Polymer dispersions and related methods and applications
A multistage emulsion polymerization process enhances vinyl ester-based polymer dispersions' resistance to capillary water uptake and dirt pickup, addressing the limitations of existing compositions for exterior paints and plasters.
Patent Information
- Application Number
- PCT/US2026/026265
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-05
- Filing Date
- 2026-05-01
- Publication Date
- 2026-11-12
AI Technical Summary
Existing vinyl ester-based polymer dispersions used in paints and plasters exhibit insufficient resistance to capillary water uptake, dirt pickup, and water resistance, making them unsuitable for exterior applications while maintaining low temperature film formation and other performance properties.
A multistage emulsion polymerization process producing polymer products with specific monomer compositions in each stage, resulting in a polymer dispersion with enhanced resistance to capillary water uptake and improved dirt-pickup resistance, using monomers like vinyl esters of C6-C20 carboxylic acids, vinyl acetate, ethylene, and alkyl esters of (meth)acrylic acid, stabilized with emulsifiers and protective colloids.
The process yields polymer dispersions with improved water resistance and reduced water permeability, suitable for exterior applications without compromising low temperature film formation and dirt-pickup resistance.
Smart Images

Figure IMGF000034_0001 
Figure IMGF000030_0001_TABLE 
Figure IMGF000030_0002_TABLE
Abstract
Description
POLYMER DISPERSIONS AND RELATED METHODS AND APPLICATIONSCROSS-REFERENCE TO RELATED APPLICATIONS
[0001] The present application claims priority to U.S. provisional patent application 63 / 800,229, filed on May 5, 2025.FIELD OF THE INVENTION
[0002] The present disclosure relates generally to polymer dispersions, their preparation and use. More particularly, this invention relates to vinyl ester / acrylic multistage polymer dispersions for use as a binder in paints and plasters exhibiting reduced water take up and reduced water permeability.BACKGROUND OF THE INVENTION
[0003] Polymer dispersions derived from vinyl esters and monomers copolymerizable therewith can be used as binders for paints, plasters, and renders. Such polymer dispersions are typically prepared by emulsion polymerization with the polymerization occurring in one or more stages. In the polymerization processes, vinyl ester-containing monomer mixtures are converted by free-radical polymerization by addition of initiators in the presence of protective colloids and / or emulsifiers. Vinyl ester-based, and particularly vinyl acetate-based copolymer dispersions, produced in one polymerization stage, offer a good balance of block resistance and low temperature film formation due to the hydroplastification effect of vinyl acetate, rendering them suitable binders for low-emission interior paints. On the downside, the hydrophilicity and relatively low glass transition temperature of poly(vinyl acetate) of 32°C render vinyl ester-based copolymer dispersions less suitable for exterior applications due to insufficient resistance to dirt pickup and / or water resistance.
[0004] Multiphase polymerization process have been investigated to overcome these deficiencies. After polymerizing a vinyl ester-based first stage polymer with a low glass transition temperature suitable for coalescent-minimized or coalescent-free low temperature film formation, a second monomer mixture with a preferably elevated glass transition temperature is polymerized to be incorporated in the preformed particles. However, there remains a continuing need for vinyl ester-based polymer dispersions that offer enhanced performance over existingcompositions when used in, for example, paints and plasters. By way of example, a significant disadvantage of current dispersions for use in exterior facade paints and plasters is a high capillary water uptake, measured as water absorption coefficient (w value) according to DIN EN-1062-3 of pristine and / or aged coatings. Therefore, it would be useful to provide polymer dispersions capable of use in, for example, paints and plasters, that offer an improved resistance against capillary water uptake, without loss of properties in other performance areas, such as low temperature film formation, a high dirt-pickup resistance, and a high permittivity for water vapor.SUMMARY OF THE INVENTION
[0005] Embodiments of the present disclosure include emulsion polymerization processes for producing polymer products comprising: (i) polymerizing, in a first stage, a first monomer composition comprising from 15 wt% to 100 wt% of at least one vinyl ester of a C6-C20 carboxylic acid and from 0 wt% to 85 wt% of at least one alkyl ester of (meth)acrylic acid, each based on the total weight of monomers in the first monomer composition, to produce a first stage polymer; (ii) polymerizing, in a second stage and in the presence of the first stage polymer, a second monomer composition comprising from 50 wt% to 95 wt% of vinyl acetate, from 5 wt% to 40 wt% of ethylene, and from 0 wt% to 25 wt% of at least one vinyl ester other than vinyl acetate, each based on the total weight of monomers in the second monomer composition, to produce a second stage polymer, and optionally (iii) polymerizing, in a third stage and in the presence of the first stage polymer and the second stage polymer, a third monomer composition comprising from 30 wt% to 100 wt% of at least one alkyl ester of (meth)acrylic acid and from 0 wt% to 20 wt% of at least one vinyl ester of a carboxylic acid, each based on the total weight of monomers in the third monomer composition, to produce a third stage polymer, wherein the first stage polymer is from 5 wt% to 40 wt%, the second stage polymer is 30 wt% or greater, and the third stage polymer is from 0 wt% to 30 wt%, each based on a total weight of the polymer product.
[0006] Embodiments of the present disclosure also include polymer dispersions produced by the foregoing process.
[0007] Embodiments of the present disclosure also include coating compositions (e.g., a facade paint or a plaster) that include (i) the polymer dispersion produced by the foregoingprocess and (ii) at least one pigment, at least one filler, or a combination of at least one pigment and at least one filler. Said coating composition may be included in a thermal insulation system.DETAILED DESCRIPTION OF THE INVENTION
[0008] Described herein is a multistage emulsion polymerization process, in which a first monomer composition comprising from 15 wt% to 100 wt% of at least one vinyl ester of a C6-C20 carboxylic acid and from 0 wt% to 85 wt% of at least one alkyl ester of (meth)acrylic acid is polymerized in a first stage to produce a first stage polymer. A second monomer composition comprising from 50 wt% to 95 wt% of vinyl acetate, from 5 wt% to 40 wt% of ethylene, and from 0 wt% to 25 wt% of at least one vinyl ester other than vinyl acetate is then polymerized in a second stage and in the presence of said first stage product to produce a second stage polymer. Optionally, a third monomer composition comprising from 30 wt% to 100 wt% of at least one alkyl ester of (meth)acrylic acid and from 0 wt% to 20 wt% of at least one vinyl ester of a carboxylic acid is then polymerized in a third stage and in the presence of said first and second stage products to produce a third stage polymer. The resultant polymer product may comprise from 5 wt% to 40 wt% of the first stage polymer, 30 wt% or greater of the second stage polymer, and from 0 wt% to 30 wt% of the third stage polymer, each based on a total weight of the polymer product.Definitions and Descriptions
[0009] As used herein, the terms “invention,” “the invention,” “this invention,” and “the present invention” are intended to refer broadly to all of the subject matter of this patent application and the claims below. Statements containing these terms should be understood not to limit the subject matter described herein or to limit the meaning or scope of the patent claims below.
[0010] As used herein, the meaning of “a,” “an,” or “the” includes singular and plural references, e.g., meaning “one or more,” unless the context clearly dictates otherwise.
[0011] All ranges disclosed herein are to be understood to encompass any and all subranges subsumed therein. For example, a stated range of “1 to 10” should be considered to include any and all subranges between (and inclusive of) the minimum value of 1 and the maximum value of 10; that is, all subranges beginning with a minimum value of 1 or more, e.g. 1 to 6.1, and ending with a maximum value of 10 or less, e.g., 5.5 to 10.
[0012] As used herein, the term “comprises” and variations thereof is open-ended, but forpurposes of the specification and as support for future claim amendments, it should be understood as alternatively disclosing more restrictive language, such as “consisting essentially of’ or “consisting of.”First Monomer Composition
[0013] The first monomer composition used in the present process comprises from 15 wt% to 100 wt% of at least one vinyl ester of a C6-C20 carboxylic acid and from 0 wt% to 85 wt% of at least one alkyl ester of (meth)acrylic acid, each based on the total weight of monomers in the first monomer composition, to produce a first stage polymer.
[0014] Examples of vinyl esters of C6-C20 carboxylic acids may include, but are not limited to, vinyl 2-ethylhexanoate, vinyl esters of saturated branched monocarboxylic acids having from 9 to 11 carbon atoms in the acid radical (e.g., VEOVA™ 9, VEOVA™ 10, and VEOVA™ 11), vinyl esters of relatively long-chain saturated or unsaturated fatty acids (e.g., vinyl laurate or vinyl stearate), vinyl esters of benzoic acid and substituted derivatives of benzoic acid (e.g., vinyl p-tert-butylbenzoate), the like, and any combination thereof.
[0015] The at least one vinyl ester of a C6-C20 carboxylic acid may be present in the first monomer composition at a concentration from 15 wt% to 100 wt%, such as from 20 wt% to 90 wt%, such as from 40 wt% to 80 wt%, such as from 50 wt% to 80 wt%, such as from 50 wt% to 75 wt%, based on the total weight of monomers in the first monomer composition.
[0016] Alkyl esters of (meth)acrylic acid encompass alkyl esters of acrylic acid and alkyl esters of methacrylic acid. The alkyl esters of (meth)acrylic acid may be C1-C22 alkyl esters of (meth)acrylic acid, preferably Cl -Cl 4 alkyl esters of (meth)acrylic acid, and mixtures thereof. Examples of alkyl esters of (meth)acrylic acid may include, but are not limited to, methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, iso-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, 2-octyl (meth)acrylate, iso-octyl(meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-propylheptyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, stearyl (meth)acrylate, isobomyl (meth)acrylate, the like, and any combination thereof. Preferred alkyl esters of (meth)acrylic acid for the first monomer composition include methyl (meth)acrylate, n-butyl (meth)acrylate, iso-butyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl acrylate, 2-octyl acrylate, n-octyl acrylate, or any combination thereof.
[0017] When present, the at least one alkyl ester of (meth)acrylic acid may be present in thefirst monomer composition at a concentration from 1 wt% to 85 wt%, such as from 10 wt% to 80 wt%, such as from 20 wt% to 60 wt%, such as from 25 wt% to 60 wt%, such as from 25 wt% to 50 wt%, based on the total weight of monomers in the first monomer composition.
[0018] Optionally, the first monomer composition may also include at least one vinyl ester of a C1-C5 carboxylic acid. Examples of vinyl esters of C1-C5 carboxylic acids may include, but are not limited to, vinyl formate, vinyl acetate, vinyl propionate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, the like, and any combination thereof.
