Thermoelectric substance of high performance

A Bi-Te-based thermoelectric material with a microstructure of varying crystal grain sizes and dispersed graphene oxide addresses the challenges of porosity and binder-related issues, enhancing electrical conductivity and reducing thermal conductivity for improved thermoelectric performance.

WO2026235222A1PCT designated stage Publication Date: 2026-11-12KOREA INST OF MATERIALS SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2025/006301
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-09
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing Bi-Te-based thermoelectric materials face challenges in achieving high electrical conductivity and low thermal conductivity due to the formation of pores and the presence of organic binders, which hinder practical application and reduce electrical properties.

Method used

A Bi-Te-based thermoelectric material with a microstructure comprising regions of different crystal grain sizes and dispersed graphene oxide (GO) is manufactured using a 3D lamination process without organic binders, allowing for improved electrical conductivity and reduced thermal conductivity.

Benefits of technology

The material exhibits enhanced thermoelectric performance by maintaining electrical conductivity and reducing thermal conductivity, achieving a high thermoelectric performance index (zT) through the use of graphene oxide, which bridges crystal grains and scatters lattice phonons.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2025006301_12112026_PF_FP_ABST
    Figure KR2025006301_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed is a composition for forming a thermoelectric substance, the composition comprising: a thermoelectric material; and an edge-oxidized graphene oxide (in which only the edge portions are selectively oxidized), wherein the edge-oxidized graphene is dispersed in the thermoelectric material.
Need to check novelty before this filing date? Find Prior Art

Description

high-performance thermoelectric materials

[0001] The present invention relates to a high-performance thermoelectric material, and more specifically, to an n-type thermoelectric material comprising a Bi-Te-based sintered body having a region of first crystal grains in which graphene oxide is dispersed and a region of second crystal grains in which graphene oxide is substantially absent and which is larger than the average size of the first crystal grains.

[0002]

[0003] Thermoelectric materials refer to energy conversion materials that generate electrical energy when a temperature difference is applied between their ends and, conversely, generate a temperature difference when electrical energy is applied. Following the discovery of thermoelectric phenomena such as the Seebeck effect, Peltier effect, and Thomson effect in the early 19th century, these materials have been used since the late 1930s, primarily in the United States and Europe, as specialized independent power sources for space and military applications utilizing thermoelectric power generation. Additionally, power generation facilities utilizing waste heat from automobiles, ships, and incinerators are being developed. Furthermore, thermoelectric cooling is widely used in refrigerators, small air conditioning systems, mobile phone heat control, electric vehicle HVAC systems, small computer-related coolers requiring precise temperature control, and cooling devices and heat exchangers for water heaters.

[0004] The power generation and cooling capabilities of thermoelectric materials can be determined through the dimensionless performance index zT = S²σT / κ (S: Seebeck coefficient, σ: electrical conductivity, T: absolute temperature, κ: thermal conductivity). High energy conversion efficiency of a thermoelectric material implies a high performance index zT; to increase the performance index, electrical conductivity and the Seebeck coefficient must be improved, while thermal conductivity must be reduced. In other words, thermoelectric materials require independent control of high electrical conductivity and low thermal conductivity.

[0005] In order to simultaneously satisfy all three factors of the above equation, optimization of thermoelectric performance by temperature is required, and Bi-Te-based materials exhibit the most suitable zT values ​​at temperatures ranging from room temperature to 573K.

[0006] To practically apply thermoelectric materials, thermoelectric devices must be constructed using materials that possess p-type and n-type semiconductor characteristics. However, to date, improvements in the thermoelectric properties of n-type Bi-Te-based thermoelectric materials have not been easily achieved compared to p-type materials. Since the properties of thermoelectric devices tend to converge toward the lower of the two types, the development of n-type thermoelectric materials with improved performance is a requirement that must be addressed for practical application.

[0007] Meanwhile, 3D printing processes are being applied to the production of thermoelectric materials to increase the freedom of shape of the materials and reduce production costs. However, since processes that repeatedly irradiate high heat sources such as lasers cause compositional deformation and many internal defects, especially in Bi-Te-based thermoelectric materials, the extrusion 3D printing technique (Materials Extrusion, ME), which extrudes powder into ink, is known to be the most suitable for the production of thermoelectric materials.

