Intermittent modified solution polymerized styrene-butadiene rubber and preparation method thereof
By using functionalized initiators and modifiers under batch polymerization conditions, the molecular weight distribution of solution-polymerized styrene-butadiene rubber is broadened, which solves the problems of narrow molecular weight distribution and high rolling resistance of the product, improves processing performance and mechanical properties, and reduces Rolling resistance of tire products.
Patent Information
- Application Number
- CN202411312680.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-10-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The molecular weight distribution of solution-polymerized styrene-butadiene rubber products caused by the batch polymerization process is narrow, resulting in insufficient processing performance and mechanical properties, and the rolling resistance of tire products is high.
The preparation method of batch-modified solution-polymerized styrene-butadiene rubber is adopted, and a functionalized initiator is used under batch polymerization conditions to introduce a cyclic amine structure to carry out end-capping, coupling and branching modification reactions to broaden the molecular weight distribution and improve processing. performance and mechanical properties, and reduce the rolling resistance of tire products.
It has improved the processing performance and mechanical properties of solution-polymerized styrene-butadiene rubber, reduced the rolling resistance of tire products, and improved the performance and application value of the product.
Smart Images

Figure CN118812781A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of synthetic rubber, and in particular relates to an intermittently modified solution-polymerized styrene-butadiene rubber and a preparation method thereof. Background Art
[0002] Solution styrene butadiene rubber (SSBR) has good low-temperature flexibility, resilience and wear resistance. The demand for SSBR in tires, retread and molded products, injection and extrusion products, medical devices, footwear and auto parts continues to grow. In recent years, SSBR has become the first choice for manufacturing high-performance tires such as green tires, anti-skid tires, ultra-light tires, energy-saving tires, etc. due to its characteristics of wear resistance, cold resistance, low heat generation, good shrinkage, good color, low ash content, high purity and fast vulcanization speed, as well as its advantages of low rolling resistance, excellent anti-slip and wear resistance.
[0003] SSBR is based on butadiene (CH2=CH-CH=CH2) and styrene (C6H5-CH=CH2) as main monomers. The polymerization of monomers is initiated by adding organic lithium into hydrocarbon solvents. After sufficient reaction, antioxidants and other additives are added. The desired sample is obtained through processes such as condensation and drying.
[0004] Linear SSBR, which is mainly used in tire manufacturing, is mainly produced by continuous polymerization during the production process. Its advantages are stable, uniform, high purity and extremely low gel content, high production efficiency and low cost, and it is suitable for mass production of general brands. However, the continuous production line will cause a significant increase in costs due to the large amount of transition materials for conversion, and is not suitable for brands with low batch production, flexible conversion, and modified or specially designed structures.
[0005] The intermittent polymerization process is a non-continuous polymerization production process. This process has the characteristics of uniform distribution of polymer residence time, great production flexibility, easy switching of varieties and grades, less transition materials, easy production of grades with special structural parameters and performance, easy adjustment according to market demand, and suitable for the production of high-end grades. However, due to the copolymerization reaction characteristics of the intermittent polymerization process, the molecular weight distribution of the obtained SSBR product is narrow, resulting in a decrease in the processing performance of the product. Summary of the invention
[0006] In view of this, the present invention provides an intermittent modified solution-polymerized styrene-butadiene rubber and a preparation method thereof, the purpose of which is to broaden the molecular weight distribution of the product by coupling modification, improve the product processing performance, enhance the product mechanical properties, and improve the problems of narrow product molecular weight distribution, decreased product processing performance and insufficient mechanical properties caused by the copolymerization reaction characteristics of the conventional intermittent polymerization process; in addition, a cyclic amine structure is introduced into the solution-polymerized styrene-butadiene rubber by a functionalized initiator, so that the modified solution-polymerized styrene-butadiene rubber produced can be used in the tire manufacturing process to reduce the rolling resistance of the tire product, thereby improving the performance of the tire product.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions.
[0008] A first aspect of the present invention provides a method for preparing an intermittently modified solution-polymerized styrene-butadiene rubber, the method comprising the following steps: 1) under intermittent polymerization conditions, styrene, butadiene, an organic solvent and a structure regulator are mixed to obtain a monomer-structure regulator mixed system, and then a functionalized initiator is added to the monomer-structure regulator mixed system to initiate a reaction and perform a polymerization reaction to obtain an intermediate polymer; 2) using a capping monomer to cap the intermediate polymer to obtain a capped polymer; 3) using a coupling agent to carry out a coupling reaction on the capped polymer to obtain a capped coupled polymer; 4) using a branching modifier to carry out a branching modification reaction to obtain a capped coupled branched modified polymer; 5) adding a terminator to terminate the reaction, thereby obtaining the intermittently modified solution-polymerized styrene-butadiene rubber.
[0009] In the above-mentioned method for preparing intermittently modified solution-polymerized styrene-butadiene rubber, in the step 1), the functionalized initiator is prepared by reacting an organic lithium (conventional initiator) and a functionalized modifier.
[0010] In the preparation method of the intermittently modified solution-polymerized styrene-butadiene rubber, the organic lithium includes at least one of n-butyl lithium, sec-butyl lithium, pentyl lithium, ethyl lithium, propyl lithium and isopropyl lithium.
[0011] In the above-mentioned method for preparing intermittently modified solution-polymerized styrene-butadiene rubber, the organic lithium comprises at least one of n-butyl lithium and sec-butyl lithium.
[0012] In the above-mentioned method for preparing intermittently modified solution-polymerized styrene-butadiene rubber, in the step 1), the functionalized modifier is an N-containing cyclic compound.
[0013] In the preparation method of the intermittently modified solution-polymerized styrene-butadiene rubber, in step 1), the functionalized modifier comprises at least one of cycloheximide and hexahydropyridine. The structural formulas of cycloheximide and hexahydropyridine are shown below.
[0014] In the present invention, the functionalized modifier includes but is not limited to at least one of cyclohexyl imine and hexahydropyridine. The functionalized modifier is used to functionalize and modify conventional organic lithium initiators. Specifically, the organic lithium and the functionalized modifier are mixed, and the H atom on the NH bond in the functionalized modifier is replaced by the Li in the organic lithium, thereby forming an organic amine lithium initiator. When the organic amine lithium initiator reacts with the monomer (styrene / butadiene), the organic amine group is linked to one end of the active chain, thereby realizing the functionalization of the polymer product structure.
[0015] In the present invention, the functionalized initiator has a cyclic amine lithium structure.
[0016] For example, the chemical reaction between the functionalized modifier and the organic lithium initiator is explained by the reaction mechanism of cyclohexyl imine and n-butyl lithium.
[0017] As shown above, cyclohexylimide and n-butyl lithium react to form cyclohexylimide lithium and n-butane. The cyclic amine lithium initiator formed by the reaction of the two initiates the polymerization reaction of the monomers, so that the cyclic compound containing the amino group is connected to one end of the reaction chain, which has a good effect on the synthetic rubber used in the tire manufacturing process to reduce the rolling resistance of the tire product.
[0018] In the present invention, the amount of the initiator added is reasonably set according to the existing solution butadiene styrene polymerization process conditions and the microstructure requirements of the synthesized product.
[0019] In the above-mentioned method for preparing intermittently modified solution-polymerized styrene-butadiene rubber, in the step 1), the molar ratio of Li to N of the organic lithium and the functionalized modifier is 1:(0.8 to 1).
[0020] In the present invention, if the molar ratio of Li to N is too small, the functional groups added to the reaction chain will be too small, and the rolling resistance performance of the subsequent tire manufacturing will decrease; when the molar ratio of Li to N exceeds 1:1, it has no effect on the performance improvement of the polymerization product, and will only cause a waste of reaction raw materials.
