Copolymerized piezoelectric nylon material
Disrupting the molecular sequence through melt polymerization reaction improves the piezoelectric properties of piezoelectric nylon materials, solves the problems of poor piezoelectric properties and complicated preparation in the existing technology, and realizes the preparation of efficient and environmentally friendly copolymerized piezoelectric nylon materials.
Patent Information
- Application Number
- CN202411015613.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-26
AI Technical Summary
Existing piezoelectric nylon materials have poor piezoelectric properties and complex preparation processes, making it difficult to achieve large-scale preparation.
Through the melt polymerization reaction of nylon 1111 salt and aminoundecanoic acid, the molecular sequence is disrupted, the strong hydrogen bonding of polyamide is weakened, and the generation of metastable intermediate phase is promoted to form a copolymerized piezoelectric nylon material with high voltage electrical properties. .
It improves the piezoelectric properties, maintains good mechanical properties and thermal stability, is suitable for large-scale industrial production, and does not require the addition of catalysts or antioxidants during the preparation process, making it green and environmentally friendly.
Smart Images

Figure CN118725290A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of products containing polymer substances, and in particular to a copolymerized piezoelectric nylon material. Background Art
[0002] Since piezoelectric polymers have good processability and are highly stable to temperature, humidity and chemicals, have high mechanical strength and are lightweight when used as piezoelectric elements, they overcome the shortcomings of inorganic piezoelectric materials such as hardness, brittleness and high mass, and are therefore widely used in sensors, transducers and other fields. Fluorinated polyethylene and piezoelectric nylon are two typical piezoelectric polymer materials. Compared with fluoropolyethylene, piezoelectric nylon has the advantages of biocompatibility, high temperature stability, high mechanical strength and easy adjustment of crystal structure.
[0003] The dipole moment of the amide group (NH-CO) in nylon is 3.7D, which is higher than the dipole moment of PVDF (1.52D). Therefore, in addition to PVDF-based polymers, nylon with a large dipole moment also has great potential as a piezoelectric and ferroelectric polymer. The piezoelectric properties of nylon originate from the unidirectional arrangement of the dipoles of the amide group, which produces a strong dipole moment perpendicular to the molecular chain. The amide groups in the structural unit can form intermolecular hydrogen bonds, and then form a hydrogen bond layer in the structure. The existence of the hydrogen bond layer and the strength of the hydrogen bond determine the difficulty of the dipole turning.
[0004] As the earliest reported and most widely studied odd-numbered nylon, PA11 has a variety of crystal forms, among which the γ and δ' crystal forms are piezoelectric. The δ' crystal form has more twisted chain conformations, weak hydrogen bonds, and larger molecular chain spacing, so that the chain skeleton can flip with the external electric field, so it is very important to control the formation of metastable crystals. However, since the δ' crystal form of PA11 is not a thermodynamically stable crystal form, it is easily affected by the external environment and undergoes crystal form transformation. In addition, the preparation process is complicated and it is difficult to achieve large-scale preparation. PA1111, which has a similar chain structure to PA11, also has a polar crystal structure and half of it is hydrogen-bonded, and the molecular chain is more likely to twist under the action of an electric field. After quenching, annealing and stretching, PA1111 exhibits a γ crystal form similar to PA11, showing good piezoelectric and ferroelectric properties, d 33 The maximum reaches -3.9pC / N, which is close to the level of PA11.
[0005] A Chinese patent with authorization announcement number CN111635522B, which was authorized on June 8, 2021, discloses a copolymer polyamide that can produce ferroelectric nylon film by simple thermal processing and a preparation method thereof. The nylon 511 salt obtained by the salt-forming reaction of nylon 11 monomer aminoundecanoic acid with pentamethylenediamine and undecanoic acid is copolymerized. The addition of nylon 511 chain segments destroys the crystalline structure of PA11. As the content of 511 chain segments increases, the hot-pressed PA11-511 film gradually transforms from the non-ferroelectric α crystal form to the ferroelectric δ' crystal form, thereby realizing the direct thermal processing to prepare ferroelectric nylon film.
