Methods of forming fluorinated vinyl ether compositions and fluorinated vinyl ether compositions formed through the methods

Pyrolyzing fluorinated carboxylic acid metal salts in non-polar aprotic solvents at specific temperatures addresses yield and purity issues in fluorinated vinyl ether production, achieving high yields and purities through minimized byproduct formation.

WO2026236492A1PCT designated stage Publication Date: 2026-11-12KALREZ USA LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/US2026/027106
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-07
Filing Date
2026-05-07
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing methods for producing fluorinated vinyl ether compositions face challenges such as low yield and purity due to clogging, flooding, and significant side reactions in fluidized bed and traditional reactors, particularly when using polar solvents.

Method used

Pyrolyzing fluorinated carboxylic acid metal salts in a non-polar aprotic solvent at temperatures between 100°C to 200°C minimizes byproduct formation, achieving high yield and purity by avoiding proton interactions and side reactions.

Benefits of technology

The method achieves fluorinated vinyl ether compositions with yields of 50% to 80% and purities above 95%, overcoming the limitations of conventional pyrolysis techniques.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2026027106_12112026_PF_FP_ABST
    Figure US2026027106_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Methods of forming fluorinated vinyl ether compositions and fluorinated vinyl ether compositions formed through the methods are provided herein. In an embodiment, a method includes the step of pyrolyzing a fluorinated carboxylic acid metal salt in a reaction mixture comprising a nonpolar aprotic solvent at a temperature of from about 100°C to about 200°C to form a fluorinated vinyl ether. The fluorinated carboxylic acid metal salt has Formula I: ROCF(CF3)CO2M (I). M in Formula I is an alkali or alkaline earth metal. R in Formulas I and II is selected from fluorinated ether, fluorinated nitrile, fluorinated carboxylic acid, fluorinated ester, fluorinated sulfonyl halide, or perfluorinated aryl.
Need to check novelty before this filing date? Find Prior Art

Description

UTILITY PATENT APPLICATIONATTORNEY DOCKET NO. DW0339-WO-PCT (421.0029PC)METHODS OF FORMING FLUORINATED VINYL ETHER COMPOSITIONS AND FLUORINATED VINYL ETHER COMPOSITIONS FORMED THROUGH THE METHODS TECHNICAL FIELD

[0001] The present disclosure generally relates to synthesis of fluorinated vinyl ether compositions. The present disclosure more particularly relates to synthesis of fluorinated vinyl ether compositions by solution phase pyrolysis of a precursor.BACKGROUND

[0002] Fluorinated polymers are used to make various products, including products used in harsh environments. For example, fluorinated polymer materials are often used as seals, binders, or separators in the semiconductor, battery, and oil and gas industries. Some fluorinated polymers, particularly perfluoroelastomers, contain crosslinks formed from cyano-group-containing monomers. The cyano-group-containing monomers are typically formed from fluorinated vinyl ethers as precursors. The fluorinated vinyl ethers are typically formed through a multi-step process that concludes with a pyrolysis step, in which an intermediate is pyrolyzed to form the fluorinated vinyl ether.

[0003] Existing methods of producing fluorinated vinyl ether compositions have shortcomings. For example, pyrolysis is often performed in a fluidized bed reactor in which a vaporized starting product is passed through a packed column of metal carbonate. Performing pyrolysis in the fluidized bed reactor facilitates efficient heat and mass transfer and regulation of residence time. However, the pyrolysis step in the fluidized bed reactor requires very specific process conditions (e.g. high temperature in each zone and rate of feed of the starting material), produces large quantities of byproducts (leading to low yield and low purity of the pyrolyzed product), and often leads to clogging or flooding of the fluidized bed (reducing process efficiency). Operation of pyrolysis in a fluidized bed reactor on a large industrial scale is challenging because of the aforementioned drawbacks and also requires significant capital investment.

[0004] One alternative to regular fluidized bed reactor is to perform pyrolysis in solid phase in a traditional reactor. However, conducting solid phase pyrolysis on an industrial scale is challenging due to processing concerns such as the need to sufficiently mix the solid components. Another known method of performing pyrolysis without the use of the fluidized bed reactor is aUTILITY PATENT APPLICATIONATTORNEY DOCKET NO. DW0339-WO-PCT (421.0029PC)solution phase pyrolysis using traditional reactor. However, solution phase pyrolysis, which traditionally employ polar aprotic solvents has many drawbacks, especially for producing fluorinated vinyl ethers that are higher boilers. Performing solution phase pyrolysis at temperatures high enough to advance the desired reaction and longer reaction time involved can lead to significant side reactions via substitution and thermal disproportionation, resulting in a variety of byproducts (and again leading to low yield and low purity of the pyrolyzed product).