[0021] In the above-mentioned method for preparing intermittently modified solution-polymerized styrene-butadiene rubber, in the step 1), the organic solvent is a hydrocarbon solvent.
[0022] In the above-mentioned method for preparing intermittently modified solution-polymerized styrene-butadiene rubber, in the step 1), the organic solvent comprises at least one of alkanes having 5 to 8 carbon atoms and cycloalkanes having 5 to 8 carbon atoms.
[0023] In the present invention, the organic solvent may be a C5 to C8 alkane or a C5 to C8 cycloalkane, or a mixture of a C5 to C8 alkane and a C5 to C8 cycloalkane.
[0024] In the above-mentioned method for preparing intermittent modified solution-polymerized styrene-butadiene rubber, in the step 1), the organic solvent comprises at least one of cyclohexane, hexane, cyclopentane, pentane, heptane, raffinate oil and benzene.
[0025] In this field, raffinate oil refers to the distillate oil remaining after the aromatics are extracted (see aromatics extraction) from the catalytic reforming product (reforming gasoline) rich in aromatics. Its main components are C6 to C8 alkanes and a certain amount of cycloalkanes, and it is a good petrochemical raw material.
[0026] In the present invention, one or more of the above organic solvents can be selected and used in combination according to actual production needs.
[0027] In the above-mentioned method for preparing intermittently modified solution-polymerized styrene-butadiene rubber, in the step 1), the structure regulator is a polar Lewis base, including at least one of a strong polar Lewis base and a weak polar Lewis base.
[0028] In the preparation method of the intermittent modified solution-polymerized styrene-butadiene rubber, the strong polar Lewis base includes at least one of diethylene glycol dimethyl ether (2G), triethylene glycol dimethyl ether (3G), dimethoxyethane (DME), 2,2-di(2-tetrahydrofuranyl)propane (DTHFP) and alkyl tetrahydrofurfuryl ether.
[0029] In the preparation method of the intermittent modified solution-polymerized styrene-butadiene rubber, the weakly polar Lewis base includes at least one of tetrahydrofuran (THF), p-dioxane (DOX), ether, triethylamine (Et3N) and sodium dodecylbenzene sulfonate.
[0030] In the present invention, according to the requirements of polymer synthesis, one, two or more of the above-mentioned strong polar Lewis bases and weak polar Lewis bases are selected and used in combination.
[0031] In the preparation method of the intermittent modified solution-polymerized styrene-butadiene rubber, the structure regulator is alkyl tetrahydrofurfuryl ether, in which the alkyl group is an alkyl group with a carbon number of 1 to 9. For example, the structure regulator is ethyl tetrahydrofurfuryl ether ETE.
[0032] In the above-mentioned method for preparing intermittently modified solution-polymerized styrene-butadiene rubber, in the step 1), the molar ratio of the structure regulator to the lithium element in the organic lithium is (0.4 to 6):1.
[0033] In the above-mentioned method for preparing intermittently modified solution-polymerized styrene-butadiene rubber, in the step 1), the mass ratio of the butadiene to the styrene is (1.5 to 9):1.
[0034] In the above method for preparing intermittently modified solution-polymerized styrene-butadiene rubber, in the step 2), the end-capping monomer comprises a conjugated olefin compound.
[0035] In the above-mentioned method for preparing intermittently modified solution-polymerized styrene-butadiene rubber, in the step 2), the end-capping monomer comprises at least one conjugated olefin compound selected from butadiene, pentadiene and isoprene.
[0036] In the present invention, one or two of the above-mentioned end-capping monomers can be selected and used in combination according to needs.
[0037] In the above-mentioned method for preparing intermittently modified solution-polymerized styrene-butadiene rubber, in the step 2), the amount of the end-capping monomer added accounts for 0.5% to 5% of the amount of the butadiene monomer fed.
[0038] In the preparation method of the intermittently modified solution-polymerized styrene-butadiene rubber, in the step 3), the coupling agent comprises at least one of a halide containing a two-arm structure, a halide containing a four-arm structure, and a siloxane compound containing a multi-arm structure of three arms or more.
[0039] In the above-mentioned method for preparing intermittently modified solution-polymerized styrene-butadiene rubber, the four-arm structure halide comprises at least one of silicon tetrachloride and tin tetrachloride.
[0040] In the preparation method of the intermittently modified solution-polymerized styrene-butadiene rubber, the siloxane compound contains at least one structure selected from the group consisting of an amino group, a methoxy group, a carboxyl group, a sulfhydryl group, a hydroxyl group and a phosphorus group.
[0041] In the preparation method of the intermittent modified solution-polymerized styrene-butadiene rubber, the siloxane compound includes at least one of 3-chloropropyltrimethoxysilane, 3-chloropropyldimethoxymethylsilane and N-[3-(triethoxysilyl)propyl]-4,5-dihydroimidazole.
[0042] In the preparation method of the intermittently modified solution-polymerized styrene-butadiene rubber, the halide containing a double-arm structure includes dichlorodiphenylsilane.
[0043] In the present invention, one, two or more of the above coupling agents are selected and used in combination according to the needs.
[0044] In the above-mentioned method for preparing intermittently modified solution-polymerized styrene-butadiene rubber, in the step 3), the molar ratio of the coupling agent to the lithium element in the organic lithium is (12 to 30):100 (or 0.12 to 0.3:1).
[0045] In the above-mentioned method for preparing intermittently modified solution-polymerized styrene-butadiene rubber, in the step 4), the branched modifier includes: an organic peroxide that can generate oxygen-containing free radicals when heated and an azo compound that can generate free radicals.
[0046] In the above-mentioned method for preparing intermittently modified solution-polymerized styrene-butadiene rubber, the organic peroxide comprises at least one of a dialkyl peroxide and a diacyl peroxide.
[0047] In the preparation method of the intermittently modified solution-polymerized styrene-butadiene rubber, the organic peroxide has at least one structure selected from the group consisting of a linear structure, a branched structure and a cyclic structure.
[0048] In the method for preparing the intermittently modified solution-polymerized styrene-butadiene rubber, the organic peroxide contains an alkyl structure with 1 to 14 carbon atoms.
[0049] In the above-mentioned method for preparing intermittently modified solution-polymerized styrene-butadiene rubber, the azo compound includes azobisisobutyronitrile.
[0050] In the present invention, one, two or more of the above organic peroxides are selected and used in combination according to needs.
[0051] In the above method for preparing intermittently modified solution-polymerized styrene-butadiene rubber, in step 4), the molar ratio of the branched modifier to the lithium element in the organic lithium is 0.5 to 1.4:1, preferably 0.8 to 1.4:1.
[0052] In the above-mentioned method for preparing intermittently modified solution-polymerized styrene-butadiene rubber, in the step 5), the terminator comprises at least one of trimethylchlorosilane, anhydrous ethanol and fatty acid.
[0053] In the present invention, the terminator includes but is not limited to auxiliary agents with termination effect such as trimethylchlorosilane, anhydrous ethanol, fatty acid, etc., and one of them can be selected and used according to needs.
[0054] In the preparation method of the intermittently modified solution-polymerized styrene-butadiene rubber, in the step 5), a terminator is added to terminate the reaction to obtain a polymer product, and the polymer product is dried to obtain the intermittently modified solution-polymerized styrene-butadiene rubber; specifically, the polymer product is transferred to a vacuum drying oven and dried at a temperature of 60°C to 70°C for 12h to 13h.
[0055] In the preparation method of the intermittent modified solution-polymerized styrene-butadiene rubber, the solution-polymerized styrene-butadiene rubber is produced by a single-pot polymerization system.
[0056] In the preparation method of the intermittent modified solution-polymerized styrene-butadiene rubber, the polymerization reaction is carried out under an inert gas protective atmosphere.