[0006] However, the piezoelectric properties of the PA11-511 ferroelectric nylon film prepared by the above method are still poor. Summary of the invention
[0007] The invention provides a copolymerized piezoelectric nylon material to solve the problem of poor piezoelectric performance of nylon materials.
[0008] In order to solve the above technical problems, the technical solution of the copolymerized piezoelectric nylon material of the present invention is:
[0009] A copolymerized piezoelectric nylon material. The preparation method of the copolymerized piezoelectric nylon material comprises the following steps: subjecting nylon 1111 salt and aminoundecanoic acid to a melt polymerization reaction to obtain the copolymerized piezoelectric nylon material.
[0010] The present invention improves the prior art and provides a copolymerized piezoelectric nylon material. Starting from the chain structure of nylon 11 (PA11) and nylon 1111 (PA1111), the molecular sequence is disrupted by copolymerization, and the strong hydrogen bonding effect of polyamide is weakened by the disorder of the chemical structure, so as to promote the generation of a metastable intermediate phase from the molecular structure level, so that it can be dipole oriented under an electric field; the copolymerized structure is PA1111 and PA11 with similar methylene lengths, which does not destroy the dipole density, but can reduce the modulus and is more likely to deform when subjected to mechanical force. The reduction in modulus and the enhancement of polarization strength jointly promote the improvement of piezoelectric performance. Moreover, the piezoelectric film with a metastable crystal form can still maintain the original crystal form when the temperature is raised to near the melting point, and no crystal form transformation occurs, and the thermal stability is excellent. The copolymerized piezoelectric nylon material prepared by the present invention still maintains good mechanical properties and has the advantages of easy processing and easy regulation of crystal form.
[0011] The copolymerized piezoelectric nylon material provided by the present invention does not require any catalyst, antioxidant, etc. to be added during the polymerization process, and is green, environmentally friendly, and economical.
[0012] In order to further improve the piezoelectric properties of the copolymerized piezoelectric nylon material, preferably, the molar ratio of the nylon 1111 salt to aminoundecanoic acid is (9-3):(1-17).
[0013] In order to further improve the preparation efficiency of nylon 1111 salt, preferably, the nylon 1111 salt is obtained by a salt-forming reaction of undecanediamine and undecanedicarboxylic acid in a solvent.
[0014] In order to further improve the utilization rate of raw materials in the salt-forming reaction, preferably, the molar ratio of the undecane dibasic acid to the undecane diamine is 1:(1.01-1.1). More preferably, the molar ratio of the undecane dibasic acid to the undecane diamine is 1:1.01.
[0015] In order to compensate for the volatilization in the salt-forming reaction, the amount of undecanediamine added is slightly excessive by 1 to 10%.
[0016] In order to further improve the reaction efficiency of the salt-forming reaction, preferably, the temperature of the salt-forming reaction is 70-75° C., the time of the salt-forming reaction is 3-4 h, and the pH during the salt-forming reaction is 7.2-7.5.
[0017] In order to further improve the reaction efficiency of the pre-polycondensation reaction, preferably, the melt polymerization reaction includes a pre-polycondensation reaction and a melt polycondensation reaction, and the pre-polycondensation reaction is carried out at 190-200° C. for 1-2 hours in an inert atmosphere.
[0018] In order to further increase the molecular weight of the copolymer, preferably, the melt polycondensation reaction is first carried out in an inert atmosphere at 230-240°C for 1-2h, the water vapor in the reaction system is discharged to normal pressure, vacuumized, and then the reaction is continued at 230-240°C for 0.5-1h.
[0019] In order to further improve the purity of the copolymer, preferably, the aminoundecanoic acid is obtained by recrystallization of a saturated solution of aminoundecanoic acid at 90-100°C. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is an infrared spectrum of the copolymerized piezoelectric nylon PA (1111-co-11) film of the present invention;
[0021] Figure 2 This is the nuclear magnetic hydrogen spectrum of the copolymerized piezoelectric nylon PA (1111-co-11) film of the present invention;
[0022] Figure 3 The DSC spectrum of the copolymerized piezoelectric nylon PA (1111-co-11) film of the present invention;
[0023] Figure 4 This is the XRD diagram of the copolymerized piezoelectric nylon PA (1111-co-11) film of the present invention. DETAILED DESCRIPTION
[0024] The technical concept of the copolymerized piezoelectric nylon material provided by the present invention is as follows:
[0025] A copolymerized piezoelectric nylon material. The preparation method of the copolymerized piezoelectric nylon material comprises the following steps: subjecting nylon 1111 salt and aminoundecanoic acid to a melt polymerization reaction to obtain the copolymerized piezoelectric nylon material.