[0005] Accordingly, it is desirable to provide a novel method of forming fluorinated vinyl ether compositions that achieve maximized yields and maximized purity (i.e. minimized byproducts) at the convenience of a traditional reactor while also being capable of implementing on an industrial scale. Furthermore, other desirable features and characteristics of the present disclosure will become apparent from the subsequent detailed description and the appended claims, taken in conjunction with the accompanying drawings and this background.BRIEF SUMMARY

[0006] This summary is provided to introduce a selection of concepts in a simplified form that are further described below in the detailed description. This summary is not intended to identify key features or essential features of the claimed subject matter, nor is it intended to be used as an aid in determining the scope of the claimed subject matter.

[0007] Methods of forming fluorinated vinyl ether compositions and fluorinated vinyl ether compositions formed through the methods are provided herein. In an embodiment, a method includes the step of pyrolyzing a fluorinated carboxylic acid metal salt in a reaction mixture comprising a nonpolar aprotic solvent at a temperature of from about 100°C to about 200°C to form a fluorinated vinyl ether. The fluorinated carboxylic acid metal salt has Formula I:ROCF(CF3)CO2M (I). M in Formula I is an alkali or alkaline earth metal. R in Formulas I and II is selected from fluorinated ether, fluorinated nitrile, fluorinated carboxylic acid, fluorinated ester, fluorinated sulfonyl halide, or perfluorinated aryl.DETAILED DESCRIPTION

[0008] The following detailed description is merely exemplary in nature and is not intended to limit the present disclosure or the application and uses thereof. Furthermore, there is no intentionUTILITY PATENT APPLICATIONATTORNEY DOCKET NO. DW0339-WO-PCT (421.0029PC)to be bound by any theory presented in the preceding background or the following detailed description.

[0009] Methods of producing fluorinated vinyl ether compositions and fluorinated vinyl ether compositions produced through the methods are provided herein. In an embodiment, a fluorinated carboxylic acid metal salt is pyrolyzed in a non-polar aprotic solvent at a temperature of about 100°C to about 200°C to form the fluorinated vinyl ether. The fluorinated carboxylic acid metal salt and the fluorinated vinyl ether have specific chemical structures as described herein that may be susceptible to excessive byproduct formation under conventional solution phase pyrolysis techniques involving polar aprotic solvents. However, it has been found that conducting pyrolysis in a non-polar aprotic solvent at a temperature within the recited range (which is sufficient to pyrolyze the subject metal salts) leads to minimized byproduct formation and achieves maximized yield and maximized purity of the resulting fluorinated vinyl ether composition, even when pyrolysis is conducted in the solution phase.

[0010] Unless specifically stated or obvious from context, as used herein, the term “about” is understood as within a range of normal tolerance in the art measured using standard measurement devices for a given measurement, for example within 2 standard deviations of the mean for a particular measurement device. For example, “about” can be understood as within 10%, 5%, 1%, 0.5%, 0.1%, 0.05%. or 0.01% of the stated value. “About” can alternatively be understood as implying the exact value stated. Unless otherwise clear from the context, all numerical values provided herein are modified by the term “about.”

[0011] As used herein, a method conducted “substantially in the absence of’ a material means that the reaction mixture contains less than 1 wt%, alternatively trace amounts that may be present but not intended, alternatively no detectable presence of the specified material.

[0012] As used herein, “solubility” refers to the amount of a substance that can dissolve in a given amount of a solvent at a specific temperature and pressure. Any values provided herein for solubility are measured at a temperature of about 25°C at atmospheric pressure and are reported in units of mg / L.UTILITY PATENT APPLICATIONATTORNEY DOCKET NO. DW0339-WO-PCT (421.0029PC)

[0013] As used herein, “boiling point” of a material refers to the temperature at which the vapor pressure of a material is equal to the external pressure acting on the material. Any values provided herein for boiling point are measured at atmospheric pressure and are reported in units of degrees Celsius (°C).

[0014] As used herein, the “molecular weight” refers to the weight average molecular weight of a substance. Any molecular weights provided herein are measured by mass spectrometry (MS) and reported in units of g / mol.

[0015] As used herein, “pyrolyze” or “pyrolyzing” means keeping the reaction mixture at conditions sufficient to begin thermally decomposing the fluorinated carboxylic acid metal salt. The term “pyrolysis” refers to the step of pyrolyzing.

[0016] The methods provided herein may be particularly suitable for pyrolyzing the fluorinated carboxylic acid metal salts described herein because they may be challenging to pyrolyze in a solution phase pyrolysis without producing significant amounts of byproducts. Without being bound by any theory, it is thought that fluorinated carboxylic acid metal salts of Formula I as described above have properties, such as high molecular weight and / or high boiling point relative to other fluorinated carboxylic acid metal salts, that may lead to significant byproduct formation during pyrolysis and decomposition of the resulting product.

