell 100 illustrated in FIG4A.

[0375] This embodiment improves upon the steps of step D and thereafter, based on the first embodiment described above. Steps A, B, and C are the same as in the first embodiment and will not be repeated here.

[0376] After steps A, B, and C, the fabrication method of a heterojunction solar cell also includes:

[0377] Step 1: Referring to Figure 14, with the second surface S of the substrate 10 facing the carrier plate (the lower side in Figure 14), the side of the substrate 10 with the second doped layer 32 formed is placed on the carrier frame of the carrier plate. A protective material layer 500 is formed on the surface of the first doped layer 31 facing away from the substrate 10. The protective material layer 500 covers the entire first surface F and covers a portion of the corresponding isolation region W of the first doped layer 31. A portion of the protective material layer 500 is also located on the side surface C. In the portion of the protective material layer 500 covering the side surface C, a portion covers the portion of the first doped layer 31 located on the side surface C, and another portion covers the portion of the second doped layer 32 located on the side surface C.

[0378] Step J: Referring to Figure 15, the structure formed in Step I is flipped over so that the first surface F of the substrate 10 faces the carrier plate. The side of the substrate 10 with the protective material layer 500 is placed on the carrier frame of the carrier plate. The edge of the protective material layer 500 corresponding to the isolation region W is blocked by the carrier frame of the carrier plate. A local area inside the edge of the protective material layer 500 is exposed from the cutout area of ​​the carrier frame of the carrier plate. A first transparent conductive layer 41 is formed on the surface of the protective material layer 500 exposed from the carrier frame of the carrier plate. The position of the protective material layer 500 corresponding to the isolation region W is not formed with the first transparent conductive layer 41. Then, a second transparent conductive layer 42 is formed on the surface of the second doped layer 32 away from the substrate 10. Part of the structure of the second transparent conductive layer 42 is located on the side C. The second transparent conductive layer 42 covers part of the side C, and part of it can cover the second doped layer 32 and part of it can cover the protective material layer 500. In this embodiment, the protective material layer 500 can be a transition metal oxide with the same conductivity type as the first doped layer 31. Alternatively, the protective material layer 500 may include a dielectric passivation layer, such as SiOx, AlOx, etc. Alternatively, the protective material layer 500 may also include a transparent conductive oxide (TCO) layer, such as SnOx, ITO, IMO, SCOT, AZO, etc.

[0379] Step K: Referring to Figure 16, a first metal seed material layer 610 is formed on the surface of the first transparent conductive layer 41 away from the substrate 10. The first metal seed material layer 610 is located on the first surface F and does not cover the isolation area W. A second metal seed material layer 620 is formed on the surface of the second transparent conductive layer 42 away from the substrate 10. Part of the structure of the second metal seed material layer 620 is located on one side of the second surface S, and part of the structure is located on the side C.

[0380] Step L, referring to Figure 17, print or spin-coat a front-side photoresist / photosensitive ink on one side of the first surface F and the second surface S of the structure formed in step K. After exposure and development, a patterned first mask material layer 71 is formed. The positions on the first mask material layer 71 corresponding to the metal contact areas Z of the first surface F and the second surface S are cut out. The remaining parts of the first surface F and the second surface S are covered by the first mask material layer 71, that is, the positions on the first metal seed material layer 610 and the second metal seed material layer 620 where the gate lines will be formed are exposed. And apply insulating adhesive 72 or other protective material to the side surface C of the structure formed in step K to edge the side surface C. Then, copper is electroplated to form a first electroplating electrode 81 on the first metal seed material layer 610 on the first surface F side of the substrate 10, and a second electroplating electrode 82 on the second metal seed layer 620 on the second surface S side of the substrate 10.

[0381] Then, a chemical solution, typically an alkaline solution, is used to clean and remove the first mask material layer 71 and the insulating adhesive 72. Since the corresponding isolation region W of the first doped layer 31 is covered by the protective material layer 500, the alkaline solution will not damage the first doped layer 31.

[0382] Step M, referring to Figures 17 and 4A, uses a metal etching solution (e.g., H2SO4 + H2O2) to clean and remove the portion of the first metal seed material layer 610 not covered by the first electroplating electrode 81 to form the first metal seed layer 61. Similarly, it cleans and removes the portion of the second metal seed material layer 620 not covered by the second electroplating electrode 82 to form the second metal seed layer 62. Then, an electrode protective layer 73 (e.g., tin / silver) is formed on the side of the first and second electroplating electrodes 81 and 82 facing away from the substrate 10 by chemical plating or other methods, forming the heterojunction cell 100 as shown in Figure 4A. The electrode protective layer 73 can be formed by electroplating, not just chemical plating. It should be noted that in this step, the portion of the protective material layer 500 located on the side C or the first surface F is partially removed to form the protective layer 50. In the example of Figure 4A, part of the protective layer 50 is located on the first surface F, and part is located on the side C. The heterojunction cell in Figure 4A is designated A4. Alternatively, in some other embodiments, as shown in FIG4b, the portion of the protective material layer 500 not covered by the first transparent conductive layer 41 and not covered by the second transparent conductive layer 42 can be cleaned and removed, exposing the corresponding isolation region W of the first doped layer 31 to form the protective layer 50.

[0383] Example 3

[0384] The method for fabricating a heterojunction cell in this embodiment is used to form the heterojunction cell 100 illustrated in Figures 5, 6, and 22.

[0385] This embodiment improves upon the steps of step I and thereafter, based on the above embodiment two. Steps A, B, and C are the same as in embodiment two, and will not be repeated here.

[0386] After steps A, B, and C, the fabrication method of a heterojunction solar cell also includes:

[0387] Step N: Referring to Figure 18, the substrate 10 with the first doped layer 31 formed is placed on the support frame of the carrier plate (not shown). That is, with the first surface F of the substrate 10 facing the carrier plate, the side of the substrate 10 with the first doped layer 31 formed is placed on the support frame of the carrier plate. A second transparent conductive layer 42 is formed on the surface of the second doped layer 32 away from the substrate 10. Part of the structure of the second transparent conductive layer 42 is located on the second surface S side, and part of the structure is located on the side C side. The second transparent conductive layer 42 covers the part of the side C side, and part of it can cover the second doped layer 32 and part of it can cover the first doped layer 31.

