Optical laminate and display device
The optical laminate with a specific configuration of light-absorbing anisotropic layers and C-plates addresses the need for high transmittance and rapid transmittance reduction, improving privacy in display devices.
Patent Information
- Application Number
- PCT/JP2026/015778
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-04-20
- Publication Date
- 2026-11-12
AI Technical Summary
Existing optical laminates in display devices, such as liquid crystal displays and OLEDs, fail to achieve high transmittance over a wide range of polar angles while rapidly decreasing transmittance beyond a certain angle, necessitating improved optical elements for privacy protection.
An optical laminate comprising a specific configuration of light-absorbing anisotropic layers and C-plates, with strategically positioned liquid crystal layers and phase difference films, to control transmittance across varying polar angles.
The laminate provides high transmittance over a wide range of polar angles and rapid reduction in transmittance beyond a certain angle, enhancing privacy by controlling visibility from oblique angles.
Smart Images

Figure JP2026015778_12112026_PF_FP_ABST
Abstract
Description
Optical laminates, display devices
[0001] This invention relates to optical laminates and display devices.
[0002] Display devices such as liquid crystal displays and organic light-emitting diodes (OLEDs) are widely used as displays in smartphones and laptops. In recent years, these devices have become thinner and lighter, making them more portable and increasingly used in public spaces. Therefore, there is a need for technologies that prevent others from viewing the content displayed on these devices, thus protecting personal and confidential information.
[0003] For example, Patent Document 1 describes an optical laminate having a first absorbing polarizer, a first phase difference film, a second phase difference film, a third phase difference film, a second absorbing polarizer, a fourth phase difference film, a fifth phase difference film, a sixth phase difference film, and a third absorbing polarizer in this order, wherein the second phase difference film and the fifth phase difference film are C plates ([Claim 10][Claim 16]
[0018] ).
[0004] Japanese Patent Publication No. 2018-189825
[0005] Recently, in order to prevent peeping as described above, there is a demand for optical elements that can achieve high transmittance over a wide range of polar angles when the polar angle is changed from the front direction, and that can rapidly decrease transmittance above a predetermined polar angle. In other words, there is a demand for both high transmittance over a wide range of polar angles and low transmittance outside of the above polar angle range. In particular, there is a growing desire to achieve a higher level of compatibility between these two characteristics. The inventors of this invention investigated the optical properties of the optical laminate described in Patent Document 1 and found that although it satisfies the conventional required characteristics, it could not meet the higher requirements of today, and further improvement was necessary.
[0006] In view of the above circumstances, the present invention aims to provide an optical laminate that exhibits high transmittance over a wide range of polar angles when the polar angle is changed from the front direction, and that can rapidly decrease transmittance beyond a certain polar angle. The present invention also aims to provide a display device.
[0007] The inventors of this invention have diligently conducted research to solve the above problems and have completed the present invention with the following configuration.
[0008] (1) An optical laminate comprising a first light-absorbing anisotropic layer, a first C plate, a second light-absorbing anisotropic layer, a second C plate, and a third light-absorbing anisotropic layer in this order, wherein the first light-absorbing anisotropic layer, the second light-absorbing anisotropic layer, and the third light-absorbing anisotropic layer are each independently a light-absorbing anisotropic layer X or a light-absorbing anisotropic layer Y, the light-absorbing anisotropic layer X has a transmittance center axis whose angle with the normal direction of the surface of the light-absorbing anisotropic layer X is 0 to 45 degrees, the light-absorbing anisotropic layer Y has an absorption axis in the in-plane direction, at least one of the first light-absorbing anisotropic layer, the second light-absorbing anisotropic layer, and the third light-absorbing anisotropic layer is a light-absorbing anisotropic layer X, and satisfies at least one of the requirements A1 to A3 described later. (2) The optical laminate according to (1), wherein at least one of the first, second, and third optical anisotropic layers is the optical anisotropic layer Y, and satisfies at least one of the requirements B1 to B3 described later. (3) The optical laminate according to (1) or (2), wherein the first and third optical anisotropic layers are optical anisotropic layers X and the second optical anisotropic layer is optical anisotropic layer Y, or the first and third optical anisotropic layers are optical anisotropic layers Y and the second optical anisotropic layer is optical anisotropic layer X. (4) The optical laminate according to any one of (1) to (3), wherein the optical anisotropic layer X and the optical anisotropic layer Y contain a dichroic substance. (5) A display device comprising the optical laminate according to any one of (1) to (4).
[0009] According to the present invention, it is possible to provide an optical laminate that exhibits high transmittance over a wide range of polar angles when the polar angle is changed from the front direction, and that can rapidly decrease transmittance beyond a certain polar angle. Furthermore, according to the present invention, it is possible to provide a display device.
[0010] This is a schematic cross-sectional view of a first embodiment of the optical laminate of the present invention. This is a schematic cross-sectional view of a modified example of the first embodiment of the optical laminate of the present invention. This is a schematic cross-sectional view of a second embodiment of the optical laminate of the present invention. This is a schematic cross-sectional view of a modified example of the second embodiment of the optical laminate of the present invention. This is a schematic cross-sectional view of a third embodiment of the optical laminate of the present invention. This is a schematic cross-sectional view of a modified example of the third embodiment of the optical laminate of the present invention. This is a schematic cross-sectional view of a fourth embodiment of the optical laminate of the present invention. This is a schematic cross-sectional view of a fifth embodiment of the optical laminate of the present invention. This is a schematic cross-sectional view of a sixth embodiment of the optical laminate of the present invention.
[0011] The present invention will now be described in detail. The following descriptions of constituent elements may be based on typical embodiments of the present invention, but the present invention is not limited to such embodiments.
[0012] The following is a definition of each term used in this specification. In this specification, a numerical range indicated by "~" means a range that includes the numbers indicated before and after "~" as the lower and upper limits, respectively.
[0013] Furthermore, in this specification, each component may be represented by a single substance or by a combination of two or more substances. When two or more substances are used in combination for each component, the content of that component refers to the total content of the combined substances unless otherwise specified.
[0014] Furthermore, in this specification, "(meth)acrylate" refers to "acrylate" or "methacrylate," "(meth)acrylic" refers to "acrylic" or "methacrylic," and "(meth)acryloyl" refers to "acryloyl" or "methacryloyl."
[0015] Furthermore, in this specification, Re(λ) and Rth(λ) represent the in-plane retardation and thickness retardation at wavelength λ, respectively. Unless otherwise specified, wavelength λ is 550 nm. In this invention, Re(λ) and Rth(λ) are values measured at wavelength λ using an AxoScan OPMF-2 (manufactured by Axometrics). By inputting the average refractive index ((nx + ny + nz) / 3) and film thickness (d) into the AxoScan, the following can be calculated in the in-plane retardation axis direction (°): Re(λ) = R0(λ) Rth(λ) = ((nx + ny) / 2 - nz) × d Note that R0(λ) is displayed as a numerical value calculated by the AxoScan OPMF-2, but it means Re(λ).
[0016] In this specification, the transmittance center axis refers to the direction that exhibits the highest transmittance when the transmittance is measured while varying the tilt angle (polar angle) and tilt direction (azimuth angle) of the surface (principal surface) of the optical absorption anisotropy layer with respect to the normal direction. Specifically, the Müller matrix at a wavelength of 550 nm is measured using an AxoScan OPMF-2 (manufactured by Axometrics). More specifically, during the measurement, the azimuth angle at which the transmittance center axis is tilted is first found, and then, within the plane containing the normal direction of the optical absorption anisotropy layer surface along that azimuth angle (a plane containing the transmittance center axis and perpendicular to the layer surface), the Müller matrix at a wavelength of 550 nm is measured while changing the polar angle, which is the angle of the optical absorption anisotropy layer surface with respect to the normal direction, from -70 to 70° in 1° increments, and the transmittance of the optical absorption anisotropy layer is derived. As a result, the direction with the highest transmittance is defined as the transmittance center axis. However, if the transmittance center axis is parallel to the normal direction of the layer surface of the anisotropic light absorption layer, the azimuth angle used to change the polar angle may be in any direction. Furthermore, if the anisotropic light absorption layer contains a dichroic substance, the transmittance center axis corresponds to the direction of the absorption axis (the long axis direction of the molecule) of the dichroic substance contained in the anisotropic light absorption layer.
[0017] Furthermore, in this specification, the refractive indices nx, ny, and nz are measured using an Abbe refractometer (NAR-4T, manufactured by Atago Corporation) with a sodium lamp (λ = 589 nm) as the light source. Wavelength dependence can be measured using a multi-wavelength Abbe refractometer DR-M2 (manufactured by Atago Corporation) in combination with an interference filter. Values from the Polymer Handbook (JOHN WILEY & SONS, INC.) and catalogs of various optical films can also be used. Examples of average refractive index values for major optical films are given below: cellulose acylate (1.48), cycloolefin polymer (1.52), polycarbonate (1.59), polymethyl methacrylate (1.49), and polystyrene (1.59).
[0018] In this specification, a C plate is defined as follows: There are two types of C plates: positive C plates and negative C plates. A positive C plate satisfies the relationship in equation (C1), and a negative C plate satisfies the relationship in equation (C2). Note that a positive C plate shows a negative value for Rth, and a negative C plate shows a positive value for Rth. Equation (C1) nz > nx ≈ ny Equation (C2) nz < nx ≈ ny Note that the above "≈" includes not only cases where the two are completely identical, but also cases where the two are substantially identical. "Substantially identical" means, for example, that (nx - ny) × d (where d is the thickness of the film) is 0 to 10 nm, preferably 0 to 5 nm, which is included in "nx ≈ ny".
[0019] The optical laminate of the present invention comprises a first light-absorbing anisotropic layer, a first C plate, a second light-absorbing anisotropic layer, a second C plate, and a third light-absorbing anisotropic layer in this order, wherein the first light-absorbing anisotropic layer, the second light-absorbing anisotropic layer, and the third light-absorbing anisotropic layer are each independently a light-absorbing anisotropic layer X or a light-absorbing anisotropic layer Y, the light-absorbing anisotropic layer X has a transmittance center axis whose angle with the normal direction of the surface of the light-absorbing anisotropic layer X is 0 to 45 degrees, the light-absorbing anisotropic layer Y has an absorption axis in the in-plane direction, and at least one of the first light-absorbing anisotropic layer, the second light-absorbing anisotropic layer, and the third light-absorbing anisotropic layer is a light-absorbing anisotropic layer X, and satisfies at least one of the following requirements A1 to A3. Requirement A1: The first optical absorption anisotropy layer is optical absorption anisotropy layer X, and a liquid crystal layer, λ / 4 layer, or λ / 2 layer containing a liquid crystal compound twisted with the thickness direction as the helical axis is disposed between the first optical absorption anisotropy layer and the first C plate. Requirement A2: The second optical absorption anisotropy layer is optical absorption anisotropy layer X, and a liquid crystal layer, λ / 4 layer, or λ / 2 layer containing a liquid crystal compound twisted with the thickness direction as the helical axis is disposed between the second optical absorption anisotropy layer and the first C plate, and between the second optical absorption anisotropy layer and the second C plate. Requirement A3: The third optical absorption anisotropy layer is optical absorption anisotropy layer X, and a liquid crystal layer, λ / 4 layer, or λ / 2 layer containing a liquid crystal compound twisted with the thickness direction as the helical axis is disposed between the third optical absorption anisotropy layer and the second C plate. In particular, it is preferable that the present invention satisfies both requirements A1 and A3, or requirement A2, in that it provides at least one of the following effects: that the transmittance becomes higher over a wide range of polar angles when the polar angle is changed from the front direction of the optical laminate, and that the transmittance can be reduced more rapidly beyond a certain polar angle (hereinafter also simply referred to as "the aspect in which the present invention has superior effects").
[0020] Furthermore, in order to obtain the effects of the present invention at multiple azimuthal angles, it is preferable that at least one of the first, second, and third light-absorbing anisotropic layers is a light-absorbing anisotropic layer Y, and that at least one of requirements B1 to B3 is satisfied. Requirement B1: The first light-absorbing anisotropic layer is a light-absorbing anisotropic layer Y, and a liquid crystal layer, λ / 4 layer, or λ / 2 layer containing a liquid crystal compound twisted with the thickness direction as the helical axis is disposed between the first light-absorbing anisotropic layer and the first C plate. Requirement B2: The second light-absorbing anisotropic layer is a light-absorbing anisotropic layer Y, and at least one of the two layers, between the second light-absorbing anisotropic layer and the first C plate, and between the second light-absorbing anisotropic layer and the second C plate, contains a liquid crystal layer, λ / 4 layer, or λ / 2 layer containing a liquid crystal compound twisted with the thickness direction as the helical axis is disposed between the second light-absorbing anisotropic layer and the first C plate, and between the second light-absorbing anisotropic layer and the second C plate. Requirement B3: The third light-absorbing anisotropic layer is light-absorbing anisotropic layer Y, and a liquid crystal layer, λ / 4 layer, or λ / 2 layer containing a liquid crystal compound that is torsionally oriented with the thickness direction as the helical axis is arranged between the third light-absorbing anisotropic layer and the second C plate.
[0021] If the optical laminate of the present invention satisfies requirement A1, it is preferable that at least one of requirements B2 and B3 is satisfied, and more preferably both requirements B2 and B3 are satisfied, in order to obtain the effects of the present invention at multiple azimuth angles. If the optical laminate of the present invention satisfies requirement A2, it is preferable that at least one of requirements B1 and B2 is satisfied, and more preferably both requirements B1 and B2 are satisfied, in order to obtain the effects of the present invention at multiple azimuth angles. If the optical laminate of the present invention satisfies requirement A3, it is preferable that at least one of requirements B2 and B3 is satisfied, and more preferably both requirements B2 and B3 are satisfied, in order to obtain the effects of the present invention at multiple azimuth angles. If the optical laminate of the present invention satisfies requirements A1 and A2, it is preferable that requirement B3 is satisfied, in order to obtain the effects of the present invention at multiple azimuth angles. If the optical laminate of the present invention satisfies requirements A1 and A3, it is preferable that requirement B2 is satisfied, in order to obtain the effects of the present invention at multiple azimuth angles.
[0022] A key feature of the optical laminate of the present invention (the first to sixth embodiments described later) is that it has a predetermined light-absorbing anisotropic layer and a predetermined phase difference layer. More specifically, it has a C-plate between the light-absorbing anisotropic layers, and a specific layer described later between the light-absorbing anisotropic layer X and the C-plate. The reason why the effects of the present invention can be obtained with the above configuration is that, firstly, the transmittance in the oblique direction is controlled by arranging the C-plate between the light-absorbing anisotropic layers. In particular, when the Rth of the C-plate is large, the transmittance can be changed more rapidly when the polar angle exceeds a predetermined value. Furthermore, by arranging the specific layer between the light-absorbing anisotropic layer X and the C-plate, the light that passes through the light-absorbing anisotropic layer X can be made more susceptible to the influence of the C-plate, and as a result, it can exhibit high transmittance over a wide range of polar angles, while rapidly changing the transmittance when the polar angle exceeds a predetermined value. More specifically, in the optical laminate of the present invention, the transmittance is high over a wide range from the front direction to a polar angle of about 30°, and the transmittance can be rapidly reduced at polar angles greater than that. Each embodiment will be described in detail below.
[0023] <<First Embodiment>> Figure 1 shows a schematic cross-sectional view of the first embodiment of the optical laminate of the present invention. The optical laminate 100A has a first light-absorbing anisotropic layer 10A, a specific layer 32, a first C plate 20A, a second light-absorbing anisotropic layer 12A, a second C plate 22A, and a third light-absorbing anisotropic layer 14A in this order. The specific layer 32 is a liquid crystal layer containing a liquid crystal compound that is twisted and oriented with the thickness direction as the helical axis (hereinafter also simply referred to as the "twist layer"), a λ / 4 layer, or a λ / 2 layer, as will be described later. The first light-absorbing anisotropic layer 10A is the light-absorbing anisotropic layer X, and the second light-absorbing anisotropic layer 12A and the third light-absorbing anisotropic layer 14A are the light-absorbing anisotropic layers Y. As will be described in detail later, the light-absorbing anisotropic layer X has a transmittance center axis whose angle with the normal direction of the surface of the light-absorbing anisotropic layer X is between 0 and 45 degrees. Also, as will be described in detail later, the light-absorbing anisotropic layer Y has an absorption axis in the in-plane direction. The optical laminate 100A corresponds to an embodiment that satisfies the above requirement A1.
