Organic peroxide formulations for polymer crosslinking
The novel organic peroxide formulation with di(t-butylperoxy)diisopropylbenzene, crosslinking coagents, and free radical traps addresses inconsistencies and by-product issues in polymer curing, ensuring consistent and improved properties in thick-walled polymer articles.
Patent Information
- Application Number
- PCT/US2026/026835
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2026-05-06
- Publication Date
- 2026-11-12
AI Technical Summary
Existing organic peroxides used for crosslinking polymers, such as DYBP, suffer from issues like inconsistent curing, generation of harmful by-products, skin irritation, and yellowing, especially in thick-walled polymer articles, which are critical for large-scale applications like chemical tanks and IBCs.
A novel organic peroxide formulation comprising di(t-butylperoxy)diisopropylbenzene, crosslinking coagents like triallyl cyanurate and alpha methyl styrene dimer, and free radical traps like quinone-containing compounds, which form a homogeneous liquid composition at elevated temperatures, providing consistent curing and preventing by-product formation.
The formulation offers longer scorch times, consistent crosslinking, reduces yellowing, and eliminates harmful by-products, ensuring better mechanical and thermal properties in crosslinked polymers, particularly in thick-walled applications.
Smart Images

Figure US2026026835_12112026_PF_FP_ABST
Abstract
Description
ORGANIC PEROXIDE FORMULATIONS FOR POLYMER CROSSLINKING
[0001] TECHNICAL FIELD
[0002] The present invention relates to novel peroxide formulations that are suitable for crosslinking polymers, preferably polyethylene, and more preferably HDPE, while simultaneously removing trapped air bubbles from the cured polymer. Polymer articles cured using the novel organic peroxide formulations described herein have good mechanical, chemical and thermal properties.
[0003] BACKGROUND
[0004] Reference to or discussion of any document or item of information in this specification is not an admission that the document or item of information, or any combination thereof was at the priority date, publicly available, known to the public, part of common general knowledge, or otherwise constitutes prior art under the applicable statutory provisions.
[0005] Organic peroxides are known initiators for curing and crosslinking polymers. Organic peroxides used in polymer crosslinking generate free radicals when heated, and while not wishing to be held to any specific theory, it is believed that the generated free radicals have sufficient energy to crosslink saturated polyethylene polymers by abstracting hydrogen atoms off the polymer chain. Generally, it is quite difficult to significantly slow the decomposition of organic peroxides (in an effort to control the polymer cross-linking process) during the free radical generation process.
[0006] In the process of rotational molding of crosslinked polymers, such as HDPE, 20 mesh to 35 mesh polymer powder containing organic peroxide and other additive are added to a hollow metal mold, which is then heated to melt and crosslink the polymer. When the polymer particles melt, a layer of molten polymer forms inside the mold containing trapped air bubbles. These air bubbles need to escape from the polymer melt before significant crosslinking occurs to avoid being permanently trapped in the crosslinked polymer. Organic peroxides with shorter half-life times versus temperature will generate more free-radicals at a fixed temperature compared to another peroxide which has a longer half-life time versus temperature. Peroxide half-life time at a fixed temperature is the time it takes for half of the peroxide concentration to decompose. If the half-life time of the selected organic peroxide at the polymer melting temperature is too short, there may not be enough time for the air bubbles to escape if the molten polymer layer is thick. The thicker the molten layer, the more time is needed for the air bubbles to escape. As a result, when faster decomposing (shorter half-life time) organic peroxides are used to crosslink polyethylene there is a greater chance for air bubbles to become trapped in the cured polymer.
[0007] Trapped air bubbles or air pockets in crosslinked polymer articles, for example cured polyethylene articles, is undesirable because the trapped air can have a deleterious effect on the mechanical, chemical and thermal properties of the cured article. This is especially significant for large scale chemical, agricultural and fuel storage tanks that can have a volume capacity in excess of 500 gallons, including volume capacities in excess of 1,000 gallons or even in excess of 16,000 gallons. This also includes the rotomolding of crosslinked HDPE Intermediate Bulk Containers (IBCs). IBCs (interchangeably referred to herein as “tanks”) are used in various industries to handle and transport bulk materials such as chemicals, pharmaceuticals, petroleum, food and beverage, and the like. Such IBCs or tanks are rotomolded from crosslinked HDPE. Trapped air bubbles is generally not an issue with thin wall tanks, e.g., tanks that have a wall thickness of < 0.50 inch. However, medium- to large-size tanks, e.g., tanks that have a volume > 1,000 gallons, and in some cases even > 10,000 gallons, have thicker walls to adequately support and contain larger bulk volumes. Wall thicknesses of such high volume IBCs often exceed 0.5 inch, including IBCs having wall thicknesses in excess of 2 inches. Thicker walled tanks require more HDPE powder to be added to the mold, and thus more trapped air bubbles form between the HDPE particles during the melting process. Additionally, in such thick layers (thick walls) of molten HDPE, air bubbles have a longer distance to travel to escape to the surface. This requires more time for the polymer to remain in a suitable fluid and molten state to enable adequate removal / escape of the trapped air bubbles.
[0008] A longer polymer melt time or scorch time provides more time for trapped air bubbles in the polymer melt to migrate through the melt and escape from the surface before significant crosslinking begins. The speed at which a particular organic peroxide decomposes at a given temperature depends upon its thermal stability, which in turn, is affected by the chemical structure of the organic peroxide. To complicate this process, gaseous decomposition by-products aregenerated upon decomposition of the peroxide, and the amounts and types of such gaseous byproducts depend on the selected organic peroxide.
[0009] Various organic peroxide-containing systems for polymer curing are described in the following references.
[0010] US Patent No. 4,555,379 describes a rotomolding composition that includes an acetylenic diperoxy compound, such as DYBP, in combination with triallyl cyanurate (TAC) or triallyl isocyanurate (TAIC) as a monomeric coagent for crosslinking ethylene homopolymer.
[0011] US 5,298,564 describes the use of 2, 4-diphenyl-4-m ethyl- 1 -pentene (alpha methyl styrene dimer, NOFMER® MSD, NOF Corporation, Japan) and at least one dialkyl organic peroxide including dicumyl peroxide, t-butyl cumyl peroxide, 2,5-di(t-butylperoxy)-2,5-dimethylhexane, 2,5-di(t-butylperoxy)-2,5-dimethylhexyne-3, di-t-butylperoxide and di(t-butylperoxy)diisopropyl benzene to simultaneously increase crosslinking and scorch time during polyethylene crosslinking.
[0012] US Patent No. 11, 118,028 describes a liquid or meltable solid organic peroxide formulation for curing solid elastomer compositions in the presence of oxygen, and lists alpha methyl styrene dimer (NOFMER® MSD, NOF Corporation, Japan) as one of many preferred coagents.
[0013] US Patent No. 11,203,672 describes organic peroxide formulations that include at least one ethylenically unsaturated organic peroxide and are liquid or near liquid, and also describes the use of NOFMER® MSD (NOF Corporation, Japan) as one of many possible suitable additives.
[0014] Traditionally, the organic peroxide used in the process of crosslinking HDPE for manufacturing large tanks, e.g., IBCs, is 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3 (DYBP). DYBP is effective for crosslinking HDPE because it has a high decomposition temperature owing to the presence of the acetylenic triple bond in its structure:At 140°C (the melting point of polyethylene), DYBP has a half-life of 3.62 hours, which provides the required melting time(scorch time) during the rotomolding process to allow trapped air bubbles to escape from the surface of the cured polymer.
[0016] However, despite its suitability as a polyethylene crosslinking agent and its prevalent use in the manufacture of thick-walled crosslinked tanks or IBCs, the organic peroxide DYBP has certain significant drawbacks associated with its use. The acetylenic triple bond of DYBP, which provides the high decomposition temperature, also results in the formation of very undesirable oily and gaseous decomposition by-products which are primary skin and inhalation irritants. Exposure to these oily and gaseous decomposition by-products during de-molding of the hot crosslinked article or direct skin contact with the final crosslinked article causes skin irritation. The byproducts of DYBP decomposition also impart a yellow color to the crosslinked article.
[0017] Additionally, while DYBP is suitable for rotational molding of crosslinked HDPE to produce large thick wall tanks due to its high thermal stability enabling long HDPE melt times (long scorch times), it is subject to inconsistent cure issues. DYBP is a volatile, liquid organic peroxide that is incompatible with HDPE. HDPE rotomolding powder containing DYBP often provides inconsistent levels of crosslinking as some of the DYBP will migrate out of the HDPE powder towards the surface of the HDPE particles and evaporate or pool around the outside of the container used to store the rotomolding powder prior to use. Such inconsistent crosslinking of polyethylene when using DYBP is a serious issue when manufacturing crosslinked EIDPE tanks for commercial and industrial use. Lastly, technically pure DYBP peroxide (-95% assay) is classified as a dangerous, type B subsidiary explosive peroxide. Thus, the maximum Llnited States Department of Transportation allowable commercial package size for the -95% assay liquid DYBP is 35 pounds, stored in a 20 liter container.
[0018] None of the references discussed above address these drawbacks associated with the use of DYBP for polyethylene or EIDPE polymer crosslinking. Thus, there is a real and urgent industrial need for a stable organic peroxide composition for HDPE polymer crosslinking that provides sufficient melt time for trapped air bubbles or pockets to escape from the polymer, is more compatible with the HDPE to provide consistent and reliable cure, prevents yellowing, and eliminates generation of undesirable primary skin and air irritant decomposition by-products.
[0019] The present invention aims to address these industrial needs using a homogeneous blend of (i) di(t-butylperoxy)diisopropylbenzene; (ii) at least one crosslinking coagent selected from thegroup consisting of triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, triallyl trimesate, pentaerythritol triallyl ether, and alpha methyl styrene dimer composition (a blend of 2,4-diphenyl-4-methyl-l -pentene and 2,4-diphenyl-4-methyl-2-pentene), preferably alpha methyl styrene dimer and at least one crosslinking coagent selected from the group consisting of triallyl organic coagents including: triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, triallyl trimesate; and (iii) least one free radical trap selected from the group consisting of a quinone-containing compound, and a nitroxide-containing compound.
[0020] SUMMARY
[0021] The organic peroxide containing composition of this invention addresses the above¬ described drawbacks associated with the use of DYBP in polymer curing.
[0022] An exemplary aspect is a novel organic peroxide formulation comprising di(t-butylperoxy)diisopropylbenzene; at least one crosslinking coagent selected from the group consisting of triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, triallyl trimesate, pentaerythrithol triallyl ether, and alpha methyl styrene dimer; and at least one free radical trap selected from the group consisting of a quinone-containing compound and a nitroxide-containing compound, wherein the organic peroxide formulation is a meltable solid that results in a homogenous liquid composition at temperatures between about 45°C and about 65°C.