[0026] Studies on existing piezoelectric nylon systems have shown that controlling the degree of chain conformation distortion and interchain hydrogen bonding to control the crystal structure and electric domain orientation is an effective means to improve the piezoelectric response of nylon. The present invention starts from the chain structure of nylon 11 (PA11) and PA1111, disrupts the molecular sequence through copolymerization, weakens the strong hydrogen bonding of polyamide by using the disorder of chemical structure, and promotes the generation of metastable intermediate phase from the molecular structure level, so that it can be dipole oriented under an electric field; the copolymer structure is PA1111 and PA11 with similar methylene length, which does not destroy the dipole density, but can reduce the modulus and is more likely to deform when subjected to mechanical force. The reduction of modulus and the enhancement of polarization strength jointly promote the improvement of piezoelectric performance. Moreover, the piezoelectric film with a metastable crystal form can still maintain the original crystal form when the temperature is raised to near the melting point, and no crystal form transformation occurs, and the thermal stability is excellent. The copolymerized piezoelectric nylon material prepared by the present invention still maintains good mechanical properties, and has the advantages of easy processing and easy regulation of crystal form.
[0027] The copolymerized piezoelectric nylon material provided by the present invention disrupts the original regular chain segments through copolymerization, increases the twisted conformation ratio of the methylene chain, and further forms more ferroelectric domains during the electric field polarization process. The crystallinity of the copolymerized system is reduced, and the modulus of the material is reduced. Under the combined effect of the two, the piezoelectric strain constant of the material, i.e., d 33 The piezoelectricity increases. This is because d 33 =P r / εY, where P r is the residual polarization intensity. The higher the content of oriented ferroelectric domains, the higher the P r The larger the size, ε is the relative dielectric constant, which does not change much before and after copolymerization; Y is the elastic modulus of the material, the smaller the elastic modulus, the larger the size. 33 The bigger.
[0028] The reaction formula of the melt polymerization reaction of nylon 1111 salt and aminoundecanoic acid in the preparation method of the copolymerized nylon material provided by the present invention is as follows:
[0029]
[0030] The copolymerized piezoelectric nylon material provided by the present invention does not require any catalyst, antioxidant, etc. to be added during the polymerization process, and is green, environmentally friendly, and economical.
[0031] In a specific embodiment, the copolymerized piezoelectric nylon material obtained by the melt polycondensation reaction can be hot-pressed to obtain a copolymerized piezoelectric nylon film, wherein the hot-pressing is to melt the PA1111-11 copolymer powder obtained by powdering the copolymerized piezoelectric nylon material and then hot-press it for 5 to 10 minutes at 10 to 12 MPa, and then quench it after the hot-pressing; the powdering is to heat the copolymerized piezoelectric nylon material in an organic solvent at 160 to 170°C for 3 to 4 hours under stirring conditions, and then cool, separate the solid and liquid, and dry to obtain the PA1111-11 copolymer powder. The film can be prepared only by hot pressing, and the preparation method is simple and efficient, and is suitable for large-scale industrial production.
[0032] In a specific embodiment, the solvent for the salt-forming reaction is anhydrous ethanol.
[0033] In a specific embodiment, the salt-forming reaction is to dissolve the undecane dicarboxylic acid and the undecane diamine in anhydrous ethanol at 70-75° C. respectively, mix them and react, and keep stirring at a constant speed during the reaction.
[0034] In a specific embodiment, after the salt-forming reaction, the nylon 1111 salt powder is obtained by filtering, washing with anhydrous ethanol, and vacuum drying. The vacuum drying temperature is 70 to 80° C., and the vacuum drying time is 12 to 16 hours.