[0008] However, in the case of thermoelectric materials produced by the ME process, if drying and sintering processes are performed after fabricating a three-dimensional shape, a large number of pores inevitably form inside, causing a problem in which electrical properties are significantly reduced.

[0009] In addition, since the ink used in the conventional ME process contains an organic binder for printing and shape retention, the binder remains after sintering, causing various negative effects in terms of the application of thermoelectric materials, such as reduced electrical conductivity and poor mechanical properties due to low relative density, which is hindering the practical application of thermoelectric ink materials.

[0010] Accordingly, it was discovered that the thermoelectric performance of a molded body formed by 3D stacking using an extrusion method with a Bi-Te-based thermoelectric ink mixed with graphene oxide without using an organic binder is improved as the thermal and electrical properties are appropriately tailored with the addition of graphene oxide, and this was derived through an analysis of its microstructure.

[0011] [Prior Art Literature]

[0012] (Patent Document 1) Republic of Korea Registered Patent 10-1292591 B1

[0013] The first objective of the present invention is to provide a thermoelectric material having a microstructure that improves electrical properties and reduces thermal conductivity in order to secure a high thermoelectric conversion performance index of a Bi-Te-based ink-based thermoelectric sintered body.

[0014] The second objective of the present invention is to provide a method for manufacturing a molded body by 3D lamination through an extrusion method while including graphene oxide and without using an organic binder, and a thermoelectric ink used therein.

[0015] The third objective of the present invention is to provide an n-type thermoelectric material comprising a sintered body obtained solely by a process of sintering the molded body without special pressure.

[0016] The fourth objective of the present invention is to provide a Bi-Te-based thermoelectric sintered body having a novel microstructure structure that exhibits excellent thermoelectric properties, comprising graphene oxide.

[0017]

[0018] In a first aspect, the present invention,

[0019] As an n-type thermoelectric material comprising a Bi-Te-based sintered body in which graphene oxide (GO) is dispersed,

[0020] The above sintered body has a microstructure comprising two or more crystal grains of different average sizes, and

[0021] The above microstructure includes a region of first grains having a first average size and a region of second grains having a second size smaller than the first size, and

[0022] Graphene oxide provides a thermoelectric material existing in the region of second crystal grains.

[0023]

[0024] In a second aspect, the present invention,

[0025] A step of preparing a thermoelectric ink by dispersing graphene oxide and alloy powder containing Bi and Te in an organic solvent;

[0026] A step of extruding the above thermoelectric ink to form a 3D laminated body; and

[0027] The method includes the step of sintering the above-mentioned molded body to form an n-type thermoelectric material comprising a Bi-Te-based sintered body in which graphene oxide (GO) is dispersed.

[0028] The above sintered body has a microstructure comprising a region of first crystal grains having a first average size and a region of second crystal grains having a second size smaller than the first size, and

[0029] A method for manufacturing a Bi-Te-based n-type thermoelectric material is provided, wherein graphene oxide exists in the region of second crystal grains.

[0030]

[0031] In the third aspect of the present invention,

[0032] The present invention provides a thermoelectric ink that does not contain an organic or inorganic binder, comprising a mixture of an organic solvent in which an alloy powder containing Bi and Te and graphene oxide (GO) are dispersed.

[0033]

[0034] In one aspect of the present invention, an n-type thermoelectric material is provided in which there are two or more regions with different average grain sizes, and graphene oxide is present in the pore regions generated during the molding and pressureless sintering process, thereby allowing electrical connections to be made without short circuits within the Bi-Te thermoelectric material even if pores are present, so as to maintain electrical conductivity characteristics while increasing the Seebeck coefficient, in addition, the grain size is diversified by the combination of the thermoelectric material powder and graphene oxide, thereby actively scattering lattice phonons and reducing the overall thermal conductivity, so as to significantly increase the thermoelectric performance index.