[0023] Another exemplary aspect is a method of preparing an organic peroxide composition, the method comprising: mixing (i) di(t-butylperoxy)diisopropylbenzene; (ii) at least one crosslinking coagent selected from the group consisting of triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, triallyl trimesate, pentaerythritol triallyl ether, and alpha methyl styrene; and (iii) at least one free radical trap selected from the group consisting of a quinone-containing compound and a nitroxide-containing compound to prepare the organic peroxide formulation.
[0024] Still another exemplary aspect is a method of cross-linking a polymer, the method comprising: mixing a molten organic peroxide composition and a polymer; and curing using a time-temperature profile such that at least 95 wt%, preferably at least 99 wt%, more preferably 100 wt%, or more of the organic peroxide of the organic peroxide formulation is decomposed during the process; wherein the molten organic peroxide composition comprises (i) di(t-butylperoxy)diisopropylbenzene; (ii) at least one crosslinking coagent selected from the groupconsisting of triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, pentaerythrithol triallyl ether, triallyl trimesate, and alpha methyl styrene dimer; and (iii) at least one free radical trap selected from the group consisting of a quinone-containing compound and a nitroxide-containing compound to prepare the organic peroxide formulation.
[0025] Still another exemplary aspect is a system for cross-linking a polymer comprising an organic peroxide formulation comprising di(t-butylperoxy)diisopropylbenzene; at least one crosslinking coagent selected from the group consisting of triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, triallyl trimesate, pentaerythrithol triallyl ether, and alpha methyl styrene dimer; and at least one free radical trap selected from the group consisting of a quinone-containing compound and a nitroxide-containing compound, wherein the organic peroxide formulation is a meltable solid that results in a homogenous liquid composition at temperatures between about 45°C and about 65°C.
[0026] BRIEF DESCRIPTION OF DRAWINGS
[0027] Drawings are provided herewith for better understanding of the invention, and illustrate the principles and features of the invention. The Drawings are not necessarily to scale and are not meant to limit the invention. In the Drawings, like numerals are used to indicate like parts throughout the various views.
[0028] FIGURE 1 is a rheograph of the elastic modulus in dN-m at 162°C, 1° arc, 100 cpm of HDPE crosslinked using the organic peroxide formulations of Comp. Ex. 1, Comp. Ex. 2 and Comp. Ex. 3.
[0029] FIGURE 2 is a rheograph of the elastic modulus in dN-m at 162°C, 1° arc, 100 cpm of HDPE crosslinked using the organic peroxide formulations of Comp. Ex. 1, Comp. Ex. 2 and Example 5.
[0030] FIGURE 3 is a variable temperature rheograph in degrees Celsius, plotting the Elastic Modulus in dN-m for each peroxide formulations of Comparative Examples 1 and 2 and Example 6 using an RPA® rheometer with a 1° arc of strain and 100 cpm frequency for crosslinking HDPE. The rheometer test parameters used a 141°C to 225°C temperature span, and FIGURE 3 includes a plot of the results between 145 °C to 225 °C of this range.
[0031] FIGURE 4 is a variable temperature rheograph where the Elastic Modulus S’ in dN-m is plotted against the Loss Modulus S” for each peroxide formulation of Example 6, Comp. Ex. 1 and Comp. Ex. 3 to determine the S’-S” crossover temperature (where S’ = S”, which is the gel temperature for the HDPE melt. The same rheometer test conditions were used as in FIGURE 3.
[0032] FIGURE 5 is a variable temperature rheograph where the Tangent Delta (which is defined as S” / S’) is plotted for each peroxide formulation of Example 6, Comp. Ex. 1 and Comp. Ex. 2. A Tangent Delta value equal to one (where S’ = S”), corresponds to the gel temperature in degrees Celsius. It is at that melt temperature where air bubbles may get trapped in the crosslinking HDPE melt. The same rheometer test conditions were used as in FIGURE 3.
[0033] FIGURE 6 is a variable temperature rheograph where the Tangent Delta is plotted for Comp. Ex 1, Comp. Ex 2, Example 6 and Example 7. The same rheometer test conditions were used as in FIGURE 3.
[0034] FIGURE 7 is a rheograph plotting the Elastic Modulus S’ (dN-m) versus time for the crosslinking of polyamide PA-11 using the novel organic peroxide formulation of Example 7. The RPA rheometer test conditions used were 195°C, 1 deg arc, 100 cpm frequency for four minutes.
[0035] FIGURE 8 is a variable temperature rheograph where the Tangent Delta is plotted for Comp. Ex 1 Comp. Ex 2 Example 6, Example 7 and Example 8. The same rheometer test conditions were used as in FIGURE 3.
[0036] DETAILED DESCRIPTION
[0037] Hereinafter various aspects of the present invention will be described in detail.
[0038] Any compositions described herein are intended to encompass compositions which consist of, consist essentially of, as well as comprise, the various constituents identified herein, unless explicitly indicated to the contrary.
[0039] As used herein, the singular forms “a”, “an” and “the” are intended to include the plural forms as well, unless the context clearly indicates otherwise. Additionally, the use of “or” is intended to include “and / or”, unless the context clearly indicates otherwise.
[0040] As used herein, the recitation of a numerical range for a variable is intended to convey that the variable can be equal to any value(s) within that range, any and all sub-ranges encompassedby the broader range, including any value(s) within that range as well as the upper and lower limits unless explicitly indicated to the contrary.
[0041] As used herein, "about" is a term of approximation that would be understood by one of skill in the art, and is intended to include minor variations such as, for example, standard deviations associated with techniques commonly used to measure the amounts of the constituent elements or components of an alloy or composite material, or other properties and characteristics. All of the values characterized by the above-described modifier "about," are also intended to include the exact numerical values disclosed herein. Moreover, all ranges include the upper and lower limits.
[0042] As used herein, the term “ambient temperature” refers to the average air temperature in a given environment that is measured with a thermometer, and ranges from 15°C to 30°C.
[0043] As used herein, the terms “liquid” and “in liquid form” mean that the corresponding material is in the form of a homogenous (no layers or solids) liquid (flowable or pourable) at the temperature recited, or in the absence of a specific recited temperature, at ambient temperature.
[0044] As used herein, the term “molten” means a material that has been liquified by the application of heat / heating to a high temperature.
[0045] As used herein, “phr” denotes parts by weight of a peroxide composition per one-hundred parts by weight of a polymer or elastomer.
[0046] As used herein, “ppm” denotes parts by weight of a peroxide composition per one-million parts by weight of a polymer or elastomer.
[0047] The terms “formulation” and “composition” are used interchangeably herein.
[0048] Peroxide names and physical properties for the organic peroxides described herein can be found in “Organic Peroxides” by Jose Sanchez and Terry N. Myers; Kirk-Othmer Encyclopedia of Chemical Technology, Fourth Ed., Volume 18, (1996), the disclosures of which are incorporated herein by reference.
[0049] Unless indicated otherwise, each individual feature, aspect or embodiment described herein is combinable with any other individual feature(s), aspect(s) or embodiment s) that is / are described herein, without limitation. Such combinations are specifically contemplated as being within thescope of the present invention, regardless of whether they are explicitly described as a combination herein.
[0050] Technical and scientific terms used herein have the meaning commonly understood by one of skill in the art to which the present description pertains, unless otherwise defined.
[0051] Trapped air in crosslinked polymer articles, such as HDPE articles, is undesirable because trapped air bubbles or air pockets can have a deleterious effect on the physical, chemical, mechanical and structural properties of the cured article. A longer polymer melting time or longer scorch time provides more time for trapped air bubbles in the polymer melt to migrate through the melt and escape to the surface before significant crosslinking begins. Thicker walled tanks require more HDPE powder to be added to the mold, and thus more trapped air bubbles and / or air pockets form between the HDPE particles during the melting process. The speed at which a particular organic peroxide decomposes at a given temperature depends upon its thermal stability, which in turn, is affected by the chemical structure of the organic peroxide.
[0052] DYBP is a common organic peroxide used in polymer crosslinking, especially in the rotational molding of crosslinked HDPE to produce thick-walled, large capacity tanks. The primary advantage of DYBP is that it is has a significantly high thermal stability (versus most organic peroxides) to enable longer HDPE melt time prior to curing the larger, thick-walled tanks and articles. However, DYBP has significant drawbacks associated with its use because DYBP generates a large amount of harmful decomposition by-products that are primary air and skin irritants, impart a yellow color to the cured product and have a noxious odor. DYBP is also incompatible with HDPE which results in loss / migration of this peroxide out of the rotomolding powder, causing inconsistent crosslinking performance. DYBP is also highly flammable and classified as an explosive material, which further limits its applicability. Thus, despite the suitability of DYBP for polymer curing because of its higher half-life, there is an urgent industrial need for alternate organic peroxide formulations that address these significant drawbacks associated with the use of DYBP.
[0053] This application is directed to novel organic peroxide formulations that unexpectedly provide a longer melting time (longer scorch time) when using a much more reactive, less thermally stable organic peroxide compared to DYBP, such as di(tert-butylperoxy)diisopropylbenzene. Longer scorch times were unexpectedly obtained with this lessthermally stable organic peroxide when used in combination with crosslinking coagents. The additives used in the practice of this invention when combined with di(tert-butylperoxy)diisopropylbenzene, unexpectedly, provides more time for the polymer particles to melt and stay molten for a longer time, to allow for air bubbles to escape the melt, while simultaneously providing a desired level of crosslinking based upon rheometer maximum torque.
[0054] Non-limiting examples of crosslinkable polymers suitable for rotational molding that can be cured using the novel organic peroxide formulations described herein include polyethylene such as linear low density polyethylenes (LLDPE), low-density polyethylenes (LDPE), medium-density polyethylenes (MDPE), high-density polyethylenes (HDPE), and ultrahigh molecular weight polyethylenes (UHMWPE), and polyamides such as PA-11 and PA-12. Preferred crosslinkable polymers for rotational molding include PA-11, PA-12, UHMWPE, MDPE, LDPE and HDPE. More preferred crosslinkable polymers for crosslinked rotational molding include MDPE, LDPE and HDPE. More preferred are MDPE and HDPE. Even more preferred is HDPE.
[0055] The novel organic peroxide formulations described herein for crosslinked polymer rotational molding application are meltable homogeneous peroxide compositions.
[0056] The preferred organic peroxide suitable for inclusion in the organic peroxide formulations described herein is di(tert-butylperoxy) diisopropylbenzene.
[0057] Organic peroxides to be excluded from the practice of this invention are dicumyl peroxide, t-butylcumyl peroxide, t-amylcumyl peroxide, isopropylcumyl-t-butyl peroxide, isopropenylcumyl-t-butyl peroxide, di(t-amylperoxy)diisopropyl benzene, di-t-amyl peroxide, di-t-butyl peroxide, peroxyketals, monoperoxycarbonates, hydroperoxides, ketone peroxides, and peroxy esters.
