A method of photocatalytic degradation of a collector in a potassium salt flotation process

The photocatalytic oxidation method using titanium dioxide composite materials to degrade the potassium salt flotation collector octadecylamine/dodecylmorpholine solves the problems of incomplete degradation and high cost in existing technologies, achieving efficient, green, and economical degradation and improving degradation efficiency.

CN116969544BActive Publication Date: 2025-11-28QINGHAI INST OF SALT LAKES OF CHINESE ACAD OF SCI
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210434406.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-24
Publication Date
2025-11-28
Estimated Expiration
2042-04-24

AI Technical Summary

Technical Problem

Existing technologies for treating the collector octadecylamine/dodecylmorpholine in potassium salt flotation processes suffer from incomplete degradation, high costs, and difficulty in industrialization, and the residues are harmful to the environment and health.

Method used

A photocatalytic oxidation method is adopted, which utilizes titanium dioxide to form a heterojunction material with a small band gap. The potassium salt flotation collector octadecylamine/dodecylmorpholine is degraded by photocatalysis, and the degradation is carried out by a photocatalytic material with a wide spectrum response.

Benefits of technology

It achieves efficient, green, and economical degradation, with a degradation rate of over 90%. The material is stable and can be used in high-salt brine systems. It can make full use of visible light to improve degradation efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116969544B_ABST
    Figure CN116969544B_ABST
Patent Text Reader

Abstract

The application discloses a method for degrading potassium salt flotation collector octadecylamine / dodecyl morpholine by a photocatalytic oxidation method, and utilizes a material with a small compound band gap of anatase titanium dioxide to obtain a heterojunction material with a wide spectral response, so that green photocatalytic degradation treatment of octadecylamine and / or dodecyl morpholine is realized. The photocatalytic oxidation technology has the advantages of mild reaction conditions, fast reaction rate, environmental friendliness and the like, and can degrade organic matters into harmless CO2 and H2O to a certain extent. The method has the advantages of simple equipment, low cost, recyclable materials and easy industrialization.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The application belongs to the technical field of inorganic chemistry, and particularly relates to a method for photocatalytic degradation of a collector in a potassium salt flotation process. BACKGROUND

[0002] The demand for potassium salt in agricultural production is huge, and at present, most potassium salts are obtained by the flotation method. Octadecylamine and dodecylmorpholine are commonly used collectors in the potassium salt flotation process, and the residual collector will affect the grade of potassium salt in actual production. After the flotation section is completed, part of the octadecylamine / dodecylmorpholine enters the salt field with the flotation tail liquid or is collected by the subsequent process, which not only affects the quality of the subsequent product, but also poses a potential threat to the fragile ecological environment of the salt lake area. In addition, octadecylamine / dodecylmorpholine has a certain irritancy to the skin and mucous membrane, and long-term contact will affect human health. Therefore, it is necessary to establish an efficient, green and economic method for treating the potassium salt flotation collector octadecylamine / dodecylmorpholine.

[0003] At present, the technologies for treating octadecylamine / dodecylmorpholine in the production process of potassium fertilizer mainly include adsorption and advanced oxidation. Wang Pingping used attapulgite and Fe3O4 composite halloysite to adsorb octadecylamine in the solution; Xia Yang used UV / H2O2 / air oxidation method to degrade and treat octadecylamine, and obtained a high degradation rate, but a strong oxidizing agent H2O2 needs to be added to the system. Wang Jian et al. used dielectric barrier discharge plasma technology to degrade the dodecylmorpholine simulated wastewater, and obtained a certain degradation effect, but the equipment of this method is relatively complex. SUMMARY

[0004] The purpose of the present application is to solve the problems of incomplete degradation, high cost, input of oxidizing chemicals and difficulty in industrialization in the current methods for treating the collector in the potassium salt flotation process. Based on the advantages of photocatalytic oxidation technology, such as mild reaction conditions, fast reaction rate, environmental friendliness and simple equipment, a method for degrading the potassium salt flotation collector octadecylamine / dodecylmorpholine by using photocatalytic oxidation is proposed. A heterojunction material with wide spectral response is obtained by using titanium dioxide composite with a small band gap, so as to realize green photocatalytic degradation and treatment of octadecylamine / dodecylmorpholine.

[0005] The present application is realized by the following technical solutions:

[0006] A method for photocatalytic degradation of a collector in a potassium salt flotation process, comprising:

[0007] adding a photocatalytic degradation material to an aqueous solution containing a potassium salt collector, dispersing to obtain a to-be-degraded system, and placing the to-be-degraded system under light irradiation for degradation;

[0008] The photocatalytic degradation material is added in an amount of 0.1-10 g / L.

