Method for producing densified cylindrical bodies and product thus obtained
By incorporating sacrificial fibres to create channels and using non-sacrificial fibres as a matrix, the method addresses the challenge of uniform densification and channel blockage, resulting in a cylindrical body with enhanced mechanical and thermal properties for high-performance applications.
Patent Information
- Application Number
- PCT/IB2026/054186
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2026-04-28
- Publication Date
- 2026-11-12
AI Technical Summary
Existing methods for producing densified cylindrical bodies face challenges in achieving uniform and deep densification, as the densification process often clogs access paths, leaving the core porous and compromising structural integrity, and the creation of internal channels is hindered by blockage, affecting mechanical and thermal properties.
A method involving sacrificial fibres is used to create internal channels within cylindrical bodies by decomposing these fibres to form channels, ensuring uniform densification and preventing process blockage, combined with non-sacrificial fibres forming the supporting matrix and a densified carbon matrix to enhance mechanical and thermal properties.
The method achieves uniform and complete densification, improving mechanical and thermal properties, ensuring the cylindrical body can withstand high mechanical and thermal stresses, suitable for high-performance applications.
Smart Images

Figure IB2026054186_12112026_PF_FP_ABST
Abstract
Description
Method for producing densified cylindrical bodies and product thus obtained★ ★ ★DESCRIPTION
[0001] . Field of the invention
[0002] . The present invention relates to the production of composite materials, in particular the production of densified cylindrical bodies initially with internal channels formed from sacrificial fibers .
[0003] . Prior art
[0004] . Materials science is a field of study concerned with the analysis and application of the properties of matter, with a particular focus on the design and discovery of new materials . This sector is highly interdisciplinary in nature, involving principles of physics, chemistry, engineering and applied sciences in order to understand and manipulate the properties of materials at atomic and molecular level . The main obj ective of materials science is to develop materials having specific properties capable of meeting the needs of advanced applications in various industrial sectors .
[0005] . One of the fundamental aspects of materials science is the understanding of the relationships between the microscopic structure of materials and their macroscopic properties . This involves the study of the arrangement of atoms, molecules and crystalline phases within a material and how these influence its physical, chemical and mechanical characteristics . The ability to manipulate these structures at microscopic level enables materials scientists to design materialshaving tailor-made properties for specific applications .
[0006] . The synthesis of materials is one of the crucial phases in the field of materials science . It comprises a series of chemical and physical processes used to create new materials or modify existing materials . These processes may comprise thin film deposition, crystal growth, powder sintering and monomer polymerisation. Each synthesis method is selected according to the desired properties of the final material and its intended applications .
[0007] . The processing of materials is another key aspect of materials science . It refers to the processes used to shape and form materials into usable components . These processes may comprise casting, forging, extrusion, rolling and moulding. Material processing is fundamental to ensure that the synthesised materials can be transformed into specific shapes and sizes required for their final applications .
[0008] . Material characterisation is the process of analysing the physical, chemical and mechanical properties of a material . This may comprise techniques such as electron microscopy, spectroscopy, X-ray diffraction and calorimetry. Characterisation is essential in order to understand how modifications in the microscopic structure of a material influence its macroscopic properties and to verify that the material meets the specifications required for its application.
[0009] . The applications of materials science are broad and varied, covering sectors such as aerospace, automotive, electronics and biomedical . In the aerospace sector, for example, materials must be lightweight yet resistant, capable of withstanding extremetemperatures and high pressures . Advanced composites, metal alloys and ceramic materials are commonly used to construct aircraft and spacecraft components . In the automotive sector, materials must offer a balance between strength, lightness and cost . Aluminium alloys, carbon fibre composites and advanced polymers are used to improve fuel efficiency and vehicle safety.
[0010] . In the electronics sector, semiconductor materials such as silicon and germanium are fundamental for the production of electronic devices such as transistors, diodes and integrated circuits . The miniaturisation of electronic devices requires materials having specific electrical and thermal properties, and materials science plays a crucial role in the development of new materials for advanced electronics . In the biomedical sector, materials must be biocompatible and capable of interacting with biological tissues without causing adverse reactions . Biomaterials, such as biodegradable polymers and bioactive ceramics, are used to produce medical implants, prostheses and drug delivery devices .
[0011] . In the production of composite materials, one of the main objectives is to achieve optimal densif ication and high structural integrity. Composite materials, consisting of two or more distinct materials, when combined, produce a material having superior properties as compared with the individual components . However, the densif ication process, which aims to reduce the porosity within the material in order to increase its density and improve the mechanical properties, has a problem that has not yet been completely solved: the clogging of the access paths to the deepest part of the componentto be densified. This phenomenon inevitably occurs when densif ication proceeds, which necessarily concentrates in the surface layer, creating a barrier that obstructs the penetration of the densifying material towards the core of the component . Consequently, while the surface may appear densified and compact, the core of the material risks remaining porous and under-densified, seriously compromising the overall structural integrity. This imbalance between surface densif ication and internal densif ication may lead to composite materials which, although having a robust external appearance, are not capable of withstanding high loads and stresses without deforming or breaking. The high structural integrity, which is essential in order to ensure the strength and durability of the composite material, is thus compromised. Addressing this problem requires innovative solutions that allow uniform and deep densif ication, avoiding clogging of the access paths and ensuring that the densifying material effectively reaches the core of the component . Only in this way will it be possible to achieve composite materials having optimal mechanical properties and real structural integrity.
[0012] . In order to achieve these objectives, techniques such as fibre reinforcement and resin impregnation are commonly used. Fibre reinforcement involves incorporating fibres of high-strength materials, such as carbon or glass, within a resin matrix. These fibres provide strength and rigidity to the composite material, while the resin matrix distributes the loads and protects the fibres from damage . Resin impregnation is the process of saturating the fibres with a liquid resin, which is then polymerised to form a solid matrix.
[0013] . The creation of internal channels within composite structures can further improve the properties of the material, facilitating processes such as fluid flow or reduction of the overall weight . The internal channels can be used to transport cooling fluids or to reduce the weight of the material without compromising its strength. However, the creation of these channels presents significant challenges, including the prevention of channel blockage during densif ication, which can hinder the performance of the material .
[0014] . The integration of sacrificial elements to form channels represents a promising approach for overcoming these challenges . The sacrificial elements are temporary materials that are incorporated into the composite material during its manufacture and subsequently removed to leave voids or channels . However, existing methods often encounter difficulties in effectively removing these elements without compromising the integrity of the material .
[0015] . Document EP 2989343 Bl describes a method for producing cylindrical bodies using a mandrel and layers of fibres . This method provides winding layers of fibres around a mandrel in order to form a hollow cylindrical body. However, the described method does not provide the formation of specific channels other than the porosity of the materials used and does not effectively prevent the blockage of these channels during densif ication, limiting the penetration of the process and, consequently, the overall effectiveness of the densif ication itself . This may lead to non-uniform densif ication and a reduction in the mechanical properties of the final material .
[0016] . Document EP 3204661 Bl presents a similar method, againwithout the use of sacrificial fibres for the formation of channels . The absence of sacrificial fibres, however, may lead to incomplete formation of the passages suitable for carrying the densif ication process in depth, negatively affecting the densif ication and therefore the final properties of the material . Without well-defined channels, the material may have non-uniform density and reduced mechanical strength, only exploiting the porosity of the material of the semifinished body which soon becomes clogged and does not allow the inflow of further densif ication material .
[0017] . Document US 10384981 B2 describes related methods, but does not provide specific details . The lack of detailed information limits the understanding of its effectiveness in channel formation and in their use in densif ication, leaving open the question as to how truly innovative or improving it may be as compared with existing methods . Without a clear description of the processes and of the results achieved, it is difficult to evaluate the impact of this method on the production of composite materials .
[0018] . Technical problem
[0019] . Therefore, there is a clear need to develop a method that effectively incorporates sacrificial fibres in order to create internal channels, particularly within cylindrical bodies in which densif ication in depth of the cylindrical body has always proved in the past to be very complicated to achieve . This would improve densif ication by avoiding blockage of the process through clogging of the surface portions of the porosity of the semi-finished body, thus optimising the overall production process and improving the qualityof the final material . An effective method should ensure complete removal of the sacrificial elements without damaging the structure of the material, allowing the formation of well-defined channels that improve the mechanical and thermal properties of the composite material .
[0020] . In summary, materials science is a continuously evolving field that plays a crucial role in the development of new materials for advanced applications . Understanding the relationships between structure and properties of materials enables proposing materials having tailor-made characteristics in order to meet the specific needs of various industrial sectors . However, the challenges in the production of composite materials, such as densif ication and the creation of internal channels, require the development of innovative methods in order to improve the performance and quality of the final materials .
