Nickel-chromium-aluminium-silicon alloy having good processability, creep resistance and corrosion resistance, and use thereof
A nickel-chromium-aluminum-silicon alloy with balanced compositions addresses the limitations of existing alloys by providing improved corrosion and creep resistance, ensuring durability in high-temperature environments for solar and nuclear applications.
Patent Information
- Application Number
- PCT/DE2026/100555
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2026-04-29
- Filing Date
- 2026-05-04
- Publication Date
- 2026-11-12
AI Technical Summary
Existing nickel-chromium alloys used in high-temperature environments with chloride and/or carbonate salt melts suffer from poor workability, corrosion resistance, and inadequate creep resistance, making them unsuitable for applications in solar tower power plants and nuclear reactors where long service life and high temperatures are required.
A nickel-chromium-aluminum-silicon alloy with specific compositions, including 3.1 to 10% chromium, 0.1 to 5% aluminum and/or silicon, and balanced elements to ensure a continuous aluminum oxide layer, improved workability, and enhanced creep resistance.
The alloy provides excellent corrosion resistance, workability, and creep resistance, enabling long-term operation in high-temperature environments up to 1000°C, suitable for solar tower power plants and nuclear reactors.
Smart Images

Figure IMGF000028_0001_TABLE 
Figure IMGF000029_0001_TABLE
Abstract
Description
[0001] Nickel-chromium-aluminum-silicon alloy with good workability, creep resistance and corrosion resistance, and its uses
[0002] The invention relates to a nickel-chromium-aluminium-silicon wrought alloy with good high-temperature corrosion resistance, good creep resistance, good high-temperature strength and improved processability.
[0003] Nickel alloys with varying nickel, chromium, aluminum, and silicon contents have long been used not only in the chemical and petrochemical industries and furnace construction due to their properties, but are also of great interest for use in solar tower power plants. These plants consist of an array of mirrors (heliostats) arranged around a tall tower. The mirrors concentrate sunlight onto the absorber (solar receiver) mounted at the top. The absorber consists of a system of tubes in which a heat transfer medium is heated. This medium circulates in a loop with intermediate storage tanks, and in a secondary circuit, a heat exchanger system converts the thermal energy into electricity with the help of a generator.The heat transfer medium is primarily a salt mixture of sodium and potassium nitrate salt melts, resulting in a maximum operating temperature of the salt of approximately 600°C, depending on the alloy used for the components [Kruizenga et al., 2013, Materials Corrosion of High Temperature Alloys Immersed in 600°C Binary Nitrate Salt, SANDIA report, SAND 2013-2526].
[0004] To increase the efficiency of solar tower power plants, the maximum operating temperature of the salts must be raised. This is possible by using, for example, chloride and / or carbonate salts as a heat transfer medium [Mehos et al., 2017, Concentrating Solar Power Gen3 Demonstration Roadmap, National Renewable Energy Lab. (NREL)]. These do not decompose at temperatures above approximately 600°C like sodium and potassium nitrate salts, but have a maximum operating temperature of up to 1000°C. Another field of application is found in the nuclear sector, where, for example, small modular reactors (SMRs) are currently being developed using molten chloride as a heat transfer medium. SMRs are small nuclear reactors with a power output of up to 300 MW(e), whose systems and components can be assembled modularly in factories.Advantages compared to conventional nuclear power plants include, for example, the presence of passive safety systems and the possibility of generating heat simultaneously or instead of generating energy.
[0005] Furthermore, these salt systems can also be used for industrial heat storage due to their large heat storage capacity. These storage systems can ensure a reliable supply for industrial processes, thereby saving raw materials needed to keep auxiliary steam boilers operating at a constant minimum load in case of outages.
[0006] The disadvantage of using these salt systems is the stronger corrosion attack at higher temperatures compared to sodium and potassium nitrate salts, especially in the area of the solar receiver or the heat absorption tubes that transport the salt and represent the hottest point in the salt circuit. This means that materials commonly used with nitrate salts, such as Alloy 800H (N08810) or Alloy 625 (N06625), cannot be used, as they would not withstand the corrosion attack by chloride and / or carbonate salts at temperatures >600°C for a sufficient duration [Shankar et al., 2013, Corrosion of Ni-containing Alloys in Molten LiCI-KCI Medium, Corrosion, 69(1), 48-57]. A minimum service life of 30 years for the absorber system is assumed [Gomez-Vidal et al., 2017, Corrosion resistance of alumina-forming alloys against molten chlorides for energy production.I: Pre-oxidation treatment and isothermal corrosion tests, Solar Energy Materials and Solar Cells, 166, 222-233], A key requirement for using an alloy in the environment described above is good high-temperature corrosion resistance in chloride and / or carbonate salt melts. This is determined not only by a continuous chromium oxide layer (Cr2O3), but especially by an underlying, ideally continuous and gapless, aluminum oxide layer (Al2O3) and / or silicon oxide layer (SiO2). Under certain conditions, the chromium ions preferentially dissolve in the chloride salt melt, which is why a reduced chromium and increased nickel content is advantageous [George Y. Lai, 1990, High-Temperature Corrosion of Engineering Alloys, ASM International, p. 170; Knosalla C. et al., 2020, Investigation on the Corrosion Behavior of Nickel-Base Alloys in Molten Chlorides for Sensible Heat Energy Applications, Advanced Engineering Materials, 22(7), 2000099], A certain silicon and / or aluminum content in the alloy can slow down this dissolution process by forming closed SiO2 and / or Al2O3 layers [George Y. Lai, 1990, High-Temperature Corrosion of Engineering Alloys, ASM International, p. 100, Fig. 6.11; Ralf Bürgel, Handbook of High-Temperature Materials Engineering, 5th revised edition, 2015, pp. 83 / 84], Furthermore, resistance in chloride salt melts is improved by reducing the carbon and chromium content, since intergranular corrosion preferentially occurs at carbide-coated grain boundaries [George Y. Lai, 1990, High-Temperature Corrosion of Engineering Alloys, ASM International, p.
