Sanitary tissues from recycled pulp compositions
Sanitary tissues made from purified post-consumer recycled pulp address contamination issues, ensuring mechanical integrity and safety for hygiene and medical uses by controlling specific chemical contaminants.
Patent Information
- Application Number
- PCT/US2026/025943
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-05
- Filing Date
- 2026-04-30
- Publication Date
- 2026-11-12
AI Technical Summary
The utilization of recycled pulp in various applications is limited due to high levels of chemical contaminants, which affect mechanical properties and safety, particularly in demanding markets like hygiene and medical products, requiring a significant reduction in contamination to meet stringent quality standards.
Sanitary tissues are developed using a composition comprising 30-100% post-consumer recycled pulp with controlled levels of specific chemical contaminants, such as glyphosphate, bisphenol-A, and PCBs, achieved through advanced purification processes.
The solution results in sanitary tissues with low contaminant levels, maintaining mechanical integrity and safety for use in demanding applications, meeting stringent quality requirements.
Smart Images

Figure IMGF000003_0001 
Figure IMGF000051_0001 
Figure IMGF000013_0001_TABLE
Abstract
Description
[0001] SANITARY TISSUES FROM RECYCLED PULP COMPOSITIONS
[0002] FIELD OF THE INVENTION
[0003] The present invention generally relates to sanitary tissues comprising pulp compositions that comprise high purity post-consumer recycled pulp.
[0004] BACKGROUND OF THE INVENTION
[0005] In the world today, hundreds of millions of tons of pulp are utilized on an annual basis. The pulps are generally produced from renewable resources. However, the utilization of virgin pulp may deplete natural resources and be a negative on energy, water, land use, etc., and increase production of greenhouse gases (GHG), primarily CO2, in the atmosphere.
[0006] Polysaccharides in fiber form are the basis of most pulps and include wood, cotton, rayon, etc. The use of recycled pulp has emerged as one solution to mitigate the issues associated with the end-of-life of virgin polysaccharides. Recovering and re-using polysaccharides diverts waste from landfills and reduces the demand for virgin materials.
[0007] The pulps may be used to produce various forms of paper, cardboards, etc. The pulp may be reclaimed as one of many forms and recycled into one of many forms including paper, cardboards, etc.
[0008] Today, in the US, the majority of reclaimed materials destined for recycling, including paper, cardboard, etc., are mixed into a single stream which is collected and processed by a material recovery facility (MRF). At the MRF, materials are sorted, washed, and packaged (e.g., in bales) for resale. Pulp-based materials can be sorted into individual materials.
[0009] However, the utilization of reclaimed pulp in recycling is currently limited due to contamination, which renders these less valuable compared to virgin pulp. A key enabler to increase the recycle rates and lowering the CO2 emissions is to reduce the contamination of recycled pulp to a level allowing broader utilization across more end markets, especially those involving demanding applications. Contamination potentially impacts macroscopic end-use performance such as reduction in mechanical properties such as strength (i.e., tensile, burst, tear, etc.,), elongation, absorbency, and impact and increased malodor and non-optimal color.
[0010] While contamination is problematic for all end market applications, demanding applications such as foods, hygiene, medical, etc., have even stricter requirements, especially on certain chemical contaminants or trace chemicals. The relevant chemical contaminants or trace chemicals may be grouped into various chemical classes depending on the chemical structure of the contaminantsor trace chemicals. Non-limiting examples of these chemical classes ofcontaminants are PF As, heavy metals, pesticides, dioxins, furans, polychlorinated biphenyls (PCBs), phthalates, polycyclic aromatic hydrocarbons (PAHs), organotins, bisphenols, isothiazolins, glyphosphate, alkyl phenols, alkylphenol ethoxylates, aromatic amines, and flame retardants. In addition, the target levels of these contaminants or trace chemicals can be extremely low. For instance, the target levels may be on the order of parts per million (ppm), parts per billion (ppb), and parts per trillion (pptr), wherein the initial contaminated material may contain levels 1,000 times the targeted levels. Net, a l,000X reduction in chemical contamination is often required.
[0011] While the recycling of pulp through various cleaning processes is known, there remains a need for recycled pulp compositions, and compositions comprising recycled pulp compositions, such as sanitary tissues, that have minimum numbers and levels of contaminants, and that also have the necessary mechanical integrity or performance level of the pulp fibers that allow them to be used in various ways.
[0012] SUMMARY OF THE INVENTION
[0013] A sanitary tissue comprising a plurality of dry fibrous structure sheets, wherein the sanitary tissue comprises from about 30 wt.% to about 100 wt.% post-consumer recycled pulp fiber; and further comprises at least one of the following:
[0014] a. less than about 100 pg / kg of glyphosphate;
[0015] b. less than 150 pg / kg of isononylphenol(mono, di, tri, and tetra)exthoxylate; c. less than 150 pg / kg of Bisphenol-A;
[0016] d. less than 25 ng / kg of 1,2,3,4,6,7,8-HpCDD;
[0017] e. less than 250 ng / kg of OCDD;
[0018] f. less than 5 ng / kg of OCDF;
[0019] g. less than 4 ng / kg of PCB 81;
[0020] h. less than 350 ng / kg of PCB 105;
[0021] i. less than 50 ng / kg of PCB 118;
[0022] j. less than 5,000 pg / kg of di-2ethylhexylphthalate;
[0023] k. less than 5,000 pg / kg of di-isononylphthalate;
[0024] l. less than 10 pg / kg of fluoranthene; and
[0025] m. less than 10 pg / kg of phenanthene;
[0026] as measured according to the Trace Chemicals Test Method.BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Fig. l is a perspective view of a test stand for measuring roll compressibility properties as detailed herein.
[0028]
[0029] The pulp compositions that are present in the sanitary tissues of the present invention comprise recycled pulp produced from reclaimed pulp. The difference between recycled and reclaimed pulp is subtle. A reclaimed pulp is a non-virgin pulp that has been collected for potential recycling into a valuable end market. Recycled pulp is produced from the reclaimed pulp after it has been rendered acceptable for use in the end market. In cases wherein the reclaimed pulp can be used as-is in an acceptable end market, then the terms are interchangeable. While use of recycled pulp is known, the present inventive compositions may comprise high amounts of recycled pulp fiber, along with both a low number of contaminants and also low amounts of said contaminants when present. Detailed herein are the types of materials that may have numerous and high levels of contaminants and methods of purifying such materials. The purer materials may then make up a percentage, up to 100% in some embodiments, of the inventive compositions. In some embodiments, the purer inventive materials comprise post-consumer recycled pulp fiber; in other embodiments they comprise post-industrial recycled pulp fiber and in still other embodiments, the purer materials may be a combination of post-consumer and post-industrial recycled pulp fiber.
[0030] Furthermore, the pulp compositions may be incorporated into various consumer products and package materials. Such inventions, for example, inventive sanitary tissue products and inventive packages, may contain low numbers and low levels of contaminants while still exhibiting consumer-expected tactile feel and overall high performance.
[0031] The inventive tissue compositions of the present invention may be characterized by the low number of contaminants present, or they may be characterized by the low amount of a particular contaminant if it is present. The inventive tissue compositions may also be characterized by their performance in various fiber-based tests, such as dry strength, wet strength, modulus, elongation, or wet burst, by their intensive properties, such as basis weight or density, or by their roll properties, such as roll bulk or roll compressibility, or by other finished product characterizations.DETAILED DESCRIPTION OF THE INVENTION
[0032] I. Definitions
[0033] As used herein, the term “pulp” refers to a fibrous composition comprising polysaccharides and may include materials originating from wood, cotton, rayon, etc. Wood pulp refers to pulp originating from a wood source.
[0034] As used herein, the term “pulp fiber” refers to the individual fibers that make-up the actual pulp. These fibers may be characterized by a range of geometric parameters including various diameters, lengths, and degree of entanglements and various polysaccharide chemistries.
[0035] As used herein, the term “paper” refers to a consolidation of pulp into a flat and relatively consistent material. The paper may contain additional additives such as binders and pigments. Paper may be further processed into other forms. Paper is typically sourced from wood pulp but cotton pulp papers are also known.
[0036] “Fiber” and / or “Filament” as used herein means an elongate particulate having an apparent length greatly exceeding its apparent width, i.e., a length to diameter ratio of at least about 10. For purposes of the present invention, a “fiber” is an elongate particulate as described above that exhibits a length of less than 5.08 cm (2 in.) and a “filament” is an elongate particulate as described above that exhibits a length of greater than or equal to 5.08 cm (2 in.).
[0037] Fibers are typically considered discontinuous in nature. Non-limiting examples of fibers include wood pulp fibers and synthetic staple fibers such as polyester fibers.
[0038] In the present invention, “fiber” refers to papermaking fibers. Papermaking fibers useful in the present invention include cellulosic fibers commonly known as wood pulp fibers. Applicable wood pulps include chemical pulps, such as Kraft, sulfite, and sulfate pulps, as well as mechanical pulps including, for example, groundwood, thermomechanical pulp and chemically modified thermomechanical pulp. Chemical pulps, however, may be preferred since they impart a superior tactile sense of softness to tissue sheets made therefrom. Pulps derived from both deciduous trees (hereinafter, also referred to as "hardwood") and coniferous trees (hereinafter, also referred to as "softwood") may be utilized. The hardwood and softwood fibers can be blended, or alternatively, can be deposited in layers to provide a stratified web. U.S. Pat. No. 4,300,981 and U.S. Pat. No.
[0039] 3,994,771 are incorporated herein by reference for the purpose of disclosing layering of hardwood and softwood fibers. Also applicable to the present invention are fibers derived from recycled paper, which may contain any or all of the above categories as well as other non-fibrous materials such as fillers and adhesives used to facilitate the original papermaking.In addition to the various wood pulp fibers, other fibers such as cotton linters, rayon, lyocell, trichomes, seed hairs, and bagasse can be used in this invention.
[0040] Other sources of cellulose in the form of fibers or capable of being spun into fibers include grasses and grain sources.
[0041] “Furnish” is an aqueous suspension of cellulose fibers that is used to make paper.
[0042] “Cellulosic pulp fiber furnish” is the mixture of fibers and other materials that are blended together in a water suspension to make paper or board.
[0043] “Dry fibrous structure” as used herein means that the fibrous structure exhibits a moisturecontent of less than 20% and / or less than 15% and / or less than 10% and / or less than 7% and / or less than 5% and / or less than 3% and / or less than 1% to 0% and or to greater than 0% by weight of the dry fibrous structure as measured according to the Water Content Test Method described herein. In one example, the dry fibrous structure of the present invention exhibits a moisture (water) content of from about 0.0001% to about 20% and / or from about 0.001% to about 15% and / or from about 0.001% to about 12% and / or from about 0.001% to about 10% and / or from about 0.001% to about 7% and / or from about 0.001% to about 5%, by weight of the dry fibrous structure.
[0044] As used herein, the term “Fibrous structure” refers to a structure that comprises one or more fibrous filaments and / or fibers. In one example, a fibrous structure according to the present invention means an orderly arrangement of filaments and / or fibers within a structure in order to perform a function. Non-limiting examples of fibrous structures of the present invention include paper, and absorbent pads (for example for diapers or feminine hygiene products).
[0045] As used herein, the term “virgin pulp” refers to pulp that has not been used to produce a material for a targeted end application. For example, virgin wood pulp is pulp that is produced from wood-based sources and has not been used for the intended purpose previously.
[0046] As used herein, the term “reclaimed pulp” refers to non-virgin pulp that has been collected for potential use in an end market. For example, reclaimed wood pulp is pulp that was originally virgin wood pulp but has already been used for an intended purpose such as paper in a 1st, 2nd, 3rd, etc. life.
[0047] As used herein, the term “recycled pulp” refers to reclaimed pulp that has been converted into a usable material with established end markets such as packaging. The recycled pulp may be purer than the reclaimed pulp fiber or may be identical except possibly in form. For example, recycled wood pulp is pulp that was reclaimed pulp and then rendered usable in the intended endmarket. Expanding further, recycled paper is sourced from reclaimed paper that is rendered acceptable for use as paper.
[0048] As used herein, the term “recycled pulp composition” refers to recycled pulp that may or may not contain virgin pulp or different types of recycled pulps at different concentrations.
[0049] As used herein, “pre-consumer” reclaimed pulp follows the ISO 5270 definition, that is, a descriptive term covering material diverted during a manufacturing process. This term excludes re-utilized material, such as rework, regrind or scrap that has been generated in a given process and is capable of being reclaimed within that same process. The term “post-industrial material” is sometimes used synonymously.
[0050] As used herein, “post-consumer” reclaimed pulp follows the ISO 5270 definition, that is, a descriptive term covering material, generated by the end-users of packages / products, that has fulfilled its intended purpose or can no longer be used (including material returned from within the distribution chain). The term “post-use” is sometimes used synonymously.
[0051] As used herein, the term “1stLife” refers to the first market use of a virgin material.
[0052] As used herein, the term “contaminant” refers to any undesirable material contained on or within the pulp. The term “chemical contaminant” refers to any undesirable chemical species on the surface of the pulp or within the bulk of the pulp and comprises the molecular or elemental composition of the contaminant. The terms may be used interchangeably depending upon the intent. As used herein, the term “contamination” refers to the sum of all contaminants and the term “chemical contamination” refers to the sum of all chemical contaminants. The chemical contaminants are grouped in classes, which include chemical contaminants that have similar chemical structure. For example, As, Hg, and Cr are non-limiting chemical contaminants in the “heavy metals” classification. Each contaminant may have different chemical attributes, such as solubility and diffusivity in the pulp, and target levels depending upon concentration and end use market. The term “contaminant” may be used interchangeably herein with the term “trace chemical”, meaning a small amount of an undesirable material on or within a pulp fiber material.
[0053] As used herein, the term “surface contaminant” refers to a contaminant that is on the surface of the pulp fiber. Similarly, the term “surface chemical contaminant” refers to the molecular or elemental composition of the surface contaminant. The surface contaminant may be attached to the surface of the pulp fiber either loosely through physical attraction forces, or more strongly through polar or other forces. In general, a surface contaminant will have less than about 80% of its surface area embedded in the pulp fiber.As used herein, the term “bulk contaminant” refers to a contaminant that is in the bulk of the pulp fiber. Similarly, the term “bulk chemical contaminant” refers to the molecular or elemental composition of the bulk contaminant. As used herein, a bulk contaminant will have more than about 95% of its surface area embedded in the pulp fiber.
[0054] As used herein, the term “surface contamination” and “surface chemical contamination” refers to the sum of all surface contaminants and all surface chemical contaminants, respectively.
[0055] As used herein, the term “bulk contamination” and “bulk chemical contamination” refers to the sum of all bulk contaminants and all bulk chemical contaminants, respectively.
[0056] As used herein, the term “total contamination” refers to the sum of the surface contamination and bulk contamination and the sum of all the surface chemical contamination and bulk chemical contamination, respectively.
[0057] As used herein, the term “permeable contaminant” refers to a chemical contaminant that is both soluble and diffusible in the pulp fiber.
[0058] As used herein, the term “impermeable contaminant” refers to a chemical contaminant that is either insoluble or non-diffusible or both in the pulp fiber.
[0059] As used herein, the term “permeable contamination” is the sum of all permeable contaminants and the term “impermeable contamination” is the sum of all impermeable contaminants. The sum of all permeable and impermeable contamination is the “chemical contamination” if described in molecular or elemental terms or just simply “the contamination” if described in general terms.
[0060] As used herein, the term “intentional contaminant” refers to a contaminant that is intentionally added by the supply chain for a specific purpose to benefit the producer, retailer, or consumer, but may not be desired in the recycled pulp fiber. Examples include print, adhesives for labels, pigments (such as TiCh), process additives (such as antioxidant (AO)), etc., that are necessary for marketing, branding, processability, and / or end use performance. As used herein, the term “intentional chemical contaminant” refers to an intentional contaminant described by its chemical composition. As used herein, the term “intentional contamination” refers to the sum of all intentional contaminants and the term “intentional chemical contamination” refers to the intentional contamination described by its chemical composition.
[0061] As used herein, the term “unintentional contaminant” refers to any contaminant not intentionally added. Examples include dirt and cross-contamination that is not intentionally added by the producer, retailer, or consumer. As used herein, the term “unintentional chemical contaminant” refers to an unintentional contaminant described by its chemical composition. Asused herein, the term “unintentional contamination” refers to the sum of all unintentional contaminants and the term “unintentional chemical contamination” refers to the unintentional contamination described by its chemical composition.
[0062] As used herein, the term “degradation melting point” refers to the temperature at which the pulp begins to substantially degrade. The degradation may be determined through endothermic or exothermic processes.
[0063] As used herein, the term “limit of quantification” or “LOQ” refers to the lower detection limit for a given chemical contaminant as determined by the analytical methods disclosed in section IX. The LOQ is a function of the methods used and may vary from test method to test method. The LOQ used herein is specific to the method listed in section IX.
[0064] As used herein, the term “ppm” refers to mass parts per million, “ppb” refers to mass parts per billion, and “pptr” refers to mass parts per trillion.
[0065] “Sanitary tissue product” as used herein means a soft, low density (i.e. < about 0.60 g / cm3) web useful as a wiping implement for post-urinary and post-bowel movement cleaning (toilet tissue), for otorhinolaryngological discharges (facial tissue), and multi-functional absorbent and cleaning uses (absorbent towels). Non-limiting examples of suitable sanitary tissue products of the present invention include paper towels, bath tissue, facial tissue, napkins, baby wipes, adult wipes, wet wipes, cleaning wipes, polishing wipes, cosmetic wipes, car care wipes, wipes that comprise an active agent for performing a particular function, cleaning substrates for use with implements, such as a Swiffer® cleaning wipe / pad. The sanitary tissue product may be convolutedly wound upon itself about a core or without a core to form a sanitary tissue product roll.
