PEM water electrolyzer MEA with unique platinum OER and hydrogen recombination catalyst layer

A large grain-size, low surface area platinum catalyst placed between the anode catalyst layer and porous transport layer in PEM electrolyzers addresses iridium scarcity and inefficiencies, enhancing durability and efficiency by acting as an oxygen evolution reaction catalyst and hydrogen recombination catalyst.

WO2026235732A2PCT designated stage Publication Date: 2026-11-12CALIFORNIA CATALYSTS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/US2025/046599
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-09-16
Filing Date
2025-09-16
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing PEM electrolyzers face challenges with iridium scarcity, high cost, and inefficiencies due to reduced iridium content leading to lower product lifetime, increased hydrogen crossover, and decreased conductivity, necessitating a more durable and abundant catalyst.

Method used

Employing a large grain-size, low surface area platinum catalyst with low oxygen affinity, placed between the anode catalyst layer and porous transport layer, which acts as an oxygen evolution reaction catalyst and hydrogen recombination catalyst, reducing iridium usage and enhancing conductivity.

Benefits of technology

The platinum catalyst extends the lifetime of PEM electrolyzers, prevents explosive hydrogen-oxygen mixtures, and maintains efficiency even at higher voltages, addressing iridium scarcity and cost issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2025046599_12112026_PF_FP_ABST
    Figure US2025046599_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The disclosure provides a platinum catalyst with large grain size, chemically reduced surfaces, and low oxophilicity which is placed on the porous transport layer or an anode catalyst layer within a membrane electrode assembly (MEA) of a proton exchange membrane (PEM) electrolyzer. This material catalyzes hydrogen recombination, enhances conductivity, and at higher voltages, supports the oxygen evolution reaction (OER).
Need to check novelty before this filing date? Find Prior Art

Description

Attorney Docket No. 00172-005W01PEM WATER ELECTROLYZER MEA WITH UNIQUE PLATINUM OER AND HYDROGEN RECOMBINATION CATALYST LAYERCROSS REFERENCE TO RELATED APPLICATIONS

[0001] This application claims priority under 35 U. S. C. §119 (e) to U. S. Provisional Application No. 63 / 695, 119, filed September 16, 2024, the disclosures of which are incorporated herein by reference for all purposes.FIELD OF THE INVENTION

[0002] The invention relates to the field of hydrogen production by water electrolysis, in particular a hydrogen production method by water electrolysis using a proton exchange membrane. The invention further relates to electrolysis catalyst materials and their placement within a membrane electrode assembly.BACKGROUND

[0003] Electrolyzers are classified according to the nature of the electrolyte employed. Most common water electrolysis hydrogen production technologies utilize one of three main technologies: alkaline water, proton exchange membrane (PEM), and solid oxide ceramic. The most promising technology for green energy-utilizing electrolyzers is a proton conducting polymeric membrane ( e. g.Nafion™), in which the membrane is electronically insulating yet conducts ions. This is because PEM technology is more tolerant of an intermittent energy supply such as found in solar, wind, and other green sources of energy. In PEM electrolyzers, water is split at the anode producing hydrogen ions (i. e., protons ) and oxygen gas. The hydrogen ions are transported across a proton exchange membrane to the cathode where they are reduced to hydrogen gas and collected. Catalysts increase the efficiency of the device by decreasing the energy required to perform the oxidation and reduction processes.SUMMARY

[0004] The disclosure provides a large grain-size, low surface area platinum catalyst with chemically reduced surfaces exhibiting low oxygen affinity. In one embodiment, the catalyst has a grain diameter of about 3-50 nm ( e. g., 5-10 nm, 10-40 nm, 20-30 nm or any value between the foregoing ranges ). In another embodiment, the catalyst has a particle diameter or cross section of about 50-1000 nm (e. g., 100-900 nm, 200-800 nm, 300-700 nm, 400-600 nm or anyAttorney Docket No. 00172-005W01value between the foregoing ranges ). In still another embodiment, the particle is irregular in shape. In another embodiment, the oxygen affinity is compared to standard platinum black composition. In another embodiment, the catalyst is layered onto a membrane electrode assembly between an anode catalyst layer (ACL) and porous transport layer (PTL). Such particles go counter to what is taught in the literature about catalysts, and the placement of such layers goes counter to what is taught about hydrogen recombination layers. The surprising result taught in this disclosure is that larger particles of Pt with low oxygen affinity are favorable.Additionally, placement of the unique Pt layer between the ACL and porous transport layer provides benefit.

[0005] The catalyst of the disclosure and its placement within the MEA convey at least three benefits: Firstly, placing the unique platinum particles between the anode catalyst layer (ACL) and porous transport layer increases the conductive interface between the ACL and the electrode. The placement permits less iridium to be used in the ACL since the iridium ( Ir) does not need to act as both an OER catalyst and a charge carrier. As the amount of Ir is decreased, the percolated conductive network throughout the device is interrupted, so another conductive material (more abundant and cheaper - such as the Pt material of the disclosure) must fill the gaps. Secondly, the unique platinum material placed "downstream" of the anode is capable of catalyzing the oxidation of any fugitive hydrogen that has crossed the membrane and might contaminate the oxygen stream. This avoids the formation of explosive mixtures in the produced oxygen stream. Thirdly, the unique platinum material can assume the role of OER catalyst once all the Ir material is passivated or degraded. This will require a rise in operating voltage, which can be automated. The inefficiencies of working at a higher voltage to keep the electrolyzer producing are offset by the longer duty cycle and delayed replacement of an MEA module. The unique reduced-surface Pt material taught herein is useful because platinum OER catalysts utilize a metallic Pt surface that is more immune to oxidation since metallic platinum (0) is the active phase in the OER.Attorney Docket No. 00172-005W01