[0057] In the above-mentioned method for preparing intermittent modified solution-polymerized styrene-butadiene rubber, in said step 1), before mixing styrene, butadiene, organic solvent and structure regulator, an inert gas is introduced into the reaction container.
[0058] In the preparation method of the intermittent modified solution-polymerized styrene-butadiene rubber, the temperature for initiating the reaction is 30°C to 60°C, and the maximum temperature for the polymerization reaction is 80°C to 140°C, preferably 90°C to 110°C.
[0059] In the above-mentioned preparation method of intermittent modified solution-polymerized styrene-butadiene rubber, the reaction temperatures of the coupling reaction and the branching modification reaction are both 60°C to 100°C, preferably 70°C to 90°C.
[0060] In the present invention, the coupling reaction and branching modification reaction are both modification reactions of the intermediate polymer.
[0061] The preparation method of the invention is suitable for anionic copolymerization of butadiene and styrene to synthesize random SSBR and is used to control the microstructure in the random SSBR.
[0062] The present invention does not specifically limit the order of adding the components before the polymerization reaction, and can be reasonably set according to the order of adding in the conventional solution-polymerized styrene-butadiene rubber preparation process. Under normal circumstances, the organic solvent, butadiene, styrene, and structure regulator, that is, the raw materials other than the organic lithium initiator are first mixed evenly, and then the system is heated to the initiation temperature of the organic lithium initiator, and finally the organic lithium initiator is added to initiate the copolymerization of styrene and butadiene. Since the preparation of solution-polymerized styrene-butadiene rubber by copolymerization of butadiene and styrene is an exothermic reaction, the temperature of the reaction system increases as the copolymerization reaction continues. About half an hour after the start of the copolymerization reaction, depending on the reaction conditions, the temperature of the reaction system can reach 80°C to 140°C (preferably 90°C to 110°C). As the polymerization reaction proceeds, the amount of monomers in the system gradually decreases, the system exothermic heat decreases, and the polymerization kettle temperature gradually decreases. When the modification step is performed, the reactor temperature is usually 60 to 100°C (preferably 70 to 90°C).
[0063] In the present invention, under the condition of single-pot polymerization process, the microstructure of the solution-polymerized styrene-butadiene rubber product is controlled by controlling the reaction temperature and the addition ratio of the structure regulator, after the initiation reaction, the end-capping monomer is added after the polymerization reaction time is 10 to 30 minutes, the coupling agent is added after the reaction for 5 to 15 minutes, the branching modifier is added after the coupling reaction for 5 to 15 minutes, and the terminator is added after the reaction for 5 to 15 minutes, and the polymerization reaction can be considered to be completed.
[0064] In the preparation method of the intermittent modified solution-polymerized styrene-butadiene rubber, the total polymerization reaction time is 0.5 h to 2 h; the total polymerization reaction time includes the polymerization reaction time after the initiation reaction, the coupling reaction time and the branching modification reaction time.
[0065] In addition, the present invention can also adjust the amount of modified segments of the product by adding a coupling agent and a branching modifier to obtain products with different mechanical properties, and improve the processing performance of the product by adding an end-capping monomer.
[0066] The preparation method of the functionalized initiator of the present invention is simple and has a fast polymerization rate, which is conducive to realizing industrial multi-batch stable production. In addition, since the raw materials are easily available, but the corresponding coupling agent and branching modifier and process parameters need to be matched, it is novel and difficult to imitate while improving production efficiency and equipment utilization.
[0067] The invention introduces a cyclic amine structure into the solution-polymerized styrene-butadiene rubber through a functionalized initiator, and the structure is beneficial to improving the rolling resistance performance of the product after mixing.
[0068] The second aspect of the present invention provides an intermittently modified solution polymerized styrene butadiene rubber, which is prepared by any of the above-mentioned methods for preparing intermittently modified solution polymerized styrene butadiene rubber.
[0069] Furthermore, the intermittently modified solution-polymerized styrene-butadiene rubber is a random solution-polymerized styrene-butadiene rubber.
[0070] Furthermore, the base rubber Mooney viscosity (ML(1+4)120°C) of the intermittently modified solution-polymerized styrene-butadiene rubber is between 60 and 120, the bound benzene content is between 10% and 40%, the vinyl content is between 30% and 70%, and the randomness is 100%.
[0071] According to the intermittent modified solution-polymerized styrene-butadiene rubber of the present invention, the preparation method of the intermittent modified solution-polymerized styrene-butadiene rubber is adopted, in an inert gas protection environment, Lewis base is used as a structural regulator, C5 to C8 alkane or C5 to C8 cycloalkane, or a mixture of C5 to C8 alkane and C5 to C8 cycloalkane is used as an organic solvent, a mixed system of organic lithium and a functionalized modifier is used to initiate a polymerization reaction, the solution-polymerized styrene-butadiene rubber is synthesized under specific process conditions, and a coupling reaction and a branching modification reaction are respectively carried out in the presence of a coupling agent and a branching modifier, and after the reaction is completed, a random solution-polymerized styrene-butadiene rubber is obtained by condensation and drying. The base rubber Mooney viscosity (ML (1+4) 120°C) of the random solution-polymerized styrene-butadiene rubber is between 60 and 120, the combined benzene content is between 10% and 40%, the vinyl content is between 30% and 70%, and the randomness is 100%. The present invention can realize engineering batch stable production, and the product has excellent mechanical properties, and the wear resistance, rolling resistance and anti-slip performance are balanced.
[0072] In the present invention, the above technical features can be freely combined to form a new technical solution without conflicting with each other.
[0073] Compared with the prior art, the technical solution of the present invention has the following beneficial technical effects: (1) Based on the intermittent polymerization process of the present invention, a cyclic amine structure is introduced into the solution polymerized styrene butadiene rubber through a functionalized initiator, so that the intermittent modified solution polymerized styrene butadiene rubber produced can reduce the rolling resistance of the tire product when used in the tire manufacturing process, thereby improving the performance of the tire product; (2) Improve the activity of functionalized polymers by introducing end-capping monomers, adjust the molecular weight distribution of products by coupling, and increase the molecular weight of products by branching modification, thereby improving processing performance and mechanical properties; (3) According to the technical solution of the present invention, a non-linear modified solution-polymerized styrene-butadiene rubber can be prepared, which improves the disadvantage that conventional linear intermittently modified solution-polymerized styrene-butadiene rubber products are difficult to process; (4) According to the preparation method of the present invention, the raw materials are easily available and of moderate price, and the modifier is easily soluble in the solvent and can be easily removed; (5) The intermittent polymerization process of the present invention is used to produce solution-polymerized styrene-butadiene rubber, and a technical platform is formed based on the intermittent polymerization process, which can be widely used in the modification of various solution-polymerized styrene-butadiene rubber products with different molecular structures and different microscopic proportions to improve product performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0074] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0075] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0076] Figure 1 This is the NMR spectrum of the solution-polymerized styrene-butadiene rubber product prepared in Example 6 of the present invention.
[0077] Figure 2 This is the nuclear magnetic spectrum of the solution-polymerized styrene-butadiene rubber product prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0078] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0079] According to some embodiments of the first aspect of the present invention, there is provided a method for preparing an intermittently modified solution-polymerized styrene-butadiene rubber, the method comprising the following steps: 1) under intermittent polymerization conditions, styrene, butadiene, an organic solvent and a structure regulator are mixed to obtain a monomer-structure regulator mixed system, and then a functionalized initiator is added to the monomer-structure regulator mixed system to initiate a reaction and perform a polymerization reaction to obtain an intermediate polymer; the functionalized initiator has a cyclic amine lithium structure; the functionalized initiator is prepared by reacting an organic lithium and a functionalized modifier; the functionalized modifier is an N-containing cyclic compound; 2) using a capping monomer to cap the intermediate polymer to obtain a capped polymer; 3) using a coupling agent to carry out a coupling reaction on the capped polymer to obtain a capped coupled polymer; 4) using a branching modifier to carry out a branching modification reaction to obtain a capped coupled branched modified polymer; 5) adding a terminator to terminate the reaction, thereby obtaining the intermittently modified solution-polymerized styrene-butadiene rubber.