[0035] In a specific embodiment, constant stirring is maintained during the entire reaction process of the pre-polycondensation reaction and the melt polycondensation reaction, and the rotation speed of the constant stirring is 300-500 rpm.
[0036] In a specific embodiment, the melting is to wrap the PA1111-11 copolymer powder with a polytetrafluoroethylene film and then melt it at a temperature 30-40°C higher than the melting point for 5-10 minutes. Furthermore, during the hot pressing molding, the melting temperature of the PA1111-11 copolymer powder is 190-210°C.
[0037] In a specific implementation manner, the quenching is to put the mold with the polytetrafluoroethylene film and the copolymerized piezoelectric nylon film into ice water for quenching.
[0038] In a specific implementation manner, the copolymerized piezoelectric nylon film is vacuum dried after the quenching, the vacuum drying temperature is 50 to 60° C., and the vacuum drying time is 12 to 24 hours.
[0039] The embodiments of the present invention are further described below in conjunction with specific examples. The chemical reagents involved in the following examples are all commercially available products unless otherwise specified.
[0040] 1. Specific embodiments of the copolymerized piezoelectric nylon material of the present invention
[0041] Example 1
[0042] The copolymerized piezoelectric nylon material of this embodiment is prepared by the following method:
[0043] 1) Preparation of nylon 1111 salt
[0044] Weigh 100g of 11-dicarboxylic acid and 11-diamine in a molar ratio of 1:1.01, dissolve the 11-dicarboxylic acid and 11-diamine in 70°C anhydrous ethanol, pour the 11-diamine solution into the 11-dicarboxylic acid solution, and perform salt reaction at 70°C. Stir at a constant speed during the reaction. A slight excess of 11-diamine makes the pH value 7.2. The reaction is stopped after 3 hours and cooled naturally to room temperature. A white precipitate is precipitated in the excess anhydrous ethanol, which is nylon 1111 salt. Filter it with a Buchner funnel, wash it repeatedly with anhydrous ethanol, and finally dry it in a vacuum drying oven at 70°C for 12 hours to obtain nylon 1111 salt powder.
[0045] 2) Recrystallization of aminoundecanoic acid
[0046] Weigh 20 g of ω-aminoundecanoic acid with a purity of 98%, prepare a saturated solution of ω-aminoundecanoic acid in 90°C water, filter through a Buchner funnel, cool at low temperature, ω-aminoundecanoic acid crystals precipitate, filter through a Buchner funnel, and dry in a vacuum oven at 60°C for 12 hours to obtain recrystallized ω-aminoundecanoic acid.
[0047] 3) Melt polymerization
[0048] A mixture of nylon 1111 salt and aminoundecanoic acid in a molar ratio of 9:1 (a total of 15 g) and 1% of the mass of nylon 1111 salt, undecanediamine, were put into a high-temperature and high-pressure reactor to ensure that the reactor was well sealed, and the nitrogen was replaced 5 times to exhaust the air in the reactor; the temperature was raised to 190°C for 1 hour and stirring began, and the temperature was maintained at 190°C for 1 hour for pre-condensation reaction, and then the temperature was raised to 230°C for insulation reaction for 1 hour; then the water vapor in the autoclave was discharged, and the pressure in the autoclave was slowly reduced to normal pressure for 1 hour, and the autoclave was evacuated to a vacuum state and the reaction was continued for 0.5 hour to stop the reaction. During the entire reaction process, the stirring was maintained at a constant speed of 300 rpm, and the PA (1111-co-11) copolymer piezoelectric nylon material was obtained naturally after cooling to room temperature.
[0049] Example 2
[0050] The copolymerized piezoelectric nylon material of this embodiment is prepared by the following method:
[0051] 1) Preparation of nylon 1111 salt
[0052] Weigh 200g of 11-dicarboxylic acid and 11-diamine in a molar ratio of 1:1.01, dissolve the 11-dicarboxylic acid and 11-diamine in 70°C anhydrous ethanol, pour the 11-diamine solution into the 11-dicarboxylic acid solution, and perform salt reaction at 70°C. Stir at a constant speed during the reaction. A slight excess of 11-diamine makes the pH value 7.2. The reaction is stopped for 3 hours and cooled naturally to room temperature. A white precipitate is precipitated in the excess anhydrous ethanol, which is nylon 1111 salt. Filter it with a Buchner funnel, wash it repeatedly with anhydrous ethanol, and finally dry it in a vacuum drying oven at 70°C for 12 hours to obtain nylon 1111 salt powder.
