Method for agglomerating solids to form briquettes and corresponding briquettes
The method of heat-treating a mixture of fine ores and additives at specific temperatures and pressures enhances briquette strength and gas permeability, addressing suboptimal characteristics in existing briquettes for direct reduction plants, resulting in efficient and sustainable briquette production.
Patent Information
- Application Number
- PCT/EP2026/062323
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-04-29
- Publication Date
- 2026-11-12
AI Technical Summary
Existing briquettes for direct reduction plants exhibit suboptimal characteristics such as strength, porosity, and pore size, which affect their performance in withstanding pressure and facilitating gas diffusion, leading to inefficient reduction processes.
A method involving the heat treatment of a mixture of fine ores, sinter feed, and additives at specific temperatures, followed by hot briquetting, to achieve a balanced ratio of strength, porosity, and pore size, utilizing binders and carbon carriers to enhance mechanical strength and gas permeability.
The method produces briquettes with improved mechanical strength and optimized gas permeability, ensuring efficient reduction processes and reduced abrasion, while minimizing environmental impact through sustainable additives.
Smart Images

Figure IMGF000013_0001_TABLE
Abstract
Description
[0001] ThyssenKrupp Steel Europe AG 257024P10WO April 29, 2026 1 / 13
[0002] Methods for agglomerating solids into briquettes and corresponding briquettes
[0003] The invention relates to a method for agglomerating a mixture of solids into briquettes for use in direct reduction plants and to corresponding briquettes.
[0004] The agglomeration of iron ore into briquettes is state of the art. US 3366 717 A and US 3 116 996 A each describe a method and a device for hot briquetting fine ores.
[0005] Briquettes for use in direct reduction plants are known, but after heat treatment they exhibit characteristic properties such as strength, porosity, and pore size, which significantly determine their quality and are not optimal for use in direct reduction plants. Strength affects the briquettes' ability to withstand the pressure of the feed column in a direct reduction plant reactor and minimizes abrasion within the reactor shaft. Furthermore, pore size and distribution influence the diffusion rate of reducing gas molecules within the briquette, which should ideally be adjusted to allow for rapid reduction. This is preferably achieved by ensuring that the pore size is as close as possible to the mean free path of the reducing gas molecules, thus maximizing diffusion rates.Since the relationship between the effective diffusion coefficient and the Knudsen diffusion coefficient is given by the quotient of porosity and tortuosity, the porosity should be high and the tortuosity low. However, the porosity should not exceed a critical threshold that could negatively affect strength, nor should it be too low, which could impair the diffusion and thus the reduction rate. Tortuosity, in turn, is strongly dependent on the microstructure—for example, if the pores are highly convoluted, it increases rapidly. Therefore, to maintain a high diffusion rate, the tortuosity should be as close to 1 as possible, ideally between 1.5 and 2.
[0006] Besides diffusion, the chemical reaction of the reducing gas with the iron oxide inside the agglomerate also has a significant influence on the rate of reduction. For this reason, a mixture is sought before hot briquetting that also positively affects the rate of the chemical reaction. It is assumed that the vacancies inside the iron oxide crystals influence the rate of the chemical reaction. Re-ThyssenKrupp Steel Europe AG 257024P10WO April 29, 2026 2 / 13
[0007] The action of the reducing gas with the iron oxides is supported. Possible measures for creating vacancies in the iron oxide crystals are based, among other things, on the principle of removing a certain number of oxygen atoms from the mixture above a specific temperature by adding, for example, carbon.
[0008] The object of the present invention is to provide a method for agglomerating a mixture of solids into briquettes and briquettes which can ensure a balanced ratio of the aforementioned characteristic properties.
[0009] This problem is solved by a method having the features of claim 1 and by a briquette having the features of claim 7. Further embodiments are described in the dependent claims.
[0010] A first teaching of the invention relates to a process for agglomerating a mixture of solids into briquettes for use in direct reduction plants, wherein the mixture is heat-treated at a temperature between 500 and 1000 °C and subsequently hot-agglomerated into briquettes in a hot briquetting plant. It is essential that the mixture contains or consists of fine ores with a mean particle size of 200 pm, sinter feed with a particle size of up to 3.0 mm, and additives.
[0011] The composition of the solid mixture significantly influences the characteristic properties such as strength, porosity, and pore size of a hot-briquetted briquette. The solids consist of a mixture of fine ores with an average grain size of 200 pm, sinter feed with a grain size of up to 3.0 mm, and additives.