[0021] . The production of densified cylindrical bodies presents challenges in achieving optimal densif ication and structural integrity. The creation of materials having reduced porosity and improved mechanical properties remains a primary objective in the production of composite materials . Techniques such as fibre reinforcement and resin impregnation are commonly employed to achieve these obj ectives . However, the integration of internal channels within composite structures can further improve the properties of the material by facilitating processes such as fluid flow or weight reduction .
[0022] . The existing methods, as described in documents EP 2989343Bl and EP 3204661 Bl, do not effectively prevent channel blockage during densif ication, limiting the penetration of the densif ication process . The absence of sacrificial fibres in some methods may lead to incomplete formation of the channels, affecting the overall densif ication . Furthermore, the lack of detailed information in related methods, such as those potentially covered in US 10384981 B2, limits the understanding of their effectiveness in channel formation and densification.
[0023] . Solut ion
[0024] . These and other objects and advantages are achieved with a method for producing a densified cylindrical body according to claim 1, as well as a densified cylindrical body according to claim 29.
[0025] . Some advantageous embodiments are the subject matter of the dependent claims .
[0026] . The disclosed method addresses the above-mentioned problems in relation to the solutions of the prior art, by incorporating sacrificial fibres in order to create internal channels within cylindrical bodies, improving densification and preventing blockage of the densification process . This approach provides the use of sacrificial fibres that decompose in order to form channels, improving the penetration of the densification process . The method results in a more efficient production process and higher-quality final products, suitable for applications requiring high mechanical and thermal performance .
[0027] . According to one aspect of the present invention, a method for producing a densified cylindrical body, initially with internalchannels, comprises providing a winding mandrel having a predetermined external diameter; forming at least one layer of main structural fibres, referred to as non-sacrif icial fibres, for example but not necessarily having a predetermined width, which will constitute the supporting matrix of the cylindrical body; overlapping or incorporating at least one layer of fibres designed to be temporarily integrated, referred to as sacrificial fibres, above the layer of non-sacrificial fibres in order to create internal channels within the final body; or, instead of steps b) and c) , separately forming an assembly, such as a non-woven fabric composed of main structural fibres, referred to as non-sacrif icial fibres, having a predetermined length and width, mixed with fibres designed to be temporarily integrated, referred to as sacrificial fibres, in order to create internal channels within the final body; wrapping the layers of fibres around the mandrel in order to form a coaxial hollow cylindrical body, having an external diameter and an internal diameter substantially equivalent to the diameter of the mandrel; where necessary, therefore not necessarily, performing a needling process on the overlap of layers b) and c) or bl ) in order to create a three-dimensional structure of main structural fibres and sacrificial fibres; where necessary, therefore not necessarily, heating the coaxial hollow cylindrical body in order to initiate the fibre consolidation process, achieving at least a partial cross-linking of binding resin provided between the fibres and if present; decomposing the sacrificial fibres in order to form elongated channels within the cylindrical body, thus improving the penetration of the densif ication process; wherenecessary, therefore not necessarily, performing a heat treatment in order to complete the cross-linking of the binding resin, achieving a semi-finished cylindrical body; subjecting the cylindrical body to a densif ication treatment in order to improve the structure of the material and its mechanical properties, exploiting the channels left by the decomposition of the sacrificial fibres; if necessary, therefore not necessarily, removing a surface layer of the material in order to re-expose the channels created by the decomposition of the sacrificial fibres where partially or totally obstructed by the densif ication process; repeating the cycles of densif ication and removal of the surface layer until the desired degree of densif ication is achieved.
[0028] . According to another aspect, the method comprises non-sacrificial fibres which are carbon fibres, selected for their high mechanical strength and thermal stability, and impregnated with an epoxy resin before winding on the mandrel .
[0029] . According to a further aspect, the method comprises sacrificial fibres which are fibres comprising cotton fibres and / or linen fibres, alternatively synthetic fibres of polypropylene (PP) and / or polyethylene terephthalate (PET) and / or polyethylene (PE) which can dissolve with the increase in temperature for example by pyrolysis, or polyvinyl alcohol (PVA) , selected for their ability to dissolve in hot water, creating elongated channels without harmful residues .
[0030] . For example, the fibres are decomposed by carbonisation or pyrolysis . Pyrolysis is a specific form of thermal decomposition thatoccurs in the absence or under conditions of severe oxygen deficiency, typically in an inert atmosphere such as nitrogen (N2) . This process is important for the transformation of biomass and polymers into value-added products . The pyrolysis of organic materials such as natural fibres typically produces three main fractions : a carbon-rich solid fraction known as char or charcoal, a complex liquid fraction called bio-oil or tar, and a gaseous fraction known as syngas, composed mainly of CO, CO2, H2 and light hydrocarbons . Operating temperatures for pyrolysis are generally above 300°C . There are different pyrolysis regimes (slow, conventional, rapid) , characterised by different heating rates and maximum temperatures, which significantly influence the relative yield of the three fractions . Carbonisation is a process, often carried out by pyrolysis, specifically aimed at maximising the production of the carbon-rich solid residue, the char. This carbonaceous residue is typically black, porous and fragile . The intrinsic fragility of char is directly connected to the phenomenon of "pulverisation" mentioned in the initial application: the original polymeric structure, flexible and resistant, is converted into a rigid carbonaceous structure that breaks easily.
[0031] . Thermal Decomposition of Cotton Fibres
[0032] . Cotton, being composed predominantly of cellulose (often more than 90% by dry weight) , shows thermal behaviour dominated by the degradation reactions of this polymer . Thermogravimetric analysis (TGA) and differential scanning calorimetry (DSC) are techniques commonly used to study these transformations .
[0033] . A. Phases of Thermal Degradation
[0034] . Thermal degradation of cotton can be divided into several main phases, which occur at specific temperature ranges :
[0035] . Phase 1 : Dehydration (T < ~150°C) : This initial phase involves the loss of water physically adsorbed on the surface of the fibres and bound through hydrogen bonds to the cellulose chains . In TGA, a slight weight loss is observed, typically in the order of 5-8%, which is completed around 100-120°C. Cotton is considered stable up to 100°C, but prolonged exposure to 120°C can begin to cause slight yellowing. At 150°C, water vapour itself may begin to chemically attack the cellulose molecule . This phase corresponds to Region I identified in some TGA studies (37-150°C) . Although it does not involve significant structural breakdown, the removal of water may influence the kinetics of the subsequent decomposition reactions .
[0036] . Phase 2 : Primary Decomposition / Pyrolysis (T ~ 150°C -425°C) : This is the phase in which the main structural degradation of cellulose occurs . Marked decomposition begins around 150°C . In an inert atmosphere (pyrolysis) , the dominant process is the depolymerisation of cellulose, which involves the breaking of the p- ( 1^4 ) -glycosidic bonds between the glucose units . This reaction leads to the formation of volatile anhydrosugars, the main component of which is levoglucosan, together with other products such as water, CO, CO2 and light hydrocarbons . This phase is characterised by the fastest and most significant weight loss observed in TGA, typically between 225°C and 425°C (TGA Region II ) . The onset temperature of this rapid decomposition (TGA onset) in an inert atmosphere is reported around 318-333°C, while the maximum weight loss rate (DTG peak, Tmax)typically occurs between 340°C and 370°C . It is during this phase that the fibre loses its structural integrity and the carbonisation process begins, leading to the formation of a fragile solid residue .
[0037] . Phase 3 : Char Formation and Oxidation (T > ~400°C) : At temperatures higher than those of the primary decomposition, the reactions continue leading to the formation of a more stable carbonaceous residue, the char. In an inert atmosphere (N2 ) , this char undergoes only a slow additional weight loss at very high temperatures . Decomposition is considered substantially completed at around 600°C, leaving a small carbonaceous residue . However, in the presence of oxygen (air) , char formed in the previous phase undergoes an exothermic oxidation reaction (flameless combustion, glowing) . This process typically occurs in the range 425-600°C (TGA Region III) , with reaction peaks observed around 480-530°C. This oxidation leads to a further and almost complete loss of mass, with minimal residues (mainly inorganic ashes) observed at 700-800°C. The presence of oxygen therefore introduces a second main phase of degradation at high temperature, absent in an inert atmosphere .
[0038] . The temperature at which cotton "pulverises" therefore corresponds to the window of the primary decomposition (Phase 2) , particularly in the range 300-400°C, where the cellulosic structure is destroyed and converted into a fragile char.
[0039] . Thermal Decomposition of Linen Fibres
[0040] . Linen is a lignocellulosic fibre, which means that in addition to cellulose (which still constitutes the majority component thereof, ~60-75%) , it contains significant quantities of hemicellulose(~15— 20% ) and lignin (~2- 5%, but this may vary) , in addition to pectins and other impurities . This more complex composition as compared with cotton is reflected in a multi-stage thermal decomposition profile .
[0041] . A. Phases of Degradation and Comparison with Cotton
[0042] . Also for linen, the general process includes dehydration, primary decomposition of the polymers and char f ormation / oxidation . However, the primary decomposition is more articulated:
[0043] . Phase 1 : Dehydration (T < ~150°C) : Similarly to cotton, loss of adsorbed water occurs, with an initial weight loss in TGA.