[0053] 2) Recrystallization of aminoundecanoic acid
[0054] Weigh 15 g of ω-aminoundecanoic acid with a purity of 98%, prepare a saturated solution of ω-aminoundecanoic acid in 90°C water, filter through a Buchner funnel, cool at low temperature, ω-aminoundecanoic acid crystals precipitate, filter through a Buchner funnel, and dry in a vacuum oven at 60°C for 12 hours to obtain recrystallized ω-aminoundecanoic acid.
[0055] 3) Melt polymerization
[0056] A mixture of nylon 1111 salt and aminoundecanoic acid in a molar ratio of 4:6 (a total of 20 g) and 1% of the mass of nylon 1111 salt, undecanediamine, were put into a high-temperature and high-pressure reactor to ensure that the reactor was well sealed, and the nitrogen was replaced 5 times to exhaust the air in the reactor; the temperature was raised to 190°C for 1 hour and stirring began, and the temperature was maintained at 190°C for 1 hour for pre-condensation reaction, and then the temperature was raised to 230°C for insulation reaction for 1 hour; then the water vapor in the autoclave was discharged, and the pressure in the autoclave was slowly reduced to normal pressure for 1 hour, and the autoclave was evacuated to a vacuum state and the reaction was continued for 0.5 hour to stop the reaction. During the entire reaction process, constant stirring was maintained at 300 rpm, and the mixture was naturally cooled to room temperature to obtain PA (1111-co-11) copolymer piezoelectric nylon material.
[0057] Example 3
[0058] The copolymerized piezoelectric nylon material of this embodiment is prepared by the following method:
[0059] Steps 1)-2) are carried out according to the preparation method of Example 2.
[0060] 3) Melt polymerization
[0061] A mixture of nylon 1111 salt and aminoundecanoic acid in a molar ratio of 15:85 (a total of 20 g) and 1% of the mass of nylon 1111 salt, undecanediamine, were put into a high-temperature and high-pressure reactor to ensure that the reactor was well sealed, and the nitrogen was replaced 5 times to exhaust the air in the reactor; the temperature was raised to 190°C for 1 hour and stirring began, and the temperature was maintained at 190°C for 1 hour for pre-condensation reaction, and then the temperature was raised to 230°C for insulation reaction for 1 hour; then the water vapor in the autoclave was discharged, and the pressure in the autoclave was slowly reduced to normal pressure for 1 hour, and the autoclave was evacuated to a vacuum state and the reaction was continued for 0.5 hour to stop the reaction. During the entire reaction process, the stirring was maintained at a constant speed of 300 rpm, and the PA (1111-co-11) copolymer piezoelectric nylon material was obtained naturally after cooling to room temperature.
[0062] 2. Comparison
[0063] Comparative Example 1
[0064] The piezoelectric nylon material of this comparative example is PA1111, which is prepared by the following method:
[0065] The preparation method of nylon 1111 salt is as follows: with reference to Example 1, 20g of nylon 1111 salt and 1% of the mass of 11-carbon diamine of nylon 1111 salt are put into a high-temperature and high-pressure reactor, the reactor is ensured to be well sealed, and nitrogen is replaced 5 times to exhaust the air in the reactor; the temperature is raised to 190°C and stirred, and then the temperature is raised to 220°C and kept for reaction for 1 hour; then the water vapor in the autoclave is discharged, and the pressure in the autoclave is slowly reduced to normal pressure for 1 hour, and the autoclave is evacuated to a vacuum state and the reaction is continued for 0.5 hours to stop the reaction. During the whole reaction process, the stirring speed is kept at 300rpm, and the piezoelectric nylon material PA1111 is obtained by natural cooling to room temperature. The melting point of the prepared PA1111 is 181°C.