[0388] Step O: Referring to Figure 19, with the second surface S side of the substrate 10 facing the carrier plate, the side of the substrate 10 with the second doped layer 32 formed is placed on the carrier frame of the carrier plate. A protective material layer 500 is formed on the surface of the first doped layer 31 facing away from the substrate 10. The protective material layer 500 corresponds to the entire first surface F and covers a portion of the corresponding isolation region W of the first doped layer 31. A portion of the structure of the protective material layer 500 is also located on the side C. In the portion of the protective material layer 500 covering the side C, a portion covers the portion of the first doped layer 31 located on the side C, and a portion covers the portion of the second transparent conductive layer 42 located on the side C. Then, the substrate 10 is flipped upside down so that with the first surface F side of the substrate 10 facing the carrier plate, the side of the substrate 10 with the protective material layer 500 formed is placed on the carrier frame of the carrier plate. The edge position of the protective material layer 500 corresponding to the isolation region W is blocked by the carrier frame of the carrier plate. In the protective material layer 500, a local area inside the edge position is exposed from the cutout area of ​​the carrier frame of the carrier plate. A first transparent conductive layer 41 is formed on the surface of the exposed area of ​​the bearing frame of the self-supporting plate of the protective material layer 500, but no first transparent conductive layer 41 is formed on the protective material layer 500 at the position corresponding to the isolation area W.

[0389] Step P, referring to Figure 20, a first metal seed material layer 610 is formed on the surface of the first transparent conductive layer 41 away from the substrate 10. The first metal seed material layer 610 is located on one side of the first surface F, but does not cover the isolation area W. A second metal seed material layer 620 is formed on the surface of the second transparent conductive layer 42 away from the substrate 10. Part of the structure of the second metal seed material layer 620 is located on one side of the second surface S, and part of the structure is located on the side C.

[0390] Step Q: Referring to Figure 21, print or spin-coat a front-side photoresist / photosensitive ink on one side of the first surface F and the second surface S of the structure formed in step P. After exposure and development, a patterned first mask material layer 71 is formed. The positions on the first mask material layer 71 corresponding to the metal contact areas Z of the first surface F and the second surface S are cut out. The remaining portions of the first surface F and the second surface S are covered by the first mask material layer 71, exposing the positions on the first metal seed material layer 610 and the second metal seed material layer 620 where the gate lines will be formed. Then, apply insulating adhesive 72 or other protective material to the side surface C of the structure formed in step P to edge the side surface C. Next, electroplating copper is performed to form a first electroplating electrode 81 on the first metal seed material layer 610 on the first surface F side of the substrate 10, and a second electroplating electrode 82 on the second metal seed layer 620 on the second surface S side of the substrate 10.

[0391] Then, a chemical solution, typically an alkaline solution, is used to clean and remove the first mask material layer 71 and the insulating adhesive 72. Since the corresponding isolation region W of the first doped layer 31 is covered by the protective material layer 500, the alkaline solution will not damage the first doped layer 31.

[0392] Step R, referring to Figures 21 and 5, uses a metal etching solution (e.g., H2SO4 + H2O2) to clean and remove the portion of the first metal seed material layer 610 not covered by the first electroplating electrode 81 to form the first metal seed layer 61; the portion of the second metal seed material layer 620 not covered by the second electroplating electrode 82 is also cleaned and removed to form the second metal seed layer 62. Then, an electrode protective layer 73 (e.g., tin / silver) is formed on the side of the first and second electroplating electrodes 81 and 82 away from the substrate 10 by chemical plating or other methods, forming the heterojunction cell 100 as shown in Figure 5. The formation method of the electrode protective layer 73 is not limited to chemical plating; electroplating can also be used. It should be noted that in this step, the portion of the protective material layer 500 located on the side C or the first surface F may be partially removed or not removed to form the protective layer 50. In the example of Figure 5, part of the protective material layer 500 is located on one side of the first surface F, and part of the structure is located on the side C. That is, in the example of Figure 5, the protective material layer 500 is retained to form the protective layer 50 and is not removed. The heterojunction cell of Figure 5 is designated as A5. Alternatively, referring to Figure 6, in some other embodiments, the entire protective layer 50 may be located on one side of the first surface F, that is, the portion of the protective material layer 500 covering the side C may be removed separately. Alternatively, referring to Figure 22, the portion of the protective material layer 500 not covered by the first transparent conductive layer 41 may be cleaned and removed to form a protective layer 50 with the same coverage area as the first transparent conductive layer 41. In this scheme, the corresponding isolation region W of the first doped layer 31 will eventually be exposed. That is, only the portion of the protective material layer 500 located below the first transparent conductive layer 41 is retained. The heterojunction cell of Figure 22 is designated as A6.

[0393] Example 4

[0394] The method for fabricating a heterojunction cell in this embodiment is used to form the heterojunction cell 100 illustrated in FIG7.

[0395] This embodiment improves upon the steps of step I and thereafter, based on the above embodiment two. Steps A, B, and C are the same as in embodiment two, and will not be repeated here.

[0396] After steps A, B, and C, the fabrication method of a heterojunction solar cell also includes:

[0397] Step S

[0398] Referring to Figure 23, a protective material layer 500 is formed on the surface of the first doped layer 31 facing away from the substrate 10. The protective material layer 500 has the same area as the first doped layer 31, that is, a portion of the structure of the protective material layer 500 corresponds to the entire first surface F and covers a portion of the corresponding isolation region W of the first doped layer 31. A portion of the structure of the protective material layer 500 is also located on the side surface C, and the portion of the protective material layer 500 located on the side surface C covers the portion of the first doped layer 31 located on the side surface C.

