Extrusion coated aluminum alloy products

The direct extrusion of a polymer melt onto metal strips, with stretching and pressure application, addresses the need for a solvent-free, thin protective layer on aluminum alloy products, improving durability and reducing processing complexity.

WO2026236338A1PCT designated stage Publication Date: 2026-11-12NOVELIS INC(US) +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/US2026/026868
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-05-06
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing metal products, such as aluminum beverage cans, require a protective layer to prevent damage from harsh beverages and maintain beverage quality, while conventional coating methods involve solvent-laden lacquers that complicate processing and result in thick coatings prone to feathering and hairing.

Method used

A process that extrudes a polymer melt directly onto a metal strip, stretching the polymer curtain before application, and applying pressure to achieve a thin, solvent-free polymer coating with enhanced bonding, suitable for aluminum alloy products.

Benefits of technology

The process reduces processing steps, minimizes feathering and hairing, and provides a thin, effective protective layer that enhances the durability and integrity of aluminum alloy products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2026026868_12112026_PF_FP_ABST
    Figure US2026026868_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Described herein are coated aluminum alloy products having a polymer coating on at least one side produced by directly applying an extruded polymer melt to a surface of the aluminum alloy product. The coated aluminum alloy products can be used in container (e.g., beverage container), automotive, transportation, industrial, and electronics applications. The process includes extruding a polymer melt through a die to form a polymer curtain; applying the polymer curtain to a first side of a metal strip (e.g., an aluminum alloy product) as the metal strip is moving in a processing direction to produce a polymer coating on the metal strip; and stretching the polymer curtain before and / or as the polymer curtain is applied to the metal strip as the polymer coating.
Need to check novelty before this filing date? Find Prior Art

Description

Attorney Docket No. 108050-1553660EXTRUSION COATED ALUMINUM ALLOY PRODUCTSCROSS-REFERENCE TO RELATED APPLICATION

[0001] This application claims the benefit of and priority to U.S. Provisional Application No.63 / 802,703, filed May 9, 2025, which is incorporated herein by reference in its entirety for all intents and purposes.FIELD

[0002] The present disclosure relates generally to metalworking and, more specifically, to aluminum alloy products coated with an extruded polymer melt and related processes and products.BACKGROUND

[0003] Certain metal products, such as aluminum beverage cans, may require or otherwise benefit from a protective layer between the metal and its contents. For example, beverage cans often must provide sufficient protection between the metal of the beverage can and the beverage contained therein to avoid damage to the metal from harsh beverages, such as sodas and colas, as well as to avoid undesirable effects to the beverage, such as discoloration or change in taste. Furthermore, metal products may further benefit from a protective layer between the metal and the exterior environment. A protective layer on the exterior of beverage cans, for example, may protect the beverage can from abrasion or other damage during production processes. The protective layer on the exterior of beverage cans may also be necessary or beneficial in applying an exterior design on the beverage can.SUMMARY

[0004] Covered embodiments of the invention are defined by the claims, not this summary. This summary is a high-level overview of various aspects of the invention and introduces some of the concepts that are further described in the Detailed Description section below. This summary is not intended to identify key or essential features of the claimed subject matter, nor is it intended to be used in isolation to determine the scope of the claimed subject matter. The subject matterAttorney Docket No. 108050-1553660should be understood by reference to appropriate portions of the entire specification, any or all drawings and each claim.

[0005] In an aspect, described herein are coated aluminum alloy products produced using a process that includes extruding a polymer melt through a die to form a polymer curtain; applying the polymer curtain to a first side of the metal strip as the metal strip is moving in a processing direction to produce a polymer coating on the metal strip; stretching the polymer curtain before and / or as the polymer curtain is applied to the metal strip as the polymer coating; and applying pressure to the polymer coating to enhance bonding between the polymer coating and the first side of the metal strip, wherein the polymer coating has an average thickness of 25 pm or less.

[0006] In some instances, a line speed of the metal strip is at least 5 times faster than an extrusion speed of the polymer melt. In some instances, a line speed of the metal strip ranges from 10 m / min to 1000 m / min, and / or an extrusion speed of the polymer melt at an orifice of the die is from 200 m / min or less.

[0007] In some instances, a distance from an orifice of the die to a point the polymer curtain contacts the metal strip ranges from 5 mm to 300 mm. In some instances, a width of an orifice of the die ranges from 50 pm to 500 pm. In some instances, the average thickness of the polymer coating is 1.5 pm to 15 pm.

[0008] In some instances, a temperature of the polymer coating ranges from 100°C to 240°C while applying the pressure to the polymer coating. In some instances, the polymer melt comprises a polymer selected from the group consisting of a copolymer of at least one olefin monomer and at least one comonomer having a free carboxylic acid, a polyolefin homopolymer, a polyolefin copolymer, and any combination thereof. In some instances, the polymer melt further comprises a wax. In some instances, the polymer melt further comprises a colorant. In some instances, the polymer of the polymer melt has a glass transition temperature of at least 85°C.

[0009] In some instances, the method may further comprise laminating a polymer film to a second side of the metal strip.

[0010] In an aspect, described herein are coated aluminum alloy products including a can end stock product prepared according to any of the foregoing processes. In some instances, the first side of the metal strip corresponds to an interior-facing side of the can end stock product.Attorney Docket No. 108050-1553660

[0011] In an aspect, described herein are coated aluminum alloy products including a beverage can comprising a body piece, a can end, and a tab on the can end, wherein the can end is formed from a can end stock prepared according to any of the foregoing processes.

[0012] In an aspect, described herein are coated aluminum alloy products including a can end stock product comprising: a metal strip having a first side and a second side; a polymer coating on the first side of the metal strip without an intervening layer therebetween, wherein the polymer coating has an average thickness of 25 pm or less; and a polymer film laminated to the second side of the metal strip, wherein the polymer film has an average thickness of from 5 pm to 150 pm.

[0013] In some instances, the average thickness of the polymer coating is 1.5 pm to 15 pm. In some instances, the polymer coating comprises a polymer selected from the group consisting of a copolymer of at least one olefin monomer and at least one comonomer having a free carboxylic acid, a polyolefin homopolymer, a polyolefin copolymer, and any combination thereof. In some instances, the polymer of the polymer coating has a glass transition temperature of at least 85°C.

[0014] In an aspect, described herein are beverage cans comprising a body piece, a can end, and a tab on the can end, wherein the can end is according to any of the foregoing coated aluminum alloy products.

[0015] Further aspects, objects, and advantages of the invention will become apparent upon consideration of the detailed description that follow.BRIEF DESCRIPTION OF THE FIGURES

[0016] FIG. 1 illustrates a sideview of a non-limiting example system according to at least one embodiment of the present disclosure for extruding a polymer melt to form a polymer coating on a metal strip.

[0017] FIG. 2 is a process flow diagram of a non-limiting example method according to at least one embodiment of the present disclosure for preparing can end stock.DETAILED DESCRIPTION OF THE INVENTION

[0018] Described herein are coated aluminum alloy products having a coating on at least one side produced by directly applying an extruded polymer melt to a surface of the aluminum alloy product. The coated aluminum alloy products can be used in container (including beverage container), automotive, transportation, industrial, and electronics applications, to name a few.Attorney Docket No. 108050-1553660

[0019] A protective coating or film may be applied to a metal strip (e.g., an aluminum alloy product) by laminating a polymer film thereto and / or applying a lacquer thereto. For example, in some conventional processes for preparing can end stock, a metal strip is lacquered on both sides. Because lacquer compositions have a relatively high solvent content, extra processing steps are needed to remove the solvent, especially when the lacquer will be in contact with a food or beverage in the final product. Advantageously, the processes of the present disclosure extrude a polymer melt directly onto a metal strip without the use of solvents, which reduces the processing steps.

