Thickened insulating paperboard and production method thereof

By using specific raw materials and process flow, the interlayer bonding force and tensile strength of insulated cardboard are improved, waterproof and fire-proof performance are enhanced, the problem of insufficient performance of existing insulated cardboard is solved, and the service life is extended.

CN114657806BActive Publication Date: 2024-11-22SHANTOUCHENGHAI DISTRICT XINANDONGSHEZAO PAPER MILL
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202011540362.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-23
Publication Date
2024-11-22
Estimated Expiration
2040-12-23

AI Technical Summary

Technical Problem

The existing insulating cardboard has weak interlayer bonding force, low tensile strength, poor waterproof and fireproof performance, and is prone to cracking during long-term use.

Method used

Use unbleached sulfate coniferous wood pulp, polyethylene glycol, polyacrylamide, acrylic-2-ethylhexyl acrylic acid and styrene copolymer, oxidized starch, tetrasodium pyrophosphate, formaldehyde, paranitrophenol, waterproof film , fiberglass mesh cloth, fireproof mud, grid-shaped carbon fiber reinforced rib plates and UV wear-resistant coatings and other raw materials, through beating, hot pressing and multi-layer structural design, the strength and waterproof and fire-resistant performance of the cardboard are improved.

Benefits of technology

It significantly improves the interlayer bonding force and tensile strength of insulating cardboard, reduces the conductivity, enhances waterproof and fire-proof performance, extends service life, and avoids cracking.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the field of paperboard production, in particular to a thickened insulating paperboard and a production method thereof. Aiming at the problem that the interlayer bonding force of the existing insulating paperboard is weak, the tensile strength is low, and the waterproof and fireproof performance during use is poor, the following scheme is proposed, wherein the thickened insulating paperboard includes 50-70 parts of unbleached kraft softwood pulp, 20-30 parts of water, 0.1-0.6 parts of polyethylene glycol, 1-5 parts of polyacrylamide, 1-6 parts of a copolymer of acrylic acid-2-ethylhexyl and styrene, 1-10 parts of oxidized starch, 1-3 parts of tetrasodium pyrophosphate, 0.1-0.5 parts of formaldehyde, 0.3-0.6 parts of p-nitrophenol, and 1-5 parts of a waterproof film. The thickened insulating paperboard of the invention has a relatively strong interlayer bonding force, a relatively high tensile strength, a relatively low electrical conductivity, a relatively good waterproof and fireproof performance during use, can also avoid cracking after long-term use, and has a longer service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of paperboard production, and in particular to a thickened insulating paperboard and a production method thereof. Background Art

[0002] A general term for insulating paperboards for the electrical industry. Air-insulated paperboards must also have a high degree of tightness and withstand voltage strength. They are made of unbleached sulphate wood pulp and are made by sticky beating. They are used in motors, power meters, etc. There are usually air-insulated paperboards and oil-insulated paperboards. Insulating paperboards are divided into flat sheets and roll sheets. The thickness is greater than 0.5 mm for flat sheets, and the thickness is 0.5 mm or less for roll sheets. The raw materials of insulating paperboards are unbleached sulphate wood pulp and cotton pulp. The two raw materials are pulped separately. Purified water must be used in production. Pipes and pulp pumps must be cleaned and washed. Impurities containing conductive components must not be mixed. Special insulating paperboard machines are used for papermaking.

[0003] However, the existing insulating paperboard has weak interlayer bonding force and low tensile strength, and has poor waterproof and fireproof performance during use. Summary of the invention

[0004] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a thickened insulating paperboard and a production method thereof.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A thickened insulating paperboard comprises the following raw materials in parts by weight: 50-70 parts of unbleached kraft softwood pulp, 20-30 parts of water, 0.1-0.6 parts of polyethylene glycol, 1-5 parts of polyacrylamide, 1-6 parts of a copolymer of 2-ethylhexyl acrylate and styrene, 1-10 parts of oxidized starch, 1-3 parts of tetrasodium pyrophosphate, 0.1-0.5 parts of formaldehyde, 0.3-0.6 parts of p-nitrophenol, 1-5 parts of a waterproof film, 1-5 parts of a glass fiber mesh cloth, 1-5 parts of fireproof mud, 1-5 parts of a grid-shaped carbon fiber reinforcing rib plate, 1-5 parts of a fireproof coating and 1-5 parts of a UV wear-resistant coating.

[0007] Preferably, the raw materials include the following parts by weight: 50 parts of unbleached kraft softwood pulp, 20 parts of water, 0.1 parts of polyethylene glycol, 1 part of polyacrylamide, 1 part of copolymer of 2-ethylhexyl acrylate and styrene, 1 part of oxidized starch, 1 part of tetrasodium pyrophosphate, 0.1 parts of formaldehyde, 0.3 parts of p-nitrophenol, 1 part of waterproof film, 1 part of glass fiber mesh cloth, 1 part of fireproof mud, 1 part of grid-like carbon fiber reinforcement plate, 1 part of fireproof coating and 1 part of UV wear-resistant coating.

