Noise reduction device and method for manufacturing noise reduction device
The noise reduction device addresses stress-related issues in magnetic cores by integrating a protective member with a synthetic resin structure, ensuring the core's integrity and functionality.
Patent Information
- Application Number
- PCT/JP2026/017337
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2026-05-01
- Publication Date
- 2026-11-12
AI Technical Summary
The process of forming a molded portion on the outer circumferential surface of a magnetic core using insert molding can cause damage or variations in the properties of the magnetic core due to pressure or stress.
A noise reduction device comprising a busbar, an annular magnetic core, a protective member, and a molded member made of synthetic resin, where the protective member is integrated with the magnetic core to shield it from stress during the molding process, using a two-layer protective structure with differing elastic moduli and thermal expansion coefficients to mitigate pressure and thermal stress.
The protective member effectively reduces stress and thermal stress on the magnetic core, preventing damage and maintaining core properties, thereby enhancing the device's durability and performance.
Smart Images

Figure JP2026017337_12112026_PF_FP_ABST
Abstract
Description
Noise reduction device and method for manufacturing noise reduction device
[0001] The present disclosure relates to a noise reduction device and a method for manufacturing the noise reduction device. This application claims priority based on Japanese Patent Application No. 2025-078250 filed on May 8, 2025, and the entire content described in the aforementioned Japanese application is incorporated herein by reference.
[0002] Patent Document 1 discloses a noise filter module in which a conductive bar is inserted through the hollow portion of a hollow cylindrical magnetic core. In the noise filter module disclosed in Patent Document 1, a molded portion is formed on the entire outer peripheral surface of the magnetic core 19 by insert molding using phenol resin, epoxy resin, unsaturated polyester, or the like.
[0003] Japanese Unexamined Patent Publication No. 2016-100618
[0004] A noise reduction device according to one aspect of the present disclosure includes: a bus bar; an annular magnetic core surrounding the bus bar; a protective member covering at least a part of a surface of the magnetic core; and a molded member made of synthetic resin, covering at least a part of a surface of the protective member and configured to be inseparably integrated with the protective member.
[0005] Figure 1A is a perspective view showing a first example of the configuration of the noise reduction device according to the first embodiment. Figure 1B is a perspective view showing a second example of the configuration of the noise reduction device according to the first embodiment. Figure 1C is a perspective view showing a third example of the configuration of the noise reduction device according to the first embodiment. Figure 2 is a front cross-sectional view showing an example of the configuration of the noise reduction device according to the first embodiment. Figure 3 is a plan cross-sectional view showing an example of the configuration of the noise reduction device according to the first embodiment. Figure 4 is a flowchart showing a first example of the manufacturing method of the noise reduction device according to the first embodiment. Figure 5 is a flowchart showing a fourth example of the manufacturing method of the noise reduction device according to the first embodiment. Figure 6 is a flowchart showing a fifth example of the manufacturing method of the noise reduction device according to the first embodiment. Figure 7 is a front cross-sectional view showing an example of the configuration of the noise reduction device according to the second embodiment. Figure 8 is a plan cross-sectional view showing an example of the configuration of the noise reduction device according to the second embodiment. Figure 9 is a flowchart showing a first example of the manufacturing method of the noise reduction device according to the second embodiment. Figure 10 is a flowchart showing a fourth example of the manufacturing method of the noise reduction device according to the second embodiment.
[0006] However, in the noise filter module disclosed in Patent Document 1, during the process of forming a molded portion on the outer circumferential surface of the magnetic core by insert molding, pressure or stress acts on the magnetic core, which may cause damage to the magnetic core or cause variations in the properties of the magnetic core due to the stress.
[0007] According to this disclosure, the magnetic core can be protected from pressure or stress generated during the process of forming a molded member made of synthetic resin that covers the magnetic core.
[0008] The embodiments of this disclosure are outlined below.
[0009] (1) The noise reduction device according to this embodiment comprises a busbar, an annular magnetic core surrounding the busbar, a protective member covering at least a portion of the surface of the magnetic core, and a molded member made of synthetic resin that covers at least a portion of the surface of the protective member and is integrally formed with the protective member. This makes it possible to protect the magnetic core from pressure or stress generated in the process of forming the molded member made of synthetic resin by the protective member.
[0010] (2) In (1) above, the protective member may include a coating member that covers at least a portion of the surface of the magnetic core. This makes it possible to form a protective member by coating at least a portion of the surface of the magnetic core.
[0011] (3) In (1) above, the magnetic core is constructed by winding a strip of magnetic material in a ring shape, and the protective member may include a synthetic resin member impregnated between adjacent strip members. This allows the protective member to protect the inside of the magnetic core as well.
[0012] (4) In (1) above, the protective member may include a resin member that covers at least a portion of the surface of the magnetic core and is separable from the magnetic core. This makes it possible to reduce the pressure or stress generated on the magnetic core through the protective member.
[0013] (5) In (1) above, the protective member may include a synthetic resin member that covers at least a portion of the surface of the magnetic core and is integrally formed with the magnetic core. This makes it possible to increase the strength of the magnetic core with the synthetic resin member.
[0014] (6) In any one of (1) to (5) above, the elastic modulus of the protective member may be lower than the elastic modulus of the molded member. This reduces the pressure or stress generated in the magnetic core due to the deformation of the protective member.
[0015] (7) In any one of (1) to (6) above, the difference between the coefficient of thermal expansion of the protective member and the coefficient of thermal expansion of the magnetic core may be smaller than the difference between the coefficient of thermal expansion of the molded member and the coefficient of thermal expansion of the magnetic core. This makes it possible to reduce the thermal stress generated in the magnetic core.
[0016] (8) In any one of (1) to (5) above, the protective member includes an inner protective member that covers at least a portion of the surface of the magnetic core and an outer protective member that covers at least a portion of the surface of the inner protective member, and the molded member covers at least a portion of the surface of the outer protective member and may be integrally and inseparably configured with the outer protective member. This allows the magnetic core to be protected by a two-layer structure of the inner protective member and the outer protective member.
[0017] (9) In (8) above, the elastic modulus of at least one of the inner protective member and the outer protective member may be lower than the elastic modulus of the molded member. This reduces the pressure or stress generated in the magnetic core by deformation of at least one of the inner protective member and the outer protective member.
[0018] (10) In (9) above, the elastic modulus of the outer protective member may be lower than that of the molded member, and the elastic modulus of the inner protective member may be lower than that of the outer protective member. This reduces the pressure or stress generated in the magnetic core as each of the inner and outer protective members deforms.