[0035]

[0036] Figure 1 is a conceptual diagram conceptually showing the microstructure of a thermoelectric material manufactured according to the present invention.

[0037] Figure 2 is a photograph showing the appearance of a thermoelectric material manufactured according to the present invention immediately after 3D printing (left) and after processing the surface following sintering heat treatment (right).

[0038] FIG. 3a is an SEM image of the internal microstructure of Example 1 manufactured according to the present invention.

[0039] Figure 3b is an enlarged SEM image of the small grain region of Figure 3a.

[0040] Figure 4 is an SEM image of the microstructure showing the effect of grain size according to the EOG content.

[0041] Figure 5 shows the results of the electrical conductivity analysis of thermoelectric materials with different EOG contents.

[0042] Figure 6 is a graph showing the change in charge concentration (n) and charge mobility (μ) of thermoelectric materials with different EOG contents.

[0043] Figure 7 shows the results of the Seebeck coefficient analysis of thermoelectric materials with different EOG contents.

[0044] Figure 8 shows the results regarding the relationship between the Seebeck coefficient and charge concentration of thermoelectric materials with different EOG contents.

[0045] Figure 9 shows the results of the thermal conductivity analysis of thermoelectric materials with different EOG contents.

[0046] Figure 10 shows the analysis results of the lattice thermal conductivity of thermoelectric materials with different EOG contents.

[0047] Figure 11 shows the results of the thermoelectric performance index (zT) analysis of thermoelectric materials with different EOG contents.

[0048]

[0049] Preferred embodiments of the present invention are described below. However, embodiments of the present invention may be modified in various different forms, and the scope of the present invention is not limited to the embodiments described below. Furthermore, the following embodiments are provided to more fully explain the present invention to those skilled in the art. Also, throughout the specification, the term "comprising" any component means that, unless specifically stated otherwise, it does not exclude other components but may include additional components.

[0050]

[0051] The first aspect of the present invention will be described.

[0052] The thermoelectric material of the present invention is an n-type thermoelectric material comprising a Bi-Te-based sintered body in which graphene oxide (GO) is dispersed.

[0053] The above Bi-Te-based sintered body may be a Bi-Sb-Te-based sintered body including Bi and Te as elements, and additionally may include at least one of Pb, Cu, and Se in addition to the main elements Bi, Sb, and Te, but the Bi-Te-based sintered body may be composed of Bi2-xSbxTe3 (where x is 0 or more and less than 2), and preferably may have a chemical composition of Bi1.7Sb0.3Te3.0.

[0054]

[0055] The graphene oxide (GO) mentioned above is a concept that includes all oxidized forms of graphene obtained by oxidizing a portion of a two-dimensional planar graphene sheet, and industrially, it may refer to graphene oxide obtained by separating it from graphite through oxidation.

[0056] Meanwhile, in terms of electrical properties, graphene oxide may be edge-oxidized graphene oxide (EOG), in which the interior is not oxidized except for the edges. Compared to general GO, which is entirely oxidized, EOG has superior electrical properties and possesses the characteristic of dispersing better in polar organic solvents, alcohols, and aqueous solutions by having functional groups such as carboxyl or carbonyl groups at the edges.

[0057] In particular, by filling the voids between the crystal grains of the thermoelectric material—that is, the pores inevitably formed within the sintered body formed by sintering after forming a 3D molded body by ink or paste—or by connecting the ends of the crystal grains to each other, a bridging effect can be provided that enables charge transfer between the crystal grains separated by the pores. Accordingly, it is possible to induce an improvement in electrical conductivity without significantly changing the charge density based on faster charge mobility within the thermoelectric material, thereby minimizing the decrease in the Seebeck coefficient.

[0058] Of course, as the amount of pores formed within the material increases, a decrease in electrical conductivity inevitably occurs; however, when an appropriate amount of graphene oxide is added, an increase in electrical conductivity due to the bridging effect occurs, causing a phenomenon where these two effects cancel each other out; thus, it is possible to tailor electrical conductivity through the addition of graphene oxide.