[0024] The specific layer 32 may be a twisted layer, a λ / 4 layer, or a λ / 2 layer, but in the configuration shown in Figure 1, the specific layer 32 is preferably a twisted layer.
[0025] The angle between the absorption axis of the second light-absorbing anisotropic layer 12A and the absorption axis of the third light-absorbing anisotropic layer 14A is preferably 0 to 30°, more preferably 0 to 20°, and even more preferably 0 to 10°, in terms of the superior effects of the present invention. When the specific layer 32 is a twisted layer, the angle between the in-plane slow axis on the surface of the specific layer 32 on the second light-absorbing anisotropic layer 12A side and the absorption axis of the second light-absorbing anisotropic layer 12A is preferably 0 to 45°, and more preferably 0 to 10°, in terms of the superior effects of the present invention. When the specific layer 32 is a λ / 4 layer, the angle between the in-plane slow axis of the λ / 4 layer and the absorption axis of the second light-absorbing anisotropic layer 12A is preferably 30 to 60°, and more preferably 40 to 50°, in terms of the superior effects of the present invention. When the specific layer 32 is a λ / 2 layer, the angle between the in-plane slow axis of the λ / 2 layer and the absorption axis of the second light absorption anisotropy layer 12A is preferably 5 to 45°, and more preferably 10 to 30°, in terms of achieving superior effects of the present invention.
[0026] Although the layers are arranged adjacent to each other in Figure 1, the configuration is not limited to this, and other components may be included between the layers. Each component will be described in detail below.
[0027] <First Light-Absorbing Anisotropic Layer, Second Light-Absorbing Anisotropic Layer, Third Light-Absorbing Anisotropic Layer> The optical laminate of the present invention includes a first light-absorbing anisotropic layer, a second light-absorbing anisotropic layer, and a third light-absorbing anisotropic layer. In the optical laminate 100A of Figure 1, the first light-absorbing anisotropic layer 10A is the light-absorbing anisotropic layer X, and the second light-absorbing anisotropic layer 12A and the third light-absorbing anisotropic layer 14A are the light-absorbing anisotropic layers Y. The light-absorbing anisotropic layers X and Y will be described in detail below.
[0028] [Light-absorbing anisotropic layer X] The light-absorbing anisotropic layer X has a transmittance center axis that makes an angle of 0 to 45° with the normal direction of the surface (main surface) of the light-absorbing anisotropic layer X. In other words, in the light-absorbing anisotropic layer X, the angle between the transmittance center axis of the light-absorbing anisotropic layer and the normal direction of the surface of the light-absorbing anisotropic layer (normal direction of the main surface of the light-absorbing anisotropic layer) is 0 to 45°. Among these, in terms of the superior effects of the present invention, the above angle is preferably 0 to 35°, more preferably 0 to 25°, even more preferably 0 to 10°, and particularly preferably 0 to 5°. The above main surface is the surface with the largest area that is perpendicular to the thickness direction.
[0029] The light-absorbing anisotropic layer X preferably contains a dichroic substance, more preferably contains a liquid crystal compound together with the dichroic substance, and even more preferably is a layer in which the orientation state of the liquid crystal compound and the dichroic substance is fixed. The dichroic substances and liquid crystal compounds that are preferably included in the light-absorbing anisotropic layer X will be described below.
[0030] (Dichroic substances) Dichroic substances are dyes whose absorbance differs depending on the direction. Dichroic substances may or may not exhibit liquid crystalline properties.
[0031] Dichroic materials are not particularly limited and include visible light absorbing materials (dichroic dyes), luminescent materials (fluorescent materials, phosphorescent materials), ultraviolet absorbing materials, infrared absorbing materials, nonlinear optical materials, carbon nanotubes, and inorganic materials (e.g., quantum rods). Conventionally known dichroic materials (dichroic dyes) can be used. Specifically, for example, paragraphs
[0067] to
[0071] of JP 2013-228706, paragraphs
[0008] to
[0026] of JP 2013-227532, paragraphs
[0008] to
[0015] of JP 2013-209367, paragraphs
[0045] to
[0058] of JP 2013-14883, paragraphs
[0012] to
[0029] of JP 2013-109090, paragraphs
[0009] to
[0017] of JP 2013-101328, JP Paragraphs
[0051] to
[0065] of Japanese Patent Publication No. 2013-037353, paragraphs
[0049] to
[0073] of Japanese Patent Publication No. 2012-063387, paragraphs
[0016] to
[0018] of Japanese Patent Publication No. Hei 11-305036, paragraphs
[0009] to
[0011] of Japanese Patent Publication No. 2001-133630, paragraphs
[0030] to
[0169] of Japanese Patent Publication No. 2011-215337, paragraphs
[0021] to
[0075] of Japanese Patent Publication No. 2010-106242, and Japanese Patent Publication No. 2010-215846 Paragraphs
[0011] to
[0025] of Japanese Patent Publication No. 2011-048311, paragraphs
[0017] to
[0069] of Japanese Patent Publication No. 2011-213610, paragraphs
[0013] to
[0133] of Japanese Patent Publication No. 2011-237513, paragraphs
[0074] to
[0246] of Japanese Patent Publication No. 2011-237513, paragraphs
[0005] to
[0051] of Japanese Patent Publication No. 2016-006502, paragraphs
[0014] to
[0032] of Japanese Patent Publication No. 2018-053167, and paragraphs
[0014] to
[0033] of Japanese Patent Publication No. 2020-011716. Paragraphs, paragraphs
[0005] to
[0041] of International Publication No. 2016 / 060173, paragraphs
[0008] to
[0062] of International Publication No. 2016 / 136561, paragraphs
[0014] to
[0033] of International Publication No. 2017 / 154835, paragraphs
[0014] to
[0033] of International Publication No. 2017 / 154695, paragraphs
[0013] to
[0037] of International Publication No. 2017 / 195833, paragraphs
[0014] to
[0034] of International Publication No. 2018 / 164252,Examples include paragraphs
[0021] to
[0030] of International Publication No. 2018 / 186503, paragraphs
[0043] to
[0063] of International Publication No. 2019 / 189345, paragraphs
[0043] to
[0085] of International Publication No. 2019 / 225468, paragraphs
[0050] to
[0074] of International Publication No. 2020 / 004106, and paragraphs
[0015] to
[0038] of International Publication No. 2021 / 044843.
[0032] Dichroic azo dye compounds are preferred as the dichroic substance. Dichroic azo dye compounds refer to azo dye compounds whose absorbance differs depending on the direction. Dichroic azo dye compounds may or may not exhibit liquid crystalline properties. If a dichroic azo dye compound exhibits liquid crystalline properties, it may exhibit either nematic or smectic properties. The temperature range in which the liquid crystalline phase is exhibited is preferably room temperature (about 20 to 28°C) to 300°C, and more preferably 50 to 200°C from the viewpoint of handling and manufacturing suitability.
[0033] From the standpoint of color adjustment, it is preferable to use at least one dye compound (first dichroic azo dye compound) having a maximum absorption wavelength in the range of 560 to 700 nm, and at least one dye compound (second dichroic azo dye compound) having a maximum absorption wavelength in the range of 455 nm or more and less than 560 nm.
[0034] In the present invention, three or more dichroic azo dye compounds may be used in combination. For example, from the viewpoint of making the light-absorbing anisotropic layer X closer to black, it is preferable to use a first dichroic azo dye compound, a second dichroic azo dye compound, and at least one dye compound (third dichroic azo dye compound) having a maximum absorption wavelength in the range of 380 nm to less than 455 nm.
[0035] The dichroic azo dye compound preferably has a crosslinking group. Examples of crosslinking groups include (meth)acryloyl group, epoxy group, oxetanyl group, and styryl group, with (meth)acryloyl group being preferred. The light-absorbing anisotropic layer X may contain a cured product (crosslinked product) of a dichroic dye having a crosslinking group (particularly a dichroic dye compound having a crosslinking group).
[0036] The content of the dichroic substance is not particularly limited, but for the reason that it increases the degree of orientation of the formed light-absorbing anisotropic layer X, it is preferably 3% by mass or more, more preferably 8% by mass or more, even more preferably 10% by mass or more, and particularly preferably 10 to 30% by mass, relative to the total mass of the light-absorbing anisotropic layer X. The dichroic substance may be used alone or in combination of two or more types. When two or more dichroic substances are used, it is preferable that their total amount is within the above range.
[0037] (Liquid Crystal Compound) The light-absorbing anisotropic layer X preferably contains a liquid crystal compound. This allows for the orientation of dichroic substances with a higher degree of orientation while suppressing the precipitation of dichroic substances. As the liquid crystal compound, either a polymer liquid crystal compound or a low-molecular-weight liquid crystal compound can be used, and a polymer liquid crystal compound is preferred because it can achieve a high degree of orientation. In addition, a polymer liquid crystal compound and a low-molecular-weight liquid crystal compound may be used in combination as the liquid crystal compound. Here, "polymer liquid crystal compound" refers to a liquid crystal compound that has repeating units in its chemical structure. Also, "low-molecular-weight liquid crystal compound" refers to a liquid crystal compound that does not have repeating units in its chemical structure. Examples of polymer liquid crystal compounds include the thermotropic liquid crystal polymer described in Japanese Patent Application Publication No. 2011-237513 and the polymer liquid crystal compounds described in paragraphs
[0012] to
[0042] of International Publication No. 2018 / 199096. Examples of low-molecular-weight liquid crystal compounds include the liquid crystal compounds described in paragraphs
[0072] to
[0088] of Japanese Patent Application Publication No. 2013-228706, and among these, liquid crystal compounds exhibiting smectic properties are preferred.
[0038] The liquid crystal compound may be fixed in the light absorption anisotropic layer X. In order to fix the liquid crystal compound in the light absorption anisotropic layer X, for example, a method of using a liquid crystal compound having a polymerizable group, aligning the liquid crystal compound, and then polymerizing the liquid crystal compound to form the light absorption anisotropic layer X may be mentioned. In this specification, the "fixed" state refers to a state in which the alignment of the liquid crystal compound is maintained. Specifically, it is preferably a state where, in a temperature range of usually 0 to 50°C, and -30 to 70°C under more severe conditions, the layer has no fluidity, and the fixed alignment form can be stably maintained without causing a change in the alignment form due to an external field or external force. The polymerizable group is not particularly limited, but a radically polymerizable or cationically polymerizable group is preferred. Examples of the radically polymerizable group include known radically polymerizable groups, and an acryloyl group or a methacryloyl group is preferred. It is known that the polymerization rate of acryloyl groups is generally fast, and acryloyl groups are preferred from the viewpoint of improving productivity, but methacryloyl groups can also be similarly used as polymerizable groups for high birefringence liquid crystals. Examples of the cationically polymerizable group include known cationically polymerizable groups, including alicyclic ether groups, cyclic acetal groups, cyclic lactone groups, cyclic thioether groups, spiro orthoester groups, and vinyloxy groups.
[0039] The content of the liquid crystal compound is not particularly limited, but from the reason that the alignment degree of the formed light absorption anisotropic layer X becomes high, it is preferably 60% by mass or more, more preferably 70% by mass or more, based on the total mass of the light absorption anisotropic layer X. The upper limit is not particularly limited, and may be less than 100% by mass. The liquid crystal compounds may be used alone or in combination of two or more kinds. When two or more liquid crystal compounds are used, their total amount is preferably within the above range.
[0040] (Other Components) The light absorption anisotropic layer X may contain components other than the components described above. Examples of other components include a vertical alignment agent and a leveling agent. Examples of the vertical alignment agent include boronic acid compounds and onium salts.
[0041] When the light absorption anisotropic layer X contains a vertical alignment agent, the content of the vertical alignment agent is preferably 0.1 to 10% by mass, more preferably 0.5 to 5% by mass, based on the total mass of the liquid crystal compound. The vertical alignment agents may be used alone or in combination of two or more kinds. When two or more kinds of the vertical alignment agents are used, the total amount thereof is preferably within the above range.
[0042] The light absorption anisotropic layer X may contain a leveling agent. When the composition for forming the light absorption anisotropic layer X, which will be described later, contains a leveling agent, surface roughness caused by drying wind applied to the surface of the light absorption anisotropic layer X is suppressed, and the dichroic substance is more uniformly aligned. The leveling agent is not particularly limited, and a leveling agent containing a fluorine atom (fluorine-based leveling agent) or a leveling agent containing a silicon atom (silicon-based leveling agent) is preferable.
[0043] When the light absorption anisotropic layer X contains a liquid crystal compound and a leveling agent, the content of the leveling agent is preferably 0.001 to 10% by mass, more preferably 0.01 to 5% by mass, based on the total mass of the liquid crystal compound. The leveling agents may be used alone or in combination of two or more kinds. When two or more kinds of the leveling agents are used, the total amount thereof is preferably within the above range.
[0044] (Composition for Forming Light Absorption Anisotropic Layer X) The light absorption anisotropic layer X is preferably formed using a composition for forming the light absorption anisotropic layer X containing a dichroic substance and a liquid crystal compound. The composition for forming the light absorption anisotropic layer X preferably contains a solvent and the like which will be described later, in addition to the dichroic substance and the liquid crystal compound, and may further contain the other components described above.
[0045] Examples of the dichroic substance contained in the composition for forming the light absorption anisotropic layer X include dichroic substances that can be contained in the light absorption anisotropic layer X. The content of the dichroic substance with respect to the total solid content mass of the composition for forming the light absorption anisotropic layer X is preferably the same as the content of the dichroic substance with respect to the total mass of the light absorption anisotropic layer X. Here, the "total solid content in the composition for forming the light absorption anisotropic layer X" refers to components excluding the solvent, and specific examples of the solid content include the dichroic substance, the liquid crystal compound, and the other components described above.
[0046] The liquid crystal compounds and other components that may be included in the composition for forming the light-absorbing anisotropic layer X are the same as the liquid crystal compounds and other components that may be included in the light-absorbing anisotropic layer X. Preferably, the content of the liquid crystal compounds and other components relative to the total solid content mass of the composition for forming the light-absorbing anisotropic layer X is the same as the content of the liquid crystal compounds and other components relative to the total mass of the light-absorbing anisotropic layer.
[0047] The composition for forming the light-absorbing anisotropic layer X preferably contains a solvent from the viewpoint of workability. Examples of solvents include organic solvents such as ketones, ethers, aliphatic hydrocarbons, alicyclic hydrocarbons, aromatic hydrocarbons, carbon halides, esters, alcohols, cellosolves, cellosolve acetates, sulfoxides, amides, and heterocyclic compounds, as well as water. These solvents may be used individually or in combination of two or more. Of these solvents, organic solvents are preferred, and carbon halides or ketones are more preferred.
[0048] If the composition for forming the light-absorbing anisotropic layer X contains a solvent, the solvent content is preferably 70 to 99% by mass, and more preferably 75 to 97% by mass, based on the total mass of the composition for forming the light-absorbing anisotropic layer X.
[0049] The composition for forming the light-absorbing anisotropic layer X may contain a polymerization initiator. The polymerization initiator is not particularly limited, but is preferably a photosensitive compound, i.e., a photopolymerization initiator. The polymerization initiator may be used alone or in combination of two or more. When the composition for forming the light-absorbing anisotropic layer X contains a polymerization initiator, the content of the polymerization initiator is preferably 0.01 to 30% by mass, and more preferably 0.1 to 15% by mass, based on the total solid content of the composition for forming the light-absorbing anisotropic layer X.
[0050] (Method for manufacturing the light-absorbing anisotropic layer X) The method for manufacturing the light-absorbing anisotropic layer X is not particularly limited, but a method comprising the steps of applying a light-absorbing anisotropic layer X-forming composition containing a dichroic substance and a liquid crystal compound to form a coated film (hereinafter also referred to as the "coated film formation step") and aligning the liquid crystal components contained in the above coated film (hereinafter also referred to as the "orientation step") in this order (hereinafter also referred to as the "this manufacturing method") is preferred because it allows for a higher degree of orientation of the dichroic substance. Note that the liquid crystal components include not only the liquid crystal compounds mentioned above, but also dichroic substances that have liquid crystal properties. Each step will be described below.
