Resin composition, pellet, and molded article

A resin composition with polycarbonate, polyester, talc, and specific additives addresses silver formation and resistance issues, ensuring heat stability and impact resistance in molded products.

WO2026234901A1PCT designated stage Publication Date: 2026-11-12MITSUBISHI ENG PLASTICS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/010054
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2026-03-16
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Polycarbonate resin compositions incorporating talc suffer from silver formation, changes in physical properties, and poor heat and humidity resistance when left standing, particularly when blended with polyester resin.

Method used

A resin composition comprising polycarbonate resin, polyester resin, talc, an organic phosphate ester compound, and a metal sulfonate salt, with specific mass ratios and concentrations to enhance heat stability and resistance.

Benefits of technology

The composition achieves excellent heat retention stability and heat resistance, suppressing silver formation and maintaining impact resistance in molded products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

A resin composition according to the present disclosure contains 5-20 parts by mass of talc (C), 0.05-0.30 parts by mass of an organic phosphoric acid ester compound (D), and 0.05-0.30 parts by mass of a sulfonic acid metal salt (E) per a total of 100 parts by mass of 50-90 parts by mass of a polycarbonate resin (A) and 10-50 parts by mass of a polyester resin (B), wherein (D) / (E), which is the mass ratio of the organic phosphoric acid ester compound (D) and the sulfonic acid metal salt (E), is 1.0 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Resin compositions, pellets, and molded articles

[0001] This invention relates to resin compositions, pellets, and molded articles. In particular, it relates to resin compositions having polycarbonate resin as a main component.

[0002] Polycarbonate resins possess excellent mechanical and thermal properties and are used in a variety of applications, primarily in the fields of office automation equipment and electronic and electrical equipment. Furthermore, as a method to improve the rigidity, strength, and dimensional properties of polycarbonate resins, it is common practice to incorporate inorganic fillers, and in fields where a good appearance is required, the inclusion of talc has been proposed (Patent Documents 1 and 2).

[0003] Japanese Patent Publication No. 2005-154582 Japanese Patent Publication No. 2007-284502

[0004] In applications where polycarbonate resin is required to be fluid, polyester resin is sometimes blended with it. To increase the rigidity of such polycarbonate and polyester resin alloys, the addition of talc has been considered. However, the addition of talc damages the polycarbonate resin. In particular, it has been found that when the resin composition is left standing, silver formation may occur in the resulting molded product, its physical properties may change, and the resulting molded product may have poor heat and humidity resistance. The present invention aims to solve these problems and provides a resin composition containing polycarbonate resin, polyester resin, and talc, which exhibits excellent heat stability and heat and humidity resistance, as well as pellets and molded products.

[0005] Based on the above problems, the inventors conducted studies and found that the above problems can be solved by further blending an organic phosphate ester compound (D) and a metal sulfonate salt (E) in a predetermined blending ratio into a resin composition containing polycarbonate resin, polyester resin, and talc. Specifically, the above problems were solved by the following means: [1] A resin composition comprising 100 parts by mass in total, consisting of 50 to 90 parts by mass of polycarbonate resin (A) and 10 to 50 parts by mass of polyester resin (B), 5 to 20 parts by mass of talc (C), 0.05 to 0.30 parts by mass of an organic phosphate ester compound (D), and 0.05 to 0.30 parts by mass of a metal sulfonate salt (E), wherein the mass ratio of the organic phosphate ester compound (D) to the metal sulfonate salt (E), (D) / (E), is 1.0 or more. [2] The resin composition according to [1], wherein the mass ratio (D) / (E) of the organic phosphate ester compound (D) to the metal sulfonate salt (E) is 2.0 to 5.0. [3] The resin composition according to [1] or [2], wherein the talc (C) content is 10 to 20 parts by mass per 100 parts by mass of the total of 50 to 90 parts by mass of the polycarbonate resin (A) and 10 to 50 parts by mass of the polyester resin (B). [4] The resin composition according to any one of [1] to [3], wherein the polyester resin (B) comprises polyethylene terephthalate resin. [5] The resin composition according to any one of [1] to [4], wherein the organic phosphate ester compound (D) comprises at least one of the compound represented by formula (P1), the compound represented by formula (P2), and the compound represented by formula (P3). (In formulas (P1) and (P2), M is independently zinc and magnesium, and R x Each of these independently represents a linear or branched alkyl group having 3 to 30 carbon atoms. (Formula (P3)) (In formula (P3), R represents a linear or branched alkyl group having 3 to 30 carbon atoms. nx represents 1 or 2.) [6] The resin composition according to any one of [1] to [5], wherein the sulfonic acid metal salt (E) comprises an aromatic sulfonic acid metal salt. [7] The resin composition according to any one of [1] to [6], wherein the mass ratio (D) / (E) of the organic phosphate ester compound (D) to the metal sulfonic acid salt (E) is 2.0 to 5.0, the talc (C) content is 10 to 20 parts by mass with respect to a total of 100 parts by mass of 50 to 90 parts by mass of the polycarbonate resin (A) and 10 to 50 parts by mass of the polyester resin (B), the polyester resin (B) comprises polyethylene terephthalate resin, the organic phosphate ester compound (D) comprises at least one of the compound represented by formula (P1), the compound represented by formula (P2), and the compound represented by formula (P3), and the metal sulfonic acid salt (E) comprises an aromatic metal sulfonic acid salt. (In formulas (P1) and (P2), M is independently zinc and magnesium, and R x Each of these independently represents a linear or branched alkyl group having 3 to 30 carbon atoms. (Formula (P3)) (In formula (P3), R represents a linear or branched alkyl group having 3 to 30 carbon atoms. nx represents 1 or 2.) [8] The resin composition according to [7], wherein the organophosphate ester compound (D) comprises the compound represented by (P3), and the sulfonic acid metal salt (E) comprises an aromatic sulfonic acid potassium salt. [9] Pellets of the resin composition according to any one of [1] to [8].

[10] A molded article formed from the resin composition according to any one of [1] to [8].

[11] A molded article formed from the pellets according to [9].

[0006] The present invention makes it possible to provide a resin composition comprising polycarbonate resin, polyester resin, and talc, which exhibits excellent heat retention stability and heat resistance, as well as pellets and molded articles.

[0007] The following describes in detail embodiments for carrying out the present invention (hereinafter simply referred to as "this embodiment"). Note that the following embodiments are illustrative examples for explaining the present invention, and the present invention is not limited to these embodiments. In this specification, "~" is used to mean that the numerical values ​​described before and after it include the lower and upper limits. Furthermore, the upper and lower limits of numerical values ​​in this specification are given as examples of this embodiment, regardless of the combination of the upper and lower limits. In this specification, preferred combinations of embodiments are more preferred embodiments. In this specification, various physical properties and characteristic values ​​are given at 23°C unless otherwise specified. If the measurement methods, etc., described in the standards shown in this specification differ from year to year, unless otherwise specified, the standards as of January 1, 2025 shall be used. If the measurement methods, etc., described in the standards shown in this specification are obsolete as of January 1, 2025, the standards at the time of obsolete shall be used.

