3D printing negative electrode, preparation method thereof and sodium ion battery

The use of 3D printing technology to prepare three-dimensional mesh framework composite anode materials with high specific surface area and high active material loading solves the problem of poor electrode performance in sodium-ion batteries and improves the energy density and electrochemical performance of the batteries.

CN118943288APending Publication Date: 2024-11-12SHANGHAI XUANYI NEW ENERGY DEV CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411363257.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing sodium-ion batteries have small electrode surface areas, low active material loading, and high impedance, resulting in poor electrochemical performance.

Method used

A composite anode material comprising a periodically arranged three-dimensional mesh framework was prepared using 3D printing technology. The material is composed of transition metal elements and carbon elements. The anode with high specific surface area and high active material loading was formed by 3D printing, freeze drying and heat treatment.

Benefits of technology

It improves the energy density and electrochemical performance of sodium-ion batteries, shortens the sodium-ion diffusion path, reduces transport impedance, improves electrolyte penetration and active sites, and enhances electrode conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943288A_ABST
    Figure CN118943288A_ABST
Patent Text Reader

Abstract

The invention provides a 3D printing negative electrode, a preparation method thereof and a sodium ion battery. The 3D printing negative electrode comprises a three-dimensional net-shaped framework which is arranged periodically, the three-dimensional net-shaped framework is made of a composite negative electrode material, the composite negative electrode material comprises transition metal elements and carbon elements, and the transition metal elements are selected from one or more of elements in the VIII family. The 3D printing negative electrode provided by the invention has relatively high specific surface area and relatively large active substance loading capacity, when the 3D printing negative electrode is applied to a sodium ion battery, the transmission impedance can be reduced while the sodium ion transmission efficiency is improved, the contact between an electrolyte and a composite negative electrode material can be improved, more reaction active sites can be improved, and the service life of the sodium ion battery is prolonged. Further, the electrochemical performance of the sodium ion battery can be improved. Compared with a traditional negative electrode material, the composite negative electrode material can improve the conductivity of a 3D printing electrode, so that the electrochemical performance such as energy density of the sodium ion battery can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrode preparation methods in electrochemical energy storage, and in particular to a 3D printed negative electrode, a preparation method thereof, and a sodium ion battery. Background Art

[0002] Lithium-ion batteries have the advantages of large capacity, low self-discharge rate, and high operating voltage, and they account for about 80% of the global energy storage market. However, due to the limited reserves and high prices of lithium resources, their industrial development is severely restricted. At the same time, sodium-ion batteries with abundant reserves and low costs have shown their advantages and are expected to become a favorable supplementary energy storage device. However, the energy density of sodium-ion batteries has not yet met the requirements of rapidly developing electronic devices. Among them, increasing the loading of electrode active materials is one of the key factors to promote the further improvement of the energy density of energy storage devices.

[0003] Electrode manufacturing and assembly play an important role in promoting the performance of electrochemical energy storage devices such as sodium ion batteries. The traditional electrode manufacturing method, coating method, has limited electrode thickness in the preparation of high-load electrodes and is generally less than 100μm. As the electrode thickness increases, it will not only weaken the bonding force between the electrode material and the current collector, but also cause the blockage of ion transmission channels, thereby affecting the penetration of the electrolyte.

[0004] In recent years, 3D printing technology has been applied to various electrochemical energy storage devices. It can accurately grasp the geometry and internal structure of electrodes from the nanoscale to the macroscale. It can not only effectively break through the limitations of traditional manufacturing process technology, but also better adjust the size, porosity and morphology of the electrode, greatly enhancing the energy density and power density of the energy storage device, thereby better meeting the needs of electrochemical energy storage devices. In addition, the "additive" manufacturing nature of 3D printing can significantly simplify the manufacturing process of the electrode, improve the preparation efficiency of high-load electrodes, and show excellent controllability in terms of electrode thickness.

[0005] Although there are reports on 3D printing methods suitable for negative electrodes, the loading capacity of the 3D printed electrodes produced therefrom still needs to be improved.

[0006] On this basis, researching and developing a 3D printed negative electrode with a large specific surface area, a high active material loading and a small impedance and its preparation method are of great significance for improving the electrochemical performance of sodium ion batteries. Summary of the invention

[0007] The main purpose of the present invention is to provide a 3D printed negative electrode, a preparation method thereof and a sodium ion battery, so as to solve the problem in the prior art that the electrode has a small specific surface area, a low active material loading, and a large impedance, resulting in poor electrochemical performance.

[0008] In order to achieve the above-mentioned object, the present invention provides a 3D printed negative electrode on the one hand, which includes a three-dimensional network skeleton arranged periodically, and the material of the three-dimensional network skeleton is a composite negative electrode material, wherein the composite negative electrode material includes a transition metal element and a carbon element, and the transition metal element is selected from one or more elements in Group VIII.

[0009] Furthermore, the 3D printed negative electrode is disc-shaped or square-shaped.

[0010] Furthermore, the 3D printed negative electrode is disc-shaped, with a bottom diameter of 0.3 to 1.3 cm and a thickness of 0.35 to 1.8 mm.

[0011] Furthermore, the three-dimensional network skeleton includes a plurality of skeleton layers stacked in sequence, each skeleton layer is composed of a plurality of linear skeletons arranged in parallel, and the extension directions of the linear skeletons in two adjacent skeleton layers are different; preferably, the three-dimensional network skeleton includes 2 to 12 skeleton layers stacked in sequence, more preferably an even number of layers.

[0012] Furthermore, in each skeleton layer, the distance between two adjacent linear skeletons is 120 to 1200 μm.

[0013] Furthermore, a grid structure is formed between two adjacent skeleton layers, and the grid area in the grid structure is 0.0144-1.44 mm 2 ; Further preferably, the shape of the grid is rectangular, square or rhombus, most preferably rectangular, and its width is 120 to 1200 μm.

[0014] Furthermore, the transition metal element is selected from one or more of the group consisting of Fe, Co and Ni.

[0015] Furthermore, in the composite negative electrode material, the weight ratio of transition metal elements to carbon elements is (4-8):(2-6).

[0016] Furthermore, in the composite negative electrode material, the weight percentage of the transition metal element is 40 to 80 wt %.

