Acoustic damping glue, film product and sound production device

By crosslinking acrylic polymers with different glass transition temperatures, acoustic damping glues that can adjust the damping coefficient and glass transition temperature are formed, which solves the problem of insufficient adaptability of acoustic damping glues in the prior art in temperature environment and improves electronic products low frequency response and sound quality.

CN118895094APending Publication Date: 2024-11-05SHENZHEN MOMA TECH CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410894099.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing acoustic damping glue has a fixed damping coefficient under different temperature environments, which cannot effectively adapt to various temperature conditions, resulting in poor transmission of high-frequency and low-frequency signals in electronic products.

Method used

The crosslinked first acrylic polymer and the second acrylic polymer are used to form an acoustic damping glue with adjustable damping coefficient and glass transition temperature through the mixing of different glass transition temperatures and damping factors, which is suitable for different usage scenarios.

Benefits of technology

It realizes flexible adjustment of the damping coefficient and glass transition temperature of the acoustic damping glue, reduces the resonance frequency, improves the response to low frequency, makes the sound more full, and is suitable for a variety of ambient temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895094A_ABST
    Figure CN118895094A_ABST
Patent Text Reader

Abstract

The embodiment of the invention relates to the technical field of acoustic damping materials, and discloses acoustic damping glue which comprises a first acrylic polymer and a second acrylic polymer which are cross-linked, and the glass transition temperature of the first acrylic polymer is higher than that of the second acrylic polymer. In the embodiment, the two linear acrylic polymers with different glass transition temperatures can be mixed according to an actual use scene, and the acoustic damping glue suitable for the current use scene is obtained by curing in the same cross-linking mode, so that the lowest resonant frequency is reduced, the response of the acoustic damping glue to low frequency is improved, and heard sound is fuller.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present application relate to the technical field of acoustic damping materials, and in particular to an acoustic damping adhesive, a film product, and a sound-generating device. Background Art

[0002] With the rapid development of science and technology, electronic products (such as smart phones, smart watches and smart headphones, etc.) are required to have better signal transmission effects at high frequencies and excellent high-fidelity effects. Electronic products usually use acoustic sound-generating components, including acoustic diaphragms. In a sound-generating device, for example, in a speaker, an acoustic diaphragm with acoustic damping glue is used as a sound-generating unit, which generates vibrations through electromagnetic induction or compression drive, and converts electrical signals into sound signals. The acoustic damping glue in the acoustic diaphragm can absorb vibration mechanical energy and convert it into heat energy and loss. The damping coefficient is the ability to describe the energy dissipation of the acoustic damping glue during the vibration process. The larger the damping coefficient, the more energy the diaphragm loses when vibrating, so that the vibration can be more effectively controlled and the distortion and resonance of the sound can be reduced.

[0003] In the prior art, the damping coefficient of the known acoustic damping glue is fixed under different temperature environments. Therefore, the existing acoustic damping glue has low adaptability to the ambient temperature and cannot adapt well to various temperature conditions. Summary of the invention

[0004] The main technical problem solved by the embodiments of the present application is how to obtain suitable acoustic damping glue according to different usage scenarios.

[0005] To solve the above technical problems, the embodiments of the present application adopt the following technical solutions:

[0006] In a first aspect of the present application, an acoustic damping adhesive is provided, comprising a first acrylic polymer and a second acrylic polymer that are cross-linked, wherein the glass transition temperature of the first acrylic polymer is greater than the glass transition temperature of the second acrylic polymer.

[0007] In some embodiments, the glass transition temperature of the first acrylic polymer is greater than 10° C., and / or the damping factor of the first acrylic polymer is greater than 2.0.

[0008] In some embodiments, the second acrylic polymer has a glass transition temperature of less than -10°C, and / or the second acrylic polymer has a damping factor of less than 1.5.

[0009] In some embodiments, the first acrylic polymer is selected from at least one of methyl methacrylate, ethyl methacrylate, acrylonitrile, etc.; and / or the second acrylic polymer is selected from at least one of ethyl acrylate, n-butyl acrylate, isooctyl acrylate, or lauryl methacrylate.

[0010] In some embodiments, the raw material of the acoustic damping glue includes hindered phenol.

[0011] In some embodiments, the raw material of the acoustic damping glue further includes a plasticizer.

