Photocuring 3D printing silicon-based ceramic core slurry as well as preparation method and application thereof
Through light-curing 3D printing of silicon-based ceramic core slurry, combined with nano-alumina and sintering processes, the problems of high shrinkage and insufficient strength of the ceramic core are solved, and the dimensional accuracy and performance of the inner cavity of the high-temperature alloy blade are improved.
Patent Information
- Application Number
- CN202410736228.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-07
AI Technical Summary
Ceramic cores have problems with high sintering and casting shrinkage during the manufacturing process, which affects the dimensional accuracy of the inner cavity of the blade. It also has insufficient strength and chemical stability when it withstands the impact of molten metal at high temperatures, making it difficult to meet the complex requirements of aero-engine blades. .
Use light-curing 3D printing silicon-based ceramic core slurry, which includes quartz glass powder, mineralizer and nano-alumina. The ceramic core is prepared through light-curing 3D printing technology, combined with appropriate sintering processes to reduce shrinkage and improve physical properties. performance.
It significantly reduces the sintering and casting shrinkage of the ceramic core, increases the room temperature and high temperature bending strength, enhances the chemical stability, and meets the dimensional accuracy and performance requirements of the aeroengine blade inner cavity.
Smart Images

Figure BDA0004881841960000111 
Figure BDA0004881841960000112 
Figure BDA0004881841960000121
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of additive manufacturing, and in particular to a photocurable 3D printing silicon-based ceramic core slurry, a preparation method and application thereof. Background Art
[0002] The inner cavity structure of aircraft engine blades is a ceramic core, which must withstand the challenges of various complex and harsh environments. Therefore, the ceramic core must have excellent performance in terms of size, strength and surface roughness.
[0003] However, with the continuous development of aviation engine technology, the technical requirements of high-temperature alloy turbine blades are also constantly improving, and the structure of the blades is becoming more and more complex. Ceramic cores as the inner cavity of the blades are usually manufactured using traditional hot injection molding. The cores have disadvantages such as long mold design and manufacturing cycle and high cost. Light-curing 3D printing technology uses the core model to form layer by layer and transform it into a three-dimensional entity. It has the advantages of no mold and short production cycle.
[0004] Ceramic cores will produce sintering shrinkage during the preparation process. For 3D printed ceramic cores, the size of the core in the three-dimensional direction can be adjusted through the digital model, which can ultimately reduce the sintering shrinkage rate of the ceramic core in the three-dimensional direction; the core will also produce different degrees of casting shrinkage during the directional solidification process, and there is no way to reduce the shrinkage rate by adjusting the digital model in this process. The high shrinkage deformation of the ceramic core during use will eventually affect the dimensional accuracy of the blade cavity. At the same time, the ceramic core needs to withstand the impact and immersion of 1500-1600℃ high-temperature metal liquid during high-temperature pouring, which requires extremely high high-temperature strength, toughness and chemical stability of the ceramic core. Therefore, in order to make the ceramic core and blade have higher dimensional accuracy and excellent performance, reducing the sintering / casting shrinkage rate of the ceramic core and improving the physical properties and chemical stability of the ceramic core during preparation and service are currently urgent problems to be solved. Summary of the invention
[0005] In view of this, the technical problem to be solved by the present invention is to provide a photocurable 3D printed silicon-based ceramic core slurry, a preparation method and application thereof. The photocurable 3D printed silicon-based ceramic core obtained by using the photocurable 3D printed silicon-based ceramic core slurry of the present invention has better physical properties and usage performance.
[0006] The present invention provides a photocurable 3D printing silicon-based ceramic core slurry, comprising:
[0007] Ceramic powder 55wt% to 65wt%;
[0008] Acrylate photosensitive resin 32wt% to 42wt%;
[0009] Dispersant 3wt%~5wt%;
[0010] The sum of the amounts of the above components is 100%;
[0011] The ceramic powder comprises:
[0012] Quartz glass powder 89wt%~98wt%;
[0013] Mineralizer 0.2wt%~10wt%;
[0014] Nano-alumina 0.1wt%~2wt%;
[0015] In the ceramic powder, the sum of the amounts of the above components is 100%.
