SiC POLYCRYSTAL SUBSTRATE AND SiC BONDED SEMICONDUCTOR SUBSTRATE

By optimizing surface roughness, grain size, and grain boundary ratios, and using a modified deposition process, the SiC polycrystalline substrate achieves enhanced bonding quality and reduced defects, improving the yield and electrical uniformity of SiC bonded semiconductor substrates.

WO2026235070A1PCT designated stage Publication Date: 2026-11-12SUMITOMO METAL MINING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/016897
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-09-25
Filing Date
2026-04-28
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

The challenge in manufacturing SiC bonded substrates lies in achieving a bonded surface with excellent surface smoothness between SiC single-crystal and polycrystalline substrates, which is crucial for reducing defects such as voids and improving yield, while also ensuring low volume resistivity and uniform electrical properties.

Method used

The SiC polycrystalline substrate is engineered with specific surface roughness, grain size, and grain boundary ratios, along with controlled deposition processes using a modified chemical vapor deposition chamber to achieve a smooth and uniform surface, thereby enhancing bonding quality and reducing resistivity variations.

Benefits of technology

The solution results in a SiC polycrystalline substrate with improved surface smoothness and uniform electrical properties, minimizing defects and increasing the yield of SiC bonded semiconductor substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026016897_12112026_PF_FP_ABST
    Figure JP2026016897_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides: a SiC polycrystal substrate having bonding surface with excellent surface smoothness; and a SiC bonded semiconductor substrate. Provided is a SiC polycrystal substrate wherein: surface roughness Sa measured at a plurality of measurement points on a main surface is not more than 0.35 nm; the standard deviation of the surface roughness Sa at the plurality of measurement points is 0.006-0.09 nm; the CV value of the surface roughness Sa at the plurality of measurement points is 2.6-30%; and the PV value of the surface roughness Sa at the plurality of measurement points is 0.015-0.25 nm.
Need to check novelty before this filing date? Find Prior Art

Description

SiC polycrystalline substrates and SiC bonded semiconductor substrates

[0001] This invention relates to a SiC polycrystalline substrate and a SiC bonded semiconductor substrate.

[0002] Silicon carbide (SiC) is a compound semiconductor material composed of silicon (Si) and carbon (C). Silicon carbide has a dielectric breakdown field strength 10 times greater than that of silicon and a band gap 3 times greater, making it an excellent semiconductor material. Furthermore, because it allows for a wide range of control over p-type and n-type characteristics necessary for device fabrication, it is expected to surpass the limitations of silicon as a material for power devices.

[0003] However, compared to conventionally widely used Si semiconductors, it is difficult to obtain large-area SiC single-crystal substrates, and the manufacturing process is also complex. For these reasons, SiC semiconductors are difficult to mass-produce and are expensive compared to Si semiconductors.

[0004] Various efforts have been made to reduce the cost of SiC semiconductors. For example, Patent Document 1 describes a method for manufacturing a SiC substrate, wherein the density of micropipes is at least 30 units / cm³. 2 The following steps are described for manufacturing a substrate (hereinafter sometimes referred to as a "SiC bonded substrate") in which a SiC single crystal layer is formed on a SiC polycrystalline substrate by preparing a SiC single crystal substrate and a SiC polycrystalline substrate, bonding the SiC single crystal substrate and the SiC polycrystalline substrate together, and then thinning the SiC single crystal substrate.

[0005] Furthermore, Patent Document 1 describes a method for manufacturing an SiC substrate, in which, before the step of bonding the SiC single crystal substrate and the SiC polycrystalline substrate, a step of implanting hydrogen ions into the SiC single crystal substrate to form a hydrogen ion implanted layer is performed, after the step of bonding the SiC single crystal substrate and the SiC polycrystalline substrate, heat treatment is performed at a temperature of 350°C or less before the step of thinning the SiC single crystal substrate, and the step of thinning the SiC single crystal substrate is a step of mechanically peeling it off at the hydrogen ion implanted layer.

[0006] This method makes it possible to obtain more SiC bonded substrates from a single SiC single crystal ingot.

[0007] Japanese Patent Publication No. 2009-117533

[0008] For SiC bonded substrates, it is crucial that defects such as voids do not occur at the bonding surface between the SiC single-crystal substrate and the SiC polycrystalline substrate, thereby reducing yield. One factor contributing to the occurrence of these defects is the poor surface smoothness of the bonding surface (main surface) of the SiC polycrystalline substrate before bonding with the SiC single-crystal substrate.

[0009] Therefore, the present invention aims to provide a SiC polycrystalline substrate and a SiC bonded semiconductor substrate having a bonded surface with excellent surface smoothness.

[0010] To solve the above problems, the SiC polycrystalline substrate of the present invention has a surface roughness Sa measured at multiple measurement points on the main surface of 0.35 nm or less, a standard deviation of the surface roughness Sa at the multiple measurement points of 0.006 nm or more and 0.09 nm or less, a CV value of the surface roughness Sa at the multiple measurement points of 2.6% or more and 30% or less, and a PV value of the surface roughness Sa at the multiple measurement points of 0.015 nm or more and 0.25 nm or less.

[0011] The standard deviation of the crystal grain size measured at multiple locations on the main surface may be 0.008 μm or more and 10.5 μm or less.

[0012] The standard deviation of the area ratio of polar surfaces scattered in each of the multiple specified area regions of the main surface may be 0.008% or more and 10.5% or less.