[0019] (11) In (8) above, at least one of the difference between the linear expansion coefficient of the inner protective member and the linear expansion coefficient of the magnetic core, and the difference between the linear expansion coefficient of the outer protective member and the linear expansion coefficient of the magnetic core, may be smaller than the difference between the linear expansion coefficient of the molded member and the linear expansion coefficient of the magnetic core. This makes it possible to reduce the thermal stress generated in the magnetic core.
[0020] (12) In (11) above, the difference between the coefficient of thermal expansion of the outer protective member and the coefficient of thermal expansion of the magnetic core may be smaller than the difference between the coefficient of thermal expansion of the molded member and the coefficient of thermal expansion of the magnetic core, and the difference between the coefficient of thermal expansion of the inner protective member and the coefficient of thermal expansion of the magnetic core may be smaller than the difference between the coefficient of thermal expansion of the outer protective member and the coefficient of thermal expansion of the magnetic core. This makes it possible to reduce the thermal stress generated in the outer protective member, the inner protective member and the magnetic core.
[0021] (13) In (12) above, the coefficient of linear expansion of the molded member may be less than three times the coefficient of linear expansion of the magnetic core. This makes it possible to reduce the thermal stress generated in the magnetic core.
[0022] (14) A method for manufacturing a noise reduction device according to this embodiment includes the steps of: arranging a protective member so as to cover at least a portion of the surface of an annular magnetic core; arranging a busbar in the hollow portion of the magnetic core; and filling a liquid synthetic resin so as to cover at least a portion of the surface of the protective member and curing the liquid synthetic resin to form a molded member that is integrally and inseparably configured with the protective member. This makes it possible to protect the magnetic core from pressure or stress generated in the step of forming the molded member made of synthetic resin with the protective member.
[0023] This disclosure can be implemented not only as a noise reduction device having the characteristic configuration described above, or as a method for manufacturing a noise reduction device including characteristic steps, but also as a power conversion device including the noise reduction device, or as a noise reduction method including characteristic steps.
[0024] The embodiments of this disclosure will be described in detail below with reference to the drawings. At least some of the embodiments described below may be combined in any way.
[0025] [1. First Embodiment] [1-1. Configuration of Noise Reduction Device] Figure 1A is a perspective view showing a first example of the configuration of the noise reduction device according to the first embodiment, Figure 1B is a perspective view showing a second example of the configuration of the noise reduction device according to the first embodiment, and Figure 1C is a perspective view showing a third example of the configuration of the noise reduction device according to the first embodiment.
[0026] Figure 1A shows the external configuration of a noise reduction device 10A that reduces normal mode noise. The noise reduction device 10A is configured by attaching a noise filter module 30 to a single busbar 20A. The noise filter module 30 includes a magnetic core and reduces normal mode noise generated on the busbar 20A.
[0027] Figure 1B shows the external configuration of the noise reduction device 10B for reducing common-mode noise. The noise reduction device 10B is configured by attaching a noise filter module 30 to two parallel busbars 20_1B and 20_2B. The noise filter module 30 includes a magnetic core and reduces common-mode noise generated on the busbars 20_1B and 20_2B.
[0028] Figure 1C shows the external configuration of a noise reduction device 10C that reduces noise generated in a three-phase AC. The noise reduction device 10C is configured by attaching a noise filter module 30 to three parallel busbars 20_1C, 20_2C, and 20_3C. Busbar 20_1C corresponds to the U phase of the three-phase AC, busbar 20_2C corresponds to the V phase of the three-phase AC, and busbar 20_3C corresponds to the W phase of the three-phase AC. The noise filter module 30 includes a magnetic core and reduces noise generated in busbars 20_1C, 20_2C, and 20_3C.
[0029] The noise reduction devices 10A, 10B, and 10C are installed, for example, in a vehicle. Specifically, the noise reduction devices 10A, 10B, and 10C are placed in a junction box that distributes power from a high-voltage battery to multiple auxiliary devices (inverters, air compressors, heaters, etc.), or are connected to power lines that transmit power supplied to the auxiliary devices. However, the noise reduction devices 10A, 10B, and 10C may also be used for applications other than vehicles. For example, the noise reduction devices 10A, 10B, and 10C may be used in a power supply system that supplies power to electrical equipment in a factory or house.
[0030] The following description will represent the configuration of the noise reduction device 10C for three-phase AC, but the configurations of the noise reduction device 10A for normal mode noise and the noise reduction device 10B for common mode noise are the same as those of the noise reduction device 10C.
[0031] Hereinafter, the longitudinal direction of the busbars 20_1C, 20_2C, and 20_3C will be referred to as the "front-to-back direction." It will also be assumed that each of the busbars 20_1C, 20_2C, and 20_3C is positioned horizontally. The horizontal direction perpendicular to the front-to-back direction will be referred to as the "left-to-right direction." Here, "right" refers to the right when facing backward, and "left" refers to the left when facing backward. The direction perpendicular to both the front-to-back and left-to-right directions will be referred to as the "up-and-down direction." However, these directions are merely for convenience based on the illustrated state and do not limit the directions.
[0032] Figure 2 is a front cross-sectional view showing an example of the configuration of a noise reduction device according to the first embodiment, and Figure 3 is a plan cross-sectional view thereof. That is, Figure 2 shows a cross-sectional view when the noise reduction device 10C is cut by a plane perpendicular to the front-rear direction, and Figure 3 shows a cross-sectional view when the noise reduction device 10C is cut by a plane perpendicular to the up-down direction.
[0033] As shown in Figures 2 and 3, the noise filter module 30 includes a first molded member 31, a protective member 32, a second molded member 33, and a magnetic core 40.
[0034] Each of the busbars 20_1C, 20_2C, and 20_3C is made of a plate-shaped conductive material such as copper, aluminum, or brass, and can carry a large current. Although not shown in the diagram, terminals are formed at both ends of each of the busbars 20_1C, 20_2C, and 20_3C. Other busbars or power lines are connected to the terminals at both ends of the busbars 20_1C, 20_2C, and 20_3C.
[0035] The first molded member 31 is attached to the busbars 20_1C, 20_2C, and 20_3C. Specifically, the first molded member 31 has a front cross-section (cross-section perpendicular to the front-to-back direction) that is elongated in the vertical direction, such as an ellipse, oblong, or rectangular shape with rounded corners, and extends in the front-to-back direction. The first molded member 31 is attached to the busbars 20_1C, 20_2C, and 20_3C such that each of the busbars 20_1C, 20_2C, and 20_3C penetrates the first molded member 31. In the following description, the front cross-sectional shape of the first molded member 31 will be assumed to be an oblong shape that is elongated in the vertical direction.
