Glass combiner for head-up display
The use of chemically tempered thin glass and injection molding to achieve bi-axial curvature addresses manufacturing challenges, resulting in a durable and optically pristine HUD combiner with improved optical performance.
Patent Information
- Application Number
- PCT/EP2026/063128
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2026-05-06
- Publication Date
- 2026-11-12
AI Technical Summary
Manufacturing a glass HUD combiner with a precise, doubly-curved surface for improved optical performance is challenging due to issues like surface defects from hot forming, optical aberrations from coating application, and adhesive-related problems in conventional methods, which affect image quality and durability.
A method involving chemically tempered thin glass, cold bending to achieve bi-axial curvature, and injection molding to permanently fix the shape, ensuring pristine optical quality and durable bonding without adhesives.
The solution provides a high-quality, doubly-curved glass combiner with superior optical properties, suitable for mass production, by maintaining the glass's pristine quality and allowing uniform coating application, while ensuring robustness and durability.
Smart Images

Figure EP2026063128_12112026_PF_FP_ABST
Abstract
Description
Glass combiner for head-up displayFIELD OF THE INVENTION
[0001] The present invention relates to the field of head-up display (HUD) devices used in vehicles. More specifically, it relates to a combiner for an HUD device comprising a glass part integrated to the dashboard of the vehicle, providing increased driver visual comfort.BACKGROUND OF THE INVENTION
[0002] There exist two types of HUD devices in vehicles. A vehicle includes cars, vans, lorries, motorbikes, buses, trams, trains, airplanes, helicopters, drones, boats and the like.
[0003] The first type of HUD device uses the windshield of the vehicle as the surface onto which a projection system projects a virtual image, which is visible to the driver. Such projection system comprises an image-generating unit (known in the art as a projector) and an image-forming mirror (also known as a beam splitter) which can be spherical, aspherical, or freely formed. This type of HUD device is costly. Such HUD device is described in CN104267498.
[0004] The second type uses a so-called combiner onto which the image is projected. Such combiner is separated from the windshield. For example, it can be a transparent plate made of glass or plastic or a suitably designed prism. A combiner is typically located above the instrument panel, also called dashboard, generally close to the windshield. It can sometimes be retracted into the dashboard or folded down parallel with the top surface of the dashboard. The combiner reflects the image generated by the projector in the direction of the driver. Such HUD device is described in US20170059872.
[0005] Particularly for combiners that stand independently from the windshield, there is a growing demand for improved optical performance to enhance the driver's experience. A key objective is to create a virtual image that appears larger and more distant than the physical display, moving the perceived image closer to the driver's far-point focus and reducing the need for eye accommodation.
[0006] This objective can be achieved by using a combiner with a specific optical prescription. Specifically, a doubly-curved or bi-axially curved surface (i.e., having distinct radii of curvature in both the horizontal and vertical axes) is required. The horizontal curvature is necessary to aesthetically and functionally align the combiner with the curved dashboard and windshield of the vehicle. The vertical curvature, in turn, provides the desired optical magnification of the projected image.
[0007] However, the manufacturing of a glass combiner with such a precise, doubly-curved surface, while maintaining pristine optical quality, presents a significant and unsolved technical challenge. Indeed, hot forming of glass is a conventional method for creating curved glass. It involves heating a glass sheet to its transition temperature (e.g., 550-800°C) and pressing it into a shaped mold. However, the high temperatures and mechanical pressure from the mold inevitably introduce surface defects, such as press marks, waviness, and other micro-distortions. These defects are magnified by the reflective surface of the combiner, leading to a distorted and low-quality virtual image. Furthermore, any functional coatings (e.g., reflective, anti-glare, or p-polarized coatings) must be applied after the bending process, as they cannot withstand the high temperatures. Applying a uniform, high-quality coating, particularly via sputtering, onto a complex, doubly-curved surface is extremely difficult and often results in non-uniform thickness, leading to optical aberrations and visual artifacts.
[0008] An alternative approach involves applying a reflective plastic foil onto a pre-formed, rigid, curved substrate. While this avoids the high temperatures of hot forming, it introduces different problems. When a flat plastic foil is stretched over a doubly-curved surface, it is prone to developing wrinkles, creases, and local deviations where the foil does not perfectly conform to the substrate's shape. These imperfections again result in significant degradation of the reflected image quality.
[0009] Cold bending, or the bending of glass at ambient temperature, is known for producing optically perfect surfaces as it involves no heat or high-pressure molding. However, this process is only feasible for creating a bend in a single direction (i.e., a simple cylindrical or conical shape). Attempting to force a glass sheet into a doubly-curved (e.g., spherical or aspherical) shape via conventional cold bending was considered to induce excessive and complex stress patterns that would either lead to immediate fracture or make it impossible to maintain the shape reliably.
[0010] Further, the glass sheet of the combiner needs to be fixed to its carrier, usually through an adhesive. Using such adhesives may lead to ageing issues, as the adhesive may lose its adhesive power over time, to creation of bubbles which render the adhesion less efficient and to an inhomogeneous covering of the glass sheet, as adhesives are usually applied only partially. The positioning itself of such adhesives may also be tricky.
[0011] Therefore, there is a need for a method to manufacture a glass HUD combiner that features a precise, bi-axially curved reflective surface for improved optical performance, while simultaneously achieving the pristine, defect-free surface quality of unformed glass and allowing for the uniform preapplication of advanced optical coatings. The solution must be robust, repeatable, and suitable for mass production in the automotive industry that also comprises a robust and durable method forfixing the glass sheet to its carrier is required.SUMMARY OF THE INVENTION
[0012] The present invention concerns a combiner for an head-up-display device of a vehicle. The combiner comprises a carrier adapted to fix the combiner to the vehicle. The combiner further comprises a glass sheet. The glass sheet has an internal face facing the carrier and an external face opposite to the internal face. The glass sheet has a thickness of 1 mm. The glass sheet is chemically tempered. The glass sheet has a horizontal curvature radius of at least 500 mm and a vertical curvature radius of at least 1000 mm. The external face of the glass sheet is coated with a reflective coating reflecting at least 10 % of incoming visible light. The entire internal face of the glass sheet is fixed to the carrier with an injected material.
[0013] The present invention also concerns a method to produce such combiner.BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Fig.la illustrates an embodiment of a combiner for an head-up display device of a vehicle according to the present invention.
[0015] Fig.lb illustrates another embodiment of a combiner for an head-up display device of a vehicle according to the present invention.