[0007] 100, Fig. 6.11],
[0008] In the temperature range of 500°C to 900°C, additions of aluminum, titanium, and / or niobium can improve strength through the precipitation of the y' and / or y” phases. The high-temperature strength and creep resistance at the specified temperatures are improved, among other things, by a high carbon content. High concentrations of solid solution strengthening elements such as chromium, aluminum, silicon, molybdenum, cobalt, and tungsten also improve the strength.
[0009] Heat resistance. Another important parameter with regard to the fatigue stress of the material due to the daily sun and cloud cycles calculated over the entire service life of the solar receiver is the alternating strength.
[0010] The compositions of the alloys SS321, Alloy 602CA, Alloy 230 and Alloy 625 according to the state of the art are listed in Table 1.
[0011] Alloy 602CA (N06025) exhibits excellent high-temperature strength and creep resistance even at temperatures above 1000°C. However, its workability is impaired, partly due to the high aluminum content. This impairment, caused by the precipitation of the gamma phase, is more pronounced with increasing aluminum content. This means the aluminum content must be high enough to form a continuous Al₂O₃ layer, but it must not be too high, as this would negatively affect workability. Similarly, excessive aluminum content reduces both cold formability and weldability. These requirements also apply to chromium and silicon. This underscores the crucial importance of precisely balancing the aluminum, silicon, and chromium content for corrosion resistance in chloride and / or carbonate salt melts at elevated temperatures.
[0012] WO 2019 / 075177 A1 discloses an improved solar tower system comprising absorber tubes, a storage tank and a heat exchanger, all containing a molten salt as a heat transfer medium at temperatures >650°C. The improvement involves manufacturing at least one of the components (absorber tubes, storage tank, and heat exchanger) from an alloy containing (in mass %) 25–45% Ni, 12–32% Cr, 0.1–2.0% Nb, up to 4% Ta, up to 1% Va, up to 2% Mn, up to 1.0% Al, up to 5% Mo, up to 5% W, up to 0.2% Ti, up to 2% Zr, up to 5% Co, up to 0.1% Y, up to 0.1% La, up to 0.1% Cs, up to 0.1% other rare earth elements, up to 0.20% C, up to 3% Si, N 0.05–0.50%, up to 0.02% B, and the remainder being Fe and impurities.EP 1065290 discloses a Ni-Cr-Al alloy comprising up to 0.1% C, up to 0.08% N, 0-2% Ta, 10-25% Cr, 0-10% Fe, up to 2% Mn, up to 2% Si, a total of 2.5-15% molybdenum and / or tungsten, 0-3% Ti, 0-1% V, 2.1-4.5% Al, up to 0.02% Zr, 0-10% Co, 0-5% Cu, up to 0.8% Hf, 0.0-0.1% Y, up to 0.03% B and remainder of Ni and impurities, which is used, among other things, in ethylene crackers.
[0013] German patent DE 10 2013 004 365 A1 discloses a nickel-based alloy consisting of (in wt%) 1.5–3.0% Si, 1.5–3.0% Al, > 0.1–3.0% Cr, where 4.0 < Al + Si + Cr < 8.0 is satisfied by the percentages of Si, Al, and Cr, Fe 0.005–0.20%, Y 0.01–0.20%, < 0.001–0.20% of one or more of the elements Hf, Zr, Al, Ce, Ti, where Y + 0.5 x Hf + Zr + 1.8 x Ti + 0.6 x (La + Ce) < 0.30 is satisfied by the percentages of Y, Hf, Zr, La, Ce, Ti, 0.001–0.10% C, 0.0005–0.10% N, 0.001–0.20% Mn, 0.0001–0.08% Mg, 0.0001–0.010% O, max. 0.015% S, max. 0.80% Cu, nickel balance, and the usual manufacturing-related impurities. This material is intended for use as an electrode material for ignition elements in internal combustion engines or as an electrode material for ignition elements in gasoline engines.
[0014] WO 2021 / 174726 A1 discloses a nickel-based alloy with a higher aluminum content comprising (in wt.%) C 0.0004 - 0.1%, W 6.0 - 9.0%, Cr 7.0 - 12.0%, Mo 1.0 - 4.0%, Co 14.0 - 17.5%, Ti 0.8 - 2.5%, Al 3.5 - 6.0%, Nb 0.8 - 2.5%, Zr 0.0005 - 0.1%, Mg 0.005 - 0.1%, Ce 0.001 - 0.1%, B 0.005 - 0.1%, Fe 0.005 - 2.0%, balance nickel.
[0015] This alloy is intended for use primarily in the field of flying gas turbines.
[0016] German patent DE 10 2020 132 219 A1 describes the use of a nickel-chromium-aluminum alloy with good processability, creep resistance, and corrosion resistance for solar tower power plants using chloride and / or carbonate salt melts as a heat transfer medium with (in mass %) 12–30% chromium, 1.8–4.0% aluminum, 0.1–7.0% iron, 0.001–0.50% silicon, 0.001–2.0% manganese, 0–1.0% titanium, 0–1.1% niobium, 0–0.5% copper, 0–5.0% cobalt, 0.0002–0.05% magnesium and / or calcium each, 0.001–0.12% carbon, 0.001–0.05% nitrogen, 0.001– 0.03% phosphorus, 0.0001 - 0.02% oxygen, max. 0.01% sulfur, max. 2.0% molybdenum, max. 2.0% tungsten, balance nickel with a minimum content of > 50% and the usual process-related impurities.
[0017] The object underlying the invention is to provide a nickel-chromium-aluminum-silicon alloy which
[0018] • good phase stability,
[0019] • good workability,
[0020] • and good corrosion resistance in chloride and / or carbonate salt melts
[0021] to elaborate.
