Battery cell, battery apparatus, electric apparatus, and energy storage apparatus
By employing a double-folded soft-pack material shell in the battery cell and optimizing the design of the positive electrode film, electrolyte composition, and separator, the problem of insufficient energy density and reliability of the battery cell is solved, achieving a balance between high energy density and high reliability.
Patent Information
- Application Number
- PCT/CN2025/094407
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-12
- Publication Date
- 2026-11-19
AI Technical Summary
Existing technologies struggle to simultaneously improve the energy density and reliability of individual battery cells, especially when thick coating layers are applied, which can lead to problems such as mechanical stress accumulation, difficulty in heat conduction, and easy damage to the packaging structure.
The soft-pack material shell with a double-folded structure, combined with appropriate positive electrode film thickness, particle size distribution, electrolyte composition and separator design, enhances the packaging strength, improves thermal management and stress buffering, and reduces the rebound rate.
It improves the energy density and reliability of individual battery cells, reduces the probability of seal area failure, and enhances battery safety and cycle life.
Smart Images

Figure CN2025094407_19112026_PF_FP_ABST
Abstract
Description
Battery cells, battery devices, electrical devices, and energy storage devices Technical Field
[0001] This application relates to the field of battery technology, and in particular to a battery cell, battery device, power consumption device, and energy storage device. Background Technology
[0002] In recent years, battery cells have been widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power plants, as well as in many fields such as power tools, electric bicycles, electric motorcycles, electric cars, military equipment, and aerospace.
[0003] With the increasing demands from national and industry standards and the market for the capacity and reliability of electrical devices, higher requirements are being placed on individual battery cells. However, existing technologies struggle to simultaneously improve these performance characteristics, which has become a pressing technical problem to be solved in this field. Summary of the Invention
[0004] In view of the above problems, this application provides a battery cell, a battery device, an electrical device, and an energy storage device, which are described below.
[0005] A first aspect of this application provides a battery cell comprising a stacked cell and a housing, wherein the stacked cell is housed within the housing, and the housing is a soft-pack material; the housing includes a first sealing region disposed at at least one end of the stacked cell extending along its width direction; the first sealing region includes a double-folded edge structure extending along its length direction, wherein an encapsulating adhesive is disposed on the double-folded edge structure, and the encapsulating adhesive is continuously disposed along its length direction and fixes the double-folded edge structure; the stacked cell includes a positive electrode, a negative electrode, and an electrolyte, wherein the positive electrode includes a positive current collector. The battery cell comprises a positive electrode film layer disposed on at least one side of the positive electrode current collector. The positive electrode film layer includes lithium transition metal phosphate particles, and at least a portion of the surface of the lithium transition metal phosphate particles is provided with carbon material. Based on the total area of particles in the cross-section of the positive electrode film layer along the thickness direction of the positive electrode sheet, the area ratio of particles with a particle size R1 satisfying R1≥1000nm is 12%-50%. The thickness of the positive electrode film layer on one side is denoted as H, where H is 70μm-120μm. When the battery cell is in a fully discharged state, the compaction density of the positive electrode sheet is 2.3g / cm³. 3 -2.6g / cm 3 The electrolyte includes a solvent, which includes dimethyl carbonate (DMC); the mass percentage of dimethyl carbonate is 18%-32% based on the total mass of the electrolyte.
[0006] Lithium-containing transition metal phosphates generally have relatively low specific capacity. Studies have shown that when the thickness H of the positive electrode film on one side is less than 70 μm, the battery capacity is difficult to meet market demand. In the embodiments of this application, by controlling the thickness H of the positive electrode film on one side within the range of 70 μm-120 μm, it is beneficial to increase the space utilization rate of the active material and further adopt a soft-pack material shell, thereby reducing the weight of the battery cell and improving the mass energy density of the battery. However, a thicker positive electrode film undergoes significant volume changes during charge-discharge cycles due to lithium insertion and delithiation, leading to the accumulation of mechanical stress, which in turn causes the electrode material to expand and contract, resulting in electrode rebound and increased thickness, increasing the mechanical stress on the packaging structure. At the same time, a thicker film means that internal heat is more difficult to conduct, easily leading to local overheating, exacerbating the side reactions and gas production of the electrolyte, and further increasing the internal pressure of the battery cell. Compared with the wound type, the stacked cell structure reduces the corner gap and improves the volumetric energy density, but the stacked cell lacks the binding effect of the wound structure, which has less limitation on the rebound of the thickly coated film layer, thus degrading the reliability of the battery cell. Compared to rigid-shell materials, pouch cells have lower mechanical strength and are less able to withstand internal pressure. Furthermore, pouch cells have lower thermal conductivity, making them more prone to heat buildup inside individual cells and further exacerbating gas generation issues. During long-term use, excessive internal pressure may cause the sealed area to be breached.
[0007] In this embodiment, the first sealing area includes a double-folded edge structure extending along the long side to further enhance the sealing strength of the first sealing area. The double-folded edge forms multiple sealing barriers by folding and encapsulating the soft-pack material twice. Even if the first folded edge structure experiences rebound stress due to the high thickness of the positive electrode film layer in the cell, or defects caused by electrolyte gas generation, the second folded edge structure can still maintain a seal. Simultaneously, due to battery processing, the soft-pack material is bonded by hot-melt bonding, and the double-folded edge makes the heat-sealed area more uniform, improving the situation of poor sealing in local areas. The sealing point is a weak point in the mechanical strength of the soft-pack cell. To further enhance the reliability of the encapsulation, the inventors set encapsulating adhesive on the double-folded edge structure. The encapsulating adhesive is continuously set along the long side and fixes the double-folded edge structure, which can cover microscopic cracks or defects in the heat-sealed area of the soft-pack material sealing area; and the double-folded edge structure has a certain elastic memory after heat sealing, and may rebound after long-term use. The encapsulating adhesive can fix the double-folded edge structure and maintain its stability. In this embodiment, the compaction density of the positive electrode sheet is further controlled to be 2.3 g / cm³ when the battery cell is fully discharged. 3 -2.6g / cm 3This approach, on the one hand, enables the battery cell to have a higher capacity, and on the other hand, provides a certain buffer space between the particle stacking structure, reducing the stress exerted on the encapsulation structure by electrode rebound. To further reduce the internal stress of the battery cell, the inventors controlled the area ratio of particles with a particle size R1 satisfying R1≥1000nm in the positive electrode film and the mass ratio of dimethyl carbonate in the electrolyte. The inventors found that, under the same expansion rate, the expansion of small particles is more easily absorbed through the micropore structure between particles than that of large particles. The absolute value of the expansion change of large particles is larger and more difficult to dissipate. When the area ratio of particles with a particle size R1 satisfying R1≥1000nm is greater than 50%, it is easy to cause stress concentration, resulting in obvious rebound and increasing the internal pressure of the battery cell. When the area ratio of particles with a particle size R1 satisfying R1≥1000nm is less than 12%, it will limit the improvement of the gradation and compaction density of the positive electrode film, and cannot effectively improve the battery capacity. Therefore, controlling the particle size R1 to satisfy R1≥1000nm with a particle area ratio of 12%-50% is beneficial for further improving the reliability of battery cells while maintaining energy density. Dimethyl carbonate (DMC) has many advantages such as low viscosity, excellent low-temperature performance, and low cost. However, if the mass ratio of DMC in the electrolyte is less than 18%, it is difficult to form a low-viscosity system, making it difficult to improve the overall ionic conductivity of the electrolyte, increasing the ohmic impedance inside the battery, and thus leading to greater Joule heat. Furthermore, chain carbonates have weak oxidation resistance, and the symmetrical structure of DMC is more prone to decomposition under high voltage or high temperature environments. If the mass ratio of DMC is higher than 32%, severe gas generation during long-cycle operation will occur, exacerbating the probability of encapsulation failure. By controlling the mass ratio of DMC in the electrolyte to 18%-32%, the low viscosity of the electrolyte and the risk of gas generation can be balanced. The above technical measures work synergistically to achieve a balance between battery energy density and reliability.
[0008] In any embodiment, the thickness of the positive electrode film layer on one side is denoted as H, where H is 90μm-120μm, and can be selected as 100μm-120μm.
[0009] A single-sided thickness of the positive electrode film within the aforementioned range is beneficial for further improving energy density. The applicant discovered that when the single-sided thickness of the positive electrode film exceeds 100 μm, the rebound phenomenon of the positive electrode sheet becomes more severe. The embodiments of this application, through a double-folded edge structure in the first sealing region, strengthen the structural strength of the casing, reducing the probability of the seal being broken due to internal stress caused by film rebound. This enhances the reliability of the battery while maintaining a high energy density.
[0010] In any embodiment, the housing includes at least one second sealing area, which is disposed at at least one end of the laminated cell along the length direction of the housing, and the second sealing area is disposed on the tab side of the laminated cell.
[0011] The second sealing area is located on the tab side. The tab needs to be connected to the lead-out component. The connection strength between the lead-out component and the shell material is relatively weak, which makes it easy for gas to escape from the second sealing area. This is conducive to directional pressure relief of the battery, reduces the impact on adjacent cells when the seal fails, and improves the overall safety and reliability of the battery device.
[0012] In any embodiment, the outer periphery of the laminated cell is provided with a plurality of rubber rings that surround in the width direction, and the rubber rings that surround in the width direction are spaced apart in the length direction.
[0013] The arrangement of rubber rings along the width of the cell at intervals along the length direction helps to increase the binding force on the cell, which is especially suitable for battery cells with thick coating layers. It can effectively reduce the rebound rate of the positive electrode film and the rebound pressure on the sealing area, thereby further reducing the probability of sealing area failure and improving the reliability of the battery cell.
[0014] In any embodiment, based on the total area of particles in the cross-section of the positive electrode film along the thickness direction of the positive electrode sheet, the area ratio of particles with a particle size R1 satisfying R1≥1000nm is 12%-37%.
[0015] When the particle area ratio of particles with a particle size R1 that satisfies R1≥1000nm is within the above range, the expansion force exerted by the rebound of large particles on the soft-pack material and sealing area is further reduced, thereby improving the reliability of the battery cell.
[0016] In any embodiment, in the cross-section of the positive electrode film along the electrode thickness direction, the median L of the spheroidality in the cumulative distribution curve of the spheroidality area of particles with a particle size R1 satisfying R1≥1000nm is... R1A50 The value is 0.6-0.8, which can be selected as 0.65-0.75, and further can be selected as 0.67-0.75.
[0017] In the cumulative area distribution curve of spheroidal density for particles with a diameter R1 satisfying R1≥1000nm, L R1A50 Within the aforementioned range, the particles are more approximately spherical, making them easy to roll. They can offset the volume changes caused by the rebound of the thick positive electrode film or the expansion during charging and discharging within a certain spatial range through the rearrangement of the stacking relationship, thereby reducing the burden on the first sealing area and improving the reliability of the battery cell.
[0018] In any embodiment, in the cross-section of the positive electrode film layer along the electrode thickness direction, the uniformity of the distribution of particles with a particle size R1 satisfying R1≥1000nm is less than or equal to 5%, which can be selected as 0.2%-2%, and further selected as 0.2%-0.9%.
[0019] If the uniformity of particle distribution with particle size R1 satisfying R1≥1000nm in the cross-section of the positive electrode film along the thickness direction of the electrode sheet is within the above range, it can effectively reduce the stress concentration in local areas of the film layer, so that the rebound stress of the thick coating film layer during cycling can be uniformly distributed throughout the entire area of the film layer, reducing the rebound rate of the positive electrode film layer, thereby improving the battery energy density while reducing the probability of packaging structure failure and improving battery reliability.
[0020] In any embodiment, the solvent in the electrolyte further includes one or both of ethyl methyl carbonate (EMC) and ethylene carbonate (EC).
[0021] In any embodiment, the mass percentage of ethyl methyl carbonate (EMC) is 39%-49% based on the total mass of the electrolyte.
[0022] Ethyl methyl carbonate (EMC) has a viscosity of 0.65 mPa·s at 25°C, which is higher than that of DMC but lower than that of EC. It also maintains good fluidity at low temperatures. Together with DMC, it helps to reduce the overall viscosity of the electrolyte, increase the migration rate of lithium ions in the electrolyte, and reduce Joule heating. Furthermore, compared with DMC, EMC has higher oxidation stability and thermal stability, which further reduces the gas production caused by electrolyte decomposition and improves the reliability of individual battery cells.
[0023] In any embodiment, the mass percentage of ethylene carbonate (EC) is 13%-22% based on the total mass of the electrolyte.
[0024] Ethylene carbonate (EC) has an extremely high dielectric constant, which can effectively dissolve lithium salts, improve the ionic conductivity of the electrolyte, and ensure the smooth migration of lithium ions. EC within the above-mentioned mass percentage range can decompose on the surface of the negative electrode active material and form a stable SEI film, reducing side reactions and improving cycle life.
[0025] In any embodiment, based on the total mass of the electrolyte, the total mass percentage of ethyl methyl carbonate (EMC) and ethylene carbonate (EC) is 52%-71%.
[0026] When the total mass content of EC and EMC is within the above range, they can complement each other, overcoming the problems of high viscosity of EC and poor thermal stability and mechanical strength of the SEI film formed by EMC. This optimizes the electrolyte performance and further reduces the pressure on the sealing area from the optimization of ionic conductivity and SEI film.
[0027] In any embodiment, the electrolyte comprises an electrolyte salt, the electrolyte salt comprising lithium hexafluorophosphate (LiPF6), wherein the concentration of lithium hexafluorophosphate in the electrolyte is 0.9 mol / L to 1.2 mol / L.
[0028] Lithium hexafluorophosphate (LiPF6) is highly soluble in carbonate solvents, forming a high-concentration electrolyte that ensures high ionic conductivity of lithium ions. It also induces a stable SEI film at a low-potential negative electrode, reducing lithium deposition and improving cycle life. However, excessively high LiPF6 concentrations significantly increase electrolyte viscosity, restricting lithium ion diffusion and decreasing ionic conductivity. Furthermore, the decomposition products of LiPF6, including PF5, react with trace amounts of water in the electrolyte to generate HF, which corrodes the electrode and SEI film, exacerbating solvent decomposition and gas production. Within the aforementioned concentration range, LiPF6 achieves an optimal balance between ionic conductivity and electrolyte stability.
[0029] In any embodiment, the mass percentage of dimethyl carbonate is 18%-26% based on the total mass of the electrolyte.
[0030] With the mass percentage of dimethyl carbonate within the above range, the introduction of EC and EMC, which account for a larger proportion, further reduces its gas generation capacity and probability, thereby improving the long-term reliability of the battery cell.
[0031] In any embodiment, the median C of the graphitization degree C value in the cumulative distribution curve of the positive electrode film obtained in the laser microscopy confocal Raman spectroscopy instrument scanning mode is... 50为 0.95-1.20, where the degree of graphitization C is I G / I D , where I G This indicates that the Raman spectrum is at 1580±100 cm⁻¹ -1 The intensity of peak G at I D This indicates that the Raman spectrum is at 1350±100 cm⁻¹ -1 The intensity of peak D at that location.
[0032] Studies have shown that the stress on the film layer under cyclic expansion easily leads to increased internal mechanical pressure, causing the encapsulation structure to fail. By controlling the cumulative distribution curve of graphitization degree C values obtained in the laser microscopy confocal Raman spectroscopy instrument scanning mode, the median C of graphitization degree is... 50 The value is 0.95-1.20, which increases the graphitization degree of the positive electrode film, improves the slippage of particles in the positive electrode film, reduces the stress concentration phenomenon during the compaction of the thick coating film, and reduces the degree of rebound of the positive electrode film due to local stress concentration during cycling, thereby increasing the volumetric energy density of the battery cell while increasing the reliability of the battery cell.
[0033] In any embodiment, the median B of the coating value B obtained in the cumulative distribution curve of the positive electrode film layer in the laser microscopy confocal Raman spectroscopy instrument scanning mode is... 50The value is 0.30-0.60, where the coating value B is I. P / I D , where I P This indicates that the Raman spectrum is at 948±100 cm⁻¹ -1 The intensity of the P peak at I D This indicates that the Raman spectrum is at 1350±100 cm⁻¹ -1 The intensity of peak D at that location.
[0034] The median B of the coating value of the positive electrode film 50 Within the above range, it is indicated that the carbon material on the surface of the positive electrode active material is relatively dense and uniform, which is beneficial to improving the slip uniformity of the positive electrode film during the rolling process, reducing the stress concentration phenomenon in the positive electrode film, reducing the rebound degree of the positive electrode sheet, and improving the reliability of the battery cell.
[0035] In any embodiment, the lithium-containing transition metal phosphate particles include iron, and the iron dissolution rate of the positive electrode film is 658ppm-1921ppm, optionally 658ppm-1485ppm.
[0036] The iron dissolved in the positive electrode film mainly originates from the lithium transition metal phosphate (LMT) of the positive electrode active material. The iron dissolution rate depends on both the number of lattice defects in the LMT and the integrity and density of the carbon material on the surface of the positive electrode active material. A lower iron dissolution rate means fewer lattice defects in the LMT, which helps reduce lattice corrosion in weak acid environments. Furthermore, a more complete and dense carbon material on the surface of the positive electrode active material inhibits the dissolution of iron ions in weak acid environments. Positive electrode films with iron dissolution rates within the above range have relatively few lattice defects and complete and dense carbon material on the surface of the positive electrode active material. This improves the compressibility and slippage of particles in the positive electrode film under high rolling pressure, increases the compaction density of the positive electrode film, reduces stress concentration, improves the energy density of the battery, and also enhances battery reliability.
[0037] In any embodiment, the positive electrode film layer further includes a conductive agent, and the total area of the agglomerated region of the conductive agent accounts for 0.5%-2.5%, optionally 0.5%-1.7%, based on the total area of the cross-section of the positive electrode film layer along the thickness direction of the electrode sheet.
[0038] Based on the total area of the cross-section along the thickness direction of the positive electrode film, the total area ratio of the agglomerated region of the conductive agent is 0.5%-2.5%, indicating that the conductive agent in the positive electrode film is uniformly dispersed and easily forms a uniform conductive network. This is particularly beneficial for reducing the kinetic degradation caused by the increase in ion transport paths in thick coating films, and reducing local polarization and even lithium plating problems during battery cycling. Simultaneously, research shows that large particles in lithium transition metal phosphate are prone to rebound. The agglomerated area of the conductive agent within the above-mentioned range can suppress the rebound of lithium transition metal phosphate by means of the uniform distribution of the conductive agent, forming mechanical constraints on the particles and even the film layer, improving the cohesive force of the film layer, reducing the probability of seal area failure, and improving battery reliability.
[0039] In any embodiment, the conductive agent comprises carbon nanotubes, which include one or more of single-walled carbon nanotubes, few-walled carbon nanotubes, and multi-walled carbon nanotubes.
[0040] The high aspect ratio of carbon nanotubes facilitates the bonding of multiple cathode particles along their thickness, forming long-range conductive pathways and increasing interparticle binding forces. This improves the kinetic performance of thick-coated cathode films, reducing localized polarization and even lithium plating during cycling, thus extending battery cycle life. Furthermore, the network structure formed within the cathode film acts as a stress propagation bridge, effectively mitigating stress concentration, reducing electrode rebound, and improving the reliability of individual battery cells. Simultaneously, carbon nanotubes possess a high specific surface area and hollow structure, resulting in excellent electrolyte retention. Thick electrodes experience significant expansion during cycling, making electrolyte extrusion easier. The presence of carbon nanotubes in the cathode film enhances electrolyte retention in thick electrodes, mitigating capacity drops during cycling and improving cycle life.