[0399] In specific implementation, step C, the step of forming the first doped layer 31, includes:

[0400] Hydrogen, silane, diborane, and carbon dioxide gases are introduced into the reaction chamber, wherein the molar volume ratio of hydrogen:silane:diborane:carbon dioxide is 300:1:0.005:0.2-600:1:0.01:0.5. The reaction pressure within the chamber is approximately 4-6 mbar, thereby forming an oxygen-containing microcrystalline film layer on the surface of the first intrinsic silicon layer 21 facing away from the substrate 10. As the oxygen-containing microcrystalline film layer gradually deposits, the carbon dioxide gas flow rate gradually decreases, while the diborane flow rate gradually increases, and the hydrogen dilution ratio gradually increases, resulting in an oxygen-containing microcrystalline film layer with a thickness of not less than 5 nm.

[0401] Then, hydrogen, silane, and diborane gases are introduced into the reaction chamber to continue depositing the subsequent oxygen-free microcrystalline host layer on the oxygen-containing microcrystalline sublayer. The molar volume ratio of hydrogen:silane:diborane gas is 300:1:0.01 to 500:1:0.04, the reaction pressure in the chamber is about 2-3 mbar, and the thickness of the formed oxygen-free microcrystalline host layer is not less than 10 nm.

[0402] The step of forming a protective material layer 500 on the surface of the first doped layer 31 opposite to the substrate 10 specifically includes:

[0403] Hydrogen, silane, diborane, and carbon dioxide gases are introduced into the reaction chamber, wherein the molar volume ratio of hydrogen:silane:diborane:carbon dioxide is 8:1:3:1 to 12:1:5:1.5; the reaction pressure in the reaction chamber is approximately 2-3 mbar, thereby forming a protective material layer 500 (oxygen-doped amorphous silicon layer) on the surface of the oxygen-free microcrystalline host layer, and the thickness of the protective material layer 500 is no more than 3 nm.

[0404] Step T, referring to Figure 24, the side of the substrate 10 with the protective material layer 500 is placed on the support frame of the carrier plate. The edge of the protective material layer 500 corresponding to the isolation region W is blocked by the support frame of the carrier plate. In the protective material layer 500, a local area inside the edge is exposed from the cutout area of ​​the support frame of the carrier plate. A first transparent conductive layer 41 is formed on the surface of the protective material layer 500 exposed from the support frame of the carrier plate. The first transparent conductive layer 41 is not formed at the position of the protective material layer 500 corresponding to the isolation region W. Then, a second transparent conductive layer 42 is formed on the surface of the second doped layer 32 away from the substrate 10. Part of the structure of the second transparent conductive layer 42 is located on the side C. The second transparent conductive layer 42 covers part of the side C, and part of it can cover the second doped layer 32 and part of it can cover the protective material layer 500.

[0405] Step U, referring to Figure 25, a first metal seed material layer 610 is formed on the surface of the first transparent conductive layer 41 away from the substrate 10. The first metal seed material layer 610 is located on the side of the first surface F and does not cover the isolation area W. A second metal seed material layer 620 is formed on the surface of the second transparent conductive layer 42 away from the substrate 10. Part of the structure of the second metal seed material layer 620 is located on the side of the second surface S and part of the structure is located on the side C.

[0406] Step V, referring to Figure 26, print or spin-coat a front-side photoresist / photosensitive ink on one side of the first surface F and the second surface S of the structure formed in step U. After exposure and development, a patterned first mask material layer 71 is formed. The positions on the first mask material layer 71 corresponding to the metal contact areas Z of the first surface F and the second surface S are cut out. The remaining portions of the first surface F and the second surface S are covered by the first mask material layer 71, exposing the positions on the first metal seed material layer 610 and the second metal seed material layer 620 where the gate lines will be formed. An insulating adhesive 72 or other protective material is then coated on the side surface C of the structure formed in step U to edge the side surface C. Then, copper is electroplated to form a first electroplating electrode 81 on the first metal seed material layer 610 on the first surface F of the substrate 10, and a second electroplating electrode 82 on the second metal seed layer 620 on the second surface S of the substrate 10.

[0407] Then, a chemical solution, typically an alkaline solution, is used to clean and remove the first mask material layer 71 and the insulating adhesive 72. Since the isolation region W is covered by the protective material layer 500, the alkaline solution will not damage the first doped layer 31.

[0408] Step X: Referring to Figures 26 and 7, the portion of the first metal seed material layer 610 not covered by the first electroplating electrode 81 is cleaned and removed using a metal etching solution (e.g., H2SO4 + H2O2) to form the first metal seed layer 61. Similarly, the portion of the second metal seed material layer 620 not covered by the second electroplating electrode 82 is cleaned and removed to form the second metal seed layer 62. Then, an electrode protective layer 73 (e.g., tin / silver) is formed on the side of the first and second electroplating electrodes 81 and 82 facing away from the substrate 10 using methods such as chemical plating, forming the heterojunction cell 100 as shown in Figure 7. The formation method of the electrode protective layer 73 is not limited to chemical plating; electroplating can also be used.

[0409] The heterojunction cell thus formed is shown in Figure 7. The heterojunction cell in Figure 7 is denoted as A7.

[0410] Comparative Example

[0411] Step 1: Prepare a silicon wafer as a substrate.

[0412] Step 2: Form a first intrinsic silicon layer on the first surface of the substrate and form a second intrinsic silicon layer on the second surface of the substrate.

[0413] Step 3: Form a second doped layer on the surface of the second intrinsic silicon layer away from the substrate, and form a first doped layer on the surface of the first intrinsic silicon layer away from the substrate.

