Nano-powder-based water-based green ceramic glaze ink for ink-jet printing and preparation method thereof

By using a combination of nanopowder and natural polysaccharide sodium alginate as a dispersant, the problem of organic solvent volatilization and insufficient dispersion stability in ceramic inkjet printing inks was solved, and a water-based green ceramic glaze ink with excellent performance and environmental protection was prepared. Achieving good inkjet printing performance and environmental friendliness.

CN118755311APending Publication Date: 2024-10-11SHAANXI UNIV OF SCI & TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410833262.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-05-17
Filing Date
2024-06-26
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The organic solvents in existing ceramic inkjet printing inks volatilize and burn, causing pollution. The large particle size of traditional glazes results in insufficient dispersion stability. The dispersants are toxic and harmful to the environment and human body.

Method used

Nanopowder is used as the basic raw material, polyvinylpyrrolidone and sodium alginate are used as dispersants, and a water-based green ceramic glaze ink with good dispersion is prepared through steps such as heating stirring, ultrasonic dispersion and ball milling.

Benefits of technology

The prepared ink has excellent performance, good dispersion stability, viscosity and surface tension that meet the needs of inkjet printing, is not easy to clog the nozzle, is friendly to the human body and the environment, and can be stored for a long time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755311A_ABST
    Figure CN118755311A_ABST
Patent Text Reader

Abstract

The invention relates to nano-powder-based water-based green ceramic glaze ink for ink-jet printing and a preparation method thereof, and the green ceramic glaze ink comprises the following components in percentage by mass: 5-10% of glaze composed of nano-powder and 90-95% of a mixed dispersant solution, the method comprises the following steps: step 1, mixing polyvinylpyrrolidone and sodium alginate according to mass percent, adding an obtained mixed dispersing agent into deionized water, heating and stirring until the mixed dispersing agent is completely dissolved, so as to obtain a mixed dispersing agent solution containing polyvinylpyrrolidone and sodium alginate; 2, glaze composed of nano powder is sequentially added into the mixed dispersing agent solution obtained in the step 1 according to the sequence of nano aluminum oxide, nano silicon oxide, calcium carbonate and nano chromic oxide to be mixed, after each kind of nano powder is added, stirring, ultrasonic dispersion and ball milling are conducted, standing is conducted for 0.9-1 h, then the next kind of nano powder is added, and finally glaze ink is obtained; the dispersing agent has the advantages of being good in dispersing stability and friendly to the human body and the environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ceramic inkjet printing, and in particular relates to a nano-powder-based water-based green ceramic glaze ink for inkjet printing and a preparation method thereof. Background Art

[0002] In recent years, ceramic inkjet printing technology has basically replaced traditional surface decoration processes due to a series of advantages such as high-quality patterns, printable concave and convex surfaces, and high production efficiency. However, the ceramic glaze inks currently on the market are mainly oily. Organic solvents with low surface tension and dielectric constant can help improve the dispersion and suspension stability of ceramic inks. However, organic solvents are volatile and will evaporate and burn when fired in the kiln, producing smoke or toxic gases and causing pollution. Therefore, energy-saving and environmentally friendly ceramic glaze inks are an urgent need in the current market.

[0003] Since the ink itself is water-based, it can be well combined with the water-based surface glaze on the tile without poor clarity, especially when printing thicker three-dimensional glaze, it has a good decorative effect. Water-based glaze ink is a better development direction for ceramic glaze ink in terms of both environmental protection and overall three-dimensional glaze decoration.

[0004] The patent application document with publication number CN103224727B discloses an environmentally friendly ceramic inkjet printing glaze ink and a preparation method thereof, wherein the ink contains the following components by mass percentage: 30-50% ceramic glaze, 15-25% organic solvent, 4-10% dispersant, 2-5% water reducer, 2-5% resin, 0.3-0.6% defoamer, 0.1-0.2% leveling agent, 0.1-0.2% pH adjuster, 2-5% viscosity adjuster, 0.1-0.3% preservative, and the balance is water. The patent application document with publication number CN116554730A discloses a high-stability water-based ceramic glaze ink suitable for inkjet printing and a preparation method thereof, wherein the water-based ceramic glaze ink includes the following raw materials: ceramic glaze particles, organic dispersant, and inorganic nano-dispersant.