[0012] The strength of a hot-briquetted briquette is primarily determined by the composition of the mixture used, the pressure, the atmosphere, and the temperature. In addition to the grain size, an optimal mixture of solids, optionally moisture content, and process temperature control can contribute to increasing mechanical strength, enabling the briquette to withstand higher loads and maintain its structural integrity. This is particularly important for use in a direct reduction plant, where the briquette is subjected to high pressure or impact loads. The strength, more precisely the cold compressive strength, of briquettes can be tested in accordance with ISO 4700:2015-08, the determination of the compressive strength of iron ore pellets for blast furnace (HO) and direct reduction (DR) processes. ThyssenKrupp Steel Europe AG 257024P10WO April 29, 2026 3 / 13
[0013] The porosity of a briquette, defined as the ratio of pore volume to total volume, is also significantly influenced by the composition of the mixture. A targeted selection and combination of solids in the mixture can control the porosity so that the briquette exhibits the desired properties in terms of density and permeability. This is crucial for achieving a specific gas permeability for briquette reduction. Common methods for determining briquette porosity include mercury porosimetry, which measures the penetration of mercury under pressure; gas adsorption methods, such as the BET method, which measures the specific surface area and can provide information about the surface porosity; and alternatively, micro-computed tomography (micro-CT or p-CT) for the 3D characterization of the internal structure, including pore size and distribution.
[0014] The pore size, which describes the dimensions of the voids within the briquette, is determined by the particle size and the distribution of the solids within the briquette. A homogeneous particle size distribution can lead to a uniform pore size, which improves the structural stability and functional properties of the briquette. This is particularly relevant for controlled gas permeability during reduction. The mean pore size in a briquette refers to the average diameter of the pores within the briquette. Pores are small voids or spaces that permeate the briquette's structure. The pore size of briquettes can be determined using CT scanning. The tortuosity, i.e., how "winding" the effective diffusion paths are in the porous medium, can preferably be derived using numerical simulation from a digital sample structure, for example, from CT data, and a virtual diffusion simulation.The basic principle of a CT scan is that X-rays illuminate a sample from many angles. A 3D volume image is reconstructed from the absorption data, particularly on a voxel-based basis. Different density regions (solid vs. pore) create contrasts, resulting in a 3D volume dataset in which each voxel has a grayscale intensity.
[0015] To produce fine ores with a mean grain size of approximately 200 pm, several ore processing steps are required:
[0016] Crushing: Ores are first reduced to the desired grain size by crushing and grinding. This can be done using various mills, such as ball mills or hammer mills. ThyssenKrupp Steel Europe AG 257024P10WO April 29, 2026 4 / 13
[0017] - Sieving: After grinding, the ores are sieved to achieve the desired grain size. Fine ores are separated using special sieving machines.
[0018] - Classification: Classification is carried out by hydrocyclones or other classification machines that further separate the fine particles and ensure an average particle size of approximately 200 pm.
[0019] Further steps are optional:
[0020] - Flotation: If necessary, the ores can be further processed by flotation to remove unwanted minerals and improve the quality of the fine ores.
[0021] - Magnetic separation: For ferrous ores, magnetic separation can be used to separate the ores from the gangue and increase purity.
[0022] The fine ores can have an iron oxide content of at least 55 or 57 wt.%, in particular at least 59 or 61 wt.%, preferably at least 63 or 65 wt.%. Depending on the ore type, the fine ores can have an iron oxide content of up to 85 wt.%, for example, up to 75 wt.%.
[0023] These steps are part of a complex process that can vary depending on the type of ore and the specific requirements.
[0024] A mean grain fraction refers to the total number of particles of a specific grain size within a material. The mean grain fraction is therefore a specific grain size class used for the characterization and classification of fine ores.