[0066] “Basis Weight” as used herein is the weight per unit area of a sample reported in lbs / 3000 ft2or g / m2and is measured according to the Basis Weight Test Method described herein.
[0067] “Machine Direction” or “MD” as used herein means the direction parallel to the flow of The fibrous structure through the fibrous structure making machine and / or sanitary tissue product manufacturing equipment.
[0068] “Cross Machine Direction” or “CD” as used herein means the direction parallel to the width of the fibrous structure making machine and / or sanitary tissue product manufacturing equipment and perpendicular to the machine direction.
[0069] “Ply” as used herein means an individual, integral fibrous structure.
[0070] “Plies” as used herein means two or more individual, integral fibrous structures disposed in a substantially contiguous, face-to-face relationship with one another, forming a multi-plyfibrous structure and / or multi -ply sanitary tissue product. It is also contemplated that an individual, integral fibrous structure can effectively form a multi-ply fibrous structure, for example, by being folded on itself.
[0071] The term “natural fibers” or “pulp fiber” as used herein, refers to fibers which comprise cellulose-based fibers, bamboo based fibers, and the like. Natural fibers also refers to nonwoody fibers, such as cotton, abaca, kenaf, sabai grass, flax, esparto grass, straw, jute hemp, bagasse, milkweed floss fibers, and pineapple leaf fibers; and woody, wood, or pulp fibers such as those obtained from deciduous and coniferous trees, including softwood fibers, such as northern and southern softwood kraft fibers; hardwood fibers, such as eucalyptus, maple, birch, and aspen. Pulp fibers can be prepared in high-yield or low-yield forms and can be pulped in any known method, including kraft, sulfite, high-yield pulping methods and other known pulping methods. The natural fibers of the present disclosure may be recycled natural fibers, virgin natural fibers or mixes thereof. Additionally, for good mechanical properties in natural fibers, it can be desirable that the natural fibers be relatively undamaged and largely unrefined or only lightly refined. The fibers can have a Canadian Standard Freeness of at least 200, more specifically at least 300, more specifically still at least 400, and most specifically at least 500.
[0072] The term “cellulose-based fibers,” as used herein, may include cellulose fibers such as wood fiber, cotton, regenerated cellulose fiber such as viscose, lyocell, rayon or Cuprammonium rayon, and high pulping yield fibers, unless specified differently. The term “cellulose-based fibers” also includes chemically treated natural fibers, such as mercerized pulps, chemically stiffened or crosslinked fibers, or sulfonated fibers. Also included are mercerized natural fibers, regenerated natural cellulosic fibers, cellulose produced by microbes, the rayon process, cellulose dissolution and coagulation spinning processes, and other cellulosic material or cellulosic derivatives. Other cellulose-based fibers included are paper broke or recycled fibers and high yield fibers. High yield pulp fibers are those fibers produced by pulping processes providing a yield of about 65% or greater, more specifically about 75% or greater, and still more specifically about 75% to about 95%. Yield is the resulting amount of processed fibers expressed as a percentage of the initial wood mass. Such pulping processes include bleached chemithermomechanical pulp (BCTMP), chemithermomechanical pulp (CTMP), pressure / pressure thermomechanical pulp (PTMP), thermomechanical pulp (TMP), thermomechanical chemical pulp (TMCP), high yield sulfite pulps, and high yield Kraft pulps, all of which leave the resulting fibers with high levels of lignin but are still considered to be natural fibers. High yield fibers are well known for their stiffness in both dry and wet states relative to typical chemically pulped fibers.The term “non-recyclable material” as used herein, refers to contaminants or materials which are believed to be unsuitable for processing in the natural fiber recycling process. However, in alternative recycling streams, the materials provided with this designation may be recyclable.
[0073] The recycle pulp of the present invention may be used to make fibrous structures.
[0074] Non-limiting examples of processes for making fibrous structures include known wet-laid processes, such as wet-laid papermaking processes, and air-laid processes, such as air-laid papermaking processes. Wet-laid and / or air-laid papermaking processes typically include a step of preparing a composition comprising a plurality of fibers that are suspended in a medium, either wet, more specifically aqueous medium, or dry, more specifically gaseous medium, such as air. The aqueous medium used for wet-laid processes is oftentimes referred to as a fiber slurry. The fiber composition is then used to deposit a plurality of fibers onto a forming wire or belt such that an embryonic fibrous structure is formed, after which drying and / or bonding the fibers together results in a fibrous structure. Further processing the fibrous structure may be carried out such that a finished fibrous structure is formed. For example, in typical papermaking processes, the finished fibrous structure is the fibrous structure that is wound on the reel at the end of papermaking, and may subsequently be converted into a finished product, e.g., a sanitary tissue product.
[0075] Non-limiting examples of other known processes and / or unit operations for making fibrous structures include fabric crepe and / or belt crepe processes, ATMOS processes, NTT processes, through-air-dried processes, uncreped through-air-dried processes, and conventional wet press processes.
[0076] The fibrous structures of the present invention may be homogeneous or may be layered in the direction normal to the machine direction. If layered, the fibrous structures may comprise at least two and / or at least three and / or at least four and / or at least five layers.
[0077] The fibrous structures of the present invention may be co-formed fibrous structures. “Coformed” as used herein means that the fibrous structure comprises a mixture of at least two different components wherein at least one of the components comprises a filament, such as a polypropylene filament, and at least one other component, different from the first component, comprises a solid additive, such as a fiber and / or a particulate. In one example, a co-formed fibrous structure comprises solid additives, such as fibers, such as wood pulp fibers and / or absorbent gel articles of manufacture and / or filler particles and / or particulate spot bonding powders and / or clays, and filaments, such as polypropylene filaments. In yet another example, a co-formed structure comprises those described in U.S. Patent Nos. 8,017,534 and 7,674,467.Other non-limiting examples of pulp composition characteristics suitable for use herein are described in U.S. Patent No. 11,252,966, the descriptions of which are incorporated herein by reference.
[0078] II. Reclaimed Pulp
[0079] During pulp fiber’s lifecycle (from production through distribution, consumer utilization, and eventual reclaiming) contamination is introduced either intentionally or unintentionally.
[0080] Non-limiting examples of intentional contamination include surface print, labels, adhesives, optical brighteners, barrier plastics like polyethylene or polypropylene or waxes, binders, pigments (such as TiCh), fillers (such as CaCO3), process additives (such as antioxidant (AO), PF As such as FEP), etc., that are necessary for marketing, branding, processability, and / or end use performance. Non-limiting examples of unintentional contamination are dirt, crosscontamination, certain heavy metals, pesticides, dioxins, furans, PCBs, PF As such as PFOA, etc. Also, unintentional contamination can be produced from reactions involving intentional contaminants, such as the oxidation of pulp to dioxins, degradation of adhesives or print binders, etc. Further, oxidation of the pulp fiber during reclaiming will produce unintentional contamination. In addition, unintentional contamination may result from interaction with products. For example, packaging materials that contain cleaning mixtures (e.g., limonene, surfactants, etc.,), food (e.g., various organics), etc., will potentially become contaminated with such products. Finally, unintentional contamination can enter the pulp fiber during production, e.g., contamination of a pulp fiber with reaction by-products, unreacted monomers, etc.
[0081] Pre-consumer reclaimed pulps generally have the lowest level of contamination due to their known composition and controlled history. It may include intentional contamination but because these are known and controlled, it is quite easy to find applications tolerating such known contaminants. In addition, pre-consumer reclaimed pulp tends to have low amounts of unintentional contamination due to the controlled history preventing external contamination.
[0082] Post-consumer reclaimed pulps are generally more contaminated than pre-consumer reclaimed pulps due to extensive cross-contamination from unknown sources resulting in high levels of unintentional contamination.
[0083] Surprisingly, recycled pulp in the present invention may allow the use of reclaimed pulp from pre-consumer and post-consumer sources in applications requiring low chemical contamination such as medical and hygiene. In addition, most recycled pulp customers desire purermaterials beyond what is available today and the recycled pulp (along with the associated packages and products containing these) of the present invention meets this requirement.
[0084] The reclaimed pulp may be in many macroscopic forms including but not limited to sheets, boards, rolls, etc.
[0085] The reclaimed pulp can be a second-life pulp (has been used only once before it entered the reclaimed pulp stream), third-life pulp (has been used twice before it entered the reclaimed pulp stream), or higher-life pulp fiber (has been used many times before it entered the reclaimed pulp stream).
[0086] The reclaimed pulp may comprise a regrind / edge-trim / in-plant waste pulp fiber or a postindustrial reclaimed pulp. The reclaimed pulp may comprise a post-industrial sheet or board.
[0087] The reclaimed pulp may comprise starch including but not limited to starches from various plants and chemically modified starches. The reclaimed pulp fiber may comprise polysaccharides, polylactic acid, polyhydroxyalkanoate, or chitin.
[0088] III. Contaminants and Contamination
[0089] The chemical contaminants in the contaminated pulp / contaminated pulp composition may be numerous and fall into various chemical classes. These chemical classes may be benign while others may be more problematic. The chemical contaminants of importance herein include but are not limited to pesticides, aldehydes, allergic fragrances, izioalines, alkylphenol ethoxylates, alkylphenols, bisphenols, dioxins, dioxin-like, furans, PCBs, organotins, metals, phthalates, polyaromatic hydrocarbons (PAHs), and PF As (including but not limited to polymeric PF As). The concentration of these chemical contaminants are typically in the ppm, ppb, and pptr type of levels. The analytical methods used to measure these contaminants have lower sensitivity limits. These limits are referred to as Limit of Quantification (LOQ).
[0090] Using the analytical methods disclosed in section IX Methods, the LOQs of the various contaminants may differ by orders of magnitude. For example, the LOQ of a typical pesticide is about 10 ppb; the LOQ of typical alkylphenol ethoxylate is about 50 ppb; the LOQ of a typical alkylphenol is about 5 ppb; the LOQ of bisphenol-A is about 5 ppb; the LOQ of typical dioxin is about 0.2 pptr; the LOQ of a typical furan is about 0.2 pptr; the LOQ of a typical PCB is about 5 pptr; the LOQ of a typical heavy metal is about 100 ppb; the LOQ of a typical organotin is about 300 pptr; the LOQ of typical phthalate is 50 ppb; the LOQ of a typical PAH is 1 ppb.
[0091] Several wood pulp based papers (a pulp composition) including two containing only virgin pulp and one containing post-consumer reclaimed pulp, were broadly classified for chemicalcontamination using the analytical methods disclosed in section IX Methods, as shown in TABLE 1. Note: To simplify the presentation of chemical contamination results, the concentration data is displayed in terms of multiples of LOQ instead of absolute weight fraction involving ppm, ppb, or pptr description. For example, if the contaminant concentration is 10 ppm and the LOQ is 1 ppm, then the concentration would be 10 X LOQ or just 10 displayed in the data tables.
[0092] TABLE 1
[0093] Chemical Contamination of Wood Pulp Based Papers
[0094] Reclaimed Post- Virgin
[0095] Consumer
[0096] #1 #2 #1
[0097] LOQ xLOQ xLOQ xLOQ
[0098] Pesticides
[0099] Diethyltoluamide (DEET) 10 ppb <1 <1 28.0
[0100] Glyphosate 10 ppb <1 <1 12.0
[0101] Alkylphenol ethoxylates
[0102] iso-Nonylphenolmonoethoxylate 50 ppb <1 <1 4.0
[0103] iso-Nonylphenoldiethoxylate 50 ppb <1 <1 6.2
[0104] iso-Nonylphenoltriethoxylate 50 ppb <1 <1 7.0
[0105] iso-Nonylphenoltetraethoxylate 50 ppb <1 <1 3.4
[0106] Bisphenols
[0107] BisphenolA 5 ppb <1 <1 32.0
[0108] Dioxins and dioxinlike and PCB
[0109] 1,2,3,4,6,7,8-HpCDD 0.2 pptr <1 <1 145.5
[0110] OCDD 0.2 pptr <1 <1 1355.0
[0111] OCDF 0.2 pptr <1 <1 43.8
[0112] PCS 81 0.05 pptf <1 <1 87.8
[0113] PCB 105 5 pptr <1 <1 73.2
[0114] PCB 118 10 pptr <1 <1 68.9
[0115] Phthalates
[0116] Di-2-et hylh exy I phthalate 50 ppb <1 <1 134.0
[0117] Diisononyl phthalate 50 ppb <1 <1 100.0
[0118] PAHs
[0119] Fluoranthene Ippb <1 <1 17.0
[0120]
[0121] Phenanthrene tppb „ 1.7 <1 13.0
[0122] As shown in the previous table, chemical contaminants of the types previously mentioned were generally not found in the papers sourced from virgin pulp compositions, which is likely representative of the broader virgin papers available today. However, high levels of the relevant chemical contaminants were found in the paper from reclaimed post-consumer pulp, again likely indicative of the broader reclaimed paper sources available today. For example, up to -1000 X LOQ was determined for OCDD and -100 X LOQ for the phthalates.
[0123] In embodiments of the present invention, said chemical contaminants in said contaminated pulp or contaminated pulp composition include at least one chemical contaminant and such isselected from the group comprising pesticides, alkyl phenols, alkylphenol ethoxylates, bisphenols, dioxins, furans, PCBs, phthalates, PAHs, PF As, or mixtures thereof.
[0124] In embodiments of the present invention, said chemical contaminants in said contaminated pulp or contaminated pulp composition include at least two chemical contaminants and such is selected from the group comprising pesticides, alkyl phenols, alkylphenol ethoxylates, bisphenols, dioxins, furans, PCBs, phthalates, PAHs, PF As, or mixtures thereof.
[0125] In embodiments of the present invention, said chemical contaminants in said contaminated pulp or contaminated pulp composition include at least three chemical contaminants and such is selected from the group comprising pesticides, alkyl phenols, alkylphenol ethoxylates, bisphenols, dioxins, furans, PCBs, phthalates, PAHs, PF As, or mixtures thereof.
[0126] In embodiments of the present invention, the pesticides comprise one or more of piperonyl butoxide, BAC, DEET, glyphosphate, and DDAC. In another embodiment of the present invention, the alkylphenol ethoxylates comprise one or more of iso-Nonylphenolmonoethoxylate, iso-Nonylphenoldiethoxylate, iso-Nonylphenoltriethoxylate, and iso-Nonylphenoltetraethoxylate. In yet another embodiment of the present invention, the alkyl phenols comprise one or more of iso-Nonylphenol, 4-tert-butylphenol, and 4-tert-Pentylphenol. In even yet another embodiment of the present invention, the bisphenols comprise bisphenol-A. In even yet another embodiment of the present invention, the dioxins comprise one or more of 1,2, 3,6,7, 8-HxCDD, 1.2.3.4.6.7.8-HpCDD, and OCDD. In even yet another embodiment of the present invention, the furans comprise OCDF. In even yet another embodiment of the present invention, the PCBs comprise one or more of PCB 77, PCB 81, PCB 126, PCB 105, PCB 114, PCB 118, PCB 123, PCB 156, and PCB 167. In event yet another embodiment of the present invention, the phthalates comprise one or more of di-2-propylheptyl phthalate, disobutyl phthalate, dibutyl phthalate, di- 1 -ethylhexyl phthalate, and diisononyl phthalate. In even yet another embodiment of the present invention, the PAHs comprise one or more of acenaphthene, acenaphthylene, anthracene, benzo[a]anthracene, benzo[b]fluoroanthene, benzo[e]pyrene, benzo[g.h.i]perylene, chrysene, cyclopenta[c.d]pyrene, flyoroanthene, fluorene, naphthalene, phenanthrene, and pyrene. In even yet another embodiment of the present invention, the organotins comprise one or more of monobutylin, dibutyltin, and dioctylin. In even yet another embodiment of the present invention, the PF As comprise one or more of Perfluorooctanoic acid and Perfluorooctane sulfonic acid.
[0127] In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise glyphosphate. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition maycomprise iso-Nonylphenolmonoethoxylate. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise iso-Nonylphenoldiethoxylate. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise iso-Nonylphenoltriethoxylate. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise iso-Nonylphenoltetraethoxylate. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise Bisphenol A. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise OCDD. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise OCDF. In embodiments of the present invention, the contaminants in contaminated pulp or contaminated pulp composition may comprise PCB 81. In embodiments of the present invention, the contaminants in contaminated pulp or contaminated pulp composition may comprise PCB 105. In embodiments of the present invention, the contaminants in contaminated pulp or contaminated pulp composition may comprise PCB 118. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise di-2-ethylhexyl phthalate. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise di-isononyl phthalate. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise fluoranthene. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise phenanthrene.