[0041] In any embodiment, the conductive agent further includes conductive carbon black.
[0042] Conductive carbon black has a high specific surface area, thus exhibiting excellent electrolyte retention capacity. Thick electrodes experience greater expansion force during cycling, making it easier for the electrolyte to be squeezed out. The distribution of conductive carbon black in the positive electrode film helps improve the electrolyte retention capacity of thick electrodes, mitigating the phenomenon of capacity drop during battery cycling and improving battery cycle life.
[0043] In any embodiment, the agglomeration region of the conductive agent includes carbon nanotubes and conductive carbon black.
[0044] Researchers have found that carbon nanotubes are prone to agglomeration due to their high surface energy, which leads to uneven dispersion in the positive electrode film layer and fails to form an effective carbon nanotube network structure. Conductive carbon black and carbon nanotubes have relatively close surface energies, and can adsorb on the surface of carbon nanotubes to form a physical barrier, increase the resistance to agglomeration of carbon nanotubes, reduce direct contact between carbon nanotubes, thereby inhibiting the agglomeration phenomenon and improving the distribution uniformity of carbon nanotubes in the positive electrode film layer. On the one hand, this helps to improve the conductivity of the thickly coated positive electrode film layer and enhance the dynamic performance of the battery; on the other hand, it helps to exert the binding effect of carbon nanotubes on the positive electrode film layer, reduce the risk of peeling off of the thickly coated positive electrode film layer, and further improve the dynamic performance and cycle life of the battery. In addition, the agglomeration of carbon nanotubes in the agglomerated region of the conductive agent will also cause local ion transmission paths in the agglomerated region of the conductive agent to be blocked. The matching of conductive carbon black can improve the lithium ion transmission capacity in this region, reduce local polarization, and further improve the cycle stability of the battery.
[0045] In any embodiment, based on the mass of the positive electrode film layer, the mass content C1 of the carbon nanotubes satisfies: 0<C1≤2.5%, and the mass content C2 of the conductive carbon black satisfies: 0<C2≤2.5%.
[0046] When the mass contents of carbon nanotubes and conductive carbon black in the positive electrode film layer are within the above ranges, the agglomeration phenomenon of carbon nanotubes can be effectively alleviated and a good conductive network structure can be formed, thereby effectively reducing the stress concentration of the positive electrode film layer and improving the reliability of the battery cell; and increasing the electrolyte retention rate of the positive electrode plate during the long cycle process, reducing the polarization degree, and improving the capacity fading problem of the battery cell.
[0047] In any embodiment, the positive electrode film layer further comprises a dispersant, and the dispersant comprises hydrogenated nitrile butadiene rubber (HNBR).
[0048] HNBR is obtained by hydrogenating and saturating the double bonds of nitrile rubber. Its highly saturated main chain structure gives it excellent oil resistance, heat resistance, and aging resistance. This allows it to remain stable in different environments and systems when used as a dispersant, without easily degrading or deteriorating, thus effectively exerting its dispersing effect. The HNBR molecular chain contains both polar nitrile groups and non-polar hydrocarbon segments. The polar nitrile groups can interact with the hydroxyl groups (-OH) or metal oxide sites on the surface of lithium transition metal phosphate particles (such as hydrogen bonding and dipole interaction), enhancing the compatibility between particles and solvents, reducing the interfacial tension between particles and solvents, especially the interfacial tension of large particles, making the particles easier to disperse uniformly, reducing aggregation caused by hydrophobicity, improving the dispersibility of large particles in the positive electrode film, and reducing stress concentration caused by rebound; the non-polar hydrocarbon segments have good oleophilicity, and can extend and disperse well in non-polar or weakly polar media, so that the particles are uniformly dispersed in the medium. When HNBR adsorbs onto the surface of particles in the slurry, its long-chain molecules form a physical barrier around the particles, preventing them from approaching each other and aggregating, thus maintaining a relatively independent dispersion. Simultaneously, HNBR reduces the surface tension between the dispersion medium and the dispersed particles, making the particles easier to wet and promoting dispersion. Furthermore, it reduces the interfacial energy between particles, particularly minimizing the aggregation of conductive agents driven by interfacial energy, thereby improving the cycle life of individual battery cells.
[0049] In any embodiment, based on the mass of the positive electrode film, the mass content of the dispersant is 0.5%-2%.
[0050] When the mass content of the dispersant is within the above range, it can achieve uniform dispersion of particles in the positive electrode film while maintaining a high loading capacity, reduce the rebound caused by stress concentration in the thick-coated lithium transition metal phosphate positive electrode film, reduce the rebound rate of the positive electrode film, and improve the reliability of the battery cell.
[0051] In any embodiment, the porosity of the positive electrode film is 14%-28%.
[0052] Within the aforementioned range, the porosity of the positive electrode film is beneficial in two ways: firstly, it improves the electrolyte's liquid retention properties, enhances the ion diffusion of thick-coated electrodes and the positive electrode film, and improves the battery's kinetic performance; secondly, it can buffer the volume increase during rebound or charge / discharge processes, reduce the impact of expansion stress on the sealing area, and maintain the battery's high reliability.
[0053] In any embodiment, the battery cell further includes a separator disposed between the positive electrode and the negative electrode. The separator includes a base film, ceramic layers disposed on both sides of the base film, and an adhesive layer disposed on at least one side of the ceramic layers away from the base film. The adhesive layer is a continuous layer with a porous structure and includes a vinylidene fluoride polymer.
[0054] The separator provided in this application uses a porous continuous layer as the adhesive layer, which has a larger bonding area compared to the adhesive layers in the prior art, thus making the adhesion between the separator and the positive electrode film layer more firm and uniform. Particles with a particle size R1 satisfying R1≥1000nm are prone to stress concentration during cycling, leading to rebound problems. The separator provided in this application, using a porous continuous layer as the adhesive layer, is particularly suitable for thick-coated stacked cells, improving the rebound phenomenon of thick-coated stacked cells during long-cycle cycling, reducing the expansion stress inside the battery, and improving the reliability of the sealing area and the overall battery cell. In addition, thick-coated cells are prone to relative displacement between the electrode and the separator during the process of dragging the outer electrode and welding the tabs, making the film layer prone to powder shedding and even the positive and negative electrodes overlapping, resulting in the risk of internal short circuit. The porous continuous layer as the adhesive layer in this application embodiment can also reduce the above risks.
[0055] In any embodiment, the positive electrode film layer has a base coating layer in the bottom region near the positive electrode current collector, and the base coating layer satisfies at least one of the following conditions: (1) the base coating layer includes a conductive agent and a binder, the conductive agent includes carbon nanotubes and conductive carbon black, and the binder includes vinylidene fluoride polymer; (2) the thickness of the base coating layer is 0.5 μm-5 μm.
[0056] The undercoating provided in this application helps improve the adhesion between the positive electrode film and the positive electrode current collector and alleviates stress concentration at large particles, thereby reducing the rebound of the positive electrode film and improving the reliability of the battery cell. Simultaneously, compared to direct contact between the positive electrode current collector and the positive electrode film, the increased contact area between the undercoating and the positive electrode film helps increase the area for electron transport between the current collector and the positive electrode film, thereby reducing the internal resistance of the electrode and improving the battery's dynamic performance.
[0057] In any embodiment, the lithium transition metal phosphate particles in the positive electrode film layer comprise components represented by the following general formula: Li m Fe x P y O j Q qFormula I, wherein Q includes one or more of Al, Na, K, Mg, Cu, Mn, Cr, Zn, Pb, Ca, Co, Ni, Sr, Nb, V, Ti, B, S, Si, N, F, Cl, and Br, with 0.8≤m≤1.15, 0.9≤x≤1, 0.95≤y≤1, 3.5≤j≤4, and 0≤q≤0.1.
[0058] Selecting appropriate modifying element Q can improve the lattice change rate of positive electrode active material during lithium insertion / extraction process, reduce oxygen activity on particle surface, improve the structural stability of material, thereby improving the specific capacity utilization level of material during cycling and improving the cycle stability of battery cell.
[0059] In any embodiment, the lithium-containing transition metal phosphate particles include titanium, and the mass content of titanium is 500ppm-8000ppm, optionally 1000ppm-3000ppm, based on the total mass of the lithium-containing transition metal phosphate particles in the positive electrode film.
[0060] Introducing titanium into lithium transition metal phosphate particles requires adding a titanium source during the preparation of the cathode active material. Titanium sources are often inert materials, and their adhesion to the surface of the lithium transition metal phosphate raw material reduces reactivity and particle size growth. Increasing the graphitization degree of the cathode active material often requires higher sintering temperatures or longer sintering times, but this also increases the particle size in the cathode film, increasing stress concentration and potentially causing film detachment. In this embodiment, by adding a high content of titanium to the lithium transition metal phosphate particles, the reactivity of the raw materials for synthesizing the cathode active material is reduced. This allows the cathode active material to achieve a high degree of graphitization while controlling the proportion of large particles, reducing the rebound rate of the cathode film, and improving both battery energy density and reliability. Simultaneously, the doping of titanium in the cathode active material helps induce lattice distortion, reduces Li-O bond energy, increases lithium-ion transport rate, and improves the battery's kinetic performance. Uneven lithium-ion diffusion in thick coated films often results in a significant lithium-ion concentration gradient. This application improves the solid-phase transport rate of the positive electrode active material by adding a high content of titanium to lithium transition metal phosphate particles, thereby addressing the kinetics of thick electrode batteries.
[0061] In any embodiment, the lithium-containing transition metal phosphate particles include vanadium, and the mass content of vanadium is 500ppm-5000ppm, optionally 500ppm-3000ppm, based on the total mass of the lithium-containing transition metal phosphate particles in the positive electrode film.
[0062] Vanadium in the positive electrode film can exist in multiple valence states. Vanadium in the +5 valence state (V5+) can be doped into phosphorus sites. Due to its large radius, it can cause lattice distortion, expanding the diffusion channels for lithium ions, thereby improving the ionic conductivity of the positive electrode active material and enhancing the battery's kinetic performance. Vanadium in the +3 valence state (V... 3 Vanadium can be doped into transition metal sites, generating lithium vacancies through charge compensation, thereby improving the electronic conductivity of the positive electrode active material. Furthermore, the increased uniformity of vanadium distribution in lithium-containing transition metal phosphate particles helps to further improve the kinetic performance and reaction uniformity of the positive electrode film, thus enhancing the kinetic and cycle performance of the battery cell. Vanadium content within the aforementioned range contributes to improving the kinetic performance of the positive electrode sheet and the kinetic performance of thick-coated lithium-containing transition metal phosphate batteries. Simultaneously, the synergistic effect of titanium, vanadium, and carbon nanotubes in the positive electrode film helps to form a good three-dimensional network, further improving the electronic and ionic conductivity of the positive electrode film, thereby further enhancing the kinetic performance of thick-coated lithium-containing transition metal phosphate batteries.
[0063] In any embodiment, the flexible packaging material includes an aluminum-plastic composite film, optionally including one or more of aluminum, polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), nylon, polyethylene terephthalate (PET), and polyethylene (PE) forming a composite film with aluminum.
[0064] In any embodiment, at least one of the laminated cells is housed within the housing, the housing having a length dimension of L0, a width dimension of W0, and a thickness dimension of H0, wherein 450mm≤L0≤1300mm, 100mm≤W0≤150mm, and 14mm≤H0≤22mm.
[0065] In any embodiment, the length dimension L0 of the housing satisfies: 450mm≤L0≤650mm.
[0066] When the length dimension L0 of the casing satisfies 450mm≤L0≤650mm, the length of the battery cell is shorter, which helps to shorten the current diffusion path, reduce the internal resistance of the electrode, thereby reducing the heat generation of the battery and improving its dynamic performance. In addition, the shorter casing length helps to shorten the diffusion path of the electrolyte during the wetting process, improve the wetting rate and uniformity of the electrolyte, further promote the uniformity of lithium ion insertion and extraction during cycling, alleviate stress concentration, reduce the rebound amplitude of the film layer, and improve the reliability of the battery cell.
[0067] When the length dimension L0 of the casing satisfies 450mm≤L0≤650mm, the battery cell has a shorter length, which is beneficial to shorten the electron transport path, reduce the internal resistance of the battery, reduce the wetting distance of the electrolyte in the electrode pores, improve the wetting uniformity, and improve the dynamic performance of the thick coating film. Especially under fast charging conditions, it can reduce the phenomenon of uneven temperature rise and uneven current density in the length direction of the electrode.
[0068] In any embodiment, the length dimension L0 of the housing satisfies: 900mm≤L0≤1300mm.
[0069] When the length dimension L0 of the casing satisfies 900mm≤L0≤1300mm, the battery cell is relatively long, which helps to reduce the volume ratio of the casing in the battery cell and increase the load ratio of active materials. At the same time, a longer battery cell can reduce the number of batteries required in the battery module, simplify the structural design of the battery module, reduce the number and complexity of structural components in the module, thereby improving the space utilization of the battery pack and thus helping to improve the volumetric energy density of the battery cell.
[0070] In any embodiment, at 25°C, the capacity of the battery cell is 105Ah-300Ah, and can be selected as 150Ah-190Ah.
[0071] A second aspect of this application provides a battery device including the battery cell of the first aspect of this application.
[0072] A third aspect of this application provides an electrical device, including the battery device of the second aspect of this application, the battery device being used to provide electrical energy.
[0073] The fourth aspect of this application provides an energy storage device, including the battery device of the second aspect of this application, the battery device being used to store electrical energy. Attached Figure Description
[0074] Figure 1 is a front view of a battery cell according to an embodiment of this application;
[0075] Figure 2 is a schematic diagram of the diaphragm according to one embodiment of this application;
[0076] Figure 3 is a schematic diagram of the diaphragm in the prior art;
[0077] Figure 4 is a schematic diagram of an electrical device according to an embodiment of this application. 5 Battery cell; 50 Housing; 51 First sealing area; 52 Second sealing area; 53 Lead-out element; 20 Separator; 201 Base film; 202 Ceramic layer; 203 Adhesive layer; X Length direction; Y Width direction; Z Thickness direction. Detailed Implementation
[0078] The following detailed description, with appropriate reference to the accompanying drawings, discloses embodiments of the battery cell, battery device, power consumption device, and energy storage device of this application. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided for the purpose of enabling those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.
[0079] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0080] Unless otherwise specified, all embodiments and optional embodiments of this application may be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure of this application.
[0081] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions, and such technical solutions shall be deemed to be included in the disclosure of this application.
[0082] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the method may also include step (c), indicating that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0083] In this application, the terms "multiple" or "various" refer to two or more kinds.
[0084] Unless otherwise stated, the terms used in this application have the common meanings as commonly understood by those skilled in the art.
[0085] Unless otherwise stated, the values of the parameters mentioned in this application can be determined using various testing methods commonly used in the art, for example, according to the testing methods given in the embodiments of this application. Unless otherwise stated, the test temperature for each parameter is 25°C.
[0086] In embodiments of this application, the battery device may include one or more battery cell assemblies for providing voltage and capacity. A battery cell assembly may include multiple pouch cell batteries connected in series, parallel, or a combination of these pouch cell batteries via a busbar. For example, a battery cell assembly is typically formed by arranging multiple pouch cell batteries; a battery cell assembly may also be a battery module, which is formed by arranging and fixing multiple pouch cell batteries into a single module. As an example, a battery module may be formed by bundling multiple battery cells together with cable ties.
[0087] The battery device can be a battery pack, which includes a housing and one or more individual battery cells housed within the housing. The individual battery cells can be battery modules, which can be housed within the housing by fixing the battery modules to the housing; alternatively, multiple pouch battery cells can be directly fixed to the housing and housed within the housing.
[0088] In embodiments of this application, the housing may include a first housing and a second housing. The first housing and the second housing are fastened together to form a closed space inside the housing for housing individual battery cells. Here, "closed" refers to covering or shutting down; it can be sealed or unsealed. The first housing may be a top cover or a bottom plate. For example, the housing may include a top cover, a frame, and a bottom plate. The top cover and the bottom plate are respectively connected to the frame, forming a closed space inside the housing for housing individual battery cells.
[0089] In embodiments of this application, the housing can be part of the vehicle's chassis structure. For example, a portion of the housing can be at least a part of the vehicle's floor, or a portion of the housing can be at least a part of the vehicle's crossbeams and longitudinal beams.
[0090] In this embodiment, the battery cell can be a rechargeable battery, which refers to a battery cell that can be recharged after discharge to activate the active materials and continue to be used; the battery cell can be a lithium-ion battery. The battery cell can be flat.
[0091] The battery mentioned in the embodiments of this application can be a single physical module comprising one or more battery cells to provide higher voltage and capacity. For example, the battery mentioned in this application can include battery cells, battery modules, or battery packs.
[0092] A single battery cell is the smallest unit that makes up a battery, capable of charging and discharging independently. When there are multiple battery cells, they are connected in series, parallel, or a combination of both via a busbar. In some embodiments, the battery can be a battery module; when there are multiple battery cells, they are arranged and fixed to form a battery module. In some embodiments, the battery can be a battery pack, comprising a housing and battery cells, with the battery cells or battery modules housed within the housing. In some embodiments, the housing can be part of the vehicle's chassis structure. For example, a portion of the housing can be at least part of the vehicle's floor, or a portion of the housing can be at least part of the vehicle's crossbeams and longitudinal beams.
[0093] In some implementations, the battery can be an energy storage device. Energy storage devices include energy storage containers, energy storage cabinets, etc.
[0094] In some embodiments, individual battery cells can be assembled into battery modules, and the number of battery cells contained in a battery module can be multiple, with the specific number adjustable according to the application and capacity of the battery module. In some embodiments, the above-mentioned battery modules can also be assembled into battery packs, and the number of battery modules contained in the battery packs can be adjusted according to the application and capacity of the battery packs.
[0095] A single battery cell includes electrode components and an electrolyte.
[0096] Electrode assemblies typically include positive and negative electrodes. The negative electrode is the electrode that absorbs or lithiates lithium ions during charging and releases or delithiates lithium during discharging. The positive electrode is the electrode that absorbs or delithiates lithium ions during charging and absorbs or lithiates lithium during discharging.
[0097] While lithium-containing transition metal phosphates offer significant advantages in cycle stability as positive electrode active materials, their intrinsic specific capacity is significantly lower than that of ternary materials. The applicant has discovered that employing a thick coating process in the electrode fabrication stage is an effective technique to compensate for the low capacity of lithium-containing phosphates, and using a soft-pack casing further reduces weight and improves the theoretical mass energy density of the battery cell. However, this process improvement also brings new technical challenges: on the one hand, thicker electrodes experience higher expansion stress during long-term cycling; on the other hand, the heat generated by thicker electrodes during operation is difficult to dissipate effectively, leading to localized high temperatures that cause electrolyte decomposition, gas generation, and increased internal battery pressure. Due to the limited mechanical strength of soft-pack packaging, internal expansion and increased pressure may cause cell bulging or even package rupture and failure.
