Temperature control agent, heat generation composition containing same, and heating element
By using an aliphatic compound with controlled particle size and solubility, the heating elements achieve stable and uniform temperature control, addressing inconsistencies in conventional methods and enhancing safety and durability.
Patent Information
- Application Number
- PCT/JP2025/039508
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2025-11-11
- Publication Date
- 2026-11-12
AI Technical Summary
Conventional temperature control methods for heating elements, such as chemical hand warmers and medical devices, face challenges in maintaining stable temperature performance due to variations in oxygen inflow, leading to inconsistent heat generation and safety issues, especially during storage and use.
Incorporating an aliphatic compound with specific properties, such as a melting point of 35°C or higher and water solubility of 5 g/100 mL or less, in particulate form with controlled particle size, to stabilize heat generation and improve uniform distribution within the exothermic composition.
The solution provides stable temperature control, reduces variations in heat characteristics, extends heat generation duration, and enhances safety by maintaining consistent heat output even under varying conditions.
Smart Images

Figure JP2025039508_12112026_PF_FP_ABST
Abstract
Description
Temperature control agent, exothermic composition containing the same, and heating element
[0001] The present invention relates to a temperature control agent used in the manufacture of heating elements such as chemical hand warmers (heat packs), warm compress structures, and meridian stimulation devices that generate heat in reaction with oxygen, a heat-generating composition containing the same, and a heating element using the same.
[0002] Heating materials that use heat-generating compositions that generate heat upon contact with oxygen or air are widely used in general as medical devices such as warm compresses and meridian-stimulating heat devices to alleviate pain through heat, or as everyday items such as hand warmers and other heating devices for protection against the cold.
[0003] The heat-generating compositions used in such heating elements most commonly contain metal powders such as iron powder, salts such as sodium chloride, water, and water-retaining agents such as activated carbon as components, and generate heat through oxidation, which occurs when the metal reacts with oxygen. Therefore, conventionally, the heat-generating characteristics have been adjusted to a desired range according to the purpose of the heating element by controlling the amount of oxygen inflow through the permeability, moisture permeability, and material of the permeable packaging material, particularly permeable (porous) film, of the bag containing the heat-generating composition.
[0004] This method allows for adjustment of factors such as the maximum heat output, rise time, and duration, and the product is designed so that these are optimized under certain conditions. However, strictly controlling the performance of the packaging material is burdensome in terms of manufacturing costs. Furthermore, even if high-performance breathable packaging material is used, if the actual amount of airflow during use does not match the design due to the manner of use or pinholes in the bag, the intended performance may not be achieved, or safety problems may arise.
[0005] Similar problems exist in medical heating devices, which require more precise temperature control. For example, transdermal medical warm compresses, which combine a heating element and a drug, are touted as offering advantages such as increased effectiveness and reduced drug dosage due to the improved efficiency of transdermal absorption through heat. However, as mentioned above, conventional temperature control methods have incomplete stability in generating the heat, resulting in unstable drug dosages due to the instability of the temperature in practice.
[0006] In relation to these problems, the present inventors have found that the temperature stability of a heating element can be improved by a method other than adjusting the amount of oxygen inflow, by including a component containing a specific aliphatic compound as a temperature control agent in the packaging material of the heating composition or the bag or container containing it (Patent Document 3).
[0007] The heating element is composed of relatively stable components and can be stored at room temperature for a certain period of time by blocking out oxygen. However, if exposed to temperature changes during storage, especially high-temperature environments, its shelf life may decrease and the maximum temperature may drop. Even with heating elements that use a temperature control agent, if stored for a long period of time, the element may not reach the intended heating temperature after opening. However, the inventors have found that this problem can be overcome by keeping the particle size of the temperature control agent within a predetermined range (Patent Document 4).
[0008] However, it was found that the phenomenon of reduced shelf life in such high-temperature environments is particularly pronounced when the amount of exothermic composition contained in the heating element is small, and even when the intended exothermic temperature is reached, there is a problem in that the subsequent temperature decrease tends to be rapid. In addition, conventional temperature control agents were prone to degradation unless the particle size was relatively large, but large particles are inconvenient to mix uniformly with other particulate components in the exothermic composition, resulting in the problem of variations in the temperature characteristics of the heating element. Therefore, further improvements in terms of safety, temperature stability, and long-term shelf life were desirable for such temperature control agents.
[0009] International Publication WO1999 / 000078, Japanese Patent Publication No. 2001-170099, International Publication WO2016 / 063815, International Publication WO2019 / 151472
[0010] The present invention aims to provide a means for achieving lower-cost and simpler temperature control of a heating element (particularly control of the maximum heat generation temperature) that can be used instead of, or in combination with, conventional temperature control by controlling the supply amount of oxygen or air using a breathable film or the like, and to prevent or reduce the decrease in heat generation temperature due to aging deterioration of the heating element and the effects of storage at high temperatures (temperature deterioration of the heat generation composition during long-term storage), and to provide a heating element using the same. Furthermore, the present invention aims to provide a more advanced temperature control means that can be used for heating elements in medical applications, and to provide an improved heating element for medical applications that is safer and more effective. In addition, the present invention aims to facilitate the uniform distribution of temperature control agent particles in the heat generation composition, reduce variations in the temperature characteristics of the heating element, enable the above-mentioned more advanced temperature control, and extend the duration of the optimal temperature during use of the heating element. In particular, the present invention aims to provide a temperature control agent that can be uniformly mixed into the heat generation composition even when used in small heating elements where the amount of heat generation composition is small, and that can extend the duration of heat generation of small heating elements.
[0011] According to the present invention, [1] a temperature control agent containing an aliphatic compound, used to control the exothermic temperature of a heating element containing an exothermic composition that reacts with oxygen to generate heat, wherein the aliphatic compound has a melting point of 35°C or higher, a water solubility of 5 g / 100 mL or less at 20°C, and is in particulate form with an average circularity of 0.70 to 1.0; [2] the temperature control agent according to [1], wherein the aliphatic compound is in particulate form that does not pass through a 325-mesh standard sieve (standard dimensions according to JIS Z8801-1: 44 μm); [3] the temperature control agent according to claim 1 or 2, wherein the aliphatic compound is in particulate form that passes through a 16-mesh standard sieve (standard dimensions according to JIS Z8801-1: 1000 μm). [4] A temperature control agent according to any one of [1] to [3], wherein the aliphatic compound contains one or more compounds selected from the group consisting of higher α-olefin copolymers, paraffin wax, myristyl myristate, polyester polyols, and polyoxyethylene fatty acid diesters; [5] A heat-generating composition that generates heat in reaction with oxygen, wherein the heat-generating composition comprises metal powder, salts, water, activated carbon, and a temperature control agent for controlling the heat generation temperature of the heat-generating composition, wherein the temperature control agent is the temperature control agent according to any one of [1] to [4]; [6] A heating element comprising the heat-generating composition according to [5] and a bag or container that is at least partially permeable and contains the heat-generating composition; [7] A heating element according to [6], wherein the bag or container is contained in an airtight outer bag that substantially blocks oxygen; [8] A heating element according to [6] or [7], used as either a disposable hand warmer or a medical device; [9] The heating element described in [8] above, wherein the medical device is either a hot compress or a heat device for stimulating meridians;
[10] A method for producing a temperature control agent according to any one of [1] to [4] above is provided, characterized in that it includes a step of atomizing a molten material obtained by melting the aliphatic compound or the temperature control agent into spherical particles.