[0058] The organic peroxide composition preferably includes a blend of meta- and para-isomers of the di(tert-butylperoxy)- diisopropylbenzene wherein the meta-isomer to the para-isomer weight (wt%) ratio can be in the range of from 100:0 to 0:100, from about 60:40 to about 90:10, from about 60:40 to about 85:15, from about 60:40 to about 80:20, from about 60:40 to about 75:25, from about 60:40 to about 70:30, from about 65:35 to about 85:15, from about 65:35 to about 80:20, from about 65:35 to about 75:25, from about 65:35 to about 70:30, from about 70:30 to about 75:25, from about 70:30 to about 80:20, from about 70:30 to about 85:15, from about 70:30to about 90:10, from about 75:25 to about 80:20, from about 75:25 to about 85:15, from about 75:25 to about 90:10, from about 80:20 to about 90:10, from about 85:15 to about 90:10, from about 80:20 to about 85:15, about 60:40, about 61:39, about 61.6:38.4, about 62:38, about 63:37, about 64:36, about 65:35, about 66:34, about 67:33, about 68:32, about 69:31, about 70:30, about 71:29, about 72:28, about 73:27, about 74:26, about 75:25, about 76:24, about 77:23, about 78:22, about 79:21, about 80:20, about 81:19, about 82:18, about 83:17, about 84:16, about 85:15, about 86:14, about 87:13, about 88:12, about 89:11, about 90:10, and the like; preferably the ratio of the meta-isomer to the para-isomer (wt%) of the di(tert-butylperoxy)diisopropylbenzene ranges from about 60:40 to about 90: 10. The meta-isomer to the para-isomer weight (wt%) ratio can be equal to any ratio(s) within any of these ranges, including the end-points of these ranges.
[0059] In another embodiment, the novel homogeneous molten organic peroxide composition comprises only the meta-isomer of di(tert-butylperoxy)diisopropylbenzene.
[0060] In another embodiment, the novel homogeneous molten organic peroxide composition comprises only the para-isomer of di(tert-butylperoxy)diisopropylbenzene.
[0061] In another embodiment, the novel homogeneous molten organic peroxide composition comprises a 78:22 ratio of the meta isomer to the para-isomer of di(tert-butylperoxy)diisopropylbenzene.
[0062] Nonlimiting examples of crosslinking coagents include triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, triallyl trimesate, alpha methyl styrene dimer, pentaerythritol triallyl ether, and the like. The novel peroxide formulations can include a combination of two or more of the crosslinking coagents described herein. The most preferred crosslinking coagents are triallyl cyanurate and alpha methyl styrene dimer.
[0063] Nonlimiting examples of free radical traps included in the novel organic peroxide formulations described herein include quinone-containing compounds and nitroxide-containing compounds. Preferred free radical traps include mono-tert-butylhydroquinone (MTBHQ), hydroquinone mono-methyl ether (HQMME), mono-tert-amylhydroquinone (MTAHQ), di-tert-amylhydroquinone (DTAHQ), di-tert-butylhydroquinone (DTBHQ), 2, 2, 6, 6-tetramethylpiperidine-l-oxyl (TEMPO), 4-hydroxy-2,2,6,6-tetramethylpiperidine-l-oxyl (4-hydroxy TEMPO or 4-OHT), and the like. The novel peroxide formulations can include a combination of two or more of the free radical traps described herein.
[0064] Non-limiting industrial processes for the production of crosslinked polymeric articles using peroxide curing include: rotational molding (rotomolding), compression molding, injection molding, transfer molding, and crosslinking polymers using steam tubes or steam autoclave operations. A preferred process for preparing crosslinked polymer articles using the peroxide formulations of this invention is a rotomolding process.
[0065] Peroxide loadings for crosslinking can vary from about 1 phr to about 10 phr, or from about 2 phr to about 8 phr, or from about 3 phr to about 6 phr, and the like depending upon the process used. The peroxide loading can be equal to any amount(s) within any of these ranges, including the end-points of these ranges. However for a rotational molding process to produce a crosslinked article, the peroxide loading can be from about 1 phr to about 3 phr, from about 1 phr to about 2 phr, from about 1 phr to about 1.5 phr, preferably from about 1 phr to about 1.3 phr.
[0066] The novel peroxide formulations described herein include the organic peroxide in an amount from about 25 wt% to about 60 wt%, from about 30 wt% to about 55 wt%, from about 35 wt% to about 45 wt%, about 30 wt%, about 32 wt%, about 34 wt%, about 36 wt%, about 37 wt%, about 38 wt%, about 42 wt%, about 44 wt%, about 46 wt%, about 48 wt%, about 52 wt%, about 54 wt%, about 56 wt%, about 58 wt%, and the like, based on a total weight of the organic peroxide formulation. The amount of organic peroxide can be equal to any amount(s) within any of these ranges, including the end-points of these ranges.
[0067] The novel peroxide formulations described herein can include the at least one crosslinking coagent in an amount from about 45 wt% to about 74 wt%, from about 47 wt% to about 72 wt%, from about 50 wt% to about 70 wt%, from about 52 wt% to about 68 wt%, from about 55 wt% to about 65 wt%, about 46 wt%, about 48 wt%, about 54 wt%, about 60 wt%, and the like, based on a total weight of the organic peroxide formulation. The amount of the crosslinking coagent can be equal to any amount(s) within any of these ranges, including the end-points of these ranges.
[0068] The novel peroxide formulations described herein can include triallyl cyanurate in an amount from about 40 wt% to about 52 wt%, about 41 wt%, about 42 wt%, about 43 wt%, about 44 wt%, about 45 wt%, about 46 wt%, about 47 wt%, about 48 wt%, about 49 wt%, and the like,based on a total weight of the organic peroxide formulation. The amount of the triallyl cyanurate can be equal to any amount(s) within any of these ranges, including the end-points of these ranges.
[0069] The novel peroxide formulations described herein can include alpha methyl styrene dimer in an amount from about 6 wt% to about 16 wt%, from about 8 wt% to about 15 wt%, from about 8 wt% to about 14 wt%, about 8 wt%, about 8.5 wt%, about 9 wt%, about 9.5 wt%, about 10.0 wt%, about 10.5 wt%, about 11 wt%, about 11.5 wt%, about 12 wt%, about 12.5 wt%, about 13 wt%, about 13.5 wt%, about 14 wt%, about 14.5 wt%, about 15 wt%, about 15.5%, about 16%and the like, based on a total weight of the organic peroxide formulation. The alpha methyl styrene dimer concentration is preferably from about 7 wt% to about 15 wt%, preferably from about 7 wt% to about 14.5 wt%, more preferably from about 8 wt% to about 12.5 wt%. The amount of the alpha methyl styrene dimer can be equal to any amount(s) within any of these ranges, including the end-points of these ranges.
[0070] The novel peroxide formulations described herein can include the at least one free radical trap in an amount from about 1 wt% to about 30 wt%, from about 5 wt% to about 25 wt%, from about 7.5 wt% to about 20 wt%, from about 10 wt% to about 15 wt%, from about 2.5 wt% to about 6.5 wt%, from about 3 wt% to about 4 wt%, and the like, based on a total weight of the organic peroxide formulation. The amount of the free radical trap can be equal to any amount(s) within any of these ranges, including the end-points of these ranges.
[0071] The novel organic peroxide formulations described herein are low melting solid mixtures, i.e., meltable solid homogenous mixtures. The individual wt% of each component of the novel organic peroxide formulation described herein is such that the total of all components is 100 wt%.
[0072] Additionally, the HOPE crosslinked articles made using the novel organic peroxide formulations described herein exhibit better color and lower Yi (yellowness index) values versus HDPE crosslinked with DYBP. Lower yellowness index values indicate less yellow color. The near complete lack of yellow color generation by the novel peroxide formulations described herein provides a more white and desirable appearance for the natural colored HDPE grades and avoids undesirable yellow tinting of the colored crosslinked HDPE grades caused by the use of DYBP.
[0073] Non-limiting aspects of the invention are summarized as follows.
[0074] Aspect 1: An organic peroxide formulation comprising: di(t-butylperoxy)diisopropylbenzene; at least one crosslinking coagent selected from the group consisting of triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, triallyl trimesate, pentaerythrithol triallyl ether, and alpha methyl styrene dimer; and at least one free radical trap selected from the group consisting of a quinone-containing compound and a nitroxide-containing compound, wherein the organic peroxide formulation is a homogenous molten organic peroxide composition at elevated temperatures.
[0075] Aspect 2: The organic peroxide formulation of Aspect 1, wherein the at least one organic peroxide is a mixture of meta- and para-di(t-butylperoxy)diisopropylbenzene in a weight ratio range of from about 100:0 to about 0: 100
[0076] Aspect 3: The organic peroxide formulation of Aspect 1 or 2, wherein the at least one organic peroxide is a mixture of meta- and para-di(t-butylperoxy)diisopropylbenzene in a weight ratio range of from about 60:40 to about 90:10.
[0077] Aspect 4: The organic peroxide formulation of any one of Aspects 1-3, wherein the at least one organic peroxide is a mixture of meta- and para-di(t-butylperoxy)diisopropylbenzene in a weight ratio range of 78:22.
[0078] Aspect 5: The organic peroxide formulation of any one of Aspects 1-4, wherein the at least one crosslinking coagent is alpha methyl styrene dimer and at least one selected from triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, pentaerythrithol triallyl ether, or triallyl trimesate.
[0079] Aspect 6: The organic peroxide formulation of any one of Aspects 1-5, wherein the at least one free radical trap is selected from the group consisting of mono-tert-butylhydroquinone (MTBHQ); hydroquinone mono-methyl ether (HQMME); mono-tert-amylhydroquinone (MTAHQ); di-tert-amylhydroquinone (DTAHQ); di-tert-butylhydroquinone (DTBHQ); TEMPO 2,2,6,6-tetramethylpiperidine-l-oxyl (TEMPO), and 4-hydroxy-2,2,6,6-tetramethylpiperidine-l-oxyl (4-OHT).
[0080] Aspect 7: The organic peroxide formulation of any one of Aspects 1-6, wherein: an amount of the di(t-butylperoxy)diisopropylbenzene is from about 25% to about 60% based on a total weight of the organic peroxide formulation; an amount of the at least one crosslinking coagent isfrom about 45% to about 74% based on a total weight of the organic peroxide formulation; and an amount of the at least one free radical trap is from about 1% to about 30% based on a total weight of the organic peroxide formulation.
[0081] Aspect 8: The organic peroxide formulation of any one of Aspects 1-6, comprising: (i) di(t-butylperoxy)diisopropylbenzene; (ii) triallyl cyanurate and alpha methyl styrene dimer; and (iii) at least one free radical trap is selected from the group consisting of mono-tert-butylhydroquinone (MTBHQ); hydroquinone mono-methyl ether (HQMME); mono-tert-amylhydroquinone (MTAHQ); di-tert-amylhydroquinone (DTAHQ); di-tert-butylhydroquinone (DTBHQ); 4-hydroxy-2,2,6,6-tetramethylpiperidine-l-oxyl (4-OHT) and 2,2,6,6-tetramethylpiperidine-l-oxyl (TEMPO).