[0008] The resin composition of this embodiment contains 50 to 90 parts by mass of polycarbonate resin (A) and 10 to 50 parts by mass of polyester resin (B), totaling 100 parts by mass, 5 to 20 parts by mass of talc (C), 0.05 to 0.30 parts by mass of an organic phosphate ester compound (D), and 0.05 to 0.30 parts by mass of a metal sulfonic acid salt (E), characterized in that the mass ratio of the organic phosphate ester compound (D) to the metal sulfonic acid salt (E), (D) / (E), is 1.0 or more. By adopting such a configuration, it is possible to provide a resin composition with excellent heat retention stability and heat resistance to moisture. Polyester resin may be added to improve the fluidity of the polycarbonate resin. Furthermore, talc may be added to the polycarbonate resin and polyester resin alloy to increase rigidity. However, adding talc often damages the polycarbonate resin. In particular, the damage tends to be more severe when untreated talc is used. Under these circumstances, the inventors considered incorporating an acidic substance to cap the reaction sites on the surface of talc (C). However, it was found that incorporating an acidic substance could impair the heat retention stability and heat resistance.

[0009] Under these circumstances, the inventors conducted further investigations and found that in this embodiment, the above problems can be solved by blending an organic phosphate ester compound (D) and a metal sulfonate salt (E) as acidic substances in a predetermined ratio. Specifically, the inventors considered incorporating a metal sulfonate salt (E) to suppress the rise in the Q value during retention. However, it was found that when a metal sulfonate salt (E) was incorporated into a resin composition containing polycarbonate resin, polyester resin, and talc, the silver generated in the molded product during retention molding worsened. On the other hand, it was found that when an organic phosphate ester compound (D) was incorporated into a resin composition containing polycarbonate resin, polyester resin, and talc, the generation of silver in the molded product during retention molding tended to be suppressed. However, it was found that when an organic phosphate ester compound (D) was incorporated, the rise in the Q value during retention could not be sufficiently suppressed, and the impact resistance significantly decreased under humid heat. It was found that incorporating a metal sulfonate salt (E) was effective in suppressing this significant decrease in impact resistance. Furthermore, surprisingly, it was found that incorporating both the organic phosphate ester compound (D) and the metal sulfonate salt (E) was beneficial in terms of the Q value. Based on the above considerations, it is presumed that in this embodiment, by incorporating both the organic phosphate ester compound (D) and the metal sulfonate salt (E) and precisely adjusting their amounts, we succeeded in providing a resin composition with excellent heat retention stability and resistance to humid heat.

[0010] The embodiments of the present invention will be described in detail below, but the description of the constituent elements described below is merely one example of an embodiment of the present invention and is not limited to these.

[0011] <Polycarbonate Resin (A)> The resin composition of this embodiment includes polycarbonate resin (A). Specifically, polycarbonate resin (A) is not particularly limited as long as it contains a carbonate ester bond--[O-R-OC(=O)]- unit in the molecular main chain (where R is an organic group, preferably a hydrocarbon group, more preferably an aliphatic group, an aromatic group, or a group containing both an aliphatic and an aromatic group, and furthermore has a linear or branched structure). In this embodiment, polycarbonate resin (A) is preferably an aromatic polycarbonate resin, and more preferably a polycarbonate resin having a bisphenol skeleton. By using such a polycarbonate resin, better heat resistance and toughness can be achieved. In this embodiment, in the polycarbonate resin having a bisphenol skeleton, it is preferable that 90 mol% or more of the total constituent units are constituent units having a bisphenol skeleton, and it is more preferable that 90 mol% or more of the total constituent units are constituent units derived from bisphenol A.

[0012] Furthermore, the viscosity-average molecular weight (Mv) of the polycarbonate resin (A) is preferably 10,000 or more, more preferably 12,000 or more, and even more preferably 15,000 or more. Setting it above the lower limit tends to further improve the durability of the resulting molded product. The upper limit of the viscosity-average molecular weight (Mv) of the polycarbonate resin (A) is preferably 50,000 or less, more preferably 40,000 or less, and even more preferably 30,000 or less. Setting it below the upper limit tends to further improve the moldability of the molded product. The viscosity-average molecular weight (Mv) is determined by using methylene chloride as the solvent, and calculating the intrinsic viscosity [η] (unit dL / g) at a temperature of 25°C using an Ubbelohde viscometer, and using Schnell's viscosity formula, i.e., η = 1.23 × 10⁻⁶. -4 ×Mv 0.83 This refers to the value calculated from [the specified values]. When using two or more types of polycarbonate resin, the viscosity-average molecular weight of the mixture is used.

[0013] The method for producing the polycarbonate resin (A) is not particularly limited, and conventionally known methods such as the phosgene method (interfacial polymerization) or the melting method (transesterification) can be used. Furthermore, when using the melting method, a polycarbonate resin with an adjusted amount of OH groups at the end groups can be used.

[0014] The polycarbonate resin (A) used in this embodiment may be recycled polycarbonate resin. In this embodiment, even when using recycled polycarbonate resin, excellent performance equivalent to that of virgin polycarbonate resin can be achieved. Recycled polycarbonate resin refers to virgin polycarbonate resin that has undergone some kind of molding or processing process, and includes not only products collected from the market, but also rejected polycarbonate resin molded products and scraps from the manufacture of polycarbonate resin molded products. Molded products include injection molded products, extruded products, and molded products formed by other manufacturing methods. Examples of recycled polycarbonate resin include those obtained by material recycling, where collected used polycarbonate resin molded products are crushed, alkaline washed, and reused as fibers, those obtained by chemical recycling (chemical decomposition method), and those obtained by mechanical recycling. Chemical recycling involves chemically decomposing collected used polycarbonate resin molded products to return them to their raw material level and resynthesize polycarbonate resin. Mechanical recycling, on the other hand, is a method that makes it possible to reliably remove contaminants from polycarbonate resin molded products more effectively than material recycling by performing more rigorous alkaline cleaning than in the material recycling method described above, or by vacuum drying at high temperatures. For example, after foreign matter is removed from used polycarbonate resin molded products, they are crushed and washed, and then pelletized using an extruder to obtain recycled polycarbonate resin. Examples of used polycarbonate resin molded products include discs, sheets (including films), meter covers, headlamp lenses, and bottles.

[0015] For further details regarding the polycarbonate resin (A), please refer to paragraphs 0013 to 0041 of Japanese Patent Publication No. 2021-084942, paragraphs 0040 to 0073 of Japanese Patent Publication No. 2019-035001, paragraphs 0016 to 0043 of Japanese Patent Publication No. 2018-103518, paragraphs 0011 to 0048 of International Publication No. 2021 / 090823, and paragraphs 0011 to 0043 of Japanese Patent Publication No. 2019-156942, in addition to the above, and these contents are incorporated herein by reference.