[0036] The first molded member 31 is made of a synthetic resin which is an insulator. The first molded member 31 holds the busbars 20_1C, 20_2C, and 20_3C in a fixed position, with each of the busbars 20_1C, 20_2C, and 20_3C separated from each other. This ensures a sufficient creepage distance between the busbars 20_1C, 20_2C, and 20_3C.
[0037] The annular magnetic core 40 surrounds the busbars 20_1C, 20_2C, and 20_3C. The magnetic core 40 is constructed by winding a strip of magnetic material in an annular shape. For example, the magnetic core 40 is a nanocrystalline alloy core. In other examples, the magnetic core 40 is an amorphous core. However, the magnetic core 40 may also be a ferrite core.
[0038] The protective member 32 is attached to the magnetic core 40 so as to cover the surface of the magnetic core 40. More specifically, the protective member 32 is formed in an annular shape that surrounds the periphery of the magnetic core 40. The protective member 32 has a hollow portion, and the first molded member 31, which holds the busbars 20_1C, 20_2C, and 20_3C, is arranged in the hollow portion of the protective member 32.
[0039] In a specific example, the protective member 32 is formed in an annular shape having an oval outer circumference that is elongated in the vertical direction and an oval inner circumference that is also elongated in the vertical direction. The shape and size of the inner circumference of the protective member 32 correspond to the shape and size of the outer circumference of the first molded member 31. That is, the outer circumference of the first molded member 31, which forms an oval shape congruent to the inner circumference of the protective member 32, is in close contact with the entire inner circumference of the oval annular protective member 32 without any gaps.
[0040] The protective member 32 according to the first embodiment includes an inner protective member 32A and an outer protective member 32B. The inner protective member 32A covers the magnetic core 40, and the outer protective member 32B covers the inner protective member 32A. That is, the inner protective member 32A is in contact with all of the outer circumferential surface, inner circumferential surface, front end surface, and rear end surface of the annular magnetic core 40, and the outer protective member 32B is in contact with all of the outer circumferential surface, inner circumferential surface, front end surface, and rear end surface of the annular inner protective member 32A. In other words, the protective member 32 has a two-layer structure consisting of an inner protective member 32A and an outer protective member 32B, with the inner protective member 32A layer (inner layer) in contact with the surface of the magnetic core 40, and the outer protective member 32B layer (outer layer) in contact with the surface of the inner protective member 32A. The outer surface of the first molded member 31 is in contact with a portion of the surface of the outer protective member 32B, specifically with the inner circumferential surface of the annular outer protective member 32B.
[0041] The inner protective member 32A and the outer protective member 32B are each made of synthetic resin. More specifically, the inner protective member 32A and the outer protective member 32B are made of different types of synthetic resin. For example, the outer protective member 32B is a core case that houses the magnetic core 40. The core case may be made of a metal material instead of, or in addition to, synthetic resin. The inner protective member 32A is a cushioning material placed between the outer protective member 32B and the magnetic core 40.
[0042] For example, the inner protection member 32A is a coating member made of a synthetic resin applied to the surface of the magnetic core 40. In this case, the inner protection member 32A can be formed by coating the surface of the magnetic core 40 with a synthetic resin. Note that in FIGS. 2 and 3, the thickness of the inner protection member 32A is enlarged for ease of understanding. For example, when the inner protection member 32A is a coating member, the thickness of the inner protection member 32A may be smaller than that shown in FIGS. 2 and 3.
[0043] In another example, the inner protection member 32A may be a synthetic resin member impregnated between the strip members constituting the magnetic core 40. In a specific example, the inner protection member 32A can be formed by immersing the magnetic core 40 in a liquid synthetic resin, allowing the synthetic resin to penetrate between the strip members of the magnetic core 40 via vacuum suction or the like, and then curing the synthetic resin. For example, by using a synthetic resin with a sufficiently low elastic modulus to exhibit flexibility as the material of the inner protection member 32A, the pressure or stress generated in the magnetic core 40 due to curing of the synthetic resin (the inner protection member 32A) can be reduced.
[0044] In still another example, the inner protection member 32A may be a resin member that is separable from the magnetic core 40. Specifically, the inner protection member 32A is composed of non-woven fabric, sponge, rubber, or the like. In this case, since the inner protection member 32A can be displaced (deformed) relative to the magnetic core 40, the pressure or stress generated in the magnetic core 40 via the inner protection member 32A can be reduced.
[0045] In another example, the inner protective member 32A may be a synthetic resin member that covers the surface of the magnetic core 40 and is integrally formed with the magnetic core 40. In one specific example, the inner protective member 32A can be formed by immersing the magnetic core 40 in a liquid synthetic resin and curing the synthetic resin. Specifically, the inner protective member 32A can be formed by placing the magnetic core 40 inside a container-shaped outer protective member 32B, injecting a liquid synthetic resin into the outer protective member 32B, and curing the synthetic resin (potting). In this case as well, by using a synthetic resin with an elastic modulus low enough to be flexible for the material of the inner protective member 32A, the pressure or stress generated on the magnetic core 40 due to the curing of the synthetic resin (inner protective member 32A) can be reduced.
[0046] The second molded member 33 is attached to the protective member 32 so as to cover its surface. More specifically, the second molded member 33 is formed in an annular shape that covers the outer circumference of the protective member 32. The second molded member 33 has a hollow portion, and the protective member 32 is placed in the hollow portion of the second molded member 33. It is also possible that the second molded member 33 covers a part of the protective member 32, and the protective member 32 is partially exposed.
[0047] In a specific example, the second molded member 33 is formed in an annular shape having an oval outer circumference that is elongated in the vertical direction and an oval inner circumference that is also elongated in the vertical direction. The shape and size of the inner circumference of the second molded member 33 correspond to the shape and size of the outer circumference of the protective member 32, that is, the shape and size of the outer circumference of the outer protective member 32B. In other words, the outer circumferential surface of the outer protective member 32B, which forms a congruent oval shape with the inner circumferential surface of the second molded member 33, is in close contact with the entire inner circumferential surface of the oval annular second molded member 33 without any gaps.
[0048] The second molded member 33 is made of a synthetic resin that is integrally and inseparably formed with the protective member 32, i.e., the outer protective member 32B. In this context, "integrally and inseparably formed" means that the two synthetic resins are connected to each other inseparably without the interposition of a separate component such as an adhesive. For example, when a liquid second synthetic resin comes into contact with a hardened first synthetic resin, the first and second synthetic resins become integrally and inseparably formed when the second synthetic resin hardens.