[0008] The present invention also proposes a method for producing thickened insulating paperboard, comprising the following steps:

[0009] S1: weigh the following raw materials in parts by weight: 50-70 parts of unbleached kraft softwood pulp, 20-30 parts of water, 0.1-0.6 parts of polyethylene glycol, 1-5 parts of polyacrylamide, 1-6 parts of copolymer of 2-ethylhexyl acrylate and styrene, 1-10 parts of oxidized starch, 1-3 parts of tetrasodium pyrophosphate, 0.1-0.5 parts of formaldehyde, 0.3-0.6 parts of p-nitrophenol, 1-5 parts of waterproof film, 1-5 parts of glass fiber mesh cloth, 1-5 parts of fireproof mud, 1-5 parts of grid-shaped carbon fiber reinforcement plate, 1-5 parts of fireproof coating and 1-5 parts of UV wear-resistant coating;

[0010] S2: Send the water described in S1 into the filter box for primary filtration, filter out large particles of impurities in the water, and then send the water after the primary filtration into the softening water equipment for softening. The softened water is then sent to the reverse osmosis and water purifier, so that water molecules and ionic mineral elements pass through the reverse osmosis membrane, while most of the inorganic salts, organic matter, bacteria, viruses, etc. dissolved in the water cannot pass through the reverse osmosis membrane, so that the permeated pure water and the non-permeated concentrated water are strictly separated to obtain purified water. The purified water can reduce the salt content, effectively remove various impurities in the water, reduce the conductive ions in the water, thereby reducing the conductivity and improving the resistivity of the outlet water;

[0011] S3: The unbleached kraft conifer pulp described in S1 is sent to a pulper for crushing to obtain crushed pulp, and the crushed pulp is sent to a pulper for beating, and polyethylene glycol, polyacrylamide, a copolymer of 2-ethylhexyl acrylate and styrene, oxidized starch, tetrasodium pyrophosphate, formaldehyde and p-nitrophenol are simultaneously put into the pulper for stirring, and the purified water described in S2 is added into the pulper for stirring together, and then the pulp after beating is sent to a paper machine for processing into a semi-finished product, and fine fibers are recovered by an air flotation machine during the processing of the paper machine, and sent to a pulper for further processing to obtain wet paper, which can increase the fine fiber content in the pulp, improve the strength of the insulating paperboard, and also improve the strength of the wet paper sheet;

[0012] S4: feeding the wet paper described in S3 into a conveyor for conveying, and the conveyor feeds the wet paper into a hot press for hot pressing to obtain insulating paperboard;

[0013] S5: Send the insulating cardboard described in S4 to the processing table, and paste and connect waterproof films on both sides of the insulating cardboard, paste and connect glass fiber mesh cloth on the two waterproof films, apply fireproof mud on the two glass fiber mesh cloths, install grid-shaped carbon fiber reinforcement plates on the surfaces of the two fireproof muds, and finally spray fireproof coating and UV wear-resistant coating on the surfaces of the two grid-shaped carbon fiber reinforcement plates to obtain thickened insulating cardboard.

[0014] Preferably, in S3, the pulping time of the pulper is 30-40 minutes, and the crushing speed in the pulper is 8000-12000 r / min.

[0015] Preferably, in S3, the beating time of the pulper is 40-60 minutes, and the crushing speed in the pulper is 4000-6000 r / min.

[0016] Preferably, in S4, the working temperature of the hot press is 130° C.-180° C., and the pressure is 0.2-0.9 MPa.

[0017] Preferably, in S5, the thickness of the waterproof film is 0.3-0.6 mm, and the thickness of the glass fiber mesh cloth is 1.5-2.5 mm.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] The thickened insulating paperboard of the present invention has strong interlayer bonding force, high tensile strength, low conductivity, good waterproof and fireproof performance when in use, can avoid cracking after long-term use, and has a longer service life. DETAILED DESCRIPTION

[0020] The technical solutions in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0021] Embodiment 1

[0022] A thickened insulating paperboard comprises the following raw materials in parts by weight: 50 parts of unbleached kraft softwood pulp, 20 parts of water, 0.1 parts of polyethylene glycol, 1 part of polyacrylamide, 1 part of a copolymer of 2-ethylhexyl acrylate and styrene, 1 part of oxidized starch, 1 part of tetrasodium pyrophosphate, 0.1 parts of formaldehyde, 0.3 parts of p-nitrophenol, 1 part of a waterproof film, 1 part of a glass fiber mesh cloth, 1 part of fireproof mud, 1 part of a grid-shaped carbon fiber reinforcing rib plate, 1 part of a fireproof coating and 1 part of a UV wear-resistant coating.

