Method for obtaining lithium in the form of lithium carbonate from a lithium-containing material
The hydrothermal digestion of lithium-containing materials with iron(III) salts addresses the inefficiencies of existing lithium extraction methods, achieving high lithium recovery with lower chemical consumption and waste, applicable to diverse lithium sources.
Patent Information
- Application Number
- PCT/EP2026/062232
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-06
- Filing Date
- 2026-04-28
- Publication Date
- 2026-11-12
AI Technical Summary
Existing lithium extraction processes from spodumene ores are resource-intensive, require large quantities of chemicals, generate significant waste, and are not applicable to all lithium-containing materials, primarily relying on salt lakes and geographically restricted sources.
A method involving hydrothermal digestion of lithium-containing materials with iron(III) salts like iron(III) sulfate, followed by pH adjustment and separation of lithium carbonate, reducing chemical consumption and waste production, and enabling extraction from a broader range of lithium sources.
Achieves nearly complete lithium mobilization with significantly reduced chemical usage and waste generation, making the process more cost-effective and environmentally friendly while being applicable to various lithium-containing materials.
Smart Images

Figure EP2026062232_12112026_PF_FP_ABST
Abstract
Description
[0001] patent application
[0002] Method for extracting lithium in the form of lithium carbonate from a lithium-containing material
[0003] The invention relates to a process for obtaining lithium in the form of lithium carbonate from a lithium-containing material. The process is suitable for obtaining lithium in the form of lithium carbonate from both natural and non-natural lithium-containing materials. This applies in particular to all lithium ores and many known lithium-containing technical materials. To date, no other process for obtaining lithium has such broad applicability. According to one embodiment of the invention, the lithium-containing material can be a lithium-containing mineral, preferably a silicate lithium-containing mineral, for example, spodumene.Furthermore, the invention is also applicable to the extraction of lithium from a lithium-containing borate glass or borosilicate glass material, as well as to the extraction of lithium from lithium-containing waste batteries and / or accumulators and / or from waste generated during the manufacture of lithium-containing batteries and / or accumulators.
[0004] Lithium, in the form of its compounds, has experienced high demand since the last decade, primarily due to its use in lithium-ion batteries. Production volume increased from 35 kilotons in 2013 (Brian Jaskula 2014) to 180 kilotons in 2023 (Brian Jaskula 2024), representing a rise of over 400% in just ten years. This increase is mainly attributable to the use of lithium-ion batteries in vehicles, whose large battery packs require significant amounts of lithium. This use, combined with rising sales of electric vehicles, explains the rapid increase in demand for lithium compounds. Syntheses for the active materials of lithium-ion batteries, typically nickel-manganese-cobalt lithium oxides (NMC) or lithium iron phosphate (LFP), start from lithium carbonate or lithium hydroxide (Dünn et al. 2015).This, and the convertibility of lithium carbonate into any other relevant lithium compound, explains the relevance of lithium carbonate in the chemical industry.
[0005] Lithium compounds are currently extracted industrially primarily from two sources: salt flats (salar), which are lithium-bearing salt lakes, and lithium-bearing ores (Battistel et al. 2020 and Swain, Badusev 2017). The extraction route via the former source, besides the presence of these salt flats, is limited to regions of the world with a dry climate, strong, dry winds, and high solar irradiance. This geographically restricts the extraction process essentially to South America, particularly Chile (Grosjean et al. 2012).
[0006] In contrast, lithium is primarily extracted from ores containing spodumene, with the minerals lepidolite and petalite playing a minor role (Gao et al. 2023). The lithium-bearing mineral spodumene is a relatively rare chain silicate belonging to the pyroxene group. It crystallizes with monoclinic symmetry, has the end-membered composition LiAl[Si20e], and typically forms short, flattened crystals with distinct longitudinal striations. Of particular regional interest in Central Europe is the zinnwaldite deposit in Zinnwald / Cinovec on the border between Germany and the Czech Republic (Schneider et al. 2017 and Qiao et al. 2024).
[0007] As is common with other ore deposits, lithium-bearing ores must first be crushed and concentrated. For the mineral spodumene, concentration is typically achieved by flotation and density separation (Tadesse et al.).
[0008] 2019). Typical concentrate contents range from 70% to 80% spodumene by mass, corresponding to a lithium content of approximately 3%. The lithium can hardly be mobilized from the α-spodumene phase contained in the generated spodumene concentrate; therefore, the concentrate undergoes a thermal treatment called calcination at 1000 °C to 1100 °C for a period of 30 minutes to 2 hours (Dessemond et al. 2019; Li et al. 2019). The term "calcination," which originally referred to lime burning and the associated decarbonization or dehydration, is now used more broadly for a variety of thermal processes, including this type of thermal treatment of α-spodumene concentrate. In this process, the α-spodumene reacts to form β-spodumene. That β-spodumene is metastable, meaning it remains a component of the concentrate even after the calcined concentrate has cooled.The calcined concentrate can then be digested with concentrated sulfuric acid at 250 °C for a period of about 30 minutes (Kuang et al.