[0013] The PV value of the 55° to 65° grain boundary ratio, which is an indicator of the orientation difference between adjacent crystal grains on the main surface, may be 3.5% or more and 8% or less, the PV value of the average grain boundary angle on the main surface may be 1° or more and 1.9° or less, and the PV value of the ratio of the 55° to 65° grain boundary ratio to the 35° to 45° grain boundary ratio on the main surface (55° to 65° grain boundary ratio / 35° to 45° grain boundary ratio) may be 0.15 or more and 0.7 or less.

[0014] The SiC polycrystalline substrate of the present invention may be used in SiC bonded semiconductor substrates.

[0015] The SiC polycrystalline substrate of the present invention may have a volume resistivity of 25 mΩcm or less.

[0016] Furthermore, in order to solve the above problems, the SiC bonded semiconductor substrate of the present invention comprises the SiC polycrystalline substrate of the present invention and a SiC single crystal substrate bonded to the main surface.

[0017] The present invention provides a SiC polycrystalline substrate and a SiC bonded semiconductor substrate having a bonded surface with excellent surface smoothness.

[0018] This is a schematic perspective view of the SiC polycrystalline substrate 100. This is a schematic diagram showing the measurement points for volume resistivity on the SiC polycrystalline substrate 100. This is a schematic side cross-sectional view showing the support substrate, SiC polycrystalline film, and SiC polycrystalline substrate in each step of the manufacturing process of the SiC polycrystalline substrate. This is a cross-sectional view of the deposition chamber 1000. This is a cross-sectional view of the deposition chamber 1000 viewed from the direction indicated by arrow B in Figure 4. This is a cross-sectional view of the deposition chamber 1000 viewed from the direction indicated by arrow D in Figure 4. This is a cross-sectional view of the deposition chamber 2000. This is a cross-sectional view of the deposition chamber 2000 viewed from the direction indicated by arrow B in Figure 7. This is a cross-sectional view of the deposition chamber 2000 viewed from the direction indicated by arrow D in Figure 7.

[0019] Embodiments of the present invention will be described in detail below with reference to the drawings. However, the present invention is not limited to the following embodiments, and various forms within the technical scope of the present invention are possible.

[0020] [SiC Polycrystalline Substrate] A SiC polycrystalline substrate is a substrate used in SiC bonded semiconductor substrates. In SiC bonded semiconductor substrates, a SiC polycrystalline substrate is a substrate that can be reinforced by directly bonding it to a SiC single crystal substrate, thereby using the SiC single crystal substrate as a support substrate.

[0021] <Shape> The shape of the SiC polycrystalline substrate may be substantially the same as that of a SiC single crystal substrate. For example, a roughly disc-shaped substrate with an orientation flat or notch, having a diameter of 100 mm or more and 305 mm or less, can be used. However, the shape is not limited to a disc shape; for example, a polygonal shape may also be used.

[0022] As an example, Figure 1 shows a schematic perspective view of a SiC polycrystalline substrate 100. The SiC polycrystalline substrate 100 is a disc-shaped substrate having a first surface 110 and a second surface 120. For example, either the first surface 110 or the second surface 120 can be used as the bonding surface (main surface), and the main surface can be bonded to a SiC single crystal substrate to manufacture a SiC bonded semiconductor substrate.

[0023] The SiC polycrystalline substrate 100 is formed in the shape of a disc, for example, with a thickness of about 200 μm to 1000 μm, and the thickness error can be set to ±2.5 μm. The thickness of the SiC bonded semiconductor substrate may be, for example, 350 μm for a diameter of 150 mm, or 500 μm for a diameter of 200 mm. The upper limit of the thickness of the SiC polycrystalline substrate is not particularly limited and does not affect the solution of the problem of the present invention, but it can be set to 1000 μm as described above.

[0024] <Crystal Structure> Examples of crystal structures for SiC polycrystalline substrates include cubic and hexagonal crystals. The SiC polycrystalline substrate may consist of any of the following: hexagonal 4H-SiC crystals, 6H-SiC crystals, and cubic 3C-SiC crystals, or a mixture thereof. Furthermore, in order to reduce defects when bonded with a SiC single crystal substrate, a dense SiC polycrystalline substrate is desired, and for example, a cubic 3C-SiC polycrystalline substrate obtained by depositing a layer of SiC polycrystalline material by chemical vapor deposition can be used.

[0025] <Deposition Surface> The deposition surface of the SiC polycrystalline substrate 100 is the main surface of the SiC polycrystalline substrate 100 where the SiC polycrystalline film is directly deposited when forming a SiC polycrystalline film on a graphite-supported substrate or the like by chemical vapor deposition (CVD). The deposition surface exposes the crystal grains of the SiC polycrystalline film, and its surface properties and flatness affect the electrical properties of the thin film.

[0026] 〈Volume Resistivity〉 The volume resistivity of the SiC polycrystalline substrate is preferably 25 mΩcm or less. The application fields of SiC devices are mainly high-withstand-voltage and high-power electronic elements, and it is important to suppress the heat loss generated with the application of a large current. In order to suppress the generation of Joule heat caused by substrate resistance, the SiC polycrystalline substrate is required to have low resistance, and this requirement can be satisfied if the volume resistivity is 25 mΩcm or less.

[0027] For substrates for high-performance electronic element applications, the volume resistivity of the SiC polycrystalline substrate is preferably 15 mΩcm or less, and more preferably 10 mΩcm or less. The lower limit of the volume resistivity is not particularly limited, but may be the measurement limit value, and if it is 3 mΩcm or more, it can be used without trouble as a substrate for high-performance electronic element applications.

