Corrosion test device and method for simulating metal material in frozen soil environment

By using activated carbon, vanadium and silica gel as soil carriers, combined with spraying systems and infrared heating lamps, the freeze-thaw cycle of the frozen soil area is simulated, and the problem that the existing technology cannot effectively simulate the frozen soil environment is solved, and the metal materials are realized High-efficiency corrosion test provides real and fast test data, meeting the corrosion research needs of metal materials in permafrost environment.

CN118883403APending Publication Date: 2024-11-01ANGANG STEEL CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202410838269.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing permafrost environment simulation test device cannot effectively simulate the active layer and permafrost layer in permafrost, and cannot truly simulate the corrosion of metal materials in the permafrost environment, resulting in inaccurate data and inability to meet the development of metal materials. need.

Method used

Use activated carbon, vanadium and silicone as soil carriers, combined with spraying systems and infrared heating lamps to simulate the freeze-thaw cycle of the frozen soil area, and obtain corrosion data of metal materials through electrochemical testing systems to achieve various environments in the frozen soil area. All-round simulation.

Benefits of technology

It realizes efficient corrosion tests of metal materials in permafrost environments, provides real and fast test data, reduces operating costs, has excellent simulation and acceleration, and can simulate multiple test parameters in the laboratory. Frost soil area test.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118883403A_ABST
    Figure CN118883403A_ABST
Patent Text Reader

Abstract

The invention provides a test device and method for simulating corrosion of a metal material in a frozen soil environment, and the method comprises the steps: adjusting the positions of a to-be-tested metal, an auxiliary electrode and a reference electrode, and enabling an electrochemical test system to obtain electrochemical measurement data in real time according to the auxiliary electrode, the reference electrode and the to-be-tested metal; the spraying duration, the negative temperature duration and the heating duration are set, and the temperature and humidity control system adopts a spraying system to control a spray head to spray the simulation liquid according to the spraying duration; after the spray head stops spraying, a simulation experiment is carried out; the simulation experiment is repeated, when the preset experiment time is met, the to-be-measured metal is taken out, the corrosion result is obtained according to one or more of corrosion weight loss, corrosion products and electrochemical measurement data of the to-be-measured metal, the manufacturing and operation cost is low, and the method has excellent simulation performance, acceleration performance and simple operability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of metal material corrosion testing, and in particular to a corrosion testing device and method for simulating metal materials in a frozen soil environment. Background Art

[0002] Frozen soil is a rock mass below 0℃ and containing ice. In my country, the area of ​​frozen soil accounts for more than 70% of the total land area. Under the harsh soil conditions and the combined effects of multiple factors, buried metal pipelines for oil transportation and urban pipelines, including gas pipelines and water pipelines, will cause varying degrees of corrosion and deformation, endangering life safety.

[0003] Frozen soil is composed of ice-containing soil or rock with a temperature below 0°C. Its physical properties are mainly controlled by the ice content, which is closely related to temperature. The soil temperature changes with the change of climate and seasons, and the properties of the frozen soil also change accordingly. Frozen soil thaws periodically with the change of seasons. If the soil freezes in winter and melts completely in summer, it is called seasonal frozen soil. If the soil layer is frozen for many years, or at least frozen for three consecutive years, it is called permafrost. The frozen soil in the permafrost area is divided into two layers, the upper layer melts in summer every year and freezes in winter, which is called the active layer; the lower layer is frozen all year round, which is called the permafrost layer.

[0004] The test methods for frozen soil corrosion mainly include outdoor field burial method and indoor simulation and acceleration method. The outdoor field burial method is the most basic method in the study of frozen soil corrosion. Its data is real and objective, but its disadvantages are long cycle, limited and scattered data, which is not conducive to the research and development of new steel grades. Compared with the burial method, the indoor simulation and acceleration method has the characteristics of easy control of test conditions, accurate parameter measurement and short test cycle, and has been widely adopted.

[0005] Regarding the test device and method for simulating the frozen soil environment, the patent document with application number 201210167742.4 discloses a tunnel drainage system and its setting method that passes through the permafrost area and the non-frozen soil area. This method is mainly used to simulate the drainage of the tunnel in the frozen soil area, and has nothing to do with the corrosion device and method for simulating the frozen soil area. The patent document with application number 201911217125.9 discloses a special device and research method for indoor testing of seasonal frozen soil. This method can perform a unidirectional freezing process of the soil according to the test requirements, and set different freezing depths to simulate seasonal frozen soil. The device is used for the freeze-thaw cycle of frozen soil, and is mainly used to observe the deformation of the land. Moreover, the device can only simulate seasonal frozen soil, and cannot simulate the active layer and permafrost in permafrost. It has limitations and is not a test device and method specifically for studying the corrosion of metals in frozen soil environments. The patent document with application number 202210932208.1 discloses a non-negative temperature frozen soil pile foundation model test system and test method. The device uses absorbent resin to simulate ice in a frozen soil environment, thereby simulating the influence of the frost heave, thaw and sinking deformation of the frozen soil layer on the force and displacement of the pile foundation. This method is also a test device for observing soil deformation, and is not a device and method specifically used for conducting corrosion tests in frozen soil environments. "Comprehensive Corrosion Prevention and Control" discloses that soils with different water contents are loaded into an electrolytic cell to conduct a study on electrochemical corrosion behavior. This method only examines the influence of soils with different water contents on corrosion behavior. The test was conducted at room temperature. The simulated corrosion environment is quite different from the environment in the frozen soil zone, and it is impossible to truly simulate the frozen soil environment.