[0009] (2018). Such digestion almost completely mobilizes the lithium present. In addition, further cations from accompanying minerals in the spodumene concentrate are typically mobilized, particularly sodium, potassium, magnesium, and iron ions. Magnesium and iron ions can be separated as hydroxides during subsequent pH adjustment using lime milk, an aqueous suspension of calcium hydroxide (Ca(OH)₂). Filtration of the resulting suspension yields lithium carbonate (Li₂CO₃) by adding sodium carbonate while simultaneously heating to 90 °C, leaving an aqueous solution of sodium sulfate and lithium carbonate (Li et al. 2019).
[0010] A significant disadvantage of this or similar processes known from the prior art for the production of lithium carbonate (Li₂CO₃) from spodumene is that large quantities of concentrated sulfuric acid are required for the aforementioned digestion of the calcined concentrate with sulfuric acid. A further disadvantage is that, consequently, large quantities of lime milk are also required for the necessary subsequent increase in pH. In total, 25 to 30 tons of chemicals are consumed per ton of the target product, lithium carbonate. Furthermore, a significant disadvantage is that 80 to 120 tons of waste are generated for every ton of lithium carbonate produced.
[0011] Furthermore, the process is very energy- and resource-intensive, even in the preliminary stages, during the production of the chemicals, due to the material flows that need to be managed. The waste products are generally not economically viable. Finally, a lithium loss of up to 20% must be expected during the purification process. Another disadvantage is that, to date, there is no process suitable for all known lithium-containing ores, with the exception of lithium compounds found in salt lakes (salars).
[0012] The object of the invention is to provide a cost-effective method for obtaining lithium carbonate from a lithium-containing ore, such as spodumene, whereby only small amounts of waste should be produced in this process.
[0013] This problem is solved by a method with the features according to claim 1. Further developments are specified in the dependent claims.
[0014] The inventive process for obtaining lithium in the form of lithium carbonate from a lithium-containing material generally comprises the process steps
[0015] ao) Pretreatment of a concentrate of the lithium-containing material, in which a thermal treatment of the lithium-containing material is carried out by tempering it,
[0016] a) Hydrothermal digestion of the concentrate of the lithium-containing material with an iron(II) salt, preferably iron(II) sulfate, and water until the lithium is completely or almost completely mobilized and transferred into an aqueous or liquid phase of a suspension resulting from the hydrothermal digestion; b) Separation of solid components of the suspension directly resulting from the hydrothermal digestion from the aqueous or liquid phase to form a digestion solution; c) Raising the pH of the digestion solution to a pH of 10 to 12 and separating any precipitates of polyvalent cations formed as hydroxides from the digestion solution;
[0017] d) Recovery of the mobilized lithium from the digestion solution freed from multivalent cations by precipitation and separation as lithium carbonate.
[0018] Nearly complete mobilization of lithium in process step a) means that at least 95% of the lithium in the lithium-containing material is mobilized. Advantageously, after each separation in steps b), c), and d), the remaining iron(III) salt or the remaining digestion solution (mother liquor) can be recycled and reused to minimize lithium losses. Specifically, after the recovery of lithium carbonate from the digestion solution freed of multivalent cations in process step d), the remaining digestion solution can be returned to process step a) and / or process step c).
[0019] The process according to the invention allows lithium to be obtained as lithium carbonate from a silicate lithium-containing material in the form of a silicate lithium-containing mineral. One or more minerals, such as spodumene, petalite, zinnwaldite, lepidolite, eucryptite, and sugilite, can be selected as starting materials. Spodumene is particularly preferred as a starting material. The invention is also applicable to non-silicate lithium-containing minerals, including lithium-containing phosphates such as amblygonite and lithium iron phosphate (LFP, LiFe₃PO₄), lithium-containing oxides, mixed oxides, and oxide hydroxides such as lithiophorite, as well as lithium-containing borates and borosilicates such as jadarite.Furthermore, the production of lithium carbonate by the inventive process from lithium-containing borate glasses or borosilicate glasses, in particular lithium oxide-aluminum oxide-silicon oxide glass ceramics (LAS glass ceramic), is possible.
[0020] In all cases where silicate lithium-containing material is used as starting material, in process step c), i.e. when raising the pH of the digestion solution to a pH of pH10 to pH12, not only do multivalent cations precipitate as hydroxides from the digestion solution, but silicon also precipitates in the form of sparingly soluble silicates, which can then also be separated from the digestion solution.