[0049] The second molded member 33 is a housing of the noise filter module 30 that accommodates the first molded member 31, the protection member 32, and the magnetic core 40.
[0050] The second molded member 33 is made of a synthetic resin of a different type from that of the protection member 32. More specifically, the second molded member 33 is made of a synthetic resin of a different type from each of the inner protection member 32A and the outer protection member 32B. The second molded member 33 may be made of the same type of synthetic resin as the protection member 32. For example, the second molded member 33 may be made of the same type of synthetic resin as either the inner protection member 32A or the outer protection member 32B. For example, the second molded member 33 is made of a synthetic resin of a different type from that of the first molded member 31. The second molded member 33 may be made of the same type of synthetic resin as the first molded member 31.
[0051] The elastic modulus of the second molded member 33 and the elastic modulus of the protection member 32 are different from each other. Specifically, the elastic modulus of the protection member 32 is lower than the elastic modulus of the second molded member 33. For example, the elastic modulus of at least one of the inner protection member 32A and the outer protection member 32B is lower than the elastic modulus of the second molded member. In a more specific example, the elastic modulus of the outer protection member 32B is lower than the elastic modulus of the second molded member 33, and the elastic modulus of the inner protection member 32A is lower than the elastic modulus of the outer protection member 32B. However, the elastic modulus of the inner protection member 32A may be higher than the elastic modulus of the outer protection member 32B. For example, the elastic modulus of the outer protection member 32B may be lower than the elastic modulus of the second molded member 33, and the elastic modulus of the inner protection member 32A may be higher than the elastic modulus of the outer protection member 32B.
[0052] The second molded member 33 is formed by being filled in a liquid synthetic resin state on the outer side of the protection member 32 attached to the magnetic core 40, and then being cured. The second molded member 33 shrinks when cured, whereby pressure or stress acts on the protection member 32, but the protection member 32 with a low elastic modulus deforms, so that the pressure or stress acting on the magnetic core 40 is reduced. Therefore, it is possible to prevent the magnetic core 40 from being damaged or the characteristics of the magnetic core 40 from varying due to stress.
[0053] The coefficient of thermal expansion of the protective member 32 and the coefficient of thermal expansion of the second molded member 33 are different from each other. Specifically, the difference between the coefficient of thermal expansion of the protective member 32 and the coefficient of thermal expansion of the magnetic core 40 is smaller than the difference between the coefficient of thermal expansion of the second molded member 33 and the coefficient of thermal expansion of the magnetic core 40. For example, at least one of the differences between the coefficient of thermal expansion of the inner protective member 32A and the coefficient of thermal expansion of the magnetic core 40, and the difference between the coefficient of thermal expansion of the outer protective member 32B and the coefficient of thermal expansion of the magnetic core 40, is smaller than the difference between the coefficient of thermal expansion of the second molded member 33 and the coefficient of thermal expansion of the magnetic core 40. In a more specific example, the difference between the linear expansion coefficient of the outer protective member 32B and the linear expansion coefficient of the magnetic core 40 is smaller than the difference between the linear expansion coefficient of the second molded member 33 and the linear expansion coefficient of the magnetic core 40, and the difference between the linear expansion coefficient of the inner protective member 32A and the linear expansion coefficient of the magnetic core 40 is smaller than the difference between the linear expansion coefficient of the outer protective member 32B and the linear expansion coefficient of the magnetic core 40. In a more specific example, the difference between the linear expansion coefficient of the inner protective member 32A and the linear expansion coefficient of the magnetic core 40 is less than 30 ppm / °C. The difference between the linear expansion coefficient of the outer protective member 32B and the linear expansion coefficient of the magnetic core 40 may also be less than 30 ppm / °C, and the difference between the linear expansion coefficient of the second molded member 33 and the magnetic core 40 may also be less than 30 ppm / °C.
[0054] Even if, during the formation stage of the second molded member 33, not only the liquid second molded member 33 but also the magnetic core 40 and protective member 32 placed inside the second molded member 33 are heated, the thermal stress acting on the magnetic core 40 can be reduced because the coefficient of linear expansion of the protective member 32 is closer to the coefficient of linear expansion of the magnetic core 40 than that of the second molded member 33.
[0055] [1-2. Method for Manufacturing a Noise Reduction Device] The method for manufacturing a noise reduction device according to the first embodiment will be described below.
[0056] [1-2-1. First Example] Figure 4 is a flowchart showing a first example of a method for manufacturing a noise reduction device according to the first embodiment. The first example is a method for manufacturing a noise reduction device 10C in which the inner protective member 32A is a painted member. Here, the method for manufacturing a noise reduction device 10C for three-phase AC is described as representative, but the methods for manufacturing a noise reduction device 10A for normal mode noise and a noise reduction device 10B for common mode noise are the same as the method for manufacturing a noise reduction device 10C.
[0057] First, the primary insert molding process is performed (step S101). The primary insert molding process is a process of insert molding the first molded member 31. The operator places the busbars 20_1C, 20_2C, and 20_3C into the mold of the first molded member 31 and performs insert molding. As a result, a unit (hereinafter also referred to as the "busbar unit") is formed in which the busbars 20_1C, 20_2C, and 20_3C and the first molded member 31 are integrated.
[0058] Next, the operator places the inner protective member 32A around the magnetic core 40 so as to cover the surface of the magnetic core 40 (step S102). Specifically, the operator applies a liquid synthetic resin to the surface of the magnetic core 40 to form the inner protective member 32A, which is a painted member, on the surface of the magnetic core 40. This forms a unit (hereinafter also referred to as the "primary core unit") in which the magnetic core 40 and the inner protective member 32A are combined. Note that the order of steps S101 and S102 is not limited to this; step S101 may be performed after step S102, or steps S101 and S102 may be performed in parallel (i.e., at least part of the execution time of step S101 and step S102 overlap).
[0059] Next, the operator places the primary core unit inside the outer protective member 32B (step S103). In the first example, the outer protective member 32B is an annular case with a hollow interior, and in step S103, the primary core unit is placed in the hollow part of the outer protective member 32B. This forms a unit (hereinafter also referred to as the "secondary core unit") which is a combination of the primary core unit and the outer protective member 32B.
[0060] The secondary core unit is annular in shape as a whole. The operator places the busbar unit in the hollow part of the annular secondary core unit within the mold of the second molding member 33 (step S104).
