Composite mineralized material as well as preparation method and application thereof

By preparing composite mineralized materials and using the complex cooperation between mineralized materials and basic materials, the problem of exceeding the standard of metal elements and organic matter in the mineralized filter element is solved, the smooth dissolution of minerals and the safety of water use is improved, and the water purification is extended The service life of the device.

CN118978201AActive Publication Date: 2024-11-19JOYOUNG CO LTD

Patent Information

Application Number
CN202411085374.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-19
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

The existing mineralized filter element has the risk of exceeding the standard of metal elements or organic matter. The huge amount of dissolution leads to unstable mineral dissolution, affecting the safety of water and the service life of the purification device.

Method used

Compound mineralized materials, including mineralized materials and basic materials, are used to form complexing and antagonistic effects through firing, soaking and carbonation, which promotes the slow dissolution of minerals, ensures the smooth release of strontium, zinc and other elements, and reduces scaling. risk.

Benefits of technology

It achieves relatively stable dissolution of minerals, improves water safety, extends the service life of the water purification device, and meets the water needs of different groups of people.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978201A_ABST
    Figure CN118978201A_ABST
Patent Text Reader

Abstract

The invention discloses a composite mineralization material as well as a preparation method and application thereof, and belongs to the technical field of mineralization materials for water purification. The preparation method comprises the following steps: (1) selecting strontium-containing ores, zinc-containing ores, metasilicic acid-containing ores and carbonate-containing ores from natural ores, respectively crushing the ores, and respectively firing at 600-800 DEG C for 1-4 hours; (2) respectively soaking the fired ores in pure water, then respectively carrying out carbonation treatment, carrying out component analysis after air drying, and screening to obtain a strontium-containing mineralized material, a zinc-containing mineralized material, a metasilicic acid-containing mineralized material, a carbonate-containing mineralized material and a base material; and (3) crushing the mineralized material and the base material again, and mixing according to a weight ratio to obtain the composite mineralized material. The composite mineralized material prepared by the method can solve the problem that metal elements and organic matters in natural ore exceed the standard, and can realize stable dissolution of minerals, reduce scaling and prolong the service life of a water purification device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a composite mineralized material and a preparation method and application thereof, belonging to the technical field of mineralized materials for water purification. Background Art

[0002] Normal human life activities cannot be separated from water. The safety of drinking water is related to the healthy development of the entire human race. At present, in order to improve the safety of drinking water, consumers often install purification devices on their own to purify the water quality, such as using reverse osmosis water purifiers or products containing water purification filters to obtain pure water that can be directly drunk.

[0003] Although previous purification devices can reduce impurities in water quality, they cannot provide mineralized water. Therefore, researchers added mineralized filters to the purification devices to dissolve mineral elements into purified water, thereby meeting the human body's needs for essential trace elements. However, the ores used in current mineralized filters have the risk of exceeding certain metal elements or organic matter standards, affecting water safety; in addition, the current dissolution volume of mineralized filters is huge, and the later dissolution volume is negligible, making it difficult to maintain a relatively stable dissolution of mineral elements, resulting in a large difference in minerals in the water treated by the newly replaced filter and the filter that has been used for a period of time. Therefore, there is a lack of a mineralized material that allows minerals to penetrate smoothly. In addition, due to the huge dissolution volume, the water purification device with added mineralized filters is more prone to scaling than the water purification device without added mineralized filters, which affects normal water output and reduces the service life of the purification device. Summary of the invention

[0004] In order to solve the above problems, a composite mineralized material and a preparation method and application thereof are provided. The composite mineralized material prepared by the method can solve the problem of excessive metal elements and organic matter in natural ores, and can achieve smooth dissolution of minerals, reduce scaling, and increase the service life of water purification equipment.