[0019] When present, the at least one vinyl ester of a C1-C5 carboxylic acid may be present in the first monomer composition at a concentration from 0.1 wt% to 40 wt%, such as from 0.1 wt% to 30 wt%, such as from 0.1 wt% to 20 wt%, such as from 0.1 wt% to 10 wt%, based on the total weight of monomers in the first monomer composition.
[0020] Optionally, the first monomer composition may also include at least one functional monomer. Examples of functional monomers may include, but are not limited to, carboxylic acidfunctional monomers, epoxy-functional monomers, silane-functional monomers, keto-functional monomers, sulfonic acid-functional monomers, ethylenically unsaturated phosphonic and phosphoric acids, ethylenically unsaturated carboxylic amides (e.g., acrylamide, methacrylamide), ethylenically unsaturated carboxylic anhydrides, the like, and any combination thereof.
[0021] Examples of carboxylic acid-functional monomers may include, but are not limited to, an ethylenically unsaturated C3-C8 monocarboxylic acid, an ethylenically unsaturated C4-C8 dicarboxylic acid, an ethylenically unsaturated C4-C8 dicarboxylic acid anhydride, the like, and any combination thereof.
[0022] The epoxy-functional monomers may be glycidyl compounds. Examples of epoxyfunctional monomers may include, but are not limited to, glycidyl acrylate, glycidyl methacrylate, allyl glycidyl ether, vinyl glycidyl ether, the like, and any combination thereof.
[0023] Examples of silane-functional monomers may include, but are not limited to, y-methacryloxypropyltris(2-methoxyethoxy)silane, trimethoxyvinylsilane, triethoxyvinylsilane, diethoxyvinylsilanol, ethoxyvinylsilanediol, triethoxyallylsilane, tripropoxyvinylsilane, triisopropoxyvinylsilane, tributoxyvinylsilane, triacetoxyvinylsilane, trimethylglycolvinylsilane, y-methacryloxypropyltrimethylglycolsilane, y-acryloxypropyltriethoxysilane, y-methacryloxypropyltrimethoxysilane, the like, and any combination thereof.
[0024] Examples of sulfonic acid-functional monomers may include, but are not limited to,vinyl sulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, an alkali metal salt of vinyl sulfonic acid, an alkali metal salt of 2-acrylamido-2-methylpropanesulfonic acid, an ammonium salt of vinyl sulfonic acid, an ammonium salt of 2-acrylamido-2-methylpropanesulfonic acid, the like, and any combination thereof. A preferred sulfonic-acid functional monomer is the sodium salt of vinyl sulfonic acid.
[0025] When present, the at least one functional monomer may be present in the first monomer composition at a concentration from 0.1 wt% to 15 wt%, such as from 0.1 wt% to 10 wt%, such as from 0.1 wt% to 5 wt%, such as from 0.1 wt% to 2 wt%, such as from 0.1 wt% to 1 wt%, based on the total weight of monomers in the first monomer composition. The first monomer composition may be free (contain 0.00 wt%) or be essentially free (contain 0.01 wt% or less) of functional monomers, based on the total weight of monomers in the first monomer composition.
[0026] Ethylene may be present in the first monomer composition. When present, ethylene may be present in the first monomer composition at a concentration from 0.1 wt% to 15 wt%, such as from 0.1 wt% to 10 wt%, such as from 0.1 wt% to 5 wt%, such as from 0.1 wt% to 2 wt%, based on the total weight of monomers in the first monomer composition.
[0027] Accordingly, the first monomer composition may include the following monomers, each based on the total weight of monomers in the first monomer composition:• from 15 wt% to 100 wt% of vinyl esters of C6-C20 carboxylic acids;• from 0 wt% to 85 wt% of at least one alkyl ester of (meth)acrylic acid;• from 0 wt% to 40 wt% of at least one vinyl ester of a C1-C5 carboxylic acid; • from 0 wt% to 15 wt% of at least one functional monomer; and• from 0 wt% to 15 wt% of ethylene.
[0028] The relative proportions of the monomers in the first monomer composition are typically controlled such that the first stage polymer product has a glass transition temperature, Tg, less than 30°C, such as from -35°C to 20°C, such as from -30°C to 0°C. All glass transition temperatures of the copolymers produced by the present process are calculated by the Fox Flory equation, l / Tg=wi / Tg,i+w2 / Tg,2+ . . . +wn / Tg,n, where wi, W2, . . . wnare the weight fractions of monomers 1, 2, . . . , n, and Tg,i, Tg,2, . . . , Tg,nare the glass transition temperatures of their respective homopolymers (in Kelvin), as obtained by radical emulsion polymerization. The Tgvalues of the majority of homopolymers are known and are listed, for example, in Polymer Handbook, 4th edition, Brandrup, Immergut, Grulke (Eds.), Wiley, 1999.Second Monomer Composition
[0029] The second monomer composition used in the present process comprises from 50 wt% to 95 wt% of vinyl acetate, from 5 wt% to 40 wt% of ethylene, and from 0 wt% to 25 wt% of at least one vinyl ester other than vinyl acetate, each based on the total weight of monomers in the second monomer composition.
[0030] The vinyl acetate may be present in the second monomer composition at a concentration from 50 wt% to 95 wt%, such as from 60 wt% to 95 wt%, such as from 65 wt% to 90 wt%, such as from 70 wt% to 90 wt%, such as from 75 wt% to 90 wt%, based on the total weight of monomers in the second monomer composition.
[0031] The ethylene may be present in the second monomer composition at a concentration from 5 wt% to 40 wt%, such as from 5 wt% to 30 wt%, such as from 5 wt% to 20 wt%, such as from 8 wt% to 17 wt%, such as from 10 wt% to 15 wt%, based on the total weight of monomers in the second monomer composition.
[0032] Examples of vinyl esters other than vinyl acetate may include, but are not limited to, vinyl formate, vinyl propionate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl 2-ethylhexanoate, vinyl esters of saturated branched monocarboxylic acids having from 9 to 11 carbon atoms in the acid radical (e.g., VeoVa™ 9, VeoVa™ 10, and VeoVa™ 11), vinyl esters of relatively long-chain saturated or unsaturated fatty acids (e.g., vinyl laurate or vinyl stearate), vinyl esters of benzoic acid and substituted derivatives of benzoic acid (e.g., vinyl p-tert-butylbenzoate), the like, and any combination thereof.
[0033] When present, the at least one vinyl ester other than vinyl acetate may be present in the second monomer composition at a concentration from 0.1 wt% to 25 wt%, such as from 1 wt% to 20 wt%, such as from 5 wt% to 15 wt%, such as from 7 wt% to 13 wt%, based on the total weight of monomers in the second monomer composition. The second monomer composition may be free (contain 0.00 wt%) or be essentially free (contain 0.01 wt% or less) of vinyl esters other than vinyl acetate, based on the total weight of monomers in the second monomer composition.
[0034] Optionally, alkyl esters of (meth)acrylic acid may be included in the second monomer composition. The alkyl esters of (meth)acrylic acid may be C1-C22 alkyl esters of (meth)acrylic acid, preferably C 1 -C 14 alkyl esters of (meth)acrylic acid, and mixtures thereof. Examples of alkyl esters of (meth)acrylic acid may include, but are not limited to, methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, iso-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-hexyl(meth)acrylate, n-octyl (meth)acrylate, 2-octyl (meth)acrylate, iso-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-propylheptyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, stearyl (meth)acrylate, isobomyl (meth)acrylate, the like, and any combination thereof. Preferred alkyl esters of (meth)acrylic acid for the second monomer composition include methyl (meth)acrylate, n-butyl (meth)acrylate, iso-butyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, or combinations thereof, more preferably n-butyl acrylate, tert-butyl acrylate, 2-ethylhexyl acrylate, 2-octyl acrylate, n-octyl acrylate, or any combination thereof.
[0035] When present, the at least one alkyl ester of (meth)acrylic acid may be present in the second monomer composition at a concentration from 0.1 wt% to 20 wt%, such as from 1 wt% to 15 wt%, such as from 1 wt% to 10 wt%, such as from 1 wt% to 5 wt%, based on the total weight of monomers in the second monomer composition. The second monomer composition may be free (contain 0.00 wt%) or be essentially free (contain 0.01 wt% or less) of alkyl esters of (meth)acrylic acid, based on the total weight of monomers in the second monomer composition.
[0036] Optionally, the second monomer composition may also include at least one functional monomer. Examples of functional monomers may include, but are not limited to, carboxylic acidfunctional monomers, epoxy-functional monomers, silane-functional monomers, keto-functional monomers, sulfonic acid-functional monomers, ethylenically unsaturated phosphonic and phosphoric acids, ethylenically unsaturated carboxylic amides (e.g., acrylamide, methacrylamide), ethylenically unsaturated carboxylic anhydrides, the like, and any combination thereof.
[0037] Examples of carboxylic acid-functional monomers may include, but are not limited to, an ethylenically unsaturated C3-C8 monocarboxylic acid, an ethylenically unsaturated C4-C8 dicarboxylic acid, an ethylenically unsaturated C4-C8 dicarboxylic acid anhydride, the like, and any combination thereof.
[0038] The epoxy-functional monomers may be glycidyl compounds. Examples of epoxyfunctional monomers may include, but are not limited to, glycidyl acrylate, glycidyl methacrylate, allyl glycidyl ether, vinyl glycidyl ether, the like, and any combination thereof.
[0039] Examples of silane-functional monomers may include, but are not limited to, y-methacryloxypropyltris(2-methoxyethoxy)silane, trimethoxyvinylsilane, triethoxyvinylsilane, diethoxyvinylsilanol, ethoxyvinylsilanediol, triethoxyallylsilane, tripropoxyvinylsilane, triisopropoxyvinylsilane, tributoxyvinylsilane, triacetoxyvinylsilane, trimethylglycolvinylsilane,y-methacryloxypropyltrimethylglycolsilane, y-acryloxypropyltriethoxysilane, y-methacryloxypropyltrimethoxysilane, the like, and any combination thereof.
[0040] Examples of sulfonic acid-functional monomers may include, but are not limited to, vinyl sulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, an alkali metal salt of vinyl sulfonic acid, an alkali metal salt of 2-acrylamido-2-methylpropanesulfonic acid, an ammonium salt of vinyl sulfonic acid, an ammonium salt of 2-acrylamido-2-methylpropanesulfonic acid, the like, and any combination thereof. A preferred sulfonic-acid functional monomer is the sodium salt of vinyl sulfonic acid.