[0025] Sinter feed is provided with a grain size distribution of up to 3.0 mm. This includes (grain) sizes starting from 1 pm, particularly from 20 pm, preferably from 50 pm up to 3.0 mm, particularly up to 2.50 mm, preferably up to 2.0 mm. Sinter feed thus refers to ores with a size distribution of up to 3.0 mm. The sinter feed can also have an iron oxide content of at least 55 or 57 wt.%, particularly at least 59 or 61 wt.%, preferably at least 63 or 65 wt.%. Depending on the ore type, the sinter feed can have an iron oxide content of up to 85 wt.%, for example, up to 75 wt.%. Iron-containing dusts in the aforementioned grain fraction can also be used as sinter feedstock, particularly by being added as supplementary feedstock. ThyssenKrupp Steel Europe AG 257024P10WO April 29, 2026 5 / 13
[0026] Additives are preferably provided in the form of a binder. Binders can be inorganic, such as containing or consisting of bentonite and / or sodium silicate. Bentonite is understood to be a material that is a mixture of various clay minerals and contains smectitic phyllosilicates, in particular montmorillonite, as its main component. The smectitic phyllosilicates, in particular montmorillonite, are present at a proportion of at least 60% by weight, in particular at least 65% by weight, and preferably at least 70% by weight. Bentonite can be used as a naturally occurring rock or as a modification of a naturally occurring rock obtained by the addition of additives or by carrying out process steps. Sodium silicate, also known as water glass, is understood to be a chemical compound of sodium oxide / sodium silicate and silicon dioxide.The use of sodium silicate as a binder is primarily due to its thermal stability under direct reduction conditions. Alternatively, organic binders are conceivable, as their polymeric or fibrous structure can promote bonding.
[0027] Additives are preferably provided in addition to binders in the form of carbon carriers. These can be of fossil origin, such as bituminous coal, anthracite coal, or coking coal produced from them, or sustainable alternatives, such as biochar from biomass. Alternatively, and preferably, carbon-containing dusts that are available as smelting residues can also be used. By adding carbon carriers, a partial pre-reduction of the solids in the mixture can be achieved before agglomeration due to the high temperatures, so that vacancies can form in the iron oxide crystals (Z-grains). These vacancies in the iron oxide can then lead to a preferred chemical reaction with a reducing gas in the briquette.
[0028] Additives can also be provided, preferably in addition to binders and carbon carriers, in the form of aggregates. These include the aggregates commonly used in metallurgy, which are rich in Al₂O₃, SiO₂, MgO, CaO, and mixtures thereof. CaO- or CaCO₃-rich fractions are particularly preferred in this context, as they can positively influence the so-called swelling behavior of iron ores. Alternatively, slags from blast furnaces, especially lime-rich granulated blast furnace slag, or converter and EAF slags can be used to adjust the basicity within a favorable range. ThyssenKrupp Steel Europe AG 257024P10WO April 29, 2026 6 / 13
[0029] The additives can also be provided with a particle size fraction of up to 3.0 mm. This therefore includes (particle) sizes starting from 1 pm, in particular from 5 pm, preferably from 10 pm, preferably from 20 pm, in particular up to 2.50 mm, preferably up to 2.0 mm.
[0030] According to one embodiment, the mixture can contain or consist of 0.30 to 15.0 wt.% additives, the remainder being fine ores and sinter feed. To improve the properties of the briquette, the additives can be present in the mixture at least 0.50 wt.%, preferably at least 0.80 wt.%, more preferably at least 1.0 wt.%, particularly preferably at least 1.20 wt.%, and further preferably at least 1.50 wt.%. To eliminate any potential disadvantages with regard to the aforementioned characteristic properties, the additives can be present in the mixture at a maximum of 13.0 wt.%, preferably at most 11.0 wt.%, more preferably at most 10.0 wt.%, particularly preferably at most 8.0 wt.%, and further preferably at most 6.0 wt.%.
[0031] According to the invention, the additives comprise binders and carbon carriers. The total amount of these in the mixture can be within the aforementioned limits.
[0032] According to one embodiment, the heat treatment of the mixture can be carried out in an indirectly heated retort. An indirectly heated retort is a special furnace or vessel used for controlled heating processes. Unlike directly heated systems, where the flame comes into direct contact with the solids in the mixture being heated, in indirectly heated retorts the flame is located in a sealed combustion chamber. This allows the heat to be transferred through the walls of the combustion chamber to the solids in the mixture without combustion products contaminating the mixture. Indirectly heated retorts allow for precise temperature control and a clean and / or defined atmosphere. As an alternative to the retort, which is usually stationary, a rotating furnace, such as a rotary kiln, which can be indirectly heated, can also be used.Furthermore, the use of indirectly heated roller hearth furnaces would also be possible, allowing the mixture to be processed, for example, in containers and thus heat-treated. Alternatively, the indirectly heated furnace can be designed as a coke oven. A coke oven, or a coke oven battery, is known as a plant for producing coke from hard coal. Due to the required phase-out of fossil fuels in steel production, coke oven batteries, among others, are being gradually phased out or shut down, so that they are being repurposed and thus used for a new application in the heat treatment of solids. (ThyssenKrupp Steel Europe AG 257024P10WO April 29, 2026 7 / 13)
[0033] The process can be carried out using hot briquetting. The process comprises several steps:
[0034] - Filling: The coke oven battery consists of several ovens arranged side by side. These ovens are filled with a mixture containing solids.