[0016] Fig.2 illustrates a slice view of the embodiment of Fig.lb.DETAILED DESCRIPTION OF ILLUSTRATIVE EMBODIMENTS
[0017] The invention will now be described further, by way of examples, with reference to the accompanying drawings, wherein like reference numerals refer to like elements in the various figures. These examples are provided by way of illustration and not of limitation. The drawings are a schematic representation and not true to scale. The drawings do not restrict the invention in any way. More advantages will be explained with examples.
[0018] In this document to a specific embodiment and include various changes, equivalents, and / or replacements of a corresponding embodiment. The same reference numbers are used throughout the drawings to refer to the same or like parts.
[0019] As used herein, spatial or directional terms, such as "inner", "outer", "above", "below", "top", "bottom", and the like, relate to the invention as it is shown in the drawing figures. However, it is tobe understood that the invention can assume various alternative orientations and, accordingly, such terms are not to be considered as limiting. Further, all numbers expressing dimensions, physical characteristics, processing parameters, quantities of ingredients, reaction conditions, and the like, used in the specification and claims are to be understood as being modified in all instances by the term "about". Accordingly, unless indicated to the contrary, the numerical values set forth in the following specification and claims are approximations that can vary depending upon the desired properties sought to be obtained by the present invention. In the following description, unless otherwise specified, expression "substantially" mean to within 10%, preferably to within 5%.
[0020] Moreover, all ranges disclosed herein are to be understood to be inclusive of the beginning and ending range values and to encompass any and all subranges subsumed therein. For example, a stated range of "1 to 10" should be considered to include any and all subranges between (and inclusive of) the minimum value of 1 and the maximum value of 10; that is, all subranges beginning with a minimum value of 1 or more, e.g. 1 to 6.1, and ending with a maximum value of 10 or less, e.g., 5.5 to 10. Further, as used herein, the terms "deposited over" or "provided over" mean deposited or provided on but not necessarily in surface contact with. For example, a coating "deposited over" a substrate does not preclude the presence of one or more other coating films of the same or different composition located between the deposited coating and the substrate.
[0021] Where the term "comprising" is used in the present description and claims, it does not exclude other elements or steps. Where an indefinite or definite article is used when referring to a singular noun e.g. "a" or "an", "the", this includes a plural of that noun unless something else is specifically stated. In this document, "configured to (or set to)" may be interchangeably used in hardware and software with, for example, "appropriate to", "having a capability to", "changed to", "made to", "capable of", or "designed to" according to a situation. In any situation, an expression "device configured to do" may mean that the device "can do" together with another device or component.
[0022] Furthermore, the terms first, second and the like in the description and in the claims, are used for distinguishing between similar elements and not necessarily for describing a sequence, either temporally, spatially, in ranking or in any other manner. It is to be understood that the terms so used are interchangeable under appropriate circumstances and that the embodiments of the invention described herein are capable of operation in other sequences than described or illustrated herein. When it is described that a constituent element (e.g., a first constituent element) is "(functionally or communicatively) coupled to" or is "connected to" another constituent element (e.g., a second constituent element), it should be understood that the constituent element may be directly connectedto the another constituent element or may be connected to the another constituent element through another constituent element (e.g., a third constituent element).
[0023] The present invention will be described with respect to particular embodiments and with reference to certain drawings but the invention is not limited thereto but only by the claims.
[0024] While some embodiments described herein include some but not other features included in other embodiments, combinations of features of different embodiments are meant to be within the scope of the invention, and form different embodiments, as would be understood by those in the art. For example, in the following claims, any of the claimed embodiments can be used in any combination.The present invention
[0025] The present invention addresses this technical problem by providing a novel manufacturing method and the resulting combiner, based on a unique and synergistic combination of the use of thin, chemically tempered glass, a cold bending process to induce a bi-axial curvature, and an injectionmolding encapsulation step to permanently fix the shape.
[0026] The present invention is based on the surprising specific combination of the following technical features: a glass sheet defined by a bi-axial curvature, the formation of this shape via the cold bending of thin, chemically tempered glass, and the permanent fixation of the resulting structure through injection-molding encapsulation. This synergistic combination unexpectedly yields an optically pristine, doubly-curved, and robustly manufactured combiner.
[0027] The combiner of the present invention comprises a thin glass sheet with a thickness of approximately 1 mm, that has been chemically tempered. The chemical tempering process creates a high compressive stress at the surface of the glass, which dramatically increases its flexibility and resistance to fracture. This specific characteristic is the critical enabler for the subsequent step.
[0028] The combiner of the present invention further requires cold bending of this prepared flat glass sheet into a mold that defines the target double curvature by having a horizontal radius of at least 500mm and a vertical radius of at least 1000 mm. The flat glass, which has already been coated with the desired high-quality reflective coating on its optically active surface, is placed into the injection mold. As the mold closes, the glass is mechanically flexed at ambient temperature, forcing it to conform to the mold's bi-axially curved shape. Because the glass is thin and chemically strengthened, it can withstand the induced stress of this bi-axial elastic deformation without fracturing. This step directly solves the problem of optical quality, as the final curved surface retains the pristine,untouched quality of the original flat glass, and the pre-applied coating remains uniform and undamaged.
[0029] However, at this stage, the double curvature is merely an elastic deformation; the glass is held under tension and would spring back to its flat state if released; requiring encapsulation. While the glass is held in its stressed, doubly-curved state within the mold, a polymer material (the "injected material," e.g., a thermoplastic elastomer) is injected into the cavity between the internal face of the glass sheet and a rigid carrier part. This injected material flows to cover the entire internal face of the glass sheet and then cures or cools. This encapsulation step acts as a structural backing that "freezes" or permanently locks the glass in its elastically deformed, doubly-curved state. The cured polymer and the rigid carrier form a composite structure that counteracts the internal stress of the bent glass, preventing it from springing back and thus making the precise optical shape permanent. It also provides a robust, uniform, and durable bond between the glass and the carrier, completely eliminating the need for traditional adhesives and their associated drawbacks (e.g., aging, bubbling, and incomplete coverage). Furthermore, it also allows for the edges of the glass to be covered, protecting them from chipping and further increasing the assembly's durability.