[0041] When present, the at least one functional monomer may be present in the second monomer composition at a concentration from 0.1 wt% to 10 wt%, such as from 0.1 wt% to 5 wt%, such as from 0.1 wt% to 3 wt%, such as from 0.2 wt% to 2 wt%, such as from 0.3 wt% to 1 wt%, based on the total weight of monomers in the second monomer composition. The second monomer composition may be free (contain 0.00 wt%) or be essentially free (contain 0.01 wt% or less) of functional monomers, based on the total weight of monomers in the second monomer composition.
[0042] Accordingly, the second monomer composition may include the following monomers, each based on the total weight of monomers in the second monomer composition:• from 50 wt% to 95 wt% of vinyl acetate;• from 5 wt% to 40 wt% of ethylene;• from 0 wt% to 25 wt% of at least one vinyl ester other than vinyl acetate;• from 0 wt% to 20 wt% of at least one alkyl ester of (meth)acrylic acid; and• from 0 wt% to 10 wt% of at least one functional monomer.
[0043] The relative proportions of the monomers in the second monomer composition are typically controlled such that the second stage polymer product has a glass transition temperature, Tg, of less than 30°C, such as from -15°C to 25°C, such as from -5°C to 20°C, such as from 0°C to 15°C, as calculated by the Fox Flory equation.
[0044] In most embodiments, the first stage polymer is arranged to have a lower glass transition temperature, Tg, than the second stage polymer, typically such that the Tgof the first stage polymer is at least 5°C, such as at least 10°C, lower than the second stage polymer.
[0045] The weight ratio of the first stage polymer to the second stage polymer is from 5:95 to 50:50, such as from 10:90 to 40:60, such as from 15:85 to 35:65.Third Monomer Composition
[0046] The optional third monomer composition used in the present process comprises from 30 wt% to 100 wt% of at least one ester, preferably at least two esters, of (meth)acrylic acid, and from 0 wt% to 20 wt% of at least one vinyl ester, each based on the total weight of monomers in the third monomer composition.
[0047] The alkyl esters of (meth)acrylic acid may be C 1 -C22 alkyl esters of (meth)acrylic acid, preferably Cl -Cl 4 alkyl esters of (meth)acrylic acid, and mixtures thereof. Examples of alkyl esters of (meth)acrylic acid may include, but are not limited to, methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, iso-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, 2-octyl (meth)acrylate, iso-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-propylheptyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, stearyl (meth)acrylate, isobomyl (meth)acrylate, the like, and any combination thereof. Preferred alkyl esters of (meth)acrylic acid for the third monomer composition include methyl (meth)acrylate, n-butyl (meth)acrylate, iso-butyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-octyl acrylate, n-octyl acrylate, or any combination thereof, more preferably methyl methacrylate and 2-ethylhexyl acrylate or n-butyl acrylate in combination.
[0048] The at least one alkyl ester of (meth)acrylic acid may be present in the third monomer composition at a concentration from 30 wt% to 100 wt%, such as from 50 wt% to 100 wt%, such as from 75 wt% to 100 wt%, such as from 90 wt% to 100 wt%, such as from 95 wt% to 100 wt%, based on the total weight of monomers in the third monomer composition.
[0049] The vinyl esters of a carboxylic acid may be vinyl esters of a C1-C20 carboxylic acid, preferably vinyl esters of a C1-C6 carboxylic acid. Examples of vinyl esters of a carboxylic acid may include, but are not limited to, vinyl formate, vinyl acetate, vinyl propionate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl 2-ethylhexanoate, vinyl esters of saturated branched monocarboxylic acids having from 9 to 11 carbon atoms in the acid radical (e.g., VeoVa™ 9, VeoVa™ 10, and VeoVa™ 11), vinyl esters of relatively long-chain saturated or unsaturated fatty acids (e.g., vinyl laurate or vinyl stearate), vinyl esters of benzoic acid and substituted derivatives of benzoic acid (e.g., vinyl p-tert-butylbenzoate), the like, and any combination thereof.
[0050] When present, the at least one vinyl ester may be present in the third monomer composition at a concentration from 0.1 wt% to 20 wt%, such as from 0.1 wt% to 15 wt%, suchas from 0.1 wt% to 10 wt%, based on the total weight of monomers in the third monomer composition. The second monomer composition may be free (contain 0.00 wt%) or be essentially free (contain 0.01 wt% or less) of vinyl esters, based on the total weight of monomers in the second monomer composition.
[0051] Optionally, the third monomer composition may also include at least one vinyl aromatic monomer. Examples of vinyl aromatic monomers may include, but are not limited to, styrene, vinyltoluene, vinylxylene, a-methylstyrene, o-chlorostyrene, the like, and any combination thereof.
[0052] When present, the at least one vinyl aromatic monomer may be present in the second monomer composition at a concentration from 0.1 wt% to 70 wt%, such as from 0.1 wt% to 50 wt%, such as from 0.1 wt% to 30 wt%, such as from 0.1 wt% to 20 wt%, such as from 0.1 wt% to 10 wt%, such as from 0.1 wt% to 5 wt%, based on the total weight of monomers in the second monomer composition. The second monomer composition may be free (contain 0.00 wt%) or be essentially free (contain 0.01 wt% or less) of vinyl aromatic monomers, based on the total weight of monomers in the second monomer composition.
[0053] Optionally, the third monomer composition may also include at least one functional monomer. Examples of functional monomers may include, but are not limited to, carboxylic acidfunctional monomers, epoxy-functional monomers, silane-functional monomers, keto-functional monomers, sulfonic acid-functional monomers, ethylenically unsaturated phosphonic and phosphoric acids, ethylenically unsaturated carboxylic amides (e.g., acrylamide, methacrylamide), ethylenically unsaturated carboxylic anhydrides, the like, and any combination thereof.
[0054] Examples of carboxylic acid-functional monomers may include, but are not limited to, an ethylenically unsaturated C3-C8 monocarboxylic acid, an ethylenically unsaturated C4-C8 dicarboxylic acid, an ethylenically unsaturated C4-C8 dicarboxylic acid anhydride, the like, and any combination thereof.
[0055] The epoxy-functional monomers may be glycidyl compounds. Examples of epoxyfunctional monomers may include, but are not limited to, glycidyl acrylate, glycidyl methacrylate, allyl glycidyl ether, vinyl glycidyl ether, the like, and any combination thereof.
[0056] Examples of silane-functional monomers may include, but are not limited to, y-methacryloxypropyltris(2-methoxyethoxy)silane, trimethoxyvinylsilane, triethoxyvinylsilane, diethoxyvinylsilanol, ethoxyvinylsilanediol, triethoxyallylsilane, tripropoxyvinylsilane,triisopropoxyvinylsilane, tributoxyvinylsilane, triacetoxyvinylsilane, trimethylglycolvinylsilane, y-methacryloxypropyltrimethylglycolsilane, y-acryloxypropyltriethoxysilane, y-methacryloxypropyltrimethoxysilane, the like, and any combination thereof.
[0057] Examples of sulfonic acid-functional monomers may include, but are not limited to, vinyl sulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, an alkali metal salt of vinyl sulfonic acid, an alkali metal salt of 2-acrylamido-2-methylpropanesulfonic acid, an ammonium salt of vinyl sulfonic acid, an ammonium salt of 2-acrylamido-2-methylpropanesulfonic acid, the like, and any combination thereof. A preferred sulfonic-acid functional monomer is the sodium salt of vinyl sulfonic acid.
[0058] When present, the at least one functional monomer may be present in the third monomer composition at a concentration from 0.1 wt% to 10 wt%, such as from 0.1 wt% to 5 wt%, such as from 0.1 wt% to 2 wt%, such as from 0.1 wt% to 1 wt%, such as from 0.1 wt% to 0.5 wt%, based on the total weight of monomers in the third monomer composition. The third monomer composition may be free (contain 0.00 wt%) or be essentially free (contain 0.01 wt% or less) of functional monomers, based on the total weight of monomers in the third monomer composition.
[0059] Accordingly, the third monomer composition may include the following monomers, each based on the total weight of monomers in the third monomer composition:• from 30 wt% to 100 wt% of at least one alkyl ester of (meth)acrylic acid;• from 0 wt% to 20 wt% of at least one vinyl ester;• from 0 wt% to 70 wt% of at least one vinyl aromatic monomer; and• from 0 wt% to 10 wt% of at least one functional monomer.
[0060] The relative proportions of the monomers in the third monomer composition are typically controlled such that the third stage polymer product has a glass transition temperature, Tg, from 5°C to 120°C, such as from 15°C to 100°C, such as from 25°C to 80°C, such as from 35°C to 60°C, as calculated by the Fox Flory equation.
[0061] In most embodiments, the second stage polymer is arranged to have a lower glass transition temperature, Tg, than the third stage polymer, typically such that the Tgof the second stage polymer is at least 5°C, such as 10°C, such as at least 20°C lower than the third stage polymer.
[0062] When present, the weight ratio of the third stage polymer to the second stage polymeris from 5:95 to 40:60, such as from 10:90 to 30:70, such as from 15:85 to 25:75.
[0063] The polymer product may contain from 5 wt% to 40 wt% (such as from 10 wt% to 35 wt%, such as from 15 wt% to 30 wt%) of the first stage polymer, 30 wt% or greater (such as 40 wt% or greater, such as 50 wt% or greater, such as 55 wt% or greater, such as 30 wt% to 95 wt%, such as 50 wt% to 90 wt% such as from 55 wt% to 85 wt%) of the second stage polymer, and from 0 wt% to 30 wt% (such as from 5 wt% to 30 wt%, such as from 10 wt% to 25 wt%, such as from 10 wt% to 20 wt%) of the third stage polymer, each based on a total weight of the polymer product.Dispersion Stabilization System
[0064] Both during and after polymerization, the multi-stage polymer described herein is stabilized in the form of an aqueous copolymer dispersion or latex. The copolymer dispersion is therefore prepared in the presence of and subsequently contains a stabilization system which generally comprises emulsifiers, in particular nonionic emulsifiers and / or anionic emulsifiers, and / or protective colloids. Mixtures of the different stabilizers can also be employed.
[0065] The amount of emulsifier employed will generally be at least 0.5 wt%, based on the total quantity of monomers in the copolymer dispersion. Generally, emulsifiers can be used in amounts up to about 8 wt%, based on the total quantity of monomers in the copolymer dispersion. Emulsifiers employed with preference herein are nonionic emulsifiers having alkylene oxide groups and / or anionic emulsifiers having sulfate, sulfonate, phosphate and / or phosphonate groups. Such emulsifiers, if desired, can be used together with molecularly or dispersely water-soluble polymers. Preferably also the emulsifiers used contain no alkylphenolethoxylate (APEO) structural units.