[0012] According to the present invention, a simple, low-cost, and reliable temperature control method is provided that can be used in addition to or as an alternative to temperature control by a breathable film in a heating element. The maximum heat generation temperature remains stable even after long-term storage, resulting in a heating element with superior temperature stability and high safety. According to the present invention, the uniformity of the distribution of temperature control agent particles in the heat generation composition is improved, reducing variations in the temperature characteristics of the heating element. Furthermore, according to the present invention, even with the same amount of heat generation composition, a heating element with a longer heat generation duration than conventional ones can be provided. Moreover, according to the present invention, in the process of forming spherical particles from the temperature control agent raw material, the range of particle sizes produced can be narrowly controlled, and when classifying large or small particles, the high fluidity improves work efficiency, reduces raw material loss, and is advantageous in manufacturing.
[0013] Surprisingly, it was found that the heating element using the heat-generating composition containing the temperature control agent of the present invention exhibits excellent quality stability during high-temperature storage, and also has a low rate of temperature drop after the heat generation stops, allowing for safe and prolonged warmth.
[0014] In particular, the present invention provides a heating element that is suitable for long-term emergency stockpiling, for example, and that poses a low risk of low-temperature burns even when used during sleep. Specifically, for example, the invention provides: - A heating element that can be used safely even while sleeping, with reduced risk of low-temperature burns due to covering with bedding; - A highly safe disposable shoe warmer that provides stable heat generation regardless of the type of shoe and does not cause a sudden temperature rise when the shoes are removed; - A transdermal medical warm compress with high temperature stability, safety, and effectiveness; - A heating element that can be used safely as a meridian stimulation device, such as moxibustion, by controlling the maximum temperature even in high temperature ranges.
[0015] Figure 1 shows examples of samples obtained by classifying the same aliphatic compound, both mechanically pulverized and atomized into spherical particles. The left image is a digital microscope photograph, and the right image is a diagram obtained by image processing of the same image for measuring the average circularity (both at 200x magnification). Figure 2 shows the results of a time-dependent degradation test in which heating bodies (Examples 1-7) containing α-olefin copolymer (melting point 58°C) atomized into spherical particles by atomization as a temperature control agent were stored at 50°C. In each panel, "Initial" represents the exothermic pattern immediately after manufacturing; "2W" represents the pattern after 2 weeks of storage; "1M" represents the pattern after 1 month of storage; and "2M" represents the pattern after 2 months of storage. Figure 3 shows the results of a time-dependent degradation test in which heating bodies (Comparative Examples 1-7) containing α-olefin copolymer (melting point 58°C) pulverized by mechanical pulverization as a temperature control agent were stored at 50°C. In each panel, "Initial" represents the heat generation pattern immediately after manufacturing; "2W" represents the pattern after 2 weeks of storage; and "1M" represents the pattern after 1 month of storage. Figure 4 shows an example of the structure of a small heating element that can be used as a meridian stimulating heat device (moxibustion device) of the present invention. Panel A is a cross-sectional view of the moxibustion device, Panel B is a perspective view of the heat generation composition tablet (1), Panel C is a perspective view of the heat generation composition tablet (1) placed in the container body (2), and Panel D is a perspective view showing the container body (2) containing the heat generation composition tablet (1) together with the adhesive-processed top material (adhesive tape) (3) attached thereto. Note that the heat generation composition tablet (1) in Figure 4 is schematically shown in its form before water (or salt water) is added (before swelling). Figure 5 shows a comparison of the exothermic behavior when excessive heat is induced between a heating element (Example 8) using an exothermic composition containing α-olefin copolymer (melting point 58°C) atomized into spherical particles by atomization as a temperature control agent, and a heating element (Comparative Example 8) using an exothermic composition containing α-olefin copolymer (melting point 58°C) pulverized by mechanical pulverization. Figure 6 shows a comparison of the exothermic behavior when excessive heat is induced between a heating element (Example 9) using an exothermic composition containing α-olefin copolymer (melting point 58°C) atomized into spherical particles by atomization as a temperature control agent, and a heating element (Comparative Example 9) using an exothermic composition containing α-olefin copolymer (melting point 58°C) pulverized by mechanical pulverization.Figure 7 shows a comparison of the exothermic behavior when excessive heat is induced between a heating element (Example 10) using an exothermic composition containing α-olefin copolymer (melting point 58°C) atomized into spherical particles by atomization as a temperature control agent, and a heating element (Comparative Example 10) using an exothermic composition containing α-olefin copolymer (melting point 58°C) pulverized by mechanical pulverization. Figure 8 shows a comparison of the exothermic behavior when excessive heat is induced between a heating element (Example 11) using an exothermic composition containing α-olefin copolymer (melting point 58°C) atomized into spherical particles by atomization as a temperature control agent, and a heating element (Comparative Example 11) using an exothermic composition containing α-olefin copolymer (melting point 58°C) pulverized by mechanical pulverization. Figure 9 shows a comparison of the exothermic behavior when excessive heat is induced between a heating element (Example 12) using an exothermic composition containing α-olefin copolymer (melting point 58°C) atomized into spherical particles by atomization as a temperature control agent, and a heating element (Comparative Example 12) using an exothermic composition containing α-olefin copolymer (melting point 58°C) pulverized by mechanical pulverization. Figure 10 shows a comparison of the exothermic behavior when excessive heat is induced between a heating element (Example 13) using an exothermic composition containing α-olefin copolymer (melting point 58°C) atomized into spherical particles by atomization as a temperature control agent, and a heating element (Comparative Example 13) using an exothermic composition containing α-olefin copolymer (melting point 58°C) pulverized by mechanical pulverization. Figure 11 shows a comparison of the exothermic behavior when excessive heat is induced between a heating element (Example 14) using an exothermic composition containing α-olefin copolymer (melting point 58°C) atomized into spherical particles by atomization as a temperature control agent, and a heating element (Comparative Example 14) using an exothermic composition containing α-olefin copolymer (melting point 58°C) pulverized by mechanical pulverization. Figure 12 shows a comparison of the exothermic behavior when excessive heat is induced between a heating element (Example 15) using an exothermic composition containing α-olefin copolymer (melting point 58°C) atomized into spherical particles by atomization as a temperature control agent, and a heating element (Comparative Example 15) using an exothermic composition containing α-olefin copolymer (melting point 58°C) pulverized by mechanical pulverization.Figure 13 shows a comparison of the temperature decrease rate over time for the heating elements of Examples 11-15 and Comparative Examples 11-15, with the temperature at which the maximum temperature was reached set to 0. The examples are shown by solid lines, and the comparative examples by dotted lines.