[0005] According to one aspect of the present application, a composite mineralized material is provided, which comprises, by weight:

[0006] 5-15 parts of mineralized material and 15-25 parts of base material, wherein the mineralized material is selected from at least one of strontium-containing mineralized material, zinc-containing mineralized material, metasilicic acid-containing mineralized material and carbonate-containing mineralized material, wherein the strontium content of the strontium-containing mineralized material is not less than 0.05%, the zinc content of the zinc-containing mineralized material is not less than 0.5%, the silicate content of the metasilicic acid-containing mineralized material is not less than 3%, and the carbonate content of the carbonate-containing mineralized material is not less than 5%;

[0007] The content of lead, cadmium, chromium, mercury and arsenic in the mineralized material is less than 0.005%;

[0008] The basic material contains 15-50% Si, 5-30% O and 5-30% C.

[0009] The above-mentioned composite mineralized material adopts the basic material as the main body, which can serve as the core carrier of the mineralized material. The mineralized material forms a complex and antagonistic effect with the basic material and is distributed on the surface and pores of the basic material. The addition of the basic material is mainly used as a load carrier. The content of the basic material is higher than that of the mineralized material, which can promote the slow dissolution of the mineralized material and make the dissolution rate of the mineral regular, thereby achieving relatively stable dissolution of the mineral; according to actual needs, the mineralized material can be selected from at least one of strontium-containing mineralized material, zinc-containing mineralized material, metasilicic acid-containing mineralized material, and carbonate-containing mineralized material, thereby achieving the dissolution of the above-mentioned minerals. The strontium content in the strontium mineralized material is not less than 0.05%, which can make the strontium ion concentration of the pure water ≥0.2mg / L after passing through, meeting the national standard for mineral water; the zinc content in the zinc mineralized material is not less than 0.5%, which can make the zinc ion concentration of the pure water ≥0.05 and ≤0.2ppm after passing through; the silicate content in the metasilicic acid mineralized material is not less than 3%, which can make the metasilicic acid concentration of the pure water ≥0.5ppm after passing through; the carbonate content in the carbonate mineralized material is not less than 5%, which can realize the alkalization of the pure water, so that the pH of the pure water is increased by 0.5-1 after passing through, and weak alkaline mineral water is obtained.

[0010] Optionally, the mineralized material is at least selected from a strontium-containing mineralized material and a zinc-containing mineralized material in a weight ratio of 8:2.

[0011] This solution can at least meet the simultaneous release of strontium and zinc, and the release of both elements is in line with the absorption law of the human body. Strontium can promote bone development, maintain normal human function, prevent cardiovascular diseases, etc.; zinc is an essential trace element for the human body, promotes growth and development, and is the main component of many synthetic enzymes in the human body.

[0012] Optionally, the mineralized material is selected from a strontium-containing mineralized material, a zinc-containing mineralized material, a metasilicic acid-containing mineralized material and a carbonate-containing mineralized material in a weight ratio of 8:2:2:1.4.

[0013] The composite mineralized material composed of the above substances can produce composite drinking water with multiple minerals: strontium, zinc, and orthosilicic acid, and can meet the weak alkaline function.

[0014] Optionally, when the particle size of the mineralized material is 80-200 mesh, the particle size of the base material is 60-300 mesh, and the composite mineralized material further includes 60-100 parts of activated carbon powder with a particle size of 60-300 mesh, and the composite mineralized material is made into a carbon rod.

[0015] The carbon rod prepared as above can be placed in a water purification device for use, thereby increasing the content of mineral elements in purified water and improving the safety of water use.

[0016] Optionally, when the particle size of the mineralized material is 1-5 mm, the particle size of the base material is 0.5-5 mm, and the composite mineralized material is directly filled into the filter element as mineralized particles.

[0017] The mineralized particles can be loaded and packed in filter elements and can be used in water purification devices, water heaters, thermos cups and other items, and can realize the remineralization function of drinking water to obtain healthy drinking water.