[0023] This embodiment also provides a method for producing thickened insulating paperboard, comprising the following steps:

[0024] S1: weigh the following raw materials in order by weight: 50 parts of unbleached kraft softwood pulp, 20 parts of water, 0.1 parts of polyethylene glycol, 1 part of polyacrylamide, 1 part of copolymer of 2-ethylhexyl acrylate and styrene, 1 part of oxidized starch, 1 part of tetrasodium pyrophosphate, 0.1 parts of formaldehyde, 0.3 parts of p-nitrophenol, 1 part of waterproof film, 1 part of glass fiber mesh cloth, 1 part of fireproof mud, 1 part of grid-shaped carbon fiber reinforcement plate, 1 part of fireproof coating and 1 part of UV wear-resistant coating;

[0025] S2: Send the water described in S1 into the filter box for primary filtration, filter out large particles of impurities in the water, and then send the water after the primary filtration into the softening water equipment for softening. The softened water is then sent to the reverse osmosis and water purifier, so that water molecules and ionic mineral elements pass through the reverse osmosis membrane, while most of the inorganic salts, organic matter, bacteria, viruses, etc. dissolved in the water cannot pass through the reverse osmosis membrane, so that the permeated pure water and the non-permeated concentrated water are strictly separated to obtain purified water. The purified water can reduce the salt content, effectively remove various impurities in the water, reduce the conductive ions in the water, thereby reducing the conductivity and improving the resistivity of the outlet water;

[0026] S3: The unbleached kraft conifer pulp described in S1 is sent to a pulper for crushing to obtain crushed pulp, and the crushed pulp is sent to a pulper for beating, and polyethylene glycol, polyacrylamide, a copolymer of 2-ethylhexyl acrylate and styrene, oxidized starch, tetrasodium pyrophosphate, formaldehyde and p-nitrophenol are simultaneously put into the pulper for stirring, and the purified water described in S2 is added into the pulper for stirring together, and then the pulp after beating is sent to a paper machine for processing into a semi-finished product, and fine fibers are recovered by an air flotation machine during the processing of the paper machine, and sent to a pulper for further processing to obtain wet paper, which can increase the fine fiber content in the pulp, improve the strength of the insulating paperboard, and also improve the strength of the wet paper sheet;

[0027] S4: feeding the wet paper described in S3 into a conveyor for conveying, and the conveyor feeds the wet paper into a hot press for hot pressing to obtain insulating paperboard;

[0028] S5: Send the insulating cardboard described in S4 to the processing table, and paste and connect waterproof films on both sides of the insulating cardboard, paste and connect glass fiber mesh cloth on the two waterproof films, apply fireproof mud on the two glass fiber mesh cloths, install grid-shaped carbon fiber reinforcement plates on the surfaces of the two fireproof muds, and finally spray fireproof coating and UV wear-resistant coating on the surfaces of the two grid-shaped carbon fiber reinforcement plates to obtain thickened insulating cardboard.

[0029] In this embodiment, in S3, the pulping time of the pulper is 30-40 minutes, and the crushing speed in the pulper is 8000-12000 r / min.

[0030] In this embodiment, in S3, the beating time of the pulper is 40-60 minutes, and the crushing speed in the pulper is 4000-6000 r / min.

[0031] In this embodiment, in S4, the working temperature of the hot press is 130° C.-180° C., and the pressure is 0.2-0.9 MPa.

[0032] In this embodiment, in S5, the thickness of the waterproof film is 0.3-0.6 mm, and the thickness of the glass fiber mesh cloth is 1.5-2.5 mm.

[0033] Table 1 Data of production water before and after purification

[0034] project Conductivity Water resistivity Normal water 25μs / cm 16.8MΩ.cm Purify water 0.8μs / cm 11.3MΩ.cm

[0035] Embodiment 2

[0036] A thickened insulating paperboard comprises the following raw materials in parts by weight: 55 parts of unbleached kraft softwood pulp, 25 parts of water, 0.2 parts of polyethylene glycol, 2 parts of polyacrylamide, 2 parts of a copolymer of 2-ethylhexyl acrylate and styrene, 2 parts of oxidized starch, 2 parts of tetrasodium pyrophosphate, 0.2 parts of formaldehyde, 0.5 parts of p-nitrophenol, 1 part of a waterproof film, 1 part of a glass fiber mesh cloth, 1 part of fireproof mud, 1 part of a grid-shaped carbon fiber reinforcing rib plate, 1 part of a fireproof coating and 1 part of a UV wear-resistant coating.

[0037] This embodiment also provides a method for producing thickened insulating paperboard, comprising the following steps:

[0038] S1: weigh the following raw materials in order by weight: 55 parts of unbleached kraft softwood pulp, 25 parts of water, 0.2 parts of polyethylene glycol, 2 parts of polyacrylamide, 2 parts of copolymer of 2-ethylhexyl acrylate and styrene, 2 parts of oxidized starch, 2 parts of tetrasodium pyrophosphate, 0.2 parts of formaldehyde, 0.5 parts of p-nitrophenol, 1 part of waterproof film, 1 part of glass fiber mesh cloth, 1 part of fireproof mud, 1 part of grid-shaped carbon fiber reinforcement plate, 1 part of fireproof coating and 1 part of UV wear-resistant coating;