[0016] <Polyester Resin (B)> The resin composition of this embodiment includes polyester resin (B). Examples of polyester resins used in this embodiment include polyethylene terephthalate resin and polybutylene terephthalate resin, with polyethylene terephthalate resin being more preferred. Polyethylene terephthalate resin is a polyester resin that includes constituent units derived from diols and constituent units derived from dicarboxylic acids, wherein 70 mol% or more of the constituent units derived from diols are derived from ethylene glycol, and 60 mol% or more of the constituent units derived from dicarboxylic acids are derived from at least one selected from terephthalic acid and its esters (preferably terephthalic acid). Preferably, 85 mol% or more, more preferably 90 mol% or more, even more preferably 95 mol% or more, and even more preferably 99 mol% or more of the constituent units derived from diols are derived from ethylene glycol. Preferably, 70 mol% or more, more preferably 80 mol% or more, and even more preferably 90 mol% or more of the constituent units derived from dicarboxylic acids are derived from at least one selected from terephthalic acid and its esters. The upper limit may be 100 mol%, and 99 mol% or less is preferred.

[0017] The polyester resin used in this embodiment may further contain other structural units derived from diols, such as structural units derived from 1,4-cyclohexanedimethanol. However, in this embodiment, it is preferable that 85 mol% or more, more preferably 90 mol% or more, even more preferably 95 mol% or more, and even more preferably 99 mol% or more of the structural units derived from diols are ethylene glycol. Furthermore, the polyester resin used in this embodiment may further contain other structural units derived from dicarboxylic acids, such as structural units derived from isophthalic acid and / or structural units derived from naphthalenedicarboxylic acid. However, in this embodiment, it is preferable that 85 mol% or more, more preferably 90 mol% or more, even more preferably 95 mol% or more, and even more preferably 99 mol% or more of the structural units derived from dicarboxylic acids are terephthalic acid and its esters.

[0018] In this embodiment, the polyester resin is composed of, preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more of all constituent units excluding the terminal groups, which are derived from diols and dicarboxylic acids.

[0019] The polyester resin contained in the polyester resin layer may be a crystalline polyester resin having a clear melting point, or an amorphous polyester resin not having a clear melting point, but it is preferable that it be a crystalline polyester resin having a melting point. The melting point of the polyester resin in this embodiment is preferably 150°C or higher, more preferably 200°C or higher, even more preferably 220°C or higher, and also preferably 300°C or lower, more preferably 290°C or lower, and even more preferably 280°C or lower. If the polyester resin layer in this embodiment contains two or more types of polyester resins, the melting point of the polyester resin is the value obtained by multiplying the melting point of each polyester resin by its mass fraction.

[0020] The intrinsic viscosity of the polyester resin is preferably 0.30 dL / g or more, more preferably 0.40 dL / g or more, and even more preferably 0.50 dL / g or more. Further, the intrinsic viscosity is preferably 2.00 dL / g or less, more preferably 1.50 dL / g or less, even more preferably 1.00 dL / g or less, and still more preferably 0.80 dL / g or less. When the polyester resin layer in the present embodiment contains two or more types of polyester resins, the intrinsic viscosity refers to the intrinsic viscosity of the polyester resin mixture.

[0021] The intrinsic viscosity is measured according to the following method. A polyester resin (pellet) is dissolved in a mixed solvent of phenol / 1,1,2,2-tetrachloroethane (mass ratio 1 / 1) by stirring at 110°C for 1 hour so that the concentration becomes 1.00 g / dL. Thereafter, the resulting solution is cooled to 30°C. Using a fully automatic solution viscometer, the falling seconds of the sample solution and the falling seconds of the solvent alone are each measured at 30°C, and the intrinsic viscosity is calculated by the following formula (1). Intrinsic viscosity = ((1 + 4K H η sp ) 0.5 -1) / (2K H C) ... (1) where η sp = η / η 0 -1, η is the falling seconds of the sample solution, η 0 is the falling seconds of the solvent alone, C is the concentration of the sample solution (g / dL), and K H is the Huggins constant. K H is set to 0.33.

[0022] In addition to the above, as the polyester resin, the polyester resins described in paragraphs 0064 to 0080 of JP-A-2016-169027, the polyester resins described in paragraphs 0010 to 0021 of JP-A-2006-111718, the polyester resins described in JP-A-2017-105873, and the polyester resins described in International Publication No. 2013 / 168804 can be referred to, and the contents of these documents are incorporated into the present specification.

[0023] In this embodiment, it is preferable that the polyester resin used is not a water-soluble polyester resin. Furthermore, it is preferable that the polyester resin used in this embodiment is not an ionic polyester resin.

[0024] <Blend of Polycarbonate Resin (A) and Polyester Resin (B)> In the resin composition of this embodiment, the composition contains 10 to 50 parts by mass of polyester resin (B) per 50 to 90 parts by mass of polycarbonate resin (A). In this embodiment, the content of polycarbonate resin (A) per 100 parts by mass of the total of polycarbonate resin (A) and polyester resin (B) is preferably 55 parts by mass or more, more preferably 60 parts by mass or more, even more preferably 65 parts by mass or more, even more preferably 70 parts by mass or more, and preferably 85 parts by mass or less, more preferably 80 parts by mass or less, and even more preferably 78 parts by mass or less. Setting the content above the lower limit tends to further improve the toughness, such as impact resistance, of the resulting molded product. Setting the content below the upper limit tends to result in the resin composition exhibiting better fluidity.

[0025] The total content of polycarbonate resin (A) and polyester resin (B) in the resin composition of this embodiment is preferably 70% by mass or more, more preferably 75% by mass or more, preferably 90% by mass or less, and more preferably 85% by mass or less, based on 100% by mass of the resin composition. The resin composition of this embodiment may contain only one type of polycarbonate resin (A) and polyester resin (B), or may contain two or more types. When two or more types of polycarbonate resin (A) and / or polyester resin (B) are included, it is preferable that the total amount is within the above range.

[0026] <Talc (C)> The resin composition of this embodiment contains talc (C). By including talc (C), the rigidity of the resulting molded product can be improved. The talc preferably has a number average particle diameter of 0.1 μm or more, more preferably 0.5 μm or more, even more preferably 1 μm or more, preferably 30 μm or less, more preferably 20 μm or less, even more preferably 10 μm or less, even more preferably 5 μm or less, and even more preferably 3 μm or less.

[0027] The talc may or may not be surface-treated. Using surface-treated talc can reduce the damage that talc inflicts on the polycarbonate resin. For surface-treated talc, refer to paragraphs 0021 to 0037 of Japanese Patent Application Publication No. 2020-045419, which are incorporated herein by reference. On the other hand, in this embodiment, it is also possible to use a configuration that does not use untreated talc. In this embodiment, since the damage that talc inflicts on the polycarbonate resin tends to be suppressed, sufficient physical properties can be ensured without relying on surface treatment agents. Untreated talc tends to be less expensive, making it more economical.

[0028] Furthermore, in this embodiment, the talc may or may not be granulated. For granulated talc, refer to paragraphs 0021 to 0039 of Japanese Patent Application Publication No. 2020-045419, which are incorporated herein by reference. On the other hand, in this embodiment, a configuration without granulated talc is also possible. In this embodiment, since the damage that talc inflicts on the polycarbonate resin tends to be suppressed, sufficient physical properties can be ensured even without granulating the talc to avoid contact with the polycarbonate resin. Ungranulated talc tends to be less expensive, making it more economical.