[0044] . Phase 2a: Hemicellulose / Pectin Decomposition (T ~ 200°C -350°C) : Due to their lower intrinsic thermal stability (amorphous, branched structure) , the hemicellulose and pectins present in linen begin to degrade at significantly lower temperatures as compared with cellulose . The onset of significant thermal decomposition for raw linen (TGA onset, TO) is in fact reported around 209-215°C. This event often appears as a shoulder or a distinct peak in the DTG curve (derivative of TGA) in the range 250-350°C, preceding the main cellulose peak. This is the key difference as compared with cotton, which does not possess these components in significant quantities .
[0045] . Phase 2b : Cellulose Decomposition (T ~ 300°C - 400°C) : The cellulosic component of linen subsequently degrades, in a temperature range similar to that observed for cotton. The main DTG peak, attributed to the decomposition of cellulose in linen, typically occurs around 350-370°C. However, for very clean linen samples (where hemicellulose and pectins have been removed) , this peak can shift to higher temperatures, up to 392 °C .
[0046] . Phase 2c: Lignin Decomposition (T ~ 200°C - 500°C) : Lignin, while beginning to decompose at relatively low temperatures (~200°C) , degrades very slowly and over an extremely wide temperature range, overlapping both the decomposition of hemicellulose and that of cellulose . Its decomposition contributes significantly to the formation of the carbonaceous residue (char) at high temperatures .
[0047] . Phase 3 : Char Formation / Oxidation (T > ~400°C) : As for cotton, a carbonaceous residue is formed. However, due to the contribution of lignin, the quantity of char produced by the pyrolysis of linen tends to be greater than that produced by cotton under the same conditions . In the presence of air, this char will undergo oxidation at high temperatures .
[0048] . Linen, therefore, begins its structural thermal degradation process at considerably lower temperatures as compared with cotton (~210°C vs ~320°C) , due to the presence of less stable components such as hemicellulose . This has direct implications on the temperature limits usable for the processing and use of untreated linen.
[0049] . Cotton and linen fibres pulverise by carbonisation when heated to temperatures sufficiently high to cause thermal decomposition of their main polymeric components (in particular cellulose) under conditions of limited oxygen. This process, pyrolysis, transforms the flexible fibrous structure into an intrinsically fragile carbonaceous residue (char) . The critical temperature threshold for the significant establishment of this phenomenon is generally above 350-400°C for both fibres, corresponding to the interval of rapid decomposition of cellulose . Raw linen willbegin to show signs of degradation at lower temperatures (~210°C) due to hemicellulose, but the complete loss of integrity associated with the carbonisation of the main structure occurs at higher temperatures, similar to those of cotton.
[0050] . According to another aspect, the method comprises the needling process in step dl ) , performed using needles with multiple barbs in order to ensure effective three-dimensional interweaving between the non-sacrif icial and sacrificial fibres . This process is specifically provided in cases where a resin and / or resin preimpregnated fibres are not used, since the presence of resin or preimpregnated fibres would make it impossible to perform the needling step . Needling, in fact, requires the fibres to be free to move and interweave under the action of the needles, a result that cannot be achieved if the fibres are already impregnated or consolidated with resin. Therefore, this technique represents an ideal solution for creating a robust and cohesive three-dimensional structure in the absence of resins, while at the same time ensuring the flexibility necessary for the subsequent steps of the process .
[0051] . According to a further aspect, the method comprises heating in step e) conducted at a temperature between 80 °C and 120 °C in order to facilitate the pre-cross-linking of the resin before the final dens ificat ion .
[0052] . According to another aspect, the method comprises the heat treatment in step g) followed by controlled cooling in order to avoid internal stresses in the semi-finished cylindrical body.
[0053] . According to a further aspect, the method comprises thedensif ication treatment in step h) achieved by infiltration of a ceramic matrix that fills the residual porosities, improving the mechanical and thermal properties of the body.
[0054] . According to another aspect, the method comprises the removal of the surface layer in step i) carried out by precision milling in order to ensure optimal access to the internal channels for the subsequent densif ication cycle .
[0055] . According to a further aspect, the method comprises the decomposition process of the sacrificial fibres in step f ) which comprises the application of an alkaline solution in order to facilitate the dissolution of the PVA fibres .
[0056] . According to another aspect, the method comprises the cycles of densif ication and removal of the surface layer in step j ) repeated at least three times in order to ensure uniform and complete densif ication of the cylindrical body.
[0057] . According to a further aspect, the method comprises the final cylindrical body intended for use in disc brake applications, exploiting its optimised structure in order to withstand high thermal and mechanical stresses .
[0058] . According to another aspect, the method comprises sacrificial fibres made of polylactic acid (PLA) , designed to thermally decompose at temperatures above 150°C, facilitating the formation of internal channels .
[0059] . According to a further aspect, the method comprises sacrificial fibres composed of cellulose, selected for their ability to be dissolved by applying a specific enzyme after the formation ofthe cylindrical body.
[0060] . According to another aspect, the method comprises sacrificial fibres made of polyvinylpyrrolidone (PVP) , designed to be removed through washing with a saline solution, creating channels without residues .
[0061] . According to a further aspect, the method comprises sacrificial fibres made of polyurethane, which can be decomposed by applying heat in an inert environment, ensuring the formation of precise channels .
[0062] . According to another aspect, the method comprises the dissolution process of the sacrificial fibres of cellulose in step f ) , which comprises the use of an organic solvent, such as acetone, for efficient removal .
[0063] . According to a further aspect, the method comprises sacrificial fibres composed of polyethylene glycol (PEG) , designed to dissolve in hot water, facilitating the creation of smooth internal channels .
[0064] . According to another aspect, the method comprises the method of decomposition of the sacrificial fibres of PLA in step f ) , which comprises an accelerated composting process, combining heat and humidity for rapid removal .
[0065] . According to a further aspect, the method comprises sacrificial fibres made of polyacrylonitrile (PAN) , designed to be eliminated through controlled oxidation, leaving defined channels in the cylindrical body.
[0066] . According to another aspect, the method comprisessacrificial fibres made of silicone rubber, designed to be removed by pyrolysis, ensuring the formation of clean internal channels .
[0067] . According to a further aspect, the invention further proposes a densified cylindrical body comprising a cylindrical core made of layers of main structural fibres, referred to as non-sacrificial fibres, which form the supporting matrix of the cylindrical body, providing mechanical strength and thermal stability; a densified carbon matrix filling the residual porosities and the channels previously formed by layers of sacrificial fibres, improving the mechanical and thermal properties of the cylindrical body and conferring a uniform and solid structure to the body; a surface processing obtained through the controlled removal of a surface layer of the cylindrical body, optimising the surface for specific applications; wherein the cylindrical body is designed for applications requiring high mechanical strength, thermal stability and structural integration, such as in high-performance braking systems .
[0068] . According to another aspect, the cylindrical body comprises non-sacrif icial fibres arranged in a cross-layered configuration in order to improve resistance to bending and torsion.
[0069] . According to a further aspect, the cylindrical body comprises the densified carbon matrix comprising graphene nanoparticles in order to further increase thermal conductivity and mechanical strength.
[0070] . According to another aspect, the cylindrical body comprises the surface processing comprising an anodisation treatment in orderto improve corrosion resistance .
[0071] . According to a further aspect, the cylindrical body comprises non-sacrif icial fibres made of a mixture of high-strength carbon fibres and aramid fibres in order to optimise impact absorption properties .
[0072] . According to another aspect, the cylindrical body comprises the densified carbon matrix further reinforced with silicon carbide fibres in order to improve hardness and wear resistance .
[0073] . According to a further aspect, the cylindrical body comprises the surface processing performed by means of a sandblasting finishing process in order to obtain a textured surface that improves adhesion in mechanical applications .
[0074] . According to another aspect, the cylindrical body comprises sacrificial fibres designed to leave an internal three-dimensional structural pattern that contributes to the reinforcement of the densified carbon matrix.
[0075] . According to a further aspect, the cylindrical body comprises the densified carbon matrix obtained through a vapour-phase carbon infiltration process, ensuring a uniform and defect-free structure .
[0076] . According to another aspect, the cylindrical body comprises the surface processing comprising a ceramic coating in order to improve resistance to high temperatures and oxidation.
[0077] . According to a further aspect, the cylindrical body comprises non-sacrif icial fibres treated with a polymer coating in order to improve compatibility with the carbon matrix and reducedelamination .
[0078] . SOME TECHNICAL EFFECTS OF THE INVENTION
[0079] . The proposed method introduces the use of sacrificial fibres in order to create internal channels within a cylindrical body, improving the densif ication process by preventing clogging. This arrangement allows better penetration of the densif ication materials, addressing a significant limitation in existing methods .