[0006] In view of this, the present invention provides a corrosion test device and method for simulating metal materials in a frozen soil environment. Summary of the invention

[0007] In view of the above-mentioned shortcomings, a corrosion test device and method for simulating metal materials in a frozen soil environment are provided. The present invention mainly uses activated carbon, vanadium, and silica gel to simulate soil, inserts the metal to be tested into the simulated soil, and uses a spray system and an infrared heating lamp to simulate the frozen soil environment for experiments. After the experiment, the corrosion data of the metal material in the frozen soil environment can be analyzed based on the corrosion weight loss of the metal to be tested, the corrosion products, and the electrochemical data during the experiment.

[0008] The technical means adopted by the present invention are as follows:

[0009] In one aspect, the present invention provides a corrosion test device for simulating metal materials in a frozen soil environment, comprising:

[0010] The box body comprises a bottom plate and a top plate which are arranged opposite to each other in a direction perpendicular to the ground, wherein the bottom plate is located on a side of the top plate close to the ground; the soil carrier, the infrared heating lamp and the nozzle are arranged in the box body;

[0011] The soil carrier comprises: an activated carbon layer, which is arranged on the side of the bottom plate close to the top plate; a bauxite layer, which is arranged on the side of the activated carbon layer close to the top plate; and a silica gel layer, which is arranged on the side of the bauxite layer close to the top plate.

[0012] The infrared heating lamp is arranged on a side of the top plate close to the silicone layer;

[0013] The nozzle is arranged on a side of the top plate close to the silicone layer, and the nozzle is connected to the spray system;

[0014] A temperature and humidity control system connected to the spray system and the infrared heating lamp;

[0015] The electrochemical testing system is connected with an auxiliary electrode, a reference electrode and a metal to be tested, wherein the auxiliary electrode, the reference electrode and the metal to be tested are inserted into the soil carrier.

[0016] Preferably, the spray system comprises:

[0017] A simulated liquid containing device, located outside the box;

[0018] A water pipe has one end located in the top plate and the other end connected to the simulated liquid containing device, and the nozzle is connected to the water pipe; a spray control system is provided on the water pipe between the top plate and the simulated liquid containing device.

[0019] Preferably, it also includes:

[0020] The bottom plate is provided with a cavity inside, and the bottom plate is provided with a plurality of holes, the holes connecting the cavity and a side of the bottom plate close to the top plate; the bottom plate is provided with a lead-out connector, the lead-out connector connecting the cavity.

[0021] Preferably, it also includes:

[0022] The sample rack is a frame structure, the sample rack is inserted into the soil carrier, and the metal to be tested is inserted into the sample rack.

[0023] On the other hand, the present invention also provides a method for simulating the corrosion test of metal materials in a frozen soil environment, which is applied to a device for simulating the corrosion test of metal materials in a frozen soil environment, comprising:

[0024] The box body comprises a bottom plate and a top plate which are arranged opposite to each other in a direction perpendicular to the ground, wherein the bottom plate is located on a side of the top plate close to the ground; the soil carrier, the infrared heating lamp and the nozzle are arranged in the box body;

[0025] The soil carrier comprises: an activated carbon layer, which is arranged on the side of the bottom plate close to the top plate; a bauxite layer, which is arranged on the side of the activated carbon layer close to the top plate; and a silica gel layer, which is arranged on the side of the bauxite layer close to the top plate.