[0051] The coating film formation step is a step of forming a coating film by applying the above-described composition for forming the light-absorbing anisotropic layer X. By using the above-described composition for forming the light-absorbing anisotropic layer X containing the solvent, or by using the composition for forming the light-absorbing anisotropic layer X in a liquid state such as a molten liquid obtained by heating, it becomes easier to apply the composition for forming the light-absorbing anisotropic layer X onto the alignment film. Known methods for applying the composition for forming the light-absorbing anisotropic layer X include roll coating, gravure printing, spin coating, wire bar coating, extrusion coating, direct gravure coating, reverse gravure coating, die coating, spray, and inkjet methods.
[0052] The object to which the composition for forming the light-absorbing anisotropic layer X is applied is not particularly limited, and an alignment film can be used as an example. The alignment film can be any film that aligns the liquid crystal components that may be contained in the composition for forming the light-absorbing anisotropic layer X. It can be formed by means such as rubbing treatment of the film surface with an organic compound (preferably a polymer), oblique deposition of an inorganic compound, formation of a layer having microgrooves, or accumulation of an organic compound (e.g., ω-tricosanoic acid, dioctadecylmethylammonium chloride, methyl stearylate) by the Langmuir-Bludget method (LB film). Furthermore, alignment films that exhibit alignment function by applying an electric field, a magnetic field, or light irradiation are also known. Among these, in the present invention, an alignment film of a polyvinyl alcohol-based resin is preferred, and from the viewpoint of uniformity of alignment, a photo-alignment film formed by light irradiation is also preferred.
[0053] The orientation step is a step in which the liquid crystal components (particularly dichroic substances) contained in the coated film are oriented. In the orientation step, it is thought that the dichroic substances are oriented along the liquid crystal compounds oriented by the orientation film. The orientation step may include a drying process. The drying process can remove components such as solvents from the coated film. The drying process may be carried out by leaving the coated film at room temperature for a predetermined time (e.g., natural drying), or by heating and / or blowing air.
[0054] The orientation step preferably includes a heat treatment. This further orients the dichroic substances contained in the coating film, resulting in a higher degree of orientation of the dichroic substances. From the viewpoint of manufacturing suitability, the heat treatment is preferably at 10 to 250°C, and more preferably at 25 to 190°C. The heating time is preferably at 1 to 300 seconds, and more preferably at 1 to 60 seconds.
[0055] The orientation step may include a cooling step performed after the heat treatment. The cooling step is a process of cooling the heated coating film to room temperature (20-25°C). This further fixes the orientation of the dichroic substances contained in the coating film, and increases the degree of orientation of the dichroic substances. The cooling method is not particularly limited and can be carried out by known methods. By the above steps, a light-absorbing anisotropic layer X can be obtained.
[0056] The present manufacturing method may include a step of curing the light-absorbing anisotropic layer X after the orientation step (hereinafter also referred to as the "curing step"). The curing step is carried out, for example, by heating and / or light irradiation (exposure). Among these, it is preferable that the curing step be carried out by light irradiation. Various light sources can be used for curing, such as infrared light, visible light or ultraviolet light, but ultraviolet light is preferred. Furthermore, ultraviolet light may be irradiated while heating during curing, or ultraviolet light may be irradiated through a filter that transmits only specific wavelengths. In addition, exposure may be carried out under a nitrogen atmosphere. When curing of the light-absorbing anisotropic layer X proceeds by radical polymerization, it is preferable to expose under a nitrogen atmosphere because the inhibition of polymerization by oxygen is reduced.
[0057] The thickness of the light-absorbing anisotropic layer X is not particularly limited, but it is preferably 0.5 to 10 μm, and more preferably 1.0 to 5.0 μm, in order to reduce the thickness of the optical laminate. The thickness of the light-absorbing anisotropic layer X referred to above is the average thickness of the light-absorbing anisotropic layer X. The average thickness is obtained by measuring the thickness of any five or more points on the light-absorbing anisotropic layer X and taking the arithmetic mean of these measurements.
[0058] [Light Absorption Anisotropic Layer Y] The light absorption anisotropic layer Y has an absorption axis in the in-plane direction. Therefore, the light absorption anisotropic layer Y has the function of converting natural light into a specific linearly polarized light, and a so-called absorbing polarizer can be considered an example of the light absorption anisotropic layer Y. As a method for checking the presence or absence of an absorption axis in the in-plane direction, place the optical film whose presence or absence of an absorption axis you wish to check on a surface light source, and then place a polarizing plate on the optical film. When the polarizing plate is rotated while maintaining a state parallel to the surface of the optical film, if the brightness of the surface light source viewed from the front changes, it can be determined that an absorption axis is present.
[0059] As the light-absorbing anisotropic layer Y, a general polarizer can be used, for example, an iodine-based polarizer, a dye-based polarizer utilizing a dichroic substance, and a polyene-based polarizer. Iodine-based polarizers and dye-based polarizers are generally made by adsorbing iodine or a dichroic dye onto polyvinyl alcohol and then stretching it. It is preferable that the light-absorbing anisotropic layer Y contains a dichroic substance, and if it contains a dichroic substance, it is preferable that the dichroic substance is horizontally oriented. The state in which the dichroic substance is horizontally oriented means that the long axis of the dichroic substance is parallel to the main surface of the light-absorbing anisotropic layer Y. However, it is not required that it be strictly parallel, and it is preferable that the angle between the long axis of the dichroic substance and the main surface of the light-absorbing anisotropic layer Y is in the range of 0 ± 20°, and preferably in the range of 0 ± 10°.
[0060] The light-absorbing anisotropic layer Y is preferably a polarizer formed using a composition containing a dichroic substance and a liquid crystal compound having polymerizable groups. The dichroic substance is not particularly limited and can be the dichroic substance described in the description of the light-absorbing anisotropic layer X. The liquid crystal compound having polymerizable groups is not particularly limited and can be the liquid crystal compound described in the description of the light-absorbing anisotropic layer X.
[0061] The thickness of the light-absorbing anisotropic layer Y is not particularly limited, but it is preferably 40 μm or less, and more preferably 25 μm or less, from the standpoint of being able to reduce the thickness of the optical laminate. The lower limit is not particularly limited, but it is often 5 μm or more. The thickness of the light-absorbing anisotropic layer Y mentioned above refers to the average thickness of the light-absorbing anisotropic layer Y. The average thickness is obtained by measuring the thickness of five or more arbitrary points on the light-absorbing anisotropic layer Y and taking the arithmetic mean of these measurements.
[0062] <First C plate and second C plate> The first C plate and the second C plate may both be positive C plates or negative C plates.
[0063] The retardation in the thickness direction of the first C plate and the second C plate at a wavelength of 550 nm is not particularly limited, but in terms of superior effects of the present invention, the absolute value of the retardation in the thickness direction of the first C plate and the second C plate at a wavelength of 550 nm is preferably 300 nm or more, more preferably 500 nm or more, and even more preferably 800 nm or more. The lower limit is not particularly limited, but may be 3000 nm or less, or 2000 nm or less.
[0064] The first C plate and the second C plate may exhibit forward dispersiveness (a characteristic in which retardation in the thickness direction decreases as the measurement wavelength increases) or inverse dispersiveness (a characteristic in which retardation in the thickness direction increases as the measurement wavelength increases), but inverse dispersiveness is preferred. Furthermore, the above-mentioned forward and inverse dispersiveness are preferably exhibited in the visible light range.
[0065] The materials constituting the first C plate and the second C plate are not particularly limited, and the first C plate and the second C plate may be layers formed using a liquid crystal compound or resin films. In particular, it is preferable that the first C plate and the second C plate are layers in which a liquid crystal compound is fixed. When the first C plate and the second C plate are layers formed using a liquid crystal compound, the liquid crystal compound can generally be classified into rod-shaped and disc-shaped types based on its shape. Furthermore, each of these can be divided into low-molecular-weight and high-molecular-weight types. Specific examples of liquid crystal compounds are the same as those described in the section on the light-absorbing anisotropic layer, so their description is omitted. The liquid crystal compound may be fixed in the first C plate and the second C plate. To fix the liquid crystal compound in the first C plate and the second C plate, for example, a method can be used in which the liquid crystal compound is oriented using a liquid crystal compound having polymerizable groups, and then the liquid crystal compound is polymerized to form the first C plate and the second C plate. The first C plate and the second C plate may be composed of liquid crystal cells. In other words, for example, a voltage may be applied to a liquid crystal cell to orient rod-shaped liquid crystal compounds vertically and use them as the first C plate and the second C plate. By using a liquid crystal cell, switching within a viewing angle range becomes possible. The first C plate and the second C plate may have a single-layer structure or a multi-layer structure. In other words, the first C plate and the second C plate may be configured in which multiple C plates are laminated directly or via other layers (e.g., an adhesive layer or bonding layer).
[0066] The thickness of the first C plate and the second C plate is preferably 0.1 to 20 μm, more preferably 0.5 to 15 μm, and even more preferably 1 to 10 μm, in terms of thinning. Note that the thickness of the C plate refers to the average thickness of the C plate. The average thickness is obtained by measuring the thickness of any five or more points on the C plate and taking the arithmetic mean of them.
[0067] <Specific Layers> The specific layers are selected from a liquid crystal layer containing a liquid crystal compound with a twisted orientation with the thickness direction as the helical axis (hereinafter also simply referred to as the "twisted layer"), a λ / 4 layer, and a λ / 2 layer. Each layer is described in detail below.
[0068] [Twisted Layer] The twisted layer is a liquid crystal layer containing a liquid crystal compound that is twisted in orientation with the thickness direction as the helical axis. Twisted orientation of the liquid crystal compound means that the liquid crystal compound is twisted from one main surface to the other main surface of the twisted layer, with the thickness direction of the twisted layer as the helical axis. Consequently, the orientation direction of the liquid crystal compound (in-plane slow phase axis direction) differs depending on its position in the thickness direction of the twisted layer. In twisted orientation, the molecular axis of the liquid crystal compound is arranged to be parallel to the main surface of the twisted layer. However, strict parallelism is not required; it is preferable that the angle between the long axis of the liquid crystal compound and the main surface of the twisted layer is within the range of 0 to 20°, and more preferably within the range of 0 to 10°. The molecular axis of the liquid crystal compound refers to the long axis of the rod-shaped liquid crystal compound if the liquid crystal compound is rod-shaped, and the axis perpendicular to the disc surface of the disc-shaped liquid crystal compound if the liquid crystal compound is disc-shaped.
[0069] Specific examples of liquid crystal compounds are the same as those described in the section on the light-absorbing anisotropic layer, so their explanation will be omitted. The twisted-oriented liquid crystal compound may be fixed. In particular, the twisted layer is preferably formed by twisting and oriented a liquid crystal compound having polymerizable groups, and then polymerizing the liquid crystal compound to fix it in place.
[0070] The twist angle of the liquid crystal compound in the twisted layer (twist angle in the orientation direction of the liquid crystal compound) is not particularly limited and is often greater than 0° and less than or equal to 360°. In terms of superior effects of the present invention, it is preferable to have a range of 45±30° (15 to 75°), 135±30° (105 to 165°), or 225±30° (195 to 255°), and more preferably within the range of 45±20° (25 to 65°), 135±20° (115 to 155°), 225±20° (205 to 245°), or 315±20° (295 to 335°). The value of the product Δnd, which is the refractive index anisotropy Δn of the twisted layer at a wavelength of 550 nm and the thickness d of the twisted layer, is not particularly limited. However, from the point of demonstrating the excellent effects of the present invention, 250 to 1000 nm is preferred, 350 to 800 nm is more preferred, and 400 to 700 nm is even more preferred. The above-mentioned torsion angle and Δnd are measured using an AxoScan (polarimeter) device from Axometrics Inc. and its device analysis software.
[0071] The Δnd of the twisted layer may exhibit forward dispersiveness (Δnd decreases as the measurement wavelength increases) or inverse dispersiveness (Δnd increases as the measurement wavelength increases), but inverse dispersiveness is preferred. Furthermore, both forward and inverse dispersiveness are preferably exhibited in the visible light range.
[0072] The twisted layer may be composed of liquid crystal cells. Using liquid crystal cells enables switching within a wide viewing angle range.
[0073] [λ / 4 layer] The λ / 4 layer is a layer that has the function of converting linearly polarized light of a specific wavelength to circularly polarized light (or circularly polarized light to linearly polarized light). More specifically, it is a layer in which the in-plane retardation at a predetermined wavelength λnm is λ / 4 (or an odd multiple thereof). Among these, the in-plane retardation Re(550) of the λ / 4 layer at a wavelength of 550 nm is preferably 100 to 200 nm, more preferably 120 to 160 nm, and even more preferably 130 to 150 nm, in terms of the advantages of the present invention.
[0074] The λ / 4 layer may exhibit forward dispersiveness (in-plane retardation decreases as the measurement wavelength increases) or inverse dispersiveness (in-plane retardation increases as the measurement wavelength increases), but inverse dispersiveness is preferred. Furthermore, both forward and inverse dispersiveness are preferably exhibited in the visible light range.
[0075] The λ / 4 layer is not particularly limited in its composition and can include a layer containing a liquid crystal compound and a stretched film. Specific examples of liquid crystal compounds are the same as those described in the section on the light-absorbing anisotropic layer, so their explanation is omitted. Among these, a layer containing a liquid crystal compound is preferred as the λ / 4 layer, a layer with a fixed liquid crystal compound is more preferred, and a layer with a fixed horizontally oriented rod-shaped liquid crystal compound is even more preferred. The state in which the rod-shaped liquid crystal compound is horizontally oriented means that the long axis of the rod-shaped liquid crystal compound is parallel to the main surface of the λ / 4 layer. It is not required that they be strictly parallel, but it is preferable that the angle between the long axis of the rod-shaped liquid crystal compound and the main surface of the λ / 4 layer is in the range of 0 ± 20°, and preferably in the range of 0 ± 10°. The λ / 4 layer may be a single-layer structure or a multi-layer structure. For example, when the λ / 4 layer is a multi-layer structure, a broadband λ / 4 layer formed by laminating a λ / 4 layer and a λ / 2 layer can be mentioned.
[0076] The λ / 4 layer may be composed of liquid crystal cells. Using liquid crystal cells enables switching within a wide viewing angle range.
[0077] The thickness of the λ / 4 layer is not particularly limited, but for the sake of thinning, it is preferably 10 μm or less, and more preferably 0.1 to 5.0 μm. The thickness of the λ / 4 layer mentioned above refers to the average thickness of the λ / 4 layer. The average thickness is obtained by measuring the thickness of any five or more points in the λ / 4 layer and taking their arithmetic mean.
[0078] [λ / 2 layer] The λ / 2 layer refers to an optical anisotropic layer in which the in-plane retardation Re(λ) at a specific wavelength λnm satisfies Re(λ) ≈ λ / 2. This equation only needs to be achieved at any wavelength in the visible light region (for example, 550 nm). In particular, the in-plane retardation Re(550) at a wavelength of 550 nm of the λ / 2 layer is preferably 210 to 300 nm, as this provides excellent benefits for the present invention. The composition of the λ / 2 layer is not particularly limited and includes a layer containing a liquid crystal compound and a stretched film. Specific examples of liquid crystal compounds are the same as those described in the section on the light absorption anisotropic layer, so their explanation is omitted.
[0079] In particular, the λ / 2 layer is preferably a layer containing a liquid crystal compound, more preferably a layer in which the liquid crystal compound is fixed, and even more preferably a layer in which horizontally oriented rod-shaped liquid crystal compounds are fixed. The state in which the rod-shaped liquid crystal compound is horizontally oriented means that the long axis of the rod-shaped liquid crystal compound is parallel to the main surface of the λ / 2 layer. It is not required that they be strictly parallel, but it is preferable that the angle between the long axis of the rod-shaped liquid crystal compound and the main surface of the λ / 2 layer is in the range of 0 ± 20°, and preferably in the range of 0 ± 10°.
[0080] The λ / 2 layer may exhibit forward dispersiveness (a characteristic in which in-plane retardation decreases as the measurement wavelength increases) or inverse dispersiveness (a characteristic in which in-plane retardation increases as the measurement wavelength increases), but inverse dispersiveness is preferred. Furthermore, the above-mentioned forward and inverse dispersiveness are preferably exhibited in the visible light range.
[0081] The λ / 2 layer may be composed of liquid crystal cells. Using liquid crystal cells enables switching within a wide viewing angle range.
[0082] The thickness of the λ / 2 layer is not particularly limited, but for the sake of thinning, it is preferably 10 μm or less, and more preferably 0.1 to 5.0 μm. The thickness of the λ / 2 layer mentioned above refers to the average thickness of the λ / 2 layer. The average thickness is obtained by measuring the thickness of any five or more points on the λ / 2 layer and taking their arithmetic mean.