[0098] This application provides a battery cell, as shown in FIG1, comprising a stacked battery cell and a housing 50, wherein the stacked battery cell is housed within the housing 50, and the housing 50 is made of a soft-pack material; the housing 50 includes a first sealing area 51, which is disposed at at least one end of the stacked battery cell extending along the width direction (Y direction); the first sealing area includes a double-folded edge structure extending along the length direction (X direction), and an encapsulating adhesive is disposed on the double-folded edge structure, the encapsulating adhesive being continuously disposed along the length direction (X direction) and fixing the double-folded edge structure; the stacked battery cell includes a positive electrode sheet, a negative electrode sheet, and a... The electrolyte, the positive electrode sheet includes a positive current collector and a positive electrode film layer disposed on at least one side of the positive current collector, the positive electrode film layer including lithium transition metal phosphate particles, and at least a portion of the surface of the lithium transition metal phosphate particles being disposed with carbon material; based on the total area of particles in the cross-section of the positive electrode film layer along the thickness direction of the positive electrode sheet, the area ratio of particles with a particle size R1 satisfying R1≥1000nm is 12%-50%; the single-sided thickness of the positive electrode film layer is denoted as H, where H is 70μm-120μm; when the battery cell is in a fully discharged state, the compaction density of the positive electrode sheet is 2.3g / cm³. 3 -2.6g / cm 3 The electrolyte includes a solvent, which includes dimethyl carbonate (DMC); the mass percentage of dimethyl carbonate is 18%-32% based on the total mass of the electrolyte.
[0099] Lithium-containing transition metal phosphates generally have relatively low specific capacity. Studies have shown that when the thickness H of the positive electrode film on one side is less than 70 μm, the battery capacity is difficult to meet market demand. In the embodiments of this application, by controlling the thickness H of the positive electrode film on one side within the range of 70 μm-120 μm, it is beneficial to increase the space utilization rate of the active material and further adopt a soft-pack material shell, thereby reducing the weight of the battery cell and improving the mass energy density of the battery. However, a thicker positive electrode film undergoes significant volume changes during charge-discharge cycles due to lithium insertion and delithiation, leading to the accumulation of mechanical stress, which in turn causes the electrode material to expand and contract, resulting in electrode rebound and increased thickness, increasing the mechanical stress on the packaging structure. At the same time, a thicker film means that internal heat is more difficult to conduct, easily leading to local overheating, exacerbating the side reactions and gas production of the electrolyte, and further increasing the internal pressure of the battery cell. Compared with the wound type, the stacked cell structure reduces the corner gap and improves the volumetric energy density, but the stacked cell lacks the binding effect of the wound structure, which has less limitation on the rebound of the thickly coated film layer, thus degrading the reliability of the battery cell. Compared to rigid-shell materials, pouch cells have lower mechanical strength and are less able to withstand internal pressure. Furthermore, pouch cells have lower thermal conductivity, making them more prone to heat buildup inside individual cells and further exacerbating gas generation issues. During long-term use, excessive internal pressure may cause the sealed area to be breached.
[0100] In this embodiment, the first sealing area includes a double-folded edge structure extending along the long side to further enhance the sealing strength of the first sealing area. The double-folded edge forms multiple sealing barriers by folding and encapsulating the soft-pack material twice. Even if the first folded edge structure experiences rebound stress due to the high thickness of the positive electrode film layer in the cell, or defects caused by electrolyte gas generation, the second folded edge structure can still maintain a seal. Simultaneously, due to battery processing, the soft-pack material is bonded by hot-melt bonding, and the double-folded edge makes the heat-sealed area more uniform, improving the situation of poor sealing in local areas. The sealing point is a weak point in the mechanical strength of the soft-pack cell. To further enhance the reliability of the encapsulation, the inventors set encapsulating adhesive on the double-folded edge structure. The encapsulating adhesive is continuously set along the long side and fixes the double-folded edge structure, which can cover microscopic cracks or defects in the heat-sealed area of the soft-pack material sealing area; and the double-folded edge structure has a certain elastic memory after heat sealing, and may rebound after long-term use. The encapsulating adhesive can fix the double-folded edge structure and maintain its stability. In this embodiment, the compaction density of the positive electrode sheet is further controlled to be 2.3 g / cm³ when the battery cell is fully discharged. 3 -2.6g / cm 3This approach, on the one hand, enables the battery cell to have a higher capacity, and on the other hand, provides a certain buffer space between the particle stacking structure, reducing the stress exerted on the encapsulation structure by electrode rebound. To further reduce the internal stress of the battery cell, the inventors controlled the area ratio of particles with a particle size R1 satisfying R1≥1000nm in the positive electrode film and the mass ratio of dimethyl carbonate in the electrolyte. The inventors found that, under the same expansion rate, the expansion of small particles is more easily absorbed through the micropore structure between particles than that of large particles. The absolute value of the expansion change of large particles is larger and more difficult to dissipate. When the area ratio of particles with a particle size R1 satisfying R1≥1000nm is greater than 50%, it is easy to cause stress concentration, resulting in obvious rebound and increasing the internal pressure of the battery cell. When the area ratio of particles with a particle size R1 satisfying R1≥1000nm is less than 12%, it will limit the improvement of the gradation and compaction density of the positive electrode film, and cannot effectively improve the battery capacity. Therefore, controlling the particle size R1 to satisfy R1≥1000nm with a particle area ratio of 12%-50% is beneficial for further improving the reliability of battery cells while maintaining energy density. Dimethyl carbonate (DMC) has many advantages such as low viscosity, excellent low-temperature performance, and low cost. However, if the mass ratio of DMC in the electrolyte is less than 18%, it is difficult to form a low-viscosity system, making it difficult to improve the overall ionic conductivity of the electrolyte, increasing the ohmic impedance inside the battery, and thus leading to greater Joule heat. Furthermore, chain carbonates have weak oxidation resistance, and the symmetrical structure of DMC is more prone to decomposition under high voltage or high temperature environments. If the mass ratio of DMC is higher than 32%, severe gas generation during long-cycle operation will occur, exacerbating the probability of encapsulation failure. By controlling the mass ratio of DMC in the electrolyte to 18%-32%, the low viscosity of the electrolyte and the risk of gas generation can be balanced. The above technical measures work synergistically to achieve a balance between battery energy density and reliability.
[0101] In this application, the term "double-folded edge" refers to the reinforced structure formed by folding the sealing area in half. By initially folding the sealing area and then bending it again in the direction or opposite to the initial fold, the sealing area exhibits greater strength compared to a single-folded edge structure, capable of withstanding greater internal pressure without being forced open and failing. Further "multiple folds," however, exponentially increase the manufacturing difficulty and cost without significantly improving the strength of the sealing area.
[0102] Lithium-containing transition metal phosphates refer to phosphate materials containing lithium and transition metal elements, and can be detected by any method known in the art. For example, they can be detected by combining X-ray diffraction (XRD) with energy dispersive spectroscopy (EDS).
[0103] In this application, the term "particle" refers to a particle in the positive electrode film layer that has a recognizable complete boundary in the field of view at a certain magnification, such as 10,000x. Defects and scratches may exist inside the particle, but a complete boundary sufficient to divide the particle cannot be identified inside the particle.
[0104] The particle identification method is as follows: The positive electrode film layer is cut along the thickness direction of the electrode sheet using an argon ion beam (for example, a Leica EMTIC3XCP device can be used, operating voltage: 6kV, operating time: 6h). After exposing the cut surface, a scanning electron microscope (SEM) is used (for example, a Hitachi SU8230 device can be used, operating voltage: 3kV, beam current: high, probe model: U (LA100), working distance <5mm) to observe the cut surface along the thickness direction of the electrode sheet. Images are acquired using a field emission scanning electron microscope at a non-edge location in the cut surface of the positive electrode film layer (after observing the electrode edge under the SEM, the field of view is adjusted to the center of the sample) in secondary electron mode. Electron micrographs are taken at 10kx magnification, and the particles in the electron micrographs are analyzed using ImageJ software (1.46r, win64 version). The specific steps for using ImageJ software are as follows: Load the scanning electron microscope (SEM) image to be analyzed; use the Cellpose plugin to identify particles, and then perform manual corrections; use ImageJ to read and analyze data. The specific method for using the Cellpose plugin to identify particles is as follows: Set the segmentation diameter parameter (diameter in the Segmentation module) to 15 pixels, click "runcyto3" to identify particles; manually mark particles in the image that were not identified by the software, were not fully identified, or were identified incorrectly. Particles that were not identified by the software, were not fully identified, or were identified incorrectly mainly include the following: 1. Particles that are too large or have scratches on their surface, making them unidentifiable or incompletely identifiable; 2. During argon ion beam cutting, scratches may be generated on the particle surface, and the software may misinterpret these scratches as particle boundaries, leading to identification errors; 3. Particles that are too small and were not successfully identified; 4. Particles located at the edge of the SEM field of view, with the interior penetrated by the edge, preventing a complete view of the morphology, resulting in identification errors due to partial identification replacing the whole.For the unidentified or misidentified particles mentioned above, manual calibration is performed as follows: Particles located at the edges of the scanning electron microscope that are not fully displayed are deleted; It is determined whether other unidentified or misidentified particles have internal cracks or scratches. If no cracks or scratches are found, the particle is considered a single particle, and its boundary is manually marked based on observation; If cracks or scratches are found within the particle, it is determined whether the cracks or scratches penetrate the particle. If not, it is considered a single particle and manually marked; If the cracks or scratches penetrate the particle, it is determined whether the cracks or scratches are linear or irregular; If the cracks or scratches are irregular, they are considered the boundary between particles, and particles are divided along this boundary; If the cracks or scratches are linear, contrast is compared; If the contrast is not obvious and there is no crack-like appearance, it is considered a scratch and marked as a single particle; If the contrast is strong and there is a crack-like appearance, it is considered the boundary between particles and marked as two particles. After manual marking, irrelevant information from the automatic image processing is deleted, thus completing the particle identification and marking in the image.
[0105] It is understandable that the particles in the cross-section of the positive electrode film along the thickness direction, especially those larger than 50 nm, mainly originate from the positive electrode active material. Therefore, the embodiments of this application can accurately and objectively reflect the distribution of lithium transition metal phosphate particles in the positive electrode film by observing and statistically analyzing the particle area in the cross-section of the positive electrode along the thickness direction.
[0106] In existing technologies, laser particle size analyzers are typically used to statistically analyze the particle size of positive electrode active materials using Malvern laser diffraction. However, the applicant's research indicates that because lithium-containing transition metal phosphate particles are prone to agglomeration, the test results obtained using Malvern laser diffraction, based on the principle of laser scattering, often only reflect the particle size of the agglomerates. This does not accurately reflect the particle size within the positive electrode active material, nor does it reflect the dispersion state of the positive electrode active material in the film layer, as the dispersion of the positive electrode active material in the film layer increases during slurry preparation and film rolling. The test results obtained by Malvern laser diffraction are affected by the particle size, specific surface area, and degree of agglomeration of the positive electrode active material. Compared to the actual dispersion in the electrode sheet, the number of large particles obtained by this test is lower than the actual value, while the number of small particles is higher. Therefore, the particle size obtained by Malvern laser diffraction cannot be equated with or analogized to the particle size statistically obtained in the embodiments of this application.
[0107] The specific method for testing the area ratio of particles with a diameter R1 satisfying R1≥1000nm in the cross-section of the positive electrode film along the electrode thickness direction is as follows: Particles in the positive electrode film are identified according to the method described above in this application. The images after particle identification and labeling are imported into ImageJ software for analysis. The scale is set based on the scanning electron microscope (SEM) images. The particle diameter, area, sphericity, and roughness of the particles in the cross-section along the electrode thickness direction of the positive electrode film are statistically analyzed using the "Feret diameter," "Area," "Round," and "Solidity" analysis functions. According to the software manual (ImageJ User Guide IJ 1.46r), the obtained "Feret" parameter represents the maximum spacing between all parallel lines in the two-dimensional projection of the particle, thus characterizing the particle diameter; the obtained "Area" parameter represents the pixel area of the particle. To ensure a statistically significant sample size, no fewer than 10 SEM images are collected for each film layer, and the particle diameter of no fewer than 1000 particles is statistically analyzed. Because particles smaller than 50nm are prone to significant errors during statistical analysis and are difficult to accurately identify, and because the particle size of conductive agents is generally smaller than 50nm, which can also introduce large errors into the statistical results, particles smaller than 50nm are not counted in the particle size statistics of this application, and the statistical data of particles whose AR, Round, or Solidity is displayed as "NaN" are deleted. The sum of the "Area" parameters of particles with a particle size R1 satisfying R1≥1000nm and the sum of the "Area" parameters of all particles are calculated, and these are respectively used as the area of particles with a particle size R1 satisfying R1≥1000nm and the total area of the counted particles. The sum of the areas of particles with a particle size R1 satisfying R1≥1000nm divided by the total area of the counted particles is used as the proportion of the area of particles with a particle size R1 satisfying R1≥1000nm in the cross-section of the positive electrode film along the thickness direction of the electrode sheet.
[0108] In some embodiments, based on the total area of particles in a cross-section of the positive electrode film along the thickness direction of the positive electrode sheet, the percentage of particle area with a particle size R1 satisfying R1≥1000nm can be selected as 12%, 12.11%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, etc. 32%, 33%, 34%, 34.89%, 34.97%, 35%, 36%, 36.71%, 36.75%, 36.83%, 36.92%, 36.95%, 37%, 38%, 38.09%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 49.99%, 50%, or any range of two of the above.
[0109] In some embodiments, the thickness of one side of the positive electrode film is denoted as H, which can be selected from 70 μm, 70.45 μm, 75 μm, 80 μm, 85 μm, 90 μm, 91.88 μm, 95 μm, 96.75 μm, 100 μm, 105 μm, 106.02 μm, 106.09 μm, 106.10 μm, 106.34 μm, 106.66 μm, 106.79 μm, 110 μm, 115 μm, 119.49 μm, 120 μm or any value range between the above two.
[0110] In some embodiments, when the battery cell is in a fully discharged state, the compaction density of the positive electrode sheet can be selected as 2.3 g / cm³. 3 2.31 g / cm 3 2.32 g / cm 3 2.33 g / cm 3 2.34 g / cm 3 2.35g / cm 3 2.36 g / cm 3 2.37 g / cm 3 2.38g / cm 3 2.39 g / cm 3 2.4g / cm 3 2.41 g / cm 3 2.42 g / cm 3 2.43 g / cm 3 2.44 g / cm 3 2.45g / cm 3 2.46 g / cm 3 2.47 g / cm 3 2.48 g / cm 3 2.49 g / cm 3 2.5g / cm 3 2.51g / cm 3 2.52g / cm 3 2.53g / cm 3 2.54 g / cm 3 2.55g / cm 3 2.56 g / cm 3 2.57g / cm 3 2.58g / cm 3 2.59g / cm 3 2.6g / cm 3 Or the range of values between any two of the above.
[0111] In this application, the fully discharged state refers to the state after the battery is placed in a 25°C oven environment, left to stand for 2 hours, and the battery temperature is maintained at 25°C, and then discharged at a constant current of 1 / 3C to 2.5V and then discharged at a constant current of 0.1C to 2.0V.
[0112] In this application, the compaction density of the positive electrode sheet can be tested using methods known in the art. As an example, the battery is placed in a 25°C oven environment and left to stand for 2 hours. After the battery temperature is maintained at 25°C, the battery is discharged at a constant current of 1 / 3C to 2.5V and then discharged at a constant current of 0.1C to 2.0V. The battery is disassembled to obtain the positive electrode sheet. The residual electrolyte is treated with dimethyl carbonate solvent, the electrode sheet is dried, and it is cut into small circular pieces with an area of S. The mass of the circular pieces is obtained as W1, and the thickness of the positive electrode sheet is measured using a micrometer. Then, the positive electrode film layer of the weighed electrode sheet is wiped off, the mass of the current collector is weighed and recorded as W2, and the thickness of the current collector is measured using a micrometer. Then, the compaction density of the positive electrode sheet is PD=(W1-W2) / [(T1-T2)×S].
[0113] In some embodiments, the mass percentage of dimethyl carbonate, based on the total mass of the electrolyte, can be selected as 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, or any range between the two above.
[0114] In some embodiments, the encapsulating adhesive includes a strip of blue adhesive. This strip of blue adhesive has high viscosity, resulting in a stronger bond to the casing sealing area, further enhancing the strength of the first sealing area and improving the reliability of the battery cell.
[0115] Dimethyl carbonate exhibits good solubility for lithium hexafluorophosphate, providing a sufficient lithium-ion concentration as an electrolyte component to meet the necessary ion conduction requirements. Furthermore, the low viscosity of dimethyl carbonate helps improve the ionic conductivity of the electrolyte, thereby enhancing the rate performance and low-temperature performance of individual battery cells.
[0116] In any embodiment, the thickness of the positive electrode film on one side is denoted as H, where H is 90μm-120μm, and can be selected as 100μm-120μm.
[0117] A single-sided thickness of the positive electrode film within the aforementioned range is beneficial for further improving energy density. The applicant discovered that when the single-sided thickness of the positive electrode film exceeds 100 μm, the rebound phenomenon of the positive electrode sheet becomes more severe. The embodiments of this application, through a double-folded edge structure in the first sealing region, strengthen the structural strength of the casing, reducing the probability of the seal being broken due to internal stress caused by film rebound. This enhances the reliability of the battery while maintaining a high energy density.
[0118] In some embodiments, as shown in FIG1, the housing 50 includes at least one second sealing area 52, the second sealing area 52 being disposed along the length direction of the housing at at least one end of the laminated cell, the second sealing area 52 being disposed on the tab side of the laminated cell.
[0119] It is understandable that the positive and negative electrodes can be located on the same side of the laminated cell, as shown in Figure 4; or they can be located on opposite sides of the laminated cell.
[0120] In some embodiments, the battery cell 5 further includes a lead 53 connected to the tab of the battery cell. For example, the lead 53 can be soldered to the tab. The lead 53 is a conductive element, and at least a portion of the lead 53 is located outside the housing 50. The lead 53 serves as the electrode lead-out end of the battery cell 5, facilitating electrical connection between the battery cell 5 and other battery cells 5 or other components. For example, the lead 53 can be in the form of a sheet.
[0121] Correspondingly, lead-out element 53 also includes a positive lead-out element and a negative lead-out element, with the positive lead-out element connected to the positive electrode tab and the negative lead-out element connected to the negative electrode tab.
[0122] In some implementations, the second sealing area is located on the tab side. The tab needs to be connected to the lead-out component. The connection strength between the lead-out component and the casing material is relatively weak, which makes it easier for gas to escape from the second sealing area. This facilitates directional pressure relief of the battery, reduces the impact on adjacent cells when the seal fails, and improves the overall safety and reliability of the battery device.
[0123] In some embodiments, the outer periphery of the laminated cell is provided with a plurality of rubber rings that surround in the width direction, and the rubber rings that surround in the width direction are spaced apart in the length direction.
[0124] The arrangement of rubber rings along the width of the cell at intervals along the length direction helps to increase the binding force on the cell, which is especially suitable for battery cells with thick coating layers. It can effectively reduce the rebound rate of the positive electrode film and the rebound pressure on the sealing area, thereby further reducing the probability of sealing area failure and improving the reliability of the battery cell.
[0125] In some embodiments, based on the total area of particles in the cross-section of the positive electrode film along the thickness direction of the positive electrode sheet, the area ratio of particles with a particle size R1 satisfying R1≥1000nm is 12%-37%.
[0126] When the particle area ratio of particles with a particle size R1 that satisfies R1≥1000nm is within the above range, the expansion force exerted by the rebound of large particles on the soft-pack material and sealing area is further reduced, thereby improving the reliability of the battery cell.