[0020] Typically, methods that directly extrude polymer melts onto a surface like a metal strip (e.g., an aluminum alloy product) yield a thick polymer coating. However, in the processes of the present disclosure, the extrusion speed of the polymer melt, the line speed of the metal strip, and the properties of the polymer are tailored so that the extruded polymer melt (also referred to as a polymer curtain herein) is stretched before application on the metal strip. These parameters allow for direct application of a thin polymer coating (e.g., 25 pm thick or less) via an extrusion method.Definitions and Descriptions

[0021] As used herein, the terms “invention,” “the invention,” “this invention” and “the present invention” are intended to refer broadly to all of the subject matter of this patent application and the claims below. Statements containing these terms should be understood not to limit the subject matter described herein or to limit the meaning or scope of the patent claims below.

[0022] In this description, reference is made to alloys identified by aluminum industry designations, such as “series” or “3xxx.” For an understanding of the number designation system most commonly used in naming and identifying aluminum and its alloys, see “International Alloy Designations and Chemical Composition Limits for Wrought Aluminum and Wrought Aluminum Alloys” or “Registration Record of Aluminum Association Alloy Designations and Chemical Compositions Limits for Aluminum Alloys in the Form of Castings and Ingot,” both published by The Aluminum Association.

[0023] As used herein, “feathering” refers to the elongation and delamination of a protective layer (e.g., polymer coating or polymer film) on the metal strip. The extent of feathering is measured by the amount of the protective layer (e.g., polymer coating or polymer film) that extends over the cut aluminum edge as a result of elongation and delamination. Can end stock is especiallyAttorney Docket No. 108050-1553660susceptible to feathering when cutting a disc from the can end stock to produce a can end. In addition, feathering is a risk at breaks in the metal, such as the orifice created when opening a beverage can.

[0024] As used herein, “hairing” refers to the formation of visible hair-like deformations in a protective layer (e.g., polymer coating or polymer film) on the metal strip. Can end stock is especially susceptible to hairing when cutting through the protective layer (e.g., polymer coating or polymer film), such as to create a score line. In some cases, hairing is a result of poor adhesion of the protective layer to the metal strip.

[0025] Reference is made in this application to alloy condition or temper. For an understanding of the alloy temper descriptions most commonly used, see “American National Standards (ANSI) H35 on Alloy and Temper Designation Systems.” An F condition or temper refers to an aluminum alloy as fabricated. An O condition or temper refers to an aluminum alloy after annealing. A TI condition or temper refers to an aluminum alloy cooled from hot working and naturally aged (e.g., at room temperature). A T2 condition or temper refers to an aluminum alloy cooled from hot working, cold worked, and naturally aged. A T3 condition or temper refers to an aluminum alloy solution heat treated, cold worked, and naturally aged. A T4 condition or temper refers to an aluminum alloy solution heat treated and naturally aged. A T5 condition or temper refers to an aluminum alloy cooled from hot working and artificially aged (at elevated temperatures). A T6 condition or temper refers to an aluminum alloy solution heat treated and artificially aged. A T7 condition or temper refers to an aluminum alloy solution heat treated and artificially overaged. A T8x condition or temper refers to an aluminum alloy solution heat treated, cold worked, and artificially aged. A T9 condition or temper refers to an aluminum alloy solution heat treated, artificially aged, and cold worked.

[0026] As used herein, the meaning of “a,” “an,” or “the” includes singular and plural references unless the context clearly dictates otherwise.

[0027] As used herein, the meaning of “room temperature” can include a temperature of from about 15°C to about 30°C, for example about 15°C, about 16°C, about 17°C, about 18°C, about 19°C, about 20°C, about 21°C, about 22°C, about 23°C, about 24°C, about 25°C, about 26°C, about 27°C, about 28°C, about 29°C, or about 30°C.

[0028] All ranges disclosed herein are to be understood to encompass any and all subranges subsumed therein. For example, a stated range of “1 to 10” should be considered to include anyAttorney Docket No. 108050-1553660and all subranges between (and inclusive of) the minimum value of 1 and the maximum value of 10; that is, all subranges beginning with a minimum value of 1 or more, e.g. 1 to 6.1, and ending with a maximum value of 10 or less, e.g., 5.5 to 10.

[0029] As used herein, the terms “invention,” “the invention,” “this invention” and “the present invention” are intended to refer broadly to all of the subject matter of this patent application and the claims below. Statements containing these terms should be understood not to limit the subject matter described herein or to limit the meaning or scope of the patent claims below.Metal Strip

[0030] The present disclosure provides processes and systems for producing a coated metal strip that may be useful in the production of can end stock. More specifically, the processes and systems extrude a polymer melt for direct application to a first side of the metal strip to form a coating thereon. The second side of the metal strip may have polymer film laminated thereon. The composition of the metal strip is not limited. The methods described herein are particularly well suited for, but not limited to, aluminum strips. The polymer film may be applied, for example, to any suitable aluminum alloy, such as a continuous coil of an aluminum alloy. Suitable aluminum alloys include, for example, 3xxx series aluminum alloys, 5xxx series aluminum alloys, and 6xxx series aluminum alloys.

[0031] Non-limiting exemplary 3xxx series aluminum alloys for use as the metal strip can include AA3002, AA3102, AA3003, AA3103, AA3103A, AA3103B, AA3203, AA3403, AA3004, AA3004A, AA3104, AA3204, AA3304, AA3005, AA3OO5A, AA3105, AA3105A, AA3105B, AA3007, AA3107, AA3207, AA3207A, AA3307, AA3009, AA3010, AA3110, AA3011, AA3012, AA3012A, AA3013, AA3014, AA3015, AA3016, AA3017, AA3019, AA3020, AA3021, AA3025, AA3026, AA3030, AA3130, or AA3065.

[0032] Non-limiting exemplary 5xxx series aluminum alloys for use as the metal strip can include AA5182, AA5183, AA5OO5, AA5005A, AA5205, AA53O5, AA5505, AA5605, AA5006, AA5106, AA5010, AA5110, AA5110A, AA5210, AA5310, AA5016, AA5017, AA5018, AA5018A, AA5019, AA5019A, AA5119, AA5119A, AA5021, AA5022, AA5023, AA5024, AA5026, AA5027, AA5028, AA5040, AA5140, AA5041, AA5042, AA5043, AA5049, AA5149, AA5249, AA5349, AA5449, AA5449A, AA5050, AA5050A, AA5050C, AA5150, AA5051, AA5O51A, AA5151, AA5251, AA5251A, AA5351, AA5451, AA5052, AA5252, AA5352,Attorney Docket No. 108050-1553660AA5154, AA5154A, AA5154B, AA5154C, AA5254, AA5354, AA5454, AA5554, AA5654, AA5654A, AA5754, AA5854, AA5954, AA5056, AA5356, AA5356A, AA5456, AA5456A, AA5456B, AA5556, AA5556A, AA5556B, AA5556C, AA5257, AA5457, AA5557, AA5657, AA5O58, AA5059, AA5070, AA5180, AA5180A, AA5082, AA5182, AA5083, AA5183, AA5183A, AA5283, AA5283A, AA5283B, AA5383, AA5483, AA5086, AA5186, AA5087, AA5187, or AA5088.

[0033] Non-limiting exemplary 6xxx series aluminum alloys for use as the metal strip can include AA6101, AA6101A, AA6101B, AA6201, AA6201A, AA6401, AA6501, AA6002, AA6003, AA6103, AA6005, AA6005A, AA6005B, AA6005C, AA6105, AA6205, AA6305, AA6006, AA6106, AA6206, AA6306, AA6008, AA6009, AA6010, AA6110, AA6110A, AA6011, AA6111, AA6012, AA6012A, AA6013, AA6113, AA6014, AA6015, AA6016, AA6016A, AA6116, AA6018, AA6019, AA6020, AA6021, AA6022, AA6023, AA6024, AA6025, AA6026, AA6027, AA6028, AA6031, AA6032, AA6033, AA6040, AA6041, AA6042, AA6043, AA6151, AA6351, AA6351A, AA6451, AA6951, AA6053, AA6055, AA6056, AA6156, AA6060, AA6160, AA6260, AA6360, AA6460, AA6460B, AA6560, AA6660, AA6061, AA6061A, AA6261, AA6361, AA6162, AA6262, AA6262A, AA6063, AA6063A, AA6463, AA6463A, AA6763, A6963, AA6064, AA6064A, AA6065, AA6066, AA6068, AA6069, AA6070, AA6081, AA6181, AA6181A, AA6082, AA6082A, AA6182, AA6091, or AA6092.