[0083] <Other Components> The first embodiment of the optical laminate of the present invention may have other components (for example, a support, an alignment film, an adhesive layer, and a bonding layer) in addition to the components described above (first light-absorbing anisotropic layer, second light-absorbing anisotropic layer, third light-absorbing anisotropic layer, first C plate, second C plate, and specific layer).
[0084] (Support) The first embodiment of the optical laminate of the present invention may have a support. The type of support is not particularly limited, and known supports can be used. In particular, a transparent support is preferred. A transparent support refers to a support with a visible light transmittance of 60% or more, preferably 80% or more, and more preferably 90% or more.
[0085] Examples of supports include glass substrates and polymer films. Materials for the polymer film include cellulose polymers; acrylic polymers having acrylic acid ester polymers such as polymethyl methacrylate and lactone ring-containing polymers; thermoplastic norbornene polymers; polycarbonate polymers; polyester polymers such as polyethylene terephthalate and polyethylene naphthalate; styrene polymers such as polystyrene and acrylonitrile styrene copolymers; polyolefin polymers such as polyethylene, polypropylene, and ethylene-propylene copolymers; vinyl chloride polymers; amide polymers such as nylon and aromatic polyamides; imide polymers; sulfone polymers; polyethersulfone polymers; polyetheretherketone polymers; polyphenylene sulfide polymers; vinylidene chloride polymers; vinyl alcohol polymers; vinyl butyral polymers; arylate polymers; polyoxymethylene polymers; epoxy polymers; or polymers obtained by mixing these polymers. Furthermore, the support is preferably removable.
[0086] (Alignment Film) The first embodiment of the optical laminate of the present invention may have an alignment film. Specifically, the alignment film may be a layer of polyvinyl alcohol and polyimide, with or without rubbing treatment; or a photo-alignment film of polyvinyl cinnamate and azo dye, with or without polarizing exposure treatment. The thickness of the alignment film is preferably 0.01 to 10 μm, and more preferably 0.01 to 1 μm.
[0087] (Adhesive layer) The first embodiment of the optical laminate of the present invention may have an adhesive layer. The adhesive layer is preferably a transparent, optically isotropic adhesive similar to those used in ordinary display devices, and is usually a pressure-sensitive adhesive.
[0088] The adhesive layer may contain appropriate additives such as crosslinking agents (e.g., isocyanate-based crosslinking agents and epoxy-based crosslinking agents), tackifiers (e.g., rosin derivative resins, polyterpene resins, petroleum resins, and oil-soluble phenolic resins), plasticizers, fillers, antioxidants, surfactants, UV absorbers, light stabilizers, and antioxidants.
[0089] (Adhesive layer) The first embodiment of the optical laminate of the present invention may have an adhesive layer. The adhesive layer exhibits adhesive properties through drying and reaction after bonding. Polyvinyl alcohol-based adhesives (PVA-based adhesives) exhibit adhesive properties upon drying, enabling bonding of materials.
[0090] Specific examples of curing adhesives that exhibit adhesive properties through reaction include active energy ray curing adhesives such as (meth)acrylate adhesives, and cationic polymerization curing adhesives. Examples of curing components in (meth)acrylate adhesives include compounds having a (meth)acryloyl group and compounds having a vinyl group. Compounds having an epoxy group or an oxetanyl group can also be used as cationic polymerization curing adhesives. Among these, UV-curing adhesives that cure with ultraviolet irradiation are preferred in terms of resistance to heat deformation.
[0091] In addition to the above, other possible components of the first embodiment of the optical laminate of the present invention include, for example, a protective layer, an oxygen barrier layer, an ultraviolet absorbing layer, and a blue light absorbing layer.
[0092] The method for manufacturing the first embodiment of the optical laminate of the present invention is not particularly limited and known methods can be used. For example, the optical laminate can be manufactured by laminating the above-mentioned components via an adhesive layer or bonding layer.
[0093] <<Modified Version of the First Embodiment>> Figure 2 shows a schematic cross-sectional view of a modified version of the first embodiment of the optical laminate of the present invention. The optical laminate 102A has, in this order, a first light-absorbing anisotropic layer 10A, a specific layer 32, a first C plate 20A, a specific layer 34, a second light-absorbing anisotropic layer 12A, a specific layer 36, a second C plate 22A, a specific layer 38, and a third light-absorbing anisotropic layer 14A. The optical laminate 102A corresponds to an embodiment that satisfies the above-mentioned requirements A1, B2, and B3. With this embodiment, the effects of the present invention can be obtained at multiple azimuth angles. In the optical laminate 102A of Figure 2, components similar to those in the optical laminate 100A of Figure 1 are denoted by the same reference numerals and their descriptions are omitted.
[0094] The preferred range for the relationship between the absorption axis of the second light-absorbing anisotropic layer 12A and the absorption axis of the third light-absorbing anisotropic layer 14A is as described above.
[0095] When the specific layer 32 is a twisted layer, the angle between the in-plane slow axis on the surface of the specific layer 32 on the side of the second light absorption anisotropy layer 12A and the absorption axis of the second light absorption anisotropy layer 12A is preferably 30 to 60°, and more preferably 35 to 55°, in terms of the advantages of the present invention.
[0096] The specific layer 34, specific layer 36, and specific layer 38 may all be a twisted layer, a λ / 4 layer, or a λ / 2 layer, but in the configuration of Figure 2, it is preferable that the specific layer 34, specific layer 36, and specific layer 38 are λ / 4 layers. When the specific layer 34 is a λ / 4 layer, the angle between the absorption axis of the second light absorption anisotropy layer 12A and the in-plane slow phase axis of the specific layer 34 (λ / 4 layer) is preferably in the range of 45 ± 20° (25 to 65°), and more preferably in the range of 45 ± 10° (35 to 55°), which is an excellent point for achieving the effects of the present invention. When the specific layer 34 is a λ / 4 layer and the specific layer 32 is a twisted layer, the angle between the in-plane slow axis of the specific layer 34 (λ / 4 layer) and the in-plane slow axis of the specific layer 32 (twisted layer) on the surface facing the specific layer 34 is preferably 90 ± 20° (in the range of 70 to 110°) and more preferably 90 ± 10° (in the range of 80 to 100°) in terms of the advantages of the present invention. When the specific layer 36 is a λ / 4 layer, the angle between the absorption axis of the second light absorption anisotropy layer 12A and the in-plane slow axis of the specific layer 36 (λ / 4 layer) is preferably 45 ± 20° (in the range of 25 to 65°) and more preferably 45 ± 10° (in the range of 35 to 55°) in terms of the advantages of the present invention. When the specific layer 38 is a λ / 4 layer, the angle between the absorption axis of the second light absorption anisotropy layer 12A and the in-plane slow axis of the specific layer 38 (λ / 4 layer) is preferably in the range of 45 ± 20° (25 to 65°) and more preferably in the range of 45 ± 10° (35 to 55°) in terms of the advantages of the present invention. When the specific layer 36 is a λ / 4 layer and the specific layer 38 is a λ / 4 layer, the angle between the in-plane slow axis of the specific layer 36 (λ / 4 layer) and the in-plane slow axis of the specific layer 38 (λ / 4 layer) is preferably in the range of 90 ± 20° (70 to 110°) and more preferably in the range of 90 ± 10° (80 to 100°) in terms of the advantages of the present invention. The configurations of the twist layer, λ / 4 layer and λ / 2 layer are as described in the first embodiment.
[0097] The optical laminate 102A of the present invention shown in Figure 2 differs from the optical laminate A shown in Figure 1 in that a specific layer is arranged between the light-absorbing anisotropic layer Y and the C plate. In Figure 2, the specific layer is arranged in all of the spaces between the light-absorbing anisotropic layer Y and the C plate, but the invention is not limited to this embodiment; it is sufficient that the specific layer is arranged in at least one of the spaces between the light-absorbing anisotropic layer Y and the C plate. By arranging the specific layer between the light-absorbing anisotropic layer Y and the C plate, the effects of the present invention are further enhanced even when the polar angle is changed at various azimuthal angles within the plane of the optical laminate. This is because, by arranging the specific layer, the light that has passed through the light-absorbing anisotropic layer Y is more susceptible to the influence of the C plate at various azimuthal angles, and as a result, the effects of the present invention are further enhanced at various azimuthal angles.
[0098] <<Second Embodiment>> Figure 3 shows a schematic cross-sectional view of a second embodiment of the optical laminate of the present invention. The optical laminate 100B has, in this order, a first light-absorbing anisotropic layer 10B, a first C plate 20B, a specific layer 40, a second light-absorbing anisotropic layer 12B, a specific layer 42, a second C plate 22B, and a third light-absorbing anisotropic layer 14B. The specific layer 40 and the specific layer 42 are twisted layers, λ / 4 layers, or λ / 2 layers. The second light-absorbing anisotropic layer 12B is a light-absorbing anisotropic layer X, and the first light-absorbing anisotropic layer 10B and the third light-absorbing anisotropic layer 14B are light-absorbing anisotropic layers Y. The optical laminate 100B corresponds to an embodiment that satisfies requirement A2 described above.
[0099] Although the layers are arranged adjacent to each other in Figure 3, the embodiment is not limited to this, and other members may be included between the layers.
[0100] As described above, the first optical absorption anisotropy layer 10B and the third optical absorption anisotropy layer 14B are optical absorption anisotropy layers Y, and the definition of optical absorption anisotropy layer Y is as described in the first embodiment of the optical laminate of the present invention. The angle between the absorption axis of the first optical absorption anisotropy layer 10B and the absorption axis of the third optical absorption anisotropy layer 14B is not particularly limited, but in terms of superior effects of the present invention, a range of 90 ± 30° (60 to 120°) is preferred, a range of 90 ± 20° (70 to 110°) is more preferred, and a range of 90 ± 10° (80 to 100°) is even more preferred. As described above, the second optical absorption anisotropy layer 12B is optical absorption anisotropy layer X, and the definition of optical absorption anisotropy layer X is as described in the first embodiment of the optical laminate of the present invention.
[0101] The definitions and preferred embodiments of the first C plate 20B and the second C plate 22B are the same as the definitions and preferred embodiments of the first C plate 20A and the second C plate 22A described in the first embodiment of the optical laminate of the present invention.
[0102] As described above, the specific layer 40 and the specific layer 42 may be a twisted layer, a λ / 4 layer, or a λ / 2 layer, but in the configuration of Figure 3, it is preferable that the specific layer 40 and the specific layer 42 are twisted layers. The configurations of the twisted layer, λ / 4 layer, and λ / 2 layer are as described in the first embodiment of the optical laminate of the present invention. When the specific layer 40 is a twisted layer, the angle between the in-plane slow axis on the surface of the specific layer 40 on the second optical absorption anisotropy layer 12B side and the absorption axis of the third optical absorption anisotropy layer 14B is preferably in the range of 0 to 20°, and more preferably in the range of 0 to 10°, in terms of achieving better effects of the present invention. When the specific layer 42 is a twisted layer, the angle between the in-plane slow axis on the surface of the specific layer 42 on the third light absorption anisotropy layer 14B side and the absorption axis of the third light absorption anisotropy layer 14B is preferably in the range of 45 ± 20° (25 to 65°) and more preferably in the range of 45 ± 10° (35 to 55°) in terms of achieving superior effects of the present invention.
[0103] A second embodiment of the optical laminate of the present invention may have other components besides those described above (first optical anisotropy layer, second optical anisotropy layer, third optical anisotropy layer, first C plate, second C plate, and specific layer). Examples of other components include those described in the first embodiment of the optical laminate of the present invention.
[0104] The method for manufacturing the second embodiment of the optical laminate of the present invention is not particularly limited and known methods can be used. For example, the optical laminate can be manufactured by laminating the above-described members via an adhesive layer or bonding agent layer.
[0105] <<Modified Version of the Second Embodiment>> Figure 4 shows a schematic cross-sectional view of a modified version of the second embodiment of the optical laminate of the present invention. The optical laminate 102B has, in this order, a first light-absorbing anisotropic layer 10B, a specific layer 44, a first C plate 20B, a specific layer 40, a second light-absorbing anisotropic layer 12B, a specific layer 42, a second C plate 22B, a specific layer 46, and a third light-absorbing anisotropic layer 14B. The optical laminate 102B corresponds to an embodiment that satisfies the above-mentioned requirements A2, B1, and B3. In the optical laminate 102B of Figure 4, components similar to those in the optical laminate 100B of Figure 3 are denoted by the same reference numerals and their description is omitted.
[0106] The angle between the absorption axis of the first light-absorbing anisotropic layer 10B and the absorption axis of the third light-absorbing anisotropic layer 14B is not particularly limited, but a range of 0 to 30° is preferred, a range of 0 to 20° is more preferred, and a range of 0 to 10° is even more preferred in terms of achieving superior effects of the present invention.
[0107] The preferred range for the relationship between the in-plane slow axis of the specific layer 40 and the absorption axis of the third light absorption anisotropy layer 14B is as described above. The preferred range for the relationship between the in-plane slow axis of the specific layer 42 and the absorption axis of the third light absorption anisotropy layer 14B is as described above.
[0108] The specific layer 44 and the specific layer 46 may both be a twisted layer, a λ / 4 layer, or a λ / 2 layer, but in the configuration of Figure 4, it is preferable that the specific layer 44 is a λ / 4 layer and the specific layer 46 is a λ / 2 layer.
[0109] When the specific layer 44 is a λ / 4 layer, the angle between the absorption axis of the first light absorption anisotropy layer 10B and the in-plane slow axis of the specific layer 44 (λ / 4 layer) (hereinafter simply referred to as "angle αB") is preferably in the range of 45 ± 20° (25 to 65°) and more preferably in the range of 45 ± 10° (35 to 55°) in terms of achieving superior effects of the present invention. When the specific layer 44 is a λ / 4 layer and the specific layer 40 is a twisted layer, the angle between the in-plane slow axis of the specific layer 44 (λ / 4 layer) and the in-plane slow axis of the specific layer 40 (twisted layer) on the surface facing the specific layer 44 is preferably in the range of 90 ± 20° (70 to 110°) and more preferably in the range of 90 ± 10° (80 to 100°) in terms of achieving superior effects of the present invention.
[0110] When the specific layer 46 is a λ / 2 layer, the angle between the absorption axis of the third light absorption anisotropy layer 14B and the in-plane slow phase axis of the specific layer 46 (λ / 2 layer) (hereinafter simply referred to as "angle βB") is preferably in the range of 22.5 ± 20° (2.5 to 42.5°) and more preferably in the range of 22.5 ± 10° (12.5 to 32.5°) in terms of achieving superior effects of the present invention. When the specific layer 46 is a λ / 2 layer and the specific layer 42 is a twisted layer, the angle between the in-plane slow phase axis of the specific layer 46 (λ / 2 layer) and the in-plane slow phase axis of the specific layer 42 (twisted layer) on the surface facing the specific layer 46 is preferably in the range of 22.5 ± 20° (2.5 to 42.5°) and more preferably in the range of 22.5 ± 10° (12.5 to 32.5°) in terms of achieving superior effects of the present invention.
[0111] <<Third Embodiment>> Figure 5 shows a schematic cross-sectional view of a third embodiment of the optical laminate of the present invention. The optical laminate 100C has, in this order, a first light-absorbing anisotropic layer 10C, a specific layer 50, a first C plate 20C, a second light-absorbing anisotropic layer 12C, a second C plate 22C, a specific layer 52, and a third light-absorbing anisotropic layer 14C. The specific layer 50 and the specific layer 52 are twisted layers, λ / 4 layers, or λ / 2 layers. The first light-absorbing anisotropic layer 10C and the third light-absorbing anisotropic layer 14C are light-absorbing anisotropic layers X, and the second light-absorbing anisotropic layer 12C is a light-absorbing anisotropic layer Y. The optical laminate 100C corresponds to an embodiment that satisfies requirements A1 and A3 described above.
[0112] Although the layers are arranged adjacent to each other in Figure 5, the embodiment is not limited to this, and other members may be included between the layers.
[0113] As described above, the first optical absorption anisotropy layer 10C and the third optical absorption anisotropy layer 14C are optical absorption anisotropy layers X, and the definition of optical absorption anisotropy layer X is as described in the first embodiment of the optical laminate of the present invention. Furthermore, the second optical absorption anisotropy layer 12C is optical absorption anisotropy layer Y, and the definition of optical absorption anisotropy layer Y is as described in the first embodiment of the optical laminate of the present invention.