[0061] Next, the secondary insert molding process is performed (step S105). The secondary insert molding process is a process of insert molding the second molded member 33. In step S104, the busbar unit and the secondary core unit, which are insert members, are placed in the mold for the second molded member 33. In this state, insert molding of the second molded member 33 is performed. As a result, the second molded member 33 is integrally and inseparably formed on the surface of the outer protective member 32B. With this, the noise reduction device 10C is completed.
[0062] During the secondary insert molding process, when the second molded member 33 is formed, pressure or stress is generated in the protective member 32 positioned inside the second molded member 33. However, because the strength of the magnetic core 40 is improved by the inner protective member 32A, which is a painted member, damage to the magnetic core 40 due to pressure or stress is prevented.
[0063] [1-2-2. Second Example] The second example is a method for manufacturing a noise reduction device 10C in which the inner protective member 32A is a synthetic resin member impregnated between the strip members constituting the magnetic core 40. The second example of the method for manufacturing the noise reduction device 10C will be described below with reference to Figure 4.
[0064] First, the primary insert molding process is performed (step S101). The primary insert molding process is the same as step S101 in the first example.
[0065] Next, the operator places the inner protective member 32A around the magnetic core 40 so as to cover the surface of the magnetic core 40 (step S102). Specifically, the operator applies liquid synthetic resin to the surface of the magnetic core 40 and then vacuums the magnetic core 40 to allow the synthetic resin to penetrate between the strip members of the magnetic core 40. The inner protective member 32A can be formed by curing the synthetic resin that has penetrated between the strip members. This forms a primary core unit in which the magnetic core 40 and the inner protective member 32A are combined.
[0066] Next, the operator places the primary core unit inside the outer protective member 32B (step S103). This step is the same as step S103 in the first example. This forms a secondary core unit in which the primary core unit and the outer protective member 32B are combined.
[0067] The operator places the busbar unit in the hollow portion of the annular secondary core unit within the mold of the second molding member 33 (step S104). This step is the same as step S104 in the first example.
[0068] Next, a secondary insert molding process is performed (step S105). The secondary insert molding process is the same as step S105 in the first example. As a result, the second molded member 33 is integrally formed on the surface of the outer protective member 32B. With this, the noise reduction device 10C is completed.
[0069] During the secondary insert molding process, when the second molded member 33 is formed, pressure or stress is generated in the protective member 32 positioned inside the second molded member 33. However, because the strength of the magnetic core 40 is improved by impregnating the synthetic resin member between the strip members of the magnetic core 40, damage to the magnetic core 40 due to pressure or stress is prevented.
[0070] [1-2-3. Third Example] The third example is a method for manufacturing a noise reduction device 10C in which the inner protective member 32A is a resin member made of nonwoven fabric, sponge, rubber, etc. The third example of the method for manufacturing the noise reduction device 10C will be described below with reference to Figure 4.
[0071] First, the primary insert molding process is performed (step S101). The primary insert molding process is the same as step S101 in the first example.
[0072] Next, the operator places the inner protective member 32A around the magnetic core 40 so as to cover the surface of the magnetic core 40 (step S102). Specifically, the operator places the inner protective member 32A, which is a flexible soft resin member, so as to cover the surface of the magnetic core 40. This forms a primary core unit in which the magnetic core 40 and the inner protective member 32A are combined.
[0073] Next, the operator places the primary core unit inside the outer protective member 32B (step S103). This step is the same as step S103 in the first example. This forms a secondary core unit in which the primary core unit and the outer protective member 32B are combined.
[0074] The operator places the busbar unit in the hollow portion of the annular secondary core unit within the mold of the second molding member 33 (step S104). This step is the same as step S104 in the first example.
[0075] Next, a secondary insert molding process is performed (step S105). The secondary insert molding process is the same as step S105 in the first example. As a result, the second molded member 33 is integrally formed on the surface of the outer protective member 32B. With this, the noise reduction device 10C is completed.
[0076] During the secondary insert molding process, when the second molded member 33 is formed, pressure or stress is generated in the protective member 32 positioned inside the second molded member 33. However, the transmission of pressure or stress to the magnetic core 40 is suppressed by the inner protective member 32A, which is a soft resin material that can be separated from the magnetic core 40, thereby preventing damage to the magnetic core 40 due to pressure or stress.
[0077] [1-2-4. Fourth Example] Figure 5 is a flowchart showing a fourth example of a method for manufacturing a noise reduction device according to the first embodiment. The fourth example is a method for manufacturing a noise reduction device 10C in which the inner protective member 32A is a synthetic resin member formed by potting.
[0078] First, the primary insert molding process is performed (step S111). The primary insert molding process is the same as step S101 described above.
[0079] Next, the operator places the magnetic core 40 inside the outer protective member 32B (step S112). In the fourth example, the outer protective member 32B is an annular case with a hollow interior, and in step S112, the magnetic core 40 is placed in the hollow part of the outer protective member 32B.
[0080] Next, potting is performed (step S113). That is, the operator injects liquid synthetic resin into the interior of the outer protective member 32B and hardens the synthetic resin. As a result, the inner protective member 32A is formed to cover the surface of the magnetic core 40, and a unit (hereinafter also referred to as the "core unit") is formed in which the magnetic core 40, the inner protective member 32A, and the outer protective member 32B are integrated.
[0081] The core unit as a whole is annular. The operator places the busbar unit in the hollow part of the annular core unit within the mold of the second molding member 33 (step S114).
[0082] Next, a secondary insert molding process is performed (step S115). The secondary insert molding process is the same as step S105 described above. As a result, the second molded member 33 is integrally formed on the surface of the outer protective member 32B. With this, the noise reduction device 10C is completed.
[0083] During the secondary insert molding process, when the second molded member 33 is formed, pressure or stress is generated in the protective member 32 placed inside the second molded member 33. However, since the inner protective member 32A, which is a synthetic resin material formed by potting, deforms due to the pressure or stress, damage to the magnetic core 40 is prevented.
[0084] [1-2-5. Fifth Example] Figure 6 is a flowchart showing a fifth example of a method for manufacturing a noise reduction device according to the first embodiment. In the fifth example, a noise reduction device 10C is manufactured by forming a first molded member 31 and a second molded member 33 in a single insert molding process.