[0034] In some embodiments, the composition of the metal strip is or includes an aluminum alloy designated as AA3104, AA5006, AA5182, or a combination thereof.

[0035] While aluminum alloy products are described in the disclosure, the methods and products apply to any metal strip. In some embodiments, the metal strip is aluminum, an aluminum alloy, magnesium, a magnesium-based material, titanium, a titanium-based material, copper, a copperbased material, steel, a steel-based material, bronze, a bronze-based material, brass, a brass-based material, a composite, a sheet used in composites, or any other suitable metal or combination of materials. The product may include monolithic materials, as well as non-monolithic materials such as roll-bonded materials, clad materials, composite materials, or various other materials. In some examples, the metal article is a metal coil, a metal strip, a metal plate, a metal sheet, a metal billet, a metal ingot, or the like.Attorney Docket No. 108050-1553660

[0036] The metal strip can be prepared from an alloy of any suitable temper. In certain examples, the alloys can be used in F, O, T3, T4, T6, or T8X tempers. The alloys can be produced by direct chill casting (including direct chill co-casting) or semi-continuous casting, continuous casting (including, for example, by use of a twin belt caster, a twin roll caster, a block caster, or any other continuous caster), electromagnetic casting, hot top casting, or any other casting method.Polymer Melt and Coating Process

[0037] The processes described herein, and products (e.g., can end stock) produced therefrom, include extruding a polymer melt to form a polymer coating on the metal strip. In particular, the processes of the present disclosure include extruding a polymer melt into a polymer curtain that is applied to a side (e g., a first side) of the metal strip to form the polymer coating thereon. The first side of the metal strip with the polymer coating thereon may, for example, correspond to an interior-facing side of a can end formed from the metal strip. Thus, the polymer coating forms a portion of the product side of the can end stock. As discussed in more detail below, a second side of the metal strip may have a polymer film laminated thereon before or after application of the polymer coating, which may be particularly useful in can end stock applications.

[0038] The use of a polymer coating may beneficially be thinner than lacquered coatings. Further, the polymer melt may beneficially be solvent free, thereby reducing the number of processing steps as compared to a lacquered coating.

[0039] The polymer melt and, consequently, the polymer coating are not particularly limited and may comprise any polymer suitable for the desired use (e.g., a can end stock for a beverage can). Such polymers may be a copolymer of at least one olefin monomer and at least one comonomer having a free carboxylic acid. The polymer units derived from the olefin monomer may be from 2 wt. % to 99 wt. %, e.g., from 10 wt. % to 95 wt. %, from 20 wt. % to 80 wt.%, from 25 wt. % to 60 wt.%, from 30 wt. % to 60 wt.%, 2 wt. %, 3 wt. %, 4 wt. %, 5 wt. %, 6 wt. %, 7 wt. %, 8 wt. %, 9 wt. %, 10 wt. %, 11 wt. %, 12 wt. %, 13 wt. %, 14 wt. %, 15 wt. %, 16 wt. %, 17 wt. %, 18 wt. %, 19 wt. %, 20 wt. %, 21 wt. %, 22 wt. %, 23 wt. %, 24 wt. %, 25 wt. %, 30 wt. %, 35 wt. %, 40 wt. %, 45 wt. %, 50 wt. %, 55 wt. %, 60 wt. %, 65 wt. %, 70 wt. %, 75 wt. %, 80 wt. %, 85 wt. %, 90 wt. %, 95 wt. %, or 99 wt. %, based on a total weight of the polymer. The polymer units derived from the at least one comonomer having a free carboxylic acid may be from 1 wt. % to 40 wt. %, e.g., from 2 wt. % to 30 wt. %, from 3 wt. % to 25 wt.%, 1 wt. %, 2 wt. %,Attorney Docket No. 108050-15536603 wt. %, 4 wt. %, 5 wt. %, 6 wt. %, 7 wt. %, 8 wt. %, 9 wt. %, 10 wt. %, 11 wt. %, 12 wt. %, 13 wt. %, 14 wt. %, 15 wt. %, 16 wt. %, 17 wt. %, 18 wt. %, 19 wt. %, 20 wt. %, 21 wt. %, 22 wt. %, 23 wt. %, 24 wt. %, 25 wt. %, 30 wt. %, 35 wt. %, or 40 wt. %, based on a total weight of the polymer. The balance of the polymer may be the at least one comonomer having a free carboxylic acid.

[0040] Examples of olefin monomers may include, but are not limited to, propylene, 1 -butene, 1 -pentene, 1 -hexene, 1 -heptene, 1 -octene, 1 -nonene, 1 -decene, 1 -undecene, 1 -dodecene, 1-tri decene, 1 -tetradecene, 1 -pentadecene, 1- hexadecene, 1 -heptadecene, 1 -octadecene, 1-nonadecene, 1-eicosene, 3-methyl-l -butene, 3-methyl- 1 -pentene, 3 -ethyl- 1 -pentene, 4-methy-l-1 -pentene, 4-methyl-l -hexene, 4,4-dimethyl-l -hexene, 4,4-dimethyl-l -pentene, 4-ethyl-l -hexene, 3 -ethyl- 1 -hexene, 9-methyl-l -decene, 11 -methyl- 1 -dodecene, 12-ethyl-l -tetradecene, the like, and any combination thereof. Examples of comonomers having a free carboxylic acid may include, but are not limited to, unsaturated carboxylic acids or anhydrides thereof and vinyl carboxylates, specifically, unsaturated carboxylic acids or anhydrides thereof, particularly selected from the group consisting of acrylic acid, methacrylic acid, and maleic acid, the like, and any combination thereof.

[0041] Examples of copolymers of at least one olefin monomer and at least one comonomer having a free carboxylic acid may include, but are not limited to, ethylene-acrylic acid (E-AA) and ethylene-methacrylic acid (E-MAA) (e.g., PRIMACOR™ available from Dow (Midland, MI), NUCREL™, available from E.L DuPont de Nemours (Wilmington, DE), and ESCOR™ available from ExxonMobil Chemical Company (Houston, TX)), low / medium / high density ethylene / acrylic acid / acrylate copolymers, ethylene / butyl / acrylate copolymers (e.g., LUCALEN™ available from Lyondellbasell (Houston, TX)), maleic acid anhydride modified low-crystalline metallocene propylene-ethylene copolymers (e.g., LICOCENE™ available from Clariant (Muttenz, Switzerland)), ethylene terpolymers with reactive functions such as maleic anhydride or epoxide (glycidyl methacrylate) (e.g., LOTADER™ and OREVAC™ available from SK Functional Polymers (Courbevoie, Ile-de-France, France)).

[0042] In some instances, the polymer melt and, consequently, the polymer coating may include a blend of polymers. For example, one or more of the foregoing copolymers of at least one olefin monomer and at least one comonomer having a free carboxylic acid may be blended with one or more polyolefin homopolymers, one or more polyolefin copolymers, the like, or anyAttorney Docket No. 108050-1553660combination thereof. Polyolefin homopolymers may be a polymer produced from one of the olefin monomers described herein. Polyolefin copolymers may be a polymer produced from two or more of the olefin monomers described herein. Examples of polyolefin homopolymers and copolymers may include, but are not limited to, low density polyethylene (LDPE) homopolymers or copolymers, linear low density polyethylene (LLDPE) homopolymers and copolymers, medium density polyethylene (MDPE) homopolymers and copolymers, high density polyethylene (HDPE) homopolymers and copolymers, high molecular weight polyethylene (PE-HMW) homopolymers and copolymers, ultra-high molecular weight polyethylene (PE-UHMW) homopolymers, and polypropylene homopolymers and copolymers, the like, and any combination thereof. Commercially available polyolefin homopolymers and copolymers may include, but are not limited to, HOSTALEN™ from Lyondellbasell, LUPOLEN™ from Lyondellbasell, ALATHON™ from Lyondellbasell, DYNEEMA™ available from Avient Corporation (Avon Lake, OH), POLYTHEN™, SPECTRA™, TROLEN™ and VESTOLEN™.the like, and any combination thereof.