[0026] The infrared heating lamp is arranged on a side of the top plate close to the silicone layer;

[0027] The nozzle is arranged on a side of the top plate close to the silicone layer, and the nozzle is connected to the spray system;

[0028] A temperature and humidity control system connected to the spray system and the infrared heating lamp;

[0029] An electrochemical testing system, connected with an auxiliary electrode, a reference electrode and a metal to be tested, wherein the auxiliary electrode, the reference electrode and the metal to be tested are inserted into the soil carrier;

[0030] Test methods, including:

[0031] S1: adjusting the position of the metal to be tested, the shortest distance between the auxiliary electrode and the metal to be tested is in the range of 3.5 cm to 4 cm, the shortest distance between the reference electrode and the metal to be tested is in the range of 1.5 cm to 2.5 cm, and the electrochemical test system acquires electrochemical measurement data in real time according to the auxiliary electrode, the reference electrode and the metal to be tested;

[0032] S2: setting the spraying time, negative temperature time and heating time, the temperature and humidity control system uses the spraying system to control the nozzle to spray the simulated liquid according to the spraying time;

[0033] S3: After the nozzle stops spraying, a simulation experiment is performed, including: placing the simulated metal material corrosion test device in a frozen soil environment under negative temperature conditions for a negative temperature period, and then the temperature and humidity control system controls the infrared heating lamp to continue heating according to the heating period;

[0034] S4: Repeat the simulation experiment of S3. When the set experimental time is met, take out the metal to be tested, and obtain the corrosion result according to one or more of the corrosion weight loss, corrosion products and electrochemical measurement data of the metal to be tested.

[0035] Preferably, the corrosion test device for simulating metal materials in a frozen soil environment further comprises: a sample rack, which is a frame structure, the sample rack is inserted into the soil carrier, and the metal to be tested is inserted into the sample rack;

[0036] The step of adjusting the position of the metal to be tested comprises:

[0037] The metal to be tested is inserted into the sample holder in a direction perpendicular to the ground, or the metal to be tested is inserted into the sample holder in a direction parallel to the ground.

[0038] Preferably, the spray system comprises: a simulated liquid containing device, located outside the box; a water pipe, one end of which is located inside the top plate and the other end is connected to the simulated liquid containing device, and the spray head is connected to the water pipe; between the top plate and the simulated liquid containing device, the water pipe is provided with a spray control system;

[0039] Before setting the spraying time, the negative temperature time and the heating time, the method further includes:

[0040] The simulated liquid is configured and loaded into the simulated liquid containing device.

[0041] Preferably, before setting the spraying time, the negative temperature time and the heating time, the method further comprises:

[0042] Set the temperature control range and humidity control range of the temperature and humidity control system.

[0043] Compared with the prior art, the present invention has the following advantages:

[0044] 1. The corrosion test device and method for simulating metal materials in a frozen soil environment provided by the present invention have low manufacturing and operation costs, and have excellent simulation, acceleration, and simple operability.

[0045] 2. The corrosion test device and method for simulating metal materials in a frozen soil environment provided by the present invention use activated carbon, alumina, and silica gel as soil carriers, which can not only absorb the solution to simulate ice when frozen, but also simulate rocks due to their granular structure. In addition, the three soil carriers can absorb various salt ions in the simulated soil solution, and fully consider the characteristics that the soil water content in the frozen soil area gradually increases from top to bottom. The three soil carriers are set in the box in the order of silica gel, alumina, and activated carbon from top to bottom, which can more realistically and effectively simulate the change of water content in the frozen soil area caused by the change of soil depth.

[0046] 3. The present invention provides a corrosion test device and method for simulating metal materials in a frozen soil environment. The temperature control system and the spray system control can simulate the periodic thawing of short-term frozen soil, the periodic freezing and thawing of seasonal frozen soil, and the long-term freezing of permafrost, thereby simulating various environments in frozen soil areas in an all-round way.

[0047] 4. The corrosion test device and method for simulating metal materials in a frozen soil environment provided by the present invention can carry out simulated frozen soil area tests with various test parameters in the laboratory through test parameters and process control, and can obtain a large amount of scientific and reasonable test data in a relatively short time, providing a convenient test method for studying the corrosion and development of metal materials in a frozen soil environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0049] Figure 1 A structural schematic diagram of a corrosion test device for simulating metal materials in a frozen soil environment provided by the present invention.

[0050] In the figure: 1. Box body; 2. Activated carbon layer; 3. Alumina layer; 4. Silica gel layer; 5. Infrared heating lamp; 6. Nozzle; 7. Temperature and humidity control system; 8. Electrochemical test system; 9. Auxiliary electrode; 10. Reference electrode; 11. Metal to be tested; 12. Simulated liquid containing device; 13. Water pipe; 14. Spray control system; 15. Lead-out connector; 16. Sample rack. DETAILED DESCRIPTION

[0051] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0052] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0053] Combination Figure 1 , Figure 1 A structural schematic diagram of a corrosion test device for simulating metal materials in a frozen soil environment provided by the present invention is provided to illustrate a specific embodiment of the corrosion test device for simulating metal materials in a frozen soil environment provided by the present invention, including:

[0054] The box body 1 comprises a bottom plate and a top plate which are arranged opposite to each other in a direction perpendicular to the ground, wherein the bottom plate is located on a side of the top plate close to the ground; a soil carrier, an infrared heating lamp 5 and a nozzle 6 are arranged in the box body 1;

[0055] The soil carrier comprises: an activated carbon layer 2, which is arranged on the side of the bottom plate close to the top plate; a vanadium layer 3, which is arranged on the side of the activated carbon layer 2 close to the top plate; and a silica gel layer 4, which is arranged on the side of the vanadium layer 3 close to the top plate.