[0012] In some embodiments, the raw material components of the acoustic damping glue include, by weight: 10 to 90 parts of a first acrylic polymer, 10 to 90 parts of a second acrylic polymer, 3 to 5 parts of a hindered phenol, 3 to 5 parts of a plasticizer, and 0.5 to 1 part of an isocyanate crosslinking agent.

[0013] In some embodiments, the thickness of the adhesive film layer is 5-50 um.

[0014] In a second aspect of the present application, an acoustic damping adhesive film is further provided, comprising a first release film, an acoustic damping adhesive, and a second release film stacked in sequence, wherein the acoustic damping adhesive layer comprises the acoustic damping adhesive described in the first aspect.

[0015] In the third aspect of the present application, a sound-generating device is also provided, including a vibration system and a magnetic circuit system coordinated with the vibration system; the vibration system includes an acoustic diaphragm and a voice coil coupled to one side of the acoustic diaphragm, the magnetic circuit system drives the voice coil to vibrate to drive the acoustic diaphragm to produce sound, and the acoustic diaphragm includes a vibration membrane and the acoustic damping glue described in the first aspect.

[0016] Beneficial effects of the embodiments of the present application: Different from the prior art, the acoustic damping glue provided in the embodiments of the present application includes a first acrylic polymer and a second acrylic polymer that are cross-linked, wherein the glass transition temperature of the first acrylic polymer is greater than the glass transition temperature of the second acrylic polymer. By mixing two acrylic polymers with different damping coefficients and different glass transition temperatures, an acoustic damping glue having a damping coefficient and a glass transition temperature between the two can be obtained. The damping coefficient and glass transition temperature of the acoustic damping glue change with the change of the mixing ratio of the two. Therefore, according to the actual use scenario, the acoustic damping glue suitable for the current scenario can be determined, the minimum resonance frequency can be reduced, and the response of the acoustic damping glue to low frequencies can be improved, so that the sound heard is fuller. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] One or more embodiments are exemplarily described by pictures in the corresponding drawings, and these exemplified descriptions do not constitute limitations on the embodiments. Elements with the same reference numerals in the drawings represent similar elements, and unless otherwise stated, the figures in the drawings do not constitute proportional limitations.

[0018] Figure 1 is a molecular structure diagram of a 4-functional phenolic polymer provided in one embodiment of the present application;

[0019] Figure 2 is a molecular structure diagram of a bifunctional phenolic polymer provided in one embodiment of the present application;

[0020] Figure 3 is a molecular structure diagram of a benzene plasticizer provided in one embodiment of the present application;

[0021] Figure 4 This is a schematic diagram of the structure of an acoustic damping film product provided by an embodiment of the present application;

[0022] Figure 5 This is a performance test result diagram of an acoustic damping glue provided by an embodiment of the present application. DETAILED DESCRIPTION

[0023] The present application is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present application, but do not limit the present application in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements can also be made without departing from the concept of the present application. These all belong to the protection scope of the present application.

[0024] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0025] It should be noted that, if there is no conflict, the various features in the embodiments of the present application can be combined with each other, all within the scope of protection of the present application. In addition, although the functional module division is performed in the device schematic diagram and the logical order is shown in the flow chart, in some cases, the steps shown or described can be performed in a sequence different from the module division in the device or the flow chart. In addition, the words "first", "second", "third", etc. used herein do not limit the data and execution order, but only distinguish the same items or similar items with basically the same functions and effects.

[0026] Unless otherwise defined, all technical and scientific terms used in this specification have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used in this specification and in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used in this specification includes any and all combinations of one or more of the related listed items.

[0027] In addition, the technical features involved in each embodiment of the present application described below can be combined with each other as long as they do not conflict with each other.

[0028] In a first aspect of the present application, an acoustic damping adhesive is provided, comprising a first acrylic polymer and a second acrylic polymer that are cross-linked, wherein the glass transition temperature of the first acrylic polymer is greater than the glass transition temperature of the second acrylic polymer.