[0080] . By forming layers of non-sacrif icial fibres as the main structure and overlapping them or integrating them with sacrificial fibres, the method ensures that the channels are effectively created and uniformly distributed within the body that is created once the sacrificial fibres have decomposed. This layered structure is wrapped around a mandrel, forming a coaxial hollow cylindrical body, which is crucial for maintaining the desired dimensions and structural integrity during processing.
[0081] . The decomposition of the sacrificial fibres in order to form elongated and branched channels within the cylindrical body facilitates the densif ication process, allowing more uniform and complete filling of the residual voids . This results in a semifinished cylindrical body having improved mechanical properties and reduced porosity.
[0082] . The repeated cycles of densif ication and removal of the surface layer ensure that the channels remain accessible and functional, contributing to the efficiency and overall quality of the final product . This iterative process allows the desired level of densif ication to be achieved, making the method suitable for high-performance applications .
[0083] . The organisation of the non-sacrif icial fibres forming the core of the cylindrical body provides mechanical strength and thermal stability, ensuring the structural integrity of the densified cylinder. This configuration supports the entire framework, allowing the body to withstand high mechanical and thermal stresses, which is essential for high-performance applications such as braking systems .
[0084] . The inclusion of a densified carbon matrix filling the residual porosities and the channels formed by the sacrificial fibres improves the mechanical and thermal properties of the cylindrical body. This results in a uniform and solid structure, improving the ability of the material to manage stress and heat, which is crucial for applications requiring high durability and performance .
[0085] . The controlled removal of a surface layer optimises the surface for specific applications, ensuring that the final product meets precise functionality and performance requirements . This process allows the surface characteristics to be refined, which are critical in applications wherein the surface properties significantly influence performance .
[0086] . ALTERNATIVE EMBODIMENTS
[0087] . In one embodiment, the method for producing a densified cylindrical body with internal channels provides the use of carbon fibres as a non-sacrif icial structural component, selected for their high mechanical strength and thermal stability.
[0088] . These fibres are impregnated with an epoxy or phenolic resin in order to improve adhesion and structural integrity.
[0089] . In another embodiment, the sacrificial fibres are made of polyvinyl alcohol (PVA) , which can be dissolved in hot water in order to create elongated channels without leaving harmful residues .
[0090] . Alternatively, the sacrificial fibres could be composed of polylactic acid (PLA) , designed to thermally decompose at temperatures above 150°C, facilitating the formation of internal channels .
[0091] . The process may also comprise a needling technique in order to interweave the non-sacrif icial and sacrificial fibres, creating a robust three-dimensional structure . The cylindrical body is then subj ected to a controlled heating process in order to partially cure the resin, followed by decomposition of the sacrificial fibres in order to form the channels .
[0092] . According to an implementation variant, a subsequent densif ication treatment, possibly involving infiltration of a ceramic matrix, improves the mechanical and thermal properties of the material . The surface layer of the material is then precision milled in order to expose the channels, ensuring optimal access for further densif ication cycles .
[0093] . This method can be adapted for various applications, such as high-performance braking systems, by adjusting the materials of the fibres and the processing conditions in order to meet specific performance requirements .
[0094] . In one embodiment, the densified cylindrical body is constructed using non-sacrif icial fibres made of high-strength carbon fibres, which provide excellent mechanical strength and thermal stability .
[0095] . These fibres are arranged in a cross-layered configuration in order to improve the resistance of the body to bending and torsion. The carbon matrix is further reinforced with graphene nanoparticles, significantly increasing thermal conductivity and mechanical strength .
[0096] . In another embodiment, the surface of the cylindrical body undergoes an anodisation process, improving the corrosion resistance of the surface, making the cylindrical body suitable for harsh environments .
[0097] . Alternatively, the non-sacrif icial fibres could be a mixture of carbon and aramid fibres, optimising impact absorption properties . The carbon matrix can also be reinforced with silicon carbide fibres in order to improve hardness and wear resistance . Furthermore, the surface could be finished with a sandblasting process in order to create a textured surface, improving adhesion in mechanical applications .
[0098] . In another embodiment, the sacrificial fibres are designed to leave an internal three-dimensional structural pattern, contributing to the reinforcement of the carbon matrix, obtained through a vapour-phase carbon infiltration process, ensuring a uniform and defect-free structure . The surface can also be coated with a ceramic layer in order to improve resistance to high temperatures and oxidation, making the cylindrical body ideal for high-performance braking systems .
[0099] . DEFINITIONS
[0100] . non-sacrif icial fibres" in light of the mentioned priorart, it is important to clarify their role and their distinctive characteristics as compared with sacrificial fibres . The "non-sacrificial fibres" can be defined as follows :
[0101] . Non-Sacrif icial Fibres :
[0102] . Role in the Process : Non-sacrif icial fibres constitute the main structure of the cylindrical body. They are intended to remain an integral part of the final product and are not removed during any step of the production process, except in order to obtain external working surfaces having the desired dimensions and tolerances .
[0103] . Material Characteristics : These fibres are generally made of materials that confer mechanical strength, thermal stability and chemical compatibility with the resins used in the impregnation and densif ication process .
[0104] . Examples of Materials : They may comprise carbon fibres, glass fibres or other high-performance fibres known for their ability to contribute to the structural properties of the final body.
[0105] . Comparison with Sacrificial Fibres : Unlike sacrificial fibres, non-sacrif icial fibres are not designed to be removed and do not participate in the formation of internal channels . Instead, they provide the supporting matrix of the cylindrical body.
[0106] . In the context of the patent, "non-sacrif icial fibres" refers to the primary structural fibres used in the production of a densified cylindrical body. These fibres form the main framework of the cylinder and remain part of the final product . Unlike sacrificial fibres, non-sacrif icial fibres are not removed during the manufacturing process .
[0107] . The non-sacrif icial fibres are typically made of materials that provide mechanical strength, thermal stability and chemical compatibility with the resins used in the impregnation and densif ication process . Examples of such materials comprise carbon fibres, glass fibres and other high-performance fibres known for their ability to improve the structural properties of the final body.
[0108] . These fibres serve as the supporting matrix of the cylindrical body, providing support and stability. In the patent, the non-sacrif icial fibres are contrasted with sacrificial fibres, designed to be removed in order to create internal channels . The non-sacrificial fibres, on the other hand, contribute to the overall strength and durability of the final product .
[0109] . sacrificial fibres" are a crucial element in the innovative method for creating internal channels within a densified cylindrical body. Here is a detailed definition of these fibres, with examples and dissolution methods :
[0110] . Sacrificial Fibres :
[0111] . Role in the Process : The sacrificial fibres are temporarily incorporated into the cylindrical body during the manufacturing process . Their main purpose is to create empty structures or channels within the finished material .
[0112] . Material Characteristics : These fibres are made of materials designed to be easily removed or decomposed during or after the manufacture of the final product . This removal process is crucial for creating the desired channels .
[0113] . Examples of Materials :
[0114] . Cotton and / or linen fibres : They can be pulverised by pyrolysis .
[0115] . PVA fibres (polyvinyl alcohol) : They can be dissolved in water or aqueous solutions .
[0116] . PLA fibres (polylactic acid) : They can be decomposed through heat in a controlled environment .
[0117] . Cellulose fibres : They can be dissolved using specific chemical solvents or enzymes .
[0118] . Dissolution Processes :
[0119] . Chemical Dissolution: Use of specific solvents that dissolve or break the sacrificial fibres without damaging the non-sacrificial fibres .
[0120] . Thermal Dissolution: Application of heat to thermally decompose the sacrificial fibres, taking care not to compromise the structure of the material .
[0121] . Mechanical Dissolution: In some cases, the sacrificial fibres can be removed by mechanical actions, such as milling or abrasion, if combined with other dissolution methods .
[0122] . Advantages of the Use of Sacrificial Fibres : Creation of internal channels that can improve the penetration of the densif ication process and improve the functional properties of the final product, such as weight reduction or the creation of paths for fluids or air.
[0123] . In the context of the patent, the term "sacrificial fibres" refers to temporary fibres used in the production of a densified cylindrical body. These fibres perform a temporary role during theproduction process . They are incorporated into the cylindrical structure in order to create empty channels within the final material .
[0124] . The sacrificial fibres are made of materials designed to be easily removed or decomposed during or after the manufacture of the final product . This removal process is necessary to form the desired channels . Examples of materials used for the sacrificial fibres comprise cotton and / or linen fibres which can dissolve with the increase in temperature for example by carbonisation, or polyvinyl alcohol (PVA) , which can dissolve in water, polylactic acid (PLA) , which decomposes with heat, and cellulose, which can be dissolved using specific solvents or enzymes .
[0125] . The process of removing these fibres may involve chemical dissolution, thermal decomposition or mechanical actions . The creation of internal channels through the use of sacrificial fibres improves the densif ication process and can improve the functional properties of the final product, such as weight reduction or the creation of paths for fluids or air.