[0005] However, the above existing technologies are all improvements on traditional glazes, and there are still difficulties to be solved in terms of glaze viscosity, surface tension, dispersion stability, etc., among which dispersion stability is an important technical difficulty. The particle size of traditional glazes is generally in the micron level, which is greatly affected by its own gravity and has insufficient dispersion stability. In addition, the selected dispersants are all toxic and harmful to the environment and human body. Summary of the invention

[0006] In order to overcome the deficiencies of the above-mentioned prior art, the purpose of the present invention is to provide a nano-powder-based water-based green ceramic glaze ink for inkjet printing and a preparation method thereof. By using nano-powder as the basic raw material, the glaze ink with excellent performance can be prepared. In addition, polyvinyl pyrrolidone and sodium alginate are used as dispersants to prepare glaze ink with good dispersibility. The present invention has the advantages of good dispersion stability and being friendly to the human body and the environment.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is:

[0008] A nano-powder-based water-based green ceramic glaze ink for inkjet printing comprises, by mass percentage, 5-10% of a glaze composed of nano-powder and 90-95% of a mixed dispersant solution.

[0009] The mixed dispersant solution comprises, by mass percentage, 1-10% of a mixed dispersant and 90-99% of deionized water, wherein the mixed dispersant comprises 70%-90% of polyvinyl pyrrolidone and 10%-30% of sodium alginate.

[0010] The glaze composed of the nanometer powder includes, by mass percentage, 50-60% of nanometer silicon oxide, 5-15% of nanometer aluminum oxide, 30-40% of calcium carbonate and 1-5% of nanometer chromium oxide.

[0011] The present invention also provides a method for preparing a nano-powder-based water-based green ceramic glaze ink for inkjet printing, comprising the following steps:

[0012] Step 1: According to the mass percentage, polyvinyl pyrrolidone: sodium alginate = (70%-90%): (10%-30%) are mixed to obtain a mixed dispersant, and the mixed dispersant is added to deionized water, and the mixed dispersant: deionized water = (1-10%): (90-99%), and heated and stirred at 50-70° C. for 5-10 minutes until the mixed dispersant is completely dissolved to obtain a mixed dispersant solution containing polyvinyl pyrrolidone and sodium alginate;

[0013] Step 2: Add the glaze composed of nano powders to the mixed dispersant solution obtained in step 1 in sequence, wherein the glaze composed of nano powders includes nano aluminum oxide, nano silicon oxide, calcium carbonate and nano chromium oxide. The glaze composed of nano powders is added to the mixed dispersant solution obtained in step 1 in the order of nano aluminum oxide, nano silicon oxide, calcium carbonate and nano chromium oxide, and mixed. Each time a nano powder is added, stirring is performed for 0.1-0.2h, ultrasonic dispersion is performed for 0.9-1h, ball milling is performed for 0.45-0.5h, and then the next nano powder is added after standing for 0.9-1h, so as to finally obtain glaze ink. In terms of mass percentage, the glaze composed of nano powders: the mixed dispersant solution obtained in step 1 = (5-10%): (90-95%).

[0014] The glaze composed of the nano powder comprises, by mass percentage, 50-60% of nano silicon oxide, 5-15% of nano aluminum oxide, 30%-40% of calcium carbonate and 1-5% of nano chromium oxide.

[0015] Compared with the prior art, the present invention has the following advantages:

[0016] (1) The raw material of the present invention is nano powder with a small particle size, and the prepared glaze ink has excellent performance, especially good dispersion stability and is not easy to clog the nozzle.