[0029] The talc (C) content in the resin composition of this embodiment is 5 parts by mass or more, preferably 7 parts by mass or more, more preferably 10 parts by mass or more, even more preferably 12 parts by mass or more, even more preferably 15 parts by mass or more, and 20 parts by mass or less, based on 100 parts by mass of the total of polycarbonate resin (A) and polyester resin (B). Setting the talc (C) content above the lower limit tends to further improve the rigidity of the resulting molded product. Setting the talc (C) content below the upper limit tends to more effectively suppress the generation of silver and changes in the Q value during the retention molding of the resin composition.

[0030] The talc (C) content in the resin composition of this embodiment is preferably 4% by mass or more, more preferably 7% by mass or more, even more preferably 9% by mass or more, even more preferably 11% by mass or more, and preferably 20% by mass or less, and more preferably 18% by mass or less, based on 100% by mass of the resin composition. The resin composition of this embodiment may contain only one type of talc (C) or may contain two or more types. When two or more types of talc (C) are included, it is preferable that the total amount is within the above range.

[0031] <Organophosphate ester compound (D)> The resin composition of this embodiment contains an organic phosphate ester compound (D). The inclusion of the organic phosphate ester compound (D) tends to suppress the generation of silver in molded products during stagnant molding.

[0032] The type or the like of the organic phosphate ester compound (D) is not particularly limited, but a phosphate ester compound having an aliphatic chain with 3 to 30 carbon atoms is preferred, a phosphate ester compound having a linear or branched alkyl group with 3 to 30 carbon atoms is more preferred, a phosphate ester compound having a linear or branched alkyl group with 10 to 30 carbon atoms is still more preferred, and a phosphate ester compound having a linear or branched alkyl group with 15 to 25 carbon atoms is even more preferred. Even more preferably, the organic phosphate ester compound (D) comprises at least one selected from the group consisting of a compound represented by formula (P1), a compound represented by formula (P2), and a compound represented by formula (P3), and further preferably comprises the compound represented by formula (P3).

[0033] (In formula (P1) and formula (P2), M each independently represents zinc or magnesium, and R x each independently represents a linear or branched alkyl group having 3 to 30 carbon atoms.) In formula (P3) (In formula (P3), R represents a linear or branched alkyl group having 3 to 30 carbon atoms. nx represents 1 or 2.)

[0034] In formula (P1) and formula (P2), M each independently represents zinc or magnesium, and zinc is preferred. In formula (P1) and formula (P2), R x each independently represents a linear or branched alkyl group having 3 to 30 carbon atoms, a linear or branched alkyl group having 10 to 30 carbon atoms is preferred, and a linear or branched alkyl group having 15 to 25 carbon atoms is more preferred.

[0035] In formula (P3), R represents a linear or branched alkyl group having 3 to 30 carbon atoms, a linear or branched alkyl group having 10 to 30 carbon atoms is preferred, and a linear or branched alkyl group having 15 to 25 carbon atoms is more preferred. In formula (P3), nx represents 1 or 2, and a mixture of the compound where nx is 1 and the compound where nx is 2 is preferred. The mixing mass ratio of the compound where nx is 1 to the compound where nx is 2 is preferably 10 to 70:90 to 30.

[0036] The content of the organic phosphate ester compound (D) in the resin composition of this embodiment is 0.05 parts by mass or more, preferably 0.07 parts by mass or more, more preferably 0.10 parts by mass or more, even more preferably 0.12 parts by mass or more, and also preferably 0.30 parts by mass or less, preferably 0.28 parts by mass or less, and even more preferably 0.24 parts by mass or less, based on 100 parts by mass of the total of the polycarbonate resin (A) and polyester resin (B). Setting the content above the lower limit tends to more effectively suppress silver formation during the retention molding of the resin composition. The resin composition of this embodiment may contain only one type of organic phosphate ester compound (D), or it may contain two or more types. When two or more types of organic phosphate ester compounds (D) are included, it is preferable that the total amount is within the above range.

[0037] <Sulfonic acid metal salt (E)> The resin composition of this embodiment contains sulfonic acid metal salt (E). By incorporating sulfonic acid metal salt (E), the increase in the Q value of the resin composition during retention can be effectively suppressed, and the impact resistance of the molded product after moist heat treatment can be maintained at a high level.

[0038] The metal sulfonic acid salt (E) used in this embodiment preferably includes an aromatic metal sulfonic acid salt. The metal sulfonic acid salt (E) is preferably an alkali metal salt and / or an alkaline earth metal salt, and more preferably an alkali metal salt. Examples of alkali metals constituting the metal sulfonic acid salt (E) include lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), etc., among which sodium, potassium, and cesium are preferred, sodium and potassium are more preferred, and potassium is even more preferred. Examples of alkaline earth metals constituting the metal sulfonic acid salt (E) include beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), and radium (Ra), with magnesium and calcium being preferred.

[0039] The sulfonic acid metal salt (E) is preferably an alkali metal salt and / or an alkaline earth metal salt of diphenylsulfonic acid, more preferably an alkali metal salt of diphenylsulfonic acid, and even more preferably a potassium salt of diphenylsulfonic acid.

[0040] Examples of preferred metal sulfonic acid salts (E) include dipotassium diphenylsulfon-3,3'-disulfonate, potassium diphenylsulfon-3-sulfonate, sodium benzenesulfonate, sodium (poly)styrenesulfonate, sodium p-toluenesulfonate, sodium (branched) dodecylbenzenesulfonate, sodium trichlorobenzenesulfonate, potassium benzenesulfonate, potassium styrenesulfonate, potassium (poly)styrenesulfonate, potassium p-toluenesulfonate, potassium (branched) dodecylbenzenesulfonate, potassium trichlorobenzenesulfonate, cesium benzenesulfonate, cesium (poly)styrenesulfonate, cesium p-toluenesulfonate, cesium (branched) dodecylbenzenesulfonate, cesium trichlorobenzenesulfonate, etc., with potassium diphenylsulfon-3-sulfonate being more preferred.

[0041] The content of the metal sulfonate salt (E) in the resin composition of this embodiment is preferably 0.05 parts by mass or more, and preferably 0.30 parts by mass or less, more preferably 0.20 parts by mass or less, more preferably 0.15 parts by mass or less, and even more preferably 0.10 parts by mass or less, and more preferably 0.08 parts by mass or less, based on 100 parts by mass of the total of the polycarbonate resin (A) and polyester resin (B). Setting the content above the lower limit can more effectively suppress the rise in the Q value during the retention molding of the resin composition, and tends to maintain better impact resistance of the resulting molded product after the humidity and heat resistance test. Setting the content below the upper limit tends to more effectively suppress the generation of silver during the retention molding of the resin composition. The resin composition of this embodiment may contain only one type of metal sulfonate salt (E), or it may contain two or more types. When two or more types of metal sulfonate salt (E) are included, it is preferable that the total amount is within the above range.

