Battery cell coating and preparation method thereof
The three-layer powder coating of the battery cell is formed through plasma spraying process and heat treatment. Combined with the surface treatment of the sealant, it solves the problem of insufficient insulation protection performance of the power battery cell and achieves efficient insulation, adhesion and wear resistance properties, which is suitable for new applications. Battery cell production for energy vehicles.
Patent Information
- Application Number
- CN202411077245.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-10-25
AI Technical Summary
The existing power battery cell insulation protection process has problems such as average insulation performance, slow coating speed, low production efficiency, easy breakage, and poor compatibility with CTP/CTC structures. Existing powder coating materials cannot fully meet the requirements for cell insulation protection. .
Three layers of powder are sprayed sequentially using the plasma spraying process to form a base layer with a thickness of 25-75um, an intermediate layer with a thickness of 50-100um, and a working layer coating with a thickness of 100-1000um. The powders are phase-changed and fused through heat treatment, and finally immersed in the sealing agent. Method to form a surface protective layer, forming excellent insulation, adhesion and wear resistance.
It achieves the excellent insulation performance, moisture and heat resistance stability and high and low temperature impact performance of the battery cells. It has good adhesion to the aluminum substrate, is not easy to be damaged, and is corrosion-resistant. The process is simple and easy to produce on a large scale.
Smart Images

Figure CN118835192A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of power battery production, and specifically relates to a battery core coating and a preparation method thereof. Background Art
[0002] With the rapid development of new energy vehicles, power battery technology is also making continuous breakthroughs. Consumers have higher and higher requirements for driving range and fast charging speed, and the corresponding challenges for power batteries are also increasing. As the "heart" of new energy vehicles, power batteries face multiple challenges such as high voltage, high temperature and environmental corrosion. At present, the voltage platform of new energy vehicles is gradually increasing. Performance models such as Tesla Model Y, Xiaomi SU7 MAX, and Zeekr 007 have adopted 800V or even 1000V high-voltage platforms, which makes the insulation safety protection of battery cells particularly important.
[0003] In traditional power battery production, insulation protection between cells is mainly achieved by coating the cells with insulating films, which are usually blue or transparent organic films such as PET and PP. The industry calls the process of coating cells with PET films "blue film coating". However, the insulating film coating process has disadvantages such as general insulation performance, slow coating speed, low production efficiency, easy damage during the PACK process, and poor compatibility with structures such as CTP / CTC. It has gradually been replaced by new technical processes such as powder spraying and UV coating.
[0004] Powder spraying refers to the process of spraying powder materials onto the surface of a workpiece using a spray gun, and then forming a uniform coating after leveling and curing. Battery core powder spraying refers to the process of spraying powder materials onto the surface of a battery core using a powder spraying process, and then forming a coating after curing. This coating has excellent electrical insulation properties, and the adhesion and bonding strength between the coating and the substrate are high, which is more conducive to the realization of structures such as CTC / CTP, and is therefore favored by the new energy vehicle manufacturing industry.
[0005] However, in actual production and manufacturing, there are very few special powder coating materials suitable for battery cell spraying, and the existing powder coating materials cannot fully meet the many requirements of battery cell insulation protection. Summary of the invention
[0006] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a battery cell coating and a preparation method thereof, wherein the prepared battery cell coating has excellent insulation, adhesion, wear resistance, corrosion resistance and other properties.
[0007] To achieve the above object, the present invention provides the following technical solutions: In a first aspect, a method for preparing a battery cell coating is provided, comprising the following steps: S1. Spraying a first spraying powder on the outer surface of the battery cell housing substrate by a plasma spraying process to form a primer coating with a thickness of 25-75 um; S2, spraying a second spraying powder on the primer coating by a plasma spraying process to form an intermediate layer coating with a thickness of 50-100 um; S3, spraying the third spraying powder on the intermediate layer coating by a plasma spraying process to form a working layer coating with a thickness of 100-1000 um; S4, heating the sprayed battery cell shell to make the third spraying powder, the second spraying powder and the first spraying powder undergo phase change to obtain a heat-treated battery cell shell; S5. Post-treat the surface of the heat-treated battery cell shell by a sealing agent immersion method to form a surface protection layer with a thickness of 50-100 um.