[0017] Furthermore, the active material surface loading of the 3D printed electrode is 50-220 mg / cm 2 , with a specific surface area of ​​300-400m 2 / g.

[0018] In order to achieve the above-mentioned purpose, another aspect of the present invention also provides a method for preparing the above-mentioned 3D printed negative electrode provided by the present application, and the preparation method comprises: step S1, designing a printing model according to the size and shape of the target device, and importing it into a 3D printing device, and setting 3D printing parameters; step S2, mixing a composite negative electrode material precursor, a binder and a dispersant to obtain a 3D printing slurry; step S3, loading the 3D printing slurry into a 3D printing device, and performing 3D printing according to the 3D printing parameters to obtain a 3D printed product; step S4, freeze-drying the 3D printed product to obtain a freeze-dried product; step S5, heat-treating the freeze-dried product in an inert atmosphere to obtain a 3D printed negative electrode.

[0019] Furthermore, the shape of the 3D printed negative electrode is disc-shaped, and the 3D printing parameters include: the bottom diameter of the 3D printed negative electrode is 0.3-1.3 cm, the number of layers is 2-12 layers, the propulsion gas pressure is 0.2-0.6 MPa, the printing speed is 0.5-2 mm / s, and the printing needle diameter is 250-600 μm.

[0020] Furthermore, the preparation process of the composite negative electrode material precursor in step S2 includes: step S2-1, mixing the transition metal source, the carbon source and the solvent and performing a hydrothermal reaction or a static treatment to obtain a product system containing the precursor; step S2-2, centrifuging the product system to obtain a solid phase product; step S2-3, vacuum drying the solid phase product to obtain a composite negative electrode material precursor.

[0021] Furthermore, the weight ratio of the transition metal source, the carbon source and the solvent is (1-15):(5-70):(994-915).

[0022] Furthermore, the transition metal source is selected from one or more of the group consisting of cobalt salts, iron salts, and nickel salts; more preferably, the cobalt salt is selected from one or more of the group consisting of cobalt nitrate, cobalt chloride, and cobalt acetate; the iron salt is selected from one or more of the group consisting of ferric nitrate, ferric chloride, and ferric sulfate; the nickel salt is selected from one or more of the group consisting of nickel nitrate, nickel chloride, and nickel sulfate.

[0023] Furthermore, the carbon source is selected from one or more of the group consisting of 2-methylimidazole, fumaric acid, urea, phthalic acid, and polyvinyl pyrrolidone.

[0024] Furthermore, the solvent is selected from one or more of the group consisting of water, N,N-dimethylformamide, methanol, ethanol, and tetrahydrofuran.

[0025] Furthermore, the temperature of the hydrothermal reaction is 100-180° C., and the time is 4-12 hours.

[0026] Furthermore, the temperature of the static treatment is 20 to 30° C., and the time is 2 to 10 hours.

[0027] Furthermore, the rotation speed of the centrifugal treatment is 3000-10000 rpm, and the time is 3-10 min.

[0028] Furthermore, the temperature of the vacuum drying treatment is 60-100° C., the time is 600-960 min, and the vacuum degree is 80-100 kPa.

[0029] Furthermore, the weight ratio of the composite negative electrode material precursor, the binder and the dispersant is (3-5):(2-3):(3-4).

[0030] Furthermore, the binder is selected from one or more of the group consisting of polyether ketone, sodium carboxymethyl cellulose, styrene-butadiene rubber, sodium alginate, and polyacrylic acid.

[0031] Furthermore, the dispersant is selected from water and / or N,N-dimethylformamide.

[0032] Furthermore, step S2 includes: mixing the composite negative electrode material precursor, the binder and the dispersant, and obtaining a 3D printing slurry after degassing.

[0033] Furthermore, the degassing treatment is carried out in a degassing device, which includes a staged degassing process, preferably a four-stage degassing treatment, wherein the degassing speed of the first stage is 700-900rpm, and the time is 2-5min, the degassing speed of the second stage is 1800-2400rpm, and the time is 3-12min, the degassing speed of the third stage is 600-1000rpm, and the time is 2-5min, and the degassing speed of the fourth stage is 1800-2600rpm, and the time is 0.25-5min.

[0034] Furthermore, the freeze-drying treatment is carried out at a temperature of -50 to -30°C and for a time of 48 to 72 hours.

[0035] Furthermore, the heat treatment temperature is 500-900° C., and the time is 1-12 hours.

[0036] Furthermore, the inert atmosphere is selected from one or more of the group consisting of nitrogen, argon, and a mixture of argon and hydrogen; more preferably, the inert atmosphere is a mixture of argon and hydrogen, and the volume ratio of argon to hydrogen in the mixture is 90:10.

[0037] Another aspect of the present invention provides a sodium ion battery, comprising a positive electrode, a negative electrode, an electrolyte, and a separator arranged between the positive electrode and the negative electrode, wherein the negative electrode is the above-mentioned 3D printed negative electrode provided in the present application.

[0038] By applying the technical solution of the present invention, the above-mentioned 3D printed negative electrode provided in the present application includes a three-dimensional mesh skeleton arranged periodically, which has a high specific surface area and a large active material loading amount. When it is applied to a sodium ion battery, on the one hand, it can shorten the sodium ion diffusion path, while improving the sodium ion transmission efficiency and reducing the transmission impedance. On the other hand, it can improve the contact between the electrolyte and the composite negative electrode material, and improve the penetration of the electrolyte in the 3D printed negative electrode, thereby increasing more reaction active sites, and further improving the electrochemical properties of the sodium ion battery, such as the energy density.

[0039] The material of the three-dimensional network skeleton in the present application is a composite negative electrode material. Compared with traditional negative electrode materials, the composite negative electrode material in the present application includes specific types of transition metal elements and carbon elements, which can improve the conductivity of the 3D printed electrode, thereby improving the electrochemical properties of the sodium ion battery, such as the energy density. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0041] Figure 1 The printed model introduced into the 3D printer in Example 1 of the present application is shown;

[0042] Figure 2 A scanning electron microscope image (SEM image) of the 3D printed negative electrode prepared in Example 1 of the present application is shown;

[0043] Figure 3 The nitrogen adsorption and desorption curve of the 3D printed negative electrode prepared in Example 1 of the present application is shown;

[0044] Figure 4 A cyclic charge and discharge curve of a sodium ion battery assembled using the 3D printed negative electrode prepared in Example 1 of the present application is shown. DETAILED DESCRIPTION

[0045] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0046] As described in the background technology, the existing electrodes have small specific surface area, low active material loading, and large impedance, resulting in poor electrochemical performance. In order to solve the above technical problems, the first aspect of the present application provides a 3D printed negative electrode, which includes a three-dimensional mesh skeleton arranged periodically, and the material of the three-dimensional mesh skeleton is a composite negative electrode material, wherein the composite negative electrode material includes a transition metal element and a carbon element, and the transition metal element is selected from one or more elements in Group VIII.