[0006] The disclosure provides a membrane electrode assembly (MEA) device for water splitting comprising a cathode; an anode; a cathode current collector in contact with the cathode; an anode current collector in contact with the anode; a hydrogen evolution reaction (HER) cathode-catalyst layer (CCL) on the cathode; an anode catalyst layer (ACL) on the anode; and a proton exchange membrane (PEM) electrolyte placed between the cathode catalyst layer (CCL) and the anode catalyst layer (ACL); wherein the ACL comprises a large grain-size, low surface area platinum (LGLS-Pt) catalyst with chemically reduced surfaces exhibiting low oxygen affinity. In one embodiment, the ACL is directly contacting a membrane. In a further embodiment, the LGLS-Pt catalyst is applied to a titanium, stainless steel, or membrane by a method selected from the group consisting of spray deposition, slot die coating, and blade coating. In still another or further embodiment, the LGLS-Pt catalyst acts as an oxygen evolution reaction catalyst or a hydrogen recombination catalyst. In yet another or further embodiment, the LGLS-Pt catalyst has a grain diameter size of about 3-50 nm or a particle size of about 50-1000 nm. In another embodiment, the device further comprises a current collector. In a further embodiment, the current collector is a graphite plate or a titanium bipolar plate.

[0007] The disclosure also provides an electrode assembly device comprising a porous transport layer device having a large grainsize, low surface area platinum (LGLS-Pt) catalyst with chemically reduced surfaces exhibiting low oxygen affinity. In one embodiment, the LGLS-Pt catalyst acts as an oxygen evolution reaction catalyst or a hydrogen recombination catalyst. In another embodiment, the LGLS-Pt catalyst has a grain diameter size of about 3-50 nm or a particle size of about 50-1000 nm.

[0008] The disclosure provides an anode catalyst layer (ACL) device comprising a large grain-size, low surface area platinum (LGLS-Pt) catalyst with chemically reduced surfaces exhibiting low oxygen affinity. In one embodiment, the ACL device comprises an anode comprising titanium or stainless steel. In another embodiment, the ACL device is directly contacting a membrane. In yet another or further embodiment, the LGLS-Pt catalyst is applied to the anode or membrane by a method selected from the group consisting of sprayAttorney Docket No. 00172-005W01deposition, slot die coating, and blade coating. In still another or further embodiment, the LGLS-Pt catalyst acts as an oxygen evolution reaction catalyst or a hydrogen recombination catalyst. In still another or further embodiment, the LGLS-Pt catalyst has a grain diameter size of about 3-50 nm or a particle size of about 50-1000 nm. In another embodiment, the device further comprises a current collector. In a further embodiment, the current collector is a graphite plate or a titanium bipolar plate.

[0009] The disclosure provides a platinum catalyst characterized in that (a) a grain of the catalyst is about 3-30 nm in diameter;(b) a particle of the catalyst is about 50-1000 nm in diameter; (c) particles of the catalyst are irregularly shaped, lack a repeated geometry, are dendritic or any combination thereof; and (d) the catalyst has low oxygen affinity compared to standard platinum black catalysts.

[0010] The disclosure also provides a method of converting platinum oxide to platinum metal, the method comprising disperse a platinum dioxide particular material in an inert media, wherein the inert media is selected from borosilicate glass beads of a diameter of about 3 mm to 212 um or finely ground sodium chloride (NaCl), or a mixture thereof in mass ratios of 5: 1 to 200: 1; and annealing at about 150-400 °C in H2 / Ar or H2 / N2.

[0011] The disclosure also provides a method comprising dissolve a chloroplatinic acid precursor in water and sodium nitrate; heat the chloroplatinic acid precursor solution to about 150 °C for about 50 minutes; heat the chloroplatinic acid precursor solution to about 500 °C for 30 minutes to convert the chloroplatinic acid to platinum dioxide; allow the platinum dioxide to cool; wash the platinum dioxide in water by centrifugation; disperse the platinum dioxide in an inert media, wherein the inert media is selected from borosilicate glass beads of a diameter of about 3 mm to 212 um, or finely ground sodium chloride (NaCl), or a mixture thereof in mass ratios of 5: 1 to 200: 1; and annealing the platinum at about 150-400 ' C in H2 / Ar or H2 / N2.BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1A-B provides schematics of embodiments of the disclosure. (A) provides an exploded view of a membrane electrodeAttorney Docket No. 00172-005W01assembly comprising a layer containing the catalysts of the disclosure. (B) provides an exemplary electrolytic cell embodiment for water splitting.

[0013] Figure 2 is an image of a catalyst sample on a titanium porous transport layer (PTL).

[0014] Figure 3 provides dynamic light scattering (DLS) data showing the large particle size as applied as a protective and recombination coating on the PTL.

[0015] Figure 4 shows the performance of unique chemically-reduced Pt catalyst under 5-bar differential pressure. In this formulation, the catalysts are used as an oxygen evolution reaction catalyst. The cathode is pressurized to 5 bar and the anode is at ambient pressure, leading to increased hydrogen diffusion to the anode side of the cell. The cell is cycled between 1. 6A / cm2and OA and OV to facilitate chemical reactions between the diffused hydrogen species and the catalyst. As shown on this diagram, this Pt-containing catalyst is more robust under these operating conditions due to its chemically reduced surface structure. This chemical reduction of catalyst materials during intermittent operation is a known degradation mechanism for current iridium-based electrolyzers.

[0016] Figure 5 shows the performance data on an 80-micron membrane at 80 °C for the formulation where it is acting as an oxygen evolution reaction catalyst. This data was taken in a PEMWE cell.