[0029] It is understood by those skilled in the art that the glass transition temperature is the temperature at which a polymer changes from a highly elastic state to a glassy state, and refers to the transition temperature of an amorphous polymer (including the non-crystalline part of a crystalline polymer) from a glassy state to a highly elastic state or from the latter to the former. It is the lowest temperature at which the macromolecular chain of an amorphous polymer can move freely, and is also the upper limit of the working temperature of the product, usually represented by Tg. Below the glass transition temperature, the polymer is usually in a solid state, and neither the molecular chain nor the chain segment can move, but the atoms (or groups) constituting the molecule vibrate at their equilibrium position; at the glass transition temperature, although the molecular chain cannot move, the chain segment begins to move, showing a highly elastic property. As the temperature rises further, the entire molecular chain begins to move, showing a viscous flow property.

[0030] Crosslinking is a chemical or physical process that allows two or more molecules to be linked together through covalent bonds or other types of bonds to form a three-dimensional network structure. This process can enhance the mechanical properties, thermal stability, chemical stability and durability of the material.

[0031] In this embodiment, the glass transition temperatures of the two types of acrylic polymers that undergo cross-linking are different, wherein the glass transition temperature of the first acrylic polymer is greater than the glass transition temperature of the second acrylic polymer. Therefore, the glass transition temperature of the polymer material obtained after cross-linking is between the glass transition temperature of the first acrylic polymer and the glass transition temperature of the second acrylic polymer. It can be seen that the glass transition temperature of the above-mentioned acoustic damping glue is lower than the glass transition temperature of the first acrylic polymer and greater than the glass transition temperature of the second acrylic polymer.

[0032] It can be seen that the glass transition temperature of the acoustic damping glue obtained by selecting two acrylic polymers with different glass transition temperatures and cross-linking them is between the two, and materials with different glass transition temperatures can be obtained according to the different ratios of the two. Therefore, the above-mentioned acoustic damping glue can be adapted to a variety of practical scenarios and has strong applicability.

[0033] In some embodiments, the glass transition temperature of the first acrylic polymer is greater than 10° C. For example, the first acrylic polymer is selected from at least one of methyl methacrylate, ethyl methacrylate, acrylonitrile, and the like.

[0034] The glass transition temperature of the second acrylic polymer is less than -10° C. For example, the second acrylic polymer is selected from at least one of ethyl acrylate, n-butyl acrylate, isooctyl acrylate, and lauryl methacrylate.

[0035] Among them, the glass transition temperature of the first acrylic polymer is significantly different from the glass transition temperature of the second acrylic polymer. Therefore, the glass transition temperature of the material obtained by mixing the above two acrylic polymers covers a larger range, and the glass transition temperature of the acoustic damping glue obtained after the first acrylic polymer and the second acrylic polymer are cross-linked is between the glass transition temperatures of the above two acrylic polymers. It can be seen that by selecting the first acrylic polymer and the second acrylic polymer with a large temperature difference for cross-linking, the obtained acoustic damping glue can adapt to a wider variety of actual situations and ambient temperatures.

[0036] In some embodiments, the damping factor of the first acrylic polymer is greater than 2.0. The damping factor of the second acrylic polymer is less than 1.5.

[0037] Among them, the damping factor of the first acrylic polymer is quite different from that of the second acrylic polymer. Therefore, the damping factor of the material obtained by mixing the above two acrylic polymers covers a wider range, and the damping factor of the acoustic damping glue obtained after the first acrylic polymer and the second acrylic polymer are cross-linked is between the damping factors of the above two acrylic polymers. It can be seen that by cross-linking the first acrylic polymer and the second acrylic polymer with a large difference in damping factors, the obtained acoustic damping glue can adapt to a wider variety of actual situations and ambient temperatures.

[0038] In some embodiments, the raw material of the acoustic damping glue includes hindered phenol.

[0039] Hindered phenol is a phenolic compound with a special steric hindered structure, which can not only improve the damping factor of the acoustic damping glue, but also improve the temperature resistance of the acoustic damping glue. The molecular structure of hindered phenol includes "phenol-containing" functional groups, and the number of "phenol-containing" functional groups will affect the damping factor of the acoustic damping glue. However, it is not the case that the more "phenol-containing" functional groups there are, the better the effect of improving the damping factor of the acoustic damping glue. For example, in some embodiments, 2-functional phenolic polymers and 4-functional phenolic polymers have a better effect on improving the damping factor of the acoustic damping glue; compared with 4-functional phenolic polymers, 2-functional phenolic polymers have better compatibility and flexibility, and can more effectively improve the damping factor of the acoustic damping glue.