[0066] Examples of suitable nonionic emulsifiers include acyl, alkyl, oleyl, and alkylaryl ethoxylates. These products are commercially available, for example, under the name GENAPOL®, LUTENSOL® or EMULAN®. They include, for example, ethoxylated mono-, di-, and tri-alkylphenols (EO degree: 3 to 50, alkyl substituent radical: C4 to C12) and also ethoxylated fatty alcohols (EO degree: 3 to 80; alkyl radical: C8 to C36), especially C10-C14 fatty alcohol (3-40) ethoxylates, C11-C15 oxo-process alcohol (3-40) ethoxylates, C16-C18 fatty alcohol (11-80) ethoxylates, Cl 1 oxo-process alcohol (3-40) ethoxylates, C13 oxo-process alcohol (3-40) ethoxylates, polyoxyethylenesorbitan monooleate with 20 ethylene oxide groups, copolymers of ethylene oxide and propylene oxide having a minimum ethylene oxide content of 10 wt%, the polyethylene oxide (4-40) ethers of oleyl alcohol, and the polyethene oxide (4-40) ethers ofnonylphenol. Particularly suitable are the polyethylene oxide (4-40) ethers of fatty alcohols, more particularly of oleyl alcohol, stearyl alcohol or Cn alkyl alcohols.
[0067] The amount of nonionic emulsifiers used in preparing the copolymer dispersions herein is typically up to about 8 wt%, such as up to about 5 wt%, such as up to about 3 wt%, based on the total monomer quantity. Mixtures of nonionic emulsifiers can also be employed.
[0068] Examples of suitable anionic emulsifiers include sodium, potassium, and ammonium salts of linear aliphatic carboxylic acids of chain length C12-C20, sodium hydroxyoctadecanesulfonate, sodium, potassium, and ammonium salts of hydroxy fatty acids of chain length Ci2-C2oand their sulfonation and / or sulfation and / or acetylation products, alkyl sulfates, including those in the form of triethanolamine salts, alkyl(Cio-C2o) sulfonates, alkyl(Cw-C20) arylsulfonates, and their sulfonation products, lignosulfonic acid and its calcium, magnesium, sodium, and ammonium salts, resin acids, hydrogenated and dehydrogenated resin acids, and their alkali metal salts, dodecylated sodium diphenyl ether disulfonate, sodium alkyl sulfate, sulfated alkyl or aryl ethoxylate with EO degree between 1 and 30, for example ethoxylated sodium lauryl ether sulfate or a salt of a bisester, preferably of a bis-C4-Ci8 alkyl ester, of a sulfonated dicarboxylic acid having 4 to 8 carbon atoms, or a mixture of these salts, preferably sulfonated salts of esters of succinic acid, more preferably salts, such as alkali metal salts, of bis-C4-Ci8 alkyl esters of sulfonated succinic acid, or phosphates of polyethoxylated alkanols. Particularly suitable are sodium or potassium alkyl sulfates such as sodium lauryl sulfate, and sodium, potassium or ammonium salts of sulfated C10-C16 alkyl ethoxylates with an EO degree between 1 and 30.
[0069] The amount of anionic emulsifiers used can typically range from about 0.1% to about 3.0 wt%, such as from about 0.1% to about 2.0 wt%, such as from about 0.25% to about 1.0 wt%, based on the total monomer quantity. Mixtures of anionic emulsifiers can also be employed.
[0070] Also suitable as stabilizers for the present dispersions are copolymerizable nonionic and anionic surfactants such as those disclosed in US 2014 / 0243552. Other suitable copolymerizable surfactants are sold under the trade names HITENOL® BC, HITENOL® KH, HITENOL® AR, ADEKA REASOAP SR, and ADEKA REASOAP ER.
[0071] Along with emulsifiers, the aqueous copolymer dispersions employed in accordance with the present development may also comprise as part of the stabilizer system a selected type of protective colloid based on cellulose ethers, polyvinylalcohol, polyvinylpyrrolidone, polyacrylic acid, maleic acid styrene copolymers or other water soluble polymers. Suitable protective colloidsused in the copolymer dispersions herein include water-soluble or water-dispersible polymeric modified natural substances based on cellulose ethers. Such cellulose ethers have a viscosity, when tested as a 1 wt% aqueous in water at 25°C, of 5 mPa s to 5,000 mPa s, such as of 10 mPa s to about 1,500 mPa s, such as 10 mPa s to 500 mPa s. Mixtures of cellulose ethers may be used to achieve these viscosity values. Examples of suitable cellulose ether materials include methyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, ethyl hydroxyethyl cellulose, methyl hydroxyethyl cellulose and combinations of these cellulose ethers.
[0072] Another suitable protective colloid is polyvinylalcohol. Suitable polyvinylalcohols have a degree of hydrolysis of 60 to 100 mol% and a viscosity of the 4% aqueous solution at 20°C of 2 mPa s to 70 mPa s, such as from 4 mPa s to 40 mPa s.
[0073] The protective colloids can be used individually or in combination. In the case of combinations, the two or more colloids can each differ in their molecular weights or they can differ in their molecular weights and in their chemical composition, such as the degree of hydrolysis, for example.
[0074] When protective colloids are used, the amount thereof, based on the total amount of monomers used, is typically from 0.1 to 5 parts by weight, such as from 0.3 to 3 parts by weight.
[0075] If the weight ratio of the second stage polymer to the third stage polymer is less than 80:20, the present dispersions preferably do not comprise any protective colloid at all, or the amount of protective colloid, based on the total amount of monomers used, is less than 1 wt%, such as less than 0.5 wt%.
[0076] In addition to the emulsifiers and protective colloids that are used during the emulsion polymerization of the copolymers herein, it is also possible to add further emulsifiers, protective colloids and / or other stabilizers after the polymerization.Preparation of the Polymer Dispersion
[0077] The desired copolymer dispersion is produced by multi-stage emulsion polymerization of the monomers and stabilizing system described above in an aqueous medium and in the presence of one or more free radical initiators. Suitable free radical initiators include hydrogen peroxide, benzoyl peroxide, cyclohexanone peroxide, isopropyl cumyl hydroperoxide, persulfates of potassium, of sodium and of ammonium, peroxides of saturated monobasic aliphatic carboxylic acids having an even number of carbon atoms and a C8-C12 chain length, tert-butyl hydroperoxide, di-tert-butyl peroxide, diisopropyl percarbonate, azoisobutyronitrile, acetylcyclohexanesulfonylperoxide, tert-butyl perbenzoate, tert-butyl peroctanoate, bis(3,5,5-trimethyl)hexanoyl peroxide, tert-butyl perpivalate, hydroperoxypinane, p-methane hydroperoxide. The abovementioned compounds can also be used within redox systems, using transition metal salts, such as iron(II) salts, or other reducing agents. Zinc and alkali metal salts of oxymethanesulfinic acid, 2-hydroxy-2-sulfmicacetic acid, and 2-hydroxy-2-sulfonicacetic acid, hydroxylamine salts, sodium dialkyldithiocarbamate, sodium bisulfite, ammonium bisulfite, sodium dithionite, diisopropyl xanthogen disulfide, ascorbic acid, tartaric acid, and isoascorbic acid can also be used as reducing agents.
[0078] The multi-stage emulsion polymerization may be carried out in accordance with the customary techniques of emulsion polymerization. Preferably, the process is carried out by polymerizing in a first stage the first monomer composition in an aqueous phase in the presence of emulsifiers, initiators and, if desired, protective colloids, at suitable temperatures of, for example from 20°C to 120°C, such as 40°C to 110°C, and such as 50°C to 95°C to produce a first polymer phase. The reaction temperature may also be ramped up during of the polymerization as described in U.S. patent application 2017 / 029544.
[0079] After the complete or virtually complete conversion of at least 85%, such as at least 90%, such as at least 95% of the first stage monomers, the second monomer composition is polymerized in a second stage in the aqueous phase in the presence of the first polymer phase as well as emulsifiers, initiators and, if desired, protective colloids, at suitable temperatures of, for example, from 20°C to 120°C, such as 40°C to 110°C, such as from 60°C to 100°C, such as from 75°C to 95°C, to produce the second polymer phase and thereby to obtain polymer particles comprising the first and second polymer phase. The emulsion polymerization of the second stage can be performed with or without a pre-emulsion, preferably without a pre-emulsion.
[0080] After the complete or virtually complete conversion of at least 85%, such as at least 90%, such as at least 95% of the second stage monomers, the third monomer composition may optionally be polymerized in a third stage in the aqueous phase in the presence of the first and second polymer phases as well as emulsifiers, initiators and, if desired, protective colloids, at suitable temperatures of, for example, from 20°C to 120°C, such as 40°C to 110°C, 60°C to 100°C, such as from 75 °C to 95 °C, to produce the third polymer phase and thereby to obtain polymer particles comprising the first, second, and third polymer phases. The emulsion polymerization of the third stage can be performed with or without a pre-emulsion, preferably without a pre-emulsion.
[0081] In some embodiments, it may be desirable to pre-polymerize a small amount (less than 20 wt%) of the first monomer composition to produce an in-situ seed before the remaining amounts of the first, second, and optionally third monomer compositions are sequentially metered into the reactor to form the final polymer dispersion (or polymer product).
[0082] The molecular weight of the various copolymers in the copolymer dispersions herein can be adjusted by adding small amounts of one or more molecular weight regulator substances, also known as chain transfer agents (CTA). These CT As are generally used in an amount of up to 2 wt%, based on the total weight of the monomers in first, second, and third monomer compositions. It is possible to use all of the CTAs known to the skilled artisan. Preference is given to organic thio compounds such as methylthiol, ethylthiol, n-propylthiol n-butylthiol, n-hexylthiol, n-octylthiol, n-decylthiol, n-dodecylthiol, n-tetradecylthiol, hexadecylthiol, n-octadecylthiol, cyclohexylthiol, isopropylthiol, tert-butylthiol, tert-nonylthiol, tert-dodecylthiol, 4-methylbenzenethiol, 2-mercaptopropionic acid, isooctyl 3-mercaptopropionate, 4,4'-thiobisbenzenethiol, pentaerythritol tetrakis(2-mercaptoacetate) and pentaerythritol tetrakis(3-mercaptopropionate) .