[0017] Figure 6 shows redox behavior of conventional, high surface-area and high oxophilicity catalyst referred to conventionally as 'Platinum Black' ) in a PEM water electrolysis cell heated to 80 °C (line "a") and redox behavior of the unique, chemically reduced Pt-formulation under the same conditions (line "b"). The unique formulation generates less current at 1.2V in the forward direction and less current at 0. 8V in the reverse direction. By roughly integrating the positive area under the curve between 0. 6V and 1.35V for both the unique formulation and the platinum black material, an estimate of the total surface oxidative charge passed can be determined. Here, the platinum black formulation passes approximately 7 times the amount of charge within thisAttorney Docket No. 00172-005W01region, indicating a much greater oxophilicity relative to the more inert formulation disclosed here. This result indicates that the unique formulation is more resistant to electrochemical oxidation and reduction.DETAILED DESCRIPTION

[0018] As used herein and in the appended claims, the singular forms "a, " "an, " and "the" include plural referents unless the context clearly dictates otherwise. Thus, for example, reference to "a solar cell" includes a plurality of solar cells and reference to "the material" includes reference to one or more materials and equivalents thereof known to those skilled in the art, and so forth.

[0019] Also, the use of "or" means "and / or" unless stated otherwise. Similarly, "comprise, " "comprises, " "comprising" "include, " "includes, " and "including" are interchangeable and not intended to be limiting.

[0020] It is to be further understood that where descriptions of various embodiments use the term "comprising, " those skilled in the art would understand that in some specific instances, an embodiment can be alternatively described using language "consisting essentially of" or "consisting of. "

[0021] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood to one of ordinary skill in the art to which this disclosure belongs. Although any methods and reagents similar or equivalent to those described herein can be used in the practice of the disclosed methods and compositions, the exemplary methods and materials are now described.

[0022] The word "exemplary" is used throughout this application to mean "serving as an example, instance, or illustration. " Any system, method, device, technique, feature or the like described herein as "exemplary" is not necessarily to be construed as preferred or advantageous over other features.

[0023] A "conductive material" as used herein refers to a material that allows the flow of an electrical current in one or more directions. Materials made of metal are common electrical conductors. Electrical current is generated by the flow of negatively charged electrons, positively charged holes, and positiveAttorney Docket No. 00172-005W01or negative ions in some cases. Examples of conductive materials, include but are not limited to, metals, alloys, metal containing compounds, graphite, and conductive polymers. Examples of good conducting metals include but are not limited to, silver, copper, gold, aluminum, molybdenum, zinc, lithium, tungsten, brass, nickel, iron, palladium, platinum, and tin.

[0024] An "electrocatalyst" as used herein refers to a catalyst that participates in an electrochemical reaction, and which modifies or increases the rate of the electrochemical reaction without being substantially consumed in the process. The electrocatalyst assists in transferring electrons between the electrode and reactants, and / or facilitates an intermediate chemical transformation described by an overall half-reaction.

[0025] An "electrochemical reaction" as used herein refers to a process either caused or accompanied by the passage of an electrons or an electric current and involving in most cases the transfer of electrons between two substances. The energy of an electric current can then be used to bring about many chemical reactions that do not occur spontaneously. Examples of "electrochemical reactions" include the chlorine evolution reaction, the oxygen evolution reaction, the hydrogen evolution reaction, the carbon dioxide reduction reaction, the electrochemical water splitting reaction, the nitrogen reduction reaction, and the oxygen reduction reaction.

[0026] Electrocatalysts are used both to speed up electrode reactions and to enable them to occur close to their thermodynamically predicted potentials. An electrocatalyst is said to reduce the overvoltage for an electrode reaction. An example is the water electrolysis cell; electrocatalysts in these systems lower the minimum voltage necessary for electrolysis to occur, and to keep it low as the rate of electrolysis at the electrodes is increased--this may permit higher efficiency of operation.

[0027] A component of a proton exchange membrane (PEM) electrolyzer is the membrane electrode assembly (MEA), which is essentially composed of five layers. The central layer is the polymer proton-conducting membrane (typically Nafion™). On either side of the membrane are catalyst layers. Each layer contains a catalyst designed for either hydrogen evolution or water oxidation.Attorney Docket No. 00172-005W01Finally, adj acent to each catalyst layer is a porous transport layer. The porous transport layers should be porous and electrically conducting to allow the reactants to flow away from the catalyst layers and to conduct the electrons that are part of the electrochemical reactions.

[0028] PEM water electrolyzers have high power density and excellent load-following capability, which makes them a promising technology for sustainable hydrogen production in the context of large-scale energy storage. However, due to the harsh environment (e. g., low pH, potential > 1. 5V, and high oxygen concentration on the anode) in a PEM system, the choice of electro-catalyst is limited to platinum group metals (PGMs ). Typically, carbon supported platinum (Pt / C) is used for the hydrogen evolution reaction (HER) on the cathode side, while iridium ( Ir) based catalysts are used for the oxygen evolution reaction (OER) on the anode side.

[0029] To date, iridium oxide remains the only viable water oxidation catalyst in PEM water electrolyzers. Every other known catalyst material ( e. g., ruthenium oxide, manganese-based oxides, etc. ) suffer from poor stability, often lasting less than a few days at industrial current densities ( lA / cm2or higher). There is growing concern about the world' s ability satisfy the projected market for green-hydrogen PEM electrolyzers due to the scarcity of iridium. At current projected growth rates, by 2050 hydrogen production in Europe alone will require more iridium than is currently produced worldwide every year. Moreover, iridium mining is geographically concentrated, with South Africa responsible for roughly 90% of global iridium production. This point-source leads to concerns about regional bottlenecks and strategic security of supply.