[0080] According to some embodiments of the first aspect of the present invention, the organic lithium includes at least one of n-butyl lithium, sec-butyl lithium, pentyl lithium, ethyl lithium, propyl lithium and isopropyl lithium.
[0081] According to some embodiments of the first aspect of the present invention, in step 1), the functionalized modifier comprises at least one of cycloheximide and hexahydropyridine. The structural formulas of cycloheximide and hexahydropyridine are shown below.
[0082] In the present invention, the functionalized modifier includes but is not limited to at least one of cycloheximide and hexahydropyridine. The functionalized modifier is used to functionalize conventional organic lithium initiators. The functionalized initiator has a cyclic amine lithium structure.
[0083] For example, the chemical reaction between the functionalized modifier and the organic lithium initiator is explained by the reaction mechanism of cyclohexyl imine and n-butyl lithium.
[0084] As shown above, cyclohexylimide and n-butyl lithium react to form cyclohexylimide lithium and n-butane. The cyclic amine lithium initiator formed by the reaction of the two initiates the polymerization reaction of the monomers, so that the cyclic compound containing the amino group is connected to one end of the reaction chain, which has a good effect on the synthetic rubber used in the tire manufacturing process to reduce the rolling resistance of the tire product.
[0085] According to some embodiments of the first aspect of the present invention, the polymerization reaction is carried out under an inert gas protective atmosphere.
[0086] According to some embodiments of the first aspect of the present invention, in the step 1), the molar ratio of Li to N between the initiator and the functionalized modifier is 1:(0.8 to 1) (eg, 1:0.85, 1:0.9 or 1:0.95).
[0087] If the molar ratio of Li to N is too small, fewer functional groups will be added to the reaction chain, and the rolling resistance performance of the subsequent tire manufacturing will decrease; when the molar ratio of Li to N exceeds 1:1, it will have no effect on the performance improvement of the polymerization product, and will only cause a waste of reaction raw materials.
[0088] According to some embodiments of the first aspect of the present invention, in step 1), the organic solvent includes at least one hydrocarbon solvent selected from C5 to C8 alkanes and C5 to C8 cycloalkanes.
[0089] In the present invention, the organic solvent may be a C5 to C8 alkane or a C5 to C8 cycloalkane, or a mixture of a C5 to C8 alkane and a C5 to C8 cycloalkane.
[0090] According to some embodiments of the first aspect of the present invention, in step 1), the organic solvent includes at least one of cyclohexane, hexane, cyclopentane, pentane, heptane, raffinate and benzene.
[0091] According to some embodiments of the first aspect of the present invention, in step 1), the structure regulator is a polar Lewis base, including at least one of a strong polar Lewis base and a weak polar Lewis base. The strong polar Lewis base includes at least one of diethylene glycol dimethyl ether (2G), triethylene glycol dimethyl ether (3G), dimethoxyethane (DME), 2,2-di(2-tetrahydrofuranyl)propane (DTHFP) and alkyl tetrahydrofurfuryl ether. The weak polar Lewis base includes at least one of tetrahydrofuran THF, p-dioxane DOX, ether, triethylamine Et3N and sodium dodecylbenzene sulfonate.
[0092] In the present invention, according to the requirements of polymer synthesis, one, two or more of the above-mentioned strong polar Lewis bases and weak polar Lewis bases are selected and used in combination.
[0093] According to some embodiments of the first aspect of the present invention, in step 1), the structure regulator is alkyl tetrahydrofurfuryl ether, in which the alkyl group is C1 to C9 alkyl (e.g., methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl or octyl). For example, the structure regulator is ethyl tetrahydrofurfuryl ether ETE.
[0094] According to some embodiments of the first aspect of the present invention, in step 1), the molar ratio of the structure regulator to the organic lithium is (0.4 to 6):1 (for example, 0.5:1, 1:1, 2:1, 3:1, 4:1 or 5:1).
[0095] According to some embodiments of the first aspect of the present invention, in step 1), the mass ratio of the butadiene to the styrene is (1.5 to 9):1 (for example, 2:1, 3:1, 4:1, 5:1, 6:1 or 8:1).
[0096] According to some embodiments of the first aspect of the present invention, in step 2), the end-capping monomer includes at least one conjugated olefin compound selected from the group consisting of butadiene, pentadiene and isoprene.
[0097] According to some embodiments of the first aspect of the present invention, in the step 2), the amount of the end-capping monomer added is 0.5% to 5% (eg, 1%, 2%, 3%, 4% or 4.5%) of the amount of the butadiene monomer fed.
[0098] According to some embodiments of the first aspect of the present invention, in step 3), the coupling agent includes at least one of a halide containing a double-arm structure, a halide containing a four-arm structure, and a siloxane compound containing a three-arm or multi-arm structure. Wherein, the halide containing a double-arm structure includes dichlorodiphenylsilane; the halide containing a four-arm structure includes at least one of silicon tetrachloride and tin tetrachloride; and the siloxane compound contains at least one structure of an amino group, a methoxy group, a carboxyl group, a sulfhydryl group, a hydroxyl group, and a phosphorus group.
[0099] According to some embodiments of the first aspect of the present invention, the siloxane compound includes at least one of 3-chloropropyltrimethoxysilane, 3-chloropropyldimethoxymethylsilane and N-[3-(triethoxysilyl)propyl]-4,5-dihydroimidazole.
[0100] In the present invention, one, two or more of the above coupling agents are selected and used in combination according to the needs.
[0101] According to some embodiments of the first aspect of the present invention, the molar ratio of the coupling agent to the lithium element in the organic lithium is (12 to 30):100 (for example, 15:100, 18:100, 20:100, 22:100, 25:100 or 28:100).
[0102] According to some embodiments of the first aspect of the present invention, in step 4), the branched modifier includes an organic peroxide that can generate oxygen-containing free radicals when heated and an azo compound that can generate free radicals. The organic peroxide includes at least one of a dialkyl peroxide and a diacyl peroxide. The azo compound includes azobisisobutyronitrile.
[0103] According to some embodiments of the first aspect of the present invention, the organic peroxide contains an alkyl structure with a C atom number of 1 to 14 (e.g., 2, 3, 4, 6, 8, 10 or 12). The organic peroxide has at least one of a linear structure, a branched structure and a cyclic structure.
[0104] According to some embodiments of the first aspect of the present invention, in the step 4), the molar ratio of the branched modifier to the lithium element in the organic lithium is 0.5 to 1.4:1 (for example, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1.0:1, 1.1:1 or 1.2:1), preferably 0.8 to 1.4:1.
[0105] According to some embodiments of the first aspect of the present invention, the terminator includes at least one of trimethylchlorosilane, anhydrous ethanol and fatty acid.
[0106] According to some embodiments of the first aspect of the present invention, the solution-polymerized styrene-butadiene rubber is produced by a single-pot polymerization system.
[0107] According to some embodiments of the first aspect of the present invention, the temperature for initiating the reaction is 30°C to 60°C (for example, 40°C or 50°C), and the maximum temperature for the polymerization reaction is 80°C to 140°C (for example, 90°C, 100°C, 110°C, 120°C or 130°C), preferably 90°C to 110°C (for example, 95°C, 100°C or 105°C).
[0108] According to some embodiments of the first aspect of the present invention, the reaction temperatures of the coupling reaction and the branching modification reaction are both 60°C to 100°C (e.g., 65°C, 70°C, 80°C, 85°C or 90°C), preferably 70°C to 90°C (e.g., 75°C, 80°C or 85°C).