[0017] (2) The dispersant polyvinyl pyrrolidone used in the present invention has the general properties of water-soluble polymer compounds, such as colloid protection, film-forming property, adhesion, hygroscopicity, solubilization or coagulation, but its most distinctive feature, and therefore its excellent solubility and physiological compatibility, are valued by people. It is widely used in medicine, food, cosmetics and other fields closely related to people's health. The dispersant sodium alginate used in the present invention is a natural polysaccharide, which has the stability, solubility, adhesion and safety required for pharmaceutical preparation excipients, and has been widely used in the food industry and the field of medicine. Therefore, the dispersants used in the present invention are all food-grade compounds, which are friendly to the human body and the environment.

[0018] In summary, the present invention uses nanopowder as the basic raw material to prepare a glaze ink with excellent performance, and uses polyvinyl pyrrolidone and sodium alginate as dispersants to prepare a glaze ink with good dispersibility. The ink of the present invention has good quality stability, can be stored for a long time, and has good inkjet printing performance. The viscosity of the ink is 10-30mPa·s and the surface tension is 40-60mN / m. The present invention has the advantages of good dispersion stability and being friendly to the human body and the environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1It is the relationship between the viscosity, stress and shear rate of the glaze ink of the present invention; wherein the abscissa is the shear rate, and the ordinate is the shear force and viscosity.

[0020] Figure 2 It is a curve diagram of the relationship between the surface tension of the glaze ink of the present invention and time; wherein the abscissa is time and the ordinate is surface tension.

[0021] Figure 3 The figure is a graph showing the change of the ink stability index of the glaze ink of the present invention over time; wherein the horizontal axis is time and the vertical axis is the stability index.

[0022] Figure 4 It is the infrared spectrum of the glaze ink of the present invention.

[0023] Figure 5 is a scanning electron microscope photo of a fired sample of the glaze ink of the present invention, Figure 5 (a) is the magnification of 1100 times, Figure 5 (b) is the magnification of 10,000 times. DETAILED DESCRIPTION

[0024] The technical solution adopted by the present invention is further introduced below in conjunction with the accompanying drawings and embodiments.

[0025] Example 1

[0026] A nano-powder-based water-based green ceramic glaze ink for inkjet printing comprises, by mass percentage, 10% of a glaze composed of nano-powder and 90% of a mixed dispersant solution.

[0027] A method for preparing nano-powder-based water-based green ceramic glaze ink for inkjet printing comprises the following steps:

[0028] Step 1: According to the mass percentage, polyvinyl pyrrolidone: sodium alginate = 70%: 30% is mixed to obtain a mixed dispersant, and the mixed dispersant is added into deionized water, and the mixed dispersant: deionized water is 10%: 90%, and a magnetic stirrer is used to heat and stir at 70° C. for 5 minutes until the mixed dispersant is completely dissolved to obtain a mixed dispersant solution containing polyvinyl pyrrolidone and sodium alginate;

[0029] Step 2: Add the glaze composed of nanopowders to the mixed dispersant solution obtained in step 1 in sequence, wherein the glaze composed of nanopowders includes 15% nano-alumina, 50% nano-silicon oxide, 33% calcium carbonate and 2% nano-chromium oxide. The glaze composed of nanopowders is added to the mixed dispersant solution obtained in step 1 in the order of nano-alumina, nano-silicon oxide, calcium carbonate and nano-chromium oxide, and mixed. Each time a nanopowder is added, it is stirred for 0.1h using a magnetic stirrer, ultrasonically dispersed for 1h, ball milled for 0.45h, and then allowed to stand for 1h before adding the next nanopowder to finally obtain a glaze ink; in terms of mass percentage, the glaze composed of nanopowders: the mixed dispersant solution obtained in step 1 = 10%:90%.

[0030] Example 2

[0031] A nano-powder-based water-based green ceramic glaze ink for inkjet printing comprises, by mass percentage, 5% of a glaze composed of nano-powder and 95% of a mixed dispersant solution.