[0127] In some embodiments, in the cross-section of the positive electrode film along the electrode thickness direction, the median L of the spheroidality in the cumulative distribution curve of the spheroidality area of particles with a particle size R1 satisfying R1≥1000nm is... R1A50 The value is 0.6-0.8, which can be selected as 0.65-0.75, and further can be selected as 0.67-0.75.
[0128] The specific method for testing the sphericity of particles with a diameter R1 satisfying R1≥1000nm in a cross-section along the thickness direction of the positive electrode film is as follows: Particles in the positive electrode film are identified using the method described above in this application. Images after particle identification and labeling are imported into ImageJ software for analysis. Scale settings are completed based on the scanning electron microscope image. The particle diameter and sphericity of the particles in the cross-section along the thickness direction of the positive electrode film are statistically analyzed using the "Feret diameter" and "Round" analysis functions. According to the software manual (ImageJ User Guide IJ 1.46r), the "Feret" parameter obtained from the analysis represents the maximum spacing between all parallel lines in the two-dimensional projection of the particle, thus characterizing the particle diameter. According to the software manual (ImageJ User Guide IJ 1.46r), the "Round" parameter obtained from the analysis represents the ratio of the pixel area of the particle to the area of a circle with the fitted major axis as its diameter, which can be used to characterize the sphericity of the particle. The closer the particle is to a sphere, the closer the ratio of the pixel area to the area of the circle with the fitted major axis as its diameter is to 1. Therefore, the "Round" parameter of the obtained particles is used to characterize the sphericity of the particles. To ensure a statistically significant sample size, at least 10 scanning electron microscope images were acquired for each film layer, and the particle size of at least 1000 particles was counted. The sphericity of the obtained particles with a particle size R1 satisfying R1≥1000nm was arranged in ascending order, and the cumulative distribution curve of the sphericity of the cathode film particles was obtained by plotting sphericity on the horizontal axis and the cumulative area ratio on the vertical axis. R1A50 The cumulative distribution curve of the sphericity L value for particles with particle size R1 satisfying R1≥1000nm is the sphericity L value corresponding to the cumulative area ratio of the vertical axis being 50%.
[0129] In some embodiments, in the cross-section of the positive electrode film along the electrode thickness direction, the median L of the spheroidality in the cumulative distribution curve of the spheroidality area of particles with a particle size R1 satisfying R1≥1000nm is... R1A50 The values can be 0.6, 0.61, 0.62, 0.63, 0.64, 0.65, 0.66, 0.67, 0.673, 0.68, 0.687, 0.69, 0.7, 0.71, 0.72, 0.73, 0.74, 0.745, 0.75, 0.76, 0.77, 0.78, 0.79, 0.8, or any value range between the two mentioned above.
[0130] Those skilled in the art can control the sphericity of particles using any known process. For example, the sphericity of particles can be adjusted through processes such as grinding, polishing, chemical etching, mechanical stirring, extrusion, coating, granulation, and adding surfactants, as well as by adjusting the parameters of each process.
[0131] In the cumulative area distribution curve of spheroidal density for particles with a diameter R1 satisfying R1≥1000nm, L R1A50 Within the aforementioned range, the particles are more approximately spherical, making them easy to roll. They can offset the volume changes caused by the rebound of the thick positive electrode film or the expansion during charging and discharging within a certain spatial range through the rearrangement of the stacking relationship, thereby reducing the burden on the first sealing area and improving the reliability of the battery cell.
[0132] In some embodiments, in the cross-section of the positive electrode film layer along the electrode thickness direction, the uniformity of the distribution of particles with a particle size R1 satisfying R1≥1000nm is less than or equal to 5%, which can be selected as 0.2%-2%, and more preferably 0.2%-0.9%.
[0133] The uniformity of particle distribution with particle size R1 satisfying R1≥1000nm in the cross-section of the positive electrode film along the electrode thickness direction can be tested using methods known in the art. As an example, the cross-section of the positive electrode film along the electrode thickness direction is divided into three layers of equal thickness: a lower layer close to the positive current collector, an upper layer far from the positive current collector, and a middle layer between the upper and lower layers. Ten non-overlapping fields of view are selected in each of the upper, middle, and lower layers, and scanning electron microscope (SEM) images are taken at 10kx magnification. The 30 SEM images are imported into ImageJ software for analysis. According to the above-mentioned "test method for the area proportion of particles with diameter R1 satisfying R1≥1000nm in the cross-section of the positive electrode film along the electrode thickness direction", the area proportion of particles with diameter R1 satisfying R1≥1000nm in the 30 images is obtained, totaling 30 values. The range of the 30 values is the distribution uniformity of particles with diameter R1 satisfying R1≥1000nm in the cross-section of the positive electrode film along the electrode thickness direction, where the range is the difference between the maximum and minimum values among the 30 values. The smaller the uniformity of the distribution of particles with a diameter R1 of ≥1000nm in the cross-section of the positive electrode film along the thickness direction of the electrode sheet, the more uniform the distribution of large particles with a diameter R1 of ≥1000nm in the positive electrode film. This helps to reduce stress concentration at large particles in the positive electrode film, reduce the rebound rate of the positive electrode film and the impact on the casing and sealing area, and improve the reliability of the battery cell.
[0134] In some embodiments, the uniformity of particle distribution with particle size R1 satisfying R1≥1000nm in the cross-section of the positive electrode film along the electrode thickness direction can be selected as 0.01%, 0.1%, 0.2%, 0.24%, 0.3%, 0.4%, 0.45%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 0.99%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.47%, 1.5%, 1.6%, 1.7%, 1.8%, 1.81%, 1.82%, 1.85%, 1.9%, 1.94%, 1.95%, 1.98%, 1 0.99%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.45%, 2.5%, 2.6%, 2.7%, 2.8%, 2.81%, 2.82%, 2.83%, 2.85%, 2.9%, 2.94%, 2.98%, 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 4.91%, 5%, or any range of two of the above.
[0135] In some embodiments, the uniformity of particle distribution with particle size R1 satisfying R1≥1000nm in the cross-section of the positive electrode film along the electrode thickness direction is 0.2%-2%.
[0136] In some embodiments, the uniformity of particle distribution with particle size R1 satisfying R1≥1000nm in the cross-section of the positive electrode film along the electrode thickness direction is 0.2%-0.9%.
[0137] If the uniformity of particle distribution with particle size R1 satisfying R1≥1000nm in the cross-section of the positive electrode film along the thickness direction of the electrode sheet is within the above range, it can effectively reduce the stress concentration in local areas of the film layer, so that the rebound stress of the thick coating film layer during cycling can be uniformly distributed throughout the entire area of the film layer, reducing the rebound rate of the positive electrode film layer, thereby improving the battery energy density while reducing the probability of packaging structure failure and improving battery reliability.
[0138] In some embodiments, the solvent in the electrolyte further includes one or both of ethyl methyl carbonate (EMC) and ethylene carbonate (EC).
[0139] The types and quantities of solvents and electrolyte salts in an electrolyte can be obtained by methods known to those skilled in the art. For example, the composition of the electrolyte can be determined by liquid chromatography, ultraviolet spectrophotometry, or ultraviolet-visible spectrophotometry. Exemplarily, a battery cell is disassembled, and the free electrolyte is obtained from it. The free electrolyte in the battery cell is diluted 3 to 10 times with acetonitrile to obtain a diluted electrolyte solution to be tested. Using a GC-MS 3100 organic component gas chromatograph, the above diluted electrolyte solution is placed in the instrument for full-scan qualitative analysis. The injection port temperature is 250°C, and the scan range is 35 μm to 270 μm. After the test, a total ion chromatogram of each organic compound is obtained. The peak positions in the chromatograms are compared with the corresponding organic compounds, and the percentage content of each organic compound is calculated based on the peak area. For example, an ion chromatograph (IC) can be used to test the content of inorganic substances in an electrolyte. A quantitative amount of electrolyte (the concentration of the dilution solution is in the middle of the standard curve) is weighed, and the volume is adjusted to 100 mL with ultrapure water. The ion chromatograph automatically injects the sample for detection, tests the ion chromatogram of inorganic substances, and compares the corresponding inorganic substances according to the peak positions of the chromatogram.
[0140] In some embodiments, the mass percentage of ethyl methyl carbonate (EMC) is 39%-49% based on the total mass of the electrolyte.
[0141] In some embodiments, the mass percentage of ethyl methyl carbonate (EMC) based on the total mass of the electrolyte can be selected as 39%, 40%, 40.3%, 41%, 42%, 43%, 43.3%, 44%, 45%, 46%, 47%, 47.3%, 48%, 49%, or any range between the two above.
[0142] Ethyl methyl carbonate (EMC) has a viscosity of 0.65 mPa·s at 25°C, which is higher than that of DMC but lower than that of EC. It also maintains good fluidity at low temperatures. Together with DMC, it helps to reduce the overall viscosity of the electrolyte, increase the migration rate of lithium ions in the electrolyte, and reduce Joule heating. Furthermore, compared with DMC, EMC has higher oxidation stability and thermal stability, which further reduces the gas production caused by electrolyte decomposition and improves the reliability of individual battery cells.
[0143] In some embodiments, the mass percentage of ethylene carbonate (EC) is 13%-22% based on the total mass of the electrolyte.
[0144] In some embodiments, based on the total mass of the electrolyte, the mass percentage of ethylene carbonate (EC) can be selected as 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, or any value range between the two above.
[0145] Ethylene carbonate (EC) has an extremely high dielectric constant, which can effectively dissolve lithium salts, improve the ionic conductivity of the electrolyte, and ensure the smooth migration of lithium ions. EC within the above-mentioned mass percentage range can decompose on the surface of the negative electrode active material and form a stable SEI film, reducing side reactions and improving cycle life.
[0146] In some embodiments, the total mass percentage of ethyl methyl carbonate (EMC) and ethylene carbonate (EC) is 52%-71% based on the total mass of the electrolyte.
[0147] In some embodiments, the total mass percentage of ethyl methyl carbonate (EMC) and ethylene carbonate (EC), based on the total mass of the electrolyte, can be selected as 52%, 53%, 54%, 54.66%, 55%, 56%, 57%, 58%, 59%, 60%, 60.66%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 68.66%, 69%, 70%, 71%, or any range between the two above.
[0148] When the total mass content of EC and EMC is within the above range, they can complement each other, overcoming the problems of high viscosity of EC and poor thermal stability and mechanical strength of the SEI film formed by EMC. This optimizes the electrolyte performance and further reduces the pressure on the sealing area from the optimization of ionic conductivity and SEI film.
[0149] In some embodiments, the electrolyte comprises an electrolyte salt, which includes lithium hexafluorophosphate (LiPF6) at a concentration of 0.9 mol / L to 1.2 mol / L.
[0150] In some embodiments, the concentration of lithium hexafluorophosphate in the electrolyte is 0.9 mol / L, 0.95 mol / L, 1.0 mol / L, 1.05 mol / L, 1.1 mol / L, 1.15 mol / L, 1.2 mol / L, or any value range between the two.
[0151] Lithium hexafluorophosphate (LiPF6) is highly soluble in carbonate solvents, forming a high-concentration electrolyte that ensures high ionic conductivity of lithium ions. It also induces a stable SEI film at a low-potential negative electrode, reducing lithium deposition and improving cycle life. However, excessively high LiPF6 concentrations significantly increase electrolyte viscosity, restricting lithium ion diffusion and decreasing ionic conductivity. Furthermore, the decomposition products of LiPF6, including PF5, react with trace amounts of water in the electrolyte to generate HF, which corrodes the electrode and SEI film, exacerbating solvent decomposition and gas production. Within the aforementioned concentration range, LiPF6 achieves an optimal balance between ionic conductivity and electrolyte stability.
[0152] In some embodiments, the mass percentage of dimethyl carbonate is 18%-26% based on the total mass of the electrolyte.
[0153] With the mass percentage of dimethyl carbonate within the above range, the introduction of EC and EMC, which account for a larger proportion, further reduces its gas generation capacity and probability, thereby improving the long-term reliability of the battery cell.
[0154] In some embodiments, the electrolyte further includes vinylene carbonate (VC), wherein the mass percentage of vinylene carbonate is 0.5%-1.5% based on the total mass of the electrolyte.
[0155] Ethylene carbonate preferentially undergoes a reduction reaction on the negative electrode surface compared to other solvent components, forming a dense SEI film rich in organic lithium compounds. This SEI film exhibits high lithium-ion conductivity, which is beneficial for improving the kinetic performance of individual battery cells. The SEI film also possesses high mechanical strength and chemical stability, inhibiting the continuous decomposition of the electrolyte, thereby reducing the consumption of active lithium and the generation of side reactions and gases.
[0156] In some embodiments, the median C of the graphitization degree C in the cumulative distribution curve of the positive electrode film obtained in laser microscopy confocal Raman spectroscopy instrument scanning mode is... 50为 0.95-1.20, where the degree of graphitization C is I G / I D , where I G This indicates that the Raman spectrum is at 1580±100 cm⁻¹ -1 The intensity of peak G at I D This indicates that the Raman spectrum is at 1350±100 cm⁻¹ -1 The intensity of peak D at that location.
[0157] In this application, the graphitization degree C value of the positive electrode film can be obtained by surface scanning mode of a laser confocal Raman spectrometer. As an example, specifically, a laser confocal Raman spectrometer (high-precision Renishaw laser confocal Raman spectrometer) is used, with an excitation wavelength of 532 nm. An appropriate amount of the positive electrode film is taken and surface scanned on its surface or along the thickness direction of the electrode. The scanning area is 45 μm × 45 μm, divided into 10 × 10 grids, with grid vertices as test points, a step size of 5 μm, and a total of 100 scan points. Thus, the C values at different sites and the cumulative distribution curve of the C values in the surface scan area are obtained.
[0158] The positive electrode film in this application can be either a freshly prepared positive electrode film or a positive electrode film obtained from disassembly of a battery. The surface of a positive electrode film obtained from disassembly of a battery inevitably contains residual electrolyte salt particles. To improve testing accuracy, it is preferable to perform a surface scan on a cross-section of the positive electrode film along the electrode thickness direction to characterize the degree of graphitization of the positive electrode film.
[0159] The graphitization degree C of the positive electrode film was obtained by the ratio of the peak intensities of the G-band and D-band in the Raman spectrum. The position of the G-band peak was 1580±100 cm⁻¹. -1 Its characterization of carbon sp 2 Hybrid structure; D peak position is 1350±100 cm⁻¹ -1 It characterizes a disordered structure, where disorder refers to the irregular arrangement of carbon atoms within the structure. In graphite crystals, carbon atoms in the same layer arrange themselves in an sp... 2 Hybridization forms covalent bonds, while interlayer bonding is facilitated by van der Waals forces, making the carbon in the graphite structure prone to slip. Therefore, the C value can characterize the degree of graphitization in the cathode film. It is understandable that the degree of graphitization in the cathode film mainly originates from the graphitized carbon material within the film, i.e., the carbon material on the surface of the cathode active material. Although rich in sp... 2 Hybridized carbon nanotube conductive agents also have relatively high I0 G / I D However, due to its low content and small tube diameter, its addition to the positive electrode film results in an extreme value in the Raman surface scan test of the positive electrode film, and does not affect the graphitization degree C in the positive electrode film. 50 This has an impact. Therefore, the degree of graphitization of the positive electrode film can also be used to characterize the degree of graphitization of the positive electrode active material.
[0160] The cumulative distribution curve of graphitization degree C value refers to the curve obtained by arranging at least 100 C values in ascending order, with graphitization degree as the horizontal axis and the cumulative percentage as the vertical axis. 50 This represents the C value corresponding to a cumulative percentage of 50% on the vertical axis of the cumulative distribution curve of graphitization degree C. The median C value of graphitization degree.50 Compared to point values, it can reflect the overall graphitization degree of particles in the positive electrode film, i.e., the degree of slippage; compared to the mean value, it can reduce the influence of extreme values during the test and improve the confidence of the test results.
[0161] Those skilled in the art can control the degree of graphitization of active material particles using any known process. For example, adjusting the carbon source, sintering temperature, sintering time, sintering pressure, and sintering atmosphere can all achieve adjustments to the degree of graphitization of the active material particles. The higher the degree of graphitization of carbon on the surface of the positive electrode active material, the higher the proportion of graphitic carbon in the positive electrode film layer. This makes it easier for particles to slip using the highly graphitized carbon structures on the surface of the active material particles, reducing stress concentration in the electrode.
[0162] In some embodiments, the median C of the graphitization degree C in the cumulative distribution curve of the positive electrode film obtained in the laser microscopy confocal Raman spectroscopy instrument scanning mode is... 50 The value can be 0.95, 0.96, 0.97, 0.98, 0.99, 1.00, 1.01, 1.02, 1.03, 1.04, 1.05, 1.06, 1.07, 1.08, 1.09, 1.10, 1.11, 1.12, 1.13, 1.14, 1.15, 1.16, 1.17, 1.18, 1.19, 1.20, or any value range between the two mentioned above.
[0163] Studies have shown that the stress on the film layer under cyclic expansion easily leads to increased internal mechanical pressure, causing the encapsulation structure to fail. By controlling the cumulative distribution curve of graphitization degree C values obtained in the laser microscopy confocal Raman spectroscopy instrument scanning mode, the median C of graphitization degree is... 50 The value is 0.95-1.20, which increases the graphitization degree of the positive electrode film, improves the slippage of particles in the positive electrode film, reduces the stress concentration phenomenon during the compaction of the thick coating film, and reduces the degree of rebound of the positive electrode film due to local stress concentration during cycling, thereby increasing the volumetric energy density of the battery cell while increasing the reliability of the battery cell.
[0164] In some embodiments, the median B of the coating value B in the cumulative distribution curve of the positive electrode film obtained in laser microscopy confocal Raman spectroscopy instrument scanning mode is... 50 The value is 0.30-0.60, where the coating value B is I. P / I D , where I P This indicates that the Raman spectrum is at 948±100 cm⁻¹ -1 The intensity of the P peak at I D This indicates that the Raman spectrum is at 1350±100 cm⁻¹ -1The intensity of peak D at that location.
[0165] In this application, the coating value (B value) of the positive electrode film can be obtained by scanning with a laser confocal microscopy (LCM) spectrometer. Specifically, a high-precision Renishaw laser confocal microscopy (LCM) spectrometer is used, with an excitation wavelength of 532 nm. An appropriate amount of the positive electrode film is scanned on its surface or along a section of the electrode thickness. The scanning area is 45 μm × 45 μm, divided into 10 × 10 grids, with grid vertices as test points, a step size of 5 μm, and a total of 100 scan points. This yields the B values at different sites and the cumulative distribution curve of the B values in the scanned area.
[0166] The coating value B of the positive electrode film was obtained by the ratio of the peak intensities of the P-band and D-band in the Raman spectrum, with the P-band located at 948±100 cm⁻¹. -1 Its characterization of phosphate PO4 3- Structure; D peak position is 1350±100cm -1 Raman spectroscopy characterizes disordered structures, where disorder refers to the irregular arrangement of carbon atoms within the structure. As a surface analysis instrument, Raman spectroscopy reveals that the carbon structure peaks in the cathode film, under laser confocal Raman spectroscopy scanning mode, exhibit higher intensity compared to the phosphate structure peaks, which are more abundant in the bulk phase.