[0047] The above-mentioned 3D printed negative electrode provided in the present application includes a three-dimensional mesh skeleton arranged in a periodic manner, which has a high specific surface area and a large active material loading amount. When it is applied to a sodium ion battery, on the one hand, it can shorten the sodium ion diffusion path, while improving the sodium ion transmission efficiency and reducing the transmission impedance. On the other hand, it can improve the contact between the electrolyte and the composite negative electrode material, and improve the penetration of the electrolyte in the 3D printed negative electrode, thereby increasing more reaction active sites, and further improving the electrochemical properties of the sodium ion battery, such as the energy density.

[0048] The material of the three-dimensional network skeleton in the present application is a composite negative electrode material. Compared with traditional negative electrode materials, the composite negative electrode material in the present application includes specific types of transition metal elements and carbon elements, which can improve the conductivity of the 3D printed electrode, thereby improving the electrochemical properties of the sodium ion battery, such as the energy density.

[0049] The shape and size of the 3D printed negative electrode can be adaptively adjusted according to the type of target device. In a preferred embodiment, the 3D printed negative electrode is disc-shaped or square-shaped.

[0050] In a preferred embodiment, the 3D printed negative electrode is disc-shaped, with a bottom diameter of 0.3 to 1.3 cm and a thickness of 0.35 to 1.8 mm. When the 3D printed negative electrode is disc-shaped, its bottom diameter and thickness include but are not limited to the above ranges, and limiting it within the above ranges is beneficial to reducing its own weight while increasing energy density, thereby facilitating improving the electrochemical specific capacity of the sodium ion battery.

[0051] In a preferred embodiment, the three-dimensional mesh skeleton includes a plurality of skeleton layers stacked in sequence, each skeleton layer is composed of a plurality of linear skeletons arranged in parallel, and the extension directions of the linear skeletons in two adjacent skeleton layers are different. The use of the above-mentioned skeleton layer structure is conducive to improving the specific surface area and porosity of the 3D printed negative electrode, thereby shortening the sodium ion diffusion path, improving the sodium ion transmission efficiency, and also improving the conductivity of the 3D printed negative electrode, thereby improving the electrochemical properties such as the energy density of the sodium ion battery. Preferably, the three-dimensional mesh skeleton includes 2 to 12 layers of skeleton layers stacked in sequence, more preferably an even number of layers.

[0052] In order to further increase the specific surface area and porosity of the 3D printed negative electrode, further shorten the sodium ion diffusion path, further improve the conductivity of the 3D printed negative electrode, and thus further improve the electrochemical properties such as the energy density of the sodium ion battery, preferably, in each skeleton layer, the distance between two adjacent linear skeletons is 120 to 1200 μm.

[0053] It should be noted that in the same skeleton layer, the distance between two adjacent linear skeletons is related to the diameter of the printing needle used in the 3D printing device. The diameter of the needle in the 3D printing device includes but is not limited to 150μm, 200μm, 250μm, 400μm, 600μm, 850μm, 1200μm; preferably 250μm, 400μm, 600μm. When a needle with a diameter of 400μm is selected, the distance between two adjacent linear skeletons is 200-800μm, that is, half of the needle diameter to twice the needle diameter.

[0054] In a preferred embodiment, a grid structure is formed between two adjacent skeleton layers, and the grid area in the grid structure is 0.0144-1.44 mm 2 Compared with other settings, limiting the structure and mesh area formed by two adjacent skeleton layers within the above range is conducive to increasing the specific surface area and porosity of the 3D printed negative electrode, shortening the sodium ion diffusion path, and increasing the active material loading of the 3D printed negative electrode, thereby reducing its own weight while increasing its energy density, and further improving the electrochemical properties of the sodium ion battery, such as the energy density.

[0055] In order to further increase the specific surface area and porosity of the 3D printed negative electrode, further shorten the sodium ion diffusion path, further increase the active material loading of the 3D printed negative electrode, and thus further improve the electrochemical properties such as the energy density of the sodium ion battery, preferably, the shape of the grid is rectangular, square or diamond, most preferably rectangular, and its width is 120 to 1200 μm.

[0056] In a preferred embodiment, the transition metal element includes but is not limited to one or more of the group consisting of Fe, Co, and Ni. Compared with other types, the use of the above-mentioned types of transition metal elements is conducive to promoting the realization of the "space charge storage" mechanism, thereby improving the structural stability of the 3D printed negative electrode during the cyclic discharge process.

[0057] In order to further improve the electrical conductivity of the 3D printed electrode and better utilize the electrochemical capacity of the transition metal element, preferably, in the composite negative electrode material precursor, the weight ratio of the transition metal element to the carbon element is (4-8):(2-6).

[0058] In order to further improve the conductivity of the 3D printed electrode and better exert the electrochemical capacity of the transition metal elements, preferably, the weight percentage of the transition metal elements in the composite negative electrode material precursor is 40 to 80 wt%.

[0059] The 3D printed electrode provided in the present application has a larger active material surface loading and specific surface area than the traditional electrode. In a preferred embodiment, the active material surface loading of the 3D printed electrode is 50-220 mg / cm 2 , with a specific surface area of ​​300-400m 2 / g.

[0060] The second aspect of the present application also provides a method for preparing the above-mentioned 3D printed negative electrode provided by the present application, and the preparation method includes: step S1, designing a printing model according to the size and shape of the target device, and importing it into a 3D printing device, and setting 3D printing parameters; step S2, mixing a composite negative electrode material precursor, a binder and a dispersant to obtain a 3D printing slurry; step S3, loading the 3D printing slurry into the 3D printing device, and performing 3D printing according to the 3D printing parameters to obtain a 3D printed product; step S4, freeze-drying the 3D printed product to obtain a freeze-dried product; step S5, heat-treating the freeze-dried product in an inert atmosphere to obtain a 3D printed negative electrode.