[0066] Comparative Example 2
[0067] The piezoelectric nylon material of this comparative example is PA11, which is prepared by the following method:
[0068] 20g of aminoundecanoic acid was put into a high-temperature and high-pressure reactor to ensure that the reactor was well sealed, and nitrogen was replaced 5 times to exhaust the air in the reactor; the temperature was raised to 190℃ and stirred, and then the temperature was raised to 230℃ and kept for reaction for 1h; then the water vapor in the autoclave was discharged, and the pressure in the autoclave was slowly reduced to normal pressure for 1h, and the autoclave was evacuated to a vacuum state and the reaction was continued for 0.5h to stop the reaction. During the whole reaction process, the stirring speed was kept at 300rpm, and the piezoelectric nylon material was naturally cooled to room temperature to obtain PA11. The melting point of the prepared PA11 is 188℃.
[0069] Comparative Example 3
[0070] The copolymerized piezoelectric nylon material of this comparative example is prepared by the following method:
[0071] 1) Preparation of PA511 salt
[0072] The preparation method of nylon 1111 salt is the same as that in Experimental Example 1-3, except that the undecanediamine is replaced by pentamethylenediamine.
[0073] 2) Recrystallization of aminoundecanoic acid
[0074] The preparation method is the same as that in Experimental Example 1-3.
[0075] 3) Melt polymerization
[0076] A mixture of PA511 salt and aminoundecanoic acid in a molar ratio of 4:6 (a total of 20 g) and 1% of the mass of PA511 salt, undecanediamine, were put into a high-temperature and high-pressure reactor to ensure that the reactor was well sealed, and the nitrogen was replaced 5 times to exhaust the air in the reactor; the temperature was raised to 230°C for 1 hour and stirring began, and the pre-condensation reaction was carried out at 230°C for 1 hour, and then the temperature was raised to 250°C and kept for reaction for 1 hour; then the water vapor in the autoclave was discharged, and the pressure in the autoclave was slowly reduced to normal pressure for 1 hour, and the autoclave was evacuated to a vacuum state and the reaction was continued for 0.5 hour to stop the reaction. During the entire reaction process, the stirring was maintained at a constant speed of 300 rpm, and the PA (511-co-11) copolymer piezoelectric nylon material was obtained naturally after cooling to room temperature.
[0077] 3. Experimental Examples
[0078] Experimental Example 1
[0079] This experimental example analyzes the physical and chemical properties of copolymerized piezoelectric nylon materials by testing the performance of copolymerized piezoelectric nylon PA (1111-co-11) films. The method for preparing copolymerized piezoelectric nylon PA (1111-co-11) films from the copolymerized piezoelectric nylon materials of each embodiment is as follows:
[0080] The copolymerized piezoelectric nylon material of Example 1 was added to anhydrous ethanol and placed in a high-temperature and high-pressure reactor, kept at 160°C for 3 hours, and stirred at medium and high speed throughout the process. After cooling, it was filtered with a Buchner funnel and dried in a vacuum oven at 70°C for 12 hours to obtain a PA1111-11 copolymer powder; the PA1111-11 copolymer powder wrapped with a polytetrafluoroethylene film was melted at 205°C for 5 minutes, and then hot-pressed at a pressure of 10 MPa for 5 minutes, and then the mold with the polytetrafluoroethylene film and the sample were immediately quenched in ice water to obtain a translucent film with a thickness of about 50 μm, which was placed in a vacuum oven and dried at 50°C for 24 hours to obtain a copolymerized piezoelectric nylon PA (1111-co-11) film, which was recorded as coPA-1;
[0081] Referring to the method for preparing a film of the copolymer piezoelectric nylon material of the above-mentioned Example 1, the copolymer piezoelectric nylon material of Example 2 is added to anhydrous ethanol and placed in a high-temperature and high-pressure reactor, kept at 160°C for 3 hours, and stirred at medium to high speed throughout the process. After cooling, it is filtered with a Buchner funnel and dried in a vacuum oven at 70°C for 12 hours to obtain a PA1111-11 copolymer powder; the copolymer piezoelectric nylon PA (1111-co-11) film is formed by hot pressing (melting at 190°C for 5 minutes, hot pressing at a pressure of 10 MPa for 5 minutes) and quenching, and is recorded as coPA-2.