[0016] Preferably, the median particle size of the quartz glass powder is 6 to 8 μm.
[0017] Preferably, the mineralizer is at least one of alumina powder, silicon carbide powder, zirconium silicate powder, zirconium oxide powder, mullite powder, cristobalite, metallic silicon powder, silicon micropowder, nano silicon powder, zirconium carbide, carbon black, carbon nanotubes, nano aluminum powder, aluminum powder and graphene; and the median particle size of the mineralizer is 0.05 to 40 μm.
[0018] Preferably, the median particle size of the nano-alumina is 30 to 50 nm.
[0019] Preferably, the acrylic ester photosensitive resin is an acrylic ester monomer and an acrylic ester oligomer;
[0020] In the acrylic ester photosensitive resin, the content of acrylic ester monomers is 55 wt % to 65 wt %, and the content of acrylic ester oligomers is 35 wt % to 45 wt %.
[0021] Preferably, the acrylic acid ester monomer is at least one of 1,6-hexanediol diacrylate, 1,6-hexanediol dimethacrylate, dipropylene glycol diacrylate, trimethylolpropane triacrylate, triethylene glycol diacrylate, tripropylene glycol diacrylate, hydroxyethyl methacrylate, pentaerythritol tetraacrylate, ethoxylated pentaerythritol, dipentaerythritol hexaacrylate, isobornyl acrylate, isobornyl methacrylate, polyethylene glycol (200) diacrylate and polyethylene glycol (400) diacrylate;
[0022] The acrylate oligomer is at least one of aliphatic polyurethane acrylate, aromatic polyurethane acrylate and modified epoxy acrylate.
[0023] Preferably, the dispersant is at least one of Disperbyk-111, UV dispersant JZ-291 and BASK dispersant.
[0024] The present invention also provides a method for preparing the above-mentioned light-cured 3D printing silicon-based ceramic core slurry, comprising the following steps:
[0025] The ceramic powder, the acrylic photosensitive resin and the dispersant are mixed to obtain a photocurable 3D printing silicon-based ceramic core slurry;
[0026] The ceramic powder is obtained by mixing quartz glass powder, mineralizer and nano-alumina.
[0027] The present invention also provides a method for forming the above-mentioned light-cured 3D printed silicon-based ceramic core slurry, comprising the following steps:
[0028] A) performing photocuring 3D printing on a silicon-based ceramic core slurry to obtain a green body;
[0029] The process parameters of the light-curing 3D printing include: the curing thickness is 75-100 μm, and the curing power is set to 12-15 mW / cm 2 , the single layer curing time is 3 to 5 seconds;
[0030] B) Degreasing and sintering the green body to obtain a photocurable 3D printed silicon-based ceramic core.
[0031] The present invention also provides a light-cured 3D printed silicon-based ceramic core made by the molding method described above.
[0032] The present invention provides a photocurable 3D printing silicon-based ceramic core slurry, comprising: 55wt% to 65wt% of ceramic powder; 32wt% to 42wt% of acrylic photosensitive resin; 3wt% to 5wt% of dispersant; the sum of the amounts of the above components is 100%; the ceramic powder comprises: 89wt% to 98wt% of quartz glass powder; 0.2wt% to 10wt% of mineralizer; 0.1wt% to 2wt% of nano-alumina; in the ceramic powder, the sum of the amounts of the above components is 100%. The photocurable 3D printing silicon-based ceramic core slurry provided by the present invention uses nano-alumina as a modifier, which can cooperate well with other components to significantly inhibit the shrinkage rate of the silicon-based ceramic core. The photocurable 3D printing silicon-based ceramic core obtained by using the photocurable 3D printing silicon-based ceramic core slurry of the present invention has better physical properties and use performance.