[0022] Furthermore, it is necessary that this alloy additionally
[0023] • good heat resistance,
[0024] • good creep resistance,
[0025] • and good resistance to alternating currents
[0026] has.
[0027] This task is solved by a nickel-chromium-aluminium alloy, with (in mass-%)
[0028] Chromium > 3.1 to < 10%
[0029] aluminum and / or
[0030] Silicon 0.1 to 5%
[0031] Iron > 0.005 to 1.0%
[0032] Manganese 0.001 to < 2.0%
[0033] Titanium 0.00 to < 0.3%
[0034] Niobium 0.00 to < 2.0% Cobalt 0.00 to 30.00%
[0035] Magnesium and / or
[0036] Calcium 0.0002 to 0.05% each
[0037] Carbon 0.001 to 0.25%
[0038] Nitrogen 0.001 to 0.050%
[0039] Phosphorus 0.001 to 0.030%
[0040] Oxygen 0.0001 to 0.020%
[0041] Sulfur max. 0.010%
[0042] Molybdenum max. 10.0%
[0043] Tungsten max. 10.0%
[0044] Nickel residue with a minimum content of > 50% and the usual process-related impurities, provided that the following condition is met:
[0045] Z AI + Si > 1 %.
[0046] Advantageous further developments of the invention can be found in the associated dependent claims.
[0047] Unless otherwise stated, all alloy content specifications are in mass %.
[0048] The spreading range for the element chromium is between > 3.1 and < 10%, with preferred ranges being set as follows:
[0049] 4 to <9%
[0050] >4 to 8%
[0051] 5 to < 8%
[0052] The aluminum and / or silicon content ranges between 0.1 and 5%, whereby, depending on the application of the alloy, preferred levels may be set as follows:
[0053] 0.5 to < 5%
[0054] >0.5 to 4.8% 1.0 to 4.6%
[0055] >1.0 to 4.5%
[0056] 1.2 to 4.4%
[0057] 1.5 to 4.3%
[0058] >1.5 to 4.2%
[0059] 1.8 to 4.1%
[0060] >1.8 to 4.0%
[0061] The iron content ranges between > 0.005 and 1.0%, whereby, depending on the application, preferred contents can be set within the following ranges:
[0062] >0.01 to <1.0%
[0063] >0.05 to <1.0%
[0064] >0.1 to <1.0%
[0065] 0.2 - 0.8%
[0066] >0.2 - < 0.8 %
[0067] 0.3 - 0.7%
[0068] >0.3 - <0.7%
[0069] The same applies to the element manganese, which can be present in the alloy at a concentration of 0.1 to < 2.0%. Alternatively, the following range is also conceivable:
[0070] 0.001 - 1.5%
[0071] 0.005 - 1.0%
[0072] >0.005 - 0.5%
[0073] >0.005 - <0.5%
[0074] 0.007 - 0.1%
[0075] The titanium content is between 0 and < 0.3%. Preferably, the titanium content can be adjusted within the specified range in the alloy as follows:
[0076] 0.001 - < 0.20%
[0077] 0.001 - < 0.15%
[0078] 0.001 - < 0.10% 0.001 - < 0.05%
[0079] 0.001 - 0.02%
[0080] The Nb content is between 0 and < 2.0%. Preferably, Nb can be adjusted within the range of variation in the alloy as follows:
[0081] 0.00 - 1.7%
[0082] >0.00 - 1.50%
[0083] 0.001 - 1.30%
[0084] 0.001 - 1.00%
[0085] >0.001 - <1.00 %
[0086] >0.001 - 0.7%
[0087] >0.001 - 0.5%
[0088] >0.005 - 0.3%
[0089] >0.01 - < 0.3 %
[0090] Furthermore, the alloy can contain between 0 and 30.0% cobalt. The cobalt content can also be further restricted as follows:
[0091] 0.00 to 25.0%
[0092] 0.00 to 20.0%
[0093] 0.00 to 15.0%
[0094] >0.00 to <15.0%
[0095] 0.001 to 10.0%
[0096] 0.001 to < 10.0%
[0097] 0.001 to 8.0%
[0098] Magnesium and / or calcium are also present in concentrations of 0.0002 to 0.05%. Preferably, these elements can be adjusted in the alloy as follows:
[0099] 0.0002 - 0.03%
[0100] 0.0002 - 0.02%
[0101] 0.0005 - 0.02% The alloy contains 0.001 to 0.25% carbon. Preferably, this can be adjusted within the spreading range of the alloy as follows:
[0102] 0.001 - 0.2%
[0103] 0.001 - 0.15%
[0104] 0.005 - 0.1%
[0105] 0.01 - < 0.1%
[0106] 0.02 - 0.08%
[0107] 0.03 - < 0.08 %
[0108] 0.02 - 0.10%
[0109] 0.03 - 0.10%
[0110] This applies equally to the element nitrogen, which is present in concentrations between 0.001 and 0.05%. Preferred concentrations may be as follows:
[0111] 0.003 - < 0.04%
[0112] The alloy also contains phosphorus in amounts between 0.001 and 0.030%. Preferred amounts may be as follows:
[0113] 0.001 - 0.020%
[0114] The alloy also contains oxygen in amounts between 0.0001 and 0.020%, in particular 0.0001 to 0.010%.