[0032] A method for preparing nano-powder-based water-based green ceramic glaze ink for inkjet printing comprises the following steps:

[0033] Step 1: According to the mass percentage, polyvinyl pyrrolidone: sodium alginate = 90%: 10% is mixed to obtain a mixed dispersant, and the mixed dispersant is added into deionized water, and the mixed dispersant: deionized water = 5%: 95%, and a magnetic stirrer is used to heat and stir at 50° C. for 10 minutes until the mixed dispersant is completely dissolved to obtain a mixed dispersant solution containing polyvinyl pyrrolidone and sodium alginate;

[0034] Step 2: Add the glaze composed of nanopowders to the mixed dispersant solution obtained in step 1 in sequence, wherein the glaze composed of nanopowders includes 7% nano-alumina, 54% nano-silicon oxide, 38% calcium carbonate and 1% nano-chromium oxide. The glaze composed of nanopowders is added to the mixed dispersant solution obtained in step 1 in the order of nano-alumina, nano-silicon oxide, calcium carbonate and nano-chromium oxide, and mixed. Each time a nanopowder is added, it is stirred for 0.2h using a magnetic stirrer, ultrasonically dispersed for 0.9h, ball milled for 0.5h, and then allowed to stand for 1h before adding the next nanopowder to finally obtain a glaze ink; in terms of mass percentage, the glaze composed of nanopowders: the mixed dispersant solution obtained in step 1 = 5%:95%.

[0035] Example 3

[0036] A nano-powder-based water-based green ceramic glaze ink for inkjet printing comprises, by mass percentage, 7% of a glaze composed of nano-powder and 93% of a mixed dispersant solution.

[0037] A method for preparing nano-powder-based water-based green ceramic glaze ink for inkjet printing comprises the following steps:

[0038] Step 1: According to the mass percentage, polyvinyl pyrrolidone: sodium alginate = 80%: 20% is mixed to obtain a mixed dispersant, and the mixed dispersant is added into deionized water, and the mixed dispersant: deionized water = 7%: 93%, and a magnetic stirrer is used to heat and stir at 60° C. for 7 minutes until the mixed dispersant is completely dissolved to obtain a mixed dispersant solution containing polyvinyl pyrrolidone and sodium alginate;

[0039] Step 2: Add the glaze composed of nanopowders to the mixed dispersant solution obtained in step 1 in sequence, wherein the glaze composed of nanopowders includes 12% nano-alumina, 52% nano-silicon oxide, 33% calcium carbonate and 3% nano-chromium oxide. The glaze composed of nanopowders is added to the mixed dispersant solution obtained in step 1 in the order of nano-alumina, nano-silicon oxide, calcium carbonate and nano-chromium oxide, and mixed. Each time a nanopowder is added, it is stirred for 0.2h using a magnetic stirrer, ultrasonically dispersed for 1h, ball milled for 0.5h, and then allowed to stand for 1h before adding the next nanopowder to finally obtain a glaze ink; in terms of mass percentage, the glaze composed of nanopowders: the mixed dispersant solution obtained in step 1 = 7%:93%.

[0040] Example 4

[0041] A nano-powder-based water-based green ceramic glaze ink for inkjet printing comprises, by mass percentage, 6% of a glaze composed of nano-powder and 94% of a mixed dispersant solution.

[0042] A method for preparing nano-powder-based water-based green ceramic glaze ink for inkjet printing comprises the following steps:

[0043] Step 1: According to the mass percentage, polyvinyl pyrrolidone: sodium alginate = 90%: 10% is mixed to obtain a mixed dispersant, and the mixed dispersant is added into deionized water, and the mixed dispersant: deionized water = 6%: 94%, and a magnetic stirrer is used to heat and stir at 70° C. for 5 minutes until the mixed dispersant is completely dissolved to obtain a mixed dispersant solution containing polyvinyl pyrrolidone and sodium alginate;

[0044] Step 2: Add the glaze composed of nanopowders to the mixed dispersant solution obtained in step 1 in sequence, wherein the glaze composed of nanopowders includes 5% nano-alumina, 55% nano-silicon oxide, 36% calcium carbonate and 4% nano-chromium oxide. The glaze composed of nanopowders is added to the mixed dispersant solution obtained in step 1 in the order of nano-alumina, nano-silicon oxide, calcium carbonate and nano-chromium oxide, and mixed. Each time a nanopowder is added, it is stirred for 0.2h using a magnetic stirrer, ultrasonically dispersed for 1h, ball milled for 0.5h, and then allowed to stand for 1h before adding the next nanopowder to finally obtain glaze ink; in terms of mass percentage, the glaze composed of nanopowders: the mixed dispersant solution obtained in step 1 = 6%: 94%.