[0061] The present application adopts 3D printing technology, which is convenient for controlling the morphology and structure of the negative electrode at the microscopic and macroscopic scales. According to the size of the target device, the printing model is designed and the 3D printing parameters are set to facilitate the subsequent preparation of a 3D printed negative electrode with a specific morphology and structure, so that the skeleton therein is arranged periodically, thereby forming a three-dimensional network skeleton structure arranged periodically. The 3D printing slurry used in the present application includes a composite negative electrode material precursor, a binder and a dispersant. The 3D printed product obtained after 3D printing with the 3D printing slurry is freeze-dried to remove the dispersant while exerting its pore-forming effect. After the subsequent heat treatment process, the binder sublimates at high temperature to further exert its pore-forming effect. At the same time, the negative electrode composite material precursor is heated to carbonize and reduced in an inert atmosphere to generate single particles of transition metals, thereby forming a composite negative electrode material containing carbon elements and transition metal elements, and forming a three-dimensional network skeleton. The 3D printed negative electrode prepared by the above preparation method has a high specific surface area and a large active material loading. When it is applied to sodium ion batteries, on the one hand, it can shorten the sodium ion diffusion path, improve the sodium ion transmission efficiency and reduce the transmission impedance; on the other hand, it can improve the contact between the electrolyte and the composite negative electrode material, and improve the penetration of the electrolyte in the 3D printed negative electrode, thereby increasing more reaction active sites, and further improving the electrochemical properties of the sodium ion battery, such as the energy density.

[0062] Moreover, compared with traditional negative electrode materials, the above-mentioned composite negative electrode material in the present application includes specific types of transition metal elements and carbon elements, which can improve the conductivity of the 3D printed electrode, thereby improving the electrochemical properties such as the energy density of the sodium ion battery.

[0063] In addition, the above-mentioned 3D printed negative electrode preparation method provided in the present application has a simple process flow and can improve the preparation efficiency of 3D printed electrodes.

[0064] In a preferred embodiment, the shape of the 3D printed negative electrode is disc-shaped, and the 3D printing parameters include: the bottom diameter of the 3D printed negative electrode is 0.3-1.3 cm, the number of layers is 2-12 layers, the propulsion pressure is 0.2-0.6 MPa, the printing speed is 0.5-2 mm / s, and the printing needle diameter is 250-600 μm. The 3D printing parameters include but are not limited to the above ranges. Limiting them within the above ranges is conducive to controlling the morphology and structure of the negative electrode at the microscopic and macroscopic scales, and is conducive to forming a three-dimensional network skeleton structure with a periodic arrangement, thereby facilitating the improvement of the specific surface area and active material loading of the 3D printed negative electrode, thereby facilitating the shortening of the sodium ion diffusion path, improving the sodium ion transmission efficiency, and reducing the transmission impedance. At the same time, it is also conducive to improving the contact between the electrolyte and the composite negative electrode material, and is conducive to improving the penetration of the electrolyte in the 3D printed negative electrode, thereby facilitating the improvement of the electrochemical properties such as the energy density of the sodium ion battery.

[0065] In a preferred embodiment, the preparation process of the composite negative electrode material precursor in step S2 includes: step S2-1, mixing the transition metal source, the carbon source and the solvent and performing a hydrothermal reaction or a static treatment to obtain a product system containing the precursor; step S2-2, centrifuging the product system to obtain a solid phase product; step S2-3, vacuum drying the solid phase product to obtain a composite negative electrode material precursor. The hydrothermal reaction or static treatment can make the transition metal source and the carbon source grow to form a precursor to obtain a product system containing the precursor, and then the product system is centrifuged to separate the solid phase product, and the solid phase product is vacuum dried to remove the residual solvent therein to obtain a composite negative electrode material precursor.

[0066] In order to better exert the electrochemical performance of the subsequently prepared composite negative electrode material, preferably, the weight ratio of the transition metal source, the carbon source and the solvent is (1-15):(5-70):(994-915).

[0067] In a preferred embodiment, the transition metal source includes but is not limited to one or more of the group consisting of cobalt salts, iron salts, and nickel salts. Compared with other types, the use of the above types of salts as transition metal sources is conducive to promoting the realization of the "space charge storage" mechanism, thereby improving the structural stability of the electrode during the cyclic discharge process.

[0068] In order to further improve the success and controllability of the preparation of transition metal element particles, preferably, cobalt salts include but are not limited to one or more of the group consisting of cobalt nitrate, cobalt chloride, and cobalt acetate; iron salts include but are not limited to one or more of the group consisting of ferric nitrate, ferric chloride, and ferric sulfate; nickel salts include but are not limited to one or more of the group consisting of nickel nitrate, nickel chloride, and nickel sulfate.

[0069] The carbon source of the present application adopts an organic carbon source, and its type is not particularly limited, as long as it can be carbonized during the subsequent heat treatment and doped and coated with transition metal elements. In a preferred embodiment, the carbon source is one or more of the group consisting of but not limited to 2-methylimidazole, fumaric acid, urea, phthalic acid, and polyvinyl pyrrolidone.

[0070] In a preferred embodiment, the solvent includes but is not limited to one or more of the group consisting of water, N,N-dimethylformamide, methanol, ethanol, and tetrahydrofuran. Compared with other types, the use of the above types of solvents is conducive to improving the dispersibility and compatibility of the transition metal source and the carbon source, and is convenient for subsequent processing.

[0071] In order to improve the generation rate of the precursor, and thus improve the generation rate of the composite negative electrode material precursor prepared subsequently, preferably, the temperature of the hydrothermal reaction is 100 to 180° C., and the time is 4 to 12 hours.

[0072] In order to improve the generation rate of the precursor, and thus improve the generation rate of the composite negative electrode material precursor prepared subsequently, preferably, the temperature of the static treatment is 20 to 30° C., and the time is 2 to 10 hours.

[0073] In a preferred embodiment, the speed of the centrifugal treatment is 3000-10000 rpm, and the time is 3-10 min. The speed and time of the centrifugal treatment include but are not limited to the above ranges, and limiting them within the above ranges is conducive to improving the separation and treatment efficiency of the product system, thereby helping to improve the purity of the solid phase product.