[0030] The present invention is based on the technical synergy of : The desired double curvature is only achievable via cold bending because hot forming would destroy the optical quality, while this cold bending into a bi-axial shape is only possible because the glass is thin and chemically tempered. The shape achieved by cold bending is then only made permanent by the encapsulation step, which freezes the elastic deformation. Thus, the invention provides a complete solution to the stated problem, delivering a high-quality, doubly-curved glass combiner with superior optical properties in a manner that is efficient and scalable for manufacturing.Combiner
[0031] The present invention proposes a combiner for an head-up-display (HUD) device of a vehicle. A vehicle refers to any kind of vehicles such as (but not restricted to) a car, a van, a lorry, a motorbike, a bus, a tram, a train, a boat, a drone, an airplane, an helicopter and the like.Carrier
[0032] The combiner comprises a carrier adapted to fix the combiner to the vehicle's interior. Such carrier is usually made of a material chosen among thermoplastics such as for example polybutylene terephthalate (PBT), polycarbonate-acrylonitrile butadiene styrene (PC-ABS), polyamide (PA6), polyamide copolymer (PA66), polyoxymethylene (POM), polypropylene (PP), thermoplasticelastomers (TPE) or thermosets material such as polyurethane (PUR), epoxies (EP) with or without fillers to bring additional properties, such as glass fibers for mechanical reinforcement. The carrier could also be made of metallic material such as zamac, aluminum, magnesium (thixomolding). The carrier plate may be made of a fiber reinforced plastic, talc reinforced plastic or glass beads reinforced plastic. The carrier could also be made of glass, ceramic, stone, marble, wood or any other material suitable to produce a carrier.Glass sheet
[0033] The combiner further comprises a glass sheet. The glass sheet has an internal face facing the carrier and an external face opposite to the internal face.
[0034] The glass sheet has a composition that is not particularly limited. The glass sheet may be a soda-lime-silicate glass, an alumino-silicate glass, an alkali-free glass, a boro-silicate glass, etc. Preferably, the glass sheet of the invention is made of a soda-lime glass or an alumino-silicate glass.
[0035] In some embodiments, the glass sheet has a composition comprising, in a content expressed in percentages of the total weight of the glass:SiO255 - 85%AI2O30 - 30%B2O30 - 20%Na2O 0 - 25%CaO 0 - 20%MgO 0 - 15%K2O 0 - 20%BaO 0 - 20%.
[0036] In some embodiments, the glass sheet has a composition comprising, in a content expressed in percentages of the total weight of the glass:SiO255 - 70%AI2O30 - 25%B2O30 - 10%Na2O 5 - 20%CaO 0 - 15%MgO 0 - 15%K2O 0 - 10%BaO 0 - 5%.
[0037] In some embodiments, the glass sheet has a composition comprising, in a content expressed in percentages of the total weight of the glass:SiO258 - 70%AI2O30 - 20%B2O30 - 5%CaO 0 - 3%MgO 0 - 12%Na2O 10 - 20%K2O 0 - 5%BaO 0 - 5%.
[0038] In some embodiments, the glass sheet has a composition comprising, in a content expressed in percentages of the total weight of the glass:SiO265 - 70%AI2O34 - 8%B2O30 - 1%CaO 0 - 2%MgO 7 - 12%Na2O 14 - 18%K2O 0 - 2%BaO 0 - 1%.Such composition is a good compromise between the mechanical performances of the glass after chemical strengthening and cost optimization. More preferably, the glass sheet has the following composition comprising the following components in weight percentage, expressed with respect to the total weight of glass composition:60 < SiO2 < 80 wt% 65 < SiO2 < 78 % 65 < SiO2 < 78 wt% 65 < SiO2 < 68 wt% 5 < Na2O < 20 wt% 5 < Na2O < 20 % 5 < Na2O < 20 wt% 14 < Na 20 < 18 wt% 0 < K2O < 12 wt% 0.9 < K2O < 12 % 1.0 < K2O < 8.0 wt% 0.8 < K2O < 1.2 wt% 1 < AI2O3 < 8 wt% 3.0 < AI2O3 < 8 % 3.0 < AI2O3 < 6 wt% 5.0 < AI2O3 < 6.2 wt% 0 < CaO < 10.0 wt% 0.4 < CaO < 8 % 0.4 < CaO < 8 wt% 0.5 < CaO < 1.5 wt% 0 < MgO < 12 wt% 4 < MgO < 10 % 4 < MgO < 10 wt% 8.5 < MgO < 10.5 wt%
[0039] Preferably these compositions comprise the alkali-earth oxides at the ratio of MgO / (MgO+CaO)) > 0.5, more preferably 0.88 < [MgO / (MgO+CaO)] < 1. Preferably these compositions comprise the alkali oxides at the ratio of 0.05 < K2O / (K2O+Na2O) <0.7.
[0040] In some embodiments, the glass sheet has a composition comprising, in a content expressed in percentages of the total weight of the glass:SiO265 - 75%AI2O30 - 3%B2O30 - 1%CaO 5 - 10%MgO 4 - 8%Na2O 10 - 15%K2O 0 - 1%BaO 0 - 1%.
[0041] In some embodiments, the glass sheet has a composition comprising, in a content expressed in percentages of the total weight of the glass:SiO255 - 70%AI2O311 - 20%B2O30 - 5%CaO 0 - 3%MgO 4 - 8%Na2O 10 - 18%K2O 0 - 7%BaO 0 - 1%.
[0042] The glass sheet according to the invention may be a glass sheet obtained by a floating process, a drawing process, a rolling process or any other process known to manufacture a glass sheet starting from a molten glass composition. In some embodiments, the glass sheet is a float glass sheet. The term "float glass sheet" is understood to mean a glass sheet formed by the float glass process, which consists in pouring the molten glass onto a bath of molten tin, under reducing conditions.
[0043] According to an advantageous embodiment of the invention, combinable with previous embodiments on base glass composition, the glass sheet has a composition comprising a total iron (expressed in terms of Fe2O3) equal to or lower than 0.100 wt%, preferably equal to or lower than 0.080 wt%, equal to or lower than 0.060 wt%, equal to or lower than 0.040 wt%, equal to or lowerthan 0.020 wt%. The glass sheet has a composition comprising a total iron (expressed in terms of Fe2O3) preferably equal to or greater than 0.002 wt%, preferably equal to or greater than 0.005 wt%, preferably equal to or greater than 0.010 wt%, preferably equal to or greater than 0.012 wt%, preferably equal to or greater than 0.015 wt%. A total iron (expressed in the form of Fe2O3) content of less than or equal to 0.100 wt% makes it possible to obtain a glass sheet with almost no visible coloration and allowing a high degree of flexibility in aesthetic designs. The minimum value makes it possible not to be excessively damaging to the cost of the glass as such, low iron values often require expensive, very pure, starting materials and also purification of these.