[0045] Example 5

[0046] A nano-powder-based water-based green ceramic glaze ink for inkjet printing comprises, by mass percentage, 8% of glaze composed of nano-powder and 92% of mixed dispersant solution.

[0047] A method for preparing nano-powder-based water-based green ceramic glaze ink for inkjet printing comprises the following steps:

[0048] Step 1: According to the mass percentage, polyvinyl pyrrolidone: sodium alginate = 80%: 20% is mixed to obtain a mixed dispersant, and the mixed dispersant is added into deionized water, and the mixed dispersant: deionized water = 8%: 92%, and a magnetic stirrer is used to heat and stir at 70° C. for 7 minutes until the mixed dispersant is completely dissolved to obtain a mixed dispersant solution containing polyvinyl pyrrolidone and sodium alginate;

[0049] Step 2: Add the glaze composed of nanopowders to the mixed dispersant solution obtained in step 1 in sequence, wherein the glaze composed of nanopowders includes 10% nano-alumina, 53% nano-silicon oxide, 32% calcium carbonate and 5% nano-chromium oxide. The glaze composed of nanopowders is added to the mixed dispersant solution obtained in step 1 in the order of nano-alumina, nano-silicon oxide, calcium carbonate and nano-chromium oxide, and mixed. Each time a nanopowder is added, it is stirred for 0.1h using a magnetic stirrer, ultrasonically dispersed for 1h, ball milled for 0.5h, and then allowed to stand for 1h before adding the next nanopowder to finally obtain a glaze ink; in terms of mass percentage, the glaze composed of nanopowders: the mixed dispersant solution obtained in step 1 = 8%:92%.

[0050] The present invention adopts a mixture of dispersant polyvinyl pyrrolidone and sodium alginate. The specific functional group of polyvinyl pyrrolidone is strongly adsorbed on the surface of nano powder particles, generating steric hindrance, and the solvent chain is extended in the continuous phase, thereby forming a physical barrier, thereby changing the free movement trend of the nano powder and stabilizing the ink system. At the same time, the dispersant polyvinyl pyrrolidone and sodium alginate in the glaze ink system and the polymer on the surface of the oxide in the system are negatively charged, have electrostatic repulsion, and make the ink system more stable.

[0051] The ink of the present invention has good quality stability, can be stored for a long time, and has good inkjet printing performance. The viscosity of the ink is 10-30 mPa·s, and the surface tension is 40-60 mN / m. In the inkjet printing process, it has good fluidity and spraying effect, is not easy to clog the nozzle, will not form hanging drops on the nozzle, can be well adsorbed on the inkjet printing carrier, and improves the accuracy of the inkjet printing product.

[0052] When the dispersant content is 5wt% (PVP: sodium alginate = 9:1) and the glaze solid content is 5wt%, the performance of the glaze ink is as follows: Figure 1-5 .

[0053] like Figure 1 As shown in the figure, as the shear rate increases, the viscosity gradually decreases. This indicates that the ink exhibits shear thinning. The ink has pseudoplastic fluid properties. As the shear rate increases, the shear stress gradually increases. The final viscosity obtained from the figure is 22.60 mPa·s, and the glaze ink prepared by the invention meets the expected requirements.

[0054] like Figure 2 As shown, the final surface tension is 51.347 mN / m, indicating that the glaze ink prepared by the present invention meets the requirements of inkjet printers.