[0030] Material use-reduction has the most potential to slow the effects of these issues. Use-reduction can mean using less Ir per electrolyzer, using more abundant and geographically diverse replacement materials, or a mix of approaches. At the current scale of production, catalyst cost is only about 5% of a completed PEM electrolyzer. However as systems grow in size, to MW range and beyond, the balance-of-plant costs will drop due to economies of scale and catalyst costs will become a larger fraction of overall cost of a completed PEM unit.Attorney Docket No. 00172-005W01

[0031] There are several responses to the forecasted shortfall in Ir availability: Increase mineral production, decrease the amount used per kilowatt of electrolyzer capacity, or recycle iridium from spent cells. Firstly, iridium is a byproduct of other precious metal mining so increasing production to meet the demand of one small subcomponent of a larger mining operation is unlikely to occur due to both the financial burden of the other extracted metals but also on a historically slow investment response by the mining industry.Secondly, while current iridium recovery rates are reasonable (but can improving), overall recovery of the precious metal is low compared to other minerals due to high process costs. Market pressures will eventually encourage new innovations in precious metal recovery methods, but timing those innovations is impossible and they will likely not be rapid enough to meet forecast demand in the early stages of the hydrogen electrolyzer ramp-up. That leaves reduction of Ir on a per-kilowatt basis as the best option for meeting projected demand. Unfortunately, minimizing the amount of iridium in a PEM system leads to lower product lifetime, less efficient electrochemical reactions, curtailed power density, and lower rate of hydrogen production. These factors increase the total lifetime cost of a system and ultimately drives up the cost of green hydrogen.

[0032] State-of-the-art PEM electrolyzers use unsupported Ir or IrO2catalysts for the OER on the anode. A recent analysis suggests that large-scale application of PEM electrolyzers could be enabled by reducing the Ir loading in an individual MEA down to 0.05 mg of Ir cm-2. This Ir density reduction can be achieved by making the anode layer thinner or by decreasing the amount of Ir, or a combination of approaches. Such drastic reduction of Ir density brings its own problems by increasing resistivity between the anode catalyst layer (ACL) and the porous transport layer, and lowering lifetimes as the scarce catalyst becomes pacified or degraded over time.

[0033] The first problem with using thinner proton-conducting membranes to support reduced Ir is that, while thin membranes can increase efficiency, they can also allow increased hydrogen gas crossover between the cathode and anode sides of the MEA. SafeAttorney Docket No. 00172-005W01operation of PEM electrolyzers relies on effective gas separation by the membranes to avoid the formation of explosive hydrogen / oxygen mixtures. Decreases in the thickness of the membrane mean higher efficiency, but also higher crossover rates. Hydrogen recombination catalysts enable higher efficiency by allowing thinner membranes because they recombine hydrogen with oxygen, thereby reducing the potential for explosive stoichiometry.

[0034] The second problem with reducing Ir content in the ACL is the concomitant lowered conductivity within the porous transport layer. Sufficient Ir metal is needed in the ACL, not only to catalyze the OER, but also to carry the electric current through the MEA. It does this by forming a contiguous network of Ir or IrO2nanoparticles. If reductions in Ir content are implemented, an alternative conductive material will need to be added to the ACL or porous transport layer to ensure conductivity across the membrane.

[0035] The third problem with reducing Ir content in the ACL is the lower lifetime of the expensive membrane assembly due to reduced material that is steadily being passivated or degraded. Given a relentless rate of incapacitation, ACLs with higher catalyst loadings will last longer than alternatives with lower loadings. Particularly in green energy applications, with frequent interruptions in the power supply, catalysts degrade in PEM electrolyzers at an increased rate. This requires an expensive maintenance procedure wherein the unit is taken off-line to replace the MEA with one containing fresh Ir anode material.

[0036] Conventional practice teaches away from the compositions and devices of the disclosure, instead recommending that catalysts be small particles with high surface areas and oxygen rich surfaces. Additionally, the prior art teaches away from the placement of this material as set forth in the disclosure.

[0037] The disclosure provides a large grain-size, low surface area platinum (LGLS-Pt) catalyst with chemically reduced surfaces exhibiting low oxygen affinity that can be layered into a membrane electrode assembly between an ACL and porous transport layer. The LGLS-Pt catalyst material of the disclosure has the unique ability to take over the OER after the Ir catalyst is exhausted, albeit at higher voltages. When running in low capacity-factor applications,Attorney Docket No. 00172-005W01such as when utilizing normally curtailed electrons from wind and solar energy sources, the lower efficiency of the high-voltage backup catalyst is less impactful. In high capacity-factor systems, such in many continuous industry processes, an uninterrupted supply of hydrogen at the highest possible efficiency is most important, even with the cost of higher operating voltages once the LGLS-Pt catalyst takes over, rather than gradually reducing hydrogen output as the ACL Ir catalysts die.

[0038] The placement of the LGLS-Pt catalyst material of the disclosure is also disclosed to be a successful application in the MEA of a PEM electrolyzer. To achieve a solution to all three problems listed above, the LGLS-Pt catalyst material is placed between the ACL and its porous transport layer. Placement, as taught in the prior art, reduces the usefulness of a hydrogen recombination catalyst and limits the functions it can perform.Additionally, the LGLS-Pt particles are not considered by the literature to be stable in the ACL of a PEM electrolyzer making its placement as described herein surprising and against conventional knowledge. The LGLS-Pt catalyst material and layer arrangement described herein solves all three problems described above.

[0039] This disclosure also provides two methods for making the LGLS-Pt material: (i) annealing standard catalysts in a reducing or inert atmosphere and (ii) synthetically through oxidized platinic precursors, optionally followed by annealing in reducing or inert atmosphere. The resulting product is placed into the MEA in three different ways: 1) coated on the porous transport layer; 2) coated onto the anode material; or 3) integrated into the anode material. The LGLS-Pt layer assembly has three favorable traits: 1) it catalyzes recombination of hydrogen that has crossed to the anode side of the MEA; 2) it increases overall conductivity of the anode catalyst layer and PTL to facilitate lower loadings of Ir catalysts; and 3) it acts as an OER catalysts at higher voltages.