[0021] Particularly when using a silicate lithium-containing mineral as the starting material, process step ao), preceding the hydrothermal digestion in process step a), is advantageous as a pretreatment of the concentrated mineral. This pretreatment involves a thermal treatment of the mineral, also known as calcination, by annealing it, preferably at a temperature in the range of 900 °C to 1100 °C, and especially preferably for a period of 30 minutes to 2 hours. This is because silicate lithium-containing minerals largely exist in a phase from which the lithium can hardly be mobilized. In the case of spodumene, this applies to the α-spodumene phase.During the thermal treatment, which in the case of spodumene is preferably carried out at a temperature in the range of 1000 °C to 1100 °C, the α-spodumene reacts to form β-spodumene, which is metastable and remains a component of the thermally treated concentrate even after cooling. Furthermore, the thermal treatment of α-spodumene, as well as the thermal treatment of other lithium-containing materials, can be carried out in a process step ao) in the presence of soda (sodium carbonate, Na₂CO₃), which in the case of spodumene is preferably carried out at a temperature in the range of 700 °C to 800 °C. The thermal treatment of the silicate lithium-containing mineral or other lithium-containing materials generally facilitates the mobilization of lithium.The problem mentioned above, which arises in the prior art, is circumvented according to the invention by using an iron(III) salt, preferably iron(III) sulfate hydrate, hereinafter referred to as iron(III) sulfate. The process according to the invention bypasses the classical digestion with concentrated sulfuric acid and replaces it with a digestion using an iron(III) salt such as iron(III) sulfate, iron(III) chloride, or iron(III) nitrate, or with one of their respective hydrates. Iron(III) salts such as iron(III) sulfate, iron(III) chloride, or iron(III) nitrate also react acidic, thereby releasing protons into the solution. Surprisingly, it was found that the presence of iron(III) ions, for example in the form of aquo complexes or mixed aquo complexes with other anions such as sulfate or hydrogen sulfate, is crucial for successful digestion.Furthermore, when comparing a hydrothermal digestion with iron(III) sulfate with a hydrothermal digestion carried out with sulfuric acid at the same molality, it was surprisingly found that with iron(III) sulfate a lithium mobilization of about 98% could be achieved within three hours, while with sulfuric acid the lithium mobilization after the same digestion time was only about 44%.
[0022] According to an advantageous embodiment of the invention, the process comprises a process step preceding process step a), in which the concentrate of the silicate lithium-containing material is produced for hydrothermal digestion. In the case of a lithium-containing mineral, this can be done, as usual, by crushing an ore containing the lithium-containing mineral and subsequently concentrating the lithium-containing mineral, for example by flotation and / or density separation.
[0023] According to a further embodiment of the invention, the lithium-containing material can originate from used lithium-containing batteries and / or accumulators and / or from waste generated during the production of lithium-containing batteries and / or accumulators. Advantageously, the lithium-containing material is already available in a comminuted and concentrated form as a so-called black mass, resulting from the application of mechanical comminution processes typically carried out prior to actual recycling. The black mass contains metals for the production of cathode materials, including lithium, and in this form is directly suitable for hydrothermal digestion according to process step a).According to one embodiment of the inventive method, the lithium-containing material originates at least partially from lithium-containing nickel-manganese-cobalt batteries and / or nickel-manganese-cobalt accumulators (NMC) and / or lithium iron phosphate batteries and / or lithium iron phosphate accumulators (LFP).
[0024] The hydrothermal digestion in process step a) is preferably carried out with solid-liquid mass ratios of 1:2 to 1:10, particularly preferably in the range of 1:2 to 1:4. For the hydrothermal digestion according to the invention, it is advantageous to use 1.25 to 4 times, for example 2.5 times, the mass of iron(III) sulfate hydrate (Fe2(SO4)3 ■ n H2O) compared to the mass of the concentrate of the lithium-containing material, optionally compared to the mass of the concentrate of the silicate lithium-containing mineral pretreated by thermal treatment, as in the case of spodumene.
[0025] Hydrothermal digestion can be carried out in any gas-tight, corrosion-resistant pressure vessel suitable for the thermal treatment of substances under pressure, for example, in an autoclave. The digestion temperature is advantageously in the range of 200 °C to 300 °C, typically 230 °C. The duration of the hydrothermal digestion, which corresponds to the period during which the digestion temperature is maintained, is generally 2 to 3 hours.
[0026] The suspension produced during hydrothermal digestion in process step a) can be filtered in process step b) to separate solid components, with the liquid phase now containing the lithium as the digestion solution. Depending on the starting material used and the iron(II) salt used for the hydrothermal digestion, other mobilized components such as iron, aluminum, silicon, and sulfate may also be present in the digestion solution. Depending on the purity of the original concentrate, sodium, potassium, and magnesium may also be mobilized.
[0027] According to an advantageous embodiment of the invention, the digestion solution can be recycled after the separation of solid components in process step b) by being fed back into process step a), the hydrothermal digestion of further lithium-containing material. In this way, the digestion solution can be recycled and recovered repeatedly after the separation of solid components, for example as a filtrate or as a permeate, until a lithium concentration necessary for subsequent lithium precipitation is achieved in the digestion solution. Alternatively, a permeate from membrane filtration can be recycled, preferably after lithium carbonate precipitation. The latter option is particularly advantageous if otherwise an accumulation of interfering ions would occur in the digestion solution.