[0016] Temperature Control Agent The temperature control agent of the present invention is characterized by containing one or more aliphatic compounds having a melting point of 35°C or higher and a water solubility of 5 g / 100 mL or less at 20°C. The above solubility is preferably 3 g / 100 mL or less, and more preferably 1 g / 100 mL or less. The preferred melting point of the aliphatic compound varies depending on the application of the heating element and can be appropriately selected, but from the viewpoint of preventing deterioration of the exothermic properties during storage, it is generally 35°C or higher, preferably 38°C or higher, and the upper limit is generally 70°C or lower, preferably 65°C or lower, from the viewpoint of the safety of the heating element. In this specification, "aliphatic compound" means an organic compound in which all carbon atoms in the molecule are linked in a single chain, or a compound in which the carbon atom chain has a branched structure but does not contain a cyclic structure, and includes anhydrides of chain dicarboxylic acids, imides, lactones of oxy acids, cyclic ethers, etc., which have a cyclic structure containing oxygen and nitrogen, but are closely related to the chain compound that is the parent compound, and whose rings can easily open to become chain compounds.
[0017] Aliphatic compounds having such properties can be selected from among higher α-olefin copolymers, various paraffin waxes such as plant-derived, animal-derived, or petroleum-derived, myristyl myristate, polyester polyols, and polyoxyethylene fatty acid diesters. In this specification, higher α-olefin copolymer refers to a copolymer of two or more α-olefins having 10 to 35 carbon atoms, or one or more α-olefins having 10 to 35 carbon atoms and one or more other olefins. That is, a higher α-olefin copolymer is a copolymer of two or more α-olefins having 10 to 35 carbon atoms, or a copolymer of one or more α-olefins having 10 to 35 carbon atoms and one or more other olefins.
[0018] The higher α-olefin copolymer used in the present invention may be a main-chain crystalline polyolefin in which the main chain folds and crystallizes, but a side-chain crystalline polyolefin having a certain amount of long-chain α-olefins in the side chains is preferred. Side-chain crystalline polyolefins have sharp melting behavior. When not melted, they are not sticky, which is convenient. Such side-chain crystalline polyolefins are manufactured and sold under trade names such as "HS Crystal" (Toyokuni Oil Co., Ltd.) and are commercially available. Similarly, paraffin wax (e.g., Nippon Seiro), myristyl myristate (e.g., Croda Japan), polyester polyol (e.g., DIC, Toyokuni Oil Co., Ltd.), polyoxyethylene fatty acid diester (e.g., Sanyo Chemical Industries, Ltd.), and higher α-olefin copolymers are also commercially available.
[0019] The melting point is measured using a differential scanning calorimeter as follows: 5 mg to 15 mg of the sample is placed in an aluminum (Al) container, and an Al crimped cover is placed over it and sealed under constant pressure. Using the Al container and clamp cover as a reference, the temperature is increased at a heating rate of 5°C / min from the estimated melting point of -50°C to the estimated melting point of +30°C. After holding for 5 minutes, it is cooled at the same rate and held at the estimated melting point of -50°C for 5 minutes. This is repeated twice, and the DSC curve of the second cycle (2nd run) is measured. The melting point is read from the endothermic main peak that appears in the DSC curve due to the endothermic reaction associated with the melting of the sample.
[0020] The solubility in water at 20°C can be measured by dissolving the sample in 100 g (100 mL) of water at 20°C and reading the mass of the maximum amount that can be dissolved (the limit at which it no longer dissolves).
[0021] The aliphatic compounds contained in the temperature control agent of the present invention can be used by processing raw materials in the form of pellets, powders, blocks, etc., at room temperature into spherical particles. Any known method applicable to resins can be used to produce the spherical particles. Examples of methods that can produce a large quantity of spherical particles relatively easily include powder melting and atomization. By selecting appropriate conditions in these methods, the size of the resulting spherical particles can be controlled to a desired range.
[0022] The powder melting method involves introducing powdered raw materials, for example, into a flame or thermal plasma, or into a vertical tubular furnace or tower kiln, to melt them at a temperature above their melting point, and then forming them into a spherical shape due to the surface tension of the molten material itself. Alternatively, a dispersion of the raw materials in a solvent or the like may be sprayed into a flame or thermal plasma, vertical tubular furnace, etc., from a nozzle, and the dispersion medium may be evaporated to form a spherical shape.
[0023] The atomization method involves melting a raw material in the form of a powder or bulk material in a heat-resistant container, dropping or spraying the molten material through a nozzle or the like, and rapidly cooling and solidifying it to form a sphere. Any method that can heat the raw material above its melting point is acceptable. The melting of the raw material is preferably carried out in an atmosphere such as air, an inert gas, or a vacuum.
[0024] Various known atomization methods can be used as appropriate. For example, any of the following methods can be suitably used: gas atomization, centrifugal atomization, hybrid atomization, water atomization, etc.
[0025] For example, in the gas atomization method, the melting temperature is preferably 50 to 200°C, and more preferably 70 to 150°C. The opening diameter of the nozzle for injecting the molten material is preferably 0.2 to 3.0 mm, and more preferably 0.5 to 2.0 mm. Examples of gases include air and argon gas. The injection pressure of the fluid is preferably 0.3 to 5 MPa, and more preferably 0.5 to 3 MPa. In the centrifugal atomization method, the melting temperature is preferably 50 to 200°C, and more preferably 70 to 150°C. The diameter of the nozzle at the bottom of the crucible can be appropriately selected depending on the physical properties of the material to be powdered, the desired particle size, production speed, and the scale of the equipment. As for the material of the disc, any material with a melting point higher than the melting temperature and that is resistant to thermal shock can be appropriately selected.
[0026] The aliphatic compound contained in the temperature control agent of the present invention is in particulate form with an average circularity of 0.70 to 1.0. The average circularity can preferably be 0.75 or higher, 0.76 or higher, 0.77 or higher, or 0.78 or higher, and more preferably 0.79 or higher. The methods for measuring and calculating the circularity of individual particles and the average circularity of a particle group will be described in detail in the examples.
[0027] In this specification, the particle size of aliphatic compounds is indicated by separation using a standard sieve (Tyler sieve). The size of the sieve opening is generally indicated in "mesh" or "μm" (the standard dimension (μm) for the opening of a metal sieve in JIS Z8801-1 (2006), also called the nominal size), and their correspondence is well known. Conventional temperature control agents were preferably in particulate form that does not pass through a 60-mesh standard sieve (opening 250 μm), and further preferably contained particulate form that passes through a 16-mesh standard sieve (opening 1000 μm). However, according to the present invention, there is no limitation on particle size, and even aliphatic compounds with small particle sizes that were previously preferred to be excluded can be suitably used as temperature control agents. Therefore, commercially available aliphatic compounds can be appropriately selected and formed into spherical particles and used as is in the temperature control agents of the present invention.