[0059] Edge-oxidized graphene oxide refers to graphene oxide in which only the edge portions are selectively oxidized. As shown in the exemplary and conceptual chemical formula below, it refers to graphene with a two-dimensional planar structure in which only the edges or corner portions are oxidized and primarily carboxylated. In the case of graphene oxide (GO) produced by oxidizing graphene, oxygen is present not only at the edges of the two-dimensional plane but also within the interior due to oxidation. In contrast, EOG exists in a state where only the edge portions are oxidized, and it is known that the electrical properties on the graphene surface are superior to those of simple graphene oxide.

[0060]

[0061] At this time, the graphene oxide in which only the edge portions are selectively oxidized may have the edge portions of the graphene oxidized by 5% to 50%, 5% to 30%, 5% to 10%, 10% to 50%, 10% to 30%, or 30% to 50%. If the graphene oxide is oxidized to less than 5% of the edge portions of the graphene, there is a problem in that the oxidized graphene material is difficult to bond with the thermoelectric material or disperse within the film; if it is oxidized to more than 50%, not only is it difficult to prevent the formation of defects on the surface during edge oxidation, but there is also a problem in that connectivity within the graphene material is broken. Generally, the degree of oxidation of the edge portions and the criteria for referring to the degree of oxidation may vary depending on the method of manufacturing the graphene oxide in which only the edge portions are selectively oxidized. Meanwhile, the above % is based on the number of rings present at the edge.

[0062] In the present invention, the EOG may have an oxygen atom content of, for example, 1-15%, 5-15%, 2-15%, or 5-10%.

[0063] The graphene oxide may be included in an amount of 0.01 to 5 wt%, 0.01 to 1 wt%, 0.01 to 0.2 wt%, 0.02 to 0.15 wt%, 0.02 to 0.12 wt%, 0.02 to 0.1 wt%, or 0.05 to 0.15 wt% with respect to the entire sintered body containing graphene oxide or the raw material forming the thermoelectric material prior to sintering, namely the Bi-Te alloy powder.

[0064] In terms of the electrical conductivity and performance index of the thermoelectric material, graphene oxide can preferably be added in a range of 0.05 to 0.15 weight% or 0.02 to 0.1 weight%, more preferably in a range of 0.08 to 0.12 weight%.

[0065] Although there is no particular reason to limit the content of graphene oxide to the above range, when added at approximately 0.1 wt%, it exhibited a very excellent thermoelectric performance index zT value.

[0066] The above-mentioned sintered body has a microstructure including two or more regions of crystal grains, and, for example, has a region of first crystal grains and a region of second crystal grains.

[0067] The second crystal grains existing in the region of the second crystal grains are regions where crystal grains having a second average size exist, and graphene oxide exists in this region of the second crystal grains, and second crystal grains having a second average size smaller than the first average size of the first crystal grains exist around the graphene oxide.

[0068] When graphene oxide is present in combination with a thermoelectric material, it can hinder atomic movement / diffusion in the direction perpendicular to the graphene plane, thereby inhibiting the free three-dimensional growth of crystal grains, and crystal grains with a relatively small average size are formed around them. Consequently, some of the graphene oxide may be located in the pore regions formed in the microstructure. By strengthening electrical connections, it may prevent the degradation of the electrical properties of the thermoelectric material or even improve them. In one embodiment, the pore may exist in the region of the second crystal grains. In another embodiment, the pore may also exist in the region of the first crystal grains, and graphene oxide may also exist in this pore.

[0069] In other embodiments, graphene oxide may be partially present in the first crystal grain region, but is substantially absent, and the proportion may be 10% or less, 5% or less, or 1% or less of the total graphene oxide.

[0070] In another embodiment, a portion of the graphene oxide may exist across the boundary between the region of the first crystal grains and the region of the second crystal grains. The proportion of the graphene oxide existing at the boundary may be 25%, 15% or less, or 10% or less of the total graphene oxide.