[0043] When blended with another polymer, the copolymers of at least one olefin monomer and at least one comonomer having a free carboxylic acid may be present in the polymer melt or polymer coating in an amount from 1 wt. % to 98 wt. %, e.g., from 3 wt. % to 90 wt. %, from 5 wt. % to 80 wt.%, from 7 wt. % to 70 wt.%, from 10 wt. % to 65 wt.%, 1 wt. %, 2 wt. %, 3 wt. %, 4 wt. %, 5 wt. %, 6 wt. %, 7 wt. %, 8 wt. %, 9 wt. %, 10 wt. %, 11 wt. %, 12 wt. %, 13 wt. %, 14 wt. %, 15 wt. %, 16 wt. %, 17 wt. %, 18 wt. %, 19 wt. %, 20 wt. %, 21 wt. %, 22 wt. %, 23 wt. %, 24 wt. %, 25 wt. %, 30 wt. %, 35 wt. %, 40 wt. %, 45 wt. %, 50 wt. %, 55 wt. %, 60 wt. %, 65 wt. %, 70 wt. %, 75 wt. %, 80 wt. %, 85 wt. %, 90 wt. %, 95 wt. %, or 98 wt. %, based on a total weight of the polymer melt or polymer coating. When included in the polymer melt or polymer coating, the polyolefin homopolymers and the polyolefin copolymers, cumulatively, may be present in the polymer melt or polymer coating from 1 wt. % to 98 wt. %, e.g., from 3 wt. % to 90 wt. %, from 5 wt. % to 80 wt.%, from 7 wt. % to 70 wt.%, from 10 wt. % to 65 wt.%, 1 wt. %, 2 wt. %, 3 wt. %, 4 wt. %, 5 wt. %, 6 wt. %, 7 wt. %, 8 wt. %, 9 wt. %, 10 wt. %, 11 wt. %, 12 wt. %, 13 wt. %, 14 wt. %, 15 wt. %, 16 wt. %, 17 wt. %, 18 wt. %, 19 wt. %, 20 wt. %, 21 wt. %, 22 wt. %, 23 wt. %, 24 wt. %, 25 wt. %, 30 wt. %, 35 wt. %, 40 wt. %, 45 wt. %, 50 wt. %, 55 wt. %, 60 wt. %, 65 wt. %, 70 wt. %, 75 wt. %, 80 wt. %, 85 wt. %, 90 wt. %, 95 wt. %, or 98 wt. %, based on a total weight of the polymer melt or polymer coating.Attorney Docket No. 108050-1553660

[0044] The polymer of the polymer melt and polymer coating may be tailored to provide desired properties including, for example, melt temperature, stretching, strength, the like, and any combination thereof.

[0045] The polymer may have a glass transition temperature (Tg) of at least about 85°C, at least about 90°C, at least about 100°C, at least about 120°C, at least about 130°C, from about 85°C to about 250°C, from about 85°C to about 225°C, from about 85°C to about 200°C, from about 100°C to about 200°C, or from about 120°C to about 200°C. The glass transition temperature is measured using differential scanning calorimetry according to ASTM D3418 with a ramp rate of 10 °C / min.

[0046] Physical characteristics of the polymer composition, such as melt viscosity, rheology, tensile strength, surface hardness, coefficient of friction, wear resistance, and crystallinity, may be further adapted and modified by incorporation of one or more additional components, examples of which include, without limitation, additives selected from the group consisting of additional polymers, tackifiers, antistatic agents, slip / mould release agents, waxes, stabilizers, antioxidants, plasticizers, nucleating agents, thixotroping agents, pigments and colorants, dyestuffs, fluorescing agents and fillers, including nanofillers. Typically, these additives may be present at less than 5 wt. % each, more preferably less than 2 wt. %, even more preferably less than 0.5 wt. % each, relative to the total weight of the polymer composition.

[0047] For example, the polymer melt and, consequently, the polymer coating may include one or more waxes (e.g., paraffin waxes, microcrystalline waxes, polyethylene waxes, polypropylene waxes, by-product polyethylene waxes, Fischer-Tropsch waxes, oxidized Fischer-Tropsch waxes and functionalized waxes such as hydroxy stearamide waxes and fatty amide waxes) or other additives. Said additives may be useful for tailoring properties like lubricity, melt temperature, and the like of the polymer melt.

[0048] In another example, the polymer melt and, consequently, the polymer coating may include a colorant. The colorant used in the polymer melt is not particularly limited. Suitable colorants include, for example, titanium dioxide and carbon black.

[0049] In yet another example, the polymer melt and, consequently, the polymer coating may be substantially-free (i.e., contain less than 0.01 wt. %) of fluorinated compounds (e.g., per- and polyfluoroalkyl substances) and / or bisphenol-A (BPA). The polymer melt and, consequently, the polymer coating may be devoid of fluorinated compounds and BPA. In other words, in some cases,Attorney Docket No. 108050-1553660the polymer coating may contain no fluorinated compounds (i.e., 0 wt. %) and / or no BPA (i.e., 0 wt. %).

[0050] In another example, the polymer melt and, consequently, the polymer coating may include a polyorganosiloxane, which may improve wear resistance of the resultant coating, particularly silanol-terminated polydialkylsiloxanes as well as end-capped polyorganosiloxanes.

[0051] In yet another example, the polymer melt and, consequently, the polymer coating may include stabilizers and / or antioxidants, which may be added to protect the polymer composition from degradation caused by reaction with oxygen induced by such things as heat or light. High molecular weight hindered phenols and multifunctional phenols such as sulfur and phosphorous-containing phenol may be useful as stabilizers and / or antioxidants.

[0052] FIG. 1 illustrates a sideview of a non-limiting example system for extruding a polymer melt 108 to form a polymer coating 112 on a metal strip 100. Because the polymer melt 108 is extruded directly onto the metal strip 100, there is no intervening layer between the polymer coating 112 and the metal strip 100.

[0053] The metal strip 100 may then be passed through a series of rollers, illustrated as three rollers 102a- 102c, in a processing direction. Between two of the rollers, illustrated as between a first roller 102a and a second roller 102b, a polymer melt 108 is applied to a first surface 101 of the metal strip 100. More specifically, the polymer melt 108 is extruded through a die 104 having an orifice 106. Upon extrusion through the orifice 106, the polymer melt 108 forms a polymer curtain 110 that contacts the first surface 101 of the metal strip 100 to form the polymer coating 112 on the metal strip 100. The line speed of the metal strip 100 and extrusion speed (or extrusion rate) of the polymer curtain 110 are each set so that the polymer curtain 110 is stretched in the processing direction before and / or as the polymer curtain 110 is applied to the metal strip 100 to form the polymer coating 112 thereon. The next roller, illustrated as the second roller 102b, may apply pressure to the polymer coating 112 to enhance bonding between the polymer coating 112 and the first surface 101 of the metal strip 100. The polymer coating 112 at application before the second roller 102b compared to after the second roller 102b may be substantially the same thickness (i.e., each thickness being within 0.5 pm of each other). In other words, little or no thickness reduction of the polymer coating results from the pressure application by the second roller 102b.Attorney Docket No. 108050-1553660

[0054] The orifice 106 of the die 104 may have a length dimension and a width dimension. The length dimension is perpendicular to the processing direction and along a width of the metal strip 100 (i.e., extending through the plane of the sideview illustrated in FIG. 1). The length of the orifice 106 of the die 104 may be any length that is sufficient to cover the desired amount of the width of the metal strip 100.