[0114] The definitions and preferred embodiments of the first C plate 20C and the second C plate 22C are the same as the definitions and preferred embodiments of the first C plate 20A and the second C plate 22A described in the first embodiment of the optical laminate of the present invention.
[0115] As described above, the specific layer 50 and the specific layer 52 may be a twisted layer, a λ / 4 layer, or a λ / 2 layer, but in the configuration of Figure 5, it is preferable that the specific layer 50 and the specific layer 52 are twisted layers. The configurations of the twisted layer, λ / 4 layer, and λ / 2 layer are as described in the first embodiment of the optical laminate of the present invention. When the specific layer 50 is a twisted layer, the angle between the in-plane slow axis on the surface of the specific layer 50 on the second optical absorption anisotropy layer 12C side and the absorption axis of the second optical absorption anisotropy layer 12C is preferably in the range of 0 to 20°, and more preferably in the range of 0 to 10°, in terms of achieving better effects of the present invention. When the specific layer 52 is a twisted layer, the angle between the in-plane slow axis on the surface of the specific layer 52 on the second light absorption anisotropy layer 12C side and the absorption axis of the second light absorption anisotropy layer 12C is preferably in the range of 0 to 20°, and more preferably in the range of 0 to 10°, in terms of achieving superior effects of the present invention.
[0116] A third embodiment of the optical laminate of the present invention may have other components besides those described above (first optical anisotropy layer, second optical anisotropy layer, third optical anisotropy layer, first C plate, second C plate, and specific layer). Examples of other components include those described in the first embodiment of the optical laminate of the present invention.
[0117] The method for manufacturing the third embodiment of the optical laminate of the present invention is not particularly limited and known methods can be used. For example, the optical laminate can be manufactured by laminating the above-described components via an adhesive layer or bonding agent layer.
[0118] <<Deformability of the Third Embodiment>> Figure 6 shows a schematic cross-sectional view of a modified example of the third embodiment of the optical laminate of the present invention. The optical laminate 102C has, in this order, a first light-absorbing anisotropic layer 10C, a specific layer 50, a first C plate 20C, a specific layer 54, a second light-absorbing anisotropic layer 12C, a specific layer 56, a second C plate 22C, a specific layer 52, and a third light-absorbing anisotropic layer 14C. In the optical laminate 102C of Figure 6, components similar to those in the optical laminate 100C of Figure 5 are given the same reference numerals and their descriptions are omitted.
[0119] The specific layer 54 and the specific layer 56 may both be a twisted layer, a λ / 4 layer, or a λ / 2 layer, but in the configuration of Figure 6, it is preferable that the specific layer 54 is a λ / 4 layer and the specific layer 56 is a λ / 2 layer.
[0120] When the specific layer 54 is a λ / 4 layer, the angle between the absorption axis of the second light absorption anisotropy layer 12C and the in-plane slow axis of the specific layer 54 (λ / 4 layer) (hereinafter simply referred to as "angle αC") is preferably in the range of 45 ± 20° (25 to 65°) and more preferably in the range of 45 ± 10° (35 to 55°) in terms of achieving superior effects of the present invention. When the specific layer 54 is a λ / 4 layer and the specific layer 50 is a twisted layer, the angle between the in-plane slow axis of the specific layer 54 (λ / 4 layer) and the in-plane slow axis of the specific layer 50 (twisted layer) on the surface facing the specific layer 54 is preferably in the range of 90 ± 20° (70 to 110°) and more preferably in the range of 90 ± 10° (80 to 100°) in terms of achieving superior effects of the present invention.
[0121] When the specific layer 56 is a λ / 2 layer, the angle between the absorption axis of the second light absorption anisotropy layer 12C and the in-plane slow phase axis of the specific layer 56 (λ / 2 layer) is preferably in the range of 22.5 ± 20° (2.5 to 42.5°) and more preferably in the range of 22.5 ± 10° (12.5 to 32.5°) in terms of achieving superior effects of the present invention. When the specific layer 56 is a λ / 2 layer and the specific layer 52 is a twisted layer, the angle between the in-plane slow phase axis of the specific layer 56 (λ / 2 layer) and the in-plane slow phase axis of the specific layer 52 (twisted layer) on the surface facing the specific layer 56 is preferably in the range of 22.5 ± 20° (2.5 to 42.5°) and more preferably in the range of 22.5 ± 10° (12.5 to 32.5°) in terms of achieving superior effects of the present invention.
[0122] <<Fourth Embodiment>> Figure 7 shows a schematic cross-sectional view of the fourth embodiment of the optical laminate of the present invention. The optical laminate 100D has, in this order, a first light-absorbing anisotropic layer 10D, a specific layer 60, a first C plate 20D, a specific layer 62, a second light-absorbing anisotropic layer 12D, a specific layer 64, a second C plate 22D, and a third light-absorbing anisotropic layer 14D. The specific layers 60, 62, and 64 are twisted layers, λ / 4 layers, or λ / 2 layers. The first light-absorbing anisotropic layer 10D and the second light-absorbing anisotropic layer 12D are light-absorbing anisotropic layers X, and the third light-absorbing anisotropic layer 14D is a light-absorbing anisotropic layer Y. The optical laminate 100D corresponds to an embodiment that satisfies requirements A1 and A2 described above.
[0123] Although the layers are arranged adjacent to each other in Figure 7, the embodiment is not limited to this, and other members may be included between the layers.
[0124] As described above, the first optical absorption anisotropy layer 10D and the second optical absorption anisotropy layer 12D are optical absorption anisotropy layers X, and the definition of optical absorption anisotropy layer X is as described in the first embodiment of the optical laminate of the present invention. Furthermore, the third optical absorption anisotropy layer 14D is optical absorption anisotropy layer Y, and the definition of optical absorption anisotropy layer Y is as described in the first embodiment of the optical laminate of the present invention.
[0125] The definitions and preferred embodiments of the first C plate 20D and the second C plate 22D are the same as the definitions and preferred embodiments of the first C plate 20A and the second C plate 22A described in the first embodiment of the optical laminate of the present invention.
[0126] As described above, the specific layer 60, specific layer 62, and specific layer 64 may be a twisted layer, a λ / 4 layer, or a λ / 2 layer, but in the configuration of Figure 7, it is preferable that the specific layer 60, specific layer 62, and specific layer 64 are twisted layers. The configurations of the twisted layer, λ / 4 layer, and λ / 2 layer are as described in the first embodiment of the optical laminate of the present invention.
[0127] A fourth embodiment of the optical laminate of the present invention may have other components besides those described above (first light-absorbing anisotropic layer, second light-absorbing anisotropic layer, third light-absorbing anisotropic layer, first C plate, second C plate, and specific layer). Examples of other components include those described in the first embodiment of the optical laminate of the present invention.
[0128] The method for manufacturing the fourth embodiment of the optical laminate of the present invention is not particularly limited and known methods can be used. For example, the optical laminate can be manufactured by laminating the above-described members via an adhesive layer or bonding layer.
[0129] <<Fifth Embodiment>> Figure 8 shows a schematic cross-sectional view of the fifth embodiment of the optical laminate of the present invention. The optical laminate 100E has, in this order, a first light-absorbing anisotropic layer 10E, a specific layer 70, a first C plate 20E, a specific layer 72, a second light-absorbing anisotropic layer 12E, a specific layer 74, a second C plate 22E, a specific layer 74, and a third light-absorbing anisotropic layer 14E. The specific layers 70, 72, 74, and 76 are twisted layers, λ / 4 layers, or λ / 2 layers. The first light-absorbing anisotropic layer 10E, the second light-absorbing anisotropic layer 12E, and the third light-absorbing anisotropic layer 14E are light-absorbing anisotropic layers X. The optical laminate 100E corresponds to an embodiment that satisfies the above-described requirements A1, A2, and A3.
[0130] Although the layers are arranged adjacent to each other in Figure 8, the embodiment is not limited to this, and other members may be included between the layers.
[0131] As described above, the first optical absorption anisotropy layer 10E, the second optical absorption anisotropy layer 12E, and the third optical absorption anisotropy layer 14E are optical absorption anisotropy layers X, and the definition of optical absorption anisotropy layer X is as described in the first embodiment of the optical laminate of the present invention.
[0132] The definitions and preferred embodiments of the first C plate 20E and the second C plate 22E are the same as the definitions and preferred embodiments of the first C plate 20A and the second C plate 22A described in the first embodiment of the optical laminate of the present invention.
[0133] As described above, the specific layers 70, 72, 74, and 76 may be twisted layers, λ / 4 layers, and λ / 2 layers, but in the configuration of Figure 8, it is preferable that the specific layers 70, 72, 74, and 76 are twisted layers. The configurations of the twisted layers, λ / 4 layers, and λ / 2 layers are as described in the first embodiment of the optical laminate of the present invention.
[0134] A fifth embodiment of the optical laminate of the present invention may have other components besides those described above (first light-absorbing anisotropic layer, second light-absorbing anisotropic layer, third light-absorbing anisotropic layer, first C plate, second C plate, and specific layer). Examples of other components include those described in the first embodiment of the optical laminate of the present invention.
[0135] The method for manufacturing the fifth embodiment of the optical laminate of the present invention is not particularly limited and known methods can be used. For example, the optical laminate can be manufactured by laminating the above-described members via an adhesive layer or bonding layer.
[0136] The optical laminate of the present invention includes a first optical absorption anisotropy layer, a second optical absorption anisotropy layer, and a third optical absorption anisotropy layer, but may also include another optical absorption anisotropy layer. Examples of the other optical absorption anisotropy layers include the optical absorption anisotropy layer X and optical absorption anisotropy layer Y described above. Furthermore, the optical laminate of the present invention may include two or more other optical absorption anisotropy layers. For example, the optical laminate 100F, which is a sixth embodiment of the optical laminate of the present invention shown in Figure 9, includes a first optical absorption anisotropy layer 10F, a specific layer 80, a first C plate 20F, a second optical absorption anisotropy layer 12F, a second C plate 22F, a third optical absorption anisotropy layer 14F, a third C plate 24F, and a fourth optical absorption anisotropy layer 16F. The first optical absorption anisotropy layer 10F is optical absorption anisotropy layer X, and the second optical absorption anisotropy layer 12F, the third optical absorption anisotropy layer 14F, and the fourth optical absorption anisotropy layer 16 are optical absorption anisotropy layer Y. The specific layer 80 is a twisted layer, a λ / 4 layer, or a λ / 2 layer.
[0137] The optical laminate 100F corresponds to an embodiment that includes four light-absorbing anisotropic layers. As shown in this embodiment, the optical laminate of the present invention may include four or more light-absorbing anisotropic layers. There is no particular upper limit to the number of light-absorbing anisotropic layers in the optical laminate of the present invention, but it may be five or less. Furthermore, even when the optical laminate of the present invention includes four or more light-absorbing anisotropic layers, it is preferable that C plates are arranged between the light-absorbing anisotropic layers that are spaced apart from each other. In other words, the present invention preferably provides an optical laminate comprising three or more light-absorbing anisotropic layers spaced apart from each other, and a C plate positioned between two adjacent light-absorbing anisotropic layers among the three or more light-absorbing anisotropic layers, wherein the three or more light-absorbing anisotropic layers are either light-absorbing anisotropic layers X or light-absorbing anisotropic layers Y, and one or more of the three or more light-absorbing anisotropic layers are light-absorbing anisotropic layers X, and if one of the two light-absorbing anisotropic layers flanking the C plate is a light-absorbing anisotropic layer X, a specific layer is positioned between the C plate and the light-absorbing anisotropic layer X, and if both of the two light-absorbing anisotropic layers flanking the C plate are light-absorbing anisotropic layers X, a specific layer is positioned between the C plate and one of the two light-absorbing anisotropic layers, and between the C plate and the other of the two light-absorbing anisotropic layers.
[0138] <<Applications>> The optical laminate of the present invention can be applied to various applications. For example, the optical laminate of the present invention can be applied to a display device. A display device including the optical laminate of the present invention has excellent image visibility over a wide range of extreme angles from the front of the display device, and also has excellent anti-peeping performance because the image visibility can be rapidly reduced from a predetermined extreme angle. The display element used in the display device including the optical laminate of the present invention is not particularly limited, and examples include liquid crystal cells, organic electroluminescent (hereinafter abbreviated as "EL") display panels, and plasma display panels. Of these, liquid crystal cells or organic EL display panels are preferred. That is, the display device of the present invention is preferably a liquid crystal display device using a liquid crystal cell as the display element, or an organic EL display device using an organic EL display panel as the display element. Some image display devices are thin and can be molded into curved surfaces. Since the optical laminate used in the present invention is thin and easily bendable, it can be suitably applied to display devices with curved display surfaces.
[0139] Furthermore, the optical laminate of the present invention is also applicable to sensor devices. When the optical laminate of the present invention is applied to a sensor device, for example, by placing the optical laminate of the present invention in front of the light-receiving element of the sensor device, light from the front direction can reach the light-receiving element, but light from an oblique direction cannot reach the light-receiving element.
[0140] Furthermore, the wavelength of light targeted by the optical laminate of the present invention is not particularly limited and may be visible light or infrared light (for example, near-infrared light). In other words, the light whose transmittance is controlled by the optical laminate of the present invention may be visible light or infrared light.
[0141] The features of the present invention will be described in more detail below with reference to examples and comparative examples. The materials, amounts used, proportions, processing content, and processing procedures shown in the following examples can be modified as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below.
[0142] <Example 1> [Preparation of Light-Absorbing Anisotropic Layer 1 (Vertical Orientation)] (Preparation of Substrate) The following components were placed in a mixing tank, stirred, and then heated at 90°C for 10 minutes. The resulting composition was then filtered through filter paper with an average pore size of 34 μm and a sintered metal filter with an average pore size of 10 μm to prepare a dope. The solid content concentration of the dope was 23.5% by mass, and the solvent of the dope was methylene chloride / methanol / butanol = 81 / 18 / 1 (mass ratio).
[0143] -------------------------------------------------- Cellulose acylate dope -------------------------------------------------- Cellulose acylate (acetyl substitution degree 2.86, viscosity-average degree of polymerization 310) 100 parts by mass Sugar ester compound 1 (formula (S4) below) 6.0 parts by mass Sugar ester compound 2 (formula (S5) below) 2.0 parts by mass Silica particle dispersion (AEROSIL R972, manufactured by Nippon Aerosil Co., Ltd.) 0.1 parts by mass Solvent (methylene chloride / methanol / butanol) 351.9 parts by mass
[0144]
[0145]
[0146] The dope prepared as described above was cast using a drum film-forming machine. The dope was cast from the die so that it was in contact with a metal support cooled to 0°C, and then the resulting web (film) was peeled off the drum. The drum was made of SUS (stainless steel).
[0147] After the casting process, the obtained web (film) was peeled from the drum and dried for 20 minutes in a tenter device at 30-40°C during film transport, using clips to hold both ends of the web in place. Subsequently, the web was further dried by zone heating while being transported on a roll. The obtained web was knurled and then wound up to form cellulose acylate film A1. The thickness of the obtained cellulose acylate film A1 was 60 μm, the in-plane retardation Re(550) at a wavelength of 550 nm was 1 nm, and the thickness-direction retardation Rth(550) at a wavelength of 550 nm was 35 nm.
[0148] (Formation of specific layer UL1) The specific layer-forming composition UL1, described later, was continuously applied to the cellulose acylate film A1 using a wire bar. The cellulose acylate film with the coating was dried with 60°C hot air for 60 seconds, and then heated with 300 mJ / cm using an LED (light emitting diode) lamp (center wavelength 365 nm). 2 A specific layer UL1 was fabricated on the cellulose acylate film A1 by irradiation under the following irradiation conditions. The thickness of the specific layer UL1 was 0.4 μm. -------------------------------------------------- Composition of the specific layer-forming composition UL1 -------------------------------------------------- ・UA-306T (manufactured by Kyoeisha Chemical Co., Ltd.) 9.23 parts by mass ・Boron acid compound B-1 below 2.40 parts by mass ・IRGACUREOXE-02 (manufactured by BASF) 0.35 parts by mass ・Surfactant S-1 below 0.024 parts by mass ・Butyl acetate 74.80 parts by mass ・Methyl ethyl ketone 13.20 parts by mass --------------------------------------------------
[0149] Boronic acid compound B-1
[0150]
[0151] Surfactant S-1 (The numerical value indicated for each repeating unit represents the content (mass%) of each repeating unit relative to the total number of repeating units. n is 9. The weight-average molecular weight is 11000. Ac represents an acetyl group.)