[0055] like Figure 3 As shown, the ink stability index gradually increases with time, but from the overall situation, the ink stability index is always small and does not change much, indicating that the glaze ink prepared by the present invention has good stability and can meet the inkjet printer's demand for ink stability.

[0056] like Figure 4 As shown, PVP is at 2940 cm -1 The CH stretching vibration peak at 1290 cm -1 The CN stretching vibration peak at 3437 cm -1 The OH stretching vibration peaks at 1655 cm -1The C=O stretching vibration peak and the OH bending vibration overlap peak at the bottom left move. PVP attracts certain covalent bonds during the mixing process, causing its absorption peak to shift. Calcium carbonate 1415cm -1 The asymmetric stretching vibration of the CO bond of nano-silicon oxide, nano-aluminum oxide and nano-chromium oxide is shifted to the right. -1 Some strong metal oxide covalent bonds at the site all shift upward or absorb. Analysis shows that the dispersant PVP or sodium alginate wraps them, weakening the absorption peaks of these covalent bonds. Figure 4 It can be seen that the specific functional groups of polyvinyl pyrrolidone used in the present invention are strongly adsorbed on the surface of nanopowder particles, generating steric hindrance, and the solvent chains extend in the continuous phase to form a physical barrier, thereby changing the free movement tendency of the nanopowder and stabilizing the ink system.

[0057] like Figure 5 As shown in (a), the glaze surface is smooth and contains some granular substances. Figure 5 As shown in (b), the granular material is composed of hexagonal particles. As can be seen from the figure, the glaze ink of the present invention can be well adsorbed on the inkjet printing carrier, thereby improving the accuracy of the inkjet printing product.

Claims

1. A nano-powder-based water-based green ceramic glaze ink for inkjet printing, characterized in that: According to the mass percentage, the glaze comprises 5-10% of nano powder and 90-95% of mixed dispersant solution.

2. The nano-powder-based water-based green ceramic glaze ink for inkjet printing according to claim 1, characterized in that: The mixed dispersant solution comprises, by mass percentage, 1-10% of a mixed dispersant and 90-99% of deionized water, wherein the mixed dispersant comprises 70%-90% of polyvinyl pyrrolidone and 10%-30% of sodium alginate.

3. The nano-powder-based water-based green ceramic glaze ink for inkjet printing according to claim 1, characterized in that: The glaze composed of the nanometer powder includes, by mass percentage, 50-60% of nanometer silicon oxide, 5-15% of nanometer aluminum oxide, 30-40% of calcium carbonate and 1-5% of nanometer chromium oxide.

4. A method for preparing a nano-powder water-based green ceramic glaze ink for inkjet printing according to any one of claims 1 to 3, characterized in that: The following steps are involved: Step 1: According to the mass percentage, polyvinyl pyrrolidone: sodium alginate = (70%-90%): (10%-30%) are mixed to obtain a mixed dispersant, and the mixed dispersant is added to deionized water, and the mixed dispersant: deionized water = (1-10%): (90-99%), and heated and stirred at 50-70° C. for 5-10 minutes until the mixed dispersant is completely dissolved to obtain a mixed dispersant solution containing polyvinyl pyrrolidone and sodium alginate; Step 2: Add the glaze composed of nano powders to the mixed dispersant solution obtained in step 1 in sequence, wherein the glaze composed of nano powders includes nano aluminum oxide, nano silicon oxide, calcium carbonate and nano chromium oxide. The glaze composed of nano powders is added to the mixed dispersant solution obtained in step 1 in the order of nano aluminum oxide, nano silicon oxide, calcium carbonate and nano chromium oxide, and mixed. Each time a nano powder is added, stirring is performed for 0.1-0.2h, ultrasonic dispersion is performed for 0.9-1h, ball milling is performed for 0.45-0.5h, and then the next nano powder is added after standing for 0.9-1h, so as to finally obtain glaze ink. In terms of mass percentage, the glaze composed of nano powders: the mixed dispersant solution obtained in step 1 = (5-10%): (90-95%).