[0009] The wavelength range of the light is λ≥200 nm.

[0010] The content of the potassium salt collector in the aqueous solution is 1-200 mg / L.

[0011] The pH of the system to be degraded is 0-13, preferably 5.5-7.5.

[0012] The degradation time t is ≥30 min.

[0013] The photocatalytic degradation material is titanium dioxide.

[0014] In the technical solution, the collector is octadecylamine and / or dodecylmorpholine.

[0015] In the technical solution, the photocatalytic degradation material is anatase titanium dioxide.

[0016] In the technical solution, the photocatalytic degradation material comprises a base and a doping substance, wherein the base is titanium dioxide.

[0017] The mass of the doping substance accounts for 0.5%-50% of the total mass of the photocatalytic degradation material.

[0018] The doping substance is one or more of black titanium dioxide, α-iron oxide and γ-iron oxide (the band gap of the above materials is relatively low, and the purpose of doping is to reduce the band gap of the anatase titanium dioxide material, so that the composite material responds to a wider wavelength range of light, and the response spectrum range is extended to the visible light range).

[0019] In the technical solution, the preparation method of the photocatalytic degradation material comprises:

[0020] Hydrofluoric acid is added to an acetic acid solution to obtain a first solution, alkyl titanate and a doping substance are added to the first solution, and a first mixture is obtained after stirring uniformly, the first mixture is transferred to a reaction kettle, and is reacted at 150-300 ℃ for 12-30 h, after the reaction is completed, the precipitate is collected and washed and dried to obtain the photocatalytic degradation material;

[0021] The molar fraction of acetic acid in the first solution is 70-90%.

[0022] The molar fraction of hydrofluoric acid in the first solution is 1.0-8.0%.

[0023] The doping substance is one or more of black titanium dioxide, α-iron oxide and γ-iron oxide.

[0024] The adding amount of the alkyl titanate is 0.5% to 4.5% of the molar fraction of the added acetic acid (the adding amount is determined to ensure that the alkyl titanate can be hydrolyzed as much as possible);

[0025] The adding amount of the doping substance is 0.075wt% to 7.5wt% of the mass of the alkyl titanate (in the case that the alkyl titanate is used as a titanium source and the hydrolysis degree is controlled in the range of 60% to 70%, to ensure that the mass of the doping substance in the finally obtained photocatalytic degradation material accounts for 0.5% to 50% of the mass of the substrate titanium dioxide);

[0026] In the technical solution, the alkyl titanate is at least one of tetrabutyl titanate, tetraethyl titanate and tetraisopropyl titanate.

[0027] In the technical solution, when the doping substance is alpha-iron oxide and / or gamma-iron oxide, the tetralkyl titanate and the doping substance are added to the first solution, and the pH of the first solution is ensured to be 3.0 to 4.0, and the adding amount of the doping substance is 0.075wt% to 7.5wt% of the mass of the alkyl titanate.

[0028] In the technical solution, the dried precipitate is calcined at 400°C to 600°C for 2 to 10 hours to obtain the wide-spectrum and low-cost photocatalytic degradation material.

[0029] The advantages and beneficial effects of the present application are as follows:

[0030] The present application uses titanium dioxide to composite black titanium dioxide, alpha-iron oxide, gamma-iron oxide and other materials as a photocatalyst to degrade potassium salt flotation collector octadecylamine and / or dodecylmorpholine. Titanium dioxide has stable performance and high photocatalytic activity, and by compositing black titanium dioxide, alpha-iron oxide and gamma-iron oxide, the band gap of the composite material can be reduced, a heterojunction system with wide-spectrum response is obtained, the material can respond to a wider range of light, and the degradation efficiency of the photocatalytic material on octadecylamine and / or dodecylmorpholine is improved.

[0031] The main advantages are as follows:

[0032] 1. The process of the present application is simple, has good degradation effect, and has strong practical applicability;

[0033] 2. The prepared photocatalyst has stable performance, and the material is resistant to acid and alkali, and can be used in high-salt brine systems;

[0034] 3. By doping, the material can respond to visible light, can fully utilize sunlight, and can improve the degradation efficiency of the method on potassium salt flotation reagent octadecylamine and / or dodecylmorpholine. BRIEF DESCRIPTION OF DRAWINGS

[0035] Figure 1is the degradation efficiency graph of octadecylamine / dodecylmorpholine degraded by the anatase titanium dioxide doped with 5% black titanium dioxide synthesized in Example 1 of the present application.