[0152]
[0153] (Formation of a resin layer containing PVA (polyvinyl alcohol)) The resin layer-forming composition 1 containing PVA, as described below, was applied to the specific layer of the obtained cellulose acylate film with the specific layer using a wire bar. After the coating was formed, the obtained cellulose acylate film was dried with hot air at 60°C for 60 seconds, and then with hot air at 100°C for 120 seconds to form a resin layer AL1 containing PVA. The thickness of the resin layer AL1 containing PVA was 0.15 μm.
[0154] ------------------------------------------------------------------- Composition 1 for forming a resin layer ------------------------------------------------------------------- ・Modified polyvinyl alcohol PVA-1 1.81 parts by mass ・Water 75.39 parts by mass ・Methanol 22.80 parts by mass -------------------------------------------------------------------
[0155] (Modified polyvinyl alcohol PVA-1) Note that the composition ratio of each repeating unit is based on mol%.
[0156]
[0157] (Formation of light-absorbing anisotropic layer) The following light-absorbing anisotropic layer-forming composition P1 was continuously applied to the obtained PVA-containing resin layer AL1 using a wire bar, and the coating was heated at 120°C for 60 seconds, then cooled to room temperature (23°C). Next, the coating was heated at 75°C for 60 seconds and cooled again to room temperature. After that, an LED lamp (center wavelength 365 nm) was used to illuminate the coating from the normal direction at an illuminance of 200 mW / cm². 2A light-absorbing anisotropic layer 1 was fabricated on a resin layer AL1 containing PVA by irradiating it for 2 seconds under the specified irradiation conditions. The thickness of the light-absorbing anisotropic layer 1 was 1.75 μm. The angle between the transmittance center axis of the fabricated light-absorbing anisotropic layer 1 and the normal direction of the surface (main surface) of the light-absorbing anisotropic layer 1 was found to be 0° when examined using the method described above.
[0158] --------------------------------------------------------------------------- Composition P1 for forming anisotropic light-absorbing layer --------------------------------------------------------------------------- • 0.76 parts by mass of the following dichroic substance D-1 • 0.04 parts by mass of the following dichroic substance D-2 • 1.13 parts by mass of the following dichroic substance D-3 • 4.10 parts by mass of the following polymer liquid crystal compound P-1 • 2.54 parts by mass of the following liquid crystal compound L-1 • 0.13 parts by mass of IRGACURE OXE-2 (manufactured by BASF) • 0.05 parts by mass of the following orientation agent E-1 • 0.016 parts by mass of the following surfactant S-2 • 82.11 parts by mass of cyclopentanone • 9.12 parts by mass of benzyl alcohol ---------------------------------------------------------------------------
[0159] Dichroic substance D-1
[0160]
[0161] Dichroic substance D-2
[0162]
[0163] Dichroic substance D-3
[0164]
[0165] Polymeric liquid crystal compound P-1 (The numerical values indicated for each repeating unit ("59", "15", "26") represent the content (mass %) of each repeating unit relative to the total number of repeating units. The weight-average molecular weight is 21,000.)
[0166]
[0167] Liquid crystal compound L-1 [A mixture of the following liquid crystal compounds (RA), (RB), and (RC) in a mass ratio of 84:14:2]
[0168]
[0169] Orienting agent E-1
[0170]
[0171] Surfactant S-2 (The numerical values indicated for each repeating unit ("40", "40", "20") represent the content (mass %) of each repeating unit relative to the total number of repeating units. The weight-average molecular weight is 11,000.)
[0172]
[0173] (Formation of protective layer B1) The protective layer-forming composition B1 described below was continuously applied to the obtained light-absorbing anisotropic layer 1 using a wire bar to form a coating film. Next, the coating film was dried with 80°C hot air for 60 seconds to form protective layer B1, and then cooled to room temperature (23°C). After that, an LED lamp (center wavelength 365 nm) was used to illuminate the coating film from the normal direction at an illuminance of 200 mW / cm². 2 An optical film was fabricated by irradiating the light-absorbing anisotropic layer 1 for 2 seconds under the specified irradiation conditions, thereby forming a protective layer B1. The thickness of the protective layer B1 was 1.0 μm.
[0174] --------------------------------------------------------------------------- Composition B1 for forming a protective layer --------------------------------------------------------------------------- • UA-306T (manufactured by Kyoeisha Chemical Co., Ltd.) 19.42 parts by mass • IRGACURE OXE-2 (manufactured by BASF) 0.56 parts by mass • The above surfactant S-2 0.02 parts by mass • Isopropyl alcohol 67.38 parts by mass • Propylene glycol monomethyl ether 12.62 parts by mass
[0175] [Fabrication of Light Absorption Anisotropic Layer 2 (Horizontal Orientation)] Using the same method as for the polarizing plate 02 with a single-sided protective film described in International Publication No. 2015 / 166991, a light absorption anisotropic layer (polarizer) with a thickness of 8 μm and one side exposed was fabricated. Next, the single-plate transmittance of the light absorption anisotropic layer 2 at a wavelength of 550 nm was measured using a spectrophotometer VAP-7070 (JASCO Corporation) and found to be 43%. Furthermore, when the fabricated light absorption anisotropic layer 2 was placed on a surface light source, and a polarizing plate was placed on top of the light absorption anisotropic layer 2, and the polarizing plate was rotated while maintaining a state parallel to the light absorption anisotropic layer 2, the brightness of the surface light source when viewed from the front changed, confirming that the absorption axis of the light absorption anisotropic layer 2 is in the plane of the light absorption anisotropic layer 2.
[0176] [Preparation of C plate 1] An optical film 1A was prepared in the same manner as in Example 5 of Japanese Patent Application Publication No. 2016-105127, except that the thickness of the phase difference layer was changed, and a phase difference layer 1A formed using a rod-shaped liquid crystal compound was placed on a peelable support consisting of a substrate and an alignment film. The Re(550) of the phase difference layer 1A in the optical film 1A was 0 nm and the Rth(550) was -250 nm. The average inclination angle of the long axis of the rod-shaped liquid crystal compound in the phase difference layer 1A with respect to the film surface was 0° in all cases, confirming that the rod-shaped liquid crystal compound was oriented perpendicular to the film surface.
[0177] Two optical films 1A prepared as described above were prepared and bonded together using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) so that their phase difference layers faced each other. By peeling off one of the release supports, an optical film 1B was prepared in which the phase difference layer 1B was positioned on the release support. The Re(550) of the phase difference layer 1B in optical film 1B was 0 nm and the Rth(550) was -500 nm.
[0178] Next, two of the optical films 1B prepared as described above were prepared and bonded together using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) so that their phase difference layers 1B faced each other. A C plate 1 was then fabricated on the release support by peeling off one of the release supports. The Re(550) of the C plate 1 was 0 nm and the Rth(550) was -1000 nm.
[0179] [Preparation of Twist Layer 1] A release support was prepared by rubbing the surface of a 75 μm polyethylene terephthalate (PET) film (manufactured by Fujifilm Corporation). The following twist layer forming composition 1 was applied to the rubbing surface of the prepared release support using a bar coater to form a coating film with a thickness of 3.1 μm. Next, the obtained film was heated and aged for 90 seconds at a film surface temperature of 60°C, and then 300 mJ / cm² was applied to the coating film at 100°C. 2 By irradiating with ultraviolet light, the orientation of the liquid crystal compound was fixed to form a twisted layer 1, and a peelable support and the twisted layer 1 were fabricated. Analysis using AxoScan OPMF-2 (Axometrics) confirmed that in the obtained twisted layer 1, the Δnd between the refractive index anisotropy Δn of the twisted layer 1 at a wavelength of 550 nm and the thickness d of the twisted layer 1 was 500 nm. Furthermore, the twisted layer 1 contained a liquid crystal compound that was twisted and oriented along a helical axis extending in the thickness direction. Analysis using AxoScan OPMF-2 (Axometrics) confirmed that the twist angle of the helical liquid crystal compound was 225°.
[0180] --------------------------------------------------------------------------- Twist layer forming composition 1------------------------------------------------------------ Methyl ethyl ketone 233 parts by mass Cyclohexanone 12 parts by mass The following rod-shaped liquid crystal compound 201 83 parts by mass The following rod-shaped liquid crystal compound 202 15 parts by mass The following rod-shaped liquid crystal compound 203 2 parts by mass Polyfunctional monomer A-TMMT (manufactured by Shin Nakamura Chemical Industry Co., Ltd.) 1 part by mass IRGACURE 819 (manufactured by BASF) 4 parts by mass The following surfactant F-4 0.05 parts by mass The following surfactant F-5 0.01 parts by mass The following chiral agent 1 0.277 parts by mass------------------------------------------------------------
[0181] Rod-shaped liquid crystal compound 201
[0182]
[0183] Rod-shaped liquid crystal compound 202 [In the following formula, Me represents a methyl group.]
[0184]
[0185] Rod-shaped liquid crystal compound 203 [In the following formula, Me represents a methyl group.]
[0186]
[0187] Surfactant F-4
[0188]
[0189] Surfactant F-5
[0190]
[0191] Chiral agent 1
[0192]
[0193] [Fabrication of Optical Laminate A1] The C plate 1 was bonded to the exposed surface of the light-absorbing anisotropic layer 2 fabricated above using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the release support was peeled off. Next, the exposed surface of the separately prepared light-absorbing anisotropic layer 2 fabricated above was bonded to the bonded C plate 1 using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)). At this time, the two bonded light-absorbing anisotropic layers 2 were bonded so that their absorption axes were parallel. Next, the separately prepared C plate 1 was bonded to the protective film of the bonded light-absorbing anisotropic layer 2 using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the release support was peeled off. Next, the surface of the twisted layer 1 prepared above was bonded to the bonded C plate 1 via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the release support was peeled off. At this time, the twisted layer 1 was bonded so that the in-plane slow axis on the C plate 1 side surface of the twisted layer 1 and the absorption axis of the light absorption anisotropy layer 2 were parallel. Finally, the protective layer B1 of the optical film containing the light absorption anisotropy layer 1 prepared above was bonded to the bonded twisted layer 1 via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) to prepare the optical laminate A1. The layer structure of the fabricated optical laminate A1 consisted of "optical absorption anisotropy layer 1 / twisted layer 1 / C plate 1 / optical absorption anisotropy layer 2 / C plate 1 / optical absorption anisotropy layer 2" in this order. When the optical laminate A1 was observed from the optical absorption anisotropy layer 1 side, the in-plane slow axis of twisted layer 1 on the optical absorption anisotropy layer 2 side of the surface was rotated clockwise by the aforementioned twist angle, relative to the in-plane slow axis of twisted layer 1 on the optical absorption anisotropy layer 1 side.
[0194] <Example 2> [Preparation of λ / 4 layer] (Synthesis of monomer mA-1) 50.0 g of 4-aminocyclohexanol, 48.3 g of triethylamine, and 800 g of N,N-dimethylacetamide were weighed into a 2 L three-necked flask equipped with a stirring blade, thermometer, dropping funnel, and reflux duct, and the mixture was stirred under ice cooling. Next, 47.5 g of methacrylate chloride was added dropwise to the flask over 40 minutes using a dropping funnel, and after the addition was complete, the reaction mixture was stirred at 40°C for 2 hours. After the reaction mixture was cooled to room temperature (23°C), the reaction mixture was filtered by suction to remove the precipitated salt. The obtained organic phase was transferred to a 2 L three-necked flask equipped with a stirring blade, thermometer, dropping funnel, and reflux duct, and stirred under water cooling. Next, N,N-dimethylaminopyridine (10.6 g) and triethylamine (65.9 g) were added to the flask. Using a dropping funnel, 4-n-octyloxycinnamic acid chloride (127.9 g), which had been previously dissolved in tetrahydrofuran (125 g), was added dropwise to the flask over 30 minutes. After the addition was complete, the reaction mixture was stirred at 50°C for 6 hours. After the reaction mixture was cooled to room temperature, it was separated and washed with water. The resulting organic layer was dried over anhydrous magnesium sulfate, and the resulting solution was concentrated to obtain a yellowish-white solid. The obtained yellowish-white solid was heated and dissolved in methyl ethyl ketone (400 g), and recrystallization was performed to obtain 76 g of monomer mA-1 as a white solid (yield 40%).
[0195]
[0196] (Other monomers) Cyclomer M-100 (manufactured by Daicel Corporation) was used as the monomer mB-1 that forms the repeating unit B-1.
[0197]
[0198] (Synthesis of Polymer R-1) In a flask equipped with a condenser, thermometer, and stirrer, 2-butanone (5 parts by mass) was charged as a solvent, and the mixture was refluxed by heating in a water bath while 5 mL / min of nitrogen was flowed into the flask. A solution of monomer mA-1 (1.2 parts by mass), monomer mB-1 (8.8 parts by mass), 2,2'-azobis(isobutyronitrile) (1 part by mass) as a polymerization initiator, and 2-butanone (5 parts by mass) as a solvent was added dropwise over 3 hours, and the resulting reaction mixture was stirred while maintaining reflux for another 3 hours. After the reaction was complete, the reaction mixture was allowed to cool to room temperature, and 2-butanone (30 parts by mass) was added to dilute the reaction mixture to obtain a polymer solution with a polymer concentration of approximately 20% by mass. The obtained polymer solution was added to a large excess of methanol to precipitate the polymer, the precipitate was filtered off, and the resulting solid was washed with a large amount of methanol. The mixture was then air-dried at 50°C for 12 hours to obtain polymer R-1 having photo-orienting groups.
[0199] (Preparation of the composition for photo-alignment film formation) The photo-alignment film formation composition 1 was prepared as follows: -------------------
[0200] Thermal acid generator D-1
[0201]
[0202] (Formation of λ / 4 plate) The above-mentioned photo-alignment film-forming composition 1 was applied to one side of a 40 μm thick cellulose acylate film (TAC substrate; manufactured by Fujifilm Corporation, TG40) using a bar coater. Then, the film coated with the photo-alignment film-forming composition 1 was dried on a hot plate at 125°C for 2 minutes to remove the solvent and form a precursor film with a thickness of 0.3 μm. The obtained precursor film was then irradiated with polarized ultraviolet light (8 mJ / cm²). 2 A photo-alignment film 1 was formed by heating (using an ultra-high pressure mercury lamp). Next, the following phase difference layer forming composition 1 was applied onto the photo-alignment film 1 using a bar coater. The coating formed on the photo-alignment film 1 was heated to 120°C with hot air, then cooled to 60°C, and then heated at a wavelength of 365 nm and a pressure of 100 mJ / cm² using a high-pressure mercury lamp under a nitrogen atmosphere. 2 The coating is irradiated with ultraviolet light, followed by heating to 120°C while applying 500 mJ / cm² of UV light. 2 The coating film was irradiated with ultraviolet light. Following the above procedure, the orientation of the liquid crystal compound was fixed, and a λ / 4 layer was fabricated. The resulting laminate (cellulose acylate film / photo-alignment film 1 / λ / 4 layer) had a Re(550) of 140 nm and was a λ / 4 plate.