[0055] The width of the orifice 106 of the die 104 is the dimension of the opening in the processing direction. In some embodiments, the orifice 106 of the die 104 has an average width of from 50 pm to 500 pm, e.g., from 50 pm to 450 pm, from 50 pm to 400 pm, from 50 pm to 350 pm, from 50 pm to 300 pm, from 100 pm to 500 pm, from 100 pm to 450 pm, from 100 pm to 400 pm, from 100 pm to 350 pm, from 100 pm to 300 pm, from 150 pm to 500 pm, from 150 pm to 450 pm, from 150 pm to 400 pm, from 150 pm to 350 pm, from 150 pm to 300 pm, from 200 pm to 500 pm, from 200 pm to 450 pm, from 200 pm to 400 pm, from 200 pm to 350 pm, from 200 pm to 300 pm, from 250 pm to 500 pm, from 250 pm to 450 pm, from 250 pm to 400 pm, from 250 pm to 350 pm, from 250 pm to 300 pm, from 300 pm to 500 pm, from 300 pm to 450 pm, from 300 pm to 400 pm, or from 300 pm to 350 pm. Examples of suitable average widths of the orifice 106 of the die 104 include 50 pm, 75 pm, 100 pm, 125 pm, 150 pm, 175 pm, 200 pm, 225 pm, 250 pm, 275 pm, 300 pm, 325 pm, 350 pm, 375 pm, 400 pm, 425 pm, 450 pm, 475 pm, 500 pm, and any width therebetween.

[0056] In some embodiments, the distance from the orifice 106 to a point where the polymer curtain contacts the metal strip 100 may range from 5 mm to 300 mm, e.g., from 5 mm to 250 mm, from 5 mm to 200 mm, from 5 mm to 100 mm, from 5 mm to 50 mm, from 25 mm to 300 mm, from 25 mm to 250 mm, from 25 mm to 200 mm, from 25 mm to 150 mm, from 25 mm to 100 mm, from 100 mm to 300 mm, from 100 mm to 250 mm, from 100 mm to 200 mm, from 150 mm to 300 mm, from 150 mm to 250 mm, from 150 mm to 200 mm, from 200 mm to 300 mm, from 200 mm to 250 mm, or from 250 mm to 300 mm. Examples of suitable distances from the orifice 106 to where the polymer curtain contacts the metal strip 100 include 5 mm, 25 mm, 50 mm, 75 mm, 100 mm, 125 mm, 150 mm, 175 mm, 200 mm, 225 mm, 250 mm, 275 mm, 300 mm, , and any distance therebetween.

[0057] In some embodiments, the metal strip 100 may be preheated to a temperature ranging from 70°C to 90°C, e.g., from 70°C to 80°C, from 75°C to 85°C, or from 80°C to 90°C. ExamplesAttorney Docket No. 108050-1553660of suitable temperatures include 70°C, 75°C, 80°C, 85°C, 90°C, and any temperature therebetween.

[0058] The temperature of the polymer melt 108 at the orifice 106 may range from 100°C to 240°C, e.g., from 100°C to 220°C, from 100°C to 200°C, from 100°C to 180°C, from 100°C to 160°C, from 100°C to 140°C, from 120°C to 240°C, from 120°C to 220°C, from 120°C to 200°C, from 120°C to 180°C, from 120°C to 160°C, from 140°C to 200°C, from 140°C to 180°C, from 160°C to 240°C, from 160°C to 220°C, or from 160°C to 200°C. Examples of suitable temperatures include 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 190°C, 195°C, 200°C, 205°C, 210°C, 215°C, 220°C, 225°C, 230°C, 235°C, 240°C, and any temperature therebetween.

[0059] The temperature of the polymer coating 112 while the roller (illustrated as roller 102b) applies the pressure to the polymer coating 112 should be high enough to maintain pliability in the coating for improved bonding but low enough to maintain sufficient solidification of the polymer so that the thickness of the coating is not substantially changed. The temperature of the polymer coating 112 during pressure application may range from 50°C to 240°C, e.g., from 50°C to 220°C, from 50°C to 200°C, from 50°C to 150°C, from 50°C to 130°C, from 50°C to 110°C, from 50°C to 90°C, from 70°C to 240°C, from 70°C to 220°C, from 70°C to 200°C, from 70°C to 150°C, from 70°C to 130°C, from 70°C to 110°C, from 70°C to 90°C, from 90°C to 150°C, from 90°C to 130°C, or from 90°C to 110°C. Examples of suitable temperatures include 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 190°C, 195°C, 200°C, 205°C, 210°C, 215°C, 220°C, 225°C, 230°C, 235°C, 240°C, and any temperature therebetween.

[0060] A line speed of the metal strip 100 is the speed at which the metal strip 100 is moving in the processing direction when the polymer curtain 110 contacts the metal strip 100. In some embodiments, the line speed of the metal strip 100 may range from 10 meters per minute (m / min) to 1000 m / min, e.g., from 10 m / min to 50 m / min, from 20 m / min to 75 m / min, from 50 m / min to 250 m / min, from 75 m / min to 300 m / min, from 150 m / min to 400 m / min, from 250 m / min to 550 m / min, from 350 m / min to 650 m / min, from 450 m / min to 750 m / min, from 550 m / min to 850 m / min, or from 650 m / min to 1000 m / min. Examples of suitable line speeds of the metal strip 100 include 10 m / min, 25 m / min, 50 m / min, 75 m / min, 100 m / min, 150 m / min, 200 m / min, 250 m / min,Attorney Docket No. 108050-1553660300 m / min, 350 m / min, 400 m / min, 450 m / min, 500 m / min, 550 m / min, 600 m / min, 650 m / min, 700 m / min, 750 m / min, 800 m / min, 850 m / min, 900 m / min, 950 m / min, 1000 m / min, and any line speed therebetween.

[0061] An extrusion speed of the polymer melt 108 is the speed at which the polymer curtain 110 is moving as the polymer curtain 110 leaves the orifice 106 of the die 104. In some embodiments, the extrusion speed of the metal strip may be 200 m / min or less, e.g., 150 m / min or less, 100 m / min or less, 50 m / min or less, from 1 m / min to 200 m / min, from 1 m / min to 150 m / min, from 1 m / min to 100 m / min, from 1 m / min to 50 m / min, from 5 m / min to 50 m / min, from 25 m / min to 75 m / min, from 50 m / min to 100 m / min, from 75 m / min to 125 m / min, from 100 m / min to 150 m / min, or from 125 m / min to 200 m / min. Examples of suitable line speeds of the metal strip 100 include 1 m / min, 5 m / min, 10 m / min, 15 m / min, 20 m / min, 25 m / min, 30 m / min, 35 m / min, 40 m / min, 45 m / min, 50 m / min, 60 m / min, 70 m / min, 80 m / min, 90 m / min, 100 m / min, 125 m / min, 150 m / min, 175 m / min, 200 m / min, and any extrusion speed therebetween.

[0062] In some embodiments, the line speed of the metal strip 100 is at least 5 times faster than an extrusion speed of the polymer melt 108, e.g., at least 10 times faster, at least 15 times faster, 5 times faster to 50 times faster, 5 times faster to 40 times faster, 5 times faster to 30 times faster, 10 times faster to 50 times faster, 10 times faster to 40 times faster, 10 times faster to 30 times faster, 15 times faster to 50 times faster, 15 times faster to 40 times faster, or 5 times faster to 30 times faster. Examples of a suitable number of times faster (of the line speed as compared to the extrusion speed of the polymer melt) include 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, and any number therebetween.

[0063] In some embodiments, the polymer coating has an average thickness of 25 pm or less, e.g., from 1.5 pm to 25 pm, from 1.5 pm to 20 pm, from 1.5 pm to 15 pm, from 1.5 pm to 10 pm, from 1.5 pm to 5 pm, from 3 pm to 25 pm, from 3 pm to 20 pm, from 3 pm to 15 pm, from 3 pm to 10 pm, from 5 pm to 25 pm, from 5 pm to 20 pm, from 5 pm to 15 pm, from 5 pm to 10 pm, from 10 pm to 25 pm, from 10 pm to 20 pm, or from 10 pm to 15 pm. Examples of suitable average thicknesses of the polymer coating include 1.5 pm, 2 pm, 3 pm, 4 pm, 5 pm, 6 pm, 7 pm, 8 pm, 9 pm, 10 pm, 11 pm, 12 pm, 13 pm, 14 pm, 15 pm, 16 pm, 17 pm, 18 pm, 19 pm, 20 pm, 21 pm, 22 pm, 23 pm, 24 pm, 25 pm, and any thickness therebetween.Attorney Docket No. 108050-1553660Polymer Film and Laminating Process

[0064] The processes described herein, and products (e.g., can end stock) produced therefrom, may optionally include laminating a polymer film to the metal strip. In particular, the processes of the present disclosure may include laminating the polymer film on a side (e.g., the second side) of the metal strip. The second side may correspond to an exterior-facing side of a can end formed from the metal strip. Thus, the polymer film forms a portion of the public side of the can end stock.