[0085] First, the operator places the inner protective member 32A around the magnetic core 40 so as to cover the surface of the magnetic core 40 (step S121). For example, the operator applies a synthetic resin to the surface of the magnetic core 40 to form the inner protective member 32A, which is a painted member, on the surface of the magnetic core 40. In another example, the operator applies a liquid synthetic resin to the magnetic core 40 and uses vacuum suction to form the inner protective member 32A, which is impregnated with synthetic resin between the strip members of the magnetic core 40. In yet another example, the operator places the inner protective member 32A, which is a soft resin member, around the magnetic core 40. This forms a primary core unit in which the magnetic core 40 and the inner protective member 32A are combined.
[0086] Next, the operator places the primary core unit inside the outer protective member 32B (step S122). For example, the outer protective member 32B is an annular case with a hollow interior, and in step S122, the primary core unit is placed in the hollow part of the outer protective member 32B. This forms a secondary core unit by combining the primary core unit and the outer protective member 32B.
[0087] The operator places busbars 20_1C, 20_2C, and 20_3C in the hollow portion of the annular secondary core unit within the molds of the first molding member 31 and the second molding member 33 (step S123).
[0088] Next, the insert molding process is performed (step S124). The insert molding process is a process of insert molding the first molding member 31 and the second molding member 33. In step S123, the insert members, which are busbars 20_1C, 20_2C, 20_3C and the secondary core unit, are placed in the molds for the first molding member 31 and the second molding member 33. In this state, the insert molding of the first molding member 31 and the second molding member 33 is performed. As a result, the first molding member 31 and the second molding member 33 are integrally formed on the surface of the outer protective member 32B. With this, the noise reduction device 10C is completed.
[0089] [2. Second Embodiment] [2-1. Configuration of Noise Reduction Device] The following description will be representative of the configuration of the noise reduction device for three-phase AC, but the configurations of the noise reduction device for normal mode noise and the noise reduction device for common mode noise are the same as those of the noise reduction device for three-phase AC.
[0090] Figure 7 is a front cross-sectional view showing an example of the configuration of a noise reduction device according to the second embodiment, and Figure 8 is a plan cross-sectional view thereof. That is, Figure 7 shows a cross-sectional view when the noise reduction device 50 is cut by a plane perpendicular to the front-rear direction, and Figure 8 shows a cross-sectional view when the noise reduction device 50 is cut by a plane perpendicular to the up-down direction.
[0091] As shown in Figures 7 and 8, the noise filter module 60 includes a first molded member 61, a protective member 62, a second molded member 63, and a magnetic core 70.
[0092] The first molded member 61 is attached to the busbars 20_1C, 20_2C, and 20_3C. Specifically, the first molded member 61 has an elongated oval front cross-section that is long in the vertical direction and extends in the front-to-back direction. The first molded member 61 is attached to the busbars 20_1C, 20_2C, and 20_3C such that each of the busbars 20_1C, 20_2C, and 20_3C passes through the first molded member 61.
[0093] The first molded member 61 is made of a synthetic resin which is an insulator. The first molded member 61 holds the busbars 20_1C, 20_2C, and 20_3C in a fixed position, with each of the busbars 20_1C, 20_2C, and 20_3C separated from each other. This ensures a sufficient creepage distance between the busbars 20_1C, 20_2C, and 20_3C.
[0094] The annular magnetic core 70 surrounds the busbars 20_1C, 20_2C, and 20_3C. The magnetic core 70 is constructed by winding a strip of magnetic material in an annular shape. For example, the magnetic core 70 is a nanocrystalline alloy core. In other examples, the magnetic core 70 is an amorphous core. However, the magnetic core 70 may also be a ferrite core.
[0095] The protective member 62 is attached to the magnetic core 70 so as to cover its surface. More specifically, the protective member 62 is formed in an annular shape that surrounds the magnetic core 70. The protective member 62 has a hollow portion, and the first molded member 61, which holds the busbars 20_1C, 20_2C, and 20_3C, is positioned in the hollow portion of the protective member 62.
[0096] In a specific example, the protective member 62 is formed in an annular shape having an oval outer circumference that is elongated in the vertical direction and an oval inner circumference that is also elongated in the vertical direction. The shape and size of the inner circumference of the protective member 62 correspond to the shape and size of the outer circumference of the first molded member 61. That is, the outer circumference of the first molded member 61, which forms an oval shape congruent to the inner circumference of the protective member 62, is in close contact with the entire inner circumference of the oval annular protective member 62 without any gaps.
[0097] The protective member 62 according to the second embodiment is a single resin member. The protective member 62 may also be a core case made of a metal material instead of, or in addition to, synthetic resin.
[0098] For example, the protective member 62 is a coated member made of synthetic resin painted on the surface of the magnetic core 70. In this case, the protective member 62 can be formed by painting the surface of the magnetic core 70 with synthetic resin. Note that in Figures 7 and 8, the thickness of the protective member 62 is shown to be large for ease of understanding. For example, if the protective member 62 is a coated member, the thickness of the protective member 62 may be smaller than that shown in Figures 7 and 8.
[0099] In other examples, the protective member 62 may be a synthetic resin member impregnated between the strip members constituting the magnetic core 70. In a specific example, the protective member 62 can be formed by immersing the magnetic core 70 in a liquid synthetic resin, allowing the synthetic resin to penetrate between the strip members of the magnetic core 70 by vacuum suction or the like, and then curing the synthetic resin. For example, by using a synthetic resin with a sufficiently low elastic modulus (for example, an elastic modulus low enough to be flexible) as the material for the protective member 62, the pressure or stress generated in the magnetic core 70 due to the curing of the synthetic resin (protective member 62) can be reduced.
[0100] In another example, the protective member 62 may be made of a synthetic resin, such as fluororubber, that has high heat resistance with a heat resistance temperature higher than the temperature at which it was inserted during molding, and also has flexibility (low modulus of elasticity).
[0101] The second molded member 63 is attached to the protective member 62 so as to cover its surface. More specifically, the second molded member 63 is formed in an annular shape that covers the outer circumference of the protective member 62. The second molded member 63 has a hollow portion, and the protective member 62 is placed in the hollow portion of the second molded member 63. It is also possible that the second molded member 63 covers a portion of the protective member 62, leaving the protective member 62 partially exposed.
[0102] In a specific example, the second molded member 63 is formed in an annular shape having an oval outer circumference that is elongated in the vertical direction and an oval inner circumference that is also elongated in the vertical direction. The shape and size of the inner circumference of the second molded member 63 correspond to the shape and size of the outer circumference of the protective member 62. That is, the outer circumference of the protective member 62, which forms an oval shape congruent to the inner circumference of the second molded member 63, is in close contact with the entire inner circumference of the oval annular second molded member 63 without any gaps.