[0126] . A "densified cylindrical body" refers to a cylindrical structure that has undergone a process to increase the density of the structure itself . This process involves compacting the material to reduce porosity and improve the mechanical properties of the cylindrical structure, such as strength and stability.
[0127] . In the context of the patent, the method involves the use of both sacrificial and non-sacrif icial fibres . The sacrificial fibres create internal channels by being removed or decomposing during production. These channels improve the densif ication process byallowing better penetration of the materials used to fill any residual voids .
[0128] . The non-sacrif icial fibres form the main structure of the cylinder, providing structural integrity and remaining part of the final product . The combination of these fibres results in a densified cylindrical body with improved functional properties, suitable for applications requiring high mechanical and thermal performance .
[0129] . The "process for decomposing the sacrificial fibres" refers to the method used to remove or decompose the sacrificial fibres incorporated in a cylindrical body during the production thereof . These fibres are designed to be temporary and are included in order to create internal channels within the final material . During or after the production process, the sacrificial fibres undergo decomposition or removal, which are necessary to form the desired channels . This process may involve different techniques :
[0130] . Chemical dissolution: This method uses specific solvents to dissolve the sacrificial fibres without affecting the structural fibres . For example, polyvinyl alcohol (PVA) fibres can dissolve in water or in aqueous solutions .
[0131] . Thermal decomposition: This technique applies heat to decompose the sacrificial fibres . Thermal decomposition represents one of the most effective and preferable techniques for the removal of sacrificial fibres, thanks to the numerous advantages it offers . This process uses heat to decompose the sacrificial fibres in a controlled and precise manner. For example, polylactic acid (PLA) fibres can be easily decomposed when exposed to specific temperaturesin a controlled environment . Among the main advantages of thermal decomposition is its ability to ensure uniform and complete removal of the sacrificial fibres, without leaving undesired residues that could compromise the quality of the final product, except carbon powders which contribute to the subsequent densif ication step. Furthermore, the process is highly scalable and can be easily integrated into industrial production lines, making it ideal for large-scale applications . A further benefit is represented by the possibility of precisely adjusting the temperature and time parameters, adapting the process to the specific characteristics of the fibres used. This level of control minimises the risk of damaging the surrounding materials, preserving the structural integrity of the product . Thermal decomposition is also an environmentally sustainable solution, since many sacrificial fibres, such as PLA, are biodegradable and decompose into non-toxic by-products, reducing the environmental impact of the process . Finally, the absence of chemical solvents or aggressive agents makes this technique safer for operators and simpler to manage as compared with other removal methods . In summary, thermal decomposition stands out as the preferable choice for the removal of the sacrificial fibres, combining efficiency, precision, sustainability and safety in a single process .
[0132] . Mechanical actions : In some cases, mechanical methods such as milling or abrasion can assist in the removal of the sacrificial fibres, often in combination with other decomposition techniques .
[0133] . The removal of these fibres creates internal channels that improve the densif ication process, improving the properties of thematerial by allowing better penetration of the materials used to fill any residual voids .
[0134] . The "needling process" refers to a technique used in the production of composite materials, in particular in the context of creating a three-dimensional structure from layers of fibres . This process provides the use of needles to mechanically interweave the fibres, improving the structural integrity and cohesion of the material .
[0135] . In this method, needles provided with hooks penetrate through the layers of fibres, pulling some fibres from one layer to another . This action creates a more integrated and robust structure by interweaving the fibres, which can improve the mechanical properties of the final product .
[0136] . The needling process is particularly useful when combining different types of fibres, such as non-sacrif icial fibres and sacrificial fibres, in order to ensure that they remain firmly in position during the subsequent production steps . This technique can improve the overall strength and stability of the composite material, making it suitable for applications requiring high performance and durability.
[0137] . The term "densification treatment" refers to a process used to increase the density of a cylindrical body. This process involves compacting the material to reduce porosity and improve the mechanical properties of the structure, such as strength and stability.
[0138] . In the context of the patent, the densification treatment takes place after the formation of the cylindrical body, whichcomprises both sacrificial and non-sacrif icial fibres . The sacrificial fibres create internal channels by being removed or decomposed during production. These channels facilitate the densif ication process by allowing better penetration of the materials used to fill any residual voids .
[0139] . The densif ication treatment may involve various techniques, such as the application of pressure, heat or the introduction of additional materials to fill the voids within the structure . This process aims to improve the integrity and overall performance of the cylindrical body, making it suitable for applications requiring high mechanical and thermal performance .
[0140] . The phrase "Removing a surface layer of the material in order to re-expose the channels created by the decomposition of the sacrificial fibres" refers to a specific step in the production process of a densified cylindrical body. This step provides the removal of a thin outer layer of material from the surface of the cylindrical body. The purpose of this removal is to reveal or reopen the internal channels that have been formed by the decomposition of the sacrificial fibres .
[0141] . During the production process, the sacrificial fibres are incorporated into the cylindrical structure . These fibres are designed to decompose or be removed, creating empty channels within the material . With the densif ication step, these channels may become partially or completely obstructed by the densif ication process .
[0142] . By removing the surface layer, the process ensures that these channels are accessible again. This step is important formaintaining the functionality of the channels, which can be used for various purposes, such as increasing the depth and homogeneity of densif ication . The removal is typically carried out through precision techniques such as milling or abrasion, ensuring that the channels are optimally exposed for further processing or uses .
[0143] . Figures
[0144] . Further features and advantages of the invention will appear from the following description of preferred examples of embodiment thereof, given by way of non-limiting indication, with reference to the accompanying figures in which:-figure 1 schematically illustrates in axonometry a winding step around a winding mandrel of a first layer of non-sacrif icial fibres and of at least one layer of sacrificial fibres; this step represented herein is only exemplary, since the non-sacrif icial fibres and the sacrificial fibres can be immersed in a matrix, for example a resin matrix, and can be previously interwoven or overlapped or entangled in a non-woven fabric and form a single winding layer around the winding mandrel;-figure 2 illustrates an enlargement of a sector of the hollow cylindrical body just wound wherein, merely by way of example, four alternating layers of non-sacrif icial fibres and sacrificial fibres are schematically represented, wherein each fibre is immersed in a matrix;-figure 3 schematically represents in axonometry a further step wherein the rotation of the mandrel synchronised with a needling tool can be seen, having an undulating movement suitable for causing itsmultiple needles to penetrate radially into the hollow cylindrical body and allowing the barbs of the needles to needle the fibres and move them radially, creating a three-dimensional structure of non-sacrificial and sacrificial fibres;-figure 4 schematically illustrates in axonometry a cutting step of a hollow cylindrical body extracted from the winding mandrel, wherein the longitudinally extended hollow cylindrical body is cut into "rings" of the desired sizes in order to make a semi-finished hollow cylindrical body;-figure 5 schematically represents in axonometry a step of immersion of the semi-finished hollow cylindrical body in a bath for dissolving the sacrificial fibres, a bath which is schematically represented herein and can have a different reaction fluid according to the material of the sacrificial fibres, from hot water, or alkaline solution, or saline solution, or organic solvent, so as to dissolve or disintegrate or dissolve the sacrificial fibres and create continuous or substantially continuous internal channels in an inlet network for densif ication;-figure 6 schematically illustrates in axonometry a step of heating the semi-finished cylindrical body in an oven for crosslinking the matrix, for example resin; this step is usually provided before the step of figure 5, but according to the material of the matrix it could also be provided afterwards; this step can occur in air but also in a controlled atmosphere environment, and in this case the inflow of a fluid for controlling the internal atmosphere of the oven is provided;-figures 7 and 8 schematically represent in axonometry two densif ication steps ( figure 8 and removal of a surface layer (figure 7) which can be performed recursively, providing a densif ication step in a suitable oven with a controlled environment of the semi-finished hollow cylindrical body and subsequently a step of removing a surface layer obstructing the internal channels due to densif ication; then subsequently a densif ication step and then a removal step, and so on until a densified cylindrical body having the desired characteristics is obtained; in this densif ication step the internal environment of the oven is supplied with an inflow of densifying material, for example a densif ication gas or liquid, gas or liquid which will penetrate into the semi-finished cylindrical body as well as into the sponge-like matrix also thanks to the internal channels obtained from the dissolution or disintegration of the sacrificial fibres;
[0145] . f igure 9 schematically represents in axonometry a step of finishing the external surface of the densified cylindrical body into a finished product .