[0056] The infrared heating lamp 5 is arranged on one side of the top plate close to the silicone layer 4;

[0057] The nozzle 6 is arranged on one side of the top plate close to the silicone layer 4, and the nozzle 6 is connected to the spray system;

[0058] A temperature and humidity control system 7 connected to the spray system and the infrared heating lamp 5;

[0059] The electrochemical testing system 8 is connected with an auxiliary electrode 9, a reference electrode 10 and a metal to be tested 11, and the auxiliary electrode 9, the reference electrode 10 and the metal to be tested 11 are inserted into a soil carrier.

[0060] It is understandable that the material of the box 1 is transparent plexiglass, which is convenient for observation during operation. The box 1 is filled with activated carbon, alumina and silica gel, which can not only adsorb the solution to simulate ice when frozen, but also simulate rocks due to its granular structure. Activated carbon, alumina and silica gel are all adsorbent. These three carriers can fully adsorb various salt ions in the simulated soil solution, and the order of the adsorption capacity of the three carriers is activated carbon> alumina> silica gel. Therefore, the different soil moisture contents in the real frozen soil area are simulated according to the different adsorption capacities of the three carriers. Considering that the soil moisture content in the frozen soil area environment increases from top to bottom, the three soil carriers are set in the box 1 in the order of silica gel, alumina and activated carbon from top to bottom.

[0061] An infrared heating lamp 5 and a nozzle 6 are arranged on the upper part of the box 1. Under the control of the temperature and humidity control system 7, infrared heating or spraying is performed according to the experimental needs to simulate the periodic freezing and thawing of seasonal frozen soil, the periodic thawing of short-term frozen soil, or the long-term freezing of permafrost.

[0062] The electrochemical testing system 8 is connected to the metal to be tested 11, the auxiliary electrode 9 and the reference electrode 10 respectively. The electrochemical testing system 8 is used to measure the polarization resistance, corrosion current, etc. of the metal to be tested 11 during the embedding process, and can calculate the instantaneous corrosion rate of the metal to be tested 11.

[0063] Activated carbon, bauxite and silica gel are used as soil carriers for simulating frozen soil environment and placed in layers, and a solution with the same physical and chemical properties as the target frozen soil environment is prepared and mixed with the target soil. The metal 11 to be tested is placed in the simulated soil, and controlled by the temperature and humidity control system 7 and the spray system to simulate the periodic freezing and thawing of seasonal frozen soil, the periodic thawing of short-term frozen soil or the long-term freezing of permafrost.

[0064] Compared with the prior art, the present invention has the following advantages:

[0065] The corrosion test device and method for simulating metal materials in a frozen soil environment provided by the present invention have low manufacturing and operation costs, excellent simulation, acceleration, and simple operability. The corrosion test device and method for simulating metal materials in a frozen soil environment provided by the present invention adopt activated carbon, alumina, and silica gel as soil carriers, which can not only adsorb solutions to simulate ice when frozen, but also simulate rocks due to their own granular structure. In addition, the three soil carriers can adsorb various salt ions in the simulated soil solution, and fully consider the characteristics that the soil water content in the frozen soil area gradually increases from top to bottom. The three soil carriers are arranged in the box 1 in the order of silica gel, alumina, and activated carbon from top to bottom, which more realistically and effectively simulates the change of water content in the frozen soil area caused by the change of soil depth. The corrosion test device and method for simulating metal materials in a frozen soil environment provided by the present invention, the temperature control system and the spray system control to achieve the simulation of the periodic thawing of short-term frozen soil, the periodic freezing and thawing of seasonal frozen soil, and the long-term freezing of permafrost, and simulate various environments in the frozen soil area in an all-round way. The present invention provides a corrosion test device and method for simulating metal materials in a frozen soil environment. Through test parameter and process control, simulated frozen soil area tests with various test parameters can be carried out in the laboratory, and a large amount of scientific and reasonable test data can be obtained in a relatively short time, providing a convenient test method for studying the corrosion and development of metal materials in a frozen soil environment.

[0066] In some optional embodiments, continue to refer to Figure 1 , sprinkler system, including:

[0067] The simulated liquid containing device 12 is located outside the box 1;

[0068] The water pipe 13 has one end located in the top plate and the other end connected to the simulated liquid containing device 12 . The nozzle 6 is connected to the water pipe 13 . A spray control system 14 is provided on the water pipe 13 between the top plate and the simulated liquid containing device 12 .