[0033] The experimental results show that the silicon-based ceramic core slurry for 3D printing of the present invention is used for light-curing 3D printing, and the apparent porosity of the silicon-based ceramic core obtained is 29.18% to 34.53%, the water absorption rate is 18.24% to 23.56%, and the volume density is 1.49 to 1.58 g / cm 3The maximum pore size is 0.228~0.286mm; the room temperature flexural strength test value is not less than 3.24MPa, and the high temperature flexural strength test value is not less than 25.13MPa; the sintering shrinkage rates of the ceramic core in the three-dimensional directions of length, width and height are 1.76%~3.97%, 1.64%~3.47% and 1.67%~4.04% respectively, and the casting shrinkage rates of the ceramic core in the three-dimensional directions of length, width and height are 1.74%~7.17%, 3.41%~9.26% and 6.27%~11.29% respectively. DETAILED DESCRIPTION
[0034] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] The present invention provides a photocurable 3D printing silicon-based ceramic core slurry, comprising:
[0036] Ceramic powder 55wt% to 65wt%;
[0037] Acrylate photosensitive resin 32wt% to 42wt%;
[0038] Dispersant 3wt%~5wt%;
[0039] The sum of the amounts of the above components is 100%;
[0040] The ceramic powder comprises:
[0041] Quartz glass powder 89wt%~98wt%;
[0042] Mineralizer 0.2wt%~10wt%;
[0043] Nano-alumina 0.1wt%~2wt%;
[0044] In the ceramic powder, the sum of the amounts of the above components is 100%.
[0045] About ceramic powder:
[0046] The median particle size of the quartz glass powder is 6-8 μm, for example, 7 μm.
[0047] The mineralizer is at least one of alumina powder, silicon carbide powder, zirconium silicate powder, zirconium oxide powder, mullite powder, cristobalite, metallic silicon powder, silicon micropowder, nano silicon powder, nano aluminum powder, aluminum powder, zirconium carbide, carbon nanotubes, carbon black and graphene; the median particle size of the mineralizer is 0.05 to 40 μm, such as 20 μm, 5 μm, and 0.1 μm.
[0048] The median particle size of the nano-alumina is 30-50 nm, such as 30 nm, 40 nm, and 50 nm.
[0049] About acrylic photosensitive resin:
[0050] The acrylic ester photosensitive resin is an acrylic ester monomer and an acrylic ester oligomer. In the acrylic ester photosensitive resin, the content of the acrylic ester monomer is 55wt% to 65wt%, and the content of the acrylic ester oligomer is 35wt% to 45wt%.
[0051] The acrylic ester monomer is at least one of 1,6-hexanediol diacrylate (HDDA), 1,6-hexanediol dimethacrylate (HDDMA), dipropylene glycol diacrylate (DPGDA), trimethylolpropane triacrylate (TMPTA), triethylene glycol diacrylate (TEGDA), tripropylene glycol diacrylate (TPGDA), hydroxyethyl methacrylate (HEMA), pentaerythritol tetraacrylate (PET4A), ethoxylated pentaerythritol tetraacrylate (PPTTA), dipentaerythritol hexaacrylate (DPHA), isobornyl acrylate (IBOA), isobornyl methacrylate (IBOMA), polyethylene glycol (200) diacrylate (PEG (200) DA) and polyethylene glycol (400) diacrylate (PEG (400) DA).
[0052] The acrylate oligomer is at least one of aliphatic urethane acrylate, aromatic urethane acrylate and modified epoxy acrylate. The aliphatic urethane acrylate is selected from at least one of difunctional aliphatic urethane acrylate oligomer, trifunctional aliphatic urethane acrylate and waterborne aliphatic urethane acrylate; the aromatic urethane acrylate is selected from at least one of trifunctional aromatic urethane acrylate oligomer, aromatic urethane modified acrylate and aromatic urethane diacrylate; the modified epoxy acrylate is selected from at least one of epoxy acrylate oligomer, bisphenol A epoxy acrylate and silicone modified epoxy acrylate.
[0053] The dispersant is at least one of Disperbyk-111, UV dispersant JZ-291 and BASK dispersant.