[0146] . Description of some examples of preferred embodiment
[0147] . According to a general embodiment, the method for producing a densified cylindrical body 1 comprises the following steps : providing a winding mandrel 2 with a predetermined external diameter d; forming at least one layer of main structural fibres, referred to as non-sacrif icial fibres 3, which will constitute a component of the supporting matrix of the cylindrical body 1 ; overlapping at least one layer of fibres designed to be temporarily integrated, referred to as sacrificial fibres 4, interposed or integrated into the layer of non-sacrificial fibres 3 to create, when these sacrificial fibres 4 are decomposed, temporary internal channels 5 within the body before densif ication 7 ; or, instead of steps b) and c) , separately forming an assembly, such as a non-woven fabric composed of main structural fibres, referred to as non-sacrif icial fibres 3, mixed with fibres designed to be temporarily integrated, referred to as sacrificial fibres 4, to create temporary internal channels 5 within the body 7; wrapping said at least one layer of non-sacrif icial fibres 3 around the mandrel 2 to form a hollow cylindrical body 6 coaxial to the mandrel 2, having a predetermined external diameter D and a predetermined internal diameter d, wherein said internal diameter d is substantially equal to the diameter of the mandrel d; decomposing the sacrificial fibres 4 to form elongated internal channels 5 within the cylindrical body 7; subjecting the cylindrical body 7 to a densif ication treatment to improve the material structure and its mechanical properties, utilizing the internal channels 5 left by the decomposition of the sacrificial fibres 4 to densify the cylindrical body in depth, rendering it a densified cylindrical body 1.
[0148] . According to a general embodiment, a densified cylindrical body 1 comprises a cylindrical core consisting of layers of main structural fibres, referred to as non-sacrif icial fibres 3, which form the supporting matrix of the cylindrical body, providing mechanical strength and thermal stability; a densified carbon matrix filling the residual porosities and channels 5 previously formed by layers of sacrificial fibres 4 decomposed before densif ication, improving the mechanical and thermal properties of the cylindrical body andconferring a uniform and solid structure to the body; a surface processing obtained through the controlled removal of a surface layer 20 of the cylindrical body, optimizing the surface for specific applications .
[0149] . The invention has a series of significant advantages that derive from the implementation of essential features in the production process of the densified cylindrical body. First of all, the use of a winding mandrel is crucial to ensure that the cylindrical body maintains perfect coaxiality and high dimensional precision. This is fundamental to ensure that the final product meets the standards required for high-performance applications, where precision is of primary importance .
[0150] . The non-sacrif icial fibres, which constitute the supporting matrix of the body, are selected for their ability to provide mechanical strength and thermal stability. These fibres, often made from materials such as carbon, are impregnated with resins that improve their structural integrity, contributing to forming a robust core resistant to mechanical and thermal stresses .
[0151] . An innovative aspect of the invention is the integration of the sacrificial fibres . These fibres, designed to be temporary, are incorporated into the cylindrical body during the winding step. Once decomposed, they create internal channels that are essential for the densif ication process . These channels significantly improve the penetration of the densif ication materials, allowing a more uniform and complete filling of the residual porosities . This not only accelerates the densif ication process, but also improves itseffectiveness, resulting in a cylindrical body having superior mechanical properties and reduced porosity.
[0152] . The winding around the mandrel not only ensures the formation of a hollow cylindrical body with precise dimensions, but also facilitates the subsequent decomposition of the sacrificial fibres . The formation of internal channels through the decomposition of the sacrificial fibres is a key step that allows optimization of the densif ication treatment . This treatment, which may comprise the infiltration of a ceramic matrix, further improves the mechanical and thermal properties of the cylindrical body, ensuring a uniform and solid structure .
[0153] . In summary, the invention not only introduces an innovative method for producing densified cylindrical bodies, but does so by improving each step of the process, from the initial dimensional precision to the final densif ication, ensuring that the final product is suitable for applications requiring high mechanical and thermal performance .
[0154] . Furthermore, advantages of each essential feature comprise : the cylindrical core provides mechanical strength and thermal stability essential for high-performance applications . The densified carbon matrix further improves the mechanical and thermal properties, ensuring a uniform and solid structure . An important aspect is the improved and rapid densif ication achieved thanks to the internal channels left free by the dissolved or disintegrated sacrificial fibres . These channels facilitate the penetration of the densif ication materials, allowing a more uniform and complete filling, which resultsin a cylindrical body having superior mechanical properties and reduced porosity. The surface processing optimizes the surface for specific applications, improving the functionality and performance of the cylindrical body.
[0155] . According to a further embodiment, after step d) the following step is provided: performing on the overlap of layers b) and c) or bl) a needling process, by means of a needling tool 8, to create a three-dimensional structure of main structural fibres 3 and sacrificial fibres 4. This process improves the structural integrity of the cylindrical body.
[0156] . According to a further embodiment, after step d) or dl ) the following step is provided: heating the hollow cylindrical body 6 or 9 to initiate the consolidation process of the non-sacrif icial fibres 3, obtaining at least a partial cross-linking of a binding resin 10 placed around said fibres . This step improves the cohesion of the material .
[0157] . According to a further embodiment, the decomposition of the sacrificial fibres 4 is specified to improve the penetration of gas or liquid 11 of the subsequent densif ication process . This improves the effectiveness of the densif ication treatment .
[0158] . According to a further embodiment, after step f) the following step is provided: performing a heat treatment to complete the cross-linking of the binding resin 10, obtaining a semi-finished cylindrical body 9. This ensures the stability of the body before the final densif ication .
[0159] . According to a further embodiment, after step h) thefollowing step is provided: removing a surface layer 12 of the material to re-expose the channels 5 created by the decomposition of the sacrificial fibres 4 where partially or totally obstructed by the densif ication process . This ensures the accessibility of the channels for further densif ication cycles .
[0160] . According to a further embodiment, after step h) the following step is provided: repeating the cycles of densif ication and removal of the surface layer 12 until the desired degree of densif ication is achieved. This ensures uniform and complete densif ication .
[0161] . According to a further embodiment, said step dl) is modified as follows : performing on the overlap of layers b) and c) or bl) a radial needling process 8 to create a three-dimensional structure 13 of main structural fibres or non-sacrif icial fibres 3 and sacrificial fibres 4. This improves the cohesion of the material .
[0162] . According to a further embodiment, in said step b) , at least one layer of main structural fibres or non-sacrif icial fibres 3 is formed with dimensions such as to produce, with the subsequent step d) , a hollow cylindrical body 6 with dimensions greater in axial extension than a finished product, so that after step d) or after step h) , it is cut, with a cutting tool 14, to a desired axial dimension in a semi-finished product 9. This allows obtaining a final product with the desired dimensions .
[0163] . According to a further embodiment, the non-sacrif icial fibres 3 are carbon fibres, selected for their high mechanical strength and thermal stability, and are impregnated with an epoxyresin 10 before winding on the mandrel . This improves the structural integrity of the body.
[0164] . According to a further embodiment, the sacrificial fibres 4 are polyvinyl alcohol PVA fibres, selected for their ability to dissolve in hot water, creating elongated channels without harmful residues . This ensures the cleanliness of the channels .
[0165] . According to a further embodiment, the needling process 8 in step dl) is performed using needles 15 with multiple barbs to ensure effective three-dimensional interweaving between the non-sacrificial fibres 3 and sacrificial fibres 4. This improves the cohesion of the material .
[0166] . According to a further embodiment, the heating in step e) is conducted at a temperature between 80°C and 120°C to facilitate the pre-cross-linking of the resin 10 before the final densif ication . This optimizes the consolidation process .
[0167] . According to a further embodiment, the heat treatment in step g) is followed by controlled cooling to avoid internal stresses in the semi-finished cylindrical body 9. This improves the stability of the body.
[0168] . According to a further embodiment, the densif ication treatment in step h) is achieved by infiltration of a ceramic matrix that fills the residual porosities, improving the mechanical and thermal properties of the body. This increases the strength and durability of the body.
[0169] . According to a further embodiment, the removal of the surface layer 12 in step i) is carried out by precision milling toensure optimal access to the internal channels 5 for the subsequent densif ication cycle . This ensures the functionality of the channels .
[0170] . According to a further embodiment, the decomposition process of the sacrificial fibres 4 in step f) comprises the application of an alkaline solution 16 to facilitate the dissolution of the PVA fibres . This improves the efficiency of the removal of the sacrificial fibres .
[0171] . According to a further embodiment, the cycles of densif ication and removal of the surface layer 12 in step j ) are repeated at least three times to ensure uniform and complete densif ication of the cylindrical body 1. This ensures the quality of the final product .
[0172] . According to a further embodiment, the final cylindrical body 1 is intended for use in disc brake applications, leveraging its optimized structure to withstand high thermal and mechanical stresses . This makes the body suitable for high-performance applications .
[0173] . According to a further embodiment, the sacrificial fibres 4 are made of polylactic acid PLA, designed to thermally decompose at temperatures above 150°C, facilitating the formation of internal channels 5 capable of maintaining a gas flow with laminar behaviour. This improves the formation of the channels .
[0174] . According to a further embodiment, the sacrificial fibres 4 are composed of cellulose, selected for their ability to be dissolved by applying a specific enzyme after the formation of the cylindrical body. This improves the removal of the sacrificial fibres .
[0175] . According to a further embodiment, the sacrificial fibres 4are made of polyvinylpyrrolidone PVP, designed to be removed through washing with a saline solution 17, creating channels 5 without residues . This ensures the cleanliness of the channels .