[0167] Those skilled in the art can control the coating value of active material particles using any known process. For example, adjusting the carbon source type, carbon source addition amount, sintering temperature, sintering time, sintering pressure, and sintering atmosphere can all achieve adjustments to the coating value of active material particles. The coating value (B-value) reflects the density of the carbon material on the surface of lithium transition metal phosphate particles. The denser the carbon material, the lower the relative intensity of the phosphate structure detected in the Raman spectrum, and the smaller the coating value (B-value) of the cathode film.
[0168] The cumulative distribution curve of the coverage value (B value) is a curve obtained by arranging at least 100 B values in ascending order, with the coverage value on the horizontal axis and the cumulative percentage on the vertical axis. 50 The B value is the value corresponding to the cumulative number of values on the vertical axis of the cumulative distribution curve of the coverage value B value when the cumulative number accounts for 50%.
[0169] In some embodiments, the median B of the coating value B in the cumulative distribution curve of the positive electrode film obtained in laser microscopy confocal Raman spectroscopy instrument scanning mode is... 50The values can be 0.3, 0.31, 0.32, 0.33, 0.34, 0.35, 0.355, 0.36, 0.368, 0.369, 0.37, 0.38, 0.39, 0.4, 0.41, 0.42, 0.43, 0.44, 0.446, 0.45, 0.456, 0.46, 0.47, 0.48, 0.49, 0.5, 0.51, 0.52, 0.53, 0.54, 0.55, 0.56, 0.57, 0.58, 0.59, 0.6, or any value range between the two mentioned above.
[0170] To reduce the impact of extreme coating values caused by non-particle regions in the positive electrode film on the test results, the median coating value B was used. 50 Evaluate the density of carbon material on the surface of the positive electrode active material.
[0171] The median B of the coating value of the positive electrode film 50 Within the above range, it is indicated that the carbon material on the surface of the positive electrode active material is relatively dense and uniform, which is beneficial to improving the slip uniformity of the positive electrode film during the rolling process, reducing the stress concentration phenomenon in the positive electrode film, reducing the rebound degree of the positive electrode sheet, and improving the reliability of the battery cell.
[0172] In some embodiments, the lithium-containing transition metal phosphate particles include iron, and the iron dissolution rate of the positive electrode film is 658ppm-1921ppm, optionally 658ppm-1485ppm.
[0173] The iron dissolution rate of the positive electrode film can be tested in the following ways. Specifically, after disassembling and cleaning the electrode from the battery, it is formed into small discs with a diameter of 14 mm. Multiple small disc samples are taken to make the total sample mass about 5 g. These are added to 100.3 g of a 0.3% ascorbic acid solution (using ultrapure water as the solvent). The solution is stirred at 500 rpm for 5 minutes, and then the solution is quickly aspirated using a 5 mL syringe. The solution is filtered into a test tube using a 0.45 μm pore size filter. 1 mL of the supernatant is pipetted into a glass volumetric flask and diluted 50 times. The iron concentration in the solution is measured using an inductively coupled plasma mass spectrometer (ICP-OES). The iron dissolution rate of the positive electrode film is calculated using the formula: [(ICP test iron concentration × solution volume / mass of the solution used for volume adjustment) × 100.3 g / (mass of small disc electrode - mass of small disc current collector)]. The solution volume is 50 mL, and the mass of the solution used for volume adjustment is 1 g. Preferably, the current collector mass of the small disc is obtained by multiplying the disc's thickness by its area and density. The disc's thickness can be equivalently measured by measuring the current collector thickness in the uncoated area using a thickness gauge. It is understood that although the current collector in the coated area will expand during compaction, resulting in a slight reduction in thickness compared to the uncoated area, this reduction is negligible and will not significantly affect the test results.
[0174] In some embodiments, the lithium-containing transition metal phosphate particles include iron, and the iron dissolution rate of the positive electrode film can be 658ppm, 700ppm, 800ppm, 890pm, 900ppm, 1000ppm, 1058pm, 1076pm, 1100ppm, 1143pm, 1200ppm, 1236pm, 1300ppm, 1311pm, 1384pm, 1349pm, 1400ppm, 1485pm, 1500ppm, 1531pm, 1600ppm, 1700ppm, 1800ppm, 1921ppm, or any value between the two above.
[0175] The iron dissolved in the positive electrode film mainly originates from the lithium transition metal phosphate (LMT) of the positive electrode active material. The iron dissolution rate depends on both the number of lattice defects in the LMT and the integrity and density of the carbon material on the surface of the positive electrode active material. A lower iron dissolution rate means fewer lattice defects in the LMT, which helps reduce lattice corrosion in weak acid environments. Furthermore, a more complete and dense carbon material on the surface of the positive electrode active material inhibits the dissolution of iron ions in weak acid environments. Positive electrode films with iron dissolution rates within the above range have relatively few lattice defects and complete and dense carbon material on the surface of the positive electrode active material. This improves the compressibility and slippage of particles in the positive electrode film under high rolling pressure, increases the compaction density of the positive electrode film, reduces stress concentration, improves the energy density of the battery, and also enhances battery reliability.
[0176] In some embodiments, the positive electrode film layer further includes a conductive agent, and the total area of the agglomerated region of the conductive agent accounts for 0.5%-2.5% based on the total area of the cross-section of the positive electrode film layer along the thickness direction of the electrode sheet.
[0177] In this application, the area ratio of the conductive agent agglomeration region, based on the total area of the cross-section of the positive electrode film layer along the electrode thickness direction, can be tested using the following method. A similar method to that described above is used to observe the cross-section of the positive electrode film layer along the electrode thickness direction using a scanning electron microscope (SEM), and the area of the conductive agent agglomeration region in the SEM image is measured at 3kx magnification. Since the conductive agent is generally a carbon-based material, such as conductive carbon black or carbon nanotubes, aggregated conductive agent can be seen under high magnification in the SEM. The conductive agent agglomeration region often appears black and agglomerated compared to other areas in the positive electrode film layer. Using image analysis software, the conductive agent agglomeration region refers to the area in the SEM image where the conductive agent is clearly aggregated and appears black. Specifically, the scanning electron microscope (SEM) image at 3kx magnification is imported into ImageJ. Black conductive agent agglomeration regions with a Feret value greater than or equal to 2μm are selected, and the sum of the areas of these selected regions is recorded as the area of the conductive agent agglomeration region. The area ratio of the conductive agent agglomeration region is the ratio of its area to the total area of the imported SEM image. Three randomly selected, non-overlapping SEM images are used, and the average of these ratios is calculated as the "area ratio of the conductive agent agglomeration region based on the total area of the cross-section along the electrode thickness direction of the positive electrode film."
[0178] In some embodiments, based on the total area of the cross-section of the positive electrode film layer along the thickness direction of the electrode sheet, the total area percentage of the agglomerated region of the conductive agent can be selected as 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.68%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.41%, 2.5%, or any value range between the above two.
[0179] Based on the total area of the cross section along the thickness direction of the positive electrode film, the total area ratio of the agglomerated region of the conductive agent is 0.5%-2.5%, indicating that the conductive agent in the positive electrode film is uniformly dispersed and easily forms a uniform conductive network. This is especially beneficial for reducing the problem of decreased kinetics caused by the growth of ion transport paths in thick coating films, and reducing local polarization and even lithium plating problems generated during battery cycling.
[0180] Meanwhile, research shows that large-sized particles in lithium transition metal phosphate particles are prone to rebound. When the agglomeration area of the conductive agent is within the above range, the uniform distribution of the conductive agent can suppress the rebound of lithium transition metal phosphate, form mechanical constraints on the particles and even the film layer, improve the cohesion of the film layer, reduce the probability of failure in the sealing area, and improve the reliability of the battery.
[0181] In some embodiments, the positive electrode film layer further includes a conductive agent, and the area of the agglomerated region of the conductive agent accounts for 0.5%-1.7% based on the total area of the cross section of the positive electrode film layer along the thickness direction of the electrode sheet.
[0182] In this embodiment, the area ratio of the agglomerated region of the conductive agent is further within the above-mentioned range, indicating that the conductive agent is more uniformly distributed in the positive electrode film layer and the content of the conductive agent is low. While improving the dynamic performance of the positive electrode film layer, it helps to reduce the space occupied by the excessive conductive agent on the positive electrode active material, thereby improving the battery's dynamic performance and further increasing the battery's volumetric energy density.
[0183] In some embodiments, the conductive agent includes carbon nanotubes, which include one or more of single-walled carbon nanotubes, few-walled carbon nanotubes, and multi-walled carbon nanotubes.
[0184] In this application, the term "carbon nanotube" refers to a structure composed of carbon atoms arranged in sp... 2Graphene sheets, formed by hybrid bonding, are rolled up to form nanomaterials with several to dozens of coaxial hollow cylindrical layers. Their diameters typically range from several to tens of nanometers, while their lengths can vary from micrometers to centimeters, exhibiting a high aspect ratio. Based on the number of layers, graphene sheets can be classified into: single-walled carbon nanotubes (SWCNTs), few-walled carbon nanotubes (FWCNTs), and multi-walled carbon nanotubes (MWCNTs). Carbon nanotubes possess excellent electrical conductivity and high elastic modulus.
[0185] The high aspect ratio of carbon nanotubes facilitates the bonding of multiple positive electrode particles in the thickness direction, forming long-range conductive pathways while increasing the binding force between particles. This not only improves the dynamic performance of thickly coated positive electrode films, reducing local polarization and even lithium plating during battery cycling, thus increasing battery cycle life, but also effectively alleviates stress concentration, reduces electrode rebound, and improves the reliability of individual battery cells by forming a network structure within the positive electrode film, acting as a bridge for stress propagation.
[0186] Meanwhile, carbon nanotubes possess a high specific surface area and a hollow structure, thus exhibiting excellent electrolyte retention capabilities. Thick electrodes experience significant expansion forces during cycling, making it easier for the electrolyte to be squeezed out. The presence of carbon nanotubes in the positive electrode film helps improve the electrolyte retention capacity of thick electrodes, mitigating the capacity drop of individual cells during cycling and improving the cycle life of individual cells.
[0187] In some embodiments, the conductive agent further includes conductive carbon black.
[0188] Conductive carbon black has a high specific surface area, thus exhibiting excellent electrolyte retention capacity. Thick electrodes experience greater expansion force during cycling, making it easier for the electrolyte to be squeezed out. The distribution of conductive carbon black in the positive electrode film helps improve the electrolyte retention capacity of thick electrodes, mitigating the phenomenon of capacity drop during battery cycling and improving battery cycle life.
[0189] In some embodiments, the agglomeration regions of the conductive agent include carbon nanotubes and conductive carbon black.
[0190] Researchers have found that carbon nanotubes are prone to agglomeration due to their high surface energy, which leads to uneven dispersion in the positive electrode film layer and fails to form an effective carbon nanotube network structure. Conductive carbon black and carbon nanotubes have relatively close surface energies, and can adsorb on the surface of carbon nanotubes to form a physical barrier, increase the resistance to agglomeration of carbon nanotubes, reduce direct contact between carbon nanotubes, thereby inhibiting the agglomeration phenomenon and improving the distribution uniformity of carbon nanotubes in the positive electrode film layer. On the one hand, this helps to improve the conductivity of the thickly coated positive electrode film layer and enhance the dynamic performance of the battery; on the other hand, it helps to exert the binding effect of carbon nanotubes on the positive electrode film layer, reduce the risk of peeling off of the thickly coated positive electrode film layer, and further improve the dynamic performance and cycle life of the battery. In addition, the agglomeration of carbon nanotubes in the agglomerated region of the conductive agent will also cause local ion transport paths in the agglomerated region of the conductive agent to be blocked. The matching of conductive carbon black can improve the lithium ion transport capacity in this region, reduce local polarization, and further improve the cycle stability of the battery.
[0191] In some embodiments, based on the mass of the positive electrode film layer, the mass content C1 of the carbon nanotubes satisfies: 0<C1≤2.5%, and the mass content C2 of the conductive carbon black satisfies: 0<C2≤2.5%.
[0192] In some embodiments, based on the mass of the positive electrode film layer, the mass content C1 of the carbon nanotubes may optionally be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.67%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5% or a numerical range between any two of them.
[0193] In some embodiments, based on the mass of the positive electrode film layer, the mass content C2 of the conductive carbon black may optionally be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5% or a numerical range between any two of them.
[0194] When the mass contents of carbon nanotubes and conductive carbon black in the positive electrode film layer are within the above ranges, the agglomeration of carbon nanotubes can be effectively alleviated and a good conductive network structure can be formed, thereby effectively reducing the rebound of the thickly coated positive electrode film layer and improving the reliability of the battery cell; and increasing the electrolyte retention rate of the positive electrode plate during the long cycle process, reducing the degree of polarization, and ameliorating the capacity plunge problem of the battery cell.
[0195] In some embodiments, the positive electrode film layer further includes a dispersant, which includes hydrogenated nitrile butadiene rubber (HNBR).
[0196] HNBR is obtained by hydrogenating and saturating the double bonds of nitrile rubber. Its highly saturated main chain structure gives it excellent oil resistance, heat resistance, and aging resistance. This allows it to remain stable in different environments and systems when used as a dispersant, without easily degrading or deteriorating, thus effectively exerting its dispersing effect. The HNBR molecular chain contains both polar nitrile groups and non-polar hydrocarbon segments. The polar nitrile groups can interact with the hydroxyl groups (-OH) or metal oxide sites on the surface of lithium transition metal phosphate particles (such as hydrogen bonding and dipole interaction), enhancing the compatibility between particles and solvents, reducing the interfacial tension between particles and solvents, especially the interfacial tension of large particles, making the particles easier to disperse uniformly, reducing aggregation caused by hydrophobicity, improving the dispersibility of large particles in the positive electrode film, and reducing stress concentration caused by rebound; the non-polar hydrocarbon segments have good oleophilicity, and can extend and disperse well in non-polar or weakly polar media, so that the particles are uniformly dispersed in the medium.
[0197] When HNBR adsorbs onto the surface of particles in the slurry, its long-chain molecules form a physical barrier around the particles, preventing them from approaching each other and aggregating, thus maintaining a relatively independent dispersion. Simultaneously, HNBR reduces the surface tension between the dispersion medium and the dispersed particles, making the particles easier to wet and promoting dispersion. Furthermore, it reduces the interfacial energy between particles, particularly minimizing the aggregation of conductive agents driven by interfacial energy, thereby improving the cycle life of individual battery cells.
[0198] In some embodiments, the mass content of the dispersant is 0.5%-2% based on the mass of the positive electrode film.
[0199] In some embodiments, based on the mass of the positive electrode film, the mass content of the dispersant can be selected as 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.5%, 2%, or any value range between the two.
[0200] When the mass content of the dispersant is within the above range, it can achieve uniform dispersion of particles in the positive electrode film while maintaining a high loading capacity, reduce the rebound caused by stress concentration in the thick-coated lithium transition metal phosphate positive electrode film, reduce the rebound rate of the positive electrode film, and improve the reliability of the battery cell.
[0201] In some embodiments, the porosity of the positive electrode film is 14%-28%.
[0202] In this application, the porosity of the positive electrode film can be tested in the following way: Import the cross-sectional scanning electron microscope (SEM) image of the positive electrode film along the electrode thickness direction obtained as described above into ImageJ software. Select the line tool and use a line to mark the length of the scale bar in the image. Click "Analyze Set Scale" and set the scale parameters in the software according to the scale bar length in the image. Select the rectangle tool and select the part of the image outside the scale bar area. Use "Image Duplicate" to copy the selected area and use "Image Type 8bit" to adjust the image format. Select "Analyze Set Measurements" and choose the following five options: "Area", "Mean gray value", "Area Fraction", "Limit to threshold", and "Feret's diameter". Select 3 for "Decimal places". Then, select "Image" - "Adjust" - "Threshold" in sequence, and set 0 and 100 in the selected position of "Threshold". The pore data in the cross-sectional SEM image can then be exported using the Analyze-Measure function. Export using "Image" - "Overlay" - "Flatten" to obtain a pore image; click "Apply" in "Threshold", then click "Analyze" - "Analyze Particles", check the four columns on the left to obtain pore statistics.
[0203] It is understood that in this embodiment, "pores" in the cross-section of the positive electrode film are identified by image color difference and threshold. These "pores" are not the pore data obtained from the degassing test, but are mainly used to characterize the cross-sectional area between particles in the cross-section of the positive electrode film. This method is superior to the degassing method because the porosity obtained by the degassing method is related to the pores between particles and the pores in the carbon material on the surface of the lithium iron phosphate particles, thus failing to objectively reflect the pores between particles.
[0204] Within the aforementioned range, the porosity of the positive electrode film is beneficial in two ways: firstly, it improves the electrolyte's liquid retention properties, enhances the ion diffusion of thick-coated electrodes and the positive electrode film, and improves the battery's kinetic performance; secondly, it can buffer the volume increase during rebound or charge / discharge processes, reduce the impact of expansion stress on the sealing area, and maintain the battery's high reliability.
[0205] In some embodiments, the porosity of the positive electrode film can be selected as 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, or any value range between the two.
[0206] In some embodiments, as shown in FIG2, the battery cell further includes a separator 20 disposed between the positive electrode and the negative electrode. The separator 20 includes a base film 201, ceramic layers 202 disposed on both sides of the base film 201, and an adhesive layer 203 disposed on at least one side of the ceramic layer 202 away from the base film 201. The adhesive layer 203 is a continuous layer with a porous structure and includes a vinylidene fluoride polymer.
[0207] In some embodiments, the vinylidene fluoride polymer includes one or more of polyvinylidene fluoride (PVDF) and polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP).
[0208] In some embodiments, the vinylidene fluoride polymer includes polyvinylidene fluoride (PVDF).
[0209] As shown in Figure 3, in the prior art, the adhesive layer of the diaphragm often uses aqueous PVDF, which presents an island-like structure in the diaphragm. This is beneficial for providing gaps for cell expansion and is also convenient for manufacturing. However, such a diaphragm adhesive layer has a small contact area with the electrode and weak adhesion.
[0210] The diaphragm provided in this application uses a continuous porous layer as the adhesive layer, as shown in Figure 2. Compared with the adhesive layer in the prior art, it has a larger bonding area with the electrode, which makes the bonding between the diaphragm and the electrode more firm and uniform. Furthermore, when the positive electrode film layer rebounds, it helps to maintain the interfacial contact between the diaphragm and the positive electrode film layer, reducing the probability of film layer detachment.
[0211] It is understandable that a continuous adhesive layer may break and deform into a blocky structure during electrode manufacturing or cycling due to contact with or compression of the positive or negative electrode. The continuous structure referred to in this application means that, at the microscopic level, such as under a scanning electron microscope or optical microscope, the adhesive layer of the separator is continuous. To reflect the true morphology of the separator, during sampling, it is preferable to sample in areas of the battery where the separator's adhesive layer is not bonded to the positive or negative electrode. For example, sampling can be performed at locations beyond the positive and negative electrode; or sampling can be performed near the surface of the electrode assembly. This sampling area has less adhesion to the positive or negative electrode, providing a better reflection of the separator's true state.