[0074] In a preferred embodiment, the temperature of the vacuum drying treatment is 60-100°C, the time is 600-960 min, and the vacuum degree is 80-100 kPa. The temperature, time and vacuum degree of the vacuum drying treatment include but are not limited to the above ranges, and limiting them within the above ranges is conducive to improving the removal rate of residual solvents in the solid phase product, thereby facilitating better performance of the electrochemical performance of the composite negative electrode material.

[0075] In a preferred embodiment, the weight ratio of the composite negative electrode material precursor, the binder and the dispersant is (3-5): (2-3): (3-4). The weight ratio of the composite negative electrode material precursor, the binder and the dispersant includes but is not limited to the above range. Limiting it to the above range is conducive to improving the processability of the 3D printing slurry and facilitating subsequent 3D printing.

[0076] In order to improve the bonding performance between the composite negative electrode materials, preferably, the binder includes but is not limited to one or more of the group consisting of polyoxyethylene polyoxypropylene ether (Fluronic F127), sodium carboxymethyl cellulose, styrene-butadiene rubber, sodium alginate, and polyacrylic acid. More preferably, the viscosity of polyoxyethylene polyoxypropylene ether is 800-2000 mPa·s, the viscosity of sodium carboxymethyl cellulose is 1000-3100 mPa·s, the weight average molecular weight of styrene-butadiene rubber is 6000-8800, the viscosity of sodium alginate is 180-220 mPa·s, and the weight average molecular weight of polyacrylic acid is 3 million-4.5 million.

[0077] In a preferred embodiment, the dispersant includes but is not limited to water and / or N,N-dimethylformamide. Compared with other types, the use of the above-mentioned dispersants is conducive to improving the compatibility of the composite negative electrode material, thereby improving the processing performance and facilitating subsequent 3D printing.

[0078] The degassing treatment can remove bubbles generated during the mixing process and reduce the bubble content in the 3D printed product. In a preferred embodiment, step S2 includes: mixing the composite negative electrode material precursor, the binder and the dispersant, and obtaining the 3D printing slurry after degassing treatment.

[0079] In order to improve the degassing treatment effect and further reduce the bubbles in the 3D printed product, preferably, the degassing treatment is carried out in a degassing device, which includes a staged degassing process, preferably a four-stage degassing treatment, wherein the degassing speed of the first stage is 700-900 rpm, and the time is 2-5 min, the degassing speed of the second stage is 1800-2400 rpm, and the time is 3-12 min, the degassing speed of the third stage is 600-1000 rpm, and the time is 2-5 min, and the degassing speed of the fourth stage is 1800-2600 rpm, and the time is 0.25-5 min.

[0080] In a preferred embodiment, the freeze-drying treatment temperature is -50 to -30°C and the time is 48 to 72 hours. The freeze-drying treatment temperature and time include but are not limited to the above ranges, and limiting them within the above ranges is conducive to better play its role in removing dispersants and forming pores.

[0081] In a preferred embodiment, the heat treatment temperature is 500-900°C and the time is 1-12 hours. The heat treatment temperature and time include but are not limited to the above ranges, and limiting them within the above ranges is conducive to improving the carbonization efficiency of the binder, thereby forming a composite negative electrode material containing carbon elements and forming a three-dimensional network skeleton.

[0082] In order to improve the heat treatment effect and reduce the introduction of impurities, preferably, the inert atmosphere includes but is not limited to one or more of the group consisting of nitrogen, argon, and a mixture of argon and hydrogen. More preferably, the inert atmosphere is a mixture of argon and hydrogen, and the volume ratio of argon to hydrogen in the mixture is 90:10.

[0083] The third aspect of the present application also provides a sodium ion battery, including a positive electrode, a negative electrode, an electrolyte and a separator arranged between the positive electrode and the negative electrode, and the negative electrode is the above-mentioned 3D printed negative electrode provided by the present application. The above-mentioned 3D printed negative electrode provided by the present application has a high specific surface area and a large active material loading amount. When it is applied to a sodium ion battery, on the one hand, it can shorten the sodium ion diffusion path, while improving the sodium ion transmission efficiency and reducing the transmission impedance. On the other hand, it can improve the contact between the electrolyte and the composite negative electrode material, and improve the penetration of the electrolyte in the 3D printed negative electrode, so as to increase more reactive active sites, and then improve the energy density and other electrochemical properties of the sodium ion battery. Moreover, compared with traditional negative electrode materials, the above-mentioned 3D printed electrode provided by the present application has a high conductivity, which can improve the energy density and other electrochemical properties of the sodium ion battery.

[0084] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0085] It should be noted that the 3D printed negative electrode prepared in all the embodiments and comparative examples of the present application is assembled into a sodium ion battery. The assembly process of the sodium ion battery is as follows: a CR-2032 stainless steel button battery shell is used to assemble the sodium ion battery in an anhydrous, oxygen-free (water, oxygen content ≤ 0.01ppm) argon-protected glove box, and the positive electrode shell, 3D printed negative electrode, diaphragm, sodium sheet, gasket, and negative electrode shell are assembled in order, and an electrolyte (1.0mol / L NaClO4, EC:DMC=1:1, and an additive of 5% FEC) is injected between the 3D printed negative electrode and the sodium sheet, and the device is sealed at a pressure not higher than 0.5MPa to obtain a sodium ion battery.

[0086] The performance tests in this application include:

[0087] (1) The specific surface area of ​​the 3D printed negative electrodes prepared in all the embodiments and comparative examples of the present application was tested by nitrogen adsorption-desorption method;

[0088] (2) The performance characteristics of the sample materials were evaluated using the ASAP2020 adsorption analyzer from Micromeritics, USA, with a degassing temperature of 300 °C and an operating temperature of 77 K;

[0089] (3) The resistance of the 3D printed negative electrode prepared in this application was tested by AC impedance. The impedance test of the assembled device was performed using an IVIUMn STAT electrochemical workstation of Ivium Technologies BV of the Netherlands. The voltage was the open circuit voltage and the frequency range was 0.01 to 100,000 Hz.