[0109] The preparation method of the invention is suitable for anionic copolymerization of butadiene and styrene to synthesize random SSBR and is used to control the microstructure in the random SSBR.
[0110] According to some embodiments of the second aspect of the present invention, an intermittently modified solution-polymerized styrene-butadiene rubber is provided, which is prepared by any of the above-mentioned methods for preparing intermittently modified solution-polymerized styrene-butadiene rubber. The intermittently modified solution-polymerized styrene-butadiene rubber is a random solution-polymerized styrene-butadiene rubber, and its base rubber Mooney viscosity (ML(1+4)120°C) is 60 to 120, the bound benzene content is 10% to 40%, the vinyl content is 30% to 70%, and the randomness is 100%.
[0111] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually measured according to national standards. If there is no corresponding national standard, then it is carried out according to general international standards, conventional conditions, or according to the conditions recommended by the manufacturer. Unless otherwise specified, the various raw materials, reagents, instruments and equipment used in the present invention, etc., can be purchased from the market or can be prepared by existing methods.
[0112] It should be noted that in each embodiment and comparative example, the Agilent nuclear magnetic resonance spectrometer was used to analyze the solution polymerized styrene-butadiene rubber product. 1 H-NMR was used for analysis and characterization, where the solvent was CDCl3; infrared spectroscopy was used to test the microstructure content of the solution polymerized styrene butadiene rubber product; gel permeation chromatography was used to measure the molecular weight and molecular weight distribution of the solution polymerized styrene butadiene rubber product. A universal material testing machine was used to test the mechanical properties of the solution polymerized styrene butadiene rubber product; a DIN wear tester was used to measure the DIN wear; a dynamic mechanical thermal analyzer was used to measure the dynamic mechanical properties in tensile mode; and a Mooney viscometer was used to test the Mooney viscosity of SSBR. Among them, the Mooney viscosity of raw rubber and mixed rubber is tested according to GB / T 1232.1-2016; the tensile strength, 300% elongation and elongation at break are tested according to GB / T 528-2009; the hardness is tested according to GB / T 531.1-2008; the rebound is tested according to GB / T1681-2009; the Akron abrasion is tested according to GB / T 1689-2014; the DIN abrasion is tested according to GB / T9867-2008; the dynamic properties (tanδ, 0℃ and tanδ, 60℃) are tested according to GB / T 9870.1-2006.
[0113] Example 1 A method for preparing intermittently modified solution-polymerized styrene-butadiene rubber comprises the following steps: Under the conditions of the intermittent polymerization system, 5 g (0.008 mol) of structure regulator ethyl tetrahydrofurfuryl ether (20% mass concentration), 70 g of styrene, 630 g of butadiene, and 3400 g of cyclopentane were added to the polymerization kettle. When the temperature in the kettle reached 35°C (initiation temperature), a mixed solution of 3.4 g (0.007 mol) of n-butyl lithium (15% mass concentration) and 3 g (0.0063 mol) of cycloheximide (20% mass concentration) (i.e., functionalized initiator solution) was added thereto to initiate the reaction and start polymerization. When the polymerization reaction reached the highest temperature of 97°C, the polymerization reaction time was 19 min. After the polymerization reaction reached the peak temperature, the polymerization continued for about 30 min. 20 g of butadiene was added as a capping monomer. After 10 min of reaction, 1.3 g (0.0011 mol) of silicon tetrachloride (15% mass concentration) was added for coupling reaction. The coupling reaction temperature was 80°C. After 10 min of reaction, 4.5 g (0.0055 mol) branching modifier azobisisobutyronitrile (20% mass concentration, which means that azobisisobutyronitrile is diluted to a 20% solution) is subjected to branching modification reaction, the temperature of the branching modification reaction is 76°C, and finally it is terminated by trimethylchlorosilane. The obtained product is dried in a vacuum drying oven at 60°C for 12 hours to obtain intermittently modified solution-polymerized styrene-butadiene rubber. Among them, the molar ratio of the structure regulator to the lithium element in n-butyl lithium is 1.1:1, the molar ratio of cyclohexylimide to n-butyl lithium is 0.9:1, the molar ratio of silicon tetrachloride to the lithium element in n-butyl lithium is 0.16:1, the molar ratio of azobisisobutyronitrile to the lithium element in n-butyl lithium is 0.8:1, and the end-capping monomer accounts for 3.17% of the mass of the butadiene monomer.
[0114] The intermittently modified solution polymerized styrene butadiene rubber prepared in this example was characterized, and the results are shown in Table 1. As can be seen from Table 1, the intermittently modified solution polymerized styrene butadiene rubber is a random nonlinear solution polymerized styrene butadiene rubber.
[0115] Example 2 A method for preparing intermittently modified solution-polymerized styrene-butadiene rubber comprises the following steps: Under the conditions of the intermittent polymerization system, 5 g (0.008 mol) of structural regulator ethyl tetrahydrofurfuryl ether (20% mass concentration), 70 g of styrene, 630 g of butadiene and 3400 g of cyclopentane were added to the polymerization kettle. When the temperature in the kettle reached 35°C (initiation temperature), a mixed solution of 3.4 g (0.007 mol) of n-butyl lithium (15% mass concentration) and 3.4 g (0.007 mol) of cycloheximide (20% mass concentration) was added thereto to initiate the reaction and start polymerization. When the polymerization reaction reached the highest temperature of 115°C, the polymerization reaction time was 13 min. After the polymerization reaction reached the peak temperature (peak temperature is also called the highest temperature), the polymerization continued for about 30 min. 20 g of butadiene was added as a capping monomer. After reacting for 10 min, 1.0 g (0.0009 mol) of silicon tetrachloride (15% mass concentration) was added for coupling reaction. The coupling reaction temperature was 92°C. After reacting for 10 min, 4.5 g (0.0055 mol) branching modifier azobisisobutyronitrile (20% mass concentration) was used for branching modification reaction, the temperature of the branching modification reaction was 86°C, and finally it was terminated by trimethylchlorosilane. The obtained product was dried in a vacuum drying oven at 60°C for 12 hours to obtain intermittent modified solution-polymerized styrene-butadiene rubber. Among them, the molar ratio of the structure regulator to the lithium element in n-butyl lithium was 1.1:1, the molar ratio of cyclohexylimide to the lithium element in n-butyl lithium was 1:1, the molar ratio of silicon tetrachloride to the lithium element in n-butyl lithium was 0.13:1, the molar ratio of azobisisobutyronitrile to the lithium element in n-butyl lithium was 0.8:1, and the end-capping monomer accounted for 3.17% of the mass of the butadiene monomer.
[0116] The intermittently modified solution polymerized styrene butadiene rubber prepared in this example was characterized, and the results are shown in Table 1. As can be seen from Table 1, the intermittently modified solution polymerized styrene butadiene rubber is a random nonlinear solution polymerized styrene butadiene rubber.