[0035] - Heat treatment: The furnaces are heated to the aforementioned high temperatures. This is usually done by indirect heating, where the heat is transferred to the mixture through the furnace walls.
[0036] - Discharge: After heat treatment, the mixture is removed from the furnace or pressed out. The hot mixture is then fed into a hot briquetting plant.
[0037] According to an alternative design, the heat treatment of the mixture can also be carried out in a directly heated furnace. Directly heated furnaces for heat treatment of the mixture can be, for example, rotary kilns or continuous furnaces.
[0038] The mixture can be heat-treated at a temperature, particularly between 550 and 950 °C. The temperature can preferably be at least 600 °C, more preferably at least 650 °C. The temperature can preferably be at most 900 °C, more preferably at most 850 °C.
[0039] The specified temperature refers to the temperature of the solids or the mixture, which can be measured, for example, on the surface of the mixture using suitable measuring instruments. The specified temperature can be understood as an average value with respect to a measured area, whereby the measured area may vary depending on the measuring instrument method known and used by those skilled in the art. Preferably, the temperature is measured non-contact, for example, using a pyrometer, laser scanner, thermal imaging camera, etc. All solids, i.e., the mixture, should be brought completely to these temperatures, although the temperature within a mixture cannot be directly determined during normal operation. The temperature in the heat treatment furnace, or the temperature of the atmosphere in the heat treatment furnace, may well be higher. Alternatively, thermocouples can also be used.
[0040] The heat treatment duration can range from 2 to 400 minutes. Depending on the temperature and the throughput of the mixture, the heat treatment duration can be shorter or longer. The duration can be at least 5 minutes, preferably ThyssenKrupp Steel Europe AG 257024P10WO 29 April 2026 8 / 13
[0041] The heat treatment time should be at least 10 minutes, preferably at least 30 minutes, and in particular at most 300 minutes, preferably at most 230 minutes, and preferably at most 200 minutes. Longer heat treatment times are conceivable, but are not desirable from an economic point of view.
[0042] The atmosphere during heat treatment depends particularly on whether the heat treatment is carried out in an indirectly, preferably electrically, heated furnace or in a directly heated furnace. In an indirectly, preferably electrically heated furnace, a reducing atmosphere is established if the mixture contains additives in the form of, for example, carbon, so that the carbon also reacts with the iron oxide. If the creation of vacancies in the iron oxide is omitted, i.e., a certain pre-reduction is omitted, the process can also be carried out in an oxidizing atmosphere.In a directly heated furnace, if the mixture contains additives in the form of, for example, carbon, a reducing atmosphere is set such that the air ratio is set to less than 1.15, in particular less than 1.0, in order to generate CO formation during, for example, hydrocarbon combustion or pure hydrogen combustion.
[0043] The hot mixture can preferably be transferred directly to a hot briquetting plant without intermediate comminution, where it is hot-pressed into briquettes. The principle of hot briquetting is known, whereby the mixture is fed into a briquetting press. This can be done, for example, via a hopper or a screw conveyor. If necessary, the mixture can be pre-compacted to ensure, for example, a uniform distribution and density. The optionally pre-compacted mixture is preferably fed between a briquetting press comprising two rotating rollers. These rollers are specially shaped and have recesses that correspond to the outer contour of the desired briquette shape. The rollers exert a high (specific) pressure on the mixture, particularly in their gap, causing the solids within the recesses to be hot-compressed into solid briquettes.The shape and size of the briquettes depend primarily on the rollers and / or the settings of the briquetting press. The finished briquettes are discharged from the briquetting press and can then either be cooled and, for example, stored in a storage facility, or used directly in a direct reduction plant.