[0028] The volume resistivity of the SiC polycrystalline substrate can be measured using a volume resistivity measuring device based on the eddy current method. Examples of such an apparatus include NC-80MAP manufactured by Napson Corporation. Evaluation of the volume resistivity distribution on the film-forming surface of the SiC polycrystalline substrate is performed on the first surface 110 or the second surface 120 which are the film-forming surfaces, as indicated by the points in Figure 2, at the center point, and at equal radial distances from the center point, for a total of 9 measurement points including 8 points arranged at equal intervals in the circumferential direction, the volume resistivity can be actually measured by the eddy current method or the like.

[0029] The locations (measurement points) where the volume resistivity is measured on the first surface 110 or the second surface 120 that are the film-forming surfaces can be appropriately set other than the above-mentioned 9 locations. When the first surface 110 or the second surface 120 that are the film-forming surfaces of the SiC polycrystalline substrate 100 are circular, the total number of measurement points is preferably 5 or more, including the center point and 4 or more points arranged at equal intervals or angles in the circumferential direction at a predetermined radial distance from the center point. In particular, when a total of 9 measurement points are set as shown in Figure 2 in the present embodiment, the variation in volume resistivity on the film-forming surface can be evaluated more accurately.

[0030] The volume resistivity of the SiC polycrystalline substrate may be 25 mΩcm or less at some locations on the film-forming surface, but is preferably 25 mΩcm or less at any portion of the film-forming surface, as described above, preferably 15 mΩcm or less, and more preferably 9 mΩcm or less.

[0031] (Coefficient of Variation of Volume Resistivity) The variation in volume resistivity on the film-forming surface of the SiC polycrystalline substrate adversely affects the electrical characteristics of elements formed on the SiC bonded substrate, and causes a reduction in the manufacturing yield of elements using the SiC bonded semiconductor substrate. Therefore, in order to suppress the reduction in the manufacturing yield of elements using the SiC bonded semiconductor substrate, it is required to reduce the variation in volume resistivity on the film-forming surface of the SiC polycrystalline substrate.

[0032] In general, as an indicator of variation on the film-forming surface, the coefficient of variation (standard deviation / average value: CV value), which is obtained by dividing the standard deviation by the average value, is used. The coefficient of variation of the volume resistivity of commercially available SiC single crystal substrates is 4% or less, and the SiC polycrystalline substrate used as a support substrate for SiC bonded semiconductor substrates is expected to have a volume resistivity variation equal to or less than that of SiC single crystal substrates.

[0033] The coefficient of variation (CV value) can be calculated as "standard deviation / average value" obtained by dividing the standard deviation by the average value, based on the standard deviation and average value obtained from the volume resistivity measurement results at a plurality of measurement points on the film-forming surface, such as the nine locations described above. In order to suppress the reduction in the manufacturing yield of elements using the SiC bonded semiconductor substrate, the coefficient of variation of the volume resistivity of the SiC polycrystalline substrate is preferably 3% or less. The ideal lower limit of the coefficient of variation of volume resistivity is 0%, but 1% or more can be used as a guideline.

[0034] <Surface Roughness Sa> The main surface of the SiC polycrystalline substrate is the surface that joins with the bonding surface of the SiC single crystal substrate, so it is preferable that it be as smooth as possible. By having a smooth main surface, the occurrence of bonding defects with the bonding surface of the SiC single crystal substrate can be suppressed. The smoothness of the main surface can be indicated by the surface roughness Sa, and if the surface roughness Sa measured at multiple measurement points on the main surface is 0.35 nm or less, the occurrence of bonding defects with the bonding surface of the SiC single crystal substrate can be suppressed. If the surface roughness Sa is greater than 0.35 nm, it may be difficult to suppress the occurrence of bonding defects with the bonding surface of the SiC single crystal substrate. Furthermore, a surface roughness Sa of less than 0.05 nm is also acceptable, but considering the measurement accuracy of the device used to measure surface roughness Sa, 0.05 nm is a guideline for the lower limit. The surface roughness Sa can be calculated based on the surface roughness value measured using a contact type or non-contact type surface roughness measuring instrument.

[0035] <Standard deviation of surface roughness Sa> The standard deviation of surface roughness Sa at multiple measurement points is between 0.006 nm and 0.09 nm. As shown in Figure 2, the surface roughness Sa of the main surface is measured at a total of nine measurement points, and from these measured values, the standard deviation of surface roughness Sa at multiple measurement points on the main surface can be calculated.

[0036] When the standard deviation of surface roughness Sa at multiple measurement points is between 0.006 nm and 0.09 nm, the smoothness within the same plane of the main surface is further improved.

[0037] <CV value of surface roughness Sa> The CV value (coefficient of variation) of surface roughness Sa at multiple measurement points is between 2.6% and 30%. The CV value is obtained by dividing the standard deviation by the mean value. The CV value of surface roughness Sa can be calculated from the mean value of surface roughness Sa at a total of nine measurement points shown in Figure 2 and the above standard deviation value.

[0038] When the CV value of the surface roughness Sa at multiple measurement points is between 2.6% and 30%, the smoothness within the same plane of the main surface is further improved.

[0039] <PV value of surface roughness Sa> The PV value of surface roughness Sa at multiple measurement points is between 0.015 nm and 0.25 nm. The PV value is the difference between the maximum and minimum measured values. The PV value of surface roughness Sa can be calculated as the difference between the maximum and minimum measured values ​​of surface roughness Sa at a total of nine measurement points shown in Figure 2.

[0040] When the PV value of the surface roughness Sa at multiple measurement points is between 0.015 nm and 0.25 nm, the smoothness within the same plane of the main surface is further improved.

[0041] <Standard deviation of grain size of the main surface> It is preferable that the standard deviation of grain size measured at multiple locations on the main surface is 0.008 μm or more and 10.5 μm or less. By observing the main surface with SEM-EBSD, the grain size at multiple locations on the main surface can be measured, and the standard deviation of grain size can be calculated from all the measured grain size values ​​measured on the main surface.