[0054] The solid content of the photocurable 3D printing silicon-based ceramic core slurry is 55 vol.% to 65 vol.%, such as 60 vol.%; the viscosity is 2400 to 3660 mPa·s, such as 2894 mPa·s, 3660 mPa·s, 2648 mPa·s, 2801 mPa·s, 2986 mPa·s, 2718 mPa·s, 2400 mPa·s, 3525 mPa·s, and 3447 mPa·s. The viscosity will affect the fluidity of the slurry during the printing process, and then affect the uniformity of the particle dispersion in the slurry, and finally affect the performance of the printed sample.
[0055] The present invention provides a method for preparing the above-mentioned light-cured 3D printing silicon-based ceramic core slurry, comprising the following steps:
[0056] The ceramic powder, the acrylic photosensitive resin and the dispersant are mixed to obtain a photocurable 3D printing silicon-based ceramic core slurry;
[0057] The ceramic powder is obtained by mixing quartz glass powder, mineralizer and nano-alumina.
[0058] The mixing specifically refers to uniform mixing.
[0059] The present invention also provides a method for forming the photocurable 3D printed silicon-based ceramic core slurry described above, or the photocurable 3D printed silicon-based ceramic core slurry prepared by the preparation method described above, comprising the following steps:
[0060] A) performing photocuring 3D printing on a silicon-based ceramic core slurry to obtain a green body;
[0061] The process parameters of the light-curing 3D printing include: the curing thickness is 75-100 μm, and the curing power is set to 12-15 mW / cm 2 , the single layer curing time is 3 to 5 seconds;
[0062] B) Degreasing and sintering the green body to obtain a photocurable 3D printed silicon-based ceramic core.
[0063] In step B):
[0064] The debinding and sintering comprises:
[0065] The temperature is raised from room temperature to 200-270°C and kept for 1-3 hours, then continued to be raised to 300-400°C and kept for 1-3 hours, then continued to be raised to 500-600°C and kept for 1-2 hours, and finally continued to be raised to 1100-1300°C and kept for 4-8 hours.
[0066] The present invention also provides a photocurable 3D printed silicon-based ceramic core obtained by the molding method described above.
[0067] The present invention has no particular limitation on the sources of the raw materials used above, and they can be generally commercially available.
[0068] In order to further illustrate the present invention, a photocurable 3D printing silicon-based ceramic core slurry, a preparation method and an application thereof provided by the present invention are described in detail below in combination with embodiments, but it should not be understood as limiting the scope of protection of the present invention.
[0069] Example 1
[0070] 1) Preparation of ceramic powder:
[0071] Quartz glass powder (median particle size of 7 μm), mineralizer (alumina powder, median particle size of 20 μm) and nano-alumina (median particle size of 30 nm) are uniformly mixed to obtain ceramic powder; in the ceramic powder, the content of quartz glass powder is 89wt%, the content of mineralizer is 10wt%, and the content of nano-alumina is 1wt%.
[0072] 2) Preparation of photocurable 3D printed silicon-based ceramic core slurry:
[0073] The ceramic powder, acrylic photosensitive resin and dispersant (Disperbyk-111) of step 1) are mixed to obtain a photocurable 3D printed silicon-based ceramic core slurry; in the acrylic photosensitive resin, the content of acrylic monomer (HDDA) is 60wt%, and the content of acrylic oligomer (epoxy acrylate oligomer) is 40wt%; in the photocurable 3D printed silicon-based ceramic core slurry, the content of ceramic powder is 60wt%, the content of acrylic photosensitive resin is 35wt%, and the content of dispersant is 5wt%. The solid content of the photocurable 3D printed silicon-based ceramic core slurry is 60vol.%, and the viscosity is 2894mPa·s.