[0017] The fluorinated carboxylic acid metal salt as contemplated herein has Formula I:ROCF(CF3)CO2M (I)where M in Formula I is an alkali or alkaline earth metal. For example. M may be an alkali metal selected from lithium, sodium, potassium, or cesium. R in Formula I is selected from fluorinated ether, fluorinated nitrile, fluorinated carboxylic acid, fluorinated ester, fluorinated sulfonyl halide, or perfluorinated aryl. The fluorinated ether may be, for example, a compound having one of the following formulas: -CF2CF(CF3)-OCF3, -CF2CF(CF3)-OCF2CF3, -CF2CF(CF3)-OCF2CF2CF3, -CF2CF(CF3)-O CF2CF(CF3)-OCF2CF2CF3. -CF2CF2OCF3. -CF2CF2O-CF2CF3, or CF2CF2O-CF2CF2CF3, -CF2CF2CF2OR’, -CF2CF2CF2CF2OR’, -CF2CF2CF2CF2CF2OR’, CF2CF2CF2CF2CF2CF2OR’or -CF2-CF(CF3)-OCF2CF2CF2OR’, wherein R’ is an alkyl group. TheUTILITY PATENT APPLICATIONATTORNEY DOCKET NO. DW0339-WO-PCT (421.0029PC)alkyl group may be chosen from methyl, ethyl, propyl, isopropyl, butyl or tert-butyl. The fluorinated nitrile may have, for example, one of the following formulas: -CF2CF2CN,-CF2CF2CF2CN, -CF2CF2CF2CF2CN, -CF2CF2CF2CF2CF2CN, or -CF2CF(CF3)-O-CF2CF2)CN. The fluorinated carboxylic acid may have, for example, one of the following formulas: -CF2CF2CO2H, -CF2CF2CF2CO2H, -CF2CF2CF2CF2CO2H, -CF2CF2CF2CF2CF2CO2H, or -CF2-CF(CF3)-OCF2CF2-CO2H. The fluorinated ester may have, for example, one of the following formulas: -CF2CF2CO2R’, -CF2CF2CF2CF2CF2CO2R’. -CF2CF2CF2CF2CF2CO2R’, or CF2CF(CF3)-OCF2CF2CO2R’, wherein R’ is an alkyl group. The alkyl group may be chosen from methyl, ethyl, propyl, isopropyl, butyl or tert-butyl. The fluorinated sulfonyl halide may have, for example, one of the following formulas: -CF2CF2-SO2F, -CF2CF2CF2-SO2F, or CF2CF(CF3)OCF2CF2SO2F. The perfluorinated aryl may be, for example, a pentafluorophenyl group or a group having the formula CF2-CF(CF3)O-C6F5.

[0018] In embodiments, R has from 1 to 10 carbon atoms, alternatively from 2 to 8 carbon atoms, alternatively from 4 to 8 carbon atoms. In embodiments, R has one of the following formulas:-CF2CF(CF3)OCF2CF2CO2R’ (III);-CF2CF2CF2CF2CF2CO2R’ (IV);-CF2CF(CF3)OCF2CF2CF3 (V);-CF2-CF(CF3)-OCF2CF2CF2OR’ (VI);- CF2CF2SO2F (VII);-CF2CF(CF3)OCF2CF2SO2F (VIII);- CF2-CF(CF3)O-C6F5(IX);-CF2CF2CF2CF2CF2CN (X); or -CF2CF(CF3)OCF2CF2CN (XI)wherein R’ is an alkyl group. The alkyl group may be chosen from methyl, ethyl, propyl, isopropyl, butyl or isobutyl.

[0019] In embodiments, the fluorinated carboxylic acid metal salt is an intermediate in the method of forming the fluorinated vinyl ether. Suitable fluorinated carboxylic acid metal salts may have a weight average molecular weight of from about 150 g / mol to about 10000 g / mol,UTILITY PATENT APPLICATIONATTORNEY DOCKET NO. DW0339-WO-PCT (421.0029PC)alternatively from about 400 g / mol to about 600 g / mol, alternatively from about 350 g / mol to about 550 g / mol. Examples of suitable fluroinated carboxylic acid metal salts may include, for example, potassium methyl perfluoro(8-(fluoroformyl)-5-methyl-4,7-dioxanonanoate); potassium 2, 3, 3, 3-tetrafluoro-2-[l,l,2,3,3,3-hexafluoro-2-[l,l,2,2-tetrafluoro-2-(fluorosulfonyl)ethoxy]propoxy] propanoate; or potassium perfluoro(5-phenoxy-2-methyl-3-oxacaproate).

[0020] In embodiments, the fluorinated carboxylic acid metal salt is formed by combining a fluorinated acid halide or fluorinated acid and a metal carbonate in the nonpolar aprotic solvent at a temperature of from about 20°C to about 100°C. In embodiments, the fluorinated acid halide or fluorinated acid has the Formula XII:ROCF(CF3)CO2X (XII)where X in Formula XII is selected from F or H. In embodiments, the metal carbonate is an alkali or alkaline earth metal carbonate. For example, the metal carbonate may be an alkali metal carbonate selected from lithium carbonate, sodium carbonate, potassium carbonate, or cesium carbonate. In embodiments, potassium carbonate (K2CO3) may be particularly suitable because potassium carbonate may react with acyl fluoride more quickly than other metal carbonates, and the potassium counterion may decompose faster than other counterions.