[0028] According to an advantageous embodiment of the process, iron-containing residues contained in the separated solid components can be recovered and utilized. These residues, which arise alongside aluminosilicate components after hydrothermal digestion, can be separated from the liquid phase of the suspension directly resulting from the hydrothermal digestion. This possibility is particularly suitable when iron(II) sulfate and a hydrate of iron(III) sulfate are used as iron(III) salts, and the iron-containing residues, under suitable process conditions, contain at least some hydronium jarosite, which corresponds to the chemical formula (H3O)Fe3(SO4)2(OH)e. It has been found that a significant proportion of the sulfate contained in such a hydronium jarosite-containing residue can be recovered in the form of iron(II) sulfate by thermal treatment followed by leaching with water.For this purpose, the residue is preferably calcined at temperatures in the range of 550 °C to 650 °C, particularly at about 600 °C, for a duration of typically one to three hours. The calcined residue can then be leached with water, preferably at room temperature (20 °C), yielding a solution stream containing iron(III) sulfate. Under suitable conditions, up to about 75 wt% of the sulfate contained in the residue can be dissolved in this way. The resulting iron(III) sulfate stream can then be at least partially recycled back into process step a), the hydrothermal digestion. To adjust the desired process parameters, in particular the iron(III) and sulfate concentrations, the recycled stream can be supplemented by adding fresh iron(III) sulfate.
[0029] Several methods are available to separate the iron contained in solution during hydrothermal digestion due to the use of an iron(III) salt, such as iron(II) sulfate. These include methods such as precipitation, extraction, and nanofiltration.
[0030] According to one embodiment of the process according to the invention, the separation of iron in process step c) can be achieved by separating mobilized multivalent cations from the digestion solution by hydroxide precipitation after raising the pH, preferably by adding lime milk, to a pH of 10 to 12, and subsequent separation, preferably by filtration. Instead of filtration, usually sieve or depth filtration, separation by sedimentation is also possible. The use of lime milk to raise the pH is advantageous, among other things, when using iron(II) sulfate, because in this case calcium reacts with the sulfate ions (SCk) contained in the filtrate, which originate predominantly from the iron(II) sulfate used in the hydrothermal digestion. 2-) to calcium sulfate, which also precipitates. The advantage of the present invention compared to a prior art process in which a hydrothermal digestion with sulfuric acid is carried out could be demonstrated with regard to chemical consumption per mass of recovered lithium carbonate, particularly for an embodiment in which spodumene, as a lithium-containing material, was hydrothermally digested with iron(III) sulfate in process step a) and the pH value was raised in process step c) by adding milk of lime.In this process, only 4 tons of calcium hydroxide and 9 tons of iron sulfate are produced for each ton of lithium carbonate obtained, whereas in a previously mentioned state-of-the-art process, in which spodumene is hydrothermally digested with concentrated sulfuric acid and the pH value is also raised by adding lime milk, 25 to 30 tons of chemicals are consumed per ton of lithium carbonate obtained.
[0031] Following the separation of the polyvalent cations, lithium carbonate (Li₂CO₃) can be precipitated in process step d) by adding sodium carbonate. If sodium sulfate precipitates together with the lithium carbonate in this step, it can be separated by hot washing of the crude product. After separation of the Li₂CO₃ product, the filtrate or permeate of the Li₂CO₃ precipitation can either be combined with the solution to raise the pH or fed to the hydrothermal digestion process.
[0032] The separation of iron(III) ions from the digestion solution can be carried out in a process step (co) preceding the pH increase in process step c) by extracting the digestion solution with di(2-ethylhexyl)phosphoric acid (DEHPA), preferably at a concentration of 0.6 mol / L, in a weakly polar solvent, for example, kerosene. Depending on the iron content, multiple extractions with DEHPA or CYANEX® 572 may also be advantageous. Regardless of the choice of solvent, only iron(III) ions are extracted. Aluminum is subsequently precipitated as hydroxide during the pH increase, when the digestion solution, now free of iron(III) ions, is adjusted to a pH between pH 10 and pH 12, preferably by adding milk of lime. According to one embodiment of the process, the extracted iron(III) ions can be recycled, i.e., returned to the hydrothermal digestion process.
[0033] According to a further embodiment of the process according to the invention, in a process step co) preceding the raising of the pH value in process step dc), iron ions and aluminum ions are separated from the digestion solution by means of nanofiltration. The nanofiltration permeate obtained by such nanofiltration is then adjusted to a pH value between pH 10 and pH 12, preferably by adding lime milk.
[0034] Further details, features, and advantages of embodiments of the invention will become apparent from the following description of exemplary embodiments with reference to the accompanying drawings. These show:
[0035] Fig. 1: a flow diagram of a prior art process for obtaining lithium carbonate from a spodumene-containing ore and
[0036] Fig. 2 : a flow diagram according to an embodiment of the process according to the invention for obtaining lithium carbonate from spodumene.
[0037] Figure 1 shows an example flow diagram of the so-called spodumene process, known from the prior art. As already mentioned, spodumene-containing ores must first be crushed and concentrated, which can be done by flotation and density separation. The resulting spodumene concentrate typically has a spodumene content of 70% to 80% by mass and thus a lithium content of about 3%.