[0115] The element sulfur is present in the alloy as follows:
[0116] max. 0.010%
[0117] Furthermore, the alloy can contain between 0 and 10.0% molybdenum. The molybdenum content can also be further restricted as follows:
[0118] >0.00 to 10.0%
[0119] 0.001 to 9%
[0120] 0.001 to 8%
[0121] 0.001 to 7% 0.001 to 6.5%
[0122] 0.001 to 6%
[0123] 0.001 to 5.5%
[0124] 0.001 to 5.0%
[0125] >0.001 to <5.0%
[0126] The alloy contains 0 to 10% tungsten. Preferably, this can be adjusted within the spreading range of the alloy as follows:
[0127] >0.00 to <10.0%
[0128] 0.001 to 9%
[0129] 0.01 to 8.5%
[0130] 0.05 to <8.5%
[0131] 0.1 to 8%
[0132] 0.5 to < 8%
[0133] 0.001 to 7%
[0134] 0.001 to 6.5%
[0135] 0.001 to 6%
[0136] 0.001 to 5.5%
[0137] The nickel content is greater than or equal to 50%. It can preferably be adjusted as follows:
[0138] ≥ 55% or > 55%
[0139] ≥ 60% or > 60%
[0140] ≥ 65% or > 65%
[0141] ≥ 70% or > 70%
[0142] ≥ 75% or > 75%
[0143] Optionally, the element yttrium can be adjusted in the alloy in concentrations of 0.001 to 0.20%. Preferably, Y can be adjusted in the alloy within the specified range as follows:
[0144] 0.001 - 0.15%
[0145] 0.001 - 0.10% 0.001 - 0.08%
[0146] 0.001 - < 0.045%
[0147] 0.01 - 0.15%
[0148] Optionally, the element lanthanum can be incorporated into the alloy in amounts ranging from 0.001% to 0.20%. Preferably, lanthanum can be incorporated into the alloy within the specified range as follows:
[0149] 0.001 - 0.15%
[0150] 0.001 - 0.10%
[0151] 0.001 - 0.08%
[0152] 0.001 - 0.04%
[0153] 0.01 - 0.04%
[0154] Optionally, the element cerium can be adjusted in the alloy in concentrations of 0.001 to 0.20%. Preferably, cerium can be adjusted in the alloy within the spreading range as follows:
[0155] 0.001 - 0.15%
[0156] 0.001 - 0.10%
[0157] 0.001 - 0.08%
[0158] 0.001 - 0.04%
[0159] 0.01 - 0.04%
[0160] Alternatively, cerium mischmetal can be used in concentrations of 0.001 to 0.20% when cerium and lanthanum are added simultaneously. Preferably, the cerium mischmetal can be adjusted within the alloy's range as follows:
[0161] 0.001 - 0.15%
[0162] 0.001 - 0.10%
[0163] 0.001 - 0.08%
[0164] 0.001 - 0.04%
[0165] 0.01–0.04% Alternatively, the zirconium content may be between 0.001 and 0.20%. Preferably, zirconium can be incorporated into the alloy within this range as follows:
[0166] 0.001 - 0.15%
[0167] 0.001 - < 0.10 %
[0168] 0.001 - 0.07%
[0169] 0.001 - 0.05%
[0170] 0.02 - 0.15%
[0171] 0.02 - < 0.10 %
[0172] The hafnium content is optionally between 0.001 and 0.20%. Preferably, the hafnium content within this range can be adjusted in the alloy as follows:
[0173] 0.001 - 0.15%
[0174] 0.001 - < 0.10 %
[0175] 0.001 - 0.07%
[0176] 0.001 - 0.04%
[0177] 0.01 - 0.15%
[0178] 0.01 - < 0.10 %
[0179] When adding the aforementioned elements, the following condition must be met: FRE = 0.714 x Ce + 0.720 x La + 1.124 x Y + 1.096 x Zr + 0.560 x Hf ≤ 0.10 where the elements Ce, La, Y, Zr, Hf are the concentrations of the elements in wt.% and in the case of the simultaneous presence of the elements Ce and La, cerium mischmetal (CeMM) can alternatively be used in contents of 0.001 - 0.2%, whereby FRE is then to be set as follows:
[0180] FRE = 0.716 x CeMM + 1.124 x Y + 1.096 x Zr + 0.560 x Hf ≤ 0.10, where CeMM, Y, Zr, Hf are the concentrations of the elements in wt.%.
[0181] Alternatively, the alloy can also contain 0 to 0.60% tantalum.
[0182] Preferably, tantalum can be adjusted within the spreading range in the alloy as follows:
[0183] 0.001 - 0.60% 0.001 - 0.50%
[0184] 0.001 - 0.30%
[0185] 0.001 - 0.10%
[0186] 0.00 - <0.02%
[0187] 0.01 - 0.30%
[0188] 0.01 - 0.25%
[0189] Alternatively, the element boron can be included in the alloy as follows:
[0190] 0.0001 - 0.008%
[0191] Preferred salaries may be given as follows:
[0192] 0.0005 - 0.008%
[0193] 0.0005 - 0.004%
[0194] Furthermore, the alloy may contain a maximum of 0.5% vanadium.
[0195] Furthermore, the vanadium content can be restricted as follows:
[0196] max. 0.20%
[0197] max. 0.10%
[0198] max. 0.05%
[0199] Finally, impurities such as lead, zinc, and tin may also be present in the following concentrations:
[0200] Lead max. 0.002%
[0201] Copper max. 0.5%
[0202] Zinc max. 0.002%
[0203] Tin max. 0.002%
[0204] The alloy according to the invention is preferably melted in an open furnace, followed by treatment in a VOD (vacuum oxygen decarburization) or VLF (vacuum ladle furnace) system. However, melting and casting under vacuum is also possible, as is remelting by ESU (electroslag remelting) and / or VAR (vacuum arc remelting). After casting in ingots or as continuous casting, the alloy in the desired semi-finished product shape is optionally annealed at temperatures between 900°C and 1300°C for 0.1 hours to 100 hours, then hot-formed, optionally with intermediate annealing between 900°C and 1300°C for 0.05 hours to 100 hours. The surface of the material can optionally be chemically and / or mechanically cleaned (even several times) during and / or at the end of the process. After hot forming, cold forming with deformation rates of up to 98% into the desired semi-finished product shape may be carried out, possibly with intermediate annealing between 700°C and 1250°C for 0.1 minutes to 70 hours, if necessary.The material is first annealed under a protective gas, such as argon or hydrogen, followed by cooling in air, in a moving annealing atmosphere, or in a water bath. This is followed by solution annealing at temperatures between 700°C and 1300°C for 0.1 minutes to 70 hours, optionally under a protective gas, such as argon or hydrogen, followed by cooling in air, in a moving annealing atmosphere, or in a water bath. Chemical and / or mechanical cleaning of the material surface may be performed during and / or after the final annealing process.