[0082] Referring to the method for preparing a film of the copolymer piezoelectric nylon material in the above-mentioned Example 1, the copolymer piezoelectric nylon material of Example 3 was added to anhydrous ethanol and placed in a high-temperature and high-pressure reactor, kept at 160°C for 3 hours, and stirred at medium to high speed throughout the process. After cooling, it was filtered with a Buchner funnel and dried in a vacuum oven at 70°C for 12 hours to obtain a PA1111-11 copolymer powder; hot pressing (melting at 205°C for 5 minutes, hot pressing at a pressure of 10 MPa for 5 minutes) and quenching to obtain a copolymer piezoelectric nylon PA (1111-co-11) film, recorded as coPA-3.
[0083] The film preparation methods of PA11 of Comparative Example 1, PA1111 of Comparative Example 2, and PA (511-co-11) of Comparative Example 3 are the same as coPA-1.
[0084] Figure 1 is the infrared spectrum of PA (1111-co-11) film. Figure 1 It can be seen that 3282cm-1 (NH stretching), 2918 and 2850cm-1 (-CH2- stretching), 1635cm-1 (amide I, C=O stretching), 1548cm-1 (amide II, combined absorption peak of CH stretching and NH bending), 1278cm-1 (amide III, CN stretching), 717cm-1 (in-plane vibration absorption peak -(CH2)n-, n>4) are characteristic peaks of aliphatic nylon, indicating the successful preparation of copolymer piezoelectric nylon.
[0085] Figure 2 This is the NMR hydrogen spectrum of PA (1111-co-11) film. Figure 2 It can be seen that the signals appearing at 1.24-1.55 ppm are the chemical shifts of the hydrogen atoms on the methylene groups far from the terminal groups in the PA1111 segments and the PA11 segments (a). The signals at 1.69-1.9 ppm are the chemical shifts of the hydrogen atoms on the methylene groups at the β position connected to the amino group (c) and the hydrogen atoms on the methylene groups at the β position connected to the carbonyl group (b). The signals at 2.74-2.83 ppm are the chemical shifts of the hydrogen atoms on the methylene groups at the α position connected to the carbonyl group (d).
[0086] Figure 3 is the DSC spectrum of PA (1111-co-11) film, where Figure 3 The upper part is the structure diagram of PA (1111-co-11) film. Figure 3 It can be seen that with the increase of copolymerization ratio, the melting point first decreases and then increases, and the melting enthalpy first increases and then decreases.
[0087] Figure 4 is the XRD pattern of PA (1111-co-11) film. Figure 4 It can be seen that due to the rapid cooling process, the XRD patterns of the prepared copolymer samples all show a single diffraction peak, and the peak value corresponds to a diffraction angle of about 21.3°, which is consistent with the metastable γ crystal parameters.
[0088] Experimental Example 2
[0089] In this experimental example, the piezoelectric properties of copolymer piezoelectric nylon PA (1111-co-11) film were tested.
[0090] The piezoelectric strain constant d of PA(1111-co-11) film was determined by quasi-static method. 33 The ferroelectricity is tested by a ferroelectric tester, and important parameters are read from the hysteresis loop. The vertical intercept of the DE curve and the D axis is called the residual polarization intensity (P r ), and the transverse intercept with the E axis is called the coercive electric field (E c ), the test results are shown in Table 1.
[0091] Table 1 Piezoelectric properties test results of nylon film
[0092] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 <![CDATA[Piezoelectric strain constant d 33 (pC / N)]]> 4.2 6.2 4.5 4.0 3.2 3.6 <![CDATA[Residual polarization intensity P r (μC / cm 2 )]]> 4.0 5.0 3.7 2.5 1.5 2.0 <![CDATA[Coercive electric field E c (MV / m)]]> 41 50 53 30 48 60
[0093] It can be seen from Table 1 that the piezoelectric strain constant d of the PA (1111-co-11) film provided by the present invention is 33 , residual polarization intensity P r They are all higher than those of nylon films PA11, PA1111, and PA(511-co-11), indicating that with the occurrence of copolymerization, the original regular chain segments are disrupted, the twisted conformation ratio of the methylene chain is increased, and then during the electric field polarization process, more ferroelectric domains are formed and the modulus is reduced, which synergistically makes the piezoelectric properties of nylon significantly improved.