[0038] The lithium can hardly be mobilized from the α-spodumene phase contained in the produced spodumene concentrate. Therefore, a thermal treatment is carried out by annealing the concentrate at 1000 °C to 1100 °C for 30 minutes to 2 hours. During this process, the α-spodumene reacts to form β-spodumene. This β-spodumene is metastable and thus remains a component of the concentrate even after cooling. Subsequently, the β-spodumene-containing concentrate is digested with concentrated sulfuric acid at 250 °C for approximately 30 minutes. This digestion can almost completely mobilize the lithium. In addition, further cations from accompanying minerals in the spodumene concentrate are typically mobilized, particularly sodium ions, potassium ions, magnesium ions, and aluminum ions.After digestion and a further thermal treatment (calcination) of the spodumene concentrate, it is leached with water and subsequently filtered, leaving silicates as a residue. The filtrate is then mixed with lime milk to raise the pH and induce an initial purification precipitation. Mobilized magnesium precipitates as Mg(OH)₂ and mobilized aluminum as Al(OH)₃. Iron ions can also be precipitated as hydroxides in the same way. In addition, calcium combines with the sulfate ions (SCM) present in the filtrate, which originate predominantly from the sulfuric acid. 2-) to calcium sulfate or gypsum (CaSCk₂·2H₂O), which also precipitates. A second purification precipitation then takes place by adding sodium carbonate (Na₂CO₃), which precipitates any remaining magnesium and calcium ions in the suspension produced during the first purification precipitation as carbonates (MgCO₃ and CaCO₃, respectively). The hydroxides, sulfates, and carbonates precipitated in the first and second purification precipitations are then separated by filtration. Further sodium carbonate is added to the filtrate while simultaneously heating it to 70–90 °C to precipitate the lithium as lithium carbonate (Li₂CO₃) (production precipitation).
[0039] A significant disadvantage of this or similar processes known from the prior art for the extraction of lithium carbonate (Li2COs) from spodumene is that, per ton of the target product lithium carbonate obtained, excessive quantities of chemicals, especially concentrated sulfuric acid and lime milk, are required (25 to 30 tons), and, moreover, excessive amounts of waste products (80 to 100 tons) that are not economically viable are generated.
[0040] The flow diagram in Fig. 2 illustrates the inventive process for the production of lithium carbonate by way of example, using the production of lithium carbonate from a spodumene concentrate. For each ton of lithium carbonate produced, this process consumes only approximately 4 tons of calcium hydroxide and approximately 9 tons of iron sulfate, which represents a significant reduction in chemical consumption compared to the process route for the production of lithium carbonate from spodumene shown in Fig. 1. The inventive process can also be carried out analogously with, among other things, the starting materials petalite, zinnwaldite, lepidolite, eucryptite, and sugilite, or more generally, as listed above, with silicate lithium-containing minerals, but also with other lithium-containing materials.
[0041] The elemental composition of spodumene as the starting material is listed in Table 1 below.
[0042] Table 1: Element content of the spodumene concentrate in weight %.
[0043] Element Li Na Mg AI Si K Ca Fe
[0044]
[0045] % by weight 3~3 Ö7 Ö~5 HO 32?6 ^2 ÖJ ^2
[0046] As a pretreatment, the spodumene concentrate is thermally treated for one hour at 1100 °C to bring about a phase change from α-spodumene to β-spodumene.
[0047] For the hydrothermal digestion of spodumene with iron(III) sulfate, 45 g of the thermally pretreated spodumene concentrate and 112.5 g of iron(III) sulfate hydrate (Fe₂(SO₄)₃-n H₂O) from Honeywell Speciality Chemicals Seelze GmbH (article number 307718-500g) are placed in an autoclave (i.e., a gas-tight sealable pressure vessel for the thermal treatment of substances under pressure), comprising an autoclave bowl and an autoclave head attached to it with a seal. This corresponds to a mass ratio of 2:5. 360 g of water are added. The autoclave head with seal is placed on the autoclave bowl and closed. The entire autoclave is then placed in a heating block and heated to the digestion temperature, typically 230 °C. Once this digestion temperature is reached, the temperature is maintained for the digestion period, which is usually 3 hours.Alternatively, the digestion can then be quenched in the autoclave, or the autoclave can remain in the heating block. Furthermore, for a technical application, alternating operation is also possible, in which, after successful hydrothermal digestion in a first reactor, the heat from this first reactor can be used to heat a second reactor for further hydrothermal digestion (heat flow integration), so that only the heat losses need to be compensated for to fully heat the second reactor.
[0048] After cooling the autoclave to a temperature that allows filtration, usually—but not necessarily—below 30 °C, the autoclave head is removed, and the resulting suspension can then be filtered, preferably by sieve or depth filtration, which separates the suspension into a retentate and a permeate. A retentate is the fluid retained during the separation process. The permeate is the opposite, namely the fluid freed from the substances contained in the retentate by filtration. If the lithium concentration has not yet been reached to allow for economical lithium recovery, the digestion solution is then used to digest new β-spodumenes using additional iron(III) sulfate. This allows lithium to accumulate in the solution.In other words, the digestion solution is recycled until a lithium concentration necessary for subsequent lithium precipitation is reached. The hydrothermal digestion is carried out with solid-liquid ratios up to 1:4, with consistently quantitative lithium mobilization.