[0036] Figure 2 is the degradation efficiency graph of octadecylamine / dodecylmorpholine degraded by the anatase titanium dioxide doped with 5% black titanium dioxide synthesized in Example 1 of the present application.

[0037] Figure 3 is the degradation efficiency graph of octadecylamine / dodecylmorpholine degraded by the anatase titanium dioxide doped with 5% black titanium dioxide + 5% α-iron oxide synthesized in Example 2 of the present application.

[0038] Figure 4 is the degradation of octadecylamine at different initial concentrations in Example 3 of the present application.

[0039] Figure 5 is the degradation of octadecylamine at different amounts of photocatalyst in Example 4 of the present application.

[0040] Figure 6 is the degradation of octadecylamine at different temperatures in Example 5 of the present application.

[0041] Figure 7 is the degradation of octadecylamine at different pH in Example 6 of the present application.

[0042] Figure 8 is the influence of other salt substances in the system on the photocatalytic degradation efficiency of dodecylmorpholine in Example 7 of the present application.

[0043] For those skilled in the art, other related drawings can be obtained according to the above drawings without creative labor. DETAILED DESCRIPTION

[0044] In order to enable those skilled in the art to better understand the present application, the technical solutions of the present application will be further described below in combination with specific examples.

[0045] Comparative Example

[0046] The preparation method of anatase titanium dioxide in the present comparative example is as follows:

[0047] Step 1, 1.95 mL of deionized water and 55.8 mL of glacial acetic acid were added into a polytetrafluoroethylene liner, 0.7 mL of a 40 wt% concentrated hydrofluoric acid solution was added, and then 20 mL of tetrabutyl titanate was added dropwise into the solution, and the stirring was continued for 30 min;

[0048] Step 2, the liner was placed in a reaction kettle and put into a 180℃ oven for reaction for 24 h. After the reaction kettle was naturally cooled to room temperature, the collected precipitate was washed with anhydrous ethanol and deionized water for 3 times respectively;

[0049] Step 3, the precipitate was dried in an oven at 60 °C for 6 h, and then the sample was calcined in a muffle furnace at 400 °C for 2 h to remove organic volatile impurities, to obtain the undoped anatase titanium dioxide photocatalytic material.

[0050] 1.1 Photocatalytic degradation of octadecylamine in the flotation slurry section of the potassium salt direct flotation process

[0051] The photocatalytic method was used to degrade octadecylamine in the flotation slurry section of the potassium salt direct flotation process, wherein the initial concentration of octadecylamine was 30 mg / L, the volume was 100 mL, and 0.1 g of anatase titanium dioxide was added. The concentration of NaCl was 0.9 mol / L, the concentration of KCl was 1.2 mol / L, the concentration of MgCl2 was 0.35 mol / L, and the initial pH of the slurry was 6.5. The tail salt slurry was placed in a photo reactor, the photo reaction device was connected with a circulating water bath pump, and circulating water was passed to make the system temperature 40 °C. The pH of the slurry was adjusted to 2 with hydrochloric acid, and the light outlet of the light source was 15 cm away from the liquid surface. The degradation time was 4 h, and samples were taken at 0, 10, 20, 30, 60, 120, 180, and 240 min. The concentration of octadecylamine was tested by a spectrophotometer, and the degradation rate of octadecylamine could reach 62% after 4 h of photo degradation. The test results are shown in Table 1. Figure 1

[0052] 1.2 Photocatalytic degradation of dodecylmorpholine in the flotation slurry section of the potassium salt reverse flotation process

[0053] The photocatalytic method was used to degrade dodecylmorpholine in the flotation slurry section of the potassium salt reverse flotation process, wherein the initial concentration of dodecylmorpholine was 30 mg / L, the volume was 100 mL, and 0.1 g of anatase titanium dioxide was added. The concentration of NaCl was 0.6 mol / L, the concentration of KCl was 1.4 mol / L, the concentration of MgCl2 was 0.4 mol / L, and the initial pH of the slurry was 6.5. The tail salt slurry was placed in a photo reactor, the photo reaction device was connected with a circulating water bath pump, and circulating water was passed to make the system temperature 40 °C. The initial pH of the slurry was adjusted to 2 with hydrochloric acid, and the light outlet of the light source was 15 cm away from the liquid surface. The degradation time was 4 h, and samples were taken at 0, 10, 20, 30, 60, 120, 180, and 240 min. The concentration of dodecylmorpholine was tested by a spectrophotometer, and the degradation rate of dodecylmorpholine could reach 75% after 4 h of photo degradation. The test results are shown in Table 2. Figure 1