[0028] Furthermore, the temperature control agent of the present invention can be used by forming the aliphatic compound raw material into spherical particles, and then, if necessary, sieving (classifying) the particles to separate those that pass through from those that do not using various standard sieves, and then appropriately blending them to exhibit a desired exothermic pattern. In particular, when precise temperature control is required, it is desirable to control the particle size so that it is within a predetermined range. The aliphatic compound contained in the temperature control agent of the present invention is preferably in a particulate form that does not pass through a 325-mesh standard sieve (mesh opening 44 μm). In some cases, it is preferable that it is in a particulate form that does not pass through a 250-mesh standard sieve (mesh opening 63 μm). In addition, in order to further improve uniform dispersibility in the exothermic composition, it is preferable that it is in a particulate form that passes through a 16-mesh standard sieve (mesh opening 1000 μm), and even more preferably that it is in a particulate form that passes through a 32-mesh standard sieve (mesh opening 500 μm).
[0029] The aliphatic compound particle population may have a completely uniform particle size, and there are no particular restrictions on the particle size distribution within the population. However, it is desirable that the particles passing through a 325-mesh standard sieve (mesh opening 44 μm) account for less than 50% of the total temperature control agent (100%), and more preferably less than 30%.
[0030] In this specification, "not passing through" a sieve of a certain mesh size means that 60% or more of the material does not pass through that sieve, preferably 80% or more, and more preferably 90% or more. Most preferably 100%. Similarly, "passing through" a sieve of a certain mesh size means that 60% or more of the material passes through that sieve, preferably 80% or more, and more preferably 90% or more. Most preferably 100%.
[0031] The mechanism by which the temperature control agent of the present invention provides stability to the exothermic properties is not bound by any particular theory, but can be generally understood as follows. When the temperature control agent is added to the exothermic composition, the temperature control agent melts when the exothermic temperature reaches near the melting point of the temperature control agent, and by covering the iron powder, the oxidation reaction is inhibited and the temperature rise is suppressed. Here, the aliphatic compound component in the temperature control agent may contain not only those with a single measured melting point, but also those with a lower melting point (low-melting-point resin). One possibility is that in temperature control agents obtained by conventional mechanical grinding methods, such low-melting-point resins melt quickly and inhibit exothermic generation, thus contributing to a decrease in the exothermic temperature after high-temperature storage. On the other hand, in the case of the temperature control agent of the present invention, which contains aliphatic compounds that have been atomized into spherical particles by atomization or the like, the low-melting-point resin hardens first and forms a nucleus, and then the remaining resin components harden so as to surround this nucleus, thereby reducing the influence of the low-melting-point resin and suppressing the decrease in the exothermic temperature.
[0032] Therefore, conventionally, it was thought that using particles that do not pass through a 60-mesh standard sieve (mesh opening 250 μm) would reduce the impact of temporary changes in ambient temperature during storage compared to using finer particles, thus making accidental melting of the temperature control agent (and a decrease in the maximum exothermic temperature) less likely. However, the temperature control agent of the present invention is less affected by particle size and is thought to exhibit good performance even with smaller particles. Furthermore, conventional particles tend to have uneven dispersion in the exothermic composition, which is thought to cause variations in the time it takes to reach the maximum temperature. However, since the temperature control agent of the present invention can use smaller particles, it is thought that they disperse more uniformly in the exothermic composition, reducing variations in the temperature characteristics of the exothermic composition or heating element.
[0033] Furthermore, the maximum temperature to be achieved and the heat generation pattern differ depending on the application of the heating element. Therefore, the type and content of the temperature control agent should be selected to achieve the required heat generation performance.
[0034] For example, while a heat pack applied directly to the skin ideally generates heat at around 40°C, it is said that exceeding 43°C increases the risk of low-temperature burns due to protein denaturation. Therefore, it is desirable to design the product so that the temperature does not exceed 43°C, and if there is a possibility that the temperature will exceed 43°C, it is desirable to quickly suppress the temperature rise to the suitable 40°C. On the other hand, it is undesirable for the temperature to continue to fall after suppression, as this reduces the warming effect. Furthermore, even for heat packs applied directly to the skin, a milder heat generation of 40°C or less is preferable for those applied to the delicate abdomen of women for the purpose of relieving menstrual cramps.
[0035] On the other hand, disposable heat packs that attach to clothing are generally used at a maximum temperature of around 55°C because the skin is protected by the clothing. Small heating elements used to heat a limited area, such as moxibustion tools, are used at relatively high temperatures for a short time, but since they come into direct contact with the skin without clothing, it is desirable that they are designed not to exceed around 55°C. Furthermore, for small heating elements used as moxibustion tools, it is desirable that the temperature drops quickly after the temperature rise is suppressed. In contrast, even with small heating elements, products that provide mild thermal stimulation are preferable to maintain an appropriate temperature for a relatively long period, given the constraint of using a small amount of heat-generating composition.
[0036] Thus, since there are suitable maximum temperatures and heating patterns for each of the various heating elements, one or more aliphatic compounds having melting points close to the desired maximum temperature (for example, melting points between approximately -20°C and +10°C of the maximum temperature (i.e., the maximum temperature is within approximately +20°C to -10°C of the melting point), preferably with a melting point difference of ±8°C from the maximum temperature, and more preferably with a melting point difference of ±5°C from the maximum temperature) can be appropriately selected as a temperature control agent, and the amount added, method of addition, and addition of optional components can be designed. For example, to control the maximum temperature to about 55°C, an aliphatic compound with a melting point of 58°C can be selected.
[0037] The exothermic composition of the present invention contains at least metal powder, salts, water, and activated carbon, and further contains the temperature control agent of the present invention. The temperature control agent is as described above.
[0038] As the metal powder, iron powder is generally used, but other substances may also be used as long as they generate heat by oxidation. As the salts, inorganic salts such as sodium chloride, potassium chloride, and magnesium chloride are generally used. The exothermic composition of the present invention contains activated carbon, and may further contain a water retaining agent other than activated carbon (for example, water-absorbing polymers, vermiculite, sawdust, silica-based substances, etc.). In addition, various other conventionally known components can be added as necessary.
[0039] Examples of blending examples of these components include, for example, those composed of 35 to 80 wt% iron, 1 to 20 wt% activated carbon, 1 to 10 wt% salts, 5 to 45 wt% water, and 0 to 45 wt% of a water retaining agent other than activated carbon, with the total weight of the exothermic composition taken as 100%. The exothermic composition of the present invention preferably has a composition in the range of 30 to 70 wt% iron, 1 to 15 wt% activated carbon, 1 to 5 wt% salts, 20 to 30 wt% water, and 1 to 25 wt% of a water retaining agent other than activated carbon. The blending amount of the temperature control agent can be appropriately selected according to the intended use of the heating element, the maximum temperature to be achieved, and the like, as described above. For example, relative to 100 parts by weight of the exothermic composition having such a formulation, the temperature control agent of the present invention is added in an amount of 3 to 40 parts by weight, preferably 3 to 30 parts by weight, and mixed.