[0044] The hot briquetting plant, or briquetting press, can be set to a specific pressing pressure on the hot mixture between 20 kN / cm² and 200 kN / cm². ThyssenKrupp Steel Europe AG 257024P10WO April 29, 2026 9 / 13
[0045] The compression pressure can be set to at least 30 kN / cm², preferably at least 40 kN / cm², and preferably a maximum of 150 kN / cm², preferably a maximum of 120 kN / cm². The high specific compression pressure allows for the optimization of the mixture's physical properties, resulting in improved briquette quality. This enables a dense and stable briquette structure, ensuring greater durability and easier handling. Furthermore, the high specific compression pressure can impart greater strength and resistance to mechanical stress to the briquettes. Additionally, the high specific compression pressure can contribute to a reduction in pore size, thereby increasing the gasification efficiency of the briquettes.
[0046] A direct reduction plant is an industrial facility for producing sponge iron from iron ore without the use of a blast furnace. The process is called direct reduction and typically proceeds as follows: - Charging: Iron ore pellets are fed into the top of a plant, usually equipped with a shaft furnace. - Reduction: A reducing gas, currently consisting of carbon monoxide (CO) and hydrogen (H2), flows from bottom to top through the shaft furnace. This gas reacts with the iron ore, removing the oxygen and producing sponge iron. The process takes place at approximately 900 to 1100 °C and under pressure. - Sponge iron: The end product is a porous material known as sponge iron or DRI (direct reduced iron). After its production in the direct reduction plant, the DRI is further processed, including: - Steelmaking: DRI is commonly used in electric arc furnaces (EAF) to produce steel.It serves as a high-quality raw material that improves the quality of the final product; - Foundries: DRI can also be used in foundries to produce various metal products; - Blast furnace process: in some cases, DRI can be used as a supplement to the blast furnace process to increase efficiency and reduce coke consumption. These applications make DRI an important component of modern metallurgy and contribute to the reduction of CO2 emissions. A major advantage of direct reduction is the possibility of using (green) hydrogen as a reducing agent, which should significantly reduce CO2 emissions in the future and thus also replace blast furnaces.
[0047] MIDREX and HYL are two leading technologies for the direct reduction of iron ore. MIDREX uses carbon monoxide (CO) and hydrogen (H2) as reducing gas, which is derived from natural gas. The natural gas is split in a reformer to produce the reducing gas. MIDREX produces various forms of DRI, including cold DRI (CDRI), hot DRI (HDRI), and hot briquetted iron (HBI). HYL also uses CO and H2, but the earth gas is extracted from natural gas. ThyssenKrupp Steel Europe AG 257024P10WO April 29, 2026 10 / 13
[0048] Gas is split in a steam reformer. HYL uses a combination of in-situ reforming and partial oxidation to produce the reducing gas. HYL primarily produces HDRI and HBI. Both technologies are efficient and contribute to reducing CO2 emissions in steel production.
[0049] An Electric Smelting Furnace (ESF) is an electric furnace that will be increasingly used in steel production in the future. It utilizes an open slag bath to process deep refractory iron (DRI) at high temperatures. The ESF is loaded with DRI and additives. These additives are slag formers and / or carbon-containing admixtures. Electrical energy is used to heat the slag bath to high temperatures. The DRI is melted and further reduced in the slag bath. The molten iron is regularly drained and further processed. The slag produced is also regularly drained and can be further processed. This process optimizes energy efficiency and reduces the need for external cooling.
[0050] An electric arc furnace (EAF) operates by generating an electric arc between (graphite) electrodes and the charge material, usually scrap steel. The furnace is loaded with raw materials such as scrap steel, (sintered) iron ore, pig iron, and sometimes DRI (dry refractory iron). The electrodes generate an electric arc that reaches temperatures of up to 3500 °C, at which point the heat melts the raw materials. During the melting process, a slag layer forms, which binds unwanted components and protects the steel bath. The molten steel is drained into a steel ladle, while the slag is removed separately.
[0051] A second teaching of the invention relates to a briquette, in particular produced according to the first teaching of the invention, comprising iron oxide with a mean pore size of less than 10.0 pm, determined by CT scan, and a porosity between 10.0 and 40.0%, determined by mercury porosimetry.
[0052] The smaller the pore size, the better, because if the average pore size is less than 10.0 pm, particularly less than 9.0 pm, preferably less than 8.0 pm, this is especially advantageous for the diffusion rate of gas molecules inside the briquette. The average pore size is particularly > 0.1 pm. This is because, in this case, the pore size is on the order of the mean free path of gas molecules such as hydrogen and / or carbon monoxide in a reducing gas flowing through the pores. ThyssenKrupp Steel Europe AG 257024P10WO April 29, 2026 11 / 13
[0053] and then a “Knudsen diffusion” occurs, which is significantly faster than molecular diffusion, which takes place in large pores as in the prior art, especially when the mean pore size is greater than 10.0 pm.