[0094] Experimental Example 3
[0095] In this experimental example, the mechanical properties of the PA (1111-co-11) film were tested by a universal mechanical testing machine, and the measured elastic modulus results are shown in Table 2.
[0096] Table 2 Elastic modulus test results of nylon film
[0097] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 <![CDATA[Modulus of elasticity (N / mm 2 )]]> 470 400 405 500 430 510
[0098] It can be seen from Table 2 that the elastic modulus of the PA (1111-co-11) film provided by the present invention is lower than that of PA1111 and PA (511-co-11), and coPA-2 and coPA-3 are also lower than that of PA11. 33 =P r / εY, the test results of Experimental Example 2 show that the P r This experimental example shows that the elastic modulus Y of PA (1111-co-11) film is reduced, and the two together make d 33 The piezoelectric strain constant increases, that is, the piezoelectric performance improves. Although the elastic modulus of coPA-1 is higher than that of PA11, according to the test results in Table 1, the residual polarization intensity P of coPA-1 is higher than that of PA11. r The improvement is more obvious, and the combined effect of the two makes the piezoelectric strain constant d 33 Be improved.
[0099] Finally, it should be noted that the above-described implementation cases are only used to illustrate the preparation method, and are not intended to limit the technical solution of the present invention. Any equivalent substitutions or corresponding improvements made to the features of the present invention should be included in the scope of the claims of the present invention.
Claims
1. A copolymer piezoelectric nylon material, characterized in that: The preparation method of the copolymerized piezoelectric nylon material comprises the following steps: subjecting nylon 1111 salt and aminoundecanoic acid to a melt polymerization reaction to obtain the copolymerized piezoelectric nylon material.
2. The copolymer piezoelectric nylon material according to claim 1, characterized in that: The molar ratio of the nylon 1111 salt to aminoundecanoic acid is (9-3):(1-17).
3. The copolymerized piezoelectric nylon material according to claim 1, characterized in that: The nylon 1111 salt is obtained by a salt-forming reaction of undecanediamine and undecanedicarboxylic acid in a solvent.
4. The copolymerized piezoelectric nylon material according to claim 3, characterized in that: The molar ratio of the undecane dicarboxylic acid to the undecane diamine is 1:(1.01-1.1).
5. The copolymerized piezoelectric nylon material according to claim 3, characterized in that: The temperature of the salt-forming reaction is 70-75° C., the time of the salt-forming reaction is 3-4 hours, and the pH during the salt-forming reaction is 7.2-7.
5.
6. The copolymerized piezoelectric nylon material according to claim 1, characterized in that: The melt polymerization reaction includes a pre-polycondensation reaction and a melt polycondensation reaction. The pre-polycondensation reaction is carried out in an inert atmosphere at 190-200° C. for 1-2 hours.
7. The copolymerized piezoelectric nylon material according to claim 6, characterized in that: The melt polycondensation reaction is firstly carried out in an inert atmosphere at 230-240° C. for 1-2 hours, the water vapor in the reaction system is discharged to normal pressure, vacuumized, and then the reaction is continued at 230-240° C. for 0.5-1 hour.
8. The copolymerized piezoelectric nylon material according to claim 1, characterized in that: The amino undecanoic acid is obtained by recrystallizing a saturated amino undecanoic acid solution at 90-100°C.
Citation Information
Patent Citations
Long carbon chain aliphatic nylon PA1111 material and preparation method thereof
CN106866958A
Copolymerized nylon powder material having controllable melting point, and preparation method thereof
CN107337792A
Copolymerized polyamide capable of preparing ferroelectric nylon film through simple hot processing, and preparation method thereof
CN111635522A
Copolymerized polyamide
WO2011052464A1
Cited By
Polyesteramide microspheres, preparation method thereof and piezoelectric composite material
CN120399219A