[0083] On completion of the polymerization, a further, preferably chemical after-treatment, especially with redox catalysts, for example combinations of the above-mentioned oxidizing agents and reducing agents, may follow to reduce the level of residual unreacted monomer on the product. In addition, residual monomer can be removed in known manner, for example by physical demonomerization, i.e. distillative removal, especially by means of steam distillation, or by stripping with an inert gas. A particularly efficient combination is one of physical and chemical methods, which permits lowering of the residual monomers to very low contents (<1000 ppm, preferably <100 ppm).
[0084] The polymerized particles produced by the present process typically have a weight-averaged diameter of less than 400 nm, such as less than 300 nm, such as from 100 nm to 200 nm, such as from 120 nm to 160 nm, as measured by a combination of laser diffraction and polarization intensity differential scattering (PIDS) using a Beckman Coulter LS 13320 Particle Size Analyzer.
[0085] If any of the monomer compositions comprise keto-functional monomers, the final polymers may also contain a water-soluble cross-linking agent. Such a cross-linking agent will react with specific polymer functionalities such as carbonyl or 1,3-dicarbonyl groups as water isremoved from the coating compositions herein and as a film or coating is formed from the polymerized components.
[0086] A type of water-soluble cross-linking agent that can be used in the compositions herein comprises a compound which contains at least two hydrazine and / or hydrazide moieties. Particularly suitable are dihydrazine compounds of aliphatic dicarboxylic acids of 2 to 10, in particular 4 to 6, carbon atoms, e.g., oxalic acid dihydrazide, malonic acid dihydrazide, succinic acid dihydrazide, glutaric acid dihydrazide, adipic acid dihydrazide, sebacic acid dihydrazide, maleic acid dihydrazide, fumaric acid dihydrazide and / or itaconic acid dihydrazide. Water-soluble aliphatic dihydrazines of 2 to 4 carbon atoms, e.g., ethylene- 1,2-dihydrazine, propylene-1,3-dihydrazine or butylene- 1,4-dihydrazine, are also suitable. Adipic acid dihydrazide (ADH) is a preferred water-soluble cross-linking agent for use in the compositions herein, especially those produced from monomer compositions containing diacetone acrylamide (DAAM).
[0087] Other suitable water-soluble cross-linking agents are compounds which contain at least two amine functional moieties such as ethylene diamine and hexamethylene diamine Such crosslinking agents are preferred in combination with polymers comprising 1,3-dicarbonyl groups, such as acetoacetoxy ethyl methacrylate (AAEM).
[0088] Generally, such water-soluble cross-linking agents are post added to the dispersion such that the molar ratio of cross-linking agent functional groups to polymer functional groups is between about 0.1 and about 2.0. More preferably the molar ratio of cross-linking agent functional groups to copolymer functional groups in the blend will be between about 0.5 and 2.0.
[0089] The aqueous polymer dispersions produced by the process of the invention generally have a solids content of from 30 to 70 wt%, such as from 40 to 60 wt%, such as from 50 to 55 wt%, and a pH between 2.5 and 8, such as between 3.0 and 7, such as between 4.5 and 6.Coating Compositions
[0090] The aqueous multistage copolymer dispersions described herein are stable fluid systems which can be used to produce coating compositions suitable for coating a multitude of substrates. Suitable substrates are, for example, wood, concrete, metal, glass, ceramics, plastic, plasters, wallpaper, other paper, or painted, primed or weathered substrates. The coating composition is applied to the substrate to be coated in a manner dependent on the configuration of the coating composition. The application can, depending on the viscosity and the pigment content of the formulation and on the substrate, be effected by means of rolling, brushing, knife coating,dipping or as a spray.
[0091] Preferred uses of such coating compositions are in plasters and renders, and in facade paints, wood protection paints, and interior paints, particularly solvent- and plasticizer-free paints. When used in such applications, the aqueous multistage copolymer dispersions produced by the present process is typically combined with one or more conventional fillers and / or pigments. In this context, pigments are understood as meaning solids which have a refractive index greater than or equal to 1.75, whereas fillers are understood as meaning solids which have a refractive index of less than 1.75.
[0092] Examples of mineral fillers are alkaline earth metal oxides, alkaline earth metal carbonates and / or silicate fillers, in particular calcium carbonate, mica, feldspar, kaolin, quartz powders and / or particulate quartz fractions and marble powders and / or particulate marble fractions. When used in plasters and renders, the filler generally has a particle size of at least 40 pm, whereas when used in a paint, the filler typically has a size of 1 to 40 pm.
[0093] Pigments may be any inorganic or organic and may be color-imparting or opaque finely divided solids. Preferred pigments have a mean diameter for the primary particle of less than or equal to 1 pm, such as from 0.1 to 0.5 pm, determined by sedimentation analysis according to DIN 66115. Examples of inorganic pigments are metal oxides, such as titanium dioxide, iron oxide or zinc oxide, in particular titanium dioxide. Examples of organic pigments are phthalocyanines, in particular phthalocyanine blue, or diaryl pigments, azo pigments or quinacridone pigments.
[0094] To disperse the fillers and pigments in water, auxiliaries based on anionic or non-ionic wetting agents, such as preferably, for example, sodium pyrophosphate, sodium polyphosphate, naphthalenesulfonate, sodium polyacrylate, sodium polymaleinates and polyphosphonates such as sodium 1 -hydroxyethane- 1,1 -diphosphonate and sodium nitrilotris(methylenephosphonate), may be added.
[0095] Thickeners may also be added to the coating compositions described herein. Thickeners which may be used include, inter alia, cellulose derivates such as methylcellulose (MC), hydroxyethylcellulose (HEC) and carboxymethylcellulose. Other thickeners which may be used include casein, gum arabic, gum tragacanth, starch, sodium alginate, polyvinyl alcohol, polyvinylpyrrolidone, sodium polyacrylate and water-soluble copolymers based on acrylic and methacrylic acid, such as acrylic acid / acrylamide and methacrylic acid / acrylic ester copolymers. Hydrophobically-modified alkali soluble (acrylic) emulsions (HASE), hydrophobically-modifiedethoxylate (poly)urethanes (HEUR), and polyether polyols (PEPO) are also available. Inorganic thickeners, such as, for example, bentonites or hectorite, may also be used.
[0096] The coating compositions may also comprise crosslinking additives. Such additives may be: aromatic ketones, for example alkyl phenyl ketones, which may have one or more substituents on the phenyl ring, or benzophenone and substituted benzophenones as photoinitiators. Photoinitiators suitable for this purpose are disclosed, for example, in DE-A-3827 975 and EP-A-0417568. In addition, it is possible to use, in the coating compositions, as further additives, waxes based on paraffins and polyethylene, and matting agents, defoamers, pH modifiers, preservatives or hydrophobicizing agents, UV stabilizers, fibers, plasticizers and further additives known to those skilled in the art. Examples of coalescent agents are white spirit, TEXANOL®, TXIB®, butyl glycol, butyl diglycol, butyl dipropylene glycol, and butyl tripropylene glycol. Examples of plasticizers are dimethyl phthalate, diisobutyl phthalate, diisobutyl adipate, COASOL B® and PLASTILIT 3060®. Examples of defoamers are mineral oil defoamers or silicone defoamers. Examples of UV stabilizers are sterically hindered piperidine compounds (HALS) or benzophenone derivatives.Properties of Coating Compositions
[0097] The minimum temperature required for the polymer dispersion or coating composition to form a film is referred to as the minimum film forming temperature (MFFT) (DIN ISO 2115). The aqueous multistage copolymer dispersions herein may have a MFFT of less than 20°C, such as less than 10°C, such as less than 5°C, to allow the formulation of coating compositions with less than 2.5 weight percent, such as less than 1 weight percent of any organic solvent, plasticizer or coalescent agent. Most preferably, the paint compositions are free of any organic solvent, plasticizer or coalescent agent.
[0098] The resulting coatings exhibit reduced capillary water uptake. In particular, coatings produced from the aqueous multistage copolymer dispersions described herein usually exhibit a water absorption coefficient W24 of 0.1 kg m-2h-05or less (after 3 conditionings of the specimens), such as 0.07 kg m-2h“°5or less and a water absorption coefficient W24of 0.2 kg m-2h“°5or less during the initial immersion in water when tested in accordance with DIN EN 1062-3, as described in the Examples.
[0099] The aqueous multistage copolymer dispersions described herein can also be used as binders for paints, plaster compositions of all kinds, such as synthetic resin-bound plasters, paste-form tile adhesives, paste-form sealants and paste-form sealing compositions, as well as plaster-coated thermal insulation systems. Thermal insulation systems utilizing the present coating compositions have excellent flame retardant properties.Example Embodiments
[0100] The following numbered embodiments are contemplated. All combinations of features and embodiments are contemplated.
[0101] Embodiment 1. An emulsion polymerization process for producing a polymer product comprising: (i) polymerizing, in a first stage, a first monomer composition comprising from 15 wt% to 100 wt% of at least one vinyl ester of a C6-C20 carboxylic acid and from 0 wt% to 85 wt% of at least one alkyl ester of (meth)acrylic acid, each based on the total weight of monomers in the first monomer composition, to produce a first stage polymer; and (ii) polymerizing, in a second stage and in the presence of the first stage polymer, a second monomer composition comprising from 50 wt% to 95 wt% of vinyl acetate, from 5 wt% to 40 wt% of ethylene, and from 0 wt% to 25 wt% of at least one vinyl ester other than vinyl acetate, each based on the total weight of monomers in the second monomer composition, to produce a second stage polymer, and optionally (iii) polymerizing, in a third stage and in the presence of the first stage polymer and the second stage polymer, a third monomer composition comprising from 30 wt% to 100 wt% of at least one alkyl ester of (meth)acrylic acid and from 0 wt% to 20 wt% of at least one vinyl ester of a carboxylic acid, each based on the total weight of monomers in the third monomer composition, to produce a third stage polymer, wherein the first stage polymer is from 5 wt% to 40 wt%, the second stage polymer is 30 wt% or greater, and the third stage polymer is from 0 wt% to 30 wt%, each based on a total weight of the polymer product.
[0102] Embodiment 2. The process of Embodiment 1, wherein the first monomer composition comprising from 20 wt% to 90 wt%, preferably from 40 wt% to 80 wt%, or more preferably from 50 wt% to 80 wt% of at least one vinyl ester of a C6-C20 carboxylic acid and from 10 wt% to 80 wt%, preferably from 20 wt% to 60 wt%, or more preferably from 25 wt% to 60 wt% of at least one alkyl ester of (meth)acrylic acid, each based on the total weight of monomers in the first monomer composition
[0103] Embodiment 3. The process of any preceding Embodiment, wherein the second monomer composition comprising from 60 wt% to 95 wt%, preferably from 65 wt% to 90 wt%, or more preferably from 70 wt% to 90 wt% of vinyl acetate, from 5 wt% to 30 wt%, preferablyfrom 5 wt% to 20 wt%, or more preferably from 10 wt% to 15 wt% of ethylene, and from 0.1 wt% to 25 wt%, preferably from 5 wt% to 20 wt%, or more preferably from 5 wt% to 15 wt% of at least one vinyl ester other than vinyl acetate, each based on the total weight of monomers in the second monomer composition.