[0074] 3) A method for forming a photocurable 3D printed silicon-based ceramic core slurry, comprising the following steps:
[0075] 3-1) performing photocuring 3D printing on the photocuring 3D printing silicon-based ceramic core slurry to obtain a green body;
[0076] The process parameters of the photocuring 3D printing include: the curing thickness is 85 μm, and the curing power is set to 13 mW / cm 2 , the single layer curing time is 4s;
[0077] 3-2) degreasing and sintering the green body to obtain a photocurable 3D printed silicon-based ceramic core;
[0078] The degreasing and sintering are as follows:
[0079] The temperature was raised from room temperature to 230°C and kept for 2 hours, then raised to 350°C and kept for 2 hours, then raised to 550°C and kept for 1.5 hours, and finally raised to 1200°C and kept for 6 hours.
[0080] Example 2
[0081] The difference from Example 1 is:
[0082] 1) Preparation of ceramic powder:
[0083] Quartz glass powder (median particle size of 7 μm), mineralizer (alumina powder, median particle size of 5 μm) and nano-alumina (median particle size of 40 nm) are uniformly mixed to obtain ceramic powder; in the ceramic powder, the content of quartz glass powder is 93wt%, the content of mineralizer is 5wt%, and the content of nano-alumina is 2wt%.
[0084] In step 2), the solid content of the photocurable 3D printed silicon-based ceramic core slurry is 60 vol.%, and the viscosity is 3660 mPa·s.
[0085] The remaining steps and parameters are the same as those in Example 1 to obtain a photocurable 3D printed silicon-based ceramic core.
[0086] Example 3
[0087] The difference from Example 1 is:
[0088] 1) Preparation of ceramic powder:
[0089] Quartz glass powder (median particle size of 7 μm), mineralizer (alumina powder, median particle size of 0.1 μm) and nano-alumina (median particle size of 50 nm) are uniformly mixed to obtain ceramic powder; in the ceramic powder, the content of quartz glass powder is 98wt%, the content of mineralizer is 1.8wt%, and the content of nano-alumina is 0.2wt%.
[0090] In step 2), the solid content of the photocurable 3D printed silicon-based ceramic core slurry is 60 vol.%, and the viscosity is 2648 mPa·s.
[0091] The remaining steps and parameters are the same as those in Example 1 to obtain a photocurable 3D printed silicon-based ceramic core.
[0092] Example 4
[0093] The difference from Example 1 is:
[0094] The mineralizer alumina powder was replaced with silicon carbide powder.
[0095] In step 2), the solid content of the photocurable 3D printed silicon-based ceramic core slurry is 60 vol.%, and the viscosity is 2801 mPa·s.
[0096] The remaining steps and parameters are the same as those in Example 1 to obtain a photocurable 3D printed silicon-based ceramic core.
[0097] Example 5
[0098] The difference from Example 1 is:
[0099] The mineralizer alumina powder was replaced with zirconium silicate powder.
[0100] In step 2), the solid content of the photocurable 3D printed silicon-based ceramic core slurry is 60 vol.%, and the viscosity is 2986 mPa·s.
[0101] The remaining steps and parameters are the same as those in Example 1 to obtain a photocurable 3D printed silicon-based ceramic core.
[0102] Example 6
[0103] The difference from Example 1 is:
[0104] The mineralizer alumina powder was replaced by graphene.
[0105] In step 2), the solid content of the photocurable 3D printed silicon-based ceramic core slurry is 60 vol.%, and the viscosity is 2718 mPa·s.
[0106] The remaining steps and parameters are the same as those in Example 1 to obtain a photocurable 3D printed silicon-based ceramic core.
[0107] Example 7
[0108] The difference from Example 1 is:
[0109] 2) Preparation of photocurable 3D printed silicon-based ceramic core slurry:
[0110] The ceramic powder, acrylic photosensitive resin and dispersant (Disperbyk-111) of step 1) are mixed to obtain a photocurable 3D printed silicon-based ceramic core slurry; in the acrylic photosensitive resin, the content of acrylic monomer (HDDA) is 60wt%, and the content of acrylic oligomer (epoxy acrylate oligomer) is 40wt%; in the photocurable 3D printed silicon-based ceramic core slurry, the content of ceramic powder is 55wt%, the content of acrylic photosensitive resin is 42wt%, and the content of dispersant is 3wt%. The solid content of the photocurable 3D printed silicon-based ceramic core slurry is 55vol.%, and the viscosity is 2400mPa·s.