[0040] The LGLS-Pt catalyst material, acting as a standalone catalyst can provide a major advantage over Ir-based catalysts in low-capacity factor and low electricity cost scenarios. The LGLS-Pt catalyst material is a highly durable OER catalyst that represents a substantial reduction in cost relative to Iridium, while retainingAttorney Docket No. 00172-005W01its capability as a hydrogen recombination catalyst. Moreover, the LGLS-Pt catalyst material does not have the current or projected supply chain and scarcity issues that will necessitate a reduction in Iridium catalyst loadings. Therefore, the LGLS-Pt catalyst material represents a valuable alternative to iridium, where capital cost reductions and the durability of a system, particularly in response to variable energy input and prolonged "off" periods are crucial to deployment. The LGLS-Pt catalyst material is durable in this system as a standalone catalyst when coated onto the PTL or as the ACL in a catalyst coated membrane.

[0041] The compositions, systems and methods disclosed here allow for much higher efficiency in the OER reaction, while actively preventing the formation of platinum oxides on the surface. Platinum oxidation to PtO and PtO2at high anodic potentials leads to substantially reduced catalytic efficiency and durability. The oxide reduces the conductivity of the catalyst and blocks active sites for both OER and recombination. This oxide then leads to irreversible degradation and device failure that is accelerated upon cycling the electrolyzer on and off (where "on" refers to onset of hydrogen and oxygen production and "off" refers to a full shutdown to OV applied to the cell). The larger particles with low oxophilicity and chemically reduced surfaces, enable this system to replace Iridium-based electrolyzer MEA's and demonstrate an advantage in low-capacity factor installations where powering the electrolyzer completely off is advantageous or even necessary when paired with intermittent renewable energy. The compositions of the disclosure are durable under "full shutoff" conditions, which is unique for PTL coatings and OER catalysts.

[0042] Three methods of synthesis have been developed to produce the large grain-sized, low surface area, low oxophilicity platinum particles. The first synthetic method is by controlled annealing of commercially available platinum (Pt black, high surface area) in a reducing or inert gaseous environment. The second method is by a careful reduction of a platinic precursor such as chloroplatinic acid (available from, e.g., Millipore Sigma, STREM, and the like), through a platinum oxide intermediate, to the low oxophilic platinum particle. Alternatively, the method can be performed by a reduction of a platinic precursor such as potassium tetrachloroplatinate (available from Millipore sigma, STREM and the like) to platinum metal by ascorbic acid. General annealing processes can be found in: Palanisamy et al. General synthetic methods of chloroplatinic acid oxidation can be found in: Voorhees, V. et al. with subsequent reduction described herein (which are incorporated herein by reference for all purposes ).

[0043] For example, in a first method, generation of a stable catalytic phase can proceed through a reducing or inert anneal (e.g., Ar, N2, or a forming gas such as H2 / Ar or H2 / N2blends) at elevated temperature (e.g., about 150-400 °C) for between about 15 minutes and about 4.5 hours. This anneal process can be performed on the Pt powder alone or on the PtO2intermediate before or after it has been applied to the porous current collector used in PEM electrolysis (sintered or fibrous titanium).

[0044] In a second method one can generate the platinum catalysts by reducing an oxidized chloroplatinic acid precursor. Post synthesis, the resulting catalysts may, but do not necessarily need to, undergo thermal treatment as described above ( e.g., about 150-400 °C in H2 / Ar or H2 / N2). During this anneal process, the platinum oxide can be dispersed through inert media. Such inert media can include borosilicate glass beads of a diameter of about 3 mm to 212 um, or finely ground sodium chloride (NaCl), or a mixture of these media and mixed with the platinum oxide in mass ratios of 5: 1 or 200: 1, or any ratio in between. Careful consideration of the mixing enables facile conversion of the platinum oxide to the chemically reduced, low-oxophilicity platinum catalyst while controlling the aggregation and sintering of the particles during formation. This facilitates excellent control over the particle size, shape, and colloidal stability.

[0045] This optional annealing process can also be performed on the powder before or after being applied to the porous transport layer.

[0046] Layer deposition methods can be used to generate electrodes. For example, layers can be synthesized by: (1) spraying an ink of the prepared LGLS-Pt particles suspended in a carrier solvent (such as water, isopropanol, ethanol, or a mixture) on to anAttorney Docket No. 00172-005W01anode porous transport layer with Nation™ ionomer, Aquivion™, or other PEM ionomer, added at 0 - 20 wt %. (2) Spraying onto the anode side of the membrane that faces its porous transport layer an ink as prepared above comprising LGLS-Pt particles suspended in a carrier solvent (such as water, isopropanol, ethanol or a mixture) with Nafion™ ionomer, Aquivion™, or other PEM ionomer, at 0 - 20 wt %. This method thus creates the Anode Catalyst Layer (ACL) of the "catalyst coated membrane" (CCM) and replaces Iridium as a standalone catalyst in this formulation. (3) Application onto the side of the anode catalyst layer that faces its porous transport layer by dry pressing the annealed LGLS-Pt particles onto the anode catalyst layer.

[0047] Figure 1A is an exploded sectional view of a membrane-electrode assembly 5. Referring to Figure 1A, the membrane-electrode assembly 5 includes an anode 20 and a cathode 30 located at opposite sides of a membrane separator 10. The anode 20 includes an anode catalyst layer (ACL) 22, large-grain catalyst layer (LGLS-Pt) 24, a porous transport layer 25, and an optional carbon based material 26. The cathode 30 includes a cathode catalyst layer 32, a porous layer 34, and an optional carbon based material 36. The porous transport layer 25 and the carbon base material 26 can be described as a diffusion layer, and the porous layer 34 and the carbon base material 36 can also be referred to as another diffusion layer. A suitable thickness for the catalyst layer 24 includes, but is not limited to, a thickness greater than 1 nm, or 2 nm and / or less than 10 µm, or 100 µm.