[0018] According to another aspect of the present application, there is provided a method for preparing the composite mineralized material described in any one of the above items, comprising the following steps:

[0019] (1) selecting strontium-containing ore, zinc-containing ore, metasilicate-containing ore, and carbonate-containing ore from natural ores, crushing the above ores respectively, and calcining them at 600-800° C. for 1-4 hours respectively;

[0020] (2) soaking the fired ores in pure water, and then performing carbonation treatment on them respectively, air-drying them, and then performing component analysis to screen out the strontium-containing mineralized material, the zinc-containing mineralized material, the metasilicic acid-containing mineralized material, the carbonate-containing mineralized material, and the base material;

[0021] (3) The mineralized material and the base material are crushed again and mixed according to a weight ratio to obtain the composite mineralized material.

[0022] After the natural ore is initially screened, crushed, fired, soaked and carbonated, it is screened again to obtain the corresponding mineralized materials and basic materials. For example, after the strontium-containing ore is initially screened, crushed, fired, soaked and carbonated, it is subjected to component analysis to screen out the corresponding mineralized materials and basic materials for the subsequent preparation of composite mineralized materials.

[0023] The purpose of the crushing in step (1) is to improve the firing efficiency, reduce energy consumption, and facilitate the preliminary removal of harmful organic matter and metal elements in the ore to obtain safe and reliable mineralized materials. The firing time and temperature can be set according to the properties of the ore. When the C / O content of the natural ore exceeds 5%, the firing time is appropriately increased and the firing temperature is appropriately extended to burn out the organic components contained in the ore as much as possible. When the porosity exceeds 3m 2 / g of ore, the firing time can be appropriately reduced to reduce energy consumption.

[0024] Firing temperature can affect the amount of total dissolved solids (TDS) of composite mineralized materials after water immersion

[0025] For example, the firing temperature may be 600° C., 610° C., 620° C., 630° C., 640° C., 650° C., 660° C., 670° C., 680° C., 690° C., 700° C., 710° C., 720° C., 730° C., 740° C., 750° C., 760° C., 770° C., 780° C., 790° C., 800° C., and any temperature therebetween. The firing time may be 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, and any time therebetween.

[0026] Optionally, in step (1), the particle size of the ore after crushing is no more than 5 mm.

[0027] Optionally, the immersion time in pure water in step (2) is 12-72 hours. For example, the immersion time can be 12 hours, 16 hours, 20 hours, 24 hours, 28 hours, 32 hours, 36 hours, 40 hours, 44 hours, 48 ​​hours, 52 hours, 56 hours, 60 hours, 64 hours, 68 hours, 72 hours, and any time therebetween.

[0028] Soaking the fired ore in pure water can dissolve the powder or inorganic salts formed by the associated C / O in the mineralized material after firing in the pure water, and the residues after firing of organic matter such as C / O or moss in the base material can be dissolved in water, thereby improving the cleanliness of the mineralized material, facilitating the smooth progress of the subsequent carbonation treatment, and laying the foundation for the relatively stable dissolution of minerals.

[0029] Optionally, the carbonation treatment in step (2) is: after flushing with pure water, carbon dioxide gas is continuously introduced to keep the carbon dioxide in the water in a saturated dissolved state, and a carbonation cleaning treatment is performed, and the duration of the process is 1-4 hours.

[0030] For example, the carbonation time can be 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, and any time therebetween.

[0031] The above-mentioned carbonation cleaning treatment is to convert the calcium carbonate on the surface of the material into calcium bicarbonate and dissolve it. If the carbonation treatment time is less than 1 hour, the surface cleaning will be incomplete, and if the carbonation treatment time is more than 4 hours, excessive dissolution will occur and more material will be lost. In addition, the carbonation treatment carried out after firing can also improve the stability of minerals and achieve a relatively stable dissolution of elements.

[0032] The above-mentioned natural ore can be selected from the following areas: Hainan Chengmai volcanic rock, Pengshan Changshou mudstone, Tibet dolomite, Tianshan basalt, Changbai Mountain basalt, Kunlun Mountain phyllite, Tianshan limestone, Siming Mountain zeolite, Gongga Mountain olivine, Kunlun Mountain jade carbonate, Tianshan medical stone, Guangxi dolomite.