[0040] In some embodiments, the molecular structure of the 4-functional phenolic polymer is as follows Figure 1 As shown; the molecular structure of the 2-functional phenol polymer is as follows Figure 2 shown.

[0041] According to different hindered phenols, several embodiments of the present application are shown in Table 1. According to weight parts, the raw material composition of the acoustic damping glue includes: 30 parts of low Tg acrylic polymer; 70 parts of high Tg acrylic polymer; 1 part of isocyanate crosslinker. The hindered phenols in the above experimental examples are 0, 1, 2, 3, 4 and 5 parts respectively. As shown in Table 1 below, it can be seen that under the same low Tg acrylic polymer, high Tg acrylic polymer and isocyanate crosslinker, the more hindered phenols there are, the greater the Tg of the obtained material and the higher the damping factor.

[0042] Table 1

[0043]

[0044] It can be seen that experiments have verified that the long-chain structure in hindered phenol not only has a certain flexibility and is not easy to precipitate, but also can form strong hydrogen bonds with acrylic resin when added to the resin, greatly improving the damping effect. At the same time, hindered phenol contains a phenol structure and has high temperature resistance.

[0045] In some embodiments, the raw material of the acoustic damping glue further includes a plasticizer.

[0046] Plasticizers are aromatic hydrocarbon plasticizers containing "benzene rings", which can more effectively weaken the forces between the molecules of acoustic damping glue and increase the slippage between molecules, thereby effectively adjusting the flexibility of the molecular chain of acoustic damping glue and the processability of acoustic damping glue. Compared with other plasticizers, such as fatty acid plasticizers, citrate plasticizers, ester plasticizers and soybean oil plasticizers, aromatic hydrocarbon plasticizers have excellent high temperature resistance and low precipitation, which can effectively reduce the glass transition temperature of acoustic damping glue and improve the processability of acoustic damping glue.

[0047] According to the different plasticizers, several embodiments of the present application are shown in Table 2 below. According to the weight parts, the raw material composition of the acoustic damping glue includes: 30 parts of low Tg acrylic polymer; 70 parts of high Tg acrylic polymer; 1 part of isocyanate crosslinker; 5 parts of hindered phenol. The plasticizers in the above experimental examples are 0, 1, 2, 3, 4 and 5 parts respectively. As shown in Table 2 below, it can be seen that under the same low Tg acrylic polymer, high Tg acrylic polymer, hindered phenol and isocyanate crosslinker, the more plasticizers there are, the smaller the Tg of the obtained material and the damping factor only changes slightly.

[0048] Table 2

[0049] Control group Implementation Group Implementation Group Implementation Group Implementation Group Implementation Group Low Tg Acrylic Polymer 30 30 30 30 30 30 High Tg Acrylic Polymer 70 70 70 70 70 70 Hindered Phenol 5 5 5 5 5 5 Plasticizers 0 1 2 3 4 5 Isocyanate crosslinker 1 1 1 1 1 1 Tg(℃) 4.54 3.82 1.65 -1.12 -4.36 -7.22 Damping factor 2.68 2.67 2.67 2.68 2.67 2.68

[0050] Plasticizers can effectively adjust the flexibility of molecular chains and the processability of polymer materials, and can also play a role in mutual dissolution between two different acrylic polymers. Experimental verification shows that this benzene plasticizer (structure such as Figure 3 As shown in the figure, it not only has good compatibility with acrylic resin, but also is not easy to precipitate out when added into the resin; and because it contains benzene rings, it has certain temperature resistance and will not volatilize easily at high temperatures; in addition, the long-chain structure has excellent flexibility, which can greatly improve the plasticity of the resin and reduce the glass transition temperature, but has no effect on damping.

[0051] In some embodiments, the raw material components of the acoustic damping glue include, by weight: 10 to 90 parts of a first acrylic polymer, 10 to 90 parts of a second acrylic polymer, 3 to 5 parts of a hindered phenol, 3 to 5 parts of a plasticizer, and 0.5 to 1 part of an isocyanate crosslinking agent.