[0176] . According to a further embodiment, the sacrificial fibres 4 are made of polyurethane, which can be decomposed by applying heat in an inert environment, ensuring the formation of channels 5 having a precise shape . This improves the precision of the channels .
[0177] . According to a further embodiment, the dissolution process of the sacrificial fibres 4 of cellulose in step f) comprises the use of an organic solvent 18, such as acetone, for efficient removal . This improves the effectiveness of the removal of the fibres .
[0178] . According to a further embodiment, the sacrificial fibres 4 are composed of polyethylene glycol PEG, designed to dissolve in hot water 19, facilitating the creation of smooth internal channels 5. This improves the quality of the channels .
[0179] . According to a further embodiment, the method of decomposition of the sacrificial fibres 4 of PLA in step f ) comprises an accelerated composting process, combining heat and humidity for rapid removal . This accelerates the process of removal of the fibres .
[0180] . According to a further embodiment, the sacrificial fibres 4 are made of polyacrylonitrile PAN, designed to be eliminated through controlled oxidation, leaving defined channels 5 in the cylindrical body 9. This improves the definition of the channels .
[0181] . According to a further embodiment, the sacrificial fibres 4 are made of silicone rubber, designed to be removed by pyrolysis, ensuring the formation of clean internal channels 5 capable ofmaintaining a gas flow with laminar behaviour. This ensures the cleanliness and quality of the channels .
[0182] . According to a further embodiment, the non-sacrif icial fibres 3 are arranged in a cross-layered configuration to improve resistance to bending and torsion. This improves the mechanical strength of the body.
[0183] . According to a further embodiment, the densified carbon matrix comprises graphene nanoparticles to further increase thermal conductivity and mechanical strength. This improves the thermal and mechanical properties of the body.
[0184] . According to a further embodiment, the surface processing comprises an anodisation treatment to improve corrosion resistance . This improves the durability of the body in corrosive environments .
[0185] . According to a further embodiment, the non-sacrif icial fibres 3 are made of a mixture of high-strength carbon fibres and aramid fibres to optimise impact absorption properties . This improves the impact absorption capability of the body.
[0186] . According to a further embodiment, the densified carbon matrix is further reinforced with silicon carbide fibres to improve hardness and wear resistance . This improves the wear resistance of the body.
[0187] . According to a further embodiment, the surface processing is performed by means of a sandblasting finishing process 21 to obtain a textured surface that improves adhesion in mechanical applications . This improves the adhesion of the body.
[0188] . According to a further embodiment, the sacrificial fibres 4are designed to leave an internal three-dimensional structural pattern 13 that contributes to the reinforcement of the densified carbon matrix. This improves the internal structure of the body.
[0189] . According to a further embodiment, the densified carbon matrix is obtained through a vapour-phase carbon infiltration process, ensuring a uniform and defect-free structure . This improves the structural quality of the body.
[0190] . According to a further embodiment, the surface processing comprises a ceramic coating to improve resistance to high temperatures and oxidation. This improves the resistance of the body to extreme conditions .
[0191] . According to a further embodiment, the non-sacrif icial fibres 3 are treated with a polymer coating to improve compatibility with the carbon matrix and reduce delamination. This improves the integrity of the body.LIST OF REFERENCE NUMERALS1 densified cylindrical body2 winding mandrel3 non-sacrif icial fibres4 sacrificial fibres5 internal channels obtained by the dissolution of the sacrificial fibres6 hollow cylindrical body having an extension substantially equal to the winding mandrel7 cylindrical body8 needling tool and preferably radial needling process9 cylindrical body or semi-finished cylindrical body10 binding resin or resin or epoxy resin11 densif ication gas or liquid12 surface layer obstructing the internal channels due to densif ication13 three-dimensional structural pattern or three-dimensional structure14 cutting tool15 needling needles16 alkaline solution17 saline solution18 organic solvent19 hot water20 a surface layer of the cylindrical body for specific applications21 sandblasting finishing processSYMBOLSD external diameter of the hollow cylindrical body and of the semifinished cylindrical bodyd internal diameter of the hollow cylindrical body and of the semifinished cylindrical body and external diameter of the mandrel dl predetermined diameter of the non-sacrif icial fibres
Claims
CLAIMS1. A method for producing a densified cylindrical body ( 1 ) , comprising the following steps :a) providing a winding mandrel (2 ) with a predetermined external diameter (d) ;b) forming at least one layer of main structural fibers, referred to as non-sacrif icial fibers (3) ; non-sacrif icial fibers that will constitute a component of the supporting matrix of the cylindrical body ( 1 ) ;c) overlapping at least one layer of fibers designed to be temporarily integrated, referred to as sacrificial fibers (4 ) , interposed or integrated into the layer of non- sacrificial fibers (3) to create, when these sacrificial fibers (4 ) are decomposed, temporary internal channels (5) within the body before densif ication (7 ) ;or instead of steps b) and c) :bl ) separately forming an assembly, such as a non-woven fabric composed of main structural fibers, referred to as non-sacrif icial fibers (3) , which will constitute the supporting matrix of the cylindrical body ( 1 ) , mixed with / arranged with fibers designed to be temporarily integrated, referred to as sacrificial fibers (4 ) , interposedor integrated into the layer of non-sacrif icial fibers (3) to create, when these sacrificial fibers (4 ) are decomposed, temporary internal channels (5) within the body (7 ) ;and wherein:d) wrapping said at least one layer of non-sacrif icial fibers (3) around the mandrel (2) to form a hollow cylindrical body ( 6) coaxial to the mandrel (2 ) ; said hollow cylindrical body ( 6) having a predetermined external diameter (D) and a predetermined internal diameter (d) , wherein said internal diameter (d) is substantially equal to the diameter of the mandrel (d) ;f ) decomposing the sacrificial fibers (4 ) to form elongated internal channels (5) within the cylindrical body (7 ) ;h) subj ecting the cylindrical body (7 ) to a densif ication treatment to improve the material structure and its mechanical properties, utilizing the internal channels (5) left by the decomposition of the sacrificial fibers (4 ) to densify the cylindrical body in depth, rendering it a densified cylindrical body ( 1 ) .
2. The method for producing a densified cylindrical body ( 1 ) according to claim 1, wherein after step d) , the following step is provided:dl ) performing on the overlap of layers b) and c) or bl ) a needling process, using a needling tool ( 8 ) , to create a three-dimensional structure of main structural fibers (3) and sacrificial fibers (4 ) .3 . The method for producing a densi fied cylindrical body ( 1 ) according to claim 1 or 2 , wherein after step d) or dl ) , the following step is provided :e ) heating the hollow cylindrical body ( 6 or 9 ) to initiate the consolidation process of the non-sacri f icial fibers ( 3 ) , obtaining at least a partial cross-linking of a binding resin( 10 ) placed around said non-sacri f icial fibers .4 . The method for producing a densi fied cylindrical body ( 1 ) according to any one of claims 1 to 3 , wherein said step f ) is further speci fied as follows :f ) decomposing the sacri ficial fibers ( 4 ) to form elongated channels ( 5 ) within the cylindrical body ( 7 ) to improve the penetration of gas or liquid ( 11 ) in the subsequent densi f ication process .g)5 . The method for producing a densi fied cylindrical body ( 1 ) according to any one of claims 1 to 4 , wherein after step f ) , the following step is provided :h) performing a heat treatment to complete the cross-linking of the binding resin ( 10 ) , obtaining a semi- finished cylindrical body ( 9 ) .1 )6 . The method for producing a densi fied cylindrical body ( 1 )according to any one of claims 1 to 5, wherein after step h) , the following step is provided:i) removing a surface layer ( 12 ) of the material to re-expose the channels (5) created by the decomposition of the sacrificial fibers (4 ) where partially or completely obstructed by the densif ication process .
7. The method for producing a densified cylindrical body according to claim 6, wherein after step h) , the following step is provided: j ) repeating the cycles of densif ication and removal of the surface layer ( 12 ) until the desired degree of densif ication is achieved .k)8. The method for producing a densified cylindrical body according to any one of claims 2 to 7, wherein said step dl ) is modified as follows :dl ) performing on the overlap of layers b) and c) or bl ) a radial needling process ( 8 ) to create a three-dimensional structure ( 13) of main structural fibers or non-sacrif icial fibers (3) and sacrificial fibers (4 ) .
9. The method for producing a densified cylindrical body according to any one of claims 1 to 8, wherein:in said step b) , at least one layer of main structural fibers or non-sacrif icial fibers (3) is formed with dimensions such as toproduce, with the subsequent step d) , a hollow cylindrical body ( 6) with dimensions greater in axial extension than a finished product, so that after step d) or after step h) , it is cut, with a cutting tool ( 14 ) , to a desired axial dimension thus obtaining a semi-finished product ( 9) .