[0021] The fluorinated carboxylic acid salt may be formed prior to pyrolysis. Alternatively, formation of the fluorinated carboxylic acid salt and pyrolysis of the fluorinated carboxylic acid salt may both occur in the nonpolar aprotic solvent during the same process step.

[0022] Pyrolysis of the fluorinated carboxylic acid metal salt is conducted in the nonpolar aprotic solvent at a temperature of from about 100°C to about 200°C. The nonpolar aprotic solvent is used in the pyrolysis step to facilitate the pyrolysis of the fluorinated carboxylic acid metal salt without a significant amount of side reactions. Without being bound by any theory, it is thought that conducting pyrolysis in the nonpolar aprotic solvent leads to fewer side reactions at least partially because the nonpolar aprotic solvent does not contribute protons to facilitate additional reactions and does not provide opportunities for other interactions such as hydrogen bonding.UTILITY PATENT APPLICATIONATTORNEY DOCKET NO. DW0339-WO-PCT (421.0029PC)

[0023] In embodiments, the nonpolar aprotic solvent has a fluoride ion solubility of less than about 0.1 mg / L at a temperature of 25°C. The negligible fluoride ion solubility of the nonpolar aprotic solvent minimizes the amount of fluoride ions available to participate in unwanted side reactions that may produce byproducts that decrease the yield and purity of the resulting product. For example, in the presence of a solvent having a fluoride ion solubility outside the recited range, a fluoride ion catalyzed transesterification reaction may occur, leading to the production of decomposition products such as a diester. In embodiments, the nonpolar aprotic solvent has a boiling point of from about 100°C to about 400°C, alternatively from about 200°C to about 350°C, at atmospheric pressure. A boiling point in the recited range is high enough that the solvent does not boil at the temperatures required to pyrolyze the fluorinated carboxylic acid metal salt. Further, if the solvent has a boiling point in the recited ranges, the fluorinated vinyl ether can be separated from the solvent after pyrolysis through a distillation step.

[0024] In embodiments, the nonpolar aprotic solvent is selected from a hydrocarbon, an aromatic ether, or a combination thereof. The recited solvents have been found to be particularly suitable for the methods provided herein. In embodiments, the nonpolar aprotic solvent is a hydrocarbon selected from a linear or branched aliphatic hydrocarbon, a cyclic aliphatic hydrocarbon, an aromatic hydrocarbon, or combinations thereof. In embodiments, the nonpolar aprotic solvent is a hydrocarbon selected from decane, dodecane, tetradecane, hexadecane, octadecane, decene, dodecene, tetradecene, hexadecene, octadecene, decalin, tetralin, cycloheptane, cyclooctane, cyclodecane, cycloheptene, cyclooctene, cyclodecene, mineral oil, toluene, xylene, 1 -methylnaphthalene, diphenylmethane, or combinations thereof. In embodiments, the nonpolar aprotic solvent is an aromatic ether selected from diphenyl ether, dibenzyl ether, methoxy benzene, dimethoxy benzene, trimethoxybenzene, methoxy naphthalene, dimethoxy naphthalene, or combinations thereof. In embodiments, the nonpolar aprotic solvent is present in an amount of at least about 10 wt%, alternatively from about 10 wt% to about 70 wt%, alternatively from about 10 wt% to about 50 wt%, alternatively from about 10 wt% to about 30 wt%, alternatively from about 10 wt% to about 20 wt%, based on a total weight of the reaction mixture.

[0025] Pyrolysis is conducted at a temperature of from about 100°C to about 200°C, alternatively from about 120°C to about 200°C, alternatively from about 120°C to about 170°C,UTILITY PATENT APPLICATIONATTORNEY DOCKET NO. DW0339-WO-PCT (421.0029PC)alternatively from about 130°C to about 160°C, alternatively from about 130°C to about 155°C, alternatively from about 135°C to about 155°C. The recited temperatures are high enough to induce pyrolysis of the fluorinated carboxylic acid metal salt to form the fluorinated vinyl ether, but low enough to avoid causing thermal decomposition of the fluorinated vinyl ether once formed. The temperatures are also low enough to inhibit some fluoride ion induced side reactions.