[0414] Step 4: Place the substrate with the first doped layer formed on the carrier plate, that is, with one side of the first surface of the substrate facing the carrier plate, place the side of the substrate with the first doped layer formed on the carrier plate's support frame. The portion of the edge of the first doped layer corresponding to the isolation region is blocked by the carrier plate's support frame, while a local area inside the edge of the first doped layer is exposed from the cutout area of ​​the carrier plate's support frame. A first transparent conductive layer is formed on the surface of the first doped layer in the area exposed from the carrier plate's support frame. The portion of the first doped layer that is blocked by the carrier plate's support frame and corresponds to the isolation region does not have a first transparent conductive layer formed. Then, a second transparent conductive layer is formed on the surface of the second doped layer facing away from the substrate.

[0415] Step 5: A first metal seed material layer is formed on the surface of the first transparent conductive layer away from the substrate. The first metal seed material layer is located on the first surface and does not cover the isolation area. A second metal seed material layer is formed on the surface of the second transparent conductive layer away from the substrate. Part of the structure of the second metal seed material layer is located on one side of the second surface, and part of the structure is located on the side.

[0416] Step Six: Form patterned mask layers on one side of the first surface and one side and side of the second surface of the structure formed in Step Five, exposing the metal contact area on one side of the first surface and the metal contact area on one side of the second surface. Then, electroplate copper to form a first electroplating electrode on the first metal seed material layer on one side of the first surface of the substrate and a second electroplating electrode on the second metal seed material layer on the second surface of the substrate.

[0417] Then, a chemical solution, usually an alkaline solution, is used to clean and remove the patterned mask layer. Since the corresponding isolation region of the first doped layer is partially exposed, it will be etched by the alkaline solution, thus causing damage to the first doped layer.

[0418] Step 7: Use a metal etching solution to clean and remove the portion of the first metal seed material layer not covered by the first electroplating electrode to form the first seed layer. Then, clean and remove the portion of the second metal seed material layer not covered by the second electroplating electrode to form the second seed layer. Next, form a chemical plating protective layer on the side of the first and second electroplating electrodes facing away from the substrate using methods such as chemical plating. The battery fabricated using the comparative method is designated B1.

[0419] The heterojunction solar cells A1, A2, A3, A4, A5, A6, A7 and the comparative solar cell B1 were tested for cell performance, and the test results are recorded in Table 1 below. Where Isc is the short-circuit current; Uoc is the open-circuit voltage; FF is the fill factor; Eta is the conversion efficiency; Rsh is the parallel resistance; Rs is the series resistance; Jsc is the short-circuit current density; and PFF is the pseudo-fill factor.

[0420] Table 1: Performance test results of heterojunction cells A1, A2, A3, A4, A5, A6, and A7 of this application and heterojunction cell B1 of the comparative example.

[0421] The experimental results above show that, compared with the heterojunction cell B1 in the comparative example, the heterojunction cell A1 fabricated using the heterojunction cell fabrication method of the present application has the following characteristics: Isc short-circuit current increases; Uoc open-circuit voltage increases; FF fill factor increases; Eta conversion efficiency increases; Rsh parallel resistance decreases; Rs series resistance decreases; Jsc short-circuit current density increases; and PFF pseudo-fill factor increases.

[0422] Compared to the comparative heterojunction cell B1, the heterojunction cell A2 fabricated using the method described in this application exhibits the following characteristics: Isc short-circuit current increases; Uoc open-circuit voltage remains unchanged; FF fill factor increases; Eta conversion efficiency increases; Rsh parallel resistance increases; Rs series resistance decreases; Jsc short-circuit current density increases; and PFF pseudo-fill factor increases.

[0423] Compared to the comparative heterojunction cell B1, the heterojunction cell A3 fabricated using the heterojunction cell fabrication method of the present application has the following characteristics: Isc short-circuit current remains basically the same; Uoc open-circuit voltage remains unchanged; FF fill factor increases; Eta conversion efficiency increases; Rsh parallel resistance decreases; Rs series resistance decreases; Jsc short-circuit current density remains unchanged; and PFF pseudo-fill factor increases.

[0424] Compared to the comparative heterojunction cell B1, the heterojunction cell A4 fabricated using the method described in this application exhibits the following characteristics: Isc short-circuit current increases; Uoc open-circuit voltage remains unchanged; FF fill factor increases; Eta conversion efficiency increases; Rsh parallel resistance decreases; Rs series resistance decreases; Jsc short-circuit current density increases; and PFF pseudo-fill factor increases.

[0425] Compared to the comparative heterojunction cell B1, the heterojunction cell A5 fabricated using the method described in this application exhibits the following characteristics: Isc short-circuit current increases; Uoc open-circuit voltage remains unchanged; FF fill factor increases; Eta conversion efficiency increases; Rsh parallel resistance decreases; Rs series resistance decreases; Jsc short-circuit current density increases; and PFF pseudo-fill factor increases.

[0426] Compared to the comparative heterojunction cell B1, the heterojunction cell A6 fabricated using the method described in this application has the following characteristics: Isc short-circuit current remains essentially the same; Uoc open-circuit voltage remains unchanged; FF fill factor increases; Eta conversion efficiency increases; Rsh parallel resistance increases; Rs series resistance decreases; Jsc short-circuit current density remains essentially the same; and PFF pseudo-fill factor increases.

[0427] Compared to the comparative heterojunction cell B1, the heterojunction cell A7 fabricated using the method described in this application exhibits the following characteristics: Isc short-circuit current remains essentially the same; Uoc open-circuit voltage remains unchanged; FF fill factor increases; Eta conversion efficiency increases; Rsh parallel resistance decreases; Rs series resistance decreases; Jsc short-circuit current density remains unchanged; and PFF pseudo-fill factor increases.

[0428] Therefore, it can be seen that the heterojunction solar cell fabricated using the method of this embodiment has a high efficiency.

[0429] This application also provides a heterojunction cell 100, which is manufactured using the heterojunction cell manufacturing method described above.

[0430] This application also provides a photovoltaic module, which includes at least one cell string, and the cell string includes at least two heterojunction cells 100 as described above.

[0431] The heterojunction cells 100 can be connected together by string welding, thereby collecting the electrical energy generated by each individual heterojunction cell 100 for subsequent transmission. Of course, the heterojunction cells 100 can be arranged at intervals or stacked together in a shingled manner.