[0128] In general, the efficacy of the cleaning method of the present invention to remove a specific chemical contaminant is determined by the removal efficiency, defined as the difference in concentration of the chemical contaminant in the contaminated pulp / contaminated pulp composition and the concentration of the chemical contaminant in the purer pulp / purer pulp composition divided by the concentration of the chemical contaminant in contaminated pulp / contaminated pulp composition. However, the removal efficiency is somewhat insufficient due to the inability to determine any actual concentrations below the LOQ. For example, if a cleaning process reduces the contamination from 2 X LOQ to less than the LOQ, then the true removal efficiency could range anywhere between 50% and 100%, which is a significant difference. Thus, the removal efficiency is only completely accurate when the contaminated pulp / contaminated pulp composition and the purer pulp / purer pulp composition concentration are both above LOQ.For simplicity, if the purer pulp / purer pulp composition has a chemical contaminant concentration below LOQ, then removal efficiency is calculated by assuming the chemical contaminant concentration of the purer pulp / purer pulp composition is at the LOQ and the removal efficiency is considered a minimum value and designated with >. For the above example, the removal efficiency would be calculated as 100(2 X LOQ - 1 X LOQ) / (2 X LOQ) = 100(2-l) / 2 = 50%. Thus, the removal efficiency would be listed as > 50%. In certain cases, the purer pulp / purer pulp composition will have a higher level of a certain chemical contaminant than the initial contaminated pulp / contaminated pulp composition which contradicts the meaning of purer. This anomaly may be due to 1) measurement error / measurement variability, 2) contaminant hot spots and cold spots in the reclaimed pulp fiber, 3) external contamination during sampling, and 4) the purification process adds that specific contaminant. If this anomaly occurs consistently for a given chemical species for a given cleaning process, then such is more likely attributable to the purification process and should be more closely examined, but such was not generally the case for the cleaning processes of the present invention. Net, such isolated measurement anomalies were considered measurement error and not considered meaningful to the invention. In such cases, the removal efficiency is set to 0%.
[0129] In one embodiment, the removal efficiency of the DEET contaminant is > 70% wherein said DEET concentration in the contaminated pulp / contaminated pulp composition is at least 10 parts per billion. In another embodiment of the present invention, the removal efficiency of the DEET contaminant is > 85% wherein said DEET concentration in the contaminated pulp / contaminated pulp composition is at least 10 parts per billion.
[0130] In one embodiment of the present invention, the removal efficiency of the glyphosphate contaminant is > 50% wherein said glyphosphate concentration in the contaminated pulp / contaminated pulp composition is at least 10 parts per billion. In another embodiment of the present invention, the removal efficiency of the glyphosphate contaminant is > 90% wherein said glyphosphate concentration in the contaminated pulp / contaminated pulp composition is at least 10 parts per billion.
[0131] In one embodiment of the present invention, the removal efficiency of the isononylphenolmonoethoxylate, iso-nonylphenoldiethoxylate, iso-nonylphenoltriethoxylate, and isononylphenoltetraethoxylate contaminant are all > 50% wherein said isononylphenolmonoethoxylate, iso-nonylphenoldiethoxylate, iso-nonylphenoltriethoxylate, and isononylphenoltetraethoxylate concentration in the contaminated pulp / contaminated pulp composition is at least 50 parts per billion. In another embodiment of the present invention, theremoval efficiency of the iso-nonylphenolmonoethoxylate, iso-nonylphenoldiethoxylate, isononylphenoltriethoxylate, and iso-nonylphenoltetraethoxylate contaminant are all > 70% wherein said iso-nonylphenolmonoethoxylate, iso-nonylphenoldiethoxylate, iso-nonylphenoltriethoxylate, and iso-nonylphenoltetraethoxylate concentration in the contaminated pulp / contaminated pulp composition is at least 50 parts per billion.
[0132] In one embodiment of the present invention, the removal efficiency of the Bisphenol-A contaminant is > 50% wherein said Bisphenol-A concentration in the contaminated pulp / contaminated pulp composition is at least 5 parts per billion. In another embodiment of the present invention, the removal efficiency of the Bisphenol-A contaminant is > 95% wherein said Bisphenol-A concentration in the contaminated pulp / contaminated pulp composition is at least 5 parts per billion.
[0133] In one embodiment of the present invention, the removal efficiency of the 1, 2, 3, 4, 6,7,8-HpCDD contaminant is > 50% wherein said 1,2,3,4,6,7,8-HpCDD concentration in the contaminated pulp / contaminated pulp composition is at least 0.2 parts per trillion. In another embodiment of the present invention, the removal efficiency of the 1,2,3,4,6,7,8-HpCDD contaminant is > 85% wherein said 1,2,3,4,6,7,8-HpCDD concentration in the contaminated pulp / contaminated pulp composition is at least 0.2 parts per trillion.
[0134] In one embodiment of the present invention, the removal efficiency of the OCDD contaminant is > 50% wherein said OCDD concentration in the contaminated pulp / contaminated pulp composition is at least 0.2 parts per trillion. In another embodiment of the present invention, the removal efficiency of the OCDD contaminant is > 85% wherein said OCDD concentration in the contaminated pulp / contaminated pulp composition is at least 0.2 parts per trillion.
[0135] In one embodiment of the present invention, the removal efficiency of the PCB 81 contaminant is > 50% wherein said PCB 81 concentration in the contaminated pulp / contaminated pulp composition is at least 0.05 parts per trillion. In another embodiment of the present invention, the removal efficiency of the PCB 81 contaminant is > 85% wherein said PCB 81 concentration in the contaminated pulp / contaminated pulp composition is at least 0.05 parts per trillion.
[0136] In one embodiment of the present invention, the removal efficiency of the PCB 105 contaminant is > 50% wherein said PCB 105 concentration in the contaminated pulp / contaminated pulp composition is at least 5 parts per trillion. In another embodiment of the present invention, the removal efficiency of the PCB 105 contaminant is > 85% wherein said PCB 105 concentration in the contaminated pulp / contaminated pulp composition is at least 5 parts per trillion.In one embodiment of the present invention, the removal efficiency of the PCB 118 contaminant is > 50% wherein said PCB 118 concentration in the contaminated pulp / contaminated pulp composition is at least 10 parts per trillion. In another embodiment of the present invention, the removal efficiency of the PCB 118 contaminant is > 85% wherein said PCB 118 concentration in the contaminated pulp / contaminated pulp composition is at least 10 parts per trillion.
[0137] In embodiments of the present invention, the removal efficiency of the Di-2-ethylhexyl phthalate contaminant is > 50% wherein said Di-2-ethylhexyl phthalate concentration in the contaminated pulp / contaminated pulp composition is at least about 50 parts per billion. In another embodiment of the present invention, the removal efficiency of the Di-2-ethylhexyl phthalate contaminant is > 85% wherein said Di-2-ethylhexyl phthalate concentration in the contaminated pulp / contaminated pulp composition is at least about 50 parts per billion.
[0138] In embodiments of the present invention, the removal efficiency of the Di-isononyl phthalate contaminant is > 50% wherein said Di-isononyl phthalate contaminant concentration in the contaminated pulp / contaminated pulp composition is at least about 50 parts per billion. In another embodiment of the present invention, the removal efficiency of the Di-isononyl phthalate contaminant is > 85% wherein said Di-isononyl phthalate contaminant concentration in the contaminated pulp / contaminated pulp composition is at least about 50 parts per billion.
[0139] In embodiments of the present invention, the removal efficiency of the fluoranthene contaminant is > 50% wherein said fluoranthene concentration in the contaminated pulp / contaminated pulp composition is at least about 1 parts per billion. In another embodiment of the present invention, the removal efficiency of the fluoranthene contaminant is > 85% wherein said fluoranthene concentration in the contaminated pulp / contaminated pulp composition is at least about 1 parts per billion.
[0140] In embodiments of the present invention, the removal efficiency of the phenanthrene contaminant is > 50% wherein said phenanthrene concentration in the contaminated pulp / contaminated pulp composition is at least about 1 parts per billion. In another embodiment of the present invention, the removal efficiency of the phenanthrene contaminant is > 85% wherein said phenanthrene concentration in the contaminated pulp / contaminated pulp composition is at least about 1 parts per billion.
[0141] In embodiments of the present invention, the removal efficiency of the Perfluorooctanoic acid contaminant is > 50% wherein said Perfluorooctanoic acid concentration in the contaminated pulp / contaminated pulp composition is at least LOQ. In embodiments of the present invention,the removal efficiency of the Perfluorooctane sulfonic acid contaminant is > 50% wherein said Perfluorooctane sulfonic acid concentration in the contaminated pulp / contaminated pulp composition is at least LOQ.
[0142] In general, bulk contamination will not be appreciably removed by simple aqueous surface washing approaches of the prior art. Permeable bulk contamination can be removed by diffusion mechanisms through gradients in chemical potential, whereas bulk impermeable contamination is essentially trapped by the bulk pulp fiber, and methods to free the trapped contaminant dissolution / disintegration of the pulp fiber.
[0143] IV. Surface Purification Methods
[0144] Surface purification methods reduce surface contamination. One example of a purification process may include, but is not limited to, surface washing with a surface washing fluid that is typically water based. The reclaimed pulp fiber will generally be in the form of board, loose or compacted fibers, loose or compacted flexible packages, loose or compacted rigids, loose or compacted non-wovens, loose or compacted fibers, etc. which will be difficult to surface wash due to excessive overall size. Hence, prior to surface washing, a granulation or shredding step is preferred. The surface washing will typically include mechanical agitation to loosen surface dirt and other contaminants to allow physical removal and transfer to the washing fluid wherein the dirt or other contaminants may or may not solubilize.
[0145] Surface washing technologies are available extensively on the market for cellulosic-based reclaimed pulp fibers.
[0146] V. Bulk Purification
[0147] In general, bulk contamination will not be appreciably reduced by simple aqueous surface washing.
[0148] One example of a purification process may include, but is not limited to, extraction, which may be a preferred bulk purification method for removing permeable contaminants. Extraction involves the use of a purification solvent to remove bulk permeable contaminants through creation of a chemical potential gradient between the reclaimed pulp fiber and the solvent. The rate of permeable chemical contaminant removal will depend upon the diffusivity and solubility of the contaminant in the pulp fiber under the conditions created in the process. For high molecular weight pulp fibers, the diffusivity of large molecules indicative of chemical contaminants is quite low, especially in the solid state of the pulp fiber. In addition, the solubility may be limited due tothe high MW of the reclaimed pulp fiber and lack of enthalpic mixing. Thus, the time required to remove permeable contaminants through diffusion mechanisms can be quite long and not conducive to economically viable processes at commercial scale. Methods to resolve these time scale limitations include 1). increased diffusivity through elevated temperature and / or pulp fiber relaxation through solvent swelling, 2). decrease of diffusion path length through increased surface area to volume ratio of the reclaimed pulp fiber exposed to the solvent, 3) increased convective transport of the contaminant through the pulp fiber / solvent interface by: increased solubility of the contaminant in the solvent, increased partitioning of the contaminant within the solvent relative to the pulp fiber; increased convection around the pulp fiber / solvent interface, and increased solvent sink relative to pulp fiber sink. The solubility of the bulk purification solvent in the pulp fiber can be increased by operating the extraction at high pressures especially at, near, or above the critical pressure.
[0149] It is important for the extraction method to be scalable to large volumes at low cost. Hence, the time required for extraction should be low to allow for such scalability. In embodiments of the present invention, the total time for extraction is less than about 6 hours, preferably less than about 4 hours, more preferably less than about 2 hours, and even more preferably less than about 1 hour. If the extraction is completed in stages, then the time per stage may be less than this range but the overall time will still fall within these times.
[0150] Extractions may take place above, near, at, or below the degradation or primary melting point (whichever is lower) of the reclaimed pulp fiber. Extractions generally occur in a two-phase system involving a solvent-rich phase and a pulp fiber-rich phase. Leaching extractions are a subset of extractions typically involving a liquid state for the solvent-rich phase and a solid state for the pulp fiber-rich phase. Liquid-liquid extractions are a subset of extractions typically involving two liquid states. In an embodiment of the present invention, the extraction is leaching.
[0151] In leaching processes, the reclaimed pulp fiber may be contacted with excessive solvent during every stage and every time of the process. Such leaching processes are called flooded leaching processes. In flooded leaching processes, the mass of leaching solvent to mass of reclaimed pulp fiber exposed to the solvent at every point in time and in every stage of the process is preferably equal to or greater than about 5:1. In certain flooded leaching processes, the solvent is rapidly stirred such that the reclaimed pulp fiber is suspended in the solvent even when the density of the reclaimed pulp fiber is greater than the solvent. Such flooded leaching processes 1) ensure complete contact between the surface of the reclaimed pulp fiber and the leaching solvent and 2) lower the mass transfer resistance within the solvent boundary layer around the reclaimedpulp fiber surface due to the convective motion. Beyond stirring, similar reduced boundary layer may be achieved in flooded leaching processes by allowing the reclaimed pulp fiber to settle through the solvent by density gradient. Examples of flooded leaching processes include stirred tanks of the continuous, semi-continuous, and batch types. Additional examples of flooded leaching processes include settling tanks wherein the reclaimed pulp fiber is allowed to settle out or through the solvent that is filled inside a tank or other vessel.
[0152] In leaching processes, the solvent may be contacted with excessive pulp fiber during every stage and every time of the process. Such leaching processes are called packed leaching processes. In packed leaching processes of the current invention, the mass of leaching solvent to mass of reclaimed pulp fiber exposed to the solvent at every point in time and in every stage of the process is preferably equal to or less than about 5:1. In certain packed leaching processes, the solvent is flowed through a packed column or bed of pulp fiber. Such packed leaching processes provide efficient means for removing contaminated solvent and ensuring optimal concentration gradient. Examples of packed leaching include but are not limited due flow through packed beds, percolation extractors, screw-based extractors, Hildebrandt extractors, etc.
[0153] In some embodiments, a purification process may include an extraction that comprises flooded leaching. In embodiments of the present invention, the extraction may comprise packed leaching. In embodiments of the present invention, the extraction comprises a combination of flooded and packed leaching.
[0154] For leaching processes of the current invention, it may be beneficial to select a leaching solvent and operating temperature and pressure such that the leaching solvent is at its boiling point during the extraction. Such designs allow the solvent to be continuously refluxed, which may enable locally high concentration gradients as the refluxed solvent contacts the reclaimed pulp fiber. In embodiments of the present invention, the bulk extraction is either packed or flooded leaching or combinations of both, and the pressure of the bulk purification is about atmospheric. In embodiments of the present invention, the bulk extraction is either packed or flooded leaching or combinations of both, and the pressure of the leaching is about atmospheric, and the leaching solvent is at or near the normal boiling point. For cellulosics, preferred leaching solvents for flooded leaching have boiling points in the 2°C to 90°C range. Examples of such solvents are THF, di-ethyl ether, hexanes, acetone, ethanol, methanol, propanol, iso-propanol, MEK, and ethyl acetate or blends thereof. The leaching solvents may contain minor amounts of water (< ~25 wt% water) that are residual within the cellulosic reclaimed pulp fiber or intentionally added to any of the aforementioned solvents. In embodiments of the present invention, said leaching solvent mayhave a normal boiling point between 20°C and 90°C. In embodiments of the present invention, the leaching solvent has a normal boiling point between 20°C and 90°C and the leaching temperature is at or near the boiling point. In another embodiment of the present invention, the leaching solvent has a normal boiling point between 20°C and 90°C and the purification temperature is at or near the boiling point and the pressure is at or near atmospheric. The pressure may also be between about 0.5 atm and higher. In yet another embodiment of the present invention, the leaching solvent has a normal boiling point between 20°C and 90°C and the pressure is above atmospheric but below 1,000 atm. The leaching solvent may also have a boiling point above the leaching temperature. In even yet another embodiment of the present invention, the leaching solvent has a normal boiling point above the leaching temperature. In another embodiment of the present invention, wherein said bulk purification is leaching; wherein said leaching solvent is ethyl acetate; said temperature of said leaching is between about 20°C and about 120°C; and said pressure of said leaching is between about 0.5 atm and about 1,000 atm. In another embodiment of the present invention, wherein said bulk purification is leaching; wherein said leaching solvent is hexanes; said temperature of said leaching is between about 20°C and about 120°C; and said pressure of said leaching is between about 0.5 atm and about 1,000 atm.
[0155] Leaching solvents with a normal boiling point below the leaching temperature are also preferred due to the elevated leaching pressures. In embodiments of the present invention, the leaching solvent has a normal boiling point below the leaching temperature. In another embodiment of the present invention, the leaching solvent is di-methyl ether (DME). In an embodiment of the present invention, wherein said bulk purification is leaching; wherein said leaching solvent is DME; said temperature of said leaching is between about 20°C and about 120°C; and said pressure of said leaching is between about 2 atm and about 1,000 atm.
[0156] Preferred leaching solvents include solvents that have higher affinity for the chemical contaminants than for the reclaimed pulp fiber. Solvents with high affinity for the chemical contaminants include but are not limited to diethyl ether, MEK, ethyl acetate, THF, acetone, methylene chloride, iso-propanol, propanol, ethanol, and methanol. Other oxygenated and polar hydrocarbon solvents likely have similar desired affinity. Solvents lacking such characteristics can still be used, but higher solvent to pulp fiber ratios may be required. It is preferred that the solvent should not significantly dissolve the reclaimed pulp fiber at the temperature and pressure of the process (< ~5wt% may be dissolved). The solvent may slightly swell the reclaimed pulp fiber but not enough to cause agglomeration or coalescence. The solvents may contain water for various functional or non-functional reasons (below ~25wt%).In embodiments of the present invention, said leaching solvent is selected from the group comprising hydrocarbons. In another embodiment of the present invention, said leaching solvent is selected from the group comprising aliphatic hydrocarbons. In even another embodiment of the present invention, said leaching solvent is selected from the group comprising aromatic hydrocarbons. In even yet another embodiment of the present invention, said leaching solvent is selected from the group comprising alkanes.
[0157] In embodiments of the present invention, said leaching solvent is selected from the group comprising methane, ethane, propane, normal butane, isobutane, normal pentane, isopentane, neopentane, hexanes (normal hexane, isohexane, neohexane, heptanes), octanes, or mixtures thereof.
[0158] The temperature may be changed during the course of the extraction process but is generally consistent within a given stage of a unit operation. The pressure may be changed to vary solubility of the solvent in the reclaimed pulp fiber or to increase solubility of the chemical contaminant within the solvent.