[0104] Embodiment 4. The process of any preceding Embodiment, wherein the third stage is performed.
[0105] Embodiment 5. The process of Embodiment 4, wherein the third monomer composition comprises from 50 wt% to 100 wt%, or preferably from 75 wt% to 100 wt% of at least one alkyl ester, preferably at least two alkyl esters, of (meth)acrylic acid.
[0106] Embodiment 6. The process of any preceding Embodiment, wherein the first monomer composition further comprises from 0.1 wt% to 15 wt% of at least one functional monomer, wherein the second monomer composition further comprises from 0.1 wt% to 10 wt% of at least one functional monomer, and / or wherein the third monomer composition further comprises from 0.1 wt% to 10 wt% of at least one functional monomer.
[0107] Embodiment 7. The process of Embodiment 6, wherein the at least one functional monomer comprises a carboxylic acid-functional monomer, a sulfonic acid-functional monomer, an epoxy-functional monomer, and a silane-functional monomer, or any combination thereof.
[0108] Embodiment 8. The process of any preceding Embodiment, wherein the first stage polymer has a lower glass transition temperature, Tg, than the second stage polymer.
[0109] Embodiment 9. The process of any preceding Embodiment, wherein the second stage polymer has a lower glass transition temperature, Tg, than the third stage polymer.
[0110] Embodiment 10. The process of any preceding Embodiment, wherein the glass transition temperature Tgof the first stage polymer is at least 5°C, preferably at least 10°C, lower than the second stage polymer.
[0111] Embodiment 11. The process of any preceding Embodiment, wherein the glass transition temperature Tgof the second stage polymer is at least 5°C, preferably at least 10°C, lower than the third stage polymer.
[0112] Embodiment 12. The process of any preceding Embodiment, wherein the first stage polymer has a Tgless than 30°C, preferably from -35°C to 20°C, or more preferably from -30°C to 0°C.
[0113] Embodiment 13. The process of any preceding Embodiment, wherein the secondstage polymer has a Tgless than 30°C, preferably from -15°C to 25°C, or more preferably from -5°C to 20°C.
[0114] Embodiment 14. The process of any preceding Embodiment, wherein the third stage polymer has a Tgof 5°C to 120°C, preferably from 15°C to 100°C, or more preferably from 25°C to 80°C.
[0115] Embodiment 15. A polymer dispersion produced by the process of any of Embodiments 1-14.
[0116] Embodiment 16. The polymer dispersion of Embodiment 15 and having a minimum film forming temperature of less than 20°C, preferably less than 10°C, or more preferably less than 5°C.
[0117] Embodiment 17. The polymer dispersion of any one of Embodiments 15-16, wherein the particles of the polymer dispersion have a weight-averaged diameter of less than 400 nm, preferably less than 300 nm, as measured by laser diffraction and polarization intensity differential scattering (PIDS) using a Beckman Coulter LS 13320 Particle Size Analyzer.
[0118] Embodiment 18. A coating composition comprising the polymer dispersion of any one of Embodiments 15-17, at least one pigment and / or at least one filler.
[0119] Embodiment 19. The coating composition of Embodiment 18, wherein the coating is a facade paint or a plaster.
[0120] Embodiment 20. A thermal insulation system comprising the facade paint or plaster of Embodiment 19.
[0121] Embodiment 21. The coating composition of Embodiment 18, wherein the coating is a wood protection paint or an interior wall paint.Examples
[0122] Comparative Example 1. An aqueous solution consisting of the following ingredients was introduced into a pressure reactor equipped with a stirrer, jacket heating, and metering pumps: 25755 g of water, 84 g of sodium acetate (anhydrous), 1430 g of a 70% active aqueous solution of undecyl ethoxylate with 28 ethylene oxide units, 1112 g of a 15% active aqueous solution of sodium lauryl sulphate, 555 g of a 30% active aqueous solution of sodium vinyl sulphonate, 890 g of a 15% active aqueous solution of polyvinyl alcohol, 13.5 g of sodium metabisulfite, and 0.08 g of (NH4)2Fe(SO4)2.
[0123] The atmosphere inside the reactor was freed from oxygen and ethylene waspressurized in the reactor. At an ethylene pressure of 15 bar, a mixture of 14 g of vinyltriethoxysilane (VTES) and 1707 g of vinyl acetate (VAc), as well as 665 g of an 11% active aqueous solution of sodium peroxodisulfate was metered in. The system was heated up to internal temperature of 65°C. At 65°C, the pressure was raised to 35 bar, and a mixture of 186 g of VTES and 22680 g of VAc was metered in 210 minutes. The pressure was kept at 35 bar until 3420 g of ethylene was in the reactor. Jacket cooling was applied to remove the heat of reaction. After the end of the VAc / VTES feed, a mixture of 3885 g of methyl methacrylate (MMA) and 1665 g of 2-ethylhexyl acrylate (EHA) as well as 625 g of a 5.5% active aqueous solution of sodium peroxodisulfate was added in 30 minutes. The temperature was raised to 85°C and kept for 1 hour after all additions, and then the system was cooled down.
[0124] The properties of the resulting polymer dispersion are summarized in Table 1.
[0125] Comparative Example 2. An aqueous solution consisting of the following ingredients was introduced into a 10-liter pressure reactor equipped with a stirrer, jacket heating, and metering pumps: 3443 g of deionized water, 137 g of a 70% active aqueous solution of undecyl ethoxylate with 28 ethylene oxide units, 318 gofa l5% active aqueous solution of sodium lauryl sulfate, 96 g of a 25% active aqueous solution of sodium vinyl sulfonate, 12 g of sodium acetate (anhydrous), 1.9 g sodium metabisulfite and 1.1 g of a 1% active solution of ferrous sulfate heptahydrate. The atmosphere inside the reactor was flooded with nitrogen. A first monomer composition consisting of 2486 g of VAc, 1434 g of versatic acid vinyl ester (VEOVA®10), 478 g of n-butyl acrylate (BuA), and 29 g of VTES was prepared. 25% of the foregoing monomer composition was added into the reactor as a pre-charge. The reaction mix was heated to 80°C, and the reactor was pressurized with ethylene to 5 bar.
[0126] To start the reaction an oxidizer solution comprising 383 g deionized water and 14.3 g of sodium peroxodisulfate was added with a rate of 240 g / h. After initiation was observed through a temperature increase, the reactor temperature set-point was raised to 85°C. When the exotherm had disappeared at 85°C (indicating consumption of the pre-charged monomers), the remaining 75% of the first monomer composition was added with a constant dosage rate over 110 min, and the reactor was pressurized with 383 g of ethylene at a maximum pressure of 50 bar. With the start of the monomer addition and pressurization, the rate of addition for the oxidizer solution was reduced to a rate achieving a 20 min overrun of oxidizer solution over the monomer slow add.
[0127] After the additions, the temperature was kept at 85 °C for an additional 15 min and was then cooled to 40°C before release from the reactor.
[0128] The properties of the resulting polymer dispersion are summarized in Table 1.
[0129] Comparative Example 3. An aqueous solution consisting of the following ingredients was introduced into a 10-liter pressure reactor equipped with a stirrer, jacket heating and metering pumps: 3443 g of deionized water, 137 g of a 70% active aqueous solution of undecyl ethoxylate with 28 ethylene oxide units, 319 gofa l5% active aqueous solution of sodium lauryl sulfate, 96 g of a 25% active aqueous solution of sodium vinyl sulfonate, 12 g of sodium acetate (anhydrous), 1.9 g sodium meta bisulfite and 1.1 g of a 1% active solution of ferrous sulfate heptahydrate. The atmosphere inside the reactor was flooded with nitrogen. A first monomer composition consisting of 3347 g of VAc, 478 g of versatic acid vinyl ester (VEOVA®10), 478 g of BuA, and 29 g of VTES was prepared, and 25% of this mixture are added into the reactor as a pre-charge. The reaction mix was heated to 80°C, and the reactor was pressurized with ethylene to 5 bar.
[0130] To start the reaction an oxidizer solution comprising 383 g deionized water and 14.3 g of sodium peroxodisulfate was added with a rate of 240 g / h. After initiation was observed through a temperature increase, the reactor temperature set-point was raised to 85°C. When the exotherm had disappeared at 85°C (indicating consumption of the pre-charged monomers), the remaining 75% of the first monomer composition was added with a constant dosage rate over 110 min and the reactor was pressurized with 478 g of ethylene at a maximum pressure of 50 bar. With the start of the monomer addition and pressurization, the rate of addition for the oxidizer solution was reduced to a rate achieving a 20 min overrun of oxidizer solution over the monomer slow add.
[0131] After the additions, the temperature was kept at 85 °C for an additional 15 min and was then cooled to 40°C before release from the reactor.
[0132] The properties of the resulting polymer dispersion are summarized in Table 1.
[0133] Inventive Example 1. An aqueous solution consisting of the following ingredients was introduced into a 10-liter pressure reactor equipped with a stirrer, jacket heating and metering pumps: 3443 g of deionized water, 137 g of a 70% active aqueous solution of undecyl ethoxylate with 28 ethylene oxide units, 319 g of a 15% active aqueous solution of sodium lauryl sulfate, 96 g of a 25% active aqueous solution of sodium vinyl sulfonate, 12 g of sodium acetate(anhydrous), 1.9 g sodium meta bisulfite, and 1.1 g of a 1% active solution of ferrous sulfate heptahydrate. The atmosphere inside the reactor was flooded with nitrogen. A first monomer composition consisting of 1076 g of versatic acid vinyl ester (VEOVA®10) and 357 g of BuA was added into the reactor as a pre-charge. The reaction mix was heated to 80°C, and the reactor was pressurized with ethylene to 5 bar.