[0069] It can be understood that the simulated liquid is extracted from the simulated liquid containing device 12 for spraying to replenish the solution for the soil carrier.

[0070] In some optional embodiments, continue to refer to Figure 1 The corrosion test device for simulating metal materials in a frozen soil environment provided in this embodiment also includes:

[0071] A cavity is arranged in the bottom plate, and a plurality of holes are arranged in the bottom plate, and the holes are connected with the cavity and a side of the bottom plate close to the top plate; a lead-out connector 15 is arranged in the bottom plate, and the lead-out connector 15 is connected with the cavity.

[0072] It is understandable that the cavity is a waste liquid collection box for collecting the solution overflowed from the soil carrier during spraying or heating. The outlet connector 15 is used to outlet the waste liquid collected in the cavity.

[0073] In some optional embodiments, continue to refer to Figure 1 The corrosion test device for simulating metal materials in a frozen soil environment provided in this embodiment also includes:

[0074] The sample rack 16 is a frame structure. The sample rack 16 is inserted into the soil carrier, and the metal 11 to be tested is inserted into the sample rack 16 .

[0075] It is understandable that the sample holder 16 is used to fix the position of the metal to be tested 11. The metal to be tested 11 can be inserted into the sample holder 16 in a direction perpendicular to the ground or in a direction parallel to the ground, so as to carry out a long-scale test or a small-size test piece test. The long-scale test is used to simulate the corrosion of a large structure in a complex frozen soil environment, and the small-size test piece test is used to simulate the corrosion of a small test piece in a single frozen soil environment.

[0076] When the sample rack 16 is placed with dissimilar metals, it can be used to simulate the corrosion condition of different metal samples after coupling. At this time, the electrochemical testing system 8 can measure the galvanic potential and the galvanic current.

[0077] Continue to refer to Figure 1 The present invention also provides a method for simulating the corrosion test of metal materials in a frozen soil environment, which is applied to a device for simulating the corrosion test of metal materials in a frozen soil environment, comprising:

[0078] The box body 1 comprises a bottom plate and a top plate which are arranged opposite to each other in a direction perpendicular to the ground, wherein the bottom plate is located on a side of the top plate close to the ground; a soil carrier, an infrared heating lamp 5 and a nozzle 6 are arranged in the box body 1;

[0079] The soil carrier comprises: an activated carbon layer 2, which is arranged on the side of the bottom plate close to the top plate; a vanadium layer 3, which is arranged on the side of the activated carbon layer 2 close to the top plate; and a silica gel layer 4, which is arranged on the side of the vanadium layer 3 close to the top plate.

[0080] The infrared heating lamp 5 is arranged on one side of the top plate close to the silicone layer 4;

[0081] The nozzle 6 is arranged on one side of the top plate close to the silicone layer 4, and the nozzle 6 is connected to the spray system;

[0082] A temperature and humidity control system 7 connected to the spray system and the infrared heating lamp 5;

[0083] An electrochemical testing system 8 is connected with an auxiliary electrode 9, a reference electrode 10 and a metal to be tested 11, and the auxiliary electrode 9, the reference electrode 10 and the metal to be tested 11 are inserted into a soil carrier;

[0084] Test methods, including:

[0085] S1: Adjust the position of the metal to be tested 11, the shortest distance between the auxiliary electrode 9 and the metal to be tested 11 is 3.5 cm to 4 cm, the shortest distance between the reference electrode 10 and the metal to be tested 11 is 1.5 cm to 2.5 cm, and the electrochemical test system 8 obtains electrochemical measurement data in real time according to the auxiliary electrode 9, the reference electrode 10 and the metal to be tested 11;

[0086] S2: Setting the spraying time, negative temperature time and heating time, the temperature and humidity control system 7 uses the spraying system to control the nozzle 6 to spray the simulation liquid according to the spraying time;

[0087] S3: After the nozzle 6 stops spraying, a simulation experiment is performed, including: placing the simulated metal material corrosion test device in a frozen soil environment under negative temperature conditions for a negative temperature period, and then the temperature and humidity control system 7 controls the infrared heating lamp 5 to continue heating according to the heating period;

[0088] S4: Repeat the simulation experiment of S3. When the set experimental time is met, take out the metal 11 to be tested, and obtain the corrosion result according to one or more of the corrosion weight loss, corrosion products and electrochemical measurement data of the metal 11 to be tested.

[0089] It is understood that the electrochemical measurement data includes polarization resistance, corrosion current, etc.

[0090] When simulating the periodic thawing of seasonal frozen soil and short-term frozen soil, the box 1 first sprays the frozen soil simulation liquid according to the spraying time. After the soil carrier absorbs the solution, the three soil carriers absorb the corrosive solution in the simulated frozen soil area to a saturated state. The equipment is negative temperature for a certain period of time according to the negative temperature time. When the negative temperature ends, the infrared heating lamp 5 is started to heat up and melt the box 1 to simulate the melting state of the frozen soil environment. The soil melts and dries and loses water. After heating for a certain period of time, a cycle ends. The negative temperature and heating cycle are used to simulate the periodic thawing of seasonal frozen soil or the periodic thawing of short-term frozen soil. When simulating the thawing of short-term frozen soil, the negative temperature and heating time are shortened.