[0159] A leaching extraction process may take place in stages and be combined with additional leaching extraction processes of other types not discussed in this application. The same is true for liquid-liquid extraction processes. In addition, liquid-liquid process may be combined with leaching process in various stages to form a given purification process. In embodiments of the present invention, the number of stages is one or more than one. In another embodiment of the present invention, the number of liquid-liquid stages is more than one. In yet another embodiment of the present invention, the number of leaching stages is more than one. In still yet another embodiment of the present invention, the number of liquid-liquid stages is one or more and the number of leaching stages is one or more. A single stirred tank reactor will achieve a certain removal efficiency. The efficiency can be improved by having multiple stirred tank reactors in series wherein the reclaimed pulp fiber from the 1ststage is predominately separated from the 1ststage purification solvent and this 1ststage pulp fiber is used in the 2ndstage with fresh purification solvent. This is repeated for each additional stage. This method improves the removal efficiency at the expense of additional reactors and complexity but maintains the overall time, throughput, and solvent utilization. Practically speaking, the number of reactor stages can be anywhere from 1 to ~ 10 for stirred tank systems. If a larger number of stages are needed, then a continuous counter-current method may be used.
[0160] While not wishing to be bound by theory, the theoretical maximum contaminant removal capacity for a leaching process is based upon the thermodynamic equilibrium / partitioning of thechemical contaminants between the reclaimed pulp fiber and leaching solvent at the temperature and pressure of the process. Thermodynamic equilibrium may not be achieved due to kinetic limitations in the leaching process. This is true for the complete leaching process and is also true for each leaching stage. A higher leaching solvent to reclaimed pulp fiber mass ratio will drive both thermodynamics and kinetics in favor of purification at the expense of greater solvent consumption and greater extraction process size, which equals greater cost. Thus, a balance must be found between these important design and operational variables for the targeted chemical contaminant removal efficiency. In addition, the contaminated solvent from any stage may be used “as-is” as the solvent for another stage. Contaminated solvent at any point in the process may be renewed through known methods of distillation, filtration, ion-exchange, etc., or combinations.
[0161] Another important kinetic driver is surface area to volume ratio of the reclaimed pulp fiber within and exposed to the leaching solvent. In general, the time required to extract a chemical contaminant from a reclaimed pulp fiber is a strong function of the diffusion pathlength within the reclaimed pulp fiber. The diffusion pathlength is indirectly proportional to the surface area to volume ratio of the geometrical form of the reclaimed pulp fiber and the ability to access the surface area with leaching solvent. Hence, a higher surface area to volume ratio will produce a reduced diffusion pathlength and faster diffusion kinetics. For leaching processes, a high surface area to volume ratio is a critical parameter for quick and efficient contaminant removal both surface and bulk.
[0162] A known means for increasing the effective mass transfer through a given surface area to volume ratio and given set of conditions at the reclaimed pulp fiber solvent interface is through applying energy to the reclaimed pulp fiber such as but not limited to vibrational in the form of ultrasonic energy and / or microwave.
[0163] Following the bulk purification involving extraction, the pulp fiber may be devolatilized to produce a purer recycled pulp fiber. The contaminated solvent will contain a small amount of dissolved purer recycled pulp fiber, the extracted contaminants, and the pure leaching solvent. There are many ways to recover the purer recycled pulp fiber and bulk purification solvent independent of the extracted contaminants.
[0164] In general, a small amount of reclaimed pulp fiber may dissolve into the leaching solvent regardless of process type or solvent. In particular, low molecular weight waxes are particularly prone to solubilization into the extracting solvent. These may become problematic in distillationbased recovery of the purified solvent due to deposition of the waxes on process equipment. Methods are known to reduce this tendency. One such method is to lower the temperature of thecontaminated solvent to below the cloud point to precipitate the pulp fiber or wax phase followed by filtration. Unlike the reclaimed pulp fiber, the residual pulp fiber or waxes resulting pulp fiber from the precipitation from the contaminated solvent may contain significant chemical contamination.
[0165] Distillation and / or flash evaporation of the contaminated bulk purification solvent may be used to regenerate the solvent for re-use in the various extraction operations. However, distillation may not be economically feasible on-going considering the high solvent volume utilized in the present invention. In addition, because the chemical contaminants of interest in this invention are extremely low in concentration, the concentration of these chemical contaminants in the contaminated solvent may be correspondingly low or even lower. Thus, a preferred method to purify the contaminated solvent is through direct removal of the contaminants without volatilizing the bulk solvent phase. Such methods include precipitation, ion exchange, adsorption / absorption methods, etc. Non-limiting examples include passing the contaminated solvent through a bed of activated carbon or alumina. This method can be used alone or in combination with distillation to achieve the right level of purification at the right energy consumption. In addition, the contaminated solvent from any stage may be used “as-is” as the solvent for another stage. Contaminated solvent at any point in the process may be renewed through known methods of distillation, filtration, ion-exchange, etc., or combinations.
[0166] The purer recycled pulp fiber may contain small amounts of the solvent in either physically adsorbed or bulk absorbed form. The concentration of the solvent in the purer recycled pulp fiber may be reduced by devolatilization techniques. In an embodiment of the present invention, said purer recycled pulp fiber is devolatilized to a content of < 1 wt% solvent. In an embodiment of the present invention, said purer recycled pulp fiber is devolatilized to a content of < about 50 ppm solvent.
[0167] Multi-staged stirred tank flooded extractors operating at the boiling point of a polar organic leaching solvent provide improvements in chemical contaminant removal over existing methods. For example (as shown in Examples 1 and 2), a flooded leaching process of the present invention provided targeted contaminant removal efficiencies greater than about 50%.
[0168] In embodiments of the present invention, the leaching solvent is ethyl acetate. In yet another embodiment of the present invention, the leaching solvent is ethyl acetate and the process pressure is about atmospheric pressure. In another embodiment of the present invention, said bulk purification comprises flooded leaching in a stirred tank conducted at about 77.1 °C and about atmospheric pressure with a leaching solvent comprising ethyl acetate.In embodiments of the present invention, the leaching solvent is acetone. In yet another embodiment of the present invention, the leaching solvent is acetone and the process pressure is about atmospheric pressure. In another embodiment of the present invention, said bulk purification comprises flooded leaching in a stirred tank conducted at about 56.1 °C and about atmospheric pressure with a leaching solvent comprising acetone.
[0169] In another embodiment of the present invention (Example 1 and Tables), a bulk purification of a reclaimed pulp fiber involving recycled cellulosic paperboard comprises flooded leaching in a stirred tank involving 4 stages conducted at about 77.1 °C and about atmospheric pressure with a leaching solvent comprising ethyl acetate; wherein the ethyl acetate to first pulp fiber mass ratio is ~ 10:1 per stage for a leaching time of - 30 minutes per stage for a total ethyl acetate to recycled pulp fiber ratio of about 40: 1 and a total leaching time of about 120 minutes; wherein the % removal of the pesticides, DEET and glyphosphate, is 52.7 and > 86.7%, the alkylphenolethoxylates, isononylphenoldiethoxylate and isononylphenoltriethoxylate, is > 94.6% and > 96.2%, the alkylphenols, isononylphenol and 4-tert-pentylphenol, is > 78.3% and 80.8%, the bisphenol A is > 98.7%, the dioxins, 1,2, 3, 4, 6, 7, 8 -HpCDD and OCDD, is 74.3% and 84.3%, the OCDF is 87.1%, the PCBs, PCB 105 and PCB 118, is 89.4% and 89.5%, the organotins, dimethyltin and trimethyltin, is 98.4% and 99.5%, the phthalates, Di-2-ethylhexylphthalate and diisononylphthalate, is 98.1% and 94.0%, and the PAHs, fluoranthene and phenanthrene, is > 94.1% and 86.9% wherein the initial concentration of these contaminants in the reclaimed pulp fiber are above LOQ.
[0170] In another embodiment of the present invention (Example 2 and Tables), a bulk purification of a reclaimed pulp fiber involving a different recycled paperboard comprises flooded leaching in a stirred tank involving 4 stages conducted at about 77.1 °C and about atmospheric pressure with a leaching solvent comprising ethyl acetate; wherein the ethyl acetate to first pulp fiber mass ratio is - 10:1 per stage for a leaching time of - 30 minutes per stage for a total ethyl acetate to reclaimed pulp fiber ratio of about 40: 1 and a total leaching time of about 120 minutes; wherein the % removal of the pesticides, DEET, is > 47.4%, the alkylphenol, 4-tert-pentylphenol, is > 70.6%, the dioxins, 1,2, 3, 4, 6, 7, 8 -HpCDD and OCDD, is 59.4% and 67.5%, the OCDF is 67.3%, the PCBs, PCB 105 and PCB 118, is 78.9% and 79.6% wherein the initial concentration of these contaminants in the reclaimed pulp fiber are significantly above LOQ. The mechanical properties of paperboard produced from the purer cellulosic recycled pulp fiber are not significantly reduced compared to similar paperboard produced from the reclaimed pulp fiber (% decrease in properties < 10%).Following the flooded leaching, the purer recycled pulp fiber may be physically wetted with the residual solvent and potentially contain a small amount of absorbed solvent. As discussed earlier, there are many ways to recover the purer recycled pulp fiber and bulk purification solvent independent of the extracted contaminants. The purer recycled pulp fiber can be dried and devolatilized by many known commercial means. One method is through cyclonic drying. Another method is through melt extrusion with a devolatilization section. In embodiments of the present invention, the purer recycled pulp fiber is processed to reduce the leaching solvent to below about lwt% in the reclaimed pulp fiber and more preferably less than about 50 ppm. The contaminated solvent can be cleaned with known methods of distillation, ion exchange, filtration, etc. The resulting devolatilized reclaimed pulp fiber may be used as it or may be further processed into other forms including pellets via various processes.
[0171] VI. Recycled Pulp fiber
[0172] The purer recycled pulp fiber produced from the reclaimed pulp fiber will have a lower level of contamination relative to the reclaimed pulp fiber. The purer recycled pulp fiber from the bulk purification step may be further processed to produce other forms.
[0173] VII. EXAMPLES
[0174] In general, the established methods for purifying / cleaning reclaimed pulp fiber including water washing are currently not able to sufficiently remove chemical contaminants. Net, there is an unmet need for a cleaning technology that is capable of more completely removing chemical contamination sufficient for highly contaminated sources and for any market desiring purer recycled materials. In addition, there is an unmet need for recycled compositions that do not have, or have very low levels of, chemical contaminations.
[0175] COMPARATIVE EXAMPLE - Purification Method Using Traditional Water Washing of Reclaimed Post-Consumer Pulp Composition in Paperboard Form to Produce a Water-Washed Post-Consumer Recycled Pulp Composition
[0176] 2,500 grams of de-ionized water was added to a 5L stirred round bottom flask. In addition, ImL of Triton X=100 surfactant was added to the water. The flask was outfitted with a mechanical stirrer, one reflux condenser, and one heat jacket. The mechanical stirring was set to 400 rpm. The heating jacket was controlled by a variable voltage transformer. The heat was applied to rapidly bring the water to ~80°C) in about 5 minutes. After reaching ~80°C, the heat input was lowered tomaintain a constant temperature of ~80°C. Contaminated pulp composition in the form of Reclaimed Post-Consumer Paper was cut into 1 cm X 1 cm squares. The -250 grams of the cut Reclaimed Post-Consumer Paper was added to the round bottom flask which contained the hot water / surfactant solution. The washing was continued for -30 minutes. The stirring was terminated, and the heat was removed. The water solution was decanted from the mixture of solids and liquids. This completed washing step #1. An additional 2,500 grams of preheated water / Triton X-100 solution was added to the paperboard in the 5L round bottom to complete a second washing step. Stirring was started at 400 to 500 rpm while heating was applied sufficient to achieve ~80°C. The time to reach 80°C after the addition of the fresh-water solution to the paperboard was -5 minutes. The 2nd washing continued for a total of -30 minutes. The stirring was stopped, and the heat removed. The water solution was decanted off. This completed washing step #2. An additional 2,500 grams of preheated water / Triton X-100 solution was added to the paperboard in the 5L round bottom. Stirring was started at 400 to 500 rpm while heating was applied sufficient to achieve 80°C. The time to reach ~80°C after the addition of fresh-water solution was -5 minutes. This washing step continued for a total of -30 minutes. The stirring was stopped, and the heat removed. The water solution was decanted off. This completed washing step #3. An additional 1,000 grams of preheated fresh water / Triton X-100 solution was added to the paperboard in the 5L round bottom to complete a fourth washing step. Stirring was started at 400 to 500 rpm while heating was applied sufficient to achieve ~80°C in the water solution. The time to reach ~80°C after the addition of fresh-water solution was -5 minutes. The 4th washing continued for a total of -30 minutes. The stirring was stopped, and the heat removed. The water solution was decanted off. The paperboard contained a small amount of contaminated water solution within the porosity of the paperboard. This wet paperboard was placed in a filter funnel with 60 mesh grating to further remove residual water solution via gravity. The paperboard was then completely dried of contaminated water solution at room temperature over-night to produce the purer pulp composition. The washing solution to pulp composition ratio per stage was -10:1 for four stages giving a total washing solution to pulp composition ratio of -40:1. The washing time per stage was approximately -35 minutes per stage for a total time of -140 minutes. The contaminated pulp composition represented by Reclaimed Post-Consumer Pulp and the resulting purer pulp composition represented by the Recycled Post-Consumer Pulp discussed above was analyzed for the classes of chemical contaminants typically present in recycled materials by GALAB Laboratories GmbH (Am Schleusengraben 7, 21029 Hamburg, Germany) using the methods disclosed in section IX Methods, as shown in Table 2. For the contaminants DEET, glyphosphate,isononylphenolmonoethoxylate, isononylphenoldiethoxylate, isononylphenoltriethoxylate, isononylphenoltetraethoxylate, bisphenol A, 1,2,3,4,6,7,8-HpCDD, OCDD, OCDF, PCB 81, PCB 105, PCB 118, di2-ehtylhexylphthalate, and diisononylphthalate, the % removal was > 96.4%, 44.2%, 35.0%, 35.5%, 40.0%, 17.6%, 72.5%, 0.0%, 0.0%, 0.0%, 0.0%, 0.0%, 0.0%, 14.9%, and 10.0% respectively, which was indicative of generally poor contaminant removal especially for the dioxins, pcbs, and phthalates.
[0177] The pulp before and after the purification was characterized for water retention value. The water wash resulted in a 10.4% reduction of water-retention value which may be indicative of increased homification.
[0178] The pulp before and after the purification were processed into handsheets following Tappi T205 and then evaluated for tensile properties and chemical composition. The tensile strength for the handsheets after purification was reduced by about 11% possibly due to increased homification. The washing process removed about 6.5% ash but did not significantly remove lignin from the pulp fibers.TABLE 2
[0179] Purification Method Using Traditional Water Washing of Reclaimed Post-Consumer Pulp Composition in Paperboard Form to Produce a Water-Washed Post-Consumer Recycled Pulp Composition
[0180] Reclaimed Post-Consumer Pulp Composition
[0181] Before After
[0182] % Removed Purification Purification
[0183] LOQ xLOQ xLOQ
[0184] Pesticides
[0185] Diethyltoluamide (DEET) 10 ppb 28.0 <1 > 96.4% Glyphosate 10 ppb 12.0 6.7 44.2% Alkylphenol ethoxylates
[0186] iso-Nonylphenolmonoethoxylate 50 ppb 4.0 2.6 35.0% iso-Nonylphenoldiethoxylate 50 ppb 6.2 4.0 35.5% iso-Nonylphenoltriethoxylate 50 ppb 7.0 4.2 40.0% iso-Nonylphenoltetraethoxylate 50 ppb 3.4 2.8 17.6% Bisphenols
[0187] Bisphenol A 5 ppb 32.0 8.8 72.5% Dioxins and dioxinlike and PCB
[0188] 1,2,3,4,6,7,8-HpCDD 0.2 pptr 145.5 163.0 0.0%
[0189] OCDD 0.2 pptr 1355.0 1445.0 0.0%
[0190] OCDF 0.2 pptr 43.8 47.7 0.0%
[0191] PCB 81 0.05 pptr 87.8 92.8 0.0%
[0192] PCB 105 5 pptr 73.2 87.2 0.0%
[0193] PCB 118 10 pptr 68.9 83.2 0.0%
[0194] Phthalates
[0195] Di -2-ethylhexyl phthalate 50 ppb 134.0 114.0 14.9% Diisononyl phthalate 50 ppb 100.0 90.0 10.0% Polycyclic aromatic hydrocarbons (PAH)
[0196] Fluoranthene I ppb 17.0 dnt n. a. Phenanthrene I ppb 13.0 dnt n.a.