[0054] Example 1

[0055] In this example, anatase titanium dioxide doped with 5% black titanium dioxide was prepared by the following method:

[0056] ​​Step 1, 1.95 mL of deionized water and 55.8 mL of glacial acetic acid were added into the inner container of polytetrafluoroethylene, 0.7 mL of 40 wt% hydrofluoric acid solution was added, 0.15 g of black TiO2 was added, and then 20.0 mL of tetrabutyl titanate was added dropwise into the solution, and stirred for 30 min. Under this condition, the hydrolysis rate of tetrabutyl titanate is about 64%, and 0.15 g of black titanium dioxide is added to obtain a 5% black titanium dioxide doped anatase titanium dioxide composite.

[0057] Step 2, the inner container was placed in a reaction kettle and put into a 180°C oven for 24 h. After the reaction kettle was naturally cooled to room temperature, the collected precipitate was washed with anhydrous ethanol and deionized water for 3 times respectively;

[0058] Step 3, the precipitate was dried in a 60°C oven for 6 h, and then the sample was calcined at 400°C in a muffle furnace for 2 h to remove organic volatile impurities. A 5% black titanium dioxide doped anatase titanium dioxide photocatalytic material was obtained.

[0059] 2.1 Photocatalytic degradation of octadecylamine in the flotation slurry section of the potassium salt direct flotation process

[0060] The photocatalytic method was used to degrade octadecylamine in the flotation slurry section of the potassium salt direct flotation process, wherein the initial concentration of octadecylamine was 30 mg / L, the volume was 100 mL, 0.1 g of 5% black titanium dioxide doped anatase titanium dioxide was added. The concentration of NaCl was 0.9 mol / L, the concentration of KCl was 1.2 mol / L, the concentration of MgCl2 was 0.35 mol / L, and the initial pH of the slurry was 6.5. The flotation slurry in the direct flotation process was placed in a light reaction device, which was connected with a circulating water pump, and the system temperature was 40°C by circulating water, the slurry pH was adjusted to 2 by hydrochloric acid, and the light outlet was 15 cm away from the liquid surface. The flotation tailings in the reaction process were stirred by a magnetic stirrer at a stirring rate of 400 r / min. The degradation time was 4 h, and samples were taken at 0, 10, 20, 30, 60, 120, 180 and 240 min, and the concentration of octadecylamine was tested by ultraviolet spectrophotometry. After 4 h of light degradation, the degradation rate of octadecylamine can reach 71%. The test results are shown in Figure 2

[0061] 2.2 Photocatalytic degradation of dodecylmorpholine in the flotation slurry section of the potassium salt reverse flotation process

[0062] ​The photocatalytic method is used for degrading the dodecyl morpholine in the flotation slurry section of the potassium salt reverse flotation process, wherein the initial concentration of the dodecyl morpholine is 30 mg / L, the volume is 100 mL, 0.1 g of anatase titanium dioxide doped with 5% black titanium dioxide is added, the concentration of NaCl is 0.6 mol / L, the concentration of KCl is 1.4 mol / L, the concentration of MgCl2 is 0.4 mol / L, and the initial pH of the slurry is 6.5. The flotation slurry in the reverse flotation process is placed in a light reaction device, the light reaction device is connected with a circulating water bath pump, circulating water is passed to make the system temperature be 40 ℃. The pH of the slurry is adjusted to 2 by using hydrochloric acid, and the light outlet of the light source is 15 cm away from the liquid surface. The flotation tailings in the reaction process are stirred by using a magnetic stirrer, and the stirring rate is 400 r / min. The degradation time is 4 h, samples are taken at 0, 10, 20, 30, 60, 120, 180 and 240 min, the concentration of the dodecyl morpholine is tested by using a spectrophotometric method, and after 4 h of light degradation, the degradation rate of the dodecyl morpholine can reach 83%. The test results are shown in Table 1. Figure 2 The improvement of the degradation efficiency is due to the fact that after the substance with a small forbidden band width is doped, the band gap of the composite anatase titanium dioxide material is reduced, so that the material can be better excited by light, more oxidizing substances such as hydroxyl radicals are generated, and the degradation efficiency of the flotation reagent is accelerated.

[0063] Example 2

[0064] The anatase titanium dioxide doped with 5% black titanium dioxide and 5% α-iron oxide is prepared by the following method.