[0044] The glass sheet has a thickness of 1 mm. This value encompasses glass sheet of a thickness of 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1.0 mm, 1.1 mm, 1.2 mm, 1.3 mm and 1.4 mm.Chemical tempering / strengthening
[0045] The glass sheet is chemically tempered. Using chemically tempered glass allows to cold bend the glass sheet, and therefore to put the glass sheet in the desired form. Chemical tempering also improves the mechanical resistance of the glass sheet. The glass sheet is tempered by ion exchange, or "chemical" tempering. The process of chemical tempering comprises a step where the glass is immerged into a molten alkali salt at a temperature below the glass transition. Processes to chemically strengthen / temper glass are well known to the skilled man in the art. Typically, chemical tempering / strengthening is performed by exchanging Na+ ions by K+ ions at the surface of the glass sheet by dipping the glass sheet in a molten salt bath at a temperature below the glass transition temperature. Advantageously, the bath consist of high purity KNO3 and the treatment is performed at temperature between 350°C and 470°C, for 0.5 to 24 hours. Chemical tempering / strengthening is preferably applied for glass sheet of thickness below 3 mm, such as glass sheet of the present invention with a thickness of 1 mm.
[0046] Hence, in a preferred embodiment, the glass sheet is chemically tempered to provide a compressive stress equal to or greater than 350MPa (CS > 350MPa) and a depth of layer equal to or greater than 8pm (DoL > 8pm). In a preferred embodiment, the glass sheet is chemically tempered to provide a compressive stress equal to or greater than 400MPa (CS > 400MPa), preferably equal to or greater than 450MPa (CS > 450MPa), preferably equal to or greater than 500MPa (CS > 500MPa), preferably equal to or greater than 550MPa (CS > 550MPa), more preferably equal to or greater than 600MPa (CS > 600MPa); and / or a depth of layer (DoL) equal to or greater than 10pm (DoL > 10pm); preferably equal to or greater than 12pm (DoL > 12pm); preferably equal to or greater than 14pm (DoL > 14pm); preferably equal to or greater than 16pm (DoL > 16pm), preferably equal to or greaterthan 18pm (DoL > 18pm), more preferably equal to or greater than 20pm (DoL > 20pm).Anti-glare
[0047] In some embodiments, the external face of the glass sheet may be roughened. Roughening can be achieved by etching (acid, alkaline, liquid or vapor), laser texturing, sand blasting, embossing, rolling, mechanical polishing, engraving, and / or vapor deposition (e.g. chemical or physical vapor deposition), preferably by etching. Acid etching is preferred since it provides process control, short process time and flexibility. Such roughening provides anti-glare properties to the external face of the glass sheet of the combiner.
[0048] In some embodiments, some parts of the glass sheet may be roughened for decoration purpose and / or seamless integration. The roughening can be done on the full surface of the glass sheet, or only in some specific areas, for example close to the edges of the glass sheets, To perform such a partial roughening, common techniques can be used, such as application of a protective mask prior the etching, or sandblasting process. The roughening treatment can also be done locally, without using a protective mask, for example with embossing or laser texturing.Reflective coating
[0049] The external face of the glass sheet has a reflective coating reflecting at least 10 % of incoming visible light.
[0050] In some embodiments, instead of a reflective coating, a reflective film reflecting at least 10% of the incoming visible light is applied on the external face of the glass sheet.
[0051] In some embodiments, such reflective coating is a semi-mirror coating or a dichroic coating, without specific reflection selectivity towards light polarization.
[0052] In some embodiments, the reflective coating is a p-polarized (light) reflective coating. The p-polarized reflective coating may typically comprise at least one sequence of layers of high refractive index layers / low refractive index layers, or high / low sequence. The high / low sequence may occur more than once, meaning the sequence may be repeated at least 2 times, up to 3 or 4 times.
[0053] The p-polarized reflective coating may be a magnetron sputtered p-polarized reflective coating, having the advantage of being easily processed, easily adaptable to the selected function, and cost efficient.
[0054] The thickness of the coating is geometrical thickness expressed in nm, unless indicated otherwise.
[0055] A layer in the p-polarized reflective coating may comprise more than one sub-layer.
[0056] The p-polarized reflective coating may comprise a layer of absorbent material, having a thickness ranging from 0.2 nm to 15 nm. Such absorbent material has an average refractive index n above 1. By "absorbent material" is meant a material which absorbs a part of the visible radiation.
[0057] The p-polarized reflective coating itself may have any light transmittance, that is, a light transmittance less than 90%, less than 70%, alternatively less than 65%, alternatively less than 60%, and greater than 30%, alternatively greater than 40%, when measured on a sheet of monolithic clear float glass of 2.1 mm.
[0058] The p-polarized light reflective coating is considered a nonconductive coating, meaning its sheet resistance may be superior to 100 Ohm / square.
[0059] The p-polarized light reflective coating is sufficiently durable and resistant to scratches to be applied on the external face of the glass sheet of the combiner.
[0060] The p-polarized light reflective coating may be optimized in order to maximize the ratio of the p-polarized light reflection and total reflection (internal) at a certain angle of incidence (Rp-pol / Rin), measured at a wavelength of 550 nm + / - 100 nm. At said angle of incidence at a visible wavelength, the p-polarized light reflection is maximized and the interior reflection is minimized.
[0061] The angle of installation of the combiner may thus be selected such that the ratio Rp-pol / Rin is maximized. This has the advantage that, although the p-polarized light reflection is maximized - at that particular angle of incidence, the driver or vehicle occupant is not disturbed by the dashboard reflection (in the visible range).
[0062] Thus, an image (light) source projecting p-polarized light may be used to project an image toward the combiner according to the present invention.
[0063] In some embodiments, the combiner is provided with a p-polarized light reflective film. The film is provided preferably on the external face of the glass sheet of the combiner facing towards the vehicle interior, where it provides for optimal reflection of p-polarized light. The p-polarized light reflective film is selected for example from films comprising at least one transparent liquid crystal layer, films comprising at least one cholesteric liquid crystal layers, films comprising a plurality ofalternating polymeric interference layers, and the like. For example, a reflective film comprising liquid crystal layers can be bonded to the surface of the glass sheet as a functional foil. In this case, corresponding liquid crystal layers are applied as a stack of functional layers, for example, to carrier foils made of cellulose triacetate (TAC), polyethylene terephthalate (PET), polyethylene (PE), polyamide (PA) or other conventional polymeric materials. High precision coating processes for the manufacture of such functional liquid crystal films are available and known in the art and the functional films are commercially available. Advantageously, the foils can be applied to the external face of the glass sheet of the combiner, which surface is intended to serve as a projection surface. Commercial examples of such reflective films are available from 3M under the tradename 3M® WCF, or the reflective films available from Toray under the tradename PICASUS®VT, or the reflective films available from Fujifilm under the tradename Wavista®.Other coatings
[0064] In some embodiments, the external glass sheet may be coated with an additional coating, above the reflective coating, such as an anti-fingerprint coating and / or an hydrophobic coating.