[0008] In the present invention, the first spraying powder, the second spraying powder and the third spraying powder are sprayed on the outer surface of the battery cell shell base in sequence through a plasma spraying process, and then the three layers of spraying powder are made to undergo phase change and fuse together through heat treatment, and finally a surface protective layer is formed through surface post-treatment by a sealing agent immersion method, so that the battery cell shell with a coating has excellent insulation performance, moisture and heat stability and high and low temperature impact performance, good adhesion to the aluminum substrate, not easy to be damaged, and corrosion-resistant.
[0009] In some embodiments, in step S1, the first spraying powder is at least one of a self-fluxing aluminum-nickel alloy, an aluminum-chromium alloy, a nickel-molybdenum alloy, or an aluminum-nickel-chromium alloy.
[0010] The base coating formed by spraying the first spray powder plays an intermediate bonding role and has a relatively strong bonding with the aluminum substrate of the battery cell shell, and has a good bonding with the middle layer coating, so that the entire coating has good adhesion.
[0011] In some embodiments, in step S2, the second spraying powder is at least one of potassium titanate, silicon titanate and epoxy powder.
[0012] The intermediate layer coating formed by spraying the second spray powder can improve the durability of the coating, and at the same time has a certain insulation property and realizes impact resistance.
[0013] In some embodiments, in step S3, the third spraying powder is a spraying powder formed by sintering and ball milling at least one of aluminum oxide, silicon oxide, zirconium oxide, calcium oxide, silicon carbide, silicon nitride and yttrium oxide.
[0014] The working layer coatings formed by spraying the second spray powder are all insulating materials. On the basis of the previous two layers of coatings, they further achieve insulation, moisture and heat resistance, and high and low temperature impact performance.
[0015] In some embodiments, in steps S1, S2, and S3, the plasma spraying process includes: Using atmospheric plasma spraying APS technology, with at least one of nitrogen N2 and argon Ar2 as the main gas source, the flow rate is controlled at 30-80 g / min -1 , powder feeding rate 2-10 L / min -1 , spraying distance 50-500mm, spraying angle 0-180°, spray gun moving speed 0.1-1 m / s -1 Spraying is carried out under the conditions of.
[0016] The above plasma spraying process combined with spraying powder can achieve good adhesion and surface flatness for each layer of coating, and further improve the impact strength, moisture and heat resistance, and high and low temperature impact performance of the entire coating.
[0017] In some embodiments, in step S4, the battery cell shell after spraying is heated by infrared heating, specifically comprising: using an infrared heater with a power of 500-1000W, heating at a position 10-30cm away from the battery cell shell for 200-400s.
[0018] The above-mentioned infrared heating method can quickly and effectively realize the hot melting of the three-layer coating spray powder, so that the three layers of spray powder undergo phase change and fuse together to form a completely dense insulating coating structure. On the basis of each realizing its own function, they combine with each other to further improve the insulation, impact resistance, moisture and heat resistance and high and low temperature impact performance of the entire coating.
[0019] In some embodiments, step S5 includes: Using one or more of aluminum phosphate, sodium silicate, ethyl silicate, and silicon dioxide as the sealing agent solution; The heat-treated battery cell casing is immersed in the sealing agent solution for treatment.
[0020] Through the above-mentioned sealing agent solution immersion treatment, a surface protection layer with a thickness of 50-100um is formed after drying, which has an anti-oxidation effect and further improves the moisture and heat resistance and high and low temperature impact performance.
[0021] In some embodiments, before step S1, the method further includes: pre-treating the battery cell casing substrate to make the battery cell casing substrate clean.
[0022] Furthermore, the pre-treatment of the battery cell shell base includes: treating the battery cell shell base in at least one of the following ways: degreasing, rust removal, sandblasting, cleaning agent immersion, cleaning agent wiping, and plasma cleaning.
[0023] The above-mentioned substrate pretreatment can ensure the cleanliness of the surface of the battery cell shell, so as to better combine with the spray layer and improve the adhesion and surface smoothness of the entire coating.
[0024] In some embodiments, the thickness of the primer coating is 25-75um; the thickness of the intermediate layer coating is 50-500um; the thickness of the working layer coating is 100-1500um; and the thickness of the surface protection layer is 20-100um. More preferably, the thickness of the primer coating is 40-60um; the thickness of the intermediate layer coating is 200-400um; the thickness of the working layer coating is 400-1200um; and the thickness of the surface protection layer is 30-70um.