[0026] In embodiments, pyrolysis is conducted substantially in the absence of water, alternatively substantially in the absence of any polar solvent, alternatively substantially in the absence of any protic solvent. Conducting pyrolysis in the absence of polar and / or protic solvents reduces the occurrence of unwanted side reactions that decrease the yield and purity of the fluorinated vinyl ether. For example, in the presence of a polar and / or protic solvent, the intermediate anion of the fluorinated carboxylic acid metal salt may abstract a proton from the solvent prior to the elimination that forms the fluorinated vinyl ether, leading to the production of a reduced product such as a hydrofluoric acid (HF) adduct. In embodiments, pyrolysis is conducted in an inert environment. For example, the method may be conducted under a blanket of inert gas. The inert gas may be, for example, argon or nitrogen. Conducting pyrolysis in an inert environment inhibits unwanted side reactions because of the absence of oxygen in contact with the reaction mixture.

[0027] The fluorinated vinyl ether as contemplated herein has Formula II:ROCF=CF2(II)where R in Formula II is the same as R in Formula I and may include any of the embodiments described above for R. It has been found that the methods provided herein are particularly suitable for forming the fluorinated vinyl ethers provided herein because the properties of such fluorinated vinyl ethers, such as high molecular weight and / or high boiling point relative to other fluorinated vinyl ethers, may contribute to thermal decomposition or other unwanted side reactions.

[0028] In embodiments, the fluorinated vinyl ether has from 3 to 15 carbon atoms, alternatively from 4 to 10 carbon atoms. In embodiments, the fluorinated vinyl ether has a weight average molecular weight of from about 130 g / mol to about 750 g / mol, alternatively from about 250 g / mol to about 500 g / mol. In embodiments, the fluorinated vinyl ether has a boiling point of from aboutUTILITY PATENT APPLICATIONATTORNEY DOCKET NO. DW0339-WO-PCT (421.0029PC)-30°C to about 400°C, alternatively from about 30°C to about 300°C, alternatively from about 100°C to about 200°C, at atmospheric pressure. Examples of suitable fluorinated vinyl ethers may include, for example, methyl perfluoro(5-methyL4,7-dioxanon-8-enoate) (EVE); perfluoro(2-phenoxypropyl vinyl) ether (P2PPVE); or perfluoro-2-(fluorosulfonylethoxy)propyl vinyl ether (PSEPVE).

[0029] In embodiments, the methods provided herein further include the step of removing the fluorinated vinyl ether from the nonpolar aprotic solvent to form the fluorinated vinyl ether composition. For example, the fluorinated vinyl ether may be removed from the nonpolar aprotic solvent using vacuum and a cold trap. The fluorinated vinyl ether may be removed from the nonpolar aprotic solvent as the fluorinated vinyl ether is formed. Removing the fluorinated vinyl ether as it is formed may be particularly advantageous when the pyrolysis temperature is above 150°C because the removal inhibits any thermal decomposition of the fluorinated vinyl ether. In embodiments, removal of the fluorinated vinyl ether from the nonpolar aprotic solvent is stopped when evolution of carbon dioxide (CO2) from the reaction mixture ceases or is significantly reduced. In embodiments, removal of the fluorinated vinyl ether from the nonpolar aprotic solvent is stopped when the amount of the fluorinated carboxylic acid metal salt in the nonpolar aprotic solvent is determined to be less than about 1 g / L, alternatively less than about 0.1 g / L. Stopping the removal may contribute to the purity of the resulting fluorinated vinyl ether composition because after a certain point, less fluorinated vinyl ether may be produced and more byproducts may be produced. The resulting fluorinated vinyl ether composition may be cooled with, for example, dry ice. In embodiments, the methods further include a purification step. For example, the fluorinated vinyl ether composition may be purified by distillation or by extraction. In an embodiment, the fluorinated vinyl ether composition is purified by fractional distillation under reduced pressure.

[0030] The fluorinated vinyl ether compositions provided herein are formed by the methods provided herein. In embodiments, the fluorinated vinyl ether composition has a purity of from about 90% to about 100%, alternatively from about 95% to about 100%, based on total moles of the fluorinated vinyl ether composition. In embodiments, the fluorinated vinyl ether composition is produced with a yield of from about 45% to about 90%, alternatively from about 50% to about 80%, on a molar basis based on the total moles of the fluorinated carboxylic acid metal salt in theUTILITY PATENT APPLICATIONATTORNEY DOCKET NO. DW0339-WO-PCT (421.0029PC)reaction mixture prior to the start of pyrolysis. The recited yield and purity may not be achievable with methods not in accordance with this disclosure for the fluorinated vinyl ethers provided herein.