[0071] The average size of the first crystal grains and the second crystal grains may vary depending on the size of the raw powders, but for example, the first crystal grains may be formed in the range of 2 to 10 μm, and the size of the second crystal grains may be formed in the range of 0.1 to 1.5 μm.

[0072] The average size of the first crystal grains may be at least twice as large as the average size of the second crystal grains, and in other embodiments, may be 30%, 50%, 70%, 90%, 100%, or 150% or larger.

[0073]

[0074] A second aspect of the present invention relates to a method for manufacturing a thermoelectric material.

[0075]

[0076] The second aspect of the present invention is

[0077] A step of preparing a thermoelectric ink by dispersing graphene oxide and alloy powder containing Bi and Te in an organic solvent;

[0078] A step of extruding the above thermoelectric ink to form a 3D laminated body; and

[0079] The method includes the step of sintering the above-mentioned molded body to form an n-type thermoelectric material comprising a Bi-Te-based sintered body in which graphene oxide (GO) is dispersed.

[0080] The above sintered body has a microstructure comprising a region of first crystal grains having a first average size and a region of second crystal grains having a second size smaller than the first size, and

[0081] Graphene oxide exists in the region of the second crystal grains and is substantially not present in the region of the first crystal grains,

[0082] This invention relates to a method for manufacturing a Bi-Te-based n-type thermoelectric material.

[0083]

[0084] Meanwhile, a third aspect relates to the thermoelectric ink used in the above-mentioned manufacturing method.

[0085] Thermoelectric ink can contribute to improved thermoelectric properties by not using organic or inorganic binders, particularly organic binders commonly used in the manufacture of thermoelectric ink.

[0086] It not only completely eliminates the presence of impurities that may exist within the thermoelectric material but also reduces the formation of pores that may occur during the firing process of the organic binder, thereby increasing the density of the sintered body and consequently contributing to the improvement of the thermoelectric material's properties.

[0087] The above thermoelectric ink can be prepared by dispersing graphene oxide and Bi-Te alloy powder. Graphene oxide can be manufactured directly or purchased commercially, and Bi-Te alloy powder can be alloyed by mixing Bi raw materials and Te raw materials in a specific ratio and milling. Typically, ball milling can be used for milling, and zirconia balls can be used in a zirconia container for example. For example, milling can be performed under conditions of 100-1000 rpm for 1-24 hours or 6-18 hours, but the milling process may be modified and performed within the scope of knowledge possessed by a person skilled in the art.

[0088] The above organic solvent may be a polar organic solvent, and the polar organic solvent includes, for example, DMF (dimethylformamide), DMSO (dimethyl sulfoxide), DMA (dimethylacetamide), glycerol, and combinations thereof, and may be, for example, a mixture of DMF and glycerol, and the weight ratio of DMF and glycerol may be 1:1 to 6. The solvent may be used to have a suitable viscosity suitable for extrusion, for example, 10 to 50 parts by weight per 100 parts by weight of alloy powder.

[0089] It can be uniformly dispersed by repeatedly mixing using a mixer.

[0090] Afterward, extrusion can be performed, and the product can be transferred to a syringe and dried along with the extrusion. When glycerol is used, due to its high boiling point, drying can be performed over approximately 1 to 12 hours in the range of 200-300 ℃. After drying, the molded body undergoes a predetermined process, and firing can be performed in a hydrogen atmosphere and can be carried out for an appropriate time in the range of 300-800 ℃, preferably in the range of 400-600 ℃, for example, within the range of 1 to 12 hours.

[0091]

[0092] The present invention will be explained in detail below through examples and experimental examples.

[0093] However, the following examples and experimental examples are for the purpose of explaining the present invention, and the content of the present invention is not limited by the following examples and experimental examples.

[0094]

[0095] <Reference Example 1> Bi for Ink Production 1.7 Sb 0.3 Te 3.0 thermoelectric powder manufacturing

[0096] 1) Bi in a zirconia crucible 1.7 Sb 0.3 Te 3.0 Bi, Sb, and Te weighed to match the composition were added, along with zirconia balls equal to twice the weight of the raw materials, and alloying was carried out by ball milling at 360 rpm for 12 hours.