5. The method for preparing a nano-powder water-based green ceramic glaze ink for inkjet printing according to claim 4, characterized in that: The glaze composed of the nano powder comprises, by mass percentage, 50-60% of nano silicon oxide, 5-15% of nano aluminum oxide, 30%-40% of calcium carbonate and 1-5% of nano chromium oxide.

6. The method for preparing a nano-powder water-based green ceramic glaze ink for inkjet printing according to claim 4, characterized in that: The following steps are involved: Step 1: According to the mass percentage, polyvinyl pyrrolidone: sodium alginate = 70%: 30% is mixed to obtain a mixed dispersant, and the mixed dispersant is added into deionized water, and the mixed dispersant: deionized water is 10%: 90%, and a magnetic stirrer is used to heat and stir at 70° C. for 5 minutes until the mixed dispersant is completely dissolved to obtain a mixed dispersant solution containing polyvinyl pyrrolidone and sodium alginate; Step 2: Add the glaze composed of nanopowders to the mixed dispersant solution obtained in step 1 in sequence, wherein the glaze composed of nanopowders includes 15% nano-alumina, 50% nano-silicon oxide, 33% calcium carbonate and 2% nano-chromium oxide. The glaze composed of nanopowders is added to the mixed dispersant solution obtained in step 1 in the order of nano-alumina, nano-silicon oxide, calcium carbonate and nano-chromium oxide, and mixed. Each time a nanopowder is added, it is stirred for 0.1h using a magnetic stirrer, ultrasonically dispersed for 1h, ball milled for 0.45h, and then allowed to stand for 1h before adding the next nanopowder to finally obtain a glaze ink; in terms of mass percentage, the glaze composed of nanopowders: the mixed dispersant solution obtained in step 1 = 10%:90%.

7. The method for preparing a nano-powder water-based green ceramic glaze ink for inkjet printing according to claim 4, characterized in that: The following steps are involved: Step 1: According to the mass percentage, polyvinyl pyrrolidone: sodium alginate = 90%: 10% is mixed to obtain a mixed dispersant, and the mixed dispersant is added into deionized water, and the mixed dispersant: deionized water = 5%: 95%, and a magnetic stirrer is used to heat and stir at 50° C. for 10 minutes until the mixed dispersant is completely dissolved to obtain a mixed dispersant solution containing polyvinyl pyrrolidone and sodium alginate; Step 2: Add the glaze composed of nanopowders to the mixed dispersant solution obtained in step 1 in sequence, wherein the glaze composed of nanopowders includes 7% nano-alumina, 54% nano-silicon oxide, 38% calcium carbonate and 1% nano-chromium oxide. The glaze composed of nanopowders is added to the mixed dispersant solution obtained in step 1 in the order of nano-alumina, nano-silicon oxide, calcium carbonate and nano-chromium oxide, and mixed. Each time a nanopowder is added, it is stirred for 0.2h using a magnetic stirrer, ultrasonically dispersed for 0.9h, ball milled for 0.5h, and then allowed to stand for 1h before adding the next nanopowder to finally obtain a glaze ink; in terms of mass percentage, the glaze composed of nanopowders: the mixed dispersant solution obtained in step 1 = 5%:95%.

8. The method for preparing a nano-powder water-based green ceramic glaze ink for inkjet printing according to claim 4, characterized in that: The following steps are involved: Step 1: According to the mass percentage, polyvinyl pyrrolidone: sodium alginate = 80%: 20% is mixed to obtain a mixed dispersant, and the mixed dispersant is added into deionized water, and the mixed dispersant: deionized water = 7%: 93%, and a magnetic stirrer is used to heat and stir at 60° C. for 7 minutes until the mixed dispersant is completely dissolved to obtain a mixed dispersant solution containing polyvinyl pyrrolidone and sodium alginate; Step 2: Add the glaze composed of nanopowders to the mixed dispersant solution obtained in step 1 in sequence, wherein the glaze composed of nanopowders includes 12% nano-alumina, 52% nano-silicon oxide, 33% calcium carbonate and 3% nano-chromium oxide. The glaze composed of nanopowders is added to the mixed dispersant solution obtained in step 1 in the order of nano-alumina, nano-silicon oxide, calcium carbonate and nano-chromium oxide, and mixed. Each time a nanopowder is added, it is stirred for 0.2h using a magnetic stirrer, ultrasonically dispersed for 1h, ball milled for 0.5h, and then allowed to stand for 1h before adding the next nanopowder to finally obtain a glaze ink; in terms of mass percentage, the glaze composed of nanopowders: the mixed dispersant solution obtained in step 1 = 7%:93%.