[0052] In some embodiments, the thickness of the acoustic damping glue is 5 to 50 um. Exemplarily, the thickness of the acoustic damping glue is 5 um, 10 um, 12 um, 26 um, 35 um, 42 um, 50 um or the middle value of any two of the above values. The acoustic damping glue with a thickness range of 5 to 50 um has high strength and can also be applied to miniaturized sound-generating devices.

[0053] like Figure 4 As shown, some embodiments of the present application provide a film product 10, comprising a first release film 1, an acoustic damping adhesive 2, and a second release film 3 stacked in sequence. The acoustic damping adhesive 2 is the acoustic damping adhesive in any of the above embodiments, and has the same performance as the acoustic damping adhesive in any of the above embodiments, and will not be repeated here.

[0054] Specifically, in some embodiments of the present application, the first release film 1 is a light release film, such as a light fluorine release film for lamination, and the peeling force of the light release film is 1gf / inch-3gf / inch. The second release film 3 is a heavy release film, such as a fluorine release film for wet coating, and the peeling force of the heavy release film is 10gf / inch-15gf / inch; the thickness of the acoustic damping film can be specifically 5μm to 50μm.

[0055] In a third aspect, the present application provides a sound-generating device, including a vibration system and a magnetic circuit system matched with the vibration system; the vibration system includes an acoustic diaphragm and a voice coil coupled to one side of the acoustic diaphragm, the magnetic circuit system drives the voice coil to vibrate to drive the acoustic diaphragm to make a sound, and the acoustic diaphragm includes a diaphragm and an acoustic damping glue in any of the above embodiments. Exemplarily, the diaphragm, the acoustic damping glue, and the diaphragm are compounded into the acoustic diaphragm. Among them, the diaphragm can be a thermoplastic elastomer film such as PEEK, TPEE, TPU, PEN, TPI, etc.

[0056] When the sound-generating device is working, after the voice coil is energized, it can vibrate up and down under the driving action of the magnetic field force of the magnetic circuit system, driving the acoustic diaphragm to vibrate and generate sound, and the acoustic damping glue in the acoustic diaphragm absorbs the sound wave energy to reduce the propagation of noise. A sound-generating device including the acoustic damping glue in any of the above embodiments, such as a speaker, has excellent low-frequency performance, full bass and comfortable listening experience, and less swaying vibration during the vibration process, and more stable listening.

[0057] The following describes a method for preparing the acoustic damping adhesive in an embodiment of the present application, comprising the following steps:

[0058] (1) A high-damping acrylic acid mixed solution is prepared in advance, specifically, including the following steps H001-H006.

[0059] H001: Weigh 80% of low Tg linear acrylic polymer, add 40% of organic solvent to dilute and stir for 5 minutes at a speed of 300-400 rpm.

[0060] H002: Weigh 20% of high Tg linear acrylic polymer, add 15% of organic solvent to dissolve, add to H001 and stir for 3 minutes at a speed of 400-500rpm.

[0061] H003: Weigh 5.0% of hindered phenol, add 15% of organic solvent to dissolve it, then add it to H001 and stir for 3 minutes at a speed of 400-500 rpm.

[0062] H004: Weigh 5.0% of plasticizer, add 15% of organic solvent to dissolve, add to H001 and stir for 3 minutes at a speed of 400-500 rpm.

[0063] H005: Weigh 1% of isocyanate crosslinking agent, add 10% of organic solvent to dissolve, add to H001 and stir for 5 minutes at a speed of 400-500 rpm.

[0064] H006: After it is evenly dispersed and filtered through a 300-mesh filter, keep it for later use.

[0065] (2) Using the mixed solution in (1) to solidify and form a film, specifically, the method includes the following steps T001-T003.

[0066] T001: evenly apply or spray the above blended solution on the release film in silicone oil for wet coating;

[0067] T002: Pass the applied mixed solution through a precision coating machine and bake it for curing.

[0068] Baking temperature: 70℃, 80℃, 100℃, 120℃, 120℃, 100℃

[0069] Coating machine speed: 15~20m / min.

[0070] T003: After it solidifies, apply the light silicone oil release film to the tail of the coating machine and rewind it.

[0071] Several embodiments of the present application are provided below.

[0072] Example 1

[0073] The raw material composition of the acoustic damping adhesive includes, by weight: 90 parts of low Tg acrylic polymer; 10 parts of high Tg acrylic polymer; 1 part of isocyanate crosslinking agent; 5 parts of hindered phenol; and 5 parts of plasticizer.