[0040] The exothermic composition can be produced by mixing the essential components described above and any optional components selected as needed, using known methods, under low-oxygen or oxygen-free conditions if salt and water are added beforehand. The exothermic composition may be in powder form, and may be further processed using known methods, for example, to form cubes by tableting or sheets by rolling. When forming the exothermic composition into a solid form, binders such as cellulose (e.g., crystalline cellulose), lactose, starch, dextrin, sucrose ester, Teflon®, polyethylene glycol, and carboxymethylcellulose may be added. For example, to form a tablet-shaped solid by tableting, a tablet with the desired appropriate hardness can be obtained by adding 5 to 30 parts by weight, preferably 10 to 30 parts by weight, of a binder such as crystalline cellulose to 100 parts by weight of the exothermic composition. Such a solid form of the exothermic composition is preferable because it prevents sealing defects caused by powder adhering to the seal portion of the bag or container during packaging and eliminates variations in the exothermic temperature. Regarding the exothermic composition, salts may be mixed simultaneously with the powder raw materials at the time of mixing, or they may be added as brine.
[0041] The exothermic composition of the present invention, which contains such a temperature control agent, can be confirmed to have achieved the desired maximum temperature by measuring the temperature change over time when it reacts with oxygen in the air through a breathable packaging material (for example, a porous film with a reaction rate of 17,000 to 18,000 seconds / 100cc or a nonwoven fabric with a reaction rate of 0 seconds / 100cc (both according to the JIS P8117 method (Wang-Ren test method)) used for a bag or container to contain the exothermic composition, according to the JIS S4100 exothermic test. The exothermic test conducted for this purpose may be performed by appropriately modifying the experimental conditions to reflect the expected actual usage conditions.
[0042] The packaging heat-generating composition is filled into a bag or container for containing the heat-generating composition. This bag or container filled with the heat-generating composition can also be used as a heating element (for example, a so-called non-adhesive type hand warmer). Generally, the bag or container for containing the heat-generating composition is formed so that at least a portion of it is breathable.
[0043] The breathable packaging material constituting the bag or container for housing the exothermic composition changes the heat generation characteristics of the heating body (such as the rising rate of heat generation, heat generation duration, and heat transfer property to a heating target such as the human body or clothing) depending on its selection, and thus a known material can be appropriately selected and used so that these characteristics fall within a desired range in accordance with the intended use.
[0044] For common disposable body warmers and the like for the human body, a breathable packaging material with an air permeability of 10,000 to 40,000 seconds / 100 cc (JIS P8117 (Oken type test method)) is used. For example, 2,000 to 7,000 seconds / 100 cc is used for shoe warmers. Therefore, as the breathable packaging material for the bag or container for housing the exothermic composition, a packaging material with an air permeability of generally 2,000 to 40,000 seconds / 100 cc is used. In the case of a heating body designed to be used at a high temperature and / or for a short period of time, such as a thermotherapy device for meridian stimulation, a packaging material of 0 to 10,000 seconds / 100 cc can be used. By using the temperature control agent of the present invention, precise air permeability control becomes unnecessary depending on the application of the heating body, and the allowable range of usable breathable packaging materials is expanded.
[0045] In the present invention, the breathable packaging material used for the bag or container may be any film or sheet that is entirely or partially breathable. In general, as the breathable packaging material, a single-layer or laminated porous film or sheet is used alone or in combination with a woven fabric or nonwoven fabric, or a single-layer or laminated non-porous film or sheet is used alone or in combination with a woven fabric or nonwoven fabric and provided with needle holes. In the present invention, "film" mainly refers to a single body (including single layer and lamination; the same applies hereinafter) or a relatively thin one, and "sheet" mainly refers to a single body, a laminate of two or more single bodies, or a relatively thick one, but they are not strictly distinguished.
[0046] Generally, thermoplastic synthetic resins are used as the resins that make up the film. Specifically, polyethylene, polypropylene, polyester, polyamide, polyvinyl alcohol, polyvinyl chloride, polyvinylidene chloride, polyurethane, polystyrene, ethylene-vinyl acetate copolymer, polycarbonate, etc., are suitably used individually or in combination. Depending on the purpose, and in accordance with the appropriate required heat output, temperature, and heat-generating composition used, the resin can be appropriately selected.
[0047] In the present invention, stretched films, preferably stretched porous films, or sheets containing the same are suitably used as breathable films or sheets. Stretched porous films generally contain inorganic fillers, and breathability is achieved by the formation of interconnected pores through stretching. The degree of breathability can be controlled by controlling the diameter of these pores, etc.
[0048] Lamination is usually carried out by lamination, but is not limited to this method. Any conventionally known method can be used for lamination. For example, it may be done by thermal bonding, hot melt adhesive, or adhesive such as acrylic or urethane adhesive, and it may be a full bond or a partial bond to maintain flexibility. Preferably, the curtain spray method or dry lamination method is used.
[0049] Nonwoven fabrics are generally used in breathable packaging materials to reinforce packaging strength and improve mechanical suitability. Suitable nonwoven fabrics for lamination with the aforementioned films include those conventionally used in the fields of heating elements and medical heating devices. Examples include those containing artificial fibers such as nylon, vinylon, polyester, rayon, acetate, acrylic, polyethylene, polypropylene, and polyvinyl chloride, as well as natural fibers such as cotton, linen, and silk. Examples of nonwoven fabrics include spunbond, thermalbond, and spunlace. The basis weight of nonwoven fabrics varies depending on the specific gravity of the nonwoven material and the bulkiness resulting from different entanglement methods, but is generally about 10 g / m². 2 ~Approx. 200g / m 2 A weight of around 20g / m is suitable, especially. 2 ~Approx. 100g / m 2It is preferable.
[0050] In particular, breathable sheets made by laminating nonwoven fabrics such as nylon and polyester fibers onto stretched porous films of thermoplastic synthetic resins are commonly used.
[0051] A part of the bag or container, such as the back packaging material of a flattened bag, may be a breathable packaging material as described above, or a non-breathable packaging material. The non-breathable packaging material may be a single layer or laminated film or sheet of resin as described above, and there are no particular limitations regarding the material, thickness, composition, etc., as long as it is suitable for forming a bag or container for containing a heat-generating composition.
[0052] A bag or container for containing the heat-generating composition can be manufactured by using the above-mentioned packaging material and bonding the periphery in a manner commonly used in this art. The heating element can be basically manufactured by sealing the heat-generating composition of the present invention in this bag or container. Generally, the manufacturing of the bag or container and the manufacturing of the heating element are continuous. First, the periphery of the overlapping packaging material is bonded with heat seal or adhesive, leaving a portion open. After the heat-generating composition is poured in through the open portion, this opening is also bonded, and the heat-generating composition is sealed inside.
[0053] Furthermore, for small heating elements with a narrow application area and / or short usage time, such as moxibustion devices, the heating composition may be manufactured not in a flat bag, but in a container with a thickness of, for example, several millimeters to several centimeters. In this case as well, various types of packaging materials as described above can be used appropriately for the manufacture of the lid (top material) and the container body (cup). For example, the top material (Figure 4) may optionally contain layers such as sealant (3a), nonwoven fabric (3b), adhesive (3c), and release paper (3d) as needed. A specific example is that, starting from 3a, it may consist of LLDPE (30 μm) / PET spunlace nonwoven fabric (30 g / m²). 2) / SIS-type hot melt adhesive / PET separator (38 μm) can be used. As mentioned above, in the case of devices that utilize high temperature and / or short-term heat generation, such as moxibustion devices, a highly breathable packaging material can be used, so nonwoven fabric may be used alone for the top material and / or the container body. In this specification, "small" heating element refers to a heating element smaller than a standard so-called mini-sized disposable hand warmer, but more specifically, it refers to one with a diameter or side length of 5 cm or less, or even 3 cm or less.