[0025] It should be noted that the present invention has been found through experiments that by controlling the thickness of each coating of the base coating, the intermediate coating, and the working layer coating, the relative proportion of the first spraying powder, the second spraying powder, and the third spraying powder can be controlled, and the three layers of spraying powder undergo phase change and fuse together through heat treatment, which is conducive to obtaining relatively better insulation, impact strength, moisture and heat resistance, and high and low temperature impact performance. In addition, controlling the thickness of the surface protective layer is conducive to obtaining relatively better anti-oxidation effect, while further improving moisture and heat resistance and high and low temperature impact performance.
[0026] In a second aspect, a battery cell coating is provided, which is prepared by the preparation method described in the first aspect.
[0027] The battery cell coating prepared by the preparation method described in the first aspect can form a completely dense insulating coating structure, and has excellent insulation performance, moisture and heat resistance stability, and high and low temperature impact performance.
[0028] Compared with the prior art, the present invention has the following beneficial effects: The battery cell coating prepared by the present invention has excellent insulation, adhesion, wear resistance, corrosion resistance and other properties. Compared with the traditional insulation film coating process, the present invention uses powder coating to form a completely dense insulation coating structure, has excellent insulation performance, moisture and heat stability and high and low temperature impact performance, good adhesion to aluminum substrate, not easy to break, corrosion resistance, simple process, good product quality, easy to implement on a large scale in battery cell production. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1It is a schematic flow chart of a method for preparing a battery cell coating according to an embodiment of the present invention. DETAILED DESCRIPTION
[0030] The present invention will be further described below in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and cannot be used to limit the protection scope of the present invention.
[0031] Example 1
[0032] like Figure 1 As shown, a method for preparing a battery cell coating comprises the following steps: S1. Pretreatment of the battery cell substrate: First, use an ethanol solution with a purity of more than 99.5% to clean the surface of the battery cell shell. After standing for 5 minutes to allow the ethanol to evaporate, use a plasma cleaning machine to plasma clean the battery cell shell at a power of 1100W, a speed of 90mm / s and a cleaning height of 8mm.
[0033] S2, base coating spraying: through atmospheric plasma spraying (APS) technology, using nitrogen N2 as the gas source, controlled at a flow rate of 50 L / min -1 , powder feeding rate 4.5 L / min -1 , spraying distance 110mm, spraying angle 90°, spray gun moving speed 0.5m / s -1 Under the conditions of spraying the self-fluxing nickel-clad aluminum first spraying powder on the aluminum substrate of the battery core to form a 50um primer coating.
[0034] S3, intermediate layer spraying: through atmospheric plasma spraying (APS) technology, using nitrogen N2 as the gas source, controlled at a flow rate of 50 L / min -1 , powder feeding rate 3.6 L / min -1 , spraying distance 85mm, spraying angle 90°, spray gun moving speed 0.5m / s -1 Under the conditions of , a second spraying powder mixed with potassium titanate and silicon titanate in a mass ratio of 1:0.35 is sprayed on the primer coating to form a 300um intermediate layer coating.
[0035] S4, working layer spraying: Alumina, silicon oxide, zirconium oxide, silicon nitride and yttrium oxide with a mass ratio of 14:52:24:5:5 are first calcined in an air furnace at 1100°C for 30 minutes, and then ball-milled to form a particle size of less than 3um to obtain the third spraying powder. Through atmospheric plasma spraying (APS) technology, nitrogen N2 is used as the gas source and the flow rate is controlled at 50 L / min -1 , powder feeding rate 2.2 L / min -1 , spraying distance 85mm, spraying angle 90°, spray gun moving speed 0.3m / s -1Under the conditions, the third spraying powder is sprayed on the middle layer, and a working layer coating of 1000um is formed.
[0036] S5, phase change heat treatment: using an 800W infrared heater to heat the sprayed battery cell shell for 300s at a distance of 20cm from the workpiece, so that the coating material undergoes phase change and improves performance; S6. Surface post-treatment: Disperse 5% silicon dioxide into 100% aluminum phosphate solution, adjust the pH to 3.5-4.0 to form an immersion solution, and perform surface post-treatment on the sprayed battery shell workpiece by immersion method. After drying at 80°C, a 50um surface protection layer is formed.