[0074] Example 2

[0075] The difference between this embodiment and embodiment 1 is that, in parts by weight, the raw material composition of the acoustic damping glue includes: 80 parts of low Tg acrylic polymer; 20 parts of high Tg acrylic polymer; 1 part of isocyanate crosslinking agent; 5 parts of hindered phenol; and 5 parts of plasticizer.

[0076] Example 3

[0077] The difference between this embodiment and Embodiment 1 and Embodiment 2 is that, in parts by weight, the raw material composition of the acoustic damping glue includes: 70 parts of low Tg acrylic polymer; 30 parts of high Tg acrylic polymer; 1 part of isocyanate crosslinking agent; 5 parts of hindered phenol; and 5 parts of plasticizer.

[0078] Example 4

[0079] The difference between this embodiment and embodiments 1-3 is that, in parts by weight, the raw material composition of the acoustic damping glue includes: 60 parts of low Tg acrylic polymer; 40 parts of high Tg acrylic polymer; 1 part of isocyanate crosslinking agent; 5 parts of hindered phenol; and 5 parts of plasticizer.

[0080] Example 5

[0081] The difference between this embodiment and embodiments 1-4 is that, in parts by weight, the raw material composition of the acoustic damping glue includes: 50 parts of low Tg acrylic polymer; 50 parts of high Tg acrylic polymer; 1 part of isocyanate crosslinking agent; 5 parts of hindered phenol; and 5 parts of plasticizer.

[0082] Example 6

[0083] The difference between this embodiment and embodiments 1-5 is that, in parts by weight, the raw material composition of the acoustic damping glue includes: 40 parts of low Tg acrylic polymer; 60 parts of high Tg acrylic polymer; 1 part of isocyanate crosslinking agent; 5 parts of hindered phenol; and 5 parts of plasticizer.

[0084] Example 7

[0085] The difference between this embodiment and embodiments 1-6 is that, in parts by weight, the raw material composition of the acoustic damping glue includes: 30 parts of low Tg acrylic polymer; 70 parts of high Tg acrylic polymer; 1 part of isocyanate crosslinking agent; 5 parts of hindered phenol; and 5 parts of plasticizer.

[0086] Example 8

[0087] The difference between this embodiment and embodiments 1-7 is that, in parts by weight, the raw material composition of the acoustic damping glue includes: 20 parts of low Tg acrylic polymer; 80 parts of high Tg acrylic polymer; 1 part of isocyanate crosslinking agent; 5 parts of hindered phenol; and 5 parts of plasticizer.

[0088] Example 9

[0089] The difference between this embodiment and embodiments 1-8 is that, in parts by weight, the raw material composition of the acoustic damping glue includes: 10 parts of low Tg acrylic polymer; 90 parts of high Tg acrylic polymer; 1 part of isocyanate crosslinking agent; 5 parts of hindered phenol; and 5 parts of plasticizer.

[0090] Comparative Example 1

[0091] The difference between this embodiment and the above-mentioned embodiments 1-9 is that, in parts by weight, the raw material composition of the acoustic damping adhesive includes: 100 parts of low Tg acrylic polymer; 1 part of isocyanate cross-linking agent.

[0092] Control group 2

[0093] The difference between this embodiment and the above-mentioned embodiments 1-9 is that, in parts by weight, the raw material composition of the acoustic damping adhesive includes: 100 parts of high Tg acrylic polymer; 1 part of isocyanate cross-linking agent.

[0094] The Tg and damping factor of the acoustic damping glue provided by Examples 1-9 and Control Groups 1 and 2 were tested, and the test results are shown in Table 3 below.