[0054] The thermothermal body heating element can consist only of a bag filled with the heat-generating composition of the present invention (for example, a non-adhesive disposable hand warmer) or only a container (for example, a moxibustion device), as described above, but additional elements may be added as needed. These various elements are publicly known and may be integrated into the bag, or they may be provided as separate components to be combined during use. Examples of additional elements include various fixing means and various parts to be combined during use (for example, containers containing fragrances or medicines, sheets containing water or cosmetics, etc., used depending on the application of the thermothermal body). Examples of fixing means include adhesive layers or poultice layers formed on the surface of a part of the bag or container for containing the heat-generating composition to allow the thermothermal body to be attached, band-shaped members for wrapping around and fixing to the object to be heated, and masks, supporters, or wristbands with pockets for containing the thermothermal body. In addition, a base may be provided between the container and the adhesive layer to adjust the distance and / or space between the application site and the thermothermal body for purposes such as temperature control. Furthermore, the heating element of the present invention may use various drugs or fragrances such as camphor and menthol in combination with the adhesive layer, poultice layer, other components, or the heat-generating composition and / or packaging or container. For example, as a heat receptor, capsicum tincture, capsicum extract, capsicum powder, ginger tincture, ginger extract, ginger powder, fennel tincture, fennel extract, fennel powder, capsaicin, capsaicin derivatives, vanillyl butyl ether, vanillyl alkyl ether, nonyl vanillylamide, etc. can be added to the adhesive. As a cold receptor, l-menthol, peppermint, dl-camphor, peppermint oil, thymol, menthyl ethyl oxalate, etc. can be added to the adhesive.
[0055] The bag or container containing at least the heat-generating composition of the heating element is sealed in an outer bag that blocks oxygen and stored until use. Such outer bags are also known. For long-term storage, an outer bag that includes an aluminum layer with low oxygen permeability to minimize the oxidation reaction of iron during storage, and low water vapor permeability to minimize the release of water vapor from the outer bag, is particularly preferred.
[0056] <Manufacturing of Temperature Control Agent> An α-olefin copolymer (Toyokuni Oil Co., Ltd. "HS Crystal-6100") (in lump or powder form, melting point 58°C) was melted at 110°C in an applicator (PHAL BOK SYSTEM CO. LTD. "Nino-30"), and then the molten material was supplied to a mist nozzle (Ikeuchi Co., Ltd. "Standard Fan-Shaped Nozzle Model 1 / 4M-VVP-5010-S303") at a pump rotation speed of 55 Hz (flow rate of approximately 1.7 kg / min), atomized, and sprayed towards the inlet of a rotating drum that was being cooled while rotating. After the molten material cooled in the rotating drum and became spherical powder in the air, the powder was collected from the outlet on the opposite side of the inlet (sometimes referred to as "atomized product"). For comparison, the same α-olefin copolymer was mechanically ground using a vertical cutting mill (orient mill) and / or a quick mill, and the powder was recovered (sometimes referred to as "mechanically ground product").
[0057] The atomized and mechanically ground products were sieved in stages using JIS standard stainless steel sieves (Tokyo Screen Co., Ltd., frame dimensions 200mm diameter x 60mm, specification JIS Z8801-1:2000) with mesh sizes of 500μm, 250μm, 150μm, 105μm, 63μm, or 44μm. After removing the fractions that did not pass through 500μm and those that passed through 44μm, the following fractions were collected: 500-250μm, 250-150μm, 150-105μm, 105-63μm, and 63-44μm. The atomized products contained almost no fractions that did not pass through 500μm.
[0058] Using each fraction, the following seven types of temperature control agent samples and temperature control agent samples of 500-250 μm were prepared and used in the production of the exothermic composition: (1) 250-150 μm (2) 150-105 μm (3) 105 μm-63 μm (4) 63 μm-44 μm (5) 250-44 μm (equal weight mixture of (1)-(4) above) (6) 150-44 μm (equal weight mixture of (2)-(4) above) (7) 105-44 μm (equal weight mixture of (3) and (4) above) Representative digital microscope photographs and images (described later) of the prepared temperature control agent samples (samples (4) and (3) above) are shown in Figure 1.
[0059] <Measurement of Circularity> For each sample obtained above, the average circularity was calculated. Each temperature control agent sample, which had been atomized above, was spread out so that the particles did not overlap as much as possible, and photographed using a digital microscope (KEYENCE Corporation main unit "VHX-500F", lens "VH-Z100R") and recorded as an image. Binarization was performed using image processing software (ImageJ), and the area and perimeter of the particle projection diagram were measured for each individual particle. In this case, areas corresponding to a diameter less than half of the sieve lower limit were excluded from evaluation (for example, if the lower limit is a mesh opening of 44 μm, a diameter of 22 μm (i.e., an area of 379 μm) was excluded). 2 (The following were excluded.) The degree of circularity was calculated using the following formula: Circularity = 4π × Area / (Perimeter) 2 ... (Equation 1) The average value of 80 to 100 particles with circularity calculated in this way was taken as the average circularity of the particles in each sample of Examples 1 to 4 and Comparative Examples 1 to 4.
[0060] Table 1 shows the average circularity calculated for each sample. For Examples 5-7 and Comparative Examples 5-7, since they were prepared by blending Examples 1-4 and Comparative Examples 1-4 in weight ratio, the average circularity of the blended samples was weighted based on the number of particles contained (C in Table 1) and adopted as the average circularity of the samples.
[0061]
[0062] <Manufacturing of the Heat-Generating Composition (1)> As raw materials for the heat-generating composition, iron powder (Powdertech Co., Ltd., reduced iron powder "RDH-3M"), activated carbon (Dainen Co., Ltd., activated carbon (moist carbon) "PL-1P (30% wet)"), superabsorbent polymer (Sanyo Chemical Industries, Ltd., polyacrylate resin "ST-500D*"), crystalline cellulose (Asahi Kasei Chemicals Corporation, crystalline cellulose "TG-101"), sodium chloride (Nihon Kaisui Co., Ltd., powdered salt "EF-300"), and one of the temperature control agents manufactured above are used, with 45 parts of iron powder and activated carbon. An exothermic composition was prepared by mixing 8.4 parts of activated carbon (wet carbon), 5 parts of superabsorbent polymer, 30 parts of crystalline cellulose, 3.5 parts of sodium chloride, and 25 parts of a temperature control agent (all "parts" are in parts by weight). Specifically, considering bulk density and particle size, the crystalline cellulose, aliphatic compound (temperature control agent), superabsorbent polymer, activated carbon, sodium chloride, and iron powder were weighed and added to a beaker in that order. The mixture was thoroughly stirred with a spatula to eliminate any uneven distribution of each ingredient. The composition of each exothermic composition sample is shown in Table 2.