[0117] Example 3 A method for preparing intermittently modified solution-polymerized styrene-butadiene rubber comprises the following steps: Under the conditions of the intermittent polymerization system, 5 g (0.008 mol) of structure regulator ethyl tetrahydrofurfuryl ether (20% mass concentration), 70 g of styrene, 630 g of butadiene, and 3400 g of cyclopentane were added to the polymerization kettle. When the temperature in the kettle reached 35°C (initiation temperature), a mixed solution of 3.4 g (0.007 mol) of n-butyl lithium (15% mass concentration) and 3.4 g (0.007 mol) of cycloheximide (20% mass concentration) was added thereto to initiate the reaction and start polymerization. When the polymerization reaction reached the highest temperature of 113°C, the polymerization reaction time was 14 min. After the polymerization reaction reached the peak temperature, the polymerization continued for about 30 min. 20 g of butadiene was added as a capping monomer. After reacting for 10 min, 1.3 g (0.0011 mol) of silicon tetrachloride (15% mass concentration) was added for coupling reaction. The coupling reaction temperature was 87°C. After reacting for 10 min, 5.5 g (0.0066 mol) branching modifier azobisisobutyronitrile (20% mass concentration) was used for branching modification reaction, the temperature of the branching modification reaction was 80°C, and finally it was terminated by trimethylchlorosilane. The obtained product was dried in a vacuum drying oven at 60°C for 12 hours to obtain intermittent modified solution-polymerized styrene-butadiene rubber. Among them, the molar ratio of the structure regulator to the lithium element in n-butyl lithium was 1.1:1, the molar ratio of cyclohexylimide to n-butyl lithium was 1:1, the molar ratio of silicon tetrachloride to the lithium element in n-butyl lithium was 0.16:1, the molar ratio of azobisisobutyronitrile to the lithium element in n-butyl lithium was 0.96:1, and the end-capping monomer accounted for 3.17% of the mass of the butadiene monomer.
[0118] The intermittently modified solution polymerized styrene butadiene rubber prepared in this example was characterized, and the results are shown in Table 1. As can be seen from Table 1, the intermittently modified solution polymerized styrene butadiene rubber is a random nonlinear solution polymerized styrene butadiene rubber.
[0119] Example 4 A method for preparing intermittently modified solution-polymerized styrene-butadiene rubber comprises the following steps: Under the conditions of the intermittent polymerization system, 9 g (0.014 mol) of structure regulator ethyl tetrahydrofurfuryl ether (20% mass concentration), 266 g of styrene, 434 g of butadiene, and 3400 g of cyclopentane were added to the polymerization kettle. When the temperature in the kettle reached 35°C (initiation temperature), a mixed solution of 2.6 g (0.0054 mol) of n-butyl lithium (15% mass concentration) and 2.3 g (0.0048 mol) of cycloheximide (20% mass concentration) was added thereto to initiate the reaction and start polymerization. When the polymerization reaction reached the highest temperature of 116°C, the polymerization reaction time was 13 min. After the polymerization reaction reached the peak temperature, the polymerization continued for about 30 min. 20 g of butadiene was added as a capping monomer. After the reaction for 10 min, 1.3 g (0.0011 mol) of silicon tetrachloride (15% mass concentration) for coupling reaction, the coupling reaction temperature is 89°C, after 10 minutes of reaction, 3.5g (0.0043 mol) (20% mass concentration) of azobisisobutyronitrile as a branching modifier is added for branching modification reaction, the branching modification reaction temperature is 82°C, and finally terminated with trimethylchlorosilane, and the obtained product is dried in a vacuum drying oven at 60°C for 12h to obtain intermittent modified solution-polymerized styrene-butadiene rubber. Among them, the molar ratio of the structure regulator to the lithium element in n-butyl lithium is 2.6:1, the molar ratio of cyclohexylimide to n-butyl lithium is 0.9:1, the molar ratio of silicon tetrachloride to the lithium element in n-butyl lithium is 0.22:1, the molar ratio of azobisisobutyronitrile to the lithium element in n-butyl lithium is 0.8:1, and the end-capping monomer accounts for 4.6% of the mass of the butadiene monomer.
[0120] The intermittently modified solution polymerized styrene butadiene rubber prepared in this example was characterized, and the results are shown in Table 1. As can be seen from Table 1, the intermittently modified solution polymerized styrene butadiene rubber is a random nonlinear solution polymerized styrene butadiene rubber.
[0121] Example 5 A method for preparing intermittently modified solution-polymerized styrene-butadiene rubber comprises the following steps: Under the conditions of the intermittent polymerization system, 9g (0.014 mol) of structure regulator ethyl tetrahydrofurfuryl ether (20% mass concentration), 266g of styrene, 434g of butadiene, and 3400g of cyclopentane were added to the polymerization kettle. When the temperature in the kettle reached 35°C (initiation temperature), a mixed solution of 2.6g (0.0054 mol) of n-butyl lithium (15% mass concentration) and 2.3g (0.0048 mol) of cycloheximide (20% mass concentration) was added thereto to initiate the reaction and polymerize. When the polymerization reaction reached the highest temperature of 106°C, the polymerization reaction time was 16min. About 30min after the polymerization reaction reached the peak temperature, 20g of butadiene was added as a capping monomer. After reacting for 10min, 1.3g (0.0011 mol) of silicon tetrachloride (15% mass concentration) was added for coupling reaction. The coupling reaction temperature was 87°C. After reacting for 10min, 4.5g (0.0055 mol) branching modifier azobisisobutyronitrile (20% mass concentration) was used for branching modification reaction, the temperature of branching modification reaction was 83°C, and finally it was terminated by trimethylchlorosilane. The obtained product was dried in a vacuum drying oven at 60°C for 12 hours to obtain intermittent modified solution-polymerized styrene-butadiene rubber. Among them, the molar ratio of the structure regulator to the lithium element in n-butyl lithium was 2.6:1, the molar ratio of cyclohexylimide to n-butyl lithium was 0.9:1, the molar ratio of silicon tetrachloride to the lithium element in n-butyl lithium was 0.22:1, the molar ratio of azobisisobutyronitrile to the lithium element in n-butyl lithium was 1:1, and the end-capping monomer accounted for 4.6% of the mass of the butadiene monomer.
[0122] The intermittently modified solution polymerized styrene butadiene rubber prepared in this example was characterized, and the results are shown in Table 1. As can be seen from Table 1, the intermittently modified solution polymerized styrene butadiene rubber is a random nonlinear solution polymerized styrene butadiene rubber.
[0123] Example 6 A method for preparing intermittently modified solution-polymerized styrene-butadiene rubber comprises the following steps: Under the conditions of the intermittent polymerization system, 9 g (0.014 mol) of structure regulator ethyl tetrahydrofurfuryl ether (20% mass concentration), 266 g of styrene, 434 g of butadiene, and 3400 g of cyclopentane were added to the polymerization kettle. When the temperature in the kettle reached 35°C (initiation temperature), a mixed solution of 2.6 g (0.0054 mol) of n-butyl lithium (15% mass concentration) and 2.6 g (0.0054 mol) of cycloheximide (20% mass concentration) was added thereto to initiate the polymerization reaction. The maximum polymerization temperature was 109°C, the polymerization reaction lasted for 15 min, and the polymerization continued for about 30 min after the polymerization reached the peak temperature. 20 g of butadiene was added as a capping monomer. After the reaction lasted for 10 min, 1.3 g (0.0011 mol) of silicon tetrachloride (15% mass concentration) for coupling reaction, the coupling reaction temperature is 82℃, after 10min of reaction, 5.5g (0.0067 mol) (20% mass concentration) of azobisisobutyronitrile as a branching modifier is added for branching modification reaction, the branching modification reaction temperature is 77℃, and finally terminated with trimethylchlorosilane, and the obtained product is dried in a vacuum drying oven at 60℃ for 12h to obtain intermittent modified solution-polymerized styrene-butadiene rubber. Among them, the molar ratio of the structure regulator to the lithium element in n-butyl lithium is 2.6:1, the molar ratio of cyclohexylimide to n-butyl lithium is 1:1, the molar ratio of silicon tetrachloride to the lithium element in n-butyl lithium is 0.22:1, the molar ratio of azobisisobutyronitrile to the lithium element in n-butyl lithium is 1.3:1, and the end-capping monomer accounts for 4.6% of the mass of the butadiene monomer.
[0124] The intermittently modified solution polymerized styrene butadiene rubber prepared in this example was characterized, and the results are shown in Table 1. As can be seen from Table 1, the intermittently modified solution polymerized styrene butadiene rubber is a random nonlinear solution polymerized styrene butadiene rubber.