[0033] Optionally, the composite mineralized material has a stable strontium ion precipitation concentration, and the dissolution attenuation of the strontium ion precipitation concentration of the produced water after 2000L is ≤0.4ppm compared with the initial produced water strontium ion precipitation concentration.

[0034] According to another aspect of the present application, a water purifier is provided, which uses the above-mentioned composite mineralized material or the composite mineralized material obtained by the above-mentioned preparation method, and the water purifier is provided with a purification filter element, and the carbon rods made of the composite mineralized material and the mineralized particles made of the composite mineralized material are installed at the water purification output end of the purification filter element; or, the water purifier is provided with an RO filter element, and the carbon rods made of the composite mineralized material and the mineralized particles made of the composite mineralized material are installed in the central tube of the RO filter element.

[0035] The beneficial effects of this application include but are not limited to:

[0036] 1. The composite mineralized material of the present application can dissolve a variety of minerals as needed, according to the type and quantity of the mineralized material, thereby achieving the pure water remineralization function while meeting the water needs of different groups of people, and does not contain excessive metal elements and organic matter, thereby improving the safety and reliability of water use.

[0037] 2. The composite mineralized material of the present application can be set to different particle sizes according to the use requirements, and the particle size of the base material is adjusted accordingly for preparing carbon rods or directly filled into the filter element, thereby improving the application scenarios of the mineralized material.

[0038] 3. According to the preparation method of the composite mineralized material of the present application, the screened ore is calcined, soaked in pure water and carbonated to remove harmful substances and stabilize the mineral elements to obtain a safe and reliable multi-component mineralized material. The above treatment can make the minerals dissolve smoothly, reduce the scaling of the water purification device, and extend the service life of the water purification device. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0040] Figure 1 This is an appearance diagram of the mineralized material with a particle size of 120-200 mesh involved in Example 1 of the present application;

[0041] Figure 2 This is an appearance diagram of a carbon rod prepared by the carbon rod formula scheme 9 involved in Example 1 of the present application;

[0042] Figure 3 This is an appearance diagram of the mineralized material with a particle size of 1-5 mm involved in Example 2 of the present application. DETAILED DESCRIPTION

[0043] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0044] Unless otherwise specified, the raw materials in the examples and comparative examples of the present application were purchased through commercial channels.

[0045] Unless otherwise specified, the methods used in the examples and comparative examples of the present application are conventional methods in the prior art.

[0046] Example 1

[0047] This embodiment relates to a method for preparing a composite mineralized material, comprising the following steps:

[0048] (1) Selecting strontium-containing ore from natural ore, crushing the ore to a particle size of less than 5 mm, and calcining it for 3 hours;

[0049] (2) Soaking the fired ore in pure water for 24 hours, then rinsing with pure water and continuously introducing carbon dioxide gas to keep the carbon dioxide in the water in a saturated dissolved state, and performing carbonation cleaning treatment. The process lasts for 2 hours. After air drying, the composition analysis is performed to screen out the strontium-containing mineralized material and the basic material, wherein the strontium content in the strontium-containing mineralized material is not less than 0.05%, the content of lead, cadmium, chromium, mercury, and arsenic are all less than 0.005%, and the Si content in the basic material is 30%, the O content is 15%, and the C content is 15%;

[0050] (3) The mineralized material and the base material are crushed again, and the mineralized material is 5g, 10g, and 15g respectively, and then mixed with 25g, 20g, and 15g of the base material and 100g of activated carbon powder to prepare a carbon rod of 53*35*135. The particle size of the base material and the activated carbon powder is 60-300 mesh.

[0051] The carbon rod composite mineralized material was prepared according to the above steps. The specific conditions and the water quality of the detected water are shown in Table 1.