[0031] While at least one exemplary embodiment has been presented in the foregoing detailed description, it should be appreciated that a vast number of variations exist. It should also be appreciated that the exemplary embodiment or exemplary embodiments are only examples, and are not intended to limit the scope, applicability, or configuration of the present disclosure in any way. Rather, the foregoing detailed description will provide those skilled in the art with a convenient road map for implementing an exemplary embodiment of the present disclosure. It being understood that various changes may be made in the function and arrangement of elements described in an exemplary embodiment without departing from the scope of the present disclosure as set forth in the appended claims.EXAMPLES

[0032] Examples 1-10

[0033] The methods of Examples 1-10 are in accordance with this disclosure. For Example 1, a 3-necked flask fitted with a mechanical stirrer, thermowell, addition funnel, and a distillation head attached to a collection flask was dried and assembled while hot. The flask was flushed with nitrogen and charged with the dry metal carbonate shown in Table 1 below in the amount shown in Table 1, followed by the dry solvent shown in Table 1 in the amount shown in Table 1. The resulting slurry was heated to 80°C. Methyl perfhroro(8-(fhioroformyl)-5-methyl-4,7-dioxanonanoate) (DAE) in the amount shown in Table 1 was added drop wise over 10 minutes with mixing. The mixing continued for an additional two hours or until evolution of CO2 ceased. The temperature of the reaction vessel was raised to 160°C to pyrolyze the intermediate salt. The temperature was maintained between 150°C and 170°C for one hour. Then the reaction mixture was subjected to vacuum, and the pyrolysis products were collected in a collection flask cooled with dry ice. The collected product was fractionally distilled under reduced pressure to obtain methyl perfluoro(5-methyl-4,7-dioxanon-8-enoate) (EVE).UTILITY PATENT APPLICATIONATTORNEY DOCKET NO. DW0339-WO-PCT (421.0029PC)

[0034] For Examples 2-8, the procedure described above for Example 1 was followed, using the solvents and amounts shown in Table 1 below, except for the following differences. For Example 2, the slurry was heated to 180°C overnight under vacuum, and then the slurry was cooled to 80°C before the DAE was added. For Example 8, the DAE was added over a period of four hours, with the temperature maintained between 80°C and 100°C for the four hour period. For Example 8, pyrolysis was conducted at a temperature of 140°C.

[0035] For Example 9, the salt formation and pyrolysis were conducted in one step. The reaction mixture was heated to 135°C before the DAE was added, and the DAE was added over a two hour period while the reaction mixture was maintained at a temperature between 135 °C and 150°C. After the addition was complete, the mixture was stirred for an additional one hour at 140°C.

[0036] For Example 10, the procedure of Example 1 was followed, except that perfluoro(5-phenoxy-2-methyl-3-oxacaproy fluoride) (DA) was added instead of DAE, the DA was added over a period of 30 minutes, and pyrolysis was conducted at a temperature of 180°C for five hours. The mixture was phase separated and the bottom layer was vacuum distilled to obtain perfluoro(2-phenoxypropyl vinyl) ether (P2PPVE).Table 1 - Components of Reaction Mixture for Examples 1-8 Example Solvent Starting Material Metal CarbonateExample 1 Hexadecane DAE K2CO3(30 mL) (48.8 g) (16.79 g) Example 2 Mineral Oil DAE K2CO3(30 mL) (48.8 g) (16.79 g) Example 3 1 -Octadecene DAE K2CO3(45 mL) (97.6 g) (39.8 g) Example 4 Diphenyl Methane DAE K2CO3(10 mL) (24.4 g) (8-5 g)UTILITY PATENT APPLICATIONATTORNEY DOCKET NO. DW0339-WO-PCT (421.0029PC)Example 5 1 -Methyl Naphthalene DAE K2CO3(10 mL) (24.4 g) (8.5 g) Example 6 Diphenyl Ether DAE K2CO3(10 mL) (24.4 g) (8.5 g) Example 7 Dibenzyl Ether DAE K2CO3(30 mL) (35.0 g) (H.89 g) Example 8 1,3-Dimethoxy Benzene DAE K2CO3(185 mL) (300.0 g) (10L5 g) Example 9 1,3-Dimethoxy Benzene DAE K2CO3(185 mL) (300.0 g) (10L5 g) Example 10 1 -Octadecene DA K2CO3(100 mL) (101.61 g) (36.6 g)

[0037] The DAE used in Examples 1-9 has a CAS number of 69116-73-0 and a weight average molecular weight of about 488 g / mol.

[0038] The EVE produced in Examples 1-9 has a CAS number of 63863-43-4, a weight average molecular weight of about 422 g / mol, and a boiling point of about 151 °C at atmospheric pressure.

[0039] The P2PPVE produced in example 10 has a CAS number 24520-19-2, a weight average molecular weight of about 430 g / mol, and a boiling point 85-86°C at 26 mm Hg.