[0095] Table 3

[0096]

[0097] It can be seen from Table 3 above that by mixing different proportions of high Tg acrylic polymer and low Tg acrylic polymer, a material with a damping factor and Tg between the two acrylic polymers can be obtained. Therefore, under different environments, the ratio of the above two acrylic polymers can be changed to obtain the acoustic damping glue that is most suitable for the current usage scenario. For example, in a low temperature environment, the use of a high Tg, high damping acoustic damping glue will cause the resonant frequency F0 of the sound-generating device to be higher, so a low Tg, high damping acoustic damping glue should be used in a low temperature environment. It can be seen from Table 3 above that the damping factor of the acoustic damping glue provided by Implementation Group 7 is larger and the Tg is lower, which is more suitable for a low temperature environment. Figure 5 The damping curve and Tg curve of the acoustic damping adhesive in the acoustic damping adhesive film provided by Implementation Group 7 are shown. Figure 5 It can be seen that the Tg of the acoustic damping glue provided by implementation group 7 is -7.22°C, and the damping factor is as high as 2.68.

[0098] Different from the prior art, the beneficial effect of the embodiments of the present application is that two acrylic polymers with different glass transition temperatures are mixed, and the glass transition temperature of the obtained mixture material is between the glass transition temperatures of the above two acrylic polymers, and the damping factor of the obtained mixture material is also between the damping factors of the above two acrylic polymers. It can be seen that according to different actual scenarios and ambient temperatures, the first acrylic polymer and the second acrylic polymer can be mixed in different ratios to obtain an acoustic damping glue that matches the current usage scenario and ambient temperature.

[0099] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Under the concept of the present application, the technical features in the above embodiments or different embodiments can also be combined, the steps can be implemented in any order, and there are many other changes in different aspects of the present application as described above, which are not provided in detail for the sake of simplicity. Although the present application has been described in detail with reference to the aforementioned embodiments, a person of ordinary skill in the art should understand that the technical solutions described in the aforementioned embodiments can still be modified, or some of the technical features can be replaced by equivalents. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application.

Claims

1. An acoustic damping adhesive, characterized in that: The invention comprises a first acrylic polymer and a second acrylic polymer which are cross-linked, wherein the glass transition temperature of the first acrylic polymer is greater than the glass transition temperature of the second acrylic polymer.

2. The acoustic damping adhesive according to claim 1, characterized in that: The glass transition temperature of the first acrylic polymer is greater than 10° C., and / or the damping factor of the first acrylic polymer is greater than 2.

0.

3. The acoustic damping adhesive according to claim 1, characterized in that: The glass transition temperature of the second acrylic polymer is less than -10°C, and / or the damping factor of the second acrylic polymer is less than 1.

5.

4. The acoustic damping adhesive according to any one of claims 1 to 3, characterized in that: The first acrylic polymer is selected from at least one of methyl methacrylate, ethyl methacrylate or acrylonitrile; and / or the second acrylic polymer is selected from at least one of ethyl acrylate, n-butyl acrylate, isooctyl acrylate or lauryl methacrylate.

5. The acoustic damping adhesive according to claim 1, characterized in that: The raw materials of the acoustic damping glue include hindered phenol.

6. The acoustic damping adhesive according to claim 5, characterized in that: The raw materials of the acoustic damping glue also include a plasticizer.

7. The acoustic damping adhesive according to claim 6, characterized in that: In parts by weight, the raw material components of the acoustic damping adhesive include: 10 to 90 parts of a first acrylic polymer, 10 to 90 parts of a second acrylic polymer, 3 to 5 parts of a hindered phenol, 3 to 5 parts of a plasticizer, and 0.5 to 1 part of an isocyanate crosslinking agent.

8. The acoustic damping adhesive according to any one of claims 1 to 7, characterized in that: The thickness of the acoustic damping glue is 5-50 um.

9. A membrane product, characterized in that It comprises a first release film, an acoustic damping glue, and a second release film stacked in sequence, wherein the acoustic damping glue is the acoustic damping glue according to any one of claims 1-8.

10. A sound-generating device, characterized in that: It includes a vibration system and a magnetic circuit system matched with the vibration system; the vibration system includes an acoustic diaphragm and a voice coil combined on one side of the acoustic diaphragm, the magnetic circuit system drives the voice coil to vibrate to drive the acoustic diaphragm to make sound, and the acoustic diaphragm includes a vibration membrane and the acoustic damping glue described in any one of claims 1-8.

Citation Information

Cited By

  • Vibrating diaphragm for sound production device, sound production device and electronic equipment

    CN120574443A

  • Vibrating diaphragm for sound production device, sound production device and electronic equipment

    CN120602851A

  • Diaphragms, sound-generating devices, and electronic devices used in sound-generating devices

    CN120602851B