[0052] Table 1

[0053]

[0054] Figure 1 This is the appearance of the mineralized material with a particle size of 120-200 mesh. Figure 2 This is the appearance of the carbon rod prepared by Scheme 9 in Table 1. Figure 2 (A) is the test picture of the carbon rod. Figure 2(B) is a top view of the carbon rod. According to the data in Table 1, if the particle size of the mineralized material is too small, it will increase the loss, and if it is too large, it will fall off easily, so it is not compatible with the carbon rod. Only when the particle size is within the range of 80-200 mesh can it be compatible with the carbon rod. In addition, the particle size of the mineralized material will affect the dissolution concentration of the mineral; if the firing temperature of the ore is too low, the TDS content will increase, and there will be a risk of excessive organic matter. The firing temperature will also affect the dissolution rate of the mineral to a certain extent; in the carbon rod ratio schemes 6, 9, 13, 14, and 15, the composite mineralized materials all have stable strontium ion precipitation. Concentration, specifically, the dissolution attenuation of the strontium ion precipitation concentration in the produced water after 2000L compared with the initial produced water strontium ion precipitation concentration does not exceed 0.4ppm; at the same firing temperature, the amount of mineralized material added will affect the initial produced water strontium concentration and the produced water strontium concentration after 2000L, the more the amount of mineralized material added, the higher the initial produced water strontium concentration and the produced water strontium concentration after 2000L, but the difference between the initial produced water strontium concentration and the produced water strontium concentration after 2000L is roughly the same, which proves that the above schemes can achieve relatively stable dissolution of minerals and improve the consistency of water quality.

[0055] A water purifier is provided with a purification filter element, which can be an ultrafiltration filter element or a nanofiltration filter element. The purification filter element uses a carbon rod made of the above-mentioned composite mineralized material, and the carbon rod is specifically installed at the water purification output end of the purification filter element.

[0056] Example 2

[0057] This embodiment relates to a method for preparing a composite mineralized material, comprising the following steps:

[0058] (1) Selecting strontium-containing ore from natural ore, crushing the ore to a particle size of less than 5 mm, and calcining it for 2 hours;

[0059] (2) Soaking the fired ore in pure water for 24 hours, then rinsing with pure water and continuously introducing carbon dioxide gas to keep the carbon dioxide in the water in a saturated dissolved state, and performing carbonation cleaning treatment. The process lasts for 2 hours. After air drying, the composition analysis is performed to screen out the strontium-containing mineralized material and the basic material, wherein the strontium content in the strontium-containing mineralized material is not less than 0.05%, the content of lead, cadmium, chromium, mercury, and arsenic are all less than 0.005%, and the Si content in the basic material is about 30%, the O content is 10%, and the C content is 10%;

[0060] (3) The mineralized material and the base material are crushed and screened again to obtain 0.5-5 mm particles. The mineralized material is 100 g, 200 g, and 300 g respectively, and then mixed with 500 g of the base material to obtain a composite mineralized material. The particle size of the base material is 0.5-5 mm. The composite mineralized material is installed in the filter element of the water purification device for water quality monitoring. The specific conditions of the composite mineralized material and the water quality of the detected water are detailed in Table 2.

[0061] Table 2

[0062]

[0063]

[0064] Figure 3 The appearance of the mineralized material with a particle size of 1-5mm. According to the data in Table 2, when the mineralized material and the base material are used directly as filter elements, the particle size of the mineralized material affects the flow rate of the water purification device. If the particle size is less than 1mm, the water output of the water purification device will not be smooth and cannot be used normally. If the firing temperature is too low, the TDS content will increase, and there will be a risk of excessive organic matter. Secondly, the minerals will not be able to be dissolved smoothly. After 2000L, the strontium concentration of the produced water will not meet the standard, and the filter element needs to be replaced, which increases the cost and is inconvenient for users. At the same firing temperature, the amount of mineralized material added will affect the initial strontium concentration of the produced water and the strontium concentration of the produced water after 2000L. The amount of mineralized material added The more, the higher the initial strontium concentration in produced water and the strontium concentration in produced water after 2000L, but the differences between the initial strontium concentration in produced water and the strontium concentration in produced water after 2000L are roughly the same, which proves that the above schemes can achieve relatively stable dissolution of minerals and improve the consistency of water quality; in filter element ratio schemes 6, 10, 11, and 12, the composite mineralized material also has a stable strontium ion precipitation concentration. Specifically, the dissolution attenuation of the strontium ion precipitation concentration in produced water after 2000L compared with the initial strontium ion precipitation concentration does not exceed 0.4ppm; if the flow rate of the water purification device is too large, the dissolution of minerals will be reduced. Therefore, the filling amount can be adjusted according to different flow rate requirements to achieve the purpose of meeting the strontium concentration standard.