[0111] The remaining steps and parameters are the same as those in Example 1 to obtain a photocurable 3D printed silicon-based ceramic core.
[0112] Example 8
[0113] The difference from Example 1 is:
[0114] 2) Preparation of photocurable 3D printed silicon-based ceramic core slurry:
[0115] The ceramic powder, acrylic photosensitive resin and dispersant (Disperbyk-111) of step 1) are mixed to obtain a photocurable 3D printed silicon-based ceramic core slurry; in the acrylic photosensitive resin, the content of acrylic monomer (HDDA) is 60wt%, and the content of acrylic oligomer (epoxy acrylate oligomer) is 40wt%; in the photocurable 3D printed silicon-based ceramic core slurry, the content of ceramic powder is 64wt%, the content of acrylic photosensitive resin is 32wt%, and the content of dispersant is 4wt%. The solid content of the photocurable 3D printed silicon-based ceramic core slurry is 64vol.%, and the viscosity is 3525mPa·s.
[0116] The remaining steps and parameters are the same as those in Example 1 to obtain a photocurable 3D printed silicon-based ceramic core.
[0117] Example 9
[0118] The difference from Example 1 is:
[0119] The dispersant Disperbyk-111 was replaced with BASK dispersant. The solid content of the photocurable 3D printing silicon-based ceramic core slurry was 60 vol.%, and the viscosity was 3447 mPa·s.
[0120] The remaining steps and parameters are the same as those in Example 1 to obtain a photocurable 3D printed silicon-based ceramic core.
[0121] Example 10
[0122] The difference from Example 1 is:
[0123] 3-1) performing photocuring 3D printing on the photocuring 3D printing silicon-based ceramic core slurry to obtain a green body;
[0124] The process parameters of the light-curing 3D printing include: the curing thickness is 75 μm, and the curing power is set to 12 mW / cm 2 , the single layer curing time is 5s.
[0125] The remaining steps and parameters are the same as those in Example 1 to obtain a photocurable 3D printed silicon-based ceramic core.
[0126] Embodiment 11
[0127] The difference from Example 1 is:
[0128] 3-1) performing photocuring 3D printing on the photocuring 3D printing silicon-based ceramic core slurry to obtain a green body;
[0129] The process parameters of the photocuring 3D printing include: the curing thickness is 100 μm, and the curing power is set to 15 mW / cm 2 , the single layer curing time is 5s.
[0130] The remaining steps and parameters are the same as those in Example 1 to obtain a photocurable 3D printed silicon-based ceramic core.
[0131] Example 12
[0132] The difference from Example 1 is:
[0133] 3-2) degreasing and sintering the green body to obtain a photocurable 3D printed silicon-based ceramic core;
[0134] The degreasing and sintering are as follows:
[0135] The temperature was raised from room temperature to 200°C and kept for 3 hours, then raised to 300°C and kept for 3 hours, then raised to 500°C and kept for 2 hours, and finally raised to 1100°C and kept for 8 hours.
[0136] The remaining steps and parameters are the same as those in Example 1 to obtain a photocurable 3D printed silicon-based ceramic core.
[0137] Embodiment 13
[0138] The difference from Example 1 is:
[0139] 3-2) degreasing and sintering the green body to obtain a photocurable 3D printed silicon-based ceramic core;
[0140] The degreasing and sintering are as follows:
[0141] The temperature was raised from room temperature to 270°C and kept for 1 hour, then continued to be raised to 400°C and kept for 1 hour, then continued to be raised to 600°C and kept for 1 hour, and finally continued to be raised to 1300°C and kept for 4 hours.
[0142] The remaining steps and parameters are the same as those in Example 1 to obtain a photocurable 3D printed silicon-based ceramic core.