[0040] The collected product was weighed. The isolated yield of the product expressed as a percentage was determined by converting the amount of the starting material fluorinated acid halide (DAE or DA) into moles, converting the amount of the product (EVE or P2PPVE) into moles, dividing the moles of the product by the moles of the starting material, and multiplying byUTILITY PATENT APPLICATIONATTORNEY DOCKET NO. DW0339-WO-PCT (421.0029PC)100. The purity of the product was determined through nuclear magnetic resonance (NMR) and gas chromatography (GC) testing. The purity is expressed as a percentage on a molar basis.Table 2 - Results and Observations for Examples 1-10 Example Purity Isolated Yield ObservationsExample 1 > 98% 75.6% At 150°C, the mixture began bubbling with evolution of CO2.Example 2 > 98% 72.3% After addition of DAE, the mixture began thickening and became a crumbling solid with evolution of CO2. After 2 hours, the evolution of CO2 ceased.Example 3 > 97% 79.8% No observations recorded.Example 4 > 98% 76.6% No observations recorded.Example 5 > 97% 76.4% No observations recorded.Example 6 > 98% 78.4% No observations recorded.Example 7 > 96% 54% No observations recorded.Example 8 > 98% 77% After addition of DAE, the mixture began thickening and became a crumbling solid with evolution of CO2. At 130°C, the mixture began bubbling with evolution of CO2.Example 9 > 98% 70.2% After addition of DAE, the mixture began thickening and became a crumbling solid with evolution of CO2.Example 10 > 97% 63.2% The product contained traces of HF adduct.UTILITY PATENT APPLICATIONATTORNEY DOCKET NO. DW0339-WO-PCT (421.0029PC)

[0041] Comparative Examples 1-5

[0042] The methods of Comparative Examples 1-5 are comparative methods not in accordance with this disclosure. For Comparative Examples 1-5, the procedure described above for Example 1 was followed, using the solvents and amounts shown in Table 3 below, except for the following differences.

[0043] For Comparative Examples 1 and 3, pyrolysis was conducted for two hours. For Comparative Example 2, pyrolysis was conducted for two hours while the temperature was maintained between 150°C and 170°C. For Comparative Example 2, the salt formation and pyrolysis were conducted in one step, similar to Example 9 described above. For Comparative Example 5, pyrolysis was conducted for four hours at a temperature of 180°C.Table 3 - Components of Reaction Mixture for Comparative Examples 1-5 Example Solvent Starting Material Metal CarbonateComparative Tetraglyme DAE K2CO3 Example 1(20 mb) (48.8 g) (16.79 g) Comparative Tetraglyme DAE K2CO3 Example 2 (20 mL) (48.8 g) (16.79 g) Comparative Propylene Carbonate DAE K2CO3 Example 3 (40 mL) (48.8 g) (17.4 g) Comparative Adiponitrile DAE K2CO3 Example 4 (20 mL) (48.8 g) (16.83 g) Comparative Tetraglyme DA K2CO3 Example 5 (40 mL) (48.8 g) (17.4 g)UTILITY PATENT APPLICATIONATTORNEY DOCKET NO. DW0339-WO-PCT (421.0029PC)

[0044] The product was analyzed by NMR and GC testing. It was not possible to isolate the product because of the complicated nature of the mixture and the high amount of impurities. The estimated GC yield for Comparative Examples 1-5 was estimated using GC testing. For the comparative examples, the purity was not reported because only trace amounts or very low amounts of the desired product (EVE or P2PPVE) were produced.Table 4 - Results and Observations for Comparative Examples 1-5 Example Estimated ObservationsGC YieldComparative 20% Only trace amounts of EVE detected by GCExample 1 analysis. Distillation of the mixture providednumerous volatile species and higher boilingspecies, indicative of significant decompositionof DAE and EVE.Comparative 25% Only trace amounts of EVE detected by GCExample 2 analysis. Distillation of the mixture providednumerous volatile species and higher boilingspecies, indicative of significant decompositionof DAE and EVE.Comparative 23.9% Distillation of the mixture provided EVE alongExample 3 with many byproducts as major components.Comparative 6% Distillation of the mixture provided hydro-EVEExample 4 as major product.Comparative Not Only trace amounts of P2PPVE detected by GCExample 5 Reported analysis.UTILITY PATENT APPLICATIONATTORNEY DOCKET NO. DW0339-WO-PCT (421.0029PC)

[0045] The results of Examples 1-10 and Comparative Examples 1-5 show that pyrolyzing the intermediate fluorinated carboxylic acid metal salt in a nonpolar aprotic solvent produces the fluorinated vinyl ether product in a yield of about 50% to 80% and with purity (after distillation) of greater than 95%. However, the same method conducted in polar solvents produces negligible or very low (less than 30%) yields of the fluorinated vinyl ether product with a significant amount of byproducts.

Claims

UTILITY PATENT APPLICATIONATTORNEY DOCKET NO. DW0339-WO-PCT (421.0029PC)CLAIMS1. A method of forming a fluorinated vinyl ether composition, the method comprising the steps of:pyrolyzing a fluorinated carboxylic acid metal salt in a reaction mixture comprising a nonpolar aprotic solvent at a temperature of from about 100°C to about 200°C to form a fluorinated vinyl ether;wherein the fluorinated carboxylic acid metal salt has Formula I:ROCF(CF3)CO2M (I);wherein M in Formula I is an alkali or alkaline earth metal; andwherein the fluorinated vinyl ether has Formula II:ROCF=CF2(II);wherein R in Formulas I and II is selected from fluorinated ether, fluorinated nitrile, fluorinated carboxylic acid, fluorinated ester, fluorinated sulfonyl halide, or perfluorinated aryl.