[0065] A water purifier is provided with an RO filter element. The RO filter element uses the composite mineralized material. The mineralized particles made of the composite mineralized material are specifically installed in the central tube of the RO filter element.

[0066] Example 3

[0067] Compared with the carbon rod formula scheme 6 in Example 1, this embodiment is adjusted. The specific conditions and the water quality of the detected water are detailed in Table 3. The “-” in Table 3 represents the same as the carbon rod formula scheme 6.

[0068] Table 3

[0069]

[0070] According to the data in Table 3, in the preparation process of basic materials and mineralized materials, the particle size of the ore after crushing becomes smaller, which will increase TDS, and the strontium concentration of the initial water production and the strontium concentration of the water production after 2000L decrease. The possible reason is that the smaller the crushing particle size, the greater the contact area of ​​the ore burning, which increases the pores on the ore surface, causing some strontium substances to burn out during the firing process, and TDS is more easily dissolved; too short a pure water soaking time will increase the dissolution of TDS, which cannot meet the demand. , and the strontium concentration dissolution amount also slightly decreased. If the pure water immersion time is too long, the TDS dissolution amount does not change significantly, but the strontium concentration decreases significantly, and the strontium concentration after 2000L of water production does not meet the standard; if the carbonation treatment time is too short, the TDS will increase and the strontium concentration will decrease. If the carbonation treatment time is too long, the TDS will increase and the strontium concentration will decrease. The strontium concentration after 2000L of water production does not meet the standard. Therefore, it can be seen that the carbonation treatment needs to be within an appropriate time range. The amount of basic material added will directly affect the dissolution amount of TDS and strontium concentration. If the basic material is too much, the TDS dissolution will increase and the strontium concentration will decrease. If the basic material is too little, not only will the TDS and strontium concentration increase, but strontium will not be able to achieve relatively stable dissolution.

[0071] Example 4

[0072] Compared with the filter element formula scheme 6 in Example 2, this embodiment makes further adjustments. The specific conditions of the composite mineralized materials are detailed in Table 4, wherein the particle sizes of the zinc-containing mineralized materials, the metasilicic acid-containing mineralized materials, and the carbonate-containing mineralized materials in Table 4 are all 1-5 mm. The water quality of the water detected by the filter element prepared above is shown in Table 5.

[0073] Table 4

[0074]

[0075] Table 5

[0076]

[0077] According to the data in Table 5, the richer the types of mineralized materials added, the more mineral content in the produced water. The composition of the composite mineralized materials can be adjusted according to demand. The carbonate-containing mineralized materials will affect the initial produced water pH, but the solution with carbonate mineralized materials added and the solution without carbonate mineralized materials added have the same produced water pH after 2000L. It can be selected whether to add some carbonate mineralized materials during the use of the filter element according to demand.

[0078] The above is only the embodiment of the present application, and the protection scope of the present application is not limited by these specific embodiments, but is determined by the claims of the present application. For those skilled in the art, the present application can have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the technical ideas and principles of the present application should be included in the protection scope of the present application.