[0097] 2) Alloyed Bi 1.7 Sb 0.3 Te 3.0 After separating the powder from the zirconia balls, the powder with a size of 25 μm or less was separated by sieving and used.

[0098]

[0099] <Example 1> Preparation of Bi-Te thermoelectric material in a non-pressure sintering furnace containing 0.1 wt% EOG

[0100] Step 1: Prepare ink suitable for 3D printed body fabrication

[0101] 1) 0.01 g of EOG was added to 0.4 g of DMF and mixed using an ultrasonic cleaner for 1 hour. The EOG was purchased from Mexplorer (Korea).

[0102] 2) The prepared EOG / DMF solution and 10 g of Bi 1.7 Sb 0.3 Te 3.0 Powder and 1.25 g of glycerol were placed in a container and mixed uniformly using a mixer for 20 minutes.

[0103]

[0104] Step 2: Ink Extrusion and 3D Printing Process Fabrication

[0105] 1) The produced ink was transferred into a syringe and mounted on a 3D printer.

[0106] 2) BST (Bi-Sb-Te) molded bodies were extruded by adjusting process conditions according to the viscosity of the ink and the three-dimensional layered structure.

[0107]

[0108] Step 3: Sintering the 3D-printed body

[0109] 1) The stacked BST was heat-treated in a 250-degree oven in an H2 (hydrogen) atmosphere for 6 hours to remove the organic solvent.

[0110] 2) Afterwards, sintering was performed by heating to 500 ℃ and maintaining for 2 hours.

[0111] 3) After heat treatment, the thermoelectric material was obtained by furnace cooling in an oven.

[0112]

[0113] <Example 2> Bi-Te thermoelectric material produced by pressureless sintering containing 0.2 wt% EOG

[0114] The same process as in Example 1 was followed, but the amount of EOG was changed to 0.02 g.

[0115]

[0116] <Example 3> Bi-Te thermoelectric material produced by pressureless sintering containing 0.3 wt% EOG

[0117] The same process as in Example 1 was followed, but the amount of EOG was changed to 0.03 g.

[0118]

[0119] <Comparative Example 1> Preparation of EOG 0wt% Sample

[0120] The same process as in Example 1 was followed, but without the addition of EOG, to prepare the product.

[0121]

[0122] <Examples 4-6>

[0123] The same process as in Example 1 was followed, but 0.01 to 0.03 g of conventional GO was used instead of EOG.

[0124]

[0125] <Experimental Example 1> Microstructural Analysis of Thermoelectric Material

[0126] To confirm the microstructure of the sintered body, the sintered body obtained through the example was surface-processed, and SEM analysis was performed on the surface.

[0127] Surface processing was performed by mechanical polishing using 2000 grit sandpaper, and the sintered body before and after surface processing is as shown in Fig. 2.

[0128] To confirm the internal microstructure of the sample produced according to the present invention, the fracture surface of the sample was observed using an SEM instrument (JEOL, model name JIB-4601F).

[0129] The fracture surface of the sintered body was analyzed by SEM to obtain an image of the surface microstructure, in which small grain regions and large grain regions exist, as shown in Fig. 3a.

[0130] It was confirmed that large grain regions and small grain regions exist in the actual microstructure, just like the conceptual diagram in Fig. 1.

[0131] The image in Fig. 3b was obtained by magnifying the small grain region, and it can be seen that the EOG surrounds the small crystals. This is understood to mean that while it inhibits crystal growth to form small grain regions, the EOG connects the separated crystals by crossing the pores, thereby providing a new pathway for electron movement. Consequently, this has a favorable effect on electrical conductivity. Charge mobility (μ H It affects ) but charge density (n HIt does not cause significant changes to ). However, if the amount of pores formed within the microstructure is greater, electrical conductivity may not improve even if EOG is added. Nevertheless, along with the grain boundaries formed in various ways due to the multiplexing of grain sizes, phonon scattering between EOG and the grain boundaries occurs actively, ultimately resulting in a decrease in thermal conductivity.