[0065] Step 1, 1.95 mL of deionized water and 55.8 mL of glacial acetic acid are added to the polytetrafluoroethylene liner, 0.7 mL of a 40 wt% hydrofluoric acid solution is added, 0.15 g of black titanium dioxide and 0.15 g of α-iron oxide are added, and then 20.0 mL of tetrabutyl titanate is added dropwise to the solution, and stirred for 30 min; under this condition, the hydrolysis rate of tetrabutyl titanate is about 64%, and 0.15 g of black titanium dioxide and 0.15 g of α-iron oxide are added to obtain the anatase titanium dioxide composite material doped with 5% black titanium dioxide and 5% α-iron oxide.

[0066] Step 2, the liner is placed in a reaction kettle and put into a 180 ℃ oven for 24 h. After the reaction kettle is naturally cooled to room temperature, the collected precipitate is washed with anhydrous ethanol and deionized water for 3 times respectively;

[0067] Step 3, the precipitate is dried in a 60 ℃ oven for 6 h, and then the sample is calcined at 400 ℃ in a muffle furnace for 2 h to remove organic volatile impurities. The anatase titanium dioxide photocatalytic material doped with 5% black titanium dioxide and 5% α-iron oxide is obtained.

[0068] 3.1 Photocatalytic degradation of octadecylamine in the flotation slurry section of the direct flotation process of potash fertilizer

[0069] The photocatalytic method is used to degrade octadecylamine in the flotation slurry section of the direct flotation process of potash fertilizer, wherein the initial concentration of octadecylamine is 30 mg / L, the volume is 100 mL, and 0.1 g of anatase titanium dioxide doped with 5% black titanium dioxide + 5% alpha-iron oxide is added. The concentration of NaCl is 0.9 mol / L, the concentration of KCl is 1.2 mol / L, the concentration of MgCl2 is 0.35 mol / L, and the initial pH of the slurry is 6.5. The flotation slurry in the direct flotation process is placed in a light reaction device, which is connected to a circulating water pump. Circulating water is used to make the system temperature 40°C, and hydrochloric acid is used to adjust the pH of the slurry to 2. The light source outlet is 15 cm away from the liquid surface. The flotation tailings in the reaction process are stirred by a magnetic stirrer at a stirring rate of 400 r / min. The degradation time is 4 h, and samples are taken at 0, 10, 20, 30, 60, 120, 180, and 240 min. The concentration of octadecylamine is tested by ultraviolet spectrophotometry. After 4 h of photocatalytic degradation, the degradation rate of octadecylamine can reach 85%. The test results are shown in Figure 3 .

[0070] 3.2 Photocatalytic degradation of dodecylmorpholine in the flotation slurry section of the reverse flotation process of potash fertilizer

[0071] The photocatalytic method is used to degrade dodecylmorpholine in the flotation slurry section of the reverse flotation process of potash fertilizer, wherein the initial concentration of dodecylmorpholine is 30 mg / L, the volume is 100 mL, and 0.1 g of anatase titanium dioxide doped with 5% black titanium dioxide + 5% alpha-iron oxide is added. The concentration of NaCl is 0.6 mol / L, the concentration of KCl is 1.4 mol / L, the concentration of MgCl2 is 0.4 mol / L, and the initial pH of the slurry is 6.5. The flotation slurry in the direct flotation process is placed in a light reaction device, which is connected to a circulating water bath pump. Circulating water is used to make the system temperature 40°C, and the preparation method of anatase titanium dioxide doped with 5% black titanium dioxide + 5% alpha-iron oxide is the same as that in 3.1. Hydrochloric acid is used to adjust the pH of the slurry to 2, and the light source outlet is 15 cm away from the liquid surface. The flotation tailings in the reaction process are stirred by a magnetic stirrer at a stirring rate of 400 r / min. The degradation time is 4 h, and samples are taken at 0, 10, 20, 30, 60, 120, 180, and 240 min. The concentration of dodecylmorpholine is tested by spectrophotometry. After 4 h of photocatalytic degradation, the degradation rate of dodecylmorpholine can reach 90%. The test results are shown in Figure 3 . The improvement of degradation efficiency is due to the fact that the addition of substances with small band gap narrows the band gap of the composite anatase titanium dioxide material, making it more easily excited by light and generating more oxidative substances such as hydroxyl radicals, which accelerates the degradation efficiency of the flotation reagent.