[0065] The use of a polymer film on an exterior-facing side of a can end (e.g., as opposed to a lacquer) may beneficially improve the quality of the can end product. In particular, the polymer film imparts greater resistance to abrasion relative to conventional can end products. Furthermore, the polymer films described herein, in particular the polymer films processed according to the production methods described herein, exhibit reduced feathering and / or hairing.

[0066] The polymer film is not particularly limited and may be or include any polymer suitable for the desired use of the can end stock (e.g., as a beverage can). Suitable polymers for the polymer film include, for example, polyethylene, polypropylene, and polyethylene terephthalate (PET). In some cases, the polymer film laminated to the metal strip is a biaxially oriented polymer, such as a biaxially-oriented polyethylene terephthalate (BoPET) film.

[0067] In some embodiments, the polymer film further includes a colorant, such as a dye or a colorant. Said another way, the polymer film may be a colored polymer film (e.g., a colored PET film). As further detailed in the examples below, the use of colored polymer films has been found to beneficially improve the quality of the can end product. Relative to colorless polymer films, the colored films have been found to exhibit a low tendency for hairing. Without being bound by theory, it is believed that the presence of colorant particles in the film affect the composition of the films to facilitate smooth breaking of the film (e g., at the creation of the orifice when opening a beverage can).

[0068] The colorant used in the colored polymer film is not particularly limited. Suitable colorants include, for example, titanium dioxide (e.g., to produce a white polymer film) and carbon black (e.g., to produce a black polymer film).

[0069] In some embodiments, the polymer film has an average thickness of from 5 pm to 150 pm, e.g., from 5 pm to 125 pm, from 5 pm to 100 pm, from 5 pm to 75 pm, from 5 pm to 50 pm, from 5 pm to 25 pm, from 6 pm to 150 pm, from 6 pm to 125 pm, from 6 pm to 100 pm, from 6 pm to 75 pm, from 6 pm to 50 pm, from 6 pm to 25 pm, from 8 pm to 150 pm, from 8 pm to 125Attorney Docket No. 108050-1553660pm, from 8 pm to 100 pm, from 8 pm to 75 pm, from 8 pm to 50 pm, from 8 pm to 25 pm, from 10 pm to 150 pm, from 10 pm to 125 pm, from 10 pm to 100 pm, from 10 pm to 75 pm, from 10 pm to 50 pm, from 10 pm to 25 pm, from 12 pm to 150 pm, from 12 pm to 125 pm, from 12 pm to 100 pm, from 12 pm to 75 pm, from 12 pm to 50 pm, or from 12 pm to 25 pm. Examples of suitable average thicknesses of the polymer film include 10 pm, 15 pm, 20 pm, 25 pm, 30 pm, 35 pm, 40 pm, 45 pm, 50 pm, 55 pm, 60 pm, 65 pm, 70 pm, 75 pm, 80 pm, 85 pm, 90 pm, 95 pm, 100 pm, 105 pm, 110 pm, 115 pm, 120 pm, 125 pm, 130 pm, 135 pm, 140 pm, 145 pm, 150 pm, and any thickness therebetween.

[0070] In some embodiments, the process of the present disclosure includes laminating multiple layers of polymer film on the metal strip. In these embodiments, each layer of polymer film may independently be a polymer film as described above. In some cases, multiple layers of polymer film are laminated on the metal strip, and each of the layers are identical (e.g., in terms of composition, colorant, and / or thickness). In some cases, multiple layers of polymer film are laminated on the metal strip, and one or more of the layers are not identical (e.g., in terms of composition, colorant, and / or thickness).

[0071] Adhesion Coating

[0072] In some embodiments, a can end stock produced according to the present disclosure comprises an adhesion coating in conjunction with the laminated polymer film. In particular, an adhesion coating may be applied to the metal strip, and the polymer film may be laminated thereon. The adhesion coating beneficially fixes the polymer film to the metal strip.

[0073] As illustrated in the below examples, the adhesion coating can provide improved feathering performance. In particular, adhesion of the polymer film to the metal strip can be controlled (e.g., improved) by the selection of an appropriate adhesion coating and by controlling process parameters (such as the annealing temperature, as described below).

[0074] In some embodiments, the adhesion coating is a pretreatment applied to the metal strip, e.g., a pretreatment suited to the metal strip. Commercial examples of suitable pretreatments that can be employed as the adhesion coating include Addibond 712-CP 30 from Solvay (Brussels, Belgium).

[0075] Wax Coating

[0076] In some embodiments, a can end stock produced according to the present disclosure includes a wax coating in conjunction with the laminated polymer film and / or the adhesion coating.Attorney Docket No. 108050-1553660In some cases, for example, a wax coating may be applied to the external-facing surface of the polymer film. The wax coating beneficially improves the appearance of the can end stock. In particular, a wax coating according to the present disclosure exhibits a homogenous appearance with minimal or no streaking in appearance. In addition, the wax coating acts as lubricant to reduce friction forces on the surface. Lubrication may be necessary to ensure proper function of the machinery used in the production of the can end stock.

[0077] The wax coating may comprise a solution of wax, e.g., carnauba wax. A commercial example of suitable wax products that can be employed as the wax coating includes LUBA-print 965-A from Miinzing (Abstatt, Germany). In some embodiments, the wax coating includes a dilution of carnauba wax in water. For example, the wax coating may include a dilution of carnauba wax (e g., LUBA-print 965-A) at a volume ratio of from 1:2 to 1:50 (e.g., 1:5, 1:6, 1:8, 1:10, 1:12, 1:14, 1:16, 1:18, or 1:20) with water. Diluting the wax coating ensures that the wax coating can be pumped into a nip during commercial application and mitigate foaming, which has been found to dry and to lead to solid carnauba particles on the surface of the can end stock.

[0078] In some embodiments, the wax coating has an average thickness of from 5 mg / m2to 150 mg / m2, e.g., from 5 mg / m2to 120 mg / m2, from 5 mg / m2to 115 mg / m2, from 5 mg / m2to 110 mg / m2, from 5 mg / m2to 105 mg / m2, from 5 mg / m2to 100 mg / m2, from 6 mg / m2to 150 mg / m2, from 6 mg / m2to 120 mg / m2, from 6 mg / m2to 115 mg / m2, from 6 mg / m2to 110 mg / m2, from 6 mg / m2to 105 mg / m2, from 6 mg / m2to 100 mg / m2, from 7 mg / m2to 150 mg / m2, from 7 mg / m2to 120 mg / m2, from 7 mg / m2to 115 mg / m2, from 7 mg / m2to 110 mg / m2, from 7 mg / m2to 105 mg / m2, from 7 mg / m2to 100 mg / m2, from 8 mg / m2to 150 mg / m2, from 8 mg / m2to 120 mg / m2, from 8 mg / m2to 115 mg / m2, from 8 mg / m2to 110 mg / m2, from 8 mg / m2to 105 mg / m2, from 8 mg / m2to 100 mg / m2, from 9 mg / m2to 150 mg / m2, from 9 mg / m2to 120 mg / m2, from 9 mg / m2to 115 mg / m2, from 9 mg / m2to 110 mg / m2, from 9 mg / m2to 105 mg / m2, from 9 mg / m2to 100 mg / m2, from 10 mg / m2to 150 mg / m2, from 10 mg / m2to 120 mg / m2, from 10 mg / m2to 115 mg / m2, from 10 mg / m2to 110 mg / m2, from 10 mg / m2to 105 mg / m2, or from 10 mg / m2to 100 mg / m2.Process and System for Preparing a Can End Stock

[0079] In some aspects, the present disclosure provides processes for preparing can end stock. The processes described herein advantageously produce can end stock having a polymer coatingAttorney Docket No. 108050-1553660on a first side and a polymer film laminated on a second side, where each side has low feathering and low hairing.