[0143] Comparative Example 1
[0144] The difference from Example 1 is that (the ceramic powder does not contain nano-alumina):
[0145] 1) Preparation of ceramic powder:
[0146] Quartz glass powder (median particle size of 7 μm) and mineralizer (alumina powder, median particle size of 20 μm) are uniformly mixed to obtain ceramic powder; in the ceramic powder, the content of quartz glass powder is 89wt%, and the content of mineralizer is 11wt%.
[0147] In step 2), the solid content of the photocurable 3D printed silicon-based ceramic core slurry is 60 vol.%, and the viscosity is 2589 mPa·s.
[0148] The remaining steps and parameters are the same as those in Example 1 to obtain a photocurable 3D printed silicon-based ceramic core.
[0149] Comparative Example 2
[0150] The difference from Example 1 is (the ceramic powder does not contain a mineralizer):
[0151] 1) Preparation of ceramic powder:
[0152] Quartz glass powder (median particle size of 7 μm) and nano-alumina (median particle size of 30 nm) are uniformly mixed to obtain ceramic powder; in the ceramic powder, the content of quartz glass powder is 99wt%, and the content of nano-alumina is 1wt%.
[0153] In step 2), the solid content of the photocurable 3D printed silicon-based ceramic core slurry is 60 vol.%, and the viscosity is 2746 mPa·s.
[0154] The remaining steps and parameters are the same as those in Example 1 to obtain a photocurable 3D printed silicon-based ceramic core.
[0155] The physical properties of the light-cured 3D printed silicon-based ceramic cores prepared in Examples 1 to 17 and Comparative Example 1 were tested according to Standard No. AETM181A. The results are shown in Table 1.
[0156] Table 1 Physical properties of the photocurable 3D printed silicon-based ceramic cores prepared in Examples 1 to 17 and Comparative Examples 1 to 2
[0157]
[0158] The performance of the light-cured 3D printed silicon-based ceramic cores prepared in Examples 1 to 13 and Comparative Examples 1 to 2 was tested according to Standard No. HB5353, and the results are shown in Table 2.
[0159] Table 2 Performance of the photocurable 3D printed silicon-based ceramic cores prepared in Examples 1 to 13 and Comparative Examples 1 to 2
[0160]
[0161]
[0162] The results of Table 1 and Table 2 show that the shrinkage of 3D printed silicon-based ceramic cores is mainly caused by interlayer shrinkage and shrinkage between ceramic particles. The more fully the adjacent interlayer ceramic particles are sintered after sintering, the greater the shrinkage rate. The addition of nano-alumina increases the sintering barrier of quartz glass and reduces the sintering driving force of quartz glass powder, which helps to reduce the sintering shrinkage rate, but too much nano-alumina will lead to a decrease in bending strength. In addition, the higher the solid content and sintering temperature of the ceramic slurry, the greater the driving force during the sintering process, the higher the densification degree of the sample, and the greater the strength. Therefore, under the joint action of nano-alumina, solid content and sintering temperature, the physical properties and performance of the embodiment have reached the optimal value. It can be seen from Table 1 and Table 2 that the physical properties and performance of the embodiment of the present invention have met the casting and use requirements of high-temperature alloy blades. The prepared 3D printed ceramic core has controllable shrinkage in all directions during preparation and service, and the room temperature strength and high temperature strength are optimal, which well meets the main requirements of high-temperature alloys.
[0163] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A photocurable 3D printing silicon-based ceramic core slurry, comprising: Ceramic powder 55wt% to 65wt%; Acrylate photosensitive resin 32wt% to 42wt%; Dispersant 3wt%~5wt%; The sum of the amounts of the above components is 100%; The ceramic powder comprises: Quartz glass powder 89wt%~98wt%; Mineralizer 0.2wt%~10wt%; Nano-alumina 0.1wt%~2wt%; In the ceramic powder, the sum of the amounts of the above components is 100%.
2. The photocurable 3D printing silicon-based ceramic core slurry according to claim 1, characterized in that: The median particle size of the quartz glass powder is 6 to 8 μm.