[0037] Example 2
[0038] The difference from Example 1 is that in step S5, the power of the infrared heater is 500 W and the heating time is 200 s.
[0039] Example 3
[0040] The difference from Example 1 is that in step S4, the third spraying powder uses aluminum oxide, silicon oxide, zirconium oxide, silicon nitride and yttrium oxide in a mass ratio of 18:42:28:8:4, and the thickness of the working layer coating is 500 um.
[0041] Examples 1 to 3 are all based on the method of the present invention, with only some coating ratios and process conditions being changed.
[0042] The comparative example is a sample implemented by the PET blue film coating process traditionally used in the industry.
[0043] The workpieces obtained from the three embodiments and the comparative example were tested for insulation, adhesion, surface flatness, impact strength, moisture and heat resistance, and high and low temperature impact performance. The test results are shown in Table 1.
[0044] Table 1
[0045] As can be seen from Table 1, overall, the various properties of the battery cell coatings prepared in Examples 1 to 3 are excellent, especially the insulation performance and environmental corrosion resistance have very small differences, which far exceed the standards and requirements of the traditional industry processes of the comparative examples. This shows that the battery cell coating prepared in the embodiments of the present invention has excellent insulation, adhesion, damage resistance, corrosion resistance and other properties, and can be used in the production of power battery cells through powder spraying.
[0046] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a battery core coating, characterized in that: The following steps are involved: S1, spraying a first spraying powder on the outer surface of the battery cell housing substrate by a plasma spraying process to form a primer coating; S2, spraying a second spraying powder on the primer coating by a plasma spraying process to form an intermediate layer coating; S3, spraying a third spraying powder on the intermediate layer coating by a plasma spraying process to form a working layer coating; S4, heating the sprayed battery cell shell to make the third spraying powder, the second spraying powder and the first spraying powder undergo phase change to obtain a heat-treated battery cell shell; S5. Post-treating the surface of the heat-treated battery cell shell by a sealing agent immersion method to form a surface protective layer.
2. The preparation method according to claim 1, characterized in that: In step S1, the first spraying powder is at least one of a self-fluxing aluminum-nickel alloy, an aluminum-chromium alloy, a nickel-molybdenum alloy, and an aluminum-nickel-chromium alloy.
3. The preparation method according to claim 1, characterized in that: In step S2, the second spraying powder is at least one of potassium titanate, silicon titanate and epoxy powder.
4. The preparation method according to claim 1, characterized in that: In step S3, the third spraying powder is a spraying powder formed by sintering and ball milling at least one of aluminum oxide, silicon oxide, zirconium oxide, calcium oxide, silicon carbide, silicon nitride, and yttrium oxide.
5. The preparation method according to claim 1, characterized in that: In steps S1, S2 and S3, the plasma spraying process includes: Using atmospheric plasma spraying APS technology, with at least one of nitrogen N2 and argon Ar2 as the main gas source, the flow rate is controlled at 30-80 g / min -1 , powder feeding rate 2-10 L / min -1 , spraying distance 50-500mm, spraying angle 0-180°, spray gun moving speed 0.1-1 m / s -1 Spraying is carried out under the conditions of.
6. The preparation method according to claim 1, characterized in that: In step S4, the battery cell shell after spraying is heated by infrared heating, specifically including: using an infrared heater with a power of 500-1000W, heating at a position 10-30cm away from the battery cell shell for 200-400s.
7. The preparation method according to claim 1, characterized in that: Step S5 includes: Using one or more of aluminum phosphate, sodium silicate, ethyl silicate, and silicon dioxide as the sealing agent solution; The heat-treated battery cell casing is immersed in the sealing agent solution for treatment.
8. The preparation method according to claim 1, characterized in that: Before step S1, the method further includes: pre-treating the battery cell shell substrate to make the battery cell shell substrate clean; The pretreatment of the battery cell shell base includes: treating the battery cell shell base by at least one of degreasing, rust removal, sandblasting, cleaning agent immersion, cleaning agent wiping, and plasma cleaning.
9. The preparation method according to any one of claims 1 to 8, characterized in that: At least one of the following is met: The thickness of the primer coating is 25-75um; The thickness of the intermediate layer coating is 50-500um; The thickness of the working layer coating is 100-1500um; The thickness of the surface protection layer is 20-100 um.
10. A battery cell coating, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Cited By
Curable electrical insulation tape
EP4578921A1