[0048] The anode catalyst layer 22 can include one or more anode catalysts selected to catalyze the half reaction that occurs at the anode. Suitable anode catalysts of the anode catalyst layer 22 include, but are not limited to, oxidation catalysts. When the half reaction at the anode is the oxygen evolution reaction (OER), a suitable anode catalyst layer 22 can include, but is not limited to, FeNiOx, IrOx, RuOx, CoOx and combinations thereof. Typically, the anode catalyst layer 22 will comprise Ir.

[0049] The cathode catalyst layer 32 can include one or more cathode catalysts selected to catalyze the half reaction that occurs at the cathode 30. Suitable cathode catalysts include, but are notAttorney Docket No. 00172-005W01limited to, reduction catalysts. When the half reaction at the cathode 30 is the hydrogen evolution reaction (HER), a suitable cathode catalyst includes, but is not limited to, Pt, Ni, NiPx, CoPx, NiMo, and combinations thereof. When the half reaction at the cathode 30 is a CO2R reaction, a suitable cathode catalyst includes, but is not limited to, Pd, Cu, Cu / Au, Ag, and combinations thereof.

[0050] Figure 1B illustrates a fuels generator showing the half reactions. The illustrated portion of the fuels generator includes an anolyte 11 and a catholyte 12 separated by a membrane separator 10. The anolyte 11 can be a liquid, gas, vapor or a combination thereof. The catholyte 12 can be a liquid, gas, vapor, or a combination thereof. The anolyte 11 and catholyte 12 can each contact the membrane separator 10 or alternatively the anode 20 and cathode 30, respectively. The membrane separator 10 can comprise an ion exchange membrane. The ion exchange membrane can be a cation exchange membrane, an anion exchange membrane or comprise a bipolar membrane ( e.g., both a cation and anion exchange membrane). Figure 1B also illustrates the anode 20 and cathode 30 (see Figure 1A). The anode 20 includes, consists of, or consists essentially of a catalyst of the disclosure (LGLS-Pt) for splitting water, water vapor or other fuel source. Although Figure 1B shows the anode distinct from the membrane separator 10, anode 20 can be in contact with the membrane separator 10. Suitable anionic membranes for use in the methods and compositions of the disclosure include, but are not limited to, polyaromatic polymers, fluorinated polymers functionalized with sulfonic acid groups. An example of a suitable fluorinated polymer functionalized with sulfonic acid groups is sold under the trademark NAFION®. Suitable cation exchange membranes include, but are not limited to, polymeric materials functionalized with quaternary ammonium groups. An example of a suitable polymer functionalized with quaternary ammonium groups is sold under the trademark SELEMION®. A suitable thickness for the anion / cation exchange membrane (s ) include, but not limited to, a thickness greater than 1 pm, 5 pm, or 10 pm and / or less than 500 pm, 1000 pm.

[0051] Figure 1B further depicts one or more electrical conductors 34 that provide electrical communication between the anode 20 and the cathode 30. Suitable electrical conductorsAttorney Docket No. 00172-005W01include, but are not limited to, metal wires, conductive polymers, conductive pastes and combinations thereof. An electrical pathway includes the anode 20, the one or more electrical conductors 34 and the cathode 30. Figure IB illustrates an external bias source 36 positioned along the electrical pathway so as to apply a bias between the cathode 30 and the anode 20. Suitable external bias sources 36 include, but are not limited to, batteries, fuel cells, and grid electricity. In some instances, the external bias source 36 is a photovoltaic system that converts incident light into excited electron-hole pairs that drive a chemical reaction. The external bias source 36 is optional when the electrodes (anode and / or cathode are photoelectrodes ). For instance, in addition to the external bias source 36 or as an alternative to the external bias, the anode 20 and / or cathode 30 can be configured to act as a bias source. For instance, the anode 20 can be a photoanode that converts incident light into excited electron-hole pairs that drive a chemical reaction and / or the cathode 30 can be a photocathode that converts incident light into excited electron-hole pairs that drive a chemical reaction.

[0052] Suitable materials for the photoanode light absorbers, photocathode light absorbers, and external light absorbers include, but are not limited to, semiconductors. In some instances, the photoanode light absorbers include or consist of one or more semiconductors, the photocathode light absorbers include or consist of one or more semiconductors, and / or the external light absorbers include or consist of one or more semiconductors. Suitable semiconductors for the photoanode light absorbers include, but are not limited to, metal oxides, oxynitrides, sulfides, and phosphides that are stable in an oxidizing environment such as WO3, TiO2, and TaON. Suitable semiconductors for the photocathode light absorbers include, but are not limited to, p-type silicon, InP, CU2O, GaP, and WSe2. Suitable semiconductors for the external light absorbers include, but are not limited to, Si, GaAs, CdTe, doped indium gallium (di) selenide, and combinations thereof. In some instances, the external light absorbers, the photoanode light absorbers and / or the photocathode light absorbers are doped. For instance, a photoanode light absorber can be an n-type semiconductor while theAttorney Docket No. 00172-005W01photocathode light absorber can be a p-type semiconductor.

[0053] In operation, the electrical field at the anode 20 causes the electrons to move along the electrical pathway to the cathode 30 where the electrons react with protons in the catholyte 12 to form hydrogen gas. The resulting hydrogen gas can be stored for use as hydrogen fuel.