[0132]

[0133] Meanwhile, to examine the effect of EOG content on grain size, cross-sectional SEM images of Examples 1 to 3 and Comparative Example were compared.

[0134] As shown in Figure 4, it can be seen that as the content of EOG increases, the average size of the grains in the small grain region of the grains decreases.

[0135] Small crystal grains are clustered around the EOG, which is understood to be because the atomic diffusion of the thermoelectric material, which should occur freely in three dimensions, is partially delayed by the EOG, preventing rapid crystal grain growth.

[0136]

[0137] <Experimental Example 2> Analysis of Electrical Conductivity of Thermoelectric Materials

[0138] The average electrical conductivity was measured at 25°C intervals in a temperature range of 25 - 200°C, and the results are presented in Fig. 5.

[0139] Electrical conductivity was analyzed for changes with temperature using the NETZSCH SBA 458 Nemesis instrument.

[0140] It was confirmed that the electrical conductivity (σ) of the material with 0.1 wt% EOG added was the best, and the lowest when 0.3 wt% EOG was added. It is understood that an excess amount of EOG hinders the sintering of the material, thereby reducing the electrical conductivity (σ).

[0141] Although small grains surrounding the EOG also form some pores, which is expected to degrade electrical properties, the EOG electrically connects the grains, resulting in the electrical properties being maintained at a specific content (0.1 WT%), as shown in Fig. 5.

[0142] On the other hand, in the case of BST N-type thermoelectric materials with 0.2 or 0.3 wt% EOG added, the electrical conductivity (σ) decreases with temperature compared to PURE BST materials because the decrease in electrical conductivity (σ) due to the formation of small crystal grains and the resulting expansion of the pore region outweighs the electrical connection effect of EOG.

[0143] The reason why electrical conductivity (σ) can be maintained can be confirmed by the fact that, as shown in Fig. 6, when 0.1 wt% of EOG is added, the charge mobility is maintained without decreasing compared to pure BST due to the addition of EOG despite the presence of pores. When 0.2 or 0.3 wt% of EOG is added, the decrease in electrical conductivity is explained because the charge density is maintained at a similar level, but the charge mobility decreases rapidly.

[0144]

[0145] <Experimental Example 3> Analysis of Seebeck Coefficient of Thermoelectric Materials

[0146] The average values ​​of the Seebeck coefficients measured at 25°C intervals in the temperature range of 25 - 200°C were analyzed and presented in Figure 7. The Seebeck coefficient (S) was measured as a function of temperature along with electrical conductivity (σ) using the NETZSCH SBA 458 Nemesis instrument.

[0147] Observing that the Seebeck coefficient (S) of the material has a negative value, it can be confirmed that an n-type thermoelectric material has been fabricated. As EOG was added, the absolute value of the Seebeck coefficient increased, which is understood to be due to EOG combining with the thermoelectric powder to improve the Seebeck coefficient.

[0148] In the case of the Seebeck coefficient (S) (V / K), which is the thermoelectric voltage generated per unit temperature, all samples with added EOG exhibit improved Seebeck coefficients across the entire temperature range compared to PURE BST; this appears to be a general phenomenon where the Seebeck coefficient increases as electrical conductivity (σ) decreases. As shown in Fig. 8, regarding the relationship between the Seebeck coefficient and charge concentration, the effective mass (m d * It can be seen that the case where ) is included in EOG is larger. For this reason, the reason why the Seebeck coefficient (S) is larger than that of PURE BST is explained by the following relationship.

[0149]

[0150] m* : effective mass, n : charge concentration, T : temperature, kB : Boltzmann constant

[0151]

[0152] <Experimental Example 4> Analysis of Thermal Conductivity of Thermoelectric Materials

[0153] The average values ​​of thermal conductivity measured at 25 ℃ intervals in a temperature range of 25 - 200 ℃ were analyzed and presented in Fig. 9.

[0154] Thermal conductivity was calculated by measuring thermal diffusivity using NETZSCH’s LFA-457 instrument and using the specific heat and density values.