[0039] S2: Send the water described in S1 into the filter box for primary filtration, filter out large particles of impurities in the water, and then send the water after the primary filtration into the softening water equipment for softening. The softened water is then sent to the reverse osmosis and water purifier, so that water molecules and ionic mineral elements pass through the reverse osmosis membrane, while most of the inorganic salts, organic matter, bacteria, viruses, etc. dissolved in the water cannot pass through the reverse osmosis membrane, so that the permeated pure water and the non-permeated concentrated water are strictly separated to obtain purified water. The purified water can reduce the salt content, effectively remove various impurities in the water, reduce the conductive ions in the water, thereby reducing the conductivity and improving the resistivity of the outlet water;

[0040] S3: The unbleached kraft conifer pulp described in S1 is sent to a pulper for crushing to obtain crushed pulp, and the crushed pulp is sent to a pulper for beating, and polyethylene glycol, polyacrylamide, a copolymer of 2-ethylhexyl acrylate and styrene, oxidized starch, tetrasodium pyrophosphate, formaldehyde and p-nitrophenol are simultaneously put into the pulper for stirring, and the purified water described in S2 is added into the pulper for stirring together, and then the pulp after beating is sent to a paper machine for processing into a semi-finished product, and fine fibers are recovered by an air flotation machine during the processing of the paper machine, and sent to a pulper for further processing to obtain wet paper, which can increase the fine fiber content in the pulp, improve the strength of the insulating paperboard, and also improve the strength of the wet paper sheet;

[0041] S4: feeding the wet paper described in S3 into a conveyor for conveying, and the conveyor feeds the wet paper into a hot press for hot pressing to obtain insulating paperboard;

[0042] S5: Send the insulating cardboard described in S4 to the processing table, and paste and connect waterproof films on both sides of the insulating cardboard, paste and connect glass fiber mesh cloth on the two waterproof films, apply fireproof mud on the two glass fiber mesh cloths, install grid-shaped carbon fiber reinforcement plates on the surfaces of the two fireproof muds, and finally spray fireproof coating and UV wear-resistant coating on the surfaces of the two grid-shaped carbon fiber reinforcement plates to obtain thickened insulating cardboard.

[0043] In this embodiment, in S3, the pulping time of the pulper is 30-40 minutes, and the crushing speed in the pulper is 8000-12000 r / min.

[0044] In this embodiment, in S3, the beating time of the pulper is 40-60 minutes, and the crushing speed in the pulper is 4000-6000 r / min.

[0045] In this embodiment, in S4, the working temperature of the hot press is 130° C.-180° C., and the pressure is 0.2-0.9 MPa.

[0046] In this embodiment, in S5, the thickness of the waterproof film is 0.3-0.6 mm, and the thickness of the glass fiber mesh cloth is 1.5-2.5 mm.

[0047] Embodiment 3

[0048] A thickened insulating paperboard comprises the following raw materials in parts by weight: 60 parts of unbleached kraft softwood pulp, 25 parts of water, 0.2 parts of polyethylene glycol, 3 parts of polyacrylamide, 3 parts of a copolymer of 2-ethylhexyl acrylate and styrene, 3 parts of oxidized starch, 3 parts of tetrasodium pyrophosphate, 0.2 parts of formaldehyde, 0.2 parts of p-nitrophenol, 1 part of a waterproof film, 1 part of a glass fiber mesh cloth, 1 part of fireproof mud, 1 part of a grid-shaped carbon fiber reinforcing rib plate, 1 part of a fireproof coating and 1 part of a UV wear-resistant coating.

[0049] This embodiment also provides a method for producing thickened insulating paperboard, comprising the following steps:

[0050] S1: weigh the following raw materials in order by weight: 60 parts of unbleached kraft softwood pulp, 25 parts of water, 0.2 parts of polyethylene glycol, 3 parts of polyacrylamide, 3 parts of copolymer of 2-ethylhexyl acrylate and styrene, 3 parts of oxidized starch, 3 parts of tetrasodium pyrophosphate, 0.2 parts of formaldehyde, 0.2 parts of p-nitrophenol, 1 part of waterproof film, 1 part of glass fiber mesh cloth, 1 part of fireproof mud, 1 part of grid-shaped carbon fiber reinforcement plate, 1 part of fireproof coating and 1 part of UV wear-resistant coating;

[0051] S2: Send the water described in S1 into the filter box for primary filtration, filter out large particles of impurities in the water, and then send the water after the primary filtration into the softening water equipment for softening. The softened water is then sent to the reverse osmosis and water purifier, so that water molecules and ionic mineral elements pass through the reverse osmosis membrane, while most of the inorganic salts, organic matter, bacteria, viruses, etc. dissolved in the water cannot pass through the reverse osmosis membrane, so that the permeated pure water and the non-permeated concentrated water are strictly separated to obtain purified water. The purified water can reduce the salt content, effectively remove various impurities in the water, reduce the conductive ions in the water, thereby reducing the conductivity and improving the resistivity of the outlet water;