[0205] The alloy according to the invention can be readily produced and used in the product forms of strip, sheet, rod, wire, powder, longitudinally welded tube and seamless tube.
[0206] The alloy according to the invention is preferably intended for use in solar tower power plants using chloride and / or carbonate salt melts as a heat transfer medium. Furthermore, the alloy is intended for use in heat storage systems, salt processing, nuclear applications, ammonia crackers, and waste-to-energy plants.
[0207] It can be used for all components that come into contact with the molten salt in the temperature range of 200 - 1000°C.
[0208] It can be used, for example, for the absorber (solar receiver) in the tower of a solar power plant and / or for the heat exchanger to the power generation cycle (for example via a steam turbine) and / or for the storage and / or the transport pipes, whereby the application in the heat exchanger, storage and / or transport pipes can also be extended to other power plants such as nuclear power generation as well as to heat storage or exchangers and plants for the processing of molten salt.
[0209] The chloride and / or carbonate salt melts may preferably consist of the following mixtures:
[0210] MgCl2-KCl
[0211] MgCl2-NaCl
[0212] MgCl2-KCl-NaCl
[0213] MgCl2-NaCl-CaCl2
[0214] MgCl2-NaCl-KCl-CaCl2
[0215] MgCl2-ZnCl2-NaCl
[0216] MgCl2-ZnCl2-KCl
[0217] MgCl2-ZnCl2-CaCl2
[0218] ZnCl2-NaCl-KCl
[0219] ZnCl2-CaCl2-KCl
[0220] ZnCl2-CaCl2-NaCl
[0221] MnCI2-KCI-NaCI
[0222] NaCl-LiCl
[0223] KCI-NaCI
[0224] LiCI-KCI
[0225] LiCI-KCI-CsCI
[0226] Na2CO3-K2CO3-Li2CO3
[0227] Li2CO3-Na2CO3
[0228] Li2CO3-K2CO3
[0229] Na2CO3-K2CO3
[0230] NaCl-Na2CO3
[0231] The mixture may preferably consist of the following compositions:
[0232] 60-75% zinc chloride, 2-15% sodium chloride and 15-30% potassium chloride; 30-50% magnesium chloride and 50-70% potassium chloride
[0233] 25-40% sodium carbonate, 25-40% potassium carbonate and 25-40% lithium carbonate
[0234] The minimum operating temperature is 200°C. It may be limited as follows:
[0235] min. 250°C
[0236] min. 300°C
[0237] min. 350°C
[0238] min. 400°C
[0239] min. 450°C
[0240] min. 500°C
[0241] min. 550°C
[0242] > 550°C
[0243] The maximum operating temperature is 1000°C. It may be limited as follows:
[0244] max. 950°C
[0245] max. 900°C
[0246] max. 850°C
[0247] max. 830°C
[0248] < 830°C
[0249] max. 800°C
[0250] Evaluation of the properties:
[0251] Corrosion resistance
[0252] For an alloy containing aluminum, the formation of a continuous, closed aluminum oxide layer is crucial for corrosion resistance in chloride- and / or carbonate-containing melts at elevated temperatures. This requires minimum concentrations of the elements essential for oxide layer formation, in this case chromium and aluminum. Giggins and Pettit demonstrated that at 1200°C, concentrations between 3.5–11.0% Al and 0–40% Cr are necessary for the formation of an external Al₂O₃ layer and the prevention of internal oxidation of the aluminum [Giggins and Pettit, 1971, Oxidation of Ni-Cr-Al Alloys Between 1000° and 1200°C, J. Electrochem. Soc., 118(11), 1782–1790].
[0253] The minimum aluminum content required for formation can be significantly reduced by the addition of chromium, a phenomenon also known as the "third-element effect" [David Young, 2008, High Temp oxidation and corrosion of metals, Elsevier, pp. 334-341]. Furthermore, the formation of a continuous Al₂O₃ layer is possible for alloys with an Al content of < 3%, such as Alloy 602CA, at lower temperatures under certain atmospheres [Schiek et al., 2015, Scale Formation of Alloy 602 CA During Isothermal Oxidation at 800-1100°C in Different Types of Water Vapor Containing Atmospheres, Oxidation of Metals, 84(5-6), 661-694].
[0254] With a silicon content of < 3% and a suitable oxygen partial pressure, a SiO2 layer can also form, which has a positive influence on the isothermal and cyclic oxidation behavior [R. Bürgel, Handbook of High-Temperature Materials Engineering, 5th revised edition, 2015, p. 111],
[0255] The addition of small amounts of reactive elements such as zirconium, yttrium or cerium can further improve oxidation resistance, among other things.
[0256] A gap in the Al₂O₃ layer provides a preferred point of attack for corrosion in chloride and / or carbonate salt-containing environments. Chlorine and chloride ions lead to accelerated corrosion. The mechanism is described in detail by Grabke et al. [Grabke et al., 1995, Effects of chlorides, hydrogen chloride, and sulfur dioxide in the oxidation of steels below deposits, Corrosion Science, 37(7), 1023-1043]. According to [Kruizenga, 2012, Corrosion Mechanisms in Chloride and Carbonate Salts, SANDIA report, SAND 2012-7594], the chromium content should not be too high, as Cr ions preferentially dissolve into the molten salt under certain conditions. A sufficiently high aluminum content can slow down this process by forming a closed Al2O3 layer [George Y. Lai, 1990, High-Temperature Corrosion of Engineering Alloys, ASM International, p. 100, Fig. 6.11],
[0257] The chromium content should not be too low, as the components may be exposed to salt on the inside and ambient air on the outside. If the chromium content falls below the critical threshold, oxides other than Cr₂O₃ form, such as iron and / or nickel oxides, which exhibit significantly lower oxidation resistance than a protective passive layer of Cr₂O₃. Therefore, a sufficiently high chromium content is necessary to ensure oxidation resistance at elevated temperatures of up to 1000°C in ambient air.