[0134] To start the reaction an oxidizer solution comprising 383 g deionized water and 14.3 g of sodium peroxodisulfate was added with a rate of 240 g / h. After initiation was observed through a temperature increase, the reactor temperature set-point was raised to 85°C. When the exotherm had disappeared at 85°C (indicating consumption of the pre-charged monomers), a second monomer composition prepared of 2486 g of VAc, 358 g of versatic acid vinyl ester (VEOVA®10), 120 g of BuA, and 29 g of VTES was added with a constant dosage rate over 110 min and the reactor was pressurized with 383 g of ethylene at a maximum pressure of 50 bar. With the start of the monomer addition and pressurization, the rate of addition for the oxidizer solution was reduced to a rate achieving a 20 min overrun of oxidizer solution over the monomer slow add.
[0135] After the additions, the temperature was kept at 85 °C for an additional 15 min and was then cooled to 40°C before release from the reactor.
[0136] The properties of the resulting polymer dispersion are summarized in Table 1.
[0137] Inventive Example 2. An aqueous solution consisting of the following ingredients was introduced into a 10 liter pressure reactor equipped with a stirrer, jacket heating and metering pumps: 3443 g of deionized water, 137 g of a 70% active aqueous solution of undecyl ethoxylate with 28 ethylene oxide units, 319 g of a 15% active aqueous solution of sodium lauryl sulfate, 96 g of a 25% active aqueous solution of sodium vinyl sulfonate, 12 g of sodium acetate (anhydrous), 1.9 g sodium meta bisulfite, and 1.1 g of a 1% active solution of ferrous sulfate heptahydrate. The atmosphere inside the reactor was flooded with nitrogen. A first monomer composition consisting of 897 g of versatic acid vinyl ester (VEOVA®10) and 299 g of BuA was added into the reactor as a pre-charge. The reaction mix was heated to 80°C, and the reactor was pressurized with ethylene to 5 bar.
[0138] To start the reaction an oxidizer solution comprising 383 g deionized water and 14.3 g of sodium peroxodisulfate was added with a rate of 255 g / h. After initiation was observed through a temperature increase, the reactor temperature set-point was raised to 85°C. When theexotherm had disappeared at 85°C (indicating consumption of the pre-charged monomers), a second monomer composition prepared of 2072 g of VAc, 299 g of versatic acid vinyl ester (VEOVA®10), 100 g of BuA, and 29 g of VTES was added with a constant dosage rate over 80 min and the reactor was pressurized with 319 g of ethylene at a maximum pressure of 50 bar. With the start of the monomer addition and pressurization, the rate of addition for the oxidizer solution was reduced to a rate reaching 70% of added oxidizer solution 5 min before end of the monomer addition.
[0139] 5 min before the addition of the second monomer composition ends, the addition of oxidizer solution was stopped and a third monomer composition consisting of 558 g of MMA and 239 g of EHA was added over 50 min.
[0140] When all of the third monomer composition was in the remaining 30% of the oxidizer solution was added within 20 min.
[0141] After the additions, the temperature was kept at 85 °C for an additional 15 min and was then cooled to 40°C before release from the reactor.
[0142] The properties of the resulting polymer dispersion are summarized in Table 1.
[0143] Inventive Example 3. An aqueous solution consisting of the following ingredients was introduced into a 10 liter pressure reactor equipped with a stirrer, jacket heating and metering pumps: 3411 g of deionized water, 203 g of a 70% active aqueous solution of undecyl ethoxylate with 28 ethylene oxide units, 316 g of a 15% active aqueous solution of sodium lauryl sulfate, 95 g of a 25% active aqueous solution of sodium vinyl sulfonate, 12 g of sodium acetate (anhydrous), 1.9 g sodium meta bisulfite, and 1.1 g of a 1% active solution of ferrous sulfate heptahydrate. The atmosphere inside the reactor was flooded with nitrogen. A first monomer composition consisting of 568 g of versatic acid vinyl ester (VEOVA®10) and 190 g of BuA was added into the reactor as a pre-charge. The reaction mix was heated to 85°C, and the reactor was pressurized with ethylene to 5 bar.
[0144] To start the reaction an oxidizer solution comprising 379 g deionized water and 14.3 g of sodium peroxodisulfate was added with a rate of 255 g / h. After initiation was observed and the exotherm had disappeared (indicating consumption of the pre-charged monomers), a second monomer composition prepared of 2797 g of VAc and 29 g of VTES was added with a constant dosage rate over 80 min and the reactor was pressurized with 392 g of ethylene at a maximum pressure of 50 bar. With the start of the monomer addition and pressurization, the rateof addition for the oxidizer solution was reduced to a rate reaching 70% of added oxidizer solution 5 min before end of the monomer addition.
[0145] 5 min before the addition of the second monomer composition ends, the addition of oxidizer solution was stopped and a third monomer composition consisting of 553 g of MMA and 237 g of EHA was added over 50 min.
[0146] When all of the third monomer composition was in the remaining 30% of the oxidizer solution was added within 20 min.
[0147] After the additions, the temperature was kept at 85 °C for an additional 15 min and was then cooled to 40°C before release from the reactor.
[0148] The properties of the resulting polymer dispersion are summarized in Table 1.
[0149] Inventive Example 4. An aqueous solution consisting of the following ingredients was introduced into a 10 liter pressure reactor equipped with a stirrer jacket heating and metering pumps: 3475 g of deionized water, 138 g of a 70% active aqueous solution of undecyl ethoxylate with 28 ethylene oxide units, 321 g of a 15% active aqueous solution of sodium lauryl sulfate, 48 g of a hydroxyethyl cellulose (HEC) with a Brookfield viscosity of 100-180 mPa s (25°C, 5% solution), 96 g of a 25% active aqueous solution of sodium vinyl sulfonate, 12 g of sodium acetate (anhydrous), 1.9 g sodium meta bisulfite and 1.1 g of a 1% active solution of ferrous sulfate heptahydrate. The atmosphere inside the reactor was flooded with nitrogen. A first monomer composition consisting of 483 g of versatic acid vinyl ester (VEOVA®10) and 483 g of BuA was added into the reactor as a pre-charge. The reaction mix was heated to 80°C, and the reactor was pressurized with ethylene to 5 bar.
[0150] To start the reaction an oxidizer solution comprising 386 g deionized water and 14.5 g of sodium peroxodisulfate was added with a rate of 240 g / h. After initiation was observed through a temperature increase, the reactor temperature set-point was raised to 85°C. When the exotherm had disappeared at 85°C (indicating consumption of the pre-charged monomers), a second monomer composition prepared of 3378 g of VAc and 29 g of VTES was added with a constant dosage rate over 110 min and the reactor was pressurized with 483 g of ethylene at a maximum pressure of 50 bar. With the start of the monomer addition and pressurization, the rate of addition for the oxidizer solution was reduced to a rate achieving a 20 min overrun of oxidizer solution over the monomer slow add.
[0151] After the additions, the temperature was kept at 85 °C for an additional 15 min andwas then cooled to 40°C before release from the reactor.
[0152] The properties of the resulting polymer dispersion are summarized in Table 1.
[0153] Inventive Example 5. An aqueous solution consisting of the following ingredients was introduced into a 10 liter pressure reactor equipped with a stirrer, jacket heating and metering pumps: 3411 g of deionized water, 203 g of a 70% active aqueous solution of undecyl ethoxylate with 28 ethylene oxide units, 316 g of a 15% active aqueous solution of sodium lauryl sulfate, 95 g of a 25% active aqueous solution of sodium vinyl sulfonate, 12 g of sodium acetate (anhydrous), 1.9 g sodium meta bisulfite, and 1.1 g of a 1% active solution of ferrous sulfate heptahydrate. The atmosphere inside the reactor was flooded with nitrogen. A first monomer composition consisting of 395 g of versatic acid vinyl ester (VEOVA®10) and 395 g of BuA was added into the reactor as a pre-charge. The reaction mix was heated to 85°C, and the reactor was pressurized with ethylene to 5 bar.
[0154] To start the reaction an oxidizer solution comprising 379 g deionized water and 14.3 g of sodium peroxodisulfate was added with a rate of 255 g / h. After initiation was observed and the exotherm had disappeared (indicating consumption of the pre-charged monomers), a second monomer composition prepared of 2763 g of VAc and 29 g of VTES was added with a constant dosage rate over 80 min and the reactor was pressurized with 395 g of ethylene at a maximum pressure of 50 bar. With the start of the monomer addition and pressurization, the rate of addition for the oxidizer solution was reduced to a rate reaching 70% of added oxidizer solution 5 min before end of the monomer addition.
[0155] 5 min before the addition of the second monomer composition ends, the addition of oxidizer solution was stopped and a third monomer composition consisting of 553 g of MMA and 237 g of EHA was added over 50 min.
[0156] When all of the third monomer composition was in the remaining 30% of the oxidizer solution was added within 20 min.
[0157] After the additions, the temperature was kept at 85°C for an additional 15 min and was then cooled to 40°C before release from the reactor.
[0158] The properties of the resulting polymer dispersion are summarized in Table 1.Table 1: Properties of the polymer dispersionsSolid content Brookfield MFFT pH dw(nm)3(%)■ viscosity (mPa s)2(°C)4Comp. Ex. 1 54.1 1280 5.1 280 0 Comp. Ex. 2 53.5 1160 5.0 117 0 Comp. Ex. 3 52.7 1330 4.9 134 0 Ex. 1 52.7 1160 5.0 143 0 Ex. 2 51.6 1050 4.9 144 0 Ex. 3 53.3 820 5.1 131 0 Ex. 4 53.1 2550 5.0 153 0 Ex. 5 53.2 200 5.0 144 01gravimetric determination after 24 h drying at 110°C2measurement conditions: 20°C, 20 rpm, spindle 33weight-average particle diameter as determined by a Beckman Coulter LS 13320 Particle Size Analyzer4The minimum film forming temperature (MFFT) is defined as the lowest temperature at which a polymer dispersion coalesces when laid on a substrate as a thin film, thereby forming clear transparent film.