[0052] S3: The unbleached kraft conifer pulp described in S1 is sent to a pulper for crushing to obtain crushed pulp, and the crushed pulp is sent to a pulper for beating, and polyethylene glycol, polyacrylamide, a copolymer of 2-ethylhexyl acrylate and styrene, oxidized starch, tetrasodium pyrophosphate, formaldehyde and p-nitrophenol are simultaneously put into the pulper for stirring, and the purified water described in S2 is added into the pulper for stirring together, and then the pulp after beating is sent to a paper machine for processing into a semi-finished product, and fine fibers are recovered by an air flotation machine during the processing of the paper machine, and sent to a pulper for further processing to obtain wet paper, which can increase the fine fiber content in the pulp, improve the strength of the insulating paperboard, and also improve the strength of the wet paper sheet;

[0053] S4: feeding the wet paper described in S3 into a conveyor for conveying, and the conveyor feeds the wet paper into a hot press for hot pressing to obtain insulating paperboard;

[0054] S5: Send the insulating cardboard described in S4 to the processing table, and paste and connect waterproof films on both sides of the insulating cardboard, paste and connect glass fiber mesh cloth on the two waterproof films, apply fireproof mud on the two glass fiber mesh cloths, install grid-shaped carbon fiber reinforcement plates on the surfaces of the two fireproof muds, and finally spray fireproof coating and UV wear-resistant coating on the surfaces of the two grid-shaped carbon fiber reinforcement plates to obtain thickened insulating cardboard.

[0055] In this embodiment, in S3, the pulping time of the pulper is 30-40 minutes, and the crushing speed in the pulper is 8000-12000 r / min.

[0056] In this embodiment, in S3, the beating time of the pulper is 40-60 minutes, and the crushing speed in the pulper is 4000-6000 r / min.

[0057] In this embodiment, in S4, the working temperature of the hot press is 130° C.-180° C., and the pressure is 0.2-0.9 MPa.

[0058] In this embodiment, in S5, the thickness of the waterproof film is 0.3-0.6 mm, and the thickness of the glass fiber mesh cloth is 1.5-2.5 mm.

[0059] Embodiment 4

[0060] A thickened insulating paperboard comprises the following raw materials in parts by weight: 60 parts of unbleached kraft softwood pulp, 25 parts of water, 0.3 parts of polyethylene glycol, 4 parts of polyacrylamide, 3 parts of a copolymer of 2-ethylhexyl acrylate and styrene, 4 parts of oxidized starch, 3 parts of tetrasodium pyrophosphate, 0.4 parts of formaldehyde, 0.4 parts of p-nitrophenol, 1 part of a waterproof film, 1 part of a glass fiber mesh cloth, 1 part of fireproof mud, 1 part of a grid-shaped carbon fiber reinforcing rib plate, 1 part of a fireproof coating and 1 part of a UV wear-resistant coating.

[0061] This embodiment also provides a method for producing thickened insulating paperboard, comprising the following steps:

[0062] S1: weigh the following raw materials in order by weight: 60 parts of unbleached kraft softwood pulp, 25 parts of water, 0.3 parts of polyethylene glycol, 4 parts of polyacrylamide, 3 parts of copolymer of 2-ethylhexyl acrylate and styrene, 4 parts of oxidized starch, 3 parts of tetrasodium pyrophosphate, 0.4 parts of formaldehyde, 0.4 parts of p-nitrophenol, 1 part of waterproof film, 1 part of glass fiber mesh cloth, 1 part of fireproof mud, 1 part of grid-shaped carbon fiber reinforcement plate, 1 part of fireproof coating and 1 part of UV wear-resistant coating;

[0063] S2: Send the water described in S1 into the filter box for primary filtration, filter out large particles of impurities in the water, and then send the water after the primary filtration into the softening water equipment for softening. The softened water is then sent to the reverse osmosis and water purifier, so that water molecules and ionic mineral elements pass through the reverse osmosis membrane, while most of the inorganic salts, organic matter, bacteria, viruses, etc. dissolved in the water cannot pass through the reverse osmosis membrane, so that the permeated pure water and the non-permeated concentrated water are strictly separated to obtain purified water. The purified water can reduce the salt content, effectively remove various impurities in the water, reduce the conductive ions in the water, thereby reducing the conductivity and improving the resistivity of the outlet water;

[0064] S3: The unbleached kraft conifer pulp described in S1 is sent to a pulper for crushing to obtain crushed pulp, and the crushed pulp is sent to a pulper for beating, and polyethylene glycol, polyacrylamide, a copolymer of 2-ethylhexyl acrylate and styrene, oxidized starch, tetrasodium pyrophosphate, formaldehyde and p-nitrophenol are simultaneously put into the pulper for stirring, and the purified water described in S2 is added into the pulper for stirring together, and then the pulp after beating is sent to a paper machine for processing into a semi-finished product, and fine fibers are recovered by an air flotation machine during the processing of the paper machine, and sent to a pulper for further processing to obtain wet paper, which can increase the fine fiber content in the pulp, improve the strength of the insulating paperboard, and also improve the strength of the wet paper sheet;