[0155] When EOG is included, the 0.1wt% and 0.3wt% EOG samples exhibit lower thermal conductivity values ​​compared to PURE BST across the entire temperature range. In contrast, the sample containing 0.2wt% EOG actually shows higher thermal conductivity than PURE BST.

[0156] The reason for the results shown in Fig. 9 above can be explained by the lattice thermal conductivity in Fig. 10. When 0.2 and 0.3 wt% EOG are added, the lattice thermal conductivity values ​​are calculated to be higher compared to PURE BST. In contrast, the 0.1 wt% EOG sample exhibits the lowest lattice thermal conductivity value. In other words, the decrease in thermal conductivity of the 0.1 wt% EOG content sample can be interpreted as being due to the effective reduction of lattice thermal conductivity.

[0157]

[0158] <Experimental Example 5> Performance index (zT) of the thermoelectric material produced according to the present invention

[0159] Based on the results of Figures 5, 7, and 9 above, the dimensionless performance index zT value according to temperature was calculated as shown in Figure 11. As a result, the 0.1 WT% EOG-added BST material showed high dimensionless performance index values ​​across the entire temperature range and achieved a maximum zT value of approximately 0.7. This figure is the highest result when compared to other N-type materials based on ink-based thermoelectric material manufacturing.

Claims

1. An n-type thermoelectric material comprising a Bi-Te-based sintered body in which graphene oxide (GO) is dispersed, The above sintered body has a microstructure comprising two or more crystal grains of different average sizes, and The above microstructure includes a region of first grains having a first average size and a region of second grains having a second size smaller than the first size, and Graphene oxide exists in the region of the second crystal grains, Thermoelectric material.

2. In Paragraph 1, A thermoelectric material having a first average size of 2 to 10 μm and a second average size of 0.1 to 1.5 μm.

3. In Paragraph 1, The above Bi-Te-based n-type thermoelectric material is a thermoelectric material having a composition of Bi2-xSbxTe3 (where x is greater than or equal to 0 and less than 2).

4. In Paragraph 1, The above graphene oxide is a thermoelectric material that additionally exists at the boundary between the region of the first crystal grains and the region of the second crystal grains.

5. In Paragraph 1, The above graphene oxide is included in an amount of 0.05 to 0.15 weight% relative to the sintered body, in a thermoelectric material.

6. In Paragraph 1, The above graphene oxide is included in an amount of 0.08 to 0.12 weight% relative to the sintered body, in a thermoelectric material.

7. The thermoelectric material according to claim 1, wherein the graphene oxide comprises edge-oxidized graphene oxide.

8. A thermoelectric material according to claim 1, wherein a portion of the graphene oxide is located in a pore existing in the region of the second crystal grains.

9. A step of preparing a thermoelectric ink by dispersing graphene oxide and an alloy powder containing Bi and Te in an organic solvent; A step of extruding the above thermoelectric ink to form a 3D laminated body; and The method includes the step of sintering the above-mentioned molded body to form an n-type thermoelectric material comprising a Bi-Te-based sintered body in which graphene oxide (GO) is dispersed. The above sintered body has a microstructure comprising a region of first crystal grains having a first average size and a region of second crystal grains having a second size smaller than the first size, and Graphene oxide exists in the region of the second crystal grains and is substantially not present in the region of the first crystal grains, Method for manufacturing a Bi-Te-based n-type thermoelectric material.

10. A method of manufacturing in which the thermoelectric ink according to claim 9 does not contain a binder.

11. A method of manufacturing according to claim 9, wherein the organic solvent comprises a polar organic solvent.

12. A manufacturing method according to claim 9, wherein the sintering is performed at 300 to 800 ℃.

13. A manufacturing method according to claim 9, further comprising a drying step at 200-300 ℃ prior to the sintering.

14. A manufacturing method according to claim 9, wherein the sintering is performed in a hydrogen atmosphere.

15. A method of manufacturing according to claim 9, wherein the graphene oxide is mixed in a ratio of 0.01 to 1 weight% with respect to the alloy powder.

16. A method of manufacturing according to claim 9, wherein the alloy powder further comprises Sb.