[0082] Aspect 9: The organic peroxide formulation of any one of Aspects 1-7, comprising: (i) di(t-butylperoxy)diisopropylbenzene; (ii) triallyl cyanurate and alpha methyl styrene dimer; and (iii) mono-tert-butylhydroquinone (MTBHQ).
[0083] Aspect 10: The organic peroxide formulation of any one of Aspects 1-7, comprising: (i) di(t-butylperoxy)diisopropylbenzene; (ii) triallyl cyanurate and alpha methyl styrene dimer; and (iii) hydroquinone mono-methyl ether (HQMME) and 4-hydroxy-2,2,6,6-tetramethylpiperidine-l-oxyl (4-OHT).
[0084] Aspect 11: The organic peroxide formulation of any one of Aspects 1-7, comprising: (i) di(t-butylperoxy)diisopropylbenzene; (ii) triallyl cyanurate and alpha methyl styrene dimer; and (iii) di-tert-amylhydroquinone (DTAHQ) and 4-hydroxy-2,2,6,6-tetramethylpiperidine-l-oxyl (4-OHT).
[0085] Aspect 12: A method of preparing an organic peroxide composition, the method comprising: mixing (i) di(t-butylperoxy)diisopropylbenzene; (ii) at least one crosslinking coagent selected from the group consisting of triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, triallyl trimesate, pentaerythrithol triallyl ether, and alpha methyl styrene dimer; and (iii) at least one free radical trap selected from the group consisting of a quinone-containing compound and a nitroxide-containing compound to prepare the organic peroxide formulation.
[0086] Aspect 13: The method of Aspect 12, wherein the at least one organic peroxide is a mixture of meta- and para-di(t-butylperoxy)diisopropylbenzene in a weight ratio range of from about 100:0 to about 0:100
[0087] Aspect 14: The method of Aspect 12 or 13, wherein the at least one organic peroxide is a mixture of meta- and para-di(t-butylperoxy)diisopropylbenzene in a weight ratio range of from about 60:40 to about 90: 10.
[0088] Aspect 15: The method of any one of Aspect 12 or 13, wherein the at least one organic peroxide is a mixture of meta- and para- di(t-butylperoxy)diisopropylbenzene in a weight ratio range of 78:22.
[0089] Aspect 16: The method of any one of Aspects 12-15, wherein the at least one crosslinking coagent is alpha methyl styrene dimer and at least one selected from triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, pentaerythrithol triallyl ether, or triallyl trimesate.
[0090] Aspect 17: The method of any one of Aspects 12-16, wherein the at least one free radical trap is selected from the group consisting of mono-tert-butylhydroquinone (MTBHQ); hydroquinone mono-methyl ether (HQMME); mono-tert-amylhydroquinone (MTAHQ); di-tert-amylhydroquinone (DTAHQ); di-tert-butylhydroquinone (DTBHQ); 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxyl (4-OHT); and 2,2,6,6-tetramethylpiperidine-1-oxyl (TEMPO).
[0091] Aspect 18: The method of any one of Aspects 12-17, wherein an amount of the di(t-butylperoxy)diisopropylbenzene is from about 25% to about 60%; an amount of the at least one crosslinking coagent is from about 45% to about 74%; and an amount of the at least one free radical trap is from about 1% to about 30%, based on a total weight of the organic peroxide formulation.
[0092] Aspect 19: A method of cross-linking a polymer, the method comprising: mixing a molten organic peroxide composition and a polymer; and curing using a time-temperature profde such that at least 95 wt% or more of the organic peroxide, preferably at least 99 wt%, more preferably 100 wt% of the organic peroxide, of the organic peroxide formulation is decomposed during the process; wherein the molten organic peroxide composition comprises: (i) di(t-butylperoxy)diisopropylbenzene; (ii) at least one crosslinking coagent selected from the group consisting of triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, pentaerythrithol triallyl ether, triallyl trimesate and alpha methyl styrene dimer; and (iii) at least one free radical trapselected from the group consisting of a quinone-containing compound and a nitroxide-containing compound to prepare the organic peroxide formulation.
[0093] Aspect 20: The method of Aspect 19, wherein the at least one organic peroxide is a mixture of meta- and para-di(t-butylperoxy)diisopropylbenzene in a weight ratio range of from about 100:0 to about 0:100
[0094] Aspect 21: The method of Aspect 19 or 20, wherein the at least one organic peroxide is a mixture of meta- and para-di(t-butylperoxy)diisopropylbenzene in a weight ratio range of from about 60:40 to about 90: 10.
[0095] Aspect 22: The method of any one of Aspects 19-21, wherein the at least one organic peroxide is a mixture of meta- and para- di(t-butylperoxy)diisopropylbenzene in a weight ratio range of 78:22.
[0096] Aspect 23: The method of any one of Aspects 19-22, wherein the at least one crosslinking coagent is alpha methyl styrene dimer and at least one selected from triallyl cyanurate triallyl isocyanurate, triallyl trimellitate, pentaerythrithol triallyl ether, and triallyl trimesate.
[0097] Aspects 24: The method of any one of Aspects 19-23, wherein the at least one free radical trap is selected from the group consisting of mono-tert-butylhydroquinone (MTBHQ); hydroquinone mono-methyl ether (HQMME); mono-tert-amylhydroquinone (MTAHQ); di-tert-amylhydroquinone (DTAHQ); di-tert-butylhydroquinone (DTBHQ); 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxyl (4-OHT); and 2,2,6,6-tetramethylpiperidine-1-oxyl (TEMPO).
[0098] Aspects 25: The method of any one of Aspects 19-24, wherein an amount of the di(t-butylperoxy)diisopropylbenzene is from about 25% to about 60%; an amount of the at least one crosslinking coagent is from about 45% to about 74%; and an amount of the at least one free radical trap is from about 1% to about 30%, based on a total weight of the organic peroxide formulation.
[0099] Aspects 26: The method of any one of Aspects 19-25, wherein the polymer is a polyethylene selected from the group consisting of ultra-high molecular weight polyethylene (UHMWPE), high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE), and linear low density polyethylene (LLDPE).
[0100] Aspect 27: The method of any one of Aspects 19-26, wherein the organic peroxide formulation is added to the polymer in an amount from about 1 phr to about 10 phr.
[0101] Aspect 28: A system for crosslinking a polymer, wherein the system comprises an organic peroxide formulation comprising: di(t-butylperoxy)diisopropylbenzene; at least one crosslinking coagent selected from the group consisting of triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, triallyl trimesate, pentaerythrithol triallyl ether, and alpha methyl styrene dimer; and at least one free radical trap selected from the group consisting of a quinone-containing compound and a nitroxide-containing compound, wherein the organic peroxide formulation is a homogenous melt.
[0102] Aspect 29: The system of Aspect 28, wherein the at least one organic peroxide is a mixture of meta- and para-di(t-butylperoxy)diisopropylbenzene in a weight ratio range of from about 100:0 to about 0:100
[0103] Aspect 30: The system of Aspects 28 or 29, wherein the at least one organic peroxide is a mixture of meta- and para-di(t-butylperoxy)diisopropylbenzene in a weight ratio range of from about 60:40 to about 90: 10.
[0104] Aspect 31: The system of any one of Aspects 28-30, wherein the at least one organic peroxide is a mixture of meta- and para-di(t-butylperoxy)diisopropylbenzene in a weight ratio range of 78:22.
[0105] Aspect 32: The system of any one of Aspects 28-31, wherein the at least one crosslinking coagent is alpha methyl styrene dimer and at least one selected from triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, pentaerythrithol triallyl ether, or triallyl trimesate.
[0106] Aspect 33: The system of any one of Aspects 28-32, wherein the at least one free radical trap is selected from the group consisting of mono-tert-butylhydroquinone (MTBHQ); hydroquinone mono-methyl ether (HQMME); mono-tert-amylhydroquinone (MTAHQ); di-tert-amylhydroquinone (DTAHQ); di-tert-butylhydroquinone (DTBHQ); 2, 2, 6, 6-tetramethylpiperidine-1-oxyl (TEMPO); and 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxyl (4-OHT).
[0107] Aspect 34: The system of any one of Aspects 28-33, wherein the organic peroxide formulation comprises: di(t-butylperoxy)diisopropylbenzene; triallyl cyanurate and alpha methyl styrene dimer; and at least one free radical trap is selected from the group consisting of mono-tert-butylhydroquinone (MTBHQ); hydroquinone mono-methyl ether (HQMME); mono-tert-amylhydroquinone (MTAHQ); di-tert-amylhydroquinone (DTAHQ); di-tert-butylhydroquinone (DTBHQ); 4-hydroxy-2,2,6,6-tetramethylpiperidine-l-oxyl (4-OHT); and 2, 2,6,6-tetramethylpiperidine-l-oxyl (TEMPO).
[0108] Aspect 35: The system of any one of Aspects 28-34, wherein the organic peroxide formulation comprises: the di(t-butylperoxy)diisopropylbenzene in an amount from about 25% to about 60% based on a total weight of the organic peroxide formulation; the at least one crosslinking coagent in an amount from about 45%> to about 74% based on a total weight of the organic peroxide formulation; and the at least one free radical trap in an amount from about 1% to about 30% based on a total weight of the organic peroxide formulation.
[0109] Aspect 36: The system of any one of Aspects 28-35, wherein the organic peroxide formulation comprises: di(t-butylperoxy)diisopropylbenzene; triallyl cyanurate and alpha methyl styrene dimer; and mono-tert-butylhydroquinone (MTBHQ).
[0110] Aspect 37: The system of any one of Aspects 28-35, wherein the organic peroxide formulation comprises: di(t-butylperoxy)diisopropylbenzene; triallyl cyanurate and alpha methyl styrene dimer; and hydroquinone mono-methyl ether (HQMME) and 4-hydroxy-2,2,6,6-tetramethylpiperidine-l-oxyl (4-OHT).
[0111] Aspect 38: The system of any one of Aspects 28-35, wherein the organic peroxide formulation comprises: di(t-butylperoxy)diisopropylbenzene; triallyl cyanurate and alpha methyl styrene dimer; and di-tert-amylhydroquinone (DTAHQ) and 4-hydroxy-2, 2,6,6-tetramethylpiperidine-l-oxyl (4-OHT).
[0112] Aspect 39: A method of cross-linking a polymer, the method comprising: applying the system of any one of Aspects 28-38 to the polymer; and curing using a time-temperature profile such that at least 95 wt% or more of the organic peroxide, preferably at least 99 wt% to ideally 100 wt% of the organic peroxide, of the organic peroxide formulation is decomposed during the process.