3. The photocurable 3D printing silicon-based ceramic core slurry according to claim 1, characterized in that: The mineralizer is at least one of alumina powder, silicon carbide powder, zirconium silicate powder, zirconium oxide powder, mullite powder, cristobalite, metallic silicon powder, silicon micropowder, nano silicon powder, zirconium carbide, carbon black, carbon nanotubes, nano aluminum powder, aluminum powder and graphene; the median particle size of the mineralizer is 0.05-40 μm.
4. The photocurable 3D printing silicon-based ceramic core slurry according to claim 1, characterized in that: The median particle size of the nano-alumina is 30 to 50 nm.
5. The photocurable 3D printing silicon-based ceramic core slurry according to claim 1, characterized in that: The acrylic ester photosensitive resin is an acrylic ester monomer and an acrylic ester oligomer; In the acrylic ester photosensitive resin, the content of acrylic ester monomers is 55 wt % to 65 wt %, and the content of acrylic ester oligomers is 35 wt % to 45 wt %.
6. The photocurable 3D printing silicon-based ceramic core slurry according to claim 5, characterized in that: The acrylic acid ester monomer is at least one of 1,6-hexanediol diacrylate, 1,6-hexanediol dimethacrylate, dipropylene glycol diacrylate, trimethylolpropane triacrylate, triethylene glycol diacrylate, tripropylene glycol diacrylate, hydroxyethyl methacrylate, pentaerythritol tetraacrylate, ethoxylated pentaerythritol, dipentaerythritol hexaacrylate, isobornyl acrylate, isobornyl methacrylate, polyethylene glycol (200) diacrylate and polyethylene glycol (400) diacrylate; The acrylate oligomer is at least one of aliphatic polyurethane acrylate, aromatic polyurethane acrylate and modified epoxy acrylate.
7. The photocurable 3D printing silicon-based ceramic core slurry according to claim 1, characterized in that: The dispersant is at least one of Disperbyk-111, UV dispersant JZ-291 and BASK dispersant.
8. A method for preparing the photocurable 3D printing silicon-based ceramic core slurry according to any one of claims 1 to 7, comprising the following steps: The ceramic powder, the acrylic photosensitive resin and the dispersant are mixed to obtain a photocurable 3D printing silicon-based ceramic core slurry; The ceramic powder is obtained by mixing quartz glass powder, mineralizer and nano-alumina.
9. A method for forming a photocurable 3D printed silicon-based ceramic core slurry according to any one of claims 1 to 7, comprising the following steps: A) performing photocuring 3D printing on a silicon-based ceramic core slurry to obtain a green body; The process parameters of the light-curing 3D printing include: the curing thickness is 75-100 μm, and the curing power is set to 12-15 mW / cm 2 , the single layer curing time is 3 to 5 seconds; B) Degreasing and sintering the green body to obtain a photocurable 3D printed silicon-based ceramic core.
10. The light-cured 3D printed silicon-based ceramic core obtained by the molding method according to claim 9.
Citation Information
Patent Citations
Nanometer composite ceramic core
CN104072156A
Making method of silicon-based ceramic core with adjustable thermal expansion coefficient
CN104086161A
Method used for improving residual compressive stress of laser additive manufacturing component
CN108480631A
Ceramic material for 3D light curing formation printing and preparation method of ceramic element
CN109400177A
Ceramic core slurry for 3D printing as well as preparation method and application of ceramic core slurry
CN113563059A
Cited By
Preparation method and application of 3D printing silicon-based ceramic core
CN117534451A
A preparation method and application of a 3D printed silicon-based ceramic core
CN117534451B
Photo-curing additive manufacturing-hot pressing injection composite molding preparation method of aluminum-silicon-based ceramic core
CN118989251A
Graphene enhanced photocuring 3D printing silicon-based ceramic as well as preparation method and application thereof
CN119143489A
Graphene-reinforced photocured 3D printed silicon-based ceramic and preparation method and application thereof
CN119143489B