[0103] The second molded member 63 is made of synthetic resin and is integrally and inseparably constructed with the protective member 62.
[0104] The second molded member 63 is a housing for the noise filter module 60, which accommodates the first molded member 61, the protective member 62, and the magnetic core 70.
[0105] The second molded member 63 is made of a different type of synthetic resin than the protective member 62. The second molded member 63 may be made of the same type of synthetic resin as the protective member 62. For example, the second molded member 63 is made of a different type of synthetic resin than the first molded member 61. The second molded member 63 may be made of the same type of synthetic resin as the first molded member 61.
[0106] The elastic modulus of the second molded member 63 and the elastic modulus of the protective member 62 are different. Specifically, the elastic modulus of the protective member 62 is lower than that of the second molded member 63.
[0107] The second molded member 63 is formed by filling the outside of the protective member 62 attached to the magnetic core 70 with liquid synthetic resin, and then curing it. When the second molded member 63 hardens, it shrinks, and this causes pressure or stress to act on the protective member 62. However, because the protective member 62 has a low elastic modulus, it deforms, reducing the pressure or stress acting on the magnetic core 70. This prevents damage to the magnetic core 70 and prevents variations in the properties of the magnetic core 70 due to stress.
[0108] The coefficient of thermal expansion of the protective member 62 and the coefficient of thermal expansion of the second molded member 63 are different from each other. Specifically, the difference between the coefficient of thermal expansion of the protective member 62 and the coefficient of thermal expansion of the magnetic core 70 is smaller than the difference between the coefficient of thermal expansion of the second molded member 63 and the coefficient of thermal expansion of the magnetic core 70.
[0109] Even if, during the formation stage of the second molded member 63, not only the liquid second molded member 63 but also the magnetic core 70 and protective member 62 positioned inside the second molded member 63 are heated, the thermal stress acting on the magnetic core 70 can be reduced because the coefficient of linear expansion of the protective member 62 is closer to the coefficient of linear expansion of the magnetic core 70 than that of the second molded member 63.
[0110] [2-2. Method for Manufacturing a Noise Reduction Device] The method for manufacturing a noise reduction device according to the second embodiment will be described below.
[0111] [2-2-1. First Example] Figure 9 is a flowchart showing a first example of a method for manufacturing a noise reduction device according to the second embodiment. The first example is a method for manufacturing a noise reduction device 50 in which the protective member 62 is a painted member. Here, the method for manufacturing a noise reduction device 50 for three-phase AC is described as representative, but the methods for manufacturing a noise reduction device for normal mode noise and a noise reduction device for common mode noise are the same as the method for manufacturing a noise reduction device 50 for three-phase AC.
[0112] First, the primary insert molding process is performed (step S201). The primary insert molding process is a process of insert molding the first molded member 61. The operator places the busbars 20_1C, 20_2C, and 20_3C into the mold of the first molded member 61 and performs insert molding. As a result, a busbar unit is formed in which the busbars 20_1C, 20_2C, and 20_3C and the first molded member 61 are integrated.
[0113] Next, the operator places the protective member 62 around the magnetic core 70 so as to cover the surface of the magnetic core 70 (step S202). Specifically, the operator applies synthetic resin to the surface of the magnetic core 70, forming the protective member 62, which is a painted member, on the surface of the magnetic core 70. This forms a core unit in which the magnetic core 70 and the protective member 62 are combined. Note that the order of steps S201 and S202 is not limited to this; step S201 may be performed after step S202, or steps S201 and S202 may be performed in parallel (i.e., at least part of the execution time of step S201 and step S202 may overlap).
[0114] The core unit is annular in shape as a whole. The operator places the busbar unit in the hollow part of the annular core unit within the mold of the second molding member 63 (step S203).
[0115] Next, a secondary insert molding process is performed (step S204). The secondary insert molding process is a process of insert molding the second molded member 63. In step S203, the busbar unit and core unit, which are insert members, are placed in the mold for the second molded member 63. In this state, insert molding of the second molded member 63 is performed. As a result, the second molded member 63 is integrally formed on the surface of the protective member 62. With this, the noise reduction device 50 is completed.
[0116] During the secondary insert molding process, when the second molded member 63 is formed, pressure or stress is generated in the protective member 62 positioned inside the second molded member 63. However, because the protective member 62, which is a painted member, improves the strength of the magnetic core 70, damage to the magnetic core 70 due to pressure or stress is prevented.
[0117] [2-2-2. Second Example] The second example is a method for manufacturing a noise reduction device 50 in which the protective member 62 is a synthetic resin member impregnated between the strip members constituting the magnetic core 70. The second example of the method for manufacturing the noise reduction device 50 will be described below with reference to Figure 9.
[0118] First, the primary insert molding process is performed (step S201). The primary insert molding process is the same as step S201 in the first example.
[0119] Next, the operator places the protective member 62 around the magnetic core 70 so as to cover the surface of the magnetic core 70 (step S202). Specifically, the operator applies liquid synthetic resin to the surface of the magnetic core 70 and then vacuums the magnetic core 70 to allow the synthetic resin to penetrate between the strip members of the magnetic core 70. The protective member 62 can be formed by curing the synthetic resin that has penetrated between the strip members. This forms a core unit in which the magnetic core 70 and the protective member 62 are combined.
[0120] The operator places the busbar unit in the hollow portion of the annular core unit within the mold of the second molding member 63 (step S203). This step is the same as step S203 in the first example.
[0121] Next, a secondary insert molding process is performed (step S204). The secondary insert molding process is the same as step S204 in the first example. As a result, the second molded member 63 is integrally formed on the surface of the protective member 62. With this, the noise reduction device 50 is completed.
[0122] During the secondary insert molding process, when the second molded member 63 is formed, pressure or stress is generated in the protective member 62 positioned inside the second molded member 63. However, because the strength of the magnetic core 70 is improved by impregnating the synthetic resin member between the strip members of the magnetic core 70, damage to the magnetic core 70 due to pressure or stress is prevented.
[0123] [2-2-3. Third Example] The third example is a method for manufacturing a noise reduction device 50 in which the protective member 62 is made of a synthetic resin (fluororubber) that has high heat resistance and flexibility (low modulus of elasticity). The third example of the method for manufacturing the noise reduction device 50 will be described below with reference to Figure 9.
[0124] First, the primary insert molding process is performed (step S201). The primary insert molding process is the same as step S201 in the first example.