[0212] The separator provided in this application uses a porous continuous layer as the adhesive layer, which has a larger bonding area compared to the adhesive layers in the prior art, thus making the adhesion between the separator and the positive electrode film layer more firm and uniform. Particles with a particle size R1 satisfying R1≥1000nm are prone to stress concentration during cycling, leading to rebound problems. The separator provided in this application, using a porous continuous layer as the adhesive layer, is particularly suitable for thick-coated stacked cells, improving the rebound phenomenon of thick-coated stacked cells during long-cycle cycling, reducing the expansion stress inside the battery, and improving the reliability of the sealing area and the overall battery cell. In addition, thick-coated cells are prone to relative displacement between the electrode and the separator during the process of dragging the outer electrode and welding the tabs, making the film layer prone to powder shedding and even the positive and negative electrodes overlapping, resulting in the risk of internal short circuit. The porous continuous layer as the adhesive layer in this application embodiment can also reduce the above risks.
[0213] In some embodiments, the base film may be made of one or more of the following materials, including but not limited to glass fiber, nonwoven fabric, polyethylene (PE), and polypropylene (PP).
[0214] In some embodiments, the ceramic layer includes one or more of alumina (Al2O3), zirconium oxide (ZrO2), titanium oxide (TiO2), silicon oxide (SiO2), and boron nitride (BN).
[0215] Ceramic particles possess flame retardancy and high hardness, making them resistant to deformation under heat and exhibiting excellent dimensional stability. The low thermal conductivity of ceramic materials further prevents certain thermal runaway points in the battery from expanding into overall thermal runaway, thereby improving the safety performance of individual battery cells.
[0216] In some embodiments, the positive electrode film layer has a base coating layer in the bottom region near the positive electrode current collector. The base coating layer includes a conductive agent and a binder. The conductive agent includes carbon nanotubes and conductive carbon black, and the binder includes vinylidene fluoride polymer.
[0217] In some embodiments, the positive electrode film layer has an undercoat layer in the bottom region near the positive electrode current collector, and the thickness of the undercoat layer is 0.5 μm-5 μm.
[0218] In some embodiments, the thickness of the base coating can be selected as 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm or any value range between the two.
[0219] The undercoating provided in this application helps improve the adhesion between the positive electrode film and the positive electrode current collector and alleviates stress concentration at large particles, thereby reducing the rebound of the positive electrode film and improving the reliability of the battery cell. Simultaneously, compared to direct contact between the positive electrode current collector and the positive electrode film, the increased contact area between the undercoating and the positive electrode film helps increase the area for electron transport between the current collector and the positive electrode film, thereby reducing the internal resistance of the electrode and improving the battery's dynamic performance.
[0220] In some embodiments, the lithium transition metal phosphate particles in the positive electrode film layer comprise components represented by the following general formula:
[0221] Li m Fe x P y O j Q q Formula I,
[0222] Wherein, Q includes one or more of Al, Na, K, Mg, Cu, Mn, Cr, Zn, Pb, Ca, Co, Ni, Sr, Nb, V, Ti, B, S, Si, N, F, Cl, and Br, with 0.8≤m≤1.15, 0.9≤x≤1, 0.95≤y≤1, 3.5≤j≤4, and 0≤q≤0.1.
[0223] In some implementations, m can be selected as 0.8, 0.85, 0.9, 0.95, 0.98, 1.00, 1.03, 1.05, 1.08, 1.10, 1.13, 1.15, or any value range between two of these; x can be selected as 0.9, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98, 0.99, 1.0, or any value range between two of these. y can be 0.95, 0.96, 0.97, 0.98, 0.99, 1.00 or any value between two of these; j can be 3.5, 3.6, 3.7, 3.8, 3.9, 4 or any value between two of these; q can be 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1 or any value between two of these.
[0224] Selecting appropriate modifying element Q can improve the lattice change rate of positive electrode active material during lithium insertion / extraction process, reduce oxygen activity on particle surface, improve the structural stability of material, thereby improving the specific capacity utilization level of material during cycling and improving the cycle stability of battery cell.
[0225] In some embodiments, the lithium-containing transition metal phosphate particles include titanium, and the mass content of titanium is 500ppm-8000ppm, optionally 1000ppm-3000ppm, based on the total mass of the lithium-containing transition metal phosphate particles in the positive electrode film.
[0226] The types and contents of elements in lithium transition metal phosphate particles in the positive electrode film can be tested using any method known in the art. As an example, inductively coupled plasma atomic emission spectrometry (ICP-AES) was used to test the titanium content, referring to Appendix C of GB / T 33822-2017.
[0227] In some embodiments, based on the total mass of lithium transition metal phosphate particles in the positive electrode film, the mass content of titanium can be selected as 500ppm, 600ppm, 700ppm, 800ppm, 900ppm, 1000ppm, 1100ppm, 1200ppm, 1400ppm, 1500ppm, 1600ppm, 1700ppm, 1800ppm, 1900ppm, 2000ppm, 2100ppm, 2200ppm, 2300ppm, 2400ppm, 2500ppm, 2600ppm, 2700ppm, 2800ppm, 2900ppm, 3000ppm, 3500ppm, 4000ppm, 4500ppm, 5000ppm, 5500ppm, 6000ppm, 6500ppm, 7000ppm, 7500ppm, 8000ppm, or any value range between the two.
[0228] Introducing titanium into lithium transition metal phosphate particles requires adding a titanium source during the preparation of the cathode active material. Titanium sources are often inert materials, and their adhesion to the surface of the lithium transition metal phosphate raw material reduces reactivity and particle size growth. Increasing the graphitization degree of the cathode active material often requires higher sintering temperatures or longer sintering times, but this also increases the particle size in the cathode film, increasing stress concentration and potentially causing film detachment. In this embodiment, by adding a high content of titanium to the lithium transition metal phosphate particles, the reactivity of the raw materials for synthesizing the cathode active material is reduced. This allows the cathode active material to achieve high graphitization while controlling the proportion of large particles, reducing the rebound rate of the cathode film, and improving battery energy density while maintaining battery reliability.
[0229] Meanwhile, the doping of titanium in the positive electrode active material is beneficial for inducing lattice distortion, reducing Li-O bond energy, increasing lithium-ion transport rate, and improving the kinetic performance of the battery. In thick coated films, lithium-ion diffusion is uneven, often accompanied by a significant lithium-ion concentration gradient. This application's embodiments improve the solid-phase transport rate of the positive electrode active material by adding a high content of titanium to lithium-containing transition metal phosphate particles, thus addressing the kinetic problems of thick electrode batteries.
[0230] In some embodiments, the lithium-containing transition metal phosphate particles include vanadium, and the vanadium content is 500ppm-5000ppm, optionally 500ppm-3000ppm, based on the total mass of the lithium-containing transition metal phosphate particles in the positive electrode film.
[0231] In some embodiments, the vanadium content can be selected as 500ppm, 600ppm, 700ppm, 800ppm, 900ppm, 1000ppm, 1100ppm, 1200ppm, 1400ppm, 1500ppm, 1600ppm, 1700ppm, 1800ppm, 1900ppm, 2000ppm, 2100ppm, 2200ppm, 2300ppm, 2400ppm, 2500ppm, 2600ppm, 2700ppm, 2800ppm, 2900ppm, 3000ppm, 3500ppm, 4000ppm, 4500ppm, or 5000ppm, based on the total mass of lithium transition metal phosphate particles in the positive electrode film.
[0232] Vanadium in the positive electrode film can exist in multiple valence states. Vanadium in the +5 valence state (V5+) can be doped into phosphorus sites. Due to its large radius, it can cause lattice distortion, expanding the diffusion channels for lithium ions, thereby improving the ionic conductivity of the positive electrode active material and enhancing the battery's kinetic performance. Vanadium in the +3 valence state (V... 3 +) can be doped into transition metal sites, generating lithium vacancies through charge compensation, thereby improving the electronic conductivity of the positive electrode active material. Furthermore, the increased uniformity of vanadium distribution in lithium-containing transition metal phosphate particles helps to further improve the kinetic performance and reaction uniformity of the positive electrode film, thus enhancing the kinetic and cycle performance of the battery cell.
[0233] Vanadium content within the aforementioned range helps improve the kinetic performance of the positive electrode and the kinetic performance of thick-coated lithium transition metal phosphate batteries. Simultaneously, the synergistic effect of titanium, vanadium, and carbon nanotubes in the positive electrode film helps form a good three-dimensional network, further improving the electronic and ionic conductivity of the positive electrode film, thereby further enhancing the kinetic performance of thick-coated lithium transition metal phosphate batteries.
[0234] In some embodiments, the lithium-containing transition metal phosphate in the positive electrode film includes one or more of lithium iron phosphate, lithium manganese phosphate, lithium fluorinated vanadium phosphate, lithium manganese iron phosphate, and their modified materials.
[0235] In some embodiments, the lithium-containing transition metal phosphate in the positive electrode film includes one or more of lithium iron phosphate and its doped and modified materials, and coating and modified materials.
[0236] The aforementioned lithium-containing transition metal phosphate materials exhibit good thermal stability and cycle stability, which helps to improve the safety and cycle performance of batteries.
[0237] In some embodiments, the flexible packaging material includes an aluminum-plastic composite film, optionally including one or more of aluminum, polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), nylon, polyethylene terephthalate (PET), and polyethylene (PE) in a composite film formed with aluminum.
[0238] Compared to rigid materials such as aluminum and steel shells, soft-pack materials are lighter, which is beneficial for further improving the energy density of lithium transition metal phosphate batteries.
[0239] In some embodiments, at least one of the laminated cells is housed within the housing, the housing having a length dimension of L0, a width dimension of W0, and a thickness dimension of H0, wherein 450mm≤L0≤1300mm, 100mm≤W0≤150mm, and 14mm≤H0≤22mm.
[0240] In some implementations, L0 can be selected as 450mm, 460mm, 470mm, 480mm, 490mm, 500mm, 510mm, 520mm, 530mm, 540mm, 550mm, 560mm, 570mm, 580mm, 590mm, 600mm, 610mm, 620mm, 630mm, 640mm, 650mm, 660mm, 670mm, 680mm, 690mm, 700mm, 710mm, 720mm, 750mm, 800mm, 850mm, 900mm, 950mm, 1000mm, 1050mm, 1100mm, 1150mm, 1200mm, 1250mm, 1300mm, or a range of values between any two of the above.
[0241] In some implementations, W0 can be selected as 100mm, 110mm, 120mm, 130mm, 140mm, 150mm or any value range between the two mentioned above.
[0242] In some implementations, H0 can be selected as 14mm, 15mm, 16mm, 17mm, 18mm, 19mm, 20mm, 21mm, 22mm or any value range between the two mentioned above.
[0243] In some embodiments, the length dimension L0 of the housing satisfies: 450mm≤L0≤650mm.
[0244] When the length dimension L0 of the casing satisfies 450mm≤L0≤650mm, the length of the battery cell is shorter, which helps to shorten the current diffusion path, reduce the internal resistance of the electrode, thereby reducing the heat generation of the battery and improving its dynamic performance. In addition, the shorter casing length helps to shorten the diffusion path of the electrolyte during the wetting process, improve the wetting rate and uniformity of the electrolyte, further promote the uniformity of lithium ion insertion and extraction during cycling, alleviate stress concentration, reduce the rebound amplitude of the film layer, and improve the reliability of the battery cell.
[0245] In some implementations, the length dimension L0 of the housing satisfies: 900mm≤L0≤1300mm.
[0246] When the length dimension L0 of the casing satisfies 900mm≤L0≤1300mm, the battery cell is relatively long, which helps to reduce the volume ratio of the casing in the battery cell and increase the load ratio of active materials. At the same time, a longer battery cell can reduce the number of batteries required in the battery module, simplify the structural design of the battery module, reduce the number and complexity of structural components in the module, thereby improving the space utilization of the battery pack and thus helping to improve the volumetric energy density of the battery cell.
[0247] In some embodiments, at 25°C, the capacity of the battery cell is 105Ah-300Ah, optionally 150Ah-190Ah.
[0248] In this application, the capacity of a single battery cell has a meaning known in the art and can be tested using methods known in the art. As an example, the battery is charged to 3.65V at a charging rate of 0.5C (the nominal capacity), then charged at a constant voltage of 3.65V to 0.05C, left to stand for 10 minutes, and then discharged to 2.5V at a discharging rate of 1C, left to stand for 10 minutes. The capacity during the discharge process is calculated using the formula C = I × t, with the unit being Ah.
[0249] In some embodiments, at 25°C, the capacity of the battery cell can be selected as 125Ah, 130Ah, 135Ah, 140Ah, 145Ah, 150Ah, 155Ah, 160Ah, 165Ah, 170Ah, 175Ah, 180Ah, 185Ah, 190Ah, 200Ah, 210Ah, 220Ah, 230Ah, 240Ah, 250Ah, 260Ah, 270Ah, 280Ah, 290Ah, 300Ah, or any value range between the two.
[0250] In some embodiments, the positive current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0251] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0252] In some embodiments, the negative electrode film layer includes a negative electrode active material. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, and hard carbon. However, this application is not limited to these materials, and other conventional materials that can be used as battery negative electrode active materials may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0253] In some embodiments, the negative electrode film layer may optionally include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0254] In some embodiments, the negative electrode film may optionally include a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0255] In some embodiments, the negative electrode film may optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)).
[0256] In some embodiments, the negative electrode sheet can be prepared by dispersing the components used to prepare the negative electrode sheet, such as the negative electrode active material, conductive agent, binder and any other components, in a solvent (e.g., deionized water) to form a negative electrode slurry; coating the negative electrode slurry onto the negative electrode current collector, and then obtaining the negative electrode sheet after drying, compaction and other processes.
[0257] A second aspect of this application provides a battery device, including the battery cell provided in the first aspect of this application.
[0258] The battery device disclosed in this application can be used in electrical devices that use the battery device as a power source or in various energy storage systems that use the battery device as an energy storage element. Besides vehicles, the battery device can also be used in, but is not limited to, mobile phones, tablets, laptops, electric toys, power tools, electric vehicles, electric cars, ships, spacecraft, etc. Electric toys can include stationary or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, etc. Spacecraft can include airplanes, rockets, space shuttles, and spacecraft, etc.
[0259] In addition, this application also provides an electrical device that uses a battery as a power source, the electrical device including at least one of the battery cell, battery module, or battery pack provided in this application. The battery cell, battery module, or battery pack can be used as a power source for the electrical device, or as an energy storage unit for the electrical device.
[0260] As the electrical device, a single battery cell, a battery module, or a battery pack can be selected according to its usage requirements.
[0261] Figure 4 shows an example of an electrical device. The electrical device disclosed in this application can be a gasoline-powered vehicle, a natural gas-powered vehicle, or a new energy vehicle. New energy vehicles can be pure electric vehicles, hybrid electric vehicles, or range-extended electric vehicles, etc. A battery device is installed inside the vehicle, and the battery device can be located at the bottom, front, or rear of the vehicle. The battery device can be used to power the vehicle; for example, the battery device can serve as the vehicle's operating power source. The vehicle may also include a controller and a motor. The controller is used to control the battery device to supply power to the motor, for example, for the vehicle's starting, navigation, and operating power needs. In some embodiments of this application, the battery device can not only serve as the vehicle's operating power source but also as the vehicle's drive power source, replacing or partially replacing gasoline or natural gas to provide driving power to the vehicle.
[0262] This application also provides an energy storage device that uses a battery as a power source. The energy storage device can be, but is not limited to, an energy storage container, an energy storage cabinet, an energy storage power station, an energy storage battery pack, or a portable energy storage system.
[0263] Example
[0264] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.
[0265] Example 1
[0266] (1) Preparation of positive electrode active material
[0267] Lithium carbonate, iron phosphate, titanium dioxide, vanadium pentoxide, sucrose, glucose, and polyethylene glycol were added to deionized water and mixed in a premixing tank. The ratio of lithium carbonate to iron phosphate was such that the molar ratio of lithium to iron was 1.025:1.0. Based on the total mass of the mixed raw materials, the mass content of sucrose was 2%, the mass content of glucose was 4%, and the mass content of polyethylene glycol was 5%. After uniform mixing, a mixed raw material with a solid content of 38% was obtained.
[0268] Among them, the particle size Dv50 of lithium carbonate is 6μm; the morphology of iron phosphate particles is spherical; titanium dioxide and vanadium pentoxide are both nanoparticles; the purity of sucrose is ≥98%; the moisture content of glucose is <0.5%; and the weight average molecular weight of polyethylene glycol is 1500.
[0269] The mixed raw materials were ground twice in a sand mill. After coarse grinding for 1 hour, fine grinding was performed. During the grinding process, the slurry temperature was controlled to be less than 40℃ to obtain a mixed slurry. The particle size Dv50 of the solid particles in the mixed slurry was 0.45μm. Spray drying was performed to obtain a dried precursor powder. After drying, its particle size D50 was 55.55μm.
[0270] The precursor powder was subjected to a two-stage heating sintering process in a nitrogen atmosphere to obtain the positive electrode active material: the temperature was increased from 25℃ to 450℃ at a heating rate of 2℃ / min (first heating stage), and held for 3 hours; the temperature was then increased from 450℃ to 780℃ at a heating rate of 5℃ / min (second heating stage), and held for 12 hours; the air volume in the heating stage was greater than that in the isothermal stage, with a ratio of 1.5:1, and the total air volume was 1350 cm³. 3 / h, after which the temperature is lowered; the lithium iron phosphate positive electrode active material with carbon material on the surface is obtained by air jet pulverization with a particle size Dv50 of 1.65μm. The total mass of the positive electrode active material has a Ti element content of 1050ppm and a V element content of 950ppm.
[0271] The aforementioned D50 and Dv50 refer to data obtained through the Malvern laser scattering method.
[0272] (2) Preparation of positive electrode sheet
[0273] The above-mentioned positive electrode active material, conductive agent, and binder polyvinylidene fluoride were mixed in a solvent N-methylpyrrolidone at a mass ratio of 95:2:3. The mixture was thoroughly mixed, stirred, and dispersed in a stirring tank to form a positive electrode slurry. After the stirring process, the positive electrode slurry was transported to the coating process. The conductive agent consisted of conductive carbon black and multi-walled carbon nanotubes at a mass ratio of 1:1, with the conductive carbon black having a specific surface area of 80 m². 2 / g, oil absorption value of 180mL / 100g, average length of carbon nanotubes of 20μm, specific surface area of 280m². 2 / g.
[0274] The positive electrode slurry was transferred and coated onto aluminum foil, dried, and then hot-pressed to obtain a positive electrode sheet with a single-sided thickness of 106.9 μm and a compaction density of 2.35 g / cm³. 3 The positive electrode sheet. The compaction density here refers to the compaction density of the battery cell under full discharge conditions. The transfer coating speed is 20 m / min. The hot pressing process includes three hot rolling processes, with the hot rolling pressure increasing sequentially to 40 tons, 60 tons, and 80 tons; the hot rolling temperature is 60℃. Before the first hot rolling compaction, the electrode sheet is heated to 40℃.
[0275] The positive electrode sheets are slit and punched into specified shapes, and then the punched positive electrode sheets are sorted by weight using a weighing and sorting machine for stacking by a stacking machine.
[0276] Among them, in the cross-section of the positive electrode film along the electrode thickness direction, in the cumulative distribution curve of the spheroidal area of particles with particle size R1 satisfying R1≥1000nm, the median L of spheroidality is... R1A50 The median C of the graphitization degree of the positive electrode film is 0.689. 50 The median value of the positive electrode film coating, B, is 1.009. 50 The value is 0.46; the iron dissolution rate of the positive electrode material is 974 ppm; based on the total area of the cross-section of the positive electrode film along the thickness direction of the electrode sheet, the area ratio of the agglomeration region of the conductive agent is 1.68%; the porosity of the positive electrode film is 16.03%.