[0091] When simulating long-term freezing of permafrost, the frozen soil simulation liquid is sprayed according to the spraying time, so that the three soil carriers absorb the corrosion solution in the simulated frozen soil area to a saturated state. The heating time is set to 0, that is, after the soil carrier absorbs the solution, the corrosion test device simulating the metal material in the frozen soil environment continues to freeze at negative temperature, so that the soil carrier in the box 1 is frozen, simulating the long-term freezing state of the frozen soil environment until the end of the test.

[0092] When the simulated permafrost changes with the seasons and the upper layer melts while the lower layer freezes all year round, short-term infrared heating is carried out according to the experimental needs to make the upper layer melt and the lower layer continue to freeze, which is used to simulate the active layer and permafrost layer of permafrost.

[0093] During the experiment, the spraying time can be 30min-60min, the negative temperature time can be 1h-3600h, and the heating time can be 1h-12h. Of course, the spraying time, negative temperature time and heating time can be set as needed, and this embodiment does not make any specific restrictions on this.

[0094] In some optional embodiments, referring to Figure 1, the corrosion test device for simulating metal materials in a frozen soil environment further includes: a sample rack 16, which is a frame structure, the sample rack 16 is inserted into the soil carrier, and the metal 11 to be tested is inserted into the sample rack 16;

[0095] Adjust the position of the metal 11 to be tested, including:

[0096] The metal to be tested 11 is inserted into the sample holder 16 in a direction perpendicular to the ground, or the metal to be tested 11 is inserted into the sample holder 16 in a direction parallel to the ground.

[0097] It is understandable that the sample holder 16 is used to fix the position of the metal to be tested 11. The metal to be tested 11 can be inserted into the sample holder 16 in a direction perpendicular to the ground or in a direction parallel to the ground, so as to carry out a long-scale test or a small-size test piece test. The long-scale test is used to simulate the corrosion of a large structure in a complex frozen soil environment, and the small-size test piece test is used to simulate the corrosion of a small test piece in a single frozen soil environment.

[0098] In some optional embodiments, continue to refer to Figure 1 The spray system includes: a simulated liquid containing device 12, which is located outside the box body 1; a water pipe 13, one end of which is located inside the top plate and the other end is connected to the simulated liquid containing device 12, and the nozzle 6 is connected to the water pipe 13; between the top plate and the simulated liquid containing device 12, the water pipe 13 is provided with a spray control system 14;

[0099] Before setting the spraying time, negative temperature time and heating time, it also includes:

[0100] The simulated liquid is prepared and placed in the simulated liquid containing device 12 .

[0101] It is understood that the simulation solution is prepared using analytically pure and deionized water. Different salts can be added to the simulation solution according to actual needs. For example, 0.067g / L CaCl2, 0.21g / L NaCl, 0.083g / L Na2SO4, 0.126g / L MgSO4, 0.145g / L KNO3 and 0.087g / L NaHCO3 can be added. Alternatively, 2.13 mole fraction of Cl - , 0.852 mole fraction of SO4 2- , 0.121 mole fraction of HCO3 - and 0.141 mole fraction of NO3 - , but not limited to this.

[0102] In some optional embodiments, before setting the spraying time, the negative temperature time and the heating time, the following steps are further included:

[0103] Set the temperature control range and humidity control range of the temperature and humidity control system.

[0104] It is understandable that the temperature control range can be -40°C-60°C, and the humidity control range can be 30%RH-80RH. Of course, it is not limited to this and can be set according to actual needs.

[0105] In some optional embodiments, a corrosion experiment of cyclic freeze-thaw of seasonal frozen soil is simulated using X80 steel as the metal to be tested, including:

[0106] Preparation of simulation solution: Use analytically pure and deionized water to prepare soil simulation solution. In order to achieve the purpose of accelerated corrosion, the salt concentration of the simulation solution is 5 times that of the target soil, that is, it also includes components of 0.067g / L CaCl2, 0.21g / L NaCl, 0.083g / L Na2SO4, 0.126g / L MgSO4, 0.145g / L KNO3 and 0.087g / L NaHCO3.

[0107] Place the X80 steel test piece on the sample rack in a direction perpendicular to the ground and carry out the long-scale test.

[0108] Since the order of adsorption capacity of the three carriers is activated carbon > alumina > silica gel, and considering that the moisture content of the soil in the permafrost area gradually increases from top to bottom, the three soil carriers are set in the box in the order of silica gel, alumina and activated carbon from top to bottom.