[0113] Aspect 40: The method of Aspect 39, wherein the polymer is a polyethylene selected from the group consisting of ultra-high molecular weight polyethylene (UHMWPE), high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE), and linear low density polyethylene (LLDPE).
[0114] EXAMPLES
[0115] The principles of the present invention, as well as certain exemplary features and embodiments thereof, will now be described with reference to the following non-limiting examples.
[0116] A. MEASUREMENT TECHNIQUES
[0117] RHEOLOGY MEASUREMENTS FOR CROSSLINKING HDPE
[0118] To follow the crosslinking of HDPE, test method ASTM D5289-12 - Vulcanization Using Rotorless Cure Meters - was used on an Alpha Technologies RPA® 2000 rheometer (“the RPA® 2000 rheometer”). The RPA® 2000 rheometer is essentially a moving die rheometer and can be used to study the crosslinking and scorch time behavior of various polymers, elastomers and rubbers. The RPA® 2000 rheometer is capable of conducting both isothermal and variable temperature crosslinking studies. Using this rheometer, physical properties including the polymer elastic modulus S’ (dN-m), the loss modulus S” (dN-m), Real Polymer Viscosity r (Pa-sec), and Tangent Delta were measured.
[0119] Unless otherwise stated, for crosslinking evaluations, the RPA® 2000 rheometer was set to 190°C with a 1 degree arc of applied strain and a set oscillation frequency of 100 cpm (cycles per minute) with a set time of 12 minutes. This instrument follows the S’ elastic modulus in dN-m versus time using the 190°C, 1 degree arc of applied strain and 100 cpm frequency. For each example, 4.45 grams of powdered HDPE was weighed using a two-place flat top digital Mettler balance and placed between two Dartek® polymer sheets supplied by the manufacturer of the RPA® 2000 rheometer. The sample sandwiched between the two Dartek® sheets was placed on the lower die of the RPA® 2000 rheometer when the lower die was at a temperature of 190°C. Once the sample was placed on the lower die, the upper die (also heated to 190°C) was brought down on the lower die and a pressure of 80 psi was applied. After 12 minutes, the crosslinking ofthe HDPE, the tsl(min) scorch time, and the time to 90% of cure in minutes (tc90), all at 190°C, were measured by the instrument.
[0120] Unless otherwise stated, for lower temperature scorch time evaluations, the RPA® 2000 rheometer was set to 162°C with a 1 degree arc of applied strain and a set oscillation frequency of 100 cpm (cycles per minute) with a set time of 12 minutes. The testing procedure was similar to that for the 190°C crosslinking evaluations (except for the lower temperature setting). The tsl(min) scorch time at 162°C was measured by the RPA® 2000 rheometer. In some cases the rheometer was used to measure various physical properties using a non-isothermal, variable temperature profile from 141°C to 225°C at 3°C / min ramp using a 1 degree arc and 100 cpm frequency.
[0121] YELLOW INDEX (Yi) MEASUREMENT
[0122] HDPE samples were cured in the RPA 2000 rheometer using the 141°Cto 225°C, 3°C / min, 1 deg arc, 100 cpm variable temperature cure profile. The crosslinked HDPE samples obtained from the RPA® 2000 rheometer were tested for color, e g., Yi (yellowness index) using a Datacolor Spectro 750 benchtop spectrophotometer. The spectrophotometer instrument was first calibrated using a black standard, a white standard and a green standard supplied with the instrument before measuring the crosslinked HDPE test specimens for color. Spectrophotometer settings included using a Large Aperture, Specular Included, and 0% UV / Filter. The Hunter L, a, b color values as well as Yi (Yellowness Index) were measured with this spectrophotometer.
[0123] B. EXPERIMENTAL DETAILS
[0124] In the examples described herein, various units have been abbreviated as follows:
[0125] Yi (color measurement) = Yellowness Index (higher Yi means more yellow color)
[0126] L (color measurement) (L=100 White, L=0 Black)
[0127] a (color measurement) ( +a Red; -a Green)
[0128] b (color measurement) (+b Yellow; -b Blue)
[0129] MH (dN-m) = Maximum torque in deci-Newton-meters; relates to crosslinking attained.
[0130] Tsl. O (min) = Time in minutes to achieve a 1.0 dN-m increase from minimum torque.
[0131] Tc90 (min) = Time in minutes to achieve 90% of the total cure time.
[0132] The following materials are used in the examples described herein:
[0133] DYBP = 2,5-di(t-butylperoxy)-2,5-dimethylhexyne-3
[0134] VC = Vul-Cup® R = m / p-di(t-butylperoxy)diisopropylbenzene with a meta / para ratio of 78 / 22.
[0135] 4-OHT = 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl.
[0136] TEMPO = 2,2,6,6-tetramethylpiperidine-1-oxyl.
[0137] MSD = NOFMER® MSD from NOF Corporation, Japan = alpha methyl styrene dimer that is a blend of 93 wt% 2,4-diphenyl-4-methyl-1-pentene and 7 wt% 2,4-diphenyl-4-methyl-2-pentene coagents.
[0138] MSD-H = AMSD, GRH (Kowa American Corporation) = alpha methyl styrene dimer that is a blend of 97.6 wt% 2,4-diphenyl-4-methyl-1-pentene and 2.4 wt% 2,4-diphenyl-4-methyl-2-pentene coagents.
[0139] MSD-U = AMSD, GRU (Kowa American Corporation) = alpha methyl styrene dimer that is a blend of >99 wt% 2,4-diphenyl-4-methyl-1-pentene and < 0.2wt% 2,4-diphenyl-4-methyl-2-pentene coagents.
[0140] HQMME = hydroquinone mono-methyl ether
[0141] MTBHQ = mono-tertiary butyl hydroquinone
[0142] MTAHQ= mono-tert-amylhydroquinone
[0143] DTAHQ = di-tert-amylhydroquinone
[0144] DTBHQ = di-tert-butylhydroquinone
[0145] TAC = triallyl cyanurate
[0146] TAIC = triallyl isocyanurate
[0147] TATM = triallyl trimellitate
[0148] TATMT = triallyl trimesate
[0149] PETE = pentaerythritol triallyl ether
[0150] DCP = dicumyl peroxide.
[0151] PREPARATION OF COMPARATIVE EXAMPLES 1-5 AND INVENTIVE EXAMPLES 1-8
[0152] Organic peroxide formulations C1-C5 and E1-E8 for Comparative Examples 1-5 and Examples 1-8, respectively, were prepared as described in TABLE 1. Each organic peroxide formulation is a low-melting, homogeneous, solid mixture that produces a homogeneous melt at elevated temperatures between about 45°C to about 68°C, preferably between about 55°C to 65°C, more preferably about 60°C to about 68°C. As these organic peroxide formulations are mixtures, the various percentages of all individual components making up a peroxide formulation were designed to add up to one hundred percent (100%) by weight.
[0153] Specifically, for each example, a total of 10.000 grams of each organic peroxide formulation was prepared and weighed using a four-place digital Mettler Analytical balance, and then placed into a four-dram clear glass vial. Each component of the formulation was weighed separately into the glass vial, and the total weight of the resulting peroxide composition was 10.000 grams. Typically, the solid components were added first, followed by the liquid components. A small magnetic stir bar was then added to the vial, and the vial was sealed with a screw cap closure having a Teflon® inner seal.
[0154] TABLE 1
[0155] All the HDPE samples used for testing on the RPA® 2000 rheometer were prepared as follows. HDPE samples of Comp. Ex. 1-5 and Examples 1-6 used in rheometer testing were prepared in the following manner. For each example, a sealed four-dram clear glass vial containing the 10.000 grams of the solid organic peroxide formulation was placed in a hot air oven set to about 67°C for approximately 30 to 45 minutes until all components melted. Each vial also contained a small magnetic stir bar. Once the contents were molten, the vial was placed on a magnetic hot plate stirrer set to about 60°C and a medium-high stir speed. The vial was mixed for one to two minutes to ensure homogeneity, which was visually inspected through the clear glass of the vial. Using the same four place Mettler Analytical digital balance, a glass bullet mixer container was placed on the balance and 50.000 grams of powdered HDPE was weighed into the container, followed by careful addition of the homogeneous molten peroxide composition to the HDPE in the various phr amounts shown in TABLE 2. Afterwards a metal mixing blade with rubber seal and plastic screw cap was firmly attached to the glass bullet mixer container. The HDPE powder containing the peroxide composition within the glass bullet mixer assembly was then placed on the bullet mixer motor and was mixed at high speed for about eight minutes. After this mixing process, the powdered HDPE mixed with the peroxide formulation was transferred from the bullet mixer container to a clean, clear glass jar and sealed with a screw cap and labeled.This process was performed to make all the HDPE samples used for testing on the RPA® 2000 rheometer.
[0156] Following the preparation of the HDPE samples, the crosslinking and scorch time performance for each sample was measured according to the procedures described herein, and the results thereof are shown in TABLE 2.
[0157] TABLE 2
[0158] Referring to TABLE 2, Comp. Ex. 1 used a combination of DYBP and TAC as the HDPE curing system, which provides a long, desirable HDPE melt time based on the long tsl(min) scorch time of 10.64 minutes at the process temperature of 162°C. Good crosslinking at 190°C for Comp. Ex. 1 is represented by the MH maximum torque value of 11.12 dN-m. The long tsl(min) scorch time at 162°C of 10.64 minutes for Comp. Ex. 1 represents the desirable longer HPDE polymer melt time in the mold which allows trapped air bubbles in the polymer melt to escape, prior to the final crosslinking phase at elevated temperatures during the rotomolding process. The desirablelonger scorch time at 162°C for DYBP is naturally achieved due to DYBP’s higher half-life properties (high thermal stability).
[0159] Comp. Ex. 2 is another HDPE curing system that replaces DYBP with VC as the organic peroxide in the novel organic peroxide formulation. VC is considerably less thermally stable than DYBP. The curing system of Comp. Ex. 2 also includes MTBHQ as a free-radical trap. The tsl(min) scorch time at 162°C was significantly reduced to 6.14 minutes for Comp. Ex. 2 versus the more desirable tsl(min) scorch time of 10.64 minutes at 162°C for Comp. Ex. 1, because of the lower thermal stability of VC compared to DYBP. The shorter scorch time (tsl at 162°C) of the curing system of Comp. Ex. 2 renders it only suitable for thin wall rotomolding applications. If the curing system of Comp. Ex. 2 is used for curing HDPE for application in thick wall IBCs, the speed of HDPE curing would be too fast because of the short tsl(min) scorch time at 162°C. This faster curing peroxide would result in air bubbles being trapped within the HDPE for thick (> 0.5 inch) rotomolded walls, which would consequently decrease the mechanical strength of such HDPE rotomolded walls and the IBCs that include such walls.