[0203] ------------------------------------------------------------------- Phase difference layer forming composition 1 -------------------
[0204] Polymerizable liquid crystal compound L-4
[0205]
[0206] Polymerizable liquid crystal compound L-5
[0207]
[0208] Polymerizable liquid crystal compound L-6
[0209]
[0210] Polymerizable liquid crystal compound A-1
[0211]
[0212] Polymerization initiator S-2
[0213]
[0214] Surfactant F-1
[0215]
[0216] [Fabrication of Optical Laminate A2] The λ / 4 layer in the λ / 4 plate was bonded to the exposed surface of the light-absorbing anisotropic layer 2 fabricated above using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)), and the support (cellulose acylate film) of the λ / 4 plate was peeled off. At this time, the bonding was performed so that the angle between the absorption axis of the light-absorbing anisotropic layer 2 and the in-plane slow phase axis of the λ / 4 layer was 45°. Next, the C plate was bonded to the surface of the bonded λ / 4 layer using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)), and the release support was peeled off. Next, the exposed surface of the λ / 4 layer of the separately prepared λ / 4 plate was bonded to the bonded C plate 1 via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the support (cellulose acylate film) of the λ / 4 plate was peeled off. At this time, the two bonded λ / 4 layers were bonded so that their slow phase axes were orthogonal. Next, the exposed surface of the separately prepared light-absorbing anisotropic layer 2 was bonded to the surface of the bonded λ / 4 layer via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)). At this time, the two bonded light-absorbing anisotropic layers 2 were bonded so that their absorption axes were parallel. The angle between the in-plane slow phase axis of the λ / 4 layer and the absorption axis of the bonded light-absorbing anisotropic layer 2 was 45°. Next, the exposed surface of the λ / 4 layer of the separately prepared λ / 4 plate was bonded to the protective film of the bonded light-absorbing anisotropic layer 2 using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the support (cellulose acylate film) of the λ / 4 plate was peeled off. At this time, the bonded λ / 4 layer was bonded so that the angle between the in-plane slow axis and the absorption axis of the light-absorbing anisotropic layer 2 was 45°. Next, the separately prepared C plate 1 was bonded to the surface of the bonded λ / 4 layer using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the peelable support was peeled off.Next, the surface of the twisted layer 1 prepared above was bonded to the bonded C plate 1 via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the release support was peeled off. At this time, the bond was made such that the angle between the in-plane slow axis on the C plate 1 side surface of the twisted layer 1 and the absorption axis of the optical absorption anisotropy layer 2 was 45°. Finally, the exposed surface of the optical absorption anisotropy layer 1 prepared above was bonded to the bonded twisted layer 1 via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) to prepare the optical laminate A2. The layer structure of the fabricated optical laminate A2 consisted of the following layers in this order: "Optical absorption anisotropy layer 1 / Twist layer 1 / C plate 1 / λ / 4 layer / Optical absorption anisotropy layer 2 / λ / 4 layer / C plate 1 / λ / 4 layer / Optical absorption anisotropy layer 2". When the optical laminate A2 was observed from the optical absorption anisotropy layer 1 side, the in-plane slow axis of twist layer 1 on the optical absorption anisotropy layer 2 side was located at a position rotated clockwise by the aforementioned twist angle, relative to the in-plane slow axis of twist layer 1 on the optical absorption anisotropy layer 1 side.
[0217] <Example 3> [Preparation of C plate 2] An optical film 2A was prepared in the same manner as in Example 5 of Japanese Patent Application Publication No. 2016-105127, except that the thickness of the phase difference layer was changed, and a phase difference layer 2A formed using a rod-shaped liquid crystal compound was arranged on a peelable support consisting of a substrate and an alignment film. The Re(550) of the phase difference layer 2A in the optical film 2A was 0 nm and the Rth(550) was -300 nm. The average inclination angle of the long axis of the rod-shaped liquid crystal compound in the phase difference layer 2A with respect to the film surface was 0° in all cases, confirming that the rod-shaped liquid crystal compound was oriented perpendicular to the film surface.
[0218] Two optical films 2A prepared as described above were prepared and bonded together using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) so that their phase difference layers 2A faced each other. By peeling off one of the release supports, an optical film 2B was prepared in which a phase difference layer 2B was placed on the release support. The Re(550) of the phase difference layer 2B in optical film 2B was 0 nm and the Rth(550) was -600 nm.
[0219] Next, the optical film 2B prepared above and the optical film 2A prepared separately were bonded together using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) so that their respective phase difference layers faced each other, and the release support of the optical film 2A was peeled off to prepare the C plate 2 on the release support. The Re(550) of the C plate 2 was 0 nm and the Rth(550) was -900 nm.
[0220] [Preparation of C-plate 3] Two optical films 2B prepared as described above were prepared and bonded together using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) so that their phase difference layers faced each other. C-plate 3 was then prepared on the release support by peeling off one of the release supports. The Re(550) of C-plate 3 was 0 nm and the Rth(550) was -1200 nm.
[0221] [Fabrication of Light-Absorbing Anisotropic Layer 3 (Vertical Orientation)] Except for changing the light-absorbing anisotropic layer forming composition P2 described below to the light-absorbing anisotropic layer forming composition P2 in the fabrication of light-absorbing anisotropic layer 1 (vertical orientation), the light-absorbing anisotropic layer 3 (vertical orientation) was fabricated following the same procedure as for light-absorbing anisotropic layer 1 (vertical orientation).
[0222] --------------------------------------------------------------------------- Composition P2 for forming anisotropic light-absorbing layer --------------------------------------------------------------------------- • Dichroic substance D-1 0.76 parts by mass • Dichroic substance D-2 0.04 parts by mass • Dichroic substance D-3 1.13 parts by mass • Polymer liquid crystal compound P-1 4.10 parts by mass • Liquid crystal compound L-1 2.54 parts by mass • IRGACURE OXE-2 (manufactured by BASF) 0.13 parts by mass • Orienting agent E-1 0.05 parts by mass • Surfactant S-2 0.008 parts by mass • Cyclopentanone 82.11 parts by mass • Benzyl alcohol 9.12 parts by mass ---------------------------------------------------------------------------
[0223] [Fabrication of Optical Laminate A3] The C plate 3 was bonded to the exposed surface of the light-absorbing anisotropic layer 2 fabricated above via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the release support was peeled off. Next, the surface of the twisted layer 1 fabricated above was bonded to the bonded C plate 3 via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the release support was peeled off. At this time, the bonding was performed so that the angle between the in-plane slow axis on the C plate 3 side surface of the twisted layer 1 and the absorption axis of the light-absorbing anisotropic layer 2 was 45°. Next, the protective layer B1 of the optical film containing the light-absorbing anisotropic layer 3 prepared above was bonded to the bonded twisted layer 1 via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)). Then, the surface of the separately prepared twisted layer 1 was bonded to the cellulose acylate film of the optical film containing the bonded light-absorbing anisotropic layer 3 via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the release support was peeled off. At this time, the bonding was performed so that the angle between the in-plane slow axis on the surface of the twisted layer 1 on the light-absorbing anisotropic layer 3 side and the absorption axis of the light-absorbing anisotropic layer 2 was parallel. Next, the C-plate 2 prepared above was bonded to the bonded twisted layer 1 via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the release support was peeled off. Finally, the exposed surface of the separately prepared light-absorbing anisotropic layer 2 was bonded to the bonded C-plate 2 via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) to create an optical laminate A3. At this time, the two bonded light-absorbing anisotropic layers 2 were bonded so that their absorption axes were orthogonal. The layer structure of the fabricated optical laminate A3 was as follows: "light-absorbing anisotropic layer 2 / C-plate 2 / twisted layer 1 / light-absorbing anisotropic layer 3 / twisted layer 1 / C-plate 3 / light-absorbing anisotropic layer 2".
[0224] <Example 4> [Preparation of C plate 4] Optical film 1B and optical film 2B prepared above were prepared and bonded together using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) so that their phase difference layers faced each other. C plate 4 was prepared on the release support by peeling off one of the release supports. The Re(550) of C plate 4 was 0 nm and the Rth(550) was -1100 nm.
[0225] [Preparation of C plate 5] An optical film 3A was prepared in the same manner as in Example 5 of Japanese Patent Application Publication No. 2016-105127, except that the thickness of the phase difference layer was changed, and a phase difference layer 3A formed using a rod-shaped liquid crystal compound was arranged on a peelable support consisting of a substrate and an alignment film. The Re(550) of the phase difference layer 3A in the optical film 3A was 0 nm and the Rth(550) was -350 nm. The average inclination angle of the long axis of the rod-shaped liquid crystal compound in the phase difference layer 3A with respect to the film surface was 0° in all cases, confirming that the rod-shaped liquid crystal compound was oriented perpendicular to the film surface.
[0226] Optical films 2A and 3A prepared as described above were prepared and bonded together using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) so that their phase difference layers faced each other. By peeling off one of the release supports, an optical film 3B was prepared in which a phase difference layer 3B was placed on the release support. The Re(550) of the phase difference layer 3B in optical film 3B was 0 nm and the Rth(550) was -650 nm.
[0227] The C plate 3 and optical film 3B prepared as described above were bonded together using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) so that the C plate 3 and the phase difference layer 3B faced each other. The C plate 5 was then fabricated on the release support by peeling off the release support of the optical film 3B. The Re(550) of the C plate 5 was 0 nm and the Rth(550) was -1850 nm.
[0228] [Preparation of Twist Layer 2] In the preparation of twist layer 1, twist layer 2 was prepared by following the same procedure as for twist layer 1, except that twist layer forming composition 1 was changed to twist layer forming composition 2 described below, and the thickness of the coating film was adjusted to 2.5 μm. Analysis using AxoScan OPMF-2 (manufactured by Axometrics) confirmed that in the obtained twist layer 2, the Δnd between the refractive index anisotropy Δn of twist layer 2 at a wavelength of 550 nm and the thickness d of twist layer 2 was 400 nm. Furthermore, twist layer 2 contained a liquid crystal compound that was twisted and oriented along a helical axis extending in the thickness direction. Analysis using AxoScan OPMF-2 (manufactured by Axometrics) confirmed that the twist angle of the helical liquid crystal compound was 225°.
[0229] --------------------------------------------------------------------------- Twist layer forming composition 2------------------------------------------------------------ Methyl ethyl ketone 233 parts by mass Cyclohexanone 12 parts by mass The above rod-shaped liquid crystal compound 201 83 parts by mass The above rod-shaped liquid crystal compound 202 15 parts by mass The above rod-shaped liquid crystal compound 203 2 parts by mass Polyfunctional monomer A-TMMT (manufactured by Shin Nakamura Chemical Industry Co., Ltd.) 1 part by mass IRGACURE 819 (manufactured by BASF) 4 parts by mass The above surfactant F-4 0.05 parts by mass The above surfactant F-5 0.01 parts by mass The above chiral agent 1 0.347 parts by mass------------------------------------------------------------
[0230] [Preparation of λ / 2 layer] (Formation of alignment film 2) The following alignment film forming composition 2 was continuously applied to one side of a 40 μm thick cellulose acylate film (TAC substrate; manufactured by Fujifilm Corporation, TG40) using a #14 wire bar. After application, the obtained cellulose acylate film was dried with 60°C hot air for 60 seconds, and then with 100°C hot air for 120 seconds to form a coating film.
[0231] ------------------------------------------------------------------ Composition 2 for forming an orientation film ------------------------------------------------------------------ 10 parts by mass of the above modified polyvinyl alcohol PVA-1 308 parts by mass of water 70 parts by mass of methanol 29 parts by mass of isopropanol 0.8 parts by mass of photopolymerization initiator (Irgacure 2959, manufactured by BASF) ------------------------------------------------------------------
[0232] The above coating was subjected to a continuous rubbing process. At this time, the longitudinal direction of the long film and the transport direction were parallel, and the angle between the longitudinal direction of the film and the rotation axis of the rubbing roller was set to 90°. That is, with the film width direction as 0° and the film longitudinal direction as 90°, and observing from the orientation film side and representing the clockwise direction as a positive value with respect to the film width direction, the rotation axis of the rubbing roller was 0°. Orientation film 2 was formed using the above procedure.
[0233] (Formation of λ / 2 layer) A phase difference layer forming composition 2 containing a discotic liquid crystal compound of the composition described below was continuously coated onto the alignment film 2 prepared above using a #5.0 wire bar to create a λ / 2 layer. The film transport speed (V) was set to 26 m / min. To dry the solvent of the phase difference layer forming composition 2 and to mature the orientation of the discotic liquid crystal compound, it was heated with hot air at 130°C for 90 seconds, followed by hot air at 100°C for 60 seconds, and then UV irradiation at 80°C to fix the orientation of the liquid crystal compound. A λ / 2 layer was formed on the alignment film 2 using the above procedure to obtain a λ / 2 plate. The in-plane retardation of the λ / 2 layer at a wavelength of 550 nm was 270 nm. The average inclination angle of the disc surface of the discotic liquid crystal compound with respect to the film surface was 90°, confirming that the discotic liquid crystal compound was oriented perpendicular to the film surface.
[0234] --------------------------------------------------------------------------- Composition of Phase Difference Layer Forming Composition 2 --------------------------------------------------------------------------- • Discotic liquid crystal-1 80 parts by mass • Discotic liquid crystal-2 20 parts by mass • Alignment film interface orientation agent-1 0.55 parts by mass • Alignment film interface orientation agent-2 0.05 parts by mass • Surfactant F-2 0.09 parts by mass • Modified trimethylolpropane triacrylate 10 parts by mass • Photopolymerization initiator (Irgacure 907, manufactured by BASF) 3.0 parts by mass • Methyl ethyl ketone 200 parts by mass ---------------------------------------------------------------------------
[0235] Discotic LCD-1
[0236]
[0237] Discotic LCD-2
[0238]
[0239] Orientation film interface orientation agent - 1
[0240]
[0241] Orientation film interface orientation agent - 2
[0242]
[0243] Surfactant F-2
[0244]
[0245] [Fabrication of Optical Laminate A4] The λ / 2 layer in the λ / 2 plate was bonded to the exposed surface of the light-absorbing anisotropic layer 2 fabricated above using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)). At this time, the bonding was performed so that the angle between the absorption axis of the light-absorbing anisotropic layer 2 and the in-plane slow-phase axis of the λ / 4 layer was 22.5°. Next, the C plate 5 was bonded to the bonded λ / 2 layer using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the release support was peeled off. Next, the surface of the twist layer 1 fabricated above was bonded to the bonded C plate 5 using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the release support was peeled off. At this time, the twisted layer 1 was bonded so that the angle between the in-plane slow axis on the surface of the twisted layer 1 on the C plate 5 side and the absorption axis of the light absorption anisotropy layer 2 was 45°. Next, the protective layer B1 of the optical film containing the light absorption anisotropy layer 3 prepared above was bonded to the bonded twisted layer 1 via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)). Next, the surface of the twisted layer 2 prepared above was bonded to the cellulose acylate film of the optical film containing the bonded light absorption anisotropy layer 3 via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the release support was peeled off. At this time, the twisted layer 2 was bonded so that the angle between the in-plane slow axis on the surface of the twisted layer 2 on the light absorption anisotropy layer 3 side and the absorption axis of the light absorption anisotropy layer 2 was parallel. Next, the prepared C plate 4 was bonded to the bonded twisted layer 2 via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the release support was peeled off. Next, the exposed λ / 4 layer side of the separately prepared λ / 4 plate was bonded to the bonded C plate 4 via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the support (cellulose acylate film) of the λ / 4 plate was peeled off.At this time, the bonded λ / 4 layer was bonded so that the angle between the in-plane slow axis and the absorption axis of the optical absorption anisotropy layer 2 was 45°. Finally, the exposed surface of the optical absorption anisotropy layer 2 prepared above was bonded to the bonded λ / 4 layer via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) to create optical laminate A4. The layer configuration of the prepared optical laminate A4 was as follows: "optical absorption anisotropy layer 2 / λ / 4 layer / C plate 4 / twisted layer 2 / optical absorption anisotropy layer 3 / twisted layer 1 / C plate 5 / λ / 2 layer / optical absorption anisotropy layer 2".
[0246] <Example 5> [Preparation of Optical Laminate A5] The surface of the twisted layer 1 prepared above was bonded to the protective layer B1 of the optical film containing the light-absorbing anisotropic layer 3 prepared above via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the release support was peeled off. Next, the C plate 5 prepared above was bonded to the bonded twisted layer 1 via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the release support was peeled off. Next, the exposed surface of the light-absorbing anisotropic layer 2 prepared above was bonded to the bonded C plate 5 via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)). At this time, the twisted layer 1 was bonded to the C-plate 5 side surface so that the in-plane slow axis and the absorption axis of the light absorption anisotropy layer 2 were parallel. Next, the prepared C-plate 4 was bonded to the protective film of the bonded light absorption anisotropy layer 2 via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the release support was peeled off. Next, the surface of the prepared twisted layer 2 was bonded to the bonded C-plate 4 via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the release support was peeled off. At this time, the twisted layer 2 was bonded so that the angle between the in-plane slow axis and the absorption axis of the light absorption anisotropy layer 2 was parallel. Finally, a protective layer B1 of an optical film containing the light-absorbing anisotropic layer 3 prepared separately was bonded to the bonded twisted layer 2 via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) to create an optical laminate A5. The layer structure of the fabricated optical laminate A5 consisted of "light-absorbing anisotropic layer 3 / twisted layer 2 / C plate 4 / light-absorbing anisotropic layer 2 / C plate 5 / twisted layer 1 / light-absorbing anisotropic layer 3" in this order.