[0063]
[0064] <Manufacturing of a small heating element> A small heating element consisting of a container body (2) containing a heat-generating composition tablet (1) and a top material (3), similar to the example shown in Figure 4, was manufactured as follows.
[0065] 1.2 g of the exothermic composition prepared as described above was weighed and compressed into tablets using Fuji Pharmaceutical Machinery Co., Ltd.'s "Quick Mini FY-TQM-30 Desktop Prototype Tablet Press" (compression pressure 10 kN). A male die (punch) with a diameter of 13.9 mm and a receiving die (die) with an inner diameter of 14 mm were used to produce cylindrical tablets with a diameter of 14 mm and a thickness of 5 mm.
[0066] The container for housing the heat-generating composition tablets was manufactured as follows: First, a male mold in the shape of a truncated cone with a base diameter of 20 mm, a top diameter of 15 mm, and a height of 8 mm was prepared, and a female mold for receiving the tablets with a cylindrical shape with a hole of 21 mm in diameter and a height of 25 mm was prepared. The male mold was heated to 105°C. A moldable nonwoven fabric (Asahi Kasei Corporation thermoformable PET spunbond nonwoven fabric "Smash Y15250" (basis weight 250 g / m²)) was placed on the female mold. 2) was pressed and pushed in with a heated male mold, held for 3 seconds, then cooled by blowing room-temperature compressed air for an additional 3 seconds, and the male mold was immediately pulled out from the female mold to produce a cup-shaped molded article.
[0067] A tablet was placed in the molded nonwoven fabric cup, and a top material (PET separator (38 μm) / rubber-based hot-melt pressure-sensitive adhesive (100 g / m 2 ) / PET spunlace nonwoven fabric (basis weight 50 g / m 2 ) / PET film (12 μm) / PE film (30 μm)) was attached to the upper part of the container (the bottom surface side of the truncated cone) using a cylindrical welding mold heated to 160°C. Further, 0.39 g of a 2% sodium sulfite aqueous solution was injected from the top material using a syringe. The resultant was hermetically sealed in an airtight outer bag (PET (12 μm) / aluminum foil (7 μm) / LLDPE (50 μm), manufactured by Toho Processing Co., Ltd.) to obtain heat generators of Examples 1 to 7 and Comparative Examples 1 to 7, respectively.
[0068] <Measurement of Melting Point and Solubility> The melting point of the aliphatic compound was measured using a differential scanning calorimeter. As the measurement apparatus, a differential scanning calorimeter (DSC6220, all the above measurement instruments are manufactured by Seiko Instruments Inc.) connected to a fully automatic cooling unit and an analysis system (EXSTAR6000 thermal analysis rheology system, the software being DSC Muse measurement software and DSC Muse standard analysis software) was used, and as sample containers, an open-type sample container made of Al, φ5.2 H2.5 (50 μL), and an open-type sample container made of Al (crimp cover) were used.
[0069] 5 mg to 15 mg of a sample was placed in an Al container, an Al crimp cover was placed thereon, and a constant pressure was applied to seal the container. Using the Al container + crimp cover as a reference, the temperature was raised from -50°C of the estimated melting point to +30°C of the estimated melting point at a temperature elevation rate of 5°C / min. After holding for 5 minutes, the mixture was cooled at the same rate and held at the estimated melting point of -50°C for 5 minutes. This was repeated twice, and the DSC curve of the second cycle (2nd-run) was measured. The melting point was determined as described above from the endothermic peak appearing on the DSC curve due to the endotherm accompanying the melting of the sample.
[0070] The solubility of an aliphatic compound powder in water was measured by dissolving it in 100 g (100 mL) of water at 20°C and reading the mass at which it could no longer dissolve.
[0071] The melting point of the α-olefin copolymer used was 58°C. Its solubility was less than 1 g / 100 mL.
[0072] <Age-Restoration Test (Storage Test)> The storage test was conducted using an Advantec Toyo Co., Ltd. low-temperature constant temperature and humidity chamber THE051FA at 50°C and 35% relative humidity. Two weeks of storage at 50°C is equivalent to one year of storage at room temperature. Similarly, four weeks (one month) at 50°C is considered equivalent to 1.5 years at room temperature, and eight weeks (two months) is considered equivalent to 3.0 years. The temperature setting of 50°C was determined considering conversion to room temperature using an Arrhenius plot, as well as warehouse storage and maritime container transport.
[0073] <Heat Generation Test of Small Heating Devices> The heat generation test was conducted in accordance with the method of JIS S4100 "Disposable Hand Warmers," under the conditions of an ambient temperature of 20±1℃, a wind speed of 0.5 m / s or less (windless), an ambient humidity of 55-70%, and a heating element temperature of 30±1℃ in a heating device consisting of a heater and a circulating constant-temperature water bath. Since small heating devices are applied directly to the skin when in use, the device was attached directly to the surface of the heater for measurement.
[0074] Specifically, the heat generation test was conducted using a tank-shaped heater measuring W615 x D410 x H60 mm (using an 8 mm thick PVC plate) placed in a constant temperature room set to 20°C and 65% humidity. 8 L / min of hot water was circulated from an adjacent circulating constant temperature water bath to control the surface temperature of the heater (PVC plate) to 30°C. A PET separator was removed from a small heating element sample, a temperature sensor was attached to the hot-melt adhesive near the center of the bottom surface, and the sample was then attached to the PVC plate on the heater surface (temperature measuring device: Chino Graphic Recorder KR2S00; sensor: Anritsu Keiki Co., Ltd., "ST-22E-005").
[0075] The results are shown in Figures 2 and 3. The evaluation of the results is shown in Tables 3 and 4.
[0076]
[0077] Figures 2 and 3 and Tables 3 and 4 show that conventional heating elements using temperature control agents deteriorate relatively quickly after storage at high temperatures compared to heating elements using the temperature control agent of the present invention, and cannot maintain their performance for a long period of time. In contrast, heating elements using the temperature control agent of the present invention maintained stable and good performance even after long-term storage at high temperatures, even when containing small-sized particles. In particular, Example 4 consisted only of small-sized particles, and although its evaluation was inferior to the other examples, good results were obtained even when some particles of this size were included (Examples 5 to 7).
[0078] Furthermore, in each of the examples, the degree of temperature decrease 1 to 10 minutes after reaching the maximum temperature tended to be smaller compared to the comparative example's heating element. Also, the duration of heat generation after reaching 40°C until the temperature fell below 40°C tended to be longer in the examples' heating elements. The temperature decrease rate was calculated using the following formula: Temperature decrease rate (%) = {(Maximum heat generation temperature - Temperature at a given point in time) / Maximum heat generation temperature} × 100 ... (Formula 2)
[0079] <Manufacturing of the Heat-Generating Composition (2)> The raw materials for the heat-generating composition are iron powder (Höganäs Japan Co., Ltd. Reduced Iron Powder "InSIP"), activated carbon (Dainen Co., Ltd. Activated Carbon (Wet Carbon) "PL-1P (30% Wet)"), and vermiculite (Belmitec Co., Ltd.) An exothermic composition was prepared by mixing 56 parts iron powder, 8.9 parts activated carbon (moist carbon), 5.2 parts vermiculite, 2.6 parts superabsorbent polymer, 3.6 parts sodium chloride, 23.7 parts water, and 10 or 20 parts of the temperature control agent (all "parts" are by weight) using "No. 1"), superabsorbent polymer (Sanyo Chemical Industries, Ltd. polyacrylate resin "ST-500D*"), sodium chloride (Nippon Kaisui Co., Ltd. powdered salt "EF-300"), water, and one of the temperature control agents prepared as described above. Specifically, each weighed raw material was sealed in a PE bag and shaken well for 30 seconds to mix thoroughly and eliminate any uneven distribution of the raw materials. The composition of each exothermic composition sample is shown in Table 5.