[0125] Figure 1 The NMR spectrum of the solution-polymerized styrene-butadiene rubber prepared in this embodiment is shown. Figure 1 At around 3.7 ppm 1 The H MNR peak is attributed to the proton peak of the polymer obtained after branching modification.
[0126] It can be seen from Table 1 that under the same reaction time, the polymerization reaction temperature and the modification reaction temperature of the embodiment are both within the design range, and by comparison, it can be seen that when the molar ratio of the coupling agent to the lithium element in the organic lithium is (0.12 to 0.3):1, and the molar ratio of the branched modifier to the lithium element in the organic lithium is (0.8 to 1.4):1, the change in the molecular structure of the polymer can be achieved, thereby affecting the product performance.
[0127] Depend on Figure 1 It can be seen that after the polymerization, random nonlinear solution polymerized styrene butadiene rubber is obtained through coagulation and drying, and the sample is randomly distributed.
[0128] Comparative Example 1 Except that no branching modifier was added, the polymerization reaction temperature (here specifically the maximum temperature of the polymerization reaction) and the branching modification temperature were slightly changed, the rest of the contents of this comparative example were the same as those of Example 6. See Table 1 for specific process conditions and product characterization. Figure 2 The NMR spectrum of the solution-polymerized styrene-butadiene rubber prepared in this comparative example is shown.
[0129] Comparative Example 2 Except that no coupling agent was added, the polymerization reaction temperature (here specifically the maximum temperature of the polymerization reaction) and the branching modification temperature were slightly changed, the rest of the contents of this comparative example were the same as those of Example 6. See Table 1 for specific process conditions and product characterization.
[0130] Comparative Example 3 This comparative example is the same as Example 6 except that the molar ratio of the branching modifier to the lithium element in the organic lithium is 1.5:1, the polymerization temperature (here specifically the maximum temperature of the polymerization reaction) and the branching modification temperature are slightly changed. See Table 1 for specific process conditions and product characterization.
[0131] Comparative Example 4 Except that no functionalized modifier was added (initiator was n-butyl lithium), the polymerization temperature (here specifically the maximum temperature of the polymerization reaction) and the branching modification temperature were slightly changed, the rest of the contents of this comparative example were the same as those of Example 6. See Table 1 for specific process conditions and product characterization.
[0132] Table 1 Relevant process parameters, microstructure and randomness of intermittently modified solution-polymerized styrene-butadiene rubber Note: The polymerization reaction temperature specifically refers to the maximum temperature of the polymerization reaction.
[0133] As can be seen from Table 1, the intermittently modified solution-polymerized styrene-butadiene rubber obtained in Examples 1-3 have similar microstructures, and the intermittently modified solution-polymerized styrene-butadiene rubber obtained in Examples 4-6 have similar microstructures, and they all belong to random high Mooney viscosity solution-polymerized styrene-butadiene rubber. Comparative Examples 1-4 adjust the process conditions based on the technical solution of Example 6, and the intermittently modified solution-polymerized styrene-butadiene rubber obtained also has a random structure, but the microstructure changes, the molecular weight (Mn2) of the macromolecular peak is significantly reduced, and the Mooney viscosity of the raw rubber after modification is reduced.
[0134] Specifically, relative to Comparative Example 1, the molecular weight distribution of the intermittently modified solution-polymerized styrene-butadiene rubber prepared in Example 6 with the addition of a branched modifier is wider, and the Mooney viscosity of the modified raw rubber is higher. Therefore, the main function of the branched modifier is to widen the molecular weight distribution of the solution-polymerized styrene-butadiene rubber product and to increase the Mooney viscosity of the intermittently modified solution-polymerized styrene-butadiene rubber product.
[0135] Compared with Comparative Example 2, the molecular weight (Mn2) of the macromolecular peak of the intermittently modified solution-polymerized styrene-butadiene rubber prepared in Example 6 with the addition of a coupling agent is significantly increased, and the Mooney viscosity of the modified raw rubber is relatively high. Therefore, the addition of a coupling agent is beneficial to improving the Mooney viscosity of the intermittently modified solution-polymerized styrene-butadiene rubber product.
[0136] Compared with Comparative Example 3, the molar ratio of the branched modifier to the lithium element in the organic lithium in Example 6 is lower, the microstructure of the prepared intermittently modified solution-polymerized styrene-butadiene rubber has a higher content of bound benzene, the molecular weight of the base peak (Mn1) and the molecular weight of the macromolecular peak (Mn2) are relatively high, and the Mooney viscosity of the modified raw rubber is higher. Therefore, a reasonable usage ratio of the branched modifier to the organic lithium is beneficial to changing the microstructure of the intermittently modified solution-polymerized styrene-butadiene rubber product.
[0137] Comparative Example 5 This comparative example is the same as Example 3 except that no functionalized modifier is added (initiator is n-butyl lithium instead), the polymerization temperature and branching modification temperature are slightly changed. Specific process conditions and product characterization are shown in Table 1.
[0138] Mechanical properties of solution-polymerized styrene-butadiene rubber products The intermittently modified solution-polymerized styrene-butadiene rubber obtained in each embodiment and comparative example of the present invention and its mixed rubber and tire products were tested. The results are shown in Table 2.
[0139] Table 2 Related properties of intermittently modified solution-polymerized styrene-butadiene rubber, its compounded rubber and tire products .
[0140] As can be seen from Table 2, compared with Comparative Example 1, the mixed rubber Mooney of the product obtained in Example 6 is lower, the tensile strength is higher, the Akron wear and DIN wear of the tire product are lower, the anti-skid performance (tanδ, 0℃) is better, and the rolling resistance (tanδ, 60℃) is lower. Compared with Comparative Example 2, the tensile strength of the product obtained in Example 6 is higher, the anti-skid performance (tanδ, 0℃) is better, and the rolling resistance (tanδ, 60℃) is lower. Compared with Comparative Example 3, the tensile strength of the product obtained in Example 6 is higher, the anti-skid performance (tanδ, 0℃) is better, and the rolling resistance (tanδ, 60℃) is lower. Compared with Comparative Example 4, the tensile strength of the product obtained in Example 6 is higher, the anti-skid performance (tanδ, 0℃) is better, and the rolling resistance (tanδ, 60℃) is lower. For comparative example 5, the mixed rubber Mooney of the product obtained in Example 3 is lower, the tensile strength is higher, the Akron abrasion and DIN abrasion of the tire product are lower, the anti-skid performance (tanδ, 0℃) is better, and the rolling resistance (tanδ, 60℃) is lower. Therefore, from Examples 3 and 6, as well as Comparative Examples 1-5, it can be seen that the technical solution of the present invention is suitable for the production of intermittently modified solution-polymerized styrene-butadiene rubber with non-microstructure, which is beneficial to reducing the rolling resistance (tanδ, 60℃) of the tire product prepared from the solution-polymerized styrene-butadiene rubber product, thereby improving the fuel consumption performance of the tire product.
[0141] Combining the structural analysis of Table 1 and Table 2, it can be seen that the present invention introduces cyclic amine functional groups into the solution-polymerized styrene butadiene rubber product through a functionalized initiator, which affects the rolling resistance of the solution-polymerized styrene butadiene rubber product, and can reduce the rolling resistance (tanδ, 60°C) of the tire product prepared from the solution-polymerized styrene butadiene rubber product, thereby improving the fuel consumption performance of the tire product; the intermediate polymer is modified by a coupling agent, which can improve the Mooney viscosity and tensile strength of the solution-polymerized styrene butadiene rubber product. In addition, the present invention adopts a technical solution of first coupling and then branching the intermediate polymer product, which is conducive to forming a network molecular structure of the solution-polymerized styrene butadiene rubber product produced, thereby improving the mechanical properties of the product.