Claims

1. A composite mineralized material, characterized in that: By weight, it includes: 5-15 parts of mineralized material and 15-25 parts of base material, wherein the mineralized material is selected from at least one of strontium-containing mineralized material, zinc-containing mineralized material, metasilicic acid-containing mineralized material and carbonate-containing mineralized material, wherein the strontium content of the strontium-containing mineralized material is not less than 0.05%, the zinc content of the zinc-containing mineralized material is not less than 0.5%, the silicate content of the metasilicic acid-containing mineralized material is not less than 3%, and the carbonate content of the carbonate-containing mineralized material is not less than 5%; The content of lead, cadmium, chromium, mercury and arsenic in the mineralized material is less than 0.005%; The basic material contains 15-50% silicon, 5-30% oxygen and 5-20% carbon.

2. The composite mineralized material according to claim 1, characterized in that: The mineralized material is at least selected from a strontium-containing mineralized material and a zinc-containing mineralized material in a weight ratio of 8:

2.

3. The composite mineralized material according to claim 1, characterized in that: When the particle size of the mineralized material is 80-200 meshes, the particle size of the base material is 60-300 meshes, and the composite mineralized material further comprises 60-100 parts of activated carbon powder with a particle size of 60-300 meshes, and the composite mineralized material is made into a carbon rod.

4. The composite mineralized material according to claim 1, characterized in that: When the particle size of the mineralized material is 1-5 mm, the particle size of the base material is 0.5-5 mm, and the composite mineralized material is directly filled into the filter element as mineralized particles.

5. The method for preparing the composite mineralized material according to any one of claims 1 to 4, characterized in that: The steps include: (1) selecting strontium-containing ore, zinc-containing ore, metasilicate-containing ore, and carbonate-containing ore from natural ores, crushing the above ores respectively, and calcining them at 600-800° C. for 1-4 hours respectively; (2) soaking the fired ores in pure water, and then performing carbonation treatment on them respectively, air-drying them, and then performing component analysis to screen out the strontium-containing mineralized material, the zinc-containing mineralized material, the metasilicic acid-containing mineralized material, the carbonate-containing mineralized material, and the base material; (3) The mineralized material and the base material are crushed again and mixed according to a weight ratio to obtain the composite mineralized material.

6. The preparation method according to claim 5, characterized in that: In step (1), the particle size of the ore after crushing is no more than 5 mm.

7. The preparation method according to claim 5, characterized in that: The immersion time in pure water in step (2) is 12-72 hours.

8. The preparation method according to claim 5, characterized in that: The carbonation treatment in step (2) is as follows: after rinsing with pure water, carbon dioxide gas is continuously introduced to keep the carbon dioxide in the water in a saturated dissolved state, and a carbonation cleaning treatment is performed. The duration of the process is 1-4 hours.

9. The preparation method according to claim 5, characterized in that: The composite mineralized material has a stable strontium ion precipitation concentration, and the dissolution attenuation of the strontium ion precipitation concentration of the produced water after 2000L is ≤0.4ppm compared with the initial strontium ion precipitation concentration of the produced water.

10. A water purifier, using the composite mineralized material according to any one of claims 1 to 4 or the composite mineralized material obtained by the preparation method according to any one of claims 5 to 9, characterized in that: The water purifier is provided with a purification filter element, and the carbon rod made of the composite mineralized material and the mineralized particles made of the composite mineralized material are installed at the purified water output end of the purification filter element; or, the water purifier is provided with an RO filter element, and the carbon rod made of the composite mineralized material and the mineralized particles made of the composite mineralized material are installed in the central tube of the RO filter element.

Citation Information

Patent Citations

  • Water-purifying filter element base material composition capable of resisting bacteria, sterilizing and supplementing mineral substances of human body and application thereof

    CN103496769A

  • Mixed water purifying filter material

    CN103880096A

  • Modified dolomites for hardening and tempering desalination water

    CN105692856A

  • Alkalescence zinc and strontium mineralized composite sintered activated carbon filter element and preparation method thereof

    CN108675429A

  • Extrusion molding strontium mineralization filter element and preparation method thereof

    CN112919850A

Cited By

  • Water quality information display method and device, water treatment equipment and storage medium

    CN119881258A