Method for manufacturing substrate for magnetic recording medium

The method of firing, grinding, and polishing steatite molded bodies, combined with HIP treatment and a heat-resistant film, addresses the need for high heat resistance and specific modulus in magnetic recording medium substrates, enhancing stability and reducing manufacturing costs.

WO2026235084A1PCT designated stage Publication Date: 2026-11-12RESONAC HARD DISK CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/017038
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-04-30
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

The challenge is to produce a magnetic recording medium substrate with high heat resistance and specific modulus at a low cost, while minimizing fluttering during high-speed rotation, which is essential for increasing storage capacity and stability in hard disk drives.

Method used

A method involving a firing step for a steatite molded body, followed by grinding and polishing processes, including HIP treatment to enhance mechanical properties and apply a heat-resistant film, resulting in a steatite sintered body with improved heat resistance and specific modulus.

Benefits of technology

The method enables the production of magnetic recording medium substrates with enhanced heat resistance and specific modulus, reducing fluttering and ensuring stable reading and writing in hard disk drives at a lower cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026017038_12112026_PF_FP_ABST
    Figure JP2026017038_12112026_PF_FP_ABST
Patent Text Reader

Abstract

A method for manufacturing a substrate for a magnetic recording medium, the method comprising a firing step for firing a steatite molded body having a plate-like shape while rotating the same.
Need to check novelty before this filing date? Find Prior Art

Description

Manufacturing method for substrates for magnetic recording media

[0001] This disclosure relates to a method for manufacturing a substrate for a magnetic recording medium.

[0002] In recent years, with the development of the internet network and the expansion of big data utilization, the amount of data stored in data centers has continued to increase. From the perspective of securing space in data centers, there is a demand for hard disk drives with high storage capacity per unit.

[0003] Attempts to increase the storage capacity per standardized hard disk drive include, for example, increasing the storage capacity per magnetic recording medium and increasing the number of magnetic recording media that can be placed inside the drive case.

[0004] In attempts to increase the storage capacity per magnetic recording medium, L1 0 FePt alloy having a type crystal structure and L1 0 Assist recording media that use CoPt alloys with a specific crystal structure in their magnetic layers are attracting attention. In these assist recording media, the surface of the magnetic recording media is locally assisted by irradiating it with near-field light and microwaves, thereby reducing the coercivity of the magnetic recording media and enabling writing. When manufacturing assist recording media containing FePt alloys and CoPt alloys in the magnetic layer, it is necessary to raise the substrate temperature to 400°C or higher, requiring the substrate to have high heat resistance.

[0005] Attempts to increase the number of magnetic recording media that can be housed inside a drive case require thinning the circuit board. However, thinning the circuit board can sometimes cause fluttering of the magnetic recording media. Fluttering is the rattling of the magnetic recording media that occurs when it is rotated at high speed. If the fluttering of the magnetic recording media becomes large, stable reading and writing may become difficult in a hard disk drive.

[0006] To suppress fluttering of magnetic recording media, for example, Patent Document 1 describes using a material with a high specific modulus of elasticity (Young's modulus divided by glass density) as the material for the substrate of the magnetic recording media.

[0007] Japanese Patent Application Publication No. 2015-026414

[0008] One aspect of this disclosure aims to provide a method for manufacturing a magnetic recording medium substrate that can produce a magnetic recording medium substrate with excellent heat resistance and specific modulus at low cost.

[0009] One aspect of the present disclosure is a method for manufacturing a substrate for a magnetic recording medium, which includes a firing step of firing a steatite molded body having a plate-like shape while rotating it.

[0010] According to one aspect of this disclosure, a method for manufacturing a magnetic recording medium substrate that has excellent heat resistance and specific modulus can be produced at low cost.

[0011] This is a schematic perspective view showing an example of the structure of a firing apparatus. This is a schematic perspective view showing an example of the structure of a grinding machine. This is a schematic perspective view showing an example of the structure of an inner and outer circumference grinding machine. This is a schematic perspective view showing an example of the structure of an inner circumference polishing machine. This is a schematic perspective view showing an example of the structure of an outer circumference polishing machine. This is a schematic perspective view showing an example of the structure of a polishing machine. This is a schematic cross-sectional view showing an example of a magnetic recording medium manufactured by the manufacturing method of the magnetic recording medium of the embodiment of this disclosure. This is a schematic perspective view showing an example of the structure of a magnetic recording and playback device.

[0012] In recent years, the demand for increased storage capacity in hard disk drives has been relentless, requiring even higher heat resistance and specific modulus of elasticity for magnetic recording medium substrates. Furthermore, to ensure substitutability with conventional magnetic recording medium substrates, the manufacturing cost must be equivalent to that of conventional substrates.

[0013] The method for manufacturing a substrate for a magnetic recording medium according to the embodiment of this disclosure (hereinafter simply referred to as "this embodiment") can provide a substrate for a magnetic recording medium with excellent heat resistance and specific modulus at a low cost.

[0014] The details of the manufacturing method for a magnetic recording medium substrate according to this embodiment are described below.

[0015] (Method for manufacturing a substrate for a magnetic recording medium) The method for manufacturing a substrate for a magnetic recording medium according to this embodiment includes a firing step and may optionally include a grinding step, an inner and outer circumference grinding step, an inner circumference polishing step, an outer circumference polishing step, a polishing step, a secondary polishing step, and other steps.

[0016] By applying the magnetic recording medium substrate obtained by the manufacturing method of the magnetic recording medium substrate according to this embodiment to a magnetic recording medium and a hard disk drive, fluttering is reduced. As a result, magnetic recording media and hard disk drives capable of stable reading and writing can be provided at a low cost.

[0017] The shape of the magnetic recording medium substrate obtained by the manufacturing method of the magnetic recording medium substrate according to this embodiment is not particularly limited and can be appropriately selected according to the purpose. From the viewpoint of application to magnetic recording media and hard disk drives, the magnetic recording medium substrate is preferably disc-shaped with an opening in the center. A magnetic recording medium can be manufactured by sequentially laminating a magnetic layer, a protective layer, a lubricating film, etc., on a disc-shaped magnetic recording medium substrate. In a hard disk drive, the central part of the obtained magnetic recording medium is attached to the rotation axis of a spindle motor and rotated, and information can be read from and written to the magnetic recording medium while a magnetic head is levitating and moving on the surface of the magnetic recording medium.

[0018] The magnetic recording medium substrate obtained by the manufacturing method of the magnetic recording medium substrate according to this embodiment can be used to increase the number of magnetic recording media that can be housed in a standardized hard disk drive case by processing the steatite sintered body, described later, to a predetermined size. For this reason, it is preferable that it can be housed in a standardized hard disk drive case, i.e., a 2.5-inch hard disk drive case or a 3.5-inch hard disk drive case. For a 2.5-inch hard disk drive, a magnetic recording medium substrate having a disc shape with a maximum diameter of about 67 mm and an inner diameter of about 20 mm may be used. For a 3.5-inch hard disk drive, a magnetic recording medium substrate having a disc shape with a maximum diameter of about 97 mm and an inner diameter of about 25 mm may be used.