[0197] % Increase
[0198] Water Retention Value (g / g) 1.25+ / - 0.1 1.12+ / - 0.01 -10.4%
[0199] FQAFines Level (%) 9.4+ / - 0.0 10.1+ / - 0.2 7.4%
[0200] Handsheet Tensile Strength (kN / m) 1.8+ / - 0.1 1.6+ / - 0.1 -11.1% Handsheet Zero Span Tensile Strength (kg-f) 8.41 + / -0.32 8.20 + / - 0.34 -2.5% Compositional information wt% % Removed Ash(%) 6.2 5.8 6.5%
[0201] Klason Lignin (%) 14.2+ / - 0.1 14.3+ / - 0.3 -0.7%
[0202] Acid soluble Lignin (%) 0.9+ / - 0.0 0.9+ / - 0.1 0.0%
[0203] % Lignin Level 15.2+ / - 0.1 15.2+ / - 0.3 0.0%
[0204]
[0205] INVENTIVE EXAMPLE 1 -Ethyl Acetate Leaching of Reclaimed Post-Consumer Pulp Composition in Paperboard Form to Produce a Purified Post-Consumer Recycled Pulp Composition
[0206] 2,500 grams of ethyl acetate was added to a 5L stirred round bottom flask. The flask was outfitted with a mechanical stirrer, one reflux condenser, and one heat jacket. The mechanicalstirring was set to 400 rpm. The heating jacket was controlled by a variable voltage transformer. The heat was applied to rapidly bring the ethyl acetate to boiling (-77.1 °C) in about 5 minutes. After reaching the boiling point of ethyl acetate, the heat input was lowered to achieve a consistent reflux rate of -10 ml / min at the boiling point of ~77.1°C. Contaminated pulp composition in the form of Reclaimed Post-Consumer Pulp Composition in paperboard form was cut into 1 cm X 1 cm squares. The -250 grams of the cut Reclaimed Post-Consumer Pulp Composition in paperboard form was added to the round bottom flask which contained the boiling ethyl acetate. The extraction was continued for -30 minutes. The stirring was terminated, and the heat was removed. The ethyl acetate was decanted from the mixture of solids and liquids. An additional 2,500 grams of preheated fresh ethyl acetate at or near the boiling point was added to the paperboard in the 5L round bottom to complete a second extraction step. Stirring was started at 400 to 500 rpm while heating was applied sufficient to reflux the ethyl acetate at -10 mL / min. The time to reach reflux after the addition of fresh ethyl acetate to the paperboard was -5 minutes. The 2nd extraction continued for a total of -30 minutes. The stirring was stopped, and the heat removed. The ethyl acetate was decanted off. An additional 2,500 grams of preheated fresh ethyl acetate at or near the boiling point was added to the paperboard in the 5L round bottom to complete a third extraction step. Stirring was started at 400 to 500 rpm while heating was applied sufficient to reflux the ethyl acetate at -10 mL / min. The time to reach reflux after the addition of fresh ethyl acetate to the paperboard was -5 minutes. The 3rd extraction continued for a total of -30 minutes. The stirring was stopped, and the heat removed. The ethyl acetate was decanted off. An additional 2,500 grams of preheated fresh ethyl acetate at or near the boiling point was added to the paperboard in the 5L round bottom to complete a fourth extraction step. Stirring was started at 400 to 500 rpm while heating was applied sufficient to reflux the ethyl acetate at -10 mL / min. The time to reach reflux after the addition of fresh ethyl acetate to the paperboard was -5 minutes. The 4th extraction continued for a total of -30 minutes. The stirring was stopped, and the heat removed. The ethyl acetate was decanted off. The paperboard contained a small amount of contaminated solvent residual within the porosity of the paperboard. This wet paperboard was placed in a filter funnel with 60 mesh grating to further remove residual ethyl acetate via gravity. The paperboard was then completely dried of contaminated solvent at room temperature over-night to produce the Purified Pulp Composition or specifically Recycled Post-Consumer Pulp. The leaching solvent to pulp composition ratio per stage was -10:1 for four stages giving a total solvent to pulp composition ratio of -40:1. The leaching time per stage was approximately -35 minutes per stage for a total time of -140 minutes. The pulp composition before and after purification were analyzed for theclasses of chemical contaminants typically present in recycled materials by GALAB Laboratories GmbH (Am Schleusengraben 7, 21029 Hamburg, Germany) using the methods disclosed in section IX Methods, as shown in Table #3. For the contaminants DEET, glyphosphate, isononylphenolmonoethoxylate, isononylphenoldiethoxylate, isononylphenoltriethoxylate, isononylphenoltetraethoxylate, bisphenol A, 1,2,3,4,6,7,8-HpCDD, OCDD, OCDF, PCB 81, PCB 105, PCB 118, di2-ehtylhexylphthalate, diisononylphthalate, fluoranthene, and phenanthrene, the % removal was 74.6%, >91.7%, >93.5%, >83.9%, >85.7%, >70.6%, >96.9%, 68.0%, 75.4%, 82.5%, 87.5%, 85.8%, 87.0%, 93.4%, 84.4%, >94.1%, and 86.9%, respectively, which was indicative of outstanding removal across a broad spectrum of chemical species and classifications.
[0207] The Pulp Composition before and after the purification was characterized for water retention value. The solvent leaching resulted in a 4.8% increase in the water-retention value which may be indicative of decreased hornification, which is opposite the trend observed with traditional water washing.
[0208] The Pulp Composition before and after the purification were processed into handsheets following Tappi T205 to produce a recycled paperboard and then evaluated for tensile properties and chemical composition. The solvent leaching resulted in an 11% reduction in tensile strength despite the decreased hornification. The solvent leaching process did not remove significant ash but did significantly remove lignin at 10% removal from the pulp fibers, which is indicative of some lignin extraction possibly due to favorable partitioning between the solvent and the cellulose-based paper fibers.TABLE 3
[0209] Purification of Reclaimed Post-Consumer Fiber #1 to Produce Post-Consumer Recycled Fiber using Stirred Tank Reactor Flooded Leaching with Ethyl Acetate at Boiling Point
[0210] Reclaimed Post-Consumer Pulp Composition
[0211] Before After
[0212] % Removed Purification Purification
[0213] LOQ xLOQ xLOQ
[0214] Pesticides
[0215] Diethyltoluamide (DEET) 10 ppb 28.0 7.1 74.6%
[0216] Glyphosate 10 ppb 12.0 <1 >917%
[0217] Alkylphenol ethoxylates
[0218] iso-Nonylphenolmonoethoxylate 50 ppb 4.0 <1 > 93.5% iso-Nonylphenoldiethoxylate 50 ppb 6.2 <1 > 83.9% iso-Nonylphenoltri ethoxylate 50 ppb 7.0 <1 > 85.7% iso-Nonylphenoltetraethoxylate 50 ppb 3.4 <1 > 70.6% Bisphenols
[0219] BisphenolA 5 ppb 32.0 <1 > 969% Dioxins and dioxinlike and PCB
[0220] 1,2,3,4,6,7,8-HpCDD 0.2 ppTr 145.5 46.5 68.0%
[0221] OCDD 0.2 ppTr 1355.0 333.0 75.4%
[0222] OCDF 0.2 ppTr 43.8 7.7 S2.5%
[0223] PCB 81 0.05 ppTr 131.0 16.4 87.5%
[0224] PCB 105 5 ppTr 73.2 10.4 85.8%
[0225] PCB 118 10 ppTr 68.9 9.0 87.0%
[0226] Phthalates
[0227] Di -2-ethylhexy I phthalate 50 ppb 134.0 8.8 93.4%
[0228] Diisononyl phthalate 50 ppb 100.0 15.6 84.4%
[0229] Polycyclic aromatic hydrocarbons (PAH)
[0230] Fluoranthene 1 ppb 17.0 <1 >94.1% Phenanthrene Ippb 13.0 1.7 86.9%
[0231] % Increase
[0232] Water Retention Value (g / g) 1.25+ / - 0.1 1.31+ / - 0.19 4,8%
[0233] FQA Fines Level (%) 9.4+ / - 0.0 9.6+ / - 0.2 2 1%
[0234] Handsheet Tensile Strength (kN / m) 1.8 + / ■ 0.1 1.6 + / ■ 0.1 -11.1% Handsheet Zero Span Tensile Strength (kg-f) 8.41 + / -0.32 8.16+ / - 0.40 -3.1% Compositional Information wt% % Removed
[0235] Ash(%) 6.2 6.8 -9.7%
[0236] Klason Lignin (%) 14.2+ / - 0.1 12.8+7-0.1 9.9%
[0237] Acid soluble Lignin (%) 0.9 + / - 0.0 0.9 + / -0.0 0.0%
[0238] % Lignin Level 15.2+ / - 0.1 13.7+ / - 0.1 9.9%
[0239]
[0240] INVENTIVE EXAMPLE 2 -Acetone Leaching of Reclaimed Post-Consumer Pulp Composition in Paperboard Form to Produce a Purified Post-Consumer Recycled Pulp Composition
[0241] 2,500 grams of acetone was added to a 5L stirred round bottom flask. The flask was outfitted with a mechanical stirrer, one reflux condenser, and one heat jacket. The mechanical stirring was set to 400 rpm. The heating jacket was controlled by a variable voltage transformer. The heat was applied to rapidly bring the acetone to boiling (~52°C) in about 5 minutes. After reaching the boiling point of acetone, the heat input was lowered to achieve a consistent reflux rateof -10 ml / min at the boiling point of ~52°C. Contaminated pulp composition in the form of Reclaimed Post-Consumer Pulp Composition in paperboard form was cut into 1 cm X 1 cm squares. The -250 grams of the cut recycled Reclaimed Post-Consumer Fiber #1 was added to the round bottom flask which contained the boiling acetone. The extraction was continued for -30 minutes. The stirring was terminated, and the heat was removed. The acetone was decanted from the mixture of solids and liquids. An additional 2,500 grams of preheated fresh acetone at or near the boiling point was added to the paperboard in the 5L round bottom to complete a second extraction step. Stirring was started at 400 to 500 rpm while heating was applied sufficient to reflux the acetone at -10 mL / min. The time to reach reflux after the addition of fresh acetone to the paperboard was -5 minutes. The 2nd extraction continued for a total of -30 minutes. The stirring was stopped, and the heat removed. The acetone was decanted off. An additional 2,500 grams of preheated fresh acetone at or near the boiling point was added to the paperboard in the 5L round bottom to complete a third extraction step. Stirring was started at 400 to 500 rpm while heating was applied sufficient to reflux the acetone at -10 mL / min. The time to reach reflux after the addition of fresh acetone to the paperboard was -5 minutes. The 3rd extraction continued for a total of -30 minutes. The stirring was stopped, and the heat removed. The acetone was decanted off. An additional 2,500 grams of preheated fresh acetone at or near the boiling point was added to the paperboard in the 5L round bottom to complete a fourth extraction step. Stirring was started at 400 to 500 rpm while heating was applied sufficient to reflux the acetone at -10 mL / min. The time to reach reflux after the addition of fresh acetone to the paperboard was -5 minutes. The 4th extraction continued for a total of -30 minutes. The stirring was stopped, and the heat removed. The acetone was decanted off. The paperboard contained a small amount of contaminated solvent residual within the porosity of the paperboard. This wet paperboard was placed in a filter flask w / o vacuum to further remove residual acetone. The paperboard was then completely dried of contaminated solvent at room temperature over-night to produce the Purified Pulp Composition or specifically Recycled Post-Consumer Pulp. The leaching solvent to pulp composition ratio per stage was -10:1 for four stages giving a total solvent to pulp composition ratio of -40:1. The leaching time per stage was approximately -35 minutes per stage for a total time of -140 minutes. The Pulp Composition before and after purification were analyzed for the classes of chemical contaminants typically present in recycled materials by GALAB Laboratories GmbH (Am Schleusengraben 7, 21029 Hamburg, Germany) using the methods disclosed in section IX Methods, as shown in Table #4. For the contaminants For the contaminants DEET, glyphosphate, isononylphenolmonoethoxylate, isononylphenoldiethoxylate, isononylphenoltriethoxylate,isononylphenoltetraethoxylate, bisphenol A, 1,2,3,4,6,7,8-HpCDD, OCDD, OCDF, PCB 81, PCB 105, PCB 118, di2-ehtylhexylphthalate, and diisononylphthalate, the % removal was 85.7%, > 91.7%, > 75.0%, > 83.9%, > 85.7%, > 70.6%, > 96.9%, 89.1%, 89.8%, 85.6%, > 96.7%, 94.8%, 95.1%, 94.9%, and 12.0%, which was indicative of outstanding removal across a broad spectrum of chemical species and classifications.
[0242] The Pulp Composition before and after the purification was characterized for water retention value. The solvent leaching resulted in a 3.2% increase in the water-retention value which may be indicative of decreased hornification, which is opposite the trend observed with traditional water washing.
[0243] The Pulp Composition before and after the purification were processed into handsheets following Tappi T205 to produce a recycled paperboard and then evaluated for tensile properties and chemical composition. The solvent leaching resulted in a 17% increase in tensile strength possibly due to the decreased hornification. The solvent leaching process did not remove significant ash but did significantly remove lignin at -15% reduction from the pulp fibers, which is indicative of some lignin extraction possibly due to favorable partitioning between the solvent and the cellulose-based paper fibers.TABLE 4
[0244] Purification of Method Using Current Invention involving Acetone Leaching of Reclaimed Post- Consumer of Reclaimed Post-Consumer Pulp Composition in Paperboard Form to Produce a Purified Post-Consumer Recycled Pulp Composition
[0245] Reclaimed Post-Consumer Pulp Composition
[0246] Before After
[0247] % Removed Purification Purification
[0248] LOQ xLOQ xLOQ
[0249] Pesticides
[0250] Diethyltoluamide (DEET) lOppb 28.0 4.0 85-7% Glyphosate lOppb 12.0 <1 > 91.7% Alkylphenol ethoxylates
[0251] iso-Nonylphenolmonoethoxylate 50ppb 4.0 <1 > 75.0% iso-Nonylphenoldiethoxylate 50 ppb 6.2 <1 >839% iso-Nonylphenoltri ethoxylate 50ppb 7.0 <1 >85.7% iso-Nonylphenoltetraethoxylate 50 ppb 3.4 <1 >706% Bisphenols
[0252] Bisphenol A 50 ppb 32.0 <1 > 96.9% Dioxins and dioxinlike and PCB
[0253] 1,2,3,4,6,7,8-HpCDD 0.2 ppTr 145.5 15.8 89.1% OCDD 0.2 ppTr 1355.0 138.0 89.8% OCDF 0.2ppTr 43.8 6.3 55.6% PCB 81 0.05 ppTr 30.0 <1 > 96.7% PCB 105 5 ppTr 73.2 3.8 94.8% PCB 118 10 ppTr 68.9 3.4 95.1% Phthalates
[0254] Di-2-ethylhexyl phthalate 50 ppb 134.0 6.8 94.9% Diisononyl phthalate 50 ppb 100.0 88.0 12.0% Polycyclic aromatic hydrocarbons (PAH }
[0255] Fluoranthene 1 ppb 17.0 dnt n.a. Phenanthrene Ippb 13.0 dnt n.a.
[0256] % Increase
[0257] Water Retention Value (g / g) 1.25+ / -0.1 1.29+ / - 0.15 3.2%
[0258] FQA Fines Level (%) 9.4+ / - 0.0 9.5+ / -0.1 1.1%
[0259] Handsheet Tensile Strength (kN / m) 1.8+ / - 0.1 2.1+ / -0.1 16.7%
[0260] Handsheet Zero Span Tensile Strength (kg-f) 8.41 + / - 0.32 9.31+ / - 0.44 10.7% Compositional Information wt% % Removed
[0261] Ash(%i 6.2 6.1 1.6%
[0262] Klason Lignin (%) 14.2+ / - 0.1 12.0+ / - 0.1 15.5%
[0263] Acid soluble Lignin i%) 0.9+ / - 0.0 1.0+ / - 0.0 ■11.1%
[0264] % Lignin Level 15.2+ / - 0.1 12.9+ / - 0.1 15.1%
[0265]
[0266] VIII. Sanitary Tissue
[0267] In some embodiments, recycled cellulosic pulp compositions may be incorporated into inventive sanitary tissue products.
[0268] Without wishing to be bound by theory, the inventors have unexpectedly found the recycled pulp fiber described herein may not only exhibit a lower level of trace chemicals, but also may exhibit improved levels of pulp performance as measured by the purer recycle pulp fiber propertiesof Water Retention Value, Fines Level (Lw), Handsheet Tensile Strength, Handsheet Zero Span Tensile, and combinations of these performance factors as well. The recycled pulp fiber described herein may be unexpectedly rejuvenated in these pulp performance factors as well as exhibiting low levels of trace chemicals. Inventive sanitary tissue products comprising the recycled pulp fiber described herein may not only exhibit lower levels of trace chemicals, but also may exhibit sanitary tissue high performance levels of dry strength, wet strength, modulus, elongation, wet burst, their intensive properties, such as basis weight or density, or by their roll properties, such as roll bulk or roll compressibility, or by other finished product characterizations.
[0269] The inventive sanitary tissue products may comprise a plurality of dry fibrous structure sheets, wherein the sanitary tissue product comprises from about 30 wt.% to about 100 wt.% postconsumer recycled pulp fiber. In some embodiments the sanitary tissue product comprises from about 40 wt% to about 100 wt%, from about 50 wt% to about 100 wt%, from about 60 wt% to about 100 wt%, from about 70 wt% to about 100 wt%, from about 75wt% to about 100 wt%, from about 80 wt% to about 100 wt%, from about 85 wt% to about 100 wt%, from about 90 wt% to about 100 wt%, from about 30 wt% to about 80 wt%, from about 30 wt% to about 90 wt%, from about 40 wt% to about 90 wt%, from about 50 wt% to about 90 wt% post-consumer recycled pulp fiber.
[0270] The sanitary tissue products of the present invention may exhibit a basis weight between about 5 g / m2to about 120 g / m2and / or from about 10 g / m2to about 120 g / m2and / or from about 15 g / m2to about 110 g / m2and / or from about 20 g / m2to about 100 g / m2and / or from about 30 to 90 g / m2as measured according to the Basis Weight Test Method described herein. In addition, the sanitary tissue product of the present invention may exhibit a basis weight between about 40 g / m2to about 120 g / m2and / or from about 50 g / m2to about 110 g / m2and / or from about 55 g / m2to about 105 g / m2and / or from about 60 to 100 g / m2as measured according to the Basis Weight Test Method described herein.
[0271] The sanitary tissue products of the present invention may exhibit an initial total wet tensile strength of less than about 78 g / cm (200 g / in) and / or less than about 59 g / cm (150 g / in) and / or less than about 39 g / cm (100 g / in) and / or less than about 29 g / cm (75 g / in).