[0109] Set the humidity control range in the box to 70% ± 5% RH.

[0110] The spraying time of the spray system is set to 40 minutes, so that the three soil carriers absorb the corrosive solution of the simulated permafrost area to a saturated state; the negative temperature time is set to 48 hours, so that the soil carriers in the box are frozen, simulating the freezing state of the permafrost environment; the infrared heating time is set to 6 hours, so that the temperature in the box rises and melts, simulating the melting state of the permafrost environment; negative temperature and heating are carried out alternately to simulate the periodic thawing of seasonal frozen soil.

[0111] Electrochemical in-situ measurements such as polarization resistance and corrosion current are performed while the sample is embedded.

[0112] When the experiment reaches the specified time, the test is terminated and the metal to be corroded is taken out. In this embodiment, the specified time is 720 hours, but it is not limited thereto. The surface morphology is observed, the corrosion products are analyzed, the corrosion rate is calculated according to the method described in the standard GB / T19292.4-2003, and the electrochemical data is analyzed to obtain the corrosion results shown in Table 1:

[0113] Table 1. Corrosion rate results

[0114] Actual soil corrosion rate mm / a 0.082 The corrosion rate of this test chamber is mm / a. 0.492 Acceleration rate 6

[0115] In some optional embodiments, Q345 steel is used as the metal to be tested to simulate the corrosion experiment of long-term freezing of permafrost, including:

[0116] Preparation of simulated solution: Use analytically pure and deionized water to prepare soil simulated solution. In order to achieve the purpose of accelerating corrosion, the salt concentration of the simulated solution is 10 times that of the target soil, that is, it also includes Cl with a molar fraction of 2.13 - , 0.852 mole fraction of SO4 2- , 0.121 mole fraction of HCO3 - and 0.141 mole fraction of NO3 - .

[0117] Since the order of adsorption capacity of the three carriers is activated carbon > alumina > silica gel, and considering that the moisture content of the soil in the permafrost area gradually increases from top to bottom, the three soil carriers are set in the box in the order of silica gel, alumina and activated carbon from top to bottom.

[0118] Set the humidity control range in the box to 40% ± 5% RH.

[0119] The working time of the spray system was set to 60 min, so that the three soil carriers absorbed the corrosive solution in the simulated frozen soil area to a saturated state; the heating time was set to 0 h; the negative temperature time was set to 1800 h, so that the soil carriers in the box were frozen, simulating the long-term freezing state of the frozen soil environment.

[0120] During the embedding process, electrochemical in-situ measurements such as polarization resistance and corrosion current can be performed simultaneously.

[0121] When the experiment reaches the specified time, the test is terminated and the metal to be corroded is taken out. In this embodiment, the specified time is 1440 hours, but it is not limited thereto. The surface morphology is observed, the corrosion products are analyzed, the corrosion rate is calculated according to the method described in the standard GB / T19292.4-2003, and the electrochemical data are analyzed to obtain the corrosion results shown in Table 2 and Table 3:

[0122] Table 2. Corrosion rate results

[0123] Actual soil corrosion rate mm / a 0.067 The corrosion rate of this test chamber is mm / a. Silica gel layer 0.22, alumina layer 0.26, activated carbon layer 0.31 Average acceleration rate 12

[0124] Table 3. Polarization curve fitting results

[0125] Sample location icorr / (μA·cm-2) Ecorr / mV Silicone area 1.25 -701 Bauxite area 1.42 -752 Activated carbon area 1.67 -798

[0126] The serial numbers of the above embodiments of the present invention are only for description and do not represent the advantages or disadvantages of the embodiments.

[0127] In the above embodiments of the present invention, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0128] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A corrosion test device simulating metal materials in a frozen soil environment, characterized in that: include: The box body comprises a bottom plate and a top plate which are arranged opposite to each other in a direction perpendicular to the ground, wherein the bottom plate is located on a side of the top plate close to the ground; The soil carrier, infrared heating lamp and nozzle are arranged in the box; The soil carrier comprises: an activated carbon layer, which is arranged on the side of the bottom plate close to the top plate; a bauxite layer, which is arranged on the side of the activated carbon layer close to the top plate; and a silica gel layer, which is arranged on the side of the bauxite layer close to the top plate. The infrared heating lamp is arranged on a side of the top plate close to the silicone layer; The nozzle is arranged on a side of the top plate close to the silicone layer, and the nozzle is connected to the spray system; A temperature and humidity control system connected to the spray system and the infrared heating lamp; The electrochemical testing system is connected with an auxiliary electrode, a reference electrode and a metal to be tested, wherein the auxiliary electrode, the reference electrode and the metal to be tested are inserted into the soil carrier.