2. The method of claim 1, wherein the fluorinated carboxylic acid metal salt is pyrolyzed at a temperature of from about 135°C to about 155°C.

3. The method of claim 1, wherein pyrolysis is conducted substantially in the absence of water.

4. The method of claim 1, wherein the nonpolar aprotic solvent has a fluoride ion solubility of less than about 0.1 mg / L at a temperature of 25°C.UTILITY PATENT APPLICATIONATTORNEY DOCKET NO. DW0339-WO-PCT (421.0029PC)5. The method of claim 1, wherein the nonpolar aprotic solvent has a boiling point of from about 100°C to about 350°C at atmospheric pressure.

6. The method of claim 1, wherein the nonpolar aprotic solvent is selected from a hydrocarbon, an aromatic ether, or a combination thereof.

7. The method of claim 6, wherein the nonpolar aprotic solvent is a hydrocarbon selected from a linear or branched aliphatic hydrocarbon, a cyclic aliphatic hydrocarbon, an aromatic hydrocarbon, or combinations thereof; preferably, a hydrocarbon selected from decane, dodecane, tetradecane, hexadecane, octadecane, decene, dodecene, tetradecene, hexadecene, octadecene, decalin, tetralin, cycloheptane, cyclooctane, cyclodecane, cycloheptene, cyclooctene, cyclodecene, mineral oil, toluene, xylene, 1 -methylnaphthalene, diphenylmethane, or combinations thereof.

8. The method of claim 6, wherein the nonpolar aprotic solvent is an aromatic ether selected from diphenyl ether, dibenzyl ether, methoxy benzene, dimethoxy benzene, trimethoxybenzene, methoxy naphthalene, dimethoxy naphthalene, or combinations thereof.

9. The method of any one of claims 1 to 8, wherein the nonpolar aprotic solvent is present in an amount of at least about 10 wt%, based on a total weight of the reaction mixture.

10. The method of any one of claims 1 to 8, wherein the fluorinated vinyl ether has a weight average molecular weight of from about 130 g / mol to about 750 g / mol.

11. The method of any one of claims 1 to 8, wherein the fluorinated vinyl ether has a boiling point of from about -30 °C to about 400°C at atmospheric pressure.UTILITY PATENT APPLICATIONATTORNEY DOCKET NO. DW0339-WO-PCT (421.0029PC)12. The method of any one of claims 1 to 8, wherein R has one of the following formulas:-CF2CF(CF3)OCF2CF2CO2R’ (III);-CF2CF2CF2CF2CF2CO2R’ (IV);-CF2CF(CF3)OCF2CF2CF3 (V);-CF2-CF(CF3)-OCF2CF2CF2OR’ (VI);- CF2CF2SO2F (VII);-CF2CF(CF3)OCF2CF2SO2F (VIII);- CF2-CF(CF3)O-C6F5(IX);-CF2CF2CF2CF2CF2CN (X); or -CF2CF(CF3)OCF2CF2CN (XI)wherein R’ is an alkyl group.

13. The method of any one of claims 1 to 8, wherein the fluorinated carboxylic acid metal salt is an intermediate in the method of forming the fluorinated vinyl ether.

14. The method of any one of claims 1 to 8, further comprising the step of forming the fluorinated carboxylic acid metal salt in the nonpolar aprotic solvent.

15. The method of claim 14, wherein the step of forming the fluorinated carboxylic acid metal salt in the nonpolar aprotic solvent comprises:combining a fluorinated acid halide or fluorinated acid and a metal carbonate in the nonpolar aprotic solvent at a temperature of from about 20°C to about 100°C to form the fluorinated carboxylic acid metal salt;wherein the fluorinated acid halide or fluorinated acid has the Formula XII:ROCF2(CF3)CO2X (XII);UTILITY PATENT APPLICATIONATTORNEY DOCKET NO. DW0339-WO-PCT (421.0029PC)wherein X is selected from F or H.

16. The method of any one of claims 1 to 8, wherein the fluorinated carboxylic acid metal salt is formed prior to the pyrolysis, wherein the method is free of any purification step after the fluorinated carboxylic acid metal salt is formed and before the pyrolysis.

17. The method of any one of claims 1 to 8, further comprising the step of removing the fluorinated vinyl ether from the nonpolar aprotic solvent to form the fluorinated vinyl ether composition.

18. A fluorinated vinyl ether composition formed by the method of any one of claims 1 to 8.

19. The fluorinated vinyl ether composition of claim 18, wherein the fluorinated vinyl ether composition has a purity of from about 90% to about 100%, based on total moles of the fluorinated vinyl ether composition.