[0080] In the processes of the present disclosure, the coating process may occur before the laminating process or vice versa. In some instances, an annealing step may be included at any point after laminating. For example, the metal strip may be coated, laminated, and then annealed. In another example, the metal strip may be laminated, annealed, and then coated. In yet another example, the metal strip may be laminated, coated, and then annealed. In some embodiments, the annealing temperature is a temperature from 175°C to 300°C, e.g., from 175°C to 290°C, from 175°C to 280°C, from 175°C to 270°C, from 175°C to 260°C, from 175°C to 250°C, from 185°C to 300°C, from 185°C to 290°C, from 185°C to 280°C, from 185°C to 270°C, from 185°C to 260°C, from 185°C to 250°C, from 195°C to 300°C, from 195°C to 290°C, from 195°C to 280°C, from 195°C to 270°C, from 195°C to 260°C, from 195°C to 250°C, from 205°C to 300°C, from 205°C to 290°C, from 205°C to 280°C, from 205°C to 270°C, from 205°C to 260°C, from 205°C to 250°C, from 215°C to 300°C, from 215°C to 290°C, from 215°C to 280°C, from 215°C to 270°C, from 215°C to 260°C, from 215°C to 250°C, from 225°C to 300°C, from 225°C to 290°C, from 225°C to 280°C, from 225°C to 270°C, from 225°C to 260°C, or from 225°C to 250°C.

[0081] The duration within an annealing oven can be based on oven length and the speed of the metal strip. In some cases, the duration can be within the range of approximately 2 seconds to approximately 30 seconds, approximately 9 seconds to approximately 15 seconds, approximately 10 seconds to approximately 14 seconds, or approximately 12 seconds. In some cases, the duration can be adjusted (e.g., by adjusting the metal strip speed) as necessary to compensate for changes in the temperature within the annealing oven.

[0082] FIG. 2 is a process flow diagram of a non-limiting example method of the present disclosure for preparing can end stock. A polymer coating 204 may be applied to a first side of a metal strip 200 in a coating system 202 (e.g., a coating system of or similar to FIG. 1). A polymer film 208 may then be laminated to a second side of the metal strip 200 in a laminating system 206. The metal strip 200 having the polymer coating 204 and polymer film 208 thereon may then be annealed in an annealing system 210 to produce the can end stock 212. As discussed above, these systems 202, 206, and 210 may be in a different order.

[0083] Further, the processes for preparing can end stock of the present disclosure may optionally include preheating the metal strip before laminating and / or before coating. In someAttorney Docket No. 108050-1553660embodiments, the pre-heating temperature is a temperature from 175°C to 300°C, e.g., from 175°C to 290°C, from 175°C to 280°C, from 175°C to 270°C, from 175°C to 260°C, from 175°C to 250°C, from 185°C to 300°C, from 185°C to 290°C, from 185°C to 280°C, from 185°C to 270°C, from 185°C to 260°C, from 185°C to 250°C, from 195°C to 300°C, from 195°C to 290°C, from 195°C to 280°C, from 195°C to 270°C, from 195°C to 260°C, from 195°C to 250°C, from 205°C to 300°C, from 205°C to 290°C, from 205°C to 280°C, from 205°C to 270°C, from 205°C to 260°C, from 205°C to 250°C, from 215°C to 300°C, from 215°C to 290 °C, from 215°C to 280°C, from 215°C to 270°C, from 215°C to 260°C, from 215°C to 250°C, from 225°C to 300°C, from 225°C to 290°C, from 225°C to 280°C, from 225°C to 270°C, from 225°C to 260°C, or from 225°C to 250°C.

[0084] In some embodiments, the surface of the metal strip may be degreased (e g., using an acid solution, such as sulfuric acid, hydrofluoric acid, phosphoric acid, or combinations thereof) to clean the surface before applying a polymer coating or polymer fdm to the metal strip.Properties of Can End Stock

[0085] As noted above, the can end stock of the present disclosure, e.g., the can end stock produced according to the described processes, may advantageously exhibit a number of improved properties.

[0086] In some embodiments, the can end stock of the present disclosure exhibits low hairing. As described above, hairing refers to the formation of visible hair-like deformations in a protective layer (e.g., polymer film) on the metal strip, especially at breaks in the metal, such as the orifice created when opening a beverage can. In some aspects, the can end stock may exhibit low or no hairing during the can end making process. For example, during the stamping of a score-line (e.g., in a V-shape), a conventional can end may be particularly susceptible to hairing. The can end stock of the present disclosure, however, exhibits low or no hairing during such a process.

[0087] In some aspects, the can end stock exhibits low or no hairing during opening. For example, when a beverage can is opened, a conventional can end may be particularly susceptible to hairing. The can end stock of the present disclosure, however, may exhibit low or no hairing during such a process.

[0088] In some embodiments, the can end stock of the present disclosure may exhibit reduced feathering. In some cases, for example, the can end stock of the present disclosure may exhibitAttorney Docket No. 108050-1553660improved results on a standard feathering test. As used herein, a standard feathering test can be conducted on a can end and may include immersing a can end in a bath of deionized water at, for example, approximately 75°C for thirty minutes, rinsing the can end in cool deionized water to return the can end to room temperature, and then immediately opening the end tab of the can end. Feathering can be observed and measured on the scored panel or pour hole opening. In some cases, a feathering test can be conducted on a flat sheet of metal, such as a flat sheet of can end stock. In such cases, the feathering test can include immersing the sample in demineralized water at 80°C for forty minutes, after which the sample is allowed to cool down to room temperature and the sample can be cut and a strip of metal can be separated by pulling the strip in a direction away from the cut. In either feathering test, the amount of feathering can be measured, and the can end stock exhibiting a maximum amount of feathering less than 0.7 mm is said to pass the test.

[0089] In some examples, the can end stock described herein passes a standard feathering test. In some embodiments, the can end stock exhibits a maximum amount of feathering of less than 0.7 mm, e.g., less than 0.6, less than 0.5 mm, less than 0.4 mm, less than 0.3 mm, or less than 0.2 mm. This amount of feathering may be located at certain indicative positions along the orifice of the opened can end. The amount of feathering of the film also depends on the cutting, forming, and stamping tool design of the product.

[0090] Reference has been made in detail to various examples of the disclosed subject matter, one or more examples of which were set forth above. Each example was provided by way of explanation of the subject matter, not limitation thereof. In fact, it will be apparent to those skilled in the art that various modifications and variations may be made in the present subject matter without departing from the scope or spirit of the disclosure. For instance, features illustrated or described as part of one embodiment may be used with another embodiment to yield a still further embodiment.

[0091] The following examples will serve to further illustrate the present invention without, at the same time, however, constituting any limitation thereof. On the contrary, it is to be clearly understood that resort may be had to various embodiments, modifications, and equivalents thereof which, after reading the description herein, may suggest themselves to those skilled in the art without departing from the spirit of the invention. During the studies described in the following examples, conventional procedures were followed, unless otherwise stated. Some of the procedures are described below for illustrative purposes.Attorney Docket No. 108050-1553660EXAMPLES

[0092] Can end stock aluminum alloy sheets were coated using methods of the present disclosure and convention methods. More specifically, two curtain coating methods of the present disclosure (Examples 1 and 2) were used to apply a polymer coating on the end stock, and a conventional method (Control) was used to apply a bisphenol A-non-intent (BPAni) polymer spray coating. The coatings were tested as the product side of the can end stock.