[0277] (3) Preparation of negative electrode sheet
[0278] A mixture of artificial graphite and natural graphite (mass ratio 1:1), conductive carbon black as a conductive agent, styrene-butadiene rubber (SBR) as a binder, and sodium carboxymethyl cellulose (CMC) as a thickener are mixed evenly in a weight percentage of 96:0.5:2.0:1.5, and deionized water is added. After stirring and dispersing, a negative electrode slurry is obtained. The negative electrode slurry is coated on a copper foil substrate, and after drying, compaction, slitting, and sheet forming, a negative electrode sheet is obtained.
[0279] The negative electrode sheets are slit and punched into specified shapes, and then the punched negative electrode sheets are sorted by weight using a weighing and sorting machine for stacking by a stacking machine.
[0280] (4) Diaphragm
[0281] Polyvinylidene fluoride (PVDF) was dissolved in N-methylpyrrolidone (NMP) and stirred until homogeneous. Polyethylene glycol (PEG) was then added as a pore-forming agent and thoroughly mixed to obtain an adhesive layer solution. This adhesive layer solution was applied to the aforementioned base membrane with ceramic layers on both sides. After pre-evaporation at 80°C and drying at 110°C, the membrane was immersed in deionized water to dissolve the PEG, resulting in a membrane with a porous adhesive layer.
[0282] The thickness of the base film is 8 μm, the thickness of the single-sided ceramic layer is 3 μm, and the thickness of the single-sided adhesive layer is 1 μm.
[0283] (5) Electrolytes
[0284] In an argon-atmospheric glove box (H₂O < 0.1 ppm, O₂ < 0.1 ppm), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and ethylene carbonate (EC) were mixed thoroughly. Lithium hexafluorophosphate was then added and dissolved in the organic solvent to achieve a concentration of 1.05 mol / L. Ethylene carbonate (VC) was then added and stirred until homogeneous, yielding the electrolyte of Example 1. Based on the total mass of the electrolyte, the mass content of dimethyl carbonate was 26%, ethyl methyl carbonate was 43.3%, ethylene carbonate was 17.3%, and ethylene carbonate was 0.9%.
[0285] (6) Battery fabrication:
[0286] The positive electrode, separator, and negative electrode are stacked sequentially using a stacking machine. The separator must effectively isolate the positive and negative electrodes to obtain a stacked battery cell. The stacked battery cell is then coated with adhesive to ensure tight containment. The coated stacked battery cell is placed in an outer packaging material, an aluminum-plastic composite film, which consists of an inner polypropylene layer, a middle aluminum foil layer, and an outer nylon layer. The aluminum-plastic film outer packaging is shaped and trimmed using a punching and forming machine to achieve the desired shape and size. The aluminum-plastic film is then heat-sealed to ensure a sealing tensile strength ≥25N / 8mm. The battery undergoes vacuum baking and settling. Electrolyte is injected using a flat-tipped needle, and the battery is sealed. Finally, the soft-pack battery undergoes hot and cold pressing operations. The hot pressing temperature is 45℃, the time is 2 minutes, and the pressure is 90kg / cm². 2 The cold pressing temperature was 25℃, the time was 2 minutes, and the pressure was 90 kg / cm². 2 Finally, after processes such as formation, vacuum degassing, edge trimming, and edge folding, the battery cell is obtained, with the edge folding process being a double fold. The battery cell has a length of 600mm, a width of 125mm, and a thickness of 20mm.
[0287] The preparation methods of Examples 2-5 are basically the same as those of Example 1, except that the preparation method of the positive electrode sheet is adjusted, as follows:
[0288] Example 2
[0289] The positive electrode slurry from Example 1 was coated onto aluminum foil and dried. By adjusting the pressure, rolling speed, roll gap, holding time, number of rolling passes, and controlling the coating density in the hot pressing process, a positive electrode sheet with a single-sided thickness of 70.45 μm and a compaction density of 2.35 g / cm³ was obtained through hot pressing. 3 The positive electrode sheet. The compaction density here refers to the compaction density of the battery cell under full discharge conditions; the testing method is described below. Keeping the number of layers constant, the thickness of the battery cell is adjusted adaptively according to the thickness of the positive electrode film.
[0290] Example 3
[0291] The positive electrode slurry from Example 1 was coated onto aluminum foil and dried. By adjusting the pressure, rolling speed, roll gap, holding time, number of rolling passes, and controlling the coating density in the hot pressing process, a positive electrode sheet with a single-sided thickness of 91.88 μm and a compaction density of 2.36 g / cm³ was obtained through hot pressing. 3 The positive electrode sheet. The compaction density here refers to the compaction density of the battery cell under full discharge conditions; the testing method is described below. Keeping the number of layers constant, the thickness of the battery cell is adjusted adaptively according to the thickness of the positive electrode film.
[0292] Example 4
[0293] The positive electrode slurry from Example 1 was coated onto aluminum foil and dried. By adjusting the pressure, rolling speed, roll gap, holding time, number of rolling passes, and controlling the coating density in the hot pressing process, a positive electrode sheet with a single-sided thickness of 119.49 μm and a compaction density of 2.35 g / cm³ was obtained through hot pressing. 3 The positive electrode sheet. The compaction density here refers to the compaction density of the battery cell under full discharge conditions; the testing method is described below. Keeping the number of layers constant, the thickness of the battery cell is adjusted adaptively according to the thickness of the positive electrode film.
[0294] Example 5
[0295] The positive electrode slurry from Example 1 was coated onto aluminum foil and dried. By adjusting the pressure, rolling speed, roll gap, holding time, number of rolling passes, and controlling the coating density in the hot pressing process, a positive electrode sheet with a single-sided thickness of 96.75 μm and a compaction density of 2.55 g / cm³ was obtained through hot pressing. 3 The positive electrode sheet. The compaction density here refers to the compaction density of the battery cell under full discharge conditions; the testing method is described below. Keeping the number of layers constant, the thickness of the battery cell is adjusted adaptively according to the thickness of the positive electrode film.
[0296] The preparation methods for Examples 6 and 7 are basically the same as those for Example 1, except that the preparation method of the electrolyte is adjusted, as detailed below:
[0297] Example 6
[0298] The proportions of each solvent in the electrolyte were adjusted so that, based on the total mass of the electrolyte, dimethyl carbonate accounted for 18%, ethyl methyl carbonate for 47.3%, ethylene carbonate for 21.3%, and vinylene carbonate for 0.9%.
[0299] Example 7
[0300] The proportions of each solvent in the electrolyte were adjusted so that, based on the total mass of the electrolyte, dimethyl carbonate accounted for 32%, ethyl methyl carbonate for 40.3%, ethylene carbonate for 14.3%, and vinylene carbonate for 0.9%.
[0301] The preparation methods of Examples 8-12 are basically the same as those of Example 1, except that the preparation methods of the positive electrode active material and the positive electrode sheet are adjusted, as detailed below:
[0302] Example 8
[0303] (1) Lithium dihydrogen phosphate, ferrous oxalate, polyethylene glycol with a weight average molecular weight of 1000, polyethylene glycol with a weight average molecular weight of 1600, titanium dioxide, and vanadium pentoxide were mixed evenly in methanol and ground to obtain a mixed raw material. The ratio of lithium dihydrogen phosphate to ferrous oxalate resulted in a lithium to iron molar ratio of 1.025:1.0. The ferrous oxalate had a particle size D10 of 6.5 μm, a particle size D50 of 62 μm, and a particle size D90 of 108 μm. The ferrous oxalate contained 30.5% Fe and 0.03% ferric iron by mass.
[0304] The mixed raw materials are ball-milled multiple times and demagnetized in a ball mill to obtain a mixed slurry. The number of grinding cycles and time are controlled, and the particle size D of the resulting mixed slurry is determined. V 50 is 3.15μm.
[0305] The spray-dried slurry yields a dried precursor powder, which is light yellow in appearance and uniform in color.
[0306] The precursor powder was placed in a sintering furnace and heated from 25°C to 360°C at a rate of 2°C / min under a nitrogen atmosphere, and held at that temperature for 3.5 hours. Then, the temperature was increased to a second temperature of 780°C at a rate of 5°C / min and held at that temperature for 10 hours. Afterward, the material was cooled. Based on the total mass of the positive electrode active material, the Ti content was 1050 ppm and the vanadium content was 950 ppm.
[0307] The obtained material was crushed using an airflow pulverization method with a grading frequency of 21 Hz and a pulverizing airflow of 0.54 MPa to obtain lithium iron phosphate cathode active material with carbon material on its surface.
[0308] The D10, D50, D90, and Dv50 mentioned above refer to the data obtained by testing using the Malvern laser scattering method.
[0309] (2) Preparation of positive electrode sheet
[0310] The above-mentioned positive electrode active material, conductive agent, and binder polyvinylidene fluoride are mixed in a mass ratio of 95:2:3 with N-methylpyrrolidone as solvent. The mixture is thoroughly mixed, stirred, and dispersed in a stirring tank to form a positive electrode slurry. After the stirring process, the positive electrode slurry is conveyed to the coating process. The stirring includes pre-stirring and main stirring. The stirring speed of pre-stirring is lower than that of main stirring. The pre-stirring has an orbital speed of 25 rpm, a rotational speed of 500 rpm, and a pre-stirring time of 15 minutes. The conductive agent includes conductive carbon black and multi-walled carbon nanotubes in a mass ratio of 1:1. The specific surface area of the conductive carbon black is 80 m². 2 / g, oil absorption value of 180mL / 100g, average length of carbon nanotubes of 20μm, specific surface area of 280m². 2 / g.
[0311] The positive electrode slurry was transferred and coated onto aluminum foil, dried, and then hot-pressed to obtain a positive electrode film with a single-sided thickness of 106.34 μm and a compaction density of 2.35 g / cm³. 3 The positive electrode sheet. Here, compaction density refers to the compaction density of a single battery cell under full discharge conditions.
[0312] The hot pressing process includes three hot roller pressing processes, with the hot roller pressing pressure increasing sequentially to 35 tons, 55 tons, and 75 tons. The hot roller temperature is 65℃. Before the first hot roller compaction, the electrode sheet is heated to 50℃.
[0313] The positive electrode sheets are slit and punched into specified shapes, and then the punched positive electrode sheets are sorted by weight using a weighing and sorting machine for stacking by a stacking machine.
[0314] Example 9
[0315] (1) Preparation of positive electrode active material
[0316] Lithium carbonate, ferric phosphate, sucrose, glucose, titanium dioxide, and vanadium pentoxide were added to water and mixed in a premixing tank at 1800 rpm. The ratio of lithium carbonate to ferric phosphate resulted in a molar ratio of iron to phosphorus of 0.97. The mass content of glucose relative to ferric phosphate was 3.8%, and the mass content of sucrose relative to ferric phosphate was 1.9%.
[0317] The mixed raw materials were ground twice in a sand mill. The first grinding was performed using 0.6 mm diameter zirconia balls at 500 rpm for 1 hour, with a grinding chamber pressure of less than 0.3 MPa. The second grinding was then performed to obtain a mixed slurry. The particle size D of the mixed slurry was... V 50 is 0.435μm;
[0318] The mixed slurry is spray-dried to obtain precursor powder.
[0319] The precursor powder is sintered to obtain lithium iron phosphate cathode material. The sintering process includes:
[0320] First sintering: The precursor powder is sintered in a nitrogen atmosphere, heated from 25°C to 765°C at a heating rate of 5°C / min, and held at that temperature for 10 hours. After cooling, the first sintered product is obtained.
[0321] Grinding and mixing: Add 0.5% sucrose, 1% glucose, and 3.0% polyethylene glycol (by weight of the first sintered product) to the first sintered product; divide into two groups and grind (third grinding), wherein the particle size D of the first group is... V50 Grinding was stopped when the particle size reached 1.02 μm (grinding conditions: 550 rpm, grinding time 1 h), yielding the first group of ground products; the particle size D of the second group... V50 Grinding was stopped when the particle size reached 0.42 μm (grinding conditions: 500 rpm, grinding time 4 h), and a second set of grinding products was obtained; the first set of grinding products and the second set of grinding products were mixed at a mass ratio of 70:30 to obtain a mixed intermediate product; the mixed intermediate product was spray-dried.
[0322] Second sintering: The dried mixed intermediate product is sintered in a nitrogen atmosphere, heated from 25°C to 800°C at a heating rate of 5°C / min, and held at that temperature for 10 hours. After cooling, the second sintered product is obtained.
[0323] After sintering, the material is cooled to below 100°C, and the second sintering product is crushed using air jet milling to obtain lithium iron phosphate cathode active material with carbon material on its surface. The air jet milling stage frequency is 23Hz, and the milling pressure is 0.55MPa. Based on the total mass of the cathode active material, the mass content of Ti is 1050ppm, and the mass content of V is 950ppm.
[0324] (2) Preparation of positive electrode sheet
[0325] The above-mentioned positive electrode active material, conductive agent, and binder polyvinylidene fluoride are mixed in a mass ratio of 95:2:3 with N-methylpyrrolidone as solvent. The mixture is thoroughly mixed, stirred, and dispersed in a stirring tank to form a positive electrode slurry. After the stirring process, the positive electrode slurry is conveyed to the coating process. The stirring includes pre-stirring and main stirring. The stirring speed of pre-stirring is lower than that of main stirring. The pre-stirring has an orbital speed of 25 rpm, a rotational speed of 500 rpm, and a pre-stirring time of 15 minutes. The conductive agent includes conductive carbon black and multi-walled carbon nanotubes in a mass ratio of 1:1. The specific surface area of the conductive carbon black is 80 m². 2 / g, oil absorption value of 180mL / 100g, average length of carbon nanotubes of 20μm, specific surface area of 280m². 2 / g.
[0326] The positive electrode slurry was transferred and coated onto aluminum foil, dried, and then hot-pressed to obtain a positive electrode film with a single-sided thickness of 106.66 μm and a compaction density of 2.36 g / cm³. 3 The positive electrode sheet. The compaction density here refers to the compaction density of the battery cell under full discharge conditions. The drying temperature is 95℃, and the drying speed is 2.0 m / min.
[0327] The hot pressing process includes three hot roller pressing processes, with the hot roller pressing pressure increasing sequentially to 35 tons, 55 tons, and 75 tons. The hot roller temperature is 65℃. Before the first hot roller compaction, the electrode sheet is heated to 50℃.
[0328] The positive electrode sheets are slit and punched into specified shapes, and then the punched positive electrode sheets are sorted by weight using a weighing and sorting machine for stacking by a stacking machine.
[0329] Example 10
[0330] The preparation method of Example 10 is basically the same as that of Example 1, except that the preparation process of the positive electrode active material and the hot pressing process of the positive electrode sheet are slightly different. The specific differences include:
[0331] (1) The carbon sources in the mixed raw materials are sucrose and glucose. The mass of sucrose is 2 wt% of the mass of iron phosphate, and the mass of glucose is 5.7 wt% of the mass of iron phosphate.
[0332] (2) The heating and sintering processes are different. The precursor powder is sintered at least twice in a nitrogen atmosphere. The first sintering temperature is 750℃ and the holding time is 8 hours to obtain the initial sintered product.
[0333] 1.5 wt% (based on the mass of the initial calcination product) of glucose, 3.0 wt% (based on the mass of the initial calcination product) of polyethylene glycol, titanium dioxide, and vanadium pentoxide were added to the initial calcination product. After grinding evenly, the mixture was divided into two groups for secondary grinding. The grinding parameters for the two groups were different, and the particle size distribution (D) of the particles after grinding in the first group was controlled. V50 The particle size (D) of the second group of milled particles is 2.0 μm. V50 The particle size was 0.35 μm. The ground particles from the first and second groups were mixed at a mass ratio of 30:70, spray-dried, and then subjected to a second sintering. The second sintering temperature was 800℃, and the temperature was maintained for 10 hours.
[0334] Based on the total mass of the positive electrode active material, the mass percentage of titanium is 1050 ppm and the mass percentage of vanadium is 950 ppm.
[0335] (3) The positive electrode slurry was transferred and coated onto aluminum foil, dried, and hot-pressed to obtain a positive electrode film with a single-sided thickness of 106.79 μm and a compaction density of 2.36 g / cm³. 3 The positive electrode sheet. The compaction density here refers to the compaction density of the battery cell under full discharge conditions. The drying temperature is 95℃, and the drying speed is 2.0 m / min.
[0336] The hot pressing process includes three hot roller pressing processes, with the hot roller pressing pressure increasing sequentially to 35 tons, 55 tons, and 70 tons. The hot roller temperature is 65℃. Before the first hot roller compaction, the electrode sheet is heated to 50℃.
[0337] Example 11
[0338] The preparation method of Example 11 is basically the same as that of Example 1, except that the sintering process of the positive electrode active material and the hot pressing process of the positive electrode sheet are different. Specifically:
[0339] (1) The precursor powder was subjected to a two-stage heating sintering process in a nitrogen atmosphere to obtain the positive electrode active material: the temperature was increased from 25℃ to 440℃ at a heating rate of 2℃ / min (first heating stage), and held for 2.5h; the temperature was increased from 440℃ to 760℃ at a heating rate of 5℃ / min (second heating stage), and held for 11h; the particle size Dv was obtained by air jet milling. 50 The active cathode material is a lithium iron phosphate cathode with a carbon material on its 1.6 μm surface. The air jet milling stage frequency is 25 Hz, and the milling pressure is 0.55 MPa.
[0340] (2) The positive electrode slurry was transferred and coated onto an aluminum foil, dried, and hot-pressed to obtain a positive electrode film with a single-sided thickness of 106.10 μm and a compaction density of 2.35 g / cm³. 3 The positive electrode sheet. The compaction density here refers to the compaction density of the battery cell under full discharge conditions. The transfer coating speed is 20 m / min.
[0341] The hot pressing process includes three hot roller pressing processes, with the hot roller pressing pressure increasing sequentially to 45 tons, 60 tons, and 80 tons. The hot roller temperature is 60℃. Before the first hot roller compaction, the electrode sheet is heated to 40℃.
[0342] Example 11
[0343] The preparation method of Example 11 is similar to that of Example 8, except that in the preparation of the positive electrode sheet, the above-mentioned positive electrode active material, conductive agent, and binder polyvinylidene fluoride are uniformly mixed in the solvent N-methylpyrrolidone at a mass ratio of 94.52:1.99:2.99. Based on the total mass of the positive electrode active material, conductive agent, binder polyvinylidene fluoride and dispersant, 0.5% of the dispersant HNBR is added. The mixture is thoroughly mixed in a stirring tank, stirred, and dispersed to form a positive electrode slurry.
[0344] Example 12
[0345] The preparation method of Example 12 is similar to that of Example 11, except that in the preparation of the positive electrode sheet, the above-mentioned positive electrode active material, conductive agent, and binder polyvinylidene fluoride are uniformly mixed in the solvent N-methylpyrrolidone at a mass ratio of 93.57:1.97:2.96, and then 1.5% of the dispersant HNBR is added based on the total mass of the positive electrode active material, conductive agent, binder polyvinylidene fluoride and dispersant.
[0346] The preparation method of Example 13 is basically the same as that of Example 1, except that the preparation method of the positive electrode sheet is adjusted, as follows:
[0347] Example 13
[0348] The conductive agent used in Example 12 includes 2% conductive carbon black by mass, excluding carbon nanotubes, and the specific surface area of the conductive carbon black is 85 m². 2 / g, oil absorption value is 200ml / 100g.