[0065] S4: feeding the wet paper described in S3 into a conveyor for conveying, and the conveyor feeds the wet paper into a hot press for hot pressing to obtain insulating paperboard;

[0066] S5: Send the insulating cardboard described in S4 to the processing table, and paste and connect waterproof films on both sides of the insulating cardboard, paste and connect glass fiber mesh cloth on the two waterproof films, apply fireproof mud on the two glass fiber mesh cloths, install grid-shaped carbon fiber reinforcement plates on the surfaces of the two fireproof muds, and finally spray fireproof coating and UV wear-resistant coating on the surfaces of the two grid-shaped carbon fiber reinforcement plates to obtain thickened insulating cardboard.

[0067] In this embodiment, in S3, the pulping time of the pulper is 30-40 minutes, and the crushing speed in the pulper is 8000-12000 r / min.

[0068] In this embodiment, in S3, the beating time of the pulper is 40-60 minutes, and the crushing speed in the pulper is 4000-6000 r / min.

[0069] In this embodiment, in S4, the working temperature of the hot press is 130° C.-180° C., and the pressure is 0.2-0.9 MPa.

[0070] In this embodiment, in S5, the thickness of the waterproof film is 0.3-0.6 mm, and the thickness of the glass fiber mesh cloth is 1.5-2.5 mm.

[0071] Embodiment 5

[0072] A thickened insulating paperboard comprises the following raw materials in parts by weight: 60 parts of unbleached kraft softwood pulp, 30 parts of water, 0.3 parts of polyethylene glycol, 5 parts of polyacrylamide, 5 parts of a copolymer of 2-ethylhexyl acrylate and styrene, 10 parts of oxidized starch, 1 part of tetrasodium pyrophosphate, 0.1 part of formaldehyde, 0.3 parts of p-nitrophenol, 1 part of a waterproof film, 1 part of a glass fiber mesh cloth, 1 part of fireproof mud, 1 part of a grid-shaped carbon fiber reinforcing rib plate, 1 part of a fireproof coating and 1 part of a UV wear-resistant coating.

[0073] This embodiment also provides a method for producing thickened insulating paperboard, comprising the following steps:

[0074] S1: weigh the following raw materials in order by weight: 60 parts of unbleached kraft softwood pulp, 30 parts of water, 0.3 parts of polyethylene glycol, 5 parts of polyacrylamide, 5 parts of copolymer of 2-ethylhexyl acrylate and styrene, 10 parts of oxidized starch, 1 part of tetrasodium pyrophosphate, 0.1 parts of formaldehyde, 0.3 parts of p-nitrophenol, 1 part of waterproof film, 1 part of glass fiber mesh cloth, 1 part of fireproof mud, 1 part of grid-shaped carbon fiber reinforcement plate, 1 part of fireproof coating and 1 part of UV wear-resistant coating;

[0075] S2: Send the water described in S1 into the filter box for primary filtration, filter out large particles of impurities in the water, and then send the water after the primary filtration into the softening water equipment for softening. The softened water is then sent to the reverse osmosis and water purifier, so that water molecules and ionic mineral elements pass through the reverse osmosis membrane, while most of the inorganic salts, organic matter, bacteria, viruses, etc. dissolved in the water cannot pass through the reverse osmosis membrane, so that the permeated pure water and the non-permeated concentrated water are strictly separated to obtain purified water. The purified water can reduce the salt content, effectively remove various impurities in the water, reduce the conductive ions in the water, thereby reducing the conductivity and improving the resistivity of the outlet water;

[0076] S3: The unbleached kraft conifer pulp described in S1 is sent to a pulper for crushing to obtain crushed pulp, and the crushed pulp is sent to a pulper for beating, and polyethylene glycol, polyacrylamide, a copolymer of 2-ethylhexyl acrylate and styrene, oxidized starch, tetrasodium pyrophosphate, formaldehyde and p-nitrophenol are simultaneously put into the pulper for stirring, and the purified water described in S2 is added into the pulper for stirring together, and then the pulp after beating is sent to a paper machine for processing into a semi-finished product, and fine fibers are recovered by an air flotation machine during the processing of the paper machine, and sent to a pulper for further processing to obtain wet paper, which can increase the fine fiber content in the pulp, improve the strength of the insulating paperboard, and also improve the strength of the wet paper sheet;

[0077] S4: feeding the wet paper described in S3 into a conveyor for conveying, and the conveyor feeds the wet paper into a hot press for hot pressing to obtain insulating paperboard;

[0078] S5: Send the insulating cardboard described in S4 to the processing table, and paste and connect waterproof films on both sides of the insulating cardboard, paste and connect glass fiber mesh cloth on the two waterproof films, apply fireproof mud on the two glass fiber mesh cloths, install grid-shaped carbon fiber reinforcement plates on the surfaces of the two fireproof muds, and finally spray fireproof coating and UV wear-resistant coating on the surfaces of the two grid-shaped carbon fiber reinforcement plates to obtain thickened insulating cardboard.