[0019] The thickness of the substrate for the magnetic recording medium is not particularly limited and can be appropriately selected according to the purpose, but it is preferably 1.27 mm or less, more preferably 0.8 mm or less, and even more preferably 0.5 mm or less. In this specification, the thickness of the substrate for the magnetic recording medium refers to the length in the direction perpendicular to the main surface of the substrate. The thickness of the substrate for the magnetic recording medium may be, for example, the thickness measured at any point in the cross-section of the substrate, or it may be the average value of several measurements taken at any point. Hereafter, the definition of thickness will be defined similarly for other components.

[0020] <Firing Process> The firing process is a process of firing a steatite molded body having a plate-like shape while rotating it. The firing process can be suitably carried out by firing means.

[0021] In the firing step, it is preferable to fire the steatite molded body while rotating the steatite molded body along the conveyance direction of the steatite molded body on a conveying member. At this time, it is preferable to rotate the steatite molded body in a state where the end face of the steatite molded body faces the conveying member. More specifically, in the firing step, the steatite molded body is preferably supported such that the main surface of the steatite molded body stands upright with respect to the conveyance direction, and it is more preferable to support the steatite molded body such that the main surface of the steatite molded body is substantially parallel to the direction of gravity.

[0022] In the present specification, the "state in which the main surface of the steatite molded body stands upright with respect to the conveyance direction" means that the angle between the conveyance direction and the main surface of the steatite molded body is more than 0° and 90° or less, and is preferably approximately 90°. The terms "approximately 90°" and "substantially parallel" in the present specification may include not only the case of strictly 90° and parallel, but also the case where the deviation from 90° and parallel is 5° or less.

[0023] <<Steatite Molded Body>> The substrate for a magnetic recording medium manufactured by the method for manufacturing a substrate for a magnetic recording medium according to the present embodiment includes a steatite sintered body (MgO·SiO 2 ).

[0024] The steatite used for the steatite molded body is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include talc (Mg 3 Si 4 O 10 (OH) 2 ), kaolin (Al 2 Si 2 O 5 (OH) 4 ), feldspar (KAlSi 3 O 8 ) and magnesium oxide (MgO), and the like.

[0025] The shape of the steatite molded body is not particularly limited as long as it is a plate-like shape, and can be appropriately selected according to the purpose. From the viewpoint of application to magnetic recording media and hard disk drives, the steatite molded body preferably has a disk-like shape with an opening at the center.

[0026] There are no particular limitations on the method for manufacturing a steatite sintered body, and a suitable method can be selected depending on the purpose. For example, the following methods can be used.

[0027] Ingredients include talc (Mg 3 Si 4 O 10 (OH) 2 ), kaolin (Al 2 Si 2 O 5 (OH) 4 ), feldspar (KAlSi 3 O 8 Prepare powders such as talc and magnesium oxide (MgO). Mix these powders in appropriate proportions using a ball mill and kneader, and then mold them into a plate shape. Dry the resulting steatite molded body using air drying and a drying oven to remove moisture. With the end face of the resulting steatite molded body facing the conveying member, sinter the steatite molded body while rotating it along the conveying direction. The talc will then decompose and a steatite sintered body will be formed. The resulting steatite sintered body will be machined and surface finished to the specified dimensions.

[0028] There are no particular restrictions on the method of forming steatite into a plate shape, and a suitable method can be selected depending on the purpose. Examples include compression molding, in which powder is placed in a mold and compressed under high pressure; extrusion molding, in which a mixed powder is extruded into a desired shape using an extruder; and casting, in which a slurry-like mixture is poured into a mold and dried to form the shape.

[0029] Here, the structure of the firing apparatus for firing steatite molded bodies will be explained using Figure 1. Figure 1 is a schematic perspective view showing an example of the structure of a firing apparatus.

[0030] The firing apparatus 300 can perform firing while simultaneously rotating and conveying the steatite molded body 301. The firing apparatus 300 fires the steatite molded body 301 while rotating it along the conveying direction (arrow direction in Figure 1) with the end face of the plate-shaped steatite molded body 301 facing the conveyor 305, which is a conveying member. The steatite molded body 301 and the support member 302 are supported by a jig 306 placed on the conveyor 305. The support member 302 is connected to a sun gear 303 at its end. The sun gear 303 meshes with teeth 304 fixed to the conveyor 305. When the conveyor 305 moves in the conveying direction (arrow direction in Figure 1), the sun gear 303 is rotated in the circumferential direction, and the support member 302 and the steatite molded body 301 are similarly rotated by the rotation of the sun gear 303. By firing the steatite molded body 301 in this state, deformation of the steatite molded body 301 during firing is mitigated. In this way, the firing apparatus 300 can perform the firing process of the steatite molded body 301 continuously. As a result, processing of the steatite sintered body becomes easier, and the manufacturing cost of substrates for magnetic recording media can be reduced.

[0031] When firing is performed while rotating and transporting the steatite molded body 301 separately, in the firing apparatus 300 of Figure 1, the engagement between the sun gear 303 and the teeth 304 is disengaged, and the rotation of the support member 302 and the transport of the steatite molded body 301 by the conveyor 305 are performed independently. In this case, the conveyor 305 brings the steatite molded body 301, held by the support member 302, into the firing apparatus 300, and then stops the conveyor 305. After that, the steatite molded body 301 is fired while rotating the support member 302. After firing, the fired product is transported out of the firing apparatus 300 by the conveyor 305. When firing is performed while rotating and transporting the steatite molded body 301 separately, the transport distance by the conveyor 305 inside the firing apparatus 300 can be shortened, so the firing apparatus 300 can be made smaller.

[0032] In the firing process, it is preferable to form the steatite molded body into a disc-shaped steatite molded body 301 having an opening in the center, and to rotate the steatite molded body 301 by rotating a support member 302 inserted into the opening while firing. By firing in this manner, it becomes possible to produce magnetic recording medium substrates more simply and to reduce the manufacturing cost of magnetic recording medium substrates.

[0033] In the firing process, it is preferable to insert support members 302 into the openings of multiple steatite molded bodies 301 before firing. By firing in this manner, multiple steatite sintered bodies can be obtained in a single firing process. This increases productivity and reduces the manufacturing cost of substrates for magnetic recording media.