[0049] As previously mentioned, β-spodumene acts as an ion exchanger with respect to protons, exchanging protons from the solution for lithium ions bound to the β-spodumene. Consequently, the retentate from the filtration after hydrothermal digestion contains, in addition to hematite and potassium alum (KAI(SO4)2), the hydrogen compound HAI[Si2Oe], which corresponds to the end-membered composition LiAI[Si2Oe] of spodumene. Furthermore, depending on the chosen process conditions, iron-containing residues can also be found in the retentate alongside aluminosilicate components such as those mentioned.
[0050] In contrast, the lithium previously bound in β-spodumene is completely mobilized into the liquid phase by hydrothermal digestion and subsequently transferred into the permeate by filtration. The resulting composition of the permeate is shown in Table 2 below.
[0051] Table 2: Composition of the permeate from the filtration after hydrothermal digestion (leaching solution), mass fractions of the elements in ppm
[0052] Element mass fraction in ppm
[0053]
[0054] Li 3104 ± 51
[0055] Na 25 ± 3
[0056] AI 2270 ± 1345
[0057] Si 311 ± 21
[0058] S 37792 ± 5408
[0059] K 7 ± 1
[0060] Approximately 7 ± 1
[0061] Fe 16796 ± 139 The separation of iron, aluminum, and silicon can be achieved via several methods. The following describe the methods of precipitation, extraction, and nanofiltration.
[0062] Lithium carbonate cannot be directly precipitated from the resulting, strongly acidic filtrate. To minimize the introduction of foreign ions, calcium hydroxide is used to raise the pH. The calcium remaining in solution, due to the (albeit slight) solubility of gypsum or CaSCM, is precipitated by adding sodium oxalate (Na₂C₂O₄) in a 1.1-fold stoichiometric excess. The suspension produced in this step is separated into a permeate and a retentate by filtration, preferably by sieve and depth filtration.
[0063] The filter residue contains iron, aluminum and silicon in the form of their respective hydroxides or as silicate, as well as gypsum, i.e. CaSO4, which can exist in various hydration states, and to a small extent also calcium oxalate.
[0064] The filtrate obtained after pH adjustment is depleted in iron, aluminum, and silicon compared to the digestion solution obtained immediately after hydrothermal digestion. Most of the introduced calcium precipitates from the solution as gypsum. The remaining calcium is precipitated by adding sodium oxalate. The lithium remains in the filtrate after filtration.
[0065] Lithium carbonate (Li₂CO₃) is precipitated from the filtrate after pH adjustment by adding a stoichiometric amount of sodium carbonate. Sodium sulfate also precipitates alongside the desired lithium carbonate. The solid is then filtered off, in the embodiment shown in Fig. 2 by membrane filtration. The filter cake, or retentate, is then washed with hot water at a temperature of 90 °C. In membrane filtration, retentate refers to the fluid that, similar to the filter cake in conventional filtration, is retained by the membrane during the separation process. Permeate refers to the opposite, namely the fluid freed from the substances contained in the retentate by the membrane filtration, and thus essentially corresponds to the filtrate of conventional filtration.
[0066] Lithium carbonate with a purity of 99.5% can be obtained via this route. Both the permeate from filtration of the solid after lithium carbonate precipitation and the wash solution obtained from washing with hot water contain lithium carbonate and sodium sulfate at their solubility limits. Due to their lithium content, recycling the permeate and / or the wash solution back into the process is advantageous. The permeate and / or the wash solution is therefore preferably combined with the solution used for pH adjustment. Alternatively, recycling the filtrate and / or the wash solution back into the hydrothermal digestion step is possible.
[0067] As an alternative to precipitation, as already mentioned, there are other suitable methods for separating multivalent ions such as iron ions and aluminum ions from the digestion solution obtained immediately after hydrothermal digestion, for example in the form of extraction or nanofiltration.
[0068] During extraction, the digestion solution is extracted with 0.6 M di(2-ethylhexyl)phosphoric acid (DEHPA) in kerosene or another weakly polar solvent. Depending on the iron content, multiple extractions may be necessary. The extracted iron(III) ions can be recycled, meaning they can be returned to the hydrothermal digestion process. The previously described pH increase procedure can be used to obtain lithium carbonate.
[0069] Monovalent cations can be separated from polyvalent cations via nanofiltration. This allows for the selective separation of lithium from the polyvalent ions of aluminum and iron present in solution. The lithium-containing nanofiltration permeate is then adjusted to a pH between 10 and 12, and the lithium is precipitated as lithium carbonate (Li₂CO₃) by adding sodium carbonate.
[0070] According to an advantageous embodiment of the process, iron-containing residues can be recovered and utilized. As mentioned above, these residues, depending on the selected process conditions, are obtained as solid components alongside aluminosilicate components after hydrothermal digestion and can be separated from the liquid phase of the suspension directly resulting from the hydrothermal digestion. Under suitable process conditions, these iron-containing residues contain at least some hydronium jarosite, which corresponds to the chemical formula (H3O)Fe3(SO4)2(OH)e.