[0247] <Example 6> [Preparation of Optical Laminate A6] The surface of the twisted layer 1 prepared above was bonded to the protective layer B1 of the optical film containing the light-absorbing anisotropic layer 3 prepared above via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the release support was peeled off. Next, the C plate 5 prepared above was bonded to the bonded twisted layer 1 via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the release support was peeled off. Next, the surface of the λ / 2 layer of the λ / 2 plate prepared above was bonded to the bonded C plate 5 via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)). At this time, the twisted layer 1 was bonded to the C-plate 5 side surface such that the angle between the in-plane slow axis and the in-plane slow axis of the λ / 2 layer was 22.5°. Next, the exposed surface of the light-absorbing anisotropic layer 2 prepared above was bonded to the bonded λ / 2 layer via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)). At this time, the bonded layers were made such that the angle between the in-plane slow axis of the λ / 2 layer and the absorption axis of the light-absorbing anisotropic layer 2 was 22.5°. Next, the exposed surface of the λ / 4 layer of the prepared λ / 4 plate was bonded to the protective film of the bonded light-absorbing anisotropic layer 2 via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)). At this time, the λ / 4 layer was bonded so that the angle between the in-plane slow axis and the absorption axis of the optical absorption anisotropy layer 2 was 45°. Next, the C plate 4 prepared above was bonded to the bonded λ / 4 layer via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the release support was peeled off. Next, the surface of the twisted layer 2 prepared above was bonded to the bonded C plate 4 via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the release support was peeled off. At this time, the twisted layer 2 was bonded so that the angle between the in-plane slow axis on the C plate 4 side surface of the twisted layer 2 and the absorption axis of the optical absorption anisotropy layer 2 was 45°.Finally, a protective layer B1 of an optical film containing the light-absorbing anisotropic layer 3 prepared separately was bonded to the bonded twisted layer 2 via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) to create an optical laminate A6. The layer structure of the fabricated optical laminate A6 consisted of "light-absorbing anisotropic layer 3 / twisted layer 2 / C plate 4 / λ / 4 / light-absorbing anisotropic layer 2 / λ / 2 / C plate 5 / twisted layer 1 / light-absorbing anisotropic layer 3" in this order.
[0248] <Comparative Example 1> [Preparation of C-plate 6] The phase difference layer 3B in the optical film 3B prepared in Example 5 was used as C-plate 6.
[0249] [Preparation of C plate 7] Two optical films 3A prepared in Example 5 were prepared and bonded together using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) so that their phase difference layers faced each other. By peeling off one of the release supports, an optical film 4B was prepared in which the phase difference layer 4B was placed on the release support. The Re(550) of the phase difference layer 4B in the optical film 4B was 0 nm and the Rth(550) was -700 nm.
[0250] Next, two of the optical films 4B prepared as described above were prepared and bonded together using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) so that their phase difference layers 4B faced each other. A C plate 7 was then fabricated on the release support by peeling off one of the release supports. The Re(550) of the C plate 7 was 0 nm and the Rth(550) was -1400 nm.
[0251] [Fabrication of Optical Laminate B1] The λ / 4 layer in the λ / 4 plate was bonded to the protective film of the light-absorbing anisotropic layer 2 fabricated above via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)), and the support (cellulose acylate film) of the λ / 4 plate was peeled off. At this time, the bonding was performed so that the angle between the absorption axis of the light-absorbing anisotropic layer 2 and the in-plane slow-phase axis of the λ / 4 layer was 45°. Next, the C plate 7 was bonded to the surface of the bonded λ / 4 layer via a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)), and the peelable support was peeled off. Next, the exposed surface of the λ / 4 layer of the separately prepared λ / 4 plate was bonded to the bonded C plate 7 using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the support (cellulose acylate film) of the λ / 4 plate was peeled off. At this time, the two bonded λ / 4 layers were bonded so that their slow phase axes were orthogonal. Next, a protective film of the separately prepared light-absorbing anisotropic layer 2 was bonded to the surface of the bonded λ / 4 layer using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)). At this time, the two bonded light-absorbing anisotropic layers 2 were bonded so that their absorption axes were parallel. The angle between the in-plane slow phase axis of the λ / 4 layer and the absorption axis of the bonded light-absorbing anisotropic layer 2 was 45°. Next, the exposed surface of the λ / 4 layer of the separately prepared λ / 4 plate was bonded to the protective film of the bonded light-absorbing anisotropic layer 2 using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the support (cellulose acylate film) of the λ / 4 plate was peeled off. At this time, the bonded λ / 4 layer was bonded so that the angle between the in-plane slow phase axis and the absorption axis of the light-absorbing anisotropic layer 2 was 45°. Next, the C plate 6 was bonded to the surface of the bonded λ / 4 layer using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) and the peelable support was peeled off.Next, the exposed surface of the λ / 4 layer of the separately prepared λ / 4 plate was bonded to the bonded C plate 6 using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) to remove the support (cellulose acylate film) of the λ / 4 plate. At this time, the two layers of λ / 4 layers bonded to both sides of the C plate 6 were bonded so that their slow phase axes were orthogonal. Finally, the exposed surface of the light-absorbing anisotropic layer 2 prepared above was bonded to the surface of the bonded λ / 4 layer using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)) to create the optical laminate B1. At this time, the three bonded layers of light-absorbing anisotropic layer 2 were bonded so that their absorption axes were parallel. Furthermore, the angle between the in-plane slow-phase axis of the λ / 4 layer and the absorption axis of the bonded optical absorption anisotropy layer 2 was 45°. The layer configuration of the fabricated optical laminate B1 was as follows: "optical absorption anisotropy layer 2 / λ / 4 layer / C plate 6 / λ / 4 layer / optical absorption anisotropy layer 2 / λ / 4 layer / C plate 7 / λ / 4 layer / optical absorption anisotropy layer 2".
[0252] <Comparative Example 2> [Preparation of Optical Laminate B2] An optical laminate B2 was prepared by bonding the exposed surface of the light-absorbing anisotropic layer 2 prepared above to the protective layer B1 of the optical film containing the light-absorbing anisotropic layer 3 prepared above, using a commercially available adhesive (Opteria® NCF-D692 (film thickness: 15 μm, manufactured by Lintec Corporation)). The layer structure of the prepared optical laminate B2 consisted of "light-absorbing anisotropic layer 2 / light-absorbing anisotropic layer 3" in that order.
[0253] [Evaluation of Optical Laminate] The optical laminates of Examples 1 to 6 and Comparative Examples 1 to 2 were evaluated by the following procedure. The transmittance was measured by varying the tilt angle (polar angle) relative to the normal direction of the optical laminate surface and the tilt direction (azimuth angle). Specifically, the transmittance was determined by actually measuring the Mueller matrix at a wavelength of 550 nm using AxoScan OPMF-2 (manufactured by Axometrics). More specifically, the transmittance in the polar angle range of 50° to 70° from the normal direction was measured in all directions at 10° intervals within the plane of the optical laminate, the average value of the transmittance in the polar angle range of 50° to 70° in each azimuth was calculated, and the azimuth with the lowest average transmittance value among them was defined as "Azimuth X". Next, transmittance was measured at 5° intervals between polar angles of 0° and 70° in Azimuth X. In addition, the transmittance in the polar angle range of 50° to 70° was also measured in an azimuth where the azimuth angle was changed by 30° relative to Azimuth X. The transmittance in this evaluation is a value normalized by the maximum value among the transmittance values measured at 5° intervals between polar angles of 0° and 70°.
[0254] The evaluation criteria are shown below. A + : The transmittance in the polar angle 30° direction in Azimuth X is 75% or more, the transmittance in the polar angle range of 50° to 70° is 10% or less, and the maximum transmittance in the polar angle range of 50° to 70° in the azimuth where the azimuth angle is changed by 30° from Azimuth X is 10% or less. A: The transmittance in the polar angle 30° direction in Azimuth X is 75% or more, the transmittance in the polar angle range of 50° to 70° is 10% or less, and the maximum transmittance in the polar angle range of 50° to 70° in the azimuth where the azimuth angle is changed by 30° from Azimuth X is more than 10%. B + : The transmittance in the polar angle 30° direction in Azimuth X is 50% or more and less than 75%, the transmittance in the polar angle range of 50° to 70° is 10% or less, and the maximum transmittance in the polar angle range of 50° to 70° in the azimuth where the azimuth angle is changed by 30° from Azimuth X is 10% or less. B: The transmittance in the polar angle 30° direction in Azimuth X is 50% or more and less than 75%, the transmittance in the polar angle range of 50° to 70° is 10% or less, and the maximum transmittance in the polar angle range of 50° to 70° in the azimuth where the azimuth angle is changed by 30° from Azimuth X is more than 10%. C +C: The transmittance in the polar angle 30° direction at direction X is 30% or more but less than 50%, the transmittance in the polar angle 50-70° direction is 10% or less, and the maximum transmittance in the polar angle 50-70° direction at the direction obtained by changing the azimuth angle by 30° from direction X is 10% or less. D: The transmittance in the polar angle 30° direction at direction X is 30% or more but less than 50%, the transmittance in the polar angle 50-70° direction is 10% or less, and the maximum transmittance in the polar angle 50-70° direction at the direction obtained by changing the azimuth angle by 30° from direction X is greater than 10%. + D: The transmittance in the polar angle 30° direction at direction X is less than 30%, the transmittance in the polar angle 50-70° direction is 10% or less, and the maximum transmittance in the polar angle 50°-70° direction in the direction obtained by changing the azimuth angle by 30° from direction X is 10% or less. E: The transmittance in the polar angle 30° direction at direction X is less than 30%, the transmittance in the polar angle 50-70° direction is 10% or less, and the maximum transmittance in the polar angle 50°-70° direction in the direction obtained by changing the azimuth angle by 30° from direction X is greater than 10%.
[0255] In Tables 1 and 2, the "Y / X / Y or X / Y / X" column indicates whether the first, second, and third optical anisotropic layers included in the optical laminate are "optical anisotropic layer Y / optical anisotropic layer X / optical anisotropic layer Y" or "optical anisotropic layer X / optical anisotropic layer Y / optical anisotropic layer X". "A" indicates "optical anisotropic layer Y / optical anisotropic layer X / optical anisotropic layer Y" or "optical anisotropic layer X / optical anisotropic layer Y / optical anisotropic layer X", and "B" indicates otherwise. In Tables 1 and 2, the "Orientation X, polar angle 30°" column indicates the transmittance in the polar angle 30° direction at orientation X. In Tables 1 and 2, the column "Orientation X, Polar Angle 50-70°" represents the maximum transmittance in the polar angle direction of 50-70° at orientation X. In Tables 1 and 2, the column "Orientation X + 30°, Polar Angle 50-70°" represents the maximum transmittance in the polar angle direction of 50-70° at an orientation obtained by changing the azimuth angle by 30° from orientation X. In Tables 1 and 2, "(Vertical Orientation)" in the description of the light-absorbing anisotropic layer means that it is light-absorbing anisotropic layer X, and "(Horizontal Orientation)" in the description of the light-absorbing anisotropic layer means that it is light-absorbing anisotropic layer Y. The angles of the absorption axis and in-plane slow axis shown in Tables 1 and 2 are the angles when the optical laminate described in the examples and comparative examples in Tables 1 and 2 is observed from the light-absorbing anisotropic layer side on the upper side of the paper, with orientation X as 0° and counterclockwise rotation represented as a positive value. For example, in Example 1, this corresponds to the case where the optical laminate is observed from the side of the light-absorbing anisotropic layer 1.
[0256]
[0257]
[0258] As shown in Tables 1 and 2, the optical laminate of the present invention was confirmed to exhibit the desired effects. In particular, a comparison of Examples 1 and 2 confirmed that the effect is superior when any one of requirements B1 to B3 is met. Furthermore, a comparison of Examples 1, 3, and 5 confirmed that the effect is superior when the first and third optical absorption anisotropy layers are optical absorption anisotropy layers X and the second optical absorption anisotropy layer is optical absorption anisotropy layer Y, or when the first and third optical absorption anisotropy layers are optical absorption anisotropy layers Y and the second optical absorption anisotropy layer is optical absorption anisotropy layer X.
[0259] 100A, 102A, 100B, 102B, 100C, 102C, 100D, 102D, 100E, 100F Optical laminate 10A, 10B, 10C, 10D, 10E, 10F First light absorption anisotropy layer 12A, 12B, 12C, 12D, 12E, 12F Second light absorption anisotropy layer 14A, 14B, 14C, 14D, 14E, 14F Third light absorption anisotropy layer 16F Fourth light absorption anisotropy layer 20A, 20B, 20C, 20D, 20E, 20F First C plate 22A, 22B, 22C, 22D, 22E, 22F First C plate 24F Third C plate 32, 34, 36, 38, 40, 42, 44, 46, 50, 52, 54, 56, 60, 62, 64, 70, 72, 74, 76, 80 Specific layer
Claims
1. An optical laminate comprising, in this order: a first light-absorbing anisotropic layer, a first C plate, a second light-absorbing anisotropic layer, a second C plate, and a third light-absorbing anisotropic layer, wherein the first light-absorbing anisotropic layer, the second light-absorbing anisotropic layer, and the third light-absorbing anisotropic layer are each independently a light-absorbing anisotropic layer X or a light-absorbing anisotropic layer Y, the light-absorbing anisotropic layer X has a transmittance center axis whose angle with the normal direction of the surface of the light-absorbing anisotropic layer X is 0 to 45 degrees, the light-absorbing anisotropic layer Y has an absorption axis in the in-plane direction, and at least one of the first light-absorbing anisotropic layer, the second light-absorbing anisotropic layer, and the third light-absorbing anisotropic layer is the light-absorbing anisotropic layer X, and satisfying at least one of the following requirements A1 to A3. Requirement A1: The first light-absorbing anisotropic layer is the light-absorbing anisotropic layer X, and a liquid crystal layer, λ / 4 layer, or λ / 2 layer containing a liquid crystal compound twisted with the thickness direction as the helical axis is disposed between the first light-absorbing anisotropic layer and the first C plate. Requirement A2: The second light-absorbing anisotropic layer is the light-absorbing anisotropic layer X, and a liquid crystal layer, λ / 4 layer, or λ / 2 layer containing a liquid crystal compound twisted with the thickness direction as the helical axis is disposed between the second light-absorbing anisotropic layer and the first C plate, and between the second light-absorbing anisotropic layer and the second C plate. Requirement A3: The third light-absorbing anisotropic layer is the light-absorbing anisotropic layer X, and a liquid crystal layer, λ / 4 layer, or λ / 2 layer containing a liquid crystal compound twisted with the thickness direction as the helical axis is disposed between the third light-absorbing anisotropic layer and the second C plate.
2. The optical laminate according to claim 1, wherein at least one of the first light-absorbing anisotropic layer, the second light-absorbing anisotropic layer, and the third light-absorbing anisotropic layer is the light-absorbing anisotropic layer Y, and satisfies at least one of requirements B1 to B3. Requirement B1: The first light-absorbing anisotropic layer is the light-absorbing anisotropic layer Y, and a liquid crystal layer, λ / 4 layer, or λ / 2 layer containing a liquid crystal compound twisted with the thickness direction as the helical axis is disposed between the first light-absorbing anisotropic layer and the first C plate. Requirement B2: The second light-absorbing anisotropic layer is the light-absorbing anisotropic layer Y, and a liquid crystal layer, λ / 4 layer, or λ / 2 layer containing a liquid crystal compound twisted with the thickness direction as the helical axis is disposed between the second light-absorbing anisotropic layer and the first C plate, and between the second light-absorbing anisotropic layer and the second C plate. Requirement B3: The third light-absorbing anisotropic layer is the light-absorbing anisotropic layer Y, and a liquid crystal layer, λ / 4 layer, or λ / 2 layer containing a liquid crystal compound that is twisted in orientation with the thickness direction as the helical axis is disposed between the third light-absorbing anisotropic layer and the second C plate.
3. The optical laminate according to claim 1, wherein the first light-absorbing anisotropic layer and the third light-absorbing anisotropic layer are the light-absorbing anisotropic layer X, and the second light-absorbing anisotropic layer is the light-absorbing anisotropic layer Y, or the first light-absorbing anisotropic layer and the third light-absorbing anisotropic layer are the light-absorbing anisotropic layer Y, and the second light-absorbing anisotropic layer is the light-absorbing anisotropic layer X.
4. The optical laminate according to claim 1, wherein the light-absorbing anisotropic layer X and the light-absorbing anisotropic layer Y contain a dichroic material.
5. A display device comprising an optical laminate according to any one of claims 1 to 4.