[0090] (4) at 0.05 mA / cm 2 The electrochemical performance of the sodium ion battery was tested at a current density of 0.05 mA / cm 2 The sodium ion battery is subjected to a cycle stability test at a current density of 0.01 to 3.0 V, and the discharge area specific capacity after 30 cycles is tested, and the capacity retention rate is calculated. Among them, the assembled button battery is discharged at a constant current (to obtain the first cycle discharge capacity), and the battery is fully charged with the same current. In this process, a solid electrolyte membrane is mainly formed, resulting in irreversible capacity loss, and then the battery is still discharged at the same constant current, while recording the discharge capacity, i.e., the second cycle discharge capacity. The capacity retention rate in this application refers to: the percentage of the discharge capacity of the sodium ion battery after 30 cycles of charge and discharge to the second cycle discharge capacity.

[0091] The test results of the above items are shown in Table 1.

[0092] Example 1

[0093] A method for preparing a 3D printed negative electrode, comprising:

[0094] (1) 13.14 g of 2-methylimidazole was dissolved in 400 mL of deionized water to obtain solution A, and 2.91 g of Co(NO3)2·6H2O was dissolved in 400 mL of deionized water to obtain solution B. After the two solutions were fully dissolved, solution A was quickly poured into solution B, and stirred at room temperature for 30 min to obtain a purple mixed solution. After standing at room temperature for 4 h, a product system containing the precursor was obtained;

[0095] (2) centrifuging the product system obtained in step (1) three times to obtain a solid phase product; wherein the centrifugal speed is 6000 rpm and the time is 3 min;

[0096] (3) vacuum drying the solid phase product obtained in step (2) at 80° C. for 12 h to obtain a purple solid powder, which is a composite negative electrode material precursor;

[0097] (4) Mixing the composite negative electrode material precursor, binder F127 and deionized water prepared in step (3) in a weight ratio of 40:25:35, and performing degassing treatment in a degassing machine to obtain a 3D printing slurry; wherein the degassing treatment includes 4 stages, the degassing speed of the first stage is 800 rpm, the degassing speed of the second stage is 2000 rpm, the degassing speed of the third stage is 800 rpm, and the degassing speed of the fourth stage is 2200 rpm, and the treatment time of the 4 stages is 4 min;

[0098] (5) The 3D printing slurry prepared in step (4) is transferred to the printing needle, and the needle is designed according to the size of the target device (the bottom diameter of the CR-2032 button battery is 20 mm and the thickness is 3.2 mm). Figure 1 The printed model shown in the figure was imported into a 3D printer (Bio-Architect@SR, Hangzhou GeneFluid Biotechnology Co., Ltd.), and the 3D printing parameters were set for 3D printing to obtain a 3D printed product, wherein the shape of the 3D printed negative electrode was set to be disc-shaped, the diameter of the 3D printed negative electrode was set to be 1 cm, the number of layers was set to 4, the propulsion pressure was set to 0.6 MPa, the printing speed was set to be 1 mm / s, and the diameter of the printing needle was set to be 400 μm;

[0099] (6) freeze-drying the 3D printed product obtained in step (5) to obtain a freeze-dried product; wherein the freeze-drying temperature is -40°C and the time is 48 hours;

[0100] (7) The freeze-dried product was placed in a porcelain boat and placed in a high-temperature tube furnace with an argon atmosphere for heat treatment. The temperature was raised to 700°C at a heating rate of 2°C / min and kept at this temperature for 2 hours to obtain a 3D printed negative electrode.

[0101] After measurement, the 3D printed negative electrode obtained in Example 1 is disc-shaped, with a bottom diameter of 0.5 cm and a thickness of 0.6 mm. Figure 2 As shown, the 3D printed negative electrode prepared in Example 1 includes a three-dimensional mesh skeleton arranged periodically. Figure 1 It can be seen that the three-dimensional mesh skeleton includes multiple skeleton layers stacked in sequence, each skeleton layer is composed of multiple parallel linear skeletons, and the extension directions of the linear skeletons in two adjacent skeleton layers are perpendicular to each other. In each skeleton layer, the distance between two adjacent linear skeletons is about 300μm, and a mesh structure is formed between two adjacent skeleton layers, and the mesh area in the mesh structure is 0.04-0.64mm 2 ,The shape of the grid is rectangular, and its width is about 250 μm.

[0102] Depend on Figure 3 It can be obtained that the specific surface area of ​​the 3D printed negative electrode prepared in Example 1 is 338.1m2 / g.

[0103] Depend on Figure 4 The first cycle discharge area specific capacity of the sodium ion battery is 19.9 mAh / cm 2 , the charge area specific capacity is 12.7mAh / cm 2 .

[0104] Example 2

[0105] The difference from Example 1 is that in step (5), the number of layers of the 3D printer is set to 2.

[0106] The thickness of the prepared 3D printed negative electrode is 0.35 mm.

[0107] Example 3

[0108] The difference from Example 1 is that in step (5), the number of layers of the 3D printer is set to 6.

[0109] The thickness of the prepared 3D printed negative electrode is 0.9 mm.

[0110] Example 4

[0111] The difference from Example 1 is that in step (5), the number of layers of the 3D printer is set to 8.

[0112] The thickness of the prepared 3D printed negative electrode is 1.2 mm.

[0113] Example 5

[0114] The difference from Example 1 is that in step (5), the number of layers of the 3D printer is set to 12 layers.

[0115] The thickness of the prepared 3D printed negative electrode is 1.8 mm.

[0116] Example 6

[0117] The difference from Example 1 is that in step (5), the number of layers of the 3D printer is set to 14 layers.

[0118] The thickness of the prepared 3D printed negative electrode is 2.1 mm.

[0119] Example 7

[0120] The difference from Example 1 is that in step (5), the diameter of the printing needle of the 3D printer is 250 μm.

[0121] The mesh area in the mesh structure is 0.0144~0.25mm 2 ,The shape of the grid is rectangular, and its width is about 140μm.

[0122] Example 8

[0123] The difference from Example 1 is that in step (5), the diameter of the printing needle of the 3D printer is 600 μm.

[0124] The mesh area in the mesh structure is 0.09 to 1.44 mm 2 ,The shape of the grid is rectangular, and its width is about 380μm.

[0125] Example 9

[0126] The difference from Example 1 is that in step (5), the diameter of the printing needle of the 3D printer is 1200 μm.