[0071] It has been found that a significant proportion of the sulfate contained in such a hydronium jarosite-containing residue can be recovered in the form of iron(III) sulfate by thermal treatment followed by leaching with water. For this purpose, the residue is preferably calcined at temperatures in the range of 550 °C to 650 °C, particularly at around 600 °C, for a duration of typically one to three hours. The calcined residue is then leached with water, preferably at room temperature (20 °C), yielding a solution stream containing iron(III) sulfate. Washing has been successful up to a solid-liquid mass ratio of 1:1, followed by the application of the same quantity of wash water.
[0072] Under suitable conditions, up to approximately 75% by mass of the sulfate contained in the residue can be dissolved in this way. The resulting iron(III) sulfate stream can then be at least partially recycled back into the leaching step (hydrothermal digestion) of the process. To adjust the desired process parameters, particularly the iron(III) and sulfate concentrations, the recycled stream can be supplemented by adding fresh iron(II) sulfate ("make-up").
[0073] As described below, the iron-containing components of the residue remaining after water leaching can be reduced to magnetite:
[0074] The iron-containing solid remaining after leaching consists primarily of iron oxide phases, especially fine-crystalline hematite. This residue can be further utilized by undergoing a reduction treatment that forms magnetite (FesCM).
[0075] The reduction is preferably carried out using a gaseous reducing agent, especially hydrogen, at temperatures around 300 °C. It has been observed that, due to the very small particle size of the iron oxides present in the residue, conversion to magnetite (FesCM) is possible at significantly lower temperatures compared to conventional processes. Typically, on an industrial scale, the reduction takes place between 800 °C and 1000 °C.
[0076] The combination of the two process steps described above enables extensive material utilization of the iron-containing residues generated in the process. A portion of the iron is recycled back into the process cycle in the form of dissolved iron(II) sulfate, while the remaining portion is provided as magnetite (FesCM). This portion can be isolated from the other components by density separation or magnetic separation. In this way, almost complete utilization of the iron used can be achieved. References
[0077] Brian Jaskula (2014): US Geological Survey, Mineral Commodity Summaries. Lithium.
[0078] Brian Jaskula (2024): US Geological Survey, Mineral Commodity Summaries. Lithium.
[0079] Dunn, Jennifer B.; James, Christine; Gaines, Linda; Gallagher, Kevin; Dai, Qiang; Kelly, Jarod C. (2015): Material and Energy Flows in the Production of Cathode and Anode Materials for Lithium Ion Batteries.
[0080] Battistel, Alberto; Palagonia, Maria Sofia; Brogioli, Doriano; La Mantia, Fabio; Trocoli, Rafael (2020): Electrochemical Methods for Recovery: A Comprehensive and Critical Review. In: Advanced materials (Deerfield Beach, Fla.) 32 (23), e1905440. DOI: 10.1002 / adma.201905440;
[0081] Swain, Badusev (2017): Recovery and recycling of lithium: A review. In: Separation and Purification Technology 172, S. 388-403. DOI: 10.1016 / j.seppur.2O16.08.031.
[0082] Grosjean, Camille; Miranda, Pamela Herrera; Perrin, Marion; Poggi, Philippe (2012): Assessment of world lithium resources and consequences of their geographic distribution on the expected development oft he electric vehicle industry. In: Renewable and Sustainable Energy Reviews 16 (3), S. 1735 - 1744. DOI: 10.1016 / j.rser.2O11.11.023.
[0083] Gao, Tian.ming; Fan, Na; Chen, Wu; Dai, Tao (2023): Lithium extraction from hard rock lithium ores (spodumene, lepidolite, zinnwaldite, petalite): Technology, resources, environment and cost. In: China Geology 6 (1), S. 137-153. DOI: 10.31035 / cg2022088.
[0084] Schneider, A.; Schmidt, H.; Meven, M.; Brendler, E.; Kirchner, J.; Martin, G. et al. (2017): Lithium extraction from the mineral zinnwaldite: Part I: Effect of thermal treatment on properties and structure of zinnwaldite. In: Mineral Engineering 111, S. 55 - 67. DOI: 10.1016 / j.mineng.2017.05.006.
[0085] Qiao, Shilei; John, Timm; Loges, Anselm (2024): A Case Study from the Sn-W-Li Deposit, Zinnwald / Cinovec. In: Economic Geology 119 (4), S. 805 - 828, DOI: 10.5382 / econgeo.5074.Tadesse, Bogale; Makuei, Fidele; Albianic, Boris; Dyer, Laurence 2019): The benefication of lithium minerals from hard rock ores: A review. In: Mineral Engineering 131, S. 170-184. DOI: 10.1016 / j.mineng.2018.11.023.
[0086] Dessemond, Colin; Lajoie-Leroux, Francis; Soucy, Gervais; Laroche, Nicolas; Magnan, Jean-Frangois. (2019): Spodumene: The Lithium Market, Resources and Processes. In: Minerals 9 (6), S. 334. D0l:10.3390 / min9060334.