[0072] Example 3 (Effect of initial concentration of octadecylamine on degradation)

[0073] The octadecylamine in the flotation slurry section of the potassium fertilizer direct flotation process was degraded by photocatalysis, wherein the initial concentration of octadecylamine was 20, 40, 60, 80, 100 mg / L, the volume was 100 mL, the concentration of NaCl in the slurry was 0.9 mol / L, the concentration of KCl was 1.2 mol / L, the concentration of MgCl2 was 0.35 mol / L, and the initial pH of the slurry was 6.5. The effect of the initial concentration of octadecylamine on the degradation efficiency was investigated. 0.4 g of anatase titanium dioxide doped with 5% black titanium dioxide synthesized by the method in Example 1 was added, and the flotation slurry in the direct flotation process was placed in a light reaction device connected with a circulating water pump. Circulating water was passed to make the system temperature 20°C, hydrochloric acid was added to adjust the initial pH of the slurry to 3.0, and the light source outlet was 15 cm away from the liquid surface. The flotation tailings in the reaction process were stirred by a magnetic stirrer at a stirring rate of 400 r / min. The degradation time was 4 h, and samples were taken at 0, 10, 20, 30, 60, 120, 180, and 240 min. The concentration of octadecylamine was tested by ultraviolet spectrophotometry. Under the optimal initial concentration conditions, the degradation rate of octadecylamine after 4 h of photocatalytic degradation can reach 90%. The test results are shown in Table 1. Figure 4

[0074] Example 4 (Effect of catalyst dosage on degradation of octadecylamine)

[0075] The octadecylamine in the flotation slurry section of the potassium salt direct flotation process was degraded by photocatalysis, wherein the initial concentration of octadecylamine was 50 mg / L, the volume was 100 mL, the concentration of NaCl in the slurry was 0.9 mol / L, the concentration of KCl was 1.2 mol / L, the concentration of MgCl2 was 0.35 mol / L, and the initial pH of the slurry was 6.5. The effect of catalyst dosage on the degradation efficiency was investigated. The mass of anatase titanium dioxide synthesized by the method in Comparative Example 1 (catalyst without doping) was 0.05, 0.10, 0.15, 0.20, 0.30, 0.40, and 0.50 g, respectively. The flotation slurry in the direct flotation process was placed in a light reaction device connected with a circulating water pump. Circulating water was passed to make the system temperature 20°C, hydrochloric acid was added to adjust the initial pH of the slurry to 3.0, and the light source outlet was 15 cm away from the liquid surface. The stirring was performed by a magnetic stirrer at a stirring rate of 400 r / min. The degradation time was 4 h, and samples were taken at 0, 10, 20, 30, 60, 120, 180, and 240 min. The concentration of octadecylamine was tested by ultraviolet spectrophotometry. The degradation efficiency of octadecylamine with an initial concentration of 50 mg / L was the highest when the catalyst dosage was 0.40 g. The test results are shown in Table 2. Figure 5 ​The results show that the degradation efficiency of octadecylamine increases with the extension of degradation time. When the catalyst dosage increases from 0.05 g to 0.40 g, the degradation efficiency of octadecylamine continues to increase after 4 h of photodegradation. When the catalyst dosage is 0.40 g, the degradation rate reaches a maximum of 95%. When the catalyst dosage continues to increase to 0.50 g, the degradation rate is 85%. This phenomenon that the degradation efficiency of octadecylamine increases first and then decreases with the increase of catalyst dosage is due to the light shielding effect of excessive titanium dioxide, which hinders the degradation of octadecylamine.

[0076] Example 5 (Effect of temperature on degradation of octadecylamine)