[0258] In some studies, alloys with increasing nickel content exhibit improved corrosion resistance in chlorine-containing atmospheres, although the addition of molybdenum can potentially lead to catastrophic corrosion [Indacochea et al., 2001, High-Temperature Oxidation and Corrosion of Structural Materials in Molten Chlorides, Oxidation of Metals, 55(1), 1-16]. In contrast to the work of Indacochea et al., a molybdenum content of 16% and 13% in alloys C-276 and C-22, respectively, does not lead to catastrophic corrosion in the work of Vignarooban et al., which may be attributed to the investigated temperature range. This range is significantly higher in the studies of Indacochea et al. (725°C and 650°C, respectively) than in Vignarooban et al. (500°C and 250°C, respectively). The catastrophic corrosion observed in the work of Indacochea et al. at higher temperatures could therefore be caused by the formation of oxychlorides MoO₂. x Cl yThis can be explained by the fact that the formation of these compounds is extremely temperature-dependent [Klöwer et al., 1999, Chloride-induced oxidation of nickel-base alloys 600H, 625 and 626 Si, Proc. Conf. Eurocorr]. Further studies have shown that a reduced iron content in Alloy 625, compared to Alloy 800H, leads to a lower corrosion rate in sodium / lithium / chlorine salts at 650°C and 700°C, respectively [Gomez et al., 2016, Corrosion of alloys in a chloride molten salt (NaCl-LiCI) for solar thermal technologies, Solar Energy Materials and Solar Cells, 157, 234-244].
[0259] Shankar et al. investigated Alloy 600, Alloy 625, Alloy 690 and Alloy 800H and found that an increased nickel and reduced iron content is advantageous in a lithium / potassium chloride atmosphere at 400, 500 and 600°C [Shankar et al., 2013, Corrosion of Ni-containing Alloys in Molten LiCI-KCI Medium, Corrosion, 69(1), 48-57]. Furthermore, Alloy 625 shows a higher corrosion rate compared to Alloy 600 and Alloy 690, which could be explained by the significant molybdenum content (11 wt% in Alloy 625), since no molybdenum is present in Alloy 600 and Alloy 690.
[0260] These results regarding an increased nickel and reduced iron content were also observed in the work of Gomez-Vidal et al. [Gomez-Vidal et al., 2017, Corrosion resistance of alumina-forming alloys against molten chlorides for energy production: Pre-oxidation treatment and isothermal corrosion tests, Solar Energy Materials and Solar Cells, 166, 222-233]. Furthermore, it is also shown that an aluminum content of > 2% and < 4% in Alloy 702 increases the corrosion resistance by forming an Al2O3 layer.
[0261] In summary, increased nickel and aluminum content, and reduced chromium content, are highly advantageous with regard to corrosion from chlorine and / or carbonate salt melts. Silicon can also increase oxidation and corrosion resistance. The addition of iron and molybdenum should be avoided. (Heat resistance, creep resistance, and fatigue strength are also important considerations.)
[0262] An important point is adjusting the grain size to achieve the highest possible strength, both in terms of fatigue strength and creep strength.
[0263] Fine grain hardening (see Hall-Petch relationship) increases not only hot strength but also ductility and toughness at lower temperatures. However, this proves unsuitable for increasing strength at higher temperatures, as it is in the creep range (T > 0.4 T). m , with T m(=melting point) a coarse-grained microstructure is advantageous [R. Bürgel, Handbook of High-Temperature Materials Engineering, 5th revised edition, 2015, pp. 83 / 84]. The influence of grain size on creep strength or creep rate can also be mathematically described in the case of grain boundary sliding, whereby the grain diameter is inversely proportional to the creep rate. This means that the larger the average grain size, the lower the creep rate during grain boundary sliding, resulting in higher creep strength [R. Bürgel, Handbook of High-Temperature Materials Engineering, 5th revised edition, 2015, pp.
[0264]
[111] , In diffusion creep, i.e., at higher temperatures and lower applied stresses compared to grain boundary sliding, the creep rate exhibits a quadratic or cubic inversely proportional relationship. Thus, in this case, a coarser microstructure is even more crucial than in grain boundary sliding, which occurs at higher applied stresses than in diffusion creep [R. Bürgel, Handbook of High-Temperature Materials Engineering, 5th revised edition, 2015, pp. 117 / 119],
[0265] The dependence of fatigue strength or HCF strength (HCF = High Cycle Fatigue) on grain size is described by Haigh diagrams [R. Bürgel, Handbook of High-Temperature Materials Engineering, 5th revised edition, 2015, p.
[0266] 206 / 207], At lower temperatures, a finer-grained microstructure proves advantageous. In general, fatigue strength in the HCF (High Cycle Fatigue) and LCF (Low Cycle Fatigue) ranges increases with decreasing grain size at all temperatures [R. Bürgel, Handbook of High-Temperature Materials Engineering, 5th revised edition, 2015, p. 238],
[0267] The previous considerations show that a coarse-grained structure is advantageous with regard to creep resistance, but this has a negative effect on fatigue strength.
[0268] Therefore, adjusting the grain size is crucial to ensure a sensible compromise regarding creep and fatigue strength.
[0269] Therefore, the alloys according to the invention typically have a mean grain size of 10 to 500 µm.