[0079] In this embodiment, in S3, the pulping time of the pulper is 30-40 minutes, and the crushing speed in the pulper is 8000-12000 r / min.

[0080] In this embodiment, in S3, the beating time of the pulper is 40-60 minutes, and the crushing speed in the pulper is 4000-6000 r / min.

[0081] In this embodiment, in S4, the working temperature of the hot press is 130° C.-180° C., and the pressure is 0.2-0.9 MPa.

[0082] In this embodiment, in S5, the thickness of the waterproof film is 0.3-0.6 mm, and the thickness of the glass fiber mesh cloth is 1.5-2.5 mm.

[0083] The tensile strength, electrical conductivity and electrical strength of the existing product and the product of this embodiment are tested by means of testing equipment, and the test results are recorded;

[0084] Tensile Strength Conductivity Electrical strength Current Products 105 4% 46 Products in this program 146 1.5% 49

[0085] The results show that the thickened insulating paperboard prepared by the present invention has good tensile strength, electrical conductivity and electrical strength.

[0086] The technical progress achieved by the present invention compared with the prior art is that the interlayer bonding force of the thickened insulating paperboard of the present invention is stronger, the tensile strength is higher, the conductivity is lower, the waterproof and fireproof performance during use is better, cracking can be avoided during long-term use, and the service life is longer.

Claims

1. A thickened insulating paperboard, characterized in that: The invention comprises the following raw materials in parts by weight: 50-70 parts of unbleached kraft softwood pulp, 20-30 parts of water, 0.1-0.6 parts of polyethylene glycol, 1-5 parts of polyacrylamide, 1-6 parts of a copolymer of 2-ethylhexyl acrylate and styrene, 1-10 parts of oxidized starch, 1-3 parts of tetrasodium pyrophosphate, 0.1-0.5 parts of formaldehyde, 0.3-0.6 parts of p-nitrophenol, 1-5 parts of a waterproof film, 1-5 parts of a glass fiber mesh cloth, 1-5 parts of a fireproof mud, 1-5 parts of a grid-shaped carbon fiber reinforcing rib plate, 1-5 parts of a fireproof coating and 1-5 parts of a UV wear-resistant coating; The preparation of the thickened insulating paperboard comprises the following steps: S1: weigh the following raw materials in parts by weight: 50-70 parts of unbleached kraft softwood pulp, 20-30 parts of water, 0.1-0.6 parts of polyethylene glycol, 1-5 parts of polyacrylamide, 1-6 parts of copolymer of 2-ethylhexyl acrylate and styrene, 1-10 parts of oxidized starch, 1-3 parts of tetrasodium pyrophosphate, 0.1-0.5 parts of formaldehyde, 0.3-0.6 parts of p-nitrophenol, 1-5 parts of waterproof film, 1-5 parts of glass fiber mesh cloth, 1-5 parts of fireproof mud, 1-5 parts of grid-shaped carbon fiber reinforcement plate, 1-5 parts of fireproof coating and 1-5 parts of UV wear-resistant coating; S2: Send the water described in S1 into the filter box for primary filtration, filter out large particles of impurities in the water, and then send the water after the primary filtration into the softening water equipment for softening. The softened water is then sent to the reverse osmosis and water purifier, so that water molecules and ionic mineral elements pass through the reverse osmosis membrane, while most of the inorganic salts, organic matter, bacteria, viruses, etc. dissolved in the water cannot pass through the reverse osmosis membrane, so that the permeated pure water and the non-permeated concentrated water are strictly separated to obtain purified water. The purified water can reduce the salt content, effectively remove various impurities in the water, reduce the conductive ions in the water, thereby reducing the conductivity and improving the resistivity of the outlet water; S3: The unbleached kraft conifer pulp described in S1 is sent to a pulper for crushing to obtain crushed pulp, and the crushed pulp is sent to a pulper for beating, and polyethylene glycol, polyacrylamide, a copolymer of 2-ethylhexyl acrylate and styrene, oxidized starch, tetrasodium pyrophosphate, formaldehyde and p-nitrophenol are simultaneously put into the pulper for stirring, and the purified water described in S2 is added into the pulper for stirring together, and then the pulp after beating is sent to a paper machine for processing into a semi-finished product, and fine fibers are recovered by an air flotation machine during the processing of the paper machine, and sent to a pulper for further processing to obtain wet paper, which can increase the fine fiber content in the pulp, improve the strength of the insulating paperboard, and also improve the strength of the wet paper sheet; S4: feeding the wet paper described in S3 into a conveyor for conveying, and the conveyor feeds the wet paper into a hot press for hot pressing to obtain insulating paperboard; S5: Send the insulating cardboard described in S4 to the processing table, and paste and connect waterproof films on both sides of the insulating cardboard, paste and connect glass fiber mesh cloth on the two waterproof films, apply fireproof mud on the two glass fiber mesh cloths, install grid-shaped carbon fiber reinforcement plates on the surfaces of the two fireproof muds, and finally spray fireproof coating and UV wear-resistant coating on the surfaces of the two grid-shaped carbon fiber reinforcement plates to obtain thickened insulating cardboard.