[0054] In conjunction with a smaller average pore size compared to the prior art, a porosity between 10.0 and 40.0% provides an optimal balance between high strength and gas permeability, which can be advantageously achieved in a briquette using the first teaching of the invention. The lower the porosity, the lower the effective diffusion coefficient and thus the reduction rate. Conversely, excessively high porosity has a detrimental effect on the strength of the briquettes. The porosity can be, in particular, at least 11.0 or 12.0%, preferably at least 13.0 or 14.0%, more preferably at least 15.0 or 16.0%, and most preferably at least 17.0 or 18.0%. The porosity can be, in particular, a maximum of 38.0 or 36.0%, more preferably a maximum of 34.0 or 32.0%, and more preferably a maximum of 30.0 or 28.0%.
[0055] According to one design, a briquette can have a volume between 5 and 30 cm³. 3 exhibit. In particular, the volume can be at least 7, 8, 9 cm³.3 , preferably at least 10, 11, 12 cm 3 preferably at least 13, 14, 15 cm 3 The volume can be a maximum of 29, 28, or 27 cm³. 3 preferably a maximum of 26, 25, 24 cm 3 preferably a maximum of 23, 22, 21 cm 3 be.
[0056] According to one embodiment, a briquette can exhibit a (cold compressive) strength of at least 80 to 700 kg / briquette, determined in accordance with ISO 4700:2015-08. The high strength of hot-briquetted briquettes, in addition to providing a long shelf life and stability, which facilitates storage and transport, also allows them to withstand the pressure of the briquette column prevailing in a direct reduction plant or reactor, and minimizes abrasion in the reactor. The (cold compressive) strength, or mechanical strength, of the briquettes can be at least 90, 100, or 110 kg / briquette, preferably at least 120, 130, or 140 kg / briquette. The (cold pressure) strength or mechanical strength of the briquettes can in particular be a maximum of 650, 600, 550 kg / briquette, preferably a maximum of 500, 450, 400 kg / briquette, preferably a maximum of 370, 340, 300 kg / briquette.
[0057] If the solids or the mixture contain reducing agents such as carbon carriers, the solids may partially pre-reduce during heat treatment, resulting in voids in the briquette after hot briquetting. ThyssenKrupp Steel Europe AG 257024P10WO April 29, 2026 12 / 13
[0058] Vacancies can be detected, for example, using X-ray photoelectron spectroscopy (XPS), which allows shifts in the 0 ls and Fe 2p signals to be identified. The Fe 2p region is typically in the range of 705–730 eV. Characteristic of Fe 2+ is the position of approximately
[0059] 709.5 eV and from Fe 3+ the position of approximately 711.0 eV. If there is an oxygen deficiency (V_0), the peak of Fe 2+ at the position of approximately 709.5 eV. The 0 ls region is typically in the range of 528–533 eV. The position of approximately [missing information] is characteristic for oxygen in the lattice (Fe-O).
[0060] 529.6 eV and for an oxygen vacancy, thus a defect in the lattice with OH”, adsorbate the position of approximately 531.0 - 531.5 eV. Oxygen deficiency V_O and thus the vacancies increase with increasing defect peak at approximately 531 eV. In short, the Fe increases 2+ A peak at approximately 709.5 eV results in more reduced iron centers due to oxygen deficiency. Less Fe 3+ This is an indication of V_O. If the 0 ls peak rises to approximately 531 eV, this is a direct signature of oxygen vacancies.
[0061] Heat treatment was carried out in a chamber furnace with free-radiating heating elements on a laboratory scale. Different mixture compositions were investigated, as follows:
[0062] a) 1 wt.% bentonite with a grain fraction up to 0.2 mm, remainder sinter feed with a grain fraction up to 6.3 mm;
[0063] b) 0.5 wt.% bentonite with a grain fraction up to 0.2 mm, remainder sinter feed with a grain fraction up to 3 mm;
[0064] c) 2 wt.% bentonite with a grain fraction up to 0.2 mm, remainder fine ores with a mean grain fraction of about 200 pm;
[0065] d) 1 wt.% bentonite with a grain fraction up to 0.2 mm, remainder sinter feed with a grain fraction up to 3 mm;
[0066] e) 1 wt.% bentonite with a grain fraction up to 0.2 mm and anthracite coal 1 wt.% with a grain fraction up to 0.2 mm, , remainder fine ores with a mean grain fraction of about 200 pm and sinter feed with a grain fraction up to 3 mm;
[0067] f) 1.5 wt.% bentonite with a grain fraction up to 0.2 mm and 1 wt.% anthracite coal with a grain fraction up to 0.2 mm, remainder fine ores with a mean grain fraction of about 200 pm and sinter feed with a grain fraction up to 3 mm.