[0054] The oxidation of, for example, water generates gaseous oxygen and hydrogen cations (H+). Since the membrane separator 10 can comprise an anion exchange membrane water dissociates between or at the interface of the anion exchange membrane. For instance, the water can dissociate at the catalyst layer.EXAMPLE 1

[0055] Recognizing one can scale to larger preparations, an ink was prepared by dispersing 20.0 mg of platinum black in 1.0 mL of deionized water. The mixture was sonicated for about 1 hour. Heat was applied to a 5 cm2sintered titanium porous transport layer in 18.5% hydrochloric acid at about 85 °C for approximately 20 minutes. The porous transport layer (PTL) was removed from the acid and sonicated for about 10 minutes in fresh deionized water 3 times. The PTL was placed on a hotplate at about 120 °C and allowed to dry. The platinum black ink was loaded into an airbrush. Once the PTL was dry, it was kept on the hotplate at about 120 °C, and sprayed with the ink until the PTL was loaded to about 1 mg / cm2of platinum. The PTL was left on the hotplate at about 120 °C until it was dry, then placed in a tube furnace, and evacuated and refilled with 2% hydrogen in argon 3 times. After the third refill, 2% hydrogen in argon was allowed to flow continuously through the tube. The temperature of the tube furnace was increased to 200 °C over 30 minutes, and held at about 200 °C for about 4 hours. Then, the PTL was allowed to cool to room temperature.EXAMPLE 2

[0056] 1.3 g of chloroplatinic acid hexahydrate was dissolved in 1.3 mL of water in a 100 mL quartz crucible. 10.4 g of sodium nitrate was added and thoroughly mixed into the chloroplatinic acid solution. The crucible was capped and put in a muffle furnace. The temperature was ramped from about 20 °C to about 150 °C over the course of 15 minutes and held at about 150 °C for about 50 minutesAttorney Docket No. 00172-005W01in order to drive off any water. The temperature was then ramped from about 150 °C to 500 °C over the course of about 45 minutes and held at 500 °C for 30 minutes in order to convert the chloroplatinic acid to platinum dioxide. The mixture was allowed to cool to room temperature. 40 mL of water was added to the mixture, and the sodium salt was allowed to dissolve. The mixture was then centrifuged at about 12,000 g for 5 minutes and the supernatant removed. 40 mL of water was then added to the brown precipitate. The centrifugation, supernatant removal, and water addition steps were repeated three more times. After the final supernatant removal step, the brown precipitate was transferred into a quartz crucible and dried in a furnace at 120 °C for 1 hour. The dry powder was then mixed in a 100: 1 mass ratio of finely ground sodium chloride to brown powder and placed in a tube furnace and evacuated and refilled with 2% hydrogen in argon 3 times. After the third refill, 2% hydrogen in argon was allowed to flow continuously through the tube. The temperature of the tube furnace was increased to about 150 °C over 30 minutes, and held at about 150 °C for about 4 hours. Then, the powder was allowed to cool to room temperature. The mixture was then centrifuged in water at about 12, 000g for 5 minutes to remove the salt. It was then centrifuged again 3 more times at 12,000g for 10 minutes each. The product is then dried in air at 90 °C for about one hour.

[0057] A synthesis from either method generated well-defined metallic particles with grain-size of approximately 3 - 35 nm in diameter. The size and surface reduced the oxophilicity of the platinum surface, increasing the durability of the catalyst.EXAMPLE 3

[0058] 5.19g of potassium tetrachloroplatinate and 4.86g of polyvinylpyrrolidone (MW 40,000) was dissolved in 125 mL of water in a 1 L Erlenmeyer flask. 11 g ascorbic acid was added with an additional 125 mL of water to dissolve the precursor. The flask was then placed in a ~45 °C water bath without stirring for 2 hours. The color of solution changed from a clear red solution to an opaque black solution indicating the formation of platinum nanoparticles. Approximately 20 mL of reaction mixture was then transferred into each of 12 total centrifuge tubes and each diluted to 45 mL withAttorney Docket No. 00172-005W01water. The tubes were then centrifuged at ~15,557 g for 10 minutes and the supernatant removed. The pellet was redispersed in each tube via bath sonication with ~20 mL of water each and all suspensions were added to a 2 L beaker. In a separate flask, 510 mg of NaBH4was dissolved in 300 mL of water. Under vigorous stirring, the NaBH4solution was slowly added to the particle solution and allowed to bubble at steady rate. Once bubbles dissipated, centrifugation and supernatant removal were repeated. The pellet was dried overnight in air at room temperature. The wash step ensures the removal of the polyvinylpyrrolidone and the reduction of the particle surface.

[0059] This synthesis generated approximately 2.5 g of particles with crystallite grain size of 3-4 nm with larger particles measuring around 100 nm in diameter (see, FIG. 2).EXAMPLE 4

[0060] Prepared an ink by dispersing about 30.0 mg of platinum nanoparticles in 225 µL of deionized water, 1275 µL of isopropyl alcohol, and 18.8 µL of Nafion™ D2020. The mixture was sonicated for 1 hour. A 5 cm2sintered titanium porous transport layer was heated in 18. 5% hydrochloric acid at about 85 °C for about 20 minutes. The porous transport layer (PTL) was removed from the acid and sonicated for 10 minutes in fresh deionized water 3 times. The PTL was placed on a hotplate at about 120 °C and allowed to dry. The platinum ink was loaded into an airbrush. Once the PTL was dry, it was kept on the hotplate at about 120 °C, and sprayed with the ink until the PTL was loaded to about 1.5 mg / cm2platinum. The PTL was left on the hotplate at about 120 °C until it is dry.EXAMPLE 5

[0061] Prepared an ink by dispersing about 30.0 mg of platinum nanoparticles in 225 µL of deionized water, 1275 µL of isopropyl alcohol, and 18.8 µL of Nafion™ D2020. Sonicated the mixture for 1 hour. Lined a metal plate with a sheet of 10-mil-thick PTFE. A piece of Nafion™ 115 membrane was placed on the PTFE. A square hole was cut in a second sheet of 10-mil-thick PTFE to create a mask, and placed on top of the membrane. This stack of materials was then placed on a hotplate at about 120 °C. The platinum ink was loaded into an airbrush and sprayed onto the part of the membrane that is exposed through the mask. The membrane was left on the hotplate atAttorney Docket No. 00172-005W01about 120 °C until it is dry. The mask was removed from the membrane. Another 10-mil-thick PTFE sheet was placed on top of the membrane and another metal plate on top of the PTFE sheet. The assembly was place in a hotpress and pressed at about 120 °C for 4 minutes.EXAMPLE 6