2. The thickened insulating paperboard according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 50 parts of unbleached kraft softwood pulp, 20 parts of water, 0.1 parts of polyethylene glycol, 1 part of polyacrylamide, 1 part of copolymer of 2-ethylhexyl acrylate and styrene, 1 part of oxidized starch, 1 part of tetrasodium pyrophosphate, 0.1 parts of formaldehyde, 0.3 parts of p-nitrophenol, 1 part of waterproof film, 1 part of glass fiber mesh cloth, 1 part of fireproof mud, 1 part of grid-shaped carbon fiber reinforcement plate, 1 part of fireproof coating and 1 part of UV wear-resistant coating.

3. A method for producing thickened insulating paperboard, characterized in that: The following steps are involved: S1: weigh the following raw materials in parts by weight: 50-70 parts of unbleached kraft softwood pulp, 20-30 parts of water, 0.1-0.6 parts of polyethylene glycol, 1-5 parts of polyacrylamide, 1-6 parts of copolymer of 2-ethylhexyl acrylate and styrene, 1-10 parts of oxidized starch, 1-3 parts of tetrasodium pyrophosphate, 0.1-0.5 parts of formaldehyde, 0.3-0.6 parts of p-nitrophenol, 1-5 parts of waterproof film, 1-5 parts of glass fiber mesh cloth, 1-5 parts of fireproof mud, 1-5 parts of grid-shaped carbon fiber reinforcement plate, 1-5 parts of fireproof coating and 1-5 parts of UV wear-resistant coating; S2: Send the water described in S1 into the filter box for primary filtration, filter out large particles of impurities in the water, and then send the water after the primary filtration into the softening water equipment for softening. The softened water is then sent to the reverse osmosis and water purifier, so that water molecules and ionic mineral elements pass through the reverse osmosis membrane, while most of the inorganic salts, organic matter, bacteria, viruses, etc. dissolved in the water cannot pass through the reverse osmosis membrane, so that the permeated pure water and the non-permeated concentrated water are strictly separated to obtain purified water. The purified water can reduce the salt content, effectively remove various impurities in the water, reduce the conductive ions in the water, thereby reducing the conductivity and improving the resistivity of the outlet water; S3: The unbleached kraft conifer pulp described in S1 is sent to a pulper for crushing to obtain crushed pulp, and the crushed pulp is sent to a pulper for beating, and polyethylene glycol, polyacrylamide, a copolymer of 2-ethylhexyl acrylate and styrene, oxidized starch, tetrasodium pyrophosphate, formaldehyde and p-nitrophenol are simultaneously put into the pulper for stirring, and the purified water described in S2 is added into the pulper for stirring together, and then the pulp after beating is sent to a paper machine for processing into a semi-finished product, and fine fibers are recovered by an air flotation machine during the processing of the paper machine, and sent to a pulper for further processing to obtain wet paper, which can increase the fine fiber content in the pulp, improve the strength of the insulating paperboard, and also improve the strength of the wet paper sheet; S4: feeding the wet paper described in S3 into a conveyor for conveying, and the conveyor feeds the wet paper into a hot press for hot pressing to obtain insulating paperboard; S5: Send the insulating cardboard described in S4 to the processing table, and paste and connect waterproof films on both sides of the insulating cardboard, paste and connect glass fiber mesh cloth on the two waterproof films, apply fireproof mud on the two glass fiber mesh cloths, install grid-shaped carbon fiber reinforcement plates on the surfaces of the two fireproof muds, and finally spray fireproof coating and UV wear-resistant coating on the surfaces of the two grid-shaped carbon fiber reinforcement plates to obtain thickened insulating cardboard.

4. The method for producing thickened insulating paperboard according to claim 3, characterized in that: In S3, the pulping time of the pulper is 30-40 minutes, and the crushing speed in the pulper is 8000-12000 r / min.

5. The method for producing thickened insulating paperboard according to claim 3, characterized in that: In S3, the beating time of the pulper is 40-60 minutes, and the crushing speed in the pulper is 4000-6000 r / min.

6. The method for producing thickened insulating paperboard according to claim 3, characterized in that: In S4, the operating temperature of the hot press is 130° C.-180° C., and the pressure is 0.2-0.9 MPa.

7. The method for producing thickened insulating paperboard according to claim 3, characterized in that: In S5, the thickness of the waterproof film is 0.3-0.6 mm, and the thickness of the glass fiber mesh cloth is 1.5-2.5 mm.

8. The method for producing thickened insulating paperboard according to claim 3, characterized in that: The thickness of the grid-shaped carbon fiber reinforcement plate is 3.5-4.5 mm, and the thickness of the UV wear-resistant coating is 0.4-0.8 mm.

Citation Information