[0160] Comp. Ex. 5 is a peroxide formulation in which the TAC is completely replaced with MSD, while maintaining the same amounts of VC peroxide and MTBHQ used in Comp. Ex. 2. However, as shown in TABLE 2, completely substituting TAC with MSD and adding the peroxide formulation to HDPE at 1.0 phr resulted in insufficient crosslinking vs the DYBP result of Comp. Ex. 1. This is because the MH or maximum torque at 190°C cure temperature resulted in a torque of only 1.8 dN-m for Comp. Ex. 5, which is six time less than that obtained when using TAC in Comp. Ex. 2. Due to the very poor crosslinking performance (very low MH of 1.80 dN-m) resulting from completely substituting MSD for TAC, the tsl(min) scorch time at 162°C was unable to be measured.
[0161] In another comparative example, the VC concentration was increased from 37.4% (Comp. Ex. 5) to 68.9% (Comp. Ex. 3) resulting in a reasonable MH (dN-m) crosslinking value of 10.78 dN-m at 190°C, i.e., comparable to the crosslinking value of Comp. Ex. 1. However, despite this improvement in crosslinking observed for Comp. Ex. 3, there was still an insufficient increase in the tsl(min) scorch time at 162°C, with a low value of 7.66 for the tsl(min) value when using only MSD as the crosslinking coagent. FIGURE 1 plots the results of the scorch study of Comp. Ex. 1,Comp. Ex. 2 and Comp. Ex. 3. As seen in FIGURE 1, Comp. Ex. 3 is still curing too fast at the process temperature of 162°C.
[0162] Comp. Ex. 4 uses similar amounts of VC and MSD as in Comp. Ex. 3, but replaces the 2.60 wt% MTBHQ free-radical trap in Comp. Ex. 3 with a combination of 1.80 wt% 4OHT and 3.90 wt% HQMME in an attempt to increase the 162°C tsl(min) scorch time to match the performance of Comp. Ex. 1. Using 1.22 phr of the organic peroxide formulation of Comp. Ex. 4 in HDPE resulted in a reasonable amount of crosslinking at 190°C, but still an insufficient result in theHDPE melting time represented by the 8.15 minute tsl(min) scorch time at 162°C. The 8.15 tsl(min) scorch time attained by Comp. Ex. 4 at 162°C is still significantly lower than the 10.64 tsl(min) scorch time at 162°C for Comp. Ex. 1.
[0163] Examples 1 to 6 of TABLE 2 illustrate the unexpected superior properties of the inventive organic peroxide formulations. Referring to TABLE 2, the organic peroxide formulation of Example 1, i.e., a blend of VC, TAC, MSD and MTBHQ, provided a suitable amount of MH crosslinking of 10.90 dN-m at 190°C with an unexpected, desirable scorch time tsl(min) of 9.66 min at 162°C (resulting in a longer HDPE melting time to allow bubbles to escape). This improvement in crosslinking is also observed for Examples 2 to 6, with MH(dN-m) values ranging from about 10.92 dN-m to about 11.44 dN-m. The tsl(min) scorch time values at 162°C for Examples 1 to 6 are similar to the scorch time of Comp. Ex. 1 that uses the DYBP with a higher half-life.
[0164] In summary, the tsl(min) scorch time results at 162°C for Examples 1 to 6 are quite unexpected as the VC organic peroxide used in the preparation of the peroxide formulations of this invention is significantly lower in half-life versus the considerably higher half-life, more thermally stable DYBP peroxide. Based upon dilute solution decomposition kinetic data, the half-life of DYBP at 162°C is about 20.74 minutes, whereas the half-life of the VC peroxide at that temperature is only 5.79 minutes. In other words, at 162°C, it takes about 20.74 minutes for one-half of the DYBP peroxide to decompose, but it takes only 5.79 minutes for one-half of the VC peroxide to decompose. Thus, obtaining a similar performance for the tsl(min) scorch time at 162°C with the novel peroxide formulations described herein, that uses the VC peroxide in combination with specific crosslinking coagents and free radical traps, compared to the peroxideformulations that use DYBP, is extremely unexpected to one of ordinary skill in the art, if not seemingly impossible to achieve.
[0165] Additionally, comparing Comp. Ex. 5 (using only 60 wt% MSD as the crosslinking coagent) with Comp. Ex. 2 (using only 60 wt% TAC as the crosslinking coagent), the amount of crosslinking is significantly less when using only MSD. Thus, the singular use of MSD as a crosslinking coagent is not effective.
[0166] However, unexpectedly, the blend of MSD and TAC (as used in Examples 1 to 6) provides the desired synergy of good crosslinking, i.e., desirable MH(dN-m) values at 190°C, with desirably long tsl(min) scorch time values at 162°C when combined with free-radical traps.
[0167] Referring to TABLE 1 and TABLE 2, peroxide formulation of Example 2 uses a nearly identical amount of the blend of HQMME and 4-OHT free-radical traps used in Comp. Ex. 4. Comp. Ex. 4 included 25.5 wt% MSD as a crosslinking coagent with no TAC, and achieved a desirable level of crosslinking, i.e., 10.87 dN-m for the MH at 190°C, but a short scorch time of only a tsl(min) of 6.14 minutes. In comparison, combining MSD with TAC in Example 2 unexpectedly resulted in a desirable combination of good crosslinking at 190°C with an MH of 11.59 dN-m and desirable melting time (tsl scorch time) at 162°C of 10.07 minutes. Moreover, Example 2 required less VC peroxide to attain the same crosslinking performance compared to Comp. Ex. 4.
[0168] In summary, in each of Examples 1-6 in TABLE 2, the novel peroxide formulations that include a combination of organic peroxide, TAC, MSD and free-radical traps provided the unexpected combination of desirable crosslinking at 190°C with sufficient HDPE melting time (tsl scorch time) at 162°C.
[0169] Additionally, equivalent crosslinking (MH in dN-m at 190°C) results were obtained for the novel peroxide formulations of this invention, namely Example 5 and Example 6 versus Comp. Ex. 1 at 190°C, while providing desirable tsl (min) scorch times values at 162°C nearly equivalent to the DYBP performance of Comp. Ex. 1, which indicates the suitability of the novel organic peroxide formulations of this application for HDPE curing for thick wall articles.
[0170] Additionally, unlike the DYBP peroxide, the decomposition of the VC peroxide does not produce any harmful or noxious by-products. For example, the VC peroxide complies with theBfR (Bundesinstitut fur Risikobewertung) regulations in Germany for use in the controlled rheology of polypropylene for indirect food contact packaging applications. That is, the novel peroxide formulations of TABLE 2 provide good crosslinking with suitable melting time to allow for trapped air bubbles to escape, while overcoming the undesirable air and skin hygiene issues caused by the well-known acetylenic DYBP peroxide decomposition by-products.
[0171] Rheographs illustrating the HDPE melting time performance of Comp. Ex. 1 and Example 5 at 162°C is provided in FIGURE 2. As shown in FIGURE 2, the novel organic peroxide formulation of Example 5, using the less thermally stable VC peroxide, unexpectedly provided identical over-lapping melting time-temperature performance compared to the highly thermally stable DYBP peroxide (Comp. Ex.l) that is currently used in thick-wall rotomolding applications.
[0172] In addition to the inventive and comparative Examples described above, Comp. Ex. 6 and 7 were prepared to demonstrate the difference in reactivity between TAC (triallyl cyanurate) and TAIC (triallyl isocyanurate). The components of Comp. Ex. 6 and 7 were mixed in the amounts shown in TABLE 3, and then used as a curing system for HDPE in accordance with the procedures described herein.
[0173] TABLE 3
[0174] Rheology measurements on HDPE cured with the organic peroxide formulations of Comp. Ex. 6 and 7 are shown in TABLE 4.
[0175] TABLE 4
[0176] As shown by the results in TABLE 4, there is a difference in reactivity between TAIC and TAG. Without being held to any specific theory, the TAIC coagent may be forming a gel at lower percentage conversion, thereby resulting in undesirable lower scorch times. All other variables being equal, the TAC coagent provided higher (more desirable) scorch times when using DCP at the 145°C test temperature. At the test temperature of 162°C, DCP decomposes more rapidly, which results in a much shorter tsl(min) scorch time. However, even at a test temperature of 162°C with the faster decomposing DCP peroxide, TAC provided a more desirable (one minute longer) tsl(min) scorch time versus TAIC. Nonetheless, DCP is far too reactive at the elevated temperatures used in rotomolding processes. The tsl(min) scorch time of about two minutes at 162°C is much too short for the rotomolding process as the desired scorch time is nearly five times greater when compared to the tsl(min) performance of DYBP at that temperature. Thus, DCP is unsuitable for inclusion in a crosslinking system for HDPE rotomolding processes.
[0177] HDPE GEL POINT DETERMINATION USING S’ vs S” CROSSOVER TEMPERATURE
[0178] Using the same RPA® 2000 instrument, a variable temperature crosslinking experimental method was programmed into the instrument to follow the S’ Elastic Modulus, the S” Loss Modulus, and Tangent Delta values versus changing temperature in degrees Celsius, where the variable temperature range is from 141°C to 225°C.
[0179] Using the sample preparation procedure described herein, 4.45 grams of powdered HDPE containing the relevant peroxide formulation being studied was placed between two Dartek® sheets. When the initial set temperature of 141 °C was reached and stable for both upper and lower heated dies of the RPA® 2000 rheometer, the HDPE sample was carefully placed on the lower die and immediately the two platens were brought in contact with each other to start the variable temperature crosslinking experiment. The variable temperature range was set to begin at 141 °C and end at 225°C wherein the temperature was increased at a rate of 3°C per minute. The applied strain used was 1 degree of arc and the frequency used was 100 cpm, similar to the settings used in the isothermal crosslinking studies at 190°C and 162°C described herein.
[0180] FIGURE 3 is a rheograph of the variable temperature crosslinking of HDPE. This rheograph compares the crosslinking of Comp. Ex. 1, Comp. Ex. 2, and Example 6. FIGURE 3 is a plot of the Elastic Modulus S’ versus variable temperature, and as seen in FIGURE 3, Example 6 follows the initial melting curve of HDPE for Comp. Ex. 1, i.e., crosslinking using the comparative organic peroxide formulation that includes the DYBP high half-life peroxide.
[0181] To better study the melting of HDPE, prior to potential gelling or crosslinking of the HDPE polymer, the Elastic Modulus S’ in dN-m versus the Loss Modulus S” in dN-m for Example 6, Comp. Ex. 1 and Comp. Ex. 2 were plotted in FIGURE 4 versus varying temperature. As shown in FIGURE 4, a narrow temperature range of 162°C to 172°C was plotted to better determine the S’-S” crossover temperature, i.e., where the Elastic S’ and Loss S” modulus curves cross. The point where S’ and S” cross for each individual peroxide formulation is important, because the Elastic Modulus S’ Loss Modulus S” crossover point (where S’=S”) determines the HDPE gel point temperature. It is at this temperature where air bubbles could potentially get trapped in the rapidly crosslinking HDPE melt. Moreover, where S’ and S” cross, these two modulus values are equal, that is, the Elastic Modulus S’ in dN-m equals the Loss Modulus S” in dN-m at the crossover point. Tangent Delta is defined as the Loss Modulus S” divided by the Elastic Modulus S’. Thus Tangent Delta is a dimensionless variable, and when S’ is equal to S” at the crossover point, the Tangent Delta is equal to one.