[0125] Next, the operator places the protective member 62 around the magnetic core 70 so as to cover the surface of the magnetic core 70 (step S202). Specifically, the operator places the protective member 62 made of fluororubber so as to cover the surface of the magnetic core 70. This forms a core unit in which the magnetic core 70 and the protective member 62 are combined.
[0126] The operator places the busbar unit in the hollow portion of the annular core unit within the mold of the second molding member 63 (step S203). This step is the same as step S203 in the first example.
[0127] Next, a secondary insert molding process is performed (step S204). The secondary insert molding process is the same as step S204 in the first example. As a result, the second molded member 63 is integrally formed on the surface of the protective member 62. With this, the noise reduction device 50 is completed.
[0128] During the secondary insert molding process, when the second molded member 63 is formed, pressure or stress is generated in the protective member 62 positioned inside the second molded member 63. However, because the flexible fluororubber protective member 62 deforms due to the pressure or stress, damage to the magnetic core 70 is prevented.
[0129] [2-2-4. Fourth Example] Figure 10 is a flowchart showing a fourth example of a method for manufacturing a noise reduction device according to the second embodiment. In the fourth example, a noise reduction device 50 is manufactured by forming a first molded member 61 and a second molded member 63 in a single insert molding process.
[0130] First, the operator places the protective member 62 around the magnetic core 70 so as to cover the surface of the magnetic core 70 (step S211). For example, the operator applies a synthetic resin to the surface of the magnetic core 70 to form the protective member 62, which is a painted member, on the surface of the magnetic core 70. In another example, the operator applies a liquid synthetic resin to the magnetic core 70 and uses vacuum suction to form the protective member 62, which is impregnated with synthetic resin, between the strip members of the magnetic core 70. This forms a core unit in which the magnetic core 70 and the protective member 62 are combined.
[0131] The operator places busbars 20_1C, 20_2C, and 20_3C in the hollow portion of the annular core unit within the molds of the first molding member 61 and the second molding member 63 (step S212).
[0132] Next, the insert molding process is performed (step S213). The insert molding process is a process of insert molding the first molding member 61 and the second molding member 63. In step S212, the insert members, which are busbars 20_1C, 20_2C, 20_3C and the core unit, are placed in the molds for the first molding member 61 and the second molding member 63. In this state, the insert molding of the first molding member 61 and the second molding member 63 is performed. As a result, the first molding member 61 and the second molding member 63 are integrally formed on the surface of the protective member 62. With this, the noise reduction device 50 is completed.
[0133] [3. Supplementary Notes] The embodiments disclosed herein are illustrative in all respects and are not restrictive. The scope of rights in this disclosure is indicated by the claims rather than the embodiments described above, and includes the meaning of equivalents of the claims and all modifications within that scope.
[0134] 10A, 10B, 10C Noise reduction device 20A, 20_1B, 20_2B, 20_1C, 20_2C, 20_3C Busbar 30 Noise filter module 31 First molded member 32 Protective member 32A Inner protective member 32B Outer protective member 33 Second molded member 40 Magnetic core 50 Noise reduction device 60 Noise filter module 61 First molded member 62 Protective member 63 Second molded member 70 Magnetic core
Claims
1. A noise reduction device comprising: a busbar; an annular magnetic core surrounding the busbar; a protective member covering at least a portion of the surface of the magnetic core; and a molded member made of synthetic resin covering at least a portion of the surface of the protective member and integrally formed with the protective member.
2. The noise reduction device according to claim 1, wherein the protective member includes a coating member that covers at least a portion of the surface of the magnetic core.
3. The noise reduction device according to claim 1, wherein the magnetic core is formed by winding a strip of magnetic material in a ring shape, and the protective member includes a synthetic resin member impregnated between adjacent strip members.
4. The noise reduction device according to claim 1, wherein the protective member includes a resin member that covers at least a portion of the surface of the magnetic core and is separable from the magnetic core.
5. The noise reduction device according to claim 1, wherein the protective member includes a synthetic resin member that covers at least a portion of the surface of the magnetic core and is integrally and inseparably configured with the magnetic core.
6. The noise reduction device according to any one of claims 1 to 5, wherein the elastic modulus of the protective member is lower than the elastic modulus of the molded member.
7. The noise reduction device according to any one of claims 1 to 6, wherein the difference between the coefficient of thermal expansion of the protective member and the coefficient of thermal expansion of the magnetic core is smaller than the difference between the coefficient of thermal expansion of the molded member and the coefficient of thermal expansion of the magnetic core.
8. The noise reduction device according to any one of claims 1 to 5, wherein the protective member includes an inner protective member that covers at least a portion of the surface of the magnetic core, and an outer protective member that covers at least a portion of the surface of the inner protective member, and the molded member covers at least a portion of the surface of the outer protective member and is integrally and inseparably formed with the outer protective member.
9. The noise reduction device according to claim 8, wherein the elastic modulus of at least one of the inner protective member and the outer protective member is lower than the elastic modulus of the molded member.
10. The noise reduction device according to claim 9, wherein the elastic modulus of the outer protective member is lower than that of the molded member, and the elastic modulus of the inner protective member is lower than that of the outer protective member.
11. The noise reduction device according to claim 8, wherein at least one of the difference between the linear expansion coefficient of the inner protective member and the linear expansion coefficient of the magnetic core, and the difference between the linear expansion coefficient of the outer protective member and the linear expansion coefficient of the magnetic core, is smaller than the difference between the linear expansion coefficient of the molded member and the linear expansion coefficient of the magnetic core.
12. The noise reduction device according to claim 11, wherein the difference between the coefficient of thermal expansion of the outer protective member and the coefficient of thermal expansion of the magnetic core is smaller than the difference between the coefficient of thermal expansion of the molded member and the coefficient of thermal expansion of the magnetic core, and the difference between the coefficient of thermal expansion of the inner protective member and the coefficient of thermal expansion of the magnetic core is smaller than the difference between the coefficient of thermal expansion of the outer protective member and the coefficient of thermal expansion of the magnetic core.
13. The noise reduction device according to any one of claims 1 to 12, wherein the coefficient of linear expansion of the molded member is less than three times the coefficient of linear expansion of the magnetic core.
14. A method for manufacturing a noise reduction device, comprising the steps of: arranging a protective member so as to cover at least a portion of the surface of an annular magnetic core; arranging a busbar in the hollow portion of the magnetic core; and filling a liquid synthetic resin so as to cover at least a portion of the surface of the protective member and curing the liquid synthetic resin to form a molded member that is integrally and inseparably composed with the protective member.