[0077] The octadecylamine in the flotation slurry section of the potassium salt direct flotation process was degraded by photocatalytic method, wherein the initial concentration of octadecylamine was 50 mg / L, the volume was 100 mL, the concentration of NaCl in the slurry was 0.9 mol / L, the concentration of KCl was 1.2 mol / L, the concentration of MgCl2 was 0.35 mol / L, and the initial pH of the slurry was 6.5. The effect of temperature process parameter on the degradation efficiency was investigated. The mass of anatase titanium dioxide doped with 5% black titanium dioxide + 5% α-iron oxide synthesized by the method of Example 2 was 0.40 g. The direct flotation process was placed in a light reaction device, which was connected with a circulating water pump. Circulating water was passed to make the system temperature 20, 30, 40, 50, 60, 70, and 80 °C, respectively. Hydrochloric acid was added to adjust the pH of the slurry to 3.0. The distance between the light outlet of the light source and the liquid surface was 15 cm. The flotation tailings in the reaction process were stirred by a magnetic stirrer at a stirring rate of 400 r / min. The degradation time was 4 h, and samples were taken at 0, 10, 20, 30, 60, 120, 180, and 240 min, respectively. The concentration of octadecylamine was tested by ultraviolet spectrophotometry. The degradation rate of octadecylamine with an initial concentration of 50 mg / L increased with the increase of temperature. Considering the objective reality, the system temperature of 50 °C can meet the experimental needs. The test results are shown in Figure 6 The results show that the degradation rate of octadecylamine increases with the increase of system temperature. There are two possible reasons: first, with the increase of temperature, the ionization degree of water increases, providing more H + and OH - ions, H + consumes photo-generated e - , and prolongs the lifetime of photo-generated h + ; in addition, more OH - can be converted to ·OH, both of which promote the photodegradation of octadecylamine; second, with the increase of system temperature, the movement speed of octadecylamine molecules and free radicals in the solution system increases, which improves the energy of the molecules and the probability of effective collision, thereby increasing the reaction rate per unit time.

[0078] Example 6 (Effect of different pH conditions on degradation of octadecylamine)

[0079] The photocatalytic degradation of octadecylamine in the flotation slurry section of the potassium salt direct flotation process was carried out, with the initial concentration of octadecylamine being 50 mg / L, the volume being 100 mL, the concentration of NaCl in the slurry being 0.9 mol / L, the concentration of KCl being 1.2 mol / L, the concentration of MgCl2 being 0.35 mol / L, and the initial pH of the slurry being 6.5. The effect of the pH process parameter on the degradation efficiency was investigated. The anatase titanium dioxide doped with 5% black titanium dioxide + 5% alpha-iron oxide synthesized by the method of Example 2 was added in an amount of 0.40 g. The flotation slurry in the direct flotation process was placed in a light reaction device, which was connected to a circulating water pump to keep the system temperature at 50°C. Concentrated hydrochloric acid with a concentration of 2 mol / L or sodium hydroxide solution with a concentration of 2 mol / L was added to adjust the initial pH of the slurry. The pH of the slurry was adjusted to 1.0, 2.0, 3.0, 4.0, 5.0, 7.0, 9.0, 10.0, 11.0, 12.0, and 13.0, respectively. The light source outlet was 15 cm away from the liquid surface. The flotation tailings during the reaction process were stirred by a magnetic stirrer at a stirring rate of 400 r / min. The degradation time was 4 h, and samples were taken at 0, 10, 20, 30, 60, 120, 180, and 240 min, respectively. The concentration of octadecylamine was tested by ultraviolet spectrophotometry. The degradation rate of octadecylamine with an initial concentration of 50 mg / L was greatly affected by the pH. The degradation efficiency under acidic conditions was higher than that under neutral conditions, and the degradation efficiency under alkaline conditions was higher than that under neutral conditions. The test results are shown in Table 1. Figure 7 As can be seen from the above experimental results, the degradation rate was the highest at pH = 3, reaching 98.57%. The degradation rate was the highest at pH = 11 under alkaline conditions, reaching 53.96%. The degradation efficiency was low when the pH was near 9, and the pH of the octadecylamine saturated solution was about 9.2. It is possible that the octadecylamine existed in a molecular form under the condition of pH = 9, so the degradation efficiency was low. The degradation efficiency under strong acid (pH < 2) and strong base (pH > 12) conditions decreased by the same amount. The reason may be related to the existence form of octadecylamine (mainly the change of C-N bond electron cloud density caused by amine group), the influence of H + , OH - on photo-generated electrons, photo-generated holes, and free radicals.

[0080] Example 7 (Effect of the presence of other salt substances on the degradation of dodecylmorpholine)

[0081] The photocatalytic method is used for degrading the dodecyl morpholine in the flotation slurry section in the potassium salt reverse flotation process, the initial concentration of the dodecyl morpholine is 50 mg / L, the volume is 100 mL, 0.40 g of the anatase titanium dioxide doped with 5% black titanium dioxide synthesized by the method in the example 1 is added. A certain amount of MgCl2 is added, so that the concentration is 0.10, 0.50, 1.00 mol / L, respectively, and hydrochloric acid is added to adjust the pH of the slurry to 3.0. The reverse flotation slurry is placed in a light reaction device connected with a circulating water pump, and the circulating water is used to make the temperature of the system be 50℃, respectively, so as to explore the influence of the existence of other salt substances on the degradation of the dodecyl morpholine. The flotation tail liquid in the reaction process is stirred by a magnetic stirrer, the stirring rate is 400 r / min, and the height of the light source outlet from the surface of the liquid to be treated is controlled to be 15 cm. The samples are taken at 0, 10, 20, 30, 60, 120, 180, 240 min, the concentration of the dodecyl morpholine is tested by the ultraviolet spectrophotometry, the degradation rate of the dodecyl morpholine with the initial concentration of 50 mg / L decreases with the increase of the MgCl2 concentration, and the high concentration has a significant influence on the degradation efficiency of the dodecyl morpholine. The test results are shown in Table 1. Figure 8