[0272] The sanitary tissue products of the present invention may exhibit an initial total wet tensile strength of at least 118 g / cm (300 g / in) and / or at least 157 g / cm (400 g / in) and / or at least 196 g / cm (500 g / in) and / or at least 236 g / cm (600 g / in) and / or at least 276 g / cm (700 g / in) and / or at least 315 g / cm (800 g / in) and / or at least 354 g / cm (900 g / in) and / or at least 394 g / cm (1000 g / in) and / or from about 118 g / cm (300 g / in) to about 1968 g / cm (5000 g / in) and / or from about 157 g / cm (400g / in) to about 1181 g / cm (3000 g / in) and / or from about 196 g / cm (500 g / in) to about 984 g / cm (2500 g / in) and / or from about 196 g / cm (500 g / in) to about 787 g / cm (2000 g / in) and / or from about 196 g / cm (500 g / in) to about 591 g / cm (1500 g / in) as measured according to the Initial Total Wet Tensile Test Method described herein.
[0273] The sanitary tissue products of the present invention or kitchen towel grade sanitary tissue may exhibit a sanitary tissue or kitchen towel wet burst (peak load) strength of greater than about 3 g, greater than about 5 g, or greater than about 10 g, or greater than about 20 g, or greater than about 50 g, or greater than about 55 g, or greater than about 75 g, or greater than about 100 g, or greater than about 115 g, or greater than about 150 g, or greater than about 177 g, or greater than about 200 g, or greater than about 300 g, or greater than about 350 g, or greater than about 400 g, or greater than about 450 g, or greater than about 478 g, or greater than about 500 g, or greater than about 550 g, or greater than about 600 g, or between about 20 g and about 530 g, or between about 3 g and about 22 g, or between about 9g and about 40 g, or between about 25 g and about 52 g, or between about 230 g and about 525 g, or between about 180 g and about 525 g, or between about 200 g and about 700 g, or between 30 about 350 g and about 600 g, or between about 350 g and about 550 g, or between about 400 g and about 550 g, or between about 400 g and about 525 g, or between about 50 g and about 220 g, or between about 50 g and about 60 g, or between about 50 g and 55 g, specifically reciting all increments of 10 g within the above-recited ranges and all ranges formed therein or thereby.
[0274] The sanitary tissue products of the present invention may exhibit a density of less than about 0.60 g / cm3and / or less than about 0.30 g / cm3and / or less than about 0.20 g / cm3and / or less than about 0.10 g / cm3and / or less than about 0.07 g / cm3and / or less than about 0.05 g / cm3and / or from about 0.01 g / cm3to about 0.20 g / cm3and / or from about 0.02 g / cm3to about 0.10 g / cm3as measured according to the Density Test Method described herein.
[0275] The sanitary tissue of the present invention may be in the form of a roll of fibrous structure (single-ply or multiply), for example a dry fibrous structure roll, and may exhibit a roll bulk (in units of cm3 / g) of greater than 4 and / or greater than 6 and / or greater than 8 and / or greater than 10 and / or greater than 12 and / or to about 20 and / or to about 18 and / or to about 16 and / or to about 14 and / or from about 4 to about 20 and / or from about 4 to about 12 and / or from about 8 to about 20 and / or from about 12 to about 16.
[0276] The sanitary tissue of the present invention may be in the form of a roll of fibrous structure (single-ply or multiply), for example a dry fibrous structure roll, and may exhibit a % compressibility or % roll compressibility (in units of %) of less than 10 and / or less than 8 and / orless than 7 and / or less than 6 and / or less than 5 and / or less than 4 and / or less than 3 to about 0 and / or to about 0.5 and / or to about 1 and / or from about 4 to about 10 and / or from about 4 to about 8 and / or from about 4 to about 7 and / or from about 4 to about 6 as measured according to the Percent Roll Compressibility Test Method described herein.
[0277] The sanitary tissue products of the present invention may be in the form of sanitary tissue product rolls. Such sanitary tissue product rolls may comprise a plurality of connected, but perforated sheets of fibrous structure, that are separably dispensable from adjacent sheets. In one example, one or more ends of the roll of sanitary tissue product may comprise an adhesive and / or dry strength agent to mitigate the loss of fibers, especially wood pulp fibers from the ends of the roll of sanitary tissue product.
[0278] The sanitary tissue products of the present invention may comprise additives such as softening agents, temporary wet strength agents, permanent wet strength agents, bulk softening agents, lotions, silicones, wetting agents, latexes, especially surface-pattern-applied latexes, dry strength agents such as carboxymethylcellulose and starch, absorbency aids, and other types of additives suitable for inclusion in and / or on sanitary tissue products.
[0279] In one example, the sanitary tissue product may exhibit a geometric mean (GM) Peak Elongation of greater than 3%, greater than 5%, greater than 7.5%, greater than 10% and / or greater than 15% and / or greater than 20% and / or greater than 25% as measured according to the Tensile Test Method described herein.
[0280] In another example, the dry fibrous structures of the present invention exhibit a geometric mean (GM) Dry Tensile Strength of greater than 200 g / in and / or greater than 250 g / in and / or greater than 300 g / in and / or greater than 350 g / in and / or greater than 400 g / in and / or greater than 500 g / in and / or greater than 750 g / in as measured according to the Tensile Test Method described herein.
[0281] In still another example, the dry fibrous structures of the present invention exhibit a geometric mean (GM) Modulus of less than 20,000 g / cm and / or less than 15,000 g / cm and / or less than 10,000 g / cm and / or less than 5,000 g / cm and / or less than 3,000 g / cm and / or less than 1,500 g / cm and / or less than 1,200 g / cm to about 0 g / cm and / or to about 100 g / cm and / or to about 300 g / cm and / or to about 500 g / cm and / or to about 700 g / cm at 15 g / cm as measured according to the Tensile Test Method described herein.
[0282] The dry fibrous structures of the present invention may further comprise a skin care lotion or a carrier lotion. Examples of suitable lotions include, but are not limited to, those described in U.S. Pat. Nos. 5,607,760; 5,609,587; 5,635,191; 5,643,588; and 5,968,025, and as described inU.S. Application No. 61 / 391,353. Alternatively, sections of the dry fibrous structure may comprise the skin care lotion, and in one embodiment, the skin care lotion may be stripes oriented in a longitudinal direction of the dry fibrous structure.
[0283] Bath Tissue
[0284] An example of fibrous structures or sanitary tissue or sanitary bath tissue in accordance with the present disclosure may be prepared using a papermaking machine or process as described above or according to the method described below:
[0285] An aqueous slurry of eucalyptus pulp fibers is prepared at about 3% fiber by weight using a conventional repulper, then transferred to a hardwood fiber stock chest. The eucalyptus fiber 10 slurry of the hardwood stock chest is pumped through a stock pipe to a hardwood fan pump where the slurry consistency is reduced from about 3% by fiber weight to about 0.15% by fiber weight. The 0.15% eucalyptus slurry is then pumped and distributed in the top chamber of a multi-layered, three-chambered headbox of a Fourdrinier wet-laid papermaking machine.
[0286] Additionally, an aqueous slurry of post-consumer recycled pulp fiber is prepared at about 1.5-3% fiber by weight using a conventional repulper, then transferred to a fiber stock chest. The post-consumer recycled pulp fiber slurry may optionally be pumped through a stock pipe to be refined to a Canadian Standard Freeness (CSF) of about 630. Next, the post-consumer recycled pulp fiber is directed to a fan pump where its consistency is reduced from about 1.5-3% by fiber weight to about 0.15% by fiber weight. The post-consumer recycled pulp fiber slurry is then directed and distributed to the center and bottom chamber of a multi-layered, three-chambered headbox of a Fourdrinier wet-laid papermaking machine.
[0287] In order to impart temporary wet strength to the finished fibrous structure, a 1% dispersion of temporary wet strengthening additive (e.g., Fennorez® 91 commercially available from Kemira) is prepared and is added to the post-consumer recycled pulp fiber or eucalyptus fiber stock pipe at a rate sufficient to deliver 0.25% temporary wet strengthening additive based on the dry weight of the fibers. The absorption of the temporary wet strengthening additive is enhanced by passing the treated slurry through an in-line mixer.
[0288] The wet-laid papermaking machine has a layered headbox having a top chamber, a center chamber, and a bottom chamber where the chambers feed directly onto the forming wire (Fourdrinier wire). The eucalyptus fiber slurry of 0.15% consistency is directed to the top headbox chamber. The post-consumer recycled pulp fiber slurry is directed to the center and bottom headbox chambers. All three fiber layers are delivered simultaneously in superposed relation ontothe Fourdrinier wire to form thereon a three-layer embryonic fibrous structure (web), of which about 20% of the top side is made up of the eucalyptus and about 80% of the sheet can be made of post-consumer recycled pulp fibers, directed towards the center and bottom layers. Dewatering occurs through the Fourdrinier wire and is assisted by a deflector and wire table vacuum boxes. The Fourdrinier wire is a Legent 866A Dual Layer (0.11 mm x 0.18 mm, Asten Johnson). The speed of the Fourdrinier wire is about 800 feet per minute (fpm).
[0289] The embryonic wet fibrous structure is transferred from the Fourdrinier wire, at a fiber consistency of about 18-22% at the point of transfer, to a 3D patterned, continuous knuckle, through-air-drying belt. The speed of the 3D patterned through-air20 drying belt is 800 feet per minute (fpm), which is the same speed of the Fourdrinier wire. The 3D patterned through-air-drying belt is designed to yield a fibrous structure comprising a pattern of continuous high density knuckle region oriented approximately 75 Degrees relative to the cross direction. Each continuous high density knuckle region oriented approximately 75 Degrees relative to the cross direction is separated by a low-density discrete pillow region oriented approximately 75 Degrees relative to the cross direction. This 3D patterned through-air-drying belt is formed by casting a layer of an impervious resin surface of a continuous knuckle onto a fiber mesh supporting fabric. The supporting fabric is a 98 x 52 filament, dual layer mesh. The thickness of the resin cast is about 12.0 mils above the supporting fabric. Alternatively, the drying fabric is designed to yield a pattern of substantially machine direction oriented linear channels having a continuous network of high density (knuckle) areas. This drying fabric is formed by casting an impervious resin surface onto a fiber mesh supporting fabric. The supporting fabric is a 98 * 52 filament, dual layer mesh. The thickness of the resin cast is about 12 mils above the supporting fabric. The area of the continuous network is about 40 percent of the surface area of the drying fabric.
[0290] Further de-watering of the fibrous structure is accomplished by vacuum assisted drainage until the fibrous structure has a fiber consistency of about 20% to 30%.
[0291] While remaining in contact with the 3D patterned through-air-drying belt, the fibrous structure is pre-dried by air blow-through pre-dryers to a fiber consistency of about 50-65% by weight.
[0292] After the pre-dryers, the semi-dry fibrous structure is transferred to a Yankee dryer and adhered to the surface of the Yankee dryer with a sprayed creping adhesive. The creping adhesive is an aqueous dispersion with the actives consisting of about 80% polyvinyl alcohol (PVA 88-44), about 20% CREPETROL® 5688. CREPETROL® 5688 is commercially available from Solenis. The creping adhesive is delivered to the Yankee surface at a rate of about 0.10- 0.20% adhesivesolids based on the dry weight of the fibrous structure. The fiber consistency is increased to about 96-98% before the fibrous structure is dry-creped from the Yankee with a doctor blade.
[0293] The doctor blade has a bevel angle of about 15-25° and is positioned with respect to the Yankee dryer to provide an impact angle of about 71-81°. The Yankee dryer is operated at a temperature of about 275-350°F and a speed of about 800 fpm. The fibrous structure is wound in a roll (parent roll) using a surface driven reel drum having a surface speed of about 550-700 fpm.
[0294] Two parent rolls of the fibrous structure are then converted into a sanitary tissue product by loading the roll of fibrous structure into an unwind stand. The two parent rolls are converted with the low-density pillow side out. Alternatively, they can be converted with the high-density knuckle side out. The line speed is 550 ft / min. One parent roll of the fibrous structure is unwound and transported to an emboss stand where the fibrous structure is strained to form the emboss pattern in the fibrous structure via a 0.56” Pressure Roll Nip and then combined with the fibrous structure from the other parent roll to make a multi-ply (2-ply) sanitary tissue product. Approximately 0.5% of a proprietary quaternary amine softener may also be added to the bottom side of the multi-ply sanitary tissue product. The multi-ply sanitary tissue product is then transported to a winder where it is wound onto a core to form a log. The log of multi -ply sanitary tissue product is then transported to a log saw where the log is cut into finished multi-ply sanitary tissue product rolls. The molding member used to make the multi-ply sanitary tissue product of this example exhibits the dimensions shown in Table 4 of U.S. Serial No. 17 / 238,527 filed April 23, 2021, and assigned to The Procter & Gamble Company.
[0295] The bath tissue made via the above process may exhibit low levels of trace chemicals, such as shown in Inventive Examples 1 and 2, as well as one of more of the moisture content, GM Tensile Strength, density, basis weight, roll bulk, roll % compressibility, and initial total wet tensile strength properties as described herein.
[0296] Kitchen Paper Towel
[0297] An example of fibrous structures or sanitary tissue or kitchen paper towel in accordance with the present disclosure may be prepared using a papermaking process or machine as described above and according to the method described below:
[0298] Examples of dry fibrous structures or sanitary tissue; namely paper towels, are produced utilizing a cellulosic pulp fiber furnish consisting of about 85% post-consumer recycled pulp fiber and about 15% of unrefined hardwood Eucalyptus Bleached Kraft fiber furnish. The 85% post-consumer recycled pulp fiber may be refined as needed to maintain target wet burst at the reel. Any furnish preparation and refining methodology common to the papermaking industry can be utilized.
[0299] A 3% active solution Kymene 5221 is added to the refined softwood line prior to an in-line static mixer and 1% active solution of Wickit 1285, an ethoxylated fatty alcohol available from Ashland Inc. is added to the unrefined Eucalyptus Bleached Kraft hardwood furnish. The addition levels are 21 and 1 lbs active / ton of paper, respectively.
[0300] The post-consumer recycled pulp fiber and the unrefined hardwood Eucalyptus Bleached Kraft fiber furnish thick stocks are then blended into a single thick stock line followed by addition of 1% active carboxymethylcellulose (CMC-Finnfix) solution at 7 lbs active / ton of paper towel, and optionally, a softening agent may be added.
[0301] The thick stock is then diluted with white water at the inlet of a fan pump to a consistency of about 0.15% based on total weight of the papermaking fibers, including any optional broke fiber. The diluted fiber slurry is directed to a non-layered configuration headbox such that the wet web formed onto a Fourdrinier wire (foraminous wire). Optionally, a fines retention / drainage aid may be added to the outlet of the fan pump.
[0302] Dewatering occurs through the Fourdrinier wire and is assisted by deflector and vacuum boxes. The Fourdrinier wire is of a 5-shed, satin weave configuration having 87 machine-direction and 76 cross-direction monofilaments per inch, respectively. The speed of the Fourdrinier wire is about 750 fpm (feet per minute).
[0303] The embryonic wet web is transferred from the Fourdrinier wire at a fiber consistency of about 24% at the point of transfer, to a belt, such as a patterned belt through-air-drying resin carrying fabric. In the present case, the speed of the patterned through-air-drying fabric is approximately the same as the speed of the Fourdrinier wire. In another case, the embryonic wet web may be transferred to a patterned belt and / or fabric that is traveling slower, for example about 20% slower than the speed of the Fourdrinier wire (for example a wet molding process). Further de-watering is accomplished by vacuum assisted drainage until the web has a fiber consistency of about 30%.
[0304] While remaining in contact with the patterned belt, the web is pre-dried by air blow-through pre-dryers to a fiber consistency of about 65% by weight.
[0305] After the pre-dryers, the semi -dry web is transferred to a Yankee dryer and adhered to the surface of the Yankee dryer with a sprayed creping adhesive. The creping adhesive is an aqueous dispersion with the actives consisting of about 75% polyvinyl alcohol, and about 25% CREPETROL® R6390. Optionally, a crepe aid consisting of CREPETROL® A3025 may beapplied. CREPETROL® R6390 and CREPETROL® A3025 are commercially available from Ashland Inc., (formerly Hercules Inc.). The creping adhesive diluted to about 0.15% adhesive solids and delivered to the Yankee surface at a rate of about 2# adhesive solids based on the dry weight of the web. The fiber consistency is increased to about 97% before the web is dry creped from the Yankee with a doctor blade.
[0306] In the present case, the doctor blade has a bevel angle of about 45° and is positioned with respect to the Yankee dryer to provide an impact angle of about 101° and the reel is run at a speed that is about 15% faster than the speed of the Yankee. In another case, the doctor blade may have a bevel angle of about 25° and be positioned with respect to the Yankee dryer to provide an impact angle of about 81° and the reel is run at a speed that is about 10% slower than the speed of the Yankee. The Yankee dryer is operated at a temperature of about 177°C. and a speed of about 800 fpm. The fibrous structure is wound in a roll using a surface driven reel drum having a surface speed of about 656 feet per minute.
[0307] The fibrous structure may be subsequently converted into a two-ply paper towel product having a basis weight of about 45 to 54 g / m2 and it exhibits low levels of trace chemicals consistent with Inventive Examples 1 and 2.