[0349] The preparation method of Comparative Example 1 is basically the same as that of Example 1, except that the battery preparation process is different, specifically:
[0350] In Comparative Example 1, the folding process involves a single fold.
[0351] The preparation methods of Comparative Examples 2 and 3 are basically the same as those of Example 1, except that the preparation method of the positive electrode sheet is adjusted, as follows:
[0352] Comparative Example 2
[0353] The positive electrode slurry from Example 1 was coated onto aluminum foil and dried. By adjusting the pressure, rolling speed, roll gap, holding time, number of rolling passes, and controlling the coating density in the hot pressing process, a positive electrode film with a single-sided thickness of 65.08 μm and a compaction density of 2.35 g / cm³ was obtained through hot pressing. 3 The positive electrode sheet. The compaction density here refers to the compaction density of the battery cell under full discharge conditions; the testing method is described below. Keeping the number of layers constant, the thickness of the battery cell is adjusted adaptively according to the thickness of the positive electrode film.
[0354] Comparative Example 3
[0355] The positive electrode slurry from Example 1 was coated onto aluminum foil and dried. By adjusting the pressure, rolling speed, roll gap, holding time, number of rolling passes, and controlling the coating density in the hot pressing process, the single-sided thickness of the positive electrode film was 125.64 μm, and the compaction density was 2.52 g / cm³. 3 The positive electrode sheet. The compaction density here refers to the compaction density of the battery cell under full discharge conditions; the testing method is described below. Keeping the number of layers constant, the thickness of the battery cell is adjusted adaptively according to the thickness of the positive electrode film.
[0356] The preparation method of Comparative Example 4 is basically the same as that of Example 1, except that the preparation method of the electrolyte is adjusted, as follows:
[0357] Comparative Example 4
[0358] The proportions of each solvent in the electrolyte were adjusted so that, based on the total mass of the electrolyte, dimethyl carbonate accounted for 36%, ethyl methyl carbonate for 38.3%, ethylene carbonate for 12.3%, and vinylene carbonate for 0.9%.
[0359] The preparation method of Comparative Example 5 is basically the same as that of Example 1, except that the preparation method of the positive electrode active material is adjusted, as follows:
[0360] Comparative Example 5
[0361] The precursor powder was subjected to a two-stage heating and sintering process in a nitrogen atmosphere to obtain the positive electrode active material: the temperature was increased from 25℃ to 500℃ at a heating rate of 2℃ / min (first heating stage), and held for 3.5h; the temperature was increased from 500℃ to 800℃ at a heating rate of 5℃ / min (second heating stage), and held for 13h; the material was then subjected to air jet milling to obtain a lithium iron phosphate positive electrode active material with a particle size Dv50 of 1.6μm and a carbon material on its surface. The air jet milling stage frequency was 25Hz, and the milling pressure was 0.55MPa.
[0362] Test methods
[0363] 1. Electrode compaction density test (full load)
[0364] The battery cell was placed in a 25°C oven and left to stand for 2 hours. Once the battery temperature was maintained at 25°C, the battery was discharged at a constant current of 1 / 3C to 2.0V. The battery was then disassembled to obtain the positive electrode. The residual electrolyte was treated with dimethyl carbonate solvent, the electrode was dried, and cut into small circular pieces with an area of S. The mass of the circular pieces was obtained as W1, and the thickness of the positive electrode was measured using a micrometer. The positive electrode film layer of the weighed electrode was then wiped off, and the mass of the current collector was measured and recorded as W2. The thickness of the current collector was measured using a micrometer. The compaction density of the positive electrode film layer is PD = (W1-W2) / [(T1-T2)×S].
[0365] 2. Rebound Rate Test
[0366] The compacted positive electrode sheet was used to measure the initial one-sided thickness of the positive electrode film layer using a laser thickness gauge, denoted as T0 (in μm). This was then combined with other components and processed into a single battery cell. At 25°C, the cell was charged to 3.65V at a 0.5C charging rate (the nominal capacity of the battery cell), then charged at 3.65V to 0.05C, allowed to stand for 10 minutes, and then discharged at a 1C discharging rate to 2.5V, allowed to stand for 10 minutes. This charge-discharge cycle was completed. After repeating this cycle 100 times, the battery cell was disassembled to obtain the positive electrode sheet. After standing for 1 hour, the one-sided thickness of the positive electrode film layer after the cycle was measured using a laser thickness gauge, denoted as T1 (in μm). The rebound rate of the battery cell was calculated as: Rebound rate = (T1 - T0) / T0 × 100%.
[0367] 3. Gas production test
[0368] At 25℃, the battery cells were charged to 3.65V at a 0.5C charging rate (the nominal capacity of each cell), then charged to 0.05C at 3.65V, allowed to stand for 10 minutes, and then discharged to 2.5V at a 1C discharging rate, allowed to stand for 10 minutes. The initial thickness (T2) of the battery cells was measured in μm using a laser thickness gauge at 25℃. One charge-discharge cycle was counted. After repeating the above cycle 100 times, the cells were allowed to stand for 1 hour, and the thickness (T3) of the battery cells after the cycle was measured in μm using a laser thickness gauge. The gas production rate of the battery cells was calculated as: Gas production rate = (T3 - T2) / T2 × 100%.
[0369] The battery cells for each embodiment and comparative example were prepared according to the above method. Specific parameters and performance are shown in the tables below.
[0370] Table 1
[0371] In Comparative Example 1, only a single-folded first sealing area was provided, resulting in encapsulation failure during long-term cycling and poor reliability. In Comparative Example 2, the positive electrode film thickness was small, leading to low space occupation by the positive electrode active material and low capacity of the battery cell. In Comparative Example 3, the positive electrode film thickness was too large, resulting in severe rebound and increased pressure in the sealing area, affecting the long-term reliability of the battery cell. In Comparative Example 4, the excessive DMC content in the electrolyte easily generated gas, increasing the internal pressure of the battery cell, causing encapsulation failure, and reducing the reliability of the battery cell. In Comparative Example 5, the area ratio of particles with a particle size R1 satisfying R1≥1000nm was too large, resulting in severe rebound of the positive electrode film and easy failure of the sealing area of the battery cell.
[0372] Referring to Figure 1, the specific description of the battery cell in the embodiments of this application is as follows:
[0373] A single battery cell includes a stacked cell and a housing, wherein the stacked cell is housed within the housing, and the housing is made of a soft-pack material. The housing includes a first sealing area located at at least one end of the stacked cell extending along its width. The first sealing area includes a double-folded edge structure extending along its length, on which encapsulating adhesive is continuously disposed and fixed. The stacked cell includes a positive electrode, a negative electrode, and an electrolyte. The positive electrode includes a positive current collector and an electrolyte disposed within the housing. The positive electrode current collector has a positive electrode film layer on at least one side, the positive electrode film layer comprising lithium transition metal phosphate particles, and at least a portion of the surface of the lithium transition metal phosphate particles is provided with carbon material; based on the total area of particles in the cross-section of the positive electrode film layer along the thickness direction of the positive electrode sheet, the area ratio of particles with a particle size R1 satisfying R1≥1000nm is 12%-50%; the thickness of the positive electrode film layer on one side is denoted as H, where H is 70μm-120μm; when the battery cell is in a fully discharged state, the compaction density of the positive electrode sheet is 2.3g / cm³. 3 -2.6g / cm 3 The electrolyte includes a solvent, which includes dimethyl carbonate (DMC); the mass percentage of dimethyl carbonate is 18%-32% based on the total mass of the electrolyte.
[0374] Thus, by using a stacked cell structure, a larger thickness of the positive electrode film, high voltage density, and a larger area ratio of R1 particle size particles, the capacity and energy density of the battery cells are improved. Furthermore, the double-folded edge structure of the first sealing area and the combination of encapsulating adhesive can significantly improve the mechanical strength of the sealing area and reduce the possibility of sealing failure due to internal pressure during long-term cycling.
[0375] As can be seen from Examples 1, 8, 9, 11 and Example 10, based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the positive electrode sheet, when the area proportion of particles with a particle size R1 satisfying R1≥1000 nm is 12%-40%, the rebound rate is further reduced, which is beneficial to improving the long-term reliability of the battery cell.
[0376] Table 2
[0377] As can be seen from Examples 1, 8-11, based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the positive electrode sheet, in the area cumulative distribution curve of the spheroidicity of particles with a particle size R1 satisfying R1≥1000 nm, the median L of the spheroidicity R1A50 is 0.6-0.8; when the distribution uniformity of particles with a particle size R1 satisfying R1≥1000 nm is less than or equal to 5%, the battery cell has a relatively low rebound rate and gas production rate. In the area cumulative distribution curve of the spheroidicity of particles with a particle size R1 satisfying R1≥1000 nm, the median L of the spheroidicity R1A50 is 0.67-0.75; the distribution uniformity of particles with a particle size R1 satisfying R1≥1000 nm is in the range of 0.2%-2%, which helps to further improve the long-cycle stability of the battery.
[0378] Table 3
[0379] As can be seen from Examples 8, 11, and 12, the distribution uniformity of particles with a particle size R1 satisfying R1≥1000 nm is in the range of 0.2%-0.9%, which helps to further reduce the stress concentration degree and reduce the rebound of the positive electrode film layer, thereby improving the long-cycle reliability of the battery.
[0380] Table 4
[0381] As can be seen from the comparison between Example 1 and Example 13, the conductive agent includes carbon nanotubes, and the mass content C1 of the carbon nanotubes satisfies 0<C1≤2.5%, which is beneficial to reducing the rebound of the positive electrode film layer during the cycle process, thereby improving the long-term reliability of the battery.
[0382] It should be noted that the present application is not limited to the above-described embodiments. The above-described embodiments are merely examples, and all embodiments that have substantially the same configuration as the technical idea within the scope of the technical solution of the present application and exert the same functions and effects are included in the technical scope of the present application. Furthermore, within the scope not departing from the gist of the present application, various modifications that a person skilled in the art can conceive for the embodiments, and other configurations constructed by combining part of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A battery cell, characterized by The device includes a laminated battery cell and a housing, wherein the laminated battery cell is housed within the housing, and the housing is made of a flexible packaging material; the housing includes a first sealing area, which is disposed at at least one end of the laminated battery cell extending along the width direction; the first sealing area includes a double-folded edge structure extending along the length direction, and encapsulating adhesive is disposed on the double-folded edge structure, which is continuously disposed along the length direction and fixes the double-folded edge structure; The laminated cell includes a positive electrode, a negative electrode, and an electrolyte. The positive electrode includes a positive current collector and a positive electrode film layer disposed on at least one side of the positive current collector. The positive electrode film layer includes lithium-containing transition metal phosphate particles, and at least a portion of the surface of the lithium-containing transition metal phosphate particles is provided with carbon material. Based on the total area of particles in the cross-section of the positive electrode film along the thickness direction of the positive electrode sheet, the area ratio of particles with a particle size R1 satisfying R1≥1000nm is 12%-50%. The thickness of the positive electrode film layer on one side is denoted as H, where H is 70μm-120μm. The compaction density of the positive electrode sheet is 2.3 g / cm 3 -2.6 g / cm 3 ; The electrolyte includes a solvent, which includes dimethyl carbonate (DMC); the mass percentage of dimethyl carbonate is 18%-32% based on the total mass of the electrolyte.
2. The battery cell of claim 1, wherein, The thickness of the positive electrode film on one side is denoted as H, where H is 90μm-120μm, and can be selected as 100μm-120μm.
3. The battery cell according to claim 1 or 2, characterized in that, The housing includes at least one second sealing area, which is disposed at at least one end of the laminated cell along the length direction of the housing, and the second sealing area is disposed on the tab side of the laminated cell.
4. The battery cell according to any one of claims 1 to 3, characterized in that, The outer periphery of the laminated battery cell is provided with a plurality of rubber rings that surround it along the width direction, and the rubber rings that surround it along the width direction are spaced apart along the length direction.
5. The battery cell according to any one of claims 1 to 4, characterized in that, Based on the total area of particles in the cross-section of the positive electrode film along the thickness direction of the positive electrode sheet, the area ratio of particles with a particle size R1 satisfying R1≥1000nm is 12%-37%.
6. The battery cell according to any one of claims 1 to 5, characterized in that, In a section of the positive electrode film layer along the thickness direction of the electrode tab, the median number L of sphericity in the area cumulative distribution curve of the particles having a particle size R1 satisfying R1≥1000 nm R1A50 0.6-0.8, optionally 0.65-0.75, further optionally 0.67-0.
75.
7. The battery cell of any one of claims 1 to 6, wherein, In the cross-section of the positive electrode film layer along the thickness direction of the electrode sheet, the uniformity of the distribution of particles with a particle size R1 satisfying R1≥1000nm is less than or equal to 5%, which can be selected as 0.2%-2%, and further selected as 0.2%-0.9%.
8. The battery cell of any one of claims 1 to 7, wherein, The electrolyte also satisfies at least one of the following conditions: (1) The solvent in the electrolyte further includes one or both of ethyl methyl carbonate (EMC) and ethylene carbonate (EC); (2) Based on the total mass of the electrolyte, the mass percentage of ethyl methyl carbonate (EMC) is 39%-49%; (3) Based on the total mass of the electrolyte, the mass percentage of ethylene carbonate (EC) is 13%-22%; (4) Based on the total mass of the electrolyte, the total mass ratio of ethyl methyl carbonate (EMC) and ethylene carbonate (EC) is 52%-71%; (5) The electrolyte includes an electrolyte salt, which includes lithium hexafluorophosphate (LiPF6), and the concentration of lithium hexafluorophosphate in the electrolyte is 0.9 mol / L to 1.2 mol / L; (6) Based on the total mass of the electrolyte, the mass percentage of dimethyl carbonate is 18%-26%.
9. The battery cell of any one of claims 1 to 8, wherein, The median value C of the graphitization degree in the cumulative distribution curve of the graphitization degree C value obtained by the positive electrode film layer in the laser microscopic confocal Raman spectrometer face scanning mode 50为 0.95-1.20, wherein the graphitization degree C value is I G / I D , wherein I G represents the G peak intensity of the Raman spectrum at 1580±100 cm -1 , I D represents the D peak intensity of the Raman spectrum at 1350±100 cm -1 .
10. The battery cell of any one of claims 1 to 9, wherein, The median value B of the coating value in the cumulative distribution curve of the coating value B obtained by the positive electrode film layer under the laser microscopic confocal Raman spectrometer face scanning mode 50 is 0.30-0.60, wherein the coating value B is I P / I D , wherein I P represents the P peak intensity of the Raman spectrum at 948±100cm -1 , I D represents the D peak intensity of the Raman spectrum at 1350±100cm -1 .
11. The battery cell of any one of claims 1 to 10, wherein, The lithium-containing transition metal phosphate particles comprise an iron element, and the iron dissolution rate of the positive electrode film layer is 658ppm-1921ppm, optionally 658ppm-1485ppm.
12. The battery cell of any one of claims 1 to 11, wherein, The positive electrode film layer further comprises a conductive agent, and based on the total area of the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the total area proportion of the agglomerated regions of the conductive agent is 0.5%-2.5%, optionally 0.5%-1.7%.
13. The battery cell of claim 12, wherein, The conductive agent comprises carbon nanotubes, and the carbon nanotubes are one or more of single-walled carbon nanotubes, few-walled carbon nanotubes and multi-walled carbon nanotubes, optionally, the conductive agent further comprises conductive carbon black.
14. The battery cell according to claim 12 or 13, characterized in that, The agglomerated regions of the conductive agent comprise carbon nanotubes and conductive carbon black.
15. The battery cell of claim 14, wherein, Based on the mass of the positive electrode film layer, the mass content C1 of the carbon nanotubes satisfies: 0<C1≤2.5%, and the mass content C2 of the conductive carbon black satisfies: 0<C2≤2.5%.
16. The battery cell of any one of claims 1 to 15, wherein, The positive electrode film layer further comprises a dispersant, and the dispersant comprises hydrogenated nitrile butadiene rubber (HNBR).
17. The battery cell of claim 16, wherein, Based on the mass of the positive electrode film layer, the mass content of the dispersant is 0.5%-2%.
18. The battery cell of any one of claims 1-17, wherein, The porosity of the positive electrode film layer is 14%-28%.
19. The battery cell of any one of claims 1-18, wherein, The battery cell further comprises a separator arranged between the positive electrode sheet and the negative electrode sheet, the separator comprises a base film, ceramic layers arranged on both sides of the base film, and an adhesive layer arranged on at least one side of the ceramic layer away from the base film, the adhesive layer is a continuous layer with a porous structure, and the adhesive layer comprises a vinylidene fluoride-based polymer.
20. The battery cell of any one of claims 1-19, wherein, A primer layer is disposed in the bottom region of the positive electrode film layer adjacent to the positive electrode current collector, and the primer layer satisfies at least one of the following conditions: (1) The primer layer comprises a conductive agent and a binder, the conductive agent comprises carbon nanotubes and conductive carbon black, and the binder comprises a vinylidene fluoride polymer; (2) The thickness of the primer layer is 0.5μm-5μm.
21. The battery cell of any one of claims 1-20, wherein, The lithium-containing transition metal phosphate particles in the positive electrode film layer include a component represented by the following general formula: Li m Fe x P y O j Q q Formula I, Wherein, Q is one or more of Al, Na, K, Mg, Cu, Mn, Cr, Zn, Pb, Ca, Co, Ni, Sr, Nb, V, Ti, B, S, Si, N, F, Cl, Br, 0.8≤m≤1.15, 0.9≤x≤1, 0.95≤y≤1, 3.5≤j≤4, 0≤q≤0.
1.
22. The battery cell of any one of claims 1-21, wherein, The lithium-containing transition metal phosphate particles comprise a titanium element, and based on the total mass of the lithium-containing transition metal phosphate particles in the positive electrode film layer, the mass content of the titanium element is 500ppm-8000ppm, optionally 1000ppm-3000ppm.
23. The battery cell of any one of claims 1-22, wherein, The lithium-containing transition metal phosphate particles comprise a vanadium element, and based on the total mass of the lithium-containing transition metal phosphate particles in the positive electrode film layer, the mass content of the vanadium element is 500ppm-5000ppm, optionally 500ppm-3000ppm.
24. The battery cell of any one of claims 1-23, wherein, The soft packaging material comprises an aluminum-plastic composite film, optionally, comprises a composite film formed by aluminum and one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), nylon, polyethylene terephthalate (PET), and polyethylene (PE).
25. The battery cell of any one of claims 1-24, wherein, At least one of the laminated cells is housed within the housing, the housing having a length dimension of L0, a width dimension of W0, and a thickness dimension of H0, wherein 450mm≤L0≤1300mm, 100mm≤W0≤150mm, and 14mm≤H0≤22mm.
26. The battery cell of claim 25, wherein, The length dimension L0 of the shell satisfies: 450mm≤L0≤650mm.
27. The battery cell of claim 25, wherein, The length dimension L0 of the shell satisfies: 900mm≤L0≤1300mm.
28. The battery cell of any one of claims 1 to 27, wherein, At 25°C, the capacity of the battery cell is 105Ah-300Ah, and can be selected as 150Ah-190Ah.
29. A battery device, characterized by Includes the battery cell as described in any one of claims 1 to 28.
30. An electrical device, comprising: The electrical device includes the battery device as described in claim 29, the battery device being used to provide electrical energy.
31. An energy storage device, comprising: The energy storage device includes the battery device as described in claim 29, the battery device being used to store electrical energy.