[0127] The mesh area in the mesh structure is 0.02 to 0.03 mm 2 ,The shape of the grid is rectangular, and its width is about 800μm.

[0128] Example 10

[0129] The difference from Example 1 is that in step (1), the weight ratio of Co(NO3)2·6H2O, 2-methylimidazole and deionized water is 1:5:994.

[0130] The prepared 3D printed negative electrode includes a three-dimensional network skeleton arranged in a periodic manner. The material of the three-dimensional network skeleton is a composite negative electrode material. The weight ratio of cobalt element to carbon element in the composite negative electrode material is 2:8.

[0131] Embodiment 11

[0132] The difference from Example 1 is that in step (1), the weight ratio of Co(NO3)2·6H2O, 2-methylimidazole and deionized water is 15:70:915.

[0133] The prepared 3D printed negative electrode includes a three-dimensional network skeleton arranged in a periodic manner. The material of the three-dimensional network skeleton is a composite negative electrode material. The weight ratio of cobalt element to carbon element in the composite negative electrode material is 6:4.

[0134] Example 12

[0135] The difference from Example 1 is that in step (1), the weight ratio of Co(NO3)2·6H2O, 2-methylimidazole and deionized water is 45:225:730.

[0136] The prepared 3D printed negative electrode includes a three-dimensional network skeleton arranged in a periodic manner. The material of the three-dimensional network skeleton is a composite negative electrode material. The weight ratio of cobalt element to carbon element in the composite negative electrode material is 91:1.

[0137] Example 13

[0138] The difference from Example 1 is that in step (1), the static treatment time is 2 hours.

[0139] Embodiment 14

[0140] The difference from Example 1 is that in step (1), the static treatment time is 10 hours.

[0141] Embodiment 15

[0142] The difference from Example 1 is that in step (1), the static treatment time is 1 hour.

[0143] Example 16

[0144] The difference from Example 1 is that in step (1), the static treatment is changed to a hydrothermal reaction, and the temperature of the hydrothermal reaction is 100° C. and the time is 12 h.

[0145] Embodiment 17

[0146] The difference from Example 1 is that in step (1), the static treatment is changed to a hydrothermal reaction, and the temperature of the hydrothermal reaction is 180° C. and the time is 4 hours.

[0147] Embodiment 18

[0148] The difference from Example 1 is that in step (1), the static treatment is changed to a hydrothermal reaction, and the temperature of the hydrothermal reaction is 200° C. and the time is 1 hour.

[0149] Embodiment 19

[0150] The difference from Example 1 is that in step (4), the weight ratio of the composite negative electrode material precursor, the binder F127 and the deionized water is 5:2:3.

[0151] Embodiment 20

[0152] The difference from Example 1 is that in step (4), the weight ratio of the composite negative electrode material precursor, the binder F127 and the deionized water is 3:3:4.

[0153] Embodiment 21

[0154] The difference from Example 1 is that in step (4), the weight ratio of the composite negative electrode material precursor, the binder F127 and the deionized water is 2:4:4.

[0155] Embodiment 22

[0156] The difference from Example 1 is that the freeze-drying treatment temperature in step (6) is -30°C and the time is 72 hours.

[0157] Embodiment 23

[0158] The difference from Example 1 is that the temperature of the freeze-drying treatment in step (6) is -50°C.

[0159] Embodiment 24

[0160] The difference from Example 1 is that the heat treatment temperature in step (7) is 500° C. and the time is 12 h.

[0161] Embodiment 25

[0162] The difference from Example 1 is that the heat treatment temperature in step (7) is 900° C. and the time is 1 hour.

[0163] Embodiment 26

[0164] The difference from Example 1 is that the temperature of the heat treatment in step (7) is 400°C.

[0165] Comparative Example 1

[0166] The difference from Example 1 is that a silicon-carbon negative electrode material is used to replace the composite negative electrode material in step (4), and the remaining steps are the same as Example 1.

[0167] Comparative Example 2

[0168] The difference from Example 1 is that cobalt oxide powder (Jingding Nano New Materials, KG-Co3O4-200) is used to replace the composite negative electrode material precursor in step (3), and the remaining steps are the same as Example 1.

[0169] Comparative Example 3

[0170] The difference from Example 1 is that step (6) is omitted, that is, freeze-drying is not performed, and the 3D printed product obtained in step (5) is directly heat-treated, and the remaining steps are the same as in Example 1.

[0171] Table 1

[0172]

[0173]

[0174] From the above description, it can be seen that the above-mentioned embodiments of the present invention achieve the following technical effects: the above-mentioned 3D printed negative electrode provided by the present application includes a three-dimensional mesh skeleton arranged periodically, which has a high specific surface area and a large active material loading amount. When it is applied to a sodium ion battery, on the one hand, it can shorten the sodium ion diffusion path, while improving the sodium ion transmission efficiency and reducing the transmission impedance. On the other hand, it can improve the contact between the electrolyte and the composite negative electrode material, and improve the penetration of the electrolyte in the 3D printed negative electrode, thereby increasing more reaction active sites, and then improving the electrochemical properties of the sodium ion battery, such as the energy density.

[0175] The material of the three-dimensional network skeleton in the present application is a composite negative electrode material. Compared with traditional negative electrode materials, the composite negative electrode material in the present application includes specific types of transition metal elements and carbon elements, which can improve the conductivity of the 3D printed electrode, thereby improving the electrochemical properties of the sodium ion battery, such as the energy density.

[0176] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those described herein, for example.

[0177] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A 3D printed negative electrode, characterized in that: The 3D printed negative electrode includes a three-dimensional mesh skeleton arranged periodically, and the material of the three-dimensional mesh skeleton is a composite negative electrode material, wherein the composite negative electrode material includes a transition metal element and a carbon element, and the transition metal element is selected from one or more elements in Group VIII.