Claims
1. A method for preparing intermittently modified solution-polymerized styrene-butadiene rubber, It is characterized in that The preparation method comprises the following steps: 1) under intermittent polymerization conditions, styrene, butadiene, an organic solvent and a structure regulator are mixed to obtain a monomer-structure regulator mixed system, and then a functionalized initiator is added to the mixed system to initiate a reaction and perform a polymerization reaction to obtain an intermediate polymer; the functionalized initiator is prepared by reacting an organic lithium and a functionalized modifier; the functionalized modifier is an N-containing cyclic compound; 2) capping the intermediate polymer with a capping monomer to obtain a capped polymer; 3) using a coupling agent to carry out a coupling reaction on the end-capped polymer to obtain an end-capped coupled polymer; 4) using a branching modifier to carry out a branching modification reaction to obtain a capped coupled branched modified polymer; the branching modifier includes an organic peroxide that can generate oxygen-containing free radicals when heated and an azo compound that can generate free radicals; 5) adding a terminator to terminate the reaction, thereby obtaining the intermittently modified solution-polymerized styrene-butadiene rubber.
2. The method for preparing the intermittently modified solution-polymerized styrene-butadiene rubber according to claim 1, It is characterized in that In the step 1), the organic lithium includes at least one of n-butyl lithium, sec-butyl lithium, pentyl lithium, ethyl lithium, propyl lithium and isopropyl lithium; and the functionalized modifier includes at least one of cycloheximide and hexahydropyridine.
3. The method for preparing the intermittently modified solution-polymerized styrene-butadiene rubber according to claim 1, It is characterized in that The solution-polymerized styrene-butadiene rubber is produced by a single-pot polymerization system; the initiation reaction temperature is 30° C. to 60° C., the maximum polymerization reaction temperature is 80° C. to 140° C., the coupling reaction and the branching modification reaction temperatures are both 60° C. to 100° C., and the total polymerization reaction time is 0.5 h to 2 h; the total polymerization reaction time includes the polymerization reaction time after the initiation reaction, the coupling reaction time and the branching modification reaction time.
4. The method for preparing the intermittently modified solution-polymerized styrene-butadiene rubber according to claim 1, It is characterized in that The polymerization reaction is carried out under an inert gas protective atmosphere.
5. A method for preparing an intermittently modified solution-polymerized styrene-butadiene rubber according to any one of claims 1 to 4, It is characterized in that The organic lithium and the functionalized modifier have a molar ratio of Li to N of 1:0.8 to 1; or / and, The molar ratio of the structure regulator to the lithium element in the organic lithium is 0.4 to 6:1; or / and, The mass ratio of the butadiene to the styrene is 1.5 to 9:1; or / and, The molar ratio of the coupling agent to the lithium element in the organic lithium is 12 to 30:100; or / and, The amount of the end-capping monomer added is 0.5% to 5% of the amount of the butadiene monomer fed; or / and, The molar ratio of the branched modifier to the lithium element in the organic lithium is 0.5 to 1.4:
1.
6. A method for preparing an intermittently modified solution-polymerized styrene-butadiene rubber according to any one of claims 1 to 4, It is characterized in that In the step 1), the organic solvent comprises at least one hydrocarbon solvent selected from alkanes having 5 to 8 carbon atoms and cycloalkanes having 5 to 8 carbon atoms; or / and, In the step 1), the structure regulator is a polar Lewis base, including at least one of a strong polar Lewis base and a weak polar Lewis base; the strong polar Lewis base includes at least one of diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, dimethoxyethane, 2,2-di(2-tetrahydrofuranyl)propane and alkyl tetrahydrofurfuryl ether; or, the weak polar Lewis base includes at least one of tetrahydrofuran, p-dioxane, ethyl ether, triethylamine and sodium dodecylbenzene sulfonate; or / and, In the step 2), the end-capping monomer is at least one conjugated olefin compound selected from butadiene, pentadiene and isoprene; or / and, In the step 3), the coupling agent comprises at least one of a halide containing a two-arm structure, a halide containing a four-arm structure, and a siloxane compound containing a multi-arm structure of three arms or more; or / and, In the step 4), the organic peroxide includes at least one of a dialkyl peroxide and a diacyl peroxide; or the azo compound includes azobisisobutyronitrile; or / and, In the step 5), the terminator includes at least one of trimethylchlorosilane, anhydrous ethanol and fatty acid.
7. The method for preparing the intermittently modified solution-polymerized styrene-butadiene rubber according to claim 6, It is characterized in that In the step 1), the organic solvent comprises at least one of cyclohexane, hexane, cyclopentane, pentane, heptane, raffinate and benzene; or / and, In the step 1), the structure regulator is alkyl tetrahydrofurfuryl ether, wherein the alkyl group in the alkyl tetrahydrofurfuryl ether is an alkyl group with 1 to 9 carbon atoms.
8. The method for preparing the intermittently modified solution-polymerized styrene-butadiene rubber according to claim 6, It is characterized in that In the step 3), the halide containing a two-arm structure includes dichlorodiphenylsilane; or / and, the halide containing a four-arm structure includes at least one of silicon tetrachloride and tin tetrachloride; or, the siloxane compound contains at least one structure of an amino group, a methoxy group, a carboxyl group, a sulfhydryl group, a hydroxyl group and a phosphorus group; or / and, In the step 4), the organic peroxide contains an alkyl structure with 1 to 14 carbon atoms.
9. The method for preparing the intermittently modified solution-polymerized styrene-butadiene rubber according to claim 8, It is characterized in that The siloxane compound includes at least one of 3-chloropropyltrimethoxysilane, 3-chloropropyldimethoxymethylsilane and N-[3-(triethoxysilyl)propyl]-4,5-dihydroimidazole.
10. The method for preparing the intermittently modified solution-polymerized styrene-butadiene rubber according to claim 4, It is characterized in that In the step 1), before mixing styrene, butadiene, organic solvent and structure regulator, an inert gas is introduced into the reaction container.
11. A method for preparing an intermittently modified solution-polymerized styrene-butadiene rubber according to any one of claims 1 to 4, It is characterized in that In the step 5), a terminator is finally added to terminate the reaction to obtain a polymer product, and the polymer product is dried to obtain the intermittently modified solution-polymerized styrene-butadiene rubber; specifically comprising: The polymer product was transferred to a vacuum drying oven and dried at 60° C. to 70° C. for 12 to 13 hours.
12. An intermittently modified solution-polymerized styrene-butadiene rubber, It is characterized in that The intermittently modified solution-polymerized styrene-butadiene rubber is prepared by the method for preparing the intermittently modified solution-polymerized styrene-butadiene rubber according to any one of claims 1 to 11; The solution-polymerized styrene-butadiene rubber has a randomness of 100%, a bound benzene content of 10% to 40%, and a vinyl content of 30% to 70%.
Citation Information
Patent Citations
Hydrogenated amino functionalized styrene-butadiene rubber and preparation method thereof
CN111892669A
Functionalized solution polymerized styrene-butadiene rubber and preparation method thereof
CN116836335A
End-capped modified solution polymerized styrene-butadiene rubber and preparation method thereof
CN117487075A
Wide-distribution modified solution polymerized styrene-butadiene rubber and preparation method thereof
CN117487076A
Double-end functionalized solution polymerized styrene-butadiene rubber as well as preparation method and application thereof
CN117736375A
Cited By
Synthesis method of solution polymerized styrene-butadiene
CN120554572A
Method for testing and analyzing solution polymerized styrene-butadiene rubber
CN121027497A
A test and analysis method for solution-polymerized styrene-butadiene rubber
CN121027497B
Long-chain branching modification method of rare earth isoprene rubber and / or butadiene-isoprene rubber
CN122103413A