[0270] The grain size can preferably be within the following limits:
[0271] 10 to 300 µm
[0272] 10 to 200 µm
[0273] 10 to 100 µm
[0274] 50 to 300 µm
[0275] 60 to 300 µm
[0276] 70 to 300 µm
[0277] 75 to 280 µm
[0278] 80 to 250 µm
[0279] 20 to 250 µm
[0280] 20 to 150 µm
[0281] Besides grain size, alloying elements influence the strength of the alloy at elevated temperatures, with solid solution and / or particle hardening being particularly important. In solid solution hardening, the foreign atoms interact with the dislocations and thereby impede their sliding motion. This impediment can occur due to the atomic size difference between the substitutional atoms and the matrix atoms, or due to local shear modulus changes. Dislocations are impeded even more efficiently by particle sliding, which is why this type of hardening is preferable [R. Bürgel, Handbook of High-Temperature Materials Engineering, 5th revised edition, 2015, p. 238]. Alloying elements that partially promote both hardening mechanisms include Co, Nb, and W.
[0282] The claimed limits for the alloys “E” according to the invention (Table 2a) can therefore be justified in detail as follows:
[0283] Chromium oxides are not a suitable protective layer against corrosion caused by molten chloride salts, and chromium ions preferentially dissolve upon contact with the molten salt. Therefore, a chromium content of less than 10% should not be exceeded. However, chromium is necessary to ensure the oxidation resistance of the components at elevated temperatures of up to 1000°C in ambient air. At the same time, a chromium oxide layer enables the formation of underlying aluminum and silicon oxide layers. Therefore, a lower limit of > 3.1% is the recommended chromium content.
[0284] The formation of an aluminum and / or silicon oxide layer beneath the chromium oxide layer reduces the oxidation rate. Since the oxide layers replace or complement each other, a lower limit of 0.1% for aluminum and / or silicon can be tolerated for complete oxide layer formation. However, excessively high aluminum and silicon contents impair the alloy's workability. Therefore, an aluminum and / or silicon content of 5% represents the upper limit.
[0285] The cost of the alloy increases with the reduction of the iron content.
[0286] Below 0.005%, costs increase disproportionately because special raw materials must be used. Therefore, 0.005% iron is the lower limit for cost reasons. Since the iron chlorides that form have a low melting point, the iron content should not exceed 1%.
[0287] A minimum manganese content of 0.001% is necessary to improve processability. Manganese is limited to 2.0% because this element reduces oxidation resistance.
[0288] Titanium increases high-temperature strength. Above 1.00%, oxidation behavior can deteriorate, which is why 0.3% is the maximum value.
[0289] Even very low magnesium and / or calcium contents improve processing by binding sulfur, thus preventing the formation of low-melting-point nickel-sulfur eutectics. A minimum magnesium and / or calcium content of 0.0002% is therefore required. Excessively high levels can lead to the formation of intermetallic nickel-magnesium or nickel-calcium phases, which significantly impair processability. The magnesium and / or calcium content is therefore limited to a maximum of 0.05%.
[0290] A minimum carbon content of 0.001% is necessary for good creep resistance. Carbon is limited to a maximum of 0.25% because excessive formation of primary carbides reduces workability and resistance in molten chloride salts.
[0291] A minimum nitrogen content of 0.001% is required, which improves the material's processability. Nitrogen is limited to a maximum of 0.05% because this element reduces processability by forming coarse carbonitrides.
[0292] The oxygen content must be < 0.020% to ensure the alloy's manufacturability. Too low an oxygen content increases costs. Therefore, the oxygen content is > 0.0001%. The phosphorus content should be ≤ 0.030%, as this surface-active element impairs oxidation resistance. Too low a phosphorus content increases costs. Therefore, the phosphorus content is > 0.001%.
[0293] The sulfur content should be kept as low as possible, as this surface-active element impairs oxidation resistance. Therefore, a maximum sulfur content of 0.010% is specified.
[0294] Molybdenum is limited to a maximum of 10.0%, as this element can reduce the oxidation resistance in chloride salts at elevated temperatures.
[0295] Tungsten is limited to a maximum of 10.0%, as this element not only increases heat resistance but also reduces oxidation resistance.
[0296] Niobium also increases high-temperature resistance. However, higher concentrations significantly increase costs. Therefore, the upper limit is set at 2.0%.
[0297] This alloy can contain up to 30% cobalt to increase its high-temperature strength. Excessive cobalt levels reduce oxidation resistance in air and increase costs.
[0298] If necessary, the oxidation resistance can be further improved by adding oxygen-affine elements such as yttrium, lanthanum, hafnium, cerium, and cerium mischmetal. These elements do this by being incorporated into the oxide layer and blocking oxygen diffusion pathways at the grain boundaries. A minimum yttrium content of 0.001% is required to achieve the oxidation-resistance-enhancing effect of yttrium. For cost reasons, the upper limit is set at 0.20%.
[0299] A minimum lanthanum content of 0.001% is necessary to achieve the oxidation-resistant effect of lanthanum. For cost reasons, the upper limit is set at 0.20%.
[0300] The alloy can also contain hafnium if required. A minimum hafnium content of 0.001% is necessary to achieve the high-temperature strength and oxidation resistance benefits of hafnium. For cost reasons, the upper limit is set at 0.20% hafnium.
[0301] A minimum cerium content of 0.001% is necessary to achieve the oxidation-resistant effect of cerium. For cost reasons, the upper limit is set at 0.20%.
[0302] A minimum content of 0.001% cerium mischmetal is necessary to achieve the oxidation-resistant effect of the cerium mischmetal. For cost reasons, the upper limit is set at 0.20%.
[0303] The alloy can also contain tantalum if required, as tantalum also increases high-temperature strength. Higher contents significantly increase costs. Therefore, the upper limit is set at 0.60%. A minimum content of 0.001% is required to achieve an effect.