9. The method for preparing a nano-powder water-based green ceramic glaze ink for inkjet printing according to claim 4, characterized in that: The following steps are involved: Step 1: According to the mass percentage, polyvinyl pyrrolidone: sodium alginate = 90%: 10% is mixed to obtain a mixed dispersant, and the mixed dispersant is added into deionized water, and the mixed dispersant: deionized water = 6%: 94%, and a magnetic stirrer is used to heat and stir at 70° C. for 5 minutes until the mixed dispersant is completely dissolved to obtain a mixed dispersant solution containing polyvinyl pyrrolidone and sodium alginate; Step 2: Add the glaze composed of nanopowders to the mixed dispersant solution obtained in step 1 in sequence, wherein the glaze composed of nanopowders includes 5% nano-alumina, 55% nano-silicon oxide, 36% calcium carbonate and 4% nano-chromium oxide. The glaze composed of nanopowders is added to the mixed dispersant solution obtained in step 1 in the order of nano-alumina, nano-silicon oxide, calcium carbonate and nano-chromium oxide, and mixed. Each time a nanopowder is added, it is stirred for 0.2h using a magnetic stirrer, ultrasonically dispersed for 1h, ball milled for 0.5h, and then allowed to stand for 1h before adding the next nanopowder to finally obtain glaze ink; in terms of mass percentage, the glaze composed of nanopowders: the mixed dispersant solution obtained in step 1 = 6%: 94%.

10. The method for preparing a nano-powder-based water-based green ceramic glaze ink for inkjet printing according to claim 4, characterized in that: The following steps are involved: Step 1: According to the mass percentage, polyvinyl pyrrolidone: sodium alginate = 80%: 20% is mixed to obtain a mixed dispersant, and the mixed dispersant is added into deionized water, and the mixed dispersant: deionized water = 8%: 92%, and a magnetic stirrer is used to heat and stir at 70° C. for 7 minutes until the mixed dispersant is completely dissolved to obtain a mixed dispersant solution containing polyvinyl pyrrolidone and sodium alginate; Step 2: Add the glaze composed of nanopowders to the mixed dispersant solution obtained in step 1 in sequence, wherein the glaze composed of nanopowders includes 10% nano-alumina, 53% nano-silicon oxide, 32% calcium carbonate and 5% nano-chromium oxide. The glaze composed of nanopowders is added to the mixed dispersant solution obtained in step 1 in the order of nano-alumina, nano-silicon oxide, calcium carbonate and nano-chromium oxide, and mixed. Each time a nanopowder is added, it is stirred for 0.1h using a magnetic stirrer, ultrasonically dispersed for 1h, ball milled for 0.5h, and then allowed to stand for 1h before adding the next nanopowder to finally obtain a glaze ink; in terms of mass percentage, the glaze composed of nanopowders: the mixed dispersant solution obtained in step 1 = 8%:92%.

Citation Information

Patent Citations

  • Eco-friendly glaze ink for ceramic jet printing and preparation method thereof

    CN103224727B

  • High-stability water-based ceramic glaze ink suitable for ink-jet printing and preparation method of high-stability water-based ceramic glaze ink

    CN116554730A

  • Cobalt blue ceramic glaze ink and preparation method thereof

    CN105542552A

  • Ink jet recording method and ink jet recording ink

    JP1999091090A

  • Ink set, printing method and printed matter

    JP2020019906A