[0308] In some embodiments, the present invention is a sanitary tissue comprising a plurality of dry fibrous structure sheets, wherein the sanitary tissue comprises from about 30 wt.% to about 100 wt.% post-consumer recycled pulp fiber; and further comprises at least one of the following:
[0309] a. less than about 100 pg / kg of glyphosphate;
[0310] b. less than 150 pg / kg of isononylphenol(mono, di, tri, and tetra)exthoxylate; c. less than 150 pg / kg of Bisphenol-A;
[0311] d. less than 25 ng / kg of 1,2,3,4,6,7,8-HpCDD;
[0312] e. less than 250 ng / kg of OCDD;
[0313] f. less than 5 ng / kg of OCDF;
[0314] g. less than 4 ng / kg of PCB 81;
[0315] h. less than 350 ng / kg of PCB 105;
[0316] i. less than 50 ng / kg of PCB 118;
[0317] j. less than 5,000 pg / kg of di-2ethylhexylphthalate;
[0318] k. less than 5,000 pg / kg of di-isononylphthalate;
[0319] l. less than 10 pg / kg of fluoranthene; and
[0320] m. less than 10 pg / kg of phenanthene;
[0321] as measured according to the Trace Chemicals Test Method.In some embodiments, the sanitary tissue may comprise at least 4 of (a) - (m), at least 9 of (a) - (m), or all of (a) - (m).
[0322] In some embodiments, the sanitary tissue may comprise a residual solvent content of less than 1000 ppm, as measured according to the Trace Chemicals Test Method.
[0323] In some embodiments, the sanitary tissue may comprise from about 75 wt% to about 100 wt% post-consumer recycled pulp fiber, from about 85 wt% to about 100 wt% post-consumer recycled pulp fiber, or from about 90 wt% to about 100 wt% post-consumer recycled pulp fiber.
[0324] In some embodiments, the sanitary tissue comprises a plurality of dry fibrous structure sheets, in which the tissue, and / or the sheets, are in a roll.
[0325] In some embodiments, the sanitary tissue may exhibit one or more, in some embodiments two or more, or in some embodiments all, of the following properties:
[0326] a) a moisture content of less than 20% by weight of the sanitary tissue as measured according to the Water Content Test Method;
[0327] b) a GM Tensile Strength of greater than 200 g / in as measured according to the Tensile Test Method;
[0328] c) a density of less than about 0.60 g / cm3as measured according to the Density Test Method; and
[0329] d) a basis weight of greater than 5 g / m2to about 120 g / m2as measured according to the Basis Weight Test Method; and
[0330] e) wherein the sanitary tissue is on a roll and exhibits the following properties: i. a roll bulk of greater than 4 cm3 / g; and
[0331] ii. a % roll compressibility of less than 10% as measured according to the Percent Compressibility Test Method.
[0332] In some embodiments, the sanitary tissue is a multi-layered tissue web comprising a first fibrous layer and a second fibrous layer, wherein the first fibrous layer comprises wood fibers and the second fibrous layer comprises the post-consumer recycled pulp fiber.
[0333] IX. TEST METHODS
[0334] 1. TRACE CHEMICALS TEST METHOD
[0335] The content on a mass per mass basis of trace chemicals present in recycled pulp, tissue comprising recycle pulp, or packaging material comprising recycle pulp is determined using methods containing sample extraction and instrumental analysis approaches known of those of skill in the art and understood to be capable of extracting and detecting essentially all of a particulartrace chemical in these materials. Suitable overall method specifics vary based on the particular trace chemical being quantified, though a common overall method structure is generally followed. A suitable method generally begins with increasing the surface area of a representative recycled pulp, tissue comprising recycle pulp, or packaging material comprising recycle pulp sample by cutting, shredding, and / or milling into small particles. An extraction step is then performed using a solvent capable of dissolving or diffusing into the sample and in which the trace chemical is readily soluble. The extraction process conditions (e.g., time and temperature) are optimized to maximize trace chemical recovery and common approaches include but are not limited to Soxhlet extraction, accelerated solvent extraction, and / or ultrasonic extraction. Internal standards (usually stable-isotope-labeled versions of the trace chemicals if mass spectrometry-based detection approaches are used) are added during the extraction step to account for potential losses during extraction and subsequent processing steps. After extraction is complete, the extraction solvent is isolated and worked up for instrumental analysis. Depending on the solvent used for extraction, the required quantitation limit, and the specific instrumental approach used, generation of a specimen suitable for instrumental analysis may require multiple cleanup and / or concentration steps including but not limited to centrifugation / filtration, liquid / liquid extraction, and / or column chromatography. The trace chemical in the worked-up specimen is then quantified using instrumental methods (e.g., GC-MS, GC-MS / MS, GC-HRMS, LC-MS / MS, etc.,) known to those of skill in the art and specifically adapted to the trace chemical of interest. Suitable instrumental approaches may be developed de novo or may be based on standard, known methods for particular trace chemicals (e.g., US EPA Method 1613 in the case of dioxins and furans or US EPA 1668 for PCBs). Based on a combination of raw instrumental quantitative results, extraction solvent workup steps, original extraction volume, and starting specimen mass, the mass content of a trace chemical per mass of starting specimen material is calculated and is reported as the level of the trace chemical in the material tested. Given the generally low levels of trace chemicals present, common units used in reported levels of trace chemicals are pg / kg and ng / kg (equivalent to the ppb and ppt levels, respectively).
[0336] One of skill in the art will recognize that trace chemicals are often present at very low “trace” levels, meaning that under some circumstances, environmental and / or laboratory background levels of these same trace chemicals may give rise to false positive detects or falsely elevated results if appropriate precautions are not taken. While one of skill in the art recognizes that a suite of measures may be needed to minimize such false results, one obligatory measure isto include a true “blank” beginning with solvent carried in parallel through the extraction step, extraction solvent workup, and instrumental analysis.
[0337] Using the suitable overall methodology outlined above, one of skill in the art may quantify a range of trace chemicals potentially present in a recycled pulp, tissue comprising recycle pulp, or packaging material comprising recycle pulp sample of interest. For example, just to describe a few of the trace chemicals listed herein, the level of isononylphenol (CAS RN 11066-49-2) may be determined and reported as mass of trace chemical per mass of material in units of pg / kg. Similarly, the level of PCB 118 (CAS RN 31508-00-6) may be determined and reported in units of ng / kg, the level of OCDD (CAS RN 3268-87-9), a dioxin, may be determined and reported in units of ng / kg, the level of bisphenol A (CAS RN 80-05-7), also known as BPA, may be determined and reported in units of pg / kg, and the level of diisononyl phthalate (CAN RN 28553-12-0), also known as DINP, may be determined and reported in units of pg / kg.
[0338] 2. WATER CONTENT TEST METHOD
[0339] The water (moisture) content present in a fibrous structure is measured using the following Water Content Test Method.
[0340] A fibrous structure or portion thereof (“sample”) is placed in a conditioned room at a temperature of 73°F ± 4°F (about 23°C ± 2.2°C) and a relative humidity of 50% ± 10% for at least 24 hours prior to testing. The weight of the sample is recorded when no further weight change is detected for at least a 5 minute period. Record this weight as the “equilibrium weight” of the sample. Next, place the sample in a drying oven for 24 hours at 70°C with a relative humidity of about 4% to dry the sample. After the 24 hours of drying, immediately weigh the sample. Record this weight as the “dry weight” of the sample. The water (moisture) content of the sample is calculated as follows:
[0341] % Water (moisture) in sample = 100% x (Equilibrium weight of sample - Dry weight of sample)
[0342] Dry weight of sample
[0343] The % Water (moisture) in sample for 3 replicates is averaged to give the reported % Water (moisture) in sample.
[0344] 3. GM TENSILE STRENGTH AND OTHER TENSILE RELATED MEASURES
[0345] Tensile Test Method: Peak Elongation, Tensile Strength, TEA and Modulus
[0346] Peak Elongation, Tensile Strength, TEA and Tangent Modulus are measured on a constant rate of extension tensile tester with computer interface (a suitable instrument is the EJA Vantagefrom the Thwing-Albert Instrument Co., Wet Berlin, NJ) using a load cell for which the forces measured are within 10% to 90% of the limit of the cell. Both the movable (upper) and stationary (lower) pneumatic jaws are fitted with smooth stainless steel faced grips, 25.4 mm in height and wider than the width of the test specimen. An air pressure of about 60 psi is supplied to the jaws.
[0347] Eight usable units of a fibrous structure sample are divided into two stacks of four samples each. The samples in each stack are consistently oriented with respect to machine direction (MD) and cross direction (CD). One of the stacks is designated for testing in the MD and the other for CD. Using a one inch precision cutter (Thwing Albert JDC-1-10, or similar) cut 4 MD strips from one stack, and 4 CD strips from the other, with dimensions of 1.00 in ± 0.01 in wide by 3.0 - 4.0 in long. Each strip of one usable unit thick will be treated as a unitary specimen for testing.
[0348] Program the tensile tester to perform an extension test, collecting force and extension data at an acquisition rate of 20 Hz as the crosshead raises at a rate of 2.00 in / min (5.08 cm / min) until the specimen breaks. The break sensitivity is set to 80%, i.e., the test is terminated when the measured force drops to 20% of the maximum peak force, after which the crosshead is returned to its original position.
[0349] Set the gauge length to 1.00 inch. Zero the crosshead and load cell. Insert at least 1.0 in of the unitary specimen into the upper grip, aligning it vertically within the upper and lower jaws and close the upper grips. Insert the unitary specimen into the lower grips and close. The unitary specimen should be under enough tension to eliminate any slack, but less than 5.0 g of force on the load cell. Start the tensile tester and data collection. Repeat testing in like fashion for all four CD and four MD unitary specimens.
[0350] Program the software to calculate the following from the constructed force (g) verses extension (in) curve:
[0351] Tensile Strength is the maximum peak force (g) divided by the sample width (in) and reported as g / in to the nearest 1 g / in.
[0352] Adjusted Gauge Length is calculated as the extension measured at 3.0 g of force (in) added to the original gauge length (in).
[0353] Peak Elongation is calculated as the extension at maximum peak force (in) divided by the Adjusted Gauge Length (in) multiplied by 100 and reported as % to the nearest 0.1%
[0354] Total Energy (TEA) is calculated as the area under the force curve integrated from zero extension to the extension at the maximum peak force (g*in), divided by the product of the adjusted Gauge Length (in) and specimen width (in) and is reported out to the nearest 1 g*in / in2.Replot the force (g) verses extension (in) curve as a force (g) verses strain curve. Strain is herein defined as the extension (in) divided by the Adjusted Gauge Length (in).
[0355] Program the software to calculate the following from the constructed force (g) verses strain curve:
[0356] Tangent Modulus (Modulus) is the Modulus at 15 g / cm.
[0357] The Tensile Strength (g / in), Peak Elongation (%), Total Energy (g*in / in2) and Modulus (g / cm), which is the Tangent Modulus at 15 g / cm), are calculated for the four CD unitary specimens and the four MD unitary specimens. Calculate an average for each parameter separately for the CD and MD specimens.
[0358] Calculations:
[0359] Geometric Mean Tensile Strength = Square Root of [MD Tensile Strength (g / in) x CD Tensile Strength (g / in)]
[0360] Geometric Mean Peak Elongation = Square Root of [MD Elongation (%) x CD Elongation (%)]
[0361] Geometric Mean TEA = Square Root of [MD TEA (g*in / in2) x CD TEA (g*in / in2)] Geometric Mean Modulus = Square Root of [MD Modulus (g / cm) (at 15 g / cm) x CD Modulus (g / cm) (at 15 g / cm)]
[0362] Total Dry Tensile Strength (TDT) = MD Tensile Strength (g / in) + CD Tensile Strength (g / in)
[0363] Total TEA = MD TEA (g*in / in2) + CD TEA (g*in / in2)
[0364] Total Modulus = MD Modulus (g / cm) + CD Modulus (g / cm)
[0365] Tensile Ratio = MD Tensile Strength (g / in) / CD Tensile Strength (g / in)
[0366] 4. DENSITY TEST METHOD
[0367] The density of a web sample is measured by dividing the Basis Weight of the web sample by the Thickness of the web sample. Density units are reported as g / cm3.
[0368] Thickness Method
[0369] Thickness of a fibrous structure and / or sanitary tissue product is measured using a ProGage Thickness Tester (Thwing-Albert Instrument Company, West Berlin, NJ) with a pressure foot diameter of 2.00 inches (area of 3.14 in2) at a pressure of 95 g / in2. Four (4) samples are prepared by cutting of a usable unit such that each cut sample is at least 2.5 inches per side, avoiding creases, folds, and obvious defects. An individual specimen is placed on the anvil with the specimen centered underneath the pressure foot. The foot is lowered at 0.03 in / sec to an applied pressure of 95 g / in2. The reading is taken after 3 sec dwell time, and the foot is raised. The measure is repeatedin like fashion for the remaining 3 specimens. The caliper is calculated as the average caliper of the four specimens and is reported in mils (0.001 in) to the nearest 0.1 mils. Conversion to cm can be made using standard conversion factors.
[0370] 5. BASIS WEIGHT TEST METHOD
[0371] Basis Weight Test Method
[0372] Basis weight of a fibrous structure sample is measured by selecting twelve (12) individual fibrous structure samples and making two stacks of six individual samples each. If the individual samples are connected to one another vie perforation lines, the perforation lines must be aligned on the same side when stacking the individual samples. A precision cutter is used to cut each stack into exactly 3.5 in. x 3.5 in. squares. The two stacks of cut squares are combined to make a basis weight pad of twelve squares thick. The basis weight pad is then weighed on a top loading balance with a minimum resolution of 0.01 g. The top loading balance must be protected from air drafts and other disturbances using a draft shield. Weights are recorded when the readings on the top loading balance become constant. The Basis Weight is calculated as follows:
[0373] Basis Weight = > Weight of basis weight pad (g) x 3000 ft2
[0374] (lbs / 3000 ft2) 453.6 g / lbs x 12 samples x [12.25 in2(Area of basis weight pad) / 144 in2]
[0375] Basis Weight = Weight of basis weight pad (g) x 10,000 cm2 / m2
[0376] (g / m2) 79.0321 cm2(Area of basis weight pad) x 12 samples
[0377] 6. ROLL BULK
[0378] “Roll Bulk” as used herein is the result of measuring finished product rolls. The rolls are placed into a controlled temperature and Humidity room (TAPPI conditions, about 23°C ± 2°C and about 50% ± 2% relative humidity) for at least 24 hours to equilibrate (equilibration can be monitored by measuring roll weight every 4 hours until the mass stabilizes;). If rolls have been stored in greater than 50% relative humidity conditions, then said rolls should first be equilibrated at conditions lower than 50% relative humidity and then equilibrated at TAPPI conditions - see T-402. The rolls are weighed with the weight recorded to the hundredths of grams. The width of the rolls are measured with a ruler that shows millimeters, width recorded to the tenths of centimeter. Roll Diameter is measured according to the Percent Roll Compressibility test methodincluded herein. Roll Bulk (cmA3 / g) is then calculated by: multiplying the square of the radius of the roll (roll diameter (cm) / 2) by 3.14159 and by the roll width (cm), then dividing that by the mass of the roll (g):
[0379] / roll diameter(cmY?„ .
[0380] / cc 3.14159 * ( - 2 - - — *r°U width (cm)
[0381] Roll Bulk ( —
[0382]
[0383] roll weight (g)
[0384] The measurements are done with the roll core in place. The units “cc / g” are used interchangeably herein with “cm3 / g.”
[0385] 7. PERCENT ROLL COMPRESSIBILITY TEST METHOD
[0386] Percent Roll Compressibility (Percent Compressibility) is determined using the Roll Diameter Tester 1000 as shown in FIG. 1. It is comprised of a support stand made of two aluminum plates, a base plate 1001 and a vertical plate 1002 mounted perpendicular to the base, a sample shaft 1003 to mount the test roll, and a bar 1004 used to suspend a precision diameter tape 1005 that wraps around the circumference of the test roll. Two different weights 1006 and 1007 are suspended from the diameter tape to apply a confining force during the uncompressed and compressed measurement. All testing is performed in a conditioned room maintained at about 23 °C ± 2°C and about 50% ± 2% relative humidity.
[0387] The diameter of the test roll is measured directly using a Pi® tape or equivalent precision diameter tape (e.g., an Executive Diameter tape available from Apex Tool Group, LLC, Apex, NC, Model No. W606PD) which converts the circumferential distance into a diameter measurement, so the roll diameter is directly read from the scale. The diameter tape is graduated to 0.01 inch increments with accuracy certified to 0.001 inch and traceable to NIST. The tape is 0.25 in wide and is made of flexible metal that conforms to the curvature of the test roll but is not elongated under the 1100 g loading used for this test. If necessary, the diameter tape is shortened from its original length to a length that allows both of the attached weights to hang freely during the test, yet is still long enough to wrap completely around the test roll being measured. The cut end of the tape is modified to allow for hanging of a weight (e.g., a loop). All weights used are calibrated, Class F hooked weights, traceable to NIST.
[0388] The aluminum support stand is approximately 600 mm tall and stable enough to support the test roll horizontally throughout the test. The sample shaft 1003 is a smooth aluminum cylinder that is mounted perpendicularly to the vertical plate 1002 approximately 485 mm from the base. The shaft has a diameter that is at least 90% of the inner diameter of the roll and longer than the width of the roll. A small steal bar 1004 approximately 6.3 mm diameter is mounted perpendicularto the vertical plate 1002 approximately 570 mm from the base and vertically aligned with the sample shaft. The diameter tape is suspended from a point along the length of the bar corresponding to the midpoint of a mounted test roll. The height of the tape is adjusted such that the zero mark is vertically aligned with the horizontal midline of the sample shaft when a test roll is not present.