[0182] Using this rheological information, the gel temperature for Example 6, Comp. Ex. 1 and Comp. Ex. 2 over the 163°C to 173°C temperature range at a Tangent Delta value of one was plotted in FIGURE 5. A line drawn across the graph at Tangent Delta value of one, provides foreasy viewing of the gel temperature for each peroxide. In summary, the gel temperature attained for Example 6 was determined to be 170°C, a significant improvement over Comp. Ex. 2 (using VC organic peroxide), which has a gel point of about 164°C. The gel point of the very high halflife DYBP peroxide (Comp. Ex. 1) is about 171°C. This experimental technique to determine polymeric gel point further demonstrates the significant improvement in delaying the onset of HDPE gelation by using the novel organic peroxide formulations described herein, which further helps to prevent the trapping of air bubbles in a thicker HDPE wall during the non-isothermal rotational molding process.
[0183] Using the RPA® rheometer with a variable temperature profile of 141 °C to 225°C, organic peroxide formulations E7 and E6 listed in TABLE 1 are compared on an equal weight basis of 1.13 phr in HDPE. This comparison is a study of the effect of altering the coagent blend ratio of 2.4-diphenyl-4-methyl-l-pentene and 2,4-diphenyl-4-methyl-2-pentene type coagents. E6 uses an (MSD) alpha methyl styrene blend ratio of 93 wt% 2,4-diphenyl-4-methyl-l -pentene and 7 wt% 2.4-diphenyl-4-methyl-2-pentene. In contrast, E7 uses an (MSD-U) alpha methyl styrene blend ratio of 99 wt% 2,4-diphenyl-4-methyl-l-pentene and lwt% 2,4-diphenyl-4-methyl-2-pentene. Referring to FIGURE 6, the plot of Tangent Delta versus Temperature clearly shows an improvement (increase) in the gel point temperature to 170.6°C for peroxide formulation E7 versus a lower gel point temperature of 170°C for E6. This increase in gel point temperature is a dramatic performance improvement because organic peroxides decompose exponentially with changes in temperature. Thus, the coagent compositions of alpha methyl styrene dimer comprising various blends of 2, 4-diphenyl-4-methyl-l -pentene and the 2,4-diphenyl-4-methyl-2-pentene coagents can significantly affect the final HDPE gel point temperature or scorch time performance. This increase in gel point temperature is a dramatic performance improvement because organic peroxides decompose exponentially with changes in temperature, and higher the gel point temperature, the less likely air bubbles will be trapped in thick wall articles of crosslinked HDPE.
[0184] CROSSLINKING ROTATIONAL MOLD GRADE PA-11 USING NOVEL PEROXIDE FORMULATION
[0185] The novel peroxide formulations described herein can also be used to crosslink polyamide resins, while providing an extended polymer melt time without substantial crosslinking during the polymer melting phase.
[0186] CROSSLINKING PA- 11 WITH EXTENDED MELTING TIME PERFORMANCE
[0187] In this example, 4.44 grams of PA- 11 powdered polyamide, natural, rotomolding grade was weighed into a two-ounce cup using a four place Mettler digital analytical balance. Then 0.0666 grams of the molten novel peroxide formulation E7, which was heated to 60°C, was added to the powdered PA- 11 to create a PA- 11 polyamide composition containing 1.50 wt% of the novel E7 peroxide formulation. A small stainless steel spatula was used to carefully blend the molten peroxide formulation with the PA-11 powder. When the powdered PA-11 and the molten peroxide blend appeared uniform by visual inspection, the entire contents of the cup was poured onto a rectangular section of Dartek® film and covered with another section of film to create a sample sandwich for the RPA® Rheometer. This sample sandwich was then inserted into the rheometer which was set to a temperature of 195°C, 1 degree arc of applied strain, 100 cpm (cycles per minute), and the sample sandwich was maintained under these conditions for four minutes. The RPA® rheograph plot of the Elastic Modulus S’ (dN-m) versus time is shown in FIGURE 7. The increase in elastic modulus indicates that the PA- 11 was crosslinked with the E7 peroxide formulation. That flat bottom portion of the crosslinking curve between 0.40 and 0.62 minutes indicates that the PA-11 is molten but not undergoing any crosslinking reaction. In other words, the novel E7 peroxide formation delayed the initial crosslinking of the PA- 11 for about 0.22 minutes at 195°C.
[0188] This 0.22 minute delay in crosslinking at 195°C is very significant. As shown in TABLE 5 listing the time and temperature VC (Vul-Cup®, Arkema) peroxide half-life, the VC peroxide decomposes quite rapidly at 195°C. Referring to TABLE 5, about 62% of the peroxide remains undecomposed after only 0.20 minutes, which means 38% of the peroxide had decomposed. Yet very surprisingly, the PA-11 remained molten, with no crosslinking during this time period despite 38% of the VC peroxide having decomposed. The dramatic and highly unexpected delay in crosslinking for PA-11 is due to the novel E7 peroxide composition.
[0189] TABLE 5
[0190] COLOR MEASUREMENTS
[0191] Color Measurements of Variable Temperature Cured HDPE using the Datacolor Spectro 750 are shown in TABLE 6. Referring to TABLE 6, Comp. Ex 1 HDPE crosslinked with CE1 (i.e., DYBP peroxide) provided an intense yellow color with a Yi value of 45.16. The peroxide of this invention (Example 6) provided a crosslinked HDPE with a Yi of only 10.01. A lower Yi number indicates less yellow color. Thus this test result demonstrates that the HDPE articles cured with the novel organic peroxide compositions described herein are whiter in color (values in the lower Yi range) versus those cured with DYBP Another measurement of yellow color is the b value. The higher the b value (more positive), the greater the measured yellow' color. Crosslinked HDPE of Comp. Ex 1 provided a “b” value of 20.38 versus a “b” value of only 5.61 for crosslinked HDPE of Example 6. This further supports the Yi results obtained from the Spectrophotometer that crosslinked HDPE of Example 6, using the organic peroxide formulation E6, results in a significantly more desirable color, versus HDPE cured with Comp. Ex 1 (i.e., DYBP peroxide).
[0192] TABLE 6
[0193] COMPARISON OF DTBHQ-CONTAINING AND DTAHQ-CONTATNING PEROXIDE FORMULATIONS USING DIFFERENT DIMER GRADES (MSD-H OR MSD-U) FOR CROSSLINKING HDPE
[0194] Referring to TABLE 1, peroxide formulation E8 is compared to peroxide formulation E7, where DTAHQ was replaced with DTBHQ on an equal weight basis, while we use different grades of alpha methyl styrene dimer (MSD-H or MSD-U). Using the same variable temperature cure profde (141°C to 225°C) used previously, the Tangent Delta versus temperature was plotted in FIGURE 8 for 1.13 phr E8 peroxide formulation in HDPE (thin solid line). Where the Tangent Delta line crosses the value of 1 in FIGURE 8, an HDPE gel temperature of about 170.3°C was obtained. Thus, the E8 peroxide formulation (using MSD-H), and the E7 peroxide formulation (using MSD-U) combined with the various quinones and nitroxides of this invention, continue to show good improvement in delaying the crosslinking of HDPE to permit the escape of trapped air bubbles.
[0195] The ability of the novel peroxide compositions described herein to delay crosslinking of PA-11 and HDPE when significant peroxide decomposition occurs is highly unexpected and very desirable / valuable when crosslinking polymers using a rotomolding process.
[0196] In summary, novel organic peroxide compositions described herein can be used for polymer curing, while maintaining an extended polymer melt time with little to no crosslinking to allow the escape of any trapped bubbles prior to final crosslinking of the cured article.
[0197] As various modifications could be made in the above methods and compositions and would be apparent to those skilled in the art without departing from the scope of the invention, the disclosures herein are intended to be interpreted as illustrative and not limiting. Any numbers expressing quantities of ingredients, constituents, reaction conditions, and so forth used in the specification are to be interpreted as encompassing the exact numerical values identified herein, as well as being modified in all instances by the term “about” used as a term of approximation, and intended to include minor variations in the literally stated values as understood in the art and subject to any standard deviations found in their respective measurement techniques None of the features recited herein should be interpreted as invoking 35 U. S C. § 112, paragraph 6, unless the term “means” is explicitly used in reference to a function.
Claims
What is claimed is:
1. An organic peroxide formulation comprising:(i) di(t-butylperoxy)diisopropylbenzene;(ii) at least one crosslinking coagent selected from the group consisting of triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, triallyl trimesate, pentaerythrithol triallyl ether, and alpha methyl styrene dimer; and (iii) at least one free radical trap selected from the group consisting of a quinone- containing compound and a nitroxide-containing compound,wherein the organic peroxide formulation is a homogenous melt.
2. The organic peroxide formulation of claim 1, wherein the at least one organic peroxide is a mixture of meta- and para-di(t-butylperoxy)diisopropylbenzene in a weight ratio range of from about 100:0 to about 0: 1003. The organic peroxide formulation of claim 1 or 2, wherein the at least one organic peroxide is a mixture of meta- and para-di(t-butylperoxy)diisopropylbenzene in a weight ratio range of from about 60:40 to about 90:10.
4. The organic peroxide formulation of any one of claims 1-3, wherein the at least one organic peroxide is a eutectic mixture of meta- and para-di(t-butylperoxy)diisopropylbenzene in a weight ratio range of 78:22.
5. The organic peroxide formulation of any one of claims 1-4, wherein the at least one crosslinking coagent is alpha methyl styrene dimer and at least one selected from triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, pentaerythrithol triallyl ether, or triallyl trimesate.
6. The organic peroxide formulation of any one of claims 1-5, wherein the at least one free radical trap is selected from the group consisting of mono-tert-butylhydroquinone (MTBHQ); hydroquinone mono-methyl ether (HQMME); mono-tert-amylhydroquinone (MTAHQ); di-tert-amylhydroquinone (DTAHQ); di-tert-butylhydroquinone (DTBHQ); 2, 2,6,6-tetramethylpiperidine-1-oxyl (TEMPO); and 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxyl (4-OHT).
7. The organic peroxide formulation of any one of claims 1-6, wherein:(a.) an amount of the di(t-butylperoxy)diisopropylbenzene is from about 25% to about 60% based on a total weight of the organic peroxide formulation;(b.) an amount of the at least one crosslinking coagent is from about 45% to about 74% based on a total weight of the organic peroxide formulation; and(c.) an amount of the at least one free radical trap is from about 1% to about 30% based on a total weight of the organic peroxide formulation.