[0065] In a preferred embodiment, the external glass sheet is coated at least one anti-fingerprint layer / treatment to reduce or prevent fingerprints from registering. Anti-fingerprint (AFP) coating is a specialized surface treatment designed to reduce the visibility of fingerprints and smudges on surfaces. It is achieved by incorporating hydro- / oleophobic properties, making the surface hydrophobic (repelling water) and oleophilic (attracting oils), which minimizes fingerprint marks Advantageously, according to this embodiment, the glass article has said anti-fingerprint layer and / or an easy to clean coating and / or treatment on the first surface of the glass sheet. An anti-fingerprint coating may prove useful to avoid interferences of light from the viewing area. The fingerprints will be less visible from the outside and provide for improved aesthetics. Examples of anti-fingerprint coatings include fluorinated polyethers, silanes, fluoro-silanes, siloxanes, fluorinated siloxanes, phosphonates, fluoro-organic compounds, perfluorocarbon-containing materials, and the like. These anti-fingerprint coatings are known in the art.Cold bending
[0066] As the glass sheet is thin and is chemically tempered, it can undergo cold bending, meaning bending at a temperature below 150°C, without damages such as cracks and breaks.
[0067] In case of a combiner for a vehicle equipped with a windshield, the horizontal curvature is usually done in order for the glass sheet to follow the curvature of such windshield. The horizontalcurvature allows also to magnify the perceived image in the horizontal axis. The glass sheet has a horizontal curvature radius of at least 500 mm (HR > 500mm), equal to or greater than 1.000 mm (HR > 1.000mm), equal to or greater than 1.200 mm (HR > 1.200mm), equal to or greater than 1.500 mm (HR > 1.500mm) to avoid excessive curvature stress in the glass sheet. Preferably, the horizontal curvature radius is equal to or lower 25.000 mm (HR < 25.000mm), preferably equal to or lower 18.000 mm (HR < 18.000mm), preferably equal to or lower 10.000 mm (HR < 10.000 mm), preferably equal to or lower 8.000 mm (HR < 8.000mm), preferably equal to or lower 7.000 mm (HR < 7.000mm).
[0068] The vertical curvature allows to magnify the perceived image in the vertical axis. This is advantageous as the image looks bigger and further away from the driver as it really is. The glass sheet has a vertical curvature radius of at least 1000 mm (VR > 1.000 mm), equal to or greater than 1.200 mm (HR > 1.200mm), equal to or greater than 1.500 mm (HR > 1.500mm), equal to or greater than 2.000 mm (HR > 2.000mm) to avoid excessive curvature stress in the glass sheet. Preferably, the vertical curvature radius is equal to or lower 25.000 mm (VR < 25.000mm), preferably equal to or lower 18.000 mm (VR < 18.000mm), preferably equal to or lower 10.000 mm (VR < 10.000mm) preferably equal to or lower 8.000 mm (VR < 8.000mm) preferably equal to or lower 8.000 mm (VR < 8.000mm), preferably equal to or lower 7.000 mm (VR < 7.000 mm).
[0069] In the embodiments of the present invention wherein the combiner's bi-axially curved surface, has distinct horizontal (HR) and vertical (VR) radii of curvature, anisotropic optical magnification (i.e. the magnification factor applied to the projected image is different in the horizontal and vertical axes), can cause distortion of the projected image. However, this distortion is readily and precisely correctable by a person skilled in the art of display and projection systems by applying a pre-compensatory distortion to the initial image generated by the projector.Injection molding
[0070] The entire internal face of the glass sheet is fixed to the carrier with an injected material (20). The combiner of the present invention is indeed further characterized by a layer of a polymeric material (20) that structurally integrates the glass sheet (30) with the carrier (10). This intermediate layer, formed in-situ via injection molding, is disposed between the two components and is bonded to the entire internal face (31) of the glass sheet as well as to the carrier.
[0071] The primary function of this feature is to permanently lock the glass sheet in its elastically deformed, bi-axially curved state. By filling the space between the carrier and the stressed glass, the cured polymeric layer counteracts the internal restorative forces from the cold bending process, effectively "freezing" the precise optical shape. This method of fixation provides a complete anduniform bond across the entire surface, which inherently solves the known drawbacks of conventional adhesives, such as aging, delamination, the formation of air bubbles, and incomplete coverage. Furthermore, this full-surface bond ensures that in the event of breakage, glass shards are contained by the layer, enhancing safety.
[0072] In one embodiment, the injected material layer is a thermoplastic elastomer (TPE) or a thermoset, selected for properties such as its melt flow rate, which ensures the mold can be filled completely and uniformly to create a defect-free structural bond.
[0073] In some embodiments, the injected plastic material is a thermoplastic material. Thermoplastic material are usually not expensive. They are also very easy to inject, making implementation easier and faster. Such thermoplastic material can be a soft polyvinyl chloride or a thermoplastic elastomer, such as a thermoplastic styrenic elastomer (TPS), an acrylic-based thermoplastic elastomer, a thermoplastic polyurethane (TPU), a thermoplastic olefinic elastomer (TPO), a co-polyester (CPE) or a co-polyamide (CPA). TPS has a low viscosity range with an attractive cost. TPU could have better mechanical properties, but with a higher cost and is more difficult to process. TPS is widely used for standard automotive window encapsulation and exhibit good adhesion properties to glass, particularly when used with a dedicated primer.
[0074] In some embodiments, the melt flow rate of the thermoplastic material is at least 10 g per 10 minutes, preferably at least 30 g per 10 minutes, more preferably at least 80 g per 10 minutes, even more preferably at least 100 g per 10 minutes, measured conformed to ISO1133-l:2022 for 2.16 kg and at 230°C. The higher the melt flow rate, the more fluid the thermoplastic material. If the thermoplastic material is more fluid, then less injection gates are needed to inject the thermoplastic material. The lower the number of injection gates, the more homogeneous is the injection. There are indeed therefore less weld lines. A weld line is the line where two flow fronts meet when there is the inability of two or more flow fronts to weld, during the moulding process. These lines cause locally weak areas in the moulded part.
[0075] In some embodiments, the injected plastic material is a thermoset material. Thermoset materials are usually very fluid. They also generally show a higher resistance to temperature above 100°C.