2. The corrosion test device for simulating metal materials in a frozen soil environment according to claim 1 is characterized in that: The spray system comprises: A simulated liquid containing device, located outside the box; A water pipe has one end located in the top plate and the other end connected to the simulated liquid containing device, and the nozzle is connected to the water pipe; a spray control system is provided on the water pipe between the top plate and the simulated liquid containing device.

3. The corrosion test device for simulating metal materials in a frozen soil environment according to claim 1 or 2, characterized in that: Also includes: A cavity is provided in the bottom plate, and a plurality of holes are provided in the bottom plate, wherein the holes communicate with the cavity and a side of the bottom plate close to the top plate; The bottom plate is provided with a lead-out connector, and the lead-out connector is connected to the cavity.

4. The corrosion test device for simulating metal materials in a frozen soil environment according to claim 1 or 2, characterized in that: Also includes: The sample rack is a frame structure, the sample rack is inserted into the soil carrier, and the metal to be tested is inserted into the sample rack.

5. A corrosion test method for simulating metal materials in a frozen soil environment, characterized in that: The corrosion test device used to simulate the corrosion of metal materials in frozen soil environment includes: The box body comprises a bottom plate and a top plate which are arranged opposite to each other in a direction perpendicular to the ground, wherein the bottom plate is located on a side of the top plate close to the ground; the soil carrier, the infrared heating lamp and the nozzle are arranged in the box body; The soil carrier comprises: an activated carbon layer, which is arranged on the side of the bottom plate close to the top plate; a bauxite layer, which is arranged on the side of the activated carbon layer close to the top plate; and a silica gel layer, which is arranged on the side of the bauxite layer close to the top plate. The infrared heating lamp is arranged on a side of the top plate close to the silicone layer; The nozzle is arranged on a side of the top plate close to the silicone layer, and the nozzle is connected to the spray system; A temperature and humidity control system connected to the spray system and the infrared heating lamp; An electrochemical testing system, connected with an auxiliary electrode, a reference electrode and a metal to be tested, wherein the auxiliary electrode, the reference electrode and the metal to be tested are inserted into the soil carrier; Test methods, including: S1: adjusting the position of the metal to be tested, the shortest distance between the auxiliary electrode and the metal to be tested is in the range of 3.5 cm to 4 cm, the shortest distance between the reference electrode and the metal to be tested is in the range of 1.5 cm to 2.5 cm, and the electrochemical test system acquires electrochemical measurement data in real time according to the auxiliary electrode, the reference electrode and the metal to be tested; S2: setting the spraying time, negative temperature time and heating time, the temperature and humidity control system uses the spraying system to control the nozzle to spray the simulated liquid according to the spraying time; S3: After the nozzle stops spraying, a simulation experiment is performed, including: placing the simulated metal material corrosion test device in a frozen soil environment under negative temperature conditions for a negative temperature period, and then the temperature and humidity control system controls the infrared heating lamp to continue heating according to the heating period; S4: Repeat the simulation experiment of S3. When the set experimental time is met, take out the metal to be tested, and obtain the corrosion result according to one or more of the corrosion weight loss, corrosion products and electrochemical measurement data of the metal to be tested.

6. The method for simulating corrosion test of metal materials in a frozen soil environment according to claim 5, characterized in that: The simulated corrosion test device for metal materials in a frozen soil environment also includes: a sample rack, which is a frame structure, the sample rack is inserted into the soil carrier, and the metal to be tested is inserted into the sample rack; The step of adjusting the position of the metal to be tested comprises: The metal to be tested is inserted into the sample holder in a direction perpendicular to the ground, or the metal to be tested is inserted into the sample holder in a direction parallel to the ground.

7. The method for simulating corrosion test of metal materials in a frozen soil environment according to claim 5, characterized in that: The spray system comprises: a simulated liquid containing device, located outside the box; a water pipe, one end of which is located inside the top plate and the other end is connected to the simulated liquid containing device, and the spray head is connected to the water pipe; between the top plate and the simulated liquid containing device, the water pipe is provided with a spray control system; Before setting the spraying time, the negative temperature time and the heating time, the method further includes: The simulated liquid is configured and loaded into the simulated liquid containing device.

8. The method for simulating corrosion test of metal materials in a frozen soil environment according to claim 5, characterized in that: Before setting the spraying time, the negative temperature time and the heating time, the method further includes: Set the temperature control range and humidity control range of the temperature and humidity control system.

Citation Information

Cited By

  • Simulation evaluation method and device for corrosion resistance of metal in frozen soil environment

    CN119354861A

  • A simulation and evaluation method and device for the corrosion resistance of a metal in a frozen soil environment

    CN119354861B

  • Design method for evaluating corrosion resistance of metal in frozen soil environment

    CN119720485A

  • A design method for evaluating the corrosion resistance of metals in frozen soil environments

    CN119720485B