[0068] All mixtures a) to f) were heat-treated in an air atmosphere and brought to a temperature of 950 °C, measured using a thermocouple. The heat treatment duration was 60 minutes in each case. Following heat treatment, mixtures a) to f) were transferred to a laboratory-scale briquetting press, a specially designed [ThyssenKrupp Steel Europe AG 257024P10WO 29 April 2026 13 / 13]
[0069] The device involved a structured roller press in which the hot mixture was pressed into the gap between the two synchronously counter-rotating rollers, and the briquettes were formed through pockets in the roller surfaces at a specific pressing pressure of 50 kN / cm² with a briquette size of 10 cm². 3The briquettes were hot-formed. The resulting briquettes were subjected to tests to determine their (cold pressure) strength according to ISO 4700:2015-08, their porosity by mercury porosimetry, and their mean pore size by CT scan. The mean value from 10 briquettes of each of the corresponding mixtures a) to f) is shown in Table 1.
[0070] Briquettes made from mixture (cold printing) porosity average pore size inventive strength [%] [pm] ding [kg / briquette]
[0071] a) 120 27 34 no b) 118 25 17 no c) 143 23 12 no d) 127 24 20 no e) 131 25 8 yes f) 142 24 5 yes
[0072]
[0073] Table 1
[0074] The briquettes produced from mixture f) showed an increased concentration of oxygen vacancies, as confirmed by XPS. The proportion of the defect-associated 0 ls peak (-531.1 eV) was 10% higher in briquette e) and f) respectively compared to, for example, briquette d).
Claims
ThyssenKrupp Steel Europe AG 257024P10WO April 29, 2026 1 / 2 Patent claims 1. A process for agglomerating a mixture of solids into briquettes for use in direct reduction plants, wherein the mixture is heat-treated at a temperature between 500 and 1000 °C and subsequently hot-agglomerated into briquettes in a hot briquetting plant, characterized in that the mixture consists of fine ores with a mean particle size of 200 pm, wherein the fine ores have an iron oxide content of at least 55 and at most 85 wt.%, sinter feed with a particle size of up to 3.0 mm, wherein the sinter feed has an iron oxide content of at least 55 and at most 85 wt.%, and 0.30 to 15.0 wt.% additives, wherein the additives comprise binders and carbon carriers.
2. The method of claim 1, wherein the heat treatment of the mixture is carried out in an indirectly heated retort or an indirectly heated rotary kiln.
3. Method according to claim 1, wherein the heat treatment of the mixture is carried out in an indirectly heated coke oven or a directly and / or indirectly heated rotary kiln.
4. Method according to one of the preceding claims, wherein the mixture is heat-treated at a temperature between 650 and 1000 °C.
5. Method according to one of the preceding claims, wherein the heat treatment lasts between 2 and 400 minutes.
6. Method according to one of the preceding claims, wherein the hot briquetting plant is set with a specific pressing pressure on the hot mixture between 20 and 200 kN / cm.
7. Briquette manufactured according to any of the preceding claims, comprising iron oxide with a mean pore size of less than 10.0 pm, determined by CT scan, and a porosity between 10.0 and 40.0%, determined by mercury porosimetry.
8. Briquette according to claim 7, wherein the mean pore size is less than 9.0 pm. ThyssenKrupp Steel Europe AG 257024P10WO April 29, 2026 2 / 2 9. Briquette according to claim 7 or 8, wherein the porosity is between 18.0 and 30.0%.
10. Briquette according to any one of claims 7 to 9, wherein the briquette has a strength of at least 80 kg / briquette, determined in accordance with ISO 4700:2015-08.
11. Briquette according to any one of claims 7 to 10, wherein the briquette has a strength of at least 120 kg / briquette, determined in accordance with ISO 4700:2015.
12. Briquette according to one of claims 7 to 11, wherein the briquette has a volume between 5 and 30 cm³ 3 exhibits.