[0042] <Blend Form of Organic Phosphate Ester Compound (D) and Sulfonic Acid Metal Salt (E)> In this embodiment, the mass ratio (D) / (E) of the organic phosphate ester compound (D) and sulfonic acid metal salt (E) is 1.0 or more, preferably 1.6 or more, more preferably 1.8 or more, even more preferably 2.0 or more, preferably 10.0 or less, more preferably 8.0 or less, even more preferably 7.0 or less, even more preferably 5.0 or less, and even more preferably 4.0 or less. Setting it above the lower limit tends to more effectively suppress the generation of silver during the retention molding of the resin composition. Also, setting it below the upper limit tends to more effectively suppress the rise in the Q value during the retention molding of the resin composition, and to better maintain impact resistance after the humid heat resistance test.

[0043] <Elastomer (F)> The resin composition of this embodiment may also contain elastomer (F). By including elastomer (F), the impact resistance of the resulting molded product can be improved. Elastomer (F) can be a wide range of elastomers used to improve the impact resistance when compounded with polycarbonate resin and / or polyester resin, and core-shell type elastomers are preferred. As for core / shell type elastomers, core / shell type graft copolymers are preferred, methacrylate-butadiene-styrene copolymer, acrylonitrile-butadiene-styrene copolymer, methacrylate-styrene copolymer, and methacrylate-dimethylsiloxane-styrene copolymer are more preferred, and methacrylate-butadiene-styrene copolymer is even more preferred. Examples of commercially available products include the Kaneka series such as "Kaneka M-711" manufactured by Kaneka Corporation.

[0044] As for the elastomer (F), reference can be made to the descriptions in paragraphs 0054 to 0069 of Japanese Patent Publication No. 2022-91031 and paragraphs 0068 to 0079 of Japanese Patent Publication No. 2019-123809, which are incorporated herein by reference.

[0045] When the resin composition of this embodiment contains elastomer (F), its content is preferably 1 part by mass or more, more preferably 2 parts by mass or more, even more preferably 3 parts by mass or more, and preferably 10 parts by mass or less, more preferably 7 parts by mass or less, and even more preferably 5 parts by mass or less, based on 100 parts by mass of the total of polycarbonate resin (A) and polyester resin (B). Setting the content above the lower limit tends to further improve the toughness improvement effect, including impact resistance, of the resulting molded product. Setting the content below the upper limit tends to better maintain the rigidity of the resulting molded product. The resin composition of this embodiment may contain only one type of elastomer (F), or it may contain two or more types. When two or more types are included, it is preferable that the total amount is within the above range.

[0046] <Stabilizer (G)> The resin composition of this embodiment may contain stabilizer (G). Examples of stabilizer (G) include heat stabilizers and antioxidants. Other examples of stabilizer (G) include phenolic, amine, phosphorus, and thioether-based stabilizers. In particular, in this embodiment, it is preferable to include a phosphorus-based heat stabilizer and a phenolic antioxidant.

[0047] Any known phosphorus-based heat stabilizer can be used. Specific examples include phosphoric acid, phosphonic acid, phosphorous acid, phosphinic acid, and polyphosphate; acidic pyrophosphate metal salts such as sodium acidic pyrophosphate, potassium acidic pyrophosphate, and calcium acidic pyrophosphate; phosphates of Group 1 or Group 2 metals such as potassium phosphate, sodium phosphate, cesium phosphate, and zinc phosphate; and organic phosphate compounds, organic phosphite compounds, and organic phosphonite compounds, with organic phosphite compounds being particularly preferred.

[0048] Examples of organic phosphite compounds include triphenyl phosphite, tris(mononylphenyl) phosphite, tris(mononyl / dinonylphenyl) phosphite, tris(2,4-di-tert-butylphenyl) phosphite, monooctyldiphenyl phosphite, dioctylmonophenyl phosphite, monodecyldiphenyl phosphite, didecylmonophenyl phosphite, tridecyl phosphite, trilauryl phosphite, tristearyl phosphite, 2,2-methylenebis(4,6-di-tert-butylphenyl)octyl phosphite, distearylpentaerythritol diphosphite, bis(decyl)pentaerythritol diphosphite, bis(tridecyl)pentaerythritol diphosphite, and bis(nonylphenyl)pentaerythritol diphosphite. Examples of such organic phosphite compounds include, for example, "ADEKA Stab (registered trademark; hereinafter the same) 1178," "ADEKA Stab 2112," and "ADEKA Stab HP-10" manufactured by ADEKA Corporation, "JP-351," "JP-360," and "JP-3CP" manufactured by Johoku Chemical Industry Co., Ltd., and "Irgaphos (registered trademark; hereinafter the same) 168" manufactured by BASF.

[0049] In addition to the above, the phosphorus-based heat stabilizers used in this embodiment can also be described in paragraphs 0127 to 0133 of Japanese Patent Application Publication No. 2022-067329, and this content is incorporated herein.

[0050] As phenolic antioxidants, hindered phenolic antioxidants are preferably used. Specific examples of hindered phenolic antioxidants include pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, thiodiethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide], 2,4-dimethyl-6-(1-methylpentadecyl)phenol, diethyl[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphate, 4,6-bis(octyl) Examples include ruthiomethyl)-o-cresol, ethylenebis(oxyethylene)bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate], hexamethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 2,6-di-tert-butyl-4-(4,6-bis(octylthio)-1,3,5-triazine-2-ylamino)phenol, and 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl acrylate.

[0051] Among these, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate are preferred. Specific examples of such hindered phenol antioxidants include, for example, BASF's "Irganox (registered trademark; hereinafter the same) 1010" and "Irganox 1076," and ADEKA's "ADEKA Stab AO-50" and "ADEKA Stab AO-60."

[0052] When the resin composition of this embodiment contains a stabilizer (G), its content is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, even more preferably 0.1 parts by mass or more, even more preferably 0.2 parts by mass or more, and also preferably 3 parts by mass or less, more preferably 2 parts by mass or less, and even more preferably 1 part by mass or less, and even more preferably 0.5 parts by mass or less, based on 100 parts by mass of the total of the polycarbonate resin (A) and polyester resin (B). Setting the content above the lower limit tends to further improve the thermal stability of the resulting molded product. Setting the content below the upper limit tends to more effectively suppress mold contamination due to gas generation during molding of the resin composition. The resin composition of this embodiment may contain only one type of stabilizer (G), or it may contain two or more types. When two or more types of stabilizers (G) are included, it is preferable that the total amount is within the above range.

[0053] <Release Agent (H)> The resin composition of this embodiment may contain a release agent (H). Examples of release agents (H) include aliphatic carboxylic acids, salts of aliphatic carboxylic acids, esters of aliphatic carboxylic acids and alcohols, aliphatic hydrocarbon compounds with a number average molecular weight of 200 to 15,000, polysiloxane-based silicone oils, ketone waxes, and lite amides, with aliphatic carboxylic acids, salts of aliphatic carboxylic acids, and esters of aliphatic carboxylic acids and alcohols being preferred.