[0080]
[0081] <Preparation of Exothermic Compositions (3)> Samples of each exothermic composition with the compositions shown in Table 6 were prepared in the same manner as in "Preparation of Exothermic Compositions (2)" above. For Example 11 and Comparative Example 11, fractions of 500 to 250 μm were used, which were prepared in "Preparation of Temperature Control Agents" above and whose average circularity was measured as described in "Measurement of Circularity" above.
[0082]
[0083] <Manufacturing of disposable hand warmer-type heating elements> The heat-generating composition manufactured above was placed in packaging material to manufacture a disposable hand warmer-type heating element. 35 g of the heat-generating composition was placed in a breathable material (composed of Kojin Film & Chemicals Co., Ltd.: PET spunlace nonwoven fabric (basis weight 30 g / m)). 2 The surface material is a porous film (70 μm) (see Tables 5 and 6 for air permeability), and the adhesive material is made by Ferric Co., Ltd. (composition: paper separator 40 g / m²). 2 The contents were placed in a 95 mm x 130 mm bag with a 23 μm acrylic adhesive and a 60 μm PE film as the backing material, and then sealed by heat sealing to form a hand warmer. The prepared hand warmers were sealed in an airtight outer bag (12 μm PET, 7 μm aluminum foil, 50 μm LLDPE (Toho Kako Co., Ltd.)) and used as the heating elements for Examples 8-15 and Comparative Examples 8-15, respectively.
[0084] <Heat Generation Test of Hand Warmers> The heat generation test was conducted in a constant temperature and humidity chamber with an ambient temperature of 20±1℃, a wind speed of 0.5 m / s or less (windless), and an ambient humidity of 55-70%, using a heat generation tester compliant with JIS S4100 "Disposable Hand Warmers". For a certain period after the start of heat generation, the hand warmer was kept at a temperature where the temperature control agent did not melt without covering it with a flannel cloth. To reproduce the overheating state, excessive heat generation was artificially induced by covering the hand warmer with a flannel cloth 1.5 hours or 2 hours after the start of heat generation, causing the temperature control agent to melt. The temperature decrease rate was calculated using Equation 2 above. The heat generation patterns and the temperature decrease rates over time after reaching the maximum temperature for these heating elements are shown in Figures 5-13 and Tables 7 and 8.
[0085]
[0086]
[0087] In Examples 8 to 15, although the temperature at which the temperature rise was stopped by the melting of the temperature control agent (maximum temperature) after excessive heat generation was induced was equivalent to that of the comparative example, the subsequent rate of temperature decrease was low, and it was observed that the heating element could maintain heat generation for a longer period even after excessive heat generation was prevented.
[0088] From the above results, it became clear that the heating element using the exothermic composition containing the temperature control agent of the present invention is hardly affected by long-term storage in terms of its maximum exothermic temperature. Furthermore, even with a heating element using the same amount of exothermic composition, the temperature decrease after reaching the maximum exothermic temperature was slowed down, making it possible to provide a heating element with a longer duration of heat generation than conventional ones.
[0089] Therefore, a heating element using the exothermic composition containing the temperature control agent of the present invention has even greater temperature stability and safety compared to a heating element using a conventional temperature control agent, and can maintain its designed heating performance for a long period of time.
[0090] 1. Heat-generating composition 2. Container (main body) 3. Top material 3a. Sealant material 3b. Nonwoven fabric 3c. Adhesive 3d. Release paper
Claims
1. A temperature control agent containing an aliphatic compound, used to control the exothermic temperature of a heating element that contains an exothermic composition that reacts with oxygen to generate heat, wherein the aliphatic compound has a melting point of 35°C or higher, a water solubility of 5 g / 100 mL or less at 20°C, and is in particulate form with an average circularity of 0.70 to 1.
0.
2. The temperature control agent according to claim 1, wherein the aliphatic compound is in a particulate form that does not pass through a 325-mesh standard sieve (standard dimensions according to JIS Z8801-1: 44 μm).
3. The temperature control agent according to claim 1, wherein the aliphatic compound is in a particulate form that can pass through a 16-mesh standard sieve (standard dimensions according to JIS Z8801-1: 1000 μm).
4. The temperature control agent according to claim 1, wherein the aliphatic compound is in a particulate form that does not pass through a 325-mesh standard sieve (standard dimensions according to JIS Z8801-1: 44 μm) and is in a particulate form that passes through a 16-mesh standard sieve (standard dimensions according to JIS Z8801-1: 1000 μm).
5. The temperature control agent according to claim 1, wherein the aliphatic compound contains one or more compounds selected from the group consisting of higher α-olefin copolymers, paraffin wax, myristyl myristate, polyester polyols, and polyoxyethylene fatty acid diesters.
6. The temperature control agent according to claim 2, wherein the aliphatic compound contains one or more compounds selected from the group consisting of higher α-olefin copolymers, paraffin wax, myristyl myristate, polyester polyols, and polyoxyethylene fatty acid diesters.
7. The temperature control agent according to claim 3, wherein the aliphatic compound contains one or more compounds selected from the group consisting of higher α-olefin copolymers, paraffin wax, myristyl myristate, polyester polyols, and polyoxyethylene fatty acid diesters.
8. The temperature control agent according to claim 4, wherein the aliphatic compound contains one or more compounds selected from the group consisting of higher α-olefin copolymers, paraffin wax, myristyl myristate, polyester polyols, and polyoxyethylene fatty acid diesters.
9. An exothermic composition that generates heat in reaction with oxygen, wherein the exothermic composition comprises metal powder, salts, water, activated carbon, and a temperature control agent for controlling the exothermic temperature of the exothermic composition, characterized in that the temperature control agent is the temperature control agent according to any one of claims 1 to 8.
10. A heating element comprising the heat-generating composition according to claim 9, and a bag or container in which the heat-generating composition is contained, the bag or container being at least partially breathable.
11. The heating element according to claim 10, wherein the bag or container is housed in an airtight outer bag that substantially blocks oxygen.
12. The heating element according to claim 10, which is used as either a disposable hand warmer or a medical device.
13. The heating element according to claim 12, wherein the medical device is either a warm compress or a heat device for stimulating meridians.
14. A method for producing a temperature control agent according to any one of claims 1 to 8, characterized in that it includes a step of atomizing a molten material obtained by melting the aliphatic compound or the temperature control agent into spherical particles.