[0082] The wavelength of light determines whether the conduction band electrons in the photocatalyst can be excited to jump to the valence band to produce photo-generated holes and photo-generated electrons. The photo-generated hole is a key factor for inducing water to produce hydroxyl radicals and other active oxidation substances, and directly determines the performance efficiency of the photocatalytic material in degrading organic matter. It is found in the experiment that the degradation rate of the N-containing group in the flotation reagent is faster under the condition of full spectrum (200-2600 nm), which is not conducive to the determination of the concentration of the flotation reagent, so the light with the wavelength of 320-380 nm is used to carry out the experiment in the example.

[0083] The relational terms such as "first" and "second" are only used to distinguish one from another of the components with the same name, and do not necessarily require or imply any such actual relationship or order between the components.

[0084] The above is an exemplary description of the present application, and it should be explained that, without departing from the core of the present application, any simple modification, modification or other equivalent replacement which can not cost the creative labor of the person skilled in the art falls within the protection scope of the present application.​

Claims

1. A method for photocatalytic degradation of a collector in a potassium salt flotation process, characterized by, The application relates to a photocatalytic degradation method. The photocatalytic degradation material is added into a water solution containing a potassium salt collector, is uniformly dispersed, and a to-be-degraded system is obtained, and the to-be-degraded system is placed under light irradiation for degradation. The adding amount of the photocatalytic degradation material is 0.1-10 g / L. The wavelength range of the light is lambda>=200 nm. The content of the potassium salt collector in the water solution containing the potassium salt collector is 1-200 mg / L; and the potassium salt collector is octadecylamine and / or dodecylmorpholine. The degradation time t is >=30 min. The photocatalytic degradation material is a composite material formed by titanium dioxide and a doping substance, and the doping substance is one or more of black titanium dioxide, alpha-iron oxide and gamma-iron oxide. The mass of the doping substance accounts for 0.5%-50% of the total mass of the photocatalytic degradation material. The preparation method of the photocatalytic degradation material comprises the following steps: Hydrofluoric acid is added into an acetic acid solution to obtain a first solution, alkyl titanate and a doping substance are added into the first solution, the first mixture is uniformly stirred, the first mixture is transferred into a reaction kettle for sealing, and the reaction kettle is reacted at 150-300 DEG C for 12-30 h; after the reaction is completed, the precipitate is collected and washed and dried, and the dried precipitate is calcined at 400 DEG C-600 DEG C for 2-10 h to obtain the photocatalytic degradation material. The molar fraction of acetic acid in the first solution is 70-90%. The concentration of hydrofluoric acid in the first solution is 40 wt%. The doping substance is one or more of black titanium dioxide, alpha-iron oxide and gamma-iron oxide. The adding amount of the alkyl titanate is 0.5%-4.5% of the molar fraction of acetic acid. The adding amount of the doping substance is 0.075 wt%-7.5 wt% of the mass of the alkyl titanate.

2. The method of photocatalytic degradation of potassium salt floatation process collector according to claim 1, characterized in that, The pH of the to-be-degraded system is 1-12.

3. The method of photocatalytic degradation of potassium salt floatation process collector according to claim 1, characterized in that, The alkyl titanate is one or more of tetrabutyl titanate, tetraethyl titanate and tetraisopropyl titanate.

4. The method of photocatalytic degradation of potassium salt floatation process of collector according to claim 1, characterized in that, When the doping substance is alpha-iron oxide and / or gamma-iron oxide, the doping substance is synthesized in a laboratory or is a commercially available product; when the doping substance is black titanium dioxide, the doping substance is synthesized in a laboratory.

Citation Information

Patent Citations

  • Preparation method for ferrous titanate hollow microsphere and application thereof

    CN106861698A

  • Mesoporous surface defect Fe-N-TiO2 microsphere photocatalytic material and preparation method thereof

    CN107486228A