[0054] Examples of aliphatic carboxylic acids include saturated or unsaturated aliphatic monovalent, divalent, or trivalent carboxylic acids. Here, aliphatic carboxylic acids also include alicyclic carboxylic acids. Among these, preferred aliphatic carboxylic acids are monovalent or divalent carboxylic acids having 6 to 36 carbon atoms, and more preferably aliphatic saturated monovalent carboxylic acids having 6 to 36 carbon atoms. Specific examples of such aliphatic carboxylic acids include palmitic acid, stearic acid, caproic acid, capric acid, lauric acid, arachidic acid, behenic acid, lignoceric acid, cerotic acid, melissic acid, tetratriacontanoic acid, montanic acid, adipic acid, and azelaic acid. Examples of salts of aliphatic carboxylic acids include sodium salts, potassium salts, calcium salts, and magnesium salts.

[0055] As the aliphatic carboxylic acid in the ester of an aliphatic carboxylic acid and an alcohol, for example, the same aliphatic carboxylic acid as described above can be used. On the other hand, as the alcohol, for example, saturated or unsaturated monohydric or polyhydric alcohols can be used. These alcohols may have substituents such as fluorine atoms or aryl groups. Among these, monohydric or polyhydric saturated alcohols having 30 or fewer carbon atoms are preferred, and aliphatic or alicyclic saturated monohydric alcohols or aliphatic saturated polyhydric alcohols having 30 or fewer carbon atoms are more preferred.

[0056] Specific examples of such alcohols include octanol, decanol, dodecanol, stearyl alcohol, behenyl alcohol, ethylene glycol, diethylene glycol, glycerin, pentaerythritol, 2,2-dihydroxyperfluoropropanol, neopentylene glycol, ditrimethylolpropane, and dipentaerythritol.

[0057] Specific examples of esters of aliphatic carboxylic acids and alcohols include beeswax (a mixture mainly composed of myricyl palmitate), stearyl stearate, behenyl behenate, stearyl behenate, glycerin monopalmitate, glycerin monostearate, glycerin distearate, glycerin tristearate, pentaerythritol monopalmitate, pentaerythritol monostearate, pentaerythritol distearate, pentaerythritol tristearate, and pentaerythritol tetrastearate.

[0058] Examples of aliphatic hydrocarbons with a number-average molecular weight of 200 to 15,000 include liquid paraffin, paraffin wax, microwax, polyethylene wax, Fischer-Tropsch wax, and α-olefin oligomers having 3 to 12 carbon atoms. Here, alicyclic hydrocarbons are also included as aliphatic hydrocarbons. Furthermore, the number-average molecular weight of the aliphatic hydrocarbons is preferably 5,000 or less. Among these, paraffin wax, polyethylene wax, or partially oxided polyethylene wax are preferred, with paraffin wax and polyethylene wax being even more preferred.

[0059] Details of the release agent (H) can be found in paragraphs 0055 to 0061 of Japanese Patent Application Publication No. 2018-095706, and these contents are incorporated herein by reference.

[0060] When the resin composition of this embodiment contains a release agent (H), its content is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, even more preferably 0.1 parts by mass or more, even more preferably 0.2 parts by mass or more, and preferably 3 parts by mass or less, more preferably 2 parts by mass or less, and even more preferably 1 part by mass or less, and even more preferably 0.5 parts by mass or less, based on 100 parts by mass of the total of the polycarbonate resin (A) and polyester resin (B). Setting the content above the lower limit tends to further improve the release properties of the resin composition from the mold during molding. Setting the content below the upper limit tends to more effectively suppress mold contamination due to gas generation during molding of the resin composition. The resin composition of this embodiment may contain only one type of release agent (H), or it may contain two or more types. When two or more types of release agents (H) are included, it is preferable that the total amount is within the above range.

[0061] <Coloring Agent (I)> The resin composition of this embodiment may contain a coloring agent (I). By including a coloring agent (I), the resulting molded product can be given color. The coloring agent (I) may be a pigment or a dye, but it is preferably a pigment. The coloring agent (I) may also be an achromatic coloring agent or a chromatic coloring agent, but an achromatic coloring agent is preferred. A black coloring agent composed of two or more chromatic coloring agents is also preferred. In this embodiment, a preferred example is that the coloring agent (I) contains a black coloring agent (preferably a black pigment) and / or a white coloring agent (preferably a white pigment), and a black coloring agent is preferred. An example of a black pigment is carbon black. For carbon black, refer to the descriptions in paragraphs 0065 to 0068 of Japanese Patent Application Publication No. 2021-031633 and paragraphs 0014 to 0025 of Japanese Patent Application Publication No. 2019-056035, and this content is incorporated herein. Titanium dioxide is an example of a white pigment. Pigments such as carbon black may be blended in a masterbatch made with a thermoplastic resin (preferably polycarbonate resin and / or styrene resin, more preferably styrene resin). The carbon black content in the masterbatch is preferably 10 to 60% by mass.

[0062] When the resin composition of this embodiment contains a colorant (I), its content (excluding the amount of resin used for masterbatching) is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, even more preferably 0.1 parts by mass or more, even more preferably 0.2 parts by mass or more, even more preferably 0.3 parts by mass or more, and also preferably 3 parts by mass or less, more preferably 2 parts by mass or less, and even more preferably 1 part by mass or less, based on 100 parts by mass of the total of the polycarbonate resin (A) and polyester resin (B). The resin composition of this embodiment may contain only one type of colorant (I) or may contain two or more types. When two or more types of colorant (I) are included, it is preferable that the total amount is within the above range.

[0063] <Other Components> The resin composition of this embodiment may further contain other components not listed above. Examples of other components include thermoplastic resins other than polycarbonate resins and polyester resins, reinforcing materials, flame retardants other than metal sulfonates, flame retardant additives, ultraviolet absorbers, fluorescent whitening agents, epoxy compounds, antifogging agents, flow improvers, plasticizers, dispersants, antibacterial agents, antiviral agents, etc. Details of these components can be found in paragraphs 0107 to 0115 of Japanese Patent Application Publication No. 2014-136710, paragraphs 0106 to 0128 of Japanese Patent Application Publication No. 2015-117298, paragraphs 0055 to 0061 of Japanese Patent Application Publication No. 2018-095706, and paragraphs 0047 to 0103 of International Publication No. 2021 / 241471, the contents of which are incorporated herein by reference. The content of the other components mentioned above, if present, is, for example, 0.001% by mass or more, and for example, 5.0% by mass or less, preferably 3.0% by mass or less, and more preferably 1.0% by mass or less, based on the mass of the resin composition. In the resin composition of this embodiment, the total of polycarbonate resin (A), polyester resin (B), talc (C), organophosphate ester compound (D), and metal sulfonate salt (E) preferably accounts for 95% by mass or more of the resin composition, and more preferably 97% by mass or more. Furthermore, the total of polycarbonate resin (A), polyester resin (B), talc (C), organophosphate ester compound (D), and metal sulfonate salt (E), stabilizer (G), release agent (H), and colorant (I) preferably accounts for 97% by mass or more of the resin composition, and more preferably 99% by mass or more.