[0087] Li, Huan; Eksteen, Jacques; Kuang, Ge (2019): Recovery of lithium from mineral resources: State-of-the art and perspectives-Areview. In: Hydrometallurgy 189, S. 105129. DOI: 10.1016 / j.hydromet.2019.105129.
[0088] Kuang, Ge; Liu, Yu; Li, Huan, Xing, Shengzhou; Li, Fujie; Guo, Hui (2018): Extraction of lithium from β-spodumene using sodium sulfate solution. In: Hydrometallurgy 77, S. 49-56. DOI: 10.1016 / j.hydromet.2018.02.015.
Claims
Patent claims 1. A process for obtaining lithium in the form of lithium carbonate from a lithium-containing material, comprising the process steps ao) pretreatment of a concentrate of the lithium-containing material, in which the lithium-containing material is thermally treated by annealing it, a) hydrothermal digestion of the concentrate of the lithium-containing material with an iron(1 l) salt and water until the lithium is completely or almost completely mobilized and the lithium is transferred into a liquid phase of a suspension resulting from the hydrothermal digestion; b) Separation of solid components of the suspension directly resulting from the hydrothermal digestion from the liquid phase to form a digestion solution; c) Raising the pH of the digestion solution to a pH of pH 10 to pH 12 and separating the precipitates of multivalent cations formed as hydroxides from the digestion solution; and d) recovering the mobilized lithium from the digestion solution freed of multivalent cations by precipitation and separation as lithium carbonate.
2. Method according to claim 1, characterized in that the iron(1 l) salt used is selected from iron( 1 l) sulfate (Fe2(SO4)3), iron(1 l) nitrate (Fe(NO3)3), iron(1 l) chloride (FeCh) and their respective hydrates.
3. Method according to claim 1 or 2, characterized in that the lithium-containing material is a lithium-containing mineral.
4. The method of claim 3, characterized in that the lithium-containing mineral is a silicate lithium-containing mineral.
5. The method of claim 4, characterized in that the lithium-containing silicate mineral is selected as a starting material from the minerals spodumene, petalite, zinnwaldite, lepidolite, eucryptite and sugilite.
6. Method according to claim 3, characterized in that the lithium-containing mineral is selected from the minerals amblygonite, lithiophorite and jadarite.
7. Method according to one of claims 3 to 6, characterized in that in a process step preceding process step a) the lithium-containing mineral is comminuted and concentrated by means of flotation and / or density separation.
8. Method according to claim 1 or 2, characterized in that the lithium-containing material is derived from lithium-containing borate glasses or borosilicate glasses.
9. Method according to claim 1 or 2, characterized in that the lithium-containing material originates from lithium-containing waste batteries and / or waste accumulators and / or from waste generated during the manufacture of lithium-containing batteries and / or accumulators and is available in crushed and concentrated form for hydrothermal digestion.
10. The method of claim 9, characterized in that the lithium-containing material is at least partially derived from lithium-containing nickel-manganese-cobalt batteries and / or nickel-manganese-cobalt accumulators (NMC) and / or lithium iron phosphate batteries and / or lithium iron phosphate accumulators (LFP).
11. The method of any one of claims 1 to 10, characterized in that the hydrothermal digestion in process step a) is carried out with solid-liquid mass ratios of 1:2 to 1:10, preferably from 1:2 to 1:
4.
12. Method according to one of claims 1 to 11, characterized in that the hydrothermal digestion in process step a) is carried out at a digestion temperature in the range of 200 °C to 300 °C in a corrosion-tight, gas-tight sealable pressure vessel.
13. Method according to one of claims 1 to 12, characterized in that for the hydrothermal digestion in process step a) 1.25 to 4 times, preferably 2.5 times the mass of iron(III) salt, for example iron(III) sulfate hydrate (Fe2(SO4)3 ■ n H2O), is used in comparison to the mass of the concentrate of the lithium-containing material.
14. Method according to one of claims 1 to 13, characterized in that, after the separation of solid components in process step b), the digestion solution is again fed to process step a), the hydrothermal digestion of further lithium-containing material.
15. A method according to any one of claims 1 to 14, characterized in that the iron(III) salt is iron(III) sulfate (Fe2(SO4)3) or a hydrate of iron(III) sulfate and that iron(III) sulfate is recovered in dissolved form from the solid components containing iron and sulfate ions separated after process step b) by thermal treatment and subsequent leaching with water, wherein the recovered iron(III) sulfate in dissolved form is returned to process step a), the hydrothermal digestion.
16. Method according to one of claims 1 to 15, characterized in that in a process step co) preceding process step c) a separation of iron(III) ions from the digestion solution is carried out by extraction of the digestion solution with di(2-ethylhexyl)phosphoric acid (DEHPA) in a weakly polar solvent, for example kerosene.
17. Method according to one of claims 1 to 16, characterized in that in a process step co) preceding process step c) a separation of iron ions and aluminium ions from the digestion solution is carried out by means of nanofiltration.
18. Method according to one of claims 1 to 17, characterized in that, after the recovery of lithium carbonate from the digestion solution freed from multivalent cations in process step d), the remaining digestion solution is returned to process step a) and / or process step c).