[0432] For example, a photovoltaic module also includes an encapsulation layer and a cover plate, the encapsulation layer being used to cover the surface of the battery string and the cover plate being used to cover the surface of the encapsulation layer away from the battery string.

[0433] This application also provides a photovoltaic system, including the photovoltaic module described above.

[0434] Photovoltaic systems can be applied in photovoltaic power plants, such as ground-mounted, rooftop, and floating power plants, as well as in equipment or devices that utilize solar energy to generate electricity, such as user solar power supplies, solar streetlights, solar cars, and solar buildings. Of course, it's understandable that the application scenarios of photovoltaic systems are not limited to these; that is, photovoltaic systems can be applied in all fields that require solar energy to generate electricity. Taking a photovoltaic power generation network as an example, a photovoltaic system can include photovoltaic arrays, combiner boxes, and inverters. A photovoltaic array can be a combination of multiple photovoltaic modules; for example, multiple photovoltaic modules can form multiple photovoltaic arrays. The photovoltaic arrays are connected to combiner boxes, which collect the current generated by the photovoltaic arrays. The collected current flows through an inverter and is converted into AC power required by the mains power grid before being connected to the mains power grid to achieve solar power supply.

[0435] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0436] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent application. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims.

Claims

1. A heterojunction battery, characterized in that, include: Substrate; A first intrinsic silicon layer and a first doped layer are sequentially stacked on the first surface of the substrate; A first transparent conductive layer and a protective layer are stacked on the side of the first doped layer away from the substrate. The first transparent conductive layer covers a portion of the first surface, and the protective layer completely covers the first surface. as well as The first electroplating electrode is located on the side of the protective layer away from the substrate and is electrically connected to the first transparent conductive layer. The first surface includes an isolation region not covered by the first transparent conductive layer; a portion of the protective layer is stacked on the portion of the first doped layer corresponding to the isolation region.

2. The heterojunction battery according to claim 1, characterized in that, The protective layer further covers at least a portion of the side surface of the substrate, the side surface of the substrate being adjacent to the first surface.

3. The heterojunction solar cell according to claim 1, characterized in that, The outer contour edge of the protective layer coincides with the edge of the first surface.

4. The heterojunction battery according to claim 1, characterized in that, The first transparent conductive layer is disposed on the surface of the first doped layer opposite to the substrate; The protective layer is located on the side of the first transparent conductive layer that is away from the substrate; The first electroplating electrode is disposed on the protective layer and is electrically connected to the first transparent conductive layer through the protective layer.

5. The heterojunction battery according to claim 4, characterized in that, The outer contour edge of the protective layer coincides with the edge of the first surface; A portion of the protective layer is stacked on the surface of the first transparent conductive layer opposite to the substrate, and another portion of the protective layer is stacked on the surface of the portion of the first doped layer corresponding to the isolation region.

6. The heterojunction solar cell according to claim 4, characterized in that, The protective layer further covers at least a portion of the side surface of the substrate, wherein the side surface of the substrate is adjacent to the first surface; The heterojunction solar cell further includes a second intrinsic silicon layer, a second doped layer and a second transparent conductive layer sequentially stacked on the second surface of the substrate. The doping type of the second doped layer is opposite to that of the first doped layer, and the second surface is disposed opposite to the first surface. The second transparent conductive layer covers at least a portion of the second surface and the side surface of the substrate, and on the side surface of the substrate, a portion of the structure of the protective layer is stacked onto the side of the second transparent conductive layer opposite to the substrate.

7. The heterojunction battery according to claim 1, characterized in that, The protective layer is disposed on the surface of the first doped layer opposite to the substrate; the first transparent conductive layer is located on the side of the protective layer opposite to the substrate; The first electroplating electrode is disposed on the first transparent conductive layer.

8. The heterojunction battery according to claim 7, characterized in that, The outer contour edge of the protective layer coincides with the edge of the first surface.

9. The heterojunction battery according to claim 7, characterized in that, The protective layer further covers at least a portion of the side surface of the substrate, wherein the side surface of the substrate is adjacent to the first surface.

10. The heterojunction solar cell according to claim 9, characterized in that, The heterojunction solar cell further includes a second intrinsic silicon layer, a second doped layer and a second transparent conductive layer sequentially stacked on the second surface of the substrate. The doping type of the second doped layer is opposite to that of the first doped layer, and the second surface is disposed opposite to the first surface. The second doped layer covers at least a portion of the second surface and the side surface, the first doped layer covers at least a portion of the first surface and the side surface, and on the side surface of the substrate, a portion of the structure of the first doped layer is stacked onto the side of the second doped layer opposite to the substrate. On the side of the substrate, the protective layer is at least partially stacked on the surface of the first doped layer opposite to the substrate; The second transparent conductive layer covers at least a portion of the second surface and the side surface of the substrate, and on the side surface of the substrate, a portion of the structure of the second transparent conductive layer is stacked onto the side of the protective layer opposite to the substrate.

11. The heterojunction solar cell according to claim 10, characterized in that, On the side of the substrate, the outer contour edge of the protective layer coincides with the outer contour edge of the first doped layer.

12. The heterojunction solar cell according to claim 11, characterized in that, The first doped layer includes an oxygen-free microcrystalline host layer, and the protective layer includes an oxygen-doped amorphous silicon layer.

13. The heterojunction solar cell according to claim 12, characterized in that, The first doped layer further includes an oxygen-containing microcrystalline sublayer, which is stacked between the first intrinsic silicon layer and the oxygen-free microcrystalline host layer.

14. The heterojunction solar cell according to claim 12 or 13, characterized in that, The thickness of the protective layer is no greater than 3 nm.

15. The heterojunction solar cell according to claim 10, characterized in that, The protective layer covers a portion of one side of the side, with a portion of the structure stacked on the first doped layer and another portion of the structure stacked on the second doped layer.