[0064] As an example of a preferred resin composition of this embodiment, an example is a resin composition containing 0.10 parts by mass or more of an organic phosphate ester compound (D) and 0.10 parts by mass or less of a metal sulfonic acid salt (E) per 100 parts by mass of a total of polycarbonate resin (A) and polyester resin (B), wherein the mass ratio (D) / (E) of the organic phosphate ester compound (D) to the metal sulfonic acid salt (E) is 2.0 or more, the metal sulfonic acid salt (E) includes sodium sulfonic acid salt, the organic phosphate ester compound (D) includes a compound represented by formula (P3), and the resin composition contains 10 parts by mass or more of talc per 100 parts by mass of a total of polycarbonate resin (A) and polyester resin (B).

[0065] <Physical Properties of the Resin Composition> The resin composition of this embodiment preferably has high rigidity. Specifically, when the resin composition of this embodiment is molded into an ISO multipurpose test piece (4 mm thick) and measured according to ISO-178, the flexural modulus is preferably 3000 MPa or more, more preferably 3500 MPa or more, and even more preferably 4000 MPa or more. There is no particular upper limit for the flexural modulus, but 10000 MPa or less is practical, and even 5000 MPa or less is sufficient to meet the required performance.

[0066] The resin composition of this embodiment, when molded into a bar flow molded body with a width of 20 mm and a thickness of 2 mm under the conditions of a cylinder setting temperature of 280°C, a mold temperature of 80°C, an injection pressure of 100 MPa, an injection time of 5 seconds, and a molding cycle of 40 seconds, preferably has a flow length of 100 mm or more, more preferably 150 mm or more, even more preferably 170 mm or more, even more preferably 300 mm or less, even more preferably 250 mm or less, and even more preferably 215 mm or less.

[0067] In this embodiment, the resin composition preferably has a Q value increase rate of less than 140% of the plate molded product after 20 minutes of retention molding at a cylinder temperature of 280°C, with the Q value of the pellet as the initial value. The lower limit of the Q value increase rate is exemplified as 100% or more.

[0068] The resin composition of this embodiment preferably has a retention rate of 50% or more of the notched Charpy impact strength measured according to ISO standard 179-1 after standing an ISO multipurpose test piece (4 mm thick) in an atmosphere of 80°C and 95% relative humidity for 500 hours. The upper limit of the retention rate of the notched Charpy impact strength is exemplified as 100% or less. The flexural modulus, the rate of increase in the Q value, and the retention rate of the notched Charpy impact strength are measured according to the examples described later.

[0069] <Manufacturing of Resin Composition> There are no limitations on the manufacturing method of the resin composition of this embodiment, and a wide range of known methods for manufacturing resin compositions can be used. For example, a method may be used in which polycarbonate resin (A), polyester resin (B), talc (C), organophosphate ester compound (D), and sulfonic acid metal salt (E), as well as other components that may be added as needed, are pre-mixed using various mixers such as a tumbler or Henschel mixer, and then melt-kneaded using a mixer such as a Banbury mixer, roll, brabender, single-screw compound extruder, twin-screw compound extruder, or kneader. The melt-kneading temperature is not particularly limited, but is usually in the range of 240 to 320°C.

[0070] One form of the resin composition of this embodiment is pellets. The resin composition or pellets of this embodiment are molded into various molded articles. That is, the molded articles of this embodiment are molded articles formed from the resin composition or pellets of this embodiment. The molding method of the molded articles is not particularly specified, but examples include injection molding, ultra-high-speed injection molding, injection compression molding, two-color molding, hollow molding methods such as gas-assisted molding, molding using insulated molds, molding using rapidly heated molds, foam molding (including supercritical fluids), insert molding, IMC (in-mold coating molding) molding, extrusion molding, sheet molding, thermoforming, rotational molding, lamination molding, press molding, blow molding, etc., with injection molding being preferred among them.

[0071] Furthermore, there are no particular restrictions on the shape of the molded product in this embodiment, and it can be appropriately selected according to the application and purpose of the molded product. Examples include plate-shaped, rod-shaped, sheet-shaped, film-shaped, cylindrical, annular, circular, elliptical, polygonal, irregularly shaped, hollow, frame-shaped, box-shaped, panel-shaped, and other special shapes.

[0072] The molded product of this embodiment can be widely used in molded products containing polycarbonate resin, and even more so in molded products containing both polycarbonate resin and polyester resin. Specifically, it is preferably used in electrical and electronic equipment / components, office automation equipment / components, information terminal equipment / components, machine parts, home appliances, vehicle parts, building materials, various containers, leisure goods and miscellaneous items, lighting equipment, etc. Among vehicle parts, it is particularly suitable for large exterior parts (roof panels, roof rails, spoilers, rear garnishes, etc.).

[0073] The present invention will be described in more detail below with reference to examples. The materials, amounts used, proportions, processing content, processing procedures, etc., shown in the following examples can be modified as appropriate, as long as they do not depart from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below. If the measuring instruments, etc., used in the examples are difficult to obtain due to discontinuation or other reasons, measurements can be taken using other instruments with equivalent performance.

[0074] 1. Raw materials: The raw materials shown in Table 1 or Table 2 below were used.

[0075]

[0076] 2. Examples 1-8, Comparative Examples 1-14 <Production of Resin Composition (Pellets)> The components shown in Table 1 or Table 2 were blended in the proportions (parts by mass) indicated in Tables 3-6, mixed in a tumbler for 20 minutes, and then supplied from the upstream feeder to a twin-screw extruder (TEX30α) manufactured by Japan Steel Works, Ltd. equipped with one vent. The mixture was kneaded under the conditions of a rotation speed of 200 rpm, a discharge rate of 30 kg / hour, and a barrel temperature of 280°C. The molten resin extruded from the extruder in strand form was rapidly cooled in a water bath and pelletized using a pelletizer to obtain pellets of the polycarbonate resin composition.

[0077] <Flexural Modulus (Unit: MPa)> The obtained pellets were dried at 120°C for 5 hours, and then injection molded using an injection molding machine (Si-80-6 manufactured by Toyo Machinery & Metal Co., Ltd.) under the conditions of a cylinder temperature of 280°C and a mold temperature of 80°C to produce ISO multipurpose test specimens (4 mm thick). The flexural modulus (unit: MPa) of the obtained ISO multipurpose test specimens was measured in accordance with ISO-178.

[0078] <Bar Flow (2mmtBF, unit: mm)> The obtained pellets were dried at 120°C for 5 hours. Then, using an injection molding machine manufactured by Nissei Plastic Industrial Co., Ltd. (NEX80III: clamping force 80 tons), a bar flow molded body with a width of 20 mm and a thickness of 2 mm was injection molded under the following conditions: cylinder setting temperature 280°C, mold temperature 80°C, injection pressure 100 MPa, injection time 5 seconds, and molding cycle 40 seconds. The flow length (unit: mm) was then evaluated.