[0034] There are no particular restrictions on the firing conditions for steatite molded bodies, and they can be appropriately selected according to the purpose. For example, N 2 In a gas atmosphere, the maximum temperature can be set to 1,200°C or higher and 1,400°C or lower, the holding time in this temperature range can be set to 1 hour, the rotation speed of the steatite molded body can be preferably set to 0.1 times / min or higher and 20 times / min or lower, more preferably to 0.5 times / min or higher and 10 times / min or lower, and the moving speed can be preferably set to 10 cm / min or lower.

[0035] Steatite sintered bodies obtained through the firing process possess properties such as electrical insulation, heat resistance, and mechanical strength, and are therefore widely used in electrical components and insulators. As a result, thin sheets suitable for processing into substrates for magnetic recording media are readily available, enabling the inexpensive manufacture of such substrates.

[0036] There are no particular restrictions on the various physical properties of the steatite sintered body, and they can be appropriately selected according to the purpose. For example, a density (ρ) of approximately 2.7 g / cm³ 3 The Young's modulus (E) is approximately 125 GPa, and the specific modulus of elasticity (E / ρ) is approximately 46 GPa·cm. 3 The density (ρ) and melting point can be set to approximately 1,300°C. Conventionally, aluminum alloy substrates used as substrates for magnetic recording media have a density (ρ) of approximately 2.8 g / cm³. 3The Young's modulus (E) is approximately 75 GPa, and the specific modulus of elasticity (E / ρ) is approximately 27 GPa·cm. 3 The density (ρ) is approximately 2.5 g / cm³. 3 The Young's modulus (E) is approximately 80 GPa, and the specific modulus of elasticity (E / ρ) is approximately 32 GPa·cm. 3 The specific modulus (E / ρ) and melting point (softening point) are approximately 780°C. Comparing the physical properties of the steatite sintered body of this embodiment with those of conventional aluminum alloy substrates and glass substrates, it can be seen that the steatite sintered body of this embodiment has superior specific modulus (E / ρ) and melting point. In other words, the magnetic recording medium substrate containing the steatite sintered body of this embodiment has superior heat resistance and specific modulus compared to conventional magnetic recording medium substrates.

[0037] - HIP Treatment - It is preferable to perform HIP (Hot Isostatic Pressing) treatment on the steatite sintered body. HIP treatment is a process that uses argon gas or the like as a pressure medium and utilizes the synergistic effect of high temperature and high pressure to perform powder sintering, diffusion bonding, and removal of internal defects.

[0038] There are no particular restrictions on the various conditions used when performing HIP treatment, and they can be appropriately selected according to the purpose. However, it is preferable that the treatment temperature be between 1,200°C and 1,400°C, the pressure be between 100 MPa and 200 MPa, and the treatment time be between 1 hour and 4 hours.

[0039] When a steatite sintered body is subjected to HIP treatment, the fine voids and defects within the sintered body are compressed, thereby increasing the density of the steatite sintered body. This improves the mechanical strength and durability of the steatite sintered body.

[0040] When steatite sintered bodies are subjected to HIP treatment, their mechanical properties, such as toughness, hardness, compressive strength, and tensile strength, are improved.

[0041] When HIP treatment is applied to a steatite sintered body, defects and inhomogeneities within the steatite sintered body are corrected during the HIP treatment, thereby improving the overall homogeneity of the steatite sintered body. This results in consistently higher product quality.

[0042] Applying HIP treatment to a steatite sintered body reduces defects within the sintered body, thereby improving its fatigue resistance and enabling long-term use.

[0043] When a steatite sintered body is subjected to HIP treatment, the pores inside the steatite sintered body are closed, improving the airtightness of the steatite sintered body and reducing degassing during sputter deposition, as described later.

[0044] When a steatite sintered body is subjected to HIP treatment, it is treated in a high-temperature, high-pressure environment, which improves the chemical stability of the steatite sintered body and enhances its resistance to corrosion and oxidation.

[0045] - Heat-resistant film - The HIP-treated steatite sintered body is made of SiO 2 SiC, Si 3 N 4 and Al 2 O 3 A heat-resistant film containing one or more alloys selected from the group including may be formed on the surface. The heat-resistant film is SiO 2 SiC, Si 3 N 4 or Al 2 O 3 It may be composed of SiO 2 SiC, Si 3 N 4 and Al 2 O 3 It may be composed of two or more alloys selected from the group including [the specified alloy].

[0046] Steatite sintered bodies, formed by sintering powder, are prone to developing fine voids within them. These voids can impair the smoothness of the magnetic recording medium substrate, or they can cause cracks, reducing the mechanical strength of the substrate. By having a heat-resistant film on the surface of the steatite sintered body, the surface voids are sealed, improving the smoothness of the magnetic recording medium substrate surface. Furthermore, crack formation is suppressed, improving the mechanical strength of the magnetic recording medium substrate.

[0047] The heat-resistant film has high heat resistance. Therefore, the heat resistance of the substrate for magnetic recording media is improved when the steatite sintered body has a heat-resistant film on its surface. The specific heat resistance temperature of each material depends on the atmosphere, but SiO 2 SiC can withstand temperatures of approximately 1,000°C, SiC can withstand temperatures of approximately 1,500°C, Si 3 N 4 At approximately 1,000°C and Al 2 O 3 The temperature is approximately 1,500°C.

[0048] The heat resistance temperature of the substrate for the magnetic recording medium is preferably higher than the heating temperature of the substrate during the manufacturing process of the magnetic recording medium. 0 FePt alloy having a type crystal structure and L1 0 When using a CoPt alloy having a specific crystal structure, the heat resistance temperature of the substrate for the magnetic recording medium is preferably 400°C or higher, and more preferably 500°C or higher.

[0049] There are no particular limitations on the method for forming a heat-resistant film on the surface of a steatite sintered body, and a suitable method can be selected depending on the purpose. However, from the viewpoint of simplicity and low cost, a film formation method using a liquid is preferred. Specifically, examples include a spin coating method in which a liquid precursor is dropped onto the steatite sintered body and a film is formed using a spin coater; a dip coating method in which a thin film is formed by immersing the steatite sintered body in a liquid precursor and then pulling it out; and a spray coating method in which a liquid precursor is sprayed onto the steatite sintered body using an airbrush and a spray nozzle.

[0050] SiO 2Examples of liquid precursors for film formation include tetraethoxysilane (TEOS, chemical formula: Si(OC)). 2 H 5 ) 4 ) and methylsilisesquioxane (MSQ, chemical formula: (CH) 3 SiO 3/2 Examples include )n). After coating with these liquid precursors, the sintered body is fired at, for example, 800°C or below, thereby forming SiO on the surface of the steatite sintered body. 2 It can form a film.

[0051] Examples of liquid precursors for forming the SiC film include polysilazane-based precursors such as polymethylsilazane and silaniols. After coating with these liquid precursors, the SiC film can be formed on the surface of the steatite sintered body by firing at, for example, 800°C or higher.