16. The heterojunction solar cell according to claim 9, characterized in that, The heterojunction solar cell further includes a second intrinsic silicon layer, a second doped layer and a second transparent conductive layer sequentially stacked on the second surface of the substrate. The doping type of the second doped layer is opposite to that of the first doped layer, and the second surface is disposed opposite to the first surface. The second transparent conductive layer covers at least a portion of the second surface and the side surface of the substrate, wherein a portion of the structure of the protective layer is stacked onto the side of the second transparent conductive layer opposite to the substrate.

17. The heterojunction solar cell according to any one of claims 1 to 16, characterized in that, The protective layer comprises a transition metal oxide, and the conductivity type of the protective layer is the same as that of the first doped layer; or The protective layer includes a tunneling layer; or The protective layer includes a transparent conductive oxide layer.

18. The heterojunction solar cell according to claim 17, characterized in that, When the protective layer comprises a transition metal oxide, the thickness of the protective layer is 5-30 nm; When the protective layer includes a dielectric passivation layer, the thickness of the protective layer is 0.5-3 nm; When the protective layer includes a transparent conductive oxide layer, the thickness of the protective layer is 5-15 nm.

19. The heterojunction battery according to any one of claims 1-18, characterized in that, The substrate further includes a second surface disposed opposite to the first surface, and a side surface adjacent to the first surface and the second surface; The heterojunction solar cell further includes a second electroplated electrode, and a second intrinsic silicon layer, a second doped layer and a second transparent conductive layer sequentially stacked on the second surface. The doping type of the second doped layer is opposite to that of the first doped layer, and the second electroplated electrode is electrically connected to the second transparent conductive layer.

20. The heterojunction solar cell according to claim 19, characterized in that, The heterojunction solar cell further includes a first metal seed layer and / or a second metal seed layer, wherein the first metal seed layer is stacked on the surface of the first electroplated electrode facing the substrate, and the second metal seed layer is stacked on the surface of the second electroplated electrode facing the substrate.

21. The heterojunction solar cell according to claim 19 or 20, characterized in that, The heterojunction solar cell further includes an electrode protective layer, wherein the electrode protective layer located on one side of the first surface is stacked on the surface of the first electroplated electrode away from the substrate, and / or the electrode protective layer located on one side of the second surface is stacked on the surface of the second electroplated electrode away from the substrate.

22. The heterojunction solar cell according to any one of claims 19 to 21, characterized in that, The first intrinsic silicon layer covers at least a portion of the first surface and the side surface; The second intrinsic silicon layer covers at least a portion of the second surface and the side surface, and on the side surface of the substrate, a portion of the structure of the second intrinsic silicon layer is stacked onto the side of the first intrinsic silicon layer opposite to the substrate. The second doped layer covers at least a portion of the second surface and the side surface, and on the side surface of the substrate, a portion of the structure of the second doped layer is stacked onto the side of the first intrinsic silicon layer opposite to the substrate. The first doped layer covers at least a portion of the first surface and the side surface, and on the side surface of the substrate, a portion of the structure of the first doped layer is stacked onto the side of the second doped layer opposite to the substrate.

23. The heterojunction battery according to any one of claims 1-22, characterized in that, Each portion of the outer contour edge of the first transparent conductive layer is spaced from the edge of the first surface to define an annular isolation region on the first surface.

24. A method for fabricating a heterojunction solar cell, characterized in that, include: A substrate is provided, the substrate comprising a substrate, and a first intrinsic silicon layer and a first doped layer sequentially stacked on a first surface of the substrate; A first transparent conductive layer and a protective material layer are formed on the side of the first doped layer away from the substrate, wherein the first transparent conductive layer covers a portion of the first surface, the first surface includes an isolation region not covered by the first transparent conductive layer, the protective material layer completely covers the first surface, and a portion of the structure of the protective material layer is stacked on the portion of the first doped layer corresponding to the isolation region. A first electroplating electrode is formed by electroplating on the side of the protective material layer opposite to the substrate, and the first electroplating electrode is electrically connected to the first transparent conductive layer.

25. The method for fabricating a heterojunction solar cell according to claim 24, characterized in that, The step of forming the protective material layer includes: The second surface of the substrate is oriented towards the support frame of the carrier plate; The protective material layer is formed on the side of the first doped layer opposite to the substrate; Wherein, the protective material layer completely covers the first surface and covers at least a portion of the side surface of the substrate; or, the protective material layer completely covers the first surface, and the outer contour edge of the protective material layer coincides with the edge of the first surface.

26. The method for fabricating a heterojunction solar cell according to claim 24 or 25, characterized in that, The step of forming the first transparent conductive layer includes: The first surface of the substrate is oriented towards the support frame of the carrier plate; The first transparent conductive layer is formed on the side of the first doped layer away from the substrate, and the location of the formation of the first transparent conductive layer corresponds to the hollow portion of the bearing frame.

27. The method for fabricating a heterojunction solar cell according to claim 24, characterized in that, The step of forming a first transparent conductive layer and a protective material layer stacked on the side of the first doped layer opposite to the substrate specifically includes: A first transparent conductive layer is formed on the surface of the first doped layer that is away from the substrate; A protective material layer is formed on the surface of the first transparent conductive layer that is away from the substrate.

28. The method for fabricating a heterojunction solar cell according to claim 27, characterized in that, The step of forming a first transparent conductive layer on the surface of the first doped layer away from the substrate specifically includes: The first surface of the substrate is oriented toward the support frame of the carrier plate, and the portion of the first doped layer located on the first surface is supported by the support frame. In the portion of the first doped layer covering one side of the first surface, the area not obscured by the bearing frame forms the first transparent conductive layer.

29. The method for fabricating a heterojunction solar cell according to claim 28, characterized in that, The step of forming a protective material layer on the surface of the first transparent conductive layer opposite to the substrate specifically includes: The second surface of the substrate is supported on the support frame of the carrier plate; A protective material layer is formed on the surface of the first transparent conductive layer away from the substrate; the protective material layer is partially stacked on the surface of the first transparent conductive layer away from the substrate, and partially stacked on the surface of the portion of the isolation region corresponding to the first doped layer.