[0159] Examples 6-13 (Inventive and comparative plasters). Plasters were prepared by mixing the ingredients in Table 5 at room temperature under stirring. After dissolving and dispersing item nos. 2-5 in water, and consecutive additions of item nos. 6-9, pigment and fine fillers as per item nos. 10-12 were dispersed consecutively at a dissolver speed of about 2000 rpm. The coarse fillers as per item nos. 13-16 were then added at a dissolver speed of about 500 rpm. The solid contents of all polymer dispersions were adjusted to 50% before their addition. The resulting plasters had a solid content of approx. 84%.Table 2: Composition of the plastersParts by Pos. Supplier Descriptionweight1 Water 80TYLOSE® MH 60002 SE Tylose Thickener 0.7 YG83 MOWIPLUS® SA 300 Celanese Dispersing agent 3 4 ADDITOL® XW 330 Allnex Dispersing agent 3 5 AGITAN®218 Miinzing Defoamer 3 6 Dispersion per Comp. Ex. 1-3 or Ex. 1-5 148 7 Sodium hydroxide, 10% Base 1.3 8 White spirit Coalescent agent 3 9 Butyldiglycol acetate Coalescent agent 3 10 KRONOS® 2160 Kronos Titanium dioxide 40 Schwarzwalder11 Polyethylene FPE 930 T HDPE fibers 3 Textil-Werke12 MicaCelia 250 L Ziegler Kaolin 30 13 OMYACARB® 40 GU Omya Calcium carbonate 130 14 OMYACARB® 130 GU Omya Calcium carbonate 150 15 CAROLITH® 0.1-0.5 Omya Calcium carbonate 120 16 CAROLITH®!.5-2.0 Omya Calcium carbonate 300
[0160] The capillary water absorption coefficient (w value) is a fundamental value in construction physics. The lower the w value, the higher the resistance of a coating against the ingress of liquid water. The w values of the coatings were determined according to DIN EN 1062-3. Aerated concrete specimens (class P4-500 according to DIN EN 771-4, circular cylinder, disc area=0.0298 m2) were pre-coated with a primer on one side and dried for 24 h. Plasters containing emulsion polymers from Comparative Examples 1-3 and Inventive Examples 1-5 were applied once. The lateral surfaces of the specimens were then sealed with liquefied paraffin (m.p.=58-60°C, AppliChem). The coated specimens were dried for 7 days at 23°C and 50% relative humidity. Each specimen was weighed before its coated surface was immersed in DI water for 24 h (1stconditioning). After removing excess water, the gravimetric water uptake was determined by weighing the specimen after 30 min, 1 h, 3 h, 6 h, and 24 h. The specimens were then dried for 24 h at 45°C in an oven with recirculating air. The described process of water immersion and drying was repeated twice (2ndand 3rdconditioning). After the 3rdconditioning,the specimens were stored at 23 °C and 50% relative humidity for at least 24 h (until achieving constant weight). The water absorption coefficient was determined by a fourth immersion of the coated surface in water for 24 h and weighing of the specimen after defined immersion times, as described above. The water permeability (in kg m-2) at a given immersion time was calculated as the mass difference between the wet and dry specimen divided by the surface area of the coating. The W24-value was then calculated by dividing the water permeability after 24 h by the square root of the immersion time.
[0161] Reported in Table 3 are the actual W24 values, as obtained after conditioning the specimens three times. Also reported are the liquid water transmission rates, as obtained during the initial immersion in water (1st conditioning). The W24 value obtained during the 1stconditioning is a measure of the water permeability of pristine coatings, while the actual W24 value after three conditionings is a measure of the water permeability of aged coatings.
[0162] As can be inferred from the reported data, W24 values of both pristine and aged plasters based on inventive dispersions are significantly lower than those values of the corresponding comparative examples.
[0163] Another fundamental value in building physics is the water vapor diffusion equivalent air layer thickness (sa), which defines the thickness of an air layer providing the same resistance to water vapor diffusion as the coating. The lower the sa value, the higher is the permittivity of a coating towards water vapor, which is a desired feature. The Sd values of the coatings were determined according to EN ISO 7783:2011. After determination of the W24 value, the specimens were dried until achieving constant weight and then stored at 23 °C and 50% relative humidity for at least 24 h. They were then mounted onto glass dishes comprising a saturated aqueous ammonium dihydrogenphosphate solution, approx. 4 cm above the liquid. The interface between concrete specimens and glass dish was sealed with liquefied paraffin to prevent any water vapor exiting the test system other than through the coating. The test systems are stored for 7 days at 23 °C and 50% relative humidity and then weighed every 24 hours, until a constant weight difference is achieved. This weight difference is proportional to the water vapor diffusion flow and used to calculate sa according to the norm.
[0164] The sa value of the coating, as reported in Table 3, is obtained by subtracting the Sd value of a primed uncoated aerated concrete specimen from the Sd value of the coated concrete specimen. As can be inferred from the reported data, the Sd values of plasters based on inventivedispersions are on similar levels or slightly lower than those of the comparative examples.Coatings comprising the inventive dispersions hence demonstrate significantly improved resistance against capillary water uptake while exhibiting similar or even slightly improved water vapor permittivity.Table 3: Water absorption coefficients and sa values of the plastersPlaster Dispersion W24, 1stconditioning W24 sa (m) (kg m'2h'°5) (kg nr2h'°5)C6 Comp. Ex. 1 0.23 0.13 0.70 C7 Comp. Ex. 2 0.22 0.09 0.69 C8 Comp. Ex. 3 0.26 0.10 0.64 9 Ex. 1 0.20 0.05 0.63 10 Ex. 2 0.18 0.05 0.58 11 Ex. 3 0.16 0.06 0.60 12 Ex. 4 0.18 0.04 0.61 13 Ex. 5 0.15 0.04 0.67
[0165] While the invention has been described in detail, modifications within the spirit and scope of the invention will be readily apparent to those of skill in the art. It should be understood that aspects of the invention and portions of various embodiments and various features recited herein and / or in the appended claims may be combined or interchanged either in whole or in part. In the foregoing descriptions of the various embodiments, those embodiments which refer to another embodiment may be appropriately combined with other embodiments as will be appreciated by one of ordinary skill in the art. Furthermore, those of ordinary skill in the art will appreciate that the foregoing description is by way of example only, and is not intended to limit the invention.
Claims
CLAIMSWe claim:
1. An emulsion polymerization process for producing a polymer product comprising:(i) polymerizing, in a first stage, a first monomer composition comprising from 15 wt% to 100 wt% of at least one vinyl ester of a C6-C20 carboxylic acid and from 0 wt% to 85 wt% of at least one alkyl ester of (meth)acrylic acid, each based on the total weight of monomers in the first monomer composition, to produce a first stage polymer;(ii) polymerizing, in a second stage and in the presence of the first stage polymer, a second monomer composition comprising from 50 wt% to 95 wt% of vinyl acetate, from 5 wt% to 40 wt% of ethylene, and from 0 wt% to 25 wt% of at least one vinyl ester other than vinyl acetate, each based on the total weight of monomers in the second monomer composition, to produce a second stage polymer; andoptionally (iii) polymerizing, in a third stage and in the presence of the first stage polymer and the second stage polymer, a third monomer composition comprising from 30 wt% to 100 wt% of at least one alkyl ester of (meth)acrylic acid and from 0 wt% to 20 wt% of at least one vinyl ester of a carboxylic acid, each based on the total weight of monomers in the third monomer composition, to produce a third stage polymer,wherein the first stage polymer is from 5 wt% to 40 wt%, the second stage polymer is 30 wt% or greater, and the third stage polymer is from 0 wt% to 30 wt%, each based on a total weight of the polymer product.
2. The process of claim 1, wherein the first monomer composition comprising from 20 wt% to 90 wt%, preferably from 40 wt% to 80 wt%, or more preferably from 50 wt% to 80 wt% of at least one vinyl ester of a C6-C20 carboxylic acid and from 10 wt% to 80 wt%, preferably from 20 wt% to 60 wt%, or more preferably from 25 wt% to 60 wt% of at least one alkyl ester of (meth)acrylic acid, each based on the total weight of monomers in the first monomer composition3. The process of any preceding claim, wherein the second monomer composition comprising from 60 wt% to 95 wt%, preferably from 65 wt% to 90 wt%, or more preferably from 70 wt% topreferably from 10 wt% to 15 wt% of ethylene, and from 0.1 wt% to 25 wt%, preferably from 5 wt% to 20 wt%, or more preferably from 5 wt% to 15 wt% of at least one vinyl ester other than vinyl acetate, each based on the total weight of monomers in the second monomer composition.
4. The process of any preceding claim, wherein the third stage is performed.
5. The process of claim 4, wherein the third monomer composition comprises from 50 wt% to 100 wt%, or preferably from 75 wt% to 100 wt% of at least one alkyl ester, preferably at least two alkyl esters, of (meth)acrylic acid.
6. The process of any preceding claim, wherein the first monomer composition further comprises from 0.1 wt% to 15 wt% of at least one functional monomer, wherein the second monomer composition further comprises from 0.1 wt% to 10 wt% of at least one functional monomer, and / or wherein the third monomer composition further comprises from 0.1 wt% to 10 wt% of at least one functional monomer.
7. The process of claim 6, wherein the at least one functional monomer comprises a carboxylic acid-functional monomer, a sulfonic acid-functional monomer, an epoxy-functional monomer, and a silane-functional monomer, or any combination thereof.
8. The process of any preceding claim, wherein the first stage polymer has a lower glass transition temperature, Tg, than the second stage polymer.
9. The process of any preceding claim, wherein the second stage polymer has a lower glass transition temperature, Tg, than the third stage polymer.
10. The process of any preceding claim, wherein the glass transition temperature Tgof the first stage polymer is at least 5 °C, preferably at least 10°C, lower than the second stage polymer.
11. The process of any preceding claim, wherein the glass transition temperature Tgof the second stage polymer is at least 5°C, preferably at least 10°C, lower than the third stage polymer.
12. The process of any preceding claim, wherein the first stage polymer has a Tgless than 30°C, preferably from -35°C to 20°C, or more preferably from -30°C to 0°C.
13. The process of any preceding claim, wherein the second stage polymer has a Tgless than 30°C, preferably from -15°C to 25°C, or more preferably from -5°C to 20°C.
14. The process of any preceding claim, wherein the third stage polymer has a Tgof 5°C to 120°C, preferably from 15°C to 100°C, or more preferably from 25°C to 80°C.
15. A polymer dispersion produced by the process of any one of claims 1-14.
16. The polymer dispersion of claim 15 and having a minimum film forming temperature of less than 20°C, preferably less than 10°C, or more preferably less than 5°C.
17. The polymer dispersion of any one of claims 15-16, wherein the particles of the polymer dispersion have a weight-averaged diameter of less than 400 nm, preferably less than 300 nm, as measured by laser diffraction and polarization intensity differential scattering (PIDS) using a Beckman Coulter LS 13320 Particle Size Analyzer.
18. A coating composition comprising the polymer dispersion of any one of claims 15-17, at least one pigment and / or at least one filler.
19. The coating composition of claim 18, wherein the coating is a facade paint or a plaster.
20. A thermal insulation system comprising the facade paint or plaster of claim 19.
21. The coating composition of claim 18, wherein the coating is a wood protection paint or an interior wall paint.