2. The 3D printed negative electrode according to claim 1, characterized in that: The 3D printed negative electrode is disc-shaped or square-shaped; Preferably, the 3D printed negative electrode is disc-shaped, with a bottom diameter of 0.3 to 1.3 cm and a thickness of 0.35 to 1.8 mm; More preferably, the three-dimensional mesh skeleton comprises a plurality of skeleton layers stacked in sequence, each of the skeleton layers is composed of a plurality of linear skeletons arranged in parallel, and the extension directions of the linear skeletons in two adjacent skeleton layers are different; preferably, the three-dimensional mesh skeleton comprises 2 to 12 layers of the skeleton layers stacked in sequence, more preferably an even number of layers; Preferably, in each skeleton layer, the distance between two adjacent linear skeletons is 120 to 1200 μm; More preferably, a grid structure is formed between two adjacent skeleton layers, and the grid area in the grid structure is 0.0144-1.44 mm 2 ; Further preferably, the shape of the grid is rectangular, square or rhombus, most preferably rectangular, and its width is 120 to 1200 μm.

3. The 3D printed negative electrode according to claim 1, characterized in that: The transition metal element is selected from one or more of the group consisting of Fe, Co, and Ni; Preferably, in the composite negative electrode material, the weight ratio of the transition metal element to the carbon element is (4-8): (2~6); Preferably, in the composite negative electrode material, the weight percentage of the transition metal element is 40-80wt%.

4. The 3D printed negative electrode according to any one of claims 1 to 3, characterized in that The active material surface loading of the 3D printed electrode is 50-220 mg / cm 2 , with a specific surface area of ​​300-400m 2 / g.

5. A method for preparing a 3D printed negative electrode according to any one of claims 1 to 3, characterized in that: The preparation method comprises: Step S1, designing a printing model according to the size and shape of the target device, importing it into a 3D printing device, and setting 3D printing parameters; Step S2, mixing a composite negative electrode material precursor, a binder and a dispersant to obtain a 3D printing slurry; Step S3, loading the 3D printing slurry into the 3D printing device, and performing 3D printing according to the 3D printing parameters to obtain a 3D printed product; Step S4, freeze-drying the 3D printed product to obtain a freeze-dried product; Step S5, heat-treating the freeze-dried product in an inert atmosphere to obtain the 3D printed negative electrode.

6. The method for preparing a 3D printed negative electrode according to claim 5, characterized in that: The shape of the 3D printed negative electrode is disc-shaped, and the 3D printing parameters include: the bottom diameter of the 3D printed negative electrode is 0.3-1.3 cm, the number of layers is 2-12 layers, the propulsion gas pressure is 0.2-0.6 MPa, the printing speed is 0.5-2 mm / s, and the printing needle diameter is 250-600 μm.

7. The method for preparing a 3D printed negative electrode according to claim 5, characterized in that: The preparation process of the composite negative electrode material precursor in step S2 includes: Step S2-1, mixing a transition metal source, a carbon source and a solvent and performing a hydrothermal reaction or a static treatment to obtain a product system containing a precursor; Step S2-2, centrifuging the product system to obtain a solid phase product; Step S2-3, vacuum drying the solid phase product to obtain the composite negative electrode material precursor; Preferably, the weight ratio of the transition metal source, the carbon source and the solvent is (1-15):(5-70): (994~915); Preferably, the transition metal source is selected from one or more of the group consisting of cobalt salts, iron salts, and nickel salts; more preferably, the cobalt salt is selected from one or more of the group consisting of cobalt nitrate, cobalt chloride, and cobalt acetate; the iron salt is selected from one or more of the group consisting of iron nitrate, iron chloride, and iron sulfate; the nickel salt is selected from one or more of the group consisting of nickel nitrate, nickel chloride, and nickel sulfate; Preferably, the carbon source is selected from one or more of the group consisting of 2-methylimidazole, fumaric acid, urea, phthalic acid, and polyvinylpyrrolidone; Preferably, the solvent is selected from one or more of the group consisting of water, N,N-dimethylformamide, methanol, ethanol, and tetrahydrofuran; Preferably, the temperature of the hydrothermal reaction is 100-180°C and the time is 4-12h; Preferably, the temperature of the static treatment is 20 to 30°C and the time is 2 to 10 hours; Preferably, the rotation speed of the centrifugal treatment is 3000-10000 rpm, and the time is 3-10 min; Preferably, the temperature of the vacuum drying treatment is 60-100° C., the time is 600-960 min, and the vacuum degree is 80-100 kPa.

8. The method for preparing a 3D printed negative electrode according to claim 5, characterized in that: The weight ratio of the composite negative electrode material precursor, the binder and the dispersant is (3-5):(2-3):(3-4); Preferably, the binder is selected from one or more of the group consisting of polyetherketone, sodium carboxymethyl cellulose, styrene-butadiene rubber, sodium alginate, and polyacrylic acid; Preferably, the dispersant is selected from water and / or N,N-dimethylformamide; Preferably, the step S2 comprises: mixing the composite negative electrode material precursor, the binder and the dispersant, and obtaining the 3D printing slurry after degassing; More preferably, the degassing treatment is carried out in a degassing device, which includes a staged degassing process, preferably a four-stage degassing treatment, wherein the degassing speed of the first stage is 700-900 rpm, and the time is 2-5 min, the degassing speed of the second stage is 1800-2400 rpm, and the time is 3-12 min, the degassing speed of the third stage is 600-1000 rpm, and the time is 2-5 min, and the degassing speed of the fourth stage is 1800-2600 rpm, and the time is 0.25-5 min.

9. The method for preparing a 3D printed negative electrode according to any one of claims 5 to 8, characterized in that: The freeze-drying treatment is performed at a temperature of -50 to -30°C for 48 to 72 hours; Preferably, the heat treatment temperature is 500-900°C and the time is 1-12h; Preferably, the inert atmosphere is selected from one or more of the group consisting of nitrogen, argon, and a mixture of argon and hydrogen; more preferably, the inert atmosphere is a mixture of argon and hydrogen, and the volume ratio of argon to hydrogen in the mixture is 90:

10.

10. A sodium ion battery, comprising a positive electrode, a negative electrode, an electrolyte, and a separator disposed between the positive electrode and the negative electrode, characterized in that: The negative electrode is a 3D printed negative electrode as described in any one of claims 1 to 4.

Citation Information

Cited By

  • Method for improving performance of 3D printed battery

    CN120184389A

  • Silicon-carbon negative electrode material based on 3D printing solid electrolyte skeleton, preparation method of silicon-carbon negative electrode material and solid-state battery

    CN120933350A

  • Method for preparing high-performance sodium-ion battery hard carbon negative electrode material through 3D printing technology