[0052] Si 3 N 4 Examples of liquid precursors for forming the film include polysilazane-based precursors such as polydimethylsilazane and aminosilanes. After coating with these liquid precursors, for example, ammonia (NH4) 3 ) or nitrogen (N 2 By firing the steatite sintered body in a suitable atmosphere at a temperature of 800°C or higher, Si is formed on the surface of the steatite sintered body. 3 N 4 It can form a film.

[0053] Al 2 O 3 Examples of liquid precursors for forming the film include aluminum alkoxides such as aluminum isopropoxide and aluminum acetylacetonate. After coating with these liquid precursors, the sintered body is fired at, for example, 800°C or below to form an Al film on the surface. 2 O 3 It can form a film.

[0054] <Grinding Process> The grinding process is a process of grinding the surface of the steatite sintered body. The grinding process can be suitably carried out by a grinding means for grinding the surface of the steatite sintered body. The grinding process is sometimes also called the lapping process.

[0055] The grinding process, more specifically, is a process of grinding (lapping) the surface of the steatite sintered body using a grinding means to make the surface of the steatite sintered body smooth. Here, the grinding process will be explained in detail with reference to Figure 2. In this specification, the objects to be processed in each process may be referred to as workpieces.

[0056] As for the grinding method, there are no particular restrictions as long as it can grind the surface of the steatite sintered body to a smooth finish, and it can be appropriately selected according to the purpose.

[0057] The steatite sintered body used in the grinding process may or may not have a heat-resistant film on its surface, but it is preferable to have a heat-resistant film.

[0058] Figure 2 is a schematic perspective view showing an example of the structure of a grinding machine that performs a grinding process. The grinding machine 40, which is an example of a grinding means shown in Figure 2, comprises a holder (carrier) 30 that holds a plurality of workpieces (steatite sintered bodies) in an opening, a lower platen 21a on which the workpieces are placed, and an upper platen 21b that applies the pressure necessary to press down on the workpieces from above and perform grinding.

[0059] The lower platen 21a has teeth 42 on its outer circumference, and a sun gear 44 is located approximately in the center of the lower platen 21a. The holder 30 has teeth 32 on its outer circumference, which mesh with both the teeth 42 of the lower platen 21a and the sun gear 44. Rotating shafts 46a and 46b are installed approximately in the center of the lower platen 21a and the upper platen 21b, respectively, for rotating them.

[0060] The lower platen 21a and the upper platen 21b are embedded with abrasive material for grinding the surface of the workpiece. There are no particular restrictions on the abrasive material, and it can be appropriately selected according to the purpose. Examples include alumina (aluminum oxide), diamond, silicon carbide, and cerium oxide. The particle size and particle size distribution of the abrasive material can be appropriately selected according to the surface shape of the workpiece before and after grinding.

[0061] When performing grinding, a coolant such as water may be supplied to the lower platen 21a and the upper platen 21b as appropriate.

[0062] There are no particular restrictions on the material of the holder 30, and it can be appropriately selected according to the purpose. For example, epoxy resin reinforced by mixing in aramid fibers and glass fibers can be used.

[0063] The thickness of the holder 30 is preferably thinner than the finished thickness of the workpiece in order to prevent it from coming into contact with the upper platen 21b and hindering the grinding process.

[0064] When operating the grinding machine 40, the upper rotating shaft 46b in Figure 2 is rotated in one direction, causing the upper platen 21b to rotate in the same direction. The lower rotating shaft 46a in Figure 2 is rotated in the opposite direction to the rotation of the rotating shaft 46b, causing the lower platen 21a to rotate in the same direction as the rotating shaft 46a. As a result, the teeth 42 of the lower platen 21a and the central sun gear 44 rotate in the same direction as the rotating shaft 46a. By rotating the upper platen 21b, the lower platen 21a, and the sun gear 44, the holder 30 that meshes with these gears and the workpiece fitted into the holder 30 perform what is known as planetary motion, a combination of rotation and revolution. In this way, the workpiece can be ground with greater precision and speed.

[0065] <Inner and Outer Circumferential Grinding Process> The inner and outer circumferential grinding process is a process of grinding the inner and outer surfaces of openings in a steatite sintered body having a disc shape. The inner and outer circumferential grinding process can be suitably carried out by an inner and outer circumferential grinding means that grinds the inner and outer surfaces of openings in a steatite sintered body having a disc shape.

[0066] The inner and outer circumference grinding process is preferably performed after the grinding process and before the inner circumference polishing process and the outer circumference polishing process, which will be described later.

[0067] Figure 3 is a schematic perspective view showing an example of the structure of an internal and external grinding machine 45 that performs the internal and external grinding process. The internal and external grinding process is a process of rough grinding the inner and outer surfaces 13 of the opening 12 in a workpiece 10 which has a disc shape.

[0068] In the inner and outer circumferential grinding process, it is preferable to grind the inner surface of the opening 12 and the outer surface 13 in parallel. Specifically, the inner surface of the opening 12 located in the center of the workpiece 10 is ground with an inner grinding wheel 22, and the outer surface 13 of the workpiece 10 is ground with an outer grinding wheel 23. At this time, the inner and outer surfaces of the workpiece 10 are sandwiched between the inner grinding wheel 22 and the outer grinding wheel 23 during processing. This makes it easier to ensure the concentricity between the inner and outer diameters of the workpiece 10.

[0069] The inner grinding wheel 22 and the outer grinding wheel 23 have a wavy surface. Therefore, the inner and outer surfaces 13 of the opening 12 of the workpiece 10 can be ground. In addition, it is possible to chamfer the edges of the opening 12 and the outer surface 13 of the workpiece 10 at the same time.

[0070] <Inner Circumference Polishing Process> The inner circumference polishing process is a process of polishing the inner circumferential surface of the opening in the steatite sintered body obtained by the inner and outer circumference grinding process to make it smoother. The inner circumference polishing process can be suitably carried out by an inner circumference polishing means that polishes the inner circumferential surface of the opening in the steatite sintered body obtained by the inner and outer circumference grinding process to make it smoother.

[0071] The inner circumference polishing process is preferably performed after the inner and outer circumference grinding process described above. However, the inner circumference polishing process may also be performed before or after the outer circumference polishing process, which will be described later.

[0072] Figure 4 is a schematic perspective view showing an example of the structure of an inner circumference polishing machine 46 that performs the inner circumference polishing process. First, the workpieces 10 are stacked and set in a holder (not shown), and a brush 24 is inserted into the center of the opening 12 of the workpiece 10. Then, while pouring polishing fluid into the opening 12 of the workpiece 10, the brush 24 is rotated at high speed to polish the inner circumference surface of the workpiece 10 to a smoother surface. In this way, the inner circumference surface of the workpiece 10 is polished to a smoother surface, and the chamfered edges of the opening 12 that were removed in the inner circumference grinding process are also polished in the same way.