[0076] The thermoset material can be a polyurethane-based thermoset, a silicone-based thermoset or an ethylene-vinyl acetate-based thermoset. Due to its low viscosity, a thermoset material is easier to inject, and therefore allows to create long pieces. The temperature resistance of the combiner could also be higher. Moreover, the optical performance could be higher due to the lower stress inducedduring the process.
[0077] In some embodiments, the thickness of the injected plastic material is less than or equal to 4.0 mm, preferably less than or equal to 3.0 mm, more preferably less than or equal to 2.5 mm. The thickness of the injected plastic material is equal to or higher than 0.8 mm, preferably equal to or higher than 1.5 mm, more preferably equal to or higher than 2.0 mm. Such thickness allows to ease the injection of the injected material, while having a weak impact on the optical properties of the combiner and ensuring the rigidity of the combiner. It further allows to reduce the weight of the combiner, as the density of the injected plastic material is around 1 gr / cm3, and therefore much lower than glass.Ink layer
[0078] In some embodiments, the internal glass sheet may be covered with an ink layer.
[0079] The ink layer is not particularly limited. Suitable inks are an inorganic type ink containing a ceramic fired body or the like and an organic type ink containing a dye or a pigment and an organic resin can be used. Preferred are solvent based organic inks and more preferred are acrylic networks with color imparting pigments. Preferably, the ink layer is made by a single layer for ease of production. However, it can also comprise different sublayers, even of different materials.
[0080] The ink layer is formed, for example, by a method of printing ink. Printing methods include, but are not limited to, ink jet, screen printing, and transfer decoration over the second face of the glass sheet.
[0081] The deposition of the ink layer can be achieved by an ink jet method. The ink jet method generally forms a ink pattern while linearly moving the nozzle in one direction. The thickness of the ink layer can be adjusted by controlling the discharge amount and the discharge interval of the ink discharged from the nozzle. The inkjet method ejects a minute droplet of ink in a liquid form from a nozzle in a pulsed manner to form a predetermined pattern on the second surface. Punctate ink is formed in succession to form a ink layer of a predetermined pattern comprising a background and at least one foreground. Thereafter, the ink is dried and baked, whereby the ink is cured to form the ink layer. A UV-curable ink is used, where the bonding network is cured and solidified by subjecting the ink to UV lamps just after the droplet deposition. The order in which each layer is formed is not limited thereto.
[0082] The ink layer can applied on the glass in one layer using a digital printer. The printer applies 4types of inks : Cyan, Magenta, Yellow and Black. Each mix of these 4 inks can result in a custom color, based on the additive color mixing principle. Each drop of ink creates a colored dot that is applied from left to right on the entire width of the pattern, line by line from the top to the bottom of the glass, and instantly UV-cured. The entire pattern is obtained thanks to this accumulation of colored dots on the surface of the glass.
[0083] Also suitable method to produce the ink layer is a screen printing wherein a mesh is used to transfer ink onto a glass sheet substrate, except in areas made impermeable to the ink by a blocking stencil.
[0084] In the transfer decoration method, the transfer sheet having the ink layer is brought into close contact with the glass substrate under heating conditions, thereby transferring the ink layer to the glass substrate. The transfer sheet is formed by laminating a transfer base material (film), a coloring layer, and an adhesive layer. The transfer base material is formed of a resin material or the like to support the ink layer and the optionally adhesive layer. The ink layer is formed in a planar shape of the pattern to be transferred and is supported on the transfer substrate. The adhesive layer is a layer for bonding the ink layer to the glass substrate, and is formed in the same shape as the ink layer. When no adhesive layer is used, an ink having an adhesive property can be used as the ink layer, or an adhesive can be additionally coated on the surface of the ink layer. The glass sheet and the transfer sheet are disposed so that the second surface of the glass sheet and the adhesive layer of the transfer sheet face each other. Next, the transfer sheet is heated to soften the transfer sheet by e.g; infrared rays, superheated steam, hot plates, and the like. The softened transfer sheet is shaped by the differential pressure and adheres closely to the second surface of the glass sheet. Finally, by peeling off the transfer base material of the transfer sheet from the glass sheet, the adhesive layer and the ink layer remain on the second surface, so that the ink layer can be transferred onto the second surface.
[0085] The thickness of each individual ink layer is typically comprised between 1 pm and 50 pm. Preferably, the ink layer thicknesses is equal to or greater than 2 pm, preferably equal to or greater than 3 pm, more preferably equal to or greater than 5 pm. Preferably, the ink layer's thickness is equal to or lower than 40 pm, preferably equal to or lower than 30 pm, preferably equal to or lower than 25 pm, preferably equal to or lower than 20 pm, preferably equal to or lower than 15 pm, more preferably equal to or lower than 12 pm. The minimum and maximum thicknesses are mean values of ink layer thickness. Thickness is measured in the direction perpendicular to the glass sheet faces.
[0086] The thickness of the ink layer can be measured by any conventional method known by personskilled in that art such conventional optical microscope or profiling tools such as confocal microscope, white light interferometer or stylus profiler.
[0087] When the preferred technique of inkjet printing is used, the thickness of such inkjet-printed ink layer is typically from 1 pm to 5 pm whereas the thickness of a screen-printed ink layer is typically from 5 pm to 20 pm.Process
[0088] The present invention further refers to a method to manufacture a combiner for an head-up-display device of a vehicle, as described previously.
[0089] The method comprises the first step of providing a mould for injection moulding. The mould has a first part and a second part.
[0090] The method comprises the second step of providing a carrier in the first part of the mould. The carrier is adapted to fix the combiner to the vehicle.
[0091] The method comprises the third step of providing a glass sheet in the second part of the mould. The glass sheet has an external face facing the second part of the mould and an internal face opposite to the external face of the glass sheet. The glass sheet has a thickness of 1 mm. The glass sheet has been chemically tempered prior to be provided in the second part of the mould.
[0092] In some embodiments, the external face of the glass sheet has been roughened, prior to be provided in the second part of the mould. Roughening the external face of the glass sheet provides an anti-glare effect, for functional or decorative purposes.
[0093] The external face of the glass sheet has been coated with a reflective coating reflecting at least 10 % of incoming visible light, prior to be provided in the second part of the mould. In some embodiments, instead of a reflective coating, a reflective film, reflecting at least 10 % of incoming visible light, is applied on the external face of the glass sheet.
[0094] In some embodiments, the external face of the glass sheet has been further coated with an anti-fingerprint and / or an hydrophobic coating, above the reflective coating, prior to be provided in the second part of the mould. In some embodiments, the internal face of the glass sheet has been further coated with an ink layer, prior to be provided in the second part of the mould.