8. The organic peroxide formulation of any one of claims 1-7, comprising:(i) di(t-butylperoxy)diisopropylbenzene;(ii) triallyl cyanurate and alpha methyl styrene dimer; and(iv) at least one free radical trap is selected from the group consisting of mono-tert- butylhydroquinone (MTBHQ); hydroquinone mono-methyl ether (EIQMME); mono-tert-amylhydroquinone (MTAHQ); di-tert-amylhydroquinone (DTAHQ); di-tert-butylhydroquinone (DTBHQ); 4-hydroxy-2,2,6,6-tetramethylpiperidine-l- oxyl (4-OEIT); and 2,2,6,6-tetramethylpiperidine-l-oxyl (TEMPO).
9. The organic peroxide formulation of any one of claims 1-7, comprising:(i) di(t-butylperoxy)diisopropylbenzene;(ii) triallyl cyanurate and alpha methyl styrene dimer; and(iii) mono-tert-butylhydroquinone (MTBHQ).
10. The organic peroxide formulation of any one of claims 1-7, comprising:(i) di(t-butylperoxy)diisopropylbenzene;(ii) triallyl cyanurate and alpha methyl styrene dimer; and(iii) hydroquinone mono-methyl ether (HQMME) and 4-hydroxy-2,2,6,6- tetram ethylpiperidine- 1 -oxyl (4-OHT).
11. The organic peroxide formulation of any one of claims 1-7, comprising:(i) di(t-butylperoxy)diisopropylbenzene;(ii) triallyl cyanurate and alpha methyl styrene dimer; and(iii) di-tert-amylhydroquinone (DTAHQ) and 4-hydroxy-2, 2,6,6- tetram ethylpiperidine- 1 -oxyl (4-OHT).
12. A method of preparing an organic peroxide composition, the method comprising: mixing (i) di(t-butylperoxy)diisopropylbenzene; (ii) at least one crosslinking coagent selected from the group consisting of triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, triallyl trimesate, pentaerythrithol triallyl ether, and alpha methyl styrene dimer; and (iii) at least one free radical trap selected from the group consisting of a quinone-containing compound and a nitroxide-containing compound to prepare the organic peroxide formulation.
13. The method of claim 12, wherein the at least one organic peroxide is a mixture of meta- and para-di(t-butylperoxy)diisopropylbenzene in a weight ratio range of from about 100:0 to about 0:10014. The method of claim 12 or 13, wherein the at least one organic peroxide is a mixture of meta- and para-di(t-butylperoxy)diisopropylbenzene in a weight ratio range of from about 60:40 to about 90:10.
15. The method of any one of claims 12-13, wherein the at least one organic peroxide is a eutectic mixture of meta- and para- di(t-butylperoxy)diisopropylbenzene in a weight ratio range of 78:22.
16. The method of any one of claims 12-15, wherein the at least one crosslinking coagent is alpha methyl styrene dimer and at least one selected from triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, pentaerythrithol triallyl ether, or triallyl trimesate.
17. The method of any one of claims 12-16, wherein the at least one free radical trap is selected from the group consisting of mono-tert-butylhydroquinone (MTBHQ); hydroquinonemono-methyl ether (HQMME); mono-tert-amylhydroquinone; di-tert-amylhydroquinone;DTAHQ; di-tert-butylhydroquinone (DTBHQ); 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxyl (4-OHT); and 2,2,6,6-tetramethylpiperidine-1-oxyl (TEMPO).
18. The method of any one of claims 12-17, wherein an amount of the di(t-butylperoxy)diisopropylbenzene is from about 25% to about 60%; an amount of the at least one crosslinking coagent is from about 45% to about 74%; and an amount of the at least one free radical trap is from about 1% to about 30%, based on a total weight of the organic peroxide formulation.
19. A method of crosslinking a polymer, the method comprising:mixing a molten organic peroxide composition and a polymer; andcuring using a time-temperature profile such that at least 95 wt%, preferably at least 99 wt%, more preferably 100 wt%, or more of the di(t-butylperoxy)diisopropylbenzene is decomposed during the process;wherein the molten organic peroxide composition comprises(i) di(t-butylperoxy)diisopropylbenzene;(ii) at least one crosslinking coagent selected from the group consisting of triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, pentaerythrithol triallyl ether, triallyl trimesate and alpha methyl styrene dimer; and(iii) at least one free radical trap selected from the group consisting of a quinone- containing compound and a nitroxide-containing compound to prepare the organic peroxide formulation.
20. The method of claim 19, wherein the at least one organic peroxide is a mixture of meta- and para-di(t-butylperoxy)diisopropylbenzene in a weight ratio range of from about 100:0 to about 0:10021. The method of claim 19 or 20, wherein the at least one organic peroxide is a mixture of meta- and para-di(t-butylperoxy)diisopropylbenzene in a weight ratio range of from about 60:40 to about 90: 10.
22. The method of any one of claims 19-21, wherein the at least one organic peroxide is a eutectic mixture of meta- and para- di(t-butylperoxy)diisopropylbenzene in a weight ratio range of 78:22.
23. The method of any one of claims 19-22, wherein the at least one crosslinking coagent is alpha methyl styrene dimer and at least one selected from triallyl cyanurate triallyl isocyanurate, triallyl trimellitate, pentaerythrithol triallyl ether, and triallyl trimesate.
24. The method of any one of claims 19-23, wherein the at least one free radical trap is selected from the group consisting of mono-tert-butylhydroquinone (MTBHQ); hydroquinone mono-methyl ether (HQMME); mono-tert-amylhydroquinone; di-tert-amylhydroquinone (DTAHQ); di-tert-butylhydroquinone (DTBHQ); 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxyl (4-OHT); and 2,2,6,6-tetramethylpiperidine-1-oxyl (TEMPO).
25. The method of any one of claims 19-24, wherein an amount of the di(t-butylperoxy)diisopropylbenzene is from about 25% to about 60%; an amount of the at least one crosslinking coagent is from about 45% to about 74%; and an amount of the at least one free radical trap is from about 1% to about 30%, based on a total weight of the organic peroxide formulation.
26. The method of any one of claims 19-25, wherein the polymer is a polyethylene selected from the group consisting of ultra-high molecular weight polyethylene (UHMWPE), high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE), and linear low density polyethylene (LLDPE).
27. The method of any one of claims 19-26, wherein the organic peroxide formulation is added to the polymer in an amount from about 1 phr to about 10 phr.
28. A system for crosslinking a polymer, wherein the system comprises an organic peroxide formulation comprising:(i) di(t-butylperoxy)diisopropylbenzene;(ii) at least one crosslinking coagent selected from the group consisting of triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, triallyl trimesate, pentaerythrithol triallyl ether, and alpha methyl styrene dimer; and(iii) at least one free radical trap selected from the group consisting of a quinone- containing compound and a nitroxide-containing compound,wherein the organic peroxide formulation is a homogenous melt.
29. The system of claim 28, wherein the at least one organic peroxide is a mixture of meta- and para-di(t-butylperoxy)diisopropylbenzene in a weight ratio range of from about 100:0 to about 0:10030. The system of claim 28 or 29, wherein the at least one organic peroxide is a mixture of meta- and para-di(t-butylperoxy)diisopropylbenzene in a weight ratio range of from about 60:40 to about 90: 10.
31. The system of any one of claims 28-30, wherein the at least one organic peroxide is a mixture of meta- and para-di(t-butylperoxy)diisopropylbenzene in a weight ratio range of 78:22.
32. The system of any one of claims 28-31, wherein the at least one crosslinking coagent is alpha methyl styrene dimer and at least one selected from triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, pentaerythrithol triallyl ether, or triallyl trimesate.
33. The system of any one of claims 28-32, wherein the at least one free radical trap is selected from the group consisting of mono-tert-butylhydroquinone (MTBHQ); hydroquinone mono-methyl ether (HQMME); mono-tert-amylhydroquinone (MTAHQ); di-tert-amylhydroquinone (DTAHQ); di-tert-butylhydroquinone (DTBHQ); 2, 2,6,6-tetramethylpiperidine-1-oxyl (TEMPO); and 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxyl (4-OHT).
34. The system of any one of claims 28-33, wherein the organic peroxide formulation comprises:(i) di(t-butylperoxy)diisopropylbenzene;(ii) triallyl cyanurate and alpha methyl styrene dimer; and(iii) at least one free radical trap is selected from the group consisting of mono- tert-butylhydroquinone (MTBHQ); hydroquinone mono-methyl ether (HQMME); mono-tert-amylhydroquinone (MTAHQ); di-tert-amylhydroquinone (DTAHQ); di-tert- butylhydroquinone (DTBHQ); 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxyl (4-OHT); and 2,2,6,6-tetramethylpiperidine-1-oxyl (TEMPO).
35. The system of any one of claims 28-34, wherein the organic peroxide formulation comprises:(a.) the di(t-butylperoxy)diisopropylbenzene in an amount from about 25% to about 60% based on a total weight of the organic peroxide formulation;(b.) the at least one crosslinking coagent in an amount from about 45% to about 74% based on a total weight of the organic peroxide formulation; and(c.) the at least one free radical trap in an amount from about 1% to about 30% based on a total weight of the organic peroxide formulation.
36. The system of any one of claims 28-35, wherein the organic peroxide formulation comprises:(i) di(t-butylperoxy)diisopropylbenzene;(ii) triallyl cyanurate and alpha methyl styrene dimer; and(iii) mono-tert-butylhydroquinone (MTBHQ).
37. The system of any one of claims 28-35, wherein the organic peroxide formulation comprises:(i) di(t-butylperoxy)diisopropylbenzene;(ii) triallyl cyanurate and alpha methyl styrene dimer; and(iii) hydroquinone mono-methyl ether (HQMME) and 4-hydroxy-2,2,6,6- tetram ethylpiperidine- 1 -oxyl (4-OHT).
38. The system of any one of claims 28-35, wherein the organic peroxide formulation comprises:(i) di(t-butylperoxy)diisopropylbenzene;(ii) triallyl cyanurate and alpha methyl styrene dimer; and(iii) di-tert-amylhydroquinone (DTAHQ) and 4-hydroxy-2, 2,6,6- tetramethylpiperidine-1-oxyl (4-OHT).
39. A method of crosslinking a polymer, the method comprising:applying the system of any one of claims 28-38 to the polymer; andcuring using a time-temperature profile such that at least 95 wt% or more of the di(t-butylperoxy)diisopropylbenzene is decomposed during the process.
40. The method of claim 39, wherein the polymer is a polyethylene selected from the group consisting of ultra-high molecular weight polyethylene (UHMWPE), high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE), and linear low density polyethylene (LLDPE).