[0093] The curtain-coated Examples 1 and 2 (i) were within specification for the metal exposure tests, (ii) were within specification and showed no significant variability in dimensions, (iii) had no venting failures, (iv) had no visible blistering with a diet coke test (inverted 7 day s at 100°F), (v) were within specification for feathering, and (vi) were within specification for adhesion and blush. The Control also performed within specification except that blistering was visible with the diet coke test.ILLUSTRATIVE ASPECTS

[0094] As used below, any reference to a series of aspects (e.g., “Aspects 1-4”) or nonenumerated group of aspects (e.g., “any previous or subsequent aspect”) is to be understood as a reference to each of those aspects disjunctively (e.g., “Aspects 1-4” is to be understood as “Aspects 1, 2, 3, or 4 ”).

[0095] Aspect 1. A process of coating a metal strip, comprising: extruding a polymer melt through a die to form a polymer curtain; applying the polymer curtain to a first side of the metal strip as the metal strip is moving in a processing direction to produce a polymer coating on the metal strip; stretching the polymer curtain before and / or as the polymer curtain is applied to the metal strip as the polymer coating; and applying pressure to the polymer coating to enhance bonding between the polymer coating and the first side of the metal strip, wherein the polymer coating has an average thickness of 25 pm or less.

[0096] Aspect 2. The process of any previous or subsequent aspect, wherein a line speed of the metal strip is at least 5 times faster than an extrusion speed of the polymer melt.

[0097] Aspect 3. The process of any previous or subsequent aspect, wherein a line speed of the metal strip ranges from 10 m / min to 1000 m / min, and wherein an extrusion speed of the polymer melt at an orifice of the die is 200 m / min or less.Attorney Docket No. 108050-1553660

[0098] Aspect 4. The process of any previous or subsequent aspect, wherein a distance from an orifice of the die to a point the polymer curtain contacts the metal strip ranges from 5 mm to 300 mm.

[0099] Aspect 5. The process of any previous or subsequent aspect, wherein a width of an orifice of the die ranges from 50 pm to 500 pm.

[0100] Aspect 6. The process of any previous or subsequent aspect, wherein the average thickness of the polymer coating is 1.5 pm to 15 pm.

[0101] Aspect 7. The process of any previous or subsequent aspect, wherein a temperature of the polymer coating ranges from 100°C to 240°C while applying the pressure to the polymer coating.

[0102] Aspect 8. The process of any previous or subsequent aspect, wherein the polymer melt comprises a polymer selected from the group consisting of a copolymer of at least one olefin monomer and at least one comonomer having a free carboxylic acid, a polyolefin homopolymer, a polyolefin copolymer, and any combination thereof.

[0103] Aspect 9. The process of Aspect 8, wherein the polymer melt further comprises a wax.

[0104] Aspect 10. The process of Aspect 8 or 9, wherein the polymer melt further comprises a colorant.

[0105] Aspect 11. The process of any previous or subsequent aspect, further comprising: laminating a polymer film to a second side of the metal strip.

[0106] Aspect 12. The process of any previous or subsequent aspect, wherein the polymer of the polymer melt has a glass transition temperature of at least 85°C.

[0107] Aspect 13. A can end stock product prepared according to the process of any previous or subsequent aspect.

[0108] Aspect 14. The can end stock product of Aspect 13, wherein the first side of the metal strip corresponds to an interior-facing side of the can end stock product.

[0109] Aspect 15. A beverage can comprising a body piece, a can end, and a tab on the can end, wherein the can end is formed from a can end stock prepared according to the process of any previous or subsequent aspect.

[0110] Aspect 16. A can end stock product comprising: a metal strip having a first side and a second side; a polymer coating on the first side of the metal strip without an intervening layer therebetween, wherein the polymer coating has an average thickness of 25 pm or less; and aAttorney Docket No. 108050-1553660polymer film laminated to the second side of the metal strip, wherein the polymer film has an average thickness of from 5 pm to 150 pm.

[0111] Aspect 17. The can end stock product of Aspect 16, wherein the average thickness of the polymer coating is 1.5 pm to 15 pm.

[0112] Aspect 18. The can end stock product of any previous or subsequent aspect, wherein the polymer coating comprises a polymer selected from the group consisting of a copolymer of at least one olefin monomer and at least one comonomer having a free carboxylic acid, a polyolefin homopolymer, a polyolefin copolymer, and any combination thereof.

[0113] Aspect 19. The can end stock product of any previous or subsequent aspect, wherein the polymer of the polymer coating has a glass transition temperature of at least 85°C.

[0114] Aspect 20. A beverage can comprising a body piece, a can end, and a tab on the can end, wherein the can end is formed from the can end stock according to any previous or subsequent aspect.

[0115] All patents and publications cited herein are incorporated by reference in their entirety. The foregoing description of the embodiments, including illustrated embodiments, has been presented only for the purpose of illustration and description and is not intended to be exhaustive or limiting to the precise forms disclosed. Numerous modifications, adaptations, and uses thereof will be apparent to those skilled in the art.

Claims

Attorney Docket No. 108050-1553660WHAT IS CLAIMED IS:

1. A process of coating a metal strip, comprising:extruding a polymer melt through a die to form a polymer curtain;applying the polymer curtain to a first side of the metal strip as the metal strip is moving in a processing direction to produce a polymer coating on the metal strip;stretching the polymer curtain before and / or as the polymer curtain is applied to the metal strip as the polymer coating; andapplying pressure to the polymer coating to enhance bonding between the polymer coating and the first side of the metal strip, wherein the polymer coating has an average thickness of 25 pm or less.

2. The process of claim 1, wherein a line speed of the metal strip is at least 5 times faster than an extrusion speed of the polymer melt.

3. The process of claim 1 or 2, wherein a line speed of the metal strip ranges from 10 m / min to 1000 m / min, and wherein an extrusion speed of the polymer melt at an orifice of the die is 200 m / min or less.

4. The process of any one of claims 1-3, wherein a distance from an orifice of the die to a point the polymer curtain contacts the metal strip ranges from 5 mm to 300 mm.

5. The process of any one of claims 1-4, wherein a width of an orifice of the die ranges from 50 pm to 500 pm.

6. The process of any one of claims 1-5, wherein the average thickness of the polymer coating is 1.5 pm to 15 pm.

7. The process of any one of claims 1-6, wherein a temperature of the polymer coating ranges from 100°C to 240°C while applying the pressure to the polymer coating.Attorney Docket No. 108050-15536608. The process of any one of claims 1-7, wherein the polymer melt comprises a polymer selected from the group consisting of a copolymer of at least one olefin monomer and at least one comonomer having a free carboxylic acid, a polyolefin homopolymer, a polyolefin copolymer, and any combination thereof.

9. The process of claim 8, wherein the polymer melt further comprises a wax.

10. The process of claim 8, wherein the polymer melt further comprises a colorant.

11. The process of any one of claims 1-10, further comprising:laminating a polymer film to a second side of the metal strip.

12. The process of any one of claims 1-10, wherein the polymer of the polymer melt has a glass transition temperature of at least 85°C.

13. A can end stock product prepared according to the process of any one of claims 1-12.

14. The can end stock product of claim 13, wherein the first side of the metal strip corresponds to an interior-facing side of the can end stock product.

15. A beverage can comprising a body piece, a can end, and a tab on the can end, wherein the can end is formed from a can end stock prepared according to the process of any one of claims 1-12.

16. A can end stock product comprising:a metal strip having a first side and a second side;a polymer coating on the first side of the metal strip without an intervening layer therebetween, wherein the polymer coating has an average thickness of 25 pm or less; anda polymer film laminated to the second side of the metal strip, wherein the polymer film has an average thickness of from 5 pm to 150 pm.Attorney Docket No. 108050-155366017. The can end stock product of claim 16, wherein the average thickness of the polymer coating is 1.5 pm to 15 pm.

18. The can end stock product of any one of claims 16-17, wherein the polymer coating comprises a polymer selected from the group consisting of a copolymer of at least one olefin monomer and at least one comonomer having a free carboxylic acid, a polyolefin homopolymer, a polyolefin copolymer, and any combination thereof.

19. The can end stock product of any one of claims 16-18, wherein the polymer of the polymer coating has a glass transition temperature of at least 85°C.

20. A beverage can comprising a body piece, a can end, and a tab on the can end, wherein the can end is formed from the can end stock according to any one of claims 16-19.