[0079] <Silver Generation During Retention Molding> Using the pellets obtained above, the pellets were measured in an injection molding machine (FANUC S-2000i 150B) at a cylinder temperature of 280°C, a mold temperature of 80°C, and a screw rotation speed of 60 rpm. After retention in the cylinder for 30 seconds, 4 minutes, 8 minutes, 16 minutes, and 20 minutes, injection molding was performed at an injection speed of 20 mm / s to produce three-tiered plates measuring 50 mm x 90 mm with thicknesses of 3 mm, 2 mm, and 1 mm. The presence or absence of silver generation on the surface of the obtained test pieces was visually checked. The check was performed by five experts, and the decision was made by majority vote.

[0080] The following criteria were used for evaluation: A: No silver formation was observed for 4-minute, 8-minute, and 16-minute stays. B: No silver formation was observed for 4-minute and 8-minute stays, but silver formation was observed for 16-minute stays. C: No silver formation was observed for 4-minute stays, but silver formation was observed for 8-minute and 16-minute stays. D: Silver formation was observed for 4-minute, 8-minute, and 16-minute stays.

[0081] <Changes in Q value during retention molding> After drying the pellets obtained by the above manufacturing method at 120°C for 5 hours, the Q value was measured using a Shimadzu Corporation CFT-500EX constant force extrusion capillary rheometer under the conditions of cylinder temperature 280°C, test force 160 kgf, and melting time 7 minutes. In addition, the three-stage plate retained for 20 minutes obtained by the above manufacturing method was broken down to the size of the pellets, and the Q value was measured in the same manner, and the Q value of the three-stage plate retained for 20 minutes was compared to the Q value of the pellets (unit: ×10). -2 cm 3 The rate of increase ( / sec) was calculated. Rate of increase (%) = [Q value of the 3-stage plate after 20 minutes / Q value of the pellet] × 100 The rate of increase was evaluated as follows: A: The rate of increase was less than 140% B: The rate of increase was 140% or more C: A 3-stage plate could not be obtained because a short circuit occurred after 20 minutes of dwelling.

[0082] Impact resistance after moisture-resistant heat treatment (unit: kJ / m) 2 The obtained pellets were dried at 120°C for 5 hours, and then injection molded using an injection molding machine (Si-80-6 manufactured by Toyo Machinery & Metal Co., Ltd.) under conditions of cylinder temperature 290°C and mold temperature 110°C to produce ISO multipurpose test specimens (4 mm thick). The obtained ISO multipurpose test specimens were left to stand for 500 hours in an atmosphere of 80°C and relative humidity for moist heat treatment. The test specimens before and after moist heat treatment were subjected to notchless Charpy impact strength (unit: kJ / m) at a temperature of 23°C according to ISO standard 179-1. 2 The following was measured: NB indicates that it did not break down.

[0083] Furthermore, the retention rate of Charpy impact strength after moist heat treatment was calculated. Retention rate (%) = [Charpy impact strength after 500 hours of treatment / initial Charpy impact strength] × 100 The retention rate was evaluated as follows: A: Retention rate was 50% or more, or no fracture occurred (NB) B: Retention rate was 40% or more but less than 50% C: Retention rate was less than 40%

[0084]

[0085]

[0086]

[0087]

[0088] As is clear from the above results, molded articles formed from the resin composition of the present invention exhibited a high flexural modulus, suppressed silver formation in the molded articles during retention, low increase in Q value during retention, and excellent impact resistance after humid heat treatment (Examples 1-8). In particular, the effect of improving the Q value was exceptional. For example, as is clear from the comparison between Example 2, Comparative Example 2, and Comparative Example 4, the Q value does not improve when either the organic phosphate ester compound (D) or the metal sulfonate salt (E) is blended, but the Q value improves when both the organic phosphate ester compound (D) and the metal sulfonate salt (E) are blended. In contrast, when at least one of the organic phosphate ester compound (D) and the metal sulfonate salt (E) is not included, or when the amount blended is outside the range of the present invention, or when the mass ratio (D) / (E) is less than 1.0, one or more of the following were observed: silver formation in the molded articles during retention, an increase in Q value during retention, or a decrease in impact resistance after humid heat treatment (Comparative Examples 1-14).

[0089] Although the present invention has been described in detail using specific embodiments, it will be apparent to those skilled in the art that various modifications are possible without departing from the intent and scope of the invention.

Claims

1. A resin composition comprising 100 parts by mass in total, consisting of 50 to 90 parts by mass of polycarbonate resin (A) and 10 to 50 parts by mass of polyester resin (B), 5 to 20 parts by mass of talc (C), 0.05 to 0.30 parts by mass of an organic phosphate ester compound (D), and 0.05 to 0.30 parts by mass of a metal sulfonic acid salt (E), wherein the mass ratio of the organic phosphate ester compound (D) to the metal sulfonic acid salt (E), (D) / (E), is 1.0 or greater.

2. The resin composition according to claim 1, wherein the mass ratio (D) / (E) of the organic phosphate ester compound (D) to the metal sulfonate salt (E) is 2.0 to 5.

0.

3. The resin composition according to claim 1, wherein the talc (C) content is 10 to 20 parts by mass with respect to a total of 100 parts by mass of 50 to 90 parts by mass of polycarbonate resin (A) and 10 to 50 parts by mass of polyester resin (B).

4. The resin composition according to claim 1, wherein the polyester resin (B) comprises polyethylene terephthalate resin.

5. The resin composition according to claim 1, wherein the organic phosphate ester compound (D) comprises at least one of the compound represented by formula (P1), the compound represented by formula (P2), and the compound represented by formula (P3). (In formulas (P1) and (P2), M is independently zinc and magnesium, and R x Each of these independently represents a linear or branched alkyl group having 3 to 30 carbon atoms. (Formula (P3)) (In formula (P3), R represents a linear or branched alkyl group having 3 to 30 carbon atoms. nx represents 1 or 2.) 6. The resin composition according to claim 1, wherein the metal sulfonic acid salt (E) comprises an aromatic metal sulfonic acid salt.

7. The resin composition according to claim 1, wherein the mass ratio (D) / (E) of the organic phosphate ester compound (D) to the metal sulfonic acid salt (E) is 2.0 to 5.0, the talc (C) content is 10 to 20 parts by mass per 100 parts by mass of the total of 50 to 90 parts by mass of the polycarbonate resin (A) and 10 to 50 parts by mass of the polyester resin (B), the polyester resin (B) includes polyethylene terephthalate resin, the organic phosphate ester compound (D) includes at least one of the compound represented by formula (P1), the compound represented by formula (P2), and the compound represented by formula (P3), and the metal sulfonic acid salt (E) includes an aromatic metal sulfonic acid salt. (In formulas (P1) and (P2), M is independently zinc and magnesium, and R x Each of these independently represents a linear or branched alkyl group having 3 to 30 carbon atoms. (Formula (P3)) (In formula (P3), R represents a linear or branched alkyl group having 3 to 30 carbon atoms. nx represents 1 or 2.) 8. The resin composition according to claim 7, wherein the organic phosphate ester compound (D) comprises a compound represented by (P3), and the metal sulfonic acid salt (E) comprises a potassium aromatic sulfonic acid salt.

9. Pellets of the resin composition according to any one of claims 1 to 8.

10. A molded article formed from the resin composition according to any one of claims 1 to 8.

11. A molded article formed from the pellets described in claim 9.