[0304] The alloy can also contain zirconium if required. A minimum zirconium content of 0.001% is necessary to achieve the high-temperature strength and oxidation resistance benefits of zirconium. For cost reasons, the upper limit is set at 0.20% zirconium. Boron can also be added to the alloy if required, as it improves creep resistance. Therefore, a content of at least 0.0001% should be present. However, this surface-active element also reduces oxidation resistance. Therefore, a maximum boron content of 0.008% is specified.
[0305] Vanadium is limited to a maximum of 0.5%, as this element also reduces oxidation resistance.
[0306] Lead is limited to a maximum of 0.002% because this element reduces oxidation resistance. The same applies to zinc and tin. Table 1: Alloys according to ASTM B 168-19 1 > / ASTM B167-18 2) , ASTM B 163-18 3 >, ASTM B409-06 4) , ASTM B443-18 5) and 6) not in any STM or ASME standard. 7) from the UNS list, AMS 5550 8) All figures are given in mass percent.
[0307]
[0308] Table 2a: Alloy compositions according to the invention (E) and alloy compositions according to the prior art (T). Element content in mass %; Chg. = Batch number, or in the case of the JMatPro calculations, it corresponds to the composition number; all batches have Pb < 0.002%, Sn < 0.002% and Zn < 0.002%; *) Nominal composition. **) No formation of the / -phase.
[0309]
Claims
Patent claims 1. Nickel-chromium-aluminum alloy, with (in mass %) Chromium > 3.1 to < 10% Aluminum and / or silicon 0.1 to 5% Iron > 0.005 to 1.0% Manganese 0.001 to < 2.0% Titanium 0.00 to < 0.3% Niobium 0.00 to < 2.0% Cobalt 0.00 to 30.00% Magnesium and / or Calcium 0.0002 to 0.05% each Carbon 0.001 to 0.25% Nitrogen 0.001 to 0.050% Phosphorus 0.001 to 0.030% Oxygen 0.0001 to 0.020% Sulfur max. 0.010% Molybdenum max. 10.0% Tungsten max. 10.0% Nickel residue with a minimum content of > 50% and the usual process-related impurities, provided that the following condition is met: ∑ Al + Si > 1 %.
2. Alloy according to claim 1, with a chromium content of > 3.2 to < 10%.
3. Alloy according to any one of claims 1 to 2, having an aluminum and / or silicon content of 0.5 to < 5%.
4. Alloy according to any one of claims 1 to 2, having an iron content of >0.2 to <1.0%.
5. Alloy according to any one of claims 1 to 3, having a silicon content of > 0.1 to < 4.0%.
6. Alloy according to any one of claims 1 to 4, having a manganese content of 0.001 to 1.5%.
7. Alloy according to any one of claims 1 to 6, having a titanium content of 0.001 to < 0.3%.
8. Alloy according to any one of claims 1 to 7, having a niobium content of 0.001 to < 1.7%.
9. Alloy according to any one of claims 1 to 8, having a carbon content of 0.001 to 0.20%.
10. Alloy according to any one of claims 1 to 9 optionally containing 0.00 to 25.0% cobalt.
11. Alloy according to any one of claims 1 to 10, optionally with a yttrium content of 0.001 to 0.20%.
12. Alloy according to any one of claims 1 to 11, optionally comprising lanthanum with a content of 0.001 to 0.20%.
13. Alloy according to any one of claims 1 to 12, optionally comprising cerium with a content of 0.001 to 0.20%.
14. Alloy according to any one of claims 1 to 13, optionally with a cerium mischmetal content of 0.001 to 0.20%.
15. Alloy according to any one of claims 1 to 19, optionally comprising zirconium with a content of 0.001 to 0.20%.
16. Alloy according to any one of claims 1 to 15, optionally with a hafnium content of 0.001 to 0.20%.
17. Alloy according to any one of claims 11 to 16, wherein the following requirement must be met: FRE = 0.714 x Ce + 0.720 x La + 1.124 x Y + 1.096 x Zr + 0.560 x Hf ≤ 0.10 where the elements Ce, La, Y, Zr, Hf are the concentrations of the elements in wt.% and in the case of the simultaneous presence of the elements Ce and La, cerium mischmetal (CeMM) can alternatively be used in contents of 0.001 - 0.2%, whereby FRE is then to be set as follows: FRE = 0.716 x CeMM + 1.124 x Y + 1.096 x Zr + 0.560 x Hf ≤ 0.10, where CeMM, Y, Zr, Hf are the concentrations of the elements in wt.%.
18. Alloy according to any one of claims 1 to 17, optionally comprising boron with a content of 0.0001 to 0.008%.
19. Alloy according to any one of claims 1 to 18, further optionally containing a maximum of 0.5% vanadium.
20. Alloy according to any one of claims 1 to 19, wherein the impurities are adjusted to levels of max. 0.002% Pb, max. 0.5%, max. 0.002% Zn, max. 0.002% Sn.
21. Alloy according to any one of claims 1 to 20 for components that are in contact with molten salt.
22. Alloy according to any one of claims 1 to 21, wherein the components are exposed to temperatures from 200°C to a maximum of 1000°C.
23. Use of the alloy according to any one of claims 1 to 22 as strip, sheet, wire, rod, longitudinally welded tube or seamless tube.
24. Use of the alloy according to any one of claims 1 to 22 as a powder.
25. Use of the alloy according to any one of claims 1 to 22 for the production of strip, sheet, wire, rod, powder, longitudinally welded tube and seamless tubes.
26. Use of the alloy according to any one of claims 1 to 22 for the production of powder.
27. Use of the alloy according to any one of claims 1 to 22 in solar tower power plants.
28. Use of the alloy according to any one of claims 1 to 22 in heat storage systems.
29. Use of the alloy according to any one of claims 1 to 22 in small modular nuclear reactors.
30. Use of the alloy according to any one of claims 1 to 22 in heating and cooling systems for industrial processes.
31. Use of the alloy according to any one of claims 1 to 22 for components in chemical recycling processes.
32. Use of the alloy according to any one of claims 1 to 22 for components in industrial process heat systems.