10. The method for producing a densified cylindrical body according to any one of claims 1 to 9, wherein:the sacrificial fibers include cotton fibers; orwhereinthe sacrificial fibers include linen fibers; orwhereinthe sacrificial fibers include cotton and linen fibers; or whereinthe non-sacrif icial fibers (3) are carbon fibers; orwhereinthe non-sacrif icial fibers (3) are carbon fibers, chosen for their high mechanical strength and thermal stability, and are impregnated with an epoxy resin ( 10) before wrapping on the mandrel;and / or whereinthe non-sacrif icial fibers (3) are composed of a mixture of high-strength carbon fibers and aramid fibers to optimize impact absorption properties;and / or whereinin said step b) , forming at least one layer of main structuralfibers referred to as non-sacrif icial fibers (3) , each having a predetermined diameter (dl ) .
11. The method for producing a densified cylindrical body according to any one of claims 1 to 10, wherein:the sacrificial fibers (4 ) are polyvinyl alcohol (PVA) fibers ;or whereinthe sacrificial fibers (4 ) are fibers selected for their ability to dissolve in hot water, creating elongated channels without harmful residues ;cotton fibers or linen fibers with thermal decomposition (organic fibers with very high 80-100% loss on ignition with thermal decomposition) .
12. The method for producing a densified cylindrical body according to any one of claims 2 to 11, wherein:the needling process ( 8 ) in step dl ) is performed using needles ( 15) with multiple barbs to ensure an effective three-dimensional interweaving between the non-sacrif icial fibers (3) and sacrificial fibers (4 ) .
13. The method for producing a densified cylindrical body according to any one of claims 3 to 12, wherein:the heating in step e) is carried out at a temperature between 80°C and 120°C to facilitate the pre-cross-linking of the resin ( 10) before the final densif ication .
14. The method for producing a densified cylindrical body according to any one of claims 5 to 13, wherein:the heat treatment in step g) is followed by controlled cooling to avoid internal stresses in the semi-finished cylindrical body ( 9) .
15. The method for producing a densified cylindrical body according to any one of claims 1 to 14, wherein:the densif ication treatment in step h) is achieved through various techniques such as :• infiltration of a polymeric matrix of gases or liquids,• deposition of a metallic or ceramic matrix by infiltration of gaseous or liquid phases,• infiltration of gases or liquids filling the residual porosities, improving the mechanical and thermal properties of the body.•16. The method for producing a densified cylindrical body according to any one of claims 6 to 15, wherein:the removal of the surface layer ( 12 ) in step i) is carried out by milling thin surface layers to ensure optimal access to the internal channels (5) for the subsequent densif ication cycle;or whereinthe removal of the surface layer ( 12 ) in step i) is carried out by milling a thin surface layer to ensure optimal access to the internal channels (5) for the subsequent densification cycle, after which, if necessary, the step of removing the surface layer ( 12 ) is repeated, followed by a densification step .
17. The method for producing a densified cylindrical body according to any one of claims 1 to 16, wherein:the decomposition process of the sacrificial fibers (4 ) in step f ) includes the application of an alkaline solution ( 16) ;or whereinthe decomposition process of the sacrificial fibers (4 ) in step f ) includes the application of an alkaline solution (16) to facilitate the dissolution of PVA fibers;or whereinthe decomposition process of the sacrificial fibers (4 ) in step f ) includes thermal decomposition to facilitate the removal of the sacrificial fibers .18 . The method for producing a densified cylindrical body according to any one of claims 7 to 17, wherein:the cycles of densif ication and removal of the surface layer ( 12 ) in step j ) are repeated at least three times to ensure uniform and complete densif ication of the cylindrical body ( 1 ) .
19. The method for producing a densified cylindrical body according to any one of claims 1 to 18, wherein:the final cylindrical body ( 1 ) is intended for use in disc brake applications, leveraging its optimized structure to withstand high thermal and mechanical stresses .
20. The method for producing a densified cylindrical body according to any one of claims 1 to 19, wherein:the sacrificial fibers (4 ) are made of polylactic acid (PLA) ; or whereinthe sacrificial fibers (4 ) are made and designed to thermally decompose at temperatures above 150°C, facilitating the formation of internal channels (5) ;or whereinthe sacrificial fibers (4 ) are made of polylactic acid (PLA) , designed to thermally decompose at temperatures above 150°C, facilitating the formation of internal channels (5) ;or whereinthe sacrificial fibers (4 ) are made and designed to thermally decompose at temperatures between 500-900°C (pyrolysis process) , facilitating the formation of internal channels (5) .
21. A method for producing a densified cylindrical body according to any one of claims 1 to 20, wherein:the sacrificial fibers (4 ) are composed of cellulose, selected for their ability to be dissolved by applying a specific enzyme after the formation of the cylindrical body.
22. the method for producing a densified cylindrical body according to any one of claims 1 to 21, wherein:the sacrificial fibers (4 ) are made of polyvinylpyrrolidone (PVP) , designed to be removed through washing with a saline solution ( 17 ) , creating channels (5) without residues .
23. The method for producing a densified cylindrical body according to any one of claims 1 to 22, wherein:the sacrificial fibers (4 ) are made of polyurethane, which can be decomposed by applying heat in an inert environment, ensuring the formation of precisely shaped channels (5) .
24. The method for producing a densified cylindrical body according to any one of claims 1 to 23, wherein:the dissolution process of the sacrificial fibers (4 ) of cellulose in step f ) includes the use of an organic solvent ( 18 ) , such as acetone, for an efficient removal .
25. The method for producing a densified cylindrical body according to any one of claims 1 to 24, wherein:the sacrificial fibers (4 ) are composed of polyethylene glycol (PEG) , designed to dissolve in hot water ( 19) , facilitating the creation of smooth internal channels (5) .
26. The method for producing a densified cylindrical body according to any one of claims 1 to 25, wherein:the method of decomposition of the sacrificial fibers (4 ) of PLA in step f ) includes an accelerated composting process, combining heat and humidity for rapid removal .
27. The method for producing a densified cylindrical body according to any one of claims 1 to 26, wherein:the sacrificial fibers (4 ) are made of polyacrylonitrile (PAN) , designed to be eliminated through controlled oxidation, leaving defined channels (5) in the cylindrical body ( 9) .
28. The method for producing a densified cylindrical body according to any one of claims 1 to 27, wherein:the sacrificial fibers (4 ) are made of silicone rubber, designed to be removed by pyrolysis, ensuring the formation of clean internal channels (5) capable of maintaining a laminar gas flow.
29. A densified cylindrical body ( 1 ) , comprising:a) a cylindrical core consisting of layers of main structural fibers (3) , referred to as non-sacrif icial fibers (3) , which form the supporting matrix of the cylindrical body, providing mechanical strength and thermal stability;b) a densified carbon matrix filling the residual porosities and channels (5) previously formed by layers of sacrificial fibers (4 ) decomposed before densif ication, improving the mechanical and thermal properties of the cylindrical body and conferring a uniform and solid structure to the body;c) a surface treatment obtained through the controlled removal of a surface layer (20) of the cylindrical body, optimizing the surface for specific applications; wherein the cylindrical body is designed for applications requiring high mechanical strength, thermal stability, and structural integration, such as in high-performance braking systems .d)30. The densified cylindrical body according to claim 29, wherein :the non-sacrif icial fibers (3) are arranged in a cross- layered configuration to improve resistance to bending and torsion.
31. The densified cylindrical body according to claim 29 or30, wherein:the densified carbon matrix includes graphene nanoparticles to further increase thermal conductivity and mechanical strength.
32. The densified cylindrical body according to claim 29 or 31, wherein:the surface treatment includes an anodization process to improve corrosion resistance .
33. The densified cylindrical body according to claim 29 or 32, wherein:the non-sacrif icial fibers (3) are composed of a mixture of high-strength carbon fibers and aramid fibers to optimize impact absorption properties .
34. The densified cylindrical body according to claim 29 or 33, wherein:the densified carbon matrix is further reinforced with silicon carbide fibers to improve hardness and wear resistance .
35. The densified cylindrical body according to claim 29 or 34, wherein:surface treatment is performed through a sandblasting process(21 ) to obtain a textured surface that improves adhesion in mechanical applications .
36. The densified cylindrical body according to claim 29 or 35, wherein:the sacrificial fibers (4 ) are designed to leave an internal three-dimensional structural pattern ( 13) that contributes to the reinforcement of the densified carbon matrix .
37. The densified cylindrical body according to claim 29 or 36, wherein:the densified carbon matrix is obtained through a vapor-phase carbon infiltration process, ensuring a uniform and defect- free structure .
38. The densified cylindrical body according to claim 29 or 37, wherein:the surface treatment includes a ceramic coating to improve resistance to high temperatures and oxidation.
39. A densified cylindrical body according to claim 29 or 38, wherein :the non-sacrif icial fibers (3) are treated with a polymer coating to improve compatibility with the carbon matrix and reduce delamination .