[0389] Condition the samples at about 23°C ± 2°C and about 50% ± 2% relative humidity for 2 hours prior to testing. Rolls with cores that are crushed, bent, or damaged should not be tested. Place the test roll on the sample shaft 1003 such that the direction the paper was rolled onto its core is the same direction the diameter tape will be wrapped around the test roll. Align the midpoint of the roll’s width with the suspended diameter tape. Loosely loop the diameter tape 1004 around the circumference of the roll, placing the tape edges directly adjacent to each other with the surface of the tape lying flat against the test sample. Carefully, without applying any additional force, hang the 100 g weight 1006 from the free end of the tape, letting the weighted end hang freely without swinging. Wait 3 seconds. At the intersection of the diameter tape 1008, read the diameter aligned with the zero mark of the diameter tape and record as the Original Roll Diameter to the nearest 0.01 inches. With the diameter tape still in place, and without any undue delay, carefully hang the 1000 g weight 1007 from the bottom of the 100 g weight, for a total weight of 1100 g. Wait 3 seconds. Again read the roll diameter from the tape and record as the Compressed Roll Diameter to the nearest 0.01 inch. Calculate percent roll compressibility to the according to the following equation and record to the nearest 0.1%:
[0390] (Orqinal Roll Diameter — (Compressed Roll Diameter
[0391] % Compressibility = - . . — , „n. - x 100
[0392] Original Roll Diameter
[0393] 8. INITIAL TOTAL WET TENSILE TEST METHOD
[0394] The initial total wet tensile of a dry fibrous structure is determined using a Thwing-Albert EJA Material Tester Instrument, Cat. No. 1350, equipped with 5000 g load cell available from Thwing-Albert Instrument Company, 14 Collings Ave., W. Berlin, N.J. 08091. 10% of the 5000 g load cell is utilized for the initial total wet tensile test.
[0395] i. Sample Preparation - A sample strip of dry fibrous structure to be tested [2.54 cm (1 inch) wide by greater than 5.08 cm (2 inches)] long is obtained.
[0396] ii. Operation - The test settings for the instrument are:
[0397] Crosshead speed - 10.16 cm / minute (4.0 inches / minute)
[0398] Initial gauge length 2.54 cm (1.0 inch)
[0399] Adjust the load cell to read zero plus or minus 0.5gramsfOrce (gf)iii. Testing Samples - One end of the sample strip is placed between the upper jaws of the machine and clamped. After verifying that the sample strip is hanging straight between the lower jaws, clamp the other end of the sample strip in the lower jaws.
[0400] a. Pre-Test - Strain the sample strip to 25 gramsforce (+ / -10 gramsforce) at a strain rate of 3.38 cm / minute (1.33 inches / minute) prior to wetting the sample strip. The distance between the upper and lower jaws now being greater than 2.54 cm (1.0 inch). This distance now becomes the new zerostrain position for the forthcoming wet test described below. b. Wet Test - While the sample strip is still at 25 gramsforce (+ / -10 gramsforce), it is wetted, starting near the upper jaws, a water / 0.1% Pegosperse® ML200 (available from Lonza Inc., of Allendale, N.J.) solution [having a temperature of about 73 °F ± 4°F (about 23 °C ± 2.2°C)] is delivered to the sample strip via a 2 mL disposable pipette. Do not contact the sample strip with the pipette and do not damage the sample strip by using excessive squirting pressure. The solution is continuously added until the sample strip is visually determined to be completely saturated between the upper and lower jaws. At this point, the load cell is re-adjusted to read 0 ± 0.5 gramsforce. The sample strip is then strained at a rate of 10.16 cm / minute (4 inches / minute) and continues until the sample strip is strained past its failure point (failure point being defined as the point on the force-strain curve where the sample strip falls to 50% of its peak strength after it has been strained past its peak strength). The straining of the sample strip is initiated between 5-10 seconds after the sample is initially wetted. The initial result of the test is an array of data points in the form of load (gramsforce) versus strain (where strain is calculated as the crosshead displacement (cm of jaw movement from starting point) divided by the initial separation distance (cm) between the upper and lower jaws after the pre-test.
[0401] The sample is tested in two orientations, referred to here as MD (machine direction, i.e., in the same direction as the continuously wound reel and forming fabric) and CD (cross-machine direction, i.e., 90° from MD). The MD and CD initial wet tensile strengths are determined using the above equipment and the initial total wet tensile values are calculated in the following manner:
[0402] ITWT(g / inch)=Peak LoadMD(gf) / l (inchwidth)+Peak Loadco (gf) / l (inchwidth)
[0403] 9. SANITARY TISSUE OR TOWEL WET BURST TEST METHOD
[0404] “Wet Burst Strength” as used herein is a measure of the ability of a fibrous structure and / or a fibrous structure product incorporating a fibrous structure to absorb energy, when wet and subjected to deformation normal to the plane of the fibrous structure and / or fibrous structureproduct. The Wet Burst Test is run according to ISO 12625-9:2005, except for any deviations or modifications described below.
[0405] Wet burst strength may be measured using a Thwing-Albert Burst Tester Cat. No. 177 equipped with a 2000 g load cell commercially available from Thwing-Albert Instrument Company, Philadelphia, Pa, or an equivalent instrument.
[0406] Wet burst strength is measured by preparing four (4) multi -ply fibrous structure product samples for testing. First, condition the samples for two (2) hours at a temperature of 73° F ± 2°F (23°C ± 1°C) and a relative humidity of 50% (± 2%). Take one sample and horizontally dip the center of the sample into a pan filled with about 25 mm of room temperature distilled water. Leave the sample in the water four (4) (± 0.5) seconds. Remove and drain for three (3) (± 0.5) seconds holding the sample vertically so the water runs off in the cross-machine direction. Proceed with the test immediately after the drain step.
[0407] Place the wet sample on the lower ring of the sample holding device of the Burst Tester with the outer surface of the sample facing up so that the wet part of the sample completely covers the open surface of the sample holding ring. If wrinkles are present, discard the samples and repeat with a new sample. After the sample is properly in place on the lower sample holding ring, turn the switch that lowers the upper ring on the Burst Tester. The sample to be tested is now securely gripped in the sample holding unit. Start the burst test immediately at this point by pressing the start button on the Burst Tester. A plunger will begin to rise (or lower) toward the wet surface of the sample. At the point when the sample tears or ruptures, report the maximum reading. The plunger will automatically reverse and return to its original starting position. Repeat this procedure on three (3) more samples for a total of four (4) tests, i.e., four (4) replicates. Report the results as an average of the four (4) replicates, to the nearest gram.
[0408] 10. WATER RETENTION VALUE TEST METHOD
[0409] The water retention value of pulp was measured according to Tappi UM 256.
[0410] 11. % FINES LEVEL (FIBER QUALITY ANALYSIS TEST METHOD)
[0411] The pulp morphology including fiber length, width, coarseness, fines was characterized optically according Tappi T271 om-23 using a Fiber Quality Analyzer (FQA-360).
[0412] 12. HANDSHEET TENSILE PROPERTIES TEST METHOD
[0413] Hand sheet was made according to Tappi T205 for paper mechanical properties test. The tensile properties of hand sheet were measured according to Tappi T494.13. HANDSHEET ZERO SPAN TENSILE TEST METHOD
[0414] The Zero-span breaking strength of pulp was measured according to Tappi T231.
[0415] 14. % LIGNIN LEVEL TEST METHOD
[0416] The % lignin level in pulp was determined according to the standard protocol provided by the National Renewable Energy Laboratory. (J. Agric. Food Chem. 2010, 58, 16, 9043-9053).
[0417] X. COMBINATIONS
[0418] A. A sanitary tissue comprising a plurality of dry fibrous structure sheets, wherein the sanitary tissue comprises from about 30 wt.% to about 100 wt.% post-consumer recycled pulp fiber; and further comprises at least one of the following:
[0419] a. less than about 100 pg / kg of glyphosphate;
[0420] b. less than 150 pg / kg of isononylphenol(mono, di, tri, and tetra)exthoxylate;
[0421] c. less than 150 pg / kg of Bisphenol-A;
[0422] d. less than 25 ng / kg of 1,2,3,4,6,7,8-HpCDD;
[0423] e. less than 250 ng / kg of OCDD;
[0424] f. less than 5 ng / kg of OCDF;
[0425] g. less than 4 ng / kg of PCB 81;
[0426] h. less than 350 ng / kg of PCB 105;
[0427] i. less than 50 ng / kg of PCB 118;
[0428] j. less than 5,000 pg / kg of di-2ethylhexylphthalate;
[0429] k. less than 5,000 pg / kg of di-isononylphthalate;
[0430] l. less than 10 pg / kg of fluoranthene; and
[0431] m. less than 10 pg / kg of phenanthene;
[0432] as measured according to the Trace Chemicals Test Method.
[0433] B. The sanitary tissue of paragraph A, wherein the tissue comprises at least 4 of (a) - (m).
[0434] C. The sanitary tissue of paragraph A or B, wherein the tissue comprises at least 9 of (a) - (m). D. The sanitary tissue of any one of paragraphs A-C, wherein the tissue comprises all of (a) - (m). E. The sanitary tissue of any one of paragraphs A-D, wherein the tissue comprises a residual solvent content of less than 1000 ppm, as measured according to the Trace Chemicals Test Method.F. The sanitary tissue of any one of paragraphs A-E, wherein the tissue comprises from about 75 wt% to about 100 wt% post-consumer recycled pulp fiber.
[0435] G. The sanitary tissue of any one of paragraphs A-F, wherein the tissue comprises from about 85 wt% to about 100 wt% post-consumer recycled pulp fiber.
[0436] H. The sanitary tissue of any one of paragraphs A-G, wherein the tissue comprises from about 90 wt% to about 100 wt% post-consumer recycled pulp fiber.
[0437] I. The sanitary tissue of any one of paragraphs A-H, wherein the plurality of dry fibrous structure sheets are in a roll.
[0438] J. The sanitary tissue of any one of paragraphs A-I, wherein the sanitary tissue exhibits one or more of the following properties:
[0439] a) a moisture content of less than 20% by weight of the sanitary tissue as measured according to the Water Content Test Method;
[0440] b) a GM Tensile Strength of greater than 200 g / in as measured according to the Tensile Test Method;
[0441] c) a density of less than about 0.60 g / cm3as measured according to the Density Test Method; and
[0442] d) a basis weight of greater than 5 g / m2to about 120 g / m2as measured according to the Basis Weight Test Method; and
[0443] e) wherein the sanitary tissue is on a roll and exhibits the following properties: i. a roll bulk of greater than 4 cm3 / g; and
[0444] ii. a % roll compressibility of less than 10% as measured according to the Percent Compressibility Test Method.
[0445] K. The sanitary tissue of any one of paragraphs A-J, wherein the sanitary tissue exhibits two or more of the following properties:
[0446] a) a moisture content of less than 20% by weight of the sanitary tissue as measured according to the Water Retention Value Test Method;
[0447] b) a GM Tensile Strength of greater than 200 g / in as measured according to the Tensile Test Method;
[0448] c) a density of less than about 0.60 g / cm3as measured according to the Density Test Method; and
[0449] d) a basis weight of greater than 5 g / m2to about 120 g / m2as measured according to the Basis Weight Test Method; ande) wherein the sanitary tissue is on a roll and exhibits the following properties:
[0450] i. a roll bulk of greater than 4 cm3 / g; and
[0451] ii. a % roll compressibility of less than 10% as measured according to the Percent Compressibility Test Method.
[0452] L. The sanitary tissue of any one of paragraphs A-K, wherein the sanitary tissue exhibits all of the following properties:
[0453] a) a moisture content of less than 20% by weight of the sanitary tissue as measured according to the Water Retention Value Test Method;
[0454] b) a GM Tensile Strength of greater than 200 g / in as measured according to the Tensile Test Method;
[0455] c) a density of less than about 0.60 g / cm3as measured according to the Density Test Method; and
[0456] d) a basis weight of greater than 5 g / m2to about 120 g / m2as measured according to the Basis Weight Test Method; and
[0457] e) wherein the sanitary tissue is on a roll and exhibits the following properties:
[0458] i. a roll bulk of greater than 4 cm3 / g; and
[0459] ii. a % roll compressibility of less than 10% as measured according to the Percent Compressibility Test Method.
[0460] M. The sanitary tissue of any one of paragraphs A-L, wherein the sanitary tissue is a multi-layered tissue web comprising a first fibrous layer and a second fibrous layer, wherein the first fibrous layer comprises wood fibers and the second fibrous layer comprises the post-consumer recycled pulp fiber.
[0461] The dimensions and values disclosed herein are not to be understood as being strictly limited to the exact numerical values recited. Instead, unless otherwise specified, each such dimension is intended to mean both the recited value and a functionally equivalent range surrounding that value. For example, a dimension disclosed as “40 mm” is intended to mean “about 40 mm.”
[0462] Every document cited herein, including any cross referenced or related patent or application and any patent application or patent to which this application claims priority or benefit thereof, ishereby incorporated herein by reference in its entirety unless expressly excluded or otherwise limited. The citation of any document is not an admission that it is prior art with respect to any invention disclosed or claimed herein or that it alone, or in any combination with any other reference or references, teaches, suggests or discloses any such invention. Further, to the extent that any meaning or definition of a term in this document conflicts with any meaning or definition of the same term in a document incorporated by reference, the meaning or definition assigned to that term in this document shall govern.
[0463] While particular embodiments of the present invention have been illustrated and described, it would be obvious to those skilled in the art that various other changes and modifications can be made without departing from the spirit and scope of the invention. It is therefore intended to cover in the appended claims all such changes and modifications that are within the scope of this invention.
Claims
CLAIMSWhat is claimed is:
1. A sanitary tissue comprising a plurality of dry fibrous structure sheets, wherein the sanitary tissue comprises from about 30 wt.% to about 100 wt.% post-consumer recycled pulp fiber; and further comprises at least one of the following:a. less than about 100 pg / kg of glyphosphate;b. less than 150 pg / kg of isononylphenol(mono, di, tri, and tetra)exthoxylate;c. less than 150 pg / kg of Bisphenol-A;d. less than 25 ng / kg of 1,2,3,4,6,7,8-HpCDD;e. less than 250 ng / kg of OCDD;f. less than 5 ng / kg of OCDF;g. less than 4 ng / kg of PCB 81;h. less than 350 ng / kg of PCB 105;i. less than 50 ng / kg of PCB 118;j. less than 5,000 pg / kg of di-2ethylhexylphthalate;k. less than 5,000 pg / kg of di-isononylphthalate;l. less than 10 pg / kg of fluoranthene; andm. less than 10 pg / kg of phenanthene;as measured according to the Trace Chemicals Test Method.2 The sanitary tissue of claim 1, wherein the tissue comprises at least 4 of (a) - (m).3 The sanitary tissue of claim 1, wherein the tissue comprises at least 9 of (a) - (m).4 The sanitary tissue of claim 1, wherein the tissue comprises all of (a) - (m).5 The sanitary tissue of claim 1, wherein the tissue comprises a residual solvent content of less than 1000 ppm, as measured according to the Trace Chemicals Test Method.6 The sanitary tissue of claim 1, wherein the tissue comprises from about 75 wt% to about 100 wt% post-consumer recycled pulp fiber.
7. The sanitary tissue of claim 1, wherein the tissue comprises from about 85 wt% to about 100 wt% post-consumer recycled pulp fiber.
8. The sanitary tissue of claim 1, wherein the tissue comprises from about 90 wt% to about 100 wt% post-consumer recycled pulp fiber.9 The sanitary tissue of claim 1, wherein the plurality of dry fibrous structure sheets are in a roll.10 The sanitary tissue of claim 1, wherein the sanitary tissue exhibits one or more of the following properties:a) a moisture content of less than 20% by weight of the sanitary tissue as measured according to the Water Content Test Method;b) a GM Tensile Strength of greater than 200 g / in as measured according to the Tensile Test Method;c) a density of less than about 0.60 g / cm3as measured according to the Density Test Method; andd) a basis weight of greater than 5 g / m2to about 120 g / m2as measured according to the Basis Weight Test Method; ande) wherein the sanitary tissue is on a roll and exhibits the following properties:i. a roll bulk of greater than 4 cm3 / g; andii. a % roll compressibility of less than 10% as measured according to the Percent Compressibility Test Method.11 The sanitary tissue of claim 1, wherein the sanitary tissue exhibits two or more of the following properties:a) a moisture content of less than 20% by weight of the sanitary tissue as measured according to the Water Retention Value Test Method;b) a GM Tensile Strength of greater than 200 g / in as measured according to the Tensile Test Method;c) a density of less than about 0.60 g / cm3as measured according to the Density Test Method; andd) a basis weight of greater than 5 g / m2to about 120 g / m2as measured according to the Basis Weight Test Method; ande) wherein the sanitary tissue is on a roll and exhibits the following properties:i. a roll bulk of greater than 4 cm3 / g; andii. a % roll compressibility of less than 10% as measured according to the Percent Compressibility Test Method.The sanitary tissue of claim 1, wherein the sanitary tissue exhibits all of the following properties:a) a moisture content of less than 20% by weight of the sanitary tissue as measured according to the Water Retention Value Test Method;b) a GM Tensile Strength of greater than 200 g / in as measured according to the Tensile Test Method;c) a density of less than about 0.60 g / cm3as measured according to the Density Test Method; andd) a basis weight of greater than 5 g / m2to about 120 g / m2as measured according to the Basis Weight Test Method; ande) wherein the sanitary tissue is on a roll and exhibits the following properties:i. a roll bulk of greater than 4 cm3 / g; andii. a % roll compressibility of less than 10% as measured according to the Percent Compressibility Test Method.The sanitary tissue of claim 1, wherein the sanitary tissue is a multi-layered tissue web comprising a first fibrous layer and a second fibrous layer, wherein the first fibrous layer comprises wood fibers and the second fibrous layer comprises the post-consumer recycled pulp fiber.