[0073] The brush 24 used in the inner circumference polishing process is not particularly limited as long as it is capable of polishing the inner surface of the opening 12 of the workpiece 10, and can be appropriately selected according to the purpose.

[0074] There are no particular restrictions on the polishing fluid used in the inner circumference polishing process, and it can be appropriately selected according to the purpose. For example, a slurry dispersion liquid obtained by dispersing alumina abrasive particles in water can be used.

[0075] <Outer Surface Polishing Process> The outer surface polishing process is a process of polishing the outer surface of the steatite sintered body obtained by the inner and outer surface grinding process to make it smoother. The outer surface polishing process can be suitably carried out by an outer surface polishing means that polishes the outer surface of the steatite sintered body obtained by the inner and outer surface grinding process to make it smoother.

[0076] The outer circumference polishing process is preferably performed after the inner circumference grinding process. However, the outer circumference polishing process may also be performed before or after the inner circumference polishing process.

[0077] Figure 5 is a schematic perspective view showing an example of the structure of an outer perimeter polishing machine 47 that performs the outer perimeter polishing process. First, a jig 25 is passed through the opening of the workpiece 10 and the workpieces are stacked and set. Then, while pouring polishing fluid onto the outer perimeter surface 13 of the workpiece 10, a brush 26 is brought into contact with the stacked workpiece 10 and rotated at high speed. This makes it possible to polish the outer perimeter surface of the workpiece 10 to a smoother surface. In this way, the outer perimeter surface of the workpiece 10 is polished to a smoother surface, and the chamfered edges of the outer perimeter surface 13 that were removed in the inner and outer perimeter grinding process are also polished in the same way.

[0078] The brush 26 used in the inner circumference polishing process is not particularly limited as long as it is capable of polishing the outer circumference surface 13 of the workpiece 10, and can be appropriately selected according to the purpose.

[0079] There are no particular restrictions on the polishing fluid used in the outer surface polishing process, and it can be appropriately selected according to the purpose. For example, a slurry dispersion liquid obtained by dispersing alumina abrasive particles in water can be used.

[0080] <Polishing Process> The polishing process is a process of polishing the surface of the steatite sintered body after various grinding and polishing processes. The polishing process can be suitably carried out by polishing means for polishing the surface of the steatite sintered body.

[0081] Here, the polishing process will be explained in detail using Figure 6.

[0082] Figure 6 is a schematic perspective view showing an example of the structure of a polishing machine used for the polishing process. In the polishing process, the surface of the workpiece 10, which has undergone various grinding and polishing processes, is polished using the polishing machine 50 to further improve its smoothness.

[0083] As long as the polishing machine 50 can polish the surface of the workpiece 10 to a smooth finish, there are no particular restrictions, and it can be appropriately selected according to the purpose.

[0084] The polishing machine 50 has a configuration almost identical to that of the grinding machine 40 shown in Figure 2. Specifically, the polishing machine 50 comprises a lower platen 21a on which the workpiece 10 is placed, and an upper platen 21b for applying the necessary pressure to press down on the workpiece 10 from above and perform polishing. The workpiece 10 is placed on the lower platen 21a of the polishing machine 50 using a holder, and the workpiece 10 is polished by rotating the upper platen 21b, the lower platen 21a, and the sun gear. When polishing the workpiece 10 with the polishing machine 50, for example, a hard abrasive cloth containing urethane can be used, and a polishing liquid can be used in which the abrasive material is dispersed in water to form a slurry.

[0085] There are no particular restrictions on the abrasive material used in the polishing process; it can be appropriately selected according to the purpose. Examples include granular alumina, diamond, silicon carbide, and cerium oxide. The particle size and particle size distribution of the abrasive material can be appropriately selected according to the surface shape of the workpiece before and after grinding or polishing.

[0086] <Secondary Polishing Process> The secondary polishing process is a process in which the surface of the steatite sintered body is further polished after the polishing process. The secondary polishing process can preferably be carried out by a secondary polishing means that further polishes the surface of the steatite sintered body.

[0087] As a secondary polishing method, for example, the polishing machine 50 shown in Figure 6 can be used. When precisely polishing the workpiece 10 with the polishing machine 50 in the secondary polishing process, for example, a suede-like soft polishing cloth can be used, and a polishing liquid can be used which is a slurry formed by dispersing colloidal silica or the like in a dispersion medium such as water.

[0088] The manufacturing method for a magnetic recording medium substrate of this embodiment may include a cleaning step to remove contaminants such as abrasives. The cleaning step is not particularly limited and can be appropriately selected depending on the purpose. For example, chemical cleaning using chemicals combined with ultrasound is one example.

[0089] (Method for manufacturing a magnetic recording medium) The method for manufacturing a magnetic recording medium according to this embodiment may include a magnetic recording medium formation step, and may also include other steps as necessary.

[0090] There are no particular restrictions on the magnetic recording medium manufactured by the manufacturing method of the magnetic recording medium, and it can be appropriately selected according to the purpose. Examples include conventional magnetic recording media, magnetic recording media used in the heat-assisted method, and magnetic recording media used in the microwave-assisted method.

[0091] In the method for manufacturing a magnetic recording medium in this embodiment, a magnetic recording medium used in the heat-assisted method will be described in detail below with reference to Figure 7.

[0092] Figure 7 is a schematic cross-sectional view showing an example of a magnetic recording medium manufactured by the manufacturing method of the magnetic recording medium of this embodiment.

[0093] The magnetic recording medium shown in Figure 7 has a base layer 2, a magnetic layer 3, a protective layer 4, and a liquid lubricant layer 5 sequentially laminated on both main surfaces of the magnetic recording medium substrate 1, from the magnetic recording medium substrate 1 toward the liquid lubricant layer 5. Furthermore, SiO is present on both sides of the magnetic recording medium substrate 1. 2 SiC, Si 3 N 4 and Al 2 O 3 A heat-resistant film 1a containing the above is provided. Note that the magnetic recording medium substrate 1 is a magnetic recording medium substrate manufactured by the method for manufacturing a magnetic recording medium substrate described above, and redundant descriptions are omitted.

[0094] Figure 7 shows a magnetic recording medium substrate 1 in which each layer is laminated on both sides; however, the magnetic recording medium may also consist of a magnetic recording medium substrate 1 in which each layer is laminated on only one side.

[0095] The shape of the magnetic recording medium is not particularly limited as long as it can be applied to a magnetic recording and playback device, and can be appropriately selected according to the purpose. For example, a disc shape with an opening in the center can be used.