[0095] In some embodiments, the internal face of the glass sheet is further coated with a primer inorder to increase the adherence between the glass sheet and the injected material, prior to closing the mould. Such primer can for example be a primer containing silane. Such primer can instead or also be applied on the carrier, prior to closing the mould, therefore positioned between the carrier and the injected material to increase adhesion of the injected material to the carrier.
[0096] An advantage of the present process is to be able to make all coatings and decorations on flat glass before bending. It allows a more homogeneous coating, and is further easier to process.
[0097] The method comprises the fourth step of bending the glass sheet at ambient temperature to the second part of the mould so that the glass sheet has a horizontal curvature radius of at least 500 mm and a vertical curvature radius of at least 1000 mm.
[0098] The method comprises the fifth step of closing the mould.
[0099] The method comprises the sixth step of injecting an injectable material to fix the entire internal face of the glass sheet to the carrier to form the combiner.
[0100] In some embodiments, the injectable material is further injected to cover the edges of the glass sheet. In some embodiments, the injectable material is a thermoplastic elastomer.
[0101] The main advantage of the present method is that any coating is done prior to the bending of the glass sheet. It means the coating is done on a place surface, allowing a better homogeneity of the coating, compared to a coating done on a curved surface. As the bending is done at a low temperature (cold bending), the coating is not damaged by the bending process itself.
[0102] Referring to Fig.la, a combiner (1) for an head-up display device of a vehicle comprises a carrier (10). The carrier (10) is used to fix the combiner (1) on the interior of a vehicle (not shown). The combiner (1) further comprises a glass sheet (30). The internal face of the glass sheet (30) faces the carrier (10), while the external face (32) of the glass sheet (30) faces the interior of the vehicle (not shown) wherein the combiner (1) is fixed.
[0103] The glass sheet (30) has a horizontal curvature radius (HR) of at least 500 mm and a vertical curvature radius (VR) of at least 1000 mm. None of these curvature radii are shown at scale on the figures in order to facilitate the understanding.
[0104] The external face (32) of the glass sheet (30) is coated with a reflective coating reflecting at least 10 % of incoming visible light. Such coating is not represented on the figures.
[0105] The glass sheet (30) is adhered to the carrier (10) through injected material (20). The injected material (20) fully covers the internal face (31) of the glass sheet (30).
[0106] Fig.lb shows a similar embodiment of Fig.la, except that the carrier (10) is represented with at least one protrusion (100) in order to fix the combiner (1). Other means to fix such combiner (1) are known by the person skilled in the art.
[0107] Fig.2 shows a similar embodiment of Fig.lb, as a cross sectional view. The combiner comprises a glass sheet (30) having internal face (31) and an external face (32). The carrier (10) is represented with two protrusions (100) in order to fix the combiner (1) on the interior of a vehicle (not shown). Other means to fix such combiner (1) are known by the person skilled in the art. Only the vertical curvature radius (VR) is shown on this figure, in order not to complexify the rendering.
[0108] While the invention has been illustrated and described in detail in the drawings and foregoing description, such illustration and description are to be considered illustrative or exemplary and not restrictive. The foregoing description details certain embodiments of the invention. It will be appreciated, however, that no matter how detailed the foregoing appears in text, the invention may be practiced in many ways. The invention is not limited to the disclosed embodiments.Examples
[0109] Example 1 : The first part of the mold comprises a thermoplastic polypropylene (PP) carrier adapted to fix the combiner to the dashboard of a vehicle. A glass sheet of thickness 1.0mm and size 800mm wide and 80mm high, is chemically tempered (CS of 480MPa and DoL of 13pm). The face of the glass sheet that will be orientated to be the external face is coated with a reflective film reflecting at least 10 % of incoming visible light. The opposite (internal) face of the glass sheet is coated with an epoxy ink layer of 10pm thickness. The internal face of the glass sheet is further coated with a suitable primer in order to increase the adhesion between the glass sheet and the injected material. The glass sheet is then bended at ambient temperature to the second part of the mold so that the glass sheet has a horizontal curvature radius of 5.000 mm and a vertical curvature radius of 10.000 mm. The mold is closed and thermoplastic styrene elastomer (TPS) is injected to fix the entire internal face of the glass sheet to the carrier to form the combiner.
[0110] A horizontal optical magnification of about 116% (i.e. the final image is 16% larger in horizontal direction than the original image) and a vertical optical magnification of about 108% (i.e. the final image is 8% larger in vertical direction than the original image) are obtained when such blade is positioned on the dashboard at about 40cm from the projector.
[0111] Example 2: The first part of the mold comprises a thermoplastic polypropylene (PP) carrier adapted to fix the combiner to the dashboard of a vehicle. A glass sheet of thickness 0.7mm and size 1500mm wide and 120mm high, is chemically tempered (CS of 550MPa and DoL of 20pm). The face of the glass sheet that will be orientated to be the external face is coated with a reflective coating reflecting at least 10 % of incoming visible light, and then is coated with an anti-fingerprint coating. The opposite (internal) face of the glass sheet is coated with an epoxy ink layer of 10pm thickness. The internal face of the glass sheet is further coated with a suitable primer in order to increase the adhesion between the glass sheet and the injected material. The glass sheet is then bended at ambient temperature to the second part of the mold so that the glass sheet has a horizontal curvature radius of 2.500 mm and a vertical curvature radius of 7.000 mm. The mold is closed and thermoplastic elastomer (TPE) is injected to fix the entire internal face of the glass sheet to the carrier to form the combiner.
[0112] A horizontal optical magnification of about 114% (i.e. the final image is 14% larger in horizontal direction than the original image) and a vertical optical magnification of about 105% (i.e. the final image is 5% larger in vertical direction than the original image) are obtained when such blade is positioned on the dashboard at about 17cm from the projector.
[0113] Example 3: The first part of the mold comprises a thermoplastic polycarbonate-acrylonitrile butadiene styrene (PC-ABS) carrier adapted to fix the combiner to the dashboard of a vehicle. A glass sheet of thickness 1.3mm and size 1100mm wide and 140mm high, is chemically tempered (CS of 550MPa and DoL of 20pm). The face of the glass sheet that will be orientated to be the external face is coated with a reflective coating reflecting at least 10 % of incoming visible light, and then is further coated with an anti-fingerprint coating. The opposite (internal) face of the glass sheet is coated with a suitable primer in order to increase the adhesion between the glass sheet and the injected material. The glass sheet is then bended at ambient temperature to the second part of the mold so that the glass sheet has a horizontal curvature radius of 10.000 mm and a vertical curvature radius of 7.000 mm. The mold is closed and thermoplastic polyurethane (TPU) is injected to fix the entire internal face of the glass sheet to the carrier to form the combiner.