[0042] The main surface of the SiC polycrystalline substrate undergoes a polishing process, such as CMP, before bonding with the bonding surface of the SiC single crystal substrate. By ensuring that the standard deviation of the crystal grain size measured at multiple locations on the main surface is between 0.008 μm and 10.5 μm, this polishing process results in superior smoothness within the same plane of the main surface.

[0043] <Standard deviation of area ratio of polar planes scattered in each of multiple specified area regions of the main surface> Preferably, the standard deviation of the area ratio of polar planes scattered in each of multiple specified area regions of the main surface is 0.008% or more and 10.5% or less. In the main surface, the {111} plane in Miller indices corresponds to the polar plane. In addition to the polar {111} plane, the main surface also has non-polar planes such as the {001} plane and the {101} plane scattered therein. These polar and non-polar planes can be observed by performing SEM-EBSD measurements on the main surface and mapping the images obtained from the measurements with respect to the crystal orientation. The standard deviation of the area ratio of polar planes is obtained by calculating the area ratio of each {111} plane scattered within predetermined area regions of a set size at multiple locations on the main surface, and then calculating the standard deviation based on that area ratio. The specified area is a region set on the main surface with each of the nine points shown in Figure 2 as a reference point, and is either a circular area with a radius of 5 mm or less centered on the reference point, or a rectangular area with a length of 5 mm or less and a width of 5 mm or less.

[0044] Polar surfaces have a higher polishing rate compared to non-polar surfaces, and steps are more likely to occur between polar and non-polar surfaces. Therefore, the fewer polar surfaces there are, the better the smoothness achieved through the polishing process. For example, if the standard deviation of the area ratio of polar surfaces on the main surface is between 0.008% and 10.5%, the smoothness within the same surface of the main surface will be better achieved through the polishing process described above.

[0045] <PV value of 55° to 65° grain boundary ratio> The PV value of the 55° to 65° grain boundary ratio, which is an indicator of the orientation difference between adjacent crystal grains on the main plane, is preferably 3.5% to 8%. The 55° to 65° grain boundary corresponds to a Σ3 grain boundary, and a Σ3 grain boundary is rotated 60° around the <111> axis and (111) plane. Since SiC polycrystals are cubic, deformation is most likely to occur starting from the <111> axis and (111) plane, and therefore the 55° to 65° grain boundary is used as an indicator of orientation difference. The 55° to 65° grain boundary can be observed by performing SEM-EBSD measurements on the main plane and mapping the image obtained from the measurement to the angular difference of the grain boundary. For the main surface measurement, SEM-EBSD measurements were performed at nine points, similar to the measurement points shown in Figure 2. For each image obtained, the 55° to 65° grain boundary ratio was calculated, where the angular difference of the grain boundaries was between 55° and 65° (i.e., within a predetermined range of either 55° or more but less than 65°, or greater than 55° but less than or equal to 65°). The PV value of the 55° to 65° grain boundary ratio was obtained as the difference between the maximum and minimum values ​​of the 55° to 65° grain boundary ratio calculated for each image.

[0046] The PV value of the 55° to 65° grain boundary ratio, which is an indicator of the orientation difference between adjacent crystal grains on the main surface, is 3.5% to 8%. This polishing process results in superior smoothness within the same plane of the main surface.

[0047] <PV value of the average grain boundary angle of the main surface> It is preferable that the PV value of the average grain boundary angle of the main surface is 1° or more and 1.9° or less. Similarly to the above, the grain boundary angle can be observed by measuring the main surface using SEM-EBSD and mapping the image obtained from the measurement for the angle difference of the grain boundary. For example, similar to the measurement points shown in Figure 2, SEM-EBSD measurements can be performed at 9 points on the main surface, the average value of the grain boundary angle (average grain boundary angle) can be measured in each image obtained, and the PV value of the average grain boundary angle of the main surface can be obtained as the difference between the maximum and minimum values ​​of the average grain boundary angles of the 9 images.

[0048] By having an average grain boundary angle PV value of 1° to 1.9° on the main surface, the above polishing process results in superior smoothness within the same surface of the main surface.

[0049] <PV value of 55°-65° grain boundary ratio / 35°-45° grain boundary ratio> It is preferable that the PV value of the ratio of the 55°-65° grain boundary ratio to the 35°-45° grain boundary ratio of the main surface (55°-65° grain boundary ratio / 35°-45° grain boundary ratio) is 0.15 or more and 0.7 or less. The ratio of the 55°-65° grain boundary and the 35°-45° grain boundary can be observed by measuring the main surface using SEM-EBSD and mapping the image obtained from the measurement for the angular difference of the grain boundaries. The measurement of the main surface is performed using SEM-EBSD at 9 points, similar to the measurement points shown in Figure 2. Then, for each of the nine SEM-EBSD images from the measurement points, the 55°–65° grain boundary ratio is divided by the 35°–45° grain boundary ratio to obtain the 55°–65° grain boundary ratio / 35°–45° grain boundary ratio. The difference between the maximum and minimum values ​​of these ratios gives the PV value of 55°–65° grain boundary ratio / 35°–45° grain boundary ratio. Note that if the 55°–65° grain boundary ratio is set to a range where the grain boundary ratio is between 55° and less than 65°, the 35°–45° grain boundary ratio should also be calculated as a ratio within the range where the grain boundary ratio is between 35° and less than 45°.

[0050] When the PV value of the 55°-65° grain boundary ratio / 35°-45° grain boundary ratio is between 0.15 and 0.7, the polishing process described above results in superior smoothness within the same plane of the main surface.

[0051] [SiC Bonded Semiconductor Substrate] The SiC bonded semiconductor substrate of this embodiment comprises the SiC polycrystalline substrate described above and a SiC single crystal substrate bonded to the main surface.

[0052] A semiconductor substrate is a substrate containing semiconductors and is used in the manufacturing process of semiconductor devices. In the case of SiC bonded semiconductor substrates, the SiC polycrystalline substrate or SiC single-crystal substrate may be semiconductor, and an epitaxial growth layer may be formed on the SiC single-crystal substrate, and then devices may be formed on it. Examples of SiC devices include electronic devices that use SiC bonded semiconductor substrates as the substrate, and these have been commercialized in the form of SiC-MOSFETs, SiC SBDs (Schottky barrier diodes), and SiC power modules equipped with SiC-MOSFETs and SiC SBDs. SiC bonded semiconductor substrates are used as the substrate in these products.

[0053] [Method for Manufacturing SiC Polycrystalline Substrates] Next, an example of a method for manufacturing SiC polycrystalline substrates will be described.

[0054] <SiC Polycrystalline Film Formation Process> The SiC polycrystalline film formation process is a process (Figure 3(B)) in which a SiC polycrystalline film 20 is formed on the surface of the substrate 10 (Figure 3(A)) by the CVD method.

[0055] (SiC polycrystalline film) The SiC polycrystalline film 20 is a thin film formed on the surface of the substrate 10 by fixing the substrate 10 in the reaction furnace of a film deposition apparatus, raising the temperature inside the reaction furnace to the growth temperature (for example, 1400°C) while flowing a gas such as hydrogen or nitrogen, and then flowing a raw material gas and a carrier gas once the growth temperature is reached.

[0056] As the base material 10, a disc-shaped base material made of isotropic graphite, which is commonly used, can be used.

[0057] (Chemical vapor deposition method) As for the raw material gas, there are no particular limitations as long as it can form a SiC polycrystalline film 20, and commonly used Si-based raw material gases and C-based raw material gases can be used.

[0058] For example, as a silicon (Si)-based raw material gas, silane (SiH) 4 In addition to being able to use monochlorosilane (SiH 3 Cl), dichlorosilane (SiH 2 Cl 2 ), trichlorosilane (SiHCl 3), tetrachlorosilane (SiCl 4 ) and other chlorine-based Si source-containing gases (chloride-based sources) that contain Cl and have an etching action can be used.

[0059] Examples of the carbon (C)-based source gas include methane (CH 4 ), ethane (C 2 H 6 ), propane (C 3 H 8 ), acetylene (C 2 H 2 ) and other hydrocarbons can be used.

[0060] In addition to the above, tetramethylsilane [(CH 3 ) 4 Si], trichloromethylsilane (CH 3 Cl 3 Si), trichlorophenylsilane (C 6 H 5 Cl 3 Si), dichloromethylsilane (CH 4 Cl 2 Si), dichlorodimethylsilane [(CH 3 ) 2 SiCl 2 , chlorotrimethylsilane [(CH 3 ) 3 SiCl] and other gases containing both Si and C can also be used as the source gas.

[0061] As the carrier gas, a commonly used carrier gas can be used as long as it can spread the source gas to the underlying base material 10 without inhibiting the film formation of the SiC polycrystalline film 20. For example, hydrogen (H 2 ), which has excellent thermal conductivity and has an etching action on SiC, can be used.

[0062] In addition, in order to apply the SiC polycrystalline substrate to high-withstand-voltage and high-output electronic device applications, impurities (dopant gas) such as nitrogen or phosphorus are introduced into the SiC polycrystalline film 20. The introduced concentration of nitrogen or phosphorus is, for example, 1×10 19 / cm 3 or more.

[0063] <Substrate Exposure Process> The substrate exposure process is a process in which, after the SiC polycrystalline film formation process, the outer peripheral edge 21 of the SiC polycrystalline film 20 formed on the surface of the substrate 10 is removed, and the outer peripheral edge 11 of the substrate 10 is exposed.

[0064] As shown in Figure 3(B), the SiC polycrystalline film 20 is formed on the outer periphery of the substrate 10 by the SiC polycrystalline film formation process described above. This can then be placed in an end-face processing device, for example, and the formed SiC polycrystalline film 20 can be ground inward from the outer edge 21 to a depth of approximately 0.01 mm to 0.5 mm to expose the outer edge 11 of the substrate 10.

[0065] <SiC Polycrystalline Film Separation Process> The SiC polycrystalline film separation process involves burning the substrate 10 shown in Figure 3(C), with its outer peripheral edge exposed, in an oxygen atmosphere to separate the SiC polycrystalline film 20 from the substrate 10, as shown in Figure 3(D). By heating the substrate 10, with its outer peripheral edge 11 exposed and a SiC polycrystalline film 20 formed on its surface, in an oxygen-containing atmosphere (oxygen atmosphere) at, for example, 1000°C, the substrate 10 is burned, and a self-supporting SiC polycrystalline substrate 30 can be obtained.

[0066] <Polishing Process> In the polishing process, the thickness of the SiC polycrystalline substrate 30 is adjusted and the surface is smoothed in order to use it as a SiC bonded semiconductor substrate. First, a smooth SiC polycrystalline substrate 100 can be obtained by high-precision grinding, then by high-precision mechanical polishing, and finally by CMP polishing.

[0067] [Film Deposition Equipment] Next, we will describe an example of film deposition equipment that can be used in the SiC polycrystalline film deposition process when manufacturing SiC polycrystalline substrates.

[0068] A film deposition apparatus capable of depositing a SiC polycrystalline film 20 on a substrate 10 by the CVD method includes, for example, a housing that serves as the exterior of the deposition apparatus, a deposition chamber for depositing the SiC polycrystalline film 20 on the substrate 10, an exhaust gas introduction chamber for introducing raw material gas and carrier gas discharged from the deposition chamber to a gas outlet, a box covering the exhaust gas introduction chamber, a carbon heater for heating the deposition chamber from outside the box, a gas inlet and gas outlet located at the bottom of the deposition chamber for introducing raw material gas and carrier gas into the deposition chamber, and a substrate holder for holding the substrate 10. The deposition chamber 1000 of a typical deposition apparatus will be described in more detail below.

[0069] <Film Deposition Chamber 1000> Figure 4 is a cross-sectional view of the film deposition chamber 1000, Figure 5 is a cross-sectional view of the film deposition chamber 1000 viewed from the direction indicated by arrow B in Figure 4, and Figure 6 is a cross-sectional view of the film deposition chamber 1000 viewed from the direction indicated by arrow D in Figure 4. The film deposition chamber 1000 is shown vertically in Figures 4 and 6 and is covered by a box-shaped wall 1010 shown as a rectangle in Figure 5. The inside of the wall 1010 is the interior 1020 of the film deposition chamber 1000, and the outside is the exterior of the film deposition chamber 1000. Inside 1020, a substrate holder 1030, which has a substrate holding portion 1031 and a holder side surface 1032, holds a plurality of base substrates 10.

[0070] Furthermore, a shaft 1040 is provided on the side of the substrate holder 1030, and the shaft 1040 rotates around its central axis and a corresponding rotation axis A, causing the substrate 10 to rotate together with the substrate holder 1030. The raw material gas and carrier gas pass through the rotating substrate 10 with arrow B upstream and arrow C downstream, thereby forming a SiC polycrystalline film 20 on the substrate 10.

[0071] However, in the deposition chamber 1000, the main surface of the resulting SiC polycrystalline substrate will have poor surface smoothness even after the polishing process. The reason for this is that, inside the interior 1020 covered by the box-shaped walls 1010 of the deposition chamber 1000, the SiC polycrystalline film 20 tends to be deposited more easily on the outer periphery of the rotating substrate 10. As a result, the SiC polycrystalline film 20 is deposited thickly on the outer periphery of the substrate 10 and thinly in the center, leading to uneven deposition and variations in the deposition state on the deposition surface.

[0072] Therefore, in order to obtain a SiC polycrystalline substrate 100 having a main surface with excellent surface smoothness, it is important to use the film deposition chamber 2000 described below.

[0073] <Film Deposition Chamber 2000> Figure 7 is a cross-sectional view of the film deposition chamber 2000, Figure 8 is a cross-sectional view of the film deposition chamber 2000 viewed from the direction indicated by arrow B in Figure 7, and Figure 9 is a cross-sectional view of the film deposition chamber 2000 viewed from the direction indicated by arrow D in Figure 7. The film deposition chamber 2000 is shown vertically in Figures 7 and 9 and is covered by a box-shaped wall 2010 shown as a rectangle in Figure 8. The inside of the wall 2010 is the interior 2020 of the film deposition chamber 2000, and the outside is the exterior of the film deposition chamber 2000. Inside the interior 2020, a substrate holder 1030, which has a substrate holding portion 1031 and a holder side surface 1032, holds a plurality of base substrates 10.

[0074] Furthermore, a shaft 1040 is provided on the side of the substrate holder 1030, and the shaft 1040 rotates around its central axis and a corresponding rotation axis A, causing the substrate 10 to rotate together with the substrate holder 1030. The raw material gas and carrier gas pass through the rotating substrate 10 with arrow B upstream and arrow C downstream, thereby forming a SiC polycrystalline film 20 on the substrate 10.

[0075] The key difference between the film deposition chamber 2000 and the film deposition chamber 1000 is that the film deposition chamber 2000 has a tapered inner wall 2011 that narrows from upstream of the source gas and carrier gas toward the rotation axis A, and a tapered inner wall 2012 that widens from the rotation axis A toward the downstream of the source gas and carrier gas, whereas the film deposition chamber 1000 does not have such an inner wall.

[0076] When the deposition chamber 2000 is equipped with tapered inner walls 2011 and 2012, the flow velocity of the raw material gas is fastest at the rotation axis A. As a result, an environment is created in which the SiC polycrystalline film 20 can be easily deposited not only on the outer periphery of the substrate 10 but also in the central part where the flow velocity of the raw material gas is high. Compared to when the deposition chamber 1000 is used, a SiC polycrystalline film 20 of uniform thickness is deposited on the substrate 10. If a SiC polycrystalline film 20 of uniform thickness is deposited by chemical vapor deposition, the deposition state on the deposition surface of the film becomes uniform, and a SiC polycrystalline substrate 100 having a main surface with excellent surface smoothness can be obtained.

[0077] Furthermore, a key difference between the film deposition chamber 2000 and the film deposition chamber 1000 is that the 2000 is equipped with a raw material gas supply pipe 2030. The 2000 has multiple raw material gas supply ports 2031, through which, for example, C-based raw material gas can be supplied to the substrate 10 being deposited inside the 2020.

[0078] When depositing a SiC polycrystalline film, the vicinity of the surface of the substrate 10 is sufficiently filled with Si, but there is a high risk of C depletion. This is because the flow rate of the C-based raw material gas and the film deposition rate are very strongly correlated. When C is depleted, the ratio of C to Si near the surface of the substrate 10 changes, and as a result, the polarity and orientation of the SiC polycrystalline film are thought to change. Therefore, by supplementing the C depleted near the surface of the substrate 10 with a C-based raw material gas supplied from the raw material gas supply pipe 2030, the ratio of C to Si near the surface of the substrate 10 can be made uniform, thereby obtaining a SiC polycrystalline substrate 100 having a main surface with excellent surface smoothness.

[0079] The present invention will be described in detail below with reference to examples and comparative examples.

[0080] [Example 1] An isotropic graphite disc with a diameter of 23 cm and a thickness of 0.5 cm was prepared as a disc-shaped substrate 10, and eight substrates 10 were placed in the deposition chamber 2000 of the aforementioned deposition apparatus using a substrate holder 1030. Then, while rotating the substrates 10 by rotating the shaft 1040, a SiC polycrystalline film 20 was deposited on the substrates 10 by chemical vapor deposition for 10 hours (SiC polycrystalline film deposition process).

[0081] Regarding the film deposition conditions, the pressure, temperature, and rotation speed in the deposition chamber 2000 were set to 98 kPa, the deposition temperature to 1350°C, and the rotation speed of the substrate 10 to 10 revolutions / minute. Inside the deposition chamber 2020, the ratio of the length of the short side E on the rotation axis A in the direction parallel to the rotation axis A to the length of the long side F upstream or downstream of the substrate holder 1030 was set to E:F = 1:1.25. The length of the sides in the direction perpendicular to the rotation axis A inside the deposition chamber 2020 was kept constant without any taper or other variations.

[0082] Next, we will explain the gas conditions among the film deposition conditions. First, the gas ratio of C-based raw material gas to Si-based raw material gas was set to C / Si = 0.7. To achieve this gas ratio, acetylene (C) was added from the upstream (arrow B) in Figure 7. 2 H 2 ) Gas at 350 sccm, dichlorosilane (SiH 2 Cl 2 ) gas was introduced into the deposition chamber 2000 at a flow rate of 1000 sccm, followed by 5000 sccm of dopant nitrogen gas, and 10000 sccm of hydrogen gas as a carrier gas. Here, the acetylene and dichlorosilane introduced from upstream (arrow B) first come into contact with the outer edges of the substrate 10 and are used to form the SiC polycrystalline film 20. As a result, the acetylene and dichlorosilane are consumed from the outer edges of the substrate 10 towards the center, and the flow rates in the center become 210 sccm for acetylene and 700 sccm for dichlorosilane introduced from upstream (arrow B), causing the gas ratio to change to C / Si = 0.6. Therefore, in order to maintain this gas ratio of C / Si = 0.7 even in the center, 35 sccm of acetylene was introduced into the deposition chamber 2000 from the raw material gas supply port 2031.

[0083] Next, a disc-shaped base material 10, on which a SiC polycrystalline film 20 was deposited on both sides, was placed into an end-face processing device, and the outer periphery of the base material 10 was ground to a thickness of 0.05 mm to expose the outer edge 11 of the base material 10 (base material exposure step).

[0084] Then, in an atmospheric environment at 1000°C, the substrate 10 with its outer peripheral edge 11 exposed was heated and burned for 24 hours to separate the SiC polycrystalline film 20 from the substrate 10 (SiC polycrystalline film separation step). Subsequently, the front and back surfaces of the SiC polycrystalline substrate 30 were flattened by grinding them by 0.5 mm each (polishing step), and 16 cubic SiC polycrystalline substrates 100 were manufactured per lot. These processes were repeated for 23 lots under the same conditions to obtain 368 SiC polycrystalline substrates 100.

[0085] [Comparative Example 1] Using a film deposition apparatus equipped with a film deposition chamber 1000, 368 SiC polycrystalline substrates were manufactured in the same manner as in Example 1, except that acetylene gas was not supplied from the raw material gas supply port 2031. Because acetylene gas was not supplied from the raw material gas supply port 2031, the gas ratio at the outer edge of the substrate 10 was C / Si = 0.7, but the flow rates at the center of the substrate 10 were 210 sccm for acetylene and 700 sccm for dichlorosilane, and the gas ratio changed to C / Si = 0.6.

[0086] Using 368 sheets each of the manufactured SiC polycrystalline substrates for Example 1 and Comparative Example 1, the following measurements and evaluations were performed.

[0087] <Measurement of surface roughness Sa> Using a non-contact surface roughness measuring instrument, the surface roughness Sa of the main surface of the SiC polycrystalline substrate was measured at a total of nine measurement points, as shown in Figure 2.

[0088] <Standard deviation of surface roughness Sa> The standard deviation of surface roughness Sa was calculated from the measured values ​​of surface roughness Sa, as the standard deviation of surface roughness Sa within the same surface on the main surface.

[0089] <CV value of surface roughness Sa> From the measured values ​​of surface roughness Sa, the CV value of surface roughness Sa was calculated from the average value of surface roughness Sa at a total of nine measurement points shown in Figure 2 and the standard deviation value mentioned above.

[0090] <PV value of surface roughness Sa> The PV value of surface roughness Sa was calculated as the difference between the maximum and minimum values ​​of the surface roughness Sa measured at a total of nine measurement points shown in Figure 2.

[0091] <Standard deviation of grain size on the main surface> The grain size was measured by SEM-EBSD observation of the main surface. Then, the in-plane standard deviation was calculated from all the grain size measurements taken on the main surface.

[0092] <Standard deviation of the area ratio of polar planes on the main surface> The area ratio of polar planes on the main surface was observed by performing SEM-EBSD measurements on the main surface and mapping the resulting images for crystal orientation. The standard deviation of the area ratio of polar planes on the main surface was obtained by calculating the area ratio of {111} planes scattered in each of the multiple specified area regions of the main surface, and then calculating the standard deviation based on that area ratio.

[0093] <PV Values ​​for 55°–65° Grain Boundary Ratio> The ratio of 55°–65° grain boundaries was observed by measuring the main surface using SEM-EBSD and mapping the resulting images for the angular difference of the grain boundaries. The PV values ​​for the 55°–65° grain boundary ratio were calculated as the difference between the maximum and minimum values ​​obtained from nine measurements, similar to the measurement points shown in Figure 2.

[0094] <PV value of average grain boundary angle of the main surface> The grain boundary angle was measured on the main surface using SEM-EBSD, and the obtained images were observed by mapping the angle difference of the grain boundaries. The angle of each grain boundary on the main surface was measured, and the PV value of the average grain boundary angle of the main surface was calculated as the difference between the maximum and minimum values ​​of these angles.

[0095] <PV values ​​for 55°–65° grain boundary ratio / 35°–45° grain boundary ratio> The ratios of 55°–65° grain boundaries and 35°–45° grain boundaries were observed by measuring the main surface using SEM-EBSD and mapping the images obtained from the measurements for the angular difference of the grain boundaries. The PV values ​​for the 55°–65° grain boundary ratio / 35°–45° grain boundary ratio were calculated by taking measurements at 9 points, similar to the measurement points shown in Figure 2, and obtaining 9 values ​​by dividing the 55°–65° grain boundary ratio by the 35°–45° grain boundary ratio, and then calculating the difference between the maximum and minimum values ​​obtained.

[0096] The results are shown in Table 1.

[0097]

[0098] As shown in Table 1, in Example 1, the standard deviation of the grain size measured at multiple locations on the main surface was 0.009 μm to 10.1 μm, the standard deviation of the area ratio of polar surfaces on the main surface was 0.0095% to 10.1%, the PV value of the 55° to 65° grain boundary ratio was 3.6% to 4.3%, the PV value of the average grain boundary angle on the main surface was 1.36° to 1.47°, and the PV value of the ratio of the 55° to 65° grain boundary ratio to the 35° to 45° grain boundary ratio (55° to 65° grain boundary ratio / 35° to 45° grain boundary ratio) on the main surface was 0.17 to 0.18. Furthermore, according to the surface roughness measurement results, the surface roughness Sa was 0.3 nm or less, and from the numerical range of the standard deviation of the surface roughness Sa, the CV value (coefficient of variation), and the PV value, it was found that all SiC polycrystalline substrates in Example 1 had a uniformly smooth main surface.

[0099] On the other hand, Comparative Example 1 was obtained using a film deposition apparatus equipped with a conventional film deposition chamber 1000. Compared to Example 1, the surface roughness Sa was 0.34 nm or less, indicating inferior smoothness. Furthermore, the standard deviation of the surface roughness Sa, the CV value (coefficient of variation), the PV value, and other numerical ranges indicate that the SiC polycrystalline substrate of Comparative Example 1 was inferior in terms of uniformity in terms of smoothness.

[0100] The present invention makes it possible to realize a SiC polycrystalline substrate having a bonded surface with excellent surface smoothness, and by providing such a SiC polycrystalline substrate and a SiC bonded semiconductor substrate, it is possible to suppress a decrease in the manufacturing yield of devices using the SiC bonded semiconductor substrate.

[0101] 10: Substrate material, 11: Outer edge, 20: SiC polycrystalline film, 21: Outer edge, 30: SiC polycrystalline substrate, 100: SiC polycrystalline substrate, 110: First surface, 120: Second surface, 1000: Film deposition chamber, 1010: Wall, 1020: Interior, 1030: Substrate holder, 1031: Substrate holding part, 1032: Holder side, 1040: Shaft, 2000: Film deposition chamber, 2010: Wall, 2011: Inner wall, 2012: Inner wall, 2020: Interior, 2030: Raw material gas supply pipe, 2031: Raw material gas supply port

Claims

1. A SiC polycrystalline substrate having a surface roughness Sa measured at multiple measurement points on the main surface of 0.35 nm or less, a standard deviation of the surface roughness Sa at the multiple measurement points of 0.006 nm or more and 0.09 nm or less, a CV value of the surface roughness Sa at the multiple measurement points of 2.6% or more and 30% or less, and a PV value of the surface roughness Sa at the multiple measurement points of 0.015 nm or more and 0.25 nm or less.

2. The SiC polycrystalline substrate according to claim 1, wherein the standard deviation of the crystal grain size measured at multiple locations on the main surface is 0.008 μm or more and 10.5 μm or less.

3. The SiC polycrystalline substrate according to claim 1, wherein the standard deviation of the area ratio of polar surfaces scattered in each of the plurality of specified area regions of the main surface is 0.008% or more and 10.5% or less.

4. The SiC polycrystalline substrate according to claim 1, wherein the PV value of the 55° to 65° grain boundary ratio, which is an indicator of the orientation difference between adjacent crystal grains on the main surface, is 3.5% or more and 8% or less, the PV value of the average grain boundary angle on the main surface is 1° or more and 1.9° or less, and the PV value of the ratio of the 55° to 65° grain boundary ratio to the 35° to 45° grain boundary ratio (55° to 65° grain boundary ratio / 35° to 45° grain boundary ratio) on the main surface is 0.15 or more and 0.7 or less.

5. The SiC polycrystalline substrate according to claim 1, for use in a SiC bonded semiconductor substrate.

6. The SiC polycrystalline substrate according to claim 1, wherein the volume resistivity is 25 mΩcm or less.

7. A SiC bonded semiconductor substrate comprising: a SiC polycrystalline substrate according to claim 1; and a SiC single crystal substrate bonded to the main surface.