30. The method for fabricating a heterojunction solar cell according to claim 29, characterized in that, The substrate further includes a second intrinsic silicon layer and a second doped layer sequentially stacked on a second surface of the substrate, the second surface being disposed opposite to the first surface; the step of forming the first transparent conductive layer and the step of forming the protective material layer further includes: A second transparent conductive layer is formed on the side of the second doped layer that is away from the substrate.

31. The method for fabricating a heterojunction solar cell according to claim 30, characterized in that, The substrate also includes a side surface adjacent to the first surface and the second surface; The second transparent conductive layer covers at least a portion of the side surface of the second surface and the substrate; The protective material layer also covers at least a portion of the side surface, and a portion of the structure of the protective material layer is stacked onto the side of the second transparent conductive layer opposite to the substrate; or The outer contour edge of the protective material layer coincides with the edge of the first surface.

32. The method for fabricating a heterojunction solar cell according to claim 24, characterized in that, The step of forming a first transparent conductive layer and a protective material layer stacked on the side of the first doped layer opposite to the substrate specifically includes: A protective material layer is formed on the surface of the first doped layer that is away from the substrate; A first transparent conductive layer is formed on the surface of the protective material layer opposite to the substrate.

33. The method for fabricating a heterojunction solar cell according to claim 32, characterized in that, The substrate further includes a second intrinsic silicon layer and a second doped layer sequentially stacked on a second surface of the substrate, the second surface being disposed opposite to the first surface; the substrate also includes a side surface adjacent to the first surface and the second surface; The step of forming a protective material layer on the surface of the first doped layer away from the substrate includes, prior to the step of: A second transparent conductive layer is formed on the surface of the second doped layer opposite to the substrate, the second transparent conductive layer covering at least a portion of the second surface and the side surface.

34. The method for fabricating a heterojunction solar cell according to claim 33, characterized in that, The step of forming a protective material layer on the surface of the first doped layer away from the substrate specifically includes: A protective material layer is formed on the side of the first doped layer away from the substrate, the protective material layer completely covering the first surface and covering at least a portion of the side surface, and the protective material layer is stacked onto the second transparent conductive layer.

35. The method for fabricating a heterojunction solar cell according to claim 34, characterized in that, The step of forming a first transparent conductive layer on the surface of the protective material layer opposite to the substrate specifically includes: The first surface of the substrate is oriented toward the support frame of the carrier plate, and the portion of the protective material layer located on the first surface is supported by the support frame. In the portion of the protective material layer covering one side of the first surface, the area not obscured by the supporting frame forms the first transparent conductive layer.

36. The method for fabricating a heterojunction solar cell according to claim 32, characterized in that, The substrate further includes a second surface disposed opposite to the first surface, and a side surface adjacent to the first surface and the second surface; The step of forming a protective material layer on the surface of the first doped layer away from the substrate includes: A protective material layer is formed on the side of the first doped layer opposite to the substrate, the protective material layer covering at least a portion of the first surface and the side surface.

37. The method for fabricating a heterojunction solar cell according to claim 36, characterized in that, The step of forming a first transparent conductive layer on the surface of the protective material layer opposite to the substrate specifically includes: The first surface of the substrate is oriented toward the support frame of the carrier plate, and the portion of the protective material layer located on the first surface is supported by the support frame. In the portion of the protective material layer covering one side of the first surface, the area not obscured by the supporting frame forms the first transparent conductive layer.

38. The method for fabricating a heterojunction solar cell according to claim 37, characterized in that, The substrate further includes a second intrinsic silicon layer and a second doped layer sequentially stacked on the second surface; After the step of forming the first transparent conductive layer on the surface of the protective material layer opposite to the substrate, the method further includes: A second transparent conductive layer is formed on the surface of the second doped layer opposite to the substrate, the second transparent conductive layer covering at least a portion of the second surface and the side surface, and the second transparent conductive layer is stacked onto the protective material layer.

39. The method for manufacturing a heterojunction solar cell according to any one of claims 36 to 38, characterized in that, The substrate further includes a second intrinsic silicon layer and a second doped layer sequentially stacked on a second surface of the substrate, the second surface being disposed opposite to the first surface; In the step of forming a protective material layer on the surface of the first doped layer away from the substrate: The protective material layer covers at least a portion of the first surface and the side surface, wherein the protective material layer is stacked on the side surface of the second doped layer opposite to the substrate.

40. The method for manufacturing a heterojunction solar cell according to any one of claims 36 to 38, characterized in that, In the step of forming a protective material layer on the surface of the first doped layer away from the substrate: The protective material layer covers at least a portion of the first surface and the side surface; on the side surface, the outer contour edge of the protective material layer coincides with the outer contour edge of the first doped layer.

41. The method for fabricating a heterojunction solar cell according to claim 40, characterized in that, The first doped layer includes an oxygen-free microcrystalline host layer; The steps for forming the protective material layer include: An oxygen-doped amorphous silicon layer is formed on the surface of the first doped layer away from the substrate as a protective material layer, wherein the doping type of the oxygen-doped amorphous silicon layer is the same as that in the first doped layer.

42. The method for fabricating a heterojunction solar cell according to claim 41, characterized in that, The first doped layer further includes an oxygen-containing microcrystalline sublayer, which is stacked between the first intrinsic silicon layer and the oxygen-free microcrystalline host layer.