[0062] An approximate 5 cm2square was drawn on a metal plate. A sheet of 10-mil-thick PTFE was placed on top of the metal plate. A Nafion™ 115 membrane was then placed on top of the sheet of PTFE.7.5 mg of platinum powder was applied in a small area at the center of the membrane, within the square that was drawn on the metal plate as seen through the PTFE and membrane. A plastic spatula was used to press and smear the powder into the membrane inside the area of the 5 cm2square. Another 10-mil-thick PTFE sheet was placed on top of the membrane and another metal plate on top of the PTFE sheet. The assembly was placed in a hotpress and pressed at 120 °C for 4 minutes.

[0063] A number of embodiments have been described herein.Nevertheless, it will be understood that various modifications may be made without departing from the spirit and scope of this disclosure. Accordingly, other embodiments are within the scope of the following claims.

Claims

Attorney Docket No. 00172-005W01What is Claimed is:

1. A membrane electrode assembly (MEA) device for water splitting comprising:a cathode;an anode;a cathode current collector in contact with the cathode; an anode current collector in contact with the anode;a hydrogen evolution reaction (HER) cathode-catalyst layer (CCL) on the cathode;an anode catalyst layer (ACL) on the anode; anda proton exchange membrane (PEM) placed between the cathode catalyst layer (CCL) and the anode catalyst layer (ACL);wherein the ACL comprises a large grain-size, low surface area platinum (LGLS-Pt) catalyst with chemically reduced surfaces exhibiting low oxygen affinity.

2. The device of claim 1, wherein the ACL is directly contacting the proton exchange membrane.

3. The device of claim 1, wherein the LGLS-Pt catalyst is applied to a titanium, stainless steel, or membrane by a method selected from the group consisting of spray deposition, slot die coating, and blade coating.

4. The device of any one of the foregoing claims, wherein LGLS-Pt catalyst acts as an oxygen evolution reaction catalyst or a hydrogen recombination catalyst.

5. The device of any one of the foregoing claims, wherein the LGLS-Pt catalyst has a grain diameter size of about 3-50 nm or a particle size of about 50-1000 nm.

6. The device of claim 1, further comprising a current collector.

7. The device of claim 6, wherein the current collector is a graphite plate or a titanium plate.Attorney Docket No. 00172-005W018. An electrode assembly device comprising a porous transport layer device having a large grain-size, low surface area platinum (LGLS-Pt) catalyst with chemically reduced surfaces exhibiting low oxygen affinity.

9. The device of claim 8, wherein LGLS-Pt catalyst acts as an oxygen evolution reaction catalyst or a hydrogen recombination catalyst.

10. The device of claim 8, wherein the LGLS-Pt catalyst has a grain diameter size of about 3-50 nm or a particle size of about 50-1000 nm.

11. An anode catalyst layer (ACL) device comprising a large grainsize, low surface area platinum (LGLS-Pt) catalyst with chemically reduced surfaces exhibiting low oxygen affinity.

12. The device of claim 11, wherein the ACL device comprises an anode comprising titanium or stainless steel.

13. The device of claim 11, wherein the ACL device is directly contacting a membrane.

14. The device of claim 12 or 13, wherein the LGLS-Pt catalyst is applied to the anode or membrane by a method selected from the group consisting of spray deposition, slot die coating, and blade coating.

15. The device of any one of claims 11-14, wherein the LGLS-Pt catalyst acts as an oxygen evolution reaction catalyst or a hydrogen recombination catalyst.

16. The device of any one of claims 11-15, wherein the LGLS-Pt catalyst has a grain diameter size of about 3-50 nm or a particle size of about 50-1000 nm.Attorney Docket No. 00172-005W0117. The device of claim 11, further comprising a current collector.

18. The device of claim 17, wherein the current collector is a graphite plate or a titanium bipolar plate.

19. A platinum catalyst characterized in that:(a) a grain of the catalyst is about 3-30 nm in diameter;(b) a particle of the catalyst is about 50-1000 nm in diameter;(c) particles of the catalyst are irregularly shaped, lack a repeated geometry, are dendritic or any combination thereof; and(d) the catalyst has low oxygen affinity compared to standard platinum black catalysts.

20. A method of converting platinum oxide to platinum metal, the method comprising:disperse a platinum dioxide particular material in an inert media, wherein the inert media is selected from borosilicate glass beads of a diameter of about 3 mm to 212 um or finely ground sodium chloride (NaCl), or a mixture thereof in mass ratios of 5: 1 to 200: 1; andannealing at about 150-400 ° C in Ar or H2 / N2.

21. A method comprising:dissolve a chloroplatinic acid precursor in water and sodium nitrate;heat the chloroplatinic acid precursor solution to about 150 °C for about 50 minutes;heat the chloroplatinic acid precursor solution to about 500 °C for 30 minutes to convert the chloroplatinic acid to platinum dioxide;allow the platinum dioxide to cool;wash the platinum dioxide in water by centrifugation; disperse the platinum dioxide in an inert media, wherein the inert media is selected from borosilicate glass beads of a diameterAttorney Docket No. 00172-005W01of about 3 mm to 212 um, or finely ground sodium chloride (NaCl ), or a mixture thereof in mass ratios of 5: 1 to 200: 1; andannealing the platinum at about 150- 400 ° C in H2 / Ar or H2 / N2.