[0114] A horizontal optical magnification of about 103% (i.e. the final image is 3% larger in horizontal direction than the original image) and a vertical optical magnification of about 105% (i.e. the final image is 5% larger in vertical direction than the original image) are obtained when such blade is positioned on the dashboard at about 17cm from the projector.
[0115] Example 4: The first part of the mold comprises a thermoplastic polycarbonate-acrylonitrilebutadiene styrene (PC-ABS) carrier adapted to fix the combiner to the dashboard of a vehicle. A glass sheet of thickness 0.7mm and size 1500mm wide and 120mm high, is chemically tempered (CS of 550MPa and DoL of 20pm). The face of the glass sheet that will be orientated to be the external face is coated with a reflective coating reflecting at least 10 % of incoming visible light, and then further coated with an anti-fingerprint coating. The opposite (internal) face of the glass sheet is coated with an epoxy ink layer of 10pm thickness. The internal face of the glass sheet is further coated with a suitable primer in order to increase the adhesion between the glass sheet and the injected material. The glass sheet is then bended at ambient temperature to the second part of the mold so that the glass sheet has a horizontal curvature radius of 25.000 mm and a vertical curvature radius of 1.000 mm. The mold is closed and thermoplastic elastomer (TPE) is injected to fix the entire internal face of the glass sheet to the carrier to form the combiner.
[0116] A horizontal optical magnification of about 102% (i.e. the final image is 2% larger in horizontal direction than the original image) and a vertical optical magnification of about 142% (i.e. the final image is 42% larger in vertical direction than the original image) are obtained when such blade is positioned on the dashboard at about 21cm from the projector.
[0117] Example 5: The first part of the mold comprises a thermoplastic polypropylene (PP) carrier adapted to fix the combiner to the dashboard of a vehicle. A glass sheet of thickness 0.7mm and size 1000mm wide and 140mm high, is chemically tempered (CS of 520MPa and DoL of 18pm). The face of the glass sheet that will be orientated to be the external face is coated with a reflective coating reflecting at least 10 % of incoming visible light, and then further coated with an anti-fingerprint coating. The opposite (internal) face of the glass sheet is coated with an epoxy ink layer of 10pm thickness. The internal face of the glass sheet is further coated with a suitable primer in order to increase the adhesion between the glass sheet and the injected material. The glass sheet is then bended at ambient temperature to the second part of the mold so that the glass sheet has a horizontal curvature radius of 5.000 mm and a vertical curvature radius of 5.000 mm. The mold is closed and thermoplastic elastomer (TPE) is injected to fix the entire internal face of the glass sheet to the carrier to form the combiner.
[0118] A horizontal optical magnification of about 114% (i.e. the final image is 14% larger in horizontal direction than the original image) and a vertical optical magnification of about 114% (i.e. the final image is 14% larger in vertical direction than the original image) are obtained when such blade is positioned on the dashboard at about 36 cm from the projector.
Claims
Claims1. Combiner (1) for an head-up-display device of a vehicle comprising:a. A carrier (10) adapted to fix the combiner (1) to the vehicle;b. A glass sheet (30) having an internal face (31) facing the carrier (10) and an external face (32) opposite to the internal face (31);i. The glass sheet (30) having a thickness of 1 mm;ii. The glass sheet (30) being chemically tempered;iii. The glass sheet (30) having a horizontal curvature radius (HR) of at least 500 mm;iv. The glass sheet (30) having a vertical curvature radius (VR) of at least 1000 mm;v. The external face (32) of the glass sheet (30) having a reflective coating reflecting at least 10 % of incoming visible light;vi. The entire internal face (31) of the glass sheet (30) being fixed to the carrier (10) with injected material (20).
2. A combiner (1) according to claim 1, wherein edges of the glass sheet (30) are further covered with the injected material (20).
3. A combiner (1) according to any one of the previous claims, wherein the external face (32) of the glass sheet (30) is roughened.
4. A combiner (1) according to any one of the previous claims, wherein the internal face (31) of the glass sheet (30) comprises an ink layer.
5. A combiner (1) according to any one of the previous claims, wherein the injected material (20) is a thermoplastic elastomer.
6. A combiner (1) according to any one of the previous claims, wherein the external face (32) of the glass sheet (30) is further coated with an anti-fingerprint coating or an hydrophobic coating.
7. Method to manufacture a combiner (1) for an head-up-display device of a vehicle comprising the following steps:i. Providing a mould for injection moulding, the mould having a first part and a second part;ii. Providing a carrier (10) in the first part of the mould, the carrier being adapted to fix the combiner (1) to the vehicle;ill. Providing a glass sheet (30) in the second part of the mould, the glass sheet (30) having an external face (32) facing the second part of the mould and an internal face (31) opposite to the external face (32) of the glass sheet (30), the glass sheet (30) being chemically tempered, the glass sheet (30) having a thickness of 1 mm, the external face (32) of the glass sheet (30) being coated with a reflective coating reflecting at least 10 % of incoming visible light;iv. Bending the glass sheet (30) at ambient temperature to the second part of the mould so that the glass sheet (30) has a horizontal curvature radius (HR) of at least 500 mm and a vertical curvature radius (VR) of at least 1000 mm;v. Closing the mould;vi. Injecting an injectable material (20) to fix the entire internal face (31) of the glass sheet (30) to the carrier (10) to form the combiner (1).
8. Method according to claim 7, wherein the injectable material (20) is a thermoplastic elastomer.
9. Method according to any one of claims 7 or 8, wherein the external face (32) of the glass sheet (30) is roughened prior to being coated with a reflective coating.
10. Method according to any one of claims 7 to 9, wherein the external face (32) of the glass sheet (30) is further coated with an anti-fingerprint coating or a hydrophobic coating before being provided in the mould.
11. Method according to any one of claims 7 to 10, wherein the internal face (31) of the glass sheet (30) is covered with an ink layer before being provided in the mould.
12. Method according to any one of claims 7 to 11, wherein edges of the glass sheet (30) are covered with the injectable material (20) during the step of injection.
13. Method according to any one of claims 7 to 12, wherein the internal face (31) of the glass sheet (30) is further coated with a primer, prior to closing the mould.
14. Method according to any one of claims 7 to 13, wherein the carrier (10) is coated with a primer, prior to closing the mould.