43. The method for fabricating a heterojunction solar cell according to claim 42, characterized in that, The oxygen-containing microcrystalline sub-film layer and the oxygen-free microcrystalline host layer are formed through the following steps: Hydrogen, silane, diborane, and carbon dioxide gases are introduced into the reaction chamber, wherein the molar volume ratio of the hydrogen, silane, diborane, and carbon dioxide gases is between 300:1:0.005:0.2 and 600:1:0.01:0.5, and the reaction pressure in the reaction chamber is 4-6 mbar, so as to form the oxygen-containing microcrystalline film layer on the surface of the first intrinsic silicon layer away from the substrate; Hydrogen, silane, and diborane gases are introduced into the reaction chamber, wherein the molar volume ratio of the hydrogen, silane, and diborane gases is 300:1:0.01 to 500:1:0.04, and the reaction pressure in the reaction chamber is 2-3 mbar, so as to form the oxygen-free microcrystalline host layer on the surface of the oxygen-containing microcrystalline film layer away from the substrate.

44. The method for fabricating a heterojunction solar cell according to claim 41, characterized in that, The step of forming the oxygen-doped amorphous silicon layer as a protective material layer includes: Hydrogen, silane, diborane, and carbon dioxide are introduced into the reaction chamber, wherein the molar volume ratio of the hydrogen, silane, diborane, and carbon dioxide is from 8:1:3:1 to 12:1:5:1.5; the reaction pressure in the reaction chamber is 2-3 mbar, so as to form the oxygen-doped amorphous silicon layer on the surface of the oxygen-free microcrystalline host layer.

45. The method for fabricating a heterojunction solar cell according to any one of claims 24 to 44, characterized in that, The protective material layer comprises a transition metal oxide, and the conductivity type of the protective material layer is the same as that of the first doped layer; or The protective material layer includes a tunneling layer; or The protective material layer includes a transparent conductive oxide layer.

46. ​​The method for manufacturing a heterojunction solar cell according to any one of claims 24 to 45, characterized in that, The substrate further includes a second intrinsic silicon layer and a second doped layer sequentially stacked on a second surface of the substrate, the second surface being disposed opposite to the first surface; The method for fabricating the heterojunction solar cell further includes: A second transparent conductive layer is formed on the surface of the second doped layer that is away from the substrate; A second electroplated electrode is formed on one side of the second surface of the substrate by electroplating.

47. The method for fabricating a heterojunction solar cell according to claim 46, characterized in that, The protective material layer completely covers the first surface and covers at least a portion of the side surface of the substrate; The steps of forming the first electroplating electrode and forming the second electroplating electrode further include removing at least a portion of the protective material layer to form a protective layer.

48. The method for fabricating a heterojunction solar cell according to claim 47, characterized in that, The portion of the protective material layer that is removed includes the portion of the protective material layer located on one side of the side surface; or The portion of the protective material layer that is removed includes the portion of the protective material layer covering one side of the side and the portion covering the isolation area; or The removed portion of the protective material layer includes the portion of the protective material layer covering one side of the side surface, and the portion of the protective material layer corresponding to the non-metallic contact area of ​​the first surface.

49. The method for fabricating a heterojunction solar cell according to claim 48, characterized in that, The steps of forming the first electroplating electrode and forming the second electroplating electrode specifically include: A first metal seed material layer is formed on one side of the first surface of the substrate, and a second metal seed material layer is formed on the surface of the second transparent conductive layer opposite to the substrate, wherein the first metal seed material layer is located on the one of the first transparent conductive layer and the protective material layer that is farther away from the substrate; A first electroplating electrode is formed by electroplating a patterned mask layer on the surface of the first metal seed material layer, and a second electroplating electrode is formed by electroplating a patterned mask layer on the surface of the second metal seed material layer. Remove the mask layer; The portion of the first metal seed material layer not covered by the first electroplating electrode is removed to form a first metal seed layer, and the portion of the second metal seed material layer not covered by the second electroplating electrode is removed to form a second metal seed layer.

50. The method for fabricating a heterojunction solar cell according to claim 49, characterized in that, The patterned mask layer is formed by the following steps: A patterned first mask material layer is formed on the side of the first metal seed material layer and the second metal seed material layer away from the substrate. The first mask material layer is hollowed out at the position of the metal contact area of ​​the first surface and at the position of the metal contact area of ​​the second surface. An insulating adhesive is applied to one side of the substrate.

51. The method for fabricating a heterojunction solar cell according to claim 49, characterized in that, After the steps of removing the portion of the first metal seed material layer not covered by the first electroplating electrode and removing the portion of the second metal seed material layer not covered by the second electroplating electrode, the method further includes the step of forming an electrode protective layer on the surfaces of the first electroplating electrode and the second electroplating electrode.

52. The method for fabricating a heterojunction solar cell according to claim 51, characterized in that, The steps of removing the portion of the first metal seed material layer not covered by the first electroplating electrode, removing the portion of the second metal seed material layer not covered by the second electroplating electrode, and / or forming the electrode protective layer further include removing at least a portion of the protective material layer to form the protective material layer.

53. The method for fabricating a heterojunction solar cell according to claim 24, characterized in that, The substrate further includes a second intrinsic silicon layer and a second doped layer sequentially stacked on a second surface of the substrate, the second surface being disposed opposite to the first surface; The step of providing a substrate specifically includes: A first intrinsic silicon layer is formed on a first surface of the substrate, and a second intrinsic silicon layer is formed on a second surface of the substrate; A second doped layer is formed on the surface of the second intrinsic silicon layer opposite to the substrate, and a first doped layer is formed on the surface of the first intrinsic silicon layer opposite to the substrate.

54. The method for fabricating a heterojunction solar cell according to claim 53, characterized in that, The substrate also includes a side surface adjacent to the first surface and the second surface; The first intrinsic silicon layer covers at least a portion of the first surface and the side surface; The second intrinsic silicon layer covers at least a portion of the second surface and the side surface, and a portion of the structure of the second intrinsic silicon layer is stacked onto the side of the first intrinsic silicon layer facing away from the substrate; The second doped layer covers at least a portion of the second surface and the side surface, and a portion of the structure of the second doped layer is stacked onto the side of the first intrinsic silicon layer opposite to the substrate; The first doped layer covers at least a portion of the first surface and the side surface, and a portion of the structure of the first doped layer is stacked onto the side of the second doped layer opposite to the substrate.