[0096] <Magnetic Recording Medium Formation Process> The magnetic recording medium formation process is a process of forming a magnetic layer or the like on a substrate 1 for a magnetic recording medium. The magnetic recording medium formation process may include a soft magnetic layer formation process, a base layer formation process, a magnetic layer formation process, a protective layer formation process, and a liquid lubricant layer formation process.

[0097] <<Soft Magnetic Layer Formation Process>> The soft magnetic layer formation process is a process of forming a soft magnetic layer on the substrate 1 for magnetic recording media.

[0098] There are no particular restrictions on the method for forming the soft magnetic layer; it can be appropriately selected according to the purpose. For example, general film deposition methods such as sputtering can be used.

[0099] There are no particular restrictions on the sputtering method, and it can be appropriately selected depending on the purpose. Examples include DC (Direct Current) sputtering, DC magnetron sputtering, and RF (Radio Frequency) sputtering.

[0100] When using sputtering as a method for forming a soft magnetic layer, it is preferable to use a target containing the material for forming the soft magnetic layer. Examples of targets containing the material for forming the soft magnetic layer include soft magnetic alloys such as FeCo alloys, CoZrNb alloys, and CoTaZr alloys.

[0101] <<Substrate Formation Process>> The substrate formation process is the process of forming a substrate 2 on the soft magnetic layer. The substrate formation process may include a first substrate formation process, which is the process of forming a first substrate on the soft magnetic layer; a second substrate formation process, which is the process of forming a second substrate on the first substrate; and a third substrate formation process, which is the process of forming a third substrate on the second substrate.

[0102] There are no particular restrictions on the method for forming the underlayer 2, and it can be appropriately selected according to the purpose. For example, general film deposition methods such as sputtering can be used.

[0103] When using the sputtering method as the method for forming the base layer 2, it is preferable to use a target that contains the material for forming the base layer.

[0104] In the first subsoil formation process, there are no particular restrictions on the material used to form the first subsoil, and it can be appropriately selected according to the purpose. For example, a Cr alloy in which a bcc alloy mainly composed of Cr is (100) oriented can be used.

[0105] In the second sublayer formation process, there are no particular restrictions on the material used to form the second sublayer, and it can be appropriately selected according to the purpose. For example, a W alloy in which a bcc alloy mainly composed of W is (100) oriented can be used.

[0106] In the third subsoil formation process, there are no particular restrictions on the material used to form the third subsoil, and it can be appropriately selected according to the purpose. Examples include NaCl-type compounds. Examples of NaCl-type compounds include MgO.

[0107] <<Magnetic Layer Formation Process>> The magnetic layer formation process is a process of forming a magnetic layer 3 on the base layer 2. The magnetic layer 3 is preferably a perpendicular magnetic layer.

[0108] There are no particular restrictions on the method for forming the magnetic layer 3, and it can be appropriately selected according to the purpose. For example, general film deposition methods such as sputtering can be used.

[0109] When using the sputtering method to form the magnetic layer 3, it is preferable to use a target containing the material for forming the magnetic layer 3. There are no particular restrictions on the target containing the material for forming the magnetic layer 3, and it can be appropriately selected according to the purpose, for example, L1 0 Examples include targets containing alloys with a specific structure.

[0110] L1 0 Examples of alloys with a structure include alloys containing Fe or Co and Pt, etc. L1 0 Specific examples of alloys with a structure include FePt-based alloys and CoPt-based alloys.

[0111] From the viewpoint of improving the crystal orientation of the magnetic layer 3, the magnetic recording medium substrate 1, the soft magnetic layer, the underlayer 2, and the magnetic layer 3 are preferably heated in a laminated state during the magnetic layer formation process. As the heating means at this time, known methods such as halogen lamps, lasers, LEDs (light-emitting diodes), high-frequency and microwave electromagnetic waves can be used.

[0112] L1 0 If the FePt alloy with a structure is included, it is preferable to heat it to a high temperature of 400°C or higher in order to regularize it. The magnetic recording medium substrate 1 of this embodiment has excellent heat resistance and can therefore be suitably used in the manufacture of magnetic recording media that include a high-temperature heating process.

[0113] <<Protective layer formation process>> The protective layer formation process is the process of forming a protective layer 4 on the magnetic layer 3.

[0114] There are no particular restrictions on the method for forming the protective layer 4, and general film deposition methods can be used. Examples include the RF-CVD (Radio Frequency-Chemical Vapor Deposition) method, which decomposes a hydrocarbon-containing source gas with a high-frequency plasma to form a film; the IBD (Ion Beam Deposition) method, which ionizes the source gas with electrons emitted from a filament to form a film; and the FCVA (Filtered Cathodic Vacuum Arc) method, which uses a solid carbon target to form a film without using a source gas.

[0115] <<Liquid Lubricant Layer Formation Process>> The liquid lubricant layer formation process is a process of forming a liquid lubricant layer 5 on the protective layer 4.

[0116] The liquid lubricant layer 5 can be formed by applying a fluorine-based lubricant such as a perfluoropolyether using methods such as the dip method and the spin-coat method.

[0117] In the manufacturing method of the magnetic recording medium of this embodiment, a magnetic recording medium substrate manufactured by the manufacturing method for magnetic recording medium substrates is used. Therefore, it is possible to manufacture a magnetic recording medium that can suppress the occurrence of fluttering and perform stable reading and writing.

[0118] In the manufacturing method of the magnetic recording medium of this embodiment, a magnetic recording medium substrate manufactured by a method for manufacturing magnetic recording medium substrates is used. Therefore, the manufacturing cost of the magnetic recording medium can be reduced.

[0119] (Magnetic Recording and Reproducing Device) The magnetic recording and reproducing device of this embodiment comprises a magnetic recording medium and a magnetic head for recording and reproducing information on the magnetic recording medium, and may also include other components as needed. Note that the magnetic recording medium is the same as the magnetic recording medium obtained by the (Method for Manufacturing a Magnetic Recording Medium) described above, so redundant descriptions are omitted.

[0120] Figure 8 is a schematic perspective view showing an example of the structure of the magnetic recording and playback device of this embodiment. The hard disk drive 101, which is a magnetic recording and playback device shown in Figure 8, comprises a magnetic recording medium 111, a media drive unit 123 that drives the magnetic recording medium 111 in the recording direction, a magnetic head 124 including a recording unit and a playback unit, a head movement unit 126 that moves the magnetic head 124 relative to the magnetic recording medium 111, and a recording and playback signal processing unit 128 that processes recording and playback signals from the magnetic head 124.

[0121] In a typical hard disk drive, the magnetic recording medium is 5,000 min -1 The above process is used to achieve high-speed rotation. Therefore, if the mechanical properties of the magnetic recording medium are low, fluttering will increase, making stable reading and writing difficult in the hard disk drive. The magnetic recording medium of this embodiment includes a magnetic recording medium substrate with a high specific modulus of elasticity. Therefore, fluttering in the hard disk drive can be reduced, enabling stable reading and writing in the hard disk drive. Furthermore, since the magnetic recording medium of this embodiment uses an inexpensive magnetic recording medium substrate, it is possible to reduce the cost of the hard disk drive.

[0122] The following are examples of this embodiment, but the scope of this disclosure is not limited to these examples.

[0123] (Example 1) <Preparation of a substrate for magnetic recording media> 50% by mass of MgO powder, SiO 2 The powder was mixed at a ratio of 50% by mass. Next, an acrylic binder was added as an organic binder at a ratio of 19 parts by mass per 100 parts by mass of solid content to prepare a slurry. Subsequently, a sheet-like molded body with an average thickness of 1 mm was produced using the doctor blade method. This molded body was processed to produce a workpiece with an outer diameter of 97 mm, an inner diameter of 25 mm, and a disc shape with an opening approximately in the center. The obtained workpiece was fired using the firing apparatus shown in Figure 1. The firing conditions were N 2 In a gas atmosphere, the maximum temperature was set to 1,300°C, the holding time to 1 hour, the workpiece rotation speed to 1 revolution / minute, and the moving speed to 5 cm / minute.

[0124] The workpieces were subjected to HIP treatment after firing. The HIP treatment was performed in an air atmosphere at a temperature of 1,300°C, a pressure of 150 MPa, and a holding time of 2 hours, after which they were slowly cooled. Subsequently, the surface of the workpieces was treated with silica (SiO₂) using tetraethoxysilane (TEOS) in a spin-on-glass (SOG) process. 2 A film was formed. Specifically, the workpiece was washed with acetone, dried, and then a 10% TEOS solution diluted with ethanol was dropped onto the center of the workpiece. The TEOS film was then spin-coated onto both sides of the workpiece using a spin coater. The conditions at that time were a rotation speed of 2,000 min -1 The rotation time was set to 30 seconds. After drying the workpiece, it was fired at a temperature of 700°C, a heating rate of 5°C / min, and for 30 minutes in air. After firing, the workpiece was slowly cooled.

[0125] The obtained workpieces were subjected to grinding. Specifically, using the grinding machine 40 shown in Figure 2, multiple workpieces held in the opening of the carrier plate were subjected to planetary motion, and both main surfaces were ground using grinding pads provided on the upper and lower platens. At this time, diamond grinding wheels (product name: Trizact, manufactured by Sumitomo 3M) were used as grinding pads. These diamond grinding wheels have an outer dimension of 2.6 mm square for the protrusions, a height of 2 mm, a spacing of 1 mm between adjacent protrusions, an average particle size of diamond abrasive grains of 6 μm, and a diamond abrasive grain content of approximately 15 volume percent in the protrusions, with an acrylic resin used as a binder. In addition, a 4-way type double-sided grinding machine (16B model, manufactured by Hamai Sangyo Co., Ltd.) was used as the grinding apparatus, and the rotation speed of the platen was set to 30 min -1 The processing pressure was set to 110 g / cm². 2 Grinding was performed using water as the grinding fluid, and the amount of material removed from each side of the workpiece was approximately 100 μm.

[0126] Next, inner and outer circumference grinding was performed. Specifically, a lapping machine equipped with an inner circumference grinding wheel and an outer circumference grinding wheel, as shown in Figure 3, was used. While the laminate, consisting of multiple workpieces stacked with spacers in between with their central holes aligned, was rotated around an axis, the workpiece was clamped radially between the inner circumference grinding wheel inserted into the central hole of the workpiece and the outer circumference grinding wheel positioned on the outer circumference. While these inner circumference grinding wheels and outer circumference grinding wheels were rotated in the opposite direction to the laminate, the inner circumference grinding wheel and outer circumference grinding wheel ground the inner circumference end face and outer circumference end face of the workpiece. At this time, the inner circumference grinding wheel and outer circumference grinding wheel used contained 80 volume percent of diamond abrasive grains with an average particle size of 10 μm and used a nickel alloy as a binder. The rotation speed of the inner circumference grinding wheel was set to 1,200 min -1 and the rotation speed of the outer grinding wheel is set to 600 min -1 Then, grinding was performed for 30 seconds.

[0127] Next, inner circumference polishing was performed. Specifically, a polishing machine equipped with an inner circumference polishing brush, as shown in Figure 4, was used. While dripping polishing fluid onto the inner circumference polishing brush, the laminate was rotated around its axis, and the inner circumference polishing brush inserted into the central hole of the workpiece was rotated in the opposite direction to the workpiece while being moved up and down, thereby polishing the inner circumference end surface of the workpiece. At this time, a nylon brush was used for the inner circumference polishing brush, and an alumina slurry was used as the polishing fluid. The rotation speed of the inner circumference polishing brush was set to 300 min. -1 The polishing was performed as follows. The grinding time until the difference between the highest and lowest points of the polished surface was 10 minutes was 10 minutes.

[0128] Next, the outer perimeter was polished. Specifically, a polishing machine equipped with an outer perimeter polishing brush, as shown in Figure 5, was used. While dripping polishing fluid onto the outer perimeter polishing brush, the laminate was rotated around its axis, and the outer perimeter polishing brush was rotated in the opposite direction to the workpiece, polishing the outer perimeter end face of the workpiece. At this time, a nylon brush was used for the outer perimeter polishing brush, and an alumina slurry was used as the polishing fluid. The rotation speed of the outer perimeter polishing brush was set to 100 mins. -1 The polishing was performed as follows. The grinding time until the difference between the highest and lowest points of the polished surface was 10 minutes was 10 minutes.

[0129] Next, polishing was performed. Specifically, as a polishing machine, a 2-stage 4-way type double-sided polishing machine (manufactured by System Seiko Co., Ltd., Model 11B) equipped with a pair of upper and lower surface plates was used to polish the surface of the workpiece. At this time, a suede type (manufactured by Filwel Co., Ltd.) was used as the polishing pad. For the first-stage polishing, an aqueous solution adjusted to an acidic region of pH 1.5 by adding alumina abrasive grains with a D50 of 0.5 μm, a chelating agent and an oxidizing agent was used. For the second-stage polishing, an aqueous solution adjusted to an acidic region of pH 1.5 by adding colloidal silica abrasive grains with a D50 of 30 nm, a chelating agent and an oxidizing agent was used. The polishing time was set to 5 minutes for each stage. The processing pressure between the lower surface plate and the upper surface plate was 110 g / cm 2 . The rotational speed of the lower surface plate and the upper surface plate was 20 min -1 , the polishing amount in the first-stage polishing was set to about 1.5 μm, and the polishing amount in the second-stage polishing was set to about 0.5 μm.

[0130] The obtained substrate for a magnetic recording medium was evaluated by the following methods.

[0131] [Evaluation of Heat Resistance and Specific Modulus of Elasticity] When the heat resistance of the substrate for a magnetic recording medium of Example 1 was evaluated based on the melting point of the substrate for a magnetic recording medium, it was 1,300°C. The specific modulus of elasticity (E / ρ) of the substrate for a magnetic recording medium of Example 1 was 46 GPa·cm 3 / g. The specific modulus of elasticity (E / ρ) of the substrate for a magnetic recording medium is a value obtained by dividing the Young's modulus (E) of the substrate for a magnetic recording medium by the density (ρ). The results are shown in Table 1.

[0132] <Fabrication of Magnetic Recording Medium> Next, an assisted recording medium was manufactured using the obtained substrate for a magnetic recording medium. First, a Co-50at% Ti {Ti content 50 at%, balance Co} film with an average thickness of 50 nm was formed as a first underlayer on the substrate for a magnetic recording medium, and then heated to 200°C. Next, a NiO film with an average thickness of 5 nm was formed as a second underlayer, and then heated to 520°C. Next, as a magnetic layer, (Fe-45at% Pt-5at% Ag)-8mol% SiO with an average thickness of 12 nm 2 -4mol% Cr 2 O 3 {SiO2 in a content of 8 mol%, Cr 2 O 3 in a content of 4 mol%, with the balance (Pt content: 45 at%, Ag content: 5 at%, the balance being an Fe alloy)} film was formed. Next, as a protective layer, a DLC (Diamond-Like Carbon) film having an average thickness of 3 nm was formed. Thereafter, perfluoropolyether having an average thickness of 12 Å as a liquid lubricant layer was applied onto the surface of the DLC film by a dip method, to produce a magnetic recording medium.

[0133] The obtained magnetic recording medium was durable enough for practical use as a medium for an assisted recording type hard disk drive. The fluttering of the obtained magnetic recording medium was evaluated by the following method.

[0134] [Fluttering Evaluation Method] The magnetic recording medium of Example 1 was rotated at 10,000 min -1 , and fluttering generated on the outermost peripheral surface of the magnetic recording medium was measured using a He-Ne laser displacement meter. The results are shown in Table 1.

[0135] (Comparative Examples 1 to 2) Magnetic recording media were produced and evaluated in the same manner as in Example 1, except that glass or an aluminum alloy was used as the material of the substrate for magnetic recording media. The results are shown in Table 1.

[0136]

[0137] The magnetic recording medium of Example 1 was able to reduce fluttering more than the magnetic recording media of the respective comparative examples. Accordingly, it is found that a magnetic recording medium using a substrate for magnetic recording media with enhanced heat resistance and specific elastic modulus can reduce fluttering and perform stable reading and writing operations.

[0138] Since the magnetic recording medium of Example 1 can reduce fluttering, it can be effectively used as a medium for an assisted recording type hard disk drive. Accordingly, the magnetic recording medium, by being provided with a substrate for magnetic recording media having high heat resistance and high specific elastic modulus, makes it possible to obtain an assisted recording type hard disk drive capable of performing stable reading and writing operations.

[0139] (Comparative Example 3) A substrate for a magnetic recording medium was manufactured in the same manner as in Example 1, except that the steatite molded body was not rotated during firing. The resulting steatite sintered body warped, and the grinding time required to reduce the difference between the highest and lowest points of the polished surface to 10 μm or less was 20 minutes. As a result, productivity decreased and costs increased.

[0140] As described above, embodiments of this disclosure have been explained, but these embodiments are provided as examples only and do not limit this disclosure. The embodiments can be implemented in various other forms, and various combinations, omissions, substitutions, or modifications are possible without departing from the spirit of the invention. The embodiments and their variations are included in the scope or spirit of the invention and are included in the scope of the invention and its equivalents as described in the claims.

[0141] The embodiments of the Disclosure disclosed above are, for example, specified by the following embodiments: <1> A method for manufacturing a substrate for a magnetic recording medium, comprising a firing step of firing a steatite molded body having a plate-like shape while rotating it. <2> The method for manufacturing a substrate for a magnetic recording medium according to <1>, wherein the firing step involves firing the steatite molded body while rotating it on a transport member along the transport direction of the steatite molded body, and in the firing step, the steatite molded body is rotated with its end face facing the transport member. <3> The method for manufacturing a substrate for a magnetic recording medium according to <2>, wherein in the firing step, the steatite molded body is supported such that the main surface of the steatite molded body is upright with respect to the transport direction. <4> The method for manufacturing a substrate for a magnetic recording medium according to <3>, wherein in the firing step, the steatite molded body is supported such that the main surface of the steatite molded body is substantially parallel to the direction of gravity. <5> The steatite molded body has a disc shape with an opening in the center, and the firing step is to rotate the steatite molded body by rotating a support member inserted into the opening, as described in any one of <1> to <4>. <6> The firing step is to insert the support member into the opening of a plurality of steatite molded bodies, as described in <5>.

[0142] This application claims priority based on Japanese Patent Application No. 2025-78906, filed with the Japan Patent Office on 9 May 2025, and incorporates all the contents of the said application.

[0143] 1...Substrate for magnetic recording medium 2...Underlayer 3...Magnetic layer 4...Protective layer 5...Liquid lubricant layer 101...Hard disk drive 111...Magnetic recording medium 123...Media drive unit 124...Magnetic head 126...Head movement unit 128...Recording / playback signal processing unit 300...Firing apparatus 301...Steatite molded body 302...Support member 303...Sun gear 304...Teeth 305...Conveyor 306...Jig

Claims

1. A method for manufacturing a substrate for a magnetic recording medium, comprising a firing step of firing a steatite molded body having a plate-like shape while rotating it.

2. The method for manufacturing a substrate for a magnetic recording medium according to claim 1, wherein the firing step involves firing the steatite molded body while rotating it on a transport member along the transport direction of the steatite molded body, and in the firing step, the steatite molded body is rotated with its end face facing the transport member.

3. The method for manufacturing a substrate for a magnetic recording medium according to claim 2, wherein in the firing step, the steatite molded body is supported such that the main surface of the steatite molded body is upright with respect to the transport direction.

4. The method for manufacturing a substrate for a magnetic recording medium according to claim 3, wherein in the firing step, the steatite molded body is supported such that the main surface of the steatite molded body is substantially parallel to the direction of gravity.

5. The method for manufacturing a substrate for a magnetic recording medium according to any one of claims 1 to 4, wherein the steatite molded body has a disc shape with an opening in the center, and the firing step involves rotating the steatite molded body by rotating a support member inserted into the opening.

6. The method for manufacturing a substrate for a magnetic recording medium according to claim 5, wherein the firing